Thermal Runaway in Batteries: A Database-Driven Literature Review and Exploratory Statistical Analysis

and
Chair of Thermodynamics of Mobile Energy Conversion Systems, RWTH Aachen University, Aachen, Germany
*
Author to whom correspondence should be addressed.

Abstract

Thermal runaway (TR) in batteries remains a key safety challenge, yet its prediction is hindered by strongly coupled physics and many interdependent influencing factors. This review bridges the gap between mechanistic TR overviews and narrowly scoped experimental studies by conducting a broad database-driven review of published TR experiments. Therefore, the largest publicly available TR database to date is curated. It comprises 1703 tests from 257 papers and 203 variables describing cell properties, test conditions, and TR outcomes. Descriptive and pairwise inferential methods are applied to identify recurring patterns reported across the literature and to enable structured description of observed trends. Cathode chemistry, specific energy, and state of charge (SOC) emerge as the key associates of characteristic TR temperatures, with oxygen release from nickel-rich cathodes significantly amplifying TR severity. Aging-related effects strongly depend on the specific aging history and remain insufficiently characterized. Relative mass loss can reach 90% and is linked to the severity of TR reactions and the associated gas generation. On average, vent gas volume scales at 1.7 L/Ah, but capacity-normalized volume varies significantly with cell chemistry and SOC. H2, CO, and CO2 dominate vent gas compositions, with dependence on chemistry, SOC, and overall explosivity, while toxic and condensable species are clearly under-reported. The influence of abuse type and test setup on measured TR characteristics is highlighted, and emerging battery technologies are discussed. The database and derived trends provide a basis for benchmarking cell safety, informing pack-level design and modeling, suggesting future research directions, and supporting the development of standardized TR test protocols.

1. Introduction

In view of global climate change, the ongoing shift towards renewable energy sources has led to an increasing demand for electric energy storage solutions. Lithium-ion batteries (LIB) dominate the market in the growing electric vehicle (EV) and battery energy storage system (BESS) sectors owing to their high energy density, long cycle life, and superior charge efficiency [1,2]. Despite these advantages, safety still remains a major concern, potentially slowing down the widespread adoption of LIB [3].
With the growing number of LIB on the market, the number of fire accidents simultaneously increased [4,5]. Battery fires are often initiated by the thermal runaway (TR) of a single cell. Thermal runaway describes the sudden increase in cell temperature due to an exothermic chain reaction inside the cells’ active material that can be triggered by mechanical, electrical or thermal abuse as well as intrinsic cell failures. This chain reaction releases a lot of heat and is often accompanied by the ejection of hot, flammable, and toxic gases and particles. The TR in one cell can spread to neighboring cells, a process known as thermal propagation (TP) [6].
To increase the safety of battery systems and protect people and the environment, authorities have introduced regulations and standards to mitigate the effects of TR and TP for different application such as automotive [7,8,9], aeronautic [10], and stationary storage [11]. For instance, China’s recently adopted automotive standard, GB38031-2025, establishes rigorous safety standards, including prohibiting fires outside the battery pack, preventing vent gases in the passenger compartment, and preventing thermal propagation in the event of thermal runaway [9]. The design of fire safe battery systems provides several challenges for developers and requires extensive expertise in the thermal runaway behavior of different cells.
The growing relevance of LIB combined with the rising number of battery fire accidents, public perception of limited safety and increasing regulatory safety requirements has brought significant attention and resources to the field of thermal runaway research. According to Scopus, publications on “thermal runaway in batteries” grew exponentially from fewer than 100 to more than 1000 per year over the last decade [12]. During this period, several review papers were published that summarized the state of knowledge on TR mechanisms [6,13,14], emissions [15,16], modeling [5,17,18], detection [19,20,21], mitigation [22], accidents [23,24] and standards [24,25].
The first comprehensive reviews of TR were published by Feng et al. in 2018 [6,13]. They provided a general explanation of TR abuse by summarizing abuse conditions that lead to TR, mechanisms of the chain reactions during TR and possible mitigation measures [6]. Furthermore, they proposed a time sequence map to interpret the heat release mechanism of a cell with lithium-nickel-manganese-cobalt-oxide (NMC) cathode chemistry [13]. Key findings include that the oxidation-reduction reaction between anode and cathode is the major heat source, while the internal short circuit (ISC) acts as a trigger for this reaction but is not a major heat source itself. The fire during venting releases a lot of heat. However, most of this heat is dissipated into the surroundings rather than heating the cell.
Koch et al. measured 51 prismatic and pouch LIB with NMC cathode undergoing TR within an autoclave setup to study the vent gas volume and composition, cell mass loss and influencing factors on related parameters [26]. They identified the main gases released during TR to be CO2, CO, H2, C2H4, CH4, C2H6 and C3H6 in decreasing order and independent of vent gas volume. The vent gas volume increases roughly linearly with the cell capacity. The TR trigger temperature decreases with energy density and cell mass loss increases with decreasing onset temperature. There is a linear correlation between gaseous mass loss and total mass loss with prismatic cells having a higher solid to gas mass loss ratio than pouch cells. This study was limited to prismatic and pouch NMC cells in a capacity range of 20–81 Ah. It, therefore, disregarded other cathode chemistries as well as cylindrical cells and high and low-capacity cells. Furthermore, the focus lay on vent gases, and several other TR parameters were not investigated.
In 2019, Feng et al. summarized their activities on accelerated rate calorimetry (ARC) testing in a thermal analysis database including 42 different cells [27]. They identified three characteristic temperatures describing TR: the self-heating onset temperature T1, the TR trigger temperature T2 and the maximum TR temperature T3. T1 depends on the cell type and cathode material, not directly on specific energy. Cells aged at high temperature have higher T1, whereas cells aged at low temperature have lower T1. T3 and the maximum temperature rise rate (dT/dt)max increase with specific energy and state of charge (SOC). T3 is independent of T2. Material level test results by differential scanning calorimetry (DSC) could be linked to the ARC results and confirmed the understanding, that the anode–cathode redox-reaction is the major heat source of the TR. Limitations of this study include the restricted capacity range of 1–50 Ah as well as the focus on specific TR features and parameters.
Willstrand et al. conducted a large test campaign with 37 TR tests on a single 157 Ah prismatic NMC811 cell [28]. They observed that the trigger method impacts key parameters such as gas production rate, mass loss, and maximum temperature of the cell as much as the SOC. On the other hand, no significant differences could be observed in the results due to the different test setups, apart from differences due to potential combustion of the released gases in ambient atmosphere. This study is limited to a single cell and a few TR parameters.
Rappsilber et al. performed a meta-analysis of 76 experimental research papers published between 2000 and 2021 with the focus on heat and gas release and provided the raw data in the Supplementary Material [29]. The key findings are that the total TR heat release increases with SOC, and the specific peak heat release (kW/Wh) and total heat release (kJ/Wh) vary significantly and depend on cathode material. Cells with lithium-iron-phosphate (LFP) cathode chemistry have the highest specific total heat release. The specific quantity of gases (mmol/Wh) emitted tends to increase with SOC. The specific mass of CO (mg/Wh) increases with SOC presumably due to incomplete combustion and is higher for prismatic and pouch cells. The study limitations lie in the relatively small sample size for many statistical plots combined with the comparison of different experimental setups that may influence the results significantly. Furthermore, only a few specific TR features were analyzed.
In 2024, Finegan et al. published an open-access battery failure databank, which summarizes over 300 TR tests conducted in a custom made fractional thermal runaway calorimeter [30]. They monitored the mass and heat ejection behavior of commercial cylindrical cells under thermal and nail penetration abuse and found that heat release increases with cell capacity and mass ejected. Also, cells with silicon in their anode and high-power cells generate more heat per Ah. Multi-testing of a single cell type highlighted high variability between tests for some cells, which led to the conclusion that statistically relevant results require a high number of tests. Limitations of the study include the focus on specific TR features in a custom test setup that only allowed for testing of cylindrical 18650 and 21700 cells.
Bugryniec et al. investigated the vent gas release during TR in a meta-analysis of 60 papers [31]. They found that NMC cells generate larger specific vent gas volumes than cells with other cathode chemistries. The vent gas quantity increases with increasing SOC, and prismatic cells tend to generate higher specific vent gas volume than other cell types. LFP cells show greater toxicity than NMC cells based on HF and CO emissions and have a greater flammability hazard. The study limited its focus on TR vent gas release and disregarded other TR features.
Table 1 highlights the scope and limitations of previously discussed work. In summary, the existing large-scale TR test studies and meta-analyses obtained multiple valuable findings. However, they focused on specific aspects of TR and often used limited data to derive conclusions. Edge conditions as very high-capacity cells or new cell chemistries are not incorporated in the analyses. Furthermore, different test conditions can significantly influence key results.
Table 1. Scope and limitations of large-scale thermal runaway test studies.
This study aims to address above limitations by bridging the gap between high-level mechanistic reviews and very detailed but limited-scope experimental campaigns. It assesses the key parameters influencing thermal runaway behavior based on an in-depth review guided by an exploratory statistical analysis of a literature database on thermal runaway experiments. The primary focus of the database is on lithium-ion batteries due to the large number of studies on this cell technology. However, the thermal runaway behavior of emerging technologies, such as solid-state and sodium-ion batteries, shares many LIB TR characteristics. Respective studies are, therefore, included as well as. The database and the statistical correlations ranked by effect size were recently published in the open-access repository Zenodo [32]. To the best of the authors knowledge, this database is the largest publicly available source for thermal runaway experiments and summarizes 1703 TR tests from 257 papers in 203 variables. The aim is to provide a holistic summary of TR characteristics considering the relevant input and output parameters. The large number of samples enhances confidence in reported trends. In contrast to previous reviews, this study uses exploratory statistical analysis for the first time. Due to the high dimensionality of the database, this step is deemed necessary to allow for a structured data visualization and interpretation process. While the obtained pairwise correlations do not allow for predictive or causal modeling, associations that are consistently observable across a large number of studies can be derived. Effects of cell chemistry, format and size as well as impacts of different test specifications are investigated. Also, interactions between various results like TR temperatures, mass loss, venting characteristics, vent gases and particles paired with physics-based reasonings provide a comprehensive overview of typical TR behaviors. Gaps in the data are highlighted and serve as recommendations for future research. The findings can provide guidance in the concept stage of new battery developments, where experimental results are scarce and offer orientation to new engineers and researchers in the field. This study can be further used as a guideline for researchers on what to report when publishing experimental TR results and outlines future research directions to better understand TR in batteries.

2. Methods

The methods chapter, abstracted in Figure 1, is divided into the definition of the parameter set, the data acquisition, and the data post-processing and evaluation. Additionally, an overview of the sampled data is provided, and study limitations are outlined.
Figure 1. Schematic of the methodological workflow.

2.1. Definition of the Parameter Set

The aim of the database is to capture the relevant features in a TR experiment. Therefore, it contains 203 parameters that can be split into inputs and outputs. An overview of the parameter set with the number of valid entries per parameter is given in Figure 2. The major categories can be divided into source information, cell information, test specifications, key thermal runaway results, molar fractions of gas components and mass fractions of settleable particles. Some parameters are calculated from others. For reference, these calculations are summarized in Table 2.
Figure 2. Parameter set of the thermal runaway database with number of entries in brackets [32].
Table 2. Calculated parameters in the database.
Source information allow for identification of each paper. Cell information detail the cells investigated with regard to format, dimensions, energy stored, materials used, and thermal properties. Test specifications describe the thermal runaway boundary conditions. They include details about the trigger method and environment, initial conditions, like SOC and state of health (SOH) with specific aging parameters, cell configuration, i.e., single or multiple cell setups, as well as information on the gas and particle evaluation methods. The key thermal runaway results include the characteristic temperature definitions for self-heating onset T1, severe TR trigger T2 and maximum cell temperature T3 [27]. They are extended by the safety vent opening, voltage drop and maximum vent gas temperatures. The maximum cell temperature is divided in cell surface T3,ext and internal temperature T3,int. The maximum temperature rise rate (dT/dt)max, (relative) mass loss and different timings for TR duration estimation describe the fierceness of the TR reactions. Furthermore, the gas and particle emissions are summarized. For better comparison the total gas release and the average flow rate are additionally normalized by cell capacity. Gas composition is recorded as molar fractions of the different species measured. In case mass fractions are provided in the source, the molar fractions are calculated accordingly. Summarized over all sources, 47 different species could be measured in battery TR vent gases. Because many sources only provide the molecular formula, different isomers with the same molecular formula are condensed into a single species. Similarly, the atomic mass fractions of settleable particles analyzed in the papers are listed per chemical element. Only quantitative analyses are considered. Summarized over all sources, 34 different elements could be identified in TR abuse particles.

2.2. Data Acquisition

A thorough literature search in Google Scholar and Scopus was carried out to populate the database. In contrast to formal systematic meta-analyses, the dataset was assembled iteratively over an extended period. The search strategy was not constrained to a predefined protocol such as Preferred Reporting Items for Systematic Reviews and Meta-Analyses (PRISMA). It is, therefore, not intended to provide statistically unbiased or fully reproducible estimates. The following keywords were used in various combinations: “thermal runaway”, “batteries”, “experiments”, “vent gases”, “particles”, “lithium-ion”, “sodium-ion”, “solid-state”. In addition, first-level paper recommendations at the respective study websites as well as backward citation searches from referenced studies were considered. Studies are eligible for inclusion, if they fulfill the following criteria:
  • Thermal runaway experiments must be conducted at cell-level as a minimum. Material-level studies are excluded.
  • In case a study includes multiple different cell types or test conditions, e.g., different cathode materials or trigger methods, the reported data must be traceable to each individual test.
  • The study must be peer-reviewed or published by a reputable organization in the field, such as NREL or NASA.
  • The study must be written in English.
  • The study must be published before August 2025.
In total, 1703 TR experiments from 257 papers were added from open-access and closed-access sources. The database does not claim completeness and may be subject to selection bias but contains a significant fraction of the major studies in the field and is easily extendable.
All data were manually extracted from the sources and entered in an Excel file by a single researcher. This process mainly took between one and two hours per study, but sometimes up to six hours, depending on the reported level of detail and ease of data extraction. If data was only available in figure format, the online tool WebPlotDigitizer v4.8 [33] was used to extract the data from the plots. No further tools, e.g., based on Artificial Intelligence (AI), were applied. Inconsistent reporting across studies requires advanced domain knowledge and scientific judgement, which prohibits the use of reliable (partial) automation for data extraction. While this approach enabled consistent acquisition and interpretation of reported parameters across heterogeneous sources, it introduces potential risks of transcription errors and subjective judgment in cases of ambiguous reporting. Consequently, the database should be interpreted as a structured collection of literature data rather than a statistically controlled dataset. The primary objective is to capture a broad range of reported behaviors and enable comparative analysis across studies, rather than to provide unbiased population estimates.

2.3. Dataset Sample Overview

An overview of the sampled dataset is provided in Figure 3. Overall, the database contains several biases that need to be considered when drawing conclusions from this study.
Figure 3. Dataset sample overview—(a) year of publication; (b) cell format; (c) nominal capacity; (d) specific energy; (e) cathode material; (f) anode material; (g) abuse type; (h) test vessel type.
The oldest studies included date to the year 2011 (Figure 3a). Over the last 15 years, research on battery TR grew significantly, which is reflected by a peak TR test count of 376 in 2023. Note that 2025 studies are only included, if they were available in August. Almost half of the TR tests were conducted on cylindrical cells, followed by prismatic and pouch cells with a considerable margin (Figure 3b). Test efforts increase with larger cell size, considering investment costs and space for the required test equipment, costs for cell samples and auxiliary components such as jigs, and access to larger non-consumer cells. Therefore, cells with a capacity below 20 Ah are most often tested (Figure 3c). Additionally, self-made laboratory-scale cells fall into this range. Nevertheless, a considerable number of tests were performed over the whole capacity range up to 314 Ah. Herein, almost all cells with a capacity of over 200 Ah are LFP cells tested in 2021 or later. This aligns with the current trend towards large-format LFP cells, e.g., for battery energy storage systems (BESS). The specific energy of the cells ranges from 43–293 Wh/kg and is well distributed over the dataset (Figure 3d). Cells with NMC811 and LFP cathode material were tested most extensively, followed by lithium-cobalt-oxide (LCO), NMC532 and nickel-cobalt-aluminum-oxide (NCA) (Figure 3e). For 109 tests with NMC cathode chemistry, the exact composition was not provided. Blends of different cathode chemistries were tested rarely. This also applies to the cathode materials of sodium-ion batteries (SIB) from recent studies. Most cells contained graphite as anode material that is sometimes mixed with silicon (Figure 3f). Remarkably, in 241 tests the anode material was not provided. This number is significantly higher than for the cathode material (11). It can be speculated that these cells mostly used graphite anodes, which is assumed as a given by the respective authors. Hard carbon and soft carbon were exclusively found in SIB, while lithium-titanite-oxide (LTO) was rarely investigated. Regarding TR trigger method, overheating is the method of choice, followed by nail penetration and overcharging (Figure 3g). A few studies also investigated crush, external short circuit and combinations of external short circuit or overcharging with overheating. In overheating experiments, ARC testing is established as a standardized test approach to determine critical TR temperatures under adiabatic conditions. It represents the test vessel type with the largest test count (Figure 3h). To assess gas characteristics like total volume and composition, autoclave testing is the preferred method and follows ARC testing with the second highest number of tests in the dataset. Dedicated non-pressure-proof test chambers, combustion chambers that follow specific fire testing standards, and bunkers, i.e., large explosion-proof rooms, are also frequently used. Specialized test vessels include altitude chambers for pressure variation, cone calorimeters for battery fire analysis, fractional TR calorimeters for the calculation of different heat release contributions, hydraulic crush and nail penetration testers for mechanical abuse and ovens for elevated temperature testing.

2.4. Data Post-Processing and Evaluation

The data analysis was carried out in MATLAB R2023a. After importing the source Excel file, the dataset was reduced to variables suitable for statistical analysis and saved as a separate .mat file. For example, source information like author and DOI or non-categorizable text entries like comments were removed from the dataset, resulting in 178 remaining variables.
Given the multi-factorial nature of the dataset and the exploratory scope of this work, the statistical analyses were designed to identify potentially relevant relationships rather than to establish causal inference. The identified correlations, therefore, serve as guidance for subsequent visualization and engineering interpretation but are not suitable for statistical modeling or behavior predictions.
First, descriptive statistics are applied to obtain an initial understanding of the dataset, to identify outliers and to detect faults during data acquisition. For numeric variables, the average, minimum, maximum, median, mode, range, variance, standard deviation, 25% and 75% quartiles, interquartile range (IQR), skewness, kurtosis, covariance matrix and sample count matrix are calculated. For categorical variables, the counts and relative frequencies are evaluated for each category.
Second, inferential statistics are calculated. These can be classified into three groups: statistics between two numeric variables, a numeric and a categorical variable and two categorical variables. Categorical–categorical relationships mainly involve test input data, which do not provide insights into TR behavior, and are, therefore, disregarded. Three complementary effect size metrics are applied: Pearson’s r, Spearman’s ρ and omega-squared ω2. These metrics describe different relationship types and, therefore, do not produce conflicting results for the same variable pair. Numeric–numeric associations are calculated using Pearson’s r and Spearman’s ρ [34]. Pearson correlation describes the linear association between two continuous variables whereas Spearman correlation describes the monotonic association between two ranked variables. The latter is more robust against outliers, can identify non-linear correlations such as exponential or power law ones and can handle non-normally distributed variables. However, since it is ranked-based it loses information on the magnitude of the values. Therefore, both correlations are considered for later analysis. Both measures range between −1 and 1 with the extremes representing perfect negative/positive correlation. Effect size interpretation follows the thresholds given in Table 3, adapted from Cohen [35] since field-specific estimates are unknown. Numeric–categorical relationships are investigated using one-way analysis of variance (ANOVA), which compares the means of a numeric variable across groups of a categorical variable [34]. Categories with a sample size N < 10 are excluded from the analysis. To judge the effect size, the omega-squared ω2 value is calculated for each pair, representing the proportion of variance in the numeric variable attributable to group membership [36]. ω2 ranges from zero to one and is interpreted according to the ranges listed in Table 3, following Kirk [36].
Table 3. Interpretation of statistical effect sizes [35,36].
To judge statistical significance, first the p-value for each test is calculated. Because a large number of pairwise tests is performed, false discovery rate (FDR) correction using the Benjamini–Hochberg procedure with the significance threshold α = 0.05 is applied [37]. A correlation is considered statistically significant, if the resulting q-value falls below α. Additionally, results based on fewer than 20 samples in total were excluded to minimize coincidental associations and to ensure practical relevance.
In total, 2269 valid Pearson correlations, 2246 valid Spearman correlations and 1003 valid ANOVA tests are calculated. The results are published together with the database [32]. More advanced multivariate analyses such as MANOVA, Random Forest regression, or other machine learning approaches were not applied. While these methods are in principle capable of separating interdependent influences and estimating higher-order interactions, their reliable application requires sufficiently populated multidimensional data with limited missingness and consistent variable definitions. In the present literature-derived dataset, many variables remain sparsely populated and strongly coupled through study-specific experimental choices. Applying multivariate approaches would, therefore, require substantial preprocessing, imputation, and dimensionality reduction, potentially introducing additional assumptions and reducing interpretability. Consequently, pairwise statistics are intentionally used as an exploratory screening method to identify candidate relationships rather than to estimate independent or causal effects. The calculated pairwise statistics guide targeted visualization and engineering interpretation of the dataset. Statistically significant correlations with moderate or large effect size are predominantly considered for the discussion and an excerpt of the full results is summarized in table format in the Supplementary Material. Since correlation does not imply causality, correlations lacking plausible physical mechanisms are excluded from the tables and discussion to avoid misinterpretation. For example, a correlation between the cell mass loss and the gradient-based indicator for the self-heating onset temperature may exist statistically but lacks physical causality.
In the results visualization, additional individual filters are applied in order to mitigate shared-factor dependencies. For example, SOC was found to have a strong influence on the TR results in several studies [27,28,29,31] and is, therefore, frequently applied as additional filter variable. To enhance traceability, applied filters are documented within each figure caption. With this information each plot can be reliably recreated from the full database and the relevant sources cited therein [32]. For scatter plots an additional fit is often applied as visual aid to highlight the general trend in the data and the coefficient of determination R2 = r2 is printed. Considering the effect size thresholds defined in Table 3, the coefficient of determination can be interpreted as small, moderate, and large for R2 < 0.09, 0.09 ≤ R2 ≤ 0.25, and R2 > 0.25, respectively. Mostly, linear fits are used, but exponential and power law fits are applied for clearly nonlinear behavior or where the linear fit would result in unphysical values such as negative time duration for the given range of data. These fits do not represent validated physical models and should not be interpreted as predictive relationships, particularly in cases where data scatter is large. Statistical findings are complemented by physical reasoning and comparison with the established literature to assess plausibility. To enhance readability, qualitative statements are used to describe effect size and significance. The detailed statistics are not added in the main text for statistically significant correlations with moderate or large effect size. Instead, the interested reader is referred to the supplementary tables. For statistically relevant tests that are not discussed in the main text, additional comments are provided in the Supplementary Material.

2.5. Summary of Study Limitations

While this study aims to be the most comprehensive review of published thermal runaway experiments, several limitations must be acknowledged:
  • Because literature acquisition was iterative and partly citation-driven, selection bias cannot be excluded. Studies with higher visibility, stronger citation networks, English-language publication, or more extensive reporting may be overrepresented. The literature search is not exhaustive. Thus, important contributions may have been overlooked.
  • Data acquisition and processing by a single researcher introduces potential risks of transcription errors and subjective judgment in cases of ambiguous reporting. However, due to the extensive processing efforts, a double-blind extraction could not be employed, so this study relies on the specific domain knowledge and scientific judgment of the main author.
  • Data collection is constrained to English-language publications due to limitations in the authors’ language skills. In particular, contributions from Chinese research groups in battery thermal safety could not be covered.
  • The dataset is limited to studies published by August 2025 due to data processing and publication efforts. It, therefore, excludes the most recent work. An update of the publicly available database is targeted within the next two years.
  • Multiple variables are unevenly represented in the dataset as highlighted in Section 2.3. For instance, small-format cylindrical cells and overheating-triggered tests are overrepresented. This imbalance introduces sampling bias, which may influence the calculated statistics and observed relationships. The reported statistical trends reflect the currently available body of literature and, therefore, inherently place greater weight on conditions that have been studied more extensively.
  • The authors acknowledge the possibility of differences in the quality of published TR results due to variations in equipment, measurement methods, and presentation of results. However, they decided to avoid a quality-based weighting system because it is difficult to objectively judge the quality of the experimental work based solely on the written report. Such a system would introduce subjective rating bias. This limitation is partially mitigated by collecting a large dataset and considering only peer-reviewed studies and those from high-reputation institutions as a first-level quality control.
  • The statistical evaluation is restricted to pairwise relationships and does not quantify the independent contributions of variables. Although multivariate and machine learning approaches may provide additional insight into higher-order interactions, their application to the present literature-derived dataset is constrained by heterogeneous reporting, incomplete population of many variables, and confounding between experimental factors.
Considering these limitations, the presented results and conclusions should be interpreted as exploratory trends across a broad, non-exhaustive sample of experiments within the available literature, rather than as universal, population-level predictions of TR behavior. Applied pairwise statistics can detect frequently recurring associations, but ranking the importance of individual variables requires further multivariate analysis.

