Skip to Content
NanomaterialsNanomaterials
  • Article
  • Open Access

28 November 2026

16 Pages

Low-Temperature Integration of Gamma-Ray-Tolerant ZnO/Te Complementary Field-Effect Transistors

,
,
,
,
,
,
and
1
Graduate School of Semiconductor Technology, Pohang University of Science and Technology, Cheongam-ro 77, Nam-gu, Pohang 37673, Republic of Korea
2
Department of Electrical Engineering, Pohang University of Science and Technology, Cheongam-ro 77, Nam-gu, Pohang 37673, Republic of Korea
*
Author to whom correspondence should be addressed.
†
These authors contributed equally to this work.
Nanomaterials2026, 16(23), 1560;https://doi.org/10.3390/nano16231560 
(registering DOI)
This article belongs to the Section Nanoelectronics, Nanosensors and Devices

Abstract

Alternative channel materials enable low-temperature integration of additional electronic functions, but their use in space requires radiation tolerance at both the device and circuit levels. Here, we report the gamma-ray response of vertically integrated ZnO/Te complementary field-effect transistors (CFETs) fabricated at temperatures not exceeding 150 °C, in which the Al2O3 layers formed during the integration process also encapsulate both channels. Without passivation, the on-state currents of ZnO nFETs and Te pFETs decreased by 97% and 80%, respectively, after a total dose of 400 krad. With Al2O3 passivation, the threshold voltage shifts in both transistor types remained below 75 mV, the on-state current changed by less than 25%, and the bias-stress stability was comparable to that before irradiation. X-ray photoelectron spectroscopy results are consistent with the passivation limiting irradiation-associated changes in the ZnO surface chemistry and the oxidation of Te. After irradiation to 400 krad, CFET inverters exhibited a voltage gain of 34.6 V/V and high and low noise margins of 2.69 V and 0.92 V, respectively, at a supply voltage of 5 V, and three-stage CFET ring oscillators operated at 43.5 kHz. These results suggest that channel passivation incorporated into low-temperature vertical integration can improve the gamma-ray tolerance of ZnO/Te complementary logic intended for back-end-of-line and monolithic three-dimensional integration.

1. Introduction

Semiconductor devices used in satellites and space exploration systems must maintain stable electrical operation in radiation environments [1]. In orbit, trapped electrons and protons, solar energetic particles, and secondary photons deposit ionizing energy in electronic materials [2]. The accumulated total ionizing dose (TID) can alter key electrical parameters, including on-state current and threshold voltage, thereby degrading device performance and reliability [3,4]. These changes can compromise communication, data processing, and spacecraft control, potentially limiting mission lifetime [5]. Although shielding can reduce radiation exposure, spacecraft mass and volume constraints limit the use of thick protective layers [6]. Radiation tolerance at the material and device levels is therefore necessary to preserve electrical performance and circuit functionality. These reliability requirements also extend to alternative channel materials being investigated to complement scaled silicon circuits. Such materials offer opportunities to integrate additional devices on the wafer backside and logic or memory blocks into functional redistribution layers, where conventional silicon integration is challenging because of thermal-budget constraints, process complexity, or cost [7,8,9,10,11]. In space applications, these additional circuits are also exposed to ionizing radiation, and their degradation can affect overall system performance. Their radiation tolerance therefore needs to be evaluated together with their compatibility with the intended integration process. To evaluate the TID response of these devices under controlled laboratory conditions, gamma rays from 60Co sources are widely used because their high penetrating power allows irradiation throughout the device stack [12,13].
ZnO and tellurium (Te) are candidate materials for implementing such additional functional blocks through low-temperature complementary integration. ZnO deposited by atomic layer deposition (ALD) provides n-channel operation with low off-state current, while Te is one of the few semiconductors that provide p-channel operation in ultrathin films deposited at low temperatures [14,15,16,17]. Because both materials can be processed without high-temperature dopant activation, n- and p-channel transistors can be integrated sequentially, and complementary devices and circuits based on ZnO/Te and IGZO/Te have been reported [18,19,20,21]. Extending this material system to space electronics requires an understanding of the radiation responses of both channel materials and their combined operation in complementary circuits.
Previous studies have investigated gamma-ray irradiation effects in n-channel metal-oxide FETs, including ZnO, indium zinc oxide (IZO), and indium gallium zinc oxide (IGZO) [22,23,24]. Reported responses include threshold voltage (Vth) shifts, reductions in on-state current, increased leakage current, and degradation of subthreshold characteristics, with the specific response depending on the material system, device structure, and irradiation conditions. Gamma irradiation can affect these devices in two ways: by changing the semiconductor channel itself, including its defects and surface chemistry, or by trapping charge in the gate dielectric or at the semiconductor/dielectric interface. In a-IGZO TFTs, irradiation has been reported to change both the channel defect states and the charge trapped in the gate insulator [25,26]. Gamma-ray-induced charge trapping in Al2O3 and at the Al2O3/semiconductor interface has also been reported in metal–oxide–semiconductor structures [27]. To mitigate or recover these changes, channel-thickness optimization, electrothermal annealing, and rapid thermal annealing in O2 have been explored in IGZO TFTs [25,26]. However, these studies primarily address individual n-channel devices under specific material, irradiation, or treatment conditions. In comparison, the gamma-ray responses of emerging p-channel oxide and chalcogenide transistors remain less well established, particularly in the context of low-temperature complementary integration [28,29]. Studies of MoTe2 thin films have reported irradiation-induced defects, oxidation, and enhanced p-type doping, but have primarily examined material properties rather than the resulting changes in transistor switching characteristics [30]. Beyond the stability of individual transistors, the combined response of n- and p-channel devices must also be assessed, because irradiation-induced changes in either device can affect the operation of the complementary circuit. Unequal radiation responses can alter the electrical balance between the two transistor polarities, even when each device remains functional [31,32]. Therefore, approaches that stabilize both n- and p-channel devices and preserve their combined operation in complementary circuits are needed. In ultrathin ZnO and Te channels, surface reactions during irradiation may deplete electrons in ZnO and oxidize Te [33,34]. Charge trapping in the Al2O3 gate dielectrics may also change the transistor characteristics [3,27]. If surface reactions are the main cause of degradation, encapsulation should reduce both the chemical and electrical changes, whereas dielectric trapping may remain. We therefore compare the electrical and XPS responses of unpassivated and passivated devices to assess the two pathways.
In this work, we use the vertically integrated ZnO/Te complementary field-effect transistor (CFET) architecture reported previously [18] to examine the protective role of the Al2O3 layers formed during CFET integration and to evaluate complementary circuit operation after gamma-ray irradiation. In the CFET, the n- and p-channel transistors are stacked vertically and share a common gate, which reduces the device footprint and is compatible with monolithic three-dimensional (M3D) integration [18,35]. The entire fabrication process is performed at temperatures not exceeding 150 °C. The Al2O3 gate dielectric deposited on the lower Te channel also serves as its encapsulation layer, and a final Al2O3 overlayer encapsulates the upper ZnO channel, so that both channels are passivated within the integration sequence. Passivation layers, including Al2O3, have been reported to improve the radiation tolerance of oxide thin-film transistors [29,36,37]. Here, this protective function is examined in the ZnO/Te CFET platform by comparing both transistor polarities, with and without passivation, at the same total gamma-ray doses, and by testing circuit operation after irradiation. Compared with unpassivated devices, the passivated devices show much smaller changes in their electrical characteristics after irradiation. Across total doses of 50, 100, and 400 krad, the passivated ZnO nFETs and Te pFETs exhibit maximum Vth shift (ΔVth) values of 72 and 42 mV, respectively, with corresponding maximum on-state current deviations of 8.8% and 23.0% from their pre-irradiation values. X-ray photoelectron spectroscopy (XPS) is used to relate these electrical responses to chemical changes in the channel materials. The bias-stress stability of the passivated transistors after irradiation is comparable to that before irradiation. After irradiation to 400 krad, CFET inverters operate at a supply voltage (VDD) of 5 V with a maximum voltage gain of 34.6 V/V and high and low noise margins of 2.69 and 0.92 V, respectively, and three-stage CFET ring oscillators operate at 43.5 kHz. These results suggest that channel passivation incorporated into low-temperature vertical integration can improve the gamma-ray tolerance of ZnO/Te complementary logic for back-end-of-line (BEOL) and M3D integration.

