Rotational Bending Fatigue Resistance of 18 Near-Full Infill Patterns in FFF 3D-Printed PLA Components

,
,
and
1
Department of Mechanical Engineering, University of Salamanca (USAL), Polytechnic School of Zamora, Campus Viriato, 49029 Zamora, Spain
2
Department of Computer Science and Artificial Intelligence, University of Alicante, Campus de San Vicente del Raspeig, Ap. Correos 99, San Vicente del Raspeig, 03080 Alicante, Spain
3
Department of Construction and Agronomy, University of Salamanca (USAL), Polytechnic School of Zamora, Campus Viriato, 49029 Zamora, Spain
*
Author to whom correspondence should be addressed.

Highlights

  • Rotating-bending fatigue life of FDM-printed PLA was compared for 18 infill patterns at 20 N.
  • Infill pattern had a strong effect on fatigue life (Welch’s ANOVA, p = 6.12 × 10−11).
  • The effect of 99% versus 100% nominal infill density depended on the pattern.
  • 3D Honeycomb gave the highest mean life (11,678 cycles) but, owing to its large scatter, did not differ significantly from the other patterns.
  • A Basquin S–N curve was fitted for 3D Honeycomb between 10 N and 35 N.

Abstract

This study analyses the rotational bending fatigue behaviour of polymer parts printed using the fused deposition modelling (FDM) process. The versatility of this additive manufacturing process allows for the modification of multiple process parameters, which determine the final mechanical properties of the parts. This study evaluates the influence of the infill pattern geometry and a slight software-driven reduction in toolpath overlaps (nominal 100% vs. 99% infill density) on fatigue life. Through an initial comparative test at a constant load of 20 N on 18 different infill geometries, fatigue performance was analysed using Welch’s ANOVA with Games–Howell post-hoc comparisons, a two-way ANOVA for the six patterns printed at both infill densities, and an exploratory Weibull analysis of scatter. Infill pattern had a highly significant effect on fatigue life (p = 6.12 × 10−11), and the effect of reducing the nominal infill density from 100% to 99% depended on the pattern. The 3D Honeycomb pattern showed the highest mean fatigue life (11,678 cycles; 9051 cycles without its longest-lived specimen), although its large scatter meant that it did not differ significantly from the other patterns. Subsequently, the Wöhler S–N curve of this pattern was fitted with the Basquin model for loads between 10 N and 35 N.

1. Introduction

Additive manufacturing (AM), commonly known as 3D printing, has revolutionised industrial production by enabling the manufacture of complex three-dimensional components layer by layer from a digital CAD/STL model [1]. Among the various polymer-based AM techniques, fused deposition modelling (FDM) or fused filament fabrication (FFF) has established itself as the most widely used technology due to its operational flexibility, low production cost and suitability for rapid prototyping and small-batch functional components [2,3,4,5,6]. Polylactic acid (PLA), a biodegradable thermoplastic polyester of renewable origin, is one of the most widely used materials in FDM due to its high processability and minimal thermal deformation during printing [7,8,9,10].
Despite its many advantages, parts manufactured using FDM exhibit inherently complex and unstable mechanical properties compared to those produced using conventional techniques such as injection moulding or machining [2,5,11,12]. During the FDM process, the thermal deposition of molten filaments generates an inherently anisotropic and heterogeneous microstructure, characterised by the presence of mesostructural voids, inter-layer discontinuities (inter-bead voids) and residual thermal gradients [7,9,13,14]. When functional PLA components are subjected to dynamic operating conditions, these microstructural imperfections act as severe stress concentrators, critically reducing resistance to fatigue degradation under applied load levels significantly below the material’s static elastic limit [15,16,17]. In fused filament fabrication (FFF), deposited polymer strands act as continuous structural fibers assembled into macro-porous architectures. The interfacial bonding, spatial orientation, and three-dimensional arrangement of these extruded fibers fundamentally govern the micro-mechanical stress transfer and macroscopic fatigue endurance under cyclic loading [16,17].
In engineering applications, a considerable proportion of structural failures in polymeric mechanical components occur under cyclic dynamic loading [15,16,18]. Whilst the scientific literature has extensively addressed the characterisation of static properties (tensile and flexural strength) of PLA parts produced by FDM by varying parameters such as print orientation, layer height and extrusion temperature [2,6,13], there is a substantial gap in the study of resistance to rotating bending fatigue [19,20,21]. Rotating bending subjects the component’s surface to a state of fully reversed alternating stresses (R = −1), where the combination of cyclic tension and compression across the entire outer perimeter of the test specimen accelerates the nucleation and propagation of cracks in the mesostructural voids of the infill [18,20,21,22].
On the other hand, there is a simplified assumption that increasing the infill density to 100% (solid) always guarantees optimal and isotropic mechanical performance in FDM parts [11,23]. However, recent research suggests that the internal architecture of the geometric pattern and a controlled reduction in toolpath overlap (at 99% density) can significantly alter behaviour in terms of local stress concentration, energy dissipation through internal damping, and the direction of crack front propagation [24,25,26,27,28,29,30]. Furthermore, recent investigations on FDM process parameters and infill pattern configurations have highlighted the critical role of internal topology in modulating the dynamic fatigue response and durability of 3D-printed PLA components [31,32].
Consequently, the rationale for this work lies in the need to extend current knowledge of the rotational bending fatigue behaviour of FDM-printed polymeric materials by systematically analysing the interaction between the infill pattern geometry and internal density. The main objective of this research is to compare the fatigue life of 18 internal infill geometries using Welch’s ANOVA with Games–Howell post-hoc comparisons (which do not assume equal variances), a two-way ANOVA with heteroscedasticity-robust sensitivity analyses for the effect of nominal infill density and an exploratory Weibull analysis, and subsequently to model the fatigue life of the pattern with the highest mean life by deriving its S–N (Wöhler) curve with Basquin’s equation.

