Mechanical Properties of PBL Connectors in CA-UHPC Specimens Under Sustained Loading

,
,
,
,
and
1
Shandong Expressway Infrastructure Construction Co., Ltd., Jinan 250000, China
2
School of Intelligent Science and Engineering, Jiangsu University, Zhenjiang 212013, China
*
Author to whom correspondence should be addressed.
Buildings2026, 16(23), 4688;https://doi.org/10.3390/buildings16234688 
(registering DOI)
This article belongs to the Section Building Structures

Abstract

To investigate the effect of sustained loading on the mechanical properties of perfobond leiste (PBL) shear connectors in coarse aggregate ultra-high-performance concrete (CA-UHPC) specimens, 180-day sustained-loading tests followed by ultimate push-out tests were conducted on six specimens, with one specimen representing each configuration, to evaluate the effects of steel plate thickness, hole diameter, transverse reinforcement, concrete strength, and connector type. The results indicate that under sustained loading, the relative slip between the steel plate and the CA-UHPC develops rapidly during the initial stage and gradually stabilizes thereafter. The 180-day cumulative slip increments of the larger-hole and thicker-plate specimens were 19.2% and 26.9% lower, respectively, than those of the standard specimen. However, the individual sustained-load ratios were not identical. In particular, the calculated load ratio of the thicker-plate specimen was 39.08%, compared with 32.34% for the standard specimen. Therefore, the observed differences should be interpreted in the context of the adopted paired-loading protocol rather than attributed solely to the corresponding geometric parameters. Compared with the short-term reference results, the specimens tested after 180 days of sustained loading exhibited lower ultimate shear capacities and initial shear stiffnesses, with the differences varying according to connector configuration and material properties.

1. Introduction

Steel–concrete composite structures combine the tensile strength of steel with the compressive strength of concrete and are widely used in bridge engineering [1,2]. The composite action between steel and concrete relies on shear connectors to transfer longitudinal shear forces and restrict relative slip at the interface. Under sustained loading, concrete shrinkage and creep induce time-dependent deformation and internal force redistribution within composite members. Owing to the restraint imposed by the steel components and shear connectors, these time-dependent effects may generate additional stresses at the steel–concrete interface and influence the development of interfacial slip [3,4,5,6,7,8,9]. Therefore, understanding the long-term mechanical behavior of shear connectors is essential for evaluating the structural performance and serviceability of steel–concrete composite structures.
Headed studs are among the most widely used shear connectors because of their standardized fabrication and convenient welding procedures. However, their relatively high flexibility and susceptibility to fatigue failure under repeated loading have motivated the development of alternative connector systems. The perfobond leiste (PBL) connector, consisting of a perforated steel plate embedded in concrete, provides an alternative load-transfer mechanism. Concrete dowels formed within the perforations, together with transverse reinforcing bars passing through the holes, contribute to the transfer of interfacial shear forces. The shear resistance of PBL connectors is generally provided by the interfacial bond between steel and concrete, the shear and bearing resistance of concrete dowels, and the dowel action of transverse reinforcement; depending on the structural configuration, end-bearing effects may also contribute. Compared with conventional headed studs, PBL connectors have demonstrated high shear capacity, relatively high shear stiffness, and good fatigue resistance, making them particularly suitable for steel–concrete joints subjected to substantial shear forces [2,9,10].
Considerable experimental research has been conducted on the shear behavior of PBL connectors using push-out tests. He et al. [11] investigated PBL connectors in steel–concrete joints of hybrid bridges through 12 push-out specimens, examining the contributions of interfacial bonding, concrete dowels, and transverse reinforcement to the shear resistance. Subsequently, He et al. [12] conducted 24 push-out tests on PBL connectors using UHPC as the joint-grouting material, focusing on the effects of interfacial bonding, concrete dowels, transverse reinforcement, and steel fiber content. Tan et al. [13] further investigated the group effect of PBL connectors embedded in UHPC through push-out tests on 26 specimens, identifying the influences of concrete type, connector row number, and row spacing on the shear behavior. These studies have provided important insights into the load-transfer mechanisms, failure characteristics, and influencing parameters of PBL connectors. However, most of these investigations have primarily focused on their short-term shear behavior.
In addition to their short-term mechanical properties, the time-dependent behavior of shear connectors is also important because concrete shrinkage and creep may affect interfacial slip and the redistribution of internal forces during service. Wen et al. [14] conducted 180-day sustained-loading push-out tests on headed-stud connections, investigating the effects of loading age and stud diameter on their time-dependent behavior. Song et al. [15] combined long-term push-out tests with finite element analysis to examine the development of interfacial slip and material strains in steel–concrete composite specimens. Zhang et al. [9] conducted both short-term tests on 20 specimens and long-term tests on six PBL specimens in steel–concrete composite systems. Their parametric investigation covered hole diameter, number of holes, connector thickness, concrete strength, and transverse reinforcement diameter. The study also examined the time-dependent development of transverse reinforcement strain, interfacial slip, and stress around the perforations, and proposed a model for predicting the shear capacity of PBL connectors. The present study differs from their work primarily in the investigated cementitious material system and research focus. Specifically, this study focuses on PBL connectors embedded in CA-UHPC, rather than the steel–concrete composite system investigated in [9]. It monitors the relative slip between the steel plate and CA-UHPC during 180 days of sustained loading, followed by ultimate push-out tests to evaluate the subsequent load–slip response, ultimate shear capacity, initial shear stiffness, and failure characteristics. Furthermore, the present study extends the short-term static investigation of PBL connectors in steel–UHPC(CA) composite structures reported in [16] to sustained-loading conditions. Therefore, the contribution of this study is to provide experimental observations on the time-dependent interfacial slip and subsequent shear performance of PBL connectors specifically embedded in CA-UHPC, rather than to claim the first investigation of long-term PBL behavior or to develop another general shear-capacity prediction model.
The long-term behavior of UHPC-based composite structures is closely related to the time-dependent properties of the cementitious matrix. Owing to its high binder content and low water-to-binder ratio, conventional UHPC exhibits distinct shrinkage and creep characteristics, which are influenced by factors such as loading age, stress level, curing conditions, and fiber content [17]. The incorporation of coarse aggregates further changes the material composition and internal skeleton of UHPC. Recent studies have also investigated the engineering applications and mechanical properties of CA-UHPC, highlighting the influence of coarse aggregate incorporation on its material behavior [18,19,20]. Previous studies have examined the mechanical properties and autogenous shrinkage of CA-UHPC and have shown that coarse aggregate incorporation and mixture composition can affect its elastic modulus and shrinkage behavior [21,22]. The creep and shrinkage characteristics of CA-UHPC also depend on its mixture proportions and constituent materials. These differences may affect the local bearing behavior of concrete dowels, crack development, and stress transfer around the perforations of PBL connectors. Consequently, the long-term mechanical behavior of PBL connectors embedded in CA-UHPC should be investigated independently rather than directly inferred from the results obtained using ordinary concrete or conventional UHPC.
Regarding the short-term shear performance of PBL connectors in CA-UHPC, Duan et al. [10] conducted 12 push-out tests on UHPC–steel composite specimens containing coarse aggregates, investigating the effects of transverse reinforcement diameter, hole spacing, and hole number. More recently, Zheng et al. [16] experimentally investigated the static shear performance of PBL connectors in steel–UHPC(CA) composite structures, considering the presence of transverse reinforcement, perforated steel plate thickness, hole diameter, concrete strength, and connector configuration. These studies have established an important experimental basis for understanding the static behavior of PBL connectors in CA-UHPC. Nevertheless, the time-dependent development of interfacial slip under sustained loading and the subsequent changes in ultimate shear capacity, initial shear stiffness, and failure characteristics remain insufficiently understood. In particular, the extent to which the short-term mechanical characteristics observed in CA-UHPC-based PBL connectors are maintained after prolonged loading has not been adequately clarified.
To address these issues, this study investigates the long-term mechanical behavior of PBL connectors embedded in CA-UHPC through 180-day sustained-loading tests followed by ultimate push-out tests. Six sustained-loading specimens were examined, including five PBL configurations and one headed-stud reference configuration. The effects of transverse reinforcement, perforated steel plate thickness, hole diameter, CA-UHPC strength grade, and connector type were examined through comparisons of the measured responses. During the sustained-loading period, the time-dependent development of interfacial slip between the steel plate and CA-UHPC was monitored. Following sustained loading, ultimate push-out tests were conducted to determine the failure modes, load–slip relationships, ultimate shear capacities, and initial shear stiffnesses. By comparing the results with the corresponding short-term static test data reported in [16], this study evaluates the changes in the shear performance of PBL connectors after sustained loading. The main contribution of this research is to extend the existing static investigation of PBL connectors in CA-UHPC to their long-term service-related behavior, providing experimental evidence on the relationship between time-dependent interfacial slip and post-sustained-loading shear performance. The findings provide a reference for understanding the long-term behavior and design of PBL connectors in steel–CA-UHPC composite structures.