2. Materials and Methods

Device fabrication began with the formation of 50 nm-deep trenches in the SiO2 substrate using i-line photolithography followed by inductively coupled plasma reactive-ion etching (ICP-RIE; POSTECH Center for Semiconductor Technology Convergence, supported by the Korea Basic Science Institute, NFEC-2025-05306208). A Ti/Ni bilayer consisting of a 10 nm Ti adhesion layer and a 40 nm Ni layer was subsequently deposited by electron-beam evaporation and patterned by lift-off to form the buried source/drain (S/D) electrodes. A 4 nm Te channel layer was then deposited by DC sputtering with an Ar flow rate of 30 sccm, a working pressure of 2 mTorr, and a DC power of 20 W. The channel pattern was defined using i-line photolithography and lift-off. Subsequently, a 10 nm Al2O3 film was deposited by ALD at 150 °C using trimethylaluminum (TMA) and H2O as the precursor and oxidant, respectively. This Al2O3 layer served as both the gate dielectric for the lower Te pFET and the channel encapsulation layer. Next, a 50 nm Ni gate electrode was formed by electron-beam evaporation and lift-off using AZ5214 image-reversal photoresist. A second 10 nm Al2O3 layer was deposited by ALD at 150 °C to provide the gate dielectric for the upper nFET. A 5 nm ZnO film was deposited by ALD at 120 °C using diethylzinc (DEZ) and H2O to form the upper n-channel. The active channel region was subsequently defined by wet etching using an HCl solution prepared by mixing 5 mL of HCl with 300 mL of deionized water (wet etch station; POSTECH Center for Semiconductor Technology Convergence, supported by the Korea Basic Science Institute, NFEC-2025-02-304149). Via holes were opened through the 20 nm Al2O3 stack by wet etching in an NH4OH solution at 50 °C to enable interconnection between the lower and upper devices. A 50 nm Ni layer was deposited by electron-beam evaporation and patterned by lift-off to form the upper S/D electrodes. Finally, a 10 nm Al2O3 passivation layer was deposited by ALD at 150 °C to encapsulate the ZnO channel.
Unless otherwise noted, electrical characterization was performed in ambient air at 25 °C using a semiconductor parameter analyzer (Keithley 4200A-SCS, Tektronix, Beaverton, OR, USA). The Vth was extracted from the forward sweep using the constant-current method at a drain current of |ID| = 1 nA × (W/L) for ZnO nFETs and |ID| = 10 nA × (W/L) for Te pFETs, where W and L are the channel width and length, respectively. These criteria were selected to account for the different off-state current levels and subthreshold characteristics of the two channel materials, placing the extraction points within the gate-modulated transition region above the off-state current. Cross-sectional specimens for transmission electron microscopy (TEM) were prepared by focused ion beam milling using a Helios 650 system (FEI, Hillsboro, OR, USA). Subsequent low-energy Ar-ion milling was performed to reduce damage introduced during specimen preparation. A JEOL JEM-2100F microscope (JEOL Ltd., Tokyo, Japan) was used for high-resolution TEM (HR-TEM) imaging and energy-dispersive X-ray spectroscopy (EDS) mapping to characterize the device structure and elemental distributions. Chemical composition and oxidation states were examined by X-ray photoelectron spectroscopy (XPS) using a Thermo Scientific Nexsa G2 instrument (Thermo Fisher Scientific, Waltham, MA, USA). For the passivated samples, the Al2O3 layer was removed with an Ar gas cluster ion beam to expose the ZnO or Te surface. Gas-cluster etching was used to minimize sputter-induced changes in the chemical states. The unpassivated samples were measured without etching. Because the sample preparation differed, we compare mainly the changes before and after irradiation within each sample type. All spectra were charge-referenced to the C 1s peak at 284.8 eV and fitted with Voigt-type line shapes after Shirley background subtraction, with peak positions constrained to the following ranges. The O 1s components were located at 530.2–530.5 eV (lattice oxygen), 531.3–531.8 eV (VO-related), and 532.3–532.6 eV (hydroxyl-related), with FWHMs of 1.24–2.01 eV. The Te 3d5/2 components were located at 573.0–573.2 eV (Te0), 574.3–574.5 eV (suboxide), and 576.2 eV (Te4+), with FWHMs of 0.93–1.57 eV.
The devices were characterized before irradiation and after nominal total doses of 50, 100, and 400 krad. A separate device group was used for each dose, and the pristine characteristics of the groups were comparable. Irradiation was performed in ambient air at room temperature without bias, using a 60Co source at a dose rate of 1 kGy/h at the Advanced Radiation Technology Institute of the Korea Atomic Energy Research Institute (ARTI-KAERI, Jeongeup, Republic of Korea). Electrical measurements were performed sequentially and completed within 72 h after each irradiation. Between measurements, the devices were stored under vacuum when possible. Bias-stress measurements were performed under vacuum: a gate bias of +2 V (PBS) for ZnO nFETs or −2 V (NBS) for Te pFETs was applied with the source and drain grounded, and transfer characteristics were measured after 10, 31.6, 100, 316.2, and 1000 s. Single-event effects were not evaluated in this study and require separate testing for space applications.

