Highlights
What are the main findings?
- Spray distance is the dominant parameter affecting the microstructure and mechanical properties of HVOF-deposited MoSi2 coatings.
- A fraction of MoSi2 recomposites during HVOF spraying, forming Mo5Si3 phase.
- Optimized HVOF process parameters are obtained to deposit dense MoSi2 coatings.
What are the implications of the main findings?
- The dense MoSi2 protective coatings can be successfully fabricated via HVOF technology.
- Orthogonal experiment provides optimal parameter for HVOF MoSi2 coating deposition.
- The obtained coating exhibits a higher fracture toughness compared with pack-cementation-synthesized MoSi2 coatings.
Abstract
Refractory alloys, such as NbW5-1, are susceptible to catastrophic oxidation failure in high-temperature environments. The application of MoSi2 coatings on the surface is an effective approach to address this issue. MoSi2 coatings in the case were deposited via high velocity oxygen fuel (HVOF) spraying. A systematic orthogonal experimental design was used to investigate the effects of spray distance, powder feeder rotation speed and carrier gas flow rate on the microstructure, phase composition, porosity and mechanical properties of the coatings. The results showed that spray distance was the most important process parameter affecting coating performance. Nine coatings deposited in the case all primarily contained MoSi2 and a fraction of Mo5Si3. The coating deposited under the optimal process parameters (spray distance of 200 mm, propane pressure of 8 bar, powder feed r of 23 g/min, oxygen pressure of 10 bar, gun traverse speed of 180 mm·s−1 and carrier gas flow rate of 900 NL/h) exhibited a dense microstructure with a few isolated pores (porosity of 2.75%). This coating exhibited relatively optimal overall mechanical properties within the parameter range investigated in this study, with a Vickers hardness of 854 HV, an elastic modulus of 418 GPa and a fracture toughness of 4.41 MPa·m1/2. Therefore, high-melting-point MoSi2 coatings can be successfully deposited by using HVOF technology through its optimal process parameters.
1. Introduction
The service environments of hot-section components have become increasingly stringent with the development of high thrust-to-weight ratio aero-engines and next-generation aerospace vehicles, imposing extreme demands on the high-temperature mechanical properties and oxidation resistance of materials. Refractory metals and their alloys, such as niobium-tungsten alloys and molybdenum alloys, exhibit excellent high-temperature strength [1,2]. However, these materials exhibit a critical drawback in terms of their intrinsic oxidation resistance under high-temperature aerobic conditions, which leads to oxidation failure of the substrate within a short period [3]. This bottleneck limits the engineering application of refractory alloys in high-temperature components [4,5].
MoSi2 is widely recognized as one of the optimal candidates for the preparation of oxidation-resistant protective coatings [6]. MoSi2 coatings can be fabricated via various processes, including slurry coating, spark plasma sintering, plasma spraying, sputtering, pack cementation and hot-dip siliconizing [7,8,9,10]. The high-temperature characteristics of MoSi2 It has been extensively demonstrated that MoSi2 coating exhibits an excellent oxidation resistance, low electrical resistivity [11,12,13] and outstanding self-healing ability [14].
Pack cementation and slurry sintering are capable of producing relatively dense MoSi2 coatings. However, its preparation period is relatively long [15]. Coatings fabricated by slurry sintering can improve the high temperature performance, but pores in the coating are detrimental to the oxidation resistance [5]. Elemental doping and structural design are attempted to improve the high-temperature durability of MoSi2 coatings. The introduction of elements, such as W and Nb, can form the stable C40 or C11b crystal structures, thereby suppressing low-temperature oxidation disintegration [16,17]. In terms of structural design, the incorporation of second-phase particles, such as SiC and Al2O3, can alleviate the mismatch of coefficient of thermal expansion and improve the fracture toughness [18]. However, these approaches still largely depend on time-consuming and in situ diffusion processes. Thermal spraying technologies recently are used to the preparation of MoSi2 coatings, and it has been demonstrated that the coating microstructure can be tailored through powder morphology optimization, thereby enhancing the high-temperature performance [19]. However, a fraction of unbonded interfaces and pores remain in the coatings, which is inherently determined by the atmospheric plasma spraying (APS) technique. High-velocity oxygen-fuel (HVOF) spraying, owing to its high particle velocity and relatively moderate flame temperature [20,21,22], is capable of producing intermetallic compound coatings with low porosity and high adhesion strength [23,24,25], thus exhibiting unique advantages in the fabrication of MoSi2 coatings. Nevertheless, HVOF involves numerous process parameters with complex coupled effects [26,27], and the high melting point of MoSi2 further complicates the deposition process. To date, only limited studies have reported on the preparation of HVOF-sprayed MoSi2 coatings, and the effects of HVOF process parameters on the microstructure, phase composition, and mechanical properties of MoSi2 coatings remain insufficiently understood.
