Abstract
This study systematically investigated the bearing capacity and failure mechanisms of ultra-high-performance concrete (UHPC) pipe jacking structures using three-edge bearing tests and numerical simulations. Full-scale double-layer reinforced pipes had an inner diameter of 2.5 m and wall thicknesses of 180 mm (P1) and 200 mm (P2). The tests showed that the failure process can be divided into four stages: elastic deformation, crack propagation, reinforcement yielding, and ultimate failure. Increasing the wall thickness significantly improved performance: P2 had a cracking load 52.73% higher and an ultimate bearing capacity 5.7% higher than P1, with better deformation resistance and crack control. A theoretical model considering the plastic hinge mechanism at the pipe crown was developed, treating the three-edge load as an equivalent distributed plate load. The calculated results agreed well with experimental measurements. An ABAQUS finite element model successfully reproduced the full mechanical response from initial loading to failure. Parametric analysis indicated optimal performance at a hoop reinforcement ratio of approximately 1.4%. Even at 0.6%, the ultimate bearing capacity reached 367 kN/m, meeting current design code requirements. This study is novel in conducting full-scale UHPC pipe jacking tests, proposing a theoretical model accounting for crown plastic hinges, and establishing a finite element method that reproduces the entire failure process. Optimizing wall thickness and hoop reinforcement can enhance structural safety and durability, providing guidance for the design and engineering of pipe jacking structures.
1. Introduction
With the rapid development of urbanization, underground pipeline systems are becoming increasingly important for urban infrastructure. Pipe jacking technology is widely used in municipal engineering because it causes little disturbance to the ground surface and has high construction efficiency. However, traditional reinforced concrete pipes often suffer from cracking, leakage, and durability problems during long-term service. These problems are mainly caused by the limited mechanical properties of conventional concrete and the complex loading environment. Therefore, improving the structural performance and durability of pipeline materials has become an important research topic in underground engineering [1,2,3].
Ultra-high-performance fiber-reinforced concrete (UHPC) is an advanced cement-based composite material. It improves both strength and toughness. This improvement is achieved by optimizing particle gradation, adding ultra-fine mineral admixtures and high-range water reducers, and using the crack-bridging and energy dissipation effects of steel fibers. Compared with conventional concrete, UHPC shows clear advantages in compressive strength, tensile strength, and ductility.
Many researchers have studied the material properties of UHPC. Abu-Lebdeh et al. found that hooked-end steel fibers provide strong anchorage with the matrix and improve pull-out resistance [4]. Hybrid fiber systems can further enhance the tensile strength and post-cracking load capacity of UHPC [5,6]. Adjusting the fiber type and fiber volume fraction can reduce shrinkage cracking and improve ductility and durability [7,8,9]. Yoo et al. reported that when the fiber content is lower than 3%, both compressive strength and elastic modulus increase with fiber content because steel fibers inhibit crack propagation [10]. Ji et al. and Rong et al. investigated the dynamic mechanical properties of UHPC using split Hopkinson pressure bar tests. Their results showed that UHPC has strong strain-rate sensitivity and good energy absorption capacity [11,12]. Khosravani et al. also studied fracture characteristics of UHPC under dynamic loading [13]. In addition, curing conditions have a significant influence on UHPC performance. Steam curing and autoclave curing can improve both early-age and long-term strength [14].
UHPC has also been widely studied in structural engineering applications. Previous studies have shown that UHPC structural components have better mechanical performance than conventional concrete structures. For example, research on utility tunnel segments showed that the flexural stiffness and shear capacity of UHPC joints are 1.5–2.0 times higher than those of C50 concrete joints [15]. Liu reported that reinforced UHPC pipes have much higher bearing capacity and deformation capacity than ordinary pipes [16]. Other studies have shown that UHPC can improve structural reliability, reduce shrinkage cracking, and reduce life-cycle costs [17,18]. The length of steel fibers and hybrid fiber systems also influences the cracking load and post-cracking behavior of concrete pipes [19,20,21]. In addition, experimental studies confirmed that UHPC precast components have good potential for underground engineering applications [22]. Although many studies have investigated UHPC materials and structural applications, research on UHPC pipe jacking structures is still limited. Most previous studies focused on beams, tunnel segments, and other structural members. Few studies have examined the bearing capacity and failure mechanisms of large-diameter UHPC pipes under external loads. In particular, the crack propagation process, deformation behavior, and ultimate bearing capacity under three-edge bearing loads are not yet fully understood. Reliable theoretical models and numerical simulation methods are also still limited [23]. Recent studies further demonstrated that FRP grid reinforcement can increase the initial cracking load of UHPC pipes by about 30%, while increasing pipe thickness and applying CFRP jacketing can enhance ring stiffness by up to 422% and 115%, respectively, significantly improving structural stiffness and load-carrying capacity [24]. Moreover, research on FRP-reinforced UHPC tubular members showed that steel fibers can improve static load capacity, while fatigue loading may lead to stiffness degradation and up to a 48.86% reduction in residual bearing capacity, and a fatigue endurance limit of 0.5 Pu was recommended [25].
Therefore, this study investigates the mechanical behavior of UHPC pipe jacking structures through full-scale three-edge bearing tests, theoretical analysis, and numerical simulation. Two UHPC pipes with an inner diameter of 2.5 m and different wall thicknesses were tested. The load–displacement response, crack development, and reinforcement strain were analyzed. A theoretical model considering the plastic hinge mechanism at the pipe crown was proposed to predict the cracking load and ultimate bearing capacity. In addition, a finite element model was established using ABAQUS to simulate the full failure process. The results provide a reference for the design and optimization of UHPC pipe jacking structures.
