Skip to Content
CoatingsCoatings
  • Feature Paper
  • Article
  • Open Access

26 May 2026

21 Pages

Ce-Mediated Second-Phase-Reconstruction-Coupled Regulation of Mechanical–Corrosion Properties of As-Cast 8021 Aluminum Alloy Billet for Battery Foil

,
,
,
and
1
Key Lab of Materials Physics, School of Physics, Zhengzhou University, Zhengzhou 450052, China
2
Henan Zhongfu Industrial Co., Ltd., No. 2 Yulian Industrial Park, Zhanjie Town, Zhengzhou 451261, China
3
Faculty of Engineering, Huanghe Science and Technology College, Zhengzhou 450006, China
*
Authors to whom correspondence should be addressed.

Highlights

  • Ce-mediated second-phase reconstruction serves as a feasible strategy to optimize the performance of as-cast 8021 aluminum alloy billet for battery foil.
  • The addition of 0.2 wt.% Ce induces dispersed Al–Ce–Fe ternary phases, realizing morphological transformation and dominant reconstruction of second phases.
  • A total of 0.2 wt.% Ce endows the alloy with optimal mechanical–corrosion synergy: elongation increases by 28.8%, and corrosion current density (icorr) decreases by one order of magnitude.

Abstract

To optimize the overall performance of as-cast 8021 aluminum alloy billets for power battery foil, this study explores how Ce addition (0–0.4 wt.%) regulates microstructure, mechanical properties, and corrosion resistance via second-phase reconstruction. Microstructure characterization, mechanical property testing and electrochemical corrosion tests were performed. The results show that Ce addition first refines, then stabilizes, and finally coarsens α-Al grains. The addition of 0.2 wt.% Ce promotes the formation of tentatively identified dispersed Al–Ce–Fe ternary phases, achieving the optimal combination of ductility (elongation: 42.7%) and strength (tensile strength: 95.0 MPa), as well as superior corrosion resistance (icorr = 2.79 × 10−7 Acm−2). Excessive Ce led to possible precipitation of the Al2Ce phase and grain coarsening, deteriorating alloy properties. In conclusion, 0.2 wt.% Ce is the optimal content to balance the microstructure, mechanical and corrosion properties of 8021 aluminum alloy, providing a theoretical basis for its compositional optimization of as-cast billet for battery foil applications.

1. Introduction

The rapid development of the new energy power battery industry imposes stringent requirements on the comprehensive performance of power battery aluminum foil, the core substrate for battery current collectors. Its ductility, strength, and microstructural uniformity directly determine battery energy density, cycle life, and operational safety [1,2,3]. As a typical Al–Fe–Si alloy, 8021 aluminum alloy is widely used for power battery foil due to its moderate strength, excellent formability, good corrosion resistance, and high electrolyte compatibility. Fe (1.0~1.5 wt.%) enhances thermal stability and recrystallization resistance to support high-temperature rolling. Low Si content adjusts electrical conductivity and work hardening behavior, satisfying the matching requirements of electrical and mechanical properties for current collectors.
However, as-cast 8021 alloy exhibits serious microstructural defects [4,5,6]: coarse and non-uniform α-Al grains, plus numerous coarse acicular or flaky Al–Fe intermetallics such as Al3Fe, Al6Fe, and Al13Fe4. These phases segregate along grain boundaries, breaking matrix continuity and acting as stress concentrators, resulting in poor strength–ductility balance. Problems such as cracking and wrinkling are prone to occur during rolling processing, which seriously restricts the yield and actual service performance of battery foils. To overcome these defects, researchers have proposed three main strategies [7,8,9,10,11,12,13]: casting process optimization, heat treatment, and microalloying modification. Among them, the addition of modifiers has become the mainstream scheme for industrial application due to its economic efficiency and remarkable modification effect. This study focuses on the as-cast billet of 8021 aluminum alloy, which is the key precursor material for battery foil. The modification of as-cast microstructure is fundamental to the rolling processability and final performance of battery foil.
In the application research of rare earth modifiers, elements such as Ce, Sr and Nd have all been used for the modification exploration of Al-Fe-Si series alloys [14,15,16,17,18]. But, there are essential differences in the modification effects and industrial adaptability of different rare earth elements. Sr is prone to burnout in high-temperature melts, and its modification effect is greatly affected by the fluctuation of the melting process, which cannot completely eliminate the coarse acicular Al-Fe phase [15]. The bonding ability between Nd and Fe is weak, resulting in a limited improvement in the morphology of the Al-Fe phase, and Nd resources are scarce with high raw material cost, which is not conducive to large-scale industrial application [19,20]. In contrast, the bonding affinity between Ce and Fe is much higher than that between Al and Fe. Ce-Al compounds (such as Al11Ce3) have a high melting point and a low lattice misfit with α-Al, which can not only serve as efficient heterogeneous nucleation cores to significantly refine the matrix grains, but also combine with Fe preferentially to form granular Al-Ce-Fe ternary phases, fundamentally replacing the coarse acicular Al-Fe binary phases [17]. At the same time, Ce has good chemical stability and a low high-temperature burnout rate, making its modification effect more stable and controllable. Existing studies have confirmed that the microstructure modification effect of Ce on Al-Fe-Si series alloys is superior to that of rare earth elements such as Sr and Nd [15,17,18,19,20,21,22,23]. However, for 8021 aluminum alloy dedicated to power battery foils, systematic conclusions are lacking regarding the quantitative regulation law of Ce content gradient on its grain size, second-phase morphology and composition, and the coupling regulation mechanism of microstructure evolution on mechanical properties (hardness, tensile strength, and elongation). There is also a lack of in-depth analysis of the intrinsic relationship between microstructure and properties, and the regulation law of Ce modification on the corrosion performance of the alloy has not been clarified, which is makes it difficult to outline the precise composition optimization of 8021 aluminum alloy for power battery foils.
Based on this, this study takes 8021 aluminum alloy for power battery foils as the research object and systematically investigates the effects of Ce addition (0~0.4 wt.%) on the alloy’s phase structure, α-Al grain size, and the evolution of second-phase morphology and composition. From the perspective of the synergy and competition of strengthening mechanisms, it analyzes how Ce regulates the alloy’s microhardness, tensile strength and elongation, and reveals the influence rule of Ce modification on its corrosion performance via electrochemical tests, ultimately determining the optimal Ce content balancing the alloy’s microstructure, mechanical properties and corrosion resistance. The study’s innovation lies in its in-depth exploration of Ce’s selective modification mechanism for the high-Fe and low-Si 8021 aluminum alloy, clarifying its regulation laws for Al-Fe phase transformation and second-phase reconstruction; it also establishes a quantitative contribution model for multiple strengthening mechanisms, uncovers the micro-mechanism of hardness–strength decoupling caused by excessive Ce and the regulation mechanism of Ce on corrosion performance, thus making up for the lack of in-depth correlation analysis of microstructure–mechanical–corrosion properties of Ce-modified 8021 aluminum alloy in the existing research and providing theoretical and technical support for its composition optimization and industrial application.

