Skip to Content
CoatingsCoatings
  • Editor’s Choice
  • Article
  • Open Access

28 June 2026

21 Pages

Improving the Adsorption Performance of Eriochrome Black T Using Aluminum Oxide Films as a Nanoadsorbent

,
,
,
,
,
,
and
1
Facultad de Ciencias Exactas, Químicas y Naturales, Universidad Nacional de Misiones, Posadas 3300, Argentina
2
Consejo Nacional de Investigaciones Científicas y Técnicas (CONICET), Ciudad Autónoma de Buenos Aires 1425, Argentina
3
Programa de Materiales y Fisicoquímica (PROMyF), Instituto de Materiales de Misiones (IMaM-CONICET), Posadas 3300, Argentina
4
Laboratorio de Biotecnología Molecular, Instituto de Biotecnología Misiones “Dra. María Ebe Reca” (INBIOMIS), Posadas 3300, Argentina

Abstract

Optimizing industrial wastewater treatment systems requires efficient, cost-effective, and easily adaptable technologies. In this context, adsorption emerges as a promising alternative through the use of advanced nanostructured materials that optimize contaminant removal and facilitate their separation from the treated medium. This work evaluates the use of nanoporous anodic aluminum oxide (AAO) as a nanoadsorbent for the removal of Eriochrome Black T (EBT) dye, analyzing the effect of thermal and chemical modifications on its performance. The results demonstrated that calcination and chemical etching with NaOH, applied individually, increased removal efficiency by 10% compared to untreated AAO. Notably, the combined treatment (calcination + alkaline etching) boosted removal efficiency by 38% after 1 h of contact. Furthermore, this synergistic modification extended the viability of the process to alkaline media (up to pH 10) and allowed the material to be reused for four consecutive cycles, maintaining an 85% removal rate. Finally, the kinetic analysis elucidated the influence of the structural and chemical modifications on the adsorption rate, obtaining satisfactory correlations with various theoretical models.

1. Introduction

The vast majority of synthetic dyes used in industries such as textiles, leather, paper, and pharmaceuticals represent a critical source of water pollution, primarily due to the inefficiency of current treatment methods in removing them prior to discharge [1,2,3,4,5,6]. According to Akhouairi et al. [7], it is estimated that between 2% and 50% of total dye production is lost in industrial effluents. These substances are characterized as xenobiotic and recalcitrant compounds; their complex aromatic structures grant them high chemical stability, in addition to possessing carcinogenic and mutagenic properties [7,8]. In aquatic ecosystems, their presence obstructs sunlight penetration, which inhibits photosynthetic activity and promotes deleterious anaerobic conditions [9,10,11].
Among anionic azo dyes, Eriochrome Black T (EBT), utilized in analytical chemistry as a complexometric indicator and in the textile industry as a dye [12], exhibits low degradability under conventional treatment processes. It has been reported that concentrations as low as 1 mg·L−1 of this compound in industrial effluents pose severe environmental challenges [13], underscoring the imperative need to implement advanced treatment technologies to mitigate its impact [14].
To be applicable at an industrial scale, these technologies must be cost-effective, highly efficient, and sufficiently versatile for seamless integration into conventional effluent treatment systems [10,15,16,17,18]. Adsorption technology encompasses all these attributes, enabling the treatment of multiple contaminants with high removal efficiencies [19,20]. Furthermore, during this process, the contaminants accumulate on the adsorbent surface, facilitating their separation from the aqueous phase for subsequent regeneration and reuse [13,21,22].
Although a wide variety of adsorbents are available for dye removal from aqueous solutions, nanomaterials offer unique properties, such as a large specific surface area and high removal efficiency within short contact times [23]. Among them, polymeric nanocomposites [24], smart materials [25], metal oxides [26], and graphene derivatives [27] stand out. However, the selection of these adsorbents is mainly conditioned by high chemical synthesis costs, the difficulty of post-treatment separation and regeneration, and their low performance in real water matrices [28].
Anodic aluminum oxide (AAO) stands out as an effective nanoadsorbent for the removal of Eriochrome Black T (EBT) dye. Under optimized stirring (500 rpm) and temperature (60 °C) conditions, this material achieved removal efficiencies of up to 99% while demonstrating excellent capacity for regeneration and reuse, maintaining efficiencies above 50% [29]. Its synthesis, based on the electrochemical oxidation of aluminum alloys, represents a simple and low-cost alternative for obtaining nanoporous coatings with a high specific surface area on complex-geometry substrates, making them suitable for implementation as packing material in packed towers [30,31,32,33]. This structural feature offers an outstanding operational advantage over the conventional use of suspended alumina nanoparticles, whose recovery following effluent treatment remains challenging [11,34,35,36].
The adsorbent properties of AAO can be modulated through anodization parameters (such as electrolyte type, temperature, and voltage) or via thermal and chemical post-treatments that alter its morphology and surface chemistry. In this regard, Dwojak et al. [37] reported that AAO films synthesized in oxalic acid exhibit superior performance in EBT removal compared to those obtained in phosphoric or sulfuric acid media. On the other hand, Bitchatchi et al. [38] evaluated the regeneration capacity of AAO after the adsorption of 16 mg L−1 of EBT using three different treatments: calcination (600 °C for 4 h), chemical attack with NaOH, and enzymatic degradation of the dye with laccases. The results demonstrated that calcination is the most effective method, enabling the nanoadsorbent to be regenerated with removal efficiencies above 80% for up to three cycles, without dissolving the oxide film after successive uses, unlike what was observed with NaOH. Nonetheless, the specific effects of calcination and controlled chemical etching on the EBT adsorption capacity of these films have not been explored to date.
Calcination at moderate temperatures (400–600 °C) induces dehydration and water desorption, modifying the surface chemistry of the nanoadsorbent, while stabilizing the oxide structure and improving nanopore ordering. Concurrently, alkaline etching drives film dissolution as a function of exposure time, altering the oxide morphology [39]. Since both processes directly impact the material properties, they could modify the adsorption capacity of the AAO.
Therefore, the objective of this work is to investigate the extent to which post-treatments, such as calcination and alkaline etching, enhance the EBT removal efficiency of AAO nanoadsorbents. To this end, AAO films were synthesized via anodic oxidation of a commercial aluminum alloy (AA1050) and subjected to distinct post-treatment combinations before characterization. The resulting enhancement in EBT adsorption was evaluated at 500 rpm and 60 °C; additionally, the material’s performance under various pH levels, alongside its regeneration and reuse capacity, was systematically assessed.

2. Materials and Methods

2.1. Synthesis of the Nanoporous Anodic Aluminum Oxide

A sheet of aluminum alloy AA1050 (99.5% Al, supplied by AMEX® S.A., Ciudad Autónoma de Buenos Aires, Argentina) with 0.3 cm thickness, 1 cm wide and 15 cm long, was used as a starting material.
The substrate treatment was carried out following the steps reported by Kramer et al. [29], and the same anodization conditions were used (0.3 M oxalic acid (Anedra, Tigre, Argentina) at 40 °C, 30 V and an anodic oxidation of 1 h).

2.2. AAO Treatments

To enhance the EBT adsorption efficiency, AAO nanostructured films underwent the different treatment combinations described in Table 1.
Table 1. Treatments applied to AAO nanostructured films to improve EBT adsorption.
The samples were calcined in a muffle furnace ORL-I (ORL Hornos Eléctricos, Lomas de Zamora, Argentina) in ambient air for 4 h with a heating ramp of 10 °C·min−1. Pore widening was performed by immersing the samples in a 0.5 M NaOH (Cicarelli, San Lorenzo, Argentina) solution at 25 °C for 1 min.
Finally, after each treatment combination, the samples were washed by ultrasonication with distilled water for 5 min.