3. Results and Discussion

Figure 1a illustrates the vertically integrated ZnO/Te CFET, comprising a lower Te pFET and an upper ZnO nFET that share a common Ni gate. An Al2O3 dielectric separates each semiconductor channel from the gate. In the inverter configuration, the shared gate serves as the input terminal (VIN), and the interconnected drains form the output terminal (VOUT). The source terminals of the Te pFET and ZnO nFET are connected to the VDD and ground, respectively. The cross-sectional TEM image in Figure 1b shows the layered structure of the CFET. The corresponding EDS maps in Figure 1c show the spatial distributions of O, Al, Ni, Zn, and Te. The Te and Zn signals are located below and above the shared Ni gate, respectively, consistent with the arrangement of the lower p-channel and upper n-channel. An optical micrograph of the CFET is shown in Figure 1d. Figure 1e summarizes the fabrication sequence, in which the lower Te channel, shared Ni gate, and upper ZnO channel were formed sequentially. All fabrication steps were performed at temperatures not exceeding 150 °C. The Al2O3 layer deposited over the Te channel serves as both its gate dielectric and encapsulation layer, while a final 10 nm Al2O3 overlayer passivates the ZnO channel. Channel encapsulation is therefore incorporated into the fabrication sequence for both transistors.
Figure 1. Structure and fabrication of the vertically integrated ZnO/Te CFET. (a) Three-dimensional schematic of the vertically stacked ZnO/Te CFET. (b) Cross-sectional transmission electron microscopy (TEM) image of the CFET (scale bar: 10 nm). (c) Corresponding energy-dispersive X-ray spectroscopy (EDS) maps of O, Al, Ni, Zn, and Te. The leftmost image shows an overlay of all five elemental maps for the region marked by the dashed box in (a). (d) Optical micrograph of the CFET. (e) Fabrication sequence with a maximum process temperature of 150 °C.
Figure 2 compares the transfer characteristics of ZnO nFETs and Te pFETs with and without Al2O3 passivation before irradiation and after gamma-ray doses of 50, 100, and 400 krad. The unpassivated ZnO nFET exhibits a progressive decrease in on-state current and a positive Vth shift with increasing dose (Figure 2a). After 400 krad, the on-state current (Ion) decreases by 97.2% relative to the pristine device, from 0.581 to 0.0163 μA μm−1. The corresponding ΔVth value is +0.75 V relative to the pristine value. The hysteresis window between the forward and reverse sweeps widens from 0.79 V in the pristine device to 1.22 V after exposure to 400 krad. For the unpassivated Te pFET, both Ion and the off-state current (Ioff) decrease with increasing dose (Figure 2b). At 400 krad, Ion decreases by 80% from 0.679 to 0.136 μA μm−1, and Ioff decreases from 2.2 × 10−4 to 7.3 × 10−5 μA μm−1 compared with their pristine values. Because both currents decrease, the Ion/Ioff ratio changes only from approximately 3 × 103 to 2 × 103, and the distinction between the on and off states is preserved. These current reductions are accompanied by a negative Vth shift, with a ΔVth value of −0.69 V relative to the pristine device after 400 krad. The hysteresis between the forward and reverse sweeps remains nearly unchanged after irradiation, with voltage windows of 3.98, 3.91, 4.06, and 3.97 V for the pristine device and after irradiation at 50, 100, and 400 krad, respectively (Figure 2b). In comparison, the Al2O3-passivated ZnO nFET and Te pFET exhibit much smaller changes in their transfer characteristics over the investigated dose range (Figure 2c,d). After irradiation at 400 krad, the ΔVth magnitudes are 0.07 V for the ZnO nFET and 0.04 V for the Te pFET, while Ion changes by 2.8% and 21.4%, respectively, relative to the pristine values. Across all doses, the maximum ΔVth magnitudes are 72 and 42 mV and the maximum Ion deviations are 8.8% and 23.0% for the ZnO nFET and Te pFET, respectively. Although the Ion change in the passivated Te pFET is not negligible, it is much smaller than the 80% reduction in the unpassivated device. The passivated Te pFET exhibits a hysteresis window of 1.49 V before irradiation and 1.61, 1.51, and 1.63 V after exposure to 50, 100, and 400 krad, respectively (Figure 2d). These results indicate that the hysteresis window remains largely unchanged over the investigated dose range. Thus, the Al2O3-passivated transistors of both polarities show substantially smaller changes after irradiation than the unpassivated transistors.
Figure 2. Gamma-ray response of ZnO and Te transistors with and without Al2O3 passivation. Transfer characteristics of unpassivated (a) ZnO nFETs and (b) Te pFETs, and Al2O3-passivated (c) ZnO nFETs and (d) Te pFETs, measured before irradiation (pristine) and after exposure to doses of 50, 100, and 400 krad. All transistors have a channel length (L) of 5 μm and a channel width (W) of 10 μm.
To assess device-to-device variation, 15 devices were measured for each transistor type, passivation condition, and dose, including the pristine condition. The mean ± standard deviation of Ion and Vth is given in Table 1. The passivated devices show smaller changes in both mean Ion and Vth than the unpassivated devices, consistent with the representative curves in Figure 2.
Table 1. Ion and Vth of ZnO nFETs and Te pFETs as a function of gamma-ray dose (mean ± standard deviation of 15 devices).
To further understand the electrical responses to gamma-ray irradiation observed in the transfer characteristics, XPS spectra of unpassivated and Al2O3-passivated ZnO and Te were compared before and after exposure to 400 krad (Figure 3). In the O 1s spectra of unpassivated ZnO, the relative fitted area of the component conventionally associated with oxygen vacancies (VO) decreased from 27.5% to 22.4%, whereas the hydroxyl-related component increased from 15.9% to 23.4%. Because the assignment of O 1s sub-peaks, in particular the attribution of a component to oxygen vacancies, is not unique [38,39], we regard the following correlations as qualitative. The decrease in the VO-related component and the increase in the hydroxyl-related component indicate a change in the ZnO surface chemistry, which may contribute to the lower on-state current and positive ΔVth in Figure 2a. However, the fitted component areas do not directly show a decrease in oxygen-vacancy or donor density. Oxygen vacancies can exist as VO0, VO+, and VO2+ [40,41]. The ionized states act as shallow donors, so a decrease in their density shifts Vth positively [36]. In contrast, ionization of VO0 by irradiation releases electrons and shifts Vth negatively, as reported for gamma-irradiated IGZO TFTs [26]. The positive Vth shift in the unpassivated ZnO nFETs is therefore more consistent with a decrease in ionized vacancies than with ionization of neutral vacancies, although the XPS data cannot distinguish these charge states. The concurrent increases in the hydroxyl-related contribution and hysteresis are similar to previous observations for proton-irradiated ZnO TFTs, where hydroxyl-related surface changes were associated with increased hysteresis and Vth instability [36]. Al2O3-passivated ZnO exhibited only small changes in the corresponding components. The VO fraction changed from 14.1% to 13.2%, while the hydroxyl-related fraction changed from 12.5% to 11.8%, leaving the overall spectral profile largely unchanged. Pristine passivated ZnO shows lower VO-related and hydroxyl-related fractions than pristine unpassivated ZnO, possibly because the Al2O3 deposition or the etching for XPS modified the ZnO surface. We therefore compare the irradiation-induced changes within each sample type, not the absolute fractions. The limited changes in these component fractions are consistent with the nearly overlapping transfer curves before and after irradiation (Figure 2c), supporting the chemical and electrical stability of the passivated ZnO channel.