2. Materials and Methods

2.1. Alloy Preparation

The 8021 aluminum alloy was prepared by melting in a No. 12 graphite crucible using a 7.5 kW resistance furnace (Wanding Industrial Electric Furnace, Taizhou, China). The raw materials included industrial pure aluminum (99.7%), AlSi20, AlFe20, and AlCe20 master alloys. Before melting, raw materials and molds were preheated to 250 °C, and the graphite crucible was heated to dark red. The cut pure aluminum blocks were first added into the crucible and melted. When the temperature of the molten aluminum reached approximately 780 °C, the AlSi20, AlFe20, and AlCe20 master alloys were added into the melt batch by batch using a sampling spoon. After complete dissolution, refining flux was added, and argon gas was introduced with stirring for 5 min to remove inclusions and dissolved gas from the melt. Then, the dross on the melt surface was skimmed off. The melt was held and stabilized at about 720 °C for 15 min, and then poured into preheated molds for microstructure analysis and tensile specimens. The chemical composition of the alloy was analyzed using a Metalscan 2500 metal analyzer (Arun Ltd., West Sussex, UK). At least three points were tested on each specimen, and the average values were calculated. The measured chemical compositions of the alloys are presented in Table 1.
Table 1. Composition of 8021 aluminum alloy with different Ce contents (wt.%).

2.2. Microstructure Characterization

Samples for microstructure analysis were taken at a position 20 mm from the bottom of the cast samples. To ensure the accuracy of the analysis, all samples were taken from the same position of the cast ingots. The phase structure of the alloy was analyzed by a Bruker D8 ADVANCE X-ray diffractometer (XRD, Billerica, MA, USA). The XRD test conditions were as follows: Cu-Kα radiation was used for X-ray measurement with a wavelength of 1.54056 Å, the operating tube voltage and tube current were 40 kV and 40 mA, respectively, the scanning angle (2θ) was 20–100°, the scanning speed was 5°/min, and the scanning step was 0.02°. After the alloy samples were corroded with 0.5 vol.% HF aqueous solution, the macroscopic metallographic microstructure of the alloy was observed by an OLYMPUS DSX500 metallographic microscope (Olympus, Nagano, Japan) equipped with an image acquisition and analysis system. To obtain a metallographic structure with obvious contrast, clear grain boundaries and convenient grain size measurement, the above samples were subjected to anodic coating treatment with a DC stabilized power supply, and the specific process is shown in Table 2. The anodically coated samples were wiped clean with absolute ethanol and dried, then observed under the polarized light mode of an optical microscope. The average grain size of the alloy was counted by the artificial intercept method (GB/T6394-2002) on the metallographic structure observed by OM using the OLYCIA DSC software (version 4.2.1). The microstructure of the alloy and the morphology and composition of the second phases were analyzed by a Quanta 250 scanning electron microscope (SEM, FEI Company, Hillsboro, OR, USA) equipped with energy dispersive spectroscopy (EDS).
Table 2. Anodic coating process of 8021 aluminum alloy.

2.3. Mechanical Property Testing

The room temperature tensile properties of the samples were tested by an MTS810 universal mechanical testing machine (MTS Systems Corporation, Eden Prairie, MN, USA). According to the provisions of the national standard GB/T6397, the test samples were processed according to the tensile sample dimensions shown in Figure 1, and four sample bars were processed for each sample. The diameter was measured with a micrometer in two mutually perpendicular directions at the upper, middle and lower parts of the middle cylindrical part of the tensile sample bar, and the average value of these six measurements was taken as the diameter of the sample. The tensile test was carried out at a tensile rate of 1 mm/min, and the entire test process as well as the collection, processing and recording of data were automatically completed by the MTS application software (version 4.9). Four tensile strength data and elongation values were measured for each sample, and their average values were taken as the tensile strength and elongation of the sample. The fracture morphology of the tensile specimen was observed using SEM to analyze its fracture mechanism. The microhardness was measured by an HV-1000SPTA microhardness tester (Laizhou Weiyi Experiment Machine Manufacturing Co., Ltd., Yantai, China) (F = 9.8 N, T = 30 s), and each sample was measured 5 times, with the average value taken as the measured hardness. Average values and standard deviations were calculated from all valid parallel test data. Given the small difference and relatively large standard deviation in tensile strength, no significant statistical difference was identified among different Ce-containing alloys.
Figure 1. Schematic diagram of 8021 aluminum alloy room temperature tensile test bar.

2.4. Electrochemical Corrosion Testing

Potentiodynamic polarization curves and electrochemical impedance spectroscopy (EIS) of different samples were tested using a CHI660E electrochemical workstation (Shanghai Chenhua Instrument Co., Ltd., Shanghai, China) with a conventional three-electrode system, where a platinum sheet served as the counter electrode, a saturated calomel electrode (SCE) as the reference electrode, and the tested sample as the working electrode. A Luton chemical sample holder was used to fix the working electrode and control the exposed test area of 1 cm2. The corrosive medium was 3.5 wt.% NaCl solution. The 3.5 wt.% NaCl solution is used as a general chloride corrosion screening medium for aluminum alloys, which is widely adopted to characterize pitting corrosion sensitivity and micro-galvanic corrosion behavior. It is employed here for relative performance comparison rather than simulating the real service environment of battery foil. Prior to testing, the samples were immersed in the solution for 30 min until the open-circuit potential stabilized. For potentiodynamic polarization measurements, the scan rate was 1 mV/s with a potential range of −0.2~0.6 V (vs. SCE). For EIS tests, the frequency range was 105~10−2 Hz with a sinusoidal excitation signal amplitude of 5 mV. All tests were conducted at room temperature and repeated three times to ensure data reliability. Origin software (Origin 2022) was used to fit the Tafel region of polarization curves for obtaining corrosion potential and corrosion current density, while ZSimpWin software (version 3.60) was applied to fit EIS data with equivalent circuits for extracting electrochemical parameters, thereby analyzing the corrosion resistance differences and corrosion kinetic laws of different samples. The equivalent circuit model Rs(Qf(Rf(QRp))) was employed to fit the EIS data. This model reflects the typical electrochemical interface of aluminum alloys in chloride solution, which includes a surface passive film and a charge transfer process, corresponding to two time constants. This circuit is widely used and well recognized for aluminum alloys suffering from pitting corrosion in neutral NaCl media. Notably, the model was selected based on its physical rationality and consistency with the actual corrosion interface, rather than fitting quality alone.