2. External Pressure Load-Bearing Performance Test of Pipe Jacking
2.1. Pipeline and Corresponding Material Parameters
Two test pipes were cast for this experiment, both with an inner diameter of 2.5 m and wall thicknesses of 180 mm (P1) and 200 mm (P2). The pipes use a double-layer reinforcement system: the outer layer consists of ten 10 mm steel bars spaced at 120 mm, and the inner layer consists of ten 10 mm steel bars spaced at 100 mm. The outer protective cover is 30 mm thick, and the inner cover is 25 mm. The pipes were cast with C150-grade ultra-high-performance concrete (UHPC), which mainly comprises cement, fine sand, quartz powder, mineral admixtures such as silica fume, high-performance superplasticizers, and fine steel fibers. Key material parameters, including strength, elastic modulus, creep coefficient, and Poisson’s ratio, are listed in Table 1. The steel bars are HRB400, with a standard tensile strength of 400 MPa, an ultimate tensile strength of 540 MPa, an elastic modulus of 200 GPa, a yield strength of 400 MPa, and a yield strain of 2 × 10−3. The reinforcement design is identical for both pipes, and details of the inner and outer steel bars, including area and quantity, are given in Table 2. Figure 1 shows photos of the pipes during reinforcement installation and after concrete casting.
Table 1.
Material parameters of C150 ultra-high-performance concrete.
Table 2.
Reinforcement details of C150 ultra-high-performance concrete pipe.
Figure 1.
Photo of on-site test tube processing.
2.2. Three-Edge Bearing Test
The pipe’s three-edge bearing capacity test was performed following the three-point method in GB/T 16752-2017 [26], Test Methods for Concrete and Reinforced Concrete Drainage Pipes. First, the load was applied at a constant rate up to 80% of the estimated cracking load and held for 1 min. If no cracks appeared, the load was increased by 10% increments until the cracking load was reached and maintained for 3 min. When the crack width was below 0.2 mm, the load was further increased in 5% increments. The load at which the crack width reached 0.2 mm was recorded as the cracking load. If the crack width exceeded 0.2 mm, the previous load increment was taken as the cracking load. Afterward, the load was raised to 80% of the expected failure load and held for 1 min. If the pipe did not fail, the load was increased by 10% increments until failure. If failure still did not occur, 5% increments were applied until the pipe fully lost its load-bearing capacity. The on-site loading and test arrangement are shown in Figure 2, where Dw is the outer diameter of the pipe.
Figure 2.
External pressure loading test of the pipe and loading direction. (a) On-site loading diagram. (b) Loading schematic diagram.
The test frame, in addition to fixed components, includes upper and lower support beams that extend along the full length of the pipe. The upper support beam should have a maximum deflection under the peak load of no more than 1/720 of the pipe test length. A rubber pad is placed between the steel beam and the pipe, with the same length and width as the steel beam, a thickness of at least 25 mm, and a Shore hardness of 45–60. The lower support beam is composed of two hardwood pieces, with a cross-sectional width of at least 50 mm, a thickness of at least 25 mm, and a length not less than the pipe test length. The contact surface between the hardwood lower beams and the pipe is rounded with a radius of 12.5 mm. The net spacing between the two lower beams is 1/12 of the pipe outer diameter but not less than 25 mm. The radial load applied during the test was calculated according to Equation (1).
P = F/L
In the formula, P is defined as the radial loading value, measured in kN/m; F is defined as the total load value, measured in kN; and L is the effective length of the pipe, measured in meters.
2.3. Layout of Measuring Points
The layout for measuring displacement, steel strain, and concrete strain is shown in Figure 3. The monitoring section is located at the radial center of the pipe. Steel strain gauges are installed on both inner and outer reinforcements along the radial directions, with one gauge every 45°, giving a total of 16 points. Displacement sensors are placed on the inner concrete wall at the monitoring section. Four sensors are evenly distributed around the cross-section to ensure full coverage.
Figure 3.
Displacement and reinforcement monitoring point layout diagram.
2.4. Analysis of Test Results
2.4.1. Pipe Deformation and Failure Modes
Figure 4 shows the pipe displacement–load curve. Δx and Δy represent the horizontal and vertical displacements of the monitored section during loading, respectively.
Figure 4.
Load–displacement curves in horizontal and vertical directions of pipe. (a) Pipe P1. (b) Pipe P2.