2. Experimental Program

2.1. Material Properties

The push-out specimens were fabricated using coarse aggregate ultra-high-performance concrete (CA-UHPC) with two nominal strength grades, C120 and C140. The constituent materials included 52.5-grade Portland cement, premixed dry powder, basalt coarse aggregate, standard sand, hybrid steel fibers, a water-reducing admixture, and water.
The coarse aggregate consisted of high-strength basalt with a maximum nominal particle size of 8 mm. The premixed dry powder consisted mainly of silica fume and other supplementary powder constituents. The standard sand was clean natural river sand with a particle size of 0.5–1.0 mm and a fineness modulus of 2.4–2.8. The admixture system included water-reducing and plasticizing components.
Two types of high-strength copper-coated steel fibers were incorporated into the CA-UHPC mixtures: straight fibers with a length of 13 mm and hooked-end fibers with a length of 20 mm. For the C140 mixture, the dosages of straight and hooked-end fibers were both 97.5 kg/m3. For the C120 mixture, the corresponding dosages were both 78 kg/m3. The available original material records specify the fiber types, lengths, and mass dosages. However, the supplier’s datasheets for the steel fibers used in this study were unavailable, and their diameters and tensile strengths could not be independently verified. Therefore, these parameters are not reported to avoid introducing unverified material properties. The original mix-design records also do not specify the fiber volume fractions, and these values could not be confirmed from the available documentation. Therefore, the fiber contents are reported by mass dosage only, without estimating the corresponding volume fractions.
The mix proportions of the two CA-UHPC mixtures are presented in Table 1. It should be noted that the available original mix-design records do not specify the mass dosage of the basalt coarse aggregate or the individual proportions of the premixed dry powder constituents. These values are therefore not estimated in the present study.
Table 1. Mix Design Proportions of CA-UHPC (kg/m3).
To characterize the mechanical properties of CA-UHPC, companion specimens were prepared from the same batches during casting. In accordance with the Chinese national standard GB/T 31387-2015 [23], three 100 mm × 100 mm × 100 mm cubic specimens and three 100 mm × 100 mm × 300 mm prismatic specimens were prepared for each mixture. The mean cubic compressive strength, mean axial tensile strength, and elastic modulus were determined through the corresponding mechanical tests. The measured results are summarized in Table 2. The exact ages at which these companion specimens were tested were not documented in the available records. Accordingly, the values in Table 2 are reported as the measured material properties, without assigning a specific testing age.
Table 2. Mechanical Properties of CA-UHPC Materials.
The perforated steel plates were manufactured from Q345B structural steel, while HRB400 steel was used for the transverse reinforcement. ML15 steel was used for the headed studs in the reference specimens. The mechanical properties of these steel materials are presented in Table 3.
Table 3. Mechanical Properties of Steel Materials.
The absence of the coarse aggregate dosage and detailed premixed-powder proportions limits the reproducibility of the mixture designs and prevents an independent evaluation of the influence of coarse aggregate content on the mechanical properties of CA-UHPC.

2.2. Specimen Design, Fabrication, and Test Parameters

The PBL specimens adopted a single-hole embedded-plate configuration. The specimen configurations were selected to correspond to the nominal configurations used in the previous static push-out test program [16], thereby enabling comparison between the post-sustained-loading results and the corresponding short-term reference results. The nominal dimensions of each CA-UHPC block were 300 mm × 300 mm × 150 mm. To facilitate load application and prevent local buckling, a 20-mm-thick loading plate was welded to the upper end of the perforated steel plate, and stiffening ribs were welded to both sides of the plate. In addition, a foam insert measuring 20 mm × 50 mm × 300 mm was attached to the lower end of the steel plate to form a reserved slot, thereby simulating a non-bearing condition at the plate end.
The main geometric parameters of the PBL connectors included perforated steel plate thicknesses of 12 and 20 mm and hole diameters of 40 and 50 mm. In the reinforced configurations, an HRB400 transverse reinforcing bar with a diameter of 16 mm passed through the hole in the perforated steel plate. The unreinforced configuration was fabricated without transverse reinforcement.
For comparison, the headed-stud reference specimens consisted of four ML15 headed studs symmetrically welded to both sides of a 12-mm-thick steel plate. Each stud had a diameter of 16 mm and a length of 50 mm, with a spacing of 60 mm between the studs. The geometries and principal dimensions of the PBL and headed-stud specimens are illustrated in Figure 1.
Figure 1. Geometries of push-out specimens (dimensions in mm): (a) PBL connector specimen; (b) headed-stud specimen.
The detailed configurations and experimental parameters of the six sustained-loading specimens are summarized in Table 4.
Table 4. Parameters of Sustained Loading Push-out Specimens.
The specimen nomenclature is defined as follows. The prefix “C” denotes a sustained-loading specimen. For PBL specimens, “D” and “R” represent the thickness of the perforated steel plate and the hole diameter, respectively. The letter “Y” indicates the presence of a 16-mm-diameter transverse reinforcing bar, whereas “W” indicates its absence. The suffix “L” identifies the C120 CA-UHPC mixture, while specimens without this suffix use C140 CA-UHPC. For the headed-stud specimens, “SD” represents the steel plate thickness, and “60” denotes the spacing between the studs in millimetres.
During specimen fabrication, the perforated steel plates and transverse reinforcing bars were positioned within the formwork before concrete casting. The CA-UHPC was subsequently poured into the formwork and compacted using a vibrating rod. After casting, the specimens were covered with plastic film and demoulded after 24 h.
The demoulded specimens were then subjected to steam curing. The temperature was increased from ambient conditions to 90 °C at a rate of 10 °C/h and maintained at 90 ± 2 °C for 48 h. Subsequently, the temperature was reduced at a rate of 10 °C/h until the temperature difference between the specimen surface and the surrounding environment was no greater than 20 °C. The relative humidity during curing was maintained above 95%. The long-term push-out specimens followed the same steam-curing procedure as the static push-out specimens reported in [16].
For the subsequent ultimate push-out tests, two dial gauges with a graduation interval of 0.01 mm were arranged on opposite sides of each specimen. Their magnetic bases were fixed to the upper steel plate, while the measuring tips contacted angle sections bonded to the concrete surfaces. The average of the two readings was adopted as the relative interfacial slip.
The short-term reference results used in this study were obtained from the previous push-out test program reported in [16]. The two experimental programs involved corresponding nominal specimen configurations and CA-UHPC strength grades. However, they were conducted as separate test series, and the available records do not establish identical casting batches, curing histories, or testing ages. Accordingly, the short-term results are used as reference data for comparison rather than as matched-age unloaded controls.

