24 November 2026

30 Pages

Moisture-Dependent Bond–Slip Behavior of Foamed Polyurethane–Silt Interfaces

,
,
,
,
and
1
School of Intelligent Construction and Civil Engineering, Luoyang Institute of Science and Technology, Luoyang 471023, China
2
Henan Province Engineering Technology Research Center of Tunnel Construction and Disaster Control, Luoyang 471023, China
3
Henan Province Technology Innovation Center of Traffic Transportation Industry, Luoyang 471023, China
4
School of Intelligent Manufacturing, Luoyang Institute of Science and Technology, Luoyang 471023, China

Abstract

Foamed polyurethane grouting is widely used for rapid foundation repair, but moisture-dependent load transfer across polymer–soil interfaces remains insufficiently understood. This study investigated interfaces between foamed polyurethane and a specific silt collected from Zhengzhou, China, at water contents of 10%, 14%, and 16% under normal stresses of 100, 200, and 300 kPa. The curve-model analyses used mean experimental curves obtained from three replicate direct shear tests per condition, with 27 specimens tested in total. Peak and finite-displacement strength envelopes, inverse bond–slip identification, interpolation-based prediction, and SEM/MIP characterization were combined. Increasing water content reduced the peak strength, mobilization stiffness, shear-work index, and finite-displacement resistance. The apparent interface cohesion decreased from 270.32 to 129.30 kPa as the water content increased from 10% to 16%, whereas the interface friction angle varied non-monotonically between 26.02° and 27.37°. The selected empirical power–polynomial relation fitted the mean experimental curves over the investigated displacement range with a mean R2 of 0.9745. Within the same experimental dataset, the mean R2 values for held-out-condition interpolation in the water-content and normal-stress directions were 0.904 and 0.800, respectively. MIP results showed that the proportion of pore throats larger than 1 μm decreased from 53.85% to approximately 32%, while the fraction of 5–50 nm pore throats increased from 9.23% to 52.56%. The combined observations suggest a tentative two-stage interpretation involving reduced polymer penetration and anchorage, with an additional contribution from water-related weakening of the soil and interfacial contact at higher water content. The proposed reduction and reserve indices characterize relative changes in the tested interface response; their relevance to foundation repair requires further validation of the complete foundation–polyurethane–soil system.

1. Introduction

Settlement, subsurface voids, leakage, and local loss of support can impair the serviceability of existing buildings and underground infrastructure. Conventional excavation-based repair is often disruptive and time-consuming. Foamed polyurethane grouting provides a rapid alternative. The material expands after injection, cures within a short period, and develops sufficient mechanical strength at a relatively low density. Saleh et al. [1] reviewed the use of polyurethane grouts for weak-soil improvement and summarized their rapid curing and expansion characteristics. Liu et al. [2] showed that the mechanical response of rigid polyurethane grout was strongly dependent on its density. Foamed polyurethane grouting has also been applied to infrastructure repair. Guo et al. [3] reported the rapid treatment of voids beneath airport concrete pavement. Fang et al. [4] evaluated the response of drainage pipelines before and after trenchless polymer grouting. Wang et al. [5] subsequently conducted full-scale tests on buried drainage pipes under impact and moving loads. Li et al. [6] combined field testing and numerical analysis to examine polymer grouting around voided and corroded concrete pipes. These studies demonstrate the practical value of polyurethane grouting. However, repair performance depends not only on the strength of the cured polymer but also on load transfer across the newly formed polymer–soil interface.
The behavior of soil–structure interfaces has been studied for several decades. Potyondy [7] showed that interface friction depends on soil type, surface finish, moisture content, and the contacting construction material. Uesugi and Kishida [8] demonstrated that surface roughness and particle characteristics control the frictional resistance of sand–steel interfaces. Dove and Frost [9] further showed that sliding and particle ploughing jointly govern the peak resistance of relatively smooth particle–solid interfaces. Hu and Pu [10] developed a constitutive description that reproduced hardening, softening, and dilation during interface shear. Lam et al. [11] found that the contact condition created by support fluids could alter concrete–sand interface behavior. These findings show that interface resistance is a coupled response. It cannot be treated as an intrinsic property of the soil or solid material alone.
Water content is particularly important for interfaces involving fine-grained soils. Li et al. [12] investigated silt–cement mortar interfaces and found that water content and surface roughness affected both the shear strength and the shape of the stress–displacement curve. Murali et al. [13] compared clay–epoxy interfaces prepared on the dry side, at the optimum water content, and on the wet side of the Proctor curve. Their results showed that the compaction state affected adhesion and pre-peak mobilization. Pan et al. [14] separated concrete–silty clay interface resistance into adhesion and ploughing components. They found that moisture mainly reduced the adhesion-related contribution. These effects are also linked to the hydraulic state of unsaturated soil. Fredlund et al. [15] established that matric suction can contribute to the shear strength of unsaturated soils. Therefore, a change in water content may alter interface resistance through several mechanisms. These include changes in suction, soil stiffness, water-film continuity, particle rearrangement, and solid–solid contact.
Recent studies have extended interface research to polyurethane-based grouting materials. Li et al. [16] conducted direct shear tests on polymer–bentonite interfaces. They found that interface strength increased with normal stress and polymer density but decreased with soil water content. Li et al. [17] later used digital image correlation to examine moisture-dependent deformation and failure in bentonite–polymer composite specimens. Li et al. [18] further investigated the influence of loading direction through variable-angle shear tests and finite-element simulations. Li et al. [19] used ring-shear tests to study the static and dynamic response of polymer-silty clay interfaces. These studies confirmed that moisture, confinement, polymer properties, and loading conditions affect interface resistance. Related research has also examined polymer reinforcement within soil. Wang et al. [20] showed that permeable polyurethane penetration changed the microstructure and mechanical behavior of treated silt. Wang et al. [21] examined polymer-grouted concrete–soil interfaces and related their bond characteristics to the interface morphology and failure pattern.
Studies on polyurethane–concrete interfaces provide additional information on the load-transfer mechanism. Fang et al. [22] combined direct shear tests with SEM observations and showed that the morphology of the polymer–concrete transition zone affected interface bonding. Qin et al. [23] examined the effects of surface conditions on the shear bond performance of non-water-reactive polyurethane and concrete. Wang et al. [24] studied monotonic, cyclic, and post-cyclic interface responses. Their results showed that peak strength alone does not fully represent the evolution of interface resistance. At a smaller scale, Zhang et al. [25] used molecular dynamics simulations to investigate the shear interaction between polymer and bentonite. These studies indicate that polyurethane interface resistance develops at several scales. It includes molecular interaction, physical adhesion, local penetration, mechanical embedment, and macroscopic friction.
A continuous interface relation is required when the complete load-transfer process is considered. Early interface elements represented discontinuities through relative displacement and traction relations. Goodman et al. [26] introduced an interface element for the mechanical analysis of jointed materials. Desai et al. [27] later proposed a thin-layer element for interfaces and joints. These approaches established the importance of a suitable constitutive relation for numerical analysis. However, conventional soil–structure or rock-joint models cannot be transferred directly to an expanding polyurethane–silt interface. The latter contains a heterogeneous transition region. It may include foam cells, soil particles, penetration branches, local voids, and irregular contact zones.
Despite the progress described above, several issues remain unresolved. First, most polyurethane–soil studies emphasize peak shear strength, friction parameters, or failure modes. These quantities are important, but they do not fully describe interface load transfer. Pre-peak mobilization, peak displacement, post-peak softening, and the resistance retained at a finite displacement are also relevant. They become particularly important when local sliding or progressive debonding occurs.
Second, a model that reproduces an individual curve does not necessarily predict an untested condition. Model evaluation should therefore distinguish fitting accuracy from predictive performance. Numerical convergence should also be distinguished from parameter identifiability. Repeated optimization may converge to the same solution, while one parameter remains weakly constrained by the test curve. These issues are especially important for the post-peak branch.
Third, the connection between microscopic observations and macroscopic interface parameters remains incomplete. SEM can reveal interfacial tortuosity and localized penetration paths. MIP can describe changes in mercury-accessible pore throats. However, these observations are often discussed separately from apparent cohesion, stiffness, shear work, and finite-displacement resistance. A combined analysis is needed to determine how moisture changes penetration, anchorage, soil condition, and frictional resistance.
For foundation repair, the response of the foundation–polyurethane–soil system depends on the behavior of its constituent materials and their contacts. The polyurethane–soil interface is one component of this system. The present study isolates its shear response under prescribed normal stresses; it does not examine the foundation–polyurethane contact or the coupled deformation and load redistribution of the complete system. Foundation repair therefore provides the application context, while the experimental scope remains at the polyurethane–soil interface level. The resulting relationships and comparison indices cannot, by themselves, determine the bearing capacity, settlement, or governing failure mode of a repaired foundation.
Accordingly, the present study investigates foamed polyurethane–silt interfaces at water contents of 10%, 14%, and 16% under normal stresses of 100, 200, and 300 kPa. The study has six objectives: (1) to quantify the effects of water content and normal stress on the complete shear stress–displacement response; (2) to separate the moisture dependence of apparent cohesion from that of the normal-stress-dependent frictional component; (3) to compare empirical finite-displacement bond–slip relations and fit their shape parameters to the mean experimental curves through a global–local optimization procedure; (4) to assess within-range interpolation performance in the water-content and normal-stress directions; (5) to relate the mechanical response to SEM morphology and MIP pore-throat distributions; and (6) to define moisture-reduction and finite-displacement reserve indices for comparing the tested interface responses and to discuss their potential relevance and limitations for foundation repair. The study integrates strength envelopes, complete response curves, inverse identification, interpolation-based prediction, microstructural interpretation, and engineering indices.