Figure 4 shows that the load–displacement image of the UHPC pipe is roughly divided into three stages of horizontal (Δx) and vertical (Δy) displacement deformation. Taking pipe P1 as an example: 1. Elastic stage: In the initial loading phase, when the load is below 220 kN/m, the load–displacement curve of the pipe approximates linear variation, and the pipe structure is under elastic stress, with no cracking observed. 2. Crack development stage: As the load increases, the slope of the curve gradually changes. Numerous small cracks appear in the pipe body, and although the number of cracks increases, the width of the cracks does not vary significantly. 3. Yielding stage: This stage continues until the tensile reinforcement yields. The crack width of the pipe starts to increase, and the tensile reinforcement begins to yield. After entering the yielding stage, the increase in load is much smaller than the increase in displacement, and the crack width begins to enlarge, while the increase in the number of cracks is not significant. 4. Failure stage: At this point, the reinforcement reaches its yield limit, the peak load reaches 437 kN/m, and the pipe displacement reaches 42.3 mm. The crack width continuously increases, forming through cracks on the inner walls at the top and bottom of the pipe, with debris continually falling from the cracks accompanied by the sound of steel fibers being pulled out. As the load decreases, the pipe displacement continues to increase until failure occurs. The load–displacement trend of pipe P2 is similar to that of P1; however, due to an increase in the pipe wall thickness of 20 mm, the crack load value for the pipe P2 is 336 kN/m, which is 52.73% higher than P1. At the peak load of 462 kN/m, the displacement is only 24.5 mm. Therefore, it can be seen that the increase in the diameter-to-thickness ratio significantly enhances the anti-deformation capacity of the UHPC pipe.
2.4.2. Crack Development and Analysis
Figure 5a,b show the development of main cracks in P1 (wall thickness 180 mm) and P2 (wall thickness 200 mm) test pipes under different loads.
Figure 5.
Crack development of the test pipe. (a) Crack development of P1 (180 mm) pipeline. (b) Crack development of P2 (200 mm) pipeline.
Based on the observations from Figure 5, it can be concluded that for pipe P1, cracks first appeared on the inner wall at the crown during loading, followed by crack initiation on the inner wall at the bottom and on the outer walls on both the left and right sides. When the load reached 220 kN/m, the crack width at the inner wall at the crown increased to 0.20 mm, and this load was defined as the cracking load of the pipe. As the load increased to 369 kN/m, the crack widths at both the crown and the bottom increased rapidly, with the crack width at the inner wall at the bottom reaching 1.77 mm and that at the inner wall at the crown reaching 1.40 mm, both exceeding 1 mm. In contrast, the increase in crack width on the outer walls on the left and right sides was relatively small, with crack widths of only 0.45 mm and 0.47 mm, corresponding to 25.42% and 26.55% of the crack width at the inner wall at the bottom and 32.14% and 33.57% of that at the inner wall at the crown, respectively, all of which were less than 50%. When the load reached 437 kN/m, the reinforcement in the tensile zone at the crown yielded, resulting in a rapid increase in crack width; at this stage, the crack width at the inner wall at the crown was the largest compared with those at the inner wall at the bottom and the outer walls on the left and right sides, reaching 3.86 mm. The crack widths at the inner wall at the bottom (2.85 mm), the outer wall on the left side (1.34 mm), and the outer wall on the right side (1.41 mm) accounted for 73.83%, 34.72%, and 36.53% of the crack width at the inner wall at the crown, respectively, with the crack widths on both sides remaining below 50% of that at the crown.
Pipe P2, with a larger wall thickness, showed slower crack width growth and fewer cracks at each loading stage. Its cracking load and failure load were higher, reaching 336 kN/m and 462 kN/m, respectively. This indicates that increasing the pipe wall thickness significantly improves both cracking and failure loads. At failure, the four main cracks of P2 measured 1.85 mm, 2.27 mm, 0.53 mm, and 0.58 mm. Compared with P1, these are only 64.91%, 58.81%, 39.55%, and 41.13%, respectively. The results show that increasing the diameter-to-thickness ratio effectively limits crack width and the spread of cracks on all sides of the pipe. Figure 6 shows cracks at the pipe crown and invert. Main cracks appear at both top and bottom. Cracks on the outer sides are minor.
Figure 6.
Crack propagation at final pipe failure. (a) Bottom cracks. (b) Top cracks. (c) Overall cracks.
2.4.3. Steel Strain Analysis
Figure 7 shows the strain development of the inner and outer reinforcement layers in the two pipes. For the outer reinforcement, compressive strain occurs only at 0° and 180°, while tensile strain appears at all other points. In contrast, the inner reinforcement shows tensile strain at all measured points.
Figure 7.
Reinforcement strain of pipes P1 and P2. (a) Strain of inner reinforcement in pipe P1. (b) Strain of outer reinforcement in pipe P1. (c) Strain of inner reinforcement in pipe P2. (d) Strain of outer reinforcement in pipe P2.
According to the strain distribution diagrams, as the load gradually increases, the inner reinforcement shows tensile behavior at the crown, invert, and both lateral sides. Both compressive and tensile strains increase continuously. Before the load reaches 414 kN/m, the strain at all inner reinforcement points rises steadily. The increments are more noticeable at the crown, invert, and lateral sides. When the load reaches 412 kN/m, abrupt strain changes appear at all points of both inner and outer reinforcement. At 462 kN/m, the tensile strain of the inner reinforcement reaches 2.11 × 10−3 at the crown and 1.95 × 10−3 at the invert. The outer reinforcement strains at the left and right sides reach 1.89 × 10−3 and 1.91 × 10−3, respectively. Since the yield strain of HRB400 is about 2.0 × 10−3, the inner reinforcement has yielded, indicating structural failure of the pipe.
For pipe P2, the mechanical response is similar to that of P1. During loading, strains at the crown, invert, and both lateral sides of the inner and outer reinforcement layers increase steadily. At 452 kN/m, sudden strain changes occur at all measurement points, but the strain has not yet reached the yield level. When the load reaches 462 kN/m, the tensile strain of the inner reinforcement reaches 2.08 × 10−3 at the crown and 1.94 × 10−3 at the invert. This indicates yielding of the inner reinforcement and the onset of structural failure of the pipe.