Figure 3. X-ray photoelectron spectroscopy (XPS) analysis of ZnO and Te before and after gamma-ray irradiation at 400 krad. (a) O 1s spectra of ZnO and (b) Te 3d5/2 spectra of Te. In each panel, the spectra correspond, from left to right, to pristine unpassivated, irradiated unpassivated, pristine Al2O3-passivated, and irradiated Al2O3-passivated samples. Open circles and black lines represent the measured spectra and cumulative fits, respectively. Colored peaks indicate the fitted chemical-state components, with the annotated percentages representing their relative contributions to the total fitted peak area. All spectra were charge-referenced to the C 1s peak at 284.8 eV and fitted using Voigt-type line shapes after subtraction of a Shirley background.
The Te 3d5/2 spectra show a pronounced difference in the oxidation behavior of unpassivated and passivated Te. For unpassivated Te, the relative fitted area of the Te4+ component increased from 48.7% to 91.2% after irradiation, while the elemental Te0 component decreased from 46.9% to 6.3%. The suboxide contribution remained minor, changing from 4.4% to 2.5%. The shift from a mixed Te0/Te4+ spectrum to a predominantly Te4+ spectrum indicates substantial oxidation within the region probed by XPS. This chemical change accompanies the simultaneous decreases in on- and off-state currents, while p-type switching and the on/off current ratio remain largely preserved (Figure 2b). The association between extensive oxidation and reduced carrier transport is consistent with previous findings in Te TFTs, where the predominance of Te4+ states was accompanied by degraded field-effect mobility [16]. Al2O3-passivated Te retained nearly the same chemical-state distribution after irradiation. The Te0 component remained dominant, accounting for 97.3% and 96.7% of the fitted peak area before and after irradiation, respectively. The suboxide fraction changed only slightly, from 2.7% to 3.3%, and no distinct Te4+ component was resolved in either spectrum. The absence of a Te4+ component in pristine passivated Te, in contrast to the 48.7% Te4+ fraction in pristine unpassivated Te, suggests that the Al2O3 layer also suppresses native oxidation of Te before irradiation. The preservation of the elemental Te component agrees with the stable transfer characteristics of the passivated Te pFETs (Figure 2d). The XPS and electrical results are consistent with the role of Al2O3 passivation in limiting changes in the surface chemistry of ZnO and suppressing further oxidation of Te under gamma-ray exposure.
Based on the electrical and XPS results, Figure 4 illustrates the proposed mechanisms underlying the irradiation responses of ZnO and Te and the role of Al2O3 passivation. For unpassivated ZnO, we interpret the electrical response using a surface-depletion model, in which irradiation-associated surface reactions increase electron depletion in the ZnO channel (Figure 4a). Gamma irradiation in air generates reactive species, such as ozone and oxygen radicals, through radiolysis of air and adsorbed water [42,43]. These species may react with the exposed ZnO surface, changing the oxygen-related surface states and promoting electron capture by adsorbed oxygen. Because the ZnO channel is only 5 nm thick, such surface depletion can affect a large fraction of the channel. Within this model, a higher positive gate voltage is required to establish electron conduction, resulting in a positive Vth shift and a lower on-state current at a given gate voltage. This interpretation is consistent with the electrical changes and with previous reports that oxygen adsorption on ZnO surfaces depletes electrons, reduces conductance, and shifts Vth positively [33,44]. In addition, the positive ΔVth is opposite to the shift expected from positive charge trapped in the gate dielectric, which would shift Vth of an n-channel device negatively [3,13]. The increased hysteresis suggests that the modified surface also introduces slow charge-trapping states, in line with the increase in the hydroxyl-related XPS component.
Figure 4. Proposed mechanisms underlying the gamma-ray irradiation responses of (a) ZnO nFETs and (b) Te pFETs and the role of Al2O3 passivation. Each panel compares pristine unpassivated, irradiated unpassivated, and irradiated Al2O3-passivated devices, from left to right.
For unpassivated Te, the dominant chemical change is oxidation, as indicated by the pronounced increase in the Te4+ component and the corresponding loss of elemental Te0. In the proposed mechanism, the formation of an oxidized surface layer reduces the effective conducting thickness of the Te channel (Figure 4b). Because the Te channel is only 4 nm thick, even a thin oxidized layer consumes a substantial fraction of the channel. The resulting decrease in channel conductance accounts for the simultaneous reduction in on- and off-state currents, while the remaining Te channel retains p-type gate modulation. This interpretation is consistent with the largely preserved on/off current ratio and with previous findings associating extensive Te oxidation with degraded carrier transport [16,34].
Al2O3 passivation is expected to act as a barrier to interactions between the semiconductor surfaces and the surrounding atmosphere [45]. In this model, restricted access of ambient reactants, including radiolysis products, limits surface chemical changes in ZnO and further oxidation of Te during irradiation. The small changes in the oxygen-related XPS components of passivated ZnO and the retention of predominantly elemental Te in passivated Te are consistent with this protective role. Gamma irradiation also generates electron–hole pairs in the Al2O3 layers, and charge trapped in the gate dielectric can shift Vth [27]. The |ΔVth| of the passivated devices (72 mV or less) suggests that this contribution is small for the 10 nm Al2O3 layers under unbiased irradiation up to 400 krad. Because oxide-trapped charge generally builds up more under gate bias during irradiation [3,13], evaluation under biased irradiation remains a subject for future work. We also note that the unpassivated devices were exposed to ambient air during handling and storage between measurements as well as during irradiation; therefore, the present results do not fully separate irradiation-induced changes from ambient aging of the unpassivated channels. Nevertheless, the nearly unchanged transfer characteristics of both passivated transistor types, together with the XPS results, suggest that channel chemical stability is an important contributor to their electrical stability after gamma-ray exposure.
The bias-stress stability of the Al2O3-passivated transistors was evaluated under vacuum before and after irradiation by applying positive bias stress (PBS) to the ZnO nFETs and negative bias stress (NBS) to the Te pFETs for up to 1000 s (Figure 5). This test examines whether irradiation creates additional trap sites that respond to sustained gate bias. The Ioff in Figure 5a–d is lower than in the ambient-air measurements of Figure 2c and Figure 6a, possibly because of reduced leakage related to ambient adsorbates under vacuum. The ZnO nFETs exhibit only minor changes in their transfer characteristics during PBS (Figure 5a–d). After 1000 s, the ΔVth values are +40.6, +54.6, +59.6, and +21.5 mV for the pristine devices and those irradiated to 50, 100, and 400 krad, respectively. The shifts vary non-monotonically with dose, but their magnitudes remain below 60 mV for all conditions. The Te pFETs exhibit negative Vth shifts under NBS (Figure 5e–h). The ΔVth values after 1000 s are −193.0, −165.4, −184.0, and −173.8 mV for the pristine, 50, 100, and 400 krad conditions, respectively. These shifts are larger than those of the ZnO nFETs, but their magnitudes remain below 0.20 V for all conditions. These results show that the bias-stress-induced ΔVth values of both passivated transistor types after gamma-ray exposure up to 400 krad are comparable to those before irradiation, with no systematic increase in shift magnitude with dose. The differences among the conditions (within approximately 40 mV for both transistor types) are small and may include device-to-device variation.
