Featured Application
The developed methacrylated chitosan hydrogels are intended as multifunctional, photocrosslinkable candidates for extrusion-based 3D bioprinting and future stimuli-responsive 4D biofabrication. Their extrusion processability, photocrosslinkability, medium-dependent and acid-sensitive swelling, biodegradability, antibacterial and antioxidant activity, and cytocompatibility support their further investigation as responsive tissue-engineering materials. The potential 4D application is proposed as a future direction and was not experimentally demonstrated in the present study.
Abstract
Methacrylated chitosan hydrogels are promising multifunctional materials for extrusion-based 3D bioprinting and may provide a platform for the future development of stimuli-responsive 4D biofabrication systems. This study evaluated chitosan-based hydrogel formulations prepared at different pH values and functionalized with lanthanum oxide nanoparticles and a copper tripeptide. The materials were characterized by swelling tests in water, PBS, SBF, and acidic medium, UV–Vis spectroscopy, FT-IR analysis, preliminary extrusion-printing tests, enzymatic biodegradation, DPPH radical scavenging, antibacterial testing against Escherichia coli, and XTT cytotoxicity assessment using 1321N1 cells. The hydrogels exhibited pronounced medium-dependent swelling, with a particularly strong initial response under acidic conditions, consistent with protonation of residual amino groups in the chitosan matrix. Preliminary printing experiments demonstrated continuous extrusion and stable filament formation, while FT-IR analysis and macroscopic observations supported successful photocrosslinking. The modified hydrogels showed antibacterial and antioxidant activity, substantial enzymatic degradability, and generally acceptable cytocompatibility, although the formulation with the highest additive content at the lowest preparation pH reduced cell viability below 70%. Overall, the developed materials represent multifunctional, extrusion-processable and photocrosslinkable hydrogel candidates for 3D bioprinting. Their stimulus-sensitive swelling behavior additionally supports further investigation for future 4D biofabrication, although programmed post-printing shape transformation was not evaluated in the present study.
1. Introduction
Three-dimensional bioprinting has emerged as a promising manufacturing strategy for tissue engineering and regenerative medicine because it enables the controlled, layer-by-layer deposition of biomaterials, bioactive compounds, and living cells into spatially organized constructs [1,2]. Among the available approaches, extrusion-based bioprinting is particularly attractive due to its versatility, relatively simple instrumentation, and compatibility with highly viscous, cell-containing hydrogel formulations [3,4,5]. Nevertheless, the successful fabrication of biologically functional constructs depends strongly on the properties of the applied bioink, including its rheological behavior, printability, structural stability, biodegradability, and cytocompatibility [5,6,7,8]. These requirements become even more demanding when the printed scaffold is intended not only to support tissue regeneration but also to actively respond to changes occurring in the surrounding biological environment [9,10].
Four-dimensional bioprinting extends the concept of conventional 3D bioprinting by introducing time-dependent changes in the structure or function of printed constructs [9,11,12]. In this approach, stimuli-responsive materials are used to produce scaffolds capable of changing their volume, shape, stiffness, permeability, or biological activity in response to physical, chemical, or biological stimuli [10,11,12,13]. Temperature, light, magnetic fields, enzymes, and pH are among the most frequently investigated triggers [10,11,12]. In particular, pH-sensitive hydrogels are of considerable interest because local pH may change during inflammation, infection, tissue injury, and healing [14,15,16]. Polymers containing ionizable functional groups can convert these chemical changes into measurable variations in swelling, hydration, or mechanical behavior, thereby acting as chemically responsive or sensory polymeric systems [10,14,15].
Chitosan is a particularly promising material for the development of such responsive hydrogels. This natural polysaccharide is biodegradable, biocompatible, and readily modifiable due to the presence of primary amino and hydroxyl groups [17]. Protonation and deprotonation of the amino groups influence polymer–polymer and polymer–solvent interactions, making chitosan sensitive to the pH and ionic composition of the surrounding medium [18]. As a result, chitosan-based networks can exhibit pronounced changes in swelling and hydration under different environmental conditions [18]. However, native chitosan also has limited mechanical stability and generally requires acidic conditions for dissolution, which may restrict its direct processing as a bioink [17,19]. Chemical functionalization, including methacrylation, can address some of these limitations by introducing photocrosslinkable groups and enabling rapid stabilization of the hydrogel network after deposition [19,20].
The development of multifunctional bioink candidates also requires the incorporation of components that provide additional biological activity. Nanoparticles and other inorganic fillers can modify the physicochemical behavior of hydrogel matrices and introduce new responsive or bioactive functions [21]. Lanthanum oxide nanoparticles are attractive inorganic modifiers because of their high surface reactivity and potential to interact with surrounding chemical species [22,23,24]. Their incorporation into chitosan-based matrices may therefore affect swelling, structural organization, and interactions with the biological environment [22,23,24].
The incorporation of inorganic nanophases into hydrogel matrices is a widely investigated strategy for introducing additional physicochemical and biological functions. Metal oxide nanoparticles such as ZnO and MgO have been extensively studied as antimicrobial components of polymeric hydrogels, while silicate-based nanomaterials have also been used as reinforcing and bioactive phases in hydrogel and bioink systems [21]. In contrast, lanthanum oxide (La2O3), a rare-earth metal oxide, remains considerably less explored in photocrosslinkable polysaccharide-based hydrogels despite its emerging multifunctional biological properties [22,23,24].
La2O3 nanoparticles were selected in the present study because their reported activity extends beyond a purely structural role. Recent studies have demonstrated antibacterial activity of La2O3 against both Gram-positive and Gram-negative bacteria, including Escherichia coli, together with measurable antioxidant and redox-modulating properties [22]. Moreover, incorporation of La2O3 nanoparticles into collagen-based biomatrices has been shown to improve matrix stability while maintaining favorable cytocompatibility and promoting endothelial-cell activation and angiogenic responses [23]. In a more complex collagen–κ-carrageenan–hydroxyapatite system, La2O3-containing composites additionally supported angiogenesis, osseointegration, and bone-defect repair in vivo [24]. These findings suggest that La2O3 may act as a multifunctional inorganic component capable of contributing to antimicrobial and redox-related activity while remaining compatible with regenerative biomaterial applications [22,23,24]. Accordingly, La2O3 was selected here not as a presumed superior substitute for established ZnO, MgO, or silicate fillers, but as a comparatively underexplored rare-earth nanophase with the potential to complement the biological functionality of methacrylated chitosan and GHK–Cu within a photocrosslinkable hydrogel system.
At the same time, bioactive peptides can be introduced to improve the therapeutic functionality of the resulting material. Short antimicrobial peptides, including tripeptides, are increasingly investigated as alternatives or complements to conventional antibiotics [25,26,27]. Their small molecular size, aqueous solubility, relative stability, and capacity to interact with bacterial membranes make them promising additives for biomedical hydrogels [25,26,27]. Copper tripeptides, such as GHK–Cu, are additionally associated with biological processes involved in tissue repair and regeneration [25,28]. When incorporated into hydrogel matrices, such compounds may provide localized antimicrobial and antioxidant effects while reducing the need for systemic administration [25,28]. This feature is particularly relevant to tissue-engineering scaffolds intended for implantation, because bacterial contamination and infection can impair tissue integration, prolong inflammation, and compromise regenerative outcomes [29].
These considerations are especially important in peripheral nerve tissue engineering. Repair of peripheral nerve defects may require the implantation of nerve guidance conduits or hydrogel-based scaffolds that provide a hydrated, biodegradable, and cytocompatible environment for regenerating cells [30]. Such biomaterial systems are designed to support axonal regeneration while providing appropriate structural and biological conditions during the healing process [30]. However, surgical implantation and prolonged material–tissue contact may also create conditions in which bacterial contamination can negatively affect healing and compromise regenerative outcomes [29].
Therefore, a multifunctional material combining environmental responsiveness with antibacterial, antioxidant, biodegradable, and cytocompatible properties could be advantageous for the development of advanced scaffolds for peripheral nerve regeneration [29,30]. In this context, pH-dependent swelling may provide an adaptive response to local chemical changes [14,15], whereas antimicrobial additives may help reduce infection-related complications [25,29].
From the perspective of sensory polymers, pH-responsive hydrogels are particularly important because they can translate changes in the chemical microenvironment into measurable variations in their physical properties [14,15]. In chitosan-based systems, this response is governed mainly by the protonation and deprotonation of amino groups, which modify electrostatic interactions within the polymer network and consequently affect water uptake, swelling, and structural organization [15,17,18].
Such behavior enables the material to function as a chemically responsive platform rather than solely as a passive scaffold. In biomedical environments, local pH variations may accompany inflammation, microbial colonization, tissue injury, and healing, while pH monitoring has been proposed as a useful approach for evaluating changes in wound and tissue microenvironments [16]. Therefore, medium-dependent swelling is relevant not only to hydrogel stability but also to the assessment of its potential as a sensory polymeric material [14,15].
Methacrylated chitosan has previously been investigated as a photocrosslinkable material for tissue engineering and 3D biofabrication. Zanon et al. demonstrated that methacrylation of chitosan enables the preparation of photocrosslinkable and 3D-printable hydrogel formulations with tunable physicochemical properties [31]. Photocrosslinkable methacrylated chitosan has also been combined with gelatin-based matrices to obtain printable composite hydrogels suitable for tissue-engineering applications [32]. Furthermore, nanohybrid bioinks based on photocrosslinkable chitosan and gelatin have been developed for extrusion-based 3D bioprinting, demonstrating that incorporation of inorganic components can be used to tailor the properties and biological functionality of chitosan-based systems [33]. More recently, methacrylated chitosan has also been successfully processed using embedded 3D-printing strategies, further confirming its potential as a platform for biofabrication [34].