3. Results and Discussion

3.1. Microstructure Evolution and Regulatory Mechanism

3.1.1. Phase Structure Evolution

Figure 2 shows the XRD diffraction patterns of 8021 aluminum alloy with different Ce contents. In the Al-Ce0 sample, diffraction peaks match α-Al and Al13Fe4 (2θ = 45.8°, 66.8°). No other Al–Fe binary phases are observed, indicating that the Al-Fe phase in as-cast 8021 aluminum alloy mainly exists in the form of the Al13Fe4 phase, which is consistent with the phase characteristics of as-cast Al-Fe-Si series alloys [5]. When the Ce content increases to 0.1~0.2 wt.%, the intensity of the characteristic diffraction peak of the Al13Fe4 phase decreases gradually, the characteristic diffraction peaks of the Al6Fe phase appear at 2θ = 38.2° and 44.5° at the same time, and the intensity increases continuously with the increase in Ce content, indicating that Ce addition may induce the crystal phase transformation of the Al-Fe phase from Al13Fe4 to Al6Fe. No characteristic peak of Al2Ce phase is detected in this stage, which confirms that Ce preferentially participates in the transformation process of the Al-Fe phase within this Ce content range [17].
Figure 2. XRD patterns of 8021 aluminum alloy with different Ce contents: (a) 20–100°; (b) 42–46°.
The essence of this phase transformation process is that the bonding affinity of Ce with Fe is much higher than that of Al with Fe, and the calculation based on the EET theory also confirms that the bonding strength in the Al–Fe–Ce system is significantly higher than that in Al–Fe. Ce atoms are easy to adsorb on the grain boundaries of the Al13Fe4 phase and they destroy its lattice stability; at the same time, they form Al-Ce-Fe ternary intermediate phases such as Al8Fe4Ce and Al10Fe2Ce, which can serve as heterogeneous nucleation cores of the Al6Fe phase to further promote the phase transformation process [24]. When the Ce content is 0.2 wt.%, the characteristic peak of the Al13Fe4 phase almost disappears, and the Al6Fe phase becomes the main Al-Fe binary phase; when the Ce content further increases to 0.3~0.4 wt.%, the characteristic diffraction peaks of the Al2Ce phase appear at 2θ = 33.6° and 47.8° in the diffraction pattern, and the peak intensity increases significantly with the increase in Ce content, while the diffraction peak intensities of the α-Al matrix and Al6Fe phase have no obvious change, indicating that excessive Ce may react with Al to precipitate Al2Ce binary compounds. This process has a clear sequence and causal relationship with the Ce-induced Al13Fe4→Al6Fe transformation [17].
Combined with thermodynamic calculation, it can be known that, in the Al-Fe-Ce system, the Gibbs free energy of formation of Al6Fe and Al-Fe-Ce ternary phases is lower than that of Al13Fe4 and Al2Ce, so the Al13Fe4→Al6Fe transformation occurs preferentially after Ce addition. Only when Fe is consumed to saturation by Ce and Ce is surplus do the Ce atoms not involved in the formation of ternary phases segregate at the grain boundaries and combine with Al atoms to form the high-melting-point Al2Ce phase [24]. When the Ce content reaches 0.4 wt.%, the intensity of the characteristic peak of the Al2Ce phase reaches the maximum value, indicating that the precipitation amount of the Al2Ce phase at the grain boundaries reaches its peak at this time.

3.1.2. Quantitative Regulation of Metallographic Structure and Grain Size

Figure 3 shows the microstructural evolution of as-cast 8021 aluminum alloys with different Ce additions. The Ce-free alloy (Al-Ce0) exhibits coarse non-uniform dendritic α-Al cells with indistinct and discontinuous intercellular boundaries. As the Ce content increases to 0.2 wt.%, the dendritic structure is significantly refined, and the primary α-Al cells gradually transform into finer, more uniform and equiaxed-like morphologies with clearer and more continuous intercellular boundaries. In the range of 0.2–0.3 wt.% Ce, the refined dendritic structure remains relatively stable. When the Ce content further increases to 0.4 wt.%, secondary coarsening of the primary α-Al cells occurs, accompanied by the reappearance of coarse columnar dendrites, severe segregation of intergranular phases, and a marked deterioration in microstructural uniformity.
Figure 3. Metallographic photos of 8021 aluminum alloy with different Ce contents: (a) Al-Ce0; (b) Al-Ce1; (c) Al-Ce2; (d) Al-Ce3; (e) Al-Ce4.
Quantitative grain size analysis via anodic coating metallography (Figure 4 and Figure 5) confirms this trend. Al-Ce0 shows irregular poorly defined grains with an average size of ~85 μm. Adding 0.1 wt.% Ce sharpens boundaries, refines grains to 82 μm, and improves uniformity. At 0.2 wt.% Ce, grains reach the optimum state: fully equiaxed, clear boundaries, and an average size of 78 μm. At 0.3 wt.% Ce, grain size stays stable at 78–80 μm. At 0.4 wt.% Ce, boundaries blur, grains coarsen to 83 μm, and uniformity degrades. Overall, Ce tunes α-Al grain size in a refine–stabilize–coarsen sequence, synchronized with second-phase evolution. Low Ce (≤0.2 wt.%) forms Al-Ce-Fe ternary phases that act as potent heterogeneous nucleants to refine grains. At 0.2–0.3 wt.% Ce, dispersed ternary phases pin grain boundaries and stabilize grain size. Excess Ce (0.4 wt.%) precipitates Al2Ce phases that segregate at boundaries, disrupt continuity, weaken pinning, raise grain boundary energy, and trigger re-coarsening.
Figure 4. Metallographic photos of anodic coating of 8021 aluminum alloy with different Ce contents: (a) Al-Ce0; (b) Al-Ce1; (c) Al-Ce2; (d) Al-Ce3; (e) Al-Ce4.
Figure 5. Statistical results of grain size of 8021 aluminum alloy with different Ce contents.