3. Results and Discussion

In this chapter, the influencing factors on thermal runaway behavior revealed by the exploratory statistical analysis are visualized and discussed. The findings are structured based on TR characteristics. First, the TR temperatures are investigated, followed by the TR durations. Then, the mass loss during TR, the venting characteristics, the TR vent gases and the TR vent particles are examined. Finally, aging-related effects are discussed, the influence of different test conditions is elaborated and a perspective on emerging battery technologies is provided.

3.1. Characteristic TR Temperatures

The characteristic TR temperatures include the self-heating onset T1, TR trigger T2, maximum external T3,ext and maximum internal cell temperature T3,int as well as the safety vent opening Tvent, voltage drop TV0, maximum vent gas temperature Tgas,max and maximum temperature rise rate (dT/dt)max. Figure 4 displays schematic temperature and voltage profiles showing the characteristic temperatures during a heat-wait-seek (HWS) test in an ARC test vessel. Based on the current state of research, the key TR reactions and processes in a LIB are highlighted. These reactions are referred to in physical explanations of observed statistics in the subsequent chapters. The TR process includes the solid electrolyte interface (SEI) layer decomposition and regeneration reactions, the electrolyte vaporization, the anode–electrolyte reaction, the cathode decomposition and oxygen release, the decomposition and oxidation of the electrolyte, the lithium salt decomposition, the separator failure and internal short circuit (ISC), the anode–cathode redox-reaction, and the decomposition and oxidation of the binder [16,38,39,40,41]. Note that the exact order and the associated heat release may change based on the specific cell.
Figure 4. (a) Schematic temperature and voltage profile during a heat-wait-seek test, and (b) sequence of thermal runaway reactions in lithium-ion batteries summarized from [16,38,39,40,41].
While the indicators for the vent opening and voltage drop temperatures are self-explanatory, the indicators for the self-heating onset and TR trigger may influence the results. These temperatures are defined based on a specific temperature rise rate. The gradients are typically 0.02 K/min for T1 and 60 K/min for T2 but may range from 0.005 K/min to 0.2 K/min and 0.2 K/min to 600 K/min, respectively. The chosen gradient has a moderate effect on T1, ρ(428) = .377, q < .001, but is insignificant for T2, ρ(549) = .085, q = .089. This can be explained by the large temperature range with relatively low heating rate around T1 and the small temperature window around T2 in which the gradient grows rapidly. The maximum external temperature reading loosely depends on its indicator, F(6, 1317) = 6.57, q < .001, ω2 = .025. It can be given as an averaged maximum value over multiple tests, an averaged maximum value over multiple thermocouples, an averaged maximum value over multiple cells in a module, or as the overall maximum value. Note that the majority of T3,ext values in the database are given as the overall maximum. It is recommended to always provide the specific definitions to enhance clarity, when characteristic TR temperatures are analyzed.

3.1.1. Self-Heating Onset Temperature

The key dependencies for the self-heating onset temperature T1 are shown in Figure 5. This temperature can only be measured in an ARC setup, i.e., in quasi-adiabatic conditions. T1 shows a moderate association on the cathode material (Figure 5a). Specifically, LFP and LCO cells have higher onset temperatures around 120 °C, whereas NCA and NMC cells range between 90 °C and 100 °C. Notably, NMC622 cells have a lower median, but also the highest spread in the IQR. The self-heating onset is linked with the heat release of the SEI layer decomposition and regeneration reactions [27]. The observed differences should, therefore, not be interpreted as isolated cathode effects. Since the SEI regeneration involves reactions of the intercalated lithium in the anode lattice and the electrolyte, the chosen electrolyte and the degree of lithiation, i.e., the SOC affects the self-heating temperature. While, in principle, a strong and significant correlation can be obtained for the electrolyte composition (see Table S1), the sample size is too low for a reasonable comparison when filtering for the covariates SOC and SOH. The moderate effect of SOC is presented in Figure 5b, which is enhanced when coupled with the specific capacity and cell mass in the form of a SOC-corrected specific capacity. Specific capacity is chosen over specific energy since it scales linearly with SOC. It can be concluded that less lithium intercalated at the anode side and less specific charge content are associated with less initial heat release and, therefore, higher self-heating onset temperature. For aged cells, the aging history strongly influences T1. The aging temperature has a large effect on T1 as shown in Figure 5c. Similarly, the aging cycles are positively correlated (Figure 5d) because at lower temperature less cycles are required to degrade the cell to the same SOH. At lower cycling temperatures, lithium plating is enhanced, which leads to a less stable SEI and higher reaction rate between lithium and the electrolyte, resulting in lower self-heating onset [42,43]. At higher cycling temperature but below abusive temperatures, the SEI regeneration reaction is faster than its decomposition resulting in SEI layer growth, which in turn reduces the initial reactivity under thermal abuse conditions [42]. The observed trends mainly originate from cyclic aging studies, whereas calendar aging remains underrepresented in the dataset. Furthermore, aging temperature, cycle count, current load and achieved SOH are interdependent variables and cannot be interpreted independently. Consequently, the present analysis focuses on identifying aging-related associations with T1 rather than establishing a generalized comparison between calendar and cyclic aging mechanisms. Notably, T1 shows strong correlation with the separator material, although at low sample size after covariate filtering. However, no physical explanation can be given for the influence on T1 and it may be linked to confounding effects in the material selection for specific cells.
Figure 5. Self-heating onset temperature T1 depending on (a) cathode material (SOC = 100%, SOH = 100%), (b) SOC-corrected specific capacity and cathode material (SOH = 100%), (c) cyclic aging temperature and SOH (SOC = 100%, AgingType = cyclic), and (d) aging cycles and aging temperature (SOC = 100%, AgingType = cyclic) with common filters (TestVesselType = ARC, HeatingRateOverchargingRateNailSpeed = HWS).

3.1.2. Vent Opening Temperature

The SEI decomposition and regeneration reactions produce gases such as CO2, C2H4 and O2 that accumulate inside the cell [44]. Furthermore, the electrolyte starts vaporizing at their respective boiling temperatures, which are 91 °C for dimethyl carbonate (DMC), 110 °C for ethyl methyl carbonate (EMC), 126 °C for diethyl carbonate (DEC), 242 °C for propylene carbonate (PC) and 248 °C for ethylene carbonate (EC) at atmospheric pressure [45]. These gas generation processes cause pressure build-up and eventually lead to rupture of the cell. The vent opening temperature Tvent is a characteristic of the TR process. While prismatic and cylindrical cells have a burst disk built into the cell casing, pouch cells open less reliably at a weak spot of their foil. Due to their weaker structure, pouch cells tend to open at lower temperature compared to hard case cells as shown in Figure 6a. Similar to T1, the vent opening temperature depends on the cathode material. LFP cells open at higher temperatures, attributed to the lower initial gas generation. Thus, a strong correlation between self-heating onset and vent opening temperature can be observed (Figure 6c). Towards higher temperature, the linear fit approaches the identity line, suggesting that electrolyte vaporization becomes the driver of vent opening. Figure 6b shows the dependency on SOC and nominal capacity. No SOC dependency can be found between 0% ≤ SOC ≤ 100%. However, overcharged cells open at much lower temperatures highlighting a large effect of abuse type. During overcharge, once the cathode potential exceeds the stability limit of the electrolyte, the electrolyte decomposes, leading to continuous gas generation [46]. Notably, cell dimensions, nominal capacity and nominal energy are mainly statistically relevant (Table S2) due to overcharge tests in the database being performed on larger cells as highlighted by the color scale. When filtered for SOC = 100%, electrolyte composition and separator choice don’t show significant differences (Figure 6a). The variations in active material shape are linked to the cell format. It is worth mentioning that 27 pouch cell tests arise from the same study by Feinauer et al. [47]. They tested an NCA/LCO cell with DEC:DMC:EC:EMC electrolyte, polyethylene (PE) separator and 2-stack active material shape in an ARC test environment at different SOH. This explains the narrow ranges in the respective properties. Consequently, no strong dependency of the vent opening temperature on SOH is observed within the available dataset. However, this result should not be interpreted as evidence that SOH generally has negligible influence on vent opening behavior, as additional studies are required to underline this conclusion.
Figure 6. Vent opening temperature Tvent depending on (a) cell characteristics (SOC = 100%), (b) SOC and nominal capacity, and (c) self-heating onset temperature T1 and cathode material (SOC = 100%, SOH = 100%).

3.1.3. Voltage Drop Temperature

The voltage drop temperature TV0 is reached when an external voltage sensor reads a voltage close to zero. Voltage sensing typically relies on a minor current flow to determine the corresponding voltage. Therefore, cutting the current circuit will lead to a drop in the measured voltage. Many cylindrical cells and some prismatic cells possess a current interrupt device (CID) that cuts the current flow in case of internal pressure build-up. That is why the cell format affects the voltage drop temperature as presented in Figure 7a. The CID is triggered prior to the safety vent as all datapoints of cylindrical cells fall below the identity line in Figure 7b. A strong correlation, i.e., a large effect size can be attributed to the vent opening temperature since both phenomena can be related to the internal pressure build-up. Another mechanism for the voltage drop is the shut-down of the separator pores that restrict ion flow from anode to cathode during voltage measurement. For example, Tang et al. observed this shut-down behavior on a polypropylene separator by scanning electron microscopy [48]. Although not enough data is available for different separator types to draw statistical conclusions, the aforementioned study by Feinauer et al. on NCA/LCO pouch cells [47] reveals a voltage drop slightly above the melting temperature of the PE separator (Figure 7c). Interestingly, this behavior can be observed independent of SOH, whereas the trigger of the CID in cylindrical cells is SOH dependent due to the linkage to gas generation reactions. When the CID or the separator shutdown do not cause the voltage to drop to zero, a slow voltage decay can be typically observed during overheating experiments at elevated temperatures. This decay is attributed to the change in electrode potential due to the loss of lithium inventory by the reaction of the lithiated anode with the electrolyte, which is accelerated at higher temperature [49]. Finally, the electrochemical potential will vanish during the severe TR phase driven by internal short circuit and the anode–cathode redox-reaction, which starts from the TR trigger temperature T2 [50]. Cells with this behavior can be found on or beneath the identity line in Figure 8d. The different factors causing the voltage to drop explain the vast range of measured temperatures, e.g., for different cathode materials (Figure 7a). Understanding the relevant mechanism per test is therefore required to properly interpret TV0.
Figure 7. Voltage drop temperature TV0 depending on (a) cell characteristics (SOH = 100%), (b) vent opening temperature Tvent and format (SOC = 100%, SOH = 100%), and (c) SOH, format and cathode material (SOH < 100%, AgingType = cyclic).
Figure 8. Thermal runaway trigger temperature T2 depending on (a) cell characteristics (SOC = 100%), (b) SOC-corrected specific capacity and SOC, (c) vent opening temperature Tvent and SOC, and (d) voltage drop temperature TV0, SOC and format.

3.1.4. Thermal Runaway Trigger Temperature

The TR trigger temperature T2 is reached when the temperature rise of the cell is considered significantly fast, typically in the order of 1 K/s, indicating the start of the fierce TR. T2 is only considered in the database, if an almost homogeneous surface temperature can be expected in the test at TR onset. This, for example, excludes one-sided overheating tests with a large temperature gradient across the cell. Multiple reactions take place at this temperature, which differ depending on the exact cell chemistry. Many cathode materials undergo exothermic phase transitions accompanied by the release of oxygen at elevated temperature [6,38,41]. The released oxygen can combust the electrolyte and react with the lithiated anode [13,39]. The thermal stability of the cathode material has a major impact on T2 as shown in Figure 8a. High nickel proportion in the cathode active material results in lower TR trigger temperature, since the thermal stability decreases with increasing Ni content [51]. This behavior can be observed for NMC and NCA cells in the database. Although LFP cathodes are inherently more stable and most likely do not release significant oxygen due to the strong P=O bonds [6], the T2 median is in the same range as for low nickel content NMC cells. Therefore, other reactions must contribute to the onset of TR. The already ongoing reaction between the lithiated anode and the electrolyte is further accelerated towards T2 [39,49]. Furthermore, electrolyte decomposition occurs independent of oxygen availability [6,38]. Also, internal short circuit due to separator failure may cause TR. Lithium-manganese-oxide (LMO) has a high TR trigger temperature as well with NMC/LMO cells having the highest median T2, confirming that LMO possesses relatively high thermal stability [52,53]. Electrolyte and separator choice are tested significant with large effect size in the statistical analysis. This makes sense, given that multiple degradation reactions involve the electrolyte, and ISC caused by separator failure is a possible trigger for TR. However, when filtered for SOC = 100% in Figure 8a, these strong dependencies cannot be observed. Cells without DMC in their electrolyte, i.e., with EC:EMC mixture have slightly higher T2. Similarly, cells with ceramic-coated PE separators are slightly more resilient to TR onset. Apart from that temperatures are similar. Figure 8b shows the dependency of T2 on the SOC-corrected specific capacity. High specific capacity and high SOC lead to significantly reduced TR trigger temperature. The higher the specific capacity, the more reactive sites are present per cell mass, leading to faster temperature increase according to the first law of thermodynamics. At high SOC the anode lithiation is high, resulting in accelerated anode–electrolyte reaction [54]. Accordingly, the cathode lithiation is low, which destabilizes the structure and favors oxygen release [55,56]. This behavior is exaggerated for overcharged cells, whose points almost exclusively fall below the linear fitting line. Due to the lithium deposition on the anode surface, the anode–electrolyte reaction is further accelerated in overcharge scenarios [57,58]. Earlier heat release is also caused by the additional electrochemical decomposition of the electrolyte at the high voltage cathode [53,59]. Ren et al. cut the foil of a pouch cell before overcharge and found that when releasing the generated gases efficiently the TR onset can be significantly delayed [57]. Figure 8c depicts a linear trend between the vent opening and TR trigger temperature. Since T2 is linked to the rates of the degradation reactions, which in turn are often accompanied by gas release; these findings are reasonable. For all cells with determined venting temperature, Tvent < T2 applies, enabling early TR detection by measuring the gas concentration of initially vented gases. As mentioned in Section 3.1.3, cells exhibiting a voltage drop at or following severe TR onset can be located on or below the identity line in Figure 8d. Notably, the SOH has no significant effect on the TR trigger temperature based on the data, r(793) = .064, q = .152. With fresh cells excluded, the coefficient of determination increases to R2 = 0.07, still showing small effect size. Two larger studies were conducted by Feinauer et al. [47] and Ren et al. [60]. The former observed no impact of SOH on T2, while the latter found adverse behavior depending on aging type, current and temperature. Aging temperature is the only aging parameter with a significant Pearson correlation in the database, but small effect size, r(97) = .267, q = .024. Aging cycles and discharge C-rate have a significant positive Spearman correlation with moderate effect size. Aging cycles show a slightly positive trend when filtering out highly cycled cells above 1000 cycles. Low temperature and high current cycling enhance lithium plating, which shifts the anode–electrolyte reaction to lower temperatures similar to overcharged cells [57,60]. The number of cycles required to age the cell to a specified SOH is linked to the other aging parameters, hence the correlation.

3.1.5. Maximum External Cell Temperature

The maximum temperature a cell can reach is defined by the total heat release of all TR reactions. Since the temperature field during TR is inhomogeneous, the location of the temperature measurement matters. First, the maximum external cell temperature T3,ext is discussed and the results are shown in Figure 9. Specific energy is one of the main influencing factors on T3,ext (Figure 9b). With increasing specific energy, more reactive material is available per unit mass, resulting in larger temperature rise according to the first law of thermodynamics. The specific energy is a kind of proxy variable for the underlying cell chemistry and design choices. It is mainly influenced by the chosen cathode material and cell format, whose effects on the maximum temperature can be observed in Figure 9a. Although the effect size for cell format is small due the overall high variance within each format, a significant correlation can be confirmed, F(2, 1327) = 26.3, q < .001, ω2 = .037. Pouch cells have the highest active material to cell mass ratio, followed by cylindrical and prismatic cells. The T3,ext medians therefore follow the same order. Large effect size can be attributed to the cathode material. Initially, ISC was considered to be the main heat release mechanism in the TR process. However, although it can be an initiator, it is not a major heat source itself [13]. Indeed, TR can be triggered without ISC [61]. The current state of research suggests that, in cells with oxygen-releasing cathodes, the anode–cathode redox-reaction is the major contributor to the total heat release [13,38,39,61]. Additional reactions that are triggered at T > T2 are the decomposition and oxidation of the electrolyte and the decomposition and oxidation of the binder [38,62]. Nickel containing cells experience higher peak temperatures, due to the lower thermal stability of the cathode material [51]. Interestingly, the median peak temperature reduces slightly for high nickel NMC cells although their oxygen release is higher [51], which should result in higher heat release by the oxygen dependent reactions. This behavior may be linked to higher mass loss and subsequent lower degree of reactant conversion as will be discussed in Section 3.2. For LFP cells the cathode active material contribution to the overall heat release is minor. The anode–electrolyte reaction generates the most heat [27]. Because of the reduced overall heat release, LFP cell peak temperatures are lowest across all cathode materials. Electrolyte composition has a large and significant effect on T3,ext. This can be attributed to the variation of decomposition and oxidation behavior across different electrolytes [38]. Furthermore, electrolytes with higher boiling temperature are more likely to remain inside the cell in scenarios where safety venting occurs and thus contribute more effectively to the TR processes. A possible interdependency between cathode material and electrolyte choice must also be considered as a cause of deviations. Similarly, ceramic-coated separators seem to be preferably used in highly reactive cells as an additional safety precaution. Cells with ceramic-coated shut-down separator depict the highest median peak temperature. The statistical analysis reveals a strong positive correlation between the in-plane thermal conductivity of the cell and the measured external peak temperature. Although the sample size is small (N = 30) and interdependencies with other factors like cathode material and cell format may exist, a possible physical explanation is the enhanced propagation of the reaction front inside the cell with higher thermal conductivity. This leads to faster heat release and diffusion, which may result in higher cell surface temperature. The maximum external cell temperature positively correlates with SOC, r(1342) = .275, q < .001. The calculated small effect size originates from the overlaying effect of other covariates with stronger correlations especially for the many tests conducted at SOC = 100%. When filtering for cells with SOC < 100%, the coefficient of determination increases to R2 = 0.22. Several TR reactions depend on the degree of lithiation of the active materials. At lower SOC the heat release by the anode–electrolyte reaction is diminished due to the reduced lithium concentration [54,63,64]. Furthermore, the phase change at the cathode is mitigated and the oxygen release is limited [55,56], which reduces the heat release by the cathode–anode reaction and electrolyte combustion [64,65,66]. SOH has no significant effect on T3,ext, r(1346) = −.003, q = .979. For example, Ren et al. could only observe a decrease for cells aged with a high cycle current, which they attributed to the electrolyte consumption during cycling, whilst all other abuse types showed no effect [60]. Contrary to this, Essl et al. measured decreasing peak temperatures for all aging types tested [67]. Therefore, findings in the literature are inconclusive and further research is necessary. In contrast to previously described characteristic TR temperatures, T3,ext does not correlate a lot with other temperatures. When filtering for fully charged and fresh cells, only the TR trigger temperature has a small effect on T3,ext with R2 = 0.04. Both temperatures are linked to the thermal stability of the cell. The influence of other temperatures is negligible.
Figure 9. Maximum external cell temperature T3,ext depending on (a) cell characteristics, and (b) specific energy and cathode material, with common filters (MainTRTriggered = yes, SOC = 100%, SOH = 100%).

3.1.6. Maximum Internal Cell Temperature

As mentioned earlier, the temperature distribution during the severe TR process is very inhomogeneous. To obtain a better understanding of the actual temperature in the reaction zone, some researchers incorporated one or multiple thermocouples into the cell before abuse. Special care must be taken to ensure operator safety and to not manipulate the cell behavior with the modifications done. A typically applied process is for example described by Wang et al. [68]. Note that imminent electrolyte vaporization and the change of thermal contact resistances inside the cell due to the inserted thermocouple may slightly alter the TR behavior. The main effects on the maximum internal cell temperature T3,int are summarized in Figure 10. The ANOVA tests can only be calculated for a few categorical variables since many categories fall short of the ten-sample threshold. No significant results are identified. To still visualize the effect of cathode material, which is expected to be one of the major influencing factors, the sample count threshold for plotting is reduced to five (Figure 10a). Although based on small sample counts, a clear trend can be observed. The internal cell temperature increases with increasing nickel content in the cathode material. The higher heat release is caused by the higher oxygen release that fuels the electrolyte combustion and anode–cathode redox-reaction [38,51]. This observation is contrary to that for T3,ext and thus, suggests that the internal cell temperature is less affected by the cell mass loss than externally measured temperature. This is probably because significant heat transfer to the sensor location and heating of the inactive cell housing mass is not required before detection. The highest internal temperature measured in the database is 1266 °C. At temperatures above 1000 °C the cathode active material may react with the aluminum current collector in a thermite-like reaction enabling an additional reaction pathway with significant heat release [69,70]. Molten and re-solidified copper particles vented from the battery cell confirm local internal cell temperature above 1085 °C [71]. Naturally, the peak internal temperature is strongly correlated to the maximum external cell temperature as shown in Figure 10d. For one LFP cell with medium SOC, T3,int falls below the identity line. In this case, the temperature on the cell side where the heater was placed was higher, showcasing the overall low heat release of moderately charged LFP cells. However, for many cells the internal cell temperature exceeds the externally measured temperature by several hundred Kelvin. This highlights the necessity for internal temperature measurements to derive the true TR temperature in the reaction zone. For simulation activities, space resolved TR modeling is required, since non-dimensional models calibrated on external temperature may underestimate the TR heat release and cannot capture temperature gradients throughout the cell. By incorporating thermocouples between each of the four jellyrolls in a prismatic 156 Ah NMC532 cell, Wang et al. could for example confirm the internal reaction front propagation from one jellyroll to the next by thermal diffusion [68]. SOC and specific energy both have a strong effect on T3,int. When plotting against the SOC-corrected specific capacity a high coefficient of determination can be obtained (Figure 10b). Compared to the maximum external cell temperature, a negative correlation is found between the internal cell temperature and the self-heating onset temperature but limited to a few datapoints (Figure 10c).
Figure 10. Maximum internal cell temperature T3,int depending on (a) cathode material (SOC = 100%), (b) SOC-corrected specific capacity, cathode material and specific energy, (c) self-heating onset temperature T1 (SOC = 100%), and (d) maximum external cell temperature T3,ext, cathode material and SOC.

3.1.7. Maximum Temperature Rise Rate

The maximum temperature rise rate (dT/dt)max is an indicator for the explosivity of a TR event. Since the values span over several orders of magnitude, the logarithm is taken for statistical analysis to get closer to normally distributed data. Note that proper temperature resolution is necessary to detect the highest gradient. If the sampling frequency during the test is too low, artificial gradient damping may occur. Also, fast response thermocouples are necessary because thermal inertia of the thermocouple may be the limiting factor during very fast temperature rises. The key results of the statistical analysis are summarized in Figure 11. In line with the previously discussed oxygen release that fuels the main heat release reactions, LFP cells have temperature rise rates that are one to two orders of magnitude lower than those of LCO or nickel-containing chemistries. Meanwhile, NMC811 cells have the highest rates (Figure 11a). The fastest temperature rise rate measured is 1288 K/s, indicating explosion-like behavior. In addition to the cathode material, the composition of the electrolyte and separator also have statistically significant effects on the maximum temperature rise rate. Both dependencies can be most likely explained by confounding effects in the material selection. Feng et al. studied the gas-phase reactivity of common electrolytes and derived the following reactivity ranking: DEC = EMC > DMC > EC [72]. This aligns with the lower temperature rise rate of cells without EMC. However, the sample sizes are small and for example, the maximum external temperature variations (Figure 9a) cannot be explained with these findings. An intuitive relationship can be observed between the maximum temperature rise rate and the peak temperature measured on the external cell surface (Figure 11b) as well as inside the cell. Cells with higher heat release tend to also release the heat quicker. This may be reasoned by the self-accelerating behavior of exothermic reactions. With higher temperatures, the reaction rate increases, which in turn leads to accelerated temperature rise. A strong Pearson correlation exists for specific energy, and moderate correlations are found for SOC and energy density. The coefficient of determination for SOC even increases to R2 = 0.41, when filtered for cells with SOC < 100%. These findings are summarized in Figure 11c using the SOC-corrected specific capacity. As discussed before, many TR reactions are decelerated with lower SOC due to their dependency on the degree of active material lithiation. Furthermore, with more reactive material per unit mass and volume, respectively, heat-up is accelerated according to the first law of thermodynamics and due to closer proximity of reactive sites. This is also shown by the positive Spearman correlation of the calculated cell density showcasing that more potentially reactive mass in a smaller volume tends to result in more explosive behavior. A significant Pearson correlation for cell density does not exist due to a few outliers with unreasonable values. Interestingly, no correlation can be observed for SOH, r(561) = −.003, q = .994, but relatively little data is available for SOH < 100%.
Figure 11. Logarithmic maximum temperature rise rate log(dT/dtmax) depending on (a) cell characteristics (SOC = 100%), (b) maximum external cell temperature T3,ext (SOC = 100%), and (c) SOC-corrected specific capacity and specific energy.