2. Materials and Methods

2.1. Fatigue Testing Machine and Specimen Design

Rotational bending fatigue tests were performed using a restored TERCO MT205 Dauerprüfer testing machine (TERCO AB, Skärblacka, Sweden). The tests were conducted in a cantilever rotational bending configuration at a constant rotational speed of 3000 rpm (50 Hz cyclic loading frequency). Fully reversed alternating stress (R = −1) was applied via a mechanical dynamometer placed 4 mm from the free end of the cylindrical specimen (effective cantilever arm length L = 106 mm), generating the maximum bending moment and stress concentration at the transition shoulder radius. All tests were carried out under controlled ambient laboratory conditions of 21.5 ± 3.5° and relative humidity of 45 ± 10% RH. To prevent thermal degradation and frictional heat build-up in the spindle bearings between runs, a mandatory 5-min cooling period was enforced between consecutive tests. Although this pause primarily addresses testing rig thermal stability, previous investigations on rotational bending fatigue of FDM-printed PLA specimens under sub-critical stress regimes [6,17] have shown that failure is predominantly driven by mechanical stress concentration and crack propagation at internal mesostructural voids, without exhibiting macroscopic thermal softening. All fractured specimens in this study displayed clean mechanical fracture surfaces localized at the critical transition shoulder radius. An automatic electromechanical cut-off relay interrupted the motor and stopped the mechanical revolution counter (EMIT Model 5R, calibrated up to 5000 rpm) immediately upon physical specimen fracture. The test specimen geometry was designed using Autodesk Inventor® software(version 2024; Autodesk, Inc., San Francisco, CA, USA), in accordance with the dimensional specifications and radii indicated in the manufacturer’s manual [33,34] (Figure 1).
Figure 1. (a) Cross-section of the test specimen (lengths in mm) [19]; (b) 3D model in Autodesk Inventor®.
To ensure metrological consistency and experimental repeatability, the mechanical assembly of the restored TERCO MT205 equipment was thoroughly calibrated prior to the tests. The dynamic bending loads applied (10 N to 35 N) were verified using a calibrated digital load cell (accuracy ± 0.1 N), yielding a maximum force deviation of less than ±0.8 per cent. The axial alignment and dynamic rotational eccentricity (runout) of the clamped specimens were measured at the radius corresponding to the critical step using a digital dial gauge (Mahr MarCator 1075 R, measuring range 12.5 mm, resolution 0.001 mm); the dynamic radial run-out was strictly limited to <0.025 mm to minimise structural vibrations and parasitic bending stresses. The mechanical revolution counter (EMIT Model 5R)—coupled to the spindle via a machined aluminium sleeve with set screws—was calibrated against a stroboscopic RPM meter (Kaiser KVM-2) up to 5000 rpm, establishing a relative measurement error of less than ±0.35% at the operating frequency of 3000 rpm (50 Hz) and an automatic relay cut-off of <0.1 s following fracture.
The use of rotational bending tests on cylindrical polymer specimens makes it possible to assess the effect of notching and surface roughness caused by the stair-stepping effect in FDM layers, ensuring a symmetrical stress distribution in the transverse plane [15,34].
The mechanical setup and boundary conditions are schematically illustrated in Figure 2. The clamping shoulder (ϕ12 mm diameter) is rigidly constrained in the motor spindle, acting as a fixed support. A vertical downward load F (10 N to 35 N) is applied dynamically by the roller bearing of the mechanical dynamometer at 4 mm from the free end. This cantilever setup produces a linearly increasing bending moment M(x) = F x, reaching its maximum value Mmax= F L at the shoulder transition radius (L = 106 mm), which corresponds precisely to the critical failure section where 100% of the specimens are fractured.
Figure 2. Rotational bending fatigue setup: (a) physical mounting of the PLA specimen in the TERCO MT205 machine; (b) boundary conditions detailing the fixed clamping constraint and point load application F.

2.2. Additive Manufacturing of Test Specimens (FDM)

All test specimens were manufactured using fused deposition modelling (FDM) on a Prusa i3 MK3S+ 3D printer, using commercial PLA HD 3D filament (nominal diameter 1.75 mm, PLA Grey finish) from a single industrial production batch (GTIN/EAN-13 barcode: 8435490624085). The spools were unsealed directly from their factory vacuum packaging containing silica desiccant immediately prior to printing, thereby avoiding the need for prior oven drying.
The printing parameters were kept strictly constant across all prints: extrusion temperature of 210 °C, unheated print bed (at room temperature to prevent thermal warping of the PLA), constant layer height of 0.15 mm, extrusion multiplier of 1.0 (100% volumetric flow rate), 2 solid outer perimeters, 5 solid top layers and 4 solid bottom layers. The part was cooled using the layer fan at 100% from the second layer onwards (0% on layer 1) under controlled laboratory environmental conditions (21.5 ± 3.5 °C). The print speed was limited to ≤ 40 mm/s to ensure optimal bond between filament strands and geometric accuracy. All specimens were printed in a flat horizontal orientation on the XY print bed (longitudinal axis parallel to the build platform) in batches of up to 10 specimens per print layout (Figure 3). Slicing was executed using PrusaSlicer® (version 2.8.1) with 2 solid outer perimeters and standard top/bottom solid layers. To assess the impact of internal architecture, the geometry of the infill pattern and the nominal infill density (100% vs. 99%) were varied. A nominal 99% infill density introduces a theoretical geometric hypothesis resulting from the nominal toolpath distribution configured in the slicer between adjacent filament paths, modulating internal stiffness and preventing over-extrusion or localized heat build-up. The 18 sparse infill patterns available in PrusaSlicer were evaluated: A, Rectilinear; B, Aligned Rectilinear; C, Concentric; D, Hilbert Curve; E, Archimedean Chords; F, Octagram Spiral; G, Gyroid; N, Grid; O, Triangles; P, Stars; R, Cubic; S, Line; T, Honeycomb; U, 3D Honeycomb; W, Adaptive Cubic; X, Support Cubic; Y, Lightning; and Z, Zig Zag. PrusaSlicer permits a 100% infill density only for patterns capable of forming solid continuous volume (patterns A–F), automatically converting any other pattern to Rectilinear at 100%. Consequently, only patterns A–F were printed at both 100% and 99% nominal infill density, while the remaining 12 patterns were printed at 99% density only. The geometry of the infill pattern and the infill percentage (100% versus 99%) were varied. A 99% infill level is intended to introduce a slight reduction in toolpath overlap (a theoretical geometric hypothesis resulting from the nominal toolpath distribution configured in the slicer). A nominal 99% infill density setting in PrusaSlicer® introduces a slight software-driven reduction in toolpath overlap compared to the 100% setting. In this study, this parameter is evaluated purely as a nominal slicer configuration, and no direct physical measurements of internal void dimensions or gap geometry were performed.
Figure 3. Print bed layout in PrusaSlicer® showing a batch of 9 cylindrical PLA specimens arranged in flat horizontal orientation (XY plane).
The controlled reduction in density to 99% using PrusaSlicer® software is intended to introduce a slight reduction in toolpath overlap (a theoretical geometric hypothesis resulting from the nominal toolpath distribution configured in the slicer), a parameter recommended in the literature for modulating internal stiffness and preventing over-extrusion or localised heat build-up [23].
The 18 infill patterns tested are the sparse-infill patterns available in PrusaSlicer version 2.8.1. PrusaSlicer accepts an infill density of 100% only for patterns that can also generate solid infill (Rectilinear, Aligned Rectilinear, Concentric, Hilbert Curve, Archimedean Chords and Octagram Spiral) and switches any other pattern to Rectilinear. Therefore, only patterns A–F were printed at both 100% and 99% nominal infill density, and the other 12 patterns were printed at 99% only.
For the purposes of this research, a total of 115 test specimens were manufactured using fused deposition modelling (FDM), with the experimental programme structured into two distinct phases. Firstly, 15 additional test specimens were manufactured across five force levels (10 N, 15 N, 25 N, 30 N, and 35 N; 3 replicates per level). These, together with the 3 specimens previously tested at 20 N during the infill pattern screening phase, yielded a total of 18 test specimens evaluated across 6 force levels to determine the stress–life (S–N) curve. This sample size complies with the recommendations of ASTM E739 (Standard Practice for Statistical Analysis of Linear or Linearised Stress-Life and Strain-Life Data) for preliminary research and development testing. Secondly, for the comparative test at a constant load (20 N), 100 test specimens were manufactured, initially distributed as 4 replicates across each of the 24 evaluated configurations (6 patterns at 100% nominal infill density and 18 patterns at 99% density). In accordance with polymer characterisation methodologies (reference framework ASTM D7774/ASTM D638 [35,36]), this test was designed with an exploratory screening approach, the main objective of which is to identify relative trends and compare mechanical performance across different infill topologies. During the course of the study, and applying the data screening criteria set out in ASTM E178 [37] (Standard Practice for Dealing With Outlying Observations), thirteen test specimens from the comparative series were excluded prior to statistical analysis solely due to alignment anomalies or slippage events at the clamping jaws during assembly or testing. Consequently, 87 valid fatigue life results were retained, comprising 24 test specimens for the 100% infill density configurations and 63 test specimens for the 99% infill density configurations, as detailed in Table 1. As the retained sample comprises an average of 3 to 4 valid replicates per experimental condition, it ensures the necessary robustness for the comparative evaluation proposed within the framework of an exploratory study.
Table 1. Fatigue life (number of cycles to failure, Nf) at 20 N for all the configurations tested.
Figure 4 presents representative cross-sectional slice previews generated in PrusaSlicer® for the evaluated internal architectures, illustrating the structural contrast between continuous 3D spatial networks (e.g., 3D Honeycomb, Gyroid), conventional 2D planar grids (e.g., 2D Honeycomb, Grid), and highly sparse topology-optimized structures (e.g., Lightning, Cubic Support).
Figure 4. Representative PrusaSlicer® cross-sectional slice previews at 99% nominal infill density: (a) 3D Honeycomb; (b) 2D Honeycomb; (c) Gyroid/Zigzag; (d) Lightning.
According to technical datasheet values and published mechanical characterisations of FFF-printed PLA under flat XY orientation, the unreinforced material exhibits a nominal static ultimate tensile strength (σUTS) of 55–65 MPa and a flexural strength of 75–85 MPa. Consequently, the baseline fatigue screening load of 20 N (generating a maximum bending stress σMAX = 44.50 MPa) corresponds to approximately 68–81% of the static tensile strength, representing a realistic sub-critical high-cycle fatigue regime. The S–N stress range (10 N to 35 N; σMAX = 22.25 to 77.87MPa) spans from 35% σUTS (sub-critical fatigue) up to static yield levels [2,6,8,17].
For the purposes of this research, a total of 115 test specimens were manufactured using fused deposition modelling (FDM), with the experimental programme structured into two distinct phases. Firstly, 18 test specimens were used to determine the stress–life (S–N) curve. Secondly, for the comparative test at a constant load (20 N), a total of 100 test specimens were tested, comprising 96 nominal base specimens (24 configurations × 4 replicates) plus 4 additional setup/spare specimens manufactured to compensate for initial mounting trials (1 extra specimen in A99, B99, R99, and Z99). Prior to statistical evaluation, thirteen test specimens were excluded in accordance with ASTM E178 data screening criteria strictly due to mechanical mounting anomalies: dynamic rotational runout exceeding 0.025 mm (n = 7) or uncontrolled jaw slippage at the clamping system (n = 6). Consequently, 87 valid fatigue life results were retained (24 for 100% infill configurations and 63 for 99% infill configurations), as itemized in Table S1 of the Supplementary Materials.