3.1.3. Reconstruction Law of Second-Phase Morphology and Composition

Due to the low overall volume fraction of second phases in 8021 aluminum alloy, quantitative phase analysis via Rietveld refinement or area fraction statistics cannot be reliably performed. Therefore, the evolution of second phases is described based on qualitative XRD and SEM/EDS evidence. Combined with the XRD phase analysis and grain size quantitative characterization results, the regulation of Ce content on the microstructure of 8021 aluminum alloy is reflected not only in the evolution characteristics of α-Al grains of first refinement and then stabilization and subsequent coarsening, but also in the systematic reconstruction of the morphology, composition and distribution of second phases through phase transformation, and the evolution law of second phases has a clear synergy with the changes in grain structure. To further analyze the fine morphology and composition characteristics of the second phases induced by Ce and reveal the internal correlation between phase transformation and grain regulation, a Quanta 250 scanning electron microscope equipped with energy dispersive spectroscopy (EDS) was used to observe the alloys with different Ce contents, and the chemical composition of the second phases was analyzed in combination with point scanning and surface scanning. The results are shown in Figure 6, Figure 7, Figure 8, Figure 9 and Figure 10. EDS compositions of points B-F are listed in Table 3.
Figure 6. SEM image and EDS results of Al-Ce0 alloy: (a) low-magnification image; (b) high-magnification image; (c) map scanning image of Al; (d) map scanning image of Fe; (e) map scanning image of Si; (f) EDS results of point A.
Figure 7. SEM image and EDS results of Al-Ce1 alloy: (a) low-magnification image; (b) high-magnification image and EDS results of point B; (c) map scanning image of Al; (d) map scanning image of Fe; (e) map scanning image of Si; (f) map scanning image of Ce.
Figure 8. SEM image and EDS results of Al-Ce2 alloy: (a) low-magnification image; (b) high-magnification image and EDS results of point B; (c) map scanning image of Al; (d) map scanning image of Fe; (e) map scanning image of Si; (f) map scanning image of Ce.
Figure 9. SEM image and EDS results of Al-Ce3 alloy: (a) low-magnification image; (b) high-magnification image and EDS results of point B; (c) map scanning image of Al; (d) map scanning image of Fe; (e) map scanning image of Si; (f) map scanning image of Ce.
Figure 10. SEM image and EDS results of Al-Ce4 alloy: (a) low-magnification image; (b) high-magnification image and EDS results of point B; (c) map scanning image of Al; (d) map scanning image of Fe; (e) map scanning image of Si; (f) map scanning image of Ce.
Table 3. EDS compositional results (wt.%) for points B, C, D, E, and F in Figure 7, Figure 8, Figure 9 and Figure 10.
As revealed by SEM and EDS observations (Figure 6), the Ce-free Al-Ce0 alloy mainly contains coarse acicular and flaky Al13Fe4 second phases with a size range of 10–20 μm. These phases distribute continuously and semi-continuously along grain boundaries, splitting the α-Al matrix, while some scattered acicular phases also exist inside grains. EDS and XRD suggest that these second phases are composed only of Al and Fe with an atomic ratio close to that of Al13Fe4, and Si is uniformly distributed as a solid solution in the matrix without participating in second-phase formation. After adding 0.1 wt.% Ce (Al-Ce1), the coarse Al13Fe4 phases begin to transform morphologically: needle-like phases break into short rods of 5–10 μm, and fine granular phases precipitate at grain boundaries and inside grains (Figure 7). EDS mapping and point scanning show that these new particles contain Al, Fe, and Ce, with obvious Ce enrichment, indicating the formation of Al–Ce–Fe ternary phases. This confirms that Ce preferentially binds with Fe and triggers the phase transformation of Al–Fe compounds [17]. Si remains in solid solution, and the newly formed ternary phases act as heterogeneous nucleation cores, providing a key microstructural basis for grain refinement.
At a Ce content of 0.2 wt.% (Al-Ce2), XRD results show that Al13Fe4 peaks nearly disappear and Al6Fe likely becomes the dominant Al–Fe binary phase. The second phases undergo a fundamental change: coarse acicular phases are almost completely replaced by uniformly dispersed granular Al–Ce–Fe ternary phases of 0.5–2 μm (Figure 8). EDS at point C gives stable composition ratios of Al, Fe, and Ce, and elemental mapping confirms the consistent distribution of Ce and Fe in these granular phases. The dispersed ternary phases eliminate the matrix-splitting effect and pin grain boundaries effectively, stabilizing grain size at an optimal level. When Ce increases to 0.3 wt.% (Al-Ce3), the phase composition and morphology remain unchanged; the fine ternary particles maintain 0.5–2 μm without agglomeration (Figure 9). EDS at point D shows slightly higher Fe and lower Ce, indicating saturated Ce–Fe combination and stable phase equilibrium. With Ce further increased to 0.4 wt.% (Al-Ce4), XRD detects strong Al2Ce diffraction peaks (Figure 10). The microstructure exhibits a dual-phase feature: intergranular Al–Ce–Fe ternary phases and intragranular blocky Al2Ce binary phases. EDS tentatively identifies blocky Al–Ce phases inside grains and granular Al–Ce–Fe phases at boundaries. After Fe is fully consumed, excess Ce reacts with Al to form Al2Ce, which destroys matrix uniformity, weakens grain-boundary pinning, and causes secondary grain coarsening and deteriorated homogeneity. Si remains uniformly dissolved in the α-Al matrix in all conditions.