3.1.8. Maximum Vent Gas Temperature

During thermal runaway, the gaseous reaction products are vented from the cell. The dependencies of the maximum vent gas temperature Tgas,max are shown in Figure 12. To avoid mixing vent gas temperatures and combustion temperatures, the reported gas temperatures must be measured in vacuum, inert atmosphere or without any ignition observed during the experiment to be considered for this analysis. This inherits dependencies on the test vessel type and gas atmosphere (Figure 12a). Autoclave tests in an inert atmosphere mitigate combustion for all gas temperatures. In contrast, combustion can only be mitigated inside a combustion chamber with an air atmosphere, if the vent gas remains below its ignition temperature. Interestingly, all flameless tests in air resulted in a vent gas temperature below 500 °C, which can serve as a rough threshold for vent gas ignition. Note that the ignition temperature depends on multiple factors like vent gas composition, but such investigation is beyond the scope of this work. The cathode material has a strong effect on the vent gas temperature (Figure 12a). LFP cells can experience cold venting and gas temperatures in the database remain below 400 °C. On the contrary, the dataset shows that NMC622 cell gas temperatures reach up to 1306 °C and cover a wide range. Although the nickel content is only slightly lower, NMC532 gas temperatures are significantly lower than NMC622 temperatures. This, in combination with the high range observed for NMC622 suggests further important influencing factors. Strong positive correlations for specific energy and maximum external cell temperature can be observed (Figure 12c). With higher reactivity and heat release, the vent gas temperature increases. For almost all cells with low external surface temperature T3,ext > Tgas,max applies, whereas for many cells with high external surface temperature the vent gas temperature lies above the identity line. The NMC532 cells possess moderate specific energy resulting in modest vent gas temperature. Many significant correlations are calculated for cell size related variables. These are most likely caused by confounding effects as can be exemplarily seen in Figure 12b when plotting the cell mass, nominal capacity and cathode material together. Heavy large capacity cells have significantly lower vent gas temperatures. However, these are LFP cells and sodium-ion batteries with NaNi2/9Cu1/9Fe1/3Mn1/3O2 (Ni2Cu1Fe3Mn3) cathode material. Similar observations can be made for width, height and nominal energy. Due to limited samples no statistical conclusion can be drawn on the effect of SOC. A correlation may be anticipated because SOC and vent gas temperature both correlate with the external cell temperature, but only six tests with SOC ≠ 100% are available. Similarly, only three datapoints exist for cells with SOH < 100%. Although evaluated statistically significant for Pearson and Spearman correlations, no interpretation is attempted on this basis.
Figure 12. Maximum vent gas temperature Tgas,max depending on (a) cell characteristics and test setup, (b) cell mass, nominal capacity and cathode material, and (c) maximum external cell temperature T3,ext, specific energy and cathode material.

3.1.9. Summary of Temperature Findings

A high-level summary of the TR temperature-related findings is provided in Table 4. The strength and direction of different input parameters is given and a classification of the confidence level based on a color code is provided. Due to possible confounding effects and to improve clarity, variables are lumped into high-level parameters. This includes lumping the electrode material, electrolyte and separator choice into cell chemistry; the cell format and active material shape into cell design; the cell dimensions, cell mass, nominal capacity, and nominal energy into cell size; and the aging type, aging temperature, and aging C-rates into aging history. A moderate or large effect on all temperature variables can be attributed to cell chemistry with mostly high certainty. It is assumed that the cathode material and specifically the associated oxygen release has the largest impact. LFP and LCO cells exhibit higher self-heating onset temperatures than NMC and NCA cells, while Ni-rich NMC and NCA cells show lower TR trigger temperature and higher maximum temperature and temperature rise rate, reflecting their lower thermal stability and stronger oxygen release. The cell design affects the vent opening and voltage drop temperature significantly but has no influence on the remaining temperature parameters. Cell size has negligible effects on most variables. In case of vent opening, internal cell and maximum gas temperature, a moderate negative correlation can be anticipated, but with low confidence level due to an imminent bias by cathode material choice. The specific energy, and similarly the energy density and specific capacity, have no effect on the vent opening or voltage drop temperature, but large impact on the temperature rise rate and maximum gas temperature as well as moderate positive effect on the peak cell temperatures. A moderate decrease can be observed for the self-heating onset and TR trigger temperature rendering earlier TR onset for energy dense cells. For higher charged cells, the TR trigger temperature tends to decrease due to accelerated anode–electrolyte reaction at higher anode lithiation. Furthermore, the TR severity driven by enhanced lithiation-related reactivities increase as can be seen from the rising peak temperatures. No dependency can be observed for the self-heating onset, vent opening and voltage drop temperature for SOC in the normal operating range. Overcharge behavior will be further explored in Section 3.8. SOH and the aging history have surprisingly limited and inconsistent influences on most TR temperatures across the compiled dataset. Only low temperature aging has a large effect on the self-heating onset temperature. This suggests that aging-induced safety degradation is strongly dependent on the specific aging path and remains insufficiently characterized to draw definitive conclusions. This topic is further elaborated in Section 3.7. In summary, cell chemistry, specific energy and SOC emerge as the factors most strongly associated with TR onset temperatures, peak temperatures, and temperature rise rate.
Table 4. Summary of temperature findings with effect size indicators for directional (↑: large positive; ↗: moderate positive; ↔: small; ↘: moderate negative; ↓: large negative), and non-directional (+: large; o: moderate; –: small) input, plus color code for confidence level (high, moderate, low).

3.2. Mass Loss During TR

During a TR event the battery cell experiences a characteristic mass loss that is investigated in the following. For better comparability between different cells the relative mass loss is considered for the analysis and the key results are shown in Figure 13. When safety venting occurs due to exceeding the maximum internal cell pressure, electrolyte spray and vapor is predominantly vented from the cell [73]. This marks the first potential mass loss. During the TR reactions several vent gases are produced causing additional mass loss. A high rate of gas generation and weakened materials due to high temperature can result in a local pressure buildup, which can lead to loss of structural integrity in the active material stack, roll, and other cell components. Fine particles and even whole jellyrolls can be ejected alongside the vent gases in such scenarios [74,75]. Venting behavior and vent gas characteristics are discussed in Section 3.4 and Section 3.5, respectively. At this point, it can already be concluded that mass loss behavior depends on the cell characteristics (Figure 13a). The cathode material has a large effect on the relative mass loss. While LFP cells lose 20% of their mass on average, NCA and NMC811 cells vent over 50% of their mass during a TR event. For NMC cells an increase in mass loss with higher nickel content can be observed. The explosivity of the TR process is linked to the thermal stability of the cathode active material. When the oxygen release takes place before electrolyte dry-out, i.e., at lower temperature, electrolyte oxidation is enhanced and explosivity of the TR increases [39]. This may also explain the moderately negative correlation between severe TR trigger temperature and the relative mass loss. Electrolyte composition has a moderate effect on the relative mass loss as well. Cells with EMC containing electrolytes experience higher mass loss. Interestingly, this finding fits to the previously discussed reactivity classification by Feng et al. [72]. The higher reactivity of EMC may cause faster gas generation and subsequent internal cell damage leading to more solid ejecta. Separator choice has a moderate effect. While cells with PE or PP/PE/PP separator show low to moderate relative mass loss, cells with ceramic-coated PE separator cover a wide range of different mass losses. It is speculated that the separator material does not have a physically significant influence on the cell mass loss but is linked to other variables. For example, ceramic coated separators are used over a wide range of cells, thus the wide range in the data. Several characteristic TR temperatures have a positive correlation with the relative mass loss. The effect size for maximum internal cell temperature (Figure 13b) and vent gas temperature is large. For maximum external cell temperature, it is moderate (Figure 13e). Higher cell temperature causes more degradation of materials like current collector melting, which destabilizes the structure of the cell and results in higher mass loss. On the other hand, a high peak temperature and a high temperature rise rate are indicators for a severe and explosive TR that results in enhanced mass loss. Due to the expansion pressure, a high vent gas temperature leads to more damage in the active material structure and higher mass loss. Similar explanations can be considered for the positive correlations with the SOC-corrected specific capacity (Figure 13c) and the energy density (Figure 13d). As already discussed in Section 3.1, these variables have a strong influence on the TR behavior. With low SOC the TR process is decelerated, whereas more energy combined with smaller volume or less mass leads to a more explosive TR accommodated by higher mass loss. Note that even at SOC = 0% some mass loss occurs. This is mainly attributed to the vented electrolyte vapor and SEI decomposition products [44,76]. Interestingly, energy density has a higher effect size than specific energy. Since the internal pressure build-up and the subsequent cell damage is directly linked to the gas generation per volume, this observation is reasonable. Although cylindrical cells often eject the whole jellyroll [77,78] which results in high relative mass loss, no effect can be found for the cell format, F(2, 804) = 5.17, q = .011, ω2 = .010. As can be seen in Figure 13d, all cell formats experience a wide range of different mass losses. For SOH, only a low effect is calculated, r(807) = .087, q = .038. However, only a few datapoints of SOH < 100% are available and further research is necessary to draw conclusions.
Figure 13. Relative mass loss depending on (a) cell characteristics (SOC = 100%), (b) maximum internal cell temperature T3,int and SOC, (c) SOC-corrected specific capacity, (d) energy density and format (SOC = 100%), and (e) maximum vent gas temperature Tgas,max and maximum external cell temperature T3,ext (SOC = 100%), with common filter (MainTRTriggered = yes).
To summarize, the relative mass loss during TR spans from negligible to 90% of the total cell mass and scales strongly with cathode chemistry and with indicators of TR severity such as peak cell and gas temperatures and the temperature rise rate. Energy density is more strongly correlated with relative mass loss than specific energy, which highlights that reaction sites per unit volume play a key role in internal damage and ejecta formation. Even at SOC = 0%, non-negligible mass loss can occur due to SEI decomposition and electrolyte vaporization, implying that discharged cells still pose some safety hazards.

3.3. TR Duration

Compared with characteristic temperatures, temporal characteristics of thermal runaway have received less attention in literature. Several characteristic timings can be considered to evaluate the duration of the severe TR event. These include the time from the severe TR onset temperature T2, until the maximum cell temperature T3,ext is reached as a thermal measure; the time from the start of significant voltage drop until the voltage reaches 0 V as an electrochemical measure; or the time from the start of a significant pressure increase in the test chamber until the pressure reaches its maximum value as a fluid dynamic measure for venting duration. The latter is discussed in detail in Section 3.4.3 when reviewing the venting characteristics.

3.3.1. Time Until Maximum Temperature

Results for the time until maximum temperature are presented in Figure 14. Besides the maximum temperature rise rate discussed in Section 3.1.7 this duration provides complementary insight into the dynamics of TR as it characterizes the rate at which degradation reactions progress. Therefore, similar findings can be anticipated. Cells with LFP cathode material heat up significantly slower than NMC811 cells (Figure 14a). For LFP cells the heat-up time can be in the order of minutes, while NMC811 cells can reach their peak temperature within a few seconds. As discussed before, the cathode oxygen release that enhances the main TR reactions can be considered the key mechanism. Also, the cell format has a significant impact. Cylindrical cells heat up fastest, followed by pouch cells and prismatic cells. The latter are typically larger in size and heavier. Positive correlations for height, width and length as well as cell mass suggest that large and heavy cells tend to heat up slower. However, these correlations are confounded by the chosen cathode material as can be seen in Figure 14b. LFP cells predominantly have medium to high cell mass. A physically reasonable explanation for the longer TR duration in larger cells is that the TR reaction front needs to cover a greater distance inside the cell. This explanation is based on the theory of thermal diffusion-driven internal reaction propagation, as observed by Wang et al. [68]. Figure 14c and Figure 14d show the correlation with the maximum external cell temperature and the relative cell mass loss, respectively. Additionally, the format and cathode material are marked. An exponential fit is used in these cases to avoid unphysical negative TR durations within the data ranges. Higher peak temperature and greater cell mass loss occur simultaneously with shorter time until maximum temperature indicating a severe and explosive TR event as discussed in Section 3.2. These trends cannot only be observed globally, but also for most cathode materials individually. Overall, the cathode material choice seems to have an overarching effect on the time until the maximum temperature is reached and influences other correlations found (see also Supplementary Table S10). For example, SOC has an overall positive correlation, which is distorted by overcharged LFP cells with longer reaction duration. Little data is available for SOC < 100%. Indeed, NMC811 cells show a negative trend for partly charged cells highlighting decelerated reactions towards lower SOC. No SOH dependency statistics are calculated due to a sample count below the minimum of 20. Further investigations are necessary to reach solid conclusions. As this duration variable depends on the temporal heat transfer governed by the energy equation, additional test setup related confounders that influence heat transfer must be considered (see Section 3.9).
Figure 14. Time until maximum temperature depending on (a) cell characteristics (SOC = 100%), (b) cell mass, format and cathode material (SOC = 100%), (c) maximum external cell temperature T3,ext, format and cathode material, and (d) relative cell mass loss, format and cathode material.

3.3.2. Duration of Voltage Drop

The voltage drop during TR can have different reasons as discussed in detail in Section 3.1.3. If the voltage drop occurs simultaneously with the start of the severe TR onset at the TR trigger temperature T2, it can be linked to the anode–cathode redox-reaction and internal short circuit [50]. The time until the voltage reaches 0 V can, therefore, be used as an electrochemical measure for TR duration. Compared to the time until the maximum temperature is reached, this value is even less often derived in the literature, and only limited data is available for analysis. Although no ANOVA result is calculated for the dependency on the cathode material, it can be assumed that cathode material choice is the main confounder for most other significant statistics calculated and has a significant effect. For example, Figure 15 highlights that large, high-capacity LFP cells result in positive correlations calculated for many size variables. These cells are prismatic cells and, therefore, affect the format statistic as well. Note, that the voltage drop as an electrochemical tracer for the TR duration is a less reliable metric compared to the venting duration, as early voltage signal loss due to internal cell damage and subsequent current path interruption cannot be ruled out. Consequently, the venting duration as discussed in detail in Section 3.4.3 should always be captured.
Figure 15. Time until voltage drop depending on nominal capacity, format and cathode material.

3.4. Thermal Runaway Venting Characteristics

During thermal runaway the cell can eject electrolyte vapor and droplets, vent gases and solid particles [79]. This section discusses the venting characteristics, including the total vent gas volume, the normalized vent gas volume by nominal capacity, the venting duration, the normalized vent gas volume flow rate, the normalized particle mass, and the particle and vent gas fraction of the total mass loss.

3.4.1. Vent Gas Volume

Several approaches are used in the literature to derive the vent gas quantity or volume. A common approach is the calculation by ideal gas law when the cell is tested in an autoclave environment, i.e., a pressurized vessel at constant volume. Over the course of the TR event, the curve of the added molar quantity to this volume is calculated from the autoclave pressure and the average gas temperature. The vent gas quantity is then determined by either the peak or the equilibrium value of this curve or by applying a specific mathematical criterium [80]. Other options to derive the vent gas quantity include the use of a flow meter [81], water displacement [82], calculation from the Fourier transform infrared (FTIR) signal [83] and the subtraction of the solid ejecta mass from the total cell mass loss assuming the remainder is vent gas [84]. The vent gas volume is often provided as a more conceivable quantity. In this study, all molar quantities are converted to volume at standard ambient temperature and pressure (SATP, 25 °C & 1 atm) by ideal gas law. Other volume definitions like standard temperature and pressure (STP, 0 °C & 1 bar) are converted accordingly. If the volume definition is missing, SATP is assumed. The conversion factor from STP to SATP is 1.077 which introduces some uncertainty in case no volume definition is provided in the source. The vent gas volume depends significantly on the cell size. Large and heavy cells with high nominal energy and capacity release more gas volume. Figure 16 displays the vent gas volume against the nominal capacity. Other statistics for vent gas volume are, therefore, affected accordingly. For example, the cell format has a large effect as cylindrical cells are predominantly small and prismatic cells are typically larger, i.e., they possess low and high nominal capacity, respectively.
Figure 16. Vent gas volume depending on nominal capacity and format.

3.4.2. Normalized Vent Gas Volume

To remove this size dependency from the analysis, the nominal capacity is used as a normalization parameter, and the normalized vent gas volume is investigated in the following. On average, all cells in the database vent 1.69 L/Ah of gas as shown by the linear fit in Figure 16. However, strong variation can be observed depending on the cathode material. While the median value for LFP cells is only 0.7 L/Ah, NMC cells vent about 2 L/Ah (Figure 17a). Ranked from low to high, the order of the normalized gas volume is: LFP < NCA < LMO < LCO < NMC532 < NMC622 < NMC811. The significantly lower gas amount for LFP cells can be explained by the missing oxygen release from the cathode material compared to the other cathode materials [27]. Also, the order of NMC cells reflects the lower thermal stability and higher oxygen release for high nickel content [51]. NCA cells release the second lowest vent gas volume. This contradicts the previously discussed overall violent TR behavior of NCA cells, which is characterized by a high peak temperature, a sharp temperature rise rate, and a high relative mass loss. Notably, all NCA cells with measured normalized gas volume are cylindrical cells. The cell format has a significant effect itself (Figure 17a). Cylindrical cells vent less gas than prismatic and pouch cells. Jellyroll ejections, as often observed for cylindrical cells [77,78] may mitigate the TR reactions, which may result in less gas release. Another important factor that determines the gas volume is the degree of electrolyte degradation. Vented electrolyte vapor occupies less volume than the respective degradation products because the reactions break down the electrolyte molecules into smaller ones, thereby increasing the molar quantity. If the TR trigger temperature is high, electrolyte vapor can vanish from the cell without significant degradation, and less fuel remains available for the severe TR reactions. Thus, a negative correlation can be found for the TR trigger temperature T2 (Figure 17d). Since the TR onset depends on SOC, such dependency can be observed for the normalized gas volume as well across all cell formats (Figure 17b). With lower SOC, more electrolyte can vaporize and leave the cell before the severe TR onset in an overheating experiment. As discussed in Section 3.1, some TR reactions are mitigated at lower SOC. Accordingly the amount of gaseous reaction products is reduced resulting in lower gas volume. Another significant correlation exists with the relative cell mass loss (Figure 17c). With larger normalized gas volume, associated internal damage increases, and more mass tends to be ejected. The strong influence of cathode material choice must be noted here. No correlation can be found for SOH probably due to limited data samples with SOH < 100%. A single study by Essl et al. on a 60 Ah NMC622 pouch cell suggests that the normalized gas volume is decreasing for lower SOH [67]. Interestingly, when they considered the SOH-corrected cell capacity for normalization instead of the nominal capacity, all three aged cells tested released the same normalized gas volume. Like SOC, the gas volume can therefore be linked to the available lithium for reaction. The gas quantity indicator reflects the method of gas volume measurement and is expected to have an effect on the determined gas volume. Due to limited data, only the obvious difference between the use of peak or equilibrium values for the volume calculation by ideal gas law can be anticipated.
Figure 17. Normalized vent gas volume at standard ambient temperature and pressure (SATP) depending on (a) cell characteristics (SOC = 100%), (b) SOC and format, (c) relative cell mass loss and cathode material (SOC = 100%), and (d) TR trigger temperature T2 and SOC.

3.4.3. Venting Duration

Since the gas release is coupled to the TR reaction progress, the venting duration is a good measure to determine the TR duration. Several methods can be found in the literature. Often the pressure signal in the autoclave environment is used either directly [85] or by calculation of the molar quantity using the ideal gas law [86]. When the pressure reaches the maximum value and drops again, pressure change due to gas generation is slower than pressure change due to condensation and cool-down of gases, suggesting the main venting event is over. For tests in open environments, dynamic weighing of the cell mass allows to depict the venting duration [87]. When mass loss stops, the venting event is over. Further methods include the use of a flow meter signal [81], video recording [88], or sound recording [84]. Some other methods refer to the TR duration measurements by temperature [89] and voltage [90] as previously discussed in Section 3.3. The venting durations in the database span over several orders of magnitude from 0.2 s to 487 s with an IQR from 2 s to 11 s. Therefore, the near normally distributed assumption for the Pearson correlation is violated resulting in overall low-quality fits. More significant Spearman correlations with moderate or large effect size can be determined and exponential or power law approximations consistently result in better fits for the venting duration. Key effects are summarized in Figure 18. The cathode material and cell size are the two dominant variables. NMC811 and NCA cells have the lowest vent duration, i.e., show the most explosive behavior. LFP cells vent the longest and the venting duration is in the order of minutes compared to seconds for the other chemistries. In Figure 18b, the interplay between cell size represented by nominal capacity and cathode material is shown. The venting duration increases with cell size and a long venting duration for LFP cells is consistent for large and small cells. The power law fit suggests that the venting duration increases with the nominal capacity below linear. This is physically reasonable since in many overheating scenarios the reaction progress is limited by the low thermal conductivity direction of the active material assembly whereas the cell size often grows multidimensional. In this plot, points above the fitting line represent cells with comparatively long venting durations for a given size and vice versa. In this sense, LFP and SIB cells vent slowly, while NMC622 and NMC811 cells vent fast. Since the format is often linked to cell size, it also has a significant effect. Cylindrical cells are typically small and vent within a few seconds while larger pouch and prismatic cells vent significantly longer. Venting of large prismatic LFP cells lasts the longest. The correlation of active material shape can be explained by the linkage to cell format. A strong negative power law correlation can be observed for the relative mass loss (Figure 18c). Also, the absolute mass loss shows such negative trend. Here, the probable causality is that a short venting time, i.e., an explosive venting event leads to a higher cell mass loss due to increased internal damage by abrupt gas generation. This trend can be observed globally, but not for all cathode materials individually highlighting the large influence of cathode material choice on the venting duration. Similar observations are made in Section 3.3 with respect to the timings until maximum temperature is reached and until the cell voltage drops to 0 V. The venting duration indicator has a low insignificant effect on the results, F(3, 101) = 3.06, q = .052, ω2 = .056. This suggests that the different methods used can determine the venting duration with reasonable accuracy. Little data is available for the SOC dependency of the venting duration and no correlation exists. The available studies for SOC ≠ 100% show inconclusive results. While two studies found decreasing venting duration with increasing SOC for LCO [91] and NMC111 cells [86], Zhang et al. measured increased venting duration with SOC for a LFP cell [92]. Almost no data is available for low SOH. Essl et al. found increased venting duration with lower SOH for a NMC622 cell, suggesting a reduction in reaction speed for aged cells [67].
Figure 18. Venting duration depending on (a) cell characteristics, (b) nominal capacity and cathode material, (c) relative mass loss and cathode material.

3.4.4. Normalized Vent Gas Volume Flow Rate

From the normalized vent gas volume and the venting duration, an average normalized vent gas volume flow rate can be calculated. Results are shown in Figure 19. Values span over a wide range from 0.004–12.2 L/(Ah*s) with an IQR of 0.23–0.50 L/(Ah*s). The cathode material does not have a significant effect, F(3, 49) = 1.32, q = .334, ω2 = .018 (Figure 19a). However, only little data is available. The three remaining materials LMO, NMC622 and NMC811 release moderate to high normalized vent gas volume and possess moderate to low venting duration. For these cells, the format shows a large significant effect. Cylindrical cells vent more violently with higher flow rate than prismatic and pouch cells highlighting their often-observed violent TR. The gas atmosphere also has a moderate significant effect, but with relatively high q-value, q = .046. Tests in argon show lower normalized flow rate than tests in nitrogen. Although in principle, nitrogen may participate in the reaction by NOx formation, both gases are expected to act inert during TR and, therefore, the correlation should arise from confounders. A higher relative cell mass loss correlates with a higher flow rate across all cell formats following a power law (Figure 19b). Faster gas release leads to larger structural damage inside the cell and more mass loss. SOC has a positive correlation when filtered for SOC ≠ 100%, consistent with the lower gas release due to mitigated TR reactions at lower SOC, but this finding is only based on a few studies [86,91,92,93]. A positive correlation for SOH was again found by Essl et al. suggesting that aged cells vent less violently [67].
Figure 19. Normalized vent gas volume flow rate depending on (a) cell characteristics and test setup (SOC = 100%), and (b) relative mass loss, format and cathode material.