2.3. Preparation of EBT Solution

The Eriochrome Black T used as a pollutant dye model was provided by Sigma-Aldrich (St. Louis, MO, USA). Its characteristics are presented in Table 2.
Table 2. Physico-chemical characteristics of Eriochrome Black T.
The 16 mg·L−1 concentration EBT solution was prepared by dilution from a 400 mg·L−1 stock solution. The exact concentration of the dye was determined using a UV-visible spectrophotometer (Shimadzu UV-1800, Shimadzu Corporation, Kyoto, Japan) and the calibration curve previously reported by Kramer et al. at 532 nm. [29].

2.4. Characterization of AAO Films

The morphology of the aluminum oxide films, defined by Pore Diameter (PD) and Porosity (P), was determined by scanning electron microscopy (SEM) (SUPRA 40, Carl Zeiss NTS GmbH, Jena, Germany) before and after adsorption, as reported by Kramer et al. [29] and Bruera et al. [31].
FTIR spectra were recorded in the 4000–600 cm−1 region using an IRPrestige-21 spectrophotometer (Shimadzu Corporation, Kyoto, Japan) to characterize the surface functional groups.
The crystallinity of the samples was determined using a Rigaku SmartLab® X-ray diffractometer (Rigaku Corporation, Tokyo, Japan) (Cu Kα radiation, λ = 1.5418 Å) at a fixed incidence angle of 1°.

2.5. Adsorption Assays

2.5.1. Preliminary Studies

Triplicate adsorption experiments were conducted at 60 °C and 500 rpm using a magnetic stirring hot plate MS-H280-PRO (DLab Scientific, Beijing, China). In a typical run, 30 mL of EBT dye solution (16 mg·L−1) was treated in a 100 mL beaker with a spiral-mounted AAO adsorbent (total area: 30 cm2). The dye concentration was quantified using UV-Vis spectrophotometry. Subsequently, the removal efficiency (%R), the adsorption capacity at equilibrium (qe) and the adsorption capacity at a given time (qt) were determined using Equations (1)–(3), respectively [2,34,40].
R % = C 0 − C t C 0 × 100
q e = ( C 0 − C e ) × V a
q t = ( C 0 − C t ) × V a
where C0 is the adsorbate initial concentration (mg·L−1), Ct is the adsorbate final concentration after time t (mg·L−1), V is the volume of solution (L) and a is the effective adsorption surface area (cm2).
The effect of pH on the adsorption capacity of the AAO and AAO + 600TT + PW films was evaluated in duplicate by adjusting the pH of the dye solution (16 mg·L−1) within a range of 4.0 to 10.0 (in increments of 2.0 units) via the dropwise addition of 0.1 M HCl (Cicarelli, San Lorenzo, Argentina) and NaOH. The EBT removal efficiency was determined by UV-Vis spectroscopy at 532 nm, using calibration curves previously constructed for each pH value.
Furthermore, the point of zero charge (pHpzc) of the AAO + 600TT + PW films was determined using the pH drift method [41]. To eliminate dissolved carbon dioxide, a 0.01 M NaCl (Cicarelli, San Lorenzo, Argentina) solution was boiled and then used to prepare 30 mL aliquots, with the initial pH adjusted between 4 and 9. The samples were immersed in each solution and incubated at room temperature for 48 h. Following this period, the final pH (pHf) was measured. The difference between the final and initial pH (pHf − pH0) was then plotted against pH0. The pHpzc was identified as the point where the curve intersects the reference line.

2.5.2. Kinetic Study

To elucidate the mechanisms governing the adsorption process, kinetic studies were conducted at 60 °C and 500 rpm at an initial EBT concentration of 13 mg·L−1. The qt values (Equation (2)) were determined as a function of time for both the untreated AAO sample and the one exhibiting the highest adsorption performance. To fit the experimental data, several kinetic models were evaluated, including pseudo-first-order (PFO), pseudo-second-order (PSO), intraparticle diffusion (IPD), and Boyd’s external diffusion (ED) models; these were subsequently compared based on their correlation coefficients (R2). The mathematical expressions for these kinetic models are summarized in Table 3 [2,18,29].
Table 3. Kinetic models.

2.5.3. Reuse Performance

The reusability of the adsorbent AAO + TT600 + PW was evaluated over four consecutive cycles, determining the removal efficiency (%R) at each stage. Each cycle consisted of an adsorption phase (16 mg·L−1 EBT, 500 rpm, 60 °C, 2 h) followed by regeneration via calcination at 600 °C, based on the procedure reported by Bitchatchi et al. [38]. However, to effectively remove the dye while minimizing structural changes or thermal stress in the AAO film, the calcination time was reduced from 4 h to 1 h. Furthermore, the pore-widening process was omitted in subsequent cycles, as repeated chemical etching with NaOH leads to the progressive dissolution of the oxide layer.”

3. Results

3.1. Characterization

3.1.1. SEM Analysis

Figure 1 illustrates the morphology of the AAO films anodized in a single step (0.3 M oxalic acid, 40 °C, 30 V), subjected to various treatments. The untreated samples (AAO, Figure 1a,b) exhibited disordered nanopores, which were preferentially oriented along manufacturing defects originating from the lamination process. Furthermore, at low magnification, cracks in the oxide film and poor pore-size homogeneity were observed.
Figure 1. SEM images of anodic aluminum oxide films with different treatments before and after EBT adsorption. AAO (a,b), AAO + EBT (c), AAO + 400TT (d), AAO + 600TT (e), AAO + PW (f,g), AAO + 400TT + PW (h,i) and AAO + 600TT + PW (j,k).
After EBT adsorption, the dye completely coated the oxide surface (Figure 1c). On the other hand, no significant morphological differences were observed for the AAO samples calcined at 400 and 600 °C for 4 h (Figure 1d,e).
The effect of pore widening on the anodized samples, with and without calcination, is shown in Figure 1f–k. Alkaline etching with NaOH for 1 min effectively dissolved the oxide layer and increased pore size. This dissolution was greatest for the uncalcined samples (AAO + PW), followed by the calcined samples AAO + 400TT + PW and AAO + 600TT + PW, respectively. In the first case, refined pores with rough terminations and significant fractures in the oxide layer were observed at low SEM magnifications (Figure 1f,g). In contrast, the 400 °C heat treatment applied before pore widening mitigated excessive dissolution of the oxide layer, resulting in a crack-free surface that retained the morphological characteristics of the AAO + PW samples (Figure 1h,i). Finally, the best pore widening was achieved in samples previously calcined at 600 °C, revealing a homogeneous surface with smooth, refined pores (Figure 1j,k).
The variation in pore diameter (PD) and porosity (P) of AAO films with different treatments is shown in Figure 2. For untreated samples, and those calcined at 400 and 600 °C, no significant differences in PD were found, with values between 25 and 40 nm (Figure 2a). Pore widening significantly increased PD to values close to 55 nm for the AAO and AAO + 400TT samples. In contrast, for the AAO + 600TT + PW samples, PD was lower (46 ± 6 nm).
Figure 2. Pore diameter (a) and porosity (b) of AAO films with different treatments.
As expected, the same trend in PD was observed for P (Figure 2b).