2.3. Loading and Testing Scheme

The sustained-loading tests were conducted at the laboratory of the Hexian Branch of Jiangsu Xingou Intelligent Manufacturing Technology Co., Ltd. The six long-term specimens represented six different configurations, with one specimen tested for each configuration (n = 1). The specimens were divided into three loading groups, with two specimens in each group. For each pair, the sustained load was determined as 30% of the average short-term ultimate shear capacity of the two specimens, and the same sustained load was applied to both specimens. Because the short-term ultimate shear capacities of the paired specimens differed, their actual individual sustained-load ratios were not necessarily 30%, as reported in Table 5. The nominal 30% level was adopted as an experimental loading protocol, following previous long-term connector studies [9,14], rather than being derived from a specific bridge design load combination.
Table 5. Sustained-loading parameters and individual load ratios of the specimens.
The sustained-loading period lasted 180 days. The exact concrete ages at the beginning of sustained loading and at the subsequent ultimate push-out tests were not documented in the available experimental records. Therefore, the 180-day period reported herein refers only to the sustained-loading duration rather than the total concrete age. A Naerde concrete shrinkage testing apparatus equipped with a hydraulic jack was used to apply the sustained load. Each specimen was placed vertically on the lower bearing platform and positioned centrally between the upper and lower loading plates. One dial gauge with a graduation interval of 0.001 mm was installed on each specimen to monitor the relative displacement between the steel plate and the CA-UHPC. The readings from this single monitoring point were used directly to determine the time-dependent slip increments, without averaging measurements from multiple monitoring points. Readings were recorded daily during the first 30 days and once a week from day 31 to day 180. The sustained-loading arrangement is illustrated in Figure 2.
Figure 2. Sustained-loading push-out test setup.
Before formal loading, the specimen alignment was checked to ensure proper contact with the loading plates. The hydraulic jack was positioned centrally between the two loading plates and connected to the hydraulic pump. After the hydraulic system was checked, a preliminary loading operation was performed to verify the alignment of the loading arrangement. During formal loading, the pressure-sensor reading was monitored to control the applied load. Once the prescribed load was reached, the jacking operation was stopped, and the fastening nuts on the second loading plate were tightened to mechanically lock the loading system. The initial reading of the dial gauge was then recorded, after which the hydraulic jack and hydraulic pump were removed. The maximum rated load capacity of the sustained-loading apparatus was 1500 kN.
The sustained load was therefore introduced using a hydraulic jack and maintained through the mechanical locking arrangement. It should be noted that the available experimental records document the load reading during the initial loading and locking process but do not provide subsequent force measurements throughout the 180-day period. Consequently, possible variations in the sustained force after mechanical lock-off cannot be independently quantified. The loads listed in Table 5 represent the prescribed loads applied at the beginning of the sustained-loading period.
All sustained-loading tests were conducted in the laboratory. However, continuous records of ambient temperature and relative humidity during the 180-day loading period were not available. Therefore, the environmental conditions could not be quantitatively characterized, and no specific temperature or humidity ranges are reported in this study.
After 180 days of sustained loading, the mechanical locking arrangement was released, and the specimens were unloaded before the ultimate push-out tests. The subsequent tests were conducted using a 3000-kN (300-t) microcomputer-controlled testing machine manufactured by Shanghai Hualong Testing Instruments Co., Ltd. Before formal loading, three loading–unloading cycles between 0 and 10 kN were applied to eliminate local contact gaps and ensure proper alignment. After completing the three preloading–unloading cycles, the load was returned to zero, and both dial gauges were reset to zero before formal loading. Therefore, the relative slip recorded during the subsequent ultimate push-out test was measured incrementally from this re-zeroed reference state. The residual slip accumulated during the preceding 180-day sustained-loading period was not included in the load–slip curves obtained from the ultimate push-out tests. During the test, the relative interfacial slip was calculated as the average of the readings from two dial gauges installed on opposite sides of the specimen, each with a graduation interval of 0.01 mm.
The formal loading procedure consisted of two stages. Before reaching the peak load, force-controlled loading was applied at a rate of 2 kN/s. After reaching the peak load, the testing system was switched to displacement control at a rate of 0.2 mm/min. When the relative interfacial slip exceeded 2 mm, the displacement rate was increased to 0.5 mm/min. The test was terminated when the residual load capacity decreased to 50% of the ultimate load.

3. Time-Dependent Evolution of Interfacial Slip

Figure 3 illustrates the time-dependent development of interfacial slip between the steel plate and CA-UHPC during the 180-day sustained-loading period. To distinguish the initial relative slip from the subsequent time-dependent deformation, the relative slip recorded on the first day of loading was taken as the reference value. The cumulative time-dependent slip increment at each subsequent observation point represents the increase in relative slip compared with this initial reading. Accordingly, the reported values at 30 and 180 days refer to cumulative time-dependent slip increments rather than the total relative slip or the additional slip developed exclusively between these two observation points. The additional slip increment from day 30 to day 180 was obtained from the difference between the cumulative increments recorded at these two time points. The corresponding percentage increase was evaluated using the day-30 cumulative increment as the reference.
Figure 3. Time histories of relative slip.
The measured results indicate that interfacial slip developed nonlinearly during sustained loading, with a relatively rapid increase during the initial stage followed by a gradual reduction in the rate of development. The proportion of the 180-day cumulative slip increment accumulated during the first 30 days varied among the five PBL configurations, ranging from approximately 53.3% to 93.8%. This variation indicates that the temporal distribution of slip development was dependent on the specimen configuration. The measurements recorded at 60, 90, 120, and 150 days further illustrate the progressive development of interfacial slip, as shown in Figure 3. The curves generally became flatter as the loading duration increased. However, the differences among specimen configurations indicate that the slip development cannot be characterized by a single uniform time-dependent pattern. Therefore, the measured results are discussed according to the individual specimen configurations and the corresponding observation periods.
It should be emphasized that the 180-day observation period represents the experimental duration of the present study rather than the full service life of practical steel–CA-UHPC composite structures. Although the measured curves generally exhibited a decreasing slip development rate during the later loading stage, the differences among specimen configurations indicate that the time-dependent slip development was not governed by a single uniform pattern. Therefore, the observations obtained within 180 days provide a comparative assessment of interfacial slip evolution under the investigated sustained-loading conditions, but are insufficient to establish the long-term deformation characteristics over the entire service life of the structures.

3.1. Analysis of the Effect of Transverse Reinforcement

As shown in Figure 3 and Figure 4, the initial relative slips of the standard specimen (C-D12-R40-Y) and the specimen without transverse reinforcement (C-D12-R40-W) were 0.242 mm and 0.266 mm, respectively. The initial slip of the specimen without transverse reinforcement was therefore 9.9% higher than that of the standard specimen.
Figure 4. Cumulative time-dependent slip increments at 30 and 180 days.
During the first 30 days of sustained loading, the cumulative time-dependent slip increments of the standard and unreinforced specimens were 0.014 mm and 0.008 mm, respectively. The latter was 42.9% lower than that of the standard specimen. By day 180, the cumulative slip increments had increased to 0.026 mm and approximately 0.015 mm, respectively. Thus, the 180-day cumulative slip increment of the unreinforced specimen was 42.3% lower than that of the standard specimen.
The additional slip increments between days 30 and 180 were 0.012 mm for the standard specimen and approximately 0.007 mm for the unreinforced specimen. When the relative increase over this period was calculated consistently using the day-30 cumulative increment as the reference, the corresponding values were 85.7% and 87.5%, respectively. The difference between these two values was only 1.8 percentage points. Therefore, the measured results do not indicate that the absence of transverse reinforcement resulted in markedly greater relative slip growth during the later loading stage.
The individual sustained-load ratios of the standard and unreinforced specimens are reported in Table 5. The unreinforced specimen also exhibited lower ultimate shear capacity and initial shear stiffness after sustained loading. Therefore, its smaller measured 180-day cumulative slip increment should be considered together with its lower post-loading shear performance.

3.2. Analysis of the Effect of Steel Plate Thickness

Regarding the effect of perforated steel plate thickness, the initial relative slip of the thicker-plate specimen (C-D20-R40-Y) was 0.229 mm, which was 5.4% lower than that of the standard specimen (C-D12-R40-Y, 0.242 mm). During the first 30 days of sustained loading, the cumulative time-dependent slip increment of the thicker-plate specimen was 0.014 mm, identical to that of the standard specimen. By day 180, its cumulative increment had increased to 0.019 mm, compared with 0.026 mm for the standard specimen. Consequently, the measured 180-day cumulative slip increment of the thicker-plate specimen was 26.9% lower than that of the standard specimen.
The additional slip increment between days 30 and 180 was 0.005 mm for the thicker-plate specimen, corresponding to a 35.7% increase relative to its day-30 cumulative increment. The applied sustained loads of the standard and thicker-plate specimens were nearly identical (143.25 and 143.37 kN, respectively), whereas their individual sustained-load ratios differed (Table 5). This difference in normalized loading should be considered when interpreting the measured slip responses.

