Skip to Content
BuildingsBuildings
  • Article
  • Open Access

23 November 2026

40 Pages

Influence of Supplementary Cementitious Materials and Micro-Steel Fibers on 3D-Printed Concrete: Mechanical Characterization

,
,
,
,
and
1
The Graduate School of Natural and Applied Sciences, Dokuz Eylül University, 35390 İzmir, Türkiye
2
Department of Civil Engineering, Faculty of Engineering, Dokuz Eylül University, 35390 İzmir, Türkiye
3
Microlab, Section Materials and Environment, Faculty of Civil Engineering and Geosciences, Delft University of Technology, 2628 CN Delft, The Netherlands
*
Authors to whom correspondence should be addressed.
Buildings2026, 16(23), 4677;https://doi.org/10.3390/buildings16234677 
(registering DOI)
This article belongs to the Special Issue Advances in 3D-Printed Concrete: Quality Control, Structural Performance, and Sustainable Applications

Abstract

This study investigates the effects of substituting 0%, 20%, and 40% ground granulated blast-furnace slag (BFS) and fly ash (FA) for CEM I on the interlayer bond strength, anisotropy, and structural integrity of plain and micro steel-fiber-reinforced 3D-printed concrete, for mold-cast and printed samples, comparatively. Flexural, compressive, split tensile, shear bond, and direct tensile strength tests were performed. Results indicate different effects of BFS and FA in mold-cast and printed samples. Mold-cast samples exhibited higher strength than printed samples, except for flexural strength and toughness, where printing enhanced the toughness of plain and reinforced samples by up to 76% and 131% at 28 days. Micro-steel fiber addition successfully altered the failure behavior from brittle to ductile, enhancing the flexural toughness (by up to 17.8- to 19.6-fold), leading to deflection-hardening in specific printed mixtures (P-REF-F and P-BFS40-F). While BFS and FA exacerbated absolute anisotropy in plain mixtures, micro-steel fiber addition successfully reduced intra-directional anisotropy (Idir) by up to 71%, homogenizing directional mechanical performance. Furthermore, combining micro-steel fibers with optimized mix designs mitigated the strength loss caused by printing in plain mixtures. This study shows that a combination of microfibers and mix design optimization can compensate for the inherent weak flexural behavior of concrete.

1. Introduction

3D-printed concrete (3DPC) incorporating various volumes and types of supplementary cementitious materials (SCMs), as well as reinforcement agents such as reinforcing bars and microfibers, has attracted considerable interest in the field of construction materials [1,2,3]. The use of SCMs offers environmental friendliness as a viable replacement for OPC, since printable mixtures require a larger binder volume [4]. The choice of SCMs should be made with calculated intention, as each SCM affects the resulting printable mixture differently. Kaya et al. comparatively investigated the effects of FA and BFS at 20%, 40%, and 60% by weight on the rheological and printability properties of 3D-printable plain mortars (3DPPM). They found that FA and BFS affected the fresh and rheological properties of 3DPPM differently. They found that while FA decreased the green strength and lengthened the printability window, BFS enhanced the green strength and narrowed the printability window compared with mixtures containing OPC as the sole binder [5]. Panda and Tan investigated the effect of silica fume on the rheological properties of ternary printable mortars containing high volumes of fly ash. They reported an increase in yield stress and buildability by silica fume [6]. Muthukrishnan et al. reported that substituting 20% of OPC with rice husk ash improved the compressive and shear bond strength of fresh plain printable concrete [7]. Although the feasibility of using various SCMs in 3DPC has been extensively studied, most studies have focused on the effects of these SCMs on the rheological and printability properties of these materials, leaving research gaps regarding their effects on anisotropy and the mechanical properties of 3DPC.
On the other hand, studies on various reinforcement strategies for 3DPC have been conducted in the previous literature. Moreover, reinforcing 3DPC with microfibers that can be integrated into the mixture and extruded together is the most suitable approach to fully explore the architectural freedom of 3DPC technology [2]. In contrast, the use of other reinforcing materials, such as rebars, still presents issues, including automated implementation; additionally, their ability to be shaped into complex forms is limited [8]. Therefore, while the capacity of microfibers to replace conventional rebars depends heavily on structural requirements, loading conditions, and design considerations, their use presents a feasible alternative that maximizes architectural freedom and controls plastic shrinkage in printed composites [9].
Zat et al. investigated the effect of two microfibers, namely steel and rock wool, on the mechanical properties of 3D-printed concrete. They reported a 30% improvement in tensile strength due to microfibers and mitigation of strength loss caused by the printing process [10]. Ramezani et al. investigated the effect of different microfibers such as steel, carbon, glass, polyvinyl alcohol (PVA), polyethylene (PE), and polypropylene (PP) fibers on the fresh and mechanical properties of 3D-printed concrete mixtures and reported that fiber incorporation enhanced the flexural strength by up to 40–60% but reduced the workability and pumpability of the fresh mixture, which increased the risk of nozzle clogging and filament deformation during extrusion [11]. In their study, Xia et al. comparatively investigated the effects of various volumes of polypropylene, basalt, and steel fibers of different lengths on the fresh and hardened properties of cement-based printable mortars. They reported that optimal yield stress enhancement and mechanical property improvement were achieved using 0.7% steel fibers compared to other fiber types [8]. Also, compared to other types of fibers, micro-steel fibers provide a greater enhancement in yield stress, compressive strength, and flexural strength [8].
Short straight fibers with a typical length between 1 and 15 mm have demonstrated superior compatibility with extrusion-based 3DPC, particularly because even at higher contents (exceeding 0.3%) they promote extrusion, minimize nozzle clogging, and are prone to align parallel to the printing direction compared to longer fibers and hooked-end fibers [12,13,14].
Jia et al. examined the effect of the shape and content of steel fibers on the fresh and mechanical properties of high-strength 3D-printed cementitious composites. They used 13 mm-long straight and hooked-end steel fibers at various volumes. They reported nozzle clogging when the fiber content exceeded 1%. Additionally, they observed that straight fibers reduced matrix porosity by aligning in the printing direction during extrusion [13].
Mechanical performance, crack propagation, and durability of heterogeneous concrete structures across different manufacturing processes, such as layer-to-layer deposition or multi-layer consolidation, are highly governed by the properties of the interlayer contact zone. Accordingly, a weak interfacial zone leads to premature delamination and pronounced mechanical anisotropy [15]. Hence, it is vital for the broader field of advanced concrete technology to understand how various mixture ingredients affect the properties of the interlayer contact zone to design reliable heterogeneous concrete structures. The review of the existing literature shows that while FA and BFS represent the two most widely utilized SCMs essential for enhancing the ecological sustainability of 3DPC, which is characterized by a large binder volume, systematic comparisons of how they differentially affect the mechanical performance and directional anisotropy of plain versus microfiber-reinforced 3DPC have not been studied. Furthermore, since the effectiveness of micro-steel fiber reinforcement is governed by matrix-dependent chemical and mechanical bonding [16], a comparative understanding of how BFS and FA govern the interlayer bond strength and directional mechanical anisotropy of plain and micro-fiber-reinforced 3DPC has not been systematically investigated. Furthermore, this study experimentally maps the mechanical properties of BFS- and FA-bearing 3D-printed concrete in light of conventionally cast concrete, helping designers and engineers understand the performance differences between layered structures and conventionally cast ones in the presence of SCMs.
Hence, in the present study, the effect of substituting CEM I ordinary Portland cement (OPC) with ground granulated blast-furnace slag (BFS) and class-F fly ash (FA) on the mechanical properties and anisotropy of plain and micro-steel fiber-reinforced 3D-printed concrete has been experimentally investigated. Accordingly, printable mixtures containing 0%, 20%, and 40% of either BFS or FA by weight as a partial replacement for OPC were developed at a constant water-to-binder (w/b) ratio of 0.3, hydroxypropyl methylcellulose (HPMC) dosage of 0.14% by binder weight, and a flow diameter of 180 ± 10 mm. Micro-steel fibers were added at 0.5% of the total volume for the reinforced samples. The performance of BFS and FA on interlayer bond strength, anisotropy, and structural integrity of plain and reinforced 3DPC was comparatively studied on mold-cast and printed samples by employing various tests, including flexural, compressive, split tensile, shear bond, and direct tensile strength tests at 7 and 28 days of standard water curing.

2. Materials and Methods

2.1. Materials

CEM I 42.5R ordinary Portland cement (OPC), ground granulated blast furnace slag (BFS), and class F fly ash (FA), whose properties are presented in Figure 1, were used as binding materials. Table 1 shows their physical properties and chemical compositions. As the fine aggregate, natural river sand with a maximum particle size of 2 mm, specific gravity of 2.46, water absorption capacity of 0.67%, and fineness modulus of 1.3 was employed. Straight micro-steel fibers coated with brass, having dimensions of 13 mm in length, 0.2 mm in diameter, and an aspect ratio of 65, with a tensile strength of 2750 MPa and a Young’s modulus of 200 GPa, were added as reinforcing agents. Moreover, to achieve the required properties for printable mixtures, chemical admixtures comprising a superplasticizer (SP) based on polycarboxylate ether and a water-soluble viscosity modifier based on HPMC with a viscosity of 55.000–85.000 mPa°s were employed.
Figure 1. The particle size distribution of OPC, BFS, and FA.
Table 1. Physical properties and chemical compositions of the binders.

2.2. Method

The flowchart of the experimental methodology followed in this study is shown in Figure 2. The details of the adopted procedure are elaborated in the subsequent sections.
Figure 2. A summary of the experimental research design of this study.