3.1.2. FTIR Analysis

The FTIR spectra obtained for AAO, AAO + 600TT, and AAO + 600TT + PW (Figure 3) show characteristic peaks in the 600–4000 cm−1 range, which define the surface chemical properties of the adsorbents. In all cases, a broad band was observed in the 3000–3700 cm−1 region, characteristic of ν(OH) stretching vibrations associated with the presence of Al-OH bonds, as well as peaks near 1640 cm−1 corresponding to bending vibrations of O-H groups [10,11,36,42,43,44].
Figure 3. FTIR spectrum of some of the synthesized AAO nanoadsorbents before EBT adsorption.
The peaks at 2340 cm−1 in the spectra of AAO + 600TT and AAO + 600TT + PW can be attributed to adsorbed CO2, arising from its weak interaction with coordinatively unsaturated tetrahedral Al3+ cations acting as Lewis acid sites [44,45].
Likewise, weak peaks can be observed in the 1000–1350 cm−1 region for the heat-treated samples, associated with the bending of the Al–O–H bond (for AAO + 600TT + PW) and indicating the presence of Al=O bonds (for AAO + 600TT) [46,47].

3.1.3. XRD Analysis

Figure 4 shows the X-ray diffraction (XRD) spectra of the AAO samples with and without annealing. The absence of peaks in the diffractogram of all samples indicates an amorphous structure.
Figure 4. XRD spectra of AAO without and with annealing at 400 and 600 °C for 4 h.

3.2. EBT Adsorption

3.2.1. Effect of AAO Treatments

The impact of the treatments applied to the AAO films on EBT adsorption is illustrated in Figure 5. In general, the dye removal efficiency (%R) curves over time exhibited similar behavior across all tested samples, with two distinct zones: (a) the high-speed region, characterized by a steep slope where the maximum %R values are rapidly approached, and (b) the steady-state region where equilibrium between adsorption and desorption is established and the %R remains constant. Notably, the maximum EBT removal (approximately 100%) was observed at 160 min across all cases.
Figure 5. EBT removal efficiency as a function of contact time for AAO adsorbents subjected to different treatments.
The maximum adsorption performance was achieved with nanoadsorbents subjected to both calcination (400–600 °C) and pore widening (PW), with no significant differences observed between their respective removal curves. The AAO + 400TT + PW and AAO + 600TT + PW samples reached removal efficiencies exceeding 90% after only 60 min of contact. In contrast, individual treatments (calcination or PW alone) showed a notable improvement over the untreated material, reaching values between 80% and 90% after 60 min of testing.
The applied treatments significantly enhanced the AAO adsorption performance, yielding a 38% increase in removal efficiency within 60 min. Although total EBT removal demands longer contact times, the treatment successfully accelerated the process, achieving >90% efficiency in only 1 h.

3.2.2. Adsorption Kinetics

Based on the aforementioned results, the kinetic study was conducted using the samples that exhibited the highest EBT removal performance, along with the untreated AAO sample for comparison purposes. Given that no significant differences were observed between the calcined and pore-widened specimens (AAO + 400TT + PW and AAO + 600TT + PW), the AAO + 600TT + PW sample was selected for further analysis.
Figure 6 displays the experimental curves of qt versus time for AAO and AAO + 600TT + PW. As shown, a stark contrast in adsorption behavior is evident between the two systems. The AAO + 600TT + PW trials demonstrate a markedly faster kinetic profile with a more pronounced initial slope, achieving equilibrium (qe = 0.0130 mg·cm−2) within roughly 50–60 min. On the other hand, the AAO process exhibits a smoother, gradual increase in its initial stage, delaying equilibrium until 140–150 min (qe = 0.0130 mg·cm−2). However, the final equilibrium adsorption capacity values remained similar for both materials.
Figure 6. Adsorption capacity as a function of time for the untreated AAO and AAO + 600TT + PW samples.
Figure 7 displays the experimental data fitted to the proposed linearized kinetic models. Additionally, Table 4 summarizes the values of the corresponding fitting parameters.
Figure 7. Linearized plots of the kinetic data fitted to various adsorption models (PFO, PSO, IPD, and ED) for: (a) untreated AAO and (b) AAO + 600TT + PW nanoadsorbents.
Table 4. Kinetic parameters of different adsorption models at 13 mg·L−1 initial EBT concentrations.
Based on the R2 fitting parameter, the AAO and AAO + 600TT + PW samples were better described by the pseudo-second-order model. Furthermore, the qe values predicted by this model were closer to the experimental qe values (qe exp.).
On the other hand, the experimental data analyzed via the IPD model revealed that the qt vs. t0.5 plot (Figure 7a,b) is non-linear and does not pass through the origin, confirming that the adsorption process is controlled by multiple steps. Consequently, the model was applied in multiple segments of the curve, identifying three stages for AAO and two for AAO + 600TT + PW. These results exhibit an excellent statistical fit, with coefficients of determination (R2) close to unity in all cases.
To complement these findings, the ED model results showed a good correlation for the AAO and AAO + 600TT + PW samples, with R2 close to unity. This demonstrates that mass transfer across the liquid boundary layer significantly influences the overall adsorption process.

3.2.3. Effect of pH

Figure 8a displays the EBT adsorption results at different pH levels using AAO and AAO + 600TT + PW. For the untreated AAO nanoadsorbent, the maximum removal efficiency was achieved under acidic conditions (90% at pH 4) and decreased inversely with increasing pH, reaching the lowest removal percentage at pH 10 (40%). Conversely, the AAO + 600TT + PW films exhibited maximum EBT removal at pH 6 (95%), with no statistically significant differences observed between pH 4 and 8, where removal remained around 85%. These findings confirm a noticeable enhancement in the adsorption capacity of AAO + 600TT + PW over untreated AAO, evidenced even at pH 10, where EBT removal increased by 20% in absolute terms.
Figure 8. Effect of pH on the adsorption of EBT on AAO and AAO + 600TT + PW (a) and the pH of point zero charge (pHpzc) of AAO + 600TT + PW (b).
Since the behavior of the AAO + 600TT + PW nanoadsorbent may be related to the surface charge of the oxide, its point of zero charge (pHpzc) was determined. According to Figure 8b, the pHpzc was 7.45. Therefore, the material surface becomes protonated and net-positively charged at pH < pHpzc, whereas deprotonation at pH > pHpzc yields a net negative charge. These results indicate that physisorption, mediated by electrostatic attractions, plays a decisive role in the process, although it is not the only mechanism involved in removal within this system.

3.2.4. Reusability

The reusability of the nanoadsorbent was evaluated using the treatment combination that exhibited the highest adsorptive efficiency (AAO 600TT + PW).
Figure 9 illustrates the results of four adsorption-regeneration cycles, where the EBT removal efficiency was quantified at the end of each stage. The findings indicate that post-adsorption calcination (600 °C, 1 h) effectively regenerated the adsorbent, enabling its reuse for up to four consecutive cycles in treating EBT-colored solutions while maintaining removal efficiencies above 80%.
Figure 9. Reuse cycles (adsorption + regeneration) for the AAO 600TT + PW.

