Abstract
Alkaline passive direct methanol fuel cells (DMFCs) are seen as a potential candidate for portable power applications due to their compactness and simplicity. This study presents the development of an anion exchange membrane (AEM)-based alkaline passive DMFC and investigates the effects of key operating parameters: methanol concentration, KOH concentration, temperature and humidity on cell performance. Polarization tests, open-circuit voltage (OCV) measurements, electrochemical impedance spectroscopy (EIS) and linear sweep voltammetry (LSV) were conducted to evaluate cell performance. The results show that fuel cell performance initially improves with increasing methanol concentration, reaches an optimum, and then declines at higher concentrations. A similar trend is observed for KOH concentration. A strong interdependence between methanol and KOH concentrations is found for optimal cell performance. Specifically, for a methanol concentration of 0.5 M, the highest power density is achieved with 1 M KOH; whereas, at 1 M methanol concentration, the optimum power density shifts to a KOH concentration of 3 M. This indicates that the ideal KOH concentration for peak power density is methanol-dependent. LSV results show that fuel crossover increases with higher methanol and KOH concentrations. EIS analysis reveals that ohmic losses increase with methanol concentration but decrease with KOH concentration. The addition of KOH to methanol solution significantly enhances cell performance compared to using methanol solution alone. The fuel cell performance improves continuously with a rise in temperature, mainly due to improved electrochemical kinetics. In contrast, humidity has only a marginal effect on the cell performance: while it reduces ohmic resistance, it also increases cathode flooding and oxygen mass transfer resistance, limiting its overall benefit. This study offers a comprehensive understanding of how operating parameters influence cell performance, and emphasizes that careful selection of these parameters is essential for achieving optimal performance of passive alkaline DMFC.
1. Introduction
Greenhouse gases and global warming have numerous harmful effects on the environment, which have become increasingly evident in recent times through various calamities such as floods, forest fires, and other natural disasters [1]. The shift from hydrocarbon fuels to carbon-neutral technologies, including wind, solar, biomass, and hydrogen, is essential to restrict the temperature rise to 1.5 °C [2,3]. Hydrogen is one of the promising alternative fuels that produces no harmful emissions when used in energy devices [4]. Fuel cells are prominent in hydrogen applications [5].
In a hydrogen cell, energy is directly converted from chemical to electrical through electrochemical reactions, exhibiting greater efficiency than conventional energy devices. The only byproducts in the reaction are water and heat. As there are no moving parts, the fuel cell offers a long-lasting system with silent and environmentally friendly operation [6]. Despite being the most prevalent element on Earth, hydrogen can only be created with energy [7].
The energy density of the fuel plays a major role in selecting a fuel for the fuel cell considered for portable applications. Hydrogen has the highest theoretical gravimetric energy density of any fuel (32.7 kWh kg−1). However, as a gas at ambient conditions, its volumetric energy density is only 0.003 kWh L−1. When compressed to 700 bar, the value rises to only 1.3 kWh L−1, and liquefaction to 2.3 kWh L−1, at the cost of heavy pressure vessels or cryogenic storage. When included with the storage system, the effective gravimetric energy density of hydrogen will be reduced by an order of magnitude or more, making hydrogen difficult to use in small devices [7]. Liquid fuels avoid these storage problems and offer much higher volumetric energy densities. Methanol has a theoretical gravimetric energy density of 6.1 kWh kg−1 and a volumetric energy density of 4.8 kWh L−1. While other liquid fuels like Ethanol (8.0 kWh kg−1, 6.3 kWh L−1) and 2-propanol (9.0 kWh kg−1, 7.1 kWh L−1) are higher in energy density, their complete oxidation requires C–C bond cleavage, which is kinetically slow. Ethylene glycol (5.3 kWh kg−1, 5.9 kWh L−1) and hydrazine (5.2 kWh kg−1, 5.2 kWh L−1) have values comparable to those of methanol. Formic acid has fast oxidation kinetics but a much lower energy density (1.6 kWh kg−1, 2.0 kWh L−1) [8,9]. Also, sodium borohydride is considered one of the primary fuels for fuel cells and has a high theoretical value (9.3 kWh kg−1). But its application is limited by solubility, cost, and the regeneration of borate byproducts [10].
Direct-fed liquid fuel cells (DLFCs) are regarded as a viable alternative to hydrogen fuel cells, as liquid fuels such as methanol and propanol offer greater convenience in storage and transportation. Methanol is the preferred option among various liquid fuels due to the weak bonds (C-H) facilitating faster electrochemical kinetics. In a direct-fed methanol fuel cell (DMFC), liquid methanol is supplied to the fuel cell’s anode without a reformer. It is therefore an attractive fuel for passive, portable DLFCs.
DMFC can be classified as active or passive based on fuel delivery mechanisms and oxidant supply to the electrodes. Active mechanisms, such as pumps, fuel the anode, while blowers provide air or oxygen to the cathode [11]. For passive DMFC, the primary driving forces for the movement of reactants and products are natural phenomena, including diffusion, spontaneous convection, and capillary motion. The passive DMFC features a straightforward design and minimal parasitic power loss, making it appropriate for portable energy applications [12].
DMFC can be further categorized into proton exchange membrane (PEM) type and anion exchange membrane (AEM) type, depending on the electrolyte employed. In a PEM-based DMFC, a proton-conducting polymer membrane serves as the electrolyte, facilitating the passage of hydrogen ions from the anode to the cathode of the fuel cell [13]. Conventional PEM fuel cells commonly use PFSA-based membranes, such as Nafion, which contain fluorinated polymers associated with environmental persistence. In contrast, hydrocarbon-based AEMs can be PFAS-free, potentially reducing dependence on fluorinated materials. Additionally, the alkaline environment of AEM fuel cells enables the use of platinum-group-metal-lean and non-precious-metal catalysts, offering opportunities to reduce cost and reliance on scarce noble metals. However, the overall environmental benefits depend on the materials used throughout the cell. In an AEM-based DMFC, an anion-conducting polymer membrane is used as an electrolyte, and it conducts hydroxide ions from the cathode to the anode. AEM-based fuel cells exhibit faster electrochemical kinetics because of the alkaline environment. Also, as the alkaline environment is less corrosive, the fuel cell components can last longer. The catalysts for AEM-based DMFC shall be non-noble type, which makes the cell economical compared to the PEM-based DMFC. The AEM-based DMFC has garnered increasing interest among researchers due to its advantages [14].
AEM-based DMFC, particularly the active feed, has been reported extensively [15,16,17,18,19,20,21,22,23,24,25,26,27,28,29]. Vecchio et al. [15] assessed the performance of active methanol fuel cells with commercially available membranes and catalysts. Fe-N-C catalysts, Fumasep (FAA-3-50)-based AEM, and FAA3-based anion exchange ionomer (AEI) were used for the cell. The parameters, such as temperature and methanol concentration, were examined. Higa et al. [16] developed a polyvinyl alcohol (PVA) based AEM and studied the electrochemical and physical properties. The single-cell test utilizing an active DMFC generated up to 99.6 mW cm−2 as peak power output. Research conducted by Galvan et al. [17] reported that using a polyphenylene (TPN) membrane with anion exchange ionomer achieved a high-power output of 251.7 mW cm−2 for the active DMFC. In another study, Wang et al. [18] formulated a series of hybrid AEMs with pyridine-functionalized alcohol (PVA-Py) as the membrane matrix, incorporating variable amounts of anion exchange silica precursor (AESP) via the sol-gel process. The maximum power output obtained by the active DMFC tested with the AESP80%/(PVA-Py) membrane was 52.56 mW cm−2 at 80 °C. Ryua et al. [19] synthesized and used the quaternized chitosan-based anion exchange membrane in the active DMFC and found the cell produced a maximum power density of 10.42 mW cm−2. Prakash et al. [20] used the Tokuyama A-006 membrane for the MEA. They studied the active DMFC performance at varying parameters like temperature, concentration of methanol and KOH, oxidant flow, etc., and reported power density between 25 and 168 mW cm−2. Santasalo-Aarnio et al. [21] characterized Fumasep FAA-2 as an AEM to check its suitability for active DMFC. The AEM was found to have one order of magnitude less methanol crossover compared to Nafion115, and the AEM-based DMFC was found to have more potential to be operated with highly concentrated fuel. Sajjad et al. [22] fabricated a guanidinium-based blended AEM, and the cell performance test showed the cell produced a higher open-circuit voltage (up to 0.67 V) than commercially available AEMs (up to 0.47 V). Bunazawa et al. [23] fabricated a membrane electrode assembly (MEA) with a Tokuyama A-006 membrane and anion ionomer. Polarization tests showed better performance of active DMFC at 45.4% mass ionomer content.