3.2. Mechanical Properties

3.2.1. Mechanical Property Evolution

Room temperature tensile properties and microhardness tests were carried out on 8021 aluminum alloy with different Ce contents; the stress–strain curves are shown in Figure 11, and the quantitative test results of tensile strength, elongation and microhardness are shown in Table 4. Ce content clearly regulates mechanical properties: ductility first increases and then slightly decreases; tensile strength decreases slightly then rebounds; microhardness first drops then rises continuously.
Figure 11. Room temperature tensile stress–strain curves of 8021 aluminum alloy with different Ce contents.
Table 4. Mechanical properties of 8021 aluminum alloy with different Ce contents.
The Al-Ce0 sample exhibits high strength but limited ductility, with a tensile strength of 97.0 MPa, an elongation of 35.4%, and a microhardness of 41.6 HV. This behavior is attributed to the matrix-splitting effect induced by coarse acicular Al13Fe4 intermetallic phases and the non-uniform coarse α-Al grains in the as-cast microstructure. As the Ce content increases to 0.2 wt.% (Al-Ce2), the ductility is significantly enhanced to an optimal level, with the elongation reaching 42.7% (an increase of 20.9% compared with Al-Ce0). Meanwhile, the tensile strength (95.0 MPa) and microhardness (40.0 HV) show only minor fluctuations without obvious degradation, achieving an excellent strength–ductility synergy. With the Ce content further increasing beyond 0.2 wt.%, the elongation continues to rise gradually to 43.4% (Al-Ce3) and, finally, 45.0% (Al-Ce4), indicating a continuous improvement in ductility. Meanwhile, the microhardness increases continuously and significantly, reaching a peak of 45.7 HV at 0.4 wt.% Ce. The tensile strength first decreases to a minimum value of 91.9 MPa at 0.3 wt.% Ce, followed by a slight rebound to 92.9 MPa at 0.4 wt.% Ce. Due to the relatively small variation range and large standard deviation of tensile strength, the difference in tensile strength among these alloys is not statistically significant.

3.2.2. Tensile Fracture Morphology

Figure 12 presents the room temperature tensile fracture morphologies of 8021 aluminum alloys modified with different Ce contents. The fracture features evolve systematically with microstructural changes, revealing a clear transition in fracture mechanism. The unmodified alloy presents a relatively low-ductility fracture mode with shallow and sparse dimples and local quasi-cleavage features, showing relatively poor overall ductility. Coarse acicular Al13Fe4 phases severely disrupt the matrix, act as preferential crack initiation sites, and promote rapid intergranular crack propagation, resulting in high strength but limited ductility. With a low Ce addition, cleavage characteristics are significantly weakened, and shallow dimples begin to appear, indicating a mixed ductile–brittle fracture mode. Grain refinement and morphological transformation of Al–Fe phases reduce stress concentration, thereby improving plasticity while slightly reducing strength and hardness. Upon moderate Ce alloying, the fracture surface is fully covered by uniform, fine, and deep dimples, representing typical ductile fracture corresponding to the best ductility. Coarse acicular phases are almost entirely replaced by finely dispersed Al–Ce–Fe ternary particles that eliminate the matrix splitting effect, impede dislocation motion, and induce crack deflection and passivation. In this condition, the alloy presents the best comprehensive performance with significantly improved ductility and satisfactory strength. With a further increase in Ce, the fracture remains predominantly ductile, although dimple density decreases slightly. The uniformly distributed ternary phases remain stable, sustaining both grain refinement and dispersion strengthening. The Ce–Fe reaction reaches saturation, and the elevated Fe fraction in the ternary phase enhances dispersion hardening and raises hardness, whereas the loss of phase hindrance strengthening causes tensile strength to decline to a minimum. Excessive Ce leads to slightly coarser and shallower dimples, accompanied by a minor drop in ductility. Precipitation of blocky Al2Ce phases and grain coarsening exert adverse effects; yet, the remaining dispersed Al–Ce–Fe ternary phases effectively maintain acceptable ductility. The hard and brittle Al2Ce phases significantly increase hardness, but discontinuous grain boundaries limit strength improvement, leading to obvious hardness–strength decoupling.
Figure 12. Room temperature tensile fracture morphology of 8021 aluminum alloy with different Ce contents: (a) Al-Ce0; (b) Al-Ce1; (c) Al-Ce2; (d) Al-Ce3; (e) Al-Ce4.

3.2.3. Core Mechanism of Microstructure Property Correlation

The evolution of α-Al grain size and the morphological transformation and composition reconstruction of second phases are the key microscopic factors regulating the mechanical properties of 8021 aluminum alloy. The alloy strength is jointly determined by the synergy and competition of grain refinement strengthening ( σ H P ), phase hindrance strengthening ( σ p h ) and dispersion strengthening ( σ O r o w a n ). Based on the classic strengthening theory of aluminum alloy, a multi-mechanism strength superposition model ( σ b = σ 0 + σ H P + σ O r o w a n + σ p h ), Hall–Petch grain refinement strengthening formula ( σ H P = k y · d − 1 2 ) and Orowan dispersion strengthening formula ( σ O r o w a n = 0.4 M μ b 2 π 1 − ν · l n ( 2 r b ) λ ) were used for qualitative interpretive framework for strengthening mechanisms, and the selection of relevant parameters was consistent with the literature reports of Al-Fe-Si series alloys [5,25]. On this basis, combined with the change law of grain size and mechanical properties shown in Figure 13 and the relative contribution ratio of each strengthening mechanism given in Figure 14, the intrinsic correlation between microstructure and properties was systematically analyzed.
Figure 13. Relationship between α-Al grain size and tensile properties (a) and microhardness (b) of 8021 aluminum alloy with different Ce contents.
Figure 14. Schematic relative contribution ratios of various strengthening mechanisms in 8021 aluminum alloy with different Ce additions.
In the above formulas, σ b is the actual tensile strength of the alloy (MPa), measured by a room temperature tensile test; σ 0 is the intrinsic strength of the 8021 aluminum alloy matrix, taking a constant value of 45 MPa; σ H P is the contribution strength of Hall–Petch grain refinement strengthening (MPa); σ O r o w a n is the contribution strength of Orowan dispersion strengthening (MPa), provided by the dispersed second phases; and σ p h is the contribution strength of phase hindrance strengthening (MPa). This strengthening effect is only provided by the as-cast coarse acicular Al-Fe phases, and the contribution of granular Al–Ce–Fe and Al2Ce phases to phase hindrance strengthening is greatly reduced. k y is the Hall–Petch constant of 8021 aluminum alloy, 60 MPa·μm1/2; d is the average equivalent diameter of α-Al grains (μm), measured and counted by anodic coating metallography; M is the Taylor factor of dislocation slip system, taking the general value of aluminum alloy of 3.06; μ is the shear modulus of aluminum alloy, taking the general value of Al at room temperature of 26 GPa; b is the dislocation Burgers vector of Al atoms, taking the general value of 0.286 nm; ν is the Poisson’s ratio of Al, taking the general value of 0.33; r is the average particle size of dispersed second phases (μm); and λ is the average spacing between second phases (μm), both of which are measured and counted by SEM-EDS.
It can be seen from Figure 13 that the Ce addition amount has a significant regulatory effect on the grain size and mechanical properties of 8021 aluminum alloy and presents obvious stage characteristics. Within the range of 0~0.2 wt.% Ce, the α-Al grains are refined from 85 μm to 78 μm and the elongation is significantly increased from 35.4% to 42.7%, while the strength and hardness decrease slightly, showing the characteristics of reverse change between plasticity and strength. When the Ce content is in the range of 0.2~0.3 wt.%, the grain size tends to be stable, the plasticity decreases slightly but still maintains a high level, the hardness increases significantly, and the strength decreases to the lowest value; the alloy achieves a relatively excellent matching between strength and plasticity. When the Ce content is further increased to 0.4 wt.%, the grains coarsen to a certain extent, the plasticity remains basically stable, the hardness is greatly improved, and the strength rebounds slightly, showing typical hardness–strength decoupling behavior.
Figure 14 illustrates the schematic relative contributions of strengthening mechanisms in Ce-modified 8021 aluminum alloy. Ce addition substantially alters the dominant strengthening modes. In the Ce-free alloy, phase hindrance strengthening dominates (60%), followed by grain refinement strengthening (40%), with no effective dispersion strengthening. As Ce increases to 0.1 wt.%, phase hindrance strengthening declines rapidly, while grain refinement and dispersion strengthening rise accordingly. At 0.2–0.3 wt.% Ce, phase hindrance strengthening vanishes, and grain refinement (55%) and dispersion strengthening (45%) become the synergistic main mechanisms. With further Ce addition to 0.4 wt.%, grain refinement strengthening decreases slightly, and dispersion strengthening increases to 50% due to grain coarsening and Al2Ce precipitation.
Ce modification transforms the dominant strengthening mechanism from phase hindrance into a synergy of grain refinement and dispersion strengthening, which agrees well with microstructural and property evolution. Three stages are identified: low Ce enhances plasticity but slightly reduces strength; moderate Ce stabilizes the microstructure and achieves optimal strength–ductility balance; and excessive Ce causes hardness–strength decoupling owing to Al2Ce precipitation and grain coarsening. Grain size dominates ductility, while the combined strengthening effects control strength, and 0.2 wt.% Ce is confirmed as the optimum addition.