4. Discussion

AAO films synthesized in 0.3 M oxalic acid at 40 °C and 30 V exhibited a remarkable enhancement in their adsorption capacity for EBT after undergoing thermal and chemical treatments. To evaluate this performance, the adsorption process was conducted under the identical conditions reported by Kramer et al. [29] (60 °C and 500 rpm). Although near-complete dye decolorization was achieved for all analyzed conditions after 160 min of contact time, the post-anodization treatments reduced the time required to achieve over 80% removal to just 1 h. Compared to the untreated material, this corresponds to a 10% increase in efficiency for both the individually calcined and chemically etched samples, and a 38% increase for the combined calcination and alkaline etching treatment.
To date, there are no published studies evaluating the potential of nanoporous AAO as an EBT adsorbent in its structural coating/film presentation (non-particulate form), with the sole exception of the work by Kramer et al. [29]. A key operational advantage of the present adsorbent film is that it eliminates the need for a post-treatment filtration or separation step, which is mandatory for particulate nanoadsorbents. When comparing EBT adsorption performance in aqueous solutions with literature benchmarks, the work of Gaayda et al. [11] reported removal efficiencies up to 71% (qe = 45 mg·g−1) in 100 min with C0 = 100 mg·L−1) using aluminum oxide nanoparticles. On the other hand, Ballou et al. [34] achieved an enhanced adsorption capacity (qe between 344 and 402 mg·g−1) utilizing pseudo-boehmite and gamma-alumina nanoparticles, reaching 100% removal efficiency in 20 min. Furthermore, while studies like the one by Afridi et al. [33] utilize a two-step anodization process to obtain highly ordered nanotubular structures (which allows the theoretical estimation of the adsorbent mass through empirical equations), our work focuses on an amorphous, non-ordered AAO matrix obtained via a simpler single-step process. Consequently, due to the structural nature of our film, the adsorption capacity is strictly reported per unit area (mg·cm−2), representing a more realistic and practical metric for structural coatings where geometric surface exposure governs the process rather than total mass.
The presence of EBT adsorbed on the oxide film was confirmed via SEM analysis after 2.7 h of treatment (Figure 1c). These findings are strongly supported by the study of Kramer et al. [29], who identified the presence of this same dye on the AAO film post-EBT adsorption using SEM, EDS, and FTIR under similar experimental conditions (C0 = 16 mg. L−1, 500 rpm, 25 °C, and 24 h).
The adsorption process is governed by factors such as the chemical nature and physical properties of the adsorbent–adsorbate system, the initial adsorbate concentration, the adsorbent dosage, temperature, agitation speed, and solution pH [1,3,13]. In this regard, the enhancements observed in the EBT removal capacity are primarily attributed to the morphological and chemical modifications induced by the post-anodization treatments.
Morphological characterization results (Figure 1) revealed significant differences in pore size, porosity, and homogeneity between the untreated and modified oxide films. Under identical anodic synthesis conditions, the AAO exhibited a pore diameter of 27 nm and a porosity of 21%, values that are consistent with those reported by Kramer et al. [29].
The pore-widening process increased the pore diameter and porosity by 38% for both calcined and uncalcined AAO samples, significantly enhancing the specific surface area of the nanoadsorbent. Consequently, the enhanced EBT adsorption capacity observed for the AAO + 400TT + PW and AAO + 600TT + PW samples can be attributed to the greater availability of active sites for interaction with the dye molecules, as well as an optimal pore diameter that favors molecular diffusion into the interior of the film. This cooperative mechanism between the porous structure and chemical active sites is consistent with recent findings by Gaudel et al. [48], who observed that enlarged pores act as fast-transport pathways for diffusion, while the ultimate retention efficiency is strictly governed by the functional groups of the modified surface.
On the other hand, the individual treatments applied to the AAO (either calcination or PW alone) exhibited similar dye removal efficiency profiles over time (Figure 5). The NaOH etching was more aggressive on the samples without prior calcination, inducing delamination, cracking, and a notably more irregular surface (Figure 1f,g). This excessive dissolution of the oxide layer accounts for the lower dye adsorption compared to that achieved with the combined (calcination + PW) treatment.
According to Chen et al. [49], thermal treatment of the films at low temperatures induces pore wall thickening via the diffusion of aluminum from the substrate and ambient oxygen, which combine to form additional alumina. This structural thickening, evidenced by a decrease in pore diameter, was not discernible for the AAO synthesized via a single-step anodization without pretreatment under the aforementioned conditions (Figure 1a vs. Figure 1d,e). However, the excessive dissolution of the oxide layer was prevented by applying a prior calcination step to stabilize the material, which is consistent with the findings reported by Kozhukhova et al. [50], yielding the optimal results at 600 °C (Figure 1j,k).
The enhanced adsorption capacity cannot be attributed to a structural transition of the aluminum oxide, given that the thermal treatments were conducted at temperatures below those required for the phase change (from amorphous to crystalline) [51]. According to Roslyakov et al. [52], increasing the temperature during thermal treatment involves several mass loss stages in the oxide film: thermal desorption of water is evident up to 300 °C, whereas the decomposition of aluminum hydroxide and oxalate compounds embedded in the matrix occurs between 300 and 800 °C. Nevertheless, no significant shifts were observed in the position of the amorphous halos for the analyzed samples to evidence such structural changes.
Conversely, although modifying the oxide structure is preferentially achieved using H3PO4 and, to a lesser extent NaOH solutions [39,53,54], preliminary studies revealed a significant decrease in the EBT adsorption capacity for samples treated with a 5 wt.% H3PO4 solution. This behavior is attributed to surface deactivation or contamination resulting from the presence of phosphate functional groups. Consequently, controlled treatment with dilute NaOH solutions and short exposure times constitutes a viable alternative to induce pore widening and increase the specific surface area of the film without compromising its EBT removal efficiency.
The FTIR spectroscopic results elucidate with greater clarity the relationship between surface chemistry, the applied treatments, and the enhancement of the adsorption process. The obtained spectra demonstrated an increase in functional groups, specifically those characteristics of the high-frequency region, as a function of the applied modifications. Within the 3000–3700 cm−1 range, the AAO + 600TT sample exhibited a lower intensity band, demonstrating an -OH absorbance peak decay consistent with severe thermal dehydration. Conversely, for the same range, the AAO + 600TT + PW sample displayed a more defined and intense -OH stretching band, which is directly attributed to the alkaline post-treatment [45,55]. Spectral variations within the 1000–1350 cm−1 region further propose a chemical evolution of the alumina surface depending on the post-synthesis treatment. For the AAO + 600TT sample, the severe thermal dehydroxylation at 600 °C removes bound water and surface hydroxyls, forcing the formation of stable, terminal Al=O bonds due to the high coordination unsaturation of the aluminum sites [46]. In contrast, for the AAO + 600TT + PW sample, the subsequent chemical etching with 0.5 N NaOH breaks these surface oxo-complexes during the pore-widening process. The alkaline medium and subsequent rinsing re-hydroxylate the newly exposed pore walls, leading to the re-emergence of the Al–O–H bending vibrations in this region. Additionally, the appearance of the peaks in the 2340–2366 cm−1 region for both the AAO + 600TT and AAO + 600TT + PW spectra is also directly related to the thermal treatment and the extensive dehydroxylation of the material. The removal of chemically bound water and surface -OH groups leave coordinatively unsaturated Al3+ ions exposed, which act as high-energy Lewis acid sites capable of interacting and weakly coordinating with CO2 (either atmospheric or entrapped) [45]. The persistence of these peaks even after the chemical etching with NaOH can be attributed to the nature of the pore-widening process; the dissolution of the oxide walls continually exposes fresh alumina layers, generating new unsaturated Al3+ sites along the expanded porous structure that remain available for weak gas coordination.