2.3. Statistical Analysis

All statistical analyses were performed in Python 3.10.0 using SciPy 1.15.3 [38] and statsmodels 0.14.6 [39], with NumPy 2.2.6 and pandas 2.3.3 for data handling and matplotlib 3.10.9 for the figures. The main results were verified independently in R 4.3.1 [40]. The response variable was the fatigue life, i.e., the number of cycles to failure, Nf. All tests were two-sided with a significance level α = 0.05; p-values are reported exactly, in scientific notation when p < 0.001.
Normality of the model residuals was assessed with the Shapiro–Wilk test [41], and homogeneity of variances with Levene’s test using deviations from the group medians (Brown–Forsythe variant [42,43]), which is robust to non-normality:
z ij = y ij − y ~ i ,     W = ( N − k ) ∑ i = 1 k n i ( z ‾ i − z ‾ ) 2 ( k − 1 ) ∑ i = 1 k ∑ j = 1 n i ( z ij − z ‾ i ) 2
where k is the number of groups, ni is the number of specimens in group i, N = Σni, yij the life of specimen j of group i, ỹi the group median, and z ‾ i and z ‾ the group and overall means of zij.
Because the variances differed markedly between patterns (Section 3.2.2), the effect of the infill pattern on fatigue life at 99% nominal infill density was tested with Welch’s ANOVA [44], which does not assume equal variances:
w i =   n i s i 2 ,     y ‾ * =   ∑ i w i y ‾ i ∑ i w i ,     Λ = ∑ i = 1 k 1 − w i / ∑ j w j 2 n i − 1
F W = ∑ i w i ( y ‾ i − y ‾ * ) 2 / ( k − 1 ) 1 + 2 ( k − 2 ) k 2 − 1 Λ ,     ν 1 = k − 1 ,     ν 2 = k 2 − 1 3 Λ
where ȳi and si2 are the mean and variance of group i. Welch’s ANOVA on log10-transformed lives and the rank-based Kruskal–Wallis test [45] were used as robustness checks.
Pairwise differences between patterns were assessed with the Games–Howell procedure [46], which allows unequal variances and unequal group sizes and was therefore preferred to Tukey’s HSD test. For patterns i and j,
q ij = y ‾ i − y ‾ j 1 2 s i 2 n i + s j 2 n j ,     ν ij = s i 2 n i + s j 2 n j 2 ( s i 2 / n i ) 2 n i − 1 + ( s j 2 / n j ) 2 n j − 1
and the p-value was obtained from the studentized range distribution with k groups and νij degrees of freedom. Patterns that do not differ significantly are indicated with a compact letter display.
The longest life recorded for the 3D Honeycomb pattern (19,557 cycles) was examined with Grubbs’ test [47] and Dixon’s Q test [48]. Because neither test identified it as an outlier (Section 3.2.2), it was retained in all analyses, and its exclusion was examined as a sensitivity analysis.
The joint effect of the infill pattern (A–F) and the nominal infill density (100% and 99%) was analysed with the two-way model
y ijl = μ + α i + β j + ( α β ) ij + ε ijl
where αi is the effect of pattern i, βj the effect of infill density j, (αβ)ij their interaction and εijl the error of specimen l, subject to the sum-to-zero constraints Σiαi = Σjβj = Σi(αβ)ij = Σj(αβ)ij = 0. Because the cells were unbalanced (three or four specimens each), Type III sums of squares were used. As Type III sums of squares do not correct for heteroscedasticity or non-normality, the F-tests were repeated with a heteroscedasticity-consistent (HC3) covariance matrix [49] and on log10-transformed lives. The effect of infill density within each pattern was tested with Welch’s t-test, and the six p-values were adjusted with Holm’s method [50].
The scatter of fatigue life within each pattern was described with the two-parameter Weibull distribution [51],
F ( N f ) = 1 − exp − N f η m
where m is the Weibull modulus (shape parameter) and η is the characteristic life, by which 63.2% of the specimens are expected to have failed. The parameters were estimated by maximum likelihood [52], by maximising the log-likelihood
l ( m , η ) = n   ln m − nm   ln η + ( m − 1 ) ∑ i = 1 n ln x i − ∑ i = 1 n x i η m
where x1, …, xn are the lives of the n specimens of a pattern. The 95% confidence intervals were obtained with the profile likelihood-ratio method [52], as the set of values θ of each parameter that satisfy
2 l ( m ^ , η ^ ) − l p ( θ ) ≤   χ 1 ;   0.95 2 = 3.841
where ℓp is the profile log-likelihood. Probability plots use Bernard’s median ranks, Fi = (i − 0.3)/(n + 0.4). With three or four specimens per pattern, the Weibull analysis is exploratory: it describes the scatter of fatigue life and is not used to characterise structural reliability.