In contrast to these previously reported systems, the present study combines fungal-derived methacrylated chitosan with La2O3 nanoparticles and the copper tripeptide GHK–Cu within a single photocrosslinkable formulation. The developed materials were designed not only for extrusion-based processing and photocrosslinking, but also to provide a combination of medium-dependent swelling, antibacterial and antioxidant activity, enzymatic degradability, and cytocompatibility. Previous studies have separately demonstrated the potential of La2O3 as a biologically active inorganic component [22,23,24], GHK–Cu as a bioactive and redox-modulating peptide [25,28], and methacrylated chitosan as a photocrosslinkable material for 3D biofabrication [31,32,33,34]. To the best of our knowledge, the combined incorporation of La2O3 nanoparticles and GHK–Cu into a methacrylated fungal chitosan matrix has not previously been investigated in the context of multifunctional photocrosslinkable formulations for biofabrication. Therefore, the originality of the present work lies in integrating these components and functions within a single material platform rather than in chitosan methacrylation or photocrosslinking alone.
Therefore, medium-dependent swelling is relevant not only to hydrogel stability but also to the assessment of its potential as a sensory polymeric material. Stimuli-responsive hydrogels are increasingly investigated as functional materials for 4D biofabrication because controlled swelling, shrinking, and other time-dependent transformations may enable printed constructs to adapt to changes in their surroundings [13,35]. Importantly, stimulus-sensitive swelling of a bulk hydrogel should not itself be considered evidence of 4D behavior. In 4D printing, the response should occur after fabrication and result in a programmed, time-dependent change in the geometry, dimensions, structure, or function of the printed construct [11,12,13].
In this context, methacrylated chitosan is particularly attractive because its photocrosslinkability enables stabilization of the material after deposition [19,31], while protonation and deprotonation of residual amino groups provide an inherent mechanism for environmentally dependent swelling [15,18]. The combination of extrusion processability, photocrosslinkability, and stimulus-sensitive swelling therefore provides a rationale for considering these materials as candidates for future 4D biofabrication [11,12,13,35]. However, in the present study, 4D performance is considered a potential application rather than an experimentally demonstrated property, as programmed post-printing shape transformation was not evaluated.
The aim of this study was to develop and characterize photocrosslinkable methacrylated chitosan hydrogels functionalized with lanthanum oxide nanoparticles and a copper tripeptide. Formulations prepared under different pH conditions were evaluated in terms of swelling in water, phosphate-buffered saline, simulated body fluid, and an acidic medium. Their optical and chemical characteristics were examined using UV–Vis and FT-IR spectroscopy, while enzymatic biodegradation, antioxidant activity, antibacterial performance against Escherichia coli, and cytocompatibility toward 1321N1 cells were also assessed. The study was designed to determine whether the developed materials exhibit medium-dependent and acid-sensitive swelling together with physicochemical and biological properties relevant to their potential use as photocrosslinkable hydrogel candidates for extrusion-based 3D bioprinting, while also assessing their suitability for further development toward stimuli-responsive 4D biofabrication.
2. Materials and Methods
2.1. Materials
Fungal chitosan was used as the polymeric substrate for the preparation of methacylated chitosan hydrogels purchased at PolAura (Olsztyn, Poland). Methacrylic anhydride was used for chitosan functionalization, while acetic acid and sodium hydroxide were applied to dissolve the polymer and adjust the reaction pH. Phosphate-buffered saline (PBS) was used for hydrogel preparation and dilution. The reagents were purchased at SgimaAldrich (Poznań, Poland).
Lanthanum oxide nanoparticles (La2O3) were incorporated as an inorganic functional component using lanthanum nitrate as a precursor. A commercial copper tripeptide preparation containing glycyl-L-histidyl-L-lysine copper complex (GHK–Cu) was used as the bioactive peptide additive. Lithium phenyl-2,4,6-trimethylbenzoylphosphinate (LAP) were used as photoinitiators in preliminary photocrosslinking experiments.
Swelling studies were performed in distilled water, PBS, simulated body fluid (SBF), and an aqueous acetic acid solution adjusted to pH = 3. Enzymatic degradation studies were carried out using human lysozyme. Antioxidant activity was assessed using 2,2-diphenyl-1-picrylhydrazyl (DPPH).
Antibacterial activity was evaluated against Escherichia coli ATCC 43888. Nutrient agar supplemented with glucose was used for bacterial cultivation, while a penicillin–streptomycin solution was used as the antibacterial control. Cytocompatibility was assessed using the human 1321N1 cell line cultured in Dulbecco’s modified Eagle medium supplemented with fetal bovine serum and antibiotics.
2.2. Methods
A general idea of the novel potential bioinks is given in Figure 1.
Figure 1.
Schematic overview of the development, characterization, and prospective application of methacrylated chitosan-based photocrosslinkable bioink formulations.
2.2.1. Synthesis of Methacrylated Chitosan
Methacrylated chitosan was prepared by dissolving 0.75 g of chitosan in 50 mL of a 4% aqueous acetic acid solution. The mixture was stirred continuously at 40 °C until a homogeneous solution was obtained. After complete dissolution, the pH was adjusted to 3.5, 4.0, or 4.5, depending on the formulation. Methacrylation was initiated by adding 3 mL of methacrylic anhydride. The reaction mixture was maintained under continuous stirring, and the pH was monitored throughout the reaction. When necessary, the pH was corrected using a 5% sodium hydroxide solution. After completion of the reaction, the product was purified using membrane filtration to remove unreacted reagents and low-molecular-weight by-products. The purified polymer solutions were frozen and lyophilized to obtain dry methacrylated chitosan powders. The resulting materials were designated as 1B, 2B, and 3B, corresponding to preparation pH values of 3.5, 4.0, and 4.5, respectively.
2.2.2. Synthesis of Lanthanum Oxide Nanoparticles
Lanthanum oxide nanoparticles were synthesized by a chemical co-precipitation method using lanthanum(III) nitrate hexahydrate as the precursor. Lanthanum(III) nitrate hexahydrate, La(NO3)3·6H2O, was dissolved in deionized water under continuous magnetic stirring until a homogeneous solution was obtained. Ammonium hydroxide was then added dropwise while stirring, and the pH of the solution was adjusted to approximately 10. Under these alkaline conditions, a gelatinous lanthanum hydroxide precipitate formed according to the following chemical equation:
The resulting precipitate was separated by centrifugation and washed repeatedly with distilled water to remove residual nitrate and ammonium ions. The purified precipitate was subsequently dried and subjected to thermal treatment in a furnace at 600–800 °C for 3–5 h. During calcination, lanthanum hydroxide underwent thermal decomposition to form crystalline lanthanum oxide according to chemical equation:
After cooling to room temperature, the obtained La2O3 powder was collected and used as the nanoparticulate inorganic component in the hydrogel formulations.
2.2.3. Preparation of Hydrogel Formulations
For each formulation, 0.1 g of lyophilized methacrylated chitosan was dissolved in 2.8 mL of PBS. Photoinitiator was then added at a final concentration of 0.05%, corresponding to 1.35 mg per formulation. The functional additive suspension was prepared by dispersing 2.5 mg of La2O3 nanoparticles in 2 mL of distilled water, followed by the addition of 0.5 mL of the commercial GHK–Cu preparation. The suspension was thoroughly mixed before incorporation into the hydrogel formulations.
The following sample groups were prepared: methacrylated chitosan without additives, methacrylated chitosan with photoinitiator, methacrylated chitosan with photoinitiator and the La2O3/GHK–Cu suspension. The formulations were prepared for all three methacrylated chitosan variants, 1B, 2B, and 3B (Table 1). The La2O3/GHK–Cu suspension was thoroughly mixed immediately before incorporation into the polymer solution, and the resulting formulations were visually inspected during preparation for sedimentation, phase separation, or formation of macroscopic aggregates. The actual lanthanum content in the developed hydrogel formulations was quantitatively determined using atomic absorption spectrometry (AAS). Dried hydrogel samples containing the La2O3/GHK–Cu suspension were subjected to mineralization prior to analysis. After complete mineralization, the obtained solutions were quantitatively transferred, diluted to the required final volume with deionized water, and analyzed using a PU 9100X atomic absorption spectrometer (Philips Scientific, Cambridge, UK). Lanthanum concentrations were determined using an external calibration curve prepared from standard solutions of known La concentrations. Appropriate dilution of the samples was performed when required to ensure that the measured concentrations remained within the linear calibration range. The experimentally determined lanthanum content was expressed relative to the dry mass of the analyzed hydrogel sample and calculated according to Equation (1):
where:
CLa is the lanthanum content in the dry hydrogel sample (mg g−1).
cAAS is the lanthanum concentration determined from the AAS calibration curve (mg L−1), (V) is the final volume of the mineralized sample solution (L), and (m) is the dry mass of the analyzed hydrogel sample (g).
The experimentally determined La content was used to quantitatively verify incorporation of the La2O3-containing inorganic component into the methacrylated chitosan hydrogel matrix and to compare the actual inorganic loading among the investigated formulations.
Table 1.
Composition of the developed bioink formulations.
2.2.4. Preliminary Extrusion-Printing Tests
Preliminary extrusion-printing tests were performed to evaluate the processability of the photocrosslinkable hydrogel formulations and their ability to form continuous filaments after extrusion. The prepared hydrogel was transferred into a printing cartridge and extruded through the printing nozzle onto a non-adhesive substrate (glass). Linear paths were printed to assess extrusion continuity, filament formation, and immediate shape retention after deposition.
The printed structures were evaluated qualitatively by visual inspection and photographic documentation. Particular attention was paid to the formation of uninterrupted strands, maintenance of filament geometry after deposition, and the occurrence of local irregularities in filament width. These experiments were intended as a preliminary assessment of extrusion processability rather than a complete quantitative evaluation of printability or rheological behavior.