3. UHPC Pipeline Bearing Capacity Calculation Model
3.1. Cracking Load Analysis
According to Becerril García et al. [23], experimental tests and numerical analyses show that when the ratio of the bottom support spacing w to the pipe diameter D is less than 0.1, the three-edge load can be replaced by a flat-plate load. In the standard three-edge bearing test, w/D is 0.083. Under this condition, the flat-plate load can reasonably represent the three-edge load. This simplification helps build a simpler mechanical model of the pipe, as shown in Figure 8. The cracking load of the pipe is mainly determined by the maximum tensile stress or the maximum bending moment at the most unfavorable section. Test observations show that the maximum circumferential bending moment occurs at the inner crown of the pipe. Therefore, the cracking load can be obtained by calculating the circumferential bending moment at the crown and combining it with the tensile strength of the material.
Figure 8.
Simplified schematic diagram of the three-edge load.
When the tensile stress at the inner crown reaches the axial tensile strength of UHPC, cracking starts in the concrete. Under flat-plate loading, the cracking load per unit length of the pipe can be expressed as:
Mmax is the maximum circumferential bending moment when the elastic failure of the pipeline per unit length occurs under the action of plate load. β is the bending moment coefficient. b denotes the width of a single-sided section.
The bending moment when the tensile stress at the inner edge of the pipe top reaches the axial tensile strength is the cracking moment (Mcr):
The stress distribution of concrete in the tensile area of the double-layer reinforced UHPC pipe top is simplified to triangular and rectangular distribution. The compressive stress of concrete in the compressive area is very small, and the stress distribution is similar to triangular, as shown in Figure 9. According to the above test results, the tensile strain value of UHPC is 0.76ft, and ft represents the axial tensile strength of UHPC. εc is the compressive strain of concrete at the edge of the compressive zone under cracking load, and εt0 is the initial cracking strain of UHPC. x0 represents the height of the UHPC compression zone; xt represents the height of the UHPC tensile zone. Ms is the bending moment of the resultant force of the inner reinforcement about the neutral axis. Mc is the bending moment of the equivalent rectangular resultant force in the tensile zone about the neutral axis.
Figure 9.
Distribution of cracking bending moment at the inner section of the pipe crown.
When Mmax = Mcr, the pipeline is about to crack. Combined with (2), (3) and (4), the crack load of the pipeline is:
The calculated cracking loads Fcr are 230 kN/m and 355 kN/m for pipes P1 and P2, respectively. These values differ from the measured results by 4.21% and 5.76%, compared with the experimental values of 220 kN/m for P1 and 336 kN/m for P2. The calculated cracking moments show good agreement with the test results. This indicates that Equation (5) can effectively predict the cracking load of UHPC pipes when the tensile strength of UHPC is considered and the radial load is simplified as a plate load.
3.2. Ultimate Bearing Capacity Analysis
Once the tensile reinforcement in the pipe yields, the stiffness of the cross-section decreases significantly. The structural stability then reduces, and the pipe gradually loses its load-bearing capacity. Therefore, the ultimate bearing capacity of a UHPC pipe can be simplified by assuming a plastic hinge forms at the crown section. Under this failure mechanism, the ultimate bearing capacity of the pipe is mainly controlled by the plastic bending moment at the crown section.
The stress analysis of the cross-section of the top of the double-layer reinforced UHPC pipe is shown in Figure 10.
Figure 10.
Force analysis of the crown section of a UHPC pipe with double-layer reinforcement.
The crown section of a UHPC pipe with double-layer reinforcement can be simplified as a doubly reinforced rectangular section under bending. When plastic hinge failure occurs, the pipe reaches the ultimate limit state. At this stage, most of the concrete has cracked and no longer resists tension. Only the concrete in the compression zone near the hinge support remains effective. Both the inner and outer circumferential reinforcements are subjected to tensile stress. The concrete at the hinge support is under compression. Based on these assumptions, a force equilibrium analysis is performed for the vertical section at the pipe crown.
According to the equilibrium equation, Mv is obtained as follows:
In the formula, σvo and σvi are the outer steel bar and the inner steel bar of the vertical section in MPa. As and As′ are the cross-sectional areas of the inner and outer steel bars in mm2 and the thicknesses of the inner and outer protective layers are as and as′ in mm, respectively.
The stress–strain constitutive relationship of the reinforcement under monotonic loading proposed by Zhu [27] is adopted. In this study, the reinforcement used in the pipe has high strength and a low yield plateau. Therefore, a bilinear model is selected to describe its constitutive behavior, as shown in Figure 11.
Figure 11.
Bilinear model.
Figure 10 shows the behavior of the inner and outer reinforcement during pipe deformation. Based on the trends in the figure, the stress–strain relationship of the inner and outer reinforcement at the pipe crown and along the arch line is derived. The derivation takes the yielding of the outer reinforcement at the crown and the inner reinforcement along the arch line as the basis for section failure.
εvo and εvi are the internal tensile strains of the outer and inner steel bars of the vertical section and the outer and inner steel bars of the horizontal section, respectively; fy and fu are the yield stress and ultimate stress of the steel bar in MPa; and εy and εu are the yield strain and ultimate strain of the steel bar, respectively. Er is the elastic modulus of steel in MPa.