Many research papers have reported on AEM-based active DMFC in the recent past, but only a few works reported on AEM-based passive DMFC [30,31,32,33,34,35,36,37,38]. A few research articles on modeling and simulation studies of AEM-based DMFC have been reported recently [30,32,33]. Deng et al. [30] have formulated a model for a passive type of methanol cell, which is two-dimensional and two-phase, to analyze the influence of the microporous layer (MPL) on species movement within the cell. The data presented by Kim et al. [31] were used for the model validation. Xie et al. [32] have come up with a model that is two dimensional suited for the vapor feed type AEM passive methanol fuel cell. Since no experimental data were available on a vapor-feed cell, the experimental data of a liquid-feed cell were used for the model validation. Wang et al. [33] formulated a transient multiphase model used to analyze the operational characteristics of a passive direct methanol fuel cell in an AEM configuration. The model was validated with another mathematical model [30] at the steady-state condition.
Recently, some research studies have reported using the modified Nafion membrane by dipping it in the NaOH solution, making it sodium-conductive, and using it as CEM in the passive alkaline DMFC [34,35]. Najmi et al. [34] used such a modified membrane (Nafion117/NaOH) as CEM in the passive DMFC and evaluated its performance against a standard PEM (Nafion117) based DMFC. It was found that the Nafion117/NaOH-DMFC delivers much higher power compared to Nafion117-DMFC. In another study, Sidharthan and Joseph [35] used a Nafion 117/Na+ membrane to compare the performance with another lab-synthesized polyvinyl alcohol-titanium dioxide membrane.
Some recent attempts have been made to develop AEM-based passive µ-DMFC [36,37]. µ-DMFCs are a prominent power source for micro-electromechanical systems (MEMS), wearable devices, etc. Verjulio et al. [37] fabricated an AEM-based passive µ-DMFC and observed better performance for the gas diffusion electrode-based MEA than the catalyst-coated membrane-based MEA. Verjulio et al. [36] developed a carbon-supported CoSe2 cathode catalyst for the AEM-based passive µ-DMFC in another study. The catalyst showed a better tolerance to methanol crossover. µ-DMFCs have a much smaller active area (<0.5 cm2) compared to the regular DMFCs (>5 cm2) that are intended to power portable electronic devices. Therefore, the µ-DMFCs exhibit different thermo-fluid and electrochemical behavior than regular DMFCs.
Kim et al. [38] assembled a semi-passive (air-breathing) DMFC using a commercial membrane (A-010, TOKUYAMA, Tokyo, Japan) and reported a power density of 12.8 mW cm−2 at 0.3 V with a 7 M methanol solution. A peristaltic pump actively supplied fuel.
A synopsis of the literature review is presented in Table 1. To the best of the authors’ knowledge, only two research articles [31,39] have been reported on experimental studies of liquid-feed passive DMFC using commercial AEM membranes. Kim et al. [31] used Pd–Sn/C as a cathode catalyst in an AEM-based passive DMFC. They performed better than cells with noble metal catalysts at higher methanol concentrations. Kim et al. [39] studied the influence of hydrophobicity on alkaline electrodes in passive DMFCs. The improved alkaline electrode significantly outperformed the conventional acid electrode with a Nafion ionomer, showing a threefold increase in performance.
Table 1.
Summary of the literature survey on passive AEM DMFC.
The performance of the present passive alkaline DMFC was further evaluated against previously reported systems summarized in Table 2. Compared with previously reported passive alkaline DMFCs, the present study provides a systematic evaluation of the influence of methanol concentration, KOH concentration, temperature, and relative humidity on cell performance using a commercial Fumasep FAA-3-PK-130 membrane-based MEA. Although direct performance comparisons must account for differences in catalyst loading, membrane characteristics, active area, and operating conditions, the results demonstrate the importance of jointly optimizing fuel composition and operating conditions to improve passive DMFC performance.
Table 2.
Comparison of the performance and operating characteristics of the present AEM-DMFC with previously reported passive and semi-passive AEM-DMFC.
Although the present study demonstrates improved AEM-DMFC performance under optimized operating conditions, long-term membrane durability remains a concern. High KOH concentrations and elevated temperatures may accelerate AEM degradation, affecting hydroxide-ion transport and membrane integrity [40]. Prolonged methanol exposure may also influence membrane transport and fuel crossover. Recent studies highlight the need to balance ionic conductivity, chemical stability, and mechanical properties when developing durable AEMs [41]. Song et al. [42] further demonstrated the importance of complementary chemical and electrochemical durability assessments in PEMs. However, long-term stability of the Fumasep membrane was not evaluated in this study. Future work should investigate durability through extended cell operation and post-operation membrane characterization.
Despite the growing interest in alkaline direct methanol fuel cells, systematic investigations on fully passive AEM-DMFC systems remain limited. Most reported studies employ active reactant delivery systems, which increase system complexity and introduce parasitic power losses that are undesirable for portable applications. The distinctive contribution of this study is an integrated evaluation of how fuel composition and environmental conditions govern the performance of a fully passive, air-breathing anion exchange membrane direct methanol fuel cell (AEM-DMFC). Using a commercial AEM, the study systematically examines methanol concentration, KOH concentration, operating temperature, and relative humidity, all of which are relevant to portable applications. Polarization and power-density measurements, open-circuit voltage measurements, electrochemical impedance spectroscopy, and linear sweep voltammetry are combined to relate performance trends to hydroxide-ion transport, reaction kinetics, methanol crossover, and mass-transport limitations. Rather than treating these trends solely as changes in power output, this complementary analysis provides a mechanistic basis for identifying a practical operating window for portable power generation.
2. Experimental Details
2.1. Membrane Electrode Assembly (MEA)
The membrane electrode assembly (MEA) was commercially fabricated and supplied by Fuel Cell Store, Bryan, TX, USA. It consisted of a reinforced Fumasep FAA-3-PK-130 anion exchange membrane with a nominal thickness of 130 µm. With corresponding catalyst loadings of 4 mg cm−2 and 2 mg cm−2, platinum–ruthenium (Pt–Ru) acted as the anode catalyst, while platinum black (Pt) served as the cathode catalyst. W1S1010 gas diffusion layers were used on both electrodes, with an active area of 25 cm2 (5 cm × 5 cm). According to the manufacturer’s specifications, the membrane is supplied in dry bromide form, with a reported ion-exchange capacity of 1.1–1.4 meq g−1 and ionic conductivity of 4–8 mS cm−1 in the chloride form. The membrane’s independent OH−-form conversion procedure was not available for verification. The MEA was subjected to the activation procedure described in Section 2.3.1. Since the MEA was commercially fabricated, details regarding ionomer content, catalyst ink formulation, and hot-pressing conditions were not available.
2.2. Single-Cell Fixture
The fuel cell was constructed according to the schematic diagram presented in Figure 1. The picture also depicts the operational concept of the AEM DMFC in relation to chemical processes. The fuel cell comprises an anode end plate, methanol reservoir, anode current collector, membrane electrode assembly (MEA), cathode current collector, and cathode end plate. The current collector was constructed from 1 mm-thick 316L stainless steel plates. Sixty-four holes, each with a diameter of 0.5 cm, were drilled into the plate to facilitate the passage of reactants and products, constituting a total exposure ratio of 50%. The anode end plate, cathode end plate, and methanol reservoir were constructed from transparent acrylic sheets with a thickness of 8 mm. The gaskets used to prevent leakage were Teflon-coated. The methanol reservoir measured 50 mm × 50 mm × 10 mm, allowing it to contain a fuel mixture of 25 mL. A port was established in the methanol reservoir for fuel supply and CO2 extraction.
Figure 1.
Schematic of fuel cell assembly with working principle.
The fuel cell assembly was tightened with an eight-nut bolt arrangement. A torque wrench was used to tighten the nuts with a torque of 7 Nm applied in a star pattern. Figure 2a,b illustrate the components and the cell, respectively.
Figure 2.
(a) Fuel cell components; (b) fuel cell assembly.
2.3. Experimental Setup and Test Conditions:
A Potentiostat (VersaSTAT-3F, Princeton Applied Research-AMETEK SI, Oak Ridge, TN, USA) with an external power booster (KEPCO-BOP20-20M, KEPCO Inc., Flushing, NY, USA) was used for the polarization test, linear sweep voltammetry (LSV), and electrochemical impedance spectroscopy (EIS). The VersaStudio 2.50.3 software application was used with the potentiostat to collect and visualize the experimental data. A hot air oven (SWAMEQUIP) created different ambient temperature conditions. The fuel cell was placed inside the oven during the temperature tests. A temperature and humidity chamber (Jeio Tech—TH-TG-180, Jeio Tech, Daejeon, Republic of Korea) was used for the humidity test. The fuel cell was kept inside the humidity chamber, and different humidity conditions were created.
2.3.1. Fuel Cell Activation
The fuel cell was activated with 1 M methanol solution and kept for 12 h. It was then set to run at 0.3 V for another 12 h, followed by a polarization test. The test was repeated until a stable curve was obtained.