2. Experimental Materials and Methods

2.1. Silt and Polyurethane Materials

The soil used in this study was classified as silt and collected from Zhengzhou, Henan Province, China. The particle-size distribution was mainly composed of particles ranging from 0.05 to 0.075 mm. The optimum water content was 14%, and the corresponding maximum dry density was 1.76 g/cm3. The main physical properties of the soil are summarized in Table 1. All geotechnical tests were conducted according to the Chinese standard GB/T 50123-2019 [28].
Table 1. Reported physical properties of the tested silt.
Only one source of silt was investigated. The properties summarized in Table 1 characterize this particular soil and do not establish its representativeness for other silts or soil types. Accordingly, the measured responses and the relationships derived from them are specific to the tested soil–polyurethane combination and specimen preparation conditions; their applicability to other soils requires separate evaluation.
The polymer used in this study was a two-component polyurethane foam that does not react with water. Component A was an isocyanate, whereas Component B consisted of a polyol and selected additives. The two components are shown in Figure 1. During specimen preparation, components A and B were mixed at a ratio of 1:1. The mixture was then injected into the mold under pressure and allowed to expand and cure. Considerable heat was released during the foaming and curing process. Therefore, the mold was allowed to cool at room temperature for 1 h before demolding. The measured density, yield stress, and Young’s modulus of the cured polymer were 0.490 g/cm3, 11.67 MPa, and 291.04 MPa, respectively. These material properties were treated as constant throughout the study.
Figure 1. Non-water-reactive two-component polyurethane foam (Component A was an isocyanate; Component B consisted of a polyol and selected additives).

2.2. Specimen Preparation and Direct Shear Testing

Polymer–silt composite specimens were prepared at target initial gravimetric water contents of 10%, 14%, and 16%. The silt was prepared at a common target dry density of 1.76 g/cm3 before polyurethane injection. For the prescribed compacted-soil dimensions of 100 mm × 100 mm × 50 mm, the mold volume was 500 cm3, corresponding to a target dry-soil mass of 880 g per specimen. Water was added according to the target gravimetric water content. Thus, the preparation procedure controlled both the prescribed dry-soil mass and the molding volume, with initial water content varied between the three groups. The conditioned silt was sealed for 48 h to promote uniform moisture distribution and then compacted in five layers. Before placing each new layer, the surface of the previous layer was scarified to improve interlayer bonding. The same preparation procedure was used for all specimens. After compaction, each silt specimen measured 100 mm × 100 mm × 50 mm. Polyurethane was then injected onto the compacted silt surface and allowed to expand and cure before demolding, producing a composite specimen with a nominally planar polymer–silt interface. The preparation procedure is shown in Figure 2. Nine specimens were prepared for each water-content condition, giving a total of 27 specimens. The reported dry density denotes the common preparation target; specimen-specific as-prepared dry densities and initial void ratios were not independently determined.
Figure 2. Preparation procedure of the polymer–silt interface specimens.
The specimen preparation represents an idealized polymer–soil contact formed through polyurethane expansion and curing against compacted silt, consistent with related laboratory approaches [19,21]. However, the procedure does not reproduce field-scale grout migration, injection-pressure history, three-dimensional confinement, or natural soil fabric. Therefore, the results are interpreted as interface-level responses under the investigated laboratory conditions.
Monotonic direct shear tests were conducted at normal stresses of 100, 200, and 300 kPa for each water-content condition, giving nine test conditions with three replicates per condition. The prescribed normal load was applied before horizontal shearing, which commenced after the normal-load-induced deformation had stabilized. Vertical displacement was recorded during normal loading, while the initial compression magnitude was not treated as a separate response variable in the subsequent analysis. The resulting state was taken as the initial condition for shearing, thereby incorporating the effects of normal loading on specimen compression and interface contact into the measured response.
An adjustable split shear box was used. Before horizontal shearing, the actual polymer–silt interface position was checked, and the relative vertical position of the two box halves was adjusted to align their horizontal division with the interface. Interface positioning was therefore based on the actual interface location rather than the original specimen height.
All tests followed the same loading procedure and used the same closed-box arrangement without active drainage control. Pore-water pressure was not monitored, and the results were interpreted in terms of the overall interface shear response under the prescribed test conditions. Before shearing, the horizontal loading head was advanced by approximately 2–3 mm to take up mechanical clearance without imposing relative shear displacement on the specimen, after which the horizontal displacement reading was zeroed. Horizontal shearing was performed at a constant displacement rate of 1 mm/min, with shear load and horizontal displacement recorded throughout the test. The displacement variable s denotes the horizontal displacement recorded by the direct shear apparatus and is used as the macroscopic shear-displacement measure for the interface tests. No additional local instrumentation was used to measure specimen distortion or local interfacial slip. The analysis therefore uses the measured shear stress–horizontal displacement relationship, without converting the recorded displacement into shear strain. The apparatus and interface-positioning arrangement are shown in Figure 3.
Figure 3. Direct shear test apparatus and test procedure.
For each combination of water content and normal stress, the representative response was obtained by averaging the shear stresses from three replicate tests at corresponding horizontal displacements. The resulting mean stress–displacement data points were used to plot Figure 4. Adjacent mean points were connected by straight lines for visualization, without additional smoothing or fitting during the preparation of the experimental plots. The authors performed the experimental data processing and prepared the mean experimental curves used in the subsequent mechanical analyses.
Figure 4. Mean shear stress–displacement responses of the polyurethane–silt interfaces at water contents of 10%, 14%, and 16% under normal stresses of 100, 200, and 300 kPa. Each curve represents the average of three replicate tests.
The test matrix was used to examine the effects of water content and normal stress on the response of the selected polyurethane–silt system. The resulting representative curves provide the basis for empirical curve fitting and preliminary interpolation within the investigated conditions. With only three water-content levels and three normal-stress levels, the experimental coverage is insufficient to establish a general interface constitutive model or transferable parameter relationships for other materials and loading paths.

2.3. SEM and MIP Characterization

The polymer–silt interface morphology was examined using a KYKY-EM6200 scanning electron microscope(Beijing Zhongke Keyi, Beijing, China) at 200× magnification. Samples measuring approximately 1 cm × 1 cm were cut perpendicular to the interface. The samples were cleaned and coated with an approximately 10-nm-thick conductive metal film. They were then examined under vacuum conditions.
One field of view was selected for each water-content condition. Therefore, the SEM images were used for qualitative and semiquantitative comparisons rather than statistical analysis. The yellow interface traces marked in the original images were digitized. The contour-length ratio, peak-to-valley amplitude, and root-mean-square (RMS) height were then calculated. These parameters describe the morphology of the annotated two-dimensional interface. They do not represent the actual three-dimensional contact area.
For mercury intrusion porosimetry (MIP), selected specimens were vacuum-dried at 60–80 °C. One specimen was tested by MIP for each initial water-content condition, without independent replication. Mercury was then progressively intruded into the specimens under increasing pressure. A mercury–solid contact angle of 140° was adopted. The equivalent pore-throat diameter was calculated using the Washburn equation, as shown in Equation (1) [29].
P = − 4 γ c o s θ / d
where P is the applied mercury intrusion pressure, γ is the surface tension of mercury, θ is the mercury–solid contact angle, and d is the equivalent pore-throat diameter. Because the adopted contact angle was greater than 90°, cosθ was negative, and the calculated intrusion pressure remained positive.
The present analysis adopted three primary pore-throat classes: <5 nm, 5–50 nm, and >50 nm. The larger pore-throat range was further divided into 50–500 nm, 0.5–1 μm, 1–20 μm, and 20–100 μm [30]. The MIP results represent the distribution of mercury-accessible pore throats [31].