3.3. Analysis of the Effect of Hole Diameter

A comparison of the slip evolution patterns for different hole diameters (Figure 3 and Figure 4) shows that the initial relative slip of the larger-hole specimen (C-D12-R50-Y) was 0.182 mm, which was 24.8% lower than that of the standard specimen. During the first 30 days of sustained loading, its cumulative time-dependent slip increment reached 0.016 mm, compared with 0.014 mm for the standard specimen. Based on these values, the increment of the larger-hole specimen was approximately 14.3% higher than that of the standard specimen.
By day 180, the cumulative slip increment of the larger-hole specimen had increased to 0.021 mm, representing a 19.2% reduction relative to the standard specimen (0.026 mm). The additional slip increment between days 30 and 180 was 0.005 mm, corresponding to a 31.3% increase relative to its day-30 cumulative increment.
These results show that the larger-hole specimen exhibited a lower initial slip, a higher cumulative increment during the first 30 days, and a lower cumulative increment at the end of the 180-day period. Its individual sustained-load ratio was lower than that of the standard specimen (Table 5), which should be considered when comparing their time-dependent slip responses.

3.4. Analysis of the Effect of CA-UHPC Strength

As illustrated in Figure 3 and Figure 4, the initial relative slip of the lower-strength specimen (C-D12-R40-Y-L) was 0.349 mm, which was 44.2% higher than that of the standard specimen (0.242 mm). During the first 30 days of sustained loading, its cumulative time-dependent slip increment reached 0.045 mm, representing a 221.4% increase relative to the standard specimen (0.014 mm). By day 180, the cumulative increment had increased to 0.048 mm, compared with 0.026 mm for the standard specimen. Thus, the 180-day cumulative slip increment of the lower-strength specimen was approximately 84.6% higher than that of the standard specimen.
The additional slip increment between days 30 and 180 was only 0.003 mm for the lower-strength specimen, compared with 0.012 mm for the standard specimen. Therefore, the later-stage additional increment of the lower-strength specimen was 75.0% lower than that of the standard specimen. Based on the reported values rounded to three decimal places, the cumulative increment of the lower-strength specimen increased by approximately 6.7% from day 30 to day 180. This indicates that most of its measured time-dependent slip increment had accumulated during the first 30 days of sustained loading.
The individual sustained-load ratios of the lower-strength and standard specimens are reported in Table 5. The interpretation of the small additional slip increment measured between days 30 and 180 should also consider the measurement limitations discussed in Section 3.5.

3.5. Limitations of Long-Term Slip Measurements

The measurement resolution should be considered when interpreting the time-dependent slip results. In this study, a dial gauge with a graduation interval of 0.001 mm was used to monitor the relative slip during the 180-day sustained-loading period. The reported cumulative slip increments ranged from approximately 0.006 to 0.048 mm, corresponding to 6–48 scale divisions. However, some additional slip increments calculated between individual observation points were smaller. For example, the additional increment of 0.003 mm measured for the lower-strength specimen between days 30 and 180 corresponds to only three scale divisions.
Assuming that each dial-gauge reading was rounded to the nearest graduation, the theoretical quantization error of an individual reading is approximately ±0.0005 mm. Accordingly, the maximum quantization contribution to the difference between two readings is approximately ±0.001 mm. This estimate represents only the theoretical quantization component and should not be interpreted as the overall measurement accuracy. The available experimental records do not provide sufficient information to quantify additional uncertainty arising from instrument calibration, reading repeatability, or possible environmental and apparatus-related influences. Furthermore, only one monitoring point was used for each specimen, and no independent reference measurements or continuous environmental records were available. Consequently, the total measurement uncertainty and possible differences in slip between the two sides of each specimen could not be independently evaluated.
Therefore, although the cumulative slip increments were distinguishable within the nominal resolution of the instrument, very small differences between individual observation points and specimen configurations should be interpreted cautiously. In particular, the percentage increase calculated from the 0.003 mm later-stage increment should be regarded as approximate rather than as a highly precise measurement. The results are therefore considered indicative experimental observations rather than statistically conclusive effects of individual structural parameters. Further investigations using calibrated displacement sensors, multiple monitoring points, independent reference measurements, and environmental compensation are necessary to improve the reliability of long-term slip measurements.

4. Ultimate Shear Capacity and Failure Tests

4.1. Main Experimental Results

Table 6 summarizes the ultimate shear capacities, slip at peak load, secant shear stiffnesses, and observed failure modes of the specimens after 180 days of sustained loading. The ultimate shear capacity, Pu, is defined as the maximum load recorded during the push-out test, while Su is defined as the relative slip corresponding to Pu, representing the slip at peak load. This relationship can be expressed as
S u = s P = P u ,
Table 6. Results of Push-out Test.
The initial shear stiffness is evaluated using the secant slope of the load–slip curve at a relative slip of 0.2 mm, expressed as
K s , 0.2 = P 0.2 0.2 ,
where KS=0.2 is the secant shear stiffness at 0.2 mm slip (kN/mm), and P0.2 is the load corresponding to a relative slip of 0.2 mm (kN). The relative slip is measured from the re-zeroed reference state described in Section 2.3. The same definition and calculation procedure are used for the short-term static reference results reported in [16] to ensure consistency in the comparison. It should be noted that the residual slip accumulated during the preceding 180-day sustained-loading period was excluded from the subsequent load–slip curves because the dial gauges were reset to zero before the ultimate push-out tests. Consequently, Ks,0.2 represents the incremental secant stiffness measured during the subsequent push-out test and does not incorporate the slip accumulated during sustained loading. Although resetting the gauges changes the displacement reference origin rather than directly altering the subsequent incremental load–slip response, the reported stiffness should be interpreted as the post-sustained-loading incremental stiffness rather than a measure incorporating the entire deformation history. This distinction should be considered when comparing the present results with the short-term reference data. Compared with the short-term static test results, the main failure characteristics of the specimens after sustained loading remained generally consistent.
The internal failure morphologies of the five PBL specimens are presented in Figure 5. These photographs provide further details of the concrete dowel, transverse reinforcement, steel fibers, and steel plate around the perforations after the ultimate push-out tests. The following discussion focuses on the visible failure characteristics of each specimen. It should be noted that these post-test observations represent the final failure conditions and do not directly reveal the progressive development of internal damage during the sustained-loading period.
Figure 5. Post-test internal failure morphologies of the PBL specimens after 180 days of sustained loading: (a) C-D12-R40-Y; (b) C-D12-R40-W; (c) C-D20-R40-Y; (d) C-D12-R50-Y; and (e) C-D12-R40-Y-L. For each specimen, the left image shows the concrete side and the right image shows the steel-plate side.
Following the push-out test, the internal failure morphology of specimen C-D12-R40-Y is shown in Figure 5a. On the concrete side, crushing is visible in the upper portion of the concrete dowel. The transverse reinforcing bar exhibits slight bending before fracture, without obvious necking at the fracture section. On the steel-plate side, numerous steel fibers are visible around the concrete dowel and at the interface. Meanwhile, no pronounced deformation of the upper wall of the steel plate hole can be identified. These observations indicate that the final failure involved both the crushing of the concrete dowel and the shear fracture of the transverse reinforcement.
The internal failure morphology of specimen C-D12-R40-W is shown in Figure 5b. In the absence of transverse reinforcement, the concrete dowel was sheared off, accompanied by pronounced steel-fiber pull-out from the exposed fracture surface. No obvious deformation of the upper wall of the steel plate hole was observed. These features indicate that the failure of this specimen was predominantly associated with shear fracture of the concrete dowel, without the additional contribution of transverse reinforcement.
The internal failure morphology of specimen C-D20-R40-Y is illustrated in Figure 5c. The transverse reinforcing bar was fractured without significant visible bending deformation, while the upper portion of the concrete dowel exhibited crushing. A slight local deformation of the steel plate is also visible. Although relatively few steel fibers appear in the exposed interfacial region, no quantitative measurements of fiber distribution were conducted. Therefore, the observed appearance alone is insufficient to establish fiber segregation as the cause of the relatively low shear capacity of this specimen.
The internal failure morphology of specimen C-D12-R50-Y is presented in Figure 5d. The transverse reinforcing bar exhibited noticeable bending deformation, accompanied by necking near the fracture section. Crushing was also observed in the upper portion of the concrete dowel, while steel fibers remained visible on the exposed surfaces. These observations suggest that the final failure involved both deformation and fracture of the transverse reinforcement and local crushing of the concrete dowel.
For specimen C-D12-R40-Y-L, the internal failure morphology is shown in Figure 5e. Severe crushing and spalling were observed in the upper portion of the concrete dowel. The fractured transverse reinforcing bar was located close to the wall of the steel plate hole in the final failure state. It should be noted that this specimen was made with the C120 mixture, which differed from the C140 mixture not only in compressive strength but also in steel-fiber dosage and other mixture proportions. Therefore, the observed failure characteristics cannot be attributed exclusively to the reduction in concrete strength.
Overall, the internal failure morphologies show that the presence of transverse reinforcement was associated with different final failure characteristics. Without transverse reinforcement, the concrete dowel exhibited predominantly shear fracture, whereas the reinforced specimens generally exhibited a combination of concrete crushing and transverse reinforcement fracture. These observations provide qualitative evidence of the different failure characteristics of the specimens after sustained loading. However, they do not establish the detailed evolution of internal damage during the 180-day loading period.

4.2. Load–Slip Responses of Specimens After Sustained Loading

Figure 6 illustrates the ultimate load–slip curves of the specimens after 180 days of sustained loading. Compared with the short-term reference results reported in [16], the overall shapes of the load–slip curves were broadly similar. However, the post-sustained-loading specimens exhibited lower ultimate shear capacities and initial shear stiffnesses than the corresponding short-term reference specimens. The failure responses also differed between specimens with and without transverse reinforcement. For the specimen without transverse reinforcement, the load–slip curve showed a sharp post-peak load drop. The curve lacked a distinct gradual descending branch, indicating a typical brittle failure. In contrast, the load–slip curves of the specimens with transverse reinforcement exhibited three discernible stages: the elastic section, the strengthening section, and the platform section.
Figure 6. Overall load–slip curves of the specimens.
During the initial elastic section, the load–slip curves of the specimens with transverse reinforcement exhibited an approximately linear increase in load, indicating relatively high initial stiffness. At a relative slip of approximately 0.5 mm, the applied load reached about 80% of the corresponding ultimate capacity. With further increases in relative slip, the specimens entered the strengthening section, during which the load continued to increase toward the peak value. The relative slip corresponding to the peak load varied among the specimens rather than occurring at a common value, as summarized in Table 6. After reaching the peak load, the specimens with transverse reinforcement generally exhibited a more gradual post-peak response, corresponding to the platform section in Figure 6. In contrast, the specimen without transverse reinforcement showed a sharp post-peak load drop. The final failure morphologies shown in Figure 5 revealed concrete crushing and transverse reinforcement fracture in the reinforced specimens. These observations may help explain the differences in the post-peak responses. However, the load–slip curves and post-test failure morphologies do not directly reveal the sequence of internal damage development during loading. Therefore, the three stages are used to describe the observed macroscopic load–slip responses rather than to represent directly measured internal damage processes.
To quantify the deformation response, the slip corresponding to the peak load (Su) was compared among the six specimens. As summarized in Table 6, Su ranged from 0.53 to 1.52 mm. Specifically, the PBL specimens exhibited peak-load–slip values ranging from 0.53 to 1.31 mm, whereas the headed-stud reference specimen exhibited a value of 1.52 mm. These values represent the measured slip at peak load rather than the slip capacity evaluated in accordance with Annex B of EN 1994-1-1 [24].
In addition to the peak-load–slip Su, the post-peak deformation response was further characterized by the slip corresponding to 90% of the peak load on the descending branch S0.9Pu, which is defined as
S u 0.9 Pu = s P = 0.9 P u ,
This parameter was determined by linear interpolation between two adjacent experimental data points bracketing the 90% peak-load threshold:
S 0.9 Pu = S 1 + 0.9 P u − P 1 P 2 − P 1 S 2 − S 1 ,
where P1 and P2 are the loads at two adjacent data points on the descending branch, and S1 and S2 are their corresponding relative slips. Pu is taken from Table 6. For each specimen, the value of Pu was obtained from the ultimate shear capacity reported in Table 6. When the load did not decrease to 90% of Pu within the recorded slip range, the corresponding S0.9Pu value was designated as NR. Notably, the load–slip responses of specimens C-D12-R40-Y and C-D20-R40-Y exhibited partial load recovery after the initial post-peak decline. Consequently, the 90% peak-load threshold was reached only at a relatively large slip on the subsequent descending branch, resulting in the relatively large S0.9Pu values reported in Table 6.

4.3. Comparison of Post-Sustained-Loading Mechanical Performance with Short-Term Reference Results

To evaluate the impact of sustained loading on the ultimate shear capacity of PBL connectors, this study compared the experimental data between long-term sustained loading and conventional short-term static loading, as illustrated in Figure 7. Detailed comparisons of the shear capacities and shear stiffnesses are presented in Table 7 and Table 8.
Figure 7. Comparison of load–slip curves of the specimens: (a) C-D12-R40-Y; (b) C-D12-R40-W; (c) C-D12-R50-Y; (d) C-D20-R40-Y; (e) C-D12-R40-Y-L; and (f) C-SD12-60.
Table 7. Shear capacity comparison.
Table 8. Comparison of initial shear stiffness.
A comprehensive analysis combining Figure 5b and Figure 6, and Table 7 and Table 8 shows that the ultimate shear capacity and initial shear stiffness of the specimen without transverse reinforcement (C-D12-R40-W) were 26.8% and 25.6% lower, respectively, than the corresponding short-term reference values reported in [16]. The post-test failure morphology shown in Figure 5b reveals that the concrete dowel was sheared off, indicating that the concrete dowel region played a major role in the ultimate shear resistance of this specimen. In the absence of transverse reinforcement, the concrete dowel and the surrounding concrete shear zone appear to provide the primary resistance against the applied shear force. This failure pattern is consistent with the relatively brittle response observed in the load–slip curve. However, since the internal stress distribution and damage evolution were not monitored during the sustained-loading period, the specific process of damage accumulation cannot be directly established from the present experimental results.
Compared with the corresponding short-term reference results, the ultimate shear capacity and initial shear stiffness of the standard specimen (C-D12-R40-Y) were 12.9% and 5.9% lower, respectively. As shown by the post-test failure morphology in Figure 5a, bending and subsequent shearing-off of the transverse reinforcement occurred together with crushing of the upper portion of the concrete dowel. These observations suggest that both the transverse reinforcement and the concrete dowel contributed to the ultimate shear resistance of the specimen. The observed failure characteristics are consistent with a load-transfer mechanism involving the concrete dowel shear zone, the upper concrete compression zone, and the transverse reinforcement. However, the individual contributions of these components and their internal stress distributions during sustained loading were not directly measured. Therefore, the proposed load-transfer mechanism should be regarded as a qualitative interpretation based on the observed failure morphology and macroscopic mechanical response.
For specimen C-D12-R50-Y, the ultimate shear capacity and initial shear stiffness decreased by 9.4% and 14.5%, respectively. Compared with the standard specimen, the reduction in ultimate shear capacity was smaller, whereas the reduction in initial shear stiffness was more pronounced. The post-test failure morphology shown in Figure 5d revealed bending and necking of the transverse reinforcing bar, together with crushing in the upper portion of the concrete dowel. These observations suggest that both the transverse reinforcement and the concrete dowel were involved in the final failure process. Although an increase in hole diameter changes the geometry of the concrete dowel and may affect the local bearing conditions, the present tests did not directly measure the internal stress distribution or local deformation around the hole. Furthermore, the individual sustained-load ratio of the larger-hole specimen was 24.35%, compared with 32.34% for the standard specimen. Therefore, the observed differences in capacity and stiffness reduction should be interpreted as specimen-specific responses under the adopted loading conditions, rather than direct evidence that increasing the hole diameter mitigates the effects of sustained loading on shear capacity.
Specimen C-D20-R40-Y exhibited a 4.1% reduction in ultimate shear capacity and an 18.3% reduction in initial shear stiffness relative to its short-term results. However, its short-term and post-loading ultimate shear capacities were 366.9 kN and 352.0 kN, respectively, both lower than those of the standard specimen (442.9 kN and 385.6 kN, respectively). Therefore, the smaller percentage reduction does not indicate a higher absolute shear capacity. The individual sustained-load ratios of these specimens differed (Table 5) and should be considered when interpreting the measured reductions.
The ultimate shear capacity and initial shear stiffness of specimen C-D12-R40-Y-L decreased by 6.4% and 18.6%, respectively. The post-test failure morphology shown in Figure 5e revealed severe crushing and spalling in the upper portion of the concrete dowel, while the fractured transverse reinforcing bar was located close to the wall of the steel plate hole. These observations indicate that concrete crushing and transverse reinforcement fracture were both present in the final failure state. The post-test morphology represents the final failure state and cannot establish the location or progression of damage during the 180-day sustained-loading period. Although the transverse reinforcement may have contributed to the ultimate shear resistance, its individual contribution cannot be quantified from the available results. In addition, the C120 and C140 mixtures differed in steel-fiber dosage and other mixture proportions (Table 1). Therefore, the observed differences represent a comparison between two CA-UHPC mixture designs rather than the isolated effect of compressive strength.
In addition, the ultimate shear capacity and initial shear stiffness of the headed-stud reference specimen were 15.5% and 9.6% lower, respectively, than the corresponding short-term reference values after sustained loading. For comparison, the corresponding reductions for the standard PBL specimen were 12.9% and 5.9%, respectively. Thus, the relative reductions measured for the headed-stud specimen were numerically greater than those observed for the standard PBL specimen. This comparison is limited to the specific specimens and loading conditions investigated and does not establish the general superiority of either connector type in resisting long-term performance degradation.
As illustrated schematically in Figure 8, the post-test failure morphologies and load–slip responses suggest different load-transfer characteristics for specimens with and without transverse reinforcement. For specimens without transverse reinforcement, the concrete dowel and the surrounding lower concrete shear zone appear to provide the primary resistance. In contrast, for specimens with transverse reinforcement, the ultimate shear resistance may involve the combined contributions of the upper concrete compression zone, the transverse reinforcement, and the lower concrete shear zone. This conceptual interpretation is based on the observed post-test failure morphologies and macroscopic mechanical responses. Since the internal stress distribution and damage evolution were not directly monitored during the sustained-loading period, the proposed mechanism should be regarded as a qualitative interpretation rather than a directly verified description of the internal damage process.
Figure 8. Conceptual schematic of the proposed load-transfer mechanism and possible damage zones under sustained loading.
The relative differences in shear capacity and initial shear stiffness presented in Table 7 and Table 8 are calculated with respect to the short-term reference results reported in [16]. Since the two test series were not conducted using matched-age loaded and unloaded companion specimens, these differences should be interpreted as comparisons between the two experimental programs. Nevertheless, they provide a basis for evaluating the mechanical performance of the specimens after 180 days of sustained loading relative to the corresponding short-term reference results.

4.3.1. Analysis of the Effect of Transverse Reinforcement

The comparison of the ultimate load–slip curves for specimens with and without transverse reinforcement after long-term sustained loading is illustrated in Figure 9. Combining these results with the internal failure morphologies in Figure 5a,b, the two configurations exhibit different load-transfer characteristics.
Figure 9. Comparison of long-term shear performance with and without transverse reinforcement: (a) load–slip curves; (b) ultimate shear capacity; and (c) initial shear stiffness.
In the short-term static tests reported in [16], the ultimate shear capacity and initial shear stiffness of the specimen without transverse reinforcement were 34.5% and 28.8% lower than those of the standard specimen, respectively. After 180 days of sustained loading, the corresponding differences increased to 44.9% and 43.8%, respectively. Specifically, the unreinforced specimen exhibited an ultimate shear capacity of 212.3 kN and an initial shear stiffness of 600.0 kN/mm, compared with 385.6 kN and 1067.1 kN/mm for the standard specimen.
These comparisons indicate that the specimen without transverse reinforcement exhibited lower shear capacity and stiffness under both short-term and sustained-loading conditions. The larger differences observed in the post-sustained-loading comparison indicate a greater disparity between the two configurations under the adopted test conditions. However, these differences cannot be attributed solely to sustained-loading-induced degradation.

4.3.2. Analysis of the Effect of Perforated Steel Plate Thickness

A comparison of the short-term and long-term mechanical properties shows that the short-term ultimate shear capacity of the thicker-plate specimen (C-D20-R40-Y) was 366.9 kN, which was 17.2% lower than that of the standard specimen (C-D12-R40-Y, 442.9 kN). Following 180 days of sustained loading, the ultimate shear capacity of specimen C-D20-R40-Y was 352.0 kN, corresponding to a 4.1% difference relative to the short-term reference value of 366.9 kN. In comparison, the ultimate shear capacity of the standard specimen decreased from 442.9 kN to 385.6 kN, corresponding to a reduction of 12.9%. Consequently, the difference in ultimate shear capacity between the two specimens decreased from 17.2% under short-term static loading to approximately 8.7% after sustained loading (Figure 10).
Figure 10. Comparison of Long-term Shear Performance with Varying Steel Plate Thickness: (a) Load–slip Curves; (b) Ultimate Shear Capacity; (c) Initial Shear Stiffness.
In terms of initial shear stiffness, the short-term value of C-D20-R40-Y was 1364.1 kN/mm, which was 20.3% higher than that of the standard specimen (1133.8 kN/mm). After sustained loading, its initial shear stiffness decreased to 1114.1 kN/mm, corresponding to a reduction of 18.3%. By comparison, the initial shear stiffness of the standard specimen decreased from 1133.8 to 1067.1 kN/mm, corresponding to a reduction of 5.9%. Therefore, the thicker-plate specimen exhibited a smaller reduction in ultimate shear capacity but a greater reduction in initial shear stiffness.
The applied sustained loads of C-D20-R40-Y and D12-R40-Y were nearly identical, at 143.37 and 143.25 kN, respectively, whereas their individual sustained-load ratios differed (Table 5). This difference in normalized loading should be considered when interpreting the measured changes in shear capacity and initial stiffness.

4.3.3. Analysis of the Effect of Hole Diameter

A comparison of the mechanical properties of specimens with different hole diameters shows that the short-term ultimate shear capacity and initial shear stiffness of the larger-hole specimen (C-D12-R50-Y) were 33.0% and 8.0% higher than those of the standard specimen, respectively(Figure 11).
Figure 11. Comparison of Long-term Shear Performance with Varying Hole Diameter: (a) Load–slip Curves; (b) Ultimate Shear Capacity; (c) Initial Shear Stiffness.
After 180 days of sustained loading, the ultimate shear capacity of the larger-hole specimen reached 533.4 kN, which was 38.3% higher than that of the standard specimen (385.6 kN). However, its initial shear stiffness was 1047.0 kN/mm, approximately 1.9% lower than that of the standard specimen (1067.1 kN/mm).
The relative reductions for the larger-hole specimen were 9.4% in ultimate shear capacity and 14.5% in initial shear stiffness, compared with 12.9% and 5.9%, respectively, for the standard specimen.
These results indicate that the larger-hole specimen exhibited a smaller reduction in ultimate shear capacity but a greater reduction in initial shear stiffness than the standard specimen. The individual sustained-load ratios of the larger-hole, thicker-plate, and standard specimens are reported in Table 5. Considering these differences, the present results do not establish a definitive ranking between increasing hole diameter and increasing steel plate thickness in terms of long-term mechanical performance.

4.3.4. Analysis of the Effect of CA-UHPC Matrix Strength

The comparison of the mechanical properties of the C120 and C140 specimens should be interpreted in consideration of their different mixture proportions. As presented in Table 1, the two mixtures differ in cement content, premixed dry powder content, steel fiber dosage, sand content, water-reducing admixture dosage, and water content. Their measured mean cubic compressive strengths were 146.3 MPa and 163.4 MPa, respectively.
In the short-term static comparison, the ultimate shear capacity and initial shear stiffness of the C120 specimen (C-D12-R40-Y-L) were 273.0 kN and 492.0 kN/mm, respectively, which were 38.4% and 56.6% lower than those of the C140 standard specimen (442.9 kN and 1133.8 kN/mm) (Figure 12).
Figure 12. Comparison of Long-term Shear Performance with Varying CA-UHPC Strength: (a) Load–slip Curves; (b) Ultimate Shear Capacity; (c) Initial Shear Stiffness.
After 180 days of sustained loading, the corresponding values for the C120 specimen decreased to 255.6 kN and 400.5 kN/mm, whereas those of the standard specimen were 385.6 kN and 1067.1 kN/mm. Consequently, the differences in ultimate shear capacity and initial shear stiffness between the two specimens were 33.7% and 62.5%, respectively.
The relative reductions for the C120 specimen were 6.4% in ultimate shear capacity and 18.6% in initial shear stiffness. By comparison, the corresponding reductions for the C140 standard specimen were 12.9% and 5.9%, respectively.
These results indicate that although the C120 specimen exhibited substantially lower absolute shear capacity and stiffness, its relative reduction in ultimate shear capacity was smaller than that of the C140 specimen. Conversely, its reduction in initial shear stiffness was considerably greater. Therefore, the present results do not support the general conclusion that increasing the concrete strength grade necessarily reduces the degradation of both shear capacity and stiffness.
Furthermore, because the two CA-UHPC mixtures differed in several compositional parameters, the observed differences cannot be attributed solely to compressive strength. Accordingly, the results should be interpreted as a comparison between two CA-UHPC mixture designs with different strength grades.

4.4. Engineering Implications and Applicability of the Experimental Findings

The experimental results provide several implications for the design and evaluation of PBL connectors in steel–CA-UHPC composite structures. Under the adopted test conditions, the ultimate shear capacity and initial shear stiffness of the specimen without transverse reinforcement differed from the corresponding short-term reference values by 26.8% and 25.6%, respectively. The corresponding differences for the standard specimen were 12.9% and 5.9%, respectively. These comparisons indicate that the differences relative to the short-term reference were larger for the specimen without transverse reinforcement. However, because only one specimen was tested for each configuration and the individual sustained-load ratios were not identical, this observation should be regarded as a specimen-specific trend rather than an isolated effect of transverse reinforcement. In addition, the effects of geometric parameters on shear capacity and initial stiffness were not consistent, indicating that these two performance indicators should be considered separately in connector design and evaluation.
From the perspective of shear-capacity evaluation, the equation specified in JTG D64-2015 [25] provided relatively close estimates of the short-term reference shear capacities for most of the investigated CA-UHPC PBL configurations in the preceding static push-out tests. The present comparisons further show that the differences between post-sustained-loading results and short-term reference values were not identical for shear capacity and stiffness. Therefore, the assessment of PBL connectors subjected to sustained loading should consider not only their initial static resistance but also their measured mechanical response following sustained loading. The findings provide comparative experimental data for understanding the mechanical behavior of PBL connectors in CA-UHPC under the adopted experimental conditions.
These observations can be considered alongside previous long-term connector studies. Zhang et al. [9] investigated the time-dependent responses of PBL connectors under sustained loading, including interfacial slip, transverse reinforcement strain, and stress around the perforations. Wen et al. [14] reported rapid initial slip development followed by gradual stabilization in headed-stud connections, a temporal development pattern also observed in the present study. Because the connector types, cementitious materials, and experimental configurations differ, these comparisons are qualitative and are not intended to establish direct quantitative equivalence.
An important limitation in interpreting the present findings is the absence of matched-age unloaded companion specimens. Although the short-term reference results were obtained from corresponding nominal specimen configurations, differences in casting batches, curing histories, and testing ages could not be excluded. Differences in concrete age at testing may have affected the measured material properties of CA-UHPC and, consequently, the shear capacity and stiffness. This potential influence cannot be independently quantified because the exact testing ages and matched-age unloaded controls were unavailable. In addition, each long-term specimen configuration was represented by only one specimen, and the paired-loading protocol resulted in different individual sustained-load ratios (Table 5). Although the sustained loads were determined based on 30% of the average short-term ultimate shear capacity of each specimen pair, the actual load ratios of individual specimens were not necessarily identical. The observation period was also limited to 180 days. Furthermore, continuous records of the sustained load after mechanical lock-off and continuous environmental monitoring were unavailable. Consequently, the potential contributions of material aging, shrinkage, creep, and variations in loading conditions to the observed changes in connector performance cannot be independently quantified.
Considering these limitations, the present experimental dataset, comprising six specimens with one specimen per configuration, a single nominal sustained-load ratio, and an observation period of 180 days, does not provide sufficient information for reliable calibration and independent validation of a generalized predictive model. Therefore, the present study focuses on comparative experimental observations rather than developing a predictive model or extrapolating the results beyond the investigated observation period. Future investigations should incorporate unloaded companion specimens from the same casting batches, maintained under identical environmental conditions and tested at the same age, together with matched sustained-load ratios, replicated specimens, continuous monitoring of loading conditions, and extended observation periods to further clarify the long-term performance of PBL connectors.

5. Conclusions

In this study, 180-day sustained-loading tests followed by ultimate push-out tests were conducted on six CA-UHPC specimens, comprising five PBL configurations and one headed-stud reference configuration. The post-sustained-loading mechanical responses were compared with the corresponding short-term reference results, leading to the following conclusions:
  • Under sustained loading, the interfacial slip between the steel plate and CA-UHPC exhibited a relatively rapid increase during the initial stage, followed by a gradual reduction in the rate of development. When a consistent calculation basis was adopted, the relative increases in cumulative slip increments from day 30 to day 180 were 85.7% and 87.5% for the standard and unreinforced specimens, respectively, indicating no appreciable difference in their normalized later-stage slip development. Although the 180-day cumulative slip increment of the unreinforced specimen was 42.3% lower than that of the standard specimen, this observation should be interpreted in light of the paired-loading protocol described in Section 2.3 and the corresponding post-loading mechanical properties. Compared with the standard specimen, the 180-day cumulative slip increments of the larger-hole and thicker-plate specimens were 19.2% and 26.9% lower, respectively, whereas that of the lower-strength specimen was approximately 84.6% higher. These comparisons represent the measured responses under the adopted loading conditions and should not be interpreted as isolated causal effects of individual parameters.
  • After long-term sustained loading, the final failure modes of the specimens remain largely consistent with those under short-term static loading. Specimens without transverse reinforcement exhibited a typical brittle failure, primarily manifested as the shearing-off of the concrete dowels. In contrast, specimens with transverse reinforcement exhibited a more gradual post-peak load reduction, with the failure morphology jointly governed by the shearing-off of the transverse reinforcement and the crushing of the upper concrete dowels. Compared with the corresponding short-term reference results, the specimens tested after 180 days of sustained loading exhibited lower ultimate shear capacities and initial shear stiffnesses.
  • The post-test failure morphologies suggest that the load-transfer characteristics of the investigated PBL specimens differed according to the presence of transverse reinforcement. In the specimen without transverse reinforcement, the concrete dowel was predominantly sheared off, indicating that the concrete dowel and the surrounding concrete shear zone provided the main resistance in the absence of transverse reinforcement. In the specimens with transverse reinforcement, the observed combination of concrete-dowel crushing and transverse-reinforcement deformation or fracture suggests that both components contributed to the ultimate shear resistance. These observations provide a qualitative basis for interpreting the load-transfer mechanisms of the investigated specimens. However, since internal stresses and damage were not monitored during the 180-day sustained-loading period, the proposed mechanism does not establish the process of internal damage accumulation over time.
  • The effects of geometric parameters and CA-UHPC mixture design on post-sustained-loading performance were not uniform. The larger-hole and thicker-plate specimens exhibited reductions of 9.4% and 4.1% in ultimate shear capacity, respectively, while their initial shear stiffness reductions were 14.5% and 18.3%, respectively. The C120 specimen exhibited reductions of 6.4% in ultimate shear capacity and 18.6% in initial shear stiffness, compared with 12.9% and 5.9%, respectively, for the C140 standard specimen. These comparisons should be interpreted in light of the experimental limitations described in Section 2.3 and the differences in CA-UHPC mixture proportions.

Author Contributions

Conceptualization, H.C.; methodology, R.P.; validation, J.T.; formal analysis, Y.Z.; resources, H.C.; investigation, H.C.; data curation, Z.Y.; writing—original draft preparation, J.L.; writing—review and editing, Y.Z.; supervision, Z.Y.; project administration, R.P. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Data Availability Statement

The data presented in this study are not publicly available due to confidentiality restrictions associated with the company-owned experimental data.

Acknowledgments

The authors thank all the personnel who assisted with the collection and organization of the experimental data.

Conflicts of Interest

Authors Hongxu Cui, Zongxiao Yang, Runsheng Pei, and Jikang Tie were employed by Shandong Expressway Infrastructure Construction Co., Ltd. The remaining authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.

Abbreviations

The following abbreviations are used in this manuscript:
PBLperfobond leiste
CA-UHPCcoarse aggregate ultra-high performance concrete
UHPCultra-high-performance concrete
RCreinforced concrete

References

  1. Deng, J.H.; Yan, L.Z.; Zhou, Y.D.; Zhu, P. Study on the influence of interface slip and shear deformation on the long-term deflection of steel-UHPC composite beams. Chin. J. Appl. Mech. 2025, 42, 879–888. [Google Scholar]
  2. Hu, J.L. Review on the development of shear connectors in steel-concrete composite structures. Sichuan Build. Mater. 2017, 43, 62–63. [Google Scholar]
  3. Wang, W.F.; Tan, J.P.; Cao, M.H. Finite element analysis of the effect of shrinkage and creep on the interface behavior of steel-concrete composite beams. For. Eng. 2024, 40, 197–203. [Google Scholar]
  4. Al-deen, S.; Ranzi, G.; Vrcelj, Z. Long-term experiments of composite beams and connections. Mag. Concr. Res. 2012, 64, 849–861. [Google Scholar] [CrossRef] [Scilit]
  5. Fan, J.S.; Nie, J.G.; Wang, H. Study on long-term structural behavior of composite beams considering effects of shrinkage, creep and cracking (I): Tests and calculation. China Civ. Eng. J. 2009, 42, 8–15. [Google Scholar]
  6. Wang, Q.H.; Wang, S.Q.; Gu, F.; You, G.; Dai, R. Prediction method for long-term performance of two-span steel-concrete continuous composite beams considering shrinkage and creep effects. J. Archit. Civ. Eng. 2023, 40, 50–58. [Google Scholar]
  7. Chen, L.G. Analysis of shrinkage and creep effects in steel-concrete composite continuous girder bridges. Jiangxi Build. Mater. 2016, 187–190. [Google Scholar]
  8. Xue, W.C. Structural performance of prestressed composite beams under sustained loading for 1 year. Bridge Constr. 2003, 1–3, 15. [Google Scholar]
  9. Zhang, J.; Hu, X.M.; Kou, L.Y.; Zhang, B.; Jiang, Y.C.; Yu, H.H. Experimental study of the short-term and long-term behavior of perfobond connectors. J. Constr. Steel Res. 2018, 150, 462–474. [Google Scholar] [CrossRef] [Scilit]
  10. Duan, M.J.; Zhang, S.Y.; Wang, X.; Dong, F.H. Mechanical behavior in perfobond rib shear connector with UHPC-steel composite structure with coarse aggregate. KSCE J. Civ. Eng. 2020, 24, 1255–1267. [Google Scholar] [CrossRef] [Scilit]
  11. He, S.H.; Fang, Z.; Fang, Y.W.; Liu, M.; Liu, L.; Mosallam, A.S. Experimental study on perfobond strip connector in steel–concrete joints of hybrid bridges. J. Constr. Steel Res. 2016, 118, 169–179. [Google Scholar] [CrossRef] [Scilit]
  12. He, S.H.; Fang, Z.; Mosallam, A.S. Push-out tests for perfobond strip connectors with UHPC grout in the joints of steel-concrete hybrid bridge girders. Eng. Struct. 2017, 135, 177–190. [Google Scholar] [CrossRef] [Scilit]
  13. Tan, X.Y.; Fang, Z.; Xiong, X.W. Experimental study on group effect of perfobond strip connectors encased in UHPC. Eng. Struct. 2022, 250, 113424. [Google Scholar] [CrossRef] [Scilit]
  14. Wen, C.; Bradford, M.A.; Yang, G. Long-term behaviour of stud connections in composite structures. Eng. Struct. 2024, 313, 118266. [Google Scholar] [CrossRef] [Scilit]
  15. Song, R.N.; Zhan, Y.L.; Liu, F.; Zhao, R. Long-term push-out tests and finite element analysis of steel-concrete composite specimens. J. Traffic Transp. Eng. 2019, 19, 36–45. [Google Scholar]
  16. Zheng, Y.L.; Huang, C.; Qi, J.N.; Hu, Y.Q.; Wang, J.Q. Experimental Study on the Shear Performance of PBL Connectors in Steel-UHPC(CA) Composite Structures. China J. Highw. Transp. 2025, 38, 349–360. [Google Scholar] [CrossRef]
  17. Huang, Y.; Wang, J.; Wei, Q.; Shang, H.; Liu, X. Creep behaviour of ultra-high-performance concrete (UHPC): A review. J. Build. Eng. 2023, 69, 106187. [Google Scholar] [CrossRef] [Scilit]
  18. Deng, Y.S.; Li, W.J.; Meng, L.Q.; Zhang, K.; Song, Q.; Ma, E. Application research on coarse aggregate ultra-high performance concrete. Concrete 2024, 160–163. [Google Scholar]
  19. Liu, G.Q.; Kang, X. Experimental study on mechanical properties of ultra-high performance concrete containing coarse aggregate. China Build. Mater. Sci. Technol. 2024, 33, 67–71. [Google Scholar]
  20. Huang, W.R.; Yang, Y.Z.; Liu, Y.J.; Cui, T. Mechanical properties of ultra-high performance concrete containing coarse aggregate. J. Chin. Ceram. Soc. 2020, 48, 1747–1755. [Google Scholar]
  21. Miao, X.G.; Yuan, A.M.; Wang, K.; Chen, Q.; Wang, X.; Kong, H.; Wang, J. Mechanical and autogenous shrinkage properties of coarse aggregate ultra-high performance concrete (CA-UHPC): The effect of mineral admixtures. J. Build. Eng. 2024, 98, 111154. [Google Scholar] [CrossRef] [Scilit]
  22. Zhang, F.; Pang, K.; Zhong, R.; Li, J.; Liu, Q.; Zhang, J. Effect of key design parameters on the physical/mechanical properties of coarse aggregated UHPC and its structural response subjected to bending. Constr. Build. Mater. 2024, 448, 138189. [Google Scholar] [CrossRef] [Scilit]
  23. GB/T 31387-2015; Reactive Powder Concrete. Standards Press of China: Beijing, China, 2015.
  24. EN 1994-1-1:2004; Eurocode 4: Design of Composite Steel and Concrete Structures—Part 1-1: General Rules and Rules for Buildings. CEN: Brussels, Belgium, 2004.
  25. JTG D64-2015; Specifications for Design of Highway Steel Bridge. China Communications Press: Beijing, China, 2015.
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Article metric data becomes available approximately 24 hours after publication online.