3.3. Corrosion Behavior

3.3.1. Potentiodynamic Polarization

The potentiodynamic polarization curves of 8021 aluminum alloys with different Ce additions in 3.5% NaCl solution are shown in Figure 15, and the fitting results of electrochemical characteristic parameters such as corrosion potential (Ecorr) and corrosion current density (icorr) are presented in Table 5. The Al-Ce0 alloy exhibited a corrosion potential Ecorr of −0.70 V and corrosion current density icorr of 4.69 × 10−6 Acm−2, owing to the disruptive effect of coarse acicular Al13Fe4 phases. With 0.1~0.2 wt.% Ce, Ecorr shifted slightly negative, while icorr of Al-Ce2 decreased to 2.79 × 10−7 Acm−2 (nearly one order of magnitude lower), indicating significantly suppressed corrosion kinetics. With Ce > 0.2 wt.%, Ecorr shifted positive, but icorr increased sharply to 1.17 × 10−5 Acm−2 for Al-Ce4, indicating serious degradation of corrosion resistance. The above results confirm that appropriate Ce addition (0.1~0.2 wt.%) improves the corrosion resistance of 8021 aluminum alloy, while excessive Ce degrades it, and this trend is mainly evidenced by the variation of corrosion current density.
Figure 15. Potentiodynamic polarization curves of 8021 aluminum alloys with different Ce additions in 3.5% NaCl solution.
Table 5. Electrochemical parameters of 8021 aluminum alloys with different Ce additions.

3.3.2. Electrochemical Impedance Spectroscopy (EIS) Analysis

The EIS test results of 8021 aluminum alloys with different Ce additions in 3.5 wt.% NaCl solution are shown in Figure 16, and the corresponding fitting parameters are presented in Table 6. The equivalent circuit Rs(Qf(Rf(QRp))) was employed to fit the data, where Rs denotes solution resistance, Qf and Rf represent the surface film properties, and Q and Rp correspond to the electric double layer. All fittings exhibited high reliability with χ2 values in the order of 10−3. Nyquist plots displayed two capacitive arcs: the high-frequency arc reflects the surface film impedance, while the low-frequency arc represents the charge transfer process. Larger arc diameters indicate higher corrosion resistance. The arc diameter was largest for Al-Ce2 and smallest for Al-Ce4, with Al-Ce0, Al-Ce1, and Al-Ce3 in between, which is consistent with polarization results. Bode plots further verified these trends: the low-frequency impedance modulus |Z| was highest for Al-Ce2 and lowest for Al-Ce4. In phase–angle curves, Al-Ce2 showed the highest and broadest peak (nearly 80°), indicating a compact and protective passive film, whereas Al-Ce4 exhibited a lower peak (≈65°) shifted to high frequencies, suggesting a loose and defective layer.
Figure 16. EIS results of 8021 aluminum alloys with different Ce additions in 3.5 wt.% NaCl solution: (a) Nyquist plots; (b) Bode modulus plots; (c) Bode phase angle plots; (d) fitted equivalent circuit.
Table 6. EIS fitting parameters of 8021 aluminum alloys with different Ce additions.
Film resistance Rf served as the key indicator of surface protection: Al-Ce2 reached 8.89 × 104 Ω·cm2, about 4.9 times that of Al-Ce0, while Al-Ce4 exhibited only 0.66 × 104 Ω·cm2. The superior Rf in Al-Ce2 was attributed to dispersed Al–Ce–Fe ternary phases, whereas massive Al2Ce precipitation in Al-Ce4 severely degraded the surface film. Although Al-Ce1 possessed the highest Rp, the optimal corrosion resistance of Al-Ce2 was dominated by its greatly enhanced film resistance, which compensated for the minor drop in Rp. The dispersion exponents n ranged from 0.85 to 0.95, indicating moderate inhomogeneity of the film and double layer. Ce addition mainly modified the film compactness and interface structure rather than altering the fundamental capacitive behavior.

3.3.3. Corrosion Mechanism Analysis

The corrosion resistance is mainly controlled by microstructural features and electrochemical kinetics. Appropriate Ce addition (0.1~0.2 wt.%) transformed coarse acicular Al–Fe phases into dispersed Al–Ce–Fe ternary particles and refined α-Al grains, reducing the potential difference between second phases and the matrix to weaken micro-galvanic corrosion [26]. The significantly decreased icorr and increased film resistance Rf confirm the improved corrosion resistance. When the Ce addition is excessive (≥0.3 wt.%), the formation of Al2Ce phases and the secondary coarsening of α-Al grains become prominent. The tentatively identified Al2Ce phase exhibits a significant potential difference relative to the α-Al matrix, which promotes the formation of micro-galvanic corrosion couples and provides more active sites for pit nucleation, thereby accelerating localized corrosion [27,28]. Meanwhile, the inhomogeneous microstructure caused by grain coarsening and second-phase segregation further accelerates local corrosion propagation [29]. As a result, the corrosion current density increases sharply and the film resistance decreases significantly, leading to a marked deterioration in corrosion resistance. Based on the above results, the improved corrosion resistance by suitable Ce addition is attributed to the optimized microstructure and the reduced electrochemical activity difference, which is a reasonable interpretation supported by microstructural observations and electrochemical measurements.

4. Conclusions

(1)
Ce regulates α-Al grains in a refine–stabilize–coarsen pattern. The refinement effect is optimal at a Ce content of 0.2~0.3 wt.%, forming uniform equiaxed grains with an average size of 78~80 μm, clear grain boundaries and excellent microstructural uniformity. Meanwhile, Ce may induce the crystal form transformation of Al-Fe phases; at 0.2 wt.% Ce, tentatively identified dispersed Al-Ce-Fe ternary phases are generated, significantly replacing and transforming the coarse acicular Al-Fe binary phases. When the Ce content exceeds 0.3 wt.%, Fe is consumed to saturation, and the excess Ce reacts with Al to precipitate massive Al2Ce binary phases, which also triggers secondary grain coarsening, causes phase enrichment at grain boundaries and leads to a significant decrease in microstructural uniformity.
(2)
The regulation of Ce addition on the mechanical properties of 8021 aluminum alloy is consistent: elongation increases continuously with increasing Ce content, tensile strength decreases slightly first and then rebounds mildly, and microhardness decreases slightly at low Ce addition and then increases continuously. The optimal Ce content for mechanical properties is 0.2 wt.%, at which the elongation reaches 42.7% (increased by 20.6% compared with the Ce-free alloy), while tensile strength and hardness remain at 95.0 MPa and 40.0 HV, respectively, presenting the optimal comprehensive mechanical performance with remarkably improved ductility and matched strength. The mechanical properties are governed by the synergy and competition among grain refinement strengthening, phase hindrance strengthening, and dispersion strengthening. Elongation is significantly improved by grain refinement and second-phase reconstruction, while the evolution of second-phase morphology and composition dominates the variation of strength and hardness.
(3)
The effect of Ce content on the corrosion resistance of 8021 aluminum alloy in 3.5% NaCl solution shows a trend of first improvement and then deterioration. The alloy achieves the best corrosion resistance at 0.2 wt.% Ce, with the corrosion current density (icorr) reduced to 2.79 × 10−7 Acm−2, a reduction of nearly one order of magnitude compared with the Ce-free sample. The Al-Ce-Fe ternary phases and fine-grained structure formed with an appropriate amount of Ce can homogenize the microstructure and reduce micro-galvanic corrosion, thus slowing down the corrosion kinetic process. In contrast, the precipitation of Al2Ce binary phases and grain coarsening caused by excessive Ce form strong cathodic phases to aggravate micro-galvanic corrosion and also lead to loose surface film layers, which is unfavorable for the service stability of the battery foil billet during subsequent processing.

Author Contributions

Methodology, L.S., B.C. and B.R.; Investigation, L.S., B.R. and A.J.; Data curation, L.S. and Z.L.; Writing—original draft preparation, L.S.; Writing—review and editing, Z.L. and B.C.; Project administration, B.R., A.J. and Z.L.; Funding acquisition, B.R. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by HENAN PROVINCE SCIENCE AND TECHNOLOGY RESEARCH PLAN PROJECT, grant number 232102231007.

Institutional Review Board Statement

Not applicable.

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding authors.

Conflicts of Interest

Author Lei Shi was employed by the company Henan Zhongfu Industrial Co., Ltd. The remaining authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.