3. Results

3.1. Shear Stress–Displacement Response and Characteristic Indices

Figure 4 presents the mean shear stress–displacement responses of the polyurethane–silt interfaces at water contents of 10%, 14%, and 16% under normal stresses of 100, 200, and 300 kPa. Each curve represents the mean response of three replicate tests under the same condition, calculated at corresponding horizontal displacements as described in Section 2.2. Specifically, the stresses of the three replicates were averaged arithmetically at each common recorded displacement from 0 to 5.5 mm, at intervals of 0.025 mm. No peak alignment was applied. For strength-envelope fitting, the peak stress was first extracted from each replicate and the three peak stresses were then averaged within each condition. These means of individual peaks, rather than the peaks of the averaged curves, were used in Section 3.2. The individual peak stresses and their corresponding displacements are listed in Table A1. The curve descriptions below refer to the pointwise mean curves.
The nine curves showed similar overall response patterns. Four main stages were identified: initial shear mobilization, nonlinear hardening, post-peak softening, and finite-displacement resistance. At the beginning of loading, the shear stress increased gradually with shear displacement. The rate of stress mobilization then increased. The shear stress reached a peak at displacements from approximately 2.025 to 3.025 mm. After the peak, the shear stress decreased with increasing displacement. A stable residual plateau was not observed under all test conditions. For a mean curve with a peak plateau, the peak displacement was taken as the first sampled displacement attaining the maximum stress.
Normal stress had a clear effect on the interface response. A higher normal stress produced a higher peak shear stress and increased the shear resistance at large displacement. At a water content of 10%, the peak shear stress increased from 321.00 kPa at 100 kPa normal stress to 363.22 kPa at 200 kPa and 424.00 kPa at 300 kPa. Similar trends were observed at water contents of 14% and 16%.
Water content had the opposite effect. At the same normal stress, the peak shear stress decreased as the water content increased. Under a normal stress of 100 kPa, the peak shear stresses were 321.00, 227.09, and 181.25 kPa at water contents of 10%, 14%, and 16%, respectively. The peak strength decreased by 29.3% when the water content increased from 10% to 14%. It decreased by 43.5% when the water content increased from 10% to 16%.
The peak displacement generally increased with water content. Under a normal stress of 100 kPa, the peak displacement increased from 2.025 mm at a water content of 10% to 2.800 mm at 14% and 3.025 mm at 16%. At 300 kPa normal stress, it increased from 2.200 to 2.500 and 2.850 mm, respectively. This trend indicates that the maximum shear resistance was mobilized at a larger displacement under water conditions.
Several characteristic indices were used to quantify the interface response. The peak shear stress and the corresponding displacement were denoted by τp and sp, respectively. The interface secant stiffness, K20–60, was defined as the increase in shear stress divided by the corresponding increase in recorded horizontal displacement between 20% and 60% of the peak shear stress on the pre-peak branch, as expressed in Equation (2).
K 20 – 60 = 0.6 τ p − 0.2 τ p S 0.6 − S 0.2 = 0.4 τ p S 0.6 − S 0.2
where S0.2 and S0.6 are the recorded horizontal displacements corresponding to 20% and 60% of τp on the pre-peak branch, respectively. The unit of K20–60 is kPa/mm. This parameter characterizes the secant slope of the measured interface response and serves as an index of pre-peak shear mobilization. It is distinct from a material shear modulus, which relates shear stress to shear strain. The 20–60% interval was adopted because the initial portions of some mean experimental curves were not strictly linear. For each specimen, the first pre-peak crossings of 20% and 60% of its own peak stress were obtained by linear interpolation between adjacent recorded points.
A displacement of 5.5 mm was selected as the common endpoint for all curves. The shear stress at this displacement was denoted by τ5.5 and was used to evaluate the finite-displacement resistance of the interface. The parameter τ5.5 should not be regarded as a strict residual shear strength because a stable residual stage was not reached in every test.
The accumulated shear-work index up to a displacement of 5.5 mm was calculated as shown in Equation (3).
G 0 – 5.5 = ∫ 0 5.5 τ ( s ) d s
where s is the recorded horizontal displacement defined in Section 2.2 and τ(s) is the corresponding interface shear stress. The unit of G0–5.5 is kPa·mm, which is numerically equivalent to J/m2. This index represents the total shear resistance mobilized within the investigated displacement range.
Three independent replicate tests were performed under each testing condition (n = 3), and Figure 4 presents the mean experimental curves. To quantify between-specimen variability, the peak shear stress, displacement at peak shear stress, shear stress at 5.5 mm displacement, secant stiffness, and shear-work index were calculated separately for each replicate. For each index, the coefficient of variation (CV) was calculated within each testing condition as the sample standard deviation divided by the corresponding mean, multiplied by 100%. Across the nine testing conditions, the CVs ranged from 4.13% to 4.41% for peak shear stress, 4.94% to 5.59% for displacement at peak shear stress, 6.07% to 6.51% for shear stress at 5.5 mm displacement, 7.58% to 8.82% for secant stiffness, and 4.36% to 4.69% for the shear-work index. All experimental result curves are presented in Appendix A.
The common-displacement resistance also decreased with increasing water content. Under a normal stress of 100 kPa, τ5.5 decreased from 183.75 kPa at a water content of 10% to 131.25 kPa at 14% and 71.25 kPa at 16%. The corresponding reductions were 28.6% and 61.2%. Under 200 kPa normal stress, τ5.5 decreased from 272.41 to 216.09 and 158.62 kPa. Under 300 kPa normal stress, it decreased from 321.14 to 237.71 and 161.14 kPa.
The decrease in τ5.5 was generally greater than the decrease in τp, especially at a water content of 16%. This result indicates that moisture had a strong influence on the post-peak response. The interface retained less shear resistance after peak failure under wetter conditions.
The stiffness and shear-work indices showed similar trends. The mean K20–60 decreased by approximately 51.9% when the water content increased from 10% to 14%. The mean G0–5.5 decreased by approximately 32.3% over the same range. Both indices decreased further at a water content of 16%. Therefore, increasing water content reduced the peak shear strength, increased the displacement required to mobilize the peak resistance, weakened the pre-peak stiffness, and reduced the finite-displacement resistance of the interface. Here, mean stiffness and shear work were obtained by averaging the nine individual specimen values at each water content, with equal representation of the three normal-stress levels.

3.2. Peak and Finite-Displacement Strength Characteristics

The peak shear strength increased with normal stress under all water-content conditions. The peak strength envelope was described using the Mohr–Coulomb criterion, as shown in Equation (4). At each water content, the three means of individual specimen peaks at normal stresses of 100, 200, and 300 kPa were fitted by ordinary least squares with an intercept and equal weight for each mean.
τ p = c p + σ n t a n δ p
where τp is the mean of the three independently extracted specimen peak shear stresses at a given testing condition, cp is the apparent interface cohesion, σn is the applied normal stress, and δp is the peak interface friction angle. The parameters τp, cp, and σn are expressed in kPa. The parameter δp is expressed in degrees. The reported R2 values refer to these three group means.
The fitted intercept cp and slope tan δp are apparent parameters of the peak-strength envelope over the investigated normal-stress range. Although cp may reflect combined contributions from adhesion, mechanical interlocking, and the unsaturated state of the silt, these contributions were not independently quantified. In particular, cp is the intercept obtained by extending the fitted line to zero normal stress, rather than a directly measured zero-normal-stress bond strength. Likewise, δp describes the normal-stress dependence of the fitted peak resistance and should not be interpreted as an independently measured friction angle of the polymer–soil contact.
A similar linear relation was used to describe the interface strength at a common shear displacement of 5.5 mm, as shown in Equation (5).
τ 5.5 = c 5.5 + σ n μ 5.5
where τ5.5 is the mean interface shear stress of the three replicates at a displacement of 5.5 mm, c5.5 is the intercept of the finite-displacement strength envelope, and μ5.5 is its slope. The parameters τ5.5 and c5.5 are expressed in kPa. The parameter μ5.5 is dimensionless. The parameters c5.5 and μ5.5 are used only to compare the interface resistance at the specified displacement. They should not be interpreted as residual cohesion or a residual friction coefficient.
The fitting results are presented in Table 2 and Figure 5. The peak shear strength showed a strong linear relationship with normal stress. The coefficients of determination ranged from 0.9866 to 0.9997. This result indicates that Equation (4) provided a suitable description of the peak strength within the tested normal-stress range of 100–300 kPa. The peak stresses are means of the three individual specimen peaks; error bars show sample standard deviations.
Table 2. Peak and finite-displacement strength-envelope parameters.
Figure 5. Test result curves. (a) Peak-strength envelopes. (b) Moisture dependence of the peak envelope parameters.
The apparent interface cohesion decreased markedly with increasing water content. The value of cp decreased from 270.32 kPa at a water content of 10% to 181.73 kPa at 14%. It further decreased to 129.30 kPa at 16%. These values correspond to reductions of 32.8% and 52.2%, respectively, relative to the 10% condition. The normal-stress-dependent component changed much less. The values of tanδp were 0.5087, 0.4882, and 0.5176 at water contents of 10%, 14%, and 16%, respectively. The corresponding interface friction angles were 26.96°, 26.02°, and 27.37°, showing a small, non-monotonic variation. The small differences in the fitted friction angle are reported as descriptive differences between point estimates. Their statistical significance has not been established; therefore, these differences alone are not taken as evidence of a change in the interfacial friction mechanism.
These results show that the moisture-induced reduction in peak strength was mainly associated with the intercept of the strength envelope, whereas the slope remained relatively stable. Within the fitted linear representation, the change in peak resistance was expressed mainly through a reduction in the intercept rather than the slope. This pattern is consistent with a moisture-sensitive apparent bonding contribution, but does not independently separate bonding, suction, interlocking, and frictional mechanisms.
The differences between the fitted peak strengths and the means of the individual specimen peak stresses ranged from approximately −1.06% to 1.88%. The small differences support the use of a linear peak strength envelope within the investigated stress range.
Because only three normal-stress levels (100, 200, and 300 kPa) were investigated, the available data are insufficient to reliably establish a nonlinear strength envelope. Although nonlinear shear-strength criteria, such as that proposed by Barton and Choubey [32] for rough rock joints, have been developed, their applicability to the present polyurethane–silt interface remains uncertain. Therefore, the linear Mohr–Coulomb criterion was retained as an empirical description of the peak interface shear strength within the tested normal-stress range. Further experimental validation is required before extending its applicability beyond this range.
The finite-displacement strength also increased with normal stress. However, its relationship with normal stress was less consistent than that of the peak strength. At a water content of 10%, c5.5 and μ5.5 were 121.71 kPa and 0.6870, respectively. The coefficient of determination was 0.9726. Thus, the linear envelope provided a good description of the finite-displacement strength under this condition.
At a water content of 14%, c5.5 decreased to 88.55 kPa. The value of μ5.5 decreased to 0.5323. The corresponding coefficient of determination was 0.8948. At a water content of 16%, c5.5 further decreased to 40.44 kPa, while μ5.5 decreased to 0.4495. The coefficient of determination decreased to 0.7710. Relative to the 10% condition, c5.5 decreased by 27.2% at a water content of 14% and by 66.8% at 16%. The corresponding reductions in μ5.5 were 22.5% and 34.6%. Therefore, both the intercept and slope of the finite-displacement envelope were sensitive to water content. The reduction in the coefficient of determination also indicates greater variation in the post-peak response. This variation was most evident at a water content of 16%. The peak strength remained approximately linear with normal stress, but the resistance at 5.5 mm showed a more complex dependence on normal stress. This difference may be related to variations in post-peak softening and interface damage.
Overall, increasing water content changed the peak and finite-displacement strength envelopes in different ways. For the peak strength, the main change occurred in cp, while tanδp remained relatively stable. For the finite-displacement strength, both c5.5 and μ5.5 decreased. This result shows that moisture reduced not only the maximum interface resistance but also the resistance retained after substantial interface displacement.