Assuming that the exposed length of the reinforcement is equal to its tensile elongation length, the geometric relationship governing the deformation compatibility between the inner and outer layers of reinforcement can be derived as follows:
In the formula, Ri is the radius of the inner ring of the pipe, and simultaneously, Formulas (7) to (10) are solved:
Formula (11) is simplified as:
When Mmax = Mν, Formulas (6), (9) and (13) are brought into (5), and the ultimate bearing capacity of the pipeline when the steel bar yields can be obtained:
By using the experimental parameters of pipes P1 and P2, the calculated ultimate bearing capacities, Fcr, are 385.14 kN/m and 435.10 kN/m, respectively. Compared with the experimental values of 412 kN/m for P1 and 462 kN/m for P2, the relative errors are 6.52% and 5.82%. Considering that the calculated cracking moments, which include the tensile strength of UHPC, agree well with the experiments, Equation (14) is shown to be suitable for predicting the failure load of UHPC pipes. The calculation assumes that the three-edge load can be simplified as a flat-plate load and that failure occurs by forming a plastic hinge at the pipe crown.
4. Numerical Simulation of Pipeline Performance
4.1. Model Establishment
A UHPC pipe model was built in ABAQUS based on the experimental data. Comparison with pipe P1 in the external pressure test validated the accuracy of the model. This provides a reliable reference for nonlinear finite element analysis of UHPC pipes.
The finite element model for simulating the three-edge bearing test is shown in Figure 12. It consists of two parts: the concrete pipe and the reinforcement cage. The model uses the same dimensions and reinforcement ratio as pipe P1. The steel reinforcement is modeled with an elastoplastic constitutive law, having a maximum tensile strength of 540 MPa, a yield strength of 400 MPa, and a yield strain of 2 × 10−3. After optimizing the element type and mesh density, the concrete pipe is modeled with eight-node incompatible brick elements (C3D8I) to balance accuracy and computational cost. The reinforcement cage is represented by two-node 3D truss elements (T3D2), with element types and quantities listed in Table 3.
Figure 12.
Finite element numerical model of pipeline external pressure load test.
Table 3.
Types and quantities of elements in the three-point test model of the experimental pipeline.
To ensure that the numerical results are not affected by mesh density, a mesh convergence analysis was conducted. The results indicate that finer meshes could not meet the accuracy requirements, and the computed results varied significantly with mesh refinement. When the global mesh size was increased from 50 to 100, the variation in key parameters decreased markedly, indicating that the results had become stable. Therefore, a mesh with a global size of 100 was selected as the optimal scheme, achieving a good balance between computational accuracy and efficiency, and was adopted for all numerical simulations in this study. The performance of meshes with different sizes is shown in Figure 13.
Figure 13.
Schematic of mesh convergence for different global mesh sizes. (a) Mesh convergence behavior with a global size of 50. (b) Mesh convergence behavior with a global size of 100.
4.2. Damage Plasticity Constitutive Model for Ultra-High-Performance Concrete
The compressive constitutive relationship of UHPC is based on the CEB-FIP model proposed by Yang [28].
In the equation, εo = 3500 με, ξ = ε/εo, fc is the compressive strength, and n = Ec/Es is the ratio of the initial modulus of elasticity to the secant modulus at the peak point. According to the material performance test values provided by the manufacturer before the external pressure load test, fc is taken as 150 MPa, and n is taken as 3.316.
The tensile constitutive relationship of UHPC adopts the bilinear reinforcement model proposed by Zhang [29].
In the equation, fct is the average tensile strength, calculated based on the initial cracking strength and ultimate strength of UHPC; εca and εpc are the peak tensile strain in the elastic stage and the ultimate tensile strain, respectively. Based on the material performance test values provided by the manufacturer before the full-scale test, fct is taken as 6.4 MPa, εca as 1.71 × 10−4, and εpc as 2.0 × 10−4.
Referring to the research of existing scholars, the relevant parameters are shown in Table 4.
Table 4.
Values of other plasticity parameters.
4.3. Comparison of Simulation and Experimental Results
Figure 14a,b compare the experimental and numerical results for pipe P1, including the load–displacement curves and the variation in crack width at the crown with increasing load. In the numerical simulation, the crack width during concrete cracking is defined by the relative displacement between midpoint 1 and midpoint 2 in the plastic damage zone at the top of the pipe, as illustrated in Figure 14c.
Figure 14.
Comparison between experimental results and numerical simulation results. (a) The displacement load curve of numerical simulation and external pressure load test. (b) The comparison between the simulated load-crack width curve and the test curve. (c) The schematic diagram of simulated crack width.
The comparison in Figure 14a,b shows that before the crack width reaches 0.2 mm, the pipe remains in the elastic stage, with a linear relationship between load, displacement, and crack width. In the external pressure test, pipe P1 reached 220 kN/m at a 0.2 mm crack width, while the simulation predicted 232 kN/m, a deviation of only 5.45%. During the crack propagation stage, the load increases, but displacement and crack width change little. This is mainly due to steel fibers effectively bridging the cracks, transferring stress to uncracked areas and increasing the number of cracks without significant widening. As the load approaches the peak, a visible main crack develops on the inner top wall of the pipe. The crack width then increases rapidly, while the load rises much more slowly than displacement and crack width. After reaching the peak load, the pipe enters the failure stage. The load gradually decreases due to continuous steel fiber pullout and reinforcement yielding, while crack widths continue to grow. Despite this, the pipe shows good overall toughness. These results indicate that the simulation and statistical methods can accurately predict the load-bearing behavior and deformation of fiber-reinforced concrete pipes.