Figure 5. Bias-stress stability of Al2O3-passivated ZnO and Te transistors before and after gamma-ray irradiation. Transfer characteristics of (a–d) ZnO nFETs under positive bias stress (PBS) and (e–h) Te pFETs under negative bias stress (NBS) for stress durations up to 1000 s. Measurements are shown for (a,e) pristine devices and devices irradiated to (b,f) 50, (c,g) 100, and (d,h) 400 krad.
Figure 6. Temporal stability of Al2O3-passivated ZnO and Te transistors. Transfer characteristics of (a) a ZnO nFET and (b) a Te pFET measured initially and after 1, 3, 7, 14, and 30 days of storage in ambient air following irradiation to 400 krad.
In addition to their stability under gate-bias stress, the Al2O3-passivated devices exhibit stable transfer characteristics during storage in ambient air for 30 days after irradiation to 400 krad (Figure 6). The transfer curves of both the ZnO nFET (Figure 6a) and Te pFET (Figure 6b) remain nearly unchanged throughout the monitoring period, closely overlapping their respective initial curves. Only minor variations are observed in the current levels and turn-on characteristics. This result also supports the effectiveness of Al2O3 encapsulation against ambient exposure, which is consistent with the protective role discussed above. The bias-stress and ambient-storage results show post-irradiation stability under the tested conditions. Accelerated aging, high-temperature storage, thermal cycling, and combined radiation and temperature stress tests are needed to assess reliability for long-duration missions.
The circuit functionality of the ZnO/Te CFETs was evaluated after gamma-ray irradiation at 400 krad using complementary inverters and ring oscillators. The CFET inverter exhibits clear voltage transitions with nearly full output swings over a VDD range of 1–5 V (Figure 7a). The maximum voltage gain increases with VDD, reaching 34.6 V/V at VDD = 5 V. The supply current peaks near the switching transition and decreases away from this region, with higher peak currents observed at larger VDD values (Figure 7b). Both the low (NML) and high (NMH) noise margins increase with VDD (Figure 7c). At VDD = 5 V, NML and NMH are approximately 0.92 and 2.69 V, respectively, corresponding to a normalized total noise margin, (NML + NMH)/VDD, of approximately 0.72. The switching voltage is located well below VDD/2 (approximately 1.7 V at VDD = 5 V), which indicates that the ZnO nFET has a higher drive strength than the Te pFET and results in NMH being larger than NML. At VDD = 1 V, NMH is close to zero, so VDD of 2 V or higher is required for adequate noise margins. To evaluate dynamic circuit operation after irradiation, ring oscillators comprising three, five, and seven inverter stages were characterized. The time-domain waveforms show sustained oscillation for all three configurations at VDD = 5 V (Figure 7d). The output amplitudes (approximately 0.3–0.6 V) are much smaller than VDD. During oscillation, each inverter drives the input capacitance of the following stage, together with parasitic capacitances associated with gate–source/drain overlap and interconnects. The finite pull-up and pull-down currents limit the rate at which these capacitances are charged and discharged. The reduced swings and rounded waveforms are consistent with the output nodes reversing direction before fully settling toward the supply rails under these dynamic loading conditions [46]. The output swing may be improved by reducing gate–source/drain overlap and interconnect length to minimize parasitic capacitance, while optimizing transistor dimensions to balance drive strength and capacitive loading [46,47]. The oscillation frequency increases with VDD and decreases with the number of stages, reaching approximately 43.5, 21.5, and 16.0 kHz for the three-, five-, and seven-stage oscillators, respectively, at VDD = 5 V (Figure 7e). The average propagation delay per stage was calculated using τd = 1/(2Nfosc), where N is the number of inverter stages and fosc is the oscillation frequency. The extracted delays decrease with increasing VDD and remain comparable across the three configurations (Figure 7f), consistent with the lower oscillation frequencies arising mainly from the increased number of stages in the feedback loop. These results show static inverter operation and ring oscillation after 400 krad. The inverter transfer characteristics, gain, and noise margins describe static switching, and the ring oscillators show dynamic operation of interconnected CFET stages. The small oscillator output swing may result from limited drive current, unequal pull-up and pull-down strengths, and capacitive loading by the following stages, interconnects, and measurement setup, which prevent the output nodes from reaching the supply rails within each cycle. The output swing must be improved for reliable logic-level transfer to subsequent stages.
Figure 7. Circuit characteristics of ZnO/Te CFET inverters and ring oscillators after gamma-ray irradiation at 400 krad. (a) Voltage transfer characteristics and corresponding voltage gains of the CFET inverter at supply voltages (VDD) from 1 to 5 V. (b) Supply current (IDD) as a function of input voltage at different VDD values. (c) Low (NML) and high (NMH) noise margins and the normalized total noise margin, (NML + NMH)/VDD, as functions of VDD. (d) Output waveforms of three-, five-, and seven-stage ring oscillators at VDD = 5 V, from top to bottom. (e) Oscillation frequency and (f) propagation delay per stage as functions of VDD for the three-, five-, and seven-stage ring oscillators.
For comparison, Figure 8 shows the characteristics of comparable ZnO/Te CFET inverters and ring oscillators before irradiation. The pristine inverter shows nearly full output swings over VDD = 1–5 V and a maximum voltage gain of 38.4 V/V at VDD = 5 V (Figure 8a). The supply current peaks near the switching point and increases with VDD (Figure 8b). NML and NMH increase with VDD and reach 1.27 and 2.62 V, respectively, at VDD = 5 V, giving a normalized total noise margin of about 0.78 (Figure 8c). All three ring oscillators oscillate at VDD = 5 V (Figure 8d). The oscillation frequency increases with VDD and decreases with the number of stages; at VDD = 5 V, it is about 38, 20, and 14 kHz for the three-, five-, and seven-stage oscillators, respectively (Figure 8e). The propagation delay per stage decreases with increasing VDD (Figure 8f). After 400 krad (Figure 7), the inverter gain and NML are lower (34.6 V/V and 0.92 V), whereas NMH and the oscillation frequencies are similar or slightly higher. The ring-oscillator output swing is already small before irradiation; therefore, the small swing after irradiation is not caused mainly by irradiation.
Figure 8. Circuit characteristics of ZnO/Te CFET inverters and ring oscillators before gamma-ray irradiation. (a) Voltage transfer characteristics and corresponding voltage gains of the CFET inverter at supply voltages (VDD) from 1 to 5 V. (b) Supply current (IDD) as a function of input voltage at different VDD values. (c) Low (NML) and high (NMH) noise margins and the normalized total noise margin, (NML + NMH)/VDD, as functions of VDD. (d) Output waveforms of three-, five-, and seven-stage ring oscillators at VDD = 5 V, from top to bottom. (e) Oscillation frequency and (f) propagation delay per stage as functions of VDD for the three-, five-, and seven-stage ring oscillators.
Table 2 compares the present devices with previously reported oxide, chalcogenide, and silicon CMOS transistors. Because the irradiation conditions differ among the studies, the comparison is qualitative. The previous studies listed report n- or p-channel transistors only, whereas this work reports both polarities fabricated in one low-temperature CFET process, together with circuit operation after 400 krad.
Table 2. Radiation tolerance of oxide, chalcogenide, and silicon CMOS transistors reported previously and in this work.

4. Conclusions

We investigated the gamma-ray response of vertically integrated ZnO/Te complementary field-effect transistors fabricated at temperatures not exceeding 150 °C. Without passivation, the on-state currents of ZnO nFETs and Te pFETs decreased by 97% and 80%, respectively, after 400 krad. Al2O3 passivation incorporated into the integration process substantially reduced these changes, limiting the ΔVth values of both transistor types to below 75 mV up to 400 krad. The electrical and XPS results are consistent with a mechanism in which Al2O3 passivation preserves channel conduction by limiting surface chemical changes associated with electron depletion in ZnO and suppressing further oxidation of Te. After irradiation, the passivated devices showed ΔVth magnitudes below 60 mV for ZnO nFETs and 0.20 V for Te pFETs after 1000 s of PBS and NBS, respectively, comparable to those before irradiation. Their transfer characteristics also remained nearly unchanged over 30 days of storage in ambient air. At the circuit level, CFET inverters exhibited nearly full output swings and a maximum voltage gain of 34.6 V/V at VDD = 5 V following irradiation at 400 krad, and three-, five-, and seven-stage ring oscillators also sustained oscillation, showing that interconnected complementary devices remain functional after irradiation. Under unbiased 60Co irradiation at 1 kGy/h up to 400 krad, we evaluated both transistor polarities at multiple doses, together with XPS analysis, post-irradiation bias-stress measurements, and circuit characterization. The results show that channel passivation can be incorporated into low-temperature CFET fabrication to improve the gamma-ray tolerance of both transistor polarities. To assess applicability to space electronics compatible with BEOL and M3D integration, further work is needed: irradiation under operating bias and at different dose rates, separation of irradiation effects from ambient aging, improvement of the ring-oscillator output swing, comparison of the same circuits before and after irradiation, and statistics across multiple circuits.

Author Contributions

Conceptualization, J.-H.C. and J.-H.J.; methodology, J.-H.C. and J.-H.J.; validation, J.-H.C., J.-H.J., G.W.K. and C.B.L.; formal analysis, J.-H.C., J.-H.J., B.G.K.; investigation, J.-H.C., J.-H.J. and U.S.; data curation, J.-H.C. and N.K.; writing—original draft preparation, J.-H.C., J.-H.J., and B.H.L.; writing—review and editing, B.H.L.; visualization, J.-H.C., J.-H.J., C.B.L. and B.H.L.; supervision, B.H.L.; project administration, B.H.L.; resources, B.H.L.; funding acquisition, B.H.L., J.-H.C. and J.-H.J. contributed equally to this work. All authors have read and agreed to the published version of the manuscript.

Funding

This research was supported by Korea Basic Science Institute (National research Facilities and Equipment Center) grant (RS-2024-00434439) and by Basic Science Research Program (RS-2025-25410048) funded by the Ministry of Education (MOE), Korea and by Advanced Materials Technology Strengthening and Transfer Program (RS-2026-25541332) and by Core Technology Development Project for National Semiconductor Research Laboratory (RS-2023-00260813) through the NRF funded by the Ministry of Science and ICT (MSIT), Korea.

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Prinzie, J.; Simanjuntak, F.M.; Leroux, P.; Prodromakis, T. Low-Power Electronic Technologies for Harsh Radiation Environments. Nat. Electron. 2021, 4, 243–253. [Google Scholar] [CrossRef] [Scilit]
  2. Barth, J.L.; Dyer, C.S.; Stassinopoulos, E.G. Space, Atmospheric, and Terrestrial Radiation Environments. IEEE Trans. Nucl. Sci. 2003, 50, 466–482. [Google Scholar] [CrossRef] [Scilit]
  3. Oldham, T.R.; McLean, F.B. Total Ionizing Dose Effects in MOS Oxides and Devices. IEEE Trans. Nucl. Sci. 2003, 50, 483–499. [Google Scholar] [CrossRef] [Scilit]
  4. Barnaby, H.J. Total-Ionizing-Dose Effects in Modern CMOS Technologies. IEEE Trans. Nucl. Sci. 2006, 53, 3103–3121. [Google Scholar] [CrossRef] [Scilit]
  5. Hughes, H.L.; Benedetto, J.M. Radiation Effects and Hardening of MOS Technology: Devices and Circuits. IEEE Trans. Nucl. Sci. 2003, 50, 500–521. [Google Scholar] [CrossRef] [Scilit]
  6. Toto, E.; Lambertini, L.; Laurenzi, S.; Santonicola, M.G. Recent Advances and Challenges in Polymer-Based Materials for Space Radiation Shielding. Polymers 2024, 16, 382. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  7. Cao, W.; Bu, H.; Vinet, M.; Cao, M.; Takagi, S.; Hwang, S.; Ghani, T.; Banerjee, K. The Future Transistors. Nature 2023, 620, 501–515. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  8. Salahuddin, S.; Ni, K.; Datta, S. The Era of Hyper-Scaling in Electronics. Nat. Electron. 2018, 1, 442–450. [Google Scholar] [CrossRef] [Scilit]
  9. Datta, S.; Dutta, S.; Grisafe, B.; Smith, J.; Srinivasa, S.; Ye, H. Back-End-of-Line Compatible Transistors for Monolithic 3-D Integration. IEEE Micro 2019, 39, 8–15. [Google Scholar] [CrossRef] [Scilit]
  10. Belmonte, A.; Oh, H.; Rassoul, N.; Donadio, G.L.; Mitard, J.; Dekkers, H.; Delhougne, R.; Subhechha, S.; Vaisman Chasin, A.; van Setten, M.; et al. Capacitor-Less, Long-Retention (>400 s) DRAM Cell Paving the Way towards Low-Power and High-Density Monolithic 3D DRAM. In Proceedings of the 2020 IEEE International Electron Devices Meeting (IEDM), San Francisco, CA, USA, 12–18 December 2020; pp. 28.2.1–28.2.4. [Google Scholar] [CrossRef] [Scilit]
  11. Beyne, E.; Jourdain, A.; Beyer, G. Nano-Through Silicon Vias (nTSV) for Backside Power Delivery Networks (BSPDN). In Proceedings of the 2023 IEEE Symposium on VLSI Technology and Circuits, Kyoto, Japan, 11–16 June 2023; pp. 1–2. [Google Scholar] [CrossRef] [Scilit]
  12. Dozier, C.M.; Brown, D.B. Photon Energy Dependence of Radiation Effects in MOS Structures. IEEE Trans. Nucl. Sci. 1980, 27, 1694–1699. [Google Scholar] [CrossRef] [Scilit]
  13. Schwank, J.R.; Shaneyfelt, M.R.; Fleetwood, D.M.; Felix, J.A.; Dodd, P.E.; Paillet, P.; Ferlet-Cavrois, V. Radiation Effects in MOS Oxides. IEEE Trans. Nucl. Sci. 2008, 55, 1833–1853. [Google Scholar] [CrossRef] [Scilit]
  14. Levy, D.H.; Freeman, D.; Nelson, S.F.; Cowdery-Corvan, P.J.; Irving, L.M. Stable ZnO Thin Film Transistors by Fast Open Air Atomic Layer Deposition. Appl. Phys. Lett. 2008, 92, 192101. [Google Scholar] [CrossRef] [Scilit]
  15. Zhao, C.; Tan, C.; Lien, D.-H.; Song, X.; Amani, M.; Hettick, M.; Nyein, H.Y.Y.; Yuan, Z.; Li, L.; Scott, M.C.; et al. Evaporated Tellurium Thin Films for p-Type Field-Effect Transistors and Circuits. Nat. Nanotechnol. 2020, 15, 53–58. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  16. Kim, T.; Choi, C.H.; Byeon, P.; Lee, M.; Song, A.; Chung, K.-B.; Han, S.; Chung, S.-Y.; Park, K.-S.; Jeong, J.K. Growth of High-Quality Semiconducting Tellurium Films for High-Performance p-Channel Field-Effect Transistors with Wafer-Scale Uniformity. npj 2D Mater. Appl. 2022, 6, 4. [Google Scholar] [CrossRef] [Scilit]
  17. Kim, M.; Lee, Y.; Kim, K.; Pham, G.-H.; Kim, K.; Jun, J.H.; Lee, H.-W.; Yoon, S.; Hwang, H.J.; Sung, M.M.; et al. Processes to Enable Hysteresis-Free Operation of Ultrathin ALD Te p-Channel Field-Effect Transistors. Nanoscale Horiz. 2024, 9, 1990–1998. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  18. Kim, K.; Kim, M.; Lee, Y.; Lee, H.-W.; Jun, J.H.; Choi, J.-H.; Yoon, S.; Hwang, H.-J.; Lee, B.H. Demonstration of Vertically Stacked ZnO/Te Complementary Field-Effect Transistor. Adv. Electron. Mater. 2025, 11, 2500031. [Google Scholar] [CrossRef] [Scilit]
  19. Jun, J.H.; Lee, Y.; Lee, H.-W.; Kim, M.; Kim, S.-M.; Lee, C.B.; Kim, K.; Lee, B.H. Applications of a ZnO–Te Antiambipolar Switch for Drastic Power and Area Scaling. ACS Appl. Mater. Interfaces 2025, 17, 10815–10823. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  20. Jun, J.H.; Kim, B.G.; Kang, M.S.; Shin, U.G.; Kim, M.; Kim, K.; Lee, H.-W.; Lee, Y.; Lee, B.H. Multi-Functional ZnO–Te Heterojunction Devices Enabling Compact Frequency Quadrupler. Adv. Funct. Mater. 2026, 36, e74948. [Google Scholar] [CrossRef] [Scilit]
  21. Niu, C.; Tan, P.; Lin, J.-Y.; Long, L.; Lin, Z.; Zhang, Y.; Wang, H.; Wilk, G.D.; Ye, P.D. First Demonstration of BEOL Wafer-Scale All-ALD Channel CFETs Using IGZO and Te for Monolithic 3D Integration. In Proceedings of the 2024 IEEE International Electron Devices Meeting (IEDM), San Francisco, CA, USA, 7–11 December 2024; pp. 1–4. [Google Scholar] [CrossRef] [Scilit]
  22. Rasmidi, R.; Duinong, M.; Chee, F.P. Radiation Damage Effects on Zinc Oxide (ZnO)-Based Semiconductor Devices—A Review. Radiat. Phys. Chem. 2021, 184, 109455. [Google Scholar] [CrossRef] [Scilit]
  23. Ramirez, J.I.; Li, Y.V.; Basantani, H.; Leedy, K.; Bayraktaroglu, B.; Jessen, G.H.; Jackson, T.N. Radiation-Hard ZnO Thin Film Transistors. IEEE Trans. Nucl. Sci. 2015, 62, 1399–1404. [Google Scholar] [CrossRef] [Scilit]
  24. Indluru, A.; Holbert, K.E.; Alford, T.L. Gamma Radiation Effects on Indium-Zinc Oxide Thin-Film Transistors. Thin Solid Films 2013, 539, 342–344. [Google Scholar] [CrossRef] [Scilit]
  25. Jung, S.; Yoo, J.; Lee, H.; Park, S.; Song, H.; Kim, S.; Lim, S.; Park, M.; Jung, S.M.; Won, D.; et al. Unveiling Radiation-Tolerant Thickness in a-IGZO Thin-Film Transistors with Sub-10 nm Film and Restoring Abnormalities via Energy-Efficient Electrothermal Annealing. Nano Lett. 2025, 25, 10131–10137. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  26. Park, M.; Yoo, J.; Lee, H.; Song, H.; Kim, S.; Lim, S.; Park, S.; Jeong, J.H.; Kim, B.; Lee, K.; et al. Rapid Thermal Annealing under O2 Ambient to Recover the Deterioration by Gamma-Ray Irradiation in a-IGZO TFTs. Electron. Mater. Lett. 2025, 21, 111–118. [Google Scholar] [CrossRef] [Scilit]
  27. Ding, M. Damage Effect of ALD-Al2O3 Based Metal-Oxide-Semiconductor Structures under Gamma-Ray Irradiation. Micromachines 2021, 12, 661. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  28. Jeong, H.-Y.; Kwon, S.-H.; Joo, H.-J.; Shin, M.-G.; Jeong, H.-S.; Kim, D.-H. Radiation-Tolerant p-Type SnO Thin-Film Transistors. IEEE Electron Device Lett. 2019, 40, 1124–1127. [Google Scholar] [CrossRef] [Scilit]
  29. Lv, T.; Qin, W.; Hong, R.; You, J.; Lv, Y.; Liao, L.; Jiang, C. Radiation Stability of the p-Type SnOx TFT with Al2O3 and HfO2 Passivation Layers. ACS Appl. Electron. Mater. 2024, 6, 8748–8756. [Google Scholar] [CrossRef] [Scilit]
  30. Chaudhary, N.; Bhatt, K.; Khan, T.; Singh, R. Gamma-Induced Stress, Strain and p-Type Doping in MBE-Grown Thin Film MoTe2. Phys. Chem. Chem. Phys. 2024, 26, 22529–22538. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  31. McMorrow, J.J.; Cress, C.D.; Gaviria Rojas, W.A.; Geier, M.L.; Marks, T.J.; Hersam, M.C. Radiation-Hard Complementary Integrated Circuits Based on Semiconducting Single-Walled Carbon Nanotubes. ACS Nano 2017, 11, 2992–3000. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  32. Yatsu, K.; Lee, H.-A.; Kim, D.H.; Park, I.-J.; Kwon, H.-I. Highly Stable Oxide Thin-Film Transistor-Based Complementary Logic Circuits under X-ray Irradiation. ACS Appl. Electron. Mater. 2022, 4, 3606–3614. [Google Scholar] [CrossRef] [Scilit]
  33. Fan, Z.; Wang, D.; Chang, P.-C.; Tseng, W.-Y.; Lu, J.G. ZnO Nanowire Field-Effect Transistor and Oxygen Sensing Property. Appl. Phys. Lett. 2004, 85, 5923–5925. [Google Scholar] [CrossRef] [Scilit]
  34. Yang, S.; Cai, H.; Chen, B.; Ko, C.; Özçelik, V.O.; Ogletree, D.F.; White, C.E.; Shen, Y.; Tongay, S. Environmental Stability of 2D Anisotropic Tellurium Containing Nanomaterials: Anisotropic to Isotropic Transition. Nanoscale 2017, 9, 12288–12294. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  35. Ryckaert, J.; Schuddinck, P.; Weckx, P.; Bouche, G.; Vincent, B.; Smith, J.; Sherazi, Y.; Mallik, A.; Mertens, H.; Demuynck, S.; et al. The Complementary FET (CFET) for CMOS Scaling beyond N3. In Proceedings of the 2018 IEEE Symposium on VLSI Technology, Honolulu, HI, USA, 18–22 June 2018; pp. 141–142. [Google Scholar] [CrossRef] [Scilit]
  36. Lee, Y.; Lee, H.-W.; Kim, S.J.; Park, J.M.; Lee, B.H.; Kang, C.G. Enhanced High-Energy Proton Radiation Hardness of ZnO Thin-Film Transistors with a Passivation Layer. Nano Converg. 2025, 12, 7. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  37. Hwang, S.-H.; Yatsu, K.; Lee, D.-H.; Park, I.-J.; Kwon, H.-I. Effects of Al2O3 Surface Passivation on the Radiation Hardness of IGTO Thin Films for Thin-Film Transistor Applications. Appl. Surf. Sci. 2022, 578, 152096. [Google Scholar] [CrossRef] [Scilit]
  38. Frankcombe, T.J.; Liu, Y. Interpretation of Oxygen 1s X-ray Photoelectron Spectroscopy of ZnO. Chem. Mater. 2023, 35, 5468–5474. [Google Scholar] [CrossRef] [Scilit]
  39. Idriss, H. On the Wrong Assignment of the XPS O1s Signal at 531–532 eV Attributed to Oxygen Vacancies in Photo- and Electro-Catalysts for Water Splitting and Other Materials Applications. Surf. Sci. 2021, 712, 121894. [Google Scholar] [CrossRef] [Scilit]
  40. Popov, A.I.; Kotomin, E.A.; Maier, J. Basic Properties of the F-Type Centers in Halides, Oxides and Perovskites. Nucl. Instrum. Methods Phys. Res. B 2010, 268, 3084–3089. [Google Scholar] [CrossRef] [Scilit]
  41. Fink, K. Ab Initio Cluster Calculations for the Absorption Energies of F and F+ Centers in Bulk ZnO. Phys. Chem. Chem. Phys. 2005, 7, 2999–3004. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  42. Reed, D.T.; Van Konynenburg, R.A. Effect of Ionizing Radiation on Moist Air Systems. MRS Proc. 1987, 112, 393. [Google Scholar] [CrossRef] [Scilit]
  43. Le Caër, S. Water Radiolysis: Influence of Oxide Surfaces on H2 Production under Ionizing Radiation. Water 2011, 3, 235–253. [Google Scholar] [CrossRef] [Scilit]
  44. Kang, D.; Lim, H.; Kim, C.; Song, I.; Park, J.; Park, Y.; Chung, J. Amorphous Gallium Indium Zinc Oxide Thin Film Transistors: Sensitive to Oxygen Molecules. Appl. Phys. Lett. 2007, 90, 192101. [Google Scholar] [CrossRef] [Scilit]
  45. Huang, S.-Y.; Chang, T.-C.; Chen, M.-C.; Chen, T.-C.; Jian, F.-Y.; Chen, Y.-C.; Huang, H.-C.; Gan, D.-S. Improvement in the Bias Stability of Amorphous InGaZnO TFTs Using an Al2O3 Passivation Layer. Surf. Coat. Technol. 2013, 231, 117–121. [Google Scholar] [CrossRef] [Scilit]
  46. Mourey, D.A.; Zhao, D.A.; Sun, J.; Jackson, T.N. Fast PEALD ZnO Thin-Film Transistor Circuits. IEEE Trans. Electron Devices 2010, 57, 530–534. [Google Scholar] [CrossRef] [Scilit]
  47. Borchert, J.W.; Zschieschang, U.; Letzkus, F.; Giorgio, M.; Weitz, R.T.; Caironi, M.; Burghartz, J.N.; Ludwigs, S.; Klauk, H. Flexible Low-Voltage High-Frequency Organic Thin-Film Transistors. Sci. Adv. 2020, 6, eaaz5156. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  48. Ding, L.; Gerardin, S.; Bagatin, M.; Bisello, D.; Mattiazzo, S.; Paccagnella, A. Comparison of Radiation Degradation Induced by X-ray and 3-MeV Protons in 65-nm CMOS Transistors. Chin. Phys. B 2016, 25, 096110. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Article metric data becomes available approximately 24 hours after publication online.