3.3. Bond–Slip Modeling and Inverse Identification

Three empirical finite-displacement bond–slip relations—the bilinear, power–polynomial, and power–exponential models were evaluated to describe the mean experimental shear stress–displacement curves. Their purpose was to provide compact descriptions of the responses within the investigated displacement range, rather than to establish a general interface constitutive law. All three models were constrained by the origin, the peak point (sp, τp), and the common endpoint (se, τe), with se = 5.5 mm and τe = τ5.5. These characteristic values were extracted from the mean experimental curves. Consequently, agreement at the peak and endpoint follows from the imposed constraints and does not constitute independent validation; the fitting assessment concerns the representation of the intervening curve shapes. In Section 3.3 and Section 3.4, τp and sp denote the peak stress and peak displacement of the pointwise mean curve used for model calibration; τp here is distinct from the mean individual peak stress used for strength-envelope fitting in Section 3.2.
The coefficient of determination (R2), root-mean-square error (RMSE), mean absolute error (MAE), and Akaike information criterion (AIC) were used to evaluate the fitting performance. A higher R2 indicates better agreement between the mean experimental curves and the fitted model curves. Lower RMSE, MAE, and AIC values indicate better model performance [33].
The power–polynomial model used separate functions for the pre-peak and post-peak branches. The pre-peak response was expressed as shown in Equation (6).
τ = τ p ( s s p ) m ,   0   ≤   s   ≤   s p
where τ(s) is the interface shear stress at displacement s, τp is the peak shear stress, and sp is the corresponding peak displacement. The parameter m is a dimensionless shape parameter. It controls the pre-peak stress mobilization. A larger value of m produces slower stress mobilization at small displacements.
The post-peak response was expressed as shown in Equation (7).
τ = τ e + ( τ p − τ e ) 1 − s − s p s e − s p n ,   s p <   s   ≤   s e
where se is the endpoint displacement and τe is the shear stress at se. The parameter n is a dimensionless post-peak shape parameter. A larger value of n produces a more rapid stress decrease immediately after the peak.
The formulation distinguishes characteristic response quantities from fitted shape coefficients. The peak stress τp, peak displacement sp, and endpoint stress τe were extracted from each mean experimental curve, whereas se = 5.5 mm was selected as a common comparison displacement rather than a material-specific failure displacement. Only the dimensionless coefficients m and n were estimated by numerical fitting. For fixed characteristic points, m controls the pre-peak stress mobilization, while n controls the distribution of stress reduction along the post-peak branch. These coefficients describe curve shape; they are not independently measured material constants, shear moduli, or damage variables. Accordingly, inverse identification in this study refers to fitting these two coefficients to a prescribed representative response, rather than identifying an underlying physical constitutive mechanism.
A global–local optimization procedure was used. Differential evolution was first used for the global search. The parameter bounds were set as follows [34]:
0.2 ≤ m ≤ 8.0 ,   0.2 ≤ n ≤ 8.0
The global-search solution was then refined using a bounded nonlinear least-squares algorithm. This procedure reduced the influence of the initial parameter values.
The pre-peak and post-peak branches contained different numbers of data points. Therefore, direct minimization of the total squared error would assign a larger weight to the branch with more points. To avoid this effect, equal aggregate weights were assigned to the two branches. The residuals were also normalized by the peak shear stress. The objective function was defined as shown in Equation (8) [35].
J = 0.5 M S E p r e , n o r m + 0.5 M S E p o s t , n o r m
where J is the total objective value. The terms MSEpre,norm and MSEpost,norm are the mean squared normalized residuals for the pre-peak and post-peak branches, respectively. Each normalized residual was calculated as the difference between the fitted stresses and the corresponding mean experimental stresses divided by τp. The weighting coefficients ensured that the two branches made equal contributions to the objective function.
Each curve was independently inverted 30 times. Different predefined random seeds were used. The parameter set with the lowest objective value was selected as the final solution. The mean, standard deviation, and coefficient of variation in the identified parameters were used to assess numerical stability.
Objective-profile analysis was also performed. One parameter was varied while the other parameter was fixed at its optimum value. A 1% objective-profile interval was then determined. This interval included all parameter values that increased the minimum objective value by no more than 1%. A narrow interval indicates high numerical sensitivity. A wide interval indicates weak parameter identifiability.
The overall model comparison is presented in Table 3 and Figure 6. The bilinear model showed the lowest fitting accuracy. Its mean R2 was 0.8422. Its mean RMSE and MAE were 32.94 and 26.02 kPa, respectively. The model could not reproduce both the nonlinear pre-peak response and the curved post-peak response.
Table 3. Overall comparison of the three candidate bond–slip models.
Figure 6. Comparison of the candidate bond–slip models. (a) Mean fitting error. (b) Mean coefficient of determination.
Both nonlinear models provided much better fits. The mean R2 values of the power–polynomial and power–exponential models were 0.9745 and 0.9739, respectively. Their mean RMSE values were 13.16 and 13.31 kPa. The difference between the two nonlinear models was small.
The power–polynomial model produced a slightly lower mean MAE of 9.34 kPa. The corresponding value of the power–exponential model was 9.38 kPa. The power–polynomial model also produced the lowest mean RMSE and the lowest total AIC. It also produced the lowest RMSE in six of the nine test conditions. The power–exponential model performed best in the other three conditions. Based on the overall evaluation, the power–polynomial model was selected for subsequent parameter identification and interpolation analysis.
The final identification results of the power–polynomial model are listed in Table 4. Representative fitted curves are shown in Figure 7. The model reproduced the main features of the shear stress–displacement curves. It captured the peak position, the post-peak reduction, and the stress at 5.5 mm.
Table 4. Final inverse-identification results for the selected power–polynomial model.
Figure 7. Inverse-identification results of the power–polynomial bond–slip model under all nine water-content and normal-stress conditions.
The peak values in this table are extracted from the pointwise mean curves and are used for curve-model calibration. They are not the mean individual peaks used to fit Table 2.
The R2 values ranged from 0.9399 to 0.9935. The RMSE values ranged from 5.73 to 25.85 kPa. The best agreement was obtained for W14-N200 and W16-N200. Their R2 values were 0.9935 and 0.9906, respectively. Their RMSE values were 6.53 and 5.73 kPa.
Larger errors were obtained for W10-N200 and W10-N300. Their RMSE values were 25.85 and 24.98 kPa, respectively. The corresponding R2 values were 0.9519 and 0.9399. These mean experimental curves showed more complex pre-peak shapes. The two-parameter model could not fully reproduce these local variations. However, it still captured the main peak and post-peak characteristics.
The identified value of m ranged from 0.697 to 2.054. The value of n ranged from 0.959 to 4.878. Neither parameter showed a simple monotonic relationship with water content or normal stress. This result indicates that the curve shape was affected by interactions between moisture and normal confinement.
The 30 independent inversion runs yielded nearly identical optimal parameters, indicating numerical stability of the optimization procedure. These runs assess numerical repeatability rather than between-specimen variability.
The objective-profile results showed that the sensitivity of the two shape parameters was different. The relative profile width of m ranged from approximately 2.6% to 7.9% of its optimum value. Thus, the pre-peak parameter was well constrained for all test conditions.
The parameter n was less identifiable in some cases. Its relative profile widths were approximately 38% for W10-N200 and 37% for W10-N300. The post-peak parameter could therefore vary over a wider range without causing a clear increase in the objective value. This weak identifiability was consistent with the larger fitting errors under these two conditions.
Overall, the selected power–polynomial model provided a compact description of the mean experimental curves using two fitted shape parameters, although the post-peak parameter was less well constrained under some test conditions.