Photocrosslinking capability was assessed separately by irradiation of the methacrylated chitosan formulations in the presence of LAP at 405 nm, as described in Section 2.2.5. The combination of extrusion testing and photocrosslinking assessment was used to evaluate the basic suitability of the developed formulations for further development as photocrosslinkable materials for extrusion-based 3D bioprinting using customized bioprinter F-Nis 23151 Sygnis (Sygnis, Gdańsk, Poland).
2.2.5. UV–Vis Spectroscopy
UV–Vis measurements were performed for the unmodified hydrogel formulations, samples containing the photoinitiator, and samples containing both the photoinitiator and the La2O3/GHK–Cu suspension.
For each measurement, 0.2 mL of hydrogel was diluted with 1.8 mL of PBS and mixed until a homogeneous suspension was obtained. Spectra were recorded in the range of 200–800 nm using an Agilent 8453 UV-Visible Spectroscopy System equipped with a 5 mm quartz cuvette (Agilent, Santa Clara, CA, USA). PBS was used as the reference. The measurements were used to evaluate changes in optical absorption associated with the incorporation of the photoinitiator and bioactive additives, with particular attention to the wavelength range relevant to photocrosslinking.
2.2.6. Photocrosslinking and FT-IR Analysis
Photocrosslinking and FT-IR analyses were performed for samples 2B and 3B containing 150, 300, or 500 µL of the La2O3/GHK–Cu suspension. A small volume of each sample was mixed with LAP photoinitiator and transferred onto a glass substrate. The samples were irradiated at 405 nm for 15 min using a Halot Creality photopolymerization system and subsequently dried (3D CREALITY Halot R63D Printer, x-kom, Częstochowa, Poland). Corresponding non-irradiated samples without photoinitiator were also prepared as controls. FT-IR spectra were collected to identify the characteristic functional groups of chitosan and to evaluate changes associated with methacrylation, the incorporation of additives, and photocrosslinking.
The relative degree of chitosan methacrylation was evaluated semi-quantitatively from the FT-IR spectra of native chitosan and methacrylated formulations 1B, 2B, and 3B. For each spectrum, the absorbance of the methacrylate-associated vinylic band located at approximately 3077–3082 cm−1 was normalized to the characteristic C–O/C–O–C stretching band of the chitosan polysaccharide backbone located in the 1025–1062 cm−1 region, which was used as an internal reference. The relative methacrylation index (MI) was calculated according to Equation (2):
where:
MI—methacrylation index.
Avinyl—is the absorbance of the methacrylate-associated vinylic band at approximately 3077–3082 cm−1.
Aref—is the absorbance of the characteristic polysaccharide C–O/C–O–C band in the 1025–1062 cm−1 region.
For spectra recorded in transmittance mode, absorbance values were calculated according to Equation (3):
where (T) is the measured transmittance expressed as a percentage.
The calculated relative methacrylation indices were subsequently used to compare the extent of chitosan functionalization among formulations 1B, 2B, and 3B.
The relative degree of photocrosslinking was evaluated from the FT-IR spectra recorded before and after irradiation. The analysis was based on the decrease in the methacrylate-associated vinylic absorption band after exposure to 405 nm light. To account for differences in overall spectral intensity, the vinylic band was normalized to the characteristic C–O/C–O–C stretching band of the chitosan polysaccharide backbone, which was used as an internal reference.
The double-bond conversion (DC), used as a relative measure of the extent of photocrosslinking, was calculated according to Equation (4):
where:
Avinyl is the absorbance of the methacrylate-associated vinylic band at approximately 3077–3100 cm−1.
Aref is the absorbance of the characteristic polysaccharide C–O/C–O–C band in the 1025–1062 cm−1 region, and the subscripts “before” and “after” refer to the spectra recorded before and after photocrosslinking, respectively.
A higher DC value indicates a greater consumption of unsaturated methacrylate groups during irradiation and, consequently, a higher relative extent of photocrosslinking.
2.2.7. Swelling Measurements
The swelling behavior of lyophilized samples 1B, 2B, and 3B was evaluated in four media: distilled water, PBS, SBF, and aqueous acetic acid at pH 3.
Dry samples were weighed to determine the initial mass and then placed in the selected medium at room temperature. After 10, 30, and 60 min, the samples were removed, gently blotted to remove excess surface liquid, and weighed. The swelling degree was calculated according to Equation (5):
where m0 is the initial dry mass and mt is the mass of the swollen sample at a given time point.
2.2.8. Antibacterial Activity
Antibacterial activity was evaluated against Escherichia coli ATCC 43888. For each methacrylated chitosan variant (1B, 2B, and 3B), 8.7 mg of lyophilized material was transferred into wells of a 12-well plate. The tested formulations contained 0, 150, 300, or 500 µL of the La2O3/GHK–Cu suspension. Distilled water was added to maintain a constant liquid volume, followed by the addition of 750 µL of bacterial suspension (Table 2).
Table 2.
Samples for antibacterial activity study.
The antibacterial effect was evaluated as a function of direct contact time between the hydrogel formulations and the bacterial suspension. Samples were analyzed immediately after preparation (0 h) and after 1, 24, 48, and 72 h of incubation at 37 °C. At each time point, aliquots were collected and plated onto nutrient agar to evaluate bacterial growth.
Bacterial growth was assessed based on colony formation. Colony-forming units (CFUs) were recorded when individual colonies could be reliably counted, whereas dense non-countable growth was classified as confluent growth (CG). A bacterial suspension incubated without the tested material served as the growth control, while penicillin–streptomycin was used as the antibacterial reference control.
2.2.9. Enzymatic Degradation
Biodegradation was assessed for samples 2B and 3B without La2O3 nanoparticles or GHK–Cu. Each sample was divided into portions, dried, and weighed to determine the initial mass. Enzymatic degradation was evaluated using lysozyme as the enzyme directly involved in the degradation of the chitosan polysaccharide backbone. The photocrosslinked samples were incubated in PBS (pH 7.4) containing lysozyme at a concentration of 1.5 µg/mL at 37 °C. This concentration was selected to approximate the physiological lysozyme level reported for human serum and has previously been applied in in vitro degradation studies of chitosan-based materials, including materials developed for peripheral nerve regeneration. The samples were incubated for seven days. At selected time points, samples were removed, dried, and weighed. The percentage mass loss was calculated according to Equation (2):
where m0 is the initial dry mass and mt is the dry mass after incubation.
2.2.10. Antioxidant Activity
Antioxidant activity was determined using the DPPH radical-scavenging assay. Samples 2B and 3B were tested. For each formulation, 0.35 g of hydrogel was mixed with 1 mL of PBS and supplemented with 150, 300, or 500 µL of the La2O3/GHK–Cu suspension. Subsequently, 3 mL of a 25 mg/L DPPH solution was added.
The samples were incubated for 60 min with intermittent mixing. Absorbance was measured at 517 nm. DPPH inhibition was calculated according to Equation (3):
where A0 is the absorbance of the control and As is the absorbance of the tested sample.
2.2.11. Cytocompatibility Assessment
Cytocompatibility was evaluated using the XTT assay with 1321N1 cells. Cells were maintained at 37 °C in a humidified atmosphere containing 5% CO2 in DMEM supplemented with 10% fetal bovine serum and 1% antibiotic solution. Cells were seeded into 96-well plates at a density of approximately 1 × 104 cells per well and incubated for 24 h to allow attachment. The tested hydrogel samples were then introduced, and the cells were incubated for an additional 24 h. After exposure, the XTT reagent was added according to the manufacturer’s instructions, and the plates were incubated for approximately 2 h. Absorbance was measured at 450 nm using a microplate reader.
Cell viability was expressed as a percentage relative to untreated control. Three replicates were performed for each formulation. According to ISO 10993-5, samples resulting in cell viability of at least 70% were considered non-cytotoxic.
3. Results
3.1. Synthesis and TEM Characterization of La2O3 Nanoparticles
Lanthanum oxide nanoparticles were obtained by the co-precipitation method using lanthanum(III) nitrate hexahydrate as the precursor and ammonium hydroxide as the precipitating agent. The formation of a gelatinous lanthanum hydroxide intermediate was observed after adjustment of the reaction mixture to alkaline pH. Following repeated washing, drying, and calcination, a dry La2O3 nanopowder was obtained and subsequently used as the inorganic component of the hydrogel formulations.
Transmission electron microscopy confirmed the presence of particles with dimensions in the nanometer range. The TEM image showed irregularly shaped La2O3 particles forming larger aggregates and agglomerates (Figure 2). Individual nanoparticles were visible within the agglomerated structures, although their boundaries were not always clearly separated. The observed agglomeration is characteristic of metal oxide nanoparticles and may result from their high surface energy and strong interparticle interactions [36].
Figure 2.
TEM image of the synthesized La2O3 nanoparticles.
The TEM micrograph also indicated a non-uniform particle distribution, with both smaller primary particles and larger secondary agglomerates present in the sample. Despite the tendency to agglomerate, the image confirmed the successful preparation of nanoscale lanthanum oxide particles suitable for incorporation into the methacrylated chitosan hydrogel matrix.
3.2. Spectral Compatibility of the Formulations with Photoinitiated Crosslinking
UV–Vis spectroscopy was used to evaluate the spectral compatibility of the developed formulations with photoinitiated crosslinking. The analysis included the base methacrylated chitosan formulations designated 1B, 2B, and 3B, as well as their variants containing the LAP photoinitiator (+F) and the La2O3 nanoparticle suspension with GHK–Cu (+N). The aim of the analysis was to determine whether the polymer matrix and the incorporated additives interfered with the wavelength range required for photoinitiator activation.