4.4. Failure Modes of the Pipeline
Based on the comparison of simulation and experimental results, the pipeline failure process can be divided into four stages: elastic deformation under initial loading, stable crack propagation with multiple small cracks, unstable development with the formation of the main crack, and structural failure marked by a drop in load-bearing capacity. Using the numerical simulation results as the analysis sample, the mechanical response of key sections is examined in these four stages through stress distribution contour maps.
When the simulated load increased until the vertical displacement at the pipe crown reached 5.5 mm, the stress contour of the pipe is shown in Figure 15a. The results indicate that at a concentrated load of 232 kN/m, the tensile stress at the inner wall of the crown reached 6.4 MPa, matching the axial tensile strength of UHPC. At this stage, the crown and invert showed compressive stress on the outer side and tensile stress on the inner side. The pipe was at the transition between elastic deformation and stable crack propagation, with the crown gradually entering an inelastic state. Steel fibers began to bridge cracks and redistribute stress, causing the damaged area on the outer walls to expand. This agrees with the experimental observations, where crack widths increased little but the number of cracks grew. As a result, the pipe exhibited a “multi-point cracking” failure mode, as shown in Figure 15b.
Figure 15.
Stress contours of the pipe at different failure stages. (a) Stress contour of the pipe during the elastic deformation stage. (b) Stress contour of the pipe in the crack propagation stage. (c) Stress contour of the pipe when the inner reinforcement reaches its ultimate tensile strength. (d) Stress contour of the pipe in the structural failure stage.
When the load reached 423.54 kN/m, the stress in the inner reinforcement rose to 540 MPa, matching its ultimate tensile strength, as shown in Figure 15c. Compared with pipe P1’s failure load of 437 kN/m from the external test, the relative error was only 3.08%. Figure 15d shows the pipe’s failure pattern at the end of the simulation. The concrete in the compressive zone exhibited large plastic strains, indicating that after cracking in the tensile zone, the circumferential reinforcement reached its ultimate strain. The pipe reached its maximum load-carrying capacity and displayed a typical ductile flexural failure. This failure mode agrees well with the final behavior observed in the external load tests.
4.5. Effect of Circumferential Reinforcement Spacing on the Bearing Capacity of UHPC Pipe Jacking Pipes
Reinforcement in pipes acts as the main load-resisting skeleton, and the spacing of circumferential reinforcement significantly affects pipe performance, including cracking and ultimate strength. Assuming other parameters—such as pipe inner diameter, steel fiber content, and internal water pressure—remain constant, the influence of circumferential reinforcement spacing on mechanical behavior was investigated. Using pipe P1 as an example, the total reinforcement area is 3746 mm2. Based on this, five UHPC pipe jacking models with different circumferential reinforcement spacings were developed for finite element analysis. All models have an inner diameter of 2500 mm, a length of 2500 mm, and a wall thickness of 180 mm. Detailed parameters are given in Table 5.
Table 5.
Parameters of UHPC pipe jacking pipes with different circumferential reinforcement spacings.
Figure 16 presents the load–displacement curves from the numerical simulations of models S1–S5. As the spacing of the circumferential reinforcement decreases, the total reinforcement area increases, resulting in higher initial stiffness of the UHPC pipe. The peak load and corresponding displacement also increase. Compared with S1, the peak load and displacement of S2 increase by 48.0% and 11.8%, respectively; S3 increases by 64.0% and 13.3%; S4 increases by 82.8% and 20.1%; and S5 increases by 81.7% and 22.8%.
Figure 16.
Load–displacement curves of pipes S1–S5.
Since this study did not include comparative tests with conventional concrete pipes, pipes with similar specifications in the national standard were selected for comparison. According to GB/T 11836-2023, Concrete and Reinforced Concrete Drainage Pipes [30], when the concrete strength grade is C50, the inner diameter is 2600 mm, and the wall thickness is 245 mm, the cracking load and failure load of reinforced concrete pipes are 228 kN/m and 342 kN/m, respectively. In this study, the S1 model has a reinforcement ratio of 0.6% and a wall thickness of 180 mm. Its cracking load and failure load are 232 kN/m and 367 kN/m, respectively. Both values are higher than those required by the national standard. The wall thickness of S1 is reduced by about 26.5%. Even so, the specimen still shows better crack resistance and higher ultimate bearing capacity. This result highlights the advantages of UHPC. It can improve structural capacity, reduce wall thickness, and save materials. Considering engineering practice and the excellent mechanical properties of UHPC, a reinforcement ratio of about 1.4% is recommended for UHPC pipes.
5. Conclusions
This study conducted bearing tests and numerical simulations to systematically investigate the mechanical behavior of UHPC pipe jacking structures with an inner diameter of 2.5 m and wall thicknesses of 180 mm (P1) and 200 mm (P2). The pipes featured double-layer circumferential reinforcement, with the outer layer arranged as 10@120 mm and the inner layer as 10@100 mm. The concrete cover thicknesses were 30 mm on the outer side and 25 mm on the inner side. The pipes were cast with C150-grade UHPC and reinforced with HRB400 steel. The main conclusions are summarized as follows:
- The results of the three-edge load tests showed that the maximum displacements of pipes P1 and P2 were 42.3 mm and 24.5 mm, respectively. The cracking loads were 220 kN/m and 336 kN/m, while the ultimate loads were 437 kN/m and 462 kN/m, respectively. The deformation and failure evolution of the UHPC pipes under radial loading was clarified, and the failure process could be divided into four stages: elastic deformation, crack development, reinforcement yielding, and structural failure.