3.4. Interpolation-Based Predictive Evaluation

Two held-out-condition interpolation schemes were used to assess the model performance within the investigated water-content and normal-stress ranges. At each fixed normal stress, the results at water contents of 10% and 16% were used to estimate the response at 14%. At each fixed water content, the results at normal stresses of 100 and 300 kPa were used to estimate the response at 200 kPa. The parameters of each target condition were excluded from its interpolation calculation. This assessment provides a limited check of interpolation between tested conditions within the same experimental dataset; it does not constitute external validation using an independent experimental dataset or demonstrate predictive performance outside the investigated ranges.
For the water-content interpolation, the model parameters at water contents of 10% and 16% were used to predict the parameters at 14%. The normal stress was kept constant. Linear interpolation was performed as shown in Equation (9).
X 14 = X 10 + 2 3 ( X 16 − X 10 )
where X10, X14, and X16 are the values of a given model parameter at water contents of 10%, 14%, and 16%, respectively. The interpolation coefficient of 2/3 represents the relative position of 14% between 10% and 16%.
For the normal-stress interpolation, the model parameters at normal stresses of 100 and 300 kPa were used to predict the parameters at 200 kPa. The water content was kept constant. Linear interpolation was performed as shown in Equation (10).
X 200 = X 100 + 0.5 ( X 300 − X 100 )
where X100 and X300 denote the values of a given model parameter at normal stresses of 100 and 300 kPa, respectively, and X200 denotes its interpolated value at 200 kPa. The water content is held constant. Because 200 kPa lies midway between 100 and 300 kPa, the interpolation weight is 0.5, and the estimated parameter is the arithmetic mean of the two endpoint values.
In Equations (9) and (10), X represents sp, τp, τe, m, or n. The parameter sp is the peak displacement. The parameter τp is the peak shear stress. The parameter τe is the shear stress at the endpoint displacement of 5.5 mm. The parameters m and n control the pre-peak and post-peak curve shapes, respectively.
The interpolated parameters were substituted into Equations (6) and (7) to generate the predicted shear stress–displacement curve. The parameters and curves of the target condition were used only for comparison. They were not included in the interpolation process.
The predictive performance was evaluated using the coefficient of determination (R2), root-mean-square error (RMSE), normalized root-mean-square error (NRMSE), peak-stress error, peak-displacement error, and shear-work error. The shear-work error was calculated by comparing G0–5.5 evaluated from the predicted curve with that evaluated from the mean experimental curve. These indices evaluated both local curve features and the overall shear response.
The prediction results are presented in Table 5 and Figure 8. The water-content interpolation showed good overall performance. The three predicted curves at a water content of 14% had R2 values of 0.804, 0.957, and 0.952 under normal stresses of 100, 200, and 300 kPa, respectively. The mean R2 was 0.904. The mean RMSE and NRMSE were 24.07 kPa and 9.13%, respectively.
Table 5. Interpolation-based predictive evaluation of the bond–slip model.
Figure 8. Held-out-condition interpolation evaluation in the water-content and normal-stress directions.
The peak shear stress was predicted accurately in the water-content direction. The peak-stress errors were 0.33%, 1.65%, and 1.17% under normal stresses of 100, 200, and 300 kPa, respectively. The mean error was 1.05%. The mean peak-displacement error was 5.10%. The mean shear-work error was 4.70%.
The best prediction was obtained for W14-N200. Its R 2 was 0.957. Its NRMSE was 6.04%. The shear-work error was only 0.55%. The prediction also showed good agreement for W14-N300. The corresponding R2 was 0.952, and the NRMSE was 7.02%.
The lowest prediction accuracy in the water-content direction occurred for W14-N100. Its R2 was 0.804, and its NRMSE was 14.34%. The predicted peak stress and peak displacement remained close to the corresponding values extracted from the mean experimental curve. Their errors were 0.33% and 3.87%, respectively. However, the predicted ascending branch differed from the target curve. The interpolated value of m did not reproduce the delayed pre-peak stress mobilization under this condition. This difference increased the curve-based error, although the main characteristic points were predicted accurately.
The normal-stress interpolation showed lower overall accuracy. The predicted curves at 200 kPa had R2 values of 0.886, 0.829, and 0.686 at water contents of 10%, 14%, and 16%, respectively. The mean R2 was 0.800. The mean RMSE was 35.51 kPa. The mean NRMSE was 12.50%.
The peak shear stress remained well predicted in the normal-stress direction. The peak-stress errors ranged from 0.63% to 2.56%. The mean error was 1.50%. This result is consistent with the approximately linear variation in peak shear strength with normal stress, as described in Section 3.2.
However, the peak-displacement and shear-work predictions showed larger errors. The mean peak-displacement error was 10.31%. The mean shear-work error was 11.73%. These values were much larger than those obtained from the water-content interpolation.
The W10-N200 prediction showed the best agreement among the three normal-stress predictions. Its R2 was 0.886. Its peak-displacement and shear-work errors were 3.98% and 2.67%, respectively. The predicted curve captured the main peak and post-peak trends.
The W14-N200 prediction had an R2 of 0.829. Its peak-stress error was only 0.63%. However, its peak-displacement error reached 13.98%. The shear-work error was 13.22%. Thus, accurate prediction of the peak stress did not ensure accurate prediction of the complete curve.
The lowest accuracy was obtained for W16-N200. Its R2 was 0.686, and its NRMSE was 14.48%. The peak-stress error remained low at 1.33%. However, the peak-displacement and shear-work errors reached 12.98% and 19.28%, respectively. The main error occurred in the curve shape and the post-peak branch.
The lower accuracy of the normal-stress interpolation was associated with the nonlinear changes in sp, τe, m, and n. These parameters did not vary monotonically between 100 and 300 kPa. Linear interpolation therefore reproduced the peak strength more accurately than the complete bond–slip response.
Overall, the results show that the model had better interpolation capability in the water-content direction than in the normal-stress direction. The peak shear stress was predicted accurately in both directions. However, the complete curve was more sensitive to the peak displacement and shape parameters. The prediction of post-peak resistance was also less stable. Therefore, the proposed interpolation procedure is more suitable for estimating general response trends within the tested range than for predicting detailed curve shapes under all conditions.

3.5. SEM Morphology and MIP Pore-Throat Distribution

Figure 9 shows the macroscopic morphology of the polyurethane–silt interface. The interface was not smooth or planar. The expanding polyurethane entered the voids between soil particles. It formed a branched transition layer near the interface. Several local polymer penetration branches extended into the silt. These structures increased the geometric complexity of the contact zone.
Figure 9. Bonding interface between the polymer and silty soil.
Figure 10 shows the SEM images obtained at different water contents. A distinct boundary was observed between the polyurethane foam and the compacted silt. The boundary was irregular under all three water-content conditions. Polymer-rich regions were also observed inside the soil matrix. A representative penetration path is marked in Figure 10d. The elongated polymer region indicates that the grout entered connected voids between soil particles.
Figure 10. SEM images of the polymer–silt interface. (a) Polymer–silt interface at a water content of 10%. (b) Polymer–silt interface at a water content of 14%. (c) Polymer–silt interface at a water content of 16%. (d) Localized polymer penetration path within the silt matrix.
The interface contours marked in the SEM images were digitized. Three geometric indices were then obtained. These indices were the contour-length ratio, peak-to-valley height, and root-mean-square height. The results describe the annotated two-dimensional interface profiles. They do not represent the actual three-dimensional contact area.
The contour-length ratios were 1.098, 1.133, and 1.126 at water contents of 10%, 14%, and 16%, respectively. All values were greater than 1.0. This result confirms that the interface contours were tortuous. However, the contour-length ratio did not decrease monotonically with water content. The largest value was obtained at a water content of 14%. Therefore, water content did not simply reduce the measured contour length.
The vertical roughness showed a clearer trend. The peak-to-valley height decreased from approximately 164 μm at a water content of 10% to 124 μm at 16%. The root-mean-square height decreased from approximately 48 to 26 μm over the same range. Thus, the large-scale vertical undulations became weaker as the water content increased.
The reduction in vertical roughness indicates a flatter interface profile under wetter conditions. A flatter profile may provide less geometric resistance during shear displacement. It may also weaken the contribution of local polymer penetration branches to mechanical interlocking. However, only one representative SEM field was analyzed for each water content. Therefore, these geometric indices should be interpreted as semiquantitative evidence rather than statistical measurements.
The MIP results are presented in Figure 11 and Table 6. The pore-throat distribution changed markedly with water content. The main change was a decrease in large pore throats and an increase in pore throats within the range of 5–50 nm.
Figure 11. Pore-throat volume-fraction distributions of the polyurethane–silt interface specimens at different water contents.
Table 6. Digitized pore-throat volume fractions obtained from the MIP results.
At a water content of 10%, pore throats larger than 1 μm accounted for 53.85% of the total mercury-accessible pore volume. This proportion decreased to 32.82% at 14% water content. It further decreased slightly to 32.05% at 16%. The total proportion of pore throats larger than 50 nm decreased from 68.98% to 51.02% and 43.08%, respectively.
In contrast, the proportion of pore throats within the range of 5–50 nm increased markedly. It increased from 9.23% at a water content of 10% to 37.95% at 14% and 52.56% at 16%. The proportion of pore throats smaller than 5 nm showed the opposite trend. It decreased from 21.79% to 11.03% and 4.36%, respectively.
The changes within the larger pore-throat ranges were not uniform. The proportion of 1–20 μm pore throats decreased from 50.8% at a water content of 10% to 23.8% at 14%. It then increased slightly to 25.6% at 16%. The proportion of 20–100 μm pore throats increased from 3.1% to 9.0% and then decreased to 6.4%. These results show that moisture caused a redistribution of the accessible pore-throat structure rather than a uniform shift across all pore sizes.
The lower proportion of large mercury-accessible pore throats and the reduced vertical roughness of the selected SEM profiles suggest possible differences in interface formation among the initial water-content conditions. These observations provide indirect context for discussing polymer penetration and mechanical interlocking. However, the dried-state pore-throat distributions do not directly measure the number of wet-state penetration channels or demonstrate a reduction in grout penetration.
Overall, the SEM and MIP results showed two main trends. First, the interface became flatter in the vertical direction as the water content increased. Second, the proportion of large mercury-accessible pore throats decreased. These sample-specific trends provide descriptive evidence for the tentative mechanistic interpretation discussed in Section 4.1.