The base formulations exhibited absorption maxima in the far-UV region, at 202 nm for 1B, 201 nm for 2B, and 200 nm for 3B. Addition of the LAP photoinitiator caused only minor changes in the spectra of 1B and 2B, whereas the maximum of 3B+F shifted to 212 nm. Following incorporation of both LAP and the La2O3/GHK–Cu suspension, the absorption maxima shifted toward longer wavelengths and were recorded at 216 nm for 1B+F+N, 215 nm for 2B+F+N, and 217 nm for 3B+F+N.
The UV–Vis spectra showed that the base methacrylated chitosan formulations exhibited absorption maxima at approximately 200 nm, whereas incorporation of the photoinitiator and the La2O3/GHK–Cu suspension shifted the maxima toward longer wavelengths. This bathochromic shift indicates that the optical environment of the formulations was altered by the additional components and may reflect interactions between the methacrylated chitosan matrix, the photoinitiator, and the incorporated bioactive additives. However, the observed shift should be interpreted as evidence of a changed spectral environment rather than as direct proof of specific chemical bonding (Table 3).
Table 3.
UV–Vis absorption maxima (λmax) of the investigated methacrylated chitosan formulations and their LAP- and La2O3/GHK–Cu-containing variants.
From the perspective of photocrosslinkable biofabrication, the most important observation was the low absorbance of all formulations in the 365–405 nm region commonly employed for photoinitiated crosslinking of methacrylated hydrogel systems (Table 3) [31,32,33,34]. The spectra showed a gradual decrease in absorbance with increasing wavelength, and their overall profiles remained similar despite differences in formulation composition. This indicates that neither the hydrogel matrix nor the incorporated additives caused substantial optical attenuation in the spectral region relevant to photoinitiator activation.
Therefore, the developed formulations were considered spectrally compatible with photocrosslinking under irradiation conditions relevant to 3D biofabrication [31,32,33,34]. The low absorbance in the 365–405 nm range suggests that the investigated components should not substantially hinder light-mediated activation of the photoinitiator and subsequent formation of the photocrosslinked polymer network.
3.3. FT-IR Analysis and Photocrosslinking
The FT-IR spectrum of native chitosan exhibited the characteristic broad O–H/N–H stretching band at approximately 3356 cm−1, C–H stretching bands at approximately 2918 and 2851 cm−1, bands associated with amide and amino-group vibrations at approximately 1646 and 1589 cm−1, and intense C–O/C–O–C stretching bands in the 1150–1030 cm−1 region corresponding to the polysaccharide backbone [17,18] (Figure 3).
Figure 3.
Comparative FT-IR spectra of native chitosan and methacrylated chitosan formulations 1B, 2B, and 3B. The highlighted spectral regions indicate the principal bands associated with O–H/N–H stretching, methacrylate-related vinylic groups, C–H stretching, amide vibrations, and the polysaccharide C–O/C–O–C backbone. The spectra demonstrate progressive changes associated with chitosan methacrylation, with the highest relative methacrylation observed for formulation 3B.
The methacrylated formulations 1B, 2B, and 3B retained the characteristic chitosan backbone bands while exhibiting spectral changes consistent with the introduction of methacrylate functionalities [18,31]. In particular, changes were observed in the regions associated with amino, hydroxyl, carbonyl, and unsaturated groups. Semi-quantitative comparison of the spectra showed a progressive increase in the normalized methacrylation index, with calculated values of 0.420 for 1B, 0.510 for 2B, and 0.631 for 3B, indicating the highest relative extent of methacrylation for formulation 3B (Figure 3).
For formulations 2B and 3B containing the La2O3/GHK–Cu suspension, the principal spectral differences before and after irradiation were observed in the region assigned to vinylic =C–H vibrations at approximately 3068–3109 cm−1 and in the amide/carbonyl region around 1642–1651 cm−1. The relative intensity of the methacrylate-associated unsaturated bands decreased after irradiation, indicating consumption of carbon–carbon double bonds during photocrosslinking [19,31,32,33,34]. Quantitative evaluation based on the normalized vinylic band yielded double-bond conversion values of approximately 19.7% for 2B and 25.3% for 3B, confirming a higher relative extent of photocrosslinking for formulation 3B. The characteristic C–O and C–O–C bands of the chitosan backbone remained clearly visible after irradiation, demonstrating preservation of the polysaccharide structure (Figure 4).
Figure 4.
Representative FT-IR spectra of methacrylated chitosan formulations before and after photocrosslinking: (A) formulation 2B containing 150 µL of La2O3/GHK–Cu suspension and (B) formulation 3B containing 150 µL of La2O3/GHK–Cu suspension. The decrease in the intensity of methacrylate-associated vinylic bands after irradiation indicates consumption of unsaturated groups during photocrosslinking, while preservation of the characteristic C–O/C–O–C bands confirms maintenance of the chitosan polysaccharide backbone.
Changes in the position and intensity of the broad O–H/N–H and amide bands were also observed after incorporation of the La2O3/GHK–Cu suspension and photocrosslinking, indicating modification of the hydrogen-bonding environment and interactions between the polymer matrix and the incorporated components. Such spectral changes are consistent with modifications previously reported for functionalized and photocrosslinked chitosan-based systems [18,31]. Overall, the FT-IR results confirmed successful chemical modification of chitosan and subsequent light-induced crosslinking while preserving the characteristic polysaccharide structure.
To quantitatively compare the extent of chitosan functionalization, a relative methacrylation index (MI) was calculated from the FT-IR spectra by normalizing the methacrylate-associated vinylic band to the characteristic polysaccharide backbone band used as an internal reference [18,31]. The calculated MI values were 0.420 for 1B, 0.510 for 2B, and 0.631 for 3B. These results demonstrate a clear progressive increase in the relative extent of methacrylation in the order 1B < 2B < 3B. The highest methacrylation index was therefore obtained for formulation 3B, whereas formulation 1B exhibited the lowest value. This quantitative trend is consistent with the progressive changes observed in the methacrylate-associated spectral region and confirms that the synthesis conditions, particularly the reaction pH, influenced the extent of chitosan functionalization.
Quantitative evaluation of photocrosslinking based on the normalized methacrylate-associated vinylic band demonstrated a measurable conversion of unsaturated groups after irradiation. The calculated double-bond conversion (DC) was approximately 19.7% for formulation 2B and 25.3% for formulation 3B containing 150 µL of the La2O3/GHK–Cu suspension. Thus, formulation 3B exhibited a higher relative extent of photocrosslinking than 2B. These results are consistent with the observed decrease in the methacrylate-associated vinylic absorption band after exposure to 405 nm light and confirm consumption of unsaturated groups during formation of the photocrosslinked polymer network.
After irradiation in the presence of LAP, the methacrylated chitosan formulations formed transparent, self-supporting hydrogel specimens that retained their overall shape after removal from the casting surface. The samples exhibited a continuous gel-like structure and did not flow, providing macroscopic evidence of successful photocrosslinking. Minor differences in shape, edge regularity, and surface texture were observed among the specimens, most likely as a result of manual sample preparation, casting, and removal from the substrate. Despite these variations, all samples maintained structural integrity after irradiation, indicating that the applied photocrosslinking conditions were sufficient to generate a stable polymer network. The transparency of the obtained hydrogels also suggests that the formulations did not undergo pronounced phase separation or formation of large opaque aggregates during crosslinking (Figure 5).
Figure 5.
Photocrosslinked methacrylated chitosan hydrogel samples after irradiation in the presence of LAP.
3.4. 3D Bioprinting
The developed methacrylated chitosan hydrogel formulations exhibited good processability during extrusion-based 3D printing. The materials were smoothly extruded through the printing nozzle and formed continuous hydrogel filaments, enabling the fabrication of regular grid-like structures (Figure 6). The deposited strands maintained their continuity after extrusion and formed clearly recognizable intersecting patterns corresponding to the designed lattice geometry.
Figure 6.
(A) F-Nis bioprinter; (B) representative grid-like structures fabricated by extrusion-based 3D printing using the developed methacrylated chitosan hydrogel formulation, demonstrating continuous filament formation and preservation of the designed lattice architecture: (a) filament integrity; (b) sample 1B+F+N (c) s sample 2B+F+N ample (d) sample 83B+F+N.
The printed constructs showed good shape retention, with the overall grid architecture remaining stable after deposition. The ability to generate organized, interconnected filament arrangements demonstrates that the developed formulations possess suitable extrusion characteristics for the fabrication of three-dimensional hydrogel structures.
Successful formation of grid-like constructs, together with the demonstrated photocrosslinking of the methacrylated chitosan network, confirms the suitability of the developed formulations as photocrosslinkable hydrogel candidates for extrusion-based 3D bioprinting. Their additional medium-dependent and acid-sensitive swelling behavior provides a functional basis for their further development toward stimuli-responsive 4D biofabrication.
The successful fabrication of regular grid-like structures demonstrates that the developed methacrylated chitosan formulations possess suitable processing characteristics for extrusion-based 3D printing. The materials formed continuous filaments during deposition and preserved the designed lattice architecture after printing, confirming good extrusion processability and shape retention. These results are particularly important from the perspective of bioink development, because the ability to generate organized filament-based structures is one of the key requirements for the fabrication of spatially controlled hydrogel constructs [37,38,39,40,41].
The printing performance was also supported by the demonstrated photocrosslinking capability of the methacrylated chitosan network. FT-IR analysis confirmed changes associated with the consumption of methacrylate unsaturated groups after irradiation, while the photocrosslinked samples formed stable, self-supporting hydrogel structures. The combination of successful extrusion, preservation of the printed architecture, and subsequent light-induced stabilization confirms that the developed formulations can be effectively processed into structured hydrogel constructs [31,32,33,34].