Consequently, the aforementioned findings demonstrate that the thermal and chemical treatments performed on the AAO modify its surface chemical properties, thereby promoting new physical and chemical interactions when exposed to dye aqueous solutions, and thus enhancing the overall adsorption process.
Based on the above, the enhanced EBT adsorption resulting from the thermal treatment of AAO at 600 °C is primarily driven by modifications in the surface chemistry of the adsorbent. In this case, the adsorbate-adsorbent interaction is promoted by the affinity between the surface Al3+ cations (acting as Lewis acids) exposed on the AAO + 600TT sample and the electron-donating groups (Lewis bases) inherent to the EBT molecules. Furthermore, for the AAO + 600TT + PW nanoadsorbent, the improvement in removal efficiency can be attributed to both the Lewis acid–base interactions at the remaining sites and the increase in specific surface area. This latter effect leads to a higher density of functional groups (such as hydroxyl groups) that favor the physisorption mechanism.
Experiments conducted at various pH levels demonstrated that the adsorption process is governed by the surface chemistry of the adsorbent and the nature of the adsorbate. Within this system, dye removal proceeds via a dual mechanism involving concurrent physisorption and chemisorption, in agreement with Kramer et al. [29].
Physisorption is primarily driven by electrostatic forces between the pH-dependent AAO surface and the anionic EBT dye. At pH values below the pHpzc, the AAO surface becomes protonated, which favors the electrostatic attraction of EBT. Conversely, at pH values above the pHpzc, surface deprotonation induces negative charges, resulting in electrostatic repulsion with the dye [11,33]. This behavior accounts for the decrease in EBT removal efficiency observed under alkaline pH conditions for both the AAO and AAO + 600TT + PW nanoadsorbents. Furthermore, it confirms that physisorption is the predominant mechanism for the untreated AAO.
Additionally, the medium’s pH alters the chemical structure of the EBT. Under alkaline conditions, EBT acts as a Lewis base due to the deprotonation of its neighboring phenolic hydroxyl groups, generating negatively charged oxygen atoms and lone electron pairs. Moreover, the high-electron-density –SO3H; –N=N–; and –NO2 groups act as donor sites capable of coordinating cations [56]. Concurrently, the AAO surface exhibits a Lewis acid character because the exposed, coordinatively unsaturated Al3+ sites possess vacant orbitals capable of accepting electrons [57,58]. This characteristic supports the occurrence of chemisorption within the overall EBT adsorption process, operating alongside the aforementioned physisorption pathway.
Finally, the higher EBT removal capacity of the AAO + 600TT + PW sample than that of untreated AAO within the pH range of 6–10 (Figure 8) is attributed to the increase in specific surface area induced by alkaline etching. This treatment enhances the exposure of Al3+ sites available for chemisorption, thereby making it the dominant mechanism over physisorption under these conditions [56].
Investigating adsorption kinetics is essential to elucidating the underlying mechanisms and determining the physicochemical characteristics governing the process [40]. As displayed in Figure 6, the modification process significantly accelerates the adsorption kinetics. The AAO sample exhibits a gradual increase in qt, whereas the AAO + 600TT + PW sample shows a remarkably steeper initial slope. This drastic reduction in equilibration time highlights that the thermal and chemical treatment protocol effectively minimized mass transfer resistance, allowing faster diffusion of the dye molecules into the active sites without compromising the ultimate adsorption capacity (qe ≈ 0.0130 mg·cm−2).
Since a satisfactory fit was achieved using the PSO model in both cases, the adsorption process is understood to be primarily controlled by chemisorption (chemical adsorbate/adsorbent reactions involving ion exchange, coordination, π-π interactions, and hydrogen bonding) or by the number of unoccupied adsorption sites on the adsorbent surface [59]. Comparing these AAO results with those obtained by Kramer et al. [29] indicates that increasing the operating temperature (from 25 to 50 °C) modifies the rate-limiting step, transitioning the adsorption mechanism from physisorption to chemisorption.
Concurrently, the IPD model fits demonstrated that the overall process rate is not solely controlled by intra-particle diffusion [20]. For the untreated AAO (Figure 7a) the classic sequential steps were observed [59,60]: the first segment represents the rapid diffusion of the dye through the liquid boundary layer or film and its adsorption onto surface active sites (kid = 0.0012 mg·cm−2·min−0.5), the second segment accounts for a slower intra-particle diffusion process through narrow pores (kid = 0.0004 mg·cm−2·min−0.5), and the third segment describes the adsorption/desorption reactions on the remaining active sites leading to equilibrium (kid = 0.0003 mg·cm−2·min−0.5). On the other hand, the IPD plots for AAO + 600TT + PW (Figure 7b) exhibited only two linear segments. In this system, the first segment represents highly accelerated diffusion through the liquid boundary layer (kid = 0.0018 mg·cm−2·min−0.5) combined with the occupation of the most accessible surface-active sites. The second segment represents intra-particle diffusion and the slower internal binding of dye molecules onto vacant sites, leading to saturation and equilibrium [11]. This abrupt change, lacking the intermediate segment observed in the untreated AAO, can be attributed to enhanced mass transfer and adsorption phenomena. These are likely facilitated by the structural and chemical modifications induced by the thermal treatment (i.e., increased porosity and surface chemical changes).
To conclusively validate the nature of the first kinetic segment in both systems, the Boyd film diffusion model was applied (Figure 7). The excellent linear correlation (R2 ≈ 1.0) obtained during the initial stages confirms that the diffusion of the adsorbate through the bounding liquid film was the main limiting step at the beginning of the process. [20,61]. Furthermore, the steeper slope observed in the Boyd plot for the AAO + 600TT + PW system corroborates that the structural and chemical modifications not only optimized the internal surface area but also affected the effective strength of the boundary liquid film.
The reusability of the AAO + 600TT + PW nanoadsorbent was demonstrated over four consecutive cycles, maintaining dye removal efficiencies above 85%. Adsorbent regeneration via post-adsorption calcination at 600 °C for 1 h successfully preserved the material’s adsorption capacity in subsequent runs. This performance contrasts with alternative regeneration methods, such as utilizing dilute NaOH solutions as an eluent for dye desorption [29,33]. The 10% decrease in removal efficiency observed from the second cycle onward can be attributed to subsequent calcinations, which alter the structural and chemical properties of the oxide film [38].

5. Conclusions

A substantial enhancement in the EBT adsorption capacity was achieved by subjecting AAO to combined thermal and chemical post-treatments. The combined treatment (AAO + 600TT + PW) increased pore diameter and porosity by 38%, improved EBT removal efficiency by 38% compared to untreated AAO, and reduced the time required for over 90% decolorization to just 1 h. Pre-calcination at 600 °C stabilized the amorphous matrix, preventing layer dissolution during alkaline etching and generating highly reactive, coordinately unsaturated Al3+ Lewis acid sites.
Adsorption follows a dual physisorption–chemisorption mechanism. The structural modifications minimized mass transfer resistance, shifting the rate-limiting step from intraparticle diffusion to film (boundary layer) diffusion. Under alkaline conditions (pH 6–10), the increased exposure of the Al3+ active sites allowed Lewis’s acid–base coordination (chemisorption) to become dominant, maintaining superior removal capabilities across a broad pH range.
Furthermore, the modified nanoadsorbent maintained a dye removal efficiency above 85% over four consecutive cycles of thermal regeneration, rendering these AAO films a robust alternative for treating colored effluents.

Author Contributions

Conceptualization, G.R.K., F.A.B., C.Y.P. and R.M.B.; methodology, G.R.K., F.A.B., R.M.B., C.Y.P., A.I.N. and L.C.D.; software, G.R.K. and F.A.B.; formal analysis, G.R.K. and F.A.B.; investigation G.R.K.; resources, A.E.A. and P.D.Z.; writing—original draft preparation, G.R.K. and F.A.B.; writing—review and editing, G.R.K. and F.A.B.; supervision, A.E.A. and P.D.Z.; project administration, A.E.A.; funding acquisition, A.E.A. and P.D.Z. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the Universidad Nacional de Misiones (16/Q2364-PI).

Institutional Review Board Statement

Not applicable.

Data Availability Statement

The data presented in this study are available on reasonable request.

Acknowledgments

G.R.K., F.A.B., P.D.Z. and A.E.A. appreciate the support provided by the Universidad Nacional de Misiones. All authors are grateful to the National Scientific CONICET (Consejo Nacional de Investigaciones Científicas y Técnicas).

Conflicts of Interest

The authors declare no conflicts of interest.

Abbreviations

The following abbreviations are used in this manuscript:
AAOAnodic Aluminum Oxide
EBTEriochrome Black T
PWPore Widening
PDPore Diameter
PPorosity
SEMScanning Electron Microscopy
FTIRFourier Transform Infrared Spectroscopy
XRDX-ray Diffraction
PFOPseudo First-Order Model
PSOPseudo Second-Order Model
IPDIntraparticle Diffusion Model
EDBoyd’s External Diffusion Model