3.4.5. Normalized Particle Mass

Alongside the vent gases, a significant amount of solid ejecta is often vented from the cell during the severe TR phase. These ejecta, called particles in this study, can have different sizes from below micrometer scale to large fragments of the cell internal structure and may pose several risks like vent gas ignition, electrical arcing and structural damage [71]. To determine the mass of vented particles, the cell must be tested in a confined environment so that particle sampling as a whole is possible after the experiment. Brushes [94], scrapers [95], spatulas [96] or vacuum cleaners [71] are used for sampling. Up to 711 g or up to 64% of the cell mass is ejected as particles by the cells in the database. Therefore, a significant amount of the total energy is ejected during TR [81]. To allow a fair comparison between different cell sizes, the ejected particle mass is normalized by the nominal capacity, similar to the vent gas properties. The normalized particle mass ranges from 0–9.3 g/Ah with an IQR of 1.9–4.4 g/Ah. It positively correlates with the normalized vent gas volume as can be seen in Figure 20a. High gas generation facilitates severe structural damage inside the cell and leads to greater particle mass ejection as discussed earlier. Highly charged cells seem to eject more particle mass than cells with low SOC (Figure 20b), which aligns with the greater reactivity of high SOC cells. However, the data is scarce. Interestingly, Amano et al. found relatively high particle mass loss of ~2.4 g/Ah for a cylindrical SIB with sodium-nickel-iron-manganese-oxide (NFM111) cathode material even at SOC = 0% [97], whereas Essl et al. did not measure any particle mass loss for a NMC/LMO pouch cell up to SOC = 30% [96]. For SOH variation, no data is available and further research is necessary. Also, no significant correlations can be found for the categorical variables with sufficient data like cathode material, anode material and cell format. The in-group variance is similar to the variance across groups, suggesting that the particle mass loss depends on several significant factors and is, therefore, individual for each cell and hard to predict. Notably, particle mass loss is rarely reported for LFP cells. Many studies suggest that the particle mass loss is minor in alignment with the low relative cell mass loss discussed in Section 3.2. Though, there are some outliers with higher relative mass loss (see Figure 13a) that suggest significant particle ejection. Wang et al. measured 1.6 g/Ah of particles for a prismatic LFP cell [98]. Schöberl et al. tested a cylindrical 4680 LFP cell with significant particle ejection and a relative mass loss of 61% [77].
Figure 20. Normalized particle mass depending on (a) normalized vent gas volume, format and cathode material, and (b) SOC, format and cathode material.

3.4.6. Particle and Gas Mass Loss Fractions

The proportion of particle mass loss to total cell mass loss is visualized in Figure 21. Large, heavy and high-capacity cells as well as low energy density or low specific energy cells tend to have a lower particle mass loss fraction. Cathode and anode material choice have significant correlations with large and moderate effect size, respectively (Figure 21a). NMC811 cells show a lower particle mass loss fraction than NMC622 cells. Furthermore, most of the ejecta of SIB NFM111/hard carbon cells are solid. However, the respective study did not measure the particle mass explicitly, but determined it by subtracting the calculated gas mass from the total mass loss [97]. This or the inverse approach of subtracting the measured particle mass from the total mass loss to derive the gas mass loss are typical ways to calculate the missing variable. Such cells are positioned on the inverse identity line in Figure 21b. By assuming that the particle mass loss fraction and the gas mass loss fraction add up to one, important information on the measurement uncertainty or liquid ejecta mass are lost. Typically, the gas mass can be estimated from the measured quantity and the average molar mass, when analyzing the gas composition. However, rarely are all gas components detected (see Section 3.5), which may result in a significant calculation error. The gas mass loss is typically underestimated since heavy molecules may condensate before analysis or are disregarded ab initio. This especially becomes apparent when looking at the gas mass loss fraction for LFP cells in Figure 22. Considering that LFP cells often do not vent significant particle mass, a median gas mass loss fraction of 14% is much too low and a value way above 50% should be expected. On the other hand, a gas mass loss fraction of >100% can be attributed to incomplete gas analysis, e.g., with missing hydrogen fraction [99]. Also, particle agglomeration does not always enable the collection of all particles vented from the cell. This results in an underestimation of particle mass loss. Studies that determine both masses independently, therefore, often detect discrepancies in the mass balance as seen by the points that are farther away from the inverse identity line in Figure 21b. For clarity, it is recommended that particle and gas mass are always determined independently and the calculated residual mass is reported.
Figure 21. Particle mass loss fraction depending on (a) cell characteristics, and (b) gas mass loss fraction, cell mass and cathode material.
Figure 22. Gas mass loss fraction for different cathode materials (SOC = 100%, SOH = 100%).

3.4.7. Summary of Venting Characteristics Findings

To summarize, the total vent gas volume scales roughly linearly with the nominal cell capacity across all chemistries, with an average of 1.7 L/Ah at SATP. Chemistry-dependent trends are pronounced once normalized. LFP cells vent significantly less gas per Ah than NMC cells, and normalized vent gas volume increases with higher nickel content. Cathode materials rank in the following order regarding their normalized vent gas release: LFP < NCA < LMO < LCO < NMC532 < NMC622 < NMC811. The venting duration spans more than three orders of magnitude and is frequently associated with the cathode material and cell size. Large-format prismatic cells with LFP cathode commonly vent over tens to hundreds of seconds, whereas Ni-rich NMC and NCA cells and small cylindrical cells often exhibit more violent venting within seconds. More explosive venting with higher volume flow rate leads to a higher relative cell mass loss due to enhanced structural damage inside the cell and subsequent particle ejection. More than 60% of the cell mass can be ejected as particles in some scenarios, thus a large proportion of the overall thermal runaway energy can be vented from the cell. The proportions of particle and gas mass in the total cell mass loss vary depending on the cathode material. Gas and particle mass loss determination pose several challenges linked to the accurate measurement of gas volume and composition, as well as the complete sampling of all particles after the test. Particle and gas mass must be quantified separately from each other to estimate the calculation error in the overall mass balance and highlight uncertainties in the test setup.

3.5. Thermal Runaway Vent Gases

The vent gas composition is a key characteristic of a thermal runaway and will, therefore, be investigated in more detail in this section. It is most often analyzed by supplying a post-mortem gas sample to a gas chromatograph coupled with a mass spectrometer (GC/MS) [100]. The time of gas sampling ranges from 30 s [101] to 24 h [91] after the TR event or can be triggered at a specific temperature [102], whereas several studies do not provide any specific information. Shen et al. did not find significant differences in composition between sampling one minute or 60 min after TR suggesting that the gas-phase reactions are frozen after maximum one minute [103]. However, they only investigated components that are gaseous at room temperature. On the contrary, Chuang et al. measured significant differences depending on time of gas sampling for multiple species [104]. Note that the gas sampling and analysis temperature affect the gas components that can be detected due to imminent condensation [105]. Apart from post-mortem analysis, FTIR [83] or Raman spectroscopy [106] are sometimes used for a continuous measurement of the vent gases. Another important factor is the gas environment during the test. While nitrogen, argon or vacuum atmospheres aim to mitigate gas-phase reactions, combustion may take place in oxygen containing atmosphere. Therefore, only gas analysis studies without vent gas ignition are considered in this analysis.

3.5.1. Overview and Origin of Vent Gases

In total, the vent gas composition was analyzed for 313 of the 1703 tests in the database and 47 gases could be detected overall. This analysis does not account for isomers since most studies do not provide this information. The frequency of individual species measured as well as the mole fraction range of these species for sample counts > 19 are summarized in Figure 23a. Hydrogen H2, carbon monoxide CO and carbon dioxide CO2 are often measured and have the highest median mole fractions of XH2 = 0.223, XCO = 0.201 and XCO2 = 0.322, respectively. Small to medium size hydrocarbons are also frequently analyzed with X > 0.01 for methane CH4, ethylene C2H4, and propylene C3H6. Due to the high boiling temperatures, electrolyte vapor is rarely found. It is predominantly measured when FTIR analysis is applied with heated sampling lines. Only Zhang et al. detected a significant quantity of DMC by GC/MS analysis [58]. When investigated, the median value for DMC is XDMC = 0.06, for example. In some studies, the hydrocarbon concentration is lumped into the total amount of hydrocarbons (THC) with a median of XTHC = 0.087. Several studies also detected hydrogen fluoride HF, a toxic reaction product of lithium hexafluorophosphate LiPF6 decomposition [107]. Figure 23b shows the frequency of gas composition combinations measured with a minimum of three different species. The first combination with five species is C2H4, CH4, CO, CO2 and H2 with 246 samples. For the first combination with six species ethane C2H6 is added in 210 samples. After that, a huge drop in measuring frequency can be observed.
Figure 23. (a) gas component measuring frequency and mole fraction range (N > 19), and (b) gas composition combination frequency with minimum three gases.
The TR reaction sources for the gases mentioned in Figure 23 are summarized in Figure 24. To the best of the authors knowledge, no holistic reaction mechanism that includes all relevant TR reactions exists. A summary of all known reaction equations is beyond the scope of this work, and the interested reader is referred to the respective literature.
Figure 24. Overview of vent gases and their thermal runaway reaction sources summarized from [39,40,44,65,76,107,108,109,110,111,112,113,114,115,116,117,118,119].

3.5.2. Statistics of Main Vent Gas Species

Since most studies assume that their measured gas fractions add up to one, a fair comparison of the vent gas composition is only possible, when normalizing the mole fractions. Reported mole fractions are often biased towards lighter, more volatile species and heavier hydrocarbons are almost certainly underestimated unless specific methods like high temperature sampling and analysis are applied. The normalization is performed for the most frequent six-gas-mixture and the effect of cathode material as a key variable is visualized in Figure 25. Overall, the statistical analysis reveals nine gases with significant correlations to cathode material and moderate to large effect size. LFP cells emit significantly more hydrogen than cells with lithium metal oxide cathode with a normalized median of XH2 = 0.417 (Figure 25a). On the other hand, CO emissions are much lower for LFP cells, mainly below 10%. Here, NCA cells have the highest median of XCO = 0.393 (Figure 25b). The highest CO emissions are accompanied by the lowest CO2 emissions for NCA cells, followed by LFP cells (Figure 25c). The milder decomposition reactions and slower venting in LFP cells might favor more complete oxidation to CO2 and venting of highly flammable H2, rather than partial oxidation to CO and H2 combustion. Methane mole fractions only slightly depend on the cathode material with median values around 5% (Figure 25d). Ethylene mole fractions are lowest for NCA, moderate for LCO and highest for LFP and NMC cathode materials (Figure 25e). They mainly range between 1–10%. C2H6 fractions are the highest for LFP cells with a median of XC2H6 = 0.014 (Figure 25f). For the remaining cathode materials, the share of C2H6 often stays below 1%. The electrolyte decomposition reactions are a major source for the TR vent gases highlighted by significant correlations with large effect size for the frequently measured gases C2H4, C2H6, CO and CH4. Since the electrolyte composition is not always provided and several gases are rarely reported, for many combinations not enough data is available to calculate statistics. However, the literature, for example, suggests that EC reduction at the anode favors C2H4 production, whereas DMC reduction yields C2H6 [107,110]. Note that during electrolyte decomposition and combustion a multitude of hydrocarbons may form depending on the local conditions. Glaude et al. found several small chain hydrocarbons such as CH4, C2H2, C2H4 and C2H6 simultaneously in a DMC diffusion flame [120]. Longer chain hydrocarbons may form during radical recombination.
Figure 25. Normalized mole fraction depending on cathode material for the most frequent gas composition with six gases—(a) H2, (b) CO, (c) CO2, (d) CH4, (e) C2H4 and (f) C2H6 with common filters (MainTRTriggered = yes, SOC = 100%).
For the separator material significant differences between PE and ultra-high-molecular-weight polyethylene (UHMWPE) can be observed. However, UHMWPE is confounded by NCA cathode material showing the same behavior. Similarly, the statistics for cell format are confounded by cathode material. For example, prismatic cells vent the most hydrogen, but several prismatic cells possess LFP chemistry. Likewise, C2H4 is found the least in cylindrical cells, which contain predominantly NCA cathode material. The active material shape is linked to the cell format and thus the cathode material, explaining such dependencies. Only small effects can be attributed to the gas atmosphere for most gases. Just C4H10 is tested with a moderate effect size, but with higher mole fraction in air compared to nitrogen. These findings suggest that the initial precaution of not considering vent gas compositions measured after obvious combustion is sufficient and no significant differences between gas atmospheres exist as long as flame combustion is avoided.
Many Pearson and Spearman correlations can be found for numerical variable pairs as summarized in Table S18. An excerpt of physically interesting ones is discussed here. Note that undetected gases may have significant influence on the reported mole fractions and therefore the calculated statistics. Vent gas emissions correlate with the explosivity and severity of a TR event. For example, the CO fraction increases with increasing maximum external cell temperature (Figure 26f) and relative cell mass loss (Figure 26g), while the EMC fraction and several other hydrocarbon fractions decrease for both. Similarly, high CO fraction correlates with high vent-gas-mass-to-cell-mass ratio, while hydrocarbons like C3H6, C3H8 and C4H8 show the opposite behavior (Figure 26h). The severity of a TR event is primarily determined by the degree of reactant conversion. In the presence of sufficient oxygen released by the cathode active material, the electrolytes and their hydrocarbon decomposition products can be combusted more completely resulting in higher heat release, more gas generation and higher cell mass loss. Since oxygen release is enhanced with delithiated cathodes [55,56], the CO fraction positively correlates with SOC (Figure 26d), while secondary hydrocarbons like C5H12 negatively correlate. Similar behavior can be observed for the correlation with specific energy (Figure 26c). Energy dense cells predominantly possess higher nickel content in the cathode, which promotes oxygen liberation and favors hydrocarbon combustion [51]. A fast TR with high vent gas volume flow may hinder complete oxidation. With increasing flow rate and thus shortened residence time the CO fraction increases while the CO2 fraction decreases (Figure 26i). The degree of reactant conversion is reflected by the negative correlation of two gas mole fractions. For example, a high fraction of the reactant EMC yields a low fraction of the product CO as shown in Figure 26a. Similarly, negative correlations can be found for EC and CO, EC and C2H4, CO and CO2, O2 and CO2, H2 and CO2, respectively. Within statistically significant correlations with moderate or large effect size, rarely measured hydrocarbon fractions with more than two carbon atoms exclusively show positive correlations with each other suggesting that their formation by radical recombination is commonly enhanced under specific boundary conditions. In the same way, electrolytes correlate positively with each other. Under mild TR conditions, more unreacted electrolyte can vent from the cell. The HF fraction is also higher as shown by the positive correlation of EMC and HF in Figure 26b. Note that the measurement infrastructure must maintain proper boundary conditions for electrolyte vapors to be detected. As can be seen in Figure 26e, EMC and EC fractions are higher for higher gas analysis temperature. Interestingly, EMC fraction increases even at temperatures above its boiling temperature of 110 °C while EC fraction increases even at temperatures below its boiling temperature of 248 °C [45]. The sampling and analysis temperature must be carefully chosen. On the one hand, the gas analysis as well as the gas sampling temperature should be chosen high enough to mitigate electrolyte condensation. On the other hand, further decomposition at high temperature should be avoided.
Figure 26. (a) mole fraction of CO vs. EMC, (b) mole fraction of HF vs. EMC, (c) mole fraction of CO and C2H6 vs. specific energy (SOC = 100%), (d) mole fraction of CO and C5H12 vs. SOC, (e) mole fraction of EMC and EC vs. gas analysis temperature, (f) mole fraction of CO and EMC vs. maximum external cell temperature T3,ext, (g) mole fraction of CO and EMC vs. relative mass loss, (h) mole fraction of CO and C3H6 vs. gas mass cell fraction and (i) mole fraction of CO and CO2 vs. vent gas volume flow rate.

3.5.3. Rare Vent Gas Species

Several gases are only occasionally mentioned in a few studies. Their sample counts are less than 20 and they are, therefore, not considered for the statistical analysis. These include some electrolytes, i.e., PC and DEC, whose detection depends on their usage in the respective cell and the sampling and analysis temperatures due to their liquid nature in environmental conditions. Furthermore, several stable products and intermediates of the electrolyte decomposition and combustion reactions could be detected. Among them, water H2O is only quantified 14 times, although it should be present in most tests considering the hydrocarbon oxidation route to H2O and CO2 [107]. Indeed, when tested, the median value is XH2O = 0.039. Similar to the electrolytes, the reason may be the high vaporization temperature that requires gas sampling and analysis above 100 °C. In addition, multiple hydrocarbons and hydrocarbon derivatives can be found in the vent gas. These include shorter chain gaseous molecules as well as longer chain liquids that are mostly measured in fractions below X = 0.01: C3H4, C4H4, C5H8, C5H10, C6H6, C6H12, C6H14, C7H8, C8H10, CH2O, CH4O, C2H4O, C2H4O2, C2H6O, C7H14O2. An exception is benzene C6H6 that is measured 16 times with a significant median of XC6H6 = 0.045. For some of these molecules possible reaction pathways are provided in the literature [72,110,112,115,121]. The heaviest quantified molecule in the database is amyl acetate C7H14O2 measured by Chen et al., but no formation source is provided [122]. In one study N2 was measured in an ARC test at XN2 = 0.096 although the chamber was flushed with argon before the tests [123]. This can most likely be attributed to air leakage. In the presence of nitrogen or air, nitrogen oxide NOx can form as measured by Bordes et al. with FTIR [83]. Another research group found ammonia NH3 and hydrogen chloride HCl by FTIR and sulfur dioxide SO2 by FTIR or GC/MS with peak values of XNH3 = 0.19 [124], XHCl = 0.09 [124] and XSO2 = 0.098 [125], respectively. No chemical sources for these species are provided, and the measured peak quantities may be challenged. Amano et al. detected hydrogen cyanide HCN in very small quantities for a pouch cell [126]. They proposed that the laminated aluminum film of the pouch bag contains polyamide that may decompose to NH3 and further react to HCN in the presence of CH4 and CO during TR. Furthermore, HCN is an intermediate species of the prompt NOx formation process. Other fluorinated components such as phosphorus trifluoride PF3, phosphoryl fluoride POF3, methyl fluoride CH3F and ethyl fluoride C2H5F that, similar to HF, most likely originate from the decomposition of the electrolyte salt LiPF6 are detected by Fernandes et al. [121] and Bordes et al. [83]. Liao et al. support this theory by finding CH3F, C2H5F and other fluorinated compounds during thermal decomposition of a LiPF6 EC/DMC mixture [110].
In addition to the quantified gases in the database, some studies observed further gas components but did not provide quantitative results. For example, Sun et al. found numerous toxic organic gases for different cathode materials and SOC [127]. Zhang et al. provided a qualitative overview table of several vent gases detected for an 18650 LCO cell under different SOC including several long-chain hydrocarbons [101]. It is quite possible that future studies will observe additional vent gases not yet considered.

3.5.4. Summary of Vent Gas Findings

Across 313 tests with gas analysis, H2, CO and CO2 are the most abundant species. They are typically accompanied by small-chain hydrocarbons such as CH4, C2H4 and C3H6, and, when measured with appropriate methods, electrolyte vapors and HF. Investigation of the most frequently measured normalized gas composition with six gases shows a strong dependence on cathode material. LFP cells emit higher fractions of H2 and less CO compared to other cathode materials, reflecting differences in oxygen release and degree of reactant conversion. TR severity, characterized by high peak temperature and high mass loss, correlates with higher CO and lower hydrocarbon fractions, indicating that severe events correspond to more complete oxidation of organic components. High SOC and specific energy promote higher CO and lower heavy hydrocarbon fractions, consistent with the enhanced cathode oxygen release and electrolyte oxidation at high degrees of cathode delithiation and high energy density. Many vent gas components like electrolyte vapors and water, that are in a liquid state under ambient conditions, are strongly under-reported and their detection highly dependents on the gas sampling and analysis temperatures. When these temperatures are sufficiently high, non-negligible electrolyte mole fractions are observed. The limited number of reports on species such as HCN, NOx, HF, PF3, POF3, and other fluorinated organics suggests that TR vent gases can contain a broader and more toxic spectrum than commonly captured. Extensive gas analysis during TR is a challenging task. Several methods should be combined to capture the whole spectrum of gases. The influence of sampling time and location should be further investigated.

3.6. Thermal Runaway Vent Particles

22 tests on the elemental composition of the particles vented during TR are included in the database. The element measuring frequency and the mass fraction Y ranges are displayed in Figure 27. Typical particle measuring devices include scanning electron microscopy and energy dispersive X-ray spectroscopy (SEM/EDS), inductively coupled plasma-optical emission spectrometry (ICP-OES), inductively coupled plasma-mass spectrometry (ICP-MS), ion chromatography (IC), CHNSO element analysis, X-ray fluorescence (XRF) and X-ray diffraction (XRD). The database only considers atomistic analysis, but no molecular structures that can be, for example, determined by XRD. All cells tested possess NMC cathode material, probably because they vent significant particle mass, unlike LFP cells. Therefore, following carbon from the graphite anode with the highest mass fraction, lithium, nickel, manganese, cobalt and oxygen make up a significant fraction of the particles. Lithium is found less often since it cannot be detected by EDS due to its low molar mass. Additionally, copper and aluminum have high shares, which are mainly linked to the ejection of current collector foils and droplets [71]. Fluor and phosphor are also commonly found with significant mass fractions. These particles can be traced back to the electrolyte salt LiPF6 and its decomposition products. Moreover, miscellaneous traces of other elements are reported by a few studies. Due to the low sample counts, no statistics are evaluated and further research in this field is suggested. The database further contains information on measured particle size distributions. Measurement techniques cover sieving [71], laser diffraction [128], dynamic image analysis [71] and microscopic imaging [96]. Accordingly, distributions can be based on count [112], volume [71], mass [71], projection area [96] or random sampling [129]. Size distributions often show distinct peaks representing single active material grains and agglomerates as well as current collector pieces, respectively [71]. While sieving and laser diffraction measure a single size value, dynamic image analysis and microscopic imaging allow for particle shape analysis. Thereby, the highly non-spherical nature of vented particles can be revealed [71]. Due to the different measurement techniques, a proper comparison of size distribution results is not possible. However, the interested reader is referred to the given figure or table numbers and the respective studies in the database for further information.
Figure 27. Particle element measuring frequency and mass fraction range.

3.7. Discussion of Aging-Related Effects

The correlations of aging on the TR variables are ambiguous within the database. While some variables show significant trends, others remain insignificant or underrepresented. Therefore, this section discusses potential aging-related effects on the TR parameters from a physics perspective. Batteries age during storage and operation, which are called calendar and cyclic aging, respectively. According to Edge et al. [130] five degradation modes exist that are observable at cell level. These are loss of lithium inventory (LLI), impedance change, stoichiometric drift, and loss of active material (LAM) at both electrodes, which degrade cell performance via capacity and power fade. From a mechanistic point of view, these modes are caused by five principal degradation mechanisms: SEI layer growth, lithium plating, positive electrode decomposition and particle fracture at both electrodes. Those interact with each other and lead to thirteen interconnected secondary mechanisms [130]. SEI layer growth is accelerated at high temperature and high voltage, whereas lithium plating occurs at low temperature in combination with high charge current and high voltage. Particle fracture of the active materials is favored at low temperature and high current and may take place at different SOC levels depending on the material. Several secondary mechanisms leading to positive electrode structural change and decomposition are accelerated at high temperature, high voltage and high current. Lithium plating and particle fracture are cyclic aging effects, whereas SEI growth and positive electrode structural changes and decomposition can appear during storage and operation.
In the database, aging is characterized by multiple variables: SOH, aging type, aging charge and discharge C-rates, aging temperature, aging duration and aging cycles. While SOH is a single measure to characterize the capacity fade over lifetime, i.e., the degree of aging, the remaining variables characterize the aging history. Similar SOH values reached under different aging histories may correspond to substantially different TR responses due to inherently different mechanisms causing the capacity fade, which limits observable correlations purely based on SOH.
Lithium plating increases the reactivity during the initial phases of TR due to less stable SEI and higher reaction rate between lithium and the electrolyte [42,43]. Therefore, low temperature and high charge current aging should correlate with lower onset temperatures. The temperature behavior can at least be observed for T1, as discussed in Section 3.1.1, while the impact on T2 by the shifted anode–electrolyte reaction to lower temperatures [57,60] is insufficiently assessed and can only be shown indirectly by a correlation with aging cycles (see Section 3.1.4).
SEI thickening reduces the initial reactivity under thermal abuse conditions [42]. Thus, high temperature operation and storage as well as high current cycling should correlate with higher self-heating onset temperature T1. The temperature behavior can be observed within the data. Significant influence of aging temperature was further highlighted in previous large-scale studies [27,47].
Many aging mechanisms directly or indirectly shift the gas generation to lower temperatures or increase the initial gas content inside the cell. Therefore, the cell vent should open earlier, and CID-based voltage drop should occur at lower temperature. The latter can be observed within the database as a positive correlation between SOH and TV0 for cylindrical cells.
Beyond the observed statistics, many further aging-related effects on TR characteristics can be anticipated and are partly suggested by individual studies. For example, Essl et al. measured decreasing peak temperatures, lower normalized gas volume and less violent venting for all aging types tested [67]. From a mechanistic point of view LLI, LAM and stoichiometric drift alter the availability or change the structure, state or composition of reactants involved in the TR decomposition reactions in multiple ways (see Figure 4).
The database contains 116 tests with aged cells at SOC = 100%, which is relatively little data considering the variability in aging history and other confounding variables such as cell chemistry, for example. Tests with cyclic aging dominate, while calendar aging investigations remain scarce probably due to the longer required preconditioning phase. Additionally, a single study by Feinauer et al. [47] with 27 tests may generate significant bias. Thus, the observed relationships should be interpreted as indications of aging-dependent changes in TR behavior rather than generalized ranking of variable importance. There is a clear need for further research on aging-related TR impacts. Based on the current data we hypothesize that aged cells can show largely different onset behavior, but often less hazardous behavior during the severe TR phase.
Most aging-related TR studies are conducted under well-defined boundary conditions in laboratory setups. While this approach allows to trace individual aging patterns to specific TR outcomes and enables cross-study comparison, it lacks real-world applicability. Dedicated TR experiments on cells used in real-world applications with tracked aging history would provide valuable insight into the actual TR safety of batteries in the field in comparison to fresh cells.