3.6. Moisture Reduction Factors and Finite-Displacement Reserve

Three dimensionless indices were used to quantify the effects of water content. These indices were the peak-strength moisture-reduction factor, the finite-displacement moisture-reduction factor, and the finite-displacement reserve ratio. The water content of 10% was used as the reference condition.
The peak-strength moisture-reduction factor was defined as shown in Equation (11).
k p , w ( w , σ n ) = τ p ( w , σ n ) τ p ( 10 % , σ n )
where kp,w is the peak-strength moisture-reduction factor, w is the water content, and σn is the applied normal stress. The term τp(w,σn) is the peak interface shear strength at water content w and normal stress σn. The denominator is the peak strength at a water content of 10% under the same normal stress. The value of kp,w is equal to 1.0 for the reference condition.
A similar factor was defined for the interface resistance at a displacement of 5.5 mm, as shown in Equation (12).
k 5.5 , w ( w , σ n ) = τ 5.5 ( w , σ n ) τ 5.5 ( 10 % , σ n )
where k5.5,w is the finite-displacement moisture-reduction factor. The term τ5.5(w, σn) is the interface shear stress at a displacement of 5.5 mm. The denominator is the corresponding value at a water content of 10% under the same normal stress.
The finite-displacement reserve ratio was calculated as shown in Equation (13).
r 5.5 = τ 5.5 ( w , σ n ) τ p ( w , σ n )
where r5.5 is the proportion of peak interface strength retained at a displacement of 5.5 mm. A larger value indicates that a greater proportion of the peak resistance was retained after substantial interface displacement. This ratio does not represent a conventional residual-strength ratio because a stable residual plateau was not reached under all test conditions.
The fitted peak and finite-displacement strength envelopes in Equations (4) and (5) were used to calculate the three indices. The results are summarized in Table 7. Among these indices, kp,w was selected for graphical presentation because it directly describes the moisture-induced reduction in peak interface strength. Figure 12 shows the variation in kp,w within the tested water-content and normal-stress ranges.
Table 7. Moisture-reduction factors and finite-displacement reserve ratios within the tested range.
Figure 12. Variation in the peak-strength moisture-reduction factor kp,w with water content and normal stress. (a) Variation of kp,w with water content under different normal stresses. (b) contour distribution of kp,w within the investigated water-content and normal-stress ranges.
The peak-strength factor decreased with increasing water content. At a water content of 14%, kp,w was 0.718 under a normal stress of 100 kPa. It increased to 0.751 and 0.776 under normal stresses of 200 and 300 kPa, respectively. These values correspond to peak-strength reductions of 28.2%, 24.9%, and 22.4% relative to the 10% condition.
A larger reduction was observed at a water content of 16%. The values of kp,w were 0.564, 0.626, and 0.673 under normal stresses of 100, 200, and 300 kPa, respectively. The corresponding peak-strength reductions were 43.6%, 37.4%, and 32.7%.
The peak-strength factor increased moderately with normal stress at both elevated water contents. The lowest factor was obtained under a normal stress of 100 kPa. Thus, the relative reduction in peak strength was greater under lower normal confinement. Higher normal stress reduced the relative influence of water content, but it did not eliminate the strength loss.
The finite-displacement factor showed a similar moisture dependence. At a water content of 14%, k5.5,w ranged from 0.745 to 0.757. Its variation with normal stress was small. The interface retained approximately 75% of the reference finite-displacement resistance.
The reduction became much greater at a water content of 16%. The values of k5.5,w were 0.448, 0.503, and 0.535 under normal stresses of 100, 200, and 300 kPa, respectively. These values correspond to reductions of 55.2%, 49.7%, and 46.5%. The finite-displacement factor was lower than the corresponding peak-strength factor at all three normal stresses. Therefore, the post-peak response was more sensitive to the increase from 10% to 16% water content than the peak resistance.
The reserve ratio increased with normal stress under all water-content conditions. At a water content of 10%, r5.5 increased from 0.593 at 100 kPa to 0.696 at 200 kPa and 0.775 at 300 kPa. A similar trend was obtained at a water content of 14%. The corresponding values were 0.615, 0.698, and 0.756.
The reserve ratios at water contents of 10% and 14% were generally close. A clear reduction occurred at a water content of 16%. Under this condition, r5.5 increased from 0.472 at 100 kPa to 0.560 at 200 kPa and 0.616 at 300 kPa. Thus, high water content reduced both the absolute resistance at 5.5 mm and the proportion of peak strength retained at this displacement.
The lowest kp,w, k5.5,w, and r5.5 values were obtained at a water content of 16% under a normal stress of 100 kPa. This condition combined high moisture with low confinement. It produced the largest relative loss of peak strength and finite-displacement resistance.
Piecewise linear interpolation was applied between the tested water contents at each normal-stress level. The interpolated values of kp,w were used to construct the response surface in Figure 12. The surface shows the combined effects of water content and normal stress on the relative peak interface strength. The corresponding values of k5.5,w and r5.5 are provided in Table 7. All three factors are experimental comparison indices and should be used only within the tested range.

4. Discussion

4.1. Moisture-Dependent Micro–Macro Degradation Mechanism

The mechanical and microstructural results suggest a tentative two-stage interpretation of moisture-dependent degradation. The associated micro–macro trends are summarized in Figure 13. For comparison, the selected indices were normalized by their values at a water content of 10%, and the normalized reference value was set to 1.0.
Figure 13. Normalized micro-macro trends.
The polyurethane–silt interface resistance was governed by physical adhesion, polymer penetration, mechanical embedment, local interlocking, and friction under normal confinement. Moisture did not affect these components equally. The apparent interface cohesion cp decreased from 270.32 kPa at a water content of 10% to 129.30 kPa at 16%, which represents a reduction of 52.2%. The values of tanδp were 0.5087, 0.4882, and 0.5176, and the corresponding interface friction angles were 26.96°, 26.02°, and 27.37° at water contents of 10%, 14%, and 16%, respectively. Under the common target-density preparation protocol, the observed water-content dependence of the peak-strength envelope was expressed predominantly through a reduction in the apparent cohesion intercept. This comparison characterizes the response associated with initial water content under the adopted preparation conditions; the independent contribution of specimen-to-specimen density variation was not quantified.
For discussion, the observed changes are considered over the two tested water-content intervals. The first stage occurred between water contents of 10% and 14%. The proportion of mercury-accessible pore throats larger than 1 μm decreased from 53.85% to 32.82%, whereas the proportion of 5–50 nm pore throats increased from 9.23% to 37.95%. This pattern may be consistent with less favorable conditions for polymer penetration and anchorage, although neither effect was directly quantified. The SEM images support this interpretation by showing localized polymer penetration and an irregular transition layer.
The microstructural change was accompanied by clear mechanical degradation. From 10% to 14% water content, cp decreased by 32.8%. The mean secant stiffness K20–60 and mean shear-work index G0–5.5 decreased by approximately 51.9% and 32.3%, respectively. These coordinated changes are consistent with a possible contribution from reduced polymer penetration and mechanical anchorage.
The second stage occurred between water contents of 14% and 16%. The proportion of pore throats larger than 1 μm changed only slightly, from 32.82% to 32.05%. However, cp, stiffness, shear-work index, and finite-displacement resistance continued to decrease. The continued mechanical degradation despite the small change in the measured large-pore-throat fraction suggests that additional processes may contribute.
At higher water content, the mechanical state of the silt may become more important. A thicker water film may reduce direct polymer–soil contact and increase lubrication during sliding. Higher water content may also reduce matric suction and soften the soil skeleton [36]. These effects can promote particle rearrangement and local deformation. They were not measured directly and should therefore be regarded as inferred mechanisms.
The SEM results provide further support. The contour-length ratio remained greater than 1.0 but showed no monotonic trend. In contrast, the peak-to-valley height decreased from approximately 164 to 124 μm, and the RMS height decreased from 48 to 26 μm. The interface therefore became flatter as water content increased. A flatter profile provides less geometric resistance and may weaken the effect of localized penetration branches. Because only one representative SEM field was analyzed for each condition, these results should be treated as semiquantitative evidence.
Moisture also caused stronger degradation after the peak. At a water content of 16%, the finite-displacement reduction factor k5.5,w was lower than the peak-strength factor kp,w at all normal stresses. The reserve ratio r5.5 also decreased. Higher normal stress partly improved interface contact and limited particle rearrangement, but it did not fully offset the effect of high water content.
Overall, reduced polymer penetration and mechanical anchorage are possible contributors to the degradation observed between 10% and 14% water content. Water-related weakening of the soil and interfacial contact may additionally contribute between 14% and 16%. This interpretation provides a possible explanation for the observed mechanical trends, but the relative contributions of these processes have not been established.
The proposed two-stage interpretation is subject to several uncertainties. The MIP characterization included only one specimen per initial water-content condition, and the SEM comparison was based on one selected field of view per condition, without independent microstructural replication. Consequently, between-specimen variability and the spatial representativeness of the observations could not be quantified. The MIP results describe mercury-accessible pore throats after vacuum drying at 60–80 °C; the water-content labels refer to specimen preparation rather than the moisture state during MIP testing. Drying may induce shrinkage and alter the pore structure [30], and the magnitude of this effect was not evaluated in the present study. The measured distributions therefore cannot directly establish the pore network available during wet-state grouting or quantify polyurethane penetration. Likewise, the two-dimensional SEM profiles do not measure the three-dimensional penetration volume or contact area. The proposed interpretation is based on associations between the mechanical response and the available microstructural observations. It remains a working hypothesis requiring validation through independent replication and characterization that better preserves the wet-state structure. The three tested water contents also do not establish a distinct mechanistic transition at 14%.