References

  1. Solmaz, A.; Sari, Z.A.; Karta, M.; Turna, T.; Yücel, A.; Depci, T. Production and Characterization of Activated Carbon from Pomegranate Peel for Pharmaceutical Waste (Paracetamol) Removal: Response Surface Methodology Application. Water Air Soil Pollut. 2023, 234, 645. [Google Scholar] [CrossRef] [Scilit]
  2. Solmaz, A. Adsorption of Methylene Blue and Eriochrome Black T onto Pinecone Powders (Pinus Nigra Arn.): Equilibrium, Kinetics, and Thermodynamic Studies. Processes 2024, 12, 2044. [Google Scholar] [CrossRef] [Scilit]
  3. Rashid, R.; Shafiq, I.; Akhter, P.; Iqbal, M.J.; Hussain, M. A State-of-the-Art Review on Wastewater Treatment Techniques: The Effectiveness of Adsorption Method. Environ. Sci. Pollut. Res. 2021, 28, 9050–9066. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  4. Diorio, L.A.; Fréchou, D.M.S.; Levin, L.N. Removal of Dyes by Immobilization of Trametes Versicolor in a Solid-State Micro-Fermentation System. Rev. Argent. Microbiol. 2021, 53, 3–10. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  5. Hoppen, M.I.; Carvalho, K.Q.; Ferreira, R.C.; Passig, F.H.; Pereira, I.C.; Rizzo-Domingues, R.C.P.; Lenzi, M.K.; Bottini, R.C.R. Adsorption and Desorption of Acetylsalicylic Acid onto Activated Carbon of Babassu Coconut Mesocarp. J. Environ. Chem. Eng. 2019, 7, 102862. [Google Scholar] [CrossRef] [Scilit]
  6. De Luna, M.D.G.; Flores, E.D.; Genuino, D.A.D.; Futalan, C.M.; Wan, M.-W. Adsorption of Eriochrome Black T (EBT) Dye Using Activated Carbon Prepared from Waste Rice Hulls—Optimization, Isotherm and Kinetic Studies. J. Taiwan Inst. Chem. Eng. 2013, 44, 646–653. [Google Scholar] [CrossRef] [Scilit]
  7. Akhouairi, S.; Ouachtak, H.; Addi, A.A.; Jada, A.; Douch, J. Natural Sawdust as Adsorbent for the Eriochrome Black T Dye Removal from Aqueous Solution. Water Air Soil Pollut. 2019, 230, 181. [Google Scholar] [CrossRef] [Scilit]
  8. Zubair, M.; Jarrah, N.; Manzar, M.S.; Al-Harthi, M.; Daud, M.; Mu’azu, N.D.; Haladu, S.A. Adsorption of Erio-chrome Black T from Aqueous Phase on MgAl-, CoAl- and NiFe- Calcined Layered Double Hydroxides: Kinetic, Equilibrium and Thermodynamic Studies. J. Mol. Liq. 2017, 230, 344–352. [Google Scholar] [CrossRef] [Scilit]
  9. Sarkar, S.; Banerjee, A.; Halder, U.; Biswas, R.; Bandopadhyay, R. Degradation of Synthetic Azo Dyes of Textile Industry: A Sustainable Approach Using Microbial Enzymes. Water Conserv. Sci. Eng. 2017, 2, 121–131. [Google Scholar] [CrossRef] [Scilit]
  10. Khalid, A.; Zubair, M.; Ihsanullah. A Comparative Study on the Adsorption of Eriochrome Black T Dye from Aqueous Solution on Graphene and Acid-Modified Graphene. Arab. J. Sci. Eng. 2018, 43, 2167–2179. [Google Scholar] [CrossRef] [Scilit]
  11. El Gaayda, J.; Akbour, R.A.; Titchou, F.E.; Afanga, H.; Zazou, H.; Swanson, C.; Hamdani, M. Uptake of an Anionic Dye from Aqueous Solution by Aluminum Oxide Particles: Equilibrium, Kinetic, and Thermodynamic Studies. Groundw. Sustain. Dev. 2021, 12, 100540. [Google Scholar] [CrossRef] [Scilit]
  12. Kusumlata; Ambade, B.; Kumar, A.; Gautam, S. Sustainable Solutions: Reviewing the Future of Textile Dye Contaminant Removal with Emerging Biological Treatments. Limnol. Rev. 2024, 24, 126–149. [Google Scholar] [CrossRef] [Scilit]
  13. Ighalo, J.O.; López-Maldonado, E.A.; Igwegbe, C.A.; López López, J.R.; Méndez Herrera, P.F.; Egbosiuba, T.C.; Osaro, E.; Dulta, K.; Haskis, P.; Koulougliotis, D.; et al. A Comprehensive Review of the Adsorption of Eriochrome Black T (EBT) from Aqueous Solutions. Sustain. Chem. Environ. 2025, 12, 100299. [Google Scholar] [CrossRef] [Scilit]
  14. Gupta, V.K.; Kumar, R.; Nayak, A.; Saleh, T.A.; Barakat, M.A. Adsorptive Removal of Dyes from Aqueous Solution onto Carbon Nanotubes: A Review. Adv. Colloid Interface Sci. 2013, 193–194, 24–34. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  15. Abhinaya, M.; Parthiban, R.; Kumar, P.S.; Vo, D.-V.N. A Review on Cleaner Strategies for Extraction of Chitosan and Its Application in Toxic Pollutant Removal. Environ. Res. 2021, 196, 110996. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  16. Mittal, A.; Gupta, V.K. Adsorptive Removal and Recovery of the Azo Dye Eriochrome Black T. Environ. Toxicol. Chem. 2010, 92, 1813–1823. [Google Scholar] [CrossRef] [Scilit]
  17. Khan, A.; Ju, P.; Han, Z.; Ni, C. A Comprehensive Review on Adsorptive Removal of Azo Dyes Using Functional Materials. AQUA Water Infrastruct. Ecosyst. Soc. 2024, 73, 266–285. [Google Scholar] [CrossRef] [Scilit]
  18. Cavalcante, L.C.; De Carvalho, K.Q.; Bassetti, F.J.; Coral, L.A.A. Kinetic, Isothermal and Thermodynamic Studies of Reactive Black 5 Removal Using Rice Husk Ashes and Powdered Activated Carbon. Desalination Water Treat. 2024, 320, 100606. [Google Scholar] [CrossRef] [Scilit]
  19. Sardar, M.; Manna, M.; Maharana, M.; Sen, S. Remediation of Dyes from Industrial Wastewater Using Low-Cost Adsorbents. In Green Adsorbents to Remove Metals, Dyes and Boron from Polluted Water; Inamuddin, Ahamed, M.I., Lichtfouse, E., Asiri, A.M., Eds.; Environmental Chemistry for a Sustainable World; Springer International Publishing: Cham, Switzerland, 2021; Volume 49, pp. 377–403. [Google Scholar] [CrossRef] [Scilit]
  20. Wang, J.; Guo, X. Adsorption Isotherm Models: Classification, Physical Meaning, Application and Solving Method. Chemosphere 2020, 258, 127279. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  21. Kaur, Y.; Jasrotia, T.; Kumar, R.; Chaudhary, G.R.; Chaudhary, S. Adsorptive Removal of Eriochrome Black T (EBT) Dye by Using Surface Active Low Cost Zinc Oxide Nanoparticles: A Comparative Overview. Chemosphere 2021, 278, 130366. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  22. Jeong, S.; Kim, M.; Kim, J.; Kim, S. Evaluation of Iron Oxide and Aluminum Oxide as Potential Arsenic(V) Adsorbents. Chem. Eng. Process. 2007, 46, 1030–1039. [Google Scholar] [CrossRef] [Scilit]
  23. Roy, A.; Sharma, A.; Yadav, S.; Jule, L.T.; Krishnaraj, R. Nanomaterials for Remediation of Environmental Pollutants. Bioinorg. Chem. Appl. 2021, 2021, 1764647. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  24. Maurya, A.K.; Gogoi, R.; Manik, G. Polymer-Based Nanocomposites for Removal of Pollutants from Different Environment Using Catalytic Degradation. In Advances in Nanocomposite Materials for Environmental and Energy Harvesting Applications; Engineering Materials; Springer: Berlin/Heidelberg, Germany, 2022; pp. 331–368. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  25. Paneysar, J.S.; Jain, S.; Ahmed, N.; Barton, S.; Ambre, P.; Coutinho, E. Novel Smart Composite Materials for Industrial Wastewater Treatment and Reuse. SN Appl. Sci. 2020, 2, 1084. [Google Scholar] [CrossRef] [Scilit]
  26. Kamel, A.H.; Abd-Rabboh, H.S.M.; El-Fattah, A.A.; Stambouli, G.B.; Adeida, L. Metal Oxides and Their Composites for the Remediation of Organic Pesticides: Advanced Photocatalytic and Adsorptive Solutions. RSC Adv. 2025, 15, 6875–6901. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  27. Shanmugam, S.T.; Bukke, S.P.N.; Ravali, R.S.; Mavaluru, D.; Kumar, K.P.; Goruntla, N.; Gladys, T.M.; Ahikiriza, A.A. Graphene and its Derivative Biocomposites for Dye Adsorption. In Engineered Biocomposites for Dye Adsorption; Elsevier: Amsterdam, The Netherlands, 2026; pp. 163–176. [Google Scholar] [CrossRef] [Scilit]
  28. Crini, G.; Lichtfouse, E.; Wilson, L.D.; Morin-Crini, N. Conventional and Non-Conventional Adsorbents for Wastewater Treatment. Environ. Chem. Lett. 2019, 17, 195–213. [Google Scholar] [CrossRef] [Scilit]
  29. Kramer, G.R.; Bruera, F.A.; Zapata, P.D.; Ares, A.E. Aluminum Oxide Coatings as Nanoadsorbents for the Treatment of Effluents Colored with Eriochrome Black T. Coatings 2025, 15, 488. [Google Scholar] [CrossRef] [Scilit]
  30. Bruera, F.A.; Kramer, G.R.; Vera, M.L.; Ares, A.E. Synthesis and Morphological Characterization of Nanoporous Aluminum Oxide Films by Using a Single Anodization Step. Coatings 2019, 9, 115. [Google Scholar] [CrossRef] [Scilit]
  31. Bruera, F.A.; Kramer, G.R.; Vera, M.L.; Ares, A.E. Evaluation of the Influence of Synthesis Conditions on the Morphology of Nanostructured Anodic Aluminum Oxide Coatings on Al 1050. Surf. Interfaces 2020, 18, 100448. [Google Scholar] [CrossRef] [Scilit]
  32. Bruera, F.A.; Kramer, G.R.; Velázquez, J.E.; Sadañoski, M.A.; Fonseca, M.I.; Ares, A.E.; Zapata, P.D. Laccase Immobilization on Nanoporous Aluminum Oxide for Black Liquor Treatment. Surf. Interfaces 2022, 30, 101879. [Google Scholar] [CrossRef] [Scilit]
  33. Afridi, M.N.; Lee, J.; Kim, J.-O. Recovery of Phosphate from Wastewater Using Alumina Nanotubes. Desalination Water Treat. 2019, 144, 355–369. [Google Scholar] [CrossRef] [Scilit]
  34. Ballou, I.; Naja, J.; Bakher, Z.; Kholtei, S. Adsorption of Eriochrome Black T on Pseudo Boehmite and Gamma Alumina Synthesized from Drinking Water Treatment Sludge: A Waste-to-Recycling Approach. Recycling 2024, 9, 49. [Google Scholar] [CrossRef] [Scilit]
  35. Fernandes, E.P.; Silva, T.S.; Carvalho, C.M.; Selvasembian, R.; Chaukura, N.; Oliveira, L.M.T.M.; Meneghetti, S.M.P.; Meili, L. Efficient Adsorption of Dyes by γ-Alumina Synthesized from Aluminum Wastes: Kinetics, Isotherms, Thermodynamics and Toxicity Assessment. J. Environ. Chem. Eng. 2021, 9, 106198. [Google Scholar] [CrossRef] [Scilit]
  36. Sangor, F.I.M.S.; Al-Ghouti, M.A. Waste-to-Value: Synthesis of Nano-Aluminum Oxide (Nano-γ-Al2O3) from Waste Aluminum Foils for Efficient Adsorption of Methylene Blue Dye. Case Stud. Chem. Environ. Eng. 2023, 8, 100394. [Google Scholar] [CrossRef] [Scilit]
  37. Dwojak, L.C.; Kramer, G.R.; Zapata, P.D.; Bruera, F.A. Adsorption of Eriochrome Black T on Nanoporous Al2O3 Films Synthesized with Different Electrolytes. In Proceedings of the 9th Congress of Young Researchers in Materials (JIM 2025), Concepción del Uruguay, Argentina, 25–26 September 2025; Brühl, S., Ed.; Universidad Tecnológica Nacional: Ciudad Autónoma de Buenos Aires, Argentina, 2026; pp. 498–503. ISBN 978-950-42-0265-3. [Google Scholar]
  38. Bitchatchi, R.M.; Bruera, F.A.; Ares, A.E.; Kramer, G.R. Regeneration Performance of an Al2O3 Nanoadsorbent for the Treatment of Solutions with Eriochrome Black T. In Proceedings of the 9th Congress of Young Researchers in Materials (JIM 2025), Concepción del Uruguay, Argentina, 25–26 September 2025; Brühl, S., Ed.; Universidad Tecnológica Nacional: Ciudad Autónoma de Buenos Aires, Argentina, 2026; pp. 533–538. ISBN 978-950-42-0265-3. [Google Scholar]
  39. Hu, G.; Zhang, H.; Di, W.; Zhao, T. Study on Wet Etching of AAO Template. Appl. Phys. Res. 2009, 1, 78–82. [Google Scholar] [CrossRef] [Scilit]
  40. Li, N.; Li, X.; Yang, Y.; Liu, Y.; Zhao, L.; Zhou, Z. Adsorption-Desorption Behavior of Silver Ions on Stainless Steel as a Proxy for Disinfection of Domestic Hot Water. Desalination Water Treat. 2019, 151, 230–241. [Google Scholar] [CrossRef] [Scilit]
  41. Copello, G.J.; Villanueva, M.E.; González, J.A.; López Egües, S.; Diaz, L.E. TEOS as an Improved Alternative for Chitosan Beads Cross-linking: A Comparative Adsorption Study. J. Appl. Polym. Sci. 2014, 131, app.41005. [Google Scholar] [CrossRef] [Scilit]
  42. Jamhour, R.M.A.Q.; Al-Msiedeen, A.; Al-Faraheed, R.; Esaifan, M.; Jamhour, M. Adsorptive Removal of Hazardous Eriochrome Black T and Its Metal Complexes from Aqueous Media Using Spent Coffee Grounds. Res. Sq. 2023. epub ahead of printing. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  43. Atrak, K.; Ramazani, A.; Taghavi Fardood, S. Green Synthesis of Amorphous and Gamma Aluminum Oxide Nanoparticles by Tragacanth Gel and Comparison of Their Photocatalytic Activity for the Degradation of Organic Dyes. J. Mater. Sci. Mater. Electron. 2018, 29, 8347–8353. [Google Scholar] [CrossRef] [Scilit]
  44. Kusuma, K.B. Photocatalytic and Electrochemical Sensor for Direct Detection of Paracetamol Comprising γ-Aluminium Oxide Nanoparticles Synthesized via Sonochemical Route. Sens. Int. 2020, 1, 100039. [Google Scholar] [CrossRef] [Scilit]
  45. Szanyi, J.; Kwak, J.H. Dissecting the steps of CO2 reduction: 1. The interaction of CO and CO2 with γ-Al2O3: An in situ FTIR study. Phys. Chem. Chem. Phys. 2014, 16, 15117–15125. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  46. Naayi, S.A.; Hassan, A.I.; Salim, E.T. FTIR and X-Ray Diffraction Analysis of Al2O3 Nanostructured Thin Film Prepared at Low Temperature Using Spray Pyrolysis Method. Int. J. Nanoelectron. Mater. 2018, 11, 1–6. [Google Scholar]
  47. Rosa, D.; Rizzo, F.; Di Palma, L. Lime and pozzolan-based matrices for an efficient immobilization of hazardous waste. Chem. Eng. Sci. 2025, 313, 121735. [Google Scholar] [CrossRef] [Scilit]
  48. Gaudel, P.; Kandel, D.R.; Lee, J. In situ polymerization of PDA with the simultaneous incorporation of La-EDTA MOFs to endow poly-sulfone membranes with UF-level water permeance and NF-level lead removal efficiency. Sep. Purif. Technol. 2026, 396, 137801. [Google Scholar] [CrossRef] [Scilit]
  49. Chen, C.C.; Chen, J.H.; Chao, C.G. Post-Treatment Method of Producing Ordered Array of Anodic Aluminum Oxide Using General Purity Commercial (99.7%) Aluminum. Jpn. J. Appl. Phys. 2005, 44, 1529–1533. [Google Scholar] [CrossRef] [Scilit]
  50. Kozhukhova, A.E.; Du Preez, S.P.; Bessarabov, D.G. The Effects of Pore Widening and Calcination on Anodized Aluminum Oxide Prepared from Al6082. Surf. Coat. Technol. 2020, 383, 125234. [Google Scholar] [CrossRef] [Scilit]
  51. Mata-Zamora, M.E.; Saniger, J.M. Thermal evolution of porous anodic aluminas: A comparative study. Rev. Mex. Fis. 2005, 51, 502–509. [Google Scholar]
  52. Roslyakov, I.V.; Kolesnik, I.V.; Levin, E.E.; Katorova, N.S.; Pestrikov, P.P.; Kardash, T.Y.; Napolskii, K.S. Annealing induced structural and phase transitions in anodic aluminum oxide prepared in oxalic acid electrolyte. Surf. Coat. Technol. 2020, 381, 125159. [Google Scholar] [CrossRef] [Scilit]
  53. Sulka, G.D.; Brzózka, A.; Zaraska, L.; Jaskuła, M. Through-Hole Membranes of Nanoporous Alumina Formed by Anodizing in Oxalic Acid and Their Applications in Fabrication of Nanowire Arrays. Electrochim. Acta 2010, 55, 4368–4376. [Google Scholar] [CrossRef] [Scilit]
  54. Zaraska, L.; Sulka, G.D.; Jaskuła, M. Anodic Alumina Membranes with Defined Pore Diameters and Thicknesses Obtained by Adjusting the Anodizing Duration and Pore Opening/Widening Time. J. Solid State Electrochem. 2011, 15, 2427–2436. [Google Scholar] [CrossRef] [Scilit]
  55. Liu, X. DRIFTS study of surface of γ-alumina and its dehydroxylation. J. Phys. Chem. C 2018, 112, 5066–5073. [Google Scholar] [CrossRef] [Scilit]
  56. Tojiboyeva, F. Sorption–Spectroscopic Determination of Chromium (III) Ions Using Eriochrome Black T Immobilized on Silk Fibroin Fiber. Res. Sq. 2026. epub ahead of printing. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  57. Zaki, M.I.; Hasan, M.A.; Al-Sagheer, F.A.; Pasupulety, L. In situ FTIR spectra of pyridine adsorbed on SiO2–Al2O3, TiO2, ZrO2 and CeO2: General considerations for the identification of acid sites on surfaces of finely divided metal oxides. Colloids Surf. A Physicochem. Eng. Asp. 2001, 190, 261–274. [Google Scholar] [CrossRef] [Scilit]
  58. Busca, G. Catalytic materials based on silica and alumina: Structural features and generation of surface acidity. Prog. Mater. Sci. 2019, 104, 215–249. [Google Scholar] [CrossRef] [Scilit]
  59. Wang, C.; Liu, X.; Yang, T.; Sridhar, D.; Algadi, H.; Xu, B.B.; Guo, Z. An overview of metal-organic frameworks and their magnetic composites for the removal of pollutants. Sep. Purif. Technol. 2023, 320, 124144. [Google Scholar] [CrossRef] [Scilit]
  60. Ghibate, R.; Senhaji, O.; Taouil, R. Kinetic and thermodynamic approaches on Rhodamine B adsorption onto pomegranate peel. Case Stud. Chem. Environ. Eng. 2021, 3, 100078. [Google Scholar] [CrossRef] [Scilit]
  61. Ahmed, M.J.; Theydan, S.K. Microwave assisted preparation of microporous activated carbon from Siris seed pods for adsorption of metronidazole antibiotic. Chem. Eng. J. 2013, 214, 310–318. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.