3. Results and Discussion

3.1. Evaluation of the Impact of Infill Patterns and Nominal Infill Density (Constant Load of 20 N)

The experimental results for the number of cycles to failure (Nf) for the 18 geometries tested under a fixed load of 20 N are detailed below. Table 1 summarises the actual test results.

3.2. Inferential Statistical Analysis and Discussion

3.2.1. Two-Way ANOVA (Patterns A–F × Nominal Infill Density)

The effects of pattern geometry (A–F) and nominal infill density (100% vs. 99%) were analysed together with a two-way factorial ANOVA using Type III sums of squares (Equation (5)), which do not depend on the order in which the factors enter the model when the cells are unbalanced (three or four specimens per cell). Levene’s test did not indicate unequal variances among the 12 cells (p = 0.151), but the residuals deviated from normality (Shapiro–Wilk p = 0.020); the F-tests were therefore repeated with HC3-robust standard errors and on log10-transformed lives (Table 2).
Table 2. Two-way ANOVA (Type III sums of squares) for infill pattern (A–F) and nominal infill density.
Type III sums of squares do not add up to the total sum of squares in an unbalanced design. Sensitivity analyses: with HC3-robust F-tests, p = 3.11 × 10−11 (pattern), 0.029 (infill density) and 1.22 × 10−6 (interaction); on log10(cycles), p = 3.60 × 10−8, 0.555 and 0.004, respectively.
Pattern geometry had a highly significant effect on fatigue life (F(5, 34) = 26.94, p = 6.37 × 10−11), and the pattern × infill density interaction was also significant (F(5, 34) = 7.02, p = 1.33 × 10−4), indicating that the effect of reducing the nominal infill density from 100% to 99% depends on the pattern. Both effects remained significant in the HC3-robust and log-scale analyses. The main effect of infill density was smaller (F(1, 34) = 6.25, p = 0.017) and was not significant on the log scale (p = 0.555), because the direction of the difference changes between patterns. The effect of infill density was therefore examined within each pattern (Table 3, Figure 2).
Table 3. Effect of reducing the nominal infill density from 100% to 99% within each pattern (A–F): mean fatigue life (cycles), difference, percentage change and Welch’s t-test with Holm-adjusted p-values.
Means of three or four specimens per cell. Difference and change are 99% minus 100%, relative to 100%. t is Welch’s statistic for 100% minus 99%, with Welch–Satterthwaite degrees of freedom in brackets.
For the linear patterns Rectilinear (A) and Aligned Rectilinear (B), the mean fatigue life at 99% nominal infill density was 57.5% and 36.8% lower than at 100%, but only the difference for Rectilinear was statistically significant (Holm-adjusted p = 0.002; Table 3). This trend is consistent with the expectation that a lower infill density reduces the load-bearing cross-section [15,17]. Conversely, for the curved patterns Hilbert Curve (D) and Archimedean Chords (E), the mean life at 99% was 180.5% and 111.9% higher than at 100% (Figure 5); however, these differences were not statistically significant with four specimens per cell (Holm-adjusted p = 0.488 for both) and should be regarded as trends that require confirmation with larger samples. The infill geometry is known to affect fatigue life [53,54]; for example, a gyroid pattern gave longer fatigue lives than a tri-hexagonal pattern in carbon-fibre-reinforced PLA [53]. In the present study, however, Gyroid was among the shortest-lived patterns, and the other non-linear patterns tested at both densities (Concentric and Octagram Spiral) had lower mean lives at 99%. One possible explanation for the trends observed in the Hilbert Curve and the Archimedean Spirals is that the slight reduction, programmed into the software, in the overlap of trajectories in PrusaSlicer® could introduce a local stress redistribution mechanism that delays crack propagation. It is explicitly noted that this mechanism represents a theoretical geometric hypothesis based on the nominal distribution of trajectories, as no direct physical measurements of gap dimensions or fractographic analyses were carried out in this study.
Figure 5. Mean fatigue life (±one standard deviation) of patterns A–F at 100% and 99% nominal infill density; small markers show the individual specimens. The two-way ANOVA (Table 2) indicates a significant pattern × infill density interaction.

3.2.2. Welch’s ANOVA and Games–Howell Comparisons (18 Patterns at 99% Nominal Infill Density)

The variability of fatigue life differed strongly among the 18 patterns at 99% nominal infill density: the standard deviation ranged from 14 cycles for Lightning (Y) to 5710 cycles for 3D Honeycomb (U) and generally increased with the mean (Figure S2), and Levene’s test indicated unequal variances (p = 0.013). The residuals of the one-way model were not normally distributed (Shapiro–Wilk p = 1.07 × 10−6). Both departures depended largely on the 19,557-cycle specimen (without it, Levene p = 0.128 and Shapiro–Wilk p = 0.105; Table S3), but because the standard deviations still differed widely (from 14 to 2742 cycles), the conventional one-way ANOVA was replaced by Welch’s ANOVA, which showed a highly significant effect of the infill pattern on fatigue life (F(17, 15.4) = 59.39, p = 6.12 × 10−11). The same conclusion was obtained on log-transformed lives (F(17, 16.1) = 46.41, p = 1.68 × 10−10) and with the Kruskal–Wallis test (H(17) = 49.43, p = 5.17 × 10−5).
The longest life recorded for 3D Honeycomb (19,557 cycles) was not identified as an outlier by Grubbs’ test (G = 1.38; critical value 1.48) or by Dixon’s Q test (Q = 0.58; critical value 0.83), and it was therefore retained; because both tests have little power with only four specimens, its exclusion was also examined. Excluding it reduced the mean life of 3D Honeycomb from 11,678 to 9051 cycles and its standard deviation from 5710 to 2742 cycles, but did not change the conclusions: Welch’s ANOVA remained highly significant (p = 9.79 × 10−11) and the Games–Howell comparisons identified the same significant pairs (Tables S1–S4).
Games–Howell comparisons identified 17 significantly different pairs out of 153 (Figure 6; all pairs are listed in Table S4). Zig Zag (Z) had a significantly longer life than Rectilinear (A), Honeycomb (T), Octagram Spiral (F), Adaptive Cubic (W), Gyroid (G), Support Cubic (X) and Lightning (Y); Cubic (R) had a significantly longer life than Octagram Spiral (F), Adaptive Cubic (W), Gyroid (G), Support Cubic (X) and Lightning (Y); Line (S) and Rectilinear (A) outlasted Support Cubic (X) and Lightning (Y); and Aligned Rectilinear (B) outlasted Lightning (Y). Although 3D Honeycomb (U) had the highest mean life, its large scatter (individual lives between 6419 and 19,557 cycles) meant that it did not differ significantly from any other pattern (smallest p = 0.26). With three or four specimens per pattern, these comparisons have limited power, so a non-significant difference means that a difference was not demonstrated, not that the patterns perform equally.
Figure 6. Fatigue life of the 18 patterns at 99% nominal infill density and 20 N. Bars show the mean ± one standard deviation and dots the individual specimens. Patterns that share a letter do not differ significantly (Games–Howell, α = 0.05). The ringed point is the 19,557-cycle specimen examined in the sensitivity analysis.

3.2.3. Exploratory Weibull Analysis of Scatter

The scatter of fatigue life within each pattern was described with two-parameter Weibull distributions fitted by maximum likelihood (Equations (6)–(8); Table 4). A higher Weibull modulus m indicates a narrower relative scatter of lives. With only three or four specimens per pattern, however, m is estimated imprecisely: the 95% confidence intervals are wide (Table 4; Figure S1), and the estimate can change substantially if a single specimen is added or removed. The Weibull results are therefore used here only to describe the observed scatter, not to characterise structural reliability.
Table 4. Maximum-likelihood estimates of the Weibull modulus (m) and characteristic life (η) of the 18 patterns at 99% nominal infill density and 20 N, with 95% profile likelihood-ratio confidence intervals (CI), ordered by m. Exploratory analysis: three or four specimens per pattern.
Line (S), Rectilinear (A), and Zig Zag (Z) exhibited the narrowest scatter (m = 20.6, 14.7, and 14.1, respectively), although their confidence intervals overlapped with those of several other patterns. Among these, Zig Zag combined low dispersion with one of the longest mean fatigue lives (5732 cycles). Conversely, 3D Honeycomb displayed one of the widest relative scatters (m = 2.6, 95% CI 1.0–4.9; or m = 4.6, 95% CI 1.5–10.0, excluding the 19,557 cycles specimen; only Concentric and Hilbert Curve yielded lower Weibull moduli), which is consistent with its non-significant Games–Howell post-hoc comparisons. This experimental scatter is hypothesized to stem from its complex three-dimensional toolpath, where frequent directional changes during strand deposition may generate localized interstitial voids [55,56]; however, this remains a geometric hypothesis that requires direct microstructural verification. Lightning combined a relatively high modulus (m = 6.0) with very short fatigue lives (η = 71 cycles), demonstrating that a narrow scatter alone does not represent an engineering advantage. Figure 7 compares the measured lives with the fitted distributions for selected patterns.
Figure 7. Weibull probability plots for selected patterns at 99% nominal infill density: measured lives (Bernard median ranks), maximum-likelihood fit (solid line) and median-rank regression (dashed line). For 3D Honeycomb, the fit is shown with and without the 19,557-cycle specimen.

3.3. Wöhler Curve (S–N) for the 3D Honeycomb Pattern

The 3D Honeycomb pattern was selected for S–N characterisation over a force range of 10 N to 35 N using specimens with 99% nominal infill density because it demonstrated the highest mean fatigue life at 20 N (11,678 cycles). This selection criterion is strictly based on maximum average endurance. It is explicitly acknowledged that, due to its large experimental scatter, 3D Honeycomb did not show statistically significant superiority over other high-performing patterns in Games–Howell post-hoc comparisons (Section 3.2.2). The modelling of maximum stress and bending moments in the critical cylindrical section was carried out in Autodesk Fusion 360® (Table 5). For applications requiring high statistical predictability and minimal dispersion, patterns such as Zig Zag (m = 14.1) or Cubic (m = 6.0) represent preferable engineering choices.
Table 5. Stresses and fatigue parameters obtained for the Basquin potential regression in the 3D Honeycomb pattern.
Based on a linear regression of log (Sa) on log(2Nf), the constants were obtained from Basquin’s power-law formulation [21]:
S a = S f ′ ⋅ 2 N f b ⟹ log S a = log S f ′ + b ⋅ log 2 N f
In strict accordance with ASTM E739 recommendations, the Basquin power-law model was fitted using all 18 individual experimental fatigue results across the six force levels (Table 5). This linear regression on log-log coordinates yielded a fatigue strength coefficient of Sf′ = 374 MPa and a fatigue strength exponent of b = −0.224. The final model is:
S a = 374 ⋅ 2 N f − 0.224
The exponent b = −0.224 reflects a marked sensitivity of the printed PLA specimens to the cyclic stress amplitude. This value lies within the range reported in the literature for FFF-processed PLA components subjected to rotational bending fatigue, where Basquin slope exponents typically vary between −0.09 and −0.25 [17,19,20]. This relatively steep slope consists of a brittle behaviour in which micro-cracks nucleated in the inter-layer voids may propagate rapidly under bending, governed by progressive cumulative damage at the interfacial zones [57].

3.4. Limitations and Future Work

The statistical conclusions of this study are subject to several limitations. First, only three or four specimens were tested per configuration, which limits the power of the pairwise comparisons and makes the Weibull parameters imprecise; with groups of this size, the Games–Howell procedure may also be slightly liberal, so the four significant pairs with 0.04 < p < 0.05 should be interpreted with caution. Second, the residuals of the two-way model deviated from normality on both the original and the log scale; the conclusions were robust to heteroscedasticity (HC3) and to the log transformation, but with three or four specimens per cell, the p-values of the two-way analysis should be regarded as approximate. Third, the effect of infill density could only be assessed for the six patterns that PrusaSlicer can print at 100% (A–F), and the infill densities are nominal slicer settings rather than measured densities. Finally, the S–N curve is based on 18 specimens distributed over six load levels (3 specimens per level) and applies only within the tested range of 10–35 N. Future work should test at least 6–10 specimens per configuration for comparisons of means and 15–30 for Weibull characterisation, randomise the test order, measure the actual density and porosity of the specimens, and include fractographic analysis.
The main limitation of this study is the absence of post-fracture microscopic analysis (such as scanning electron microscopy, SEM, or optical fractography). Consequently, the discussed failure mechanisms—such as localized crack deflection along three-dimensional print paths and stress redistribution across inter-layer interfaces—are proposed as geometric and structural hypotheses based on macroscopic fatigue responses. High-resolution fractographic analysis represents an essential line of future research to directly observe micro-void coalescence, inter-strand debonding, and crack propagation modes across distinct infill geometries.
Finally, while the 5-min pause between tests ensured thermal stability of the testing rig bearings, in-situ surface temperature monitoring of the specimens was not conducted during the 50 Hz cyclic loading tests. Although post-mortem visual analysis revealed clean mechanical fractures localized at the transition shoulder radius—consistent with mechanical fatigue failure mechanisms documented in FDM-printed PLA under sub-critical stress regimes [6,17]—localized micro-scale hysteretic heating cannot be entirely ruled out. Future investigations should incorporate real-time infrared thermography (e.g., FLIR thermal imaging) to continuously monitor and quantify potential hysteretic self-heating in polymer specimens subjected to high-frequency rotational bending.
A key limitation of this work is that infill densities represent nominal slicer settings rather than physically measured densities or void fractions. Future research will incorporate high-resolution scanning electron microscopy (SEM) and X-ray micro-computed tomography (micro-CT) to directly quantify internal void geometry and real porosity.

4. Conclusions

This study has systematically and quantitatively characterised the behaviour of PLA polymer parts manufactured using fused deposition modelling (FDM) under rotational bending fatigue, providing empirical evidence on how the architecture of the infill pattern and the nominal infill density influence durability under alternating cyclic loads.
Using Welch’s and two-way analysis of variance (ANOVA), Games–Howell multiple comparisons and an exploratory Weibull analysis, the effects of infill pattern and nominal infill density on fatigue life were quantified. The following conclusions are supported by the results:
Infill pattern has a strong effect on fatigue life, both across the 18 patterns at 99% nominal infill density (Welch’s ANOVA, p = 6.12 × 10−11) and for the six patterns tested at both infill densities (two-way ANOVA, F(5, 34) = 26.94, p = 6.37 × 10−11).
The effect of reducing the nominal infill density from 100% to 99% depends on the pattern (interaction F(5, 34) = 7.02, p = 1.33 × 10−4). Within individual patterns, only Rectilinear showed a significant difference, with a longer life at 100% (Holm-adjusted p = 0.002); the higher mean lives observed at 99% for Hilbert Curve (+180.5%) and Archimedean Chords (+111.9%) were not statistically significant and require confirmation with larger samples.
3D Honeycomb (U) showed the highest mean fatigue life (11,678 cycles; 9051 cycles without its longest-lived specimen, which was not flagged as an outlier by Grubbs’ or Dixon’s test), but its large scatter meant that it did not differ significantly from any other pattern. Zig Zag (Z) and Cubic (R) combined long mean lives with significant differences from the largest number of short-lived patterns.
The exploratory Weibull analysis indicated the narrowest scatter for Line (S), Rectilinear (A) and Zig Zag (Z) (m = 20.6, 14.7 and 14.1, respectively), with Zig Zag combining narrow scatter and a long mean life (5732 cycles). With three or four specimens per pattern, the confidence intervals are wide, so these results describe scatter and do not establish structural reliability.
A Basquin S–N curve was fitted for the 3D Honeycomb pattern using all 18 individual specimens (Sa = 374 (2Nf)−0.224, R2 = 0.950) and describes its fatigue life between 10 N and 35 N. Given the small number of specimens per load level, it should not be extrapolated beyond the tested range or used as a general design tool without further validation.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/fib14120139/s1, Table S1: Complete specimen breakdown, exclusions, and valid retained samples per pattern; Table S2: Descriptive statistics of fatigue life (cycles to failure) at 20 N and 99% nominal infill density, ordered by mean, with Games–Howell letter groups (patterns sharing a letter do not differ significantly, α = 0.05). The last row repeats 3D Honeycomb without the 19,557-cycle specimen (sensitivity analysis); Table S3: Normality of residuals (Shapiro–Wilk) and homogeneity of variances (Levene’s test with median centring, Brown–Forsythe variant); Table S4: Games–Howell pairwise comparisons of the 18 patterns at 99% nominal infill density (all 153 pairs, ordered by p). Difference = mean of the first pattern minus mean of the second (cycles); df, Welch–Satterthwaite degrees of freedom; * significant at α = 0.05. With the 19,557-cycle specimen excluded, the same 17 pairs are significant; Table S5: Weibull parameters estimated by maximum likelihood (MLE, used in the revised manuscript) and by median-rank regression (MRR, used in the original submission), ordered by the MLE modulus; Figure S1: Weibull modulus m of the 18 patterns (maximum-likelihood estimates with 95% profile likelihood-ratio confidence intervals, log scale). The open marker shows 3D Honeycomb without the 19,557-cycle specimen; Figure S2: Residual diagnostics for the one-way model at 99% nominal infill density: normal Q–Q plots of residuals on the cycle and log10 scales, and pattern standard deviation versus pattern mean. Figure S3: Games–Howell p-value matrix.

Author Contributions

Conceptualization, L.A., M.C. and R.R.; Methodology, L.A., M.C. and R.R.; Software, L.A., M.C. and R.R.; Validation, L.A., M.C. and R.R.; Formal analysis, L.A., M.C. and R.R.; Investigation, L.A., F.M., M.C. and R.R.; Resources, L.A., F.M., M.C. and R.R.; Data curation, L.A. and R.R.; Writing – original draft, L.A. and R.R.; Writing – review & editing, L.A., M.C. and R.R.; Visualization, L.A., F.M., M.C. and R.R.; Supervision, L.A., M.C. and R.R.; Project administration, L.A., F.M., M.C. and R.R.; Funding acquisition, L.A., F.M., M.C. and R.R. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Data Availability Statement

The original contributions presented in this study are included in the article/Supplementary Material. Further inquiries can be directed to the corresponding author.

Conflicts of Interest

The authors declare no conflicts of interest.

Abbreviations

The following abbreviations are used in this manuscript:
AMAdditive Manufacturing
FDMFused Deposition Modelling
FFFFused Filament Fabrication
PLAPolylactic Acid
HDHigh Density/High Definition
CADComputer-Aided Design
STLStandard Triangle Language/Stereolithography
NfNumber of cycles to failure
S–NStress vs. Number of cycles
SaStress amplitude
Sf’Fatigue strength coefficient
bFatigue strength exponent
RStress ratio/Load ratio
ANOVAAnalysis of Variance
HC3Heteroscedasticity-consistent covariance estimator (type 3)
SSSum of Squares
dfDegrees of freedom
MSMean Square
FF-statistic
p-valueProbability value
CIConfidence interval
HSDHonestly Significant Difference
mWeibull modulus/Shape parameter
ηWeibull scale parameter/Characteristic life
R2Coefficient of determination/R-squared

References

  1. Gibson, I.; Rosen, D.W.; Stucker, B. Additive Manufacturing Technologies: 3D Printing, Rapid Prototyping, and Direct Digital Manufacturing, 3rd ed.; Springer: Cham, Switzerland, 2021; pp. 171–201. [Google Scholar] [CrossRef] [Scilit]
  2. Tientcheu, S.W.T.; Djouda, J.M.; Bouaziz, M.A.; Lacazedieu, E. A review on fused deposition modeling materials with analysis of key process parameters influence on mechanical properties. Int. J. Adv. Manuf. Technol. 2024, 130, 2119–2158. [Google Scholar] [CrossRef] [Scilit]
  3. Vyavahare, S.; Teraiya, S.; Panghal, D.; Kumar, S. Fused deposition modelling: A review. Rapid Prototyp. J. 2020, 26, 176–201. [Google Scholar] [CrossRef] [Scilit]
  4. Kantaros, A.; Piromalis, D. Employing a Low-Cost Desktop 3D Printer: Challenges, and How to Overcome Them by Tuning Key Process Parameters. Int. J. Mech. Appl. 2021, 10, 11–19. [Google Scholar] [CrossRef] [Scilit]
  5. Doshi, M.; Mahale, A.; Singh, S.K.; Deshmukh, S. Printing parameters and materials affecting mechanical properties of FDM-3D printed parts: Perspective and prospects. Mater. Today Proc. 2022, 50, 2269–2275. [Google Scholar] [CrossRef] [Scilit]
  6. Travieso-Rodriguez, J.A.; Jerez-Mesa, R.; Llumà, J.; Traver-Ramos, O.; Gomez-Gras, G.; Roa Rovira, J.J. Mechanical properties of 3D-printing polylactic acid parts subjected to bending stress and fatigue testing. Materials 2019, 12, 3859. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  7. Arrigo, R.; Frache, A. FDM Printability of PLA Based-Materials: The Key Role of the Rheological Behavior. Polymers 2022, 14, 1754. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  8. Liu, Z.; Wang, Y.; Wu, B.; Cui, C.; Guo, Y.; Yan, C. A critical review of fused deposition modeling 3D printing technology in manufacturing polylactic acid parts. Int. J. Adv. Manuf. Technol. 2019, 102, 2877–2889. [Google Scholar] [CrossRef] [Scilit]
  9. Bermudo Gamboa, C.; Martín Béjar, S.; Trujillo Vilches, F.J.; Sevilla Hurtado, L. Geometrical analysis in material extrusion process with polylactic acid (PLA) + carbon fiber. Rapid Prototyp. J. 2023, 29, 21–39. [Google Scholar] [CrossRef] [Scilit]
  10. Joseph Arockiam, A.; Subramanian, K.; Padmanabhan, R.G.; Selvaraj, R.; Bagal, D.K.; Rajesh, S. A review on PLA with different fillers used as a filament in 3D printing. Mater. Today Proc. 2022, 50, 2057–2064. [Google Scholar] [CrossRef] [Scilit]
  11. Birosz, M.T.; Andó, M. Effect of infill pattern scaling on mechanical properties of FDM-printed PLA specimens. Prog. Addit. Manuf. 2024, 9, 875–883. [Google Scholar] [CrossRef] [Scilit]
  12. Birosz, M.T.; Ledenyák, D.; Andó, M. Effect of FDM infill patterns on mechanical properties. Polym. Test. 2022, 113, 107654. [Google Scholar] [CrossRef] [Scilit]
  13. Chikkanna, N.; Krishnapillai, S.; Ramachandran, V. Static and dynamic flexural behaviour of printed polylactic acid with thermal annealing: Parametric optimisation and empirical modelling. Int. J. Adv. Manuf. Technol. 2022, 119, 1179–1197. [Google Scholar] [CrossRef] [Scilit]
  14. El Magri, A.; Vanaei, S.; Shirinbayan, M.; Vaudreuil, S.; Tcharkhtchi, A. An investigation to study the effect of process parameters on the strength and fatigue behavior of 3D-printed PLA-graphene. Polymers 2021, 13, 3218. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  15. Bakhtiari, H.; Aamir, M.; Tolouei-Rad, M. Effect of 3D Printing Parameters on the Fatigue Properties of Parts Manufactured by Fused Filament Fabrication: A Review. Appl. Sci. 2023, 13, 904. [Google Scholar] [CrossRef] [Scilit]
  16. Shanmugam, V.; Das, O.; Babu, N.B.K.; Marimuthu, U.; Veerasimman, A.; Deepak Joel Johnson, R.; Neisiany, R.; Hedenqvist, M.; Ramakrishna, S.; Berto, F. Fatigue behaviour of FDM-3D printed polymers, polymeric composites and architected cellular materials. Int. J. Fatigue 2021, 143, 106007. [Google Scholar] [CrossRef] [Scilit]
  17. Gomez-Gras, G.; Jerez-Mesa, R.; Travieso-Rodriguez, J.A.; Lluma-Fuentes, J. Fatigue performance of fused filament fabrication PLA specimens. Mater. Des. 2018, 140, 278–285. [Google Scholar] [CrossRef] [Scilit]
  18. Azadi, M.; Dadashi, A.; Dezianian, S.; Kianifar, M.; Torkaman, S.; Chiyani, M. High-cycle Bending Fatigue Properties of Additive-Manufactured ABS and PLA Polymers Fabricated by Fused Deposition Modeling 3D-Printing. Forces Mech. 2021, 3, 100016. [Google Scholar] [CrossRef] [Scilit]
  19. Brčić, M.; Kršćanski, S.; Brnić, J. Rotating bending fatigue analysis of printed specimens from assorted polymer materials. Polymers 2021, 13, 1020. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  20. Ftoutou, E.; Allegue, L.; Marouani, H.; Hassine, T.; Fouad, Y.; Mrad, H. Modeling of Effect of Infill Density Percentage on Rotating Bending Fatigue Behavior of Additive-Manufactured PLA Polymers. Materials 2024, 17, 471. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  21. Bermudo Gamboa, C.; Martín-Béjar, S.; Bañón García, F.; Sevilla Hurtado, L. Enhancing Fatigue Resistance of Polylactic Acid through Natural Reinforcement in Material Extrusion. Polymers 2024, 16, 2422. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  22. Kianifar, M.; Azadi, M.; Heidari, F. Evaluation of stress-controlled high-cycle fatigue characteristics in PLA-wood fused deposition modeling 3D-printed parts under bending loads. PLoS ONE 2024, 19, e0300569. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  23. Alagheband, M.; Kosarimovahhed, M.; Zhang, Q.; Jung, S. Creep and failure of 3D-printed polymers: Impact of infill patterns and densities on shear strain and strength. Eng. Fail. Anal. 2025, 175, 109568. [Google Scholar] [CrossRef] [Scilit]
  24. Alagheband, M.; Zhang, Q.; Jung, S. Investigating the influence of infill patterns and mesh modifiers on fatigue properties of 3D printed polymers. Int. J. Fatigue 2024, 187, 108463. [Google Scholar] [CrossRef] [Scilit]
  25. Hosseini, F.Z.; Kianifar, M.; Azadi, M. Impact of biological environment on bending fatigue lifetime in additive-manufactured polylactic acid fabricated by 3D-printing. Polym. Test. 2024, 138, 108562. [Google Scholar] [CrossRef] [Scilit]
  26. Kianifar, M.; Azadi, M.; Heidari, F. Effect of simulated body fluid on the fatigue resistance of 3D-printed PLA and PLA-wood structures under cyclic bending loading. Int. J. Fatigue 2025, 195, 108876. [Google Scholar] [CrossRef] [Scilit]