In this study, to elucidate the microstructural evolution behavior of MoSi2 coatings, MoSi2 coatings were deposited on NbW5-1 niobium-tungsten alloy substrates by using HVOF technology. Through an orthogonal experimental design, the effects of spray distance, powder feeder rotation speed and carrier gas flow rate on coating densification, phase composition, hardness, elastic modulus and fracture toughness were systematically investigated. The aim is to reveal the correlation between HVOF spraying process parameters and coating microstructure-mechanical properties, and to obtain the optimal parameter combination for preparing high-performance MoSi2 protective coatings on NbW5-1 alloy substrates.
2. Materials and Methods
2.1. Materials
The substrate material used in this study was NbW5-1 niobium-tungsten alloy, a typical material for ultra-high-temperature aerospace structural components, which maintains stable high-temperature strength and creep resistance under extreme service conditions exceeding 1600 °C. Annealed NbW5-1 plates were machined by wire electrical discharge machining into standard specimens of 30 mm × 40 mm × 3 mm. Its chemical composition met the requirements of aerospace material standards, as shown in Table 1.
Table 1.
Chemical compositions of NbW5-1 niobium-tungsten alloy.
The MoSi2 powder had a particle size ranging from 5 to 25 μm, and an apparent density of 2.8–3.0 g/cm3.
2.2. Coating Preparation
MoSi2 coatings were deposited under various process parameters using a BS3500 HVOF spraying system (Shaanxi Bangxin Surface Engineering Technology Co., Ltd., Xi’an, China). Prior to spraying, the substrate surfaces were grit-blasted to increase surface roughness and enhance the adhesion strength between the coating and the substrate. The MoSi2 powder was dried in an oven at 100 °C for 2 h. Coating deposition was performed according to the process parameters designed by the orthogonal experiment, as listed in Table 2 and Table 3. It should be noted that the powder feeder rotation speeds listed in Table 3 are the set values for the feeding system used in this study. Based on powder feed rate calibration, feeder rotation speeds of 6, 7, and 8 r/min correspond to actual powder feed rates of 18, 21, and 24 g/min, respectively. To maintain consistency with the original orthogonal experimental design, group designations, and figures, the powder feeder rotation speed is retained in Table 3 and the related figures. The effects of the actual powder feed rate are discussed in the following sections based on the above conversion relationship.
Table 2.
Main process parameters of HVOF spraying.
Table 3.
Orthogonal experimental design for spraying parameters.
2.3. Microstructural and Performance Characterization
The specimens were mounted via cold mounting (acrylic resin to hardener mass ratio of 5:4) and cured. The mounted samples were sequentially ground using 800-, 1000-, 1500-, and 2000-grit SiC abrasive papers, followed by fine polishing with 0.25 μm diamond paste. Finally, the polished surfaces were cleaned with ethanol and dried with cold air for subsequent characterization.
The morphology and elemental composition of the specimens were analyzed via a TESCAN MIRA4 field-emission scanning electron microscope (SEM, TESCAN, Brno, Czech Republic) equipped with an Oxford XPLORE 30 energy-dispersive spectrometer (EDS) (Oxford Instruments Nano Analysis, High Wycombe, UK). The phase constituents of the coatings were characterized by a Rigaku MiniFlex600 X-ray diffractometer (XRD) (Shimadzu, Kyoto, Japan) with Cu Kα radiation. The scanning range was 10° to 80° with a scanning speed of 10°/min.
Vickers hardness was measured by a micro-Vickers hardness tester under a load of 300 g with a dwell time of 10 s. The Vickers hardness value (HV) was calculated according to the following equation [28].
where P is the applied load (g) and d is the half-diagonal length of the indentation (mm).
The elastic modulus was determined by the Knoop indentation method, performed on the polished cross-section of the coating under a load of 300 g with a dwell time of 10 s. The relationship is expressed as [29].
Fracture toughness was evaluated by the indentation method on the polished cross-section of the coating using a digital Vickers hardness tester (Laizhou Huayin Testing Instrument Co., Ltd., Laizhou, China) under a load of 500 g with a dwell time of 30 s. During indentation, two types of cracks may form on the specimen surface. When the ratio of crack radius (c) to the indentation half-diagonal (d) satisfies c/d ≤ 2.5, the cracks are classified as Palmqvist type; when c/d ≥ 2.5, the cracks evolve into Half-Penny type. The corresponding fracture toughness KIC was calculated using the following empirical formulas.
For Palmqvist cracks (c/d ≤ 2.5) [30].
For Half-Penny cracks (c/d ≥ 2.5) [30].
where HV is the Vickers hardness, d is the half-diagonal length of the indentation (m), E is the elastic modulus (GPa) and c is the crack radius (m).
3. Results
3.1. Morphology and Phase Composition of the MoSi2 Powder
Figure 1 shows the SEM morphology and XRD pattern of the MoSi2 feedstock powder. As shown in Figure 1a, the powder consisted mainly of irregular angular particles with a relatively broad particle-size distribution, and some fine particles were attached to the surfaces of larger particles. The XRD pattern in Figure 1b indicates that MoSi2 was the predominant crystalline phase. In addition, several weak diffraction peaks were indexed to Mo5Si3, confirming the presence of a small amount of Mo5Si3 as a secondary phase in the starting powder.
Figure 1.
SEM morphology (a) and XRD pattern (b) of the MoSi2 powder.
3.2. Coating Microstructure
Cross-sectional morphologies of the nine as-sprayed MoSi2 coatings were characterized by SEM, as shown in Figure 2. Under the identical number of spraying passes, the coating thicknesses for the nine parameters were 8 μm, 5 μm, 4 μm, 6 μm, 8 μm, 15 μm, 5 μm, 50 μm and 4 μm, respectively. The significant variation in thickness among the nine coatings indicates that the spraying parameters substantially influence the deposition efficiency. Owing to the high melting point of MoSi2 (2030 °C), most process parameters failed to achieve sufficient melting of MoSi2 under the extremely short heating duration of HVOF, resulting in a rather low deposition efficiency and the coating thickness that could not meet application requirements. Within the process-parameter range investigated in this case, only the process parameters in group 8 can fulfill the thickness requirement.
Figure 2.
Cross-sectional morphologies of as-sprayed coatings under nine orthogonal experimental conditions: (a–i) sequentially correspond to Group 1–9 in Table 3.
The microstructures revealed significant differences among nine coatings in terms of densification, particle spreading behavior and defects. Most of the coatings prepared in this study exhibited obvious defects. In the cross-section of Group 1, irregular pores with diameters of approximately 5–8 μm were observed, and the particles at the pore edges appeared agglomerated, indicating insufficient melting of the powder. Local inter-lamellar separation was also present. Such defects suggested insufficient thermal and kinetic energy of the particles during deposition and limited spreading. The indenter load tends to form stress concentrations around the pores during hardness test, reducing the resistance to indentation propagation [31,32]. Group 2 exhibited a thickness fluctuation of 2–3 μm, and the thin regions contained micropores, concentrating at the inter-particle stacking gaps. The non-uniform thickness leaded to unbalanced load distribution during loading, which can cause a low elastic modulus. Group 6 displayed obvious interfacial cracks accompanied by micro-pores, these microcracks significantly can reduce the adhesion strength of the coating. Group 7 contained large pores interconnected with delamination interfaces, weakening the overall load-bearing capacity and adhesion of the coating.
The cross-sectional morphology of Group 8 exhibited a dense and a uniform microstructure. The particles were flattened and well-spread, with flattened particle thicknesses of approximately 0.8–1.2 μm. The particles were tightly bonded in a “laminated and interlocked” manner, with no visible gaps at the interfaces. The black contrast in the picture is the second phase. Only a few isolated closed pores with diameters smaller than 0.3 μm were present, randomly distributed without forming interconnected channels, and the porosity was approximately 3%. The close stacking of flattened particles substantially increased the inter-particle bonding area and interfacial bonding strength [33]. The stress can be uniformly transmitted through the continuous particle interfaces, effectively alleviating local stress concentrations during hardness test. As a result, the flattened particles exhibit strong resistance to slip, corresponding to a higher elastic modulus [34]. Furthermore, the isolated closed pores do not provide continuous oxygen transport paths, reducing the oxygen diffusion rate, which is beneficial for enhancing the oxidation resistance of the coating. Therefore, based on the cross-sectional observations, among the nine parameters, the coating deposited by Group 8 was expected to achieve superior mechanical properties.
3.3. Elemental Distribution and Phase Constituents of Coatings
To further clarify the elemental distribution characteristics of the Group 8 coating, EDS mapping was performed on its cross-section (Figure 3). The EDS mapping results indicated that Mo and Si were uniformly distributed and dispersed throughout the coating, without significant local enrichment or depletion. This uniform distribution can avoid the formation of local performance-degrading regions due to elemental segregation, providing a structural basis for the overall consistency of mechanical properties. MoSi2 is known to be susceptible to decomposition during thermal spraying [35]. X-ray diffraction will be employed to determine whether phase transformations occurred during spraying. No significant oxygen enrichment was detected in the coating, suggesting that no obvious oxidation or oxidation-induced decomposition occurred during deposition. The Nb element was entirely confined to the substrate region, and no Nb element was detected in the coating. The combined Mo and Si elemental distributions indicated that the interface between the coating and the substrate is predominantly mechanical in nature, ensuring that the coating phase composition remains dominated by the target MoSi2 phase.
Figure 3.
Elemental distribution characteristics in the Group 8 coating.
Figure 4 shows the XRD patterns of the MoSi2 coatings prepared under the nine different spraying processes in the orthogonal experiment. The overall characteristics of the diffraction patterns for all coating groups were highly similar. All coatings primarily contained MoSi2 and a fraction of Mo5Si3. Compared with the coating deposited by atmospheric plasma spraying [19], the high-velocity and low-temperature characteristics of HVOF can effectively suppress excessive decomposition of the MoSi2 powder, maximizing the content of the MoSi2 structural framework. The Mo5Si3 phase detected in coatings are brittle impurity phase, which is attributed to the partial decomposition of MoSi2 in the high-temperature jet, such as plasma-spraying [36,37]. This reaction can proceed spontaneously under the HVOF flame. Compared with MoSi2, Mo5Si3 has a lower fracture toughness, which renders MoSi2 coating cracking. In terms of oxidation resistance, MoSi2 can rapidly form a dense and continuous SiO2 protective film at elevated temperatures, exhibiting excellent high-temperature oxidation resistance [38]. In comparison, Mo5Si3 has a lower capability to form a complete SiO2 scale, which is detrimental to the high-temperature oxidation resistance of the coating [35]. Therefore, the small amount of Mo5Si3 generated in this study was unfavorable for the fracture toughness and high-temperature oxidation resistance of the MoSi2 coatings.
Figure 4.
XRD patterns of the nine coatings.
3.4. Porosity Analysis of Coatings
Figure 5 presents the porosity of the nine coatings. To identify the optimal process parameters and clarify the influence weights of each parameter on coating porosity, range analysis (R-method) was applied to the porosity data, and the effects of different process parameters on each property were systematically analyzed. The range analysis results for the porosity of each coating specimen under the orthogonal experimental design are presented in Table 4. The range of spray distance (R = 3.18) was significantly higher than that of powder feeder rotation speed (R = 2.40) and carrier gas flow rate (R = 1.33). This indicated that spray distance in the case was the mainly factor that affected the coating porosity, followed by powder feeder rotation speed and carrier gas flow rate.
Figure 5.
Porosity statistics of the nine as-sprayed coatings.
Table 4.
Range analysis table for porosity.
Figure 6 presents the dependence of the coating porosity on the different spraying process parameters. The porosity first increased and then decreased with increasing the powder feeder rotation speed. The porosity reached a peak of approximately 8.76% at rotation speed of 7 r/min, whereas the porosity decreased to 6.36% when the speed was increased to 8 r/min. It was reported that the powder feed rate per unit time is insufficient at low rotation speed, resulting in low deposition density of molten particles and a higher number of pores. The powder feeder rotation speed matched with the spraying parameters, reducing the coating porosity to a relatively low level. It should be noted that the powder feed rate was proportional to the powder feeder rotation speed. Therefore, the effect of powder feeder rotation speed on porosity essentially reflected the effect of the powder feed rate.
Figure 6.
Relationship between spraying process parameters and porosity.
The effect of carrier gas flow rate on porosity exhibited a “V-shaped” trend. The porosity reached the highest value of 8.13% at 800 NL/h and then decreased to 6.80% at a flow rate of 900 NL/h. The literature indicated that the kinetic energy imparted to the powder by the carrier gas is insufficient at low flow rate, leading to particle agglomeration and non-uniform delivery, which results in localized pore defects in the coating. Conversely, excessive gas flow disturbance destabilizes the flame flow field [39], affecting the heating, melting, and deposition behavior of the particles. Therefore, carrier gas flow rate of 900 NL/h enables uniform and stable powder delivery, thereby achieving lower coating porosity, but the coating still contained numerous micro-pores because of the high melting point of MoSi2.
The effect of spray distance on the coating porosity exhibited a monotonic positive correlation. When the spray distance increased from 200 mm to 300 mm, the porosity increased from 5.72% to 8.90%. This can be attributed to the changes in particle thermodynamic and kinetic behavior during flight [40]. At a shorter spray distance, the molten MoSi2 particles have a shorter flight time and retain sufficient thermal and kinetic energy upon reaching the substrate; the impact deformation is adequate, favoring the filling of inter-particle gaps and thus reducing porosity. With increasing spray distance, heat exchange between the particles and the environment intensifies, the particle temperature decreases, deformability declines, and the stacking of particles becomes looser, resulting in increased porosity. Meanwhile, the flame heats the powder while also increasing its velocity [41]. Within the spray distance range of this study, as the spray distance increases, the particle velocity decreases, leading to reduced deposition efficiency and an increase in porosity and other defects.
3.5. Mechanical Properties of Coatings
Figure 7 shows the Vickers hardness, elastic modulus and fracture toughness of nine MoSi2 coatings. Notable performance differences were observed among nine coatings. Group 8 exhibited the best overall properties, with the three indicators reaching 854 HV, 418 GPa and 4.41 MPa·m1/2, respectively. Group 3 showed the poorest properties with corresponding values of 256 HV, 103 GPa and 2.13 MPa·m1/2. The properties were highly consistent with the cross-sectional microstructures shown in Figure 3. Compared with the fracture toughness (2.9 MPa·m1/2) of MoSi2 coatings prepared by pack cementation [42], the fracture toughness of the Group 8 in this case was increased by approximately 52.1%. It indicated that the coating deposited by HVOF with optimal parameters has an advantage in crack propagation resistance.
Figure 7.
Mechanical properties of the nine coatings, including Vickers hardness, elastic modulus and fracture toughness.
MoSi2 exhibits a high intrinsic strength due to its covalent crystal structure, which facilitates the coating densification during HVOF [43]. The Group 8 coating exhibited the highest hardness, attributed to its low porosity and uniform distribution of the hard phase. In comparison, the other coating represented a significant decrease in hardness because of the increased porosity induced by the insufficient deformation of particles. Previous studies have indicated that the elastic modulus is primarily governed by coating density and inter-particle bonding rate [44]. Fracture toughness depends on the resistance to crack propagation [45]. In terms of the coatings with more defects, cracks propagated rapidly along inter-lamellar interfaces, resulting in the low fracture toughness. Group 8 coating only contained a fraction of isolated pores. Cracks propagation in the coating need more energy dissipation, thereby exhibiting a rather high fracture toughness.
Based on above results, the optimal process parameters identified in this case were spray distance of 200 mm, propane flow rate of 8 bar, powder feeder rotation speed of 8 r/min, oxygen pressure of 10 bar, gun traverse speed of 180 mm·s−1 and carrier gas flow rate of 900 NL/h, which can deposit MoSi2 coatings with high density and excellent mechanical properties. The high-temperature oxidation resistance of this coating will be discussed in detail in future work.
4. Conclusions
Nine MoSi2 coatings were deposited via HVOF technology through an orthogonal test, and the microstructure, phase constituents and mechanical properties were systematically discussed. The conclusions are briefly summarized as follows.
- (1)
- MoSi2 coatings can be successfully deposited on Niobium-tungsten alloy by using HVOF. The spray distance was the most important parameter affecting the microstructure and properties of MoSi2 coating.
- (2)
- Partial decomposition of MoSi2 occurred during HVOF, forming a fraction of the Mo5Si3, which led to a reduction in fracture toughness. Therefore, further enhancement of the fracture toughness can be achieved by controlling the Mo5Si3 content.
- (3)
- The Group 8 coating exhibited tightly bonded particles in a “laminated and interlocked” manner, with a few isolated micro-pores and a porosity of 2.75%, demonstrating excellent comprehensive mechanical properties: Vickers hardness of 854 HV, elastic modulus of 418 GPa and fracture toughness of 4.41 MPa·m1/2.
- (4)
- The high-melting-point characteristic of MoSi2 posed challenges for the HVOF deposition of MoSi2 coatings. Based on the orthogonal experiment, the coating with desirable phase composition, microstructure and mechanical properties was obtained under the following process parameters: spray distance of 200 mm, propane flow rate of 8 bar, powder feeder rotation speed of 8 r/min, oxygen pressure of 10 bar, gun traverse speed of 180 mm·s−1, and carrier gas flow rate of 900 NL/h.
Author Contributions
Conceptualization, H.D. and Y.Z.; methodology, C.W. and F.W. and L.W.; formal analysis, C.W.; investigation, C.W. and F.W.; writing—original draft preparation, C.W. and F.W.; writing—review and editing, H.D. and Y.Z.; supervision, H.D.; project administration, H.D. and Y.Z.; resources, Y.Z. All authors have read and agreed to the published version of the manuscript.
Funding
The research was funded by Shaanxi Province Key Research and Development Projects (Program No. 2024CY-GJHX-39).
Institutional Review Board Statement
Not applicable.
Informed Consent Statement
Not applicable.
Data Availability Statement
The raw data supporting the conclusions of this article will be made available by the authors on request.
Conflicts of Interest
The authors declare no conflicts of interest.
References
- Hu, B.L.; Quan, C.F.; Zhao, X.R.; Xing, H.R.; Shi, Z.Q.; Yi, S.F.; Wang, Q.; Yang, J.Z.; Wang, L.; Jin, B.; et al. Microstructure and performance optimization of molybdenum alloys reinforced by zirconium carbide whiskers. J. Alloys Compd. 2026, 1058, 187078. [Google Scholar] [CrossRef] [Scilit]
- Antusch, S.; Reiser, J.; Hoffmann, J.; Onea, A. Refractory materials for energy applications. Energy Technol. 2017, 5, 1064–1070. [Google Scholar] [CrossRef] [Scilit]
- Sikka, V.K.; Rosa, C.J. High temperature oxidation of Nb-10 at. % W alloy. Corros. Sci. 1980, 20, 1201–1219. [Google Scholar] [CrossRef] [Scilit]
- Han, J.Y.; Wang, L.; Hu, P.; Hu, B.L.; Ma, S.J.; Gao, L.L.; Bai, R.; Wang, Q.; Feng, R.; Jin, B.; et al. Research progress in modification of MoSi2 coatings on surface of refractory metals and their alloys, a review. Rare Met. 2025, 44, 793–821. [Google Scholar] [CrossRef] [Scilit]
- Yang, R.; Yang, H.J.; Zhang, M.; Shi, X.H.; Qiao, J.W. Refractory high-entropy aluminized coating with excellent oxidation resistance and lubricating property prepared by pack cementation method. Surf. Coat. Technol. 2023, 473, 129967. [Google Scholar] [CrossRef] [Scilit]
- Pan, X.H.; Li, C.; Niu, Y.R.; Zhong, X.; Huang, L.P.; Zeng, Y.; Zheng, X.B. Effect of Yb2O3 addition on oxidation/ablation behaviors of ZrB2-MoSi2 composite coating under different environment. Corros. Sci. 2020, 175, 108882. [Google Scholar] [CrossRef] [Scilit]
- Zhu, L.; Wang, X.H.; Ren, X.R.; Zhang, P.; Feng, P.Z. Recycling MoSi2 heating elements for preparing oxidation resistant multilayered coatings. J. Eur. Ceram. Soc. 2022, 42, 921–934. [Google Scholar] [CrossRef] [Scilit]
- Mueller, A.; Wang, G.; Rapp, R.A.; Courtright, E.L. Deposition and cyclic oxidation behavior of a protective (Mo,W)(Si,Ge)2 coating on Nb-base alloys. J. Electrochem. Soc. 1992, 139, 1266–1275. [Google Scholar] [CrossRef] [Scilit]
- Yoon, J.K.; Lee, K.H.; Kim, G.H.; Lee, J.K.; Doh, J.M.; Hong, K.T. Growth kinetics of MoSi2 coating formed by a pack siliconizing process. J. Electrochem. Soc. 2004, 151, B309. [Google Scholar] [CrossRef] [Scilit]
- Fu, T.; Zhang, Y.Y.; Shen, F.Q.; Cui, K.K.; Chen, L.Y. Microstructure and oxidation behavior of Si-MoSi2 coating deposited on Mo substrate at 600 °C and 900 °C in static air. Mater. Charact. 2022, 192, 112192. [Google Scholar] [CrossRef] [Scilit]
- Kircher, T.A.; Courtright, E.L. Engineering limitations of MoSi2 coatings. Mater. Sci. Eng. A 1992, 155, 67–74. [Google Scholar] [CrossRef] [Scilit]
- Liu, L.; Zhang, H.Q.; Lei, H.; Li, H.Q.; Gong, J.; Sun, C. Influence of different coating structures on the oxidation resistance of MoSi2 coatings. Ceram. Int. 2020, 46, 5993–5997. [Google Scholar] [CrossRef] [Scilit]
- Wang, L.; Wang, W.Y.; Fu, Q.G. The improvement of the self-healing ability of MoSi2 coatings at 900–1200 °C by introducing SiB6. J. Eur. Ceram. Soc. 2020, 40, 2896–2906. [Google Scholar] [CrossRef] [Scilit]
- Stryczniewicz, W.; Zmywaczyk, J.; Panas, A.J. Inverse problem solution for a laser ffash studies of a thin layer coatings. Int. J. Numer. Methods Heat Fluid Flow 2017, 27, 698–710. [Google Scholar] [CrossRef] [Scilit]
- Munro, T.C.; Gleeson, B. The deposition of aluminide and silicide coatings on γ-TiAl using the halide-activated pack cementation method. Met. Mater. Trans. A 1996, 27, 3761–3772. [Google Scholar] [CrossRef] [Scilit]
- Wang, Y.R.; Sun, H.F.; Sun, S.P.; Wang, H.J.; Zhao, F.L.; Zhang, Y.; Li, X.P. Effect of Nb and W alloying by arc cladding on the high-temperature oxidation resistance of MoSi2 coatings. Mater. Rep. 2025, 39, 24040229. [Google Scholar]
- Liu, L.; Zhang, L.; Liu, D. Complete elimination of pest oxidation by high entropy refractory metallic silicide (Mo0.2W0.2Cr0.2Ta0.2Nb0.2)Si2. Scr. Mater. 2020, 189, 25–29. [Google Scholar] [CrossRef] [Scilit]
- Niihara, K.; Suzuki, Y. Strong monolithic and composite MoSi2; materials by nanostructure design. Mater. Sci. Eng. A 1999, 261, 6–15. [Google Scholar] [CrossRef] [Scilit]
- Yan, J.H.; Xu, J.J.; Rafi-ud-din; Wang, Y.; Liu, L.F. Preparation of agglomerated powders for air plasma spraying MoSi2 coating. Ceram. Int. 2015, 41, 10547–10553. [Google Scholar] [CrossRef] [Scilit]
- Li, M.H.; Christofides, P.D. Computational study of particle in-flight behavior in the HVOF thermal spray process. Chem. Eng. Sci. 2006, 61, 5045–5057. [Google Scholar] [CrossRef] [Scilit]
- Mittal, G.; Paul, S. Suspension and Solution Precursor Plasma and HVOF Spray: A Review. J. Therm. Spray Technol. 2022, 31, 1443–1475. [Google Scholar] [CrossRef] [Scilit]
- Turunen, E.; Varis, T.; Gustafsson, T.E.; Keskinen, J.; Lintunen, P.; Falt, T.; Nowak, R.; Hannula, S.P. Process optimization for nanostructured HVOF-sprayed Al2O3-based ceramic coatings. J. Therm. Spray Technol. 2006, 15, 595–602. [Google Scholar] [CrossRef] [Scilit]
- Zeng, H.J.; Zhang, L.Q.; Lin, J.P.; Zhang, S.J.; Chen, G.L. TiAlNb intermetallic compound coating prepared by high velocity oxy-fuel spraying. Surf. Coat. Technol. 2011, 206, 178–184. [Google Scholar] [CrossRef] [Scilit]
- Chaves, H.; Herbst, S.; Skupsch, C. Measurement of the particle velocity in a HVOF spray with PIV under industrial conditions. J. Therm. Spray Technol. 2012, 21, 476–482. [Google Scholar] [CrossRef] [Scilit]
- Tang, S.C.; Zhang, C.Y.; Luo, X.T.; Li, C.J. Suppressing formation of spinel mixed oxides on HVOF MCrAlY bond coat via a low-power pulsed-laser remelting treatment. Corros. Commun. 2026, 9, 100013. [Google Scholar] [CrossRef] [Scilit]
- Hambrock, C.; Rannetbauer, W.; Hubmer, S.; Ramlau, R. Predicting interaction phenomena in HVOF thermal spraying of WC-CoCr, a hybrid experimental–statistical approach. J. Therm. Spray Technol. 2025, 34, 2145–2157. [Google Scholar] [CrossRef] [Scilit]
- Valarezo, A.; Shinoda, K.; Sampath, S. Effect of deposition rate and deposition temperature on residual stress of HVOF-sprayed coatings. J. Therm. Spray Technol. 2020, 29, 1322–1338. [Google Scholar] [CrossRef] [Scilit]
- Smith, R.L.; Sandland, G.E. An Accurate Method of Determining the Hardness of Metals, with Particular Reference to Those of a High Degree of Hardness. Proc. Inst. Mech. Eng. 1922, 102, 623–641. [Google Scholar] [CrossRef] [Scilit]
- Marshall, D.B.; Noma, T.; Evans, A.G. A Simple Method for Determining Elastic-Modulus-to-Hardness Ratios using Knoop Indentation Measurements. J. Am. Ceram. Soc. 1982, 65, c175–c176. [Google Scholar] [CrossRef] [Scilit]
- Costa Oliveira, F.A.; Cruz Fernandes, J. Mechanical and thermal behaviour of cordierite–zirconia composites. Ceram. Int. 2002, 28, 79–91. [Google Scholar] [CrossRef] [Scilit]
- Seitov, B.; Kurbanbekov, S.; Baltabayeva, D.; Kakimzhanov, D.; Katpayeva, K.; Temirbekov, A.; Bekbayev, S.; Mussakhan, N. Review of physical and mechanical properties, morphology, and phase structure in Cr3C2-NiCr composite coatings sprayed by HVOF method. Coatings 2025, 15, 479. [Google Scholar] [CrossRef] [Scilit]
- Wang, Y.; Xiao, W.; Wang, B.; Zhao, J.; Zhou, Z.; Li, S.; Mao, W. Influence of HVOF spray parameters on tribological behavior in CoCrFeNiMo high-entropy alloy coatings. Surf. Coat. Technol. 2025, 518, 132856. [Google Scholar] [CrossRef] [Scilit]
- Sun, C.; Guo, L.; Lu, G.; Lv, Y.; Ye, F. Interface bonding between particle and substrate during HVOF spraying. Appl. Surf. Sci. 2014, 317, 908–913. [Google Scholar] [CrossRef] [Scilit]
- Sun, J.; Li, T.; Zhang, G.P. Effect of thermodynamically metastable components on mechanical and oxidation properties of the thermal-sprayed MoSi2 based composite coating. Corros. Sci. 2019, 155, 146–154. [Google Scholar] [CrossRef] [Scilit]
- Liu, T.; Niu, Y.R.; Li, C.; Zhao, J.; Zhang, J.M.; Zeng, Y.; Zheng, X.B.; Ding, C.X. Effect of MoSi2 addition on ablation behavior of ZrC coating fabricated by vacuum plasma spray. Ceram. Int. 2018, 44, 8946–8954. [Google Scholar] [CrossRef] [Scilit]
- Reisel, G.; Wielage, B.; Steinhauser, S.; Morgenthal, I.; Scholl, R. High temperature oxidation behavior of HVOF-sprayed unreinforced and reinforced molybdenum disilicide powders. Surf. Coat. Technol. 2001, 146–147, 19–26. [Google Scholar] [CrossRef] [Scilit]
- Luo, J.C.; Li, C.; Wang, G.Q.; Chen, L.; Gao, L.L.; Dong, H.; Yang, G.J. Enhancing oxidation resistance of air plasma-sprayed MoSi2 coatings by tailoring as-sprayed coating structure. J. Eur. Ceram. Soc. 2026, 46, 118579. [Google Scholar] [CrossRef] [Scilit]
- Zhu, L.; Zhu, Y.S.; Ren, X.R.; Zhang, P.; Qiao, J.H.; Feng, P.Z. Microstructure, properties and oxidation behavior of MoSi2-MoB-ZrO2 coating for Mo substrate using spark plasma sintering. Surf. Coat. Technol. 2019, 377, 124909. [Google Scholar] [CrossRef] [Scilit]
- Kamnis, S.; Gu, S.; Lu, T.J.; Chen, C. Computational simulation of thermally sprayed WC–Co powder. Comput. Mater. Sci. 2008, 43, 1172–1182. [Google Scholar] [CrossRef] [Scilit]
- Sobolev, V.V.; Guilemany, J.M. Investigation of coating porosity formation during high-velocity oxy-fuel (HVOF) spraying. Mater. Lett. 1994, 18, 304–308. [Google Scholar] [CrossRef] [Scilit]
- Kuznetsov, Y.A.; Dobychin, A.V.; Yakovlev, D.D.; Gribakin, A.A.; Matyukhin, S.I.; Kravchenko, I.N. An analytical model of processes of heating and acceleration of particles in supersonic gas-flame spraying. Tech. Phys. 2026, 71, 425–429. [Google Scholar] [CrossRef] [Scilit]
- Jiang, L.; Zheng, B.; Wu, C.S.; Li, P.X.; Xue, T.; Wu, J.D.; Han, F.L.; Chen, Y.H. A review of Mo-Si intermetallic compounds as ultrahigh-temperature materials. Processes 2022, 10, 1772. [Google Scholar] [CrossRef] [Scilit]
- Kamnis, S.; Gu, S.; Vardavoulias, M. The influence of powder porosity on the bonding mechanism at the impact of thermally sprayed solid particles. Metal. Mater. Trans. A 2010, 41, 3517–3524. [Google Scholar] [CrossRef] [Scilit]
- Valarezo, A.; Sampath, S. An integrated assessment of process-microstructure-property relationships for thermal-sprayed NiCr coatings. J. Therm. Spray. Technol. 2011, 20, 1244–1258. [Google Scholar] [CrossRef] [Scilit]
- Suhonen, T.; Varis, T.; Turunen, E.; Liu, X.; Ge, Y.; Soderberg, O.; Hannula, S.P. The effect of microstructure on mechanical properties of HVOF sprayed WC-CoCr composite coatings. Tribologia 2009, 28, 14–28. [Google Scholar]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.