2.2.1. Printable Mixture Development and Production of Samples

Printable mixtures, from which tested samples were produced, were developed by following the mixing process presented in Figure 3. The ingredient proportions for the mixtures are presented in Table 2 for plain mixtures and in Table 3 for fiber-reinforced mixtures. The design of the plain reference mixture (REF) and the formulation of BFS- and FA-bearing unreinforced mixtures were thoroughly studied in our previous studies, where fresh and rheological properties were determined [5,17]. Mixing of the ingredients was carried out at an ambient temperature of 21 ± 3 °C using a Hobart mixer at two speeds: 60 and 120 rpm. For starters, SP was dissolved in the mixing water, to which binder-forming materials were slowly added sequentially using a round-mouth scoop while mixing at low speed. At the same speed, fine aggregate was added to the formed paste, followed by HPMC and finally micro-steel fibers for the reinforced mixtures. The mixing was finalized by high-speed mixing for 3 min. Hence, the total mixing time was 12 ± 3 min.
Figure 3. Mixing process.
Table 2. Mix proportions of the cementitious composites without fibers.
Table 3. Mix proportions of the cementitious composites with fibers.
In the present study, batch-specific consistency and printability were evaluated using standardized flow-table tests. As a widely used method for assessing the printability of 3D-printable mixtures, the flow table test is a reliable, practical indicator of yield stress and overall flowability [18,19]. By keeping the water-to-binder ratio constant at 0.3 and adjusting SP dosage to achieve a target flow diameter of 180 ± 10 mm, the mixtures were adjusted to have comparable initial rheological properties, thereby allowing their actual engineering performance to be measured at similar workability levels. While rotational rheometers yield comprehensive thixotropic data, flow-table testing provides a practical and repeatable preliminary estimation to achieve similar consistency, ensuring comparable pumpability and extrudability among the mixtures. BFS addition enhanced the flowability, leading to a decreased SP dosage, whereas FA addition reduced the flowability, demanding a higher SP dosage. The enhancement of flowability by BFS can be attributed to improved particle packing and reduction in interparticle friction [20]. On the other hand, the presence of unburnt carbon and microvoids on FA particles may reduce the effectiveness of SP [21]. Furthermore, Table 3 shows that adding micro-steel fiber at 0.5% of the total volume led to a decrease in SP dosage, except for BFS-bearing mixtures. Note that the microfiber volume was subtracted from the aggregate volume to keep the total aggregate and fiber volume constant across all mixtures. Therefore, the increase in flowability with micro-steel fiber addition may be attributed to the reduction in interparticle friction with sand volume reduction as well as the shape effect of microfibers orienting in the flow direction [22].
The developed printable mixture was poured into a screw-based pump, and printing started immediately. Mixing and printing were conducted in the laboratory under controlled ambient conditions of 22 ± 2 °C and 50 ± 10% relative humidity. For all batches, the total elapsed time from the end of mixing to the start of printing was strictly maintained at 15 ± 2 min. The printing setup of the present study included a single-screw-based pump, a 5 m-long hose, and a lab-scale gantry printer customized with 4 axes and a working space of roughly 1 m3. The extrusion was performed horizontally using a customized rectangular back nozzle measuring 15 × 41 mm (Figure 4), mounted on the printhead 14 mm above the printer bed. The selection of this nozzle type and extrusion method was made to minimize the compressive effect of vertically oriented nozzles, which are sensitive to the printhead stand-up height [23].
Figure 4. (a) Shape of the rectangular nozzle used (15 × 41 mm); (b) layer printed using this nozzle.
For printing, a printing speed of 50 mm/s, a material flow rate of 1.8 L/min, and nozzle standoff height of 14 mm were used. Consecutive layers were printed immediately to minimize printing delay. The printing path was configured as a single closed circuit, with each complete loop taking 90 s. Consequently, an interlayer time gap of 90 s is maintained before the subsequent layer is deposited onto the underlying layer. This short printing path was selected to ensure that the underlying layer surface remains in a fresh state, thereby minimizing cold joint formation and promoting adequate inter-layer matrix interdiffusion. As soon as printing was complete, the printed object was divided into smaller parts that could be conserved in the curing bath. For molded samples, prismatic steel molds were filled in 3 layers, with each layer tapped 25 times, as prescribed by TS EN 196-1 [24].
It is worth noting that the curing of both printed and molded samples was performed at ambient temperature for the first 24 h to promote setting and hardening, after which standard water curing in a temperature-controlled bath was employed until testing. During the first 24 h period, samples were covered with plastic sheets to minimize evaporation and related plastic shrinkage. At the time of testing, printed samples were saw-cut to the desired dimensions using a concrete saw-cutter.

2.2.2. Flexural Strength Assessment

The flexural strength of the developed plain and fiber-reinforced printable mixtures was assessed using a three-point bending test on the 7th and 28th days of standard water curing for molded and printed samples. The three-point bending test was performed as prescribed in TS EN 196-1 [24]. A load cell with a capacity of 100 kN was mounted on a displacement-controlled electromechanical press to detect the load. Four samples, each measuring 40 × 40 × 160 mm, were tested from each mixture at a loading rate of 0.5 mm/min with a 130 mm gap between the two supports. Samples were loaded at the midspan, and the displacement was recorded at the midspan with the help of a linear variable differential transformer (LVDT). For unreinforced samples, the area under the load–displacement curve up to the point of sudden failure during testing was considered in the toughness calculation. For reinforced specimens, the evaluation was based on the area under the load–displacement curve up to a maximum displacement of 7 mm. Thus, the toughness assessment captured the comprehensive energy absorption capacity of the micro-steel fiber-reinforced specimens, encompassing both pre-peak and post-peak responses. Printed samples were prepared and saw-cut to the desired dimensions at testing age, as explained in the previous section. The load was applied perpendicular to the printing direction, hereafter referred to as the B direction (Figure 5a).
Figure 5. Schematic representation of (a) the 3D-printed flexural specimen (40 × 40 × 160 mm) tested in the B direction and the 3D-printed compressive specimens (40 × 40 × 40 mm) tested in (b) the A direction, (c) the B direction, and (d) the C direction.

2.2.3. Compressive Strength Assessment

The performance of the developed plain and fiber-reinforced printable mixtures was assessed by conducting uniaxial compressive strength tests at 7 and 28 days, using a hydraulic press with a capacity of 3000 kN, at a loading rate of 2.4 kN/s. Experiments were performed on mold-cast and printed cubic samples measuring 40 × 40 × 40 mm, in accordance with TS EN 196-1 [24]. Figure 4 shows the 3D printing setup depicting a rectangular nozzle (15 × 41 mm) and the filament deposition process. The directional framework distinguishes between the longitudinal printing direction (X), transverse horizontal direction (Y), and build/vertical direction (Z), corresponding to structural testing orientations A, B, and C across printed layers. Accordingly, to assess the direction-dependent strength loss due to printing, printed samples were loaded in the directions parallel, perpendicular, and vertical (cross-layer) to the printing direction, as shown in Figure 5b–d. Mold-cast samples were loaded in one direction as prescribed by TS EN 196-1. A minimum of 4 samples were tested for each mixture and loading direction at every testing age.

2.2.4. Anisotropy Assessment

The effect of BFS and FA addition on the anisotropy behavior of the developed plain and micro-steel fiber-reinforced 3D-printed concrete was evaluated at 7 and 28 days by computing two complementary dimensionless metrics, namely the absolute anisotropy coefficient (I3D) and the isolated intra-directional anisotropy coefficient (Idir). First, I3D was calculated by comparing the printed compressive strengths in each loading direction against the mold-cast reference strength (σM) using Equation (1), following previous studies [25,26]. Because conventional mold-cast concrete is treated as isotropic in structural design codes, I3D depicts the combined influence of process-induced strength reduction (due to interlayer voids, lack of compaction, and weaker interfacial zones) and directional variability across the three orthogonal loading axes (A, B, and C). Second, to isolate true directional sensitivity from this overall printing-induced strength variation, Idir was quantified using Equation (2) [25]. Unlike I3D, Idir relies exclusively on intra-directional printed strength ratios (normalizing directional strengths against the printed specimens themselves rather than (σM), thereby isolating the intrinsic directional anisotropy of the layered composite. As explained in the previous section, at least 4 printed samples from each mixture were prepared and loaded in each loading direction at 7 and 28 days, as shown in Figure 5b–d. Additionally, mold-cast samples were tested in one direction in accordance with TS EN 196-1 [24]. It is worth noting that the compressive strength values utilized to compute the I3D and Idir consisted of the average compressive strength values obtained from at least 3 samples.
I 3 D = ( σ A − σ M ) 2 + ( σ B − σ M ) 2 + ( σ C − σ M ) 2 / σ M
Here, σA, σB, and σc are the average compressive strength values obtained from each loading direction, namely A, B, and C. σM is the average compressive strength obtained from mold-cast samples.
I dir = ( σ A − σ avg ) 2 + ( σ B − σ avg ) 2 + ( σ C − σ avg ) 2 / σ avg
where
σ avg = ( σ A + σ B + σ C ) / 3
Here, σavg is the average compressive strength computed from the compressive strength values (σA, σB, and σc) obtained from three loading directions, namely A, B, and C.

2.2.5. Splitting Tensile Strength Assessment

Splitting strength tests were carried out on molded and printed samples in accordance with ASTM C 496-04 [26]. Although ASTM C496 primarily specifies cylindrical specimens, the adoption of rectangular prismatic specimens (40 × 40 × 60 mm) is a well-established practice in research investigating 3D-printed cementitious materials [27,28,29]. Additionally, its equivalent, EN 12390-6, prescribes guidance on the application of prismatic samples [30]. At least 4 samples, each measuring 40 × 40 × 60 mm and with 4 layers, were tested after 7 and 28 days of standard water curing. A 2 mm-deep notch was cut along the central axis to align the loading line and promote stress concentration at the intended splitting plane. A hydraulic press with a capacity of 3000 kN was used in the tests. The loading rate was kept at 0.125 kN/s during the tests. The preparation of molded and printed samples was as described in the previous section. The loading direction for the printed samples is the A direction, as shown in Figure 6. During the tests, it was ensured that the critical interface of the printed samples was aligned with the loading line. The split tensile strength was computed using Equation (4). It is worth noting that for the notched mold-cast samples, net dimensions (dnet) along the failure plane were used to calculate the split tensile strength.
σ y = 2 × P π × L × d
Figure 6. Test setup for assessing splitting tensile strength.
Here, σy is the split tensile strength (MPa), P represents the maximum applied load (N), L represents the specimen dimension parallel to the loading direction (mm), and d represents the specimen dimension perpendicular to the loading direction (mm).

2.2.6. Interlayer Shear Bond Strength Assessment

The interlayer shear bond strength was assessed on the 7th and 28th days of curing for molded and printed samples, as in previous studies [31]. For each mixture and curing age, at least 4 samples were tested. Samples measuring 40 × 40 × 60 mm were prepared using a concrete saw cutter at the time of testing. For molded samples, a notch with a depth of 2 mm was introduced along the axis to induce stress concentration along the intended shear plane. It is worth noting that for mold-cast samples with notches, the net cross-sectional area (Anet) was measured and used to calculate shear strength. A loading rate of 0.1 kN/s was used for the experiments. Three metal rods were aligned exactly with the layers of the printed samples, as shown in Figure 7. The shear bond strength was then computed with the help of Equation (5). During testing, the observed failure was characterized by an adhesive failure along the interlayer interface, confirming the effectiveness of the test setup in evaluating bond strength.
  σ b = F b 2 A b
where σb is the shear bond strength (MPa), Fb is the maximum shear load (N), and Ab is the shear plane area (mm2) of a single shear plane. The factor 2 reflects the double-shear configuration.
Figure 7. Schematic (a) and pre-test appearance (b) of metal alignment with the layers of a printed sample for the shear bond strength test.

2.2.7. Direct Tensile Strength Assessment

The direct tensile strength was assessed by direct tensile testing of molded and printed samples at 7 and 28 days of curing, as in previous studies [22,32,33]. From each mixture, a minimum of 4 samples with 40 × 40 × 28 mm (L × W × H) dimensions were tested. In mold-cast samples, a 2 mm notch was introduced on the sides of the samples along the center axis to induce a controlled fracture. Accordingly, for the notched samples, the net cross-sectional area (Anet) along the failure plane was measured and utilized in the calculation of tensile strength. For the printed specimens, the actual net effective bonding area was measured post-failure directly from the fractured interlayer surfaces using a digital caliper and utilized in calculations. The employed testing setup is presented in Figure 8. As can be seen, samples were glued onto two metal plates using the epoxy resin SIKADUR®-31 (sourced from Sika Türkiye, İzmir, Türkiye). To prevent eccentricity, the metal plates to which the samples were glued were designed with pivoting joints that allow multi-directional rotational freedom. Tests were performed under displacement control at a rate of 1 mm/min. The direct tensile strength was computed using Equation (6).
  σ t = F t A t
where Ft is the maximum tensile load (N), and At is the cross-sectional area of the specimen (mm2).
Figure 8. The schematic illustration (a) and actual sample being pulled in direction B during the direct tensile strength test (b).

3. Results and Discussion

3.1. Flexural Performance

The effect of partially replacing OPC with BFS and FA at 20% and 40% by weight on the 7- and 28-day flexural strength and toughness of 3D-printed concrete, with and without micro-steel fibers as reinforcement, was comparatively studied in molded and printed specimens. Accordingly, recorded experimental results at 7 and 28 days of standard water curing are presented in Figure 9, Figure 10, Figure 11, Figure 12, Figure 13 and Figure 14.
Figure 9. Load–displacement curves of (a) mold-cast (M) and (b) 3D-printed (P) with and without micro-steel fiber reinforcement at 7 days.
Figure 10. Load–displacement curves of (a) mold-cast (M) and (b) 3D-printed (P) with and without micro-steel fiber reinforcement at 28 days. The curves were obtained from the specimens exhibiting mechanical responses closest to the average performance of each mixture.
Figure 11. Toughness of mold-cast and 3D-printed specimens without micro-steel fiber reinforcement at 7 and 28 days.
Figure 12. Toughness of mold-cast and 3D-printed specimens with micro-steel fiber reinforcement at 7 and 28 days.
Figure 13. Flexural strength of mold-cast and 3D-printed specimens without micro-steel fiber reinforcement at 7 and 28 days.
Figure 14. Flexural strength of mold-cast and 3D-printed specimens with micro-steel fiber reinforcement at 7 and 28 days.
Figure 9 and Figure 10 present load–displacement curves for plain and microfiber-reinforced printable mixtures, illustrating the load-bearing performance and deflection behavior of produced molded and printed samples during three-point bending flexural performance tests.
In the presented graphs, the letters “M” and “P” at the start of the mixture ID denote mold-cast and printed, respectively, indicating the production method used to make the sample. Also, the letter “F” at the end of some mixture IDs stands for fiber-reinforced. The numbers “20 or 40” indicate the replacement ratio of OPC with BFS or FA. For instance, “M-BFS20” represents a molded sample produced from a plain mixture (without fiber reinforcement) with 20% BFS as a substitute for OPC by weight. “P-BFS20-F” represents a printed sample produced from a mixture with 20% BFS as a substitute for OPC by weight and steel fibers as reinforcement. REF stands for the reference mixture, a control mixture in which OPC is the sole binding material. This nomenclature was used throughout this study. Additionally, the error bars in the presented graphs represent the standard deviation. It should be noted that the test specimens were saw-cut from a single large printed element for each mixture design. Consequently, the reported standard deviations primarily reflect local mechanical heterogeneity and intra-batch variability within the printed element.
Concurrent with visual observation, plain mold-cast and printed samples exhibited similar brittle behavior, in which failure occurred instantly, with a single crack forming at midspan and progressing directly to the loading pin in a straight path. This brittle behavior is characterized by a sharp drop in strength after peak strength is reached in the curves presented. These findings indicate that the post-crack behavior and limited energy absorption of plain 3D-printed concrete can lead to sudden element failure.
Unlike plain samples, incorporating micro-steel fibers significantly altered the failure mode of the developed 3D-printed concrete across all mixtures. With microfibers, all mixtures showed ductile failure in both molded and printed samples at 7 and 28 days. The sharp drop in strength after peak load and the initiation of the first crack did not occur in reinforced samples. Also, unlike mold-cast samples, reinforced printed ones exhibited a complex crack pattern, as in previous studies [34]. The observed complex crack pattern in fiber-reinforced printed samples may be associated with the combined effects of fiber addition and the strength difference between the bulk layer and the interlayer region, which can disrupt crack propagation across regions of different strength. In the present study, debonding of layers at the interlayer during three-point bending tests was not observed, unlike in some previous studies [27,35]. This may indicate relatively high interlayer bonding strength in the developed mixtures.
Furthermore, it can be seen that printing enhanced the post-crack energy absorption behavior of the developed mixtures, in that at 28 days, printed samples, especially P-REF and P-BFS40, exhibited a deflection-hardening behavior, unlike their molded counterparts, which showed a deflection-softening behavior, highlighting the combined effect of fiber addition and a strong matrix. The enhancement in toughness as a result of printing is evident when the toughness of molded and printed samples is analyzed, as discussed below. Apart from P-REF and P-BFS40, all other reinforced mixtures exhibited deflection softening in both molded and printed samples at 7 and 28 days.
The effect of micro-steel fiber addition on the post-crack energy absorption performance of the developed 3D-printed concrete is evident from the results shown in Figure 11 and Figure 12. Compared with plain mixtures, the addition of micro-steel fibers significantly improved the toughness of the developed composites across all mixtures and for both molded and printed samples at 7 and 28 days.
In molded samples, compared to plain samples, the addition of micro-steel fibers led to an increase in toughness by 11.7, 13.1, 19.5, 10.7, and 30.4 folds at 7 days, as well as 12.3, 13.5, 17.8, 12.3, and 12.5 folds at 28 days for M-REF-F, M-BFS20-F, M-BFS40-F, M-FA20-F, and M-FA40-F, respectively. Similarly, in printed samples, compared to plain samples, the addition of micro-steel fibers led to an increase in toughness by 9.8, 10.3, 12.4, 13.4, and 7.6 folds at 7 days, as well as 19.6, 9.4, 16.5, 12, and 8.5 folds at 28 days for P-REF-F, P-BFS20-F, P-BFS40-F, P-FA20-F, and P-FA40-F, respectively.
The increase in toughness with the addition of micro-steel fibers can be attributed to the crack-bridging effect, which considerably promotes post-crack stress transfer. Furthermore, the presence of fibers may significantly reduce plastic shrinkage cracks, leading to improved load-bearing capacity and a delay in crack formation [8].
Comparing the 28-day toughness performance of molded and printed samples in both plain and reinforced mixtures shows that, in the loading direction employed in the present study, printing slightly enhances the toughness of the developed mixtures. Accordingly, increases in toughness of 26–76% and 17–131% were observed at 28 days in printed samples of plain and reinforced mixtures, respectively, compared to their molded counterparts. This further enhancement of toughness by printing may be attributed to the layered structure of the printed samples, which lengthens the crack path through deflection. Additionally, for reinforced mixtures, printing may promote microfiber alignment parallel to the printing direction due to extrusion pressure, leading to more effective stress transfer and crack bridging, particularly when the load is applied perpendicular to the printing direction, as in this study [36]. In contrast to printed samples, mold-cast samples exhibit randomly oriented fibers, thereby limiting their crack-bridging efficiency and stress transfer, and adversely affecting their energy absorption capacity [37]. It is worth noting that since printed composites exhibit anisotropy, this behavior may vary with the loading direction. These findings demonstrate that when loaded perpendicular to the printing direction, extrusion-based 3D printing, together with a suitable mixture design, may provide a viable approach to mitigating brittle failure in structures where post-crack energy absorption is crucial. Furthermore, the observed toughness enhancement by 3D printing can be leveraged to design more ductile structural elements with improved performance against seismic and dynamic loads. Moreover, these results open the door to future research on the use of 3D-printed components for structural retrofitting of existing load-bearing elements.

3.1.1. Flexural Strength of Plain Mixtures

Figure 13 presents the 7- and 28-day flexural strength values of plain 3D-printed concrete containing 20% and 40% BFS and FA as partial replacements for OPC for molded and printed specimens. It is evident from these results that the incorporation of BFS and FA, as well as the sample preparation method, did not generally have a significant effect on the 7- and 28-day flexural strength of molded and printed samples.
In molded samples, incorporating BFS and FA as substitutes for OPC slightly enhanced the 28-day flexural strength of the developed mixtures by 7%, 14%, and 5% for M-BFS20, M-BFS40, and M-FA20, respectively, compared to M-REF. Unlike other substitution ratios, replacing 40% of OPC with FA resulted in a slight 10% decrease in strength relative to M-REF. As expected, at 7 days, incorporating BFS and FA reduced strength across all mixtures relative to REF, with losses of up to 49% (M-FA40). The increase in strength with the extension of curing for BFS- and FA-bearing mixtures further highlights the importance of curing and mold stripping time for mixtures containing SCMs. The observed loss in flexural strength for BFS- and FA- containing mixtures at 7 days can be associated with the dilution effect and the latent hydraulic behavior of these SCMs. According to previous literature, replacing OPC with BFS and FA leads to a decrease in the total mass of available reactive clinker; also, earlier studies indicate that the densification of the matrix by BFS and FA occurs through latent hydration between portlandite (Ca(OH)2) and the SCMs in the presence of moisture. Hence, based on reported findings, the strength of SCM-bearing mixtures is expected to increase further with prolonged curing [38,39].
Additionally, the recorded experimental results revealed that the difference in flexural performance between molded and printed samples was insignificant, especially with extended curing (28 days) for mixtures produced with BFS and FA. Accordingly, small decreases in strength of 5%, 17%, and 9% were observed in the printed P-BFS40, P-FA20, and P-FA40 samples compared to their molded counterparts at 28 days. P-BFS20 exhibited a slight increase in strength of 3% after printing. Unlike pozzolan-bearing mixtures, a 22% strength increase was observed in the REF mixture after printing. It may be inferred from these results that printing does not considerably affect the flexural strength of plain printable mixtures in the B-loading direction employed in the present study. It is worth noting that the anisotropic property resulting from printing may considerably affect the flexural load-bearing capacity in other loading directions [35].
Examining the effect of BFS and FA inclusion on the flexural strength of printed samples shows that the inclusion of BFS and FA caused a decrease in strength at both 7 and 28 days in comparison to REF. Accordingly, the P-FA40 mixture exhibited the highest strength loss, up to 30% and 32% at 7 and 28 days, respectively, compared to P-REF. In other mixtures, the observed loss in strength was minor, ranging from 5% to 12% at 7 days and from 9% to 29% at 28 days. At the studied sample maturity (7 and 28 days of curing), the substitution of OPC with BFS and FA did not yield any significant effect on the flexural strength values of printed samples in comparison to P-REF. Nonetheless, prior literature suggests that the strength of SCM-bearing mixtures may increase further with prolonged curing [35].

3.1.2. Flexural Strength of Micro-Steel Fiber Reinforced Mixtures

Figure 14 presents the 7- and 28-day flexural strength values for mold-cast and printed samples reinforced with micro-steel fibers. The findings show that in molded samples, incorporating micro-steel fibers slightly reduced flexural strength compared to plain mixtures. Decreases in strength of 13%, 11%, 12%, 12%, and 11% occurred for M-REF-F, M-BFS20-F, M-BFS40-F, M-FA20-F, and M-FA40-F compared to their plain counterparts at 28 days. At 7 days, strength decrements of 21%, 4%, and 17% were observed for M-REF-F, M-BFS40-F, and M-FA20-F, respectively, compared to their plain counterparts. M-BFS20-F and M-FA40-F recorded strength increases of 5% and 19% at 7 days compared to their plain counterparts at equal maturity. The decrease in strength observed with fiber addition may be associated with the balling effect of high-aspect-ratio fibers, leading to air entrapment in the vicinity of the fibers [40]. Additionally, Pham et al. reported that adding short fibers at volume fractions below 1% did not form an interconnected fiber network, thereby preventing the fibers from exhibiting a crack-bridging effect. Furthermore, previous studies reported that microfiber incorporation increased interfacial micro-voids around the fibers, which subsequently reduced the strength of the composite [41].
Examining the effect of BFS and FA addition on the flexural strength values of mold-cast reinforced printable mixtures shows that, in comparison to REF, BFS enhanced both the 7- and 28-day flexural strength of developed mixtures by 10% and 13% at 7 days, as well as 9% and 15% at both 20% and 40% replacement ratios; FA caused a decrease in strength of 8% and 23% at 20% and 40% replacement ratios at 7 days. At 28 days, FA inclusion at 20% increased strength by 6%, while at 40% it decreased strength by 7%.
In printed samples, incorporating micro-steel fibers as reinforcement resulted in a slight increase in the strength of the developed mixtures at 28 days. Compared with plain printed samples, strength increments of 27%, 12%, and 5% were observed for P-REF-F, P-BFS40-F, and P-FA20-F, respectively. P-BFS20-F exhibited a loss in strength of 24%, while P-FA40-F yielded equal performance to P-FA40. At 7 days, printed reinforced mixtures exhibited a loss of strength ranging from 10% to 29% compared to their printed plain counterparts. The observed increase in the flexural strength of printed samples with the addition of micro-steel fibers can be attributed to the fibers being oriented parallel to the printing direction, due to extrusion pressure. Furthermore, the mechanical shear resulting from screw pumping and extrusion may have enhanced fiber dispersion, thereby preventing balling and maximizing strength gains. Therefore, better fiber dispersion and fiber alignment in the printing direction may have enhanced resistance to loads applied perpendicular to the printing direction and to the aligned fibers. Previous studies have established that in extrusion-based 3DPC, where microfibers are incorporated, the optimal flexural strength of the fibers was observed when they were aligned at ±20° to the printing direction. Additionally, it was reported that the orientation of the fibers can be affected by nozzle shape, nozzle diameter, and standoff height [42]. The assessment of fiber orientation is beyond the scope of the present study. The present results show that 3D printing can enhance the flexural performance of micro steel-fiber-reinforced concrete mixtures compared with mold casting. Since concrete inherently possesses low tensile and flexural strength, this improvement offers a meaningful advantage, especially in micro-steel fiber-reinforced mixtures designed for applications requiring high flexural performance. Furthermore, these findings provide a foundation for future research on the use of 3D-printed, microfiber-reinforced concrete for more material-efficient structural components.
The findings of the present study also show the effect of printing on reinforced mixtures modified with various volumes of BFS and FA. Results indicate that the effect of printing on reinforced mixtures varied with mixture composition. Accordingly, compared with mold-cast reinforced samples, printing increased the 28-day flexural strength of the P-REF-F, P-BFS40-F, and P-FA40-F mixtures by 77%, 21%, and 2%, respectively, while slightly decreasing the strength of the P-BFS20-F and P-FA20-F mixtures by 12% and 2%, respectively.
Furthermore, examining the effect of BFS and FA addition on the strength of printed samples reinforced with micro-steel fibers shows that, in comparison to the REF mixture, the addition of BFS and FA led to a decrease in strength by 46%, 22%, 41%, and 46% for P-BFS20-F, P-BFS40-F, P-FA20-F, and P-FA40-F at 28 days, respectively. A decrease in strength upon the addition of BFS and FA in the early stages of hydration is generally attributed to dilution and the latent hydraulic behavior of these SCMs. Additionally, the use of BFS and FA has been reported to increase the yield stress in printable mixtures, which may lead to air entrainment in the absence of vibration [43,44]. In the present study, FA-bearing mixtures were produced using a higher dosage of SP to achieve the required workability; this may retard hydration, thereby lowering strength at the early stages of maturity.

3.2. Compressive Strength Performance

3.2.1. Compressive Strength of Plain Mixtures

The experimental results obtained at 7 and 28 days of standard water curing for plain and microfiber-reinforced mold-cast and printed samples produced from printable mixtures prepared with various ratios of BFS and FA as substitutes for OPC are presented in Figure 15.
Figure 15. Compressive strength of mold-cast and 3D-printed specimens without micro-steel fiber reinforcement: (a) 7 days and (b) 28 days.
The findings show that under uniaxial compressive loading, the performance of the developed 3D-printed concrete is significantly influenced by the composition of the mixture, namely the type and amount of added SCM, indicating differences in hydration kinetics, interfacial transition zone development, and latent hydraulic behavior of pozzolans. Additionally, a considerable difference in load-bearing capacity was observed between plain and reinforced printed and molded samples, indicating the effects of fabrication via extrusion and layer-stacking technologies, which inherently introduce multiple interlayer interfaces that enable orientation-dependent load-transfer mechanisms.
In plain mixtures, molded samples generally exhibited higher strength than their printed counterparts at both 7 and 28 days. Hence, it may be concluded that printing reduced strength regardless of the mixture composition. Furthermore, printed samples exhibited orientation-dependent load-bearing capacity at both 7 and 28 days in all mixtures.
Examining the effect of partially replacing OPC with BFS and FA at various ratios (namely 0%, 20%, and 40%) on the compressive strength of developed printable mixtures indicates that in molded samples, the incorporation of BFS and FA significantly enhanced the strength of developed composites, especially at 28 days. Compared with the M-REF mixture, strength increases of 32%, 42%, 10%, and 4% at 28 days, and 9%, 3%, and 3% at 7 days were observed in the M-BFS20, M-BFS40, M-FA20, and M-FA40 mixtures, respectively. Only mixture M-FA40 exhibited a 9% loss in strength at 7 days compared to M-REF. The improvement in strength with the incorporation of BFS and FA can be attributed to matrix densification via the pozzolanic reaction between Ca(OH)2 and pozzolans in the presence of moisture, which forms additional CSH gels. Additionally, the latent hydraulic behavior of pozzolans explains the observed higher strength enhancement with curing in pozzolan-bearing mixtures.
In printed samples, the effect of substituting OPC with BFS and FA on the compressive strength varied in accordance with the loading direction. In other words, the effect of printing on the compressive strength of the developed composites varied based on the loading direction in all mixtures. Compared to the P-REF mixture, the incorporation of BFS and FA enhanced the compressive strength by 2%, 11%, and 5% for P-BFS20, P-BFS40, and P-FA20 in the A loading direction at 28 days, respectively. The highest strength increase of 15% was observed at 28 days in the C loading direction for P-BFS40 compared to P-REF. At 7 days, a 10% and 29% strength increase for P-BFS20 and P-FA20 were recorded in the C loading direction compared to REF.
The load-bearing capacity of printed samples varied in accordance with the loading direction. Generally, samples exhibited the highest strength in loading direction A, followed by B and C, across all mixtures. The only exception was in the P-BFS40 mixture, where C and B, respectively, followed A.
Comparing the 28-day strength of molded samples to that of printed samples with respect to the loading direction shows that using BFS and FA resulted in greater strength loss after printing than the REF mixture. Also, the use of BFS and FA exacerbated the loss of strength due to printing, with the gap between molded and printed samples widening in their presence. In other words, although post-printing strength loss was noted in all mixtures, its magnitude increased in the presence of BFS and FA. Accordingly, in comparison to their relative molded strength, strength losses of 11%, 13%, and 26% (P-REF), 31%, 54%, and 60% (P-BFS20), 30%, 45%, and 39% (P-BFS40),15%, 24%, and 36% (P-FA20), 38%, 44%, and 46% (P-FA40) occurred when the strength recorded in the A, B, and C loading directions are compared to that of their relative molded samples respectively. The observed effect of pozzolans on the compressive strength of printed samples has been reported in previous studies [45]. It may be attributed to an increase in the volume of entrapped air during extrusion owing to the high yield stress of pozzolan-bearing mixtures and lack of vibration.

3.2.2. Compressive Strength of Micro-Steel Fiber Reinforced Mixtures

Figure 16 presents the 7- and 28-day compressive strengths of the developed mixtures with micro-steel fibers added as reinforcement. The findings show that incorporating fibers significantly improved the strength of the developed 3D-printed concrete across all mixtures and both curing ages.
Figure 16. Compressive strength of mold-cast and 3D-printed specimens with micro-steel fiber reinforcement: (a) 7 days and (b) 28 days.
In mold-cast samples, the addition of fiber increased strength across all mixtures at both 7 and 28 days. Compared to plain mixtures, fiber addition led to a strength increment of 54%, 24%, 42%, 17%, and 2% at 7 days and 50%, 3%, 8%, 13%, and 2% at 28 days for M-REF-F, M-BFS20-F, M-BFS40-F, M-FA20-F, and M-FA40-F mixtures, respectively. The largest increase in strength with the addition of microfibers was observed in the M-REF-F mixture at both ages, which may be attributed to a stronger matrix due to the relatively higher total mass of reactive clinker and its rapid hydration, as well as to the presence of fibers. Micro-steel fibers can improve the compressive strength of cementitious composites by retarding crack formation and mitigating crack propagation. Furthermore, micro-steel fibers may prevent microcracks caused by plastic shrinkage by enhancing the tensile strength of the composites. Previous research on concrete mixtures containing SCMs indicates additional strength gain over extended curing periods for such concrete composites [35]. Hence, BFS-and FA-bearing mixtures may show further strength gain with extended curing periods.
Additionally, the findings clearly show that, in the presence of micro-steel fibers, the performance of printed samples under uniaxial compressive loading differed significantly from that of molded samples, with a pronounced reduction in strength.
Comparing the 7- and 28-day compressive strength of molded samples to that of printed samples with respect to each loading direction, it can be seen that strength losses between 17% and 48% at 7 days, as well as 16% and 49% at 28 days (A); 27% and 54% at 7 days as well as 36% and 56% at 28 days (B); 37% and 63% at 7 days as well as 32% and 59% at 28 days (C) occurred in comparison to their relative molded samples at 7 and 28 days respectively.
As reported in previous studies, this reduction in strength due to printing can be attributed to the formation of multiple interfacial transition zones between layers, which act as weak points that reduce load-bearing capacity. The presence of the interlayer zone reduces the strength of printed composites by hindering moisture interdiffusion and intermixing of paste from subsequent layers, leading to weak hydrate formation across adjacent layers. Previous studies have reported the printing time gap and bleeding characteristics, as well as the structural buildup of the mixture, as the two most important parameters governing the porosity and strength of the interlayer [46,47].
Printed samples exhibited orientation-dependent load-bearing capacity in all mixtures at both 7 and 28 days. Furthermore, the loading direction with the highest load-bearing capacity varied with mixture and maturity. For instance, for the REF mixture, the loading direction with the highest strength was B at 7 days, followed by C and A; at 28 days, the ranking changed to A, C, and B, respectively.
Even though variability in the load-bearing capacity was observed in all mixtures, its magnitude varied with the mixture formulation and loading direction. Considering the highest and lowest strength values recorded for each loading direction at 28 days, the largest difference was observed between loading directions A and C, with a 35% difference in the P-FA40-F mixture. In the P-REF-F mixture, the observed difference was 4%, which was between C and B. As for the remaining mixtures, the observed differences were 19%, 21%, and 31% for P-BFS40-F, P-FA20-F, and P-BFS20-F mixtures, respectively.
The effect of micro-steel fiber addition on the compressive strength may be attributed to the orientation of fibers under extrusion pressure, which aligns most fibers parallel to the printing direction. Hence, fiber alignment may affect the load-bearing capacity depending on the direction of the applied load with respect to the fiber orientation [22,48].
Examining the effect of BFS and FA in mixtures reinforced with micro-steel fibers shows that, unlike in plain mixtures where BFS and FA addition improved the strength of molded and some printed samples, especially at 28 days, in fibrous mixtures the addition of BFS and FA did not enhance the strength in both molded and printed samples, with the exception of increases in M-BFS40-F (2%), P-BFS40-F (10%), and P-FA20-F (17%) at 7 days. In all other mixtures and sample types, the addition of BFS and FA reduced strength. The decrease in strength upon the addition of micro-steel fibers may be attributed to the balling effect, which leads to the formation of macropores in the vicinity of the fibers [13,16]. Additionally, the fiber volume used in this study is below the recommended range (2–5%) for enhanced performance under compressive loads [49,50].

3.3. Anisotropy Behavior Assessment

3.3.1. Anisotropy Quantification of Plain Mixtures

Figure 17 presents the calculated absolute anisotropy coefficient (I3D) at 7 and 28 days for plain 3D-printed concrete containing various ratios of BFS and FA. Uniform compaction of conventionally cast concrete can effectively improve the internal structure of homogeneous cement-based composites. Hence, conventionally cast concrete is fundamentally considered to exhibit isotropic behavior during modeling mainly due to the presence of formwork exerting confinement during casting and compaction [51]. Therefore, for the quantification of I3D, mold-cast samples were assumed to be homogeneous, exhibiting isotropic behavior. Hence, the I3D of mold-cast samples equals zero. Accordingly, for printed samples, the further from zero the quantified I3D, the greater the anisotropy. Previous studies have used a similar assumption for quantifying the I3D of printed composites [49,52]. It is worth noting that since I3D is quantified by comparing the strength of printed samples from each orthogonal loading direction to that of mold-cast samples, it captures the combined effect of both the overall strength reduction associated with the 3D-printing process (such as interlayer voids, weak compaction, and weaker interfacial transition zones) and isolated intra-directional anisotropy (strength variations among the different loading directions A, B, and C).
Figure 17. Absolute anisotropy coefficient (I3D) at 7 and 28 days for plain 3D-printed concrete mixtures containing varying proportions of BFS and FA.
The findings of the present study show that all mixtures exhibited anisotropic behavior at both 7 and 28 days (Figure 17). The computed I3D increased with curing prolongation in all mixtures. Furthermore, the incorporation of BFS and FA as a partial replacement for OPC did not mitigate the I3D at 7 and 28 days of standard water curing. The REF mixture exhibited the lowest anisotropy, while BFS20 had the highest at both 7 and 28 days. In comparison to the REF mixture, BFS- and FA-bearing mixtures exhibited a higher I3D at both 7 and 28 days. Accordingly, the addition of BFS and FA led to an increase in I3D of 284%, 131%, 89%, and 179% at 7 days, as well as 180%, 123%, 53%, and 150% at 28 days for BFS20, BFS40, FA20, and FA40, respectively. The obtained results indicate that while the increase in BFS content led to a reduction in I3D, the increase in FA content increased the I3D at both 7 and 28 days. Previous studies have attributed the anisotropic behavior of 3D-printed composites to differences in the properties of the filament cores and the interlayer transition zone. This heterogeneity promotes direction-dependent load-bearing behavior observed in printed composites. The increase in I3D with the addition of BFS and FA may be attributed to the fact that at early stages of hydration, SCM-bearing mixtures may lead to lower cross-linked C-S-H across successive layers due to the dilution effect and latent hydraulic behavior [53].
Figure 18 presents the effect of various BFS and FA replacement ratios for CEM I on the intra-directional anisotropy coefficient (Idir) of 3D-printed concrete modified with various ratios of BFS and FA at 7 and 28 days of curing. The quantified Idir reflects the true anisotropy between the various loading directions of printed samples, with the strength loss due to lack of compaction isolated. The recorded results show that the incorporation of BFS and FA caused an increase in Idir at both 7 and 28 days, with an exception for the FA40 mixture at 28 days, where Idir decreased by 21%. Accordingly, increases in Idir of 144%, 33%, 44%, and 50% at 7 days, as well as 164%, 28%, and 43% at 28 days were observed for BFS20, BFS40, FA20, and FA40, respectively, compared to REF. The observed increase in Idir by BFS and FA inclusion has been reported in previous studies and was attributed to the formation of a weaker interlayer region by these SCMs due to the dilution effect and latent hydraulic behavior [53].
Figure 18. Intra-directional anisotropy coefficient (Idir) at 7 and 28 days for plain 3D-printed concrete mixtures containing varying proportions of BFS and FA.
Analyzing the computed I3D and Idir in plain mixtures shows that while I3D increases with curing prolongation, Idir decreases with prolongation of curing. This may be attributed to the faster gain of strength observed in mold-cast samples than in their printed counterparts, which increases the absolute strength gap between mold-cast and printed samples. On the other hand, the decrease in Idir with curing prolongation may be attributed to the progress of hydration across printed samples, which has been found to occur with curing progression, densifying the interlayer region, and homogenizing the relative strength differences within the printed samples.

3.3.2. Anisotropy Quantification of Micro-Steel Fiber Reinforced Mixtures

Figure 19 illustrates the absolute anisotropic coefficient (I3D) for fiber-reinforced 3D-printed concrete containing various proportions of BFS and FA. Results show that the incorporation of BFS and FA in micro-steel fiber-reinforced 3D-printed composites led to an increase in the I3D in all mixtures, especially at 28 days. Increases in I3D of 24%, 61%, 31%, and 5% were recorded for BFS20-F, BFS40-F, FA20-F, and FA40-F mixtures, respectively, compared with the REF-F at 28 days. Although I3D increased in both plain and reinforced mixtures with the addition of BFS and FA, particularly at 28 days, comparisons of counterpart pairs reveal that the REF mixture experienced the most pronounced increase upon fiber reinforcement. Specifically, while microfibers caused a drastic increase in REF-F, certain SCM-bearing mixtures such as BFS20-F and FA40-F exhibited a decrease in I3D relative to their plain counterparts. Furthermore, although BFS40-F and FA20-F still showed an increase upon fiber addition, the magnitude of this increase was smaller than that observed in the REF-F. Consequently, combining microfibers with SCMs mitigated the fiber-induced escalation in I3D relative to the reinforced REF mixture containing CEM I as the sole binder. A comparison of plain and reinforced mixtures shows that at 7 days, micro-steel fiber addition increased the I3D in all mixtures except the FA40-F mixture, where it decreased by 2%. At 28 days, the incorporation of micro-steel fibers increased the I3D by 96% (REF-F), 42% (BFS40-F), and 67% (FA20-F), whereas it decreased by 13% (BFS20-F) and 17% (FA40-F). Moreover, it is observed that the addition of BFS and FA mitigated the fiber-induced increase in I3D at both 7 and 28 days. In other words, while the REF mixture experienced a drastic 96% increase in I3D upon fiber addition, the SCM-containing mixtures mitigated this increase. Nonetheless, the overall I3D values of fiber-reinforced SCM samples remained higher compared to the REF-F mixture. This may be attributed to the optimization of the fresh properties of the mixture in the presence of microfibers, enhancing the fiber-matrix ITZ. It may be inferred that SCMs may optimize fiber dispersion and matrix bonding, compensating for the negative effect of printing operations. Furthermore, the presence of SCMs may densify the Ca(OH)2-rich fiber-matrix ITZ by the formation of additional C-S-H through pozzolanic reaction.
Figure 19. Absolute anisotropy coefficient (I3D) at 7 and 28 days for micro-steel fiber-reinforced 3D-printed concrete mixtures containing varying proportions of BFS and FA.
Figure 20 presents the effect of various BFS and FA replacement ratios for CEM I on the intra-directional anisotropy coefficient (Idir) of micro-steel fiber reinforced 3D-printed concrete modified with various ratios of BFS and FA at 7 and 28 days of curing. The findings of the present study show that the inclusion of micro-steel fiber reinforcement led to a decrease in Idir in all mixtures except for P-FA40-F at 28 days. Hence, it may be inferred that the addition of microfibers may have counteracted the adverse effect of printing, homogenizing the Idir. Accordingly, Idir decreased by 71%, 24%, 11%, and 10% in reinforced P-REF-F, P-BFS20-F, P-BFS40-F, and P-FA20-F mixtures compared to their unreinforced counterpart at 28 days. Nevertheless, even though BFS- and FA-bearing mixtures performed better, reducing Idir in the presence of microfibers (than in plain ones), they still exhibited higher Idir than the P-REF-F mixture at 28 days. In comparison with P-REF-F, Idir increased by 7, 4, 4.5, and 8.25 times for P-BFS20-F, P-BFS40-F, P-FA20-F, and P-FA40-F, respectively, at 28 days.
Figure 20. Intra-directional anisotropy coefficient (Idir) at 7 and 28 days for micro-steel fiber reinforced 3D-printed concrete mixtures containing varying proportions of BFS and FA.
Analyzing the computed I3D and Idir in reinforced mixtures shows that while I3D increased with micro-steel fiber addition, especially in REF-F (96%), BFS40-F (42%), and FA20-F (67%), Idir decreases considerably with microfiber addition, decreasing by 71% in P-REF-F, 24% in P-BFS20-F, 11% in P-BFS40-F, and 10% in P-FA20-F at 28 days. The observed increase in I3D may be explained by the enhancement of mold-cast strength by fiber inclusion, whereas in printed samples, fiber addition may not fully bridge across the interlayer to compensate for the weakness of this region, which still results in reduced strength in printed samples, widening the gap compared to their molded counterpart [54]. On the other hand, Idir decreased considerably in all mixtures compared to their plain counterpart. This may be attributed to fibers enhancing interlayer strength and reducing the load-bearing discrepancy between different loading directions.

3.4. Splitting Tensile Strength Performance

3.4.1. Splitting Tensile Strength of Plain Mixtures

The experimental results illustrating the effect of partially replacing OPC with BFS and FA at 20% and 40% by weight on the 7- and 28-day split tensile strength of 3D-printed concrete are presented in Figure 21. The results show that the split tensile strength of the developed mixtures was significantly affected by the type and replacement ratio of the SCMs used, as well as by the sample-production technique.
Figure 21. Splitting tensile strength of mold-cast and 3D-printed specimens without micro-steel fiber reinforcement at 7 and 28 days.
The 7- and 28-day split tensile strength of mold-cast samples is presented in Figure 21. The findings show that incorporating BFS and FA enhanced the strength of these mixtures, especially during extended curing periods. In other words, the effect of BFS and FA additions became more pronounced as curing progressed. Accordingly, unlike on the 7th day, when BFS and FA had no significant effect, on the 28th day, strength increases of 23%, 27%, and 32% were observed compared with M-REF for M-BFS20, M-BFS40, and M-FA40, respectively. M-FA20 was an exception, with a slight 4% loss in strength.
In printed samples, strength decrement was observed in all mixtures at both ages compared to their molded counterparts. Also, the loss of strength due to printing was exacerbated by the addition of BFS and FA compared with REF. Compared to molded samples, strength decreased by 2%, 46%, 37%, 16%, and 24% at 7 days, as well as 1%, 58%, 29%, 17%, and 43% at 28 days, for P-REF, P-BFS20, P-BFS40, P-FA20, and P-FA40 mixtures, respectively. While the strength loss due to printing was negligible in the REF mixtures, it increased in BFS-and FA-bearing mixtures. This is further seen by evaluating the printed samples among themselves. It can be seen that, unlike in molded samples, the addition of BFS and FA worsened the strength of the developed 3D-printed concrete at both 7 and 28 days compared to P-REF. Strength reductions of 41%, 33%, 12%, and 47% at 7 days and 48%, 9%, 20%, and 24% at 28 days for P-BFS20, P-BFS40, P-FA20, and P-FA40, respectively, were recorded. In accordance with previous studies, the observed loss of strength in printed samples with pozzolan addition is commonly associated with slower or incomplete pozzolanic reaction at early ages, resulting in a weaker, more porous interlayer region [53].
Overall, strength gain with curing extension was observed across all mixtures, both molded and printed, suggesting improved hydration. Hence, given the latent hydraulic behavior of pozzolans, the strength of BFS- and FA-bearing mixtures is expected to improve with extended curing.

3.4.2. Splitting Tensile Strength of Micro-Steel Fiber Reinforced Mixtures

The split tensile strength values recorded at the 7th and 28th days of standard water curing for developed printable mixtures with BFS and FA substituting OPC and reinforced with micro-steel fibers are given in Figure 22.
Figure 22. Splitting tensile strength of mold-cast and 3D-printed specimens with micro-steel fiber reinforcement at 7 and 28 days.
The findings show the effect of incorporating micro-steel fibers in printable mixtures modified with BFS and FA on the split strength of molded and printed samples. Additionally, the difference in performance between printed and molded samples is clearly evident in the results.
In molded samples, the addition of micro-steel fibers significantly improved the split tensile strength performance of the developed mixtures. Strength increments of 86%, 64%, 83%, 58%, and 72% at 7 days and 104%, 70%, 63%, 82%, and 22% at 28 days for M-REF-F, M-BFS20-F, M-BFS40-F, M-FA20-F, and M-FA40-F occurred compared to plain molded samples, respectively. The increase in strength with the addition of fibers can be attributed to delayed crack formation and the crack-bridging properties of steel fibers.
Similarly, in printed samples, the addition of micro-steel fibers increased the 7- and 28-day split tensile strength of the developed mixtures. Accordingly, strength increases of 53%, 73%, 38%, 12%, and 35% at 7 days, as well as 60%, 96%, 5%, 31%, and 35% for P-REF-F, P-BFS20-F, P-BFS40-F, P-FA20-F, and P-FA40-F, occurred compared to plain printed samples, respectively. This finding demonstrates that combining micro-steel fiber with an optimized mix design can mitigate the strength loss caused by printing in plain mixtures. Previous studies have reported similar findings [10].
When examining reinforced samples, molded samples consistently yielded higher split tensile strength values than their printed counterparts across all mixtures and ages. In other words, printing reduced the strength of developed mixtures across all mixtures at both 7 and 28 days. Losses in strength of 19%, 43%, 52%, 40%, and 41% at 7 days and 22%, 51%, 54%, 40%, and 36% at 28 days for P-REF-F, P-BFS20-F, P-BFS40-F, P-FA20-F, and P-FA40-F occurred compared to mold-cast samples, respectively.
Additionally, although strength losses occurred in all mixtures, pozzolan-bearing mixtures experienced greater losses after printing than REF, which may be attributed to the latent hydraulic behavior of pozzolans.

3.5. Interlayer Shear Bond Strength Performance

3.5.1. Interlayer Shear Bond Strength of Plain Mixtures

Results presented in Figure 23 illustrate the shear bond strength performance of printable mixtures containing BFS and FA as partial substitution for OPC at 7 and 28 days of standard water curing. Figure 24 shows representative mold-cast and printed samples after a double shearing test. The observed failure mode during the double shearing test was characterized by a pure interface failure, where the shear failure occurred precisely along the shear plane corresponding to the interlayer transition line, leading to a complete separation of the layers (layer debonding) for printed samples. In molded samples, a crack pattern initiated at the notch was observed. This confirms that failure occurred along the shear plane. Similar crack patterns were reported by [31]. These findings clearly indicate that incorporating BFS and FA enhanced the shear performance of the developed mixtures at 7 and 28 days, particularly in molded samples. In molded samples, the incorporation of BFS and FA increased the shear bond strength by 25%, 45%, and 24% at 7 days, and by 11%, 31%, and 3% at 28 days for M-BFS20, M-BFS40, and M-FA20, respectively, compared to M-REF. Only M-FA40 experienced an 8% loss in strength at 7 days and a 20% loss at 28 days.
Figure 23. Shear bond strength of mold-cast and 3D-printed specimens without micro-steel fiber reinforcement at 7 and 28 days.
Figure 24. Typical failure mode for printed (a) and mold-cast (b) samples after double shearing test.
Furthermore, a decrease in shear bond strength was observed in printed samples compared to their molded counterparts in all mixtures at both 7 and 28 days. Accordingly, a decrease in strength of 39%, 67%, 54%, 78%, and 42% at 7 days and 35%, 52%, 12%, 72%, and 10% at 28 days occurred in printed samples compared to molded samples for P-REF, P-BFS20, P-BFS40, P-FA20, and P-FA40, respectively. The loss of strength due to printing has been reported in the literature and is associated with weak interlayer zones.
Examining printed samples among themselves shows that the effect of pozzolans on the shear bond strength of printable mixtures varies with the type and replacement ratio of the pozzolan. Accordingly, the utilization of 40% BFS improved strength by 10% and 76% at 7 and 28 days, respectively, compared to P-REF. Similarly, P-FA40 increased the strength by 10% at 28 days. In all other mixtures, the use of BFS and FA led to a loss in strength of 34%, 56%, and 13% at 7 days for P-BFS20, P-FA20, and P-FA40, as well as 18% and 55% at 28 days for BFS20 and FA20, respectively, compared to P-REF.

3.5.2. Interlayer Shear Bond Strength of Micro-Steel Fiber Reinforced Mixtures

The 7- and 28-day shear bond strength of developed mixtures after the addition of micro-steel fibers is given in Figure 25. Results indicate a difference in the shear performance of molded and printed samples, as well as the effect of BFS and FA on the strength of these composites.
Figure 25. Shear bond strength of mold-cast and 3D-printed specimens with micro-steel fiber reinforcement at 7 and 28 days.
In molded samples, the incorporation of micro-steel fibers enhanced the strength of the developed printable mixtures at both 7 and 28 days. Strength increments of 78%, 31%, 5%, 6%, and 1% at 7 days and 1%, 11%, 9%, 31%, and −10% occurred for M-REF-F, M-BFS20-F, M-BFS40-F, M-FA20-F, and M-FA40-F, respectively, compared to their plain counterparts.
In printed samples, the addition of microfibers enhanced the strength of the developed mixtures when 20% BFS and FA were used as OPC substitutes; in all other mixtures, it reduced the shear bond strength. Accordingly, increases in strength of 46% and 4% for P-BFS20-F, and 64% and 21% for P-FA20-F, were observed at 7 and 28 days, respectively, compared to their plain counterparts. In other mixtures, strength losses of up to 67% at 7 days and 65% at 28 days for P-BFS40-F were recorded.
Analysis of fiber-reinforced mixtures shows that, even after the addition of micro-steel fibers, the printing-induced strength loss observed in plain mixtures persisted. In comparison to molded samples, printed samples exhibited losses in strength of 66%, 64%, 86%, 67%, and 45% at 7 days, as well as 44%, 54%, 72%, 74%, and 53% at 28 days, respectively, for P-REF-F, P-BFS20-F, P-BFS40-F, P-FA20-F, and P-FA40-F. Pozzolan-bearing mixtures experienced a greater loss of strength than REF after printing.
Additionally, it was observed that, in the presence of microfibers, unlike in molded samples, where the incorporation of BFS and FA enhanced composite strength, in fiber-reinforced printed samples the addition of BFS and FA caused strength decreases at both 7 and 28 days. Strength decreases of up to 63% (P-BFS40-F) and 38% (P-FA40-F) at 7 and 28 days were observed compared to REF, respectively. Furthermore, the influence of SCM substitution on 28-day shear strength was highly dependent on the production method. While SCM incorporation, particularly BFS, enhanced or maintained the shear performance of mold-cast samples, printed counterparts experienced strength degradation at higher replacement ratios.

3.6. Direct Tensile Strength Performance

3.6.1. Direct Tensile Strength of Plain Mixtures

The interlayer tensile bond strength of printable plain mixtures containing 0%, 20%, and 40% BFS or FA as substitutes for OPC is presented in Figure 26. The figure presents results for both molded and printed samples at 7 and 28 days of standard water curing. Figure 27 presents a representative sample after direct tensile strength testing. The addition of BFS and FA as partial replacements for OPC affected the tensile strength of the developed printable 3D-printed concrete differently, depending on the replacement ratio, testing age, and sample production method.
Figure 26. Direct tensile strength of mold-cast and 3D-printed specimens without micro-steel fiber reinforcement at 7 and 28 days.
Figure 27. Typical failure after direct tensile strength test.
During direct tensile testing, the observed failure mode was characterized by a complete separation of layers at the interlayer region. For mold-cast samples, the separation occurred along the notch openings. It is worth noting that careful analysis was performed after each test to ensure that failure did not occur at the epoxy region.
In molded samples, the inclusion of BFS and FA enhanced the direct tensile strength at 7 days across all mixtures, except for FA20, compared with the REF mixture. Strength increments of 26%, 63%, and 62% were recorded from M-BFS20, M-BFS40, and M-FA40 respectively. The performance of mixture FA20 was similar to that of the REF mixture. Compared with the REF mixtures, the effect of BFS and FA addition on the tensile bond strength enhancement of the developed printable mixtures was negligible at 28 days. Accordingly, while M-BFS40 and M-FA40 exhibited slight increases of 1% and 5%, M-BFS20 and M-FA20 showed slight strength decrements of 8% and 18%, respectively.
In printed samples, the partial replacement of OPC with BFS and FA increased the direct tensile strength of the developed printable mixtures at both 7 and 28 days, particularly at a 40% replacement ratio. Accordingly, strength increments of 67% and 48% at 7 days and 14% and 17% at 28 days were observed in the P-BFS40 and P-FA40 mixtures, respectively, compared to REF. In contrast, strength decreased by 33% and 26% at 7 days, and by 8% and 49% at 28 days for P-BFS20 and P-FA20, compared to P-REF. Furthermore, strength increased with curing age across all mixtures, for both molded and printed samples. An increase in direct tensile strength was observed at a 40% replacement ratio. Previous literature suggests that such strength improvements may be attributed to the physical filler effect of BFS and FA rather than a primary pozzolanic effect [1,37]. Furthermore, while incorporating high-aspect-ratio microfibers can increase local porosity near the fibers due to the balling effect, prior studies indicate that high-volume BFS and FA can help refine the interfacial zone between the fiber and the matrix by acting as effective fillers [1,55]. The findings of this study further show that printed samples exhibited different performance from molded ones in all mixtures and both testing ages. The strength of printed samples decreases in all mixtures at both 7 and 28 days compared with molded samples. A decrease in strength of 29%, 6%, 71%, 48%, and 35% at 7 days, as well as 30%, 13%, 36%, 56%, and 21% at 28 days, for P-REF, P-BFS20, P-BFS40, P-FA20, and P-FA40, respectively, occurred in printed samples in comparison to molded ones. In other words, printing reduced the bond strength of the developed 3D-printed concrete. As expected, this can be attributed to the weakness of the interlayer zone, an intrinsic consequence of fabricating objects using extrusion-based 3D printing with concrete. The interlayer interfacial zone between adjacent layers has been reported to contain more entrapped air macropores than the bulk part of the layer, leading to a lower load-bearing capacity.
Examining the effect of BFS and FA on the post-printing interlayer bond strength of developed 3D-printed concrete shows that although the addition of BFS and FA could not make up for the loss in strength due to printing, their presence mitigated the severity of the loss in strength caused by printing. Accordingly, at 28 days, the 30% strength decrease observed in the P-REF was reduced to 13% and 21% by substituting 20% BFS and 40% FA for OPC, respectively.

3.6.2. Direct Tensile Strength of Micro-Steel Fiber Reinforced Mixtures

Figure 28 presents the 7- and 28-day direct tensile strength values recorded for the developed 3D-printed concrete with various SCM ratios and micro-steel fiber as reinforcement.
Figure 28. Direct tensile strength of mold-cast and 3D-printed specimens with micro-steel fiber reinforcement at 7 and 28 days.
The findings show that incorporating micro-steel fibers as reinforcement in mold-cast samples affected the mixtures differently, depending on mixture composition and sample maturity. In the REF mixture, produced with OPC as the sole binding material, the addition of microfibers increased the direct tensile strength by 33% at 7 days but did not affect the 28-day strength. In pozzolan-bearing mixtures, the addition of microfibers caused a slight decrease in the direct tensile strength, except for mixture M-FA20-F, where the strength increased by 40% and 39% at 7 and 28 days, respectively. In BFS-bearing mixtures, the addition of microfibers negatively affected 7-day direct tensile strength but not 28-day strength. Decrements of 9% and 18% occurred for M-BFS20-F and M-BFS40-F, respectively, compared to the plain molded values. In FA-bearing mixtures, while fiber addition improved the strength of M-FA20-F by 40% and 39% at 7 and 28 days, respectively, it decreased the strength of M-FA40-F by 16% at 7 and 28 days, respectively, compared to plain molded samples. The observed decrease in the strength of printed samples has been attributed to the weak interlayer interfacial transition zone formed during printing in previous studies. Previous studies have reported that this region is relatively weaker than the bulk matrix of the printed and molded layers, thereby reducing the strength of printed specimens [56].
In printed samples, the addition of micro-steel fibers improved the strength of the developed 3D-printed concrete at both 7 and 28 days. Strength increases of 64%, −22%, 13%, 130%, and 70% at 7 days, as well as 23%, 5%, 38%, 146%, and -13% at 28 days occurred for P-REF-F, P-BFS20-F, P-BFS40-F, P-FA20-F, and P-FA40-F compared to plain printed samples, respectively. In accordance with previous studies, the enhancement in interlayer bonding strength, such as split tensile, shear bond, and direct tensile strengths, with fiber addition can be attributed to microfibers promoting mechanical interlocking across subsequent layers, leading to fewer interconnected voids and improved resistance to crack propagation [16,57].
The findings of this study also show the effect of printing on the strength of reinforced printable mixtures modified with various ratios of BFS and FA. Results show that printing adversely affected the strength of these composites compared with molded samples at both 7 and 28 days. Accordingly, strength losses of 13%, 20%, 60%, and 14% at 7 days, and 13%, 10%, 11%, 22%, and 17% at 28 days, occurred in the P-REF-F, P-BFS20-F, P-BFS40-F, P-FA20-F, and P-FA40-F mixtures in sequence. The P-FA40-F mixture was an exception, showing a 32% increase at 7 days.

4. Conclusions

In the present study, the effects of the two most commonly employed SCMs, namely BFS and FA, on the anisotropy and mechanical properties of plain and micro-steel fiber-reinforced 3D-printed concrete were experimentally investigated. Accordingly, 3D-printed concrete with a constant water-to-binder ratio of 0.3, an HPMC dosage of 0.14% by binder weight, and a flow diameter of 180 ± 10 mm was developed by replacing 0%, 20%, and 40% of OPC by weight with either BFS or FA. Plain and microfiber-reinforced printable mixtures containing 0.5% micro steel fibers by total volume were comparatively studied in mold-cast and printed samples at 7 and 28 days of standard water curing, using various experiments targeting different properties of interest in concrete. As a result of the experiments, the following conclusions can be made:
  • The effect of BFS and FA as a substitute for OPC on the mechanical properties of plain concrete varied significantly by fabrication technique. Their inclusion generally increased the strength of mold-cast samples but reduced that of printed samples, especially at 28 days:
    • In molded samples, the 28-day strength of plain mixtures increased by 7% (M-BFS20), 14% (M-BFS40), and 5% (M-FA20) in flexural performance, 32% (M-BFS20), 42% (M-BFS40), 10% (M-FA20), and 4% (M-FA40) in compressive performance, 23% (M-BFS20), 27% (M-BFS40), and 32% (M-FA40) in splitting tensile performance, 11% (M-BFS20) and 31% (M-BFS40) in shear bond performance, as well as 1% (M-BFS40) and 5% (M-FA40) in direct tensile performance. Nonetheless, strength decrements of 10% (M-FA40) in flexure, 4% (M-FA20) in splitting tensile, 20% (M-FA40) in shear bond performance, and 8% (M-BFS20) and 18% (M-FA20) in direct tensile were observed compared to M-REF.
    • In printed samples, the 28-day strength of plain mixtures decreased by up to 32% (P-FA40) in flexure, 48% (P-BFS20), 9% (P-BFS40), 20% (P-FA20), and 24% (P-FA40) in splitting tensile; 18% (P-BFS20) and 55% (P-FA20) in shear strength, as well as 8% (P-BFS20) and 49% (P-FA20) in direct tensile strength compared to P-REF. P-BFS40 and P-FA40 showed performance enhancements of 76% and 10%, respectively, compared to P-REF at 28 days in shear bond strength.
  • Mold-cast samples generally exhibited higher strength performance than their printed counterparts in both plain and reinforced mixtures. However, printing enhanced flexural toughness across all mixtures and improved flexural strength depending on the specific mixture composition:
    • Compared to their mold-cast counterparts, the 28-day strength of plain and reinforced printed samples decreased by up to 58% (P-BFS20), and 43% (P-FA40), as well as 54% (P-BFS40-F) and 40% (P-FA20-F) in splitting tensile; 52% (P-BFS20), 72% (P-FA20), as well as 72% (P-BFS40-F) and 74% (P-FA20-F) in shear bond strength; 36% (P-BFS40) and 56% (P-FA20), as well as 11% (P-BFS40-F), 22% (P-FA20-F) in direct tensile. In flexural performance, printing led to an increase in the 28-day strength for P-BFS20 and P-REF of 3% and 22%, as well as 77%, 21%, and 2%, for P-REF-F, P-BFS40-F, and P-FA40-F, whereas it decreased the strength of P-BFS40 and P-FA20 by 5% and 17%, as well as P-BFS20-F and P-FA20-F by 12% and 2%, respectively compared to their molded counterparts.
    • Printing enhanced toughness across all mixtures included in plain samples, especially at 28 days. Accordingly, in plain mixtures, printing increased toughness by 26– 76% relative to mold-cast samples at 28 days. Similarly, compared to mold-cast samples, the increase in toughness of reinforced printed samples ranged from 17% to 131% at 28 days.
  • Printed samples exhibited direction-dependent load-bearing capacity in all mixtures in the absence or presence of micro-steel fiber reinforcement. Nonetheless, when the difference in the load-bearing capacity is comparatively examined between the REF mixture and BFS- and FA- bearing mixtures, it was observed that the strength gap between mold-cast and printed samples with respect to each loading direction grew wider in the presence of BFS and FA compared to REF. Accordingly, strength decrements of 31%, 54%, and 60% (P-BFS20), 30%, 45%, and 39% (P-BFS40),15%, 24%, and 36% (P-FA20), 38%, 44%, and 46% (P-FA40) occurred in the A, B, and C loading directions compared to their respective mold-cast counterparts. Meanwhile, strength losses in the REF mixture at 28 days were 11%, 13%, and 26% (P-REF), respectively.
  • The absolute anisotropy coefficient (I3D), which depicts the overall anisotropy of printed samples relative to their mold-cast counterparts, increased with curing age in plain mixtures and was generally exacerbated with micro-steel fiber addition—most notably causing a 96% increase in the reference mixture. However, microfiber addition actually decreased I3D in certain SCM-containing mixtures, namely BFS20-F and FA40-F at 28 days. Additionally, the incorporation of BFS and FA successfully mitigated the high fiber-induced accentuation in absolute anisotropy compared to the high increase observed