  27. Horasan, M.; Sarac, I. The fatigue responses of 3D-printed polylactic acid (PLA) parts with varying raster angles and printing speeds. Fatigue Fract. Eng. Mater. Struct. 2024, 47, 3693–3706. [Google Scholar] [CrossRef] [Scilit]
  28. Česnik, M.; Slavič, J.; Boltežar, M. Accelerated vibration-fatigue characterization for 3D-printed structures: Application to fused-filament-fabricated PLA samples. Int. J. Fatigue 2023, 171, 107574. [Google Scholar] [CrossRef] [Scilit]
  29. Milovanović, A.; Poduška, J.; Trávníček, L.; Náhlík, L.; Sedmak, A.; Milošević, M.; Berto, F. Side-groove effect on fracture mechanical fatigue testing of PLA material. Procedia Struct. Integr. 2022, 42, 847–856. [Google Scholar] [CrossRef] [Scilit]
  30. Algarni, M. Fatigue Behavior of PLA Material and the Effects of Mean Stress and Notch: Experiments and Modeling. Procedia Struct. Integr. 2022, 37, 676–683. [Google Scholar] [CrossRef] [Scilit]
  31. Dudescu, M.C.; Racz, L.; Popa, F. Effect of infill pattern on fatigue characteristics of 3D printed polymers. Mater. Today Proc. 2023, 78, 263–269. [Google Scholar] [CrossRef] [Scilit]
  32. Son Minh, P.; Nguyen, V.T.; Uyen, T.M.T.; Do, T.T.; Duong Thi Van, A.; Nguyen Le Dang, H. The effects of 3D printing designs on PLA polymer flexural and fatigue strength. J. Micromechanics Microengineering 2024, 34, 065004. [Google Scholar] [CrossRef] [Scilit]
  33. TERCO AB. Dauerprüfer MT205 Rotating Bending Fatigue Testing Machine—Instruction Manual; TERCO AB: Skärblacka, Sweden, 2020. [Google Scholar]
  34. Seifollahi, M.; Kabir, M.Z. Fatigue life assessment of notched PLA manufactured using FDM 3D-printing technique. Polymers 2026, 18, 1. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  35. ASTM D7774-17; Standard Test Method for Flexural Fatigue Properties of Plastics. ASTM International: West Conshohocken, PA, USA, 2017.
  36. ASTM D638-22; Standard Test Method for Tensile Properties of Plastics. ASTM International: West Conshohocken, PA, USA, 2022.
  37. ASTM E178-21; Standard Practice for Dealing With Outlying Observations. ASTM International: West Conshohocken, PA, USA, 2021.
  38. Virtanen, P.; Gommers, R.; Oliphant, T.E.; Haberland, M.; Reddy, T.; Cournapeau, D.; Burovski, E.; Peterson, P.; Weckesser, W.; Bright, J.; et al. SciPy 1.0: Fundamental algorithms for scientific computing in Python. Nat. Methods 2020, 17, 261–272. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  39. Seabold, S.; Perktold, J. Statsmodels: Econometric and statistical modeling with Python. In Proceedings of the 9th Python in Science Conference, Austin, TX, USA, 28 June–3 July 2010; pp. 92–96. [Google Scholar] [CrossRef] [Scilit]
  40. R Core Team. R: A Language and Environment for Statistical Computing; R Foundation for Statistical Computing: Vienna, Austria, 2023; Available online: https://www.R-project.org/ (accessed on 7 October 2026).
  41. Shapiro, S.S.; Wilk, M.B. An analysis of variance test for normality (complete samples). Biometrika 1965, 52, 591–611. [Google Scholar] [CrossRef] [Scilit]
  42. Levene, H. Robust tests for equality of variances. In Contributions to Probability and Statistics: Essays in Honor of Harold Hotelling; Olkin, I., Ghurye, S.G., Hoeffding, W., Madow, W.G., Mann, H.B., Eds.; Stanford University Press: Stanford, CA, USA, 1960; pp. 278–292. [Google Scholar]
  43. Brown, M.B.; Forsythe, A.B. Robust tests for the equality of variances. J. Am. Stat. Assoc. 1974, 69, 364–367. [Google Scholar] [CrossRef]
  44. Welch, B.L. On the comparison of several mean values: An alternative approach. Biometrika 1951, 38, 330–336. [Google Scholar] [CrossRef] [Scilit]
  45. Kruskal, W.H.; Wallis, W.A. Use of ranks in one-criterion variance analysis. J. Am. Stat. Assoc. 1952, 47, 583–621. [Google Scholar] [CrossRef]
  46. Games, P.A.; Howell, J.F. Pairwise multiple comparison procedures with unequal N’s and/or variances: A Monte Carlo study. J. Educ. Stat. 1976, 1, 113–125. [Google Scholar] [CrossRef] [Scilit]
  47. Grubbs, F.E. Procedures for detecting outlying observations in samples. Technometrics 1969, 11, 1–21. [Google Scholar] [CrossRef]
  48. Rorabacher, D.B. Statistical treatment for rejection of deviant values: Critical values of Dixon’s “Q” parameter and related subrange ratios at the 95% confidence level. Anal. Chem. 1991, 63, 139–146. [Google Scholar] [CrossRef] [Scilit]
  49. Long, J.S.; Ervin, L.H. Using heteroscedasticity consistent standard errors in the linear regression model. Am. Stat. 2000, 54, 217–224. [Google Scholar] [CrossRef] [Scilit]
  50. Holm, S. A simple sequentially rejective multiple test procedure. Scand. J. Stat. 1979, 6, 65–70. [Google Scholar]
  51. Weibull, W. A statistical distribution function of wide applicability. J. Appl. Mech. 1951, 18, 293–297. [Google Scholar] [CrossRef] [Scilit]
  52. Meeker, W.Q.; Escobar, L.A. Statistical Methods for Reliability Data; Wiley: New York, NY, USA, 1998. [Google Scholar]
  53. Dawood, L.L.; AlAmeen, E.S. Influence of infill patterns and densities on the fatigue performance and fracture behavior of 3D-printed carbon fiber-reinforced PLA composites. AIMS Mater. Sci. 2024, 11, 833–857. [Google Scholar] [CrossRef] [Scilit]
  54. Jerez-Mesa, R.; Travieso-Rodriguez, J.A.; Llumà-Fuentes, J.; Gomez-Gras, G.; Puig, D. Fatigue lifespan study of PLA parts obtained by additive manufacturing. Procedia Manuf. 2017, 13, 872–879. [Google Scholar] [CrossRef] [Scilit]
  55. Han, X.; Li, W.; Chen, S.; Liu, X.; Cui, L. Research on angle-adaptive look-ahead compensation method for five-degree-of-freedom additive manufacturing based on sech attenuation curve. Micromachines 2026, 17, 423. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  56. Gosset, A.; Barreiro-Villaverde, D.; Becerra Permuy, J.C.; Lema, M.; Ares-Pernas, A.; Abad López, M.J. Experimental and numerical investigation of the extrusion and deposition process of a poly (lactic acid) strand with fused deposition modeling. Polymers 2020, 12, 2885. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  57. Vanaei, H.R.; Shirinbayan, M.; Vanaei, S.; Fitoussi, J.; Khelladi, S.; Tcharkhtchi, A. Multi-scale damage analysis and fatigue behavior of PLA manufactured by fused deposition modeling (FDM). Rapid Prototyp. J. 2021, 27, 371–378. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.