- By simplifying the three-edge load into an equivalent plate load, a bearing capacity calculation model for UHPC pipes was established. The tensile strength of UHPC in the tensile zone and the corresponding failure mode were taken into account, and analytical expressions for the cracking load and ultimate load were derived. The calculated results showed good agreement with the experimental data, indicating that the proposed model is reliable and applicable for engineering analysis.
- A finite element model of the UHPC pipe was developed using ABAQUS, through which the load–displacement and load–crack width relationships were obtained. The simulated cracking and failure patterns were consistent with the experimental observations. Furthermore, numerical analyses were performed for pipes with five different reinforcement ratios, and the results indicated that the optimal reinforcement ratio for UHPC pipes is approximately 1.4%. The model validation demonstrates that the finite element approach can reasonably predict the macroscopic failure process and bearing performance of UHPC pipes.
- This study performed the first full-scale tests on UHPC pipe jacking systems. A bearing capacity model considering the plastic hinge mechanism was proposed. A finite element method was developed to reproduce the full failure process. Results show that wall thickness and reinforcement layout can improve structural safety and durability. This work provides guidance for pipe design optimization. Future studies can explore the effects of fiber type and hybrid mixes on crack control and impact resistance. The long-term durability of UHPC pipes under complex soils and extended service should also be investigated.
Author Contributions
Conceptualization, P.Z.; methodology, S.K.; software, Y.L.; validation, S.Y.; formal analysis, R.T.; investigation, L.H.; resources, S.K.; data curation, R.T.; writing—original draft preparation, S.M.; writing—review and editing, P.Z.; visualization, S.M.; supervision, Y.L.; project administration, S.Y.; funding acquisition, L.H. All authors have read and agreed to the published version of the manuscript.
Funding
This research was supported by the Research Project on Technological Innovation and Techno-economic Improvement of Power Transmission and Transformation Projects under the New Power System (Project No.: 5477GC25F030).
Data Availability Statement
Some or all data, models, or codes that support the findings of this study are available from the corresponding author upon reasonable request.
Conflicts of Interest
The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.
References
- Chen, X.; Mu, R.; Liu, X. Research progress on the preparation and mechanical properties of ultra-high-performance concrete. Bull. Chin. Ceram. 2024, 43, 4295–4312. [Google Scholar] [CrossRef]
- Chen, M.; Feng, J.; Zhang, T. Dynamic splitting tensile properties of ultra-high-performance concrete after exposure to high temperature. J. Build. Mater. 2025, 28, 118–126. [Google Scholar]
- Yan, X.; Yu, C.; Zhai, S. Experimental study on the mechanical performance of segment joints in prefabricated assembled utility tunnels. Sichuan Build. Sci. Res. 2017, 43, 28–31. [Google Scholar]
- Abu-Lebdeh, T.; Hamoush, S.; Heard, W.; Zornig, B. Effect of matrix strength on pullout behavior of steel fiber reinforced very-high strength concrete composites. Constr. Build. Mater. 2011, 25, 39–46. [Google Scholar] [CrossRef] [Scilit]
- Ryu, G.S.; Kang, S.T.; Park, J.J.; Koh, K.T.; Kim, S.W. Mechanical Behavior of UHPC (Ultra High Performance Concrete) According to Hybrid Use of Steel Fibers. Adv. Mater. Res. 2011, 287–290, 453–457. [Google Scholar] [CrossRef] [Scilit]
- Nguyen, D.L.; Dong, J.K.; Ryu, G.S.; Koh, K.T. Size effect on flexural behavior of ultra-high-performance hybrid fiber-reinforced concrete. Compos. Part B 2013, 45, 1104–1116. [Google Scholar] [CrossRef] [Scilit]
- Du, J.; Meng, W.N.; Khayat, K.H.; Bao, Y.; Guo, P.; Lyu, Z.; Abu-obeidah, A.; Nassif, H.; Wang, H. New development of ultra-high-performance concrete (UHPC). Compos. Part B-Eng. 2021, 224, 576–590. [Google Scholar] [CrossRef] [Scilit]
- Yu, R.; Song, Q.L.; Wang, X.P.; Zhang, Z.; Shui, Z.; Brouwers, H.J.H. Sustainable development of Ultra-High Performance Fibre Reinforced Concrete (UHPFRC): Towards to an optimized concrete matrix and efficient fibre application. J. Clean. Prod. 2017, 162, 220–233. [Google Scholar] [CrossRef] [Scilit]
- Su, Y.; Wu, C.Q.; Li, J.; Li, Z.-X.; Li, W. Development of novel ultra-high performance concrete: From material to structure. Constr. Build. Mater. 2017, 135, 517–528. [Google Scholar] [CrossRef] [Scilit]
- Yoo, D.Y.; Lee, J.H.; Yoon, Y.S. Effect of fiber content on mechanical and fracture properties of ultra high performance fiber reinforced cementitious composites. Compos. Struct. 2013, 106, 742–753. [Google Scholar] [CrossRef] [Scilit]
- Ji, X.S.; Jiang, Y.; Gao, X.J.; Sun, M. Synergistic effect of microfibers and oriented steel fibers on mechanical properties of UHPC. J. Build. Eng. 2024, 91, 16–23. [Google Scholar] [CrossRef] [Scilit]
- Rong, Z.D.; Sun, W. Experimental and numerical investigation on the dynamic tensile behavior of ultra-high performance cement based composites. Constr. Build. Mater. 2012, 31, 168–173. [Google Scholar] [CrossRef] [Scilit]
- Khosravani, M.R.; Silani, M.; Weinberg, K. Fracture studies of Ultra-High Performance Concrete using dynamic Brazilian tests. Theor. Appl. Fract. Mech. 2018, 93, 302–310. [Google Scholar] [CrossRef] [Scilit]
- Yazici, H.; Yardımci, M.Y.; Aydın, S.; Karabulut, A.Ş. Mechanical properties of reactive powder concrete containing mineral admixtures under different curing regimes. Constr. Build. Mater. 2009, 23, 1223–1231. [Google Scholar] [CrossRef] [Scilit]
- Turker, K.; Hasgul, U.; Birol, T.; Yavas, A.; Yazici, H. Hybrid fiber use on flexural behavior of ultra high performance fiber reinforced concrete beams. Compos. Struct. 2019, 229, 111400.1–111400.15. [Google Scholar] [CrossRef] [Scilit]
- Liu, L. Study on the Performance and Structural Analysis of Ultra-High-Performance Concrete Composite Pipes. Doctoral Dissertation, Wuhan University of Technology, Wuhan, China, 2018. [Google Scholar]
- Jungwirth, J.; Seidl, G.; Schmitt, V. Utilization of UHPC in Composite Structures-lightweight Composite Structure (LCS). In Proceedings of the the Second International Symposium on Ultra High Performance Concrete, Kassel, Germany, 5–7 March 2008; pp. 887–894. [Google Scholar]
- Yang, Y.; Chen, R.; Huang, Q. Optimization design and life-cycle cost analysis of UHPC utility tunnels. J. Ningxia Univ. (Nat. Sci. Ed.) 2018, 39, 227–233. [Google Scholar]
- Zhang, X. Theoretical and Numerical Study on the Three-Edge Bearing Capacity of Prestressed Concrete CylinderPipe. KSCE J. Civ. Eng. 2022, 26, 1254–1266. [Google Scholar] [CrossRef] [Scilit]
- Cao, X.; Ren, Y.-C.; Qian, K.; Fu, F.; Deng, X.-F.; Zhang, W.-J. Size effect on flexural behavior of ultra-high-performance concrete beams with different reinforcement. Structures 2022, 41, 969–981. [Google Scholar] [CrossRef] [Scilit]
- Park, Y.; Abolmaali, A.; Mohammadagha, M.; Lee, S. Structural performance of dry-cast rubberized concrete pipes with steel and synthetic fibers. Constr. Build. Mater. 2015, 77, 218–226. [Google Scholar] [CrossRef] [Scilit]
- Chen, B. Experimental Study on the Mechanical Behavior and Key Design Parameters of Reinforced Segments for Prefabricated Urban Drainage Arch Culverts. Doctoral Dissertation, Changsha University of Science & Technology, Changsha, China, 2022. [Google Scholar]
- Becerril García, D.; Moore, I.D. Evaluation and application of the flexural rigidity of a reinforced concrete pipe. J. Pipeline Syst. Eng. Pract. 2016, 7, 04015015. [Google Scholar] [CrossRef] [Scilit]
- Liao, J.; Lin, X.-C.; Zhu, D.-H.; Zheng, Y.; Zeng, J.-J.; Ma, C.-L.; Zhao, H.-C. Behavior of FRP grid-reinforced ultra-high performance concrete (UHPC) pipes under lateral compression. Case Stud. Constr. Mater. 2023, 19, e02189. [Google Scholar] [CrossRef] [Scilit]
- Fan, T.-H.; Zeng, J.-J.; Hu, X.; Chen, J.-D.; Wu, P.-P.; Liu, H.-T.; Zhuge, Y. Flexural fatigue behavior of FRP-reinforced UHPC tubular beams. Eng. Struct. 2025, 330, 119848. [Google Scholar] [CrossRef] [Scilit]
- GB/T 16752-2017; Test Methods of Concrete and Reinforced Concrete Sewer Pipes. National Technical Committee on Cement Products of Standardization Administration of China, Standards Press of China: Beijing, China, 2017.
- Zhu, Z. Theoretical and Experimental Study on the Mechanical Behavior of Drainage Pipes Rehabilitated by Cement Mortar Spraying. Doctoral Dissertation, China University of Geosciences, Wuhan, China, 2024. [Google Scholar] [CrossRef]
- Yang, J.; Fang, Z. Study on the uniaxial compressive stress-strain relationship of ultra-high-performance concrete. Concrete 2008, 7, 11–15. [Google Scholar]
- Zhang, Z.; Shao, X.; Li, W.; Zhu, P.; Chen, H. Experimental study on the axial tensile behavior of ultra-high-performance concrete. China J. Highw. Transp. 2015, 28, 50–58. [Google Scholar] [CrossRef]
- GB/T 11836—2023; Concrete and Reinforced Concrete Drainage Pipes. Ministry of Housing and Urban-Rural Development of the People’s Republic of China, China Architecture & Building Press: Beijing, China, 2023.
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.