Importantly, the printing properties are accompanied by a broad biological functionality of the developed system. The formulations exhibited cytocompatibility, enzymatic degradability, antibacterial and antioxidant activity, as well as pronounced medium-dependent swelling. The combination of printability with antimicrobial functionality is particularly relevant to the development of multifunctional bioinks for biomedical applications [42]. Taken together, these properties support the application of the developed methacrylated chitosan formulations as multifunctional photocrosslinkable hydrogel candidates for extrusion-based 3D bioprinting. Their stimulus-sensitive swelling behavior additionally provides a functional basis for further development toward responsive 4D biofabrication [11,12,13,35].
3.5. Swelling Abilities
The incubation medium and the contact time were recorded (Figure 7). The highest initial swelling values were recorded in acetic acid solution at pH 3, where both formulations exceeded 6300% after 10 min. This pronounced response can be attributed to protonation of the free amino groups of chitosan. The formation of positively charged –NH3+ groups increases electrostatic repulsion between polymer chains, promotes expansion of the hydrogel network, and facilitates penetration of water molecules [14,15,18,42]. However, the swelling degree decreased during prolonged exposure to the acidic medium. After 60 min, the values decreased to approximately 4130% for 2B and 3932% for 3B. This reduction suggests decreased structural stability of the highly swollen network under acidic conditions and may be associated with partial erosion or material loss during prolonged exposure and handling.
Figure 7.
Swelling ability of the samples.
In distilled water, the swelling degree increased continuously with time. For sample 2B, the value increased from approximately 3725% after 10 min to 4336% after 60 min, whereas sample 3B increased from approximately 5971% to 7576%. In this non-ionic medium, swelling was driven mainly by hydration of hydroxyl and amino groups and by hydrogen-bond formation between water molecules and the hydrophilic chitosan network [15,17,42]. The particularly high final swelling of 3B may indicate a more readily hydrated polymer network than that of 2B.
In PBS and SBF, the swelling response was more controlled than in distilled water or acidic medium. In PBS, sample 2B showed a gradual decrease in swelling from approximately 4387% to 3486%, while sample 3B increased from approximately 5039% to 6069%. In SBF, the swelling degree increased from approximately 3464% to 5306% for 2B and from approximately 3702% to 4677% for 3B. The presence of dissolved ions in PBS and SBF may partially screen electrostatic interactions between charged polymer groups, thereby limiting excessive network expansion [14,15]. At the same time, ion–dipole interactions and hydration of the polymer chains allow the hydrogel to maintain substantial liquid uptake.
The behavior observed in SBF may additionally be influenced by interactions of the chitosan matrix and La2O3 nanoparticles with Ca2+, Mg2+, phosphate, bicarbonate, and chloride ions. These interactions may modify local hydration and contribute to stabilization of the swollen structure. Nevertheless, the present swelling data do not allow a distinction between specific ion binding and the general effect of ionic strength. The pronounced dependence of hydrogel hydration on the surrounding medium is also consistent with the broader concept of swelling-driven structural responses in polysaccharide-based hydrogel systems [43].
Overall, the results confirmed that the developed materials exhibit pronounced medium-dependent swelling. The strongest initial response occurred under acidic conditions, while more stable swelling profiles were observed in PBS and SBF (Figure 8). Such behavior is relevant for biomedical applications because it indicates that the hydrogels are able to respond to changes in the surrounding chemical environment while retaining substantial liquid-uptake capacity under physiologically relevant conditions [14,15,18]. From the perspective of stimuli-responsive and sensory polymeric systems, the observed dependence of swelling on the incubation environment further supports the potential of these materials to translate changes in their surroundings into measurable alterations in hydration and network expansion [35,43].
Figure 8.
Schematic representation of the interactions between the photocrosslinked methacrylated chitosan/La2O3 hydrogel and water, PBS, SBF, and acetic acid solution.
3.6. Antibacterial Activity Study
The antibacterial activity of the methacrylated chitosan formulations was evaluated against Escherichia coli using samples 1B, 2B, and 3B containing 0, 150, 300, or 500 µL of the La2O3/GHK–Cu suspension. The antibacterial activity of the methacrylated chitosan formulations was evaluated against Escherichia coli using samples 1B, 2B, and 3B containing 0, 150, 300, or 500 µL of the La2O3/GHK–Cu suspension. Bacterial growth was assessed after direct material–bacteria contact for 0, 1, 24, 48, and 72 h. The results are summarized in Table 4.
Table 4.
Antibacterial activity of methacrylated chitosan formulations against Escherichia coli, expressed as the number of recovered colony-forming units (CFUs).
The untreated bacterial control showed confluent growth, confirming the viability of the bacterial suspension and the suitability of the culture conditions. In contrast, the antibiotic control showed complete inhibition of bacterial growth and served as the positive antibacterial reference. Immediately after sample preparation, confluent growth was observed for the control formulations and for several samples containing the active suspension. However, formulation 3B showed a markedly stronger response than 1B and 2B. No colonies were detected for 3B containing either 300 or 500 µL of the La2O3/GHK–Cu suspension. At the lowest additive volume of 150 µL, 4 CFUs were observed for 1B, whereas 6 CFUs were recorded for both 2B and 3B. These results indicate that the immediate antibacterial response varied among the formulations and did not follow a simple linear relationship with the amount of the active suspension.
After 1 h of contact, confluent bacterial growth persisted in the control samples. For formulations containing 500 µL of the active suspension, confluent growth was still observed for 1B and 2B, whereas only 3 CFUs were detected for 3B. At 300 µL, confluent growth was observed for all three formulations. At 150 µL, 5 CFUs were detected for 1B, 13 CFUs for 2B, and no colonies for 3B. Thus, even after a relatively short contact time, formulation 3B exhibited the strongest inhibitory effect.
The differences among the formulations became more pronounced after prolonged contact. Following 24 h of incubation, the control 1B formulation still showed confluent growth, whereas the controls 2B and 3B produced 9 and 8 CFUs, respectively. In the presence of 500 µL of the La2O3/GHK–Cu suspension, 5 CFUs were observed for 1B, 4 CFUs for 2B, and no colonies for 3B. At 300 µL, formulation 1B produced 5 CFUs, whereas both 2B and 3B completely inhibited detectable colony formation. At 150 µL, confluent growth was observed for 1B, while only 1 CFU was detected for 2B and no colonies for 3B.
A similar pattern was maintained after 48 h. The control 1B sample continued to show confluent growth, while the control 2B and 3B formulations produced 10 and 9 CFUs, respectively. For the samples containing 500 µL of active suspension, 5 CFUs were recorded for 1B, 3 CFUs for 2B, and no colonies for 3B. At 300 µL, 1B again produced 5 CFUs, whereas no colonies were detected for either 2B or 3B. At 150 µL, confluent growth persisted for 1B, while 2B produced 1 CFU and 3B showed complete inhibition.
After 72 h, the same overall trend remained evident. The control 1B formulation showed confluent growth, whereas the control 2B and 3B samples produced 8 and 6 CFUs, respectively. In the presence of 500 µL of the active suspension, the colony counts were 5 CFUs for 1B, 2 CFUs for 2B, and 0 CFUs for 3B. At 300 µL, 1B produced 5 CFUs, whereas both 2B and 3B showed no detectable colonies. At 150 µL, confluent growth was still observed for 1B, while 2B produced 1 CFU and 3B remained free of detectable colonies.
Overall, formulation 3B exhibited the strongest and most reproducible antibacterial activity. After prolonged contact, no colonies were detected for any of the 3B samples containing the La2O3/GHK–Cu suspension, irrespective of whether 150, 300, or 500 µL was used. Formulation 2B showed intermediate activity, with complete inhibition at 300 µL and only isolated colonies at 150 and 500 µL. In contrast, formulation 1B consistently showed the weakest antibacterial performance and retained measurable or confluent bacterial growth under several experimental conditions.
The results demonstrate that antibacterial activity depended not only on the presence of the La2O3/GHK–Cu suspension but also on the methacrylated chitosan formulation. Antibacterial activity of metal-oxide-containing hydrogel systems has previously been associated with interactions between inorganic nanophases and microbial cells, while La2O3 nanoparticles themselves have also demonstrated antibacterial activity against both Gram-positive and Gram-negative bacteria [22,44]. Short peptides and tripeptides may additionally contribute to antimicrobial effects through interactions with bacterial membranes and other cellular targets [25,26,27,45]. The formulation prepared at the highest pH, 3B, provided the most favorable antibacterial response. This effect may be related to differences in polymer structure, surface charge, additive dispersion, or release of active components. However, these mechanisms were not directly investigated and therefore cannot be conclusively assigned based on the present data.
A consistent dose-dependent relationship was not observed, because in several cases 150 or 300 µL produced stronger inhibition than 500 µL. This may have resulted from differences in nanoparticle aggregation, sample mixing, hydrogel viscosity, or contact between the bacterial suspension and the active components. Consequently, the antibacterial results should be interpreted as qualitative or semi-quantitative evidence of activity rather than as proof of a linear concentration-dependent effect.
The absence of colonies indicates that no viable bacteria were recovered under the applied assay conditions. Nevertheless, the present experiment does not allow a clear distinction between bacteriostatic and bactericidal effects. Additional tests, including viable-cell counting after removal of the material, live/dead staining, or determination of minimum bactericidal concentration, would be required to establish the precise mechanism of antibacterial action.
3.7. Antioxidant Activity Study
The DPPH assay demonstrated that the investigated formulations possessed measurable radical-scavenging activity and that this activity generally increased with the volume of the incorporated La2O3/GHK–Cu suspension (Figure 9). The most pronounced concentration-dependent response was observed for the 2B formulation prepared at pH 4.0, for which DPPH inhibition increased from 31% at 150 µL to 51% at 300 µL and reached 56% at 500 µL. In contrast, the 3B formulations showed a more moderate increase, from 31% to 35% over the same additive range.