2.3.2. Open Circuit Voltage (OCV)
The open-circuit voltage (OCV) was monitored continuously for 60 min after introducing the fuel solution into the cell reservoir. To minimize the influence of transient fluctuations, the representative OCV was determined by averaging the voltage readings recorded during the final 5 min of the measurement period.
Figure S1 presents the OCV variation over 60 min for the different operating conditions. An initial variation in cell voltage was observed, followed by a gradual stabilization as the measurement progressed. Towards the end of the 60 min period, the OCV profiles exhibited relatively small fluctuations. The standard deviation calculated from the final 10 recorded values (Table S1) ranged from 0.207 to 2.084 mV, indicating limited voltage variation during the final measurement period. Therefore, the average OCV over the final 5 min was used for comparison of cell performance under the different operating conditions.
2.3.3. Polarization Test
Polarization measurements were performed at room temperature (25 °C) immediately after recording the open-circuit voltage (OCV). The cell voltage was decreased from the measured OCV to 0 V in successive 10 mV steps. At each voltage step, the cell was held for 30 s, and the corresponding current was recorded. The current density was calculated by dividing the measured current by the active electrode area (25 cm2). The power density was subsequently calculated as the product of cell voltage and current density.
The repeatability of the cell performance was evaluated by conducting three consecutive polarization measurements immediately after the cell activation, followed by periodic measurements during the fuel cell testing. Each time, the standard deviation among the repeated measurements was found to be very small, confirming the repeatability of the cell performance.
2.3.4. Linear Sweep Voltammetry (LSV)
LSV quantifies the crossover of fuel in a DMFC coupled with a potentiostat. The cathode and anode act as the working electrode and reference electrode, respectively. The cathode potential was swept from 0 V to 1.2 V at 2 mV/s.
2.3.5. Electrochemical Impedance Spectroscopy (EIS)
The study used Electrochemical Impedance Spectroscopy (EIS) to analyze fuel cell losses and supplement polarization test results. The fuel cell was run at constant voltage for 10 min before EIS tests. EIS spectra were measured in potentiostatic mode, with 10 points per decade, over a frequency range spanning 100 kHz to 0.01 Hz, with an AC voltage at 20 mV amplitude, and the Nyquist curve was plotted to examine the data.
The experimental investigations were conducted using a one-factor-at-a-time (OFAT) approach, in which one operating parameter was varied while the remaining parameters were maintained constant at their specified values. Therefore, a full factorial experimental design was not employed. The investigated operating conditions are summarized in Table S2, which has been included in the Additional Data.
3. Results and Discussion
3.1. Effect of Methanol Concentration (KOH Concentration: 1 M)
The influence of methanol concentration on the performance of DMFC is studied with I-V Curve and I-P Curve, as shown in Figure 3a and Figure 3b, respectively. The methanol content varied between 0.25 M and 3 M. The KOH concentration was kept fixed at 1 M during all the experiments. The curves indicate that the overall performance of the cell (and maximum power) increases initially when the methanol concentration increases from 0.25 M to 0.5 M. The maximum fuel cell power is achieved at a methanol concentration of 0.5 M, producing a power density of 2.32 mW cm−2. Cell performance and maximum power consistently decline with a further increase in methanol content. The initial rise in cell performance with increased methanol concentration is attributable to the greater availability of methanol molecules at the anode for the electrochemical reaction. On the other hand, methanol crossover increases with increasing methanol concentration, leading to cathode overpotential and obstructing the oxygen reduction reaction. Increasing the methanol concentration beyond 0.5 M results in the predominance of methanol crossover, leading to a decline in cell performance. The methanol crossover to the cathode also increases over time. When the presence of methanol at the cathode rises above the desired level, the cathodic reaction slows down, and the performance declines. From the perspective of portable power applications, the developed AEM-DMFC demonstrated a maximum power density of 2.18 mW cm−2 at 30 °C, corresponding to an estimated peak cell power of 54.5 mW for the 25 cm2 active area. At 70 °C, the maximum power density increased to 4.06 mW cm−2, corresponding to an estimated peak power of 101.5 mW.
Figure 3.
Effect of methanol concentration on (a) current vs. voltage (I-V) curve, (b) current vs. power (I-P) curve, (c) open-circuit voltage (OCV), (d) linear sweep voltammetry curves and (e) electrochemical impedance spectra represented as Nyquist plots (constant concentration of KOH: 1 M), and (f) equivalent circuit.
To further evaluate the operational behavior of the cell, a long-duration constant-voltage test was conducted at 0.3 V for 15,000 s (approximately 4.17 h), as presented in Figure S2. The current density gradually decreased from approximately 6.6 to 1.75 mA cm−2 during this period, indicating continuous current generation accompanied by a decline in output. This test provides an additional assessment of cell operation under sustained electrical loading. However, it does not establish dynamic-load response or long-term durability. Therefore, further investigations involving dynamic-load operation, extended durability testing, and system-level integration are necessary to establish the practical suitability of the developed cell for portable power applications.
It can also be seen in Figure 3a and Figure 3b that, at low methanol concentrations (0.25 and 0.5 M), a sudden decrease in power density was observed at higher current densities. This behavior may be attributed to limited methanol availability at the anode under passive operating conditions. As current density increases, methanol consumption may exceed its diffusion-driven replenishment rate, resulting in concentration polarization and a reduction in cell voltage. Consequently, the decrease in voltage may outweigh the increase in current density, leading to a reduction in power density. This effect is expected to be more pronounced at lower methanol concentrations because of the limited fuel availability.
Figure 3c displays the relation between open-circuit voltage and methanol concentration. It can be noticed that the OCV falls progressively when the methanol content is raised. The highest OCV is at 0.25 M (0.9 V), while the lowest OCV is at 3 M (0.79 V). The membrane used in this study was Fumasep (FAA-3-PK-130, Fumatech, Bietigheim-Bissingen, Germany), with a thickness of 130 µm. As reported in previous studies [33], AEM exhibits methanol crossover, even though it is less than in polymer electrode membranes. When the crossover methanol reaches the cathode, it oxidizes in the presence of oxygen, resulting in voltage loss.
Figure 3d shows the linear sweep voltammetry curve, which indicates the methanol crossover. The KOH concentration was kept constant at 1 M during all the experiments. It can be seen from the figure that when the methanol concentration is increased, the LSV curve moves upward, which indicates an increasing methanol crossover. The crossover current density for methanol feed concentrations of 0.25 M, 1 M, and 3 M are 0.42 mA cm−2 (1.7 × 10−6 mol cm−2 s−1), 1.03 mA cm−2 (4.45 × 10−6 mol cm−2 s−1) and 1.45 mA cm−2(6.26 × 10−6 mol cm−2 s−1) in that order. Methanol crossover escalates 2.5-fold as methanol content rises from 0.25 M to 1 M and 3.6-fold as it increases to 3 M.
Figure 3a (IV Curve) shows that the activation loss is almost identical for all methanol concentrations. In contrast, the ohmic loss (the slope of the curve beyond the activation region) increases gradually with increasing concentration. As the methanol content increased, the solution’s composition became increasingly methanol-rich, thereby modifying the solvent environment. This alteration may affect ion transport characteristics, likely attributable to variations in solvent dielectric constant and enhanced methanol deprotonation in alkaline environments. KOH is essential for the conductive properties of the membrane. More KOH in the solution will provide more OH− ions; therefore, the membrane’s conductivity rises and vice versa. Meanwhile, increasing the methanol content results in diminished membrane conductivity and heightened ohmic loss. This is also apparent from Figure 3e.
Figure 3a indicates that mass transport loss is evident at methanol concentrations of 0.25 M and 0.5 M but not apparent at concentrations of 1 M and higher. The short-circuit current (SSC) increases from 2.7 mA cm−2 at 0.25 M to 6.26 mA cm−2 at 0.5 M and 11.5 mA cm−2 at 1 M. It stays at around 11.5 mA cm−2 for 2 M methanol concentration and decreases to 8.9 mA cm−2, subsequently increasing the concentration to 3 M. The mass transport loss decreases continuously as the methanol concentration increases. Increasing the methanol content in the fuel reservoir enhances the rate of methanol mass transfer by diffusion toward the catalyst layer. Therefore, the availability of methanol molecules at the catalyst layer improves, ultimately decreasing mass transport loss. This is also evident from Figure 3e.
Figure 3e displays the electrochemical impedance spectra of the fuel cell as Nyquist plots for methanol at 0.25 M, 1 M, and 3 M, while the KOH concentration is held constant at 1 M. The plot was drawn with real impedance (Zre) data against negative imaginary impedance (−Zim) data. Figure 3f shows the equivalent circuit followed for the study. In this circuit, Rs is the ohmic resistance of the membrane, electrodes, and contacts; Rct is the overall charge-transfer resistance of the methanol oxidation and oxygen reduction reactions; and a constant phase element (CPE) accounts for the non-ideal double-layer capacitance of the porous electrodes. The shape of the plot reveals different types of losses within the fuel cell. The graph displays two semi-circles representing the high-frequency and low-frequency zones. On the left side of the graph, the high-frequency arc intersects the real impedance axis. The intercept signifies the fuel cell’s ohmic resistance (Rs), encompassing both its components’ electronic resistance and the membrane’s ionic resistance. As shown in Figure 3e, the real-axis intercept (ohmic resistance) increases from 14.5 Ω cm2 to 15.8 Ω cm2 as the methanol concentration increases from 0.25 M to 3 M. The increase in methanol concentration increases the methanol content in the membrane. Hydroxide transport in AEMs proceeds through both vehicular diffusion and Grotthuss-type hopping along the hydrogen-bonded water network of the hydrophilic domains, with the vehicular contribution being dominant [43]. Methanol absorbed into the membrane is therefore likely to dilute the water in these domains, reducing their continuity and hindering OH− transport while increasing ohmic resistance. In a recent work by Guo et al. [44], the authors added a small amount (0.5 wt%) of fluorinated graphite to sulfonated poly(ether ether ketone) (SPEEK) membranes, thereby reducing water uptake and swelling while maintaining high conductivity. Even though their work on PEM-based membranes improved hydrogen fuel cells, the principle can be applied to AEM-based DMFCs. Thus, membrane composition control can enable the engineering of ion-conducting channels to maintain conductivity and improve cell performance. Future work shall investigate modifying the membrane with fillers that limit methanol uptake and crossover while keeping hydroxide-conducting pathways. Such membranes would be particularly useful in passive DMFCs, where higher methanol concentrations are needed to sustain fuel supply without pumping.
The high-frequency arc shows activation losses at both anode and cathode, representing voltage losses associated with overcoming the activation barriers for the electrode reactions. The consistency in the diameter of the high-frequency arc across different methanol concentrations suggests that activation losses remain unchanged regardless of concentration. This observation is complemented by the results in the I-V curves discussed earlier.
The right side of the Nyquist figure represents the mass transfer barrier of methanol and oxygen. Figure 3e shows that as methanol concentration rises, the arc diameter of the plot reduces. This leads to a continuous decrease in mass transport barriers. As fuel concentration increases, the availability of methanol to the catalyst layer improves. This reduces the mass transport loss, especially at higher current. The I-V curves in Figure 3a also reflect this, showing that the fuel cell has a very high mass transport loss and the lowest limiting current in a 0.5 M solution, which improves as the methanol concentration increases from this level.
To quantitatively evaluate methanol crossover, the apparent methanol flux was calculated from the crossover current density using Faraday’s law, as expressed in Equation
where JMeOH is the apparent methanol crossover flux (mol cm−2 s−1), icross is the crossover current density (A cm−2), and F is Faraday’s constant (96,485 C mol−1). The factor 6 represents the number of electrons involved in the complete oxidation of one methanol molecule. The crossover current density and the methanol crossover flux for various methanol concentrations are summarized in Table 3.
JMeOH = icross/6F
Table 3.
Effect of methanol concentration on methanol crossover.
3.2. Effect of Methanol Concentration (KOH Concentration: 3 M)
The studies on methanol concentration influencing the performance of DMFC were replicated using a 3 M KOH concentration, with the findings illustrated in Figure 4a,b. The methanol content ranged from 0.25 M to 3 M, while that of KOH remained constant at 3 M throughout all trials. A similar trend observed for the 1 M KOH concentration (Figure 3a,b) was observed for the 3 M KOH concentration as well. The cell performance and power density initially rise with increasing methanol concentration, reach an optimal point, and subsequently decline with additional increases in methanol concentration. However, in a solution of 3 M KOH concentration, the peak power density (2.81 mW cm−2) was observed at a methanol concentration of 1 M, contrary to the case of 1 M KOH, where the peak power was observed at 0.5 M methanol content. The higher optimum methanol concentration at higher KOH concentration comes from two effects. First, methanol and OH− are both anodic reactants and compete for the same active sites. As Yu et al. [45] discussed, the OH− to CH3OH ratio shows which species dominates the catalyst surface. At 1 M KOH, increasing methanol from 0.5 to 1 M lowers the ratio from 2:1 to 1:1. Methanol species then crowd the surface, leaving too little adsorbed OH− to oxidize the intermediates. At 3 M KOH, the 3:1 ratio with 1 M methanol keeps the surface balanced, while at 6:1 (0.5 M methanol) the fuel supply becomes limiting. Second, the passive cell supplies methanol only by diffusion. Higher KOH concentration speeds up anode kinetics and reduces ohmic losses, so the cell runs at higher current densities and uses methanol more quickly. At 3 M KOH, 0.5 M methanol cannot diffuse quickly enough, while 1 M creates a steeper concentration gradient that supplies enough methanol to keep up with the current. Furthermore, at 3 M KOH, the cell performance surpasses that of 1 M KOH across all methanol concentrations (0.25 M to 3 M). The cell performance is likewise reliant upon the KOH concentration. To explore this further, we evaluated the cell performance at various KOH concentrations while keeping the methanol concentration fixed, which is presented in the next section.
Figure 4.
Effect of methanol concentration on (a) current vs. voltage (I-V) curve, (b) current vs. power (I-P) curve, (c) open-circuit voltage (constant concentration of KOH: 3 M).
Figure 4a,b also show that mass transport losses are visible for nearly all methanol feed concentrations, from 0.25 M to 3 M. On the other hand, for 1 M KOH (Figure 3a,b), the mass transport losses were visible only for methanol concentrations at 0.25 M and 0.5 M. This indicates that as KOH concentration increases, mass transport loss increases. This is because for 3 M KOH, the solution will be less methanol-rich, and therefore, the catalyst site will have less methanol, resulting in higher fuel starvation than at 1 M KOH.
Figure 4c displays open-circuit voltage (OCV) with respect to methanol feed concentration, maintaining a constant potassium hydroxide (KOH) concentration of 3 M. The open-circuit voltage (OCV) progressively lowers with a rise in methanol concentration, mirroring the trend noted for 1 M KOH (Figure 3c). However, for the same methanol feed concentration, the OCV for 3 M KOH is less than the OCV for 1 M KOH. The research underscores the substantial effect of KOH concentration on fuel cell efficacy, which will be examined in the subsequent section.
The optimum methanol concentration was found to shift from 0.5 M at 1 M KOH to 1 M at 3 M KOH. This behavior suggests that the optimum fuel concentration depends on the alkaline electrolyte concentration. The higher hydroxide-ion availability at 3 M KOH may favor the anode methanol oxidation reaction, allowing the cell to benefit from a higher methanol concentration. However, increasing methanol concentration can also enhance methanol crossover, potentially causing additional voltage losses. The observed shift may therefore result from the combined effects of reactant availability, anode reaction kinetics, and methanol crossover. Since these individual effects were not independently quantified, further investigation is required to establish the precise mechanism.
3.3. Effect of KOH Concentration
Figure 5a,b show the impact of KOH concentration on the I-V curve and the I-P curve, respectively. The KOH concentration ranged from 0.5 M to 10 M, whereas the methanol content remained constant at 1 M throughout all trials. The figures show a continuous increase in overall cell performance and maximum power as the KOH concentration increases from 0.5 M to 1 M, then to 2 M, and finally to 3 M. The peak power remains almost constant for the KOH concentrations of 3 M and 5 M. Optimal cell performance is achieved at a 5 M KOH concentration, yielding a power of 3.76 mW cm−2. When KOH concentration is increased further to 10 M, cell performance decreases significantly. Hydroxyl (OH−) ions serve as the principal charge carriers within the membrane. When KOH concentration increases, the availability of OH− ions increases. This improves the conductivity of ions in the membrane, and so does the performance of the DMFC. This is true only up to specific concentrations (up to 5 M), as visible in the graphs. A further rise in KOH concentration leads to more mass transport loss, hence lowering cell performance. With the highly concentrated KOH solution, there will be more than an adequate quantity of KOH at the anode catalyst layer. Catalyst sites will be occupied mainly by KOH molecules rather than the methanol molecules. This will lead to fuel starvation and higher concentration loss, as seen in the result of 10 M concentration. The trends observed in the IV and IP curves (Figure 5a,b) are the combined effect of the phenomenon discussed above.
Figure 5.
Effect of KOH concentration on (a) current vs. voltage (I-V) curve, (b) current vs. power (I-P) curve, (c) open-circuit voltage, (d) linear sweep voltammetry curves (constant concentration of methanol: 1 M), (e) electrochemical impedance spectra represented as Nyquist plot.
Figure 5a also indicates that the gradient of the I-V curve in the ohmic region is decreasing with respect to the rise in concentration of KOH from 0.5 M to 2 M. The trend persists up to a KOH concentration of 2 M, after which the slope stabilizes at higher KOH concentrations. As previously described, the conductivity of ions in the membrane rises with higher KOH concentrations due to the enhanced availability of OH− ions. Once the trend reaches saturation, increasing the KOH concentration does not further improve the membrane conductivity. The EIS results in Figure 5e also validate the trend. Figure 5e presents the EIS curves for KOH concentrations of 0.5 M, 2 M, and 5 M. The ohmic resistance, represented by the high-frequency intercept on the x-axis, has a value of 14 Ω cm2 for 0.5 M KOH concentration. It reduces to 12 Ω cm2 for 2 M and remains constant for 5 M KOH concentration. The data indicate that when the KOH concentration increases initially, the ohmic resistance declines, enhancing the membrane’s ionic conductivity. This conductivity reaches its optimum and remains almost constant with further increases in the KOH concentration.
It is also evident from the IV curve shown in Figure 5a that the activation region improves as the KOH concentration increases. This is attributed to the higher availability of OH− ions at the anode, which enhances the methanol oxidation reaction. The EIS results depicted in Figure 5e similarly demonstrate that the high-frequency arc, indicative of activation loss, decreases progressively with a rise in KOH concentration.
Further, it can also be observed from Figure 5a that the mass transport loss is clearly visible at all KOH concentrations. The short-circuit current (SSC) keeps decreasing beyond 1 M KOH concentration. There will be more than adequate quantities of KOH at the anode catalyst layer for the highly concentrated KOH solution. This results in KOH molecules occupying the catalyst sites instead of methanol molecules, leading to higher concentration losses. The Nyquist plot in Figure 5e also clearly demonstrates this. The low-frequency arc diameter, representing mass transport resistance, increases with increased KOH concentration.
Figure 5c shows the OCV values at various KOH concentrations ranging from 0.5 M to 10 M, while methanol was kept constant at 1 M concentration. The OCV gradually decreases as the KOH concentration increases. OCV values are 0.87 V, 0.84 V, 0.81 V, 0.79 V and 0.79 V for 0.5 M, 1 M, 2 M, 3 M and 5 M, respectively. The open-circuit voltage (OCV) at KOH concentrations of 5 M and 10 M is nearly identical. The declining trend of OCV is due to the heightened methanol crossover associated with a rise in the concentration of KOH. The LSV results for the methanol crossover also confirm this, as shown in Figure 5d. At 0.5 M KOH concentration, the crossover current density is 0.5 mA cm−2, which almost doubles (1.04 mA cm−2) at 2 M and increases slightly to 1.3 mA cm−2 for 5 M KOH concentration. The initial increase in crossover current density is attributed to (i) faster electro-oxidation of the permeated methanol at the cathode, owing to the greater availability of OH−, and (ii) increased swelling and water uptake of the AEM, which widens its hydrophilic ion-conducting domains and increases methanol diffusivity. Above 2 M KOH, the higher solution viscosity and competitive adsorption of OH− on active sites offset these effects, so the crossover current density levels off [46,47,48,49]. The methanol crossover flux and crossover current density for various KOH concentrations are summarized in Table 4.
Table 4.
Effect of KOH concentration on methanol crossover.
3.4. Effect of Adding KOH into Fuel Cell
To assess the impact of adding KOH to the methanol solution, the fuel cell performance was compared with the methanol-water solution with 1 M KOH and without any KOH (only the methanol-water solution). The effect on the fuel cell performance is shown in Figure 6a (I-V curve) and 6b (I-P curve). The figure shows that the maximum power increased substantially by adding KOH. The maximum power without KOH is 0.26 mW cm−2. Meanwhile, the cell delivered a power density of 2.47 mW cm−2 with KOH in the solution, which is 9.5 times higher. The increase in performance is due to the availability of more OH− ions with the addition of KOH, which increases the ionic conductivity of the membrane as well as improves the anode electrochemical kinetics, as described earlier.
Figure 6.
Effect of adding KOH to the methanol solution on (a) current vs. voltage (I-V) curve, (b) current vs. power (I-P) curve, (c) linear sweep voltammetry curves, (d) electrochemical impedance spectra represented as a Nyquist plot (constant concentration of methanol: 1 M).
It can also be observed in the IV curve (Figure 6a) that the cell without KOH has a larger activation region, which indicates higher activation loss compared to that for 1 M KOH. Also, the IV curve without KOH has a steeper slope in the ohmic region, i.e., higher ohmic loss, than the one with 1 M KOH. This is also evident in the EIS plot shown in Figure 6d, where the high-frequency intersection on the real axis is larger for the curve without KOH, indicating higher ohmic resistance. This signifies that using additives, such as KOH or NaOH, enhances the conductivity of ions in the membrane and improves overall cell efficiency.
Figure 6a shows that the cell with 1 M KOH performs significantly better and reaches the mass-limiting condition at about 7 mA cm−2. Conversely, the limiting current acquired with the cell operating without KOH is 2.7 mA cm−2. This is also evident in the EIS curve (Figure 6d), where for the cell operating with 1 M KOH, the low-frequency arc is bigger compared to that for the cell without KOH. The EIS test was conducted in the potentiostatic mode at 0.3 V. The IV curve (Figure 6a) at 0.3 V demonstrates that the cell using 1 M KOH exhibits a significantly elevated current (7 mA cm−2) and enters the mass transport area. The cell operating without KOH has 0.7 mA cm−2 at 0.3 V and is not in the steep mass transport region; therefore, it has a minor low-frequency arc in the Nyquist plot.
The addition of KOH also elevates methanol crossover, as evidenced by the LSV results presented in Figure 6c. The crossover current density for the fuel cell without KOH is 0.46 mA cm−2, whereas for the cell with KOH, it is 1.03 mA cm−2, indicating a twofold increase. Earlier studies have shown that adding KOH can lead to membrane swelling, resulting in larger pores in the membrane, which can increase the diffusion-driven methanol crossover.
3.5. Effect of Operating Temperature
Fuel cell performance was assessed under various ambient temperature conditions. For this, the fuel cell was placed inside a hot-air oven, and temperatures were set as per the requirement. The fuel concentration was kept constant: 1 M methanol solution with 1 M KOH. We stopped experiments at 70 °C and did not go beyond this temperature, as around this temperature, we observed deformation in the fuel cell fixture, which was made of acrylic, possibly due to the thermal expansion occurring at the high temperature.
The influence of operating temperature on the performance of the passive AEM-DMFC is shown in Figure 7a. The maximum power density increased from 2.18 mW cm−2 at 30 °C to 2.98 mW cm−2 at 40 °C and 3.50 mW cm−2 at 50 °C. It remained approximately constant at 3.50 mW cm−2 at 60 °C before increasing to 4.06 mW cm−2 at 70 °C. Thus, no performance decline was observed within the investigated temperature range, although the improvement was not uniform across all temperature intervals.
Figure 7.
Effect of temperature on (a) current vs. voltage (I-V) curve and current vs. power (I-P) curve, (b) open-circuit voltage, (c) linear sweep voltammetry curves and (d) electrochemical impedance spectra represented as Nyquist plot.
The increase in power density with temperature can be associated with enhanced electrochemical reaction kinetics and reduced ohmic resistance. In the present study, the ohmic resistance decreased from 15.2 Ω cm2 at 30 °C to 11.6 Ω cm2 at 70 °C (Figure 7d), supporting the contribution of reduced ohmic losses to the improved cell performance. However, elevated temperatures may also promote methanol volatilization, water evaporation, changes in membrane hydration, and gas-bubble accumulation, potentially affecting reactant transport and cell operation. These competing effects may become more significant beyond the investigated temperature range.
The experiments were limited to 70 °C because the acrylic cell fixture exhibited deformation near this temperature. Consequently, the temperature corresponding to the maximum achievable performance and any possible performance decline above 70 °C could not be established. Further investigations using a temperature-resistant cell fixture and controlled relative humidity are required to determine the optimum operating temperature while accounting for membrane hydration, fuel evaporation, and mass-transport limitations.
The activation region in the IV curve (Figure 7a) becomes smaller with the rise in temperature. The oxidation rate at the anode and the reduction rate at the cathode both increase with elevated temperatures. The EIS curve in Figure 7d also confirms this phenomenon. The figure shows that the diameter of the high-frequency arc, indicative of activation loss, decreases as the temperature rises.
It can also be seen in the IV curves presented in Figure 7a that the gradient of the curve in the ohmic area decreases with an increase in temperature. It indicates that the ionic conductivity of the membrane improves with a temperature rise. This is also confirmed by the EIS curves (Figure 7d, which show that the high-frequency intercept with the x-axis decreases with an increase in temperature. The value of ohmic resistance at 30 °C is 15.2 Ω cm2, whereas at 70 °C, it reduces to 11.6 Ω cm2. This verifies the enhancement of ionic conductivity in the membrane with an elevation in ambient temperature.
The OCV values for different temperatures are plotted and shown in Figure 7b. The OCV values at 30 °C,40 °C,50 °C, 60 °C and 70 °C are 0.76 V, 0.8 V, 0.83 V, 0.81 V, and 0.79 V, respectively. It can be seen that the OCV values increase first, and the highest value is reported at 50 °C. However, the OCV decreases slightly with a further increase in temperature. As the temperature increases, electrochemical kinetics improve, which has a positive effect on the OCV. Meanwhile, the fuel crossover also increases with the increase in temperature, which has a negative impact on the OCV. The trend of the OCV observed in the figure is the combined effect of these two phenomena.
The correlation between the rise in fuel crossover and the increase in temperature is also apparent from the LSV results presented in Figure 7c. The crossover current density at 30 °C is 1.35 mA cm−2, which increases continuously as the temperature increases and reaches 4.12 mA cm−2 at 70 °C. As operating temperature increases, membrane hydration generally increases due to enhanced water mobility and swelling of the hydrophilic domain. This in turn increases the effective transport pathways available for methanol diffusion through the membrane.
Upon further analysis of the IV curves (Figure 7a), it is evident that mass transport losses are pronounced at lower temperatures (30 °C, 40 °C). However, they decline with rising temperatures and become invisible at elevated temperatures (60 °C and 70 °C). The short-circuit current increases continuously with an increase in temperature from 10.46 mA cm−2 at 30 °C to 24.73 mA cm−2 at 70 °C. The EIS results (Figure 7d) also validate this trend. The diameter of the lower frequency arc, representing the mass transport resistance, decreases continuously with a temperature rise. In a passive DMFC, the transport of methanol and oxygen occurs by natural processes, such as diffusion and natural convection at the anode and cathode, respectively. Fick’s law states that diffusion increases with rising temperature, leading to reduced mass transport loss at both electrodes.
3.6. Effect of Humidity
In the AEM-DMFC, water is essential for the cathodic electrochemical process. Consequently, the quantity of water at the cathode influences the performance. A passive DMFC has an open cathode structure and receives oxygen from the ambient air through natural means, such as diffusion, natural convection, etc. As the cathode is open to the atmosphere, the humidity level of the ambient air influences the cell performance. To explore this, the DMFC was tested under three different relative humidity (RH) conditions: 30%, 60%, and 90%. The fuel composition was maintained at a constant 1 M methanol and 1 M KOH solution, with the cell kept at a stable temperature of 30 °C for the testing.
The effect of relative humidity on the I-V and I-P curves is shown in Figure 8a. It is seen that the overall cell performance (and the maximum power) increases slightly but continuously when the humidity increases from 30% to 60% and then to 90%. The increase in humidity increases water availability at the cathode to drive the oxygen reduction reaction. More humidified air at the cathode also increases the water content of the membrane, thereby increasing the ion conductivity, resulting in better cell performance. The maximum power density obtained at 30% RH is 1.60 mW cm−2 and at 60% RH, it is 1.72 mW cm−2; i.e., an increase of 7.5% in the power density upon increasing the RH by 30%. The optimum power density at 90% RH is 1.82 mW cm−2, which is 5.8% higher than that at 60% RH. It can be concluded that the maximum power density increases with an increase in RH; however, the increment is not very high. This indicates that, to drive the cathode electrochemical reaction, the water that is diffused from the anode to the cathode is sufficient, and therefore the highly humidified air could not add much to the cell power. Figure 8b shows the effect of humidity on the OCV of the fuel cell. The OCV values for 30%, 60%, and 90% RH are 0.82 V, 0.79 V, and 0.79 V, respectively. It can be concluded that with the increase in RH, the OCV decreases only slightly. This is also supported by the LSV results drawn for the methanol crossover and shown in Figure 8c. The LSV graph indicates a modest rise in methanol crossover corresponding to an elevation in relative humidity levels. The crossover current density for RH of 30% is 0.76 mA cm−2, and that for RH of 60% is 0.8 mA cm−2. At 90% RH, the crossover current density rises to 0.96 mA cm−2. The membrane expansion due to increased water absorption at the higher RH could be the reason for the increase in fuel crossover.
Figure 8.
Effect of humidity on (a) current vs. voltage (I-V) curve and current vs. power (I-P) curve, (b) open-circuit voltage, (c) linear sweep voltammetry curves and (d) electrochemical impedance spectra represented as Nyquist plot.
Membrane swelling was not directly characterized in this study; therefore, the observed variation in methanol crossover cannot be directly attributed to changes in membrane swelling. Further investigation involving dimensional swelling and methanol permeability measurements is required to establish this relationship.
Membrane thickness is an important design parameter influencing the performance of AEM-DMFCs. Thinner membranes generally reduce ionic resistance but may increase methanol crossover, resulting in additional voltage and fuel-utilization losses. Consequently, thinner AEMs may favor lower methanol feed concentrations to balance improved ionic transport against crossover. The optimum KOH concentration and operating temperature may also depend on membrane thickness and its associated hydration and transport characteristics. Therefore, membrane thickness optimization, alongside operating-condition selection, is an important consideration for improving passive AEM-DMFC performance.
Figure 8a indicates that the gradient of the I-V curve in the ohmic area decreases slightly as humidity increases. This shows an increase in the conductive nature of the membrane when using humidified air. Figure 8d also displays a similar trend in the EIS curve. The ohmic resistance has a value of 17 Ω cm2 for 30% RH. It reduces slightly to 15 Ω cm2 at 60% RH and further to 14 Ω cm2 at 90% RH. Elevated humidity may promote water retention within the membrane, potentially facilitating proton transport and improving ionic conductivity.
The IV curve in Figure 8a also shows that the activation region is minimally affected by the increase in relative humidity. This observation is also validated in the Nyquist plot shown in Figure 8d, where the high-frequency arc, which represents the activation loss, maintains similar diameters for all three RH conditions. It can also be seen from the IV curve in Figure 8a that the mass transport region is clearly visible for all RH values. Figure 8d of the EIS plot exhibits a notable low-frequency arc, indicative of mass transport resistance, with the diameter of the arc progressively increasing as relative humidity rises. It indicates an increased mass transport barrier to oxygen flow at the cathode due to elevated cathode water flooding at higher relative humidity. Future studies could employ pore-scale modeling approaches, such as the lattice Boltzmann method, to investigate the effects of GDL porosity, compression, and surface wettability on liquid-water and methanol transport.
Since the anode is supplied with liquid methanol solution, external relative humidity may predominantly influence water management and oxygen transport at the cathode. Increasing RH from 30% to 90% reduced the ohmic resistance from 17 to 14 Ω cm2, while the low-frequency impedance contribution increased. These contrasting trends suggest reduced ohmic losses alongside possible mass-transfer limitations at higher humidity. However, membrane hydration and cathode flooding were not independently measured; therefore, their individual contributions cannot be conclusively established. Further investigations involving membrane hydration measurements and oxygen-reduction polarization under controlled humidity are required to distinguish these effects.
At higher relative humidity, liquid-water accumulation within the gas diffusion layer (GDL) may partially obstruct gas-transport pathways and increase oxygen mass-transfer resistance. Yan et al. [50] studied liquid-water transport in compressed GDLs using the lattice Boltzmann method and demonstrated that porosity distribution and compression significantly influence water saturation and transport pathways. Their findings provide pore-scale insight into the possible influence of GDL water accumulation on gas transport. In the present study, the increase in the low-frequency impedance contribution with relative humidity Figure 8d may indicate increased mass-transfer limitations. However, direct visualization of liquid-water accumulation was not performed; therefore, cathode flooding is considered a possible contributing mechanism rather than an experimentally confirmed phenomenon.
In summary, relative humidity affects membrane hydration and water management in passive AEM-DMFCs. The maximum power density increased from 1.60 mW cm−2 at 30% RH to 1.82 mW cm−2 at 90% RH, while ohmic resistance decreased from 17 to 14 Ω cm2. However, the increased low-frequency impedance contribution suggests possible mass-transfer limitations at higher humidity, potentially due to water accumulation within the cathode GDL. Since direct evidence of flooding was not obtained, this observation is interpreted as a possible mass-transfer effect rather than confirmed cathode flooding. Further studies involving oxygen-reduction polarization and GDL wettability and pore-structure characterization are required to verify this mechanism.
4. Conclusions
This paper presents the impact of operational parameters on the AEM-based passive DMFC. The effects of methanol concentration, KOH concentration, temperature, and humidity have been studied. The efficacy of the fuel cell improved with rising methanol content, attained an optimal level, and thereafter declined with further concentration increases. This study achieved the best fuel cell performance with a concentration of 0.5 M methanol and 1 M KOH. This investigation demonstrates a significant correlation between the methanol content yielding optimal cell performance and the concentration of KOH incorporated into the solution. The performance of the fuel cell improved with an initial increase in KOH concentration, reached an optimal level, and subsequently declined with further increase in KOH concentration. This study demonstrated optimal cell performance with 5 M KOH when utilizing 1 M methanol. It was also found that adding KOH to the fuel is essential to improve electrochemical kinetics, as an eight-fold increase in power was observed when 1 M KOH was introduced to the methanol solution, compared to that of a fuel cell operating with only methanol solution. A slight increase in cell performance was visible with a rise in humidity, and more humid air could not add much to the cell power. The LSV studies proved that methanol crossover increases consistently with increasing methanol concentration, KOH content, ambient temperature, and humidity. In this study, EIS results complemented the polarization test results and successfully revealed the nature of losses associated with fuel cells while changing operating parameters. It is advisable to select operational parameters judiciously to optimize cell performance. The present study demonstrates the influence of operating conditions on passive AEM-DMFC performance, long-term operational durability was not investigated. Extended continuous-operation testing is necessary to evaluate membrane degradation, catalyst stability, and performance retention under practical operating conditions. Future work will therefore focus on long-term discharge testing and electrochemical stability assessment to establish the durability and practical applicability of the developed cell for portable power applications.
Supplementary Materials
The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/membranes16120399/s1. Table S1: Standard deviation of the last 10 recorded OCV values; Table S2: Summary of investigated operating parameters and experimental conditions; Figure S1: Open-circuit voltage (OCV) profiles recorded over 60 min at different KOH concentrations, operating temperatures, and relative humidity levels.; Figure S2: Long-duration constant-voltage test of the AEM-DMFC at an applied cell voltage of 0.3 V, showing the variation in current density over 15,000 s.
Author Contributions
Conceptualization, N.K.S. and M.A.; methodology, N.K.S. and M.A.; software, M.A.; validation, M.A.; formal analysis, M.A., N.K.S. and S.P.M.; investigation, M.A.; resources, N.K.S.; data curation, M.A.; writing—original draft preparation, M.A. and S.P.M.; writing—review and editing, N.K.S. and R.K.; visualization, M.A. and S.P.M.; supervision, N.K.S. and R.K.; project administration, N.K.S.; funding acquisition, N.K.S. All authors have read and agreed to the published version of the manuscript.
Funding
This research received no external funding.
Institutional Review Board Statement
Not applicable.
Informed Consent Statement
Not applicable.
Data Availability Statement
The original contributions presented in this study are included in the article/Supplementary Materials. Further inquiries can be directed to the corresponding author.
Acknowledgments
The authors extend their gratitude to BITS Pilani, Dubai Campus, for offering the necessary resources to facilitate this research. The authors express their heartfelt gratitude to Prakash Kumar of the Chemical Engineering Department of BITS Pilani, Dubai Campus, for providing access to the humidity chamber.
Conflicts of Interest
The authors declare no conflict of interest.
References
- Chen, J.; Shi, X.; Gu, L.; Wu, G.; Su, T.; Wang, H.-M.; Kim, J.-S.; Zhang, L.; Xiong, L. Impacts of climate warming on global floods and their implication to current flood defense standards. J. Hydrol. 2023, 618, 129236. [Google Scholar] [CrossRef] [Scilit]
- Yang, S.; Wang, H. Pore-Scale Study of the Effect of Through-Plane Carbon Support Gradients on Catalyst Layer Performance in Proton Exchange Membrane Fuel Cells. Membranes 2026, 16, 326. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ba, T.; Zeng, H.; Wu, W.; Jiao, D.; Huang, Y. A Leaf-Vein-Inspired Composite Flow Channel for Enhanced Mass Transport and Performance in Proton Exchange Membrane Fuel Cells. Membranes 2026, 16, 287. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Nasser, B.; Kazim, H.; Sabri, M.; Tawalbeh, M.; Al-Othman, A. AI in Membrane Design and Optimization for Hydrogen Fuel Cells. Membranes 2026, 16, 97. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Harichandan, S.; Kar, S.K.; Bansal, R.; Mishra, S.K. Achieving sustainable development goals through adoption of hydrogen fuel cell vehicles in India: An empirical analysis. Int. J. Hydrogen Energy 2023, 48, 4845–4859. [Google Scholar] [CrossRef] [Scilit]
- Sharaf, O.Z.; Orhan, M.F. An overview of fuel cell technology: Fundamentals and applications. Renew. Sustain. Energy Rev. 2014, 32, 810–853. [Google Scholar] [CrossRef] [Scilit]
- Sethia, H.; Priyam, A. Review on hydrogen fuel cells as an alternative fuel. Next Energy 2025, 9, 100460. [Google Scholar] [CrossRef] [Scilit]
- Soloveichik, G.L. Liquid fuel cells. Beilstein J. Nanotechnol. 2014, 5, 1399–1418. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ong, B.C.; Kamarudin, S.K.; Basri, S. Direct liquid fuel cells: A review. Int. J. Hydrogen Energy 2017, 42, 10142–10157. [Google Scholar] [CrossRef] [Scilit]
- Ma, J.; Choudhury, N.A.; Sahai, Y. A comprehensive review of direct borohydride fuel cells. Renew. Sustain. Energy Rev. 2010, 14, 183–199. [Google Scholar] [CrossRef] [Scilit]
- Alias, M.S.; Kamarudin, S.K.; Zainoodin, A.M.; Masdar, M.S. Active direct methanol fuel cell: An overview. Int. J. Hydrogen Energy 2020, 45, 19620–19641. [Google Scholar] [CrossRef] [Scilit]
- Shrivastava, N.K.; Thombre, S.B.; Mallick, R.K. Effect of diffusion layer compression on passive DMFC performance. Electrochim. Acta 2014, 149, 167–175. [Google Scholar] [CrossRef] [Scilit]
- Shaari, N.; Kamarudin, S.K.; Bahru, R.; Osman, S.H.; Md Ishak, N.A. Progress and challenges: Review for direct liquid fuel cell. Int. J. Energy Res. 2021, 45, 6644–6688. [Google Scholar] [CrossRef] [Scilit]
- Hren, M.; Božič, M.; Fakin, D.; Kleinschek, K.S.; Gorgieva, S. Alkaline membrane fuel cells: Anion exchange membranes and fuels. Sustain. Energy Fuels 2021, 5, 604–637. [Google Scholar] [CrossRef] [Scilit]
- Vecchio, C.L.; Lyu, X.; Gatto, I.; Zulevi, B.; Serov, A.; Baglio, V.; Vecchio, C.L.; Gatto, I.; Baglio, V. Performance investigation of alkaline direct methanol fuel cell with commercial PGM-free cathodic material. J. Power Sources 2023, 561, 232732. [Google Scholar] [CrossRef] [Scilit]
- Higa, M.; Mehdizadeh, S.; Feng, S.; Endo, N.; Kakihana, Y. Cell performance of direct methanol alkaline fuel cell (DMAFC) using anion exchange membranes prepared from PVA-Based block copolymer. J. Membr. Sci. 2020, 597, 117618. [Google Scholar] [CrossRef] [Scilit]
- Galvan, V.; Shrimant, B.; Bae, C.; Prakash, G.K.S. Ionomer Significance in Alkaline Direct Methanol FuelCell to Achieve High Power with a Quarternized Poly(terphenylene) Membrane. ACS Appl. Energy Mater. 2021, 4, 5858–5867. [Google Scholar] [CrossRef] [Scilit]
- Wang, Y.; Wang, D.; Wang, J.; Wang, L. Preparation and characterization of a sol-gel derived silica/PVA-Py hybrid anion exchange membranes for alkaline fuel cell application. J. Electroanal. Chem. 2020, 873, 114342. [Google Scholar] [CrossRef] [Scilit]
- Ryu, J.; Seo, J.Y.; Choi, B.N.; Kim, W.-J.; Chung, C.-H. Quaternized chitosan-based anion exchange membrane for alkaline direct methanol fuel cells. J. Ind. Eng. Chem. 2019, 73, 254–259. [Google Scholar] [CrossRef] [Scilit]
- Prakash, G.K.S.; Krause, F.C.; Viva, F.A.; Narayanan, S.R.; Olah, G.A. Study of operating conditions and cell design on the performance of alkaline anion exchange membrane-based direct methanol fuel cells. J. Power Sources 2011, 196, 7967–7972. [Google Scholar] [CrossRef] [Scilit]
- Santasalo-Aarnio, A.; Hietala, S.; Rauhala, T.; Kallio, T. In and ex situ characterization of an anion-exchange membrane for alkaline direct methanol fuel cell (ADMFC). J. Power Sources 2011, 196, 6153–6159. [Google Scholar] [CrossRef] [Scilit]
- Sajjad, S.D.; Liu, D.; Wei, Z.; Sakri, S.; Shen, Y.; Hong, Y.; Liu, F. Guanidinium based blend anion exchange membranes for direct methanol alkaline fuel cells (DMAFCs). J. Power Sources 2015, 300, 95–103. [Google Scholar] [CrossRef] [Scilit]
- Bunazawa, H.; Yamazaki, Y. Influence of anion ionomer content and silver cathode catalyst on the performance of alkaline membrane electrode assemblies (MEAs) for direct methanol fuel cells (DMFCs). J. Power Sources 2008, 182, 48–51. [Google Scholar] [CrossRef] [Scilit]
- Song, F.; Fu, Y.; Gao, Y.; Li, J.; Qiao, J.; Zhou, X.-D.; Liu, Y. Novel Alkaline Anion-exchange Membranes Based on Chitosan/Ethenylmethylimidazoliumchloride Polymer with Ethenylpyrrolidone Composites for Low Temperature Polymer Electrolyte Fuel Cells. Electrochim. Acta 2015, 177, 137–144. [Google Scholar] [CrossRef] [Scilit]
- Yang, C.; Wang, S.; Jiang, L.; Hu, J.; Ma, W.; Sun, G. 1,2-Dimethylimidazolium-functionalized cross-linked alkaline anion exchange membranes for alkaline direct methanol fuel cells. Int. J. Hydrogen Energy 2015, 40, 2363–2370. [Google Scholar] [CrossRef] [Scilit]
- Rao, A.H.N.; Kim, H.-J.; Nam, S.; Kim, T.-H. Cardo poly(arylene ether sulfone) block copolymers with pendant imidazolium side chains as novel anion exchange membranes for direct methanol alkaline fuel cell. Polymer 2013, 54, 6918–6928. [Google Scholar] [CrossRef] [Scilit]
- Jurzinsky, T.; Bär, R.; Heppe, N.; Cremers, C.; Tübke, J. A comb-like ionomer based on poly(2,6-dimethyl-1,4-phenylene oxide) for the use as anodic binder in anion-exchange membrane direct methanol fuel cells. Solid State Ion. 2017, 303, 1–11. [Google Scholar] [CrossRef] [Scilit]
- Zhao, S.; Tsen, W.-C.; Gong, C. 3D nanoflower-like layered double hydroxide modified quaternized chitosan/polyvinyl alcohol composite anion conductive membranes for fuel cells. Carbohydr. Polym. 2020, 256, 117439. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Martinaiou, I.; Videla, A.H.A.M.; Weidler, N.; Kübler, M.; Wallace, W.D.Z.; Paul, S.; Wagner, S.; Shahraei, A.; Stark, R.W.; Specchia, S.; et al. Activity and degradation study of an Fe-N-C catalyst for ORR in Direct Methanol Fuel Cell (DMFC). Appl. Catal. B Environ. 2020, 262, 118217. [Google Scholar] [CrossRef] [Scilit]
- Deng, H.; Jiao, D.; Zu, M.; Chen, J.; Jiao, K.; Huang, X. Modeling of passive alkaline membrane direct methanol fuel cell. Electrochim. Acta 2015, 154, 430–446. [Google Scholar] [CrossRef] [Scilit]
- Kim, J.; Momma, T.; Osaka, T. Cell performance of Pd–Sn catalyst in passive direct methanol alkaline fuel cell using anion exchange membrane. J. Power Sources 2009, 189, 999–1002. [Google Scholar] [CrossRef] [Scilit]
- Xie, X.; Yu, H.; Deng, H.; Zhang, G.; Guo, T.; Sun, J.; Jiao, K. Modeling of passive vapor feed alkaline membrane direct methanol fuel cell. Appl. Therm. Eng. 2018, 131, 920–932. [Google Scholar] [CrossRef] [Scilit]
- Wang, B.; Zhou, Y.; Du, Q.; Yin, Y.; Jiao, K. Transient investigation of passive alkaline membrane direct methanol fuel cell. Appl. Therm. Eng. 2016, 100, 1245–1258. [Google Scholar] [CrossRef] [Scilit]
- Najmi, A.A.; Rowshanzamir, S.; Parnian, M.J. Investigation of NaOH concentration effect in injected fuel on the performance of passive direct methanol alkaline fuel cell with modified cation exchange membrane. Energy 2016, 94, 589–599. [Google Scholar] [CrossRef] [Scilit]
- Sidharthan, K.A.; Joseph, S. Performance evaluation of passive alkaline direct methanol fuel cell-the effect of inorganic salt and TiO2 nano fillers. Sustain. Energy Technol. Assess. 2022, 53, 102673. [Google Scholar] [CrossRef] [Scilit]
- Verjulio, R.W.; Santander, J.; Ma, J.; Alonso-Vante, N. Selective CoSe2/C cathode catalyst for passive air-breathing alkaline anion exchange membrane μ-direct methanol fuel cell (AEM-μDMFC). Int. J. Hydrogen Energy 2016, 41, 19595–19600. [Google Scholar] [CrossRef] [Scilit]
- Verjulio, R.W.; Santander, J.; Sabaté, N.; Esquivel, J.P.; Torres-Herrero, N.; Habrioux, A.; Alonso-Vante, N. Fabrication and evaluation of a passive alkaline membrane micro direct methanol fuel cell. Int. J. Hydrogen Energy 2014, 39, 5406–5413. [Google Scholar] [CrossRef] [Scilit]
- Kim, J.-H.; Kim, H.-K.; Hwang, K.-T.; Lee, J.-Y. Performance of air-breathing direct methanol fuel cell with anion-exchange membrane. Int. J. Hydrogen Energy 2010, 35, 768–773. [Google Scholar] [CrossRef] [Scilit]
- Kim, H.; Zhou, J.; Ünlü, M.; Anestis-Richard, I.; Joseph, K.; Kohl, P.A. The effect of hydrophobicity in alkaline electrodes for passive DMFC. Electrochim. Acta 2011, 56, 3085–3090. [Google Scholar] [CrossRef] [Scilit]
- Chen, C.; Tse, Y.-L.S.; Lindberg, G.E.; Knight, C.; Voth, G.A. Hydroxide solvation and transport in anion exchange membranes. J. Am. Chem. Soc. 2016, 138, 991–1000. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Neelima, J.; Singh, R.K. Recent advances in anion-exchange membranes for electrolyzers, fuel cells and redox-flow batteries. J. Mater. Chem. A 2025, 13, 36853–36880. [Google Scholar] [CrossRef] [Scilit]
- Yang, Y.; Huang, H.; Li, Z.; Xiao, C.; Haq, M.U.; Zeng, L. The durability towards anion exchange membrane fuel cells: Current status and challenges. Future Batter. 2025, 5, 100016. [Google Scholar] [CrossRef] [Scilit]
- Song, Y.; Guo, Z.; Yin, J.; Liu, M.; Tolj, I.; Grigoriev, S.A.; Ge, M.; Sun, C. Investigations of the Sulfonated Poly(ether ether ketone) Membranes with Various Degrees of Sulfonation by Considering Durability for the Proton Exchange Membrane Fuel Cell (PEMFC) Applications. Polymers 2025, 17, 2181. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Guo, Z.; Ge, M.; Zhao, Y.; Song, Y.; Ren, K.; Ou, T.; Tsim, S.; Sun, C. Fluorinated graphite-modified sulfonated poly(ether ether ketone) membranes for enhanced electrochemical performance and durability in proton exchange membrane fuel cells. J. Power Sources 2026, 696, 241504. [Google Scholar] [CrossRef] [Scilit]
- Yu, E.H.; Scott, K.; Reeve, R.W.; Yang, L.; Allen, R.G. Characterisation of platinised Ti mesh electrodes using electrochemical methods: Methanol oxidation in sodium hydroxide solutions. Electrochim. Acta 2004, 49, 2443–2452. [Google Scholar] [CrossRef] [Scilit]
- Kuznetsov, K.I.; Skorodumov, S.V.; Granchenko, P.P. Measurements of the Dynamic Viscosity and Density of KOH Solutions at Atmospheric Pressure. High Temp. 2020, 58, 806–811. [Google Scholar] [CrossRef] [Scilit]
- Prabhuram, J.; Manoharan, R. Investigation of methanol oxidation on unsupported platinum electrodes in strong alkali and strong acid. J. Power Sources 1998, 74, 54–61. [Google Scholar] [CrossRef] [Scilit]
- Luo, X.; Kushner, D.I.; Kusoglu, A. Anion exchange membranes: The effect of reinforcement in water and electrolyte. J. Membr. Sci. 2023, 685, 121945. [Google Scholar] [CrossRef] [Scilit]
- Vecchio, C.L.; Carbone, A.; Gatto, I.; Baglio, V. Investigation of Fumasep® FAA3-50 Membranes in Alkaline Direct Methanol Fuel Cells. Polymers 2023, 15, 1555. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Yan, S.; Yang, M.; Sun, C.; Xu, S. Liquid Water Characteristics in the Compressed Gradient Porosity Gas Diffusion Layer of Proton Exchange Membrane Fuel Cells Using the Lattice Boltzmann Method. Energies 2023, 16, 6010. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.