References

  1. Xu, S.A.; Wang, S.N.; Gu, Y.Y. Microstructure and adhesion properties of Ce conversion coating modified with silane coupling agent on the aluminum foil for lithium ion battery. Results Phys. 2019, 13, 102262. [Google Scholar] [CrossRef] [Scilit]
  2. Xia, X.F.; Gu, Y.Y.; Xu, S.A. Titanium conversion coatings on the aluminum foil AA 8021 used for lithium-ion battery package. Appl. Surf. Sci. 2017, 419, 447–453. [Google Scholar] [CrossRef] [Scilit]
  3. Liang, C.S.; Lv, Z.F.; Zhu, Y.L.; Xu, S.A.; Wang, H. Protection of aluminium foil AA8021 by molybdate-based conversion coatings. Appl. Surf. Sci. 2014, 288, 497–502. [Google Scholar] [CrossRef] [Scilit]
  4. Zhao, X.Y.; Jin, T.; Ding, L.P.; Wan, B.W.; Lei, X.C.; Xu, C.Z.; Zhang, C.L.; Jia, Z.H.; Liu, Q. The effect of combined cold rolling and homogenization on the microstructures and mechanical properties of twin-roll casted 8021 aluminum alloy. J. Alloys Compd. 2023, 937, 168385. [Google Scholar] [CrossRef] [Scilit]
  5. Lu, L.; Dahle, A.K. Iron-rich intermetallic phases and their role in casting defect formation in hypoeutectic Al-Si alloys. Metall. Mater. Trans. A 2005, 36, 819–835. [Google Scholar]
  6. Khalifa, W.; Samuel, F.H.; Gruzleski, J.E. Iron intermetallic phases in the Al corner of the Al-Si-Fe system. Metall. Mater. Trans. A 2003, 34, 807–825. [Google Scholar] [CrossRef] [Scilit]
  7. Pithawalla, Y.B.; Shall, M.; Deevi, S.C. Synthesis and characterization of nanocrystalline iron aluminide particles. Intermetallics 2000, 8, 1225–1231. [Google Scholar] [CrossRef] [Scilit]
  8. Chen, W.; Chen, M.H.; Jin, X.J.; Zhang, P. Effect of heating rate during annealing on microstructure and texture evolution of AA8021 aluminum foil. Mater. Res. Express 2020, 7, 096514. [Google Scholar] [CrossRef] [Scilit]
  9. Wang, W.; Sun, Q.R.; Zhang, K.M. Modification mechanism and mechanical properties of 8021 aluminum alloys. J. Mater. Eng. Perform. 2025, 34, 21886–21892. [Google Scholar] [CrossRef] [Scilit]
  10. Huang, Y.C.; Wang, Y.H.; Zhao, J.Y.; Liu, Y.; Chen, C.K.; He, G.Z. Effect of prerecovery annealing on microstructure and mechanical properties of AA8021 aluminum alloy used for aluminum plastic films. Adv. Eng. Mater. 2025, 27, 202500195. [Google Scholar] [CrossRef] [Scilit]
  11. Ji, H.H.; Wu, C.F.; Hu, D.L.; Wang, Y.Y.; Lei, Y.G. Research on melting and casting process of large-scale 8021 aluminium alloy flat ingots. Alum. Fabr. 2025, 6, 35–41. (In Chinese) [Google Scholar]
  12. Jin, X.J.; Zhao, P.Z.; Feng, D. Effect of grain size on the mechanical properties and formability of AA8021 aluminum foil. J. Mater. Eng. Perform. 2022, 31, 10354–10366. [Google Scholar] [CrossRef] [Scilit]
  13. Chen, W.; Zhao, P.Z.; Zhou, Y.L.; Pan, Y.F. Effects of homogenization conditions on the microstructures of twin-roll cast foil stock of AA8021 aluminum alloy. Mater. Sci. Forum 2016, 877, 296–302. [Google Scholar] [CrossRef] [Scilit]
  14. Mu, X.W.; Du, K.; Lü, C.; Xu, G.M. Effect of Ce content on solidification structure of 8021 aluminum alloy. Light Alloy Fabr. Technol. 2022, 50, 20–23. (In Chinese) [Google Scholar]
  15. Sun, Q.R.; Wang, W. Effects of Sr and Nd elements on microstructure and properties of 8021 aluminum alloy. Trans. Mater. Heat Treat. 2024, 45, 84–90. (In Chinese) [Google Scholar]
  16. Sun, Q.; Wang, W. Effect of Microalloying on Hot Deformation Behavior of 8021 Aluminum Alloy. Russ. J. Non-Ferr. Met. 2024, 65, 65. [Google Scholar] [CrossRef] [Scilit]
  17. Vončina, M.; Medved, J.; Steinacher, M.; Ozimič, K. The influence of La and Ce additions on the solidification of alloys from the Al–Fe system. J. Therm. Anal. Calorim. 2025, 150, 873–882. [Google Scholar] [CrossRef] [Scilit]
  18. Czerwinski, F. Cerium in aluminum alloys: A review. J. Mater. Sci. 2020, 55, 5215–5242. [Google Scholar] [CrossRef] [Scilit]
  19. Yu, L.; Lu, H.; Cheng, L.; Guo, A.; Li, R.; Zhang, Z.; Wang, W.; Shi, Y.; Wu, K. Insight on the grain refinement, iron phase transformation and mechanical properties of recycled A356 aluminum alloy with Al-Nb-B refiner. J. Alloys Compd. 2025, 1048, 185172. [Google Scholar] [CrossRef] [Scilit]
  20. Bolzoni, L.; Hari Babu, N. Towards industrial Al-Nb-B master alloys for grain refining Al-Si alloys. J. Mater. Res. Technol. 2019, 8, 5631–5638. [Google Scholar] [CrossRef] [Scilit]
  21. Liu, S.Q.; Zhao, T.; Fu, J.Y.; Zu, Q. Development of inoculants for aluminum alloy: A review. Materials 2023, 16, 5500. [Google Scholar] [CrossRef] [Scilit]
  22. Gan, J.Q.; Huang, Y.J.; Wen, C.; Du, J. Effect of Sr modification on microstructure and thermal conductivity of hypoeutectic Al−Si alloys. Trans. Nonferrous Met. Soc. China 2020, 30, 2879–2890. [Google Scholar] [CrossRef] [Scilit]
  23. Zhao, W.J.; Liu, G.Y.; Zhang, S.Q.; Ren, Y.S.; Yuan, K.; Yu, B.X.; Wang, B.; Xing, H.; Lv, G.Q.; Chen, X.H.; et al. A review of rare earth elements microalloying in aluminum alloys: Mechanisms of microstructure evolution and Performance Enhancement. J. Mater. Res. Technol. 2026, 41, 2839–2869. [Google Scholar] [CrossRef] [Scilit]
  24. Qu, H.; Liu, W.D.; Jiang, X.Y. EET analysis of melt structure and formation of main strengthening phases in Al-Fe-Ce alloy. Chin. J. Rare Met. 2020, 44, 1003–1008. (In Chinese) [Google Scholar]
  25. Li, S.X.; Jiang, H.X.; Li, Y.Q.; Zhang, L.L.; Sun, H.; He, J.; Jiang, H.C.; Zhao, J.Z. Influence of rare earth Ce on the microstructures and performances of Al-Fe alloy. Sci. China Technol. Sci. 2023, 66, 3317–3327. [Google Scholar] [CrossRef] [Scilit]
  26. Wang, P.J.; Ma, L.W.; Cheng, X.Q.; Li, X.G. Influence of grain refinement on the corrosion behavior of metallic materials: A review. Int. J. Miner. Metall. Mater. 2021, 28, 1112–1126. [Google Scholar] [CrossRef] [Scilit]
  27. Ikeuba, A.I.; Njoku, C.N.; Ekerenam, O.O.; Njoku, D.I.; Udoh, I.I.; Daniel, E.F.; Uzoma, P.C.; Etim, I.I.; Okonkwo, B.O. A review of the electrochemical and galvanic corrosion behavior of important intermetallic compounds in the context of aluminum alloys. RSC Adv. 2024, 14, 31921–31953. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  28. Zhou, X.J.; Xiong, H.Q. Corrosion behavior of Al-Ce alloys in 3.5% NaCl solution. Int. J. Electrochem. Sci. 2022, 17, 220137. [Google Scholar] [CrossRef] [Scilit]
  29. Li, C.; Luo, Y.T.; Zhou, Q.S.; Han, M.N.; Sha, S.H.; Xu, X.J. Effect of Ce element content on microstructure and corrosion resistance of highly-alloyed Al–Zn–Mg–Cu–Zr–Ti alloy. Trans. Nonferrous Met. Soc. China 2025, 35, 2148–2163. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.