Figure 9.
DPPH assay results.
The antioxidant response may result from the combined contribution of the methacrylated chitosan matrix and the incorporated bioactive components. Chitosan possesses intrinsic radical-scavenging properties associated mainly with its amino and hydroxyl groups, which may participate in electron or hydrogen donation and in the stabilization of reactive radical species [46,47]. The antioxidant activity of chitosan is influenced by several structural parameters, including molecular weight, degree of deacetylation, solubility, and accessibility of free amino groups [46,47]. In the present materials, methacrylation may have reduced the number of free amino groups available for direct radical scavenging; however, residual amino and hydroxyl groups remained present in the polymer network and could still contribute to DPPH inhibition.
GHK–Cu may provide an additional antioxidant contribution. Copper-binding peptides, including GHK, have been associated with modulation of copper-dependent oxidative processes, while GHK–Cu has been reported to reduce oxidative stress and enhance endogenous antioxidant defense pathways in biological models [25,48]. Nevertheless, these cellular and tissue-level effects should not be interpreted as direct evidence of DPPH radical neutralization. In the present cell-free assay, the observed effect may instead be related to redox interactions involving the copper–peptide complex and to its release from the hydrogel matrix.
La2O3 nanoparticles may also affect the measured antioxidant response through surface-mediated interactions with radical species. Previous studies have reported measurable antioxidant activity of La2O3 nanoparticles, although the magnitude of this effect may depend on particle morphology, surface chemistry, concentration, and synthesis conditions [22]. Therefore, the increasing inhibition observed with increasing volume of the La2O3/GHK–Cu suspension may reflect a higher availability of nanoparticle surface sites and copper tripeptide within the tested system.
The stronger antioxidant activity of the 2B series compared with the corresponding 3B samples suggests that the polymer network also influenced the accessibility or release of active components. Differences in network organization, swelling, residual amino-group availability, and interactions between chitosan and the incorporated additives may have affected their contact with DPPH radicals [46,47,48]. Because separate controls containing only methacrylated chitosan, only La2O3 nanoparticles, or only GHK–Cu were not included, the individual contribution of each component cannot be quantified. The antioxidant effect should therefore be attributed to the combined physicochemical behavior of the complete formulation [22,46,47,48].
3.8. Biodegradation Study
The enzymatic degradation of the photocrosslinked methacrylated chitosan formulations 1B, 2B, and 3B was evaluated by monitoring the percentage mass loss during incubation in PBS containing lysozyme (Figure 10). All investigated formulations underwent progressive enzymatic degradation throughout the experimental period, demonstrating that the methacrylated and photocrosslinked chitosan networks remained susceptible to lysozyme-mediated degradation.
Figure 10.
Biodegradation during 7 days.
After the first day of incubation, the mass loss reached 29.41% for 1B, 28.85% for 2B, and 22.56% for 3B. A pronounced increase in degradation was observed on the second day, when the mass loss reached 86.43%, 82.30%, and 73.33% for 1B, 2B, and 3B, respectively. After three days, degradation further increased to 93.24% for 1B, 91.41% for 2B, and 87.57% for 3B. Thus, all formulations exhibited a rapid and progressive enzymatic degradation profile, with the most pronounced mass loss occurring between the first and second day of incubation.
A consistent relationship between the formulation and degradation rate was observed throughout the experiment. Sample 1B exhibited the highest mass loss at each measurement point, followed by 2B, whereas 3B showed the greatest resistance to enzymatic degradation. The degradation order therefore remained 1B > 2B > 3B throughout the entire experimental period.
The observed degradation is directly associated with the susceptibility of the chitosan backbone to lysozyme. Lysozyme is capable of hydrolyzing β-(1→4)-glycosidic linkages within chitosan chains, resulting in progressive chain scission and disintegration of chitosan-based materials [49]. The degradation rate of chitosan hydrogels is influenced by the molecular organization of the polymer network, degree of acetylation, molecular weight, swelling capacity, and accessibility of susceptible glycosidic bonds to the enzyme [17,49].
The differences observed among 1B, 2B, and 3B are consistent with differences in the extent of chitosan methacrylation. The FT-IR analysis demonstrated a progressive increase in the relative methacrylation index from 1B to 2B and 3B. Accordingly, the lower degradation rate of 3B is consistent with the formation of a more extensively modified and subsequently photocrosslinked polymer network, which can restrict enzyme penetration and reduce the accessibility of susceptible glycosidic linkages [49]. In contrast, the lower relative methacrylation of 1B was accompanied by the highest degradation rate, while 2B exhibited intermediate behavior. This consistent relationship between methacrylation and enzymatic mass loss further demonstrates that the synthesis conditions influenced the final organization and stability of the photocrosslinked chitosan network.
Despite photocrosslinking, all three formulations retained pronounced enzymatic degradability. Water uptake by the hydrophilic hydrogel network facilitates diffusion of lysozyme into the material and promotes access of the enzyme to susceptible regions of the chitosan chains [49]. Consequently, photocrosslinking provided sufficient structural stabilization for hydrogel formation and 3D printing while maintaining the inherent biodegradability of the chitosan component.
From the perspective of sensory polymers, the observed lysozyme-dependent mass loss may also represent a potentially measurable material response to the surrounding biochemical environment. In future studies, quantitative correlation between enzyme activity and the rate of hydrogel degradation could provide the basis for developing enzyme-responsive chitosan-based sensing systems [35].
Overall, the results demonstrate controlled differences in enzymatic susceptibility among the investigated formulations. Formulation 3B showed the highest resistance to lysozyme-mediated degradation, whereas 1B degraded most rapidly and 2B exhibited intermediate behavior. The preservation of enzymatic degradability after methacrylation and photocrosslinking is particularly relevant for tissue-engineering applications, where the scaffold should provide initial structural support while remaining capable of progressive degradation and replacement by newly formed tissue [2,30,49].
3.9. Cytotoxicity Evaluation
The cytocompatibility of the methacrylated chitosan formulations was evaluated using the XTT assay (Figure 11). Cell viability depended on both the chitosan variant and the volume of the incorporated La2O3/GHK–Cu suspension. The formulations without the active suspension showed viability values of 77%, 86%, and 92% for 1B, 2B, and 3B, respectively. Thus, the highest baseline cytocompatibility was observed for formulation 3B, whereas 1B exhibited the lowest viability.
Figure 11.
XTT assay results.
A gradual decrease in cell viability was observed with increasing volume of the La2O3/GHK–Cu suspension. For formulation 1B, viability decreased from 77% without the additive to 75%, 70%, and 65% after the incorporation of 150, 300, and 500 µL, respectively. A similar but less pronounced trend was observed for formulation 2B, for which viability decreased from 86% to 82%, 78%, and 72%. Formulation 3B showed the highest viability at every tested additive level, with values of 88%, 85%, and 80% for 150, 300, and 500 µL, respectively.
Using the 70% cell-viability threshold according to ISO 10993-5, most formulations were considered non-cytotoxic [50]. The 1B sample containing 500 µL of the suspension was the only formulation that clearly reduced cell viability below this limit, reaching 65%. The 1B formulation containing 300 µL was located directly at the threshold and should therefore be interpreted with caution. In contrast, all 2B and 3B formulations remained above 70%, even at the highest additive volume.
The results indicate that increasing the amount of the La2O3/GHK–Cu suspension produced a concentration-dependent reduction in metabolic activity. This effect may be related to increased cellular exposure to the incorporated inorganic and bioactive components or to changes in the physicochemical properties of the hydrogel, such as ion release, surface interactions, or local additive concentration. Previous studies indicate that the biological response to La2O3 nanoparticles is concentration- and cell-type-dependent, supporting the need to optimize inorganic-phase loading in biomedical formulations [22,23,24]. At the same time, methacrylated chitosan-based photocrosslinkable hydrogels have previously demonstrated suitability for cytocompatible biomedical and biofabrication applications [51]. However, because the individual effects of the chitosan matrix, La2O3 nanoparticles, GHK–Cu, and other formulation components were not assessed separately in the present study, the mechanism responsible for the reduction in viability cannot be identified conclusively.
Overall, formulation 3B demonstrated the most favorable cytocompatibility profile, maintaining cell viability of at least 80% under all tested conditions. Formulation 2B also showed acceptable cytocompatibility, whereas 1B was more sensitive to increasing additive content. These findings suggest that the 3B matrix provided the best balance between incorporation of the La2O3/GHK–Cu suspension and cellular tolerance among the investigated formulations.
4. Conclusions
Methacrylated chitosan hydrogels functionalized with La2O3 nanoparticles and GHK–Cu exhibited a combination of physicochemical, processing, and biological properties relevant to the development of multifunctional photocrosslinkable materials for biofabrication. FT-IR analysis confirmed successful chitosan modification and demonstrated a progressive increase in the relative methacrylation index from 0.420 for 1B to 0.510 for 2B and 0.631 for 3B. Quantitative evaluation of photocrosslinking further showed double-bond conversion values of approximately 19.7% for 2B and 25.3% for 3B, confirming consumption of methacrylate-associated unsaturated groups during irradiation at 405 nm.
The developed formulations exhibited pronounced medium-dependent swelling, with the strongest initial response observed under acidic conditions and more controlled behavior in PBS and SBF. Because the tested media differed in both pH and ionic composition, these results should be interpreted as evidence of acid-sensitive and environment-dependent swelling rather than as definitive proof of isolated pH responsiveness. Preliminary extrusion-printing experiments demonstrated continuous filament formation, preservation of grid-like architecture, and good shape retention after deposition, supporting the suitability of the formulations for further development as photocrosslinkable materials for extrusion-based 3D bioprinting.
The biological evaluation demonstrated antibacterial and antioxidant activity, substantial lysozyme-mediated degradation, and generally acceptable cytocompatibility. Formulation 3B showed the most favorable overall performance, including the strongest antibacterial response, the highest relative methacrylation and photocrosslinking values, and the highest cytocompatibility among the investigated formulations. Formulation 2B exhibited the highest antioxidant activity, reaching 56% DPPH radical inhibition. Most formulations maintained cell viability at or above the 70% threshold, whereas only the 1B formulation containing the highest additive volume reduced viability below this level.
The progressive lysozyme-mediated mass loss also demonstrates that the photocrosslinked networks remain enzymatically degradable. From the perspective of sensory polymers, this enzyme-dependent degradation may provide a basis for future development of materials in which changes in mass, swelling, or structural integrity can be correlated with biochemical activity in the surrounding environment.
Overall, the developed methacrylated chitosan/La2O3/GHK–Cu systems represent promising multifunctional, extrusion-processable, and photocrosslinkable hydrogel candidates for 3D biofabrication. Their environmentally sensitive swelling and enzymatic response also support further investigation toward stimuli-responsive and sensory applications. Future studies will focus on detailed rheological and mechanical characterization of the formulations and 3D-printed constructs, including evaluation before and after post-stimulation, as well as optimization of their structural and biological performance for advanced tissue-engineering applications.
Author Contributions
Conceptualization, J.R.-P. and Ł.J.; methodology, J.R.-P., Ł.J. and A.S.-B.; validation, J.R.-P. and Ł.J.; investigation, M.R., A.S.-B., K.K. and Ł.J.; data curation, M.R.; writing—original draft preparation, M.R. and J.R.-P.; resources, A.S.-B., Ł.J. and J.R.-P.; supervision, J.R.-P. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by Ministry of Science and Higher Education, grant number SKN/SP/631435/2025 and National Science Centre: UMO-2024/53/N/ST8/03283.
Institutional Review Board Statement
Not applicable.
Informed Consent Statement
Not applicable.
Data Availability Statement
Data available on request.
Acknowledgments
During the preparation of this manuscript, the authors used Chat GPT for the purposes of creating/improving graphics. The authors have reviewed and edited the output and take full responsibility for the content of this publication.
Conflicts of Interest
The authors declare no conflicts of interest.
References
- Murphy, S.V.; Atala, A. 3D Bioprinting of Tissues and Organs. Nat. Biotechnol. 2014, 32, 773–785. [Google Scholar] [CrossRef] [Scilit]
- Fang, W.; Yang, M.; Wang, L.; Li, W.; Liu, M.; Jin, Y.; Wang, Y.; Yang, R.; Wang, Y.; Zhang, K.; et al. Hydrogels for 3D Bioprinting in Tissue Engineering and Regenerative Medicine: Current Progress and Challenges. Int. J. Bioprint. 2023, 9, 759. [Google Scholar] [CrossRef] [Scilit]
- Appuhamillage, G.A.; Ambagaspitiya, S.S.; Dassanayake, R.S. 3D and 4D Printing of Biomedical Materials: Current Trends, Challenges, and Future Outlook. Explor. Med. 2024, 5, 17–47. [Google Scholar] [CrossRef] [Scilit]
- Kuang, X.; Roach, D.J.; Wu, J.; Hamel, C.M.; Ding, Z.; Wang, T.; Dunn, M.L.; Qi, H.J. Advances in 4D Printing: Materials and Applications. Adv. Funct. Mater. 2019, 29, 1805290. [Google Scholar] [CrossRef] [Scilit]
- Choi, J.; Kwon, O.-C.; Jo, W.; Lee, H.J.; Moon, M.-W. 4D Printing Technology: A Review. 3D Print. Addit. Manuf. 2015, 2, 159–167. [Google Scholar] [CrossRef] [Scilit]
- Lai, J.; Wang, C.; Liu, M.; Chen, X.; He, C.; Wang, H. 4D Bioprinting of Programmed Dynamic Tissues. Bioact. Mater. 2024, 37, 348–377. [Google Scholar] [CrossRef] [Scilit]
- Placone, J.K.; Engler, A.J. Recent Advances in Extrusion-Based 3D Printing for Biomedical Applications. Adv. Healthc. Mater. 2018, 7, 1701161. [Google Scholar] [CrossRef] [Scilit]
- Ramiah, P.; du Toit, L.C.; Choonara, Y.E.; Kondiah, P.P.D.; Pillay, V. Hydrogel-Based Bioinks for 3D Bioprinting in Tissue Regeneration. Front. Mater. 2020, 7, 76. [Google Scholar] [CrossRef] [Scilit]
- Heid, S.; Boccaccini, A.R. Advancing Bioinks for 3D Bioprinting Using Reactive Fillers: A Review. Acta Biomater. 2020, 113, 1–22. [Google Scholar] [CrossRef] [Scilit]
- Hospodiuk, M.; Dey, M.; Sosnoski, D.; Ozbolat, I.T. The Bioink: A Comprehensive Review on Bioprintable Materials. Biotechnol. Adv. 2017, 35, 217–239. [Google Scholar] [CrossRef] [Scilit]
- Groll, J.; Boland, T.; Blunk, T.; Burdick, J.A.; Cho, D.-W.; Dalton, P.D.; Derby, B.; Forgacs, G.; Li, Q.; Mironov, V.A.; et al. Biofabrication: Reappraising the Definition of an Evolving Field. Biofabrication 2016, 8, 13001. [Google Scholar] [CrossRef] [Scilit]
- Elango, J.; Zamora-Ledezma, C. Rheological, Structural, and Biological Trade-Offs in Bioink Design for 3D Bioprinting. Gels 2025, 11, 659. [Google Scholar] [CrossRef] [Scilit]
- García-García, A.; Silván, U.; Pérez-Álvarez, L.; Lanceros, S. Comparing the Printability, Biological and Physicochemical Properties of Bio-Based Photo-Crosslinkable Hydrogels. Polymers 2025, 17, 2867. [Google Scholar] [CrossRef] [Scilit]
- Chimene, D.; Lennox, K.K.; Kaunas, R.R.; Gaharwar, A.K. Advanced Bioinks for 3D Printing: A Materials Science Perspective. Ann. Biomed. Eng. 2016, 44, 2090–2102. [Google Scholar] [CrossRef] [Scilit]
- Moon, S.H.; Choi, H.N.; Yang, Y.J. Natural/Synthetic Polymer Materials for Bioink Development. Biotechnol. Bioprocess Eng. 2022, 27, 482–493. [Google Scholar] [CrossRef] [Scilit]
- Gungor-Ozkerim, P.S.; Inci, I.; Zhang, Y.S.; Khademhosseini, A.; Dokmeci, M.R. Bioinks for 3D Bioprinting: An Overview. Biomater. Sci. 2018, 6, 915–946. [Google Scholar] [CrossRef] [Scilit]
- Muthukrishnan, L. Imminent Antimicrobial Bioink Deploying Cellulose, Alginate, EPS and Synthetic Polymers for 3D Bioprinting of Tissue Constructs. Carbohydr. Polym. 2021, 260, 117774. [Google Scholar] [CrossRef] [Scilit]
- Cidonio, G.; Alcala-Orozco, C.R.; Lim, K.S.; Glinka, M.; Mutreja, I.; Kim, Y.H.; Dawson, J.I.; Woodfield, T.B.F.; Oreffo, R.O.C. Osteogenic and Angiogenic Tissue Formation in High-Fidelity Nanocomposite Laponite–Gelatin Bioinks. Biofabrication 2019, 11, 35027. [Google Scholar] [CrossRef] [Scilit]
- Boleti, A.P.A.; Jacobowski, A.C.; Frihling, B.E.F.; Cruz, M.V.; Santos, K.F.D.P.; Migliolo, L.; de Andrade, L.R.M.; Macedo, M.L.R. Wound Healing: Molecular Mechanisms, Antimicrobial Peptides, and Emerging Technologies in Regenerative Medicine. Pharmaceuticals 2025, 18, 1525. [Google Scholar] [CrossRef] [Scilit]
- Adnan, S.B.; Maarof, M.; Fauzi, M.B.; Fadilah, N.I.M. Exploring the Role of Tripeptides in Wound Healing and Skin Regeneration: A Comprehensive Review. Int. J. Med. Sci. 2025, 22, 4175–4200. [Google Scholar] [CrossRef] [Scilit]
- Zheng, S.; Tu, Y.; Li, B.; Qu, G.; Li, A.; Peng, X.; Li, S.; Shao, C. Antimicrobial Peptide Biological Activity, Delivery Systems and Clinical Translation Status and Challenges. J. Transl. Med. 2025, 23, 292. [Google Scholar] [CrossRef] [Scilit]
- Apostolopoulos, V.; Bojarska, J.; Chai, T.T.; Elnagdy, S.; Kaczmarek, K.; Matsoukas, J.; New, R.; Parang, K.; Lopez, O.P.; Parhiz, H.; et al. A Global Review on Short Peptides: Frontiers and Perspectives. Molecules 2021, 26, 430. [Google Scholar] [CrossRef] [Scilit]
- Kandasamy, N. Assessment of Antibacterial Activity of Smaller Chain Tripeptides and Tetrapeptides. Drug Res. 2014, 64, 623–628. [Google Scholar] [CrossRef] [Scilit]
- Hancock, R.E.W.; Sahl, H.G. Antimicrobial and Host-Defense Peptides as New Anti-Infective Therapeutic Strategies. Nat. Biotechnol. 2006, 24, 1551–1557. [Google Scholar] [CrossRef] [Scilit]
- Ding, X.; Zhao, H.; Li, Y.; Lee, A.L.; Li, Z.; Fu, M.; Li, C.; Yang, Y.Y.; Yuan, P. Synthetic Peptide Hydrogels as 3D Scaffolds for Tissue Engineering. Adv. Drug Deliv. Rev. 2020, 160, 78–104. [Google Scholar] [CrossRef] [Scilit]
- Teixeira-Costa, B.E.; Andrade, C.T. Chitosan as a Valuable Biomolecule from Seafood Industry Waste in the Design of Green Food Packaging. Biomolecules 2021, 11, 1599. [Google Scholar] [CrossRef] [Scilit]
- Karthikeyan, S.; Dhanakodi, K.; Shanmugasundaram, K.; Surendhiran, S. Synthesis and Characterization of Lanthanum Oxide Nanoparticles: A Study on the Effects of Surfactants. Mater. Today Proc. 2022, 49, 2620–2625. [Google Scholar] [CrossRef] [Scilit]
- Rizwan, M.; Yahya, R.; Hassan, A.; Yar, M.; Azzahari, A.D.; Selvanathan, V.; Sonsudin, F.; Abouloula, C.N. pH Sensitive Hydrogels in Drug Delivery: Brief History, Properties, Swelling, and Release Mechanism, Material Selection and Applications. Polymers 2017, 9, 137. [Google Scholar] [CrossRef] [Scilit]
- Delmar, K.; Bianco-Peled, H. The Dramatic Effect of Small pH Changes on the Properties of Chitosan Hydrogels Crosslinked with Genipin. Carbohydr. Polym. 2015, 127, 28–37. [Google Scholar] [CrossRef] [Scilit]
- Thambiliyagodage, C.; Jayanetti, M.; Mendis, A.; Ekanayake, G.; Liyanaarachchi, H.; Vigneswaran, S. Recent Advances in Chitosan-Based Applications—A Review. Materials 2023, 16, 2073. [Google Scholar] [CrossRef] [Scilit]
- Percival, S.L.; McCarty, S.; Hunt, J.A.; Woods, E.J. The Effects of pH on Wound Healing, Biofilms, and Antimicrobial Efficacy. Wound Repair Regen. 2014, 22, 174–186. [Google Scholar] [CrossRef] [Scilit]
- Neumann, M.; Kofler, C.; Pester, C.W.; Stahlschmidt, U.; Karg, M.; Schmalz, H.; Agarwal, S.; Greiner, A. Stimuli-Responsive Hydrogels: The Dynamic Smart Biomaterials of Tomorrow. Macromolecules 2023, 56, 8377–8392. [Google Scholar] [CrossRef] [Scilit]
- Díaz-Payno, P.J.; Kalogeropoulou, M.; Badreldin, A.; Hagel, E.; Naranda, J.; Manferdini, C.; Paolella, F.; Gabusi, E.; Kock, L.; van Weeren, P.R.; et al. Swelling-Dependent Shape-Based Transformation of a Human Mesenchymal Stromal Cells-Laden 4D Bioprinted Construct for Cartilage Tissue Engineering. Adv. Healthc. Mater. 2023, 12, 2201891. [Google Scholar] [CrossRef] [Scilit]
- Hu, H.; Huang, C.; Galluzzi, M.; Ye, Q.; Xiao, R.; Yu, X. Editing the Shape Morphing of Monocomponent Natural Polysaccharide Hydrogel Films. Research 2021, 2021, 9786128. [Google Scholar] [CrossRef] [Scilit]
- Zu, S.; Zhang, Z.; Liu, Q.; Wang, Z.; Song, Z.; Guo, Y.; Xin, Y.; Zhang, S. 4D Printing of Core–Shell Hydrogel Capsules for Smart Controlled Drug Release. Bio-Des. Manuf. 2022, 5, 294–304. [Google Scholar] [CrossRef] [Scilit]
- Wahid, F.; Zhong, C.; Wang, H.-S.; Hu, X.-H.; Chu, L.-Q. Recent Advances in Antimicrobial Hydrogels Containing Metal Ions and Metals/Metal Oxide Nanoparticles. Polymers 2017, 9, 636. [Google Scholar] [CrossRef] [Scilit]
- Kishore, J.; Dunuwilla, T.S.; Bupesh Raja, V.K.; Louis, S.A.; Boopathy, L.K.; Saravanan, D.; Zhvania, M.; Gupta, M. Characterization of La2O3 Nanoparticles and Their Effects on Bacteria, Vero and MG63 Cells, and Zebrafish Development. Bioengineering 2025, 12, 995. [Google Scholar] [CrossRef] [Scilit]
- Vijayan, V.; Lakra, R.; Korrapati, P.S.; Kiran, M.S. Lanthanum Oxide Nanoparticle-Collagen Bio Matrix Induced Endothelial Cell Activation for Sustained Angiogenic Response for Biomaterial Integration. Colloids Surf. B Biointerfaces 2022, 216, 112589. [Google Scholar] [CrossRef] [Scilit]
- Vijayan, V.; Sreekumar, S.; Ahina, K.M.; Lakra, R.; Kiran, M.S. Lanthanum Oxide Nanoparticles Reinforced Collagen κ-Carrageenan Hydroxyapatite Biocomposite as Angio-Osteogenic Biomaterial for In Vivo Osseointegration and Bone Repair. Adv. Biol. 2023, 7, e2300039. [Google Scholar] [CrossRef] [Scilit]
- Wan, A.; Xu, Q.; Sun, Y.; Li, H. Antioxidant Activity of High Molecular Weight Chitosan and N,O-Quaternized Chitosans. J. Agric. Food Chem. 2013, 61, 6921–6928. [Google Scholar] [CrossRef] [Scilit]
- Wang, Z.; Yan, Y.; Zhang, Z.; Li, C.; Mei, L.; Hou, R.; Liu, X.; Jiang, H. Effect of Chitosan and Its Water-Soluble Derivatives on Antioxidant Activity. Polymers 2024, 16, 867. [Google Scholar] [CrossRef] [Scilit]
- Thomas, C.E. The Influence of Medium Components on Cu2+-Dependent Oxidation of Low-Density Lipoproteins and Its Sensitivity to Superoxide Dismutase. Biochim. Biophys. Acta 1992, 1128, 50–57. [Google Scholar] [CrossRef] [Scilit]
- Zhang, Q.; Yan, L.; Lu, J.; Zhou, X. Glycyl-L-Histidyl-L-Lysine-Cu2+ Attenuates Cigarette Smoke-Induced Pulmonary Emphysema and Inflammation by Reducing Oxidative Stress Pathway. Front. Mol. Biosci. 2022, 9, 925700. [Google Scholar] [CrossRef] [Scilit]
- Ahn, J.; Ryu, J.; Song, G.; Whang, M.; Kim, J. Network Structure and Enzymatic Degradation of Chitosan Hydrogels Determined by Crosslinking Methods. Carbohydr. Polym. 2019, 217, 160–167. [Google Scholar] [CrossRef] [Scilit]
- Zhu, L.; Bratlie, K.M. pH-Sensitive Methacrylated Chitosan Hydrogels with Tunable Physical and Chemical Properties. Biochem. Eng. J. 2018, 132, 38–46. [Google Scholar] [CrossRef] [Scilit]
- Maiz-Fernández, S.; Pérez-Álvarez, L.; Silván, U.; Vilas-Vilela, J.L.; Lanceros-Mendez, S. Photocrosslinkable and Self-Healable Hydrogels of Chitosan and Hyaluronic Acid. Int. J. Biol. Macromol. 2022, 216, 291–302. [Google Scholar] [CrossRef] [Scilit]
- Li, B.; Wang, L.; Xu, F.; Gang, X.; Demirci, U.; Wei, D.; Li, Y.; Feng, Y.; Jia, D.; Zhou, Y. Hydrosoluble, UV-Crosslinkable and Injectable Chitosan for Patterned Cell-Laden Microgel and Rapid Transdermal Curing Hydrogel In Vivo. Acta Biomater. 2015, 22, 59–69. [Google Scholar] [CrossRef] [Scilit]
- Zanon, M.; Chiappone, A.; Garino, N.; Canta, M.; Frascella, F.; Hakkarainen, M.; Pirri, C.F.; Sangermano, M. Microwave-Assisted Methacrylation of Chitosan for 3D Printable Hydrogels in Tissue Engineering. Mater. Adv. 2022, 3, 514–525. [Google Scholar] [CrossRef] [Scilit]
- Osi, A.R.; Zhang, H.; Chen, J.; Zhou, Y.; Wang, R.; Fu, J.; Müller-Buschbaum, P.; Zhong, Q. Three-Dimensional-Printable Thermo/Photo-Cross-Linked Methacrylated Chitosan–Gelatin Hydrogel Composites for Tissue Engineering. ACS Appl. Mater. Interfaces 2021, 13, 22902–22913. [Google Scholar] [CrossRef] [Scilit]
- Yuce-Erarslan, E.; Tutar, R.; İzbudak, B.; Alarçin, E.; Kocaaga, B.; Guner, F.S.; Emik, S.; Bal-Ozturk, A. Photo-Crosslinkable Chitosan and Gelatin-Based Nanohybrid Bioinks for Extrusion-Based 3D-Bioprinting. Int. J. Polym. Mater. Polym. Biomater. 2023, 72, 1–12. [Google Scholar] [CrossRef] [Scilit]
- Bilici, C.; Tatar, A.G.; Koc, B. A UV-Free and Cytocompatible Crosslinking Strategy for Methacrylated Chitosan Hydrogels via Bisulfite-Initiated Polymerization for Embedded 3D Bioprinting. Int. J. Biol. Macromol. 2025, 328, 147583. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.