3.8. Influence of the Type of Abuse

The type of abuse can have significant effects on the TR behavior, which are summarized in this section and visualized in Figure 28. Only cells tested at SOC ≥ 100% and SOH = 100% are considered to eliminate confounding effects. Overheating, overcharging and nail penetration are the most common abuse methods in the database with overheating being applied in the majority of tests. The vent opening (Figure 28a), voltage drop (Figure 28b) and TR trigger temperature (Figure 28c) are significantly lower for overcharged cells with large effect size for Tvent and T2, and moderate effect size for TV0. While thermally abused cells require certain temperatures to trigger electrolyte vaporization and TR reactions, electrolyte decomposition and respective heat and gas generation in overcharged cells are promoted by the cathode potential exceeding the stability limit of the electrolyte [46,53,59]. Furthermore, highly delithiated cathodes are structurally destabilized and oxygen release is favored [55,56]. When the anode is fully lithiated, lithium deposition on the anode surface accelerates the anode–electrolyte reaction [57,58]. All these phenomena shift the heat release of overcharged cells to lower temperatures. Interestingly, the type of abuse does not have a statistically significant effect on the maximum external cell temperature, F(2, 1332) = 2.52, q = .119, ω2 = .002. When filtered for SOC and SOH, a slight deviation in medians with the order nail penetration > overheating > overcharging can be observed (Figure 28d). In this context, it must be noted that in contrast to mechanically abused cells, additional heat is supplied to overcharged cells by the electrochemical charging processes and to overheated cells by the heating device. Therefore, ignoring differences in venting behavior, mechanically abused cells must generate more heat to reach the same peak temperature. A slight increase in heat release for mechanically abused cells may be attributed to the fact, that these cells did not lose any reactants due to safety venting prior to TR. The TR in nail penetrated cells is triggered abruptly and results in a sharper temperature increase compared to overcharged and overheated cells as shown in Figure 28e. Both nail penetrated and overcharged cells exhibit more explosive TR behavior with significantly higher mass loss (Figure 28f) and higher normalized vent gas volume release (Figure 28g) than overheated cells. The mass loss effect size is small due to the wide range of values within each category, F(2, 797) = 22.4, q < .001, ω2 = .051. The normalized vent gas volume effect is moderate and follows the order overcharging > nail penetration > overheating. Overcharged cells also release a larger fraction of their initial cell mass as vent gases (Figure 28h), but with low effect size, F(1, 198) = 11.4, q = .002, ω2 = .049. Note that sample size in the last two cases is relatively small for nail penetration and overcharging categories and the results are, therefore, more prone to be affected by other variables. The analysis further suggests that overcharged cells release slightly more hydrogen gas during venting compared to overheated cells, F(1, 270) = 7.07, q = .015, ω2 = .022. For other gases with enough samples to calculate statistics, i.e., CO, CO2, CH4, C2H4 and C2H6, no significant effects can be determined. No correlations exist for the time until maximum temperature and the venting duration. Other variables’ sample counts are too low to depict statistics.
Figure 28. Effect of abuse type on (a) vent opening temperature Tvent, (b) voltage drop temperature TV0, (c) TR trigger temperature T2, (d) maximum external cell temperature T3,ext, (e) logarithmic maximum temperature rise rate log(dT/dtmax), (f) relative cell mass loss, (g) normalized vent gas volume and (h) gas mass cell fraction, with common filter (SOC ≥ 100%, SOH = 100%).
Compared to nail penetration and overcharging, several different means exist to overheat a cell. These include stepwise homogenous heating with the HWS protocol in an ARC test, followed by slowly accelerating self-heating of the cell; heating with constant power (W) or power density (W/m2); and heating with a specific temperature increase rate (K/min). ARC tests typically take several hours to trigger TR, while the other methods mostly take less than an hour and can be as fast as a few seconds depending on the rate and localization of the heat source. Despite the huge difference in the time to trigger, cells behave fairly similar comparing HWS tests to other overheating methods. Studies confirm similar vent opening temperature [78], TR trigger temperature [78,131] and maximum external cell temperature [78,131,132,133] within typical variances between tests. Wei et al. measured the same maximum internal cell temperature in a HWS and a constant power side-heating test for a prismatic 60 Ah NMC532 cell, but detected different mass loss of 29% in the HWS and 40% in the constant power side-heating test [134]. Interestingly, they found that in four-cell stack TP tests the triggered cell lost significantly more mass than the neighboring cells consistent for different abuse methods. The neighboring cells, triggered mainly by large side surface heating, had an average mass loss of 33%, which is actually closer to the single cell HWS results. Song et al. also compared constant power side-heating to the HWS method for a prismatic 40 Ah LFP cell [135]. They found much lower peak cell temperature in the HWS test compared to the heated side in the constant power experiments, but the same temperature on the insulated non-heated side, suggesting that the difference is mainly driven by the additional heat supplied by the heater before TR. They further observed a slower temperature rise in the ARC test compared to the non-heated side in the constant power side-heating test.
To conclude, the added electrochemical component of overcharge induced TR results in significantly lower TR onset temperatures. Nail penetrated cells show the highest temperature rise rate probably associated with the sudden trigger of an intact cell. For the remaining result variables, no clear trends can be observed either due to small effect size or little sample count. Further research, especially on mechanically and electrically abused cells, is required to close this gap. The effect of different overheating methods on the TR behavior is inconclusive and based on exemplary studies only.

3.9. Influence of the Test Setup

The specific test setup conditions can affect the TR behavior. In addition to the type of abuse discussed in the previous section, the test setup can vary in the test vessel type, the test jig, the trigger position, the trigger rate, the gas atmosphere, the ambient conditions, and the cell count and interconnection. A synthesis of the key considerations in a TR test setup is visualized in Figure 29. Significant statistics with moderate to large effect size are reported in the Supplementary Material tables for each variable, where available. Properly interpreting the statistics is difficult due to low sample counts, many possible test setup combinations, and the expected dominant influence of other cell-specific variables. For a reasonable comparison, the data is filtered for the confounders: cathode material, SOC, SOH and type of abuse. Consequently, little data remains and many categories are pushed below the threshold of ten samples. Therefore, some case studies are explored in this section, and a physics-based analysis of potential influencing factors is attempted instead.
Figure 29. Overview of thermal runaway test setup considerations.

3.9.1. Test Vessel Type

The test vessel type mainly defines the possible gas atmospheres and ambient conditions, whose effects are discussed later. For example, inert atmospheres require gas tight vessels like autoclaves, which can employ non-atmospheric pressure conditions as well. Alternatively, specific altitude chambers can be used. Typical vessels for high temperature boundary conditions include ARC setups and ovens. Apart from these conditional effects, no further influence of the test vessel type is expected, as long as all boundary conditions are the same [28]. Additionally, requirements for specific measurements may demand a certain test vessel. These include, for example, the determination of onset temperatures, the online or post-mortem gas analysis as well as the particle sampling. Note that testing small cells in large vessels may introduce measurement uncertainties, depending on the specific setup. For example, a small cell’s minor gas release in a large-volume autoclave will result in a minor pressure increase that may not be easily detected by the high-pressure sensor used for large cells.

3.9.2. Test Jig

Many researchers use dedicated test jigs to fix the cell during the test. They range from sophisticated custom-built jigs to simple taping or wiring solutions. By holding the cell in place during TR, the risk of fault measurements due to thermocouple detachment or movement of the cell is reduced. Vendra et al. measured large variance in peak cell temperature when positioning the cell on a metal mesh compared to low variance in a clamped ARC setup [123]. When the cell thermocouples are incorporated into the jig and are not exposed to the surrounding gas, credibility of their readings is improved. Temperature readings for free standing or hanging cells are prone to be affected by the ambient gas, i.e., by showing lower values due to convective heat transfer before TR and possibly higher more fluctuating values due to the venting influence during TR. Free-standing cells, if not further insulated, also have an additional heat transfer path to the test vessel that can absorb some of the TR energy and influence the reaction progress. On another note, cell compression is recommended to obtain application relevant TR results. This is especially relevant for pouch cells, whose foil only provides limited structural support. Upon internal gas generation, the cell inflates. Hahn et al. found that uncompressed inflated cells have a longer TR duration due to a lengthened reaction path [136]. Uncompressed cells also have lower peak temperature and show less reproducible results. They proposed thermocouple movement as a possible reason. Their compressed cells had higher mass loss due to narrower gas channels and react more complete, which is depicted from the higher CO2 and CO concentrations in contrast to lower electrolyte concentrations. The material choice of the jig components is relevant as well. When the cell is in direct contact with metallic compression plates, heat dissipation to the jig is enhanced, which may alter the TR behavior. Wang et al. report the same maximum temperature rise rate, reflecting the initial rise, but a lower peak temperature for a metal jig compared to an insulated jig, due to the thermal dampening effect [68]. Similarly, Gao et al. measured lower peak temperature due to enhanced heat absorption, when comparing a steel heater to a silicon-carbide heater [137]. In prismatic and pouch cell modules, insulation material is often incorporated between cells. Thus, usage of insulated jigs is more representative for many system applications.

3.9.3. Trigger Position

For overheated and nail penetrated cells the trigger position can be varied. Golubkov et al. overheated a prismatic 50 Ah LMO cell from both large sides, one large side and all sides [138]. They found no difference beyond typical test variances for the TR trigger, maximum cell and gas temperature, as well as the mass loss. However, much more gas was released in the case of homogeneous heating by the reactor walls compared to other tests. The two-sided, fast rate (144 K/min) heating showed the shortest venting duration, highlighting more explosive TR. Chuang et al. determined around 10% higher gas release for one-sided heating compared to two-sided heating for a prismatic 280 Ah LFP cell, but no significant difference in gas composition [104]. Overheating of a prismatic 243 Ah LFP cell from different sides with the same power density was investigated by Huang et al. [139]. They observed slight differences in peak cell temperature in the order large > bottom > side heating case. The small side surface heating case showed slower temperature rise probably because that side of the prismatic cell is not directly in contact with the two jellyrolls and the winding direction prevents immediate vent gas exposure. Small side and bottom heating managed to trigger both jellyrolls more or less simultaneously. This led to a shorter venting duration in comparison to the large side heating case. The latter triggers the jellyrolls consecutively and the internal TP speed is low because of the low through-plane thermal conductivity of the jellyroll. All three cases released similar mass, suggesting that the overall degree of reaction was not altered significantly, but the reaction path changed. In addition to the heating side, the heating area can be altered. Lin et al. found that a homogenous heating coil around the large surface of a cylindrical 4695 31.9 Ah NMC811 cell resulted in lower peak temperature and less gas release, but the cell vented much faster than with localized heating by heating rod or heater mat [100]. The findings suggest that the TR reaction is more violent, leading to faster mass ejection and lower reactant conversion. However, the total mass loss as an additional indicator was not provided. Another study confirmed higher peak temperature and higher temperature rise rate for local overheating of a 10 Ah NMC pouch cell by a glow plug compared to homogeneous large surface heating [140].
In nail penetration tests, the cell can be pierced at different locations. Garcia et al. triggered an 18650 3.2 Ah NMC811 cell at the top, center and bottom of the large circumferential surface [141]. The peak temperature for the top trigger was lower compared to the other positions, but no difference in mass loss, temperature rise rate or TR duration was observed beyond the large variance between repeated tests. When comparing axial and radial penetration of a cylindrical cell, results are inconclusive. One study found higher maximum external cell temperature and higher nail tip temperature for axial penetration between the jellyroll layers [74], while another study on average measured higher peak temperature with lower mass loss for radial penetration through the jellyroll layers [142]. The former further observed faster internal TR propagation for radial penetration and concluded that the low radial thermal conductivity is reaction progress limiting [74]. Furthermore, the nail direction and position influence the venting behavior by potentially holding back material or cause vent path blockage and subsequent case rupture. This is cohesive with the generally low consistency for repeated nail penetration tests as acknowledged by Garcia et al. [141].

3.9.4. Trigger Rate and Speed

Differences in TR results are observed for different heating rates, overcharging rates or nail speeds. Therefore, legislations provide guidelines on the trigger rate or speed [9,10,11]. High heating power density either by heater surface reduction or by power increase provides the shortest heating time and lowest heat added to the cell [143]. The characteristic TR temperatures show ambiguous behavior. The vent opening temperature increases with faster heating probably due to a higher temperature gradient across the cell and cold spots for electrolyte condensation [144]. While no clear trends for the TR trigger temperature could be observed by two studies [145,146], Zhou et al. detected higher T2 for higher heating rate consistent over three 18650 cells with different cathode materials [147]. Notably, Lecompte et al. achieved vent opening and TR trigger temperatures comparable to ARC HWS for a cylindrical 21700 5 Ah NMC811 cell, when overheated by a very low controlled rate of 1.5 K/min in a continuous flow vessel [148]. This provides an alternative test method to conventional ARC tests. The maximum cell temperature increases with faster heating in many studies [28,87,149,150,151,152,153]. Others cannot determine a clear trend [135,145,146,154], notice no difference even for the peak internal temperature [143], or even found slightly lower T3,ext [147]. Similarly, the maximum temperature rise rate can be higher [135,149], lower [87], or non-monotonic [145] for faster heating. The relative cell mass loss also shows ambiguous behavior. It was measured higher [144,149], lower [28,87,147], similar [152] or without clear trend [145,146,151] for higher heating rates. Huang et al. noticed much less mass loss during the safety venting phase before TR onset in case of faster heating because of shorter time between venting and TR [139]. The total released gas quantity does not change much [28] or increases slightly with higher heating rate [104], while the venting duration tends to increase with faster heating due to less pre-heating [87,89]. No significant differences in the gas composition can be observed [104].
In case of overcharging, a higher charging C-rate leads to higher Joule heating, earlier lithium dendrite growth at the anode and an earlier electrochemical electrolyte decomposition due to higher cathode potential, which tends to decrease the overcharge SOC necessary to trigger TR [57,126,131,155,156,157,158,159,160]. The vent opening temperature [155,156] and TR trigger temperature [131,155,156,158,159] are mostly lowered accordingly. High C-rate overcharging results in a more explosive TR accompanied by higher peak temperature [57,126,131,155,158], higher maximum temperature rise rate [155,158], and higher mass loss [158]. Opposingly, one study found lower peak temperature for more rapid overcharging [159]. Wang et al. also measured higher H2 and lower CO2 fractions for faster overcharging [155].
In nail penetration tests, the penetration depth, nail diameter and nail material can be altered next to the penetration speed as done by Zhou et al. on a cylindrical 18650 3.5 Ah NMC811 cell [88]. They found higher peak temperature, lower mass loss and similar venting duration for shorter penetration depth and when changing the nail material from steel to ceramic. For thicker nails they obtained a higher peak temperature and higher mass loss. Although several nailing speeds in the range of 0.02–40 mm/s were used in the database studies, none of them investigated the effect of penetration speed on the TR parameters. However, Huang et at. [161] applied a very low nail speed of 0.02 mm/s on a 3 Ah pouch cell to encode the sequence of nail penetration events. By incorporating a thermocouple in the nail tip, they observed several temperature peaks upon intrusion. These peaks are attributed to the contact of the nail tip with the aluminum current collector foil forming a low resistance, high current ISC circuit with rapid heat generation. Intermediate drops in temperature appear when the aluminum foil ruptures, which temporarily mitigates the current flow by dramatic contact resistance increase. Based on this observation it may be concluded that altering the nail speed can modify the short circuit behavior and therefore potentially the TR behavior. Note that nail penetration does not safely trigger TR. Indeed An et al. could not force TR for cells at SOC = 50% independent of cathode material and nail diameter by fully penetrating the large surface center of each pouch cell [162].

3.9.5. Gas Atmosphere

The gas atmosphere mainly influences the likelihood of vent gas combustion. Inert atmospheres with helium, argon or nitrogen limit the vent gas combustion to the consumption of the oxygen provided by the cathode material and electrolyte decomposition. The much higher combustion degree in air atmosphere is shown by a higher CO2 and lower fuel mole fractions [78] in the vent gas after TR. No other effects on the TR variables by the gas atmosphere are observed [28].

3.9.6. Ambient Conditions

Ambient TR test conditions, i.e., start pressure and temperature, are varied in a few studies. Ding et al. could not find any correlation between TR temperatures or mass loss and ambient pressure for an overheated cylindrical 5 Ah NMC cell [163]. Contrary to that, Liu et al. observed a decrease in maximum cell temperature, a slight decrease in mass loss and slower propagation for low pressure conditions when overheating a six-cell array of cylindrical 2.2 Ah NMC532 cells at 30% and 100% SOC [164]. They concluded that low pressure could weaken both external flame combustion and internal TR reactions. Similar findings were made by Jin et al. overheating a cylindrical 2.6 Ah NMC811 cell [165] and Meng et al. overheating a cylindrical 2.6 Ah NMC523 cell [166]. The latter further determined a lower temperature rise rate at low pressure. Sun et al. consistently measured lower peak temperatures at lower pressure for different setups [167]. Reducing the ambient temperature in the test results in disproportionately lower peak cell temperature, lower temperature rise rate and slightly lower mass loss, when overheating a cylindrical 2.6 Ah NMC523 cell [166]. Zhou et al. nail penetrated a cylindrical 3.5 Ah NMC811 cell at 75% SOC and different preheating temperatures between 10 °C and 160 °C [168]. They confirmed disproportionately higher peak temperature and higher mass loss and detected more oxygen in the vent particles at higher temperature. Interestingly, at 160 °C the nail penetration could not trigger TR. The authors suggest that separator shutdown mitigated the short circuit by the nail. Wang et al. studied the overcharging behavior of 7 Ah LCO pouch cells at increasing preconditioning temperatures and also found disproportionately higher maximum cell temperature [159].

3.9.7. Multi-Cell Tests

Multi-cell test setups affect the TR characteristics as found by several studies. Higher peak temperatures can be measured during thermal propagation compared to single cell tests [125,132,169]. The effect of the electrical interconnection is inconclusive. While some studies determined higher peak temperature and faster propagation for parallelly connected cells [125,170], others could not measure significant differences between interconnection modes [171,172]. The heat conduction through the electrical connection is minor compared to that over the battery shell [170,171]. However, it is acknowledged that electrical energy may be transferred from the parallel intact cells to the triggered cell [125,172]. Zhou et al. found lower TR trigger temperature in multi-parallel setups and marked the electrical energy transfer to the triggered cell as the dominant cause [173]. For their 50 Ah prismatic LFP cell they could observe continuous discharge of the neighboring cells even after the trigger cell TR. This discharge ultimately caused vent gas ignition highlighting a severe safety hazard in parallelly connected LFP cells.

3.9.8. Summary of Test Setup Findings

The key findings of this exploratory analysis of test setup effects, based on case studies, are summarized in Table 5. Note that the given effect size indications are only rough estimates and cannot be used for definite conclusions as the confidence levels are relatively low. Many dependencies remain unknown. The determination of the self-heating temperature requires an ARC setup that heats the cell from all sides with the HWS protocol. Thus, test vessel type, trigger position and trigger rate only contain one exclusive category with no degree of freedom for T1. While the test vessel type has no effect on the TR behavior, if all other boundary conditions are consistent, the test jig influences most parameters. Most significantly the maximum external cell temperature may vary due to different heat transfer paths and secure fixation options of thermocouples. The trigger position can have moderate effects on the cell temperature and its rise rate as well as the venting behavior reflected by the different mass loss fractions Yloss,i. Similarly, the trigger rate and speed may affect most variables in specific instances. Considering the potential of gas ignition, the gas atmosphere mainly alters the peak gas temperature as well as the gas composition. Ambient conditions may affect peak temperatures and mass loss by altering the TR reactions and venting behavior. There is no information available about the onset temperatures. This also applies to multi-cell tests, which typically tend to result in higher peak temperatures. Considering all these potential dependencies, it would be beneficial to standardize efforts on a test setup that determines all relevant TR parameters. This would improve comparability across studies and increase confidence in the results.
Table 5. Summary of test setup findings with effect size indicators (+: large; o: moderate; –: small; ?: unknown; excl.: exclusive) and color code for confidence level (high, moderate, low).

3.10. Emerging Battery Technologies

In recent years, studies on emerging battery technologies such as solid-state batteries (SSB) and sodium-ion batteries (SIB) have been published. The test count in the database is too low for statistical analysis, but exemplary findings are reported in this section.

3.10.1. Solid-State Batteries

Due to missing commercial alternatives Charbonnel et al. modified a commercial NMC811 cylindrical cell into an all SSB (ASSB) with a poly(ethylene oxide)-lithium lanthanum zirconium oxide (PEO-LLZO) composite solid electrolyte and compared its TR characteristics to the original cell [174]. The ASSB had slightly lower TR trigger temperature and significantly faster reaction time but reached slightly lower peak temperature and released significantly less gas thanks to the missing liquid electrolyte. In another study, this research group additionally altered the anode material from Si-doped graphite to lithium-metal and observed very high peak temperatures around 1400 °C and explosive TR within milliseconds, but less gas generation due to further reduction of combustible material [175]. Theoretical calculations suggest that SSB with high energy density will surpass liquid electrolyte LIB heat generation and peak cell temperature during TR posing severe safety hazards [176].

3.10.2. Sodium-Ion Batteries

For SIB several empirical studies are published that compare their TR behavior to LIB with LFP and NMC chemistry. Regarding the characteristic temperatures, some studies reported the lowest self-heating onset for SIB [177,178], while others found T1 to be close to LFP cells [77,179]. Similarly, the venting temperature was lowest [178,179] or between LFP and NMC [77,177]. The TR trigger temperature, the maximum cell temperature and the maximum temperature rise rate are mostly between LFP and NMC cells with significant deviations between studies [77,177,178,179]. While for small-scale cylindrical cells the peak temperature was often measured below 400 °C [97,177,180,181,182], studies on large-format prismatic cells reported higher temperatures up to 800 °C [179,182,183]. SIB experience significant mass loss during venting between 18–75%. Due to relatively high normalized vent gas volumes of ~2 L/Ah [77,97,183] and moderate venting duration positioned between LFP and NMC cells [87], significant particle mass is vented during TR [77,97]. Li et al. monitored hot particles ejected as sparks for a 185 Ah prismatic cell, but did not observe vent gas ignition, probably due to the low vent gas temperature of 163 °C [183]. Similarly, no ignition was observed by Bordes et al. [180] and Fedoryshyna et al. [182]. Opposingly, Li et al. reported ignition in two out of three tests for a 70 Ah prismatic cell, though it exhibited self-extinguishing behavior after a short period of time [87]. Vent gas compositions are similar to LFP cells with a large fraction of electrolyte vapors [180] as well as high H2, moderate CO and high CO2 content [183]. Ping et al. measured a large methane mole fraction of XCH4 = 0.23 and low hydrogen content of XH2 = 0.06 [177]. They additionally reported possible gas generation reactions adapted from LIB reaction schemes. The TR behavior after aging was analyzed by Zhou et al. [181]. They found reduced T1, T2 and T3,ext for a SIB at SOH = 80% after over 4000 cycles highlighting slightly more critical onset conditions, but lower overall heat release for cycle-aged cells at a moderate temperature of 25 °C. To summarize, SIB experience TR with similar characteristics to LIB. Although all SIB investigated in the above studies possess lower energy density than LFP cells, their TR safety hazards can mostly be positioned between LFP and NMC cells. It also must be mentioned that, similar to LIB, several different cell chemistries, especially cathode materials are used in SIB. Their thermal stability and heat release vary and especially layered-oxide NFM111 cathodes tend to generate more heat at material-level DSC analysis than NMC111 [184]. Strictly speaking the TR behavior of SIB cannot be clustered in one group and significant differences as observed in above studies are expected.