4.2. Interpretation and Applicability of the Inverse Bond–Slip Model

The proposed model separates characteristic response values from curve-shape parameters. The peak displacement sp, peak shear stress τp, and endpoint stress τe were obtained directly from the mean experimental curves. Only the shape parameters m and n were identified by inversion. This reduced the number of unknowns and limited the coupling between strength and shape parameters.
The model was constrained to pass through three characteristic points: the origin, the peak point, and the common endpoint. It therefore preserved the main features of each curve. The parameter m controlled the pre-peak response, while n controlled the post-peak response.
The power–polynomial model clearly outperformed the bilinear model. It achieved a mean R2 of 0.9745 and a mean RMSE of 13.16 kPa. It also produced the lowest total AIC. Its performance was close to that of the power–exponential model. Therefore, it should not be regarded as the only possible model. It was selected because it provided a good balance between accuracy, simplicity, and endpoint control.
Although the inversion procedure was numerically stable, parameter identifiability varied among test conditions. The pre-peak parameter m was relatively well constrained, whereas the post-peak parameter n exhibited wider objective-profile intervals for W10_N200 and W10_N300. Both parameters should be interpreted as empirical descriptors of curve shape rather than independently validated indicators of specific interface mechanisms.
The interpolation results further defined the model applicability. The model performed better in the water-content direction, with a mean R2 of 0.904 and a mean peak stress error of 1.05%. The normal-stress interpolation was less accurate, with a mean R2 of 0.800. However, the peak shear stress remained well predicted, with a mean error of 1.50%.
The lower accuracy of the complete-curve predictions was mainly related to the nonlinear changes in sp, τe, m, and n. Peak strength varied approximately linearly with normal stress, while the curve-shape parameters showed more complex trends. Therefore, the model was more reliable for predicting peak strength than for predicting peak displacement and post-peak shape.
Overall, the proposed relation provides an empirical description of the mean experimental responses for the tested polyurethane–silt system. Its assessed scope is limited to monotonic loading, water contents of 10–16%, normal stresses of 100–300 kPa, and shear displacements up to 5.5 mm. The limited number of water-content and normal-stress levels does not establish general relationships governing parameter variation, particularly because the fitted shape parameters do not exhibit simple monotonic trends. The present results therefore support curve fitting and preliminary within-range interpolation, rather than a transferable interface constitutive model. Broader experimental coverage and independent validation are required before the relation can be used for other materials, loading paths, or general engineering predictions.

4.3. Interface-Level Implications and Limitations for Foundation Repair

The present results concern the shear response of the tested polyurethane–silt interface, which represents one contact within a possible foundation–polyurethane–soil load-transfer system. When these three components act together, the overall response depends on the foundation–polyurethane contact, deformation of the grout body and surrounding soil, and the geometry and continuity of the contacts. Depending on the configuration, load transfer may involve normal compression and bearing as well as interface shear. The present direct-shear tests do not resolve these coupled processes or establish which component governs failure.
Within the investigated conditions, higher water content reduced the interface shear resistance, while higher applied normal stress increased it. These observations identify moisture and normal confinement as relevant variables when characterizing the tested interface. However, a prescribed normal stress in a direct-shear test does not reproduce the evolving contact stresses in a repaired foundation. Likewise, the responses at different preparation water contents do not, by themselves, establish the behavior of a repaired system subjected to subsequent wetting or groundwater changes.
Within the present dataset, the lower-normal-stress condition refers to 100 kPa, the lowest applied stress. Potential engineering situations in which low-normal-stress interface behavior may be relevant include polyurethane–soil contacts beneath lightly loaded floor slabs, around grout bodies adjoining partially filled cavities, and in locally unloaded regions following loss of support. These situations may involve small or nonuniform normal contact stresses, whose magnitudes must be assessed for the actual geometry and loading conditions. Local interface normal stress should not be equated directly with nominal foundation bearing pressure. The present results provide laboratory comparisons relevant to such assessments only within the tested range; quantitative predictions for interfaces subjected to stresses below 100 kPa require additional experimental characterization.
Equation (14) provides only an illustrative nominal shear-resistance estimate for an assumed polyurethane–soil interface region:
V p = τ p A e f f
Here, τp is a representative peak interface shear stress obtained from the envelope fitted to the means of individual specimen peaks and Aeff is an assumed effective contact area. This estimate assumes that the representative peak stress is uniformly mobilized over that area. Neither the effective contact area nor simultaneous peak mobilization over a field interface was established in this study. Equation (14) therefore does not account for nonuniform stresses, progressive slip, foundation–polyurethane contact behavior, or deformation of the surrounding materials, and must not be interpreted as the bearing capacity of a repaired foundation.
The finite-displacement indices similarly describe resistance retained at the selected displacement of 5.5 mm. They provide comparisons between the investigated interface responses, but do not establish an allowable foundation displacement or a safety reserve for the complete repair system. The tests also do not provide a basis for selecting injection spacing, injection volume, or drainage measures.
The fitted parameters and reduction factors are specific to the investigated silt–polyurethane combination, including the polyurethane foam with a measured cured density of 0.490 g/cm3, and the adopted preparation and loading conditions. Their assessed scope is limited to water contents of 10–16% and normal stresses of 100–300 kPa. They should not be transferred directly to other soils or repair configurations without material-specific testing and validation.
Application to the complete foundation–polyurethane–soil system would require characterization of the foundation–polyurethane contact, the relevant bulk material behavior, and the actual contact geometry and loading conditions, followed by validation against system-level experiments or field observations. The present study provides an interface-level empirical characterization that may inform such future investigations; it does not provide a validated prediction of foundation repair performance.

5. Conclusions

This study investigated the moisture-dependent shear behavior of foamed polyurethane–silt interfaces under normal stresses of 100–300 kPa. Peak-strength analysis, inverse bond–slip modeling, interpolation-based prediction, and SEM/MIP characterization were combined. The main conclusions are as follows:
Increasing water content reduced the peak strength, pre-peak stiffness, shear-work index, and finite-displacement resistance. The apparent interface cohesion decreased from 270.32 to 129.30 kPa as the water content increased from 10% to 16%. The interface friction angles were 26.96°, 26.02°, and 27.37° at water contents of 10%, 14%, and 16%, respectively. Within the investigated range, the reduction in peak resistance was associated mainly with a decrease in the apparent envelope intercept, while the fitted slope changed comparatively little; the individual physical contributions to this change were not independently resolved.
The empirical power–polynomial relation provided a compact description of the mean experimental curves within the investigated displacement range. It achieved a mean R2 of 0.9745 and a mean RMSE of 13.16 kPa. The global–local inversion procedure was numerically stable. The model showed better interpolation performance in the water-content direction than in the normal-stress direction. The corresponding mean R2 values were 0.904 and 0.800. Peak strength was more predictable than peak displacement and post-peak curve shape.
The available SEM and MIP observations, considered together with the mechanical results, suggest a tentative two-stage interpretation of moisture-related degradation. The measured proportion of pore throats larger than 1 μm decreased from 53.85% to approximately 32%, while the fraction of 5–50 nm pore throats increased from 9.23% to 52.56%. Reduced polymer penetration and anchorage, together with water-related weakening of the soil and interfacial contact, are possible contributing processes. Their relative contributions remain unverified because the microstructural observations were not independently replicated and MIP was conducted on dried specimens.
Within the tested range, high water content combined with the lowest applied normal stress produced the greatest relative reductions in interface shear resistance. At a water content of 16% and a normal stress of 100 kPa, the peak-strength reduction factor, finite-displacement reduction factor, and reserve ratio were 0.564, 0.448, and 0.472, respectively. These factors describe relative changes in the tested interface resistance. They do not quantify the bearing capacity, settlement, or safety margin of a repaired foundation and should not be used as system-level design coefficients without further validation.
These conclusions are limited to the investigated silt, polymer density, water-content range, and normal-stress range. The bond–slip model was calibrated against mean experimental curves obtained from three replicate tests per condition. Future work should examine specimen-level variability in the identified model parameters and extend the investigation to controlled-suction tests, three-dimensional interface characterization, long-term loading, and field-scale validation.

Author Contributions

Conceptualization, X.J.; methodology, X.J. and L.Z.; software, Y.W.; validation, X.J., L.Z. and Y.W.; formal analysis, X.J.; investigation, L.Z.; resources, Q.H.; data curation, L.Z.; writing—original draft preparation, X.J.; writing—review and editing, L.Z.; visualization, Q.H.; supervision, Q.W.; project administration, L.Z.; funding acquisition, Q.H. and J.Z. All authors have read and agreed to the published version of the manuscript.

Funding

This work was supported by the National Natural Science Foundation of China (Grant No. 42507261).

Data Availability Statement

The shear stress–horizontal displacement curves for all 27 direct shear tests and the specimen-level summary values are provided in Appendix A. The complete numerical records are not publicly available because they are subject to the research group’s data-sharing restrictions. Requests for access may be addressed to the corresponding author and will be considered subject to approval by the research group.