4. Conclusions and Outlook

Lithium-ion battery fires, typically initiated by the thermal runaway of a single cell, remain a critical safety concern in electric vehicles and stationary storage applications. To mitigate battery fires by incorporating system-level design measures, the TR behavior of the cell under consideration needs to be well understood. Thermal runaway is a highly complex, multi-stage process involving coupled physics, with many interdependent influencing factors that make its onset and progression difficult to predict.
This study aims to bridge the gap between high-level mechanistic reviews and detailed but narrowly scoped experimental campaigns by providing a database-driven review with exploratory statistical analysis of the parameters that govern TR behavior. It aims to serve as the most comprehensive review of TR experiments in the literature and addresses the limitations of previous large-scale studies as listed in Table 6.
Table 6. Limitations of previous large-scale studies addressed in this review.
To this end, the largest publicly available literature database on TR experiments comprising 1703 tests from 257 papers was compiled into 203 variables that describe cell properties, test specifications, and TR outcomes in a comprehensive manner. For the first time, statistical measures are calculated to support the holistic evaluation of TR characteristics, combining descriptive statistics, correlation measures, and effect-size-based ANOVA with false-discovery-rate control. The large sample size enhances confidence in the reported correlations and enables the determination of recurring patterns in the dataset. Key findings of this analysis can be summarized as follows:
  • Cathode chemistry, specific energy and SOC are the factors most strongly associated with TR onset, peak temperatures, and temperature rise rate. Across all characteristic TR temperatures, moderate to large effects can be attributed to cathode chemistry, with the oxygen-release mechanism emerging as the primary driver. LFP and LCO cells exhibit the highest self-heating onset temperature, whereas Ni-rich NMC and NCA cells show lower TR trigger temperature, higher maximum temperature and temperature rise rate, consistent with their lower thermal stability and stronger oxygen release. Cell design mainly affects vent opening and voltage-drop temperature due to pressure-relief and current-interrupt features. Specific energy, energy density, and SOC-corrected specific capacity, respectively, show negligible effect on vent opening and voltage-drop temperature, but have a strong positive correlation with temperature rise rate and maximum gas temperature, and a moderate positive correlation with peak cell temperatures, while high values slightly reduce self-heating onset and TR trigger temperature. SOC in the normal operating range has limited influence on T1, Tvent and TV0, but higher SOC typically lowers T2 and increases TR severity via enhanced lithiation-related reactivity at the anode and cathode. SOH and the aging history show surprisingly limited and often inconsistent effects on most TR temperatures, except for low-temperature cycling, which reduces the self-heating onset due to lithium plating and destabilized SEI.
  • A significant amount of mass is vented from the cell during TR. The relative mass loss can be as high as 90% of the initial cell mass and scales strongly with cathode material and with indicators of TR severity such as peak cell and gas temperature and maximum temperature rise rate. Energy density shows a stronger correlation with relative mass loss than specific energy, highlighting that reaction intensity per unit volume and associated internal pressure build-up are key determinants of structural damage and ejecta formation. Even at SOC = 0%, non-negligible mass loss occurs due to SEI decomposition and electrolyte vaporization, implying that discharged cells remain potentially hazardous when abused.
  • The total vent gas volume scales roughly linearly with nominal capacity, with an average of 1.7 L/Ah at SATP across all chemistries, but normalization by capacity reveals pronounced cathode material dependency. LFP cells vent significantly less gas per Ah than NMC-based cells, and normalized vent gas volume increases with increasing nickel content, in the order LFP < NCA < LMO < LCO < NMC532 < NMC622 < NMC811. Venting duration spans more than three orders of magnitude and is frequently associated with cathode chemistry and cell size. Large-format prismatic LFP cells often vent over tens to hundreds of seconds, while Ni-rich NMC and NCA cells and small cylindrical cells frequently exhibit highly violent venting within seconds. Higher normalized vent gas flow rates are associated with larger relative mass loss, reflecting enhanced structural damage and particle ejection in explosive events. In extreme cases, more than 60% of the cell mass can be expelled as particles, carrying a substantial fraction of the TR energy out of the cell. The partitioning of cell mass loss into gas and particle fractions depends on cathode material and is strongly influenced by measurement methods.
  • Gas composition analysis reveals that H2, CO and CO2 are the dominant species, typically followed by small-chain hydrocarbons such as CH4, C2H4 and C3H6, and, where detected with suitable methods, electrolyte vapors and HF. The normalized six-gas composition discloses strong dependence on cathode chemistry. LFP cells emit higher fractions of H2 and lower fractions of CO than cells with lithium-metal-oxide cathodes, reflecting differences in oxygen release and degree of reactant conversion. Increased TR severity, indicated by higher peak temperatures and larger mass loss, correlates with higher CO and lower hydrocarbon fractions, consistent with more complete oxidation of organic components. Higher SOC and specific energy promote higher CO and lower heavier hydrocarbon fractions, in line with enhanced cathode oxygen release and electrolyte oxidation at high cathode delithiation and high energy density. Many components that are liquid in ambient conditions, such as electrolyte vapors and water, are strongly under-reported and their detection depends on gas sampling and analysis temperatures. Non-negligible electrolyte mole fractions are observed with proper test methods. Sparse but growing evidence for species such as HCN, NOx, PF3, POF3, and other fluorinated gases suggests that TR vent gases can be more diverse and toxic than commonly captured. Flameless venting in air is accommodated by a vent gas temperature below 500 °C, which can serve as a rough ignition threshold when developing battery systems towards “no fire” requirements.
  • The type of abuse is an important variable to consider in TR experiments. Overcharge-induced TR is characterized by additional electrochemical processes that lead to significantly lower TR onset temperatures. Nail penetration tends to produce the highest temperature rise rates due to the sudden TR initiation in fully intact cells. For many other result variables, trends across abuse types are weaker or obscured by limited sample sizes, especially for mechanical and electrical abuses.
  • Several aspects of the TR test setup strongly influence the test results. While the test vessel type itself has limited direct influence on TR behavior, if boundary conditions are matched, the test jig, trigger position, and trigger rate or speed can substantially change measured peak temperatures, temperature rise rate, venting behavior, and mass-loss fraction by altering heat transfer paths, structural constraints, as well as short-circuit and TR reaction dynamics. Gas atmosphere mainly affects vent gas temperature and composition through the possibility of gas-phase combustion. Ambient pressure and temperature as well as multi-cell configurations can shift peak temperatures, mass loss, or propagation behavior.
  • Emerging battery technologies like solid-state and sodium-ion batteries are still at risk of exhibiting severe TR. While solid-state cells may surpass liquid electrolyte LIB heat generation, the available studies suggest that SIB TR safety hazards can be mostly positioned between LFP and NMC cells, although they are lower in energy density. SIB recently entered the market, and the number of TR studies has increased since then. In contrast, experimental TR research on solid-state cells is scarce because these cells are still in development, and manufacturers keep their know-how secret. Due to the small sample size, available results are preliminary and further research on these new battery types is necessary.
  • Multiple distinct correlations between different TR result variables suggest that “typical” TR regimes exist for given combinations of input parameters. For example, small, high-Ni NMC or NCA cylindrical cells at high SOC tend to exhibit low onset temperatures, high heat release, large, normalized gas volume and flow rate, and substantial particle ejection, consistent with highly explosive TR. In contrast, large-format LFP prismatic cells often show higher onset temperatures, lower peak temperatures and temperature rise rate, reduced normalized gas volume, longer vent duration, and comparatively lower mass loss, indicative of slower, less violent TR. Such typical behaviors, while not universal, provide useful information for example during cell selection for a specific application.
The database and statistical results provide multiple entry points for practical applications. System developers and pack designers can benchmark the TR characteristics of candidate cells against a broad set of existing cells with similar chemistries, formats, and energy densities to judge safety performance in a data-informed way. Furthermore, several of the reported variables are directly relevant to battery system design, such as vent gas volume flow rate and gas temperature for sizing pressure relief devices and vent channels, or characteristic temperatures for calibrating TR and TP models. This review aims to provide a broad overview of TR characteristics, which is especially useful for new students or researchers in the field. At the same time, the analysis highlights that many variables in the database are still scarcely populated, limiting statistical rigor and underlining the need for targeted experiments in these areas. Specifically, the following future research perspectives can be identified:
  • While this database covers a large range of cell capacities, small-capacity cylindrical cells that are often off-the-shelf are overrepresented, most likely due to their abundant availability, lower requirements for testing equipment and lower testing costs. To reduce this bias and to account for the large-scale adoption of high-capacity cells, e.g., for automotive and BESS applications, studies on these cells should be prioritized.
  • As the number of aged battery systems on the market increases, understanding safety hazards related to aging have become more important. This study emphasizes the critical role of the exact aging history on TR behavior. Due to interdependencies with aging temperature, cycling current, and cycling SOC, much more data is required to draw definitive conclusions. Valuable insides would be provided by testing cells from real-world applications with a recorded operating history.
  • Overheating, particularly when used with the HWS protocol, is widely applied as the standard trigger method for TR. While ARC tests are very well suited for model development, and one-sided overheating best reflects propagation conditions in most battery systems, further research on mechanical and electrical abuse is required to draw statistical conclusions about the effects of trigger methods. In light of emerging non-propagation requirements, emphasis should also be placed on test conditions that best reflect initial cell malfunctions in full battery systems. Localized triggers with single-electrode layer damage would best reflect real-world failures due to cell manufacturing defects.
  • Extensive gas analysis during TR is a challenging task. The scope and quality of reported vent gas compositions vary significantly between studies. Holistic characterization strategies should be developed to evaluate toxicity, ignition risk and combustion pathways of battery vent gases more precisely. This will require a combination of complementary analytical techniques and systematic study of sampling time and location effects, as well as controlled sampling and analysis temperature.
  • The vent particles can inherit a significant fraction of the TR energy and pose severe safety hazards in battery systems. Nevertheless, few studies investigated the particle characteristics in detail highlighting a current research gap.
  • While the TR literature on SSB is scarce, the study count on SIB TR experiments has increased significantly over the past years. However, additional research on these emerging cell technologies is necessary to derive more rigorous conclusions on their safety behavior.
  • The compiled database highlights that many potentially relevant parameters are seldomly reported, even though they may be accessible within typical experimental setups. To improve comparability and enable more robust cross-study analysis, future work should target consistent reporting of all relevant boundary conditions and aim to maximize the number of measured output variables within practical constraints. For example, more frequent measurements of the internal cell temperature, which can be several hundred Kelvin higher than externally measured values, would provide valuable insides about the actual conditions at the core of the reactions and would support more accurate modeling. Furthermore, existing uncertainties in measuring gas quantity and composition as well as complete particle sampling should be acknowledged by separate quantification of gas and particle masses. Thereby, mass conservation can be validated and uncertainties associated with the experimental setup can be quantified.
  • A large variety of different test setups and boundary conditions can be found in reported TR experiments. To promote comparability between results and increase confidence in experimental data, efforts to develop standardized test protocols capable of capturing all relevant TR parameters should be intensified. To find common ground between stakeholders, application relevant boundary conditions should be considered.
Looking ahead, we intend to further populate the database and publish an update to this study in the future. We explicitly invite the research community to contribute data suggestions from peer-reviewed papers that we currently miss, especially investigations on less researched TR aspects. By increasing the database, the trust in observed correlations will grow and currently under-represented variables may reveal new, statistically relevant trends. This review provides a broad overview of thermal runaway characteristics and dependencies. Beyond the exploratory pairwise statistical analysis presented here, future work can apply hypothesis-driven statistical tests, multivariate modeling and clustering algorithms to verify and refine the presented conclusions and to resolve confounding effects more rigorously. Due to the sparse nature of the database, extensive data preparation is required for these investigations. Variables with low population cannot be considered because multivariate methods rely on data completeness. Thus, only a few well populated variables with rather low sample count could be analyzed with the current state of the database. Alternatively, advanced techniques must be applied to fill missing values intelligently without biasing the data. To derive reasonable conclusions on ranked contributions of individual variables from advanced statistical methods, a common data reporting standard is required. Future studies should, therefore, focus on improving data completeness across variables as well as data consistency. After collecting more data from studies with complete datasets and consistently reported variables, machine learning approaches may become viable tools to extract hidden patterns more efficiently and to predict TR results from cell characteristics and test specifications. Taking the findings from this study into consideration, we aim to develop a standardized test setup that covers all aspects of thermal runaway and minimizes setup-related effects, thereby enabling more reliable safety assessment and model development across the battery community.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/batteries12070240/s1, Table S1: Self-heating onset temperature T1—significant statistics with moderate or large effect size; Table S2: Vent opening temperature Tvent—significant statistics with moderate or large effect size; Table S3: Voltage drop temperature TV0—significant statistics with moderate or large effect size; Table S4: Thermal runaway trigger temperature T2—significant statistics with moderate or large effect size; Table S5: Maximum external cell temperature T3,ext—significant statistics with moderate or large effect size; Table S6: Maximum internal cell temperature T3,int—significant statistics with moderate or large effect size; Table S7: Logarithmic maximum temperature gradient log(dT/dtmax)—significant statistics with moderate or large effect size; Table S8: Maximum vent gas temperature Tgas,max—significant statistics with moderate or large effect size; Table S9: Relative mass loss—significant statistics with moderate or large effect size; Table S10: Time until maximum temperature—significant statistics with moderate or large effect size; Table S11: Time until voltage drop—significant statistics with moderate or large effect size; Table S12: Vent gas volume—significant statistics with moderate or large effect size; Table S13: Normalized vent gas volume—significant statistics with moderate or large effect size; Table S14: Venting duration—significant statistics with moderate or large effect size; Table S15: Normalized vent gas volume flow rate—significant statistics with moderate or large effect size; Table S16: Normalized particle mass—significant statistics with moderate or large effect size; Table S17: Particle mass loss fraction—significant statistics with moderate or large effect size; Table S18: Mole fractions of vent gases—significant statistics with moderate or large effect size.

Author Contributions

Conceptualization, F.E.; Methodology, F.E.; Formal Analysis, F.E.; Investigation, F.E.; Resources, S.P.; Data Curation, F.E.; Writing—Original Draft Preparation, F.E.; Writing—Review and Editing, S.P.; Visualization, F.E.; Supervision, S.P. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Data Availability Statement

The original data presented in the study are openly available in Zenodo at https://doi.org/10.5281/zenodo.18232447 (accessed on 26 June 2026).

Acknowledgments

During the preparation of this manuscript, the authors used ChatGPT 5 to rephrase some paragraphs and increase clarity. The authors have reviewed and edited the output and take full responsibility for the content of this publication.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Bloomberg Finance L.P. Global Energy Storage Market Records Biggest Jump Yet. Available online: https://about.bnef.com/blog/global-energy-storage-market-records-biggest-jump-yet/ (accessed on 15 December 2024).
  2. Kebede, A.A.; Kalogiannis, T.; van Mierlo, J.; Berecibar, M. A comprehensive review of stationary energy storage devices for large scale renewable energy sources grid integration. Renew. Sustain. Energy Rev. 2022, 159, 112213. [Google Scholar] [CrossRef] [Scilit]
  3. TÜV-Verband e. V. TÜV Mobility Studie 2024. 2024. Available online: https://tuev-verband.de/studien/tuev-mobility-studie-2024 (accessed on 1 June 2026).
  4. The University of Texas Fire Research Group. Battery Fire and Explosion Incidents: Database Tools. Available online: https://tools.utfireresearch.com/apps/incident_map (accessed on 15 December 2024).
  5. Peng, R.; Kong, D.; Ping, P.; Wang, G.; Gao, X.; Lv, H.; Zhao, H.; He, X.; Zhang, Y.; Dai, X. Thermal runaway modeling of lithium-ion batteries at different scales: Recent advances and perspectives. Energy Storage Mater. 2024, 69, 103417. [Google Scholar] [CrossRef] [Scilit]
  6. Feng, X.; Ouyang, M.; Liu, X.; Lu, L.; Xia, Y.; He, X. Thermal runaway mechanism of lithium ion battery for electric vehicles: A review. Energy Storage Mater. 2018, 10, 246–267. [Google Scholar] [CrossRef] [Scilit]
  7. GB 38031-2020; Electric Vehicles Traction Battery Safety Requirements. State Administration for Market Regulation. Standardization Administration of the People’s Republic of China: Beijing, China, 2020.
  8. ECE R100; Uniform Provisions Concerning the Approval of Vehicles with Regard to Specific Requirements for the Electric Power Train. 3rd ed. United Nations: New York, NY, USA, 2022.
  9. GB 38031-2025; Electric Vehicles Traction Battery Safety Requirements. State Administration for Market Regulation. Standardization Administration of the People’s Republic of China: Beijing, China, 2025.
  10. RTCA, Inc. DO-311A—Minimum Operational Performance Standards for Rechargeable Lithium Batteries and Battery Systems; RTCA, Inc.: Washington, DC, USA, 2017. [Google Scholar]
  11. The European Parliament and the Council of the European Union. Regulation (EU) 2023/1542 of the European Parliament and of the Council of 12 July 2023 Concerning Batteries and Waste Batteries, Amending Directive 2008/98/EC and Regulation (EU) 2019/1020 and Repealing Directive 2006/66/EC, 2023. Available online: https://eur-lex.europa.eu/eli/reg/2023/1542/oj/eng (accessed on 1 June 2026).
  12. Elsevier, B.V. Scopus Search: “Thermal Runaway in Batteries”. Available online: https://www.scopus.com/pages/search/publications?searchId=00f2f183-d144-40f3-b0e7-c9445386f928 (accessed on 25 August 2025).
  13. Feng, X.; Zheng, S.; He, X.; Wang, L.; Wang, Y.; Ren, D.; Ouyang, M. Time Sequence Map for Interpreting the Thermal Runaway Mechanism of Lithium-Ion Batteries With LiNixCoyMnzO2 Cathode. Front. Energy Res. 2018, 6, 126. [Google Scholar] [CrossRef] [Scilit]
  14. Wang, Q.; Mao, B.; Stoliarov, S.I.; Sun, J. A review of lithium ion battery failure mechanisms and fire prevention strategies. Prog. Energy Combust. Sci. 2019, 73, 95–131. [Google Scholar] [CrossRef] [Scilit]
  15. Li, W.; Xue, Y.; Feng, X.; Liu, J.; Zhang, F.; Rao, S.; Zhang, T.; Gao, Z.; Du, Z.; Ni, C.; et al. Enhancing understanding of particle emissions from lithium-ion traction batteries during thermal runaway: An overview and challenges. eTransportation 2024, 22, 100354. [Google Scholar] [CrossRef] [Scilit]
  16. Wang, S.; Wang, Q.; Xu, L.; Sun, Y.; Feng, X.; Wang, H. A review on mechanisms, characteristics and relating hazards of vent gases from thermally abused Li-ion batteries. J. Energy Storage 2024, 84, 110892. [Google Scholar] [CrossRef] [Scilit]
  17. Wang, G.; Ping, P.; Kong, D.; Peng, R.; He, X.; Zhang, Y.; Dai, X.; Wen, J. Advances and challenges in thermal runaway modeling of lithium-ion batteries. Innovation 2024, 5, 100624. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  18. Vujnović, N.; Hohenberg, K.; Höschele, P.; Moser, J.; Ellersdorfer, C. A comprehensive review of thermal runaway and thermal runaway propagation modelling approaches in lithium-ion batteries. J. Energy Storage 2025, 139, 118685. [Google Scholar] [CrossRef] [Scilit]
  19. Hu, D.; Huang, S.; Wen, Z.; Gu, X.; Lu, J. A review on thermal runaway warning technology for lithium-ion batteries. Renew. Sustain. Energy Rev. 2024, 206, 114882. [Google Scholar] [CrossRef] [Scilit]
  20. Kong, D.; Lv, H.; Ping, P.; Wang, G. A review of early warning methods of thermal runaway of lithium ion batteries. J. Energy Storage 2023, 64, 107073. [Google Scholar] [CrossRef] [Scilit]
  21. Zhang, X.; Chen, S.; Zhu, J.; Gao, Y. A Critical Review of Thermal Runaway Prediction and Early-Warning Methods for Lithium-Ion Batteries. Energy Mater. Adv. 2023, 4, 0008. [Google Scholar] [CrossRef] [Scilit]
  22. Ouyang, D.; Chung, Y.-H.; Liu, J.; Bai, J.; Zhou, Y.; Chen, S.; Wang, Z.; Shu, C.-M. Characteristics and mechanisms of as well as evaluation methods and countermeasures for thermal runaway propagation in lithium-ion batteries. Prog. Energy Combust. Sci. 2025, 108, 101209. [Google Scholar] [CrossRef] [Scilit]
  23. Victor Chombo, P.; Laoonual, Y.; Wongwises, S. Lessons from the Electric Vehicle Crashworthiness Leading to Battery Fire. Energies 2021, 14, 4802. [Google Scholar] [CrossRef] [Scilit]
  24. Lai, X.; Yao, J.; Jin, C.; Feng, X.; Wang, H.; Xu, C.; Zheng, Y. A Review of Lithium-Ion Battery Failure Hazards: Test Standards, Accident Analysis, and Safety Suggestions. Batteries 2022, 8, 248. [Google Scholar] [CrossRef] [Scilit]
  25. Ruiz, V.; Pfrang, A.; Kriston, A.; Omar, N.; van den Bossche, P.; Boon-Brett, L. A review of international abuse testing standards and regulations for lithium ion batteries in electric and hybrid electric vehicles. Renew. Sustain. Energy Rev. 2018, 81, 1427–1452. [Google Scholar] [CrossRef] [Scilit]
  26. Koch, S.; Fill, A.; Birke, K.P. Comprehensive gas analysis on large scale automotive lithium-ion cells in thermal runaway. J. Power Sources 2018, 398, 106–112. [Google Scholar] [CrossRef] [Scilit]
  27. Feng, X.; Zheng, S.; Ren, D.; He, X.; Wang, L.; Cui, H.; Liu, X.; Jin, C.; Zhang, F.; Xu, C.; et al. Investigating the thermal runaway mechanisms of lithium-ion batteries based on thermal analysis database. Appl. Energy 2019, 246, 53–64. [Google Scholar] [CrossRef] [Scilit]
  28. Willstrand, O.; Pushp, M.; Andersson, P.; Brandell, D. Impact of different Li-ion cell test conditions on thermal runaway characteristics and gas release measurements. J. Energy Storage 2023, 68, 107785. [Google Scholar] [CrossRef] [Scilit]
  29. Rappsilber, T.; Yusfi, N.; Krüger, S.; Hahn, S.-K.; Fellinger, T.-P.; Krug von Nidda, J.; Tschirschwitz, R. Meta-analysis of heat release and smoke gas emission during thermal runaway of lithium-ion batteries. J. Energy Storage 2023, 60, 106579. [Google Scholar] [CrossRef] [Scilit]
  30. Finegan, D.P.; Billman, J.; Darst, J.; Hughes, P.; Trillo, J.; Sharp, M.; Benson, A.; Pham, M.; Kesuma, I.; Buckwell, M.; et al. The battery failure databank: Insights from an open-access database of thermal runaway behaviors of Li-ion cells and a resource for benchmarking risks. J. Power Sources 2024, 597, 234106. [Google Scholar] [CrossRef] [Scilit]
  31. Bugryniec, P.J.; Resendiz, E.G.; Nwophoke, S.M.; Khanna, S.; James, C.; Brown, S.F. Review of gas emissions from lithium-ion battery thermal runaway failure—Considering toxic and flammable compounds. J. Energy Storage 2024, 87, 111288. [Google Scholar] [CrossRef] [Scilit]
  32. Elsner, F. Thermal Runaway in Lithium-Ion Batteries: Database and Statistical Analysis Results; Lehrstuhl für Thermodynamik Mobiler Energiewandlungssysteme und Institut für Thermodynamik: Aachen, Germany, 2026. [Google Scholar] [CrossRef]
  33. Rohatgi, A. WebPlotDigitizer v4.8. Available online: https://apps.automeris.io/wpd4/ (accessed on 1 June 2026).
  34. Gupta, B.C.; Guttman, I.; Jayalath, K. Statistics and Probability with Applications for Engineers and Scientists Using Minitab, R and JMP, 2nd ed.; Wiley: Hoboken, NJ, USA, 2020; ISBN 9781119516637. [Google Scholar]
  35. Cohen, J. Statistical Power Analysis for the Behavioral Sciences, 2nd ed.; Erlbaum: Hillsdale, NJ, USA, 1988; ISBN 0-8058-0283-5. [Google Scholar]
  36. Kirk, R.E. Practical Significance: A Concept Whose Time Has Come. Educ. Psychol. Meas. 1996, 56, 746–759. [Google Scholar] [CrossRef] [Scilit]
  37. Benjamini, Y.; Hochberg, Y. Controlling the False Discovery Rate: A Practical and Powerful Approach to Multiple Testing. J. R. Stat. Soc. Ser. B Stat. Methodol. 1995, 57, 289–300. [Google Scholar] [CrossRef] [Scilit]
  38. Zhou, H.; Parmananda, M.; Crompton, K.R.; Hladky, M.P.; Dann, M.A.; Ostanek, J.K.; Mukherjee, P.P. Effect of electrode crosstalk on heat release in lithium-ion batteries under thermal abuse scenarios. Energy Storage Mater. 2022, 44, 326–341. [Google Scholar] [CrossRef] [Scilit]
  39. Hou, J.; Feng, X.; Wang, L.; Liu, X.; Ohma, A.; Lu, L.; Ren, D.; Huang, W.; Li, Y.; Yi, M.; et al. Unlocking the self-supported thermal runaway of high-energy lithium-ion batteries. Energy Storage Mater. 2021, 39, 395–402. [Google Scholar] [CrossRef] [Scilit]
  40. Yang, H.; Zhuang, G.V.; Ross, P.N. Thermal stability of LiPF6 salt and Li-ion battery electrolytes containing LiPF6. J. Power Sources 2006, 161, 573–579. [Google Scholar] [CrossRef] [Scilit]
  41. Nie, B.; Dong, Y.; Chang, L. The evolution of thermal runaway parameters of lithium-ion batteries under different abuse conditions: A review. J. Energy Storage 2024, 96, 112624. [Google Scholar] [CrossRef] [Scilit]
  42. Feng, X.; Ren, D.; Zhang, S.; He, X.; Wang, L.; Ouyang, M. Influence of aging paths on the thermal runaway features of lithium-ion batteries in accelerating rate calorimetry tests. Int. J. Electrochem. Sci. 2019, 14, 44–58. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  43. Fleischhammer, M.; Waldmann, T.; Bisle, G.; Hogg, B.-I.; Wohlfahrt-Mehrens, M. Interaction of cyclic ageing at high-rate and low temperatures and safety in lithium-ion batteries. J. Power Sources 2015, 274, 432–439. [Google Scholar] [CrossRef] [Scilit]
  44. Golubkov, A.W.; Scheikl, S.; Planteu, R.; Voitic, G.; Wiltsche, H.; Stangl, C.; Fauler, G.; Thaler, A.; Hacker, V. Thermal runaway of commercial 18650 Li-ion batteries with LFP and NCA cathodes—Impact of state of charge and overcharge. RSC Adv. 2015, 5, 57171–57186. [Google Scholar] [CrossRef] [Scilit]
  45. Xu, K. Nonaqueous liquid electrolytes for lithium-based rechargeable batteries. Chem. Rev. 2004, 104, 4303–4417. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  46. Kahr, J.; Groher, C.; Schierer, V.; Rosenberg, E.; Jahn, M. Operando gas chromatography mass spectrometry for the continuous study of overcharge-induced electrolyte decomposition in lithium-ion batteries. J. Power Sources 2024, 615, 235038. [Google Scholar] [CrossRef] [Scilit]
  47. Feinauer, M.; Abd-El-Latif, A.A.; Sichler, P.; Aracil Regalado, A.; Wohlfahrt-Mehrens, M.; Waldmann, T. Change of safety by main aging mechanism—A multi-sensor accelerating rate calorimetry study with commercial Li-ion pouch cells. J. Power Sources 2023, 570, 233046. [Google Scholar] [CrossRef] [Scilit]
  48. Tang, X.; Zhang, G.; Wang, X.; Wei, G.; Han, G.; Zhu, J.; Wei, X.; Dai, H. Investigating the critical characteristics of thermal runaway process for LiFePO4/graphite batteries by a ceased segmented method. iScience 2021, 24, 103088. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  49. Shurtz, R.C.; Engerer, J.D.; Hewson, J.C. Predicting High-Temperature Decomposition of Lithiated Graphite: Part I. Review of Phenomena and a Comprehensive Model. J. Electrochem. Soc. 2018, 165, A3878–A3890. [Google Scholar] [CrossRef] [Scilit]
  50. Feng, X.; Zheng, S.; Ren, D.; He, X.; Wang, L.; Liu, X.; Li, M.; Ouyang, M. Key Characteristics for Thermal Runaway of Li-ion Batteries. Energy Procedia 2019, 158, 4684–4689. [Google Scholar] [CrossRef] [Scilit]
  51. Noh, H.-J.; Youn, S.; Yoon, C.S.; Sun, Y.-K. Comparison of the structural and electrochemical properties of layered Li[NixCoyMnz]O2 (x = 1/3, 0.5, 0.6, 0.7, 0.8 and 0.85) cathode material for lithium-ion batteries. J. Power Sources 2013, 233, 121–130. [Google Scholar] [CrossRef] [Scilit]
  52. Lamb, J.; Torres-Castro, L.; Hewson, J.C.; Shurtz, R.C.; Preger, Y. Investigating the Role of Energy Density in Thermal Runaway of Lithium-Ion Batteries with Accelerating Rate Calorimetry. J. Electrochem. Soc. 2021, 168, 60516. [Google Scholar] [CrossRef] [Scilit]
  53. Cui, Z.; Manthiram, A. Thermal Stability and Outgassing Behaviors of High-nickel Cathodes in Lithium-ion Batteries. Angew. Chem. Int. Ed. Engl. 2023, 62, e202307243. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  54. Liu, X.; Yin, L.; Ren, D.; Wang, L.; Ren, Y.; Xu, W.; Lapidus, S.; Wang, H.; He, X.; Chen, Z.; et al. In situ observation of thermal-driven degradation and safety concerns of lithiated graphite anode. Nat. Commun. 2021, 12, 4235. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  55. Dahn, J.R.; Fuller, E.W.; Obrovac, M.; von Sacken, U. Thermal stability of LixCoO2, LixNiO2 and λ-MnO2 and consequences for the safety of Li-ion cells. Solid State Ion. 1994, 69, 265–270. [Google Scholar]
  56. Bang, H.J.; Joachin, H.; Yang, H.; Amine, K.; Prakash, J. Contribution of the Structural Changes of LiNi0.8Co0.15Al0.05O2 Cathodes on the Exothermic Reactions in Li-Ion Cells. J. Electrochem. Soc. 2006, 153, A731–A737. [Google Scholar]
  57. Ren, D.; Feng, X.; Lu, L.; He, X.; Ouyang, M. Overcharge behaviors and failure mechanism of lithium-ion batteries under different test conditions. Appl. Energy 2019, 250, 323–332. [Google Scholar] [CrossRef] [Scilit]
  58. Zhang, Q.; Yang, K.; Niu, J.; Liu, T.; Hu, J. Research on the lower explosion limit of thermal runaway gas in lithium batteries under high-temperature and slight overcharge conditions. J. Energy Storage 2024, 79, 109976. [Google Scholar] [CrossRef] [Scilit]
  59. Zhang, G.; Wei, X.; Zhu, J.; Chen, S.; Han, G.; Dai, H. Revealing the failure mechanisms of lithium-ion batteries during dynamic overcharge. J. Power Sources 2022, 543, 231867. [Google Scholar] [CrossRef] [Scilit]
  60. Ren, D.; Hsu, H.; Li, R.; Feng, X.; Guo, D.; Han, X.; Lu, L.; He, X.; Gao, S.; Hou, J.; et al. A comparative investigation of aging effects on thermal runaway behavior of lithium-ion batteries. eTransportation 2019, 2, 100034. [Google Scholar] [CrossRef] [Scilit]
  61. Liu, X.; Ren, D.; Hsu, H.; Feng, X.; Xu, G.-L.; Zhuang, M.; Gao, H.; Lu, L.; Han, X.; Chu, Z.; et al. Thermal Runaway of Lithium-Ion Batteries without Internal Short Circuit. Joule 2018, 2, 2047–2064. [Google Scholar] [CrossRef] [Scilit]
  62. Yu, S.; Mao, Y.; Xie, J.; Xu, C.; Lu, T. Thermal runaway chain reaction determination and mechanism model establishment of NCA-graphite battery based on the internal temperature. Appl. Energy 2024, 353, 122097. [Google Scholar] [CrossRef] [Scilit]
  63. Roth, E.; Doughty, D.; Franklin, J. DSC investigation of exothermic reactions occurring at elevated temperatures in lithium-ion anodes containing PVDF-based binders. J. Power Sources 2004, 134, 222–234. [Google Scholar] [CrossRef] [Scilit]
  64. Kvasha, A.; Gutiérrez, C.; Osa, U.; Meatza, I.d.; Blazquez, J.A.; Macicior, H.; Urdampilleta, I. A comparative study of thermal runaway of commercial lithium ion cells. Energy 2018, 159, 547–557. [Google Scholar] [CrossRef] [Scilit]
  65. Shurtz, R.C.; Hewson, J.C. Review—Materials Science Predictions of Thermal Runaway in Layered Metal-Oxide Cathodes: A Review of Thermodynamics. J. Electrochem. Soc. 2020, 167, 90543. [Google Scholar] [CrossRef] [Scilit]
  66. Li, H.; Kong, X.; Liu, C.; Zhao, J. Study on thermal stability of nickel-rich/silicon-graphite large capacity lithium ion battery. Appl. Therm. Eng. 2019, 161, 114144. [Google Scholar] [CrossRef] [Scilit]
  67. Essl, C.; Golubkov, A.W.; Fuchs, A. Influence of Aging on the Failing Behavior of Automotive Lithium-Ion Batteries. Batteries 2021, 7, 23. [Google Scholar] [CrossRef] [Scilit]
  68. Wang, H.; Xu, H.; Zhao, Z.; Wang, Q.; Jin, C.; Li, Y.; Sheng, J.; Li, K.; Du, Z.; Xu, C.; et al. An experimental analysis on thermal runaway and its propagation in Cell-to-Pack lithium-ion batteries. Appl. Therm. Eng. 2022, 211, 118418. [Google Scholar] [CrossRef] [Scilit]
  69. Wu, C.; Wu, Y.; Feng, X.; Wang, H.; Zhang, F.; Chen, S.; Li, B.; Deng, T.; Ouyang, M. Ultra-high temperature reaction mechanism of LiNi0.8Co0.1Mn0.1O2 electrode. J. Energy Storage 2022, 52, 104870. [Google Scholar] [CrossRef] [Scilit]
  70. LaFollette, R.; Eskra, M.D. The Possible Role of Thermite Reactions in Thermal Runaway of Li-ion Cells with Layered Cathodes. J. Electrochem. Soc. 2024, 171, 80509. [Google Scholar] [CrossRef] [Scilit]
  71. Elsner, F.; Gerhards, P.; Berrier, G.; Vincent, R.; Dubourg, S.; Pischinger, S. Detailed Characterization of Thermal Runaway Particle Emissions from a Prismatic NMC622 Lithium-Ion Battery. Batteries 2025, 11, 225. [Google Scholar] [CrossRef] [Scilit]
  72. Feng, G.; Yang, Q.; Liu, Z.; Jiang, Z.; Zhao, C.; Wang, K.; Fuentes, A.; Chen, D.; He, X. Study of combustion characteristics of linear carbonates (DMC/DEC/EMC) and cyclic carbonate (EC): Laminar burning velocity and chemical reaction kinetics modeling. Fuel 2024, 363, 130881. [Google Scholar] [CrossRef] [Scilit]
  73. García, A.; Monsalve-Serrano, J.; Sari, R.L.; Martinez-Boggio, S. Influence of environmental conditions in the battery thermal runaway process of different chemistries: Thermodynamic and optical assessment. Int. J. Heat Mass Transf. 2022, 184, 122381. [Google Scholar] [CrossRef] [Scilit]
  74. Finegan, D.P.; Tjaden, B.; Heenan, T.M.M.; Jervis, R.; Di Michiel, M.; Rack, A.; Hinds, G.; Brett, D.J.L.; Shearing, P.R. Tracking Internal Temperature and Structural Dynamics during Nail Penetration of Lithium-Ion Cells. J. Electrochem. Soc. 2017, 164, A3285–A3291. [Google Scholar] [CrossRef] [Scilit]
  75. Finegan, D.P.; Darcy, E.; Keyser, M.; Tjaden, B.; Heenan, T.M.M.; Jervis, R.; Bailey, J.J.; Vo, N.T.; Magdysyuk, O.V.; Drakopoulos, M.; et al. Identifying the Cause of Rupture of Li-Ion Batteries during Thermal Runaway. Adv. Sci. 2018, 5, 1700369. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  76. Zhang, Y.; Wang, H.; Yu, H.; Jia, T.; Ma, C. Influence of Cathode Materials on the Characteristics of Lithium-Ion Battery Gas Generation During Thermal Runaway. Fire Technol. 2024, 61, 3935–3954. [Google Scholar] [CrossRef] [Scilit]
  77. Schöberl, J.; Ohneseit, S.; Schaeffler, S.; Förstermann, D.; Grahl, L.; Jossen, A.; Ziebert, C.; Lienkamp, M. Thermal runaway characterization of cylindrical lithium-ion and sodium-ion batteries with various sizes and energy contents. J. Power Sources 2025, 648, 237240. [Google Scholar] [CrossRef] [Scilit]
  78. Abbott, K.C.; Buston, J.E.; Gill, J.; Goddard, S.L.; Howard, D.; Howard, G.E.; Read, E.; Williams, R.C. Experimental study of three commercially available 18650 lithium ion batteries using multiple abuse methods. J. Energy Storage 2023, 65, 107293. [Google Scholar] [CrossRef] [Scilit]
  79. García, A.; Zhao, P.; Monsalve-Serrano, J.; Villalta, D.; Martinez-Boggio, S. Optical diagnostics of the venting spray and combustion behaviour during Li-ion battery thermal runaway induced by ramp heating. Appl. Therm. Eng. 2023, 218, 119308. [Google Scholar] [CrossRef] [Scilit]
  80. Hoelle, S.; Scharner, S.; Asanin, S.; Hinrichsen, O. Analysis on Thermal Runaway Behavior of Prismatic Lithium-Ion Batteries with Autoclave Calorimetry. J. Electrochem. Soc. 2021, 168, 120515. [Google Scholar] [CrossRef] [Scilit]
  81. Walker, W.Q.; Bayles, G.A.; Johnson, K.L.; Brown, R.P.; Petrushenko, D.; Hughes, P.J.; Calderon, D.T.; Darst, J.J.; Hagen, R.A.; Sakowski, B.A.; et al. Evaluation of Large-Format Lithium-Ion Cell Thermal Runaway Response Triggered by Nail Penetration using Novel Fractional Thermal Runaway Calorimetry and Gas Collection Methodology. J. Electrochem. Soc. 2022, 169, 60535. [Google Scholar] [CrossRef] [Scilit]
  82. Lammer, M.; Königseder, A.; Hacker, V. Holistic methodology for characterisation of the thermally induced failure of commercially available 18650 lithium ion cells. RSC Adv. 2017, 7, 24425–24429. [Google Scholar] [CrossRef] [Scilit]
  83. Bordes, A.; Marlair, G.; Zantman, A.; Herreyre, S.; Papin, A.; Desprez, P.; Lecocq, A. New insight on the risk profile pertaining to lithium-ion batteries under thermal runaway as affected by system modularity and subsequent oxidation regime. J. Energy Storage 2022, 52, 104790. [Google Scholar] [CrossRef] [Scilit]
  84. Wang, Y.; Song, Z.; Li, Y.; Li, C.; Ren, D.; Feng, X.; Wang, H.; Lu, L. Experimental investigation of the thermal propagation, emission identification, and venting-flow characteristics of a Li(Ni0.8Co0.1Mn0.1)O2 battery module. Case Stud. Therm. Eng. 2023, 49, 103360. [Google Scholar] [CrossRef] [Scilit]
  85. Essl, C.; Golubkov, A.W.; Fuchs, A. Comparing Different Thermal Runaway Triggers for Two Automotive Lithium-Ion Battery Cell Types. J. Electrochem. Soc. 2020, 167, 130542. [Google Scholar] [CrossRef] [Scilit]
  86. Zhang, J.; Guo, Q.; Liu, S.; Zhou, C.; Huang, Z.; Han, D. Investigation on gas generation and corresponding explosion characteristics of lithium-ion batteries during thermal runaway at different charge states. J. Energy Storage 2024, 80, 110201. [Google Scholar] [CrossRef] [Scilit]
  87. Li, Z.; Cheng, Z.; Yu, Y.; Wang, J.; Wang, L.; Mei, W.; Wang, Q. Thermal runaway comparison and assessment between sodium-ion and lithium-ion batteries. Process Saf. Environ. Prot. 2025, 193, 842–855. [Google Scholar] [CrossRef] [Scilit]
  88. Zhou, G.; Liu, Y.; Yang, S.; Zhang, Q.; Li, Y.; Lu, H.; Huang, Q.; Wei, Z.; Kong, Y.; Niu, C. Experimental study on the thermal runaway and flame dynamics of NCM811 lithium-ion batteries with critical thermal load under variable penetration condition. Int. Commun. Heat Mass Transf. 2024, 158, 107947. [Google Scholar] [CrossRef] [Scilit]
  89. Wang, P.; Xu, C.; Jiang, W.; Wang, W.; Liu, L.; Gu, J.; Fan, Z.; Zhang, M.; Huang, J.; Jiang, F.; et al. Experimental study on thermal runaway venting behaviour of LiNi0.8Co0.1Mn0.1O2 pouch cell under different sealing edge directions. J. Power Sources 2024, 621, 235327. [Google Scholar] [CrossRef] [Scilit]
  90. Aiello, L.; Hanzu, I.; Gstrein, G.; Ewert, E.; Ellersdorfer, C.; Sinz, W. Analysis and Investigation of Thermal Runaway Propagation for a Mechanically Constrained Lithium-Ion Pouch Cell Module. Batteries 2021, 7, 49. [Google Scholar] [CrossRef] [Scilit]
  91. Kennedy, R.W.; Marr, K.C.; Ezekoye, O.A. Gas release rates and properties from Lithium Cobalt Oxide lithium ion battery arrays. J. Power Sources 2021, 487, 229388. [Google Scholar] [CrossRef] [Scilit]
  92. Zhang, Q.; Song, W.; Zhou, G.; Wang, J.; Lu, H.; Guo, B.; Zhao, J.; Liang, T.; Zhang, M.; Kong, Y.; et al. Gas production dynamic characteristics and fire-explosion risk of the full cycle of thermal runaway in 70Ah lithium iron phosphate battery in confined space. Appl. Therm. Eng. 2025, 279, 127988. [Google Scholar] [CrossRef] [Scilit]
  93. Chen, H.; Yang, K.; Shao, J.; Liu, Y.; Zhang, M.; Wei, B.; Song, H.; Xiao, P.; Liu, T.; Wan, Y. Explosion dynamics for thermal runaway gases of 314 Ah LiFePO4 lithium-ion batteries triggered by overheating and overcharging. Process Saf. Environ. Prot. 2024, 192, 1238–1248. [Google Scholar] [CrossRef] [Scilit]
  94. Xu, C.; Fan, Z.; Zhang, M.; Wang, P.; Wang, H.; Jin, C.; Peng, Y.; Jiang, F.; Feng, X.; Ouyang, M. A comparative study of the venting gas of lithium-ion batteries during thermal runaway triggered by various methods. Cell Rep. Phys. Sci. 2023, 4, 101705. [Google Scholar] [CrossRef] [Scilit]
  95. Wang, H.; Wang, Q.; Jin, C.; Xu, C.; Zhao, Y.; Li, Y.; Zhong, C.; Feng, X. Detailed characterization of particle emissions due to thermal failure of batteries with different cathodes. J. Hazard. Mater. 2023, 458, 131646. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  96. Essl, C.; Golubkov, A.W.; Gasser, E.; Nachtnebel, M.; Zankel, A.; Ewert, E.; Fuchs, A. Comprehensive Hazard Analysis of Failing Automotive Lithium-Ion Batteries in Overtemperature Experiments. Batteries 2020, 6, 30. [Google Scholar] [CrossRef] [Scilit]
  97. Amano, K.O.A.; Tschirschwitz, R.; Gimadieva, E.; Köhler, F.; Krause, U. Thermal runaway and explosibility of the gas release from 18650 sodium-ion cells of NFM chemistry. J. Energy Storage 2025, 122, 116614. [Google Scholar] [CrossRef] [Scilit]
  98. Wang, G.; Kong, D.; Ping, P.; Wen, J.; He, X.; Zhao, H.; He, X.; Peng, R.; Zhang, Y.; Dai, X. Revealing particle venting of lithium-ion batteries during thermal runaway: A multi-scale model toward multiphase process. eTransportation 2023, 16, 100237. [Google Scholar] [CrossRef] [Scilit]
  99. Jia, Z.; Song, L.; Mei, W.; Yu, Y.; Meng, X.; Jin, K.; Sun, J.; Wang, Q. The preload force effect on the thermal runaway and venting behaviors of large-format prismatic LiFePO4 batteries. Appl. Energy 2022, 327, 120100. [Google Scholar] [CrossRef] [Scilit]
  100. Lin, C.; Yan, H.; Qi, C.; Mao, J.; Lao, L.; Sun, Y.; Ma, T.; Liu, D. Research on thermal runaway and gas generation characteristics of NCM811 high energy density lithium-ion batteries under different triggering methods. Case Stud. Therm. Eng. 2024, 64, 105417. [Google Scholar] [CrossRef] [Scilit]
  101. Zhang, Q.; Niu, J.; Zhao, Z.; Wang, Q. Research on the effect of thermal runaway gas components and explosion limits of lithium-ion batteries under different charge states. J. Energy Storage 2022, 45, 103759. [Google Scholar] [CrossRef] [Scilit]
  102. Somandepalli, V.; Marr, K.; Horn, Q. Quantification of Combustion Hazards of Thermal Runaway Failures in Lithium-Ion Batteries. SAE Int. J. Altern. Powertrains 2014, 3, 98–104. [Google Scholar] [CrossRef] [Scilit]
  103. Shen, H.; Guan, Y.; Li, M. Analysis of Thermal Runaway Temperature Characteristics, Gas Composition, and Thermal Runaway Products of Semi-Solid Li(Ni0.6Co0.2Mn0.2)O2 Battery. J. Electrochem. Energy Convers. Storage 2025, 22, 041009. [Google Scholar] [CrossRef] [Scilit]
  104. Chuang, Q.; Hongtao, Y.; Hao, C.; Tao, Y.; Qian, W.; Chunjing, L.; Zilin, L.; Yuemeng, Z.; Hang, W.; Qiang, W.; et al. Study on the effect of heating power density on thermal runaway and gas generation characteristics of large-format lithium iron phosphate batteries. Appl. Therm. Eng. 2025, 278, 127320. [Google Scholar] [CrossRef] [Scilit]
  105. Zhang, Y.; Wang, H.; Li, W.; Li, C. Quantitative identification of emissions from abused prismatic Ni-rich lithium-ion batteries. eTransportation 2019, 2, 100031. [Google Scholar] [CrossRef] [Scilit]
  106. Zhang, Q.; Liu, T.; Hao, C.; Qu, Y.; Niu, J.; Wang, Q.; Chen, D. In situ Raman investigation on gas components and explosion risk of thermal runaway emission from lithium-ion battery. J. Energy Storage 2022, 56, 105905. [Google Scholar] [CrossRef] [Scilit]
  107. Golubkov, A.W.; Fuchs, D.; Wagner, J.; Wiltsche, H.; Stangl, C.; Fauler, G.; Voitic, G.; Thaler, A.; Hacker, V. Thermal-runaway experiments on consumer Li-ion batteries with metal-oxide and olivin-type cathodes. RSC Adv. 2014, 4, 3633–3642. [Google Scholar] [CrossRef] [Scilit]
  108. Zheng, Y.; Shi, Z.; Ren, D.; Chen, J.; Liu, X.; Feng, X.; Wang, L.; Han, X.; Lu, L.; He, X.; et al. In-depth investigation of the exothermic reactions between lithiated graphite and electrolyte in lithium-ion battery. J. Energy Chem. 2022, 69, 593–600. [Google Scholar] [CrossRef] [Scilit]
  109. Jia, Z.; Wang, S.; Qin, P.; Li, C.; Song, L.; Cheng, Z.; Jin, K.; Sun, J.; Wang, Q. Comparative investigation of the thermal runaway and gas venting behaviors of large-format LiFePO4 batteries caused by overcharging and overheating. J. Energy Storage 2023, 61, 106791. [Google Scholar] [CrossRef] [Scilit]
  110. Liao, Z.; Zhang, S.; Zhao, Y.; Qiu, Z.; Li, K.; Han, D.; Zhang, G.; Habetler, T.G. Experimental evaluation of thermolysis-driven gas emissions from LiPF6-carbonate electrolyte used in lithium-ion batteries. J. Energy Chem. 2020, 49, 124–135. [Google Scholar] [CrossRef] [Scilit]
  111. Weber, N.; Schuhmann, S.; Tübke, J.; Nirschl, H. Chemical Thermal Runaway Modeling of Lithium-Ion Batteries for Prediction of Heat and Gas Generation. Energy Technol. 2023, 11, 2300565. [Google Scholar] [CrossRef] [Scilit]
  112. Chen, S.; Wang, Z.; Yan, W. Identification and characteristic analysis of powder ejected from a lithium ion battery during thermal runaway at elevated temperatures. J. Hazard. Mater. 2020, 400, 123169. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  113. Lombardo, G.; Ebin, B.; St. J. Foreman, M.R.; Steenari, B.-M.; Petranikova, M. Incineration of EV Lithium-ion batteries as a pretreatment for recycling—Determination of the potential formation of hazardous by-products and effects on metal compounds. J. Hazard. Mater. 2020, 393, 122372. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  114. Bak, S.-M.; Hu, E.; Zhou, Y.; Yu, X.; Senanayake, S.D.; Cho, S.-J.; Kim, K.-B.; Chung, K.Y.; Yang, X.-Q.; Nam, K.-W. Structural changes and thermal stability of charged LiNixMnyCozO2 cathode materials studied by combined in situ time-resolved XRD and mass spectroscopy. ACS Appl. Mater. Interfaces 2014, 6, 22594–22601. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  115. Liao, Z.; Zhang, S.; Li, K.; Zhao, M.; Qiu, Z.; Han, D.; Zhang, G.; Habetler, T.G. Hazard analysis of thermally abused lithium-ion batteries at different state of charges. J. Energy Storage 2020, 27, 101065. [Google Scholar] [CrossRef] [Scilit]
  116. Spotnitz, R.; Franklin, J. Abuse behavior of high-power, lithium-ion cells. J. Power Sources 2003, 113, 81–100. [Google Scholar] [CrossRef] [Scilit]
  117. Zou, K.; He, K.; Lu, S. Venting composition and rate of large-format LiNi0.8Co0.1Mn0.1O2 pouch power battery during thermal runaway. Int. J. Heat Mass Transf. 2022, 195, 123133. [Google Scholar] [CrossRef] [Scilit]
  118. Abbott, K.C.; Buston, J.E.; Gill, J.; Goddard, S.L.; Howard, D.; Howard, G.; Read, E.; Williams, R.C. Comprehensive gas analysis of a 21700 Li(Ni0.8Co0.1Mn0.1O2) cell using mass spectrometry. J. Power Sources 2022, 539, 231585. [Google Scholar] [CrossRef] [Scilit]
  119. Gong, T.; Duan, X.; Shan, Y.; Huang, L. Gas Generation in Lithium-Ion Batteries: Mechanisms, Failure Pathways, and Thermal Safety Implications. Batteries 2025, 11, 152. [Google Scholar] [CrossRef] [Scilit]
  120. Glaude, P.A.; Pitz, W.J.; Thomson, M.J. Chemical kinetic modeling of dimethyl carbonate in an opposed-flow diffusion flame. Proc. Combust. Inst. 2005, 30, 1111–1118. [Google Scholar] [CrossRef] [Scilit]
  121. Fernandes, Y.; Bry, A.; de Persis, S. Identification and quantification of gases emitted during abuse tests by overcharge of a commercial Li-ion battery. J. Power Sources 2018, 389, 106–119. [Google Scholar] [CrossRef] [Scilit]
  122. Chen, S.; Wang, Z.; Wang, J.; Tong, X.; Yan, W. Lower explosion limit of the vented gases from Li-ion batteries thermal runaway in high temperature condition. J. Loss Prev. Process Ind. 2020, 63, 103992. [Google Scholar] [CrossRef] [Scilit]
  123. Vendra, C.M.; Shelke, A.V.; Buston, J.E.; Gill, J.; Howard, D.; Read, E.; Abaza, A.; Cooper, B.; Wen, J.X. Numerical and experimental characterisation of high energy density 21700 lithium-ion battery fires. Process Saf. Environ. Prot. 2022, 160, 153–165. [Google Scholar] [CrossRef] [Scilit]
  124. Huang, Z.; Li, X.; Wang, Q.; Duan, Q.; Li, Y.; Li, L.; Wang, Q. Experimental investigation on thermal runaway propagation of large format lithium ion battery modules with two cathodes. Int. J. Heat Mass Transf. 2021, 172, 121077. [Google Scholar] [CrossRef] [Scilit]
  125. Huang, Z.; Zhao, C.; Li, H.; Peng, W.; Zhang, Z.; Wang, Q. Experimental study on thermal runaway and its propagation in the large format lithium ion battery module with two electrical connection modes. Energy 2020, 205, 117906. [Google Scholar] [CrossRef] [Scilit]
  126. Amano, K.O.A.; Hahn, S.-K.; Butt, N.; Vorwerk, P.; Gimadieva, E.; Tschirschwitz, R.; Rappsilber, T.; Krause, U. Composition and Explosibility of Gas Emissions from Lithium-Ion Batteries Undergoing Thermal Runaway. Batteries 2023, 9, 300. [Google Scholar] [CrossRef] [Scilit]
  127. Sun, J.; Li, J.; Zhou, T.; Yang, K.; Wei, S.; Tang, N.; Dang, N.; Li, H.; Qiu, X.; Chen, L. Toxicity, a serious concern of thermal runaway from commercial Li-ion battery. Nano Energy 2016, 27, 313–319. [Google Scholar] [CrossRef] [Scilit]
  128. Huang, Y.; Xu, Y.; Zhang, P.; Chen, H.; Huang, R. In-depth study of gas-solid jet and formation mechanisms during thermal runaway in ternary lithium-ion batteries. Energy 2025, 332, 135982. [Google Scholar] [CrossRef] [Scilit]
  129. Niu, H.; Chen, C.; Liu, Y.; Li, L.; Li, Z.; Ji, D.; Huang, X. Mitigating thermal runaway propagation of NCM 811 prismatic batteries via hollow glass microspheres plates. Process Saf. Environ. Prot. 2022, 162, 672–683. [Google Scholar] [CrossRef] [Scilit]
  130. Edge, J.S.; O’Kane, S.; Prosser, R.; Kirkaldy, N.D.; Patel, A.N.; Hales, A.; Ghosh, A.; Ai, W.; Chen, J.; Yang, J.; et al. Lithium ion battery degradation: What you need to know. Phys. Chem. Chem. Phys. 2021, 23, 8200–8221. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  131. Ouyang, D.; Wang, K.; Gao, T.; Wang, Z. Investigation on safety characteristics of high-nickel lithium-ion cells with anode partially doped by silicon oxide. J. Loss Prev. Process Ind. 2022, 80, 104924. [Google Scholar] [CrossRef] [Scilit]
  132. Li, H.; Shen, H.; Li, M.; Gao, Q.; Xu, C.; Feng, X. A simplified mathematical modeling approach for thermal runaway of Li(Ni0.8Co0.1Mn0.1)O2 pouch cells based on thermal runaway experimental data. J. Energy Storage 2024, 90, 111829. [Google Scholar] [CrossRef] [Scilit]
  133. Schaeffler, S.; Jossen, A. In situ measurement and modeling of internal thermal runaway propagation within lithium-ion cells under local overheating conditions. J. Power Sources 2024, 614, 234968. [Google Scholar] [CrossRef] [Scilit]
  134. Wei, D.; Zhang, M.; Zhu, L.; Chen, H.; Huang, W.; Yao, J.; Yuan, Z.; Xu, C.; Feng, X. Study on Thermal Runaway Behavior of Li-Ion Batteries Using Different Abuse Methods. Batteries 2022, 8, 201. [Google Scholar] [CrossRef] [Scilit]
  135. Song, L.; Wang, S.; Jia, Z.; Li, C.; Li, Y.; Cheng, Y.; Zhang, Y.; Yu, Y.; Jin, K.; Duan, Q.; et al. A comprehensive investigation of thermal runaway critical temperature and energy for lithium iron phosphate batteries. J. Energy Storage 2024, 86, 111162. [Google Scholar] [CrossRef] [Scilit]
  136. Hahn, A.; Doose, S.; Saathoff, D.; Kwade, A. Effect of External Compression on the Thermal Runaway of Lithium-Ion Battery Cells during Crush Tests: Insights for Improved Safety Assessment. Batteries 2023, 9, 404. [Google Scholar] [CrossRef] [Scilit]
  137. Gao, S.; Feng, X.; Lu, L.; Kamyab, N.; Du, J.; Coman, P.; White, R.E.; Ouyang, M. An experimental and analytical study of thermal runaway propagation in a large format lithium ion battery module with NCM pouch-cells in parallel. Int. J. Heat Mass Transf. 2019, 135, 93–103. [Google Scholar] [CrossRef] [Scilit]
  138. Golubkov, A.W.; Planteu, R.; Krohn, P.; Rasch, B.; Brunnsteiner, B.; Thaler, A.; Hacker, V. Thermal runaway of large automotive Li-ion batteries. RSC Adv. 2018, 8, 40172–40186. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  139. Huang, Z.; Yu, Y.; Duan, Q.; Qin, P.; Sun, J.; Wang, Q. Heating position effect on internal thermal runaway propagation in large-format lithium iron phosphate battery. Appl. Energy 2022, 325, 119778. [Google Scholar] [CrossRef] [Scilit]
  140. Amano, K.O.A.; Hahn, S.-K.; Tschirschwitz, R.; Rappsilber, T.; Krause, U. An Experimental Investigation of Thermal Runaway and Gas Release of NMC Lithium-Ion Pouch Batteries Depending on the State of Charge Level. Batteries 2022, 8, 41. [Google Scholar] [CrossRef] [Scilit]
  141. García, A.; Monsalve-Serrano, J.; Vargas Lewiski, F.d.; Golke, D. Analysis of the thermal runaway phenomenon of Nickel-Manganese-Cobalt cells induced by nail penetration through high-speed infrared imaging. J. Energy Storage 2024, 75, 109709. [Google Scholar] [CrossRef] [Scilit]
  142. Shelke, A.V.; Buston, J.E.; Gill, J.; Howard, D.; Abbott, K.C.; Goddard, S.L.; Read, E.; Howard, G.E.; Abaza, A.; Cooper, B.; et al. Characterizing and predicting 21700 NMC lithium-ion battery thermal runaway induced by nail penetration. Appl. Therm. Eng. 2022, 209, 118278. [Google Scholar] [CrossRef] [Scilit]
  143. Jin, C.; Sun, Y.; Wang, H.; Lai, X.; Wang, S.; Chen, S.; Rui, X.; Zheng, Y.; Feng, X.; Wang, H.; et al. Model and experiments to investigate thermal runaway characterization of lithium-ion batteries induced by external heating method. J. Power Sources 2021, 504, 230065. [Google Scholar] [CrossRef] [Scilit]
  144. Ping, P.; Kong, D.; Zhang, J.; Wen, R.; Wen, J. Characterization of behaviour and hazards of fire and deflagration for high-energy Li-ion cells by over-heating. J. Power Sources 2018, 398, 55–66. [Google Scholar] [CrossRef] [Scilit]
  145. Zhou, Z.; Zhou, X.; Peng, Y.; Li, L.; Cao, J.; Yang, L.; Cao, B. Quantitative study on the thermal failure features of lithium iron phosphate batteries under varied heating powers. Appl. Therm. Eng. 2021, 185, 116346. [Google Scholar] [CrossRef] [Scilit]
  146. Quintiere, J.G. On methods to measure the energetics of a lithium ion battery in thermal runaway. Fire Saf. J. 2020, 111, 102911. [Google Scholar] [CrossRef] [Scilit]
  147. Zhou, G.; Yang, S.; Liu, Y.; Zhang, Q.; Niu, C.; Lu, H.; Wei, Z.; Huang, Q. Influence of internal and external factors on thermal runaway characteristics of lithium-ion batteries induced by dual heat sources: An experimental research. Appl. Therm. Eng. 2025, 261, 125072. [Google Scholar] [CrossRef] [Scilit]
  148. Lecompte, M.; Bardi, M.; Richardet, L.; Chevillard, S.; Abada, S.; Khaled, H.; de Persis, S. Experimental Characterization of the Variability of the Thermal Runaway Phenomenon of a Li-ion Battery. In SAE Technical Paper Series. 16th International Conference on Engines & Vehicles, Capri, Italy; Lecompte, M., Bardi, M., Richardet, L., Chevillard, S., Abada, S., Khaled, H., Persis, S.d., Eds.; SAE International: Warrendale, PA, USA, 2023. [Google Scholar]
  149. Wang, Z.; Yang, H.; Li, Y.; Wang, G.; Wang, J. Thermal runaway and fire behaviors of large-scale lithium ion batteries with different heating methods. J. Hazard. Mater. 2019, 379, 120730. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  150. Zhou, Z.; Li, M.; Zhou, X.; Li, L.; Ju, X.; Yang, L. Investigating thermal runaway triggering mechanism of the prismatic lithium iron phosphate battery under thermal abuse. Renew. Energy 2024, 220, 119674. [Google Scholar] [CrossRef] [Scilit]
  151. Huang, Z.; Shen, T.; Jin, K.; Sun, J.; Wang, Q. Heating power effect on the thermal runaway characteristics of large-format lithium ion battery with Li(Ni1/3Co1/3Mn1/3)O2 as cathode. Energy 2022, 239, 121885. [Google Scholar] [CrossRef] [Scilit]
  152. Wang, J.; Wang, C.; Sun, R.; Han, C.; Li, K.; Zhang, L.; Zhang, Y.; Guo, D.; Li, S.; Wang, Z.; et al. Thermal runaway and jet flame features of 314 Ah lithium iron phosphate battery: Mechanism exploration and safety assessment. Appl. Therm. Eng. 2025, 272, 126371. [Google Scholar] [CrossRef] [Scilit]
  153. Liu, Y.; Zhang, L.; Ding, Y.; Huang, X.; Huang, X. Effect of thermal impact on the onset and propagation of thermal runaway over cylindrical Li-ion batteries. Renew. Energy 2024, 222, 119910. [Google Scholar] [CrossRef] [Scilit]
  154. Zou, K.; Lu, S. Comparative study on the influence of incident heat flux on thermal runaway fire development of large-format lithium-ion batteries. Process Saf. Environ. Prot. 2023, 176, 831–840. [Google Scholar] [CrossRef] [Scilit]
  155. Wang, K.; Wu, D.; Chang, C.; Zhang, J.; Ouyang, D.; Qian, X. Charging rate effect on overcharge-induced thermal runaway characteristics and gas venting behaviors for commercial lithium iron phosphate batteries. J. Clean. Prod. 2024, 434, 139992. [Google Scholar] [CrossRef] [Scilit]
  156. Wang, C.; Zhu, Y.; Gao, F.; Qi, C.; Zhao, P.; Meng, Q.; Wang, J.; Wu, Q. Thermal runaway behavior and features of LiFePO 4 /graphite aged batteries under overcharge. Int. J. Energy Res. 2020, 44, 5477–5487. [Google Scholar] [CrossRef] [Scilit]
  157. Guo, Q.; Liu, S.; Zhang, J.; Huang, Z.; Han, D. Effects of charging rates on heat and gas generation in lithium-ion battery thermal runaway triggered by high temperature coupled with overcharge. J. Power Sources 2024, 600, 234237. [Google Scholar] [CrossRef] [Scilit]
  158. Wang, J.; Li, Y.; Liu, F.; Fang, Z.; Gu, N.; Chen, B.; Yang, N.; Jia, Y. A comparative study of overcharge thermal runaway force-electrical-thermal characteristics and safety assessment of lithium batteries with different cathode materials. Appl. Therm. Eng. 2024, 256, 124092. [Google Scholar] [CrossRef] [Scilit]
  159. Wang, J.; Chen, B.; Li, Y.; Hu, T.; Liu, F.; Shi, M.; Ren, X.; Jia, Y.; Li, W. Multiparameter warning of lithium-ion battery overcharge-thermal runaway. J. Energy Storage 2024, 78, 110088. [Google Scholar] [CrossRef] [Scilit]
  160. Li, K.; Chen, L.; Han, X.; Gao, X.; Lu, Y.; Wang, D.; Tang, S.; Zhang, W.; Wu, W.; Cao, Y.; et al. Early warning for thermal runaway in lithium-ion batteries during various charging rates: Insights from expansion force analysis. J. Clean. Prod. 2024, 457, 142422. [Google Scholar] [CrossRef] [Scilit]
  161. Huang, S.; Du, X.; Richter, M.; Ford, J.; Cavalheiro, G.M.; Du, Z.; White, R.T.; Zhang, G. Understanding Li-Ion Cell Internal Short Circuit and Thermal Runaway through Small, Slow and In Situ Sensing Nail Penetration. J. Electrochem. Soc. 2020, 167, 90526. [Google Scholar] [CrossRef] [Scilit]
  162. An, Z.; Li, W.; Du, X.; Jia, L.; Li, Q.; Zhang, D. Experimental study on behaviors of lithium-ion cells experiencing internal short circuit and thermal runaway under nail penetration abuse condition. Appl. Therm. Eng. 2024, 247, 123058. [Google Scholar] [CrossRef] [Scilit]
  163. Ding, C.; Zhu, N.; Yu, J.; Li, Y.; Sun, X.; Liu, C.; Huang, Q.; Wang, J. Experimental investigation of environmental pressure effects on thermal runaway properties of 21700 lithium-ion batteries with high energy density. Case Stud. Therm. Eng. 2022, 38, 102349. [Google Scholar] [CrossRef] [Scilit]
  164. Liu, Y.; Niu, H.; Liu, J.; Huang, X. Layer-to-layer thermal runaway propagation of open-circuit cylindrical li-ion batteries: Effect of ambient pressure. J. Energy Storage 2022, 55, 105709. [Google Scholar] [CrossRef] [Scilit]
  165. Jin, Y.; Meng, D.; Zhao, C.-X.; Yu, J.-L.; Wang, X.-H.; Wang, J. Experimental Study on Thermal Runaway Characteristics of High-Nickel Ternary Lithium-Ion Batteries under Normal and Low Pressures. Batteries 2024, 10, 287. [Google Scholar] [CrossRef] [Scilit]
  166. Meng, D.; Weng, J.; Wang, J. Experimental Investigation on Thermal Runaway of Lithium-Ion Batteries under Low Pressure and Low Temperature. Batteries 2024, 10, 243. [Google Scholar] [CrossRef] [Scilit]
  167. Sun, Q.; Liu, H.; Wang, Z.; Meng, Y.; Xu, C.; Wen, Y.; Wu, Q. Investigation on Thermal Runaway Hazards of Cylindrical and Pouch Lithium-Ion Batteries under Low Pressure of Cruise Altitude for Civil Aircraft. Batteries 2024, 10, 298. [Google Scholar] [CrossRef] [Scilit]
  168. Zhou, G.; Liu, Y.; Yang, S.; Zhang, Q.; Li, Y.; Zhang, X.; Jiang, S.; Zhang, S.; Yuan, S. Research on the thermal runaway mechanism and eruption flame dynamics of NCM811 lithium-ion battery stimulated by the coupling abuse of heat and penetration. Appl. Therm. Eng. 2024, 253, 123785. [Google Scholar] [CrossRef] [Scilit]
  169. Mulder, B.; Schöberl, J.; Birke, K.P. Thermal Propagation Test Bench with Multi Pouch Cell Setup for Reproducibility Investigations. Batteries 2023, 9, 447. [Google Scholar] [CrossRef] [Scilit]
  170. Zhao, L.; Han, Z.; Guo, W.; Qiao, Z.; Qiu, H.; Liu, H.; Chen, M. An experimental study on thermal runaway propagation over cyclic aging lithium-ion battery modules with different electrical connections. J. Energy Storage 2024, 89, 111823. [Google Scholar] [CrossRef] [Scilit]
  171. Feng, X.; Sun, J.; Ouyang, M.; Wang, F.; He, X.; Lu, L.; Peng, H. Characterization of penetration induced thermal runaway propagation process within a large format lithium ion battery module. J. Power Sources 2015, 275, 261–273. [Google Scholar] [CrossRef] [Scilit]
  172. Xu, C.; Zhang, F.; Feng, X.; Jiang, F.; Ren, D.; Lu, L.; Yang, Y.; Liu, G.; Han, X.; Friess, B.; et al. Experimental study on thermal runaway propagation of lithium-ion battery modules with different parallel-series hybrid connections. J. Clean. Prod. 2021, 284, 124749. [Google Scholar] [CrossRef] [Scilit]
  173. Zhou, Z.; Li, M.; Zhou, X.; Ju, X.; Yang, L. Effect of the number of parallel batteries on thermal runaway evolution in LiFePO4 battery. Appl. Energy 2025, 388, 125651. [Google Scholar] [CrossRef] [Scilit]
  174. Charbonnel, J.; Darmet, N.; Deilhes, C.; Broche, L.; Reytier, M.; Thivel, P.-X.; Vincent, R. Safety Evaluation of All-Solid-State Batteries: An Innovative Methodology Using In Situ Synchrotron X-ray Radiography. ACS Appl. Energy Mater. 2022, 5, 10862–10871. [Google Scholar] [CrossRef] [Scilit]
  175. Charbonnel, J.; Dubourg, S.; Testard, E.; Broche, L.; Magnier, C.; Rochard, T.; Marteau, D.; Thivel, P.-X.; Vincent, R. Preliminary study of all-solid-state batteries: Evaluation of blast formation during the thermal runaway. iScience 2023, 26, 108078. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  176. Bates, A.M.; Preger, Y.; Torres-Castro, L.; Harrison, K.L.; Harris, S.J.; Hewson, J. Are solid-state batteries safer than lithium-ion batteries? Joule 2022, 6, 742–755. [Google Scholar] [CrossRef] [Scilit]
  177. Ping, P.; Ren, X.; Kong, D.; Gao, W.; Zhang, Y.; Yang, C.; Wang, G.; Feng, Z.; Guo, J.; Ren, J. Multi-scale thermal runaway analysis of sodium-ion batteries and comparative safety assessment with lithium-ion batteries. Compos. Part B Eng. 2025, 302, 112532. [Google Scholar] [CrossRef] [Scilit]
  178. Yue, Y.; Jia, Z.; Li, Y.; Wen, Y.; Lei, Q.; Duan, Q.; Sun, J.; Wang, Q. Thermal runaway hazards comparison between sodium-ion and lithium-ion batteries using accelerating rate calorimetry. Process Saf. Environ. Prot. 2024, 189, 61–70. [Google Scholar] [CrossRef] [Scilit]
  179. Mei, W.; Cheng, Z.; Wang, L.; Teng, A.; Li, Z.; Jin, K.; Sun, J.; Wang, Q. Thermal hazard comparison and assessment of Li-ion battery and Na-ion battery. J. Energy Chem. 2025, 102, 18–26. [Google Scholar] [CrossRef] [Scilit]
  180. Bordes, A.; Marlair, G.; Zantman, A.; Chesnaye, A.; Le Lore, P.-A.; Lecocq, A. Safety Evaluation of a Sodium-Ion Cell: Assessment of Vent Gas Emissions under Thermal Runaway. ACS Energy Lett. 2022, 7, 3386–3391. [Google Scholar] [CrossRef] [Scilit]
  181. Zhou, Q.; Li, Y.; Tang, F.; Li, K.; Rong, X.; Lu, Y.; Chen, L.; Hu, Y.-S. Thermal Stability of High Power 26650-Type Cylindrical Na-Ion Batteries. Chin. Phys. Lett. 2021, 38, 76501. [Google Scholar] [CrossRef] [Scilit]
  182. Fedoryshyna, Y.; Schaeffler, S.; Soellner, J.; Gillich, E.I.; Jossen, A. Quantification of venting behavior of cylindrical lithium-ion and sodium-ion batteries during thermal runaway. J. Power Sources 2024, 615, 235064. [Google Scholar] [CrossRef] [Scilit]
  183. Li, Z.; Yu, Y.; Wang, J.; Wang, C.; He, X.; Cheng, Z.; Li, H.; Mei, W.; Wang, Q. Thermal runaway and gas venting behaviors of large-format prismatic sodium-ion battery. Energy Storage Mater. 2025, 77, 104197. [Google Scholar] [CrossRef] [Scilit]
  184. Samigullin, R.R.; Drozhzhin, O.A.; Antipov, E.V. Comparative Study of the Thermal Stability of Electrode Materials for Li-Ion and Na-Ion Batteries. ACS Appl. Energy Mater. 2022, 5, 14–19. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.