Conflicts of Interest

The authors declare no conflicts of interest.

Appendix A

Table A1 summarizes the characteristic values of the 27 individual direct shear tests, including specimen identifiers, water contents, normal stresses, peak shear stresses, corresponding horizontal displacements, and shear stresses at 5.5 mm displacement. Peak values and their corresponding displacements were extracted separately from each individual test curve. Specimen identifiers follow the format W10-N100-R1, where W denotes water content (%), N denotes normal stress (kPa), and R denotes the replicate number. Because a stable residual plateau was not reached in all tests, the shear stress at 5.5 mm is reported as a finite-displacement resistance rather than a residual shear strength.
Table A1. Peak and finite-displacement strength-envelope parameters.
Figure A1. Curves of results from 27 original test trials.

References

  1. Saleh, S.; Yunus, N.Z.M.; Ahmad, K.; Ali, N. Improving the strength of weak soil using polyurethane grouts: A review. Constr. Build. Mater. 2019, 202, 738–752. [Google Scholar] [CrossRef] [Scilit]
  2. Liu, K.; Liang, W.; Ren, F.; Ren, J.; Wang, F.; Ding, H. The study on compressive mechanical properties of rigid polyurethane grout materials with different densities. Constr. Build. Mater. 2019, 206, 270–278. [Google Scholar] [CrossRef] [Scilit]
  3. Guo, C.; Cui, C.; Wang, F. Case study on quick treatment of voids under airport pavement by polymer grouting. J. Mater. Civ. Eng. 2020, 32, 05020006. [Google Scholar] [CrossRef] [Scilit]
  4. Fang, H.; Li, B.; Wang, F.; Wang, Y.; Cui, C. The mechanical behaviour of drainage pipeline under traffic load before and after polymer grouting trenchless repairing. Tunn. Undergr. Space Technol. 2018, 74, 185–194. [Google Scholar] [CrossRef] [Scilit]
  5. Wang, R.; Wang, F.; Xu, J.; Zhong, Y.; Li, S. Full-scale experimental study of the dynamic performance of buried drainage pipes under polymer grouting trenchless rehabilitation. Ocean Eng. 2019, 181, 121–133. [Google Scholar] [CrossRef] [Scilit]
  6. Li, B.; Wang, F.; Fang, H.; Yang, K.; Zhang, X.; Ji, Y. Experimental and numerical study on polymer grouting pretreatment technology in void and corroded concrete pipes. Tunn. Undergr. Space Technol. 2021, 113, 103842. [Google Scholar] [CrossRef] [Scilit]
  7. Potyondy, J.G. Skin friction between various soils and construction materials. Géotechnique 1961, 11, 339–353. [Google Scholar] [CrossRef] [Scilit]
  8. Uesugi, M.; Kishida, H. Frictional resistance at yield between dry sand and mild steel. Soils Found. 1986, 26, 139–149. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  9. Dove, J.E.; Frost, J.D. Peak friction behavior of smooth geomembrane–particle interfaces. J. Geotech. Geoenvironmental Eng. 1999, 125, 544–555. [Google Scholar] [CrossRef] [Scilit]
  10. Hu, L.M.; Pu, J.L. Testing and modeling of soil–structure interface. J. Geotech. Geoenvironmental Eng. 2004, 130, 851–860. [Google Scholar] [CrossRef] [Scilit]
  11. Lam, C.; Jefferis, S.A.; Martin, C.M. Effects of polymer and bentonite support fluids on concrete–sand interface shear strength. Géotechnique 2014, 64, 28–39. [Google Scholar] [CrossRef] [Scilit]
  12. Li, M.; Li, Y.; Islam, M.R. Effects of water content and interface roughness on the shear strength of silt–cement mortar interface. Soils Found. 2021, 61, 1615–1629. [Google Scholar] [CrossRef] [Scilit]
  13. Murali, N.; Gujar, P.; Ghosh, P. Performance of clay–epoxy interface at different points on Proctor curve. Appl. Clay Sci. 2022, 226, 106553. [Google Scholar] [CrossRef] [Scilit]
  14. Pan, J.; Wang, B.; Wang, Q.; Ling, X.; Fang, R.; Liu, J.; Wang, Z. An adhesion–ploughing friction model of the interface between concrete and silty clay. Constr. Build. Mater. 2023, 376, 131039. [Google Scholar] [CrossRef] [Scilit]
  15. Fredlund, D.G.; Morgenstern, N.R.; Widger, R.A. The shear strength of unsaturated soils. Can. Geotech. J. 1978, 15, 313–321. [Google Scholar] [CrossRef] [Scilit]
  16. Li, M.; Fang, H.; Du, M.; Zhang, C.; Su, Z.; Wang, F. The behavior of polymer–bentonite interface under shear stress. Constr. Build. Mater. 2020, 248, 118680. [Google Scholar] [CrossRef] [Scilit]
  17. Li, M.; Zhang, C.; Fang, H.; Du, M.; Su, Z.; Wang, F. Effects of water content on shear properties of bentonite–polymer composite structure. Eng. Geol. 2021, 287, 106098. [Google Scholar] [CrossRef] [Scilit]
  18. Li, M.; Xue, B.; Fang, H.; Zhang, S.; Wang, F. Variable angle shear test and finite element simulation of polyurethane–bentonite composite structure. Structures 2023, 48, 1722–1729. [Google Scholar] [CrossRef] [Scilit]
  19. Li, J.; Li, J.; Zhang, J.; Liu, G. Static and dynamic properties study on interface between new polymer materials and silty clay based on ring shear tests. Polymers 2023, 15, 634. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  20. Wang, C.; Guo, C.; Du, X.; Shi, M.; Liu, Q.; Xia, Y. Reinforcement of silty soil with permeable polyurethane by penetration injection. Constr. Build. Mater. 2021, 310, 124829. [Google Scholar] [CrossRef] [Scilit]
  21. Wang, L.; Yang, X.; Diao, Y.; Guo, C. Study on bonding characteristics of polymer grouted concrete–soil interface. Polymers 2024, 16, 2207. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  22. Fang, H.; Su, Z.; Li, X.; Wang, F.; Fu, Y. Interfacial bond performance between self-expansion polymer and concrete. Constr. Build. Mater. 2021, 270, 121459. [Google Scholar] [CrossRef] [Scilit]
  23. Qin, L.; Guo, C.; Sun, W.; Guan, H.; Yan, W.; Wang, F. Experimental investigation on the interfacial shear bond performance of non-water reacting polymer and concrete. Constr. Build. Mater. 2022, 331, 127351. [Google Scholar] [CrossRef] [Scilit]
  24. Wang, Y.; Wan, Y.; Guo, C.; Zeng, C.; Shao, J.; Wang, F. Experimental investigation on the monotonic, cyclic and post-cyclic interfacial behavior of non-water-reacted polymer and concrete. Constr. Build. Mater. 2021, 292, 123323. [Google Scholar] [CrossRef] [Scilit]
  25. Zhang, C.; Li, Z.; Wu, Y.; Wang, C.; Fang, H.; He, C.; Duan, C. Micromechanical properties of polymer–bentonite interface: A molecular dynamics study. Constr. Build. Mater. 2024, 420, 135638. [Google Scholar] [CrossRef] [Scilit]
  26. Goodman, R.E.; Taylor, R.L.; Brekke, T.L. A model for the mechanics of jointed rock. J. Soil Mech. Found. Div. 1968, 94, 637–659. [Google Scholar] [CrossRef] [Scilit]
  27. Desai, C.S.; Zaman, M.M.; Lightner, J.G.; Siriwardane, H.J. Thin-layer element for interfaces and joints. Int. J. Numer. Anal. Methods Geomech. 1984, 8, 19–43. [Google Scholar] [CrossRef] [Scilit]
  28. GB/T 50123-2019; Standard for Geotechnical Testing Method. China Planning Press: Beijing, China, 2019.
  29. Washburn, E.W. The dynamics of capillary flow. Phys. Rev. 1921, 17, 273–283. [Google Scholar] [CrossRef] [Scilit]
  30. Diamond, S. Pore size distributions in clays. Clays Clay Miner. 1970, 18, 7–23. [Google Scholar] [CrossRef] [Scilit]
  31. Romero, E.; Simms, P.H. Microstructure investigation in unsaturated soils: A review with special attention to contribution of mercury intrusion porosimetry and environmental scanning electron microscopy. Geotech. Geol. Eng. 2008, 26, 705–727. [Google Scholar] [CrossRef] [Scilit]
  32. Barton, N.; Choubey, V. The shear strength of rock joints in theory and practice. Rock Mech. 1977, 10, 1–54. [Google Scholar] [CrossRef] [Scilit]
  33. Akaike, H. A new look at the statistical model identification. IEEE Trans. Autom. Control 1974, 19, 716–723. [Google Scholar] [CrossRef] [Scilit]
  34. Storn, R.; Price, K. Differential evolution—A simple and efficient heuristic for global optimization over continuous spaces. J. Glob. Optim. 1997, 11, 341–359. [Google Scholar] [CrossRef] [Scilit]
  35. Coleman, T.F.; Li, Y. An interior trust region approach for nonlinear minimization subject to bounds. SIAM J. Optim. 1996, 6, 418–445. [Google Scholar] [CrossRef] [Scilit]
  36. Lu, N.; Likos, W.J. Suction stress characteristic curve for unsaturated soil. J. Geotech. Geoenvironmental Eng. 2006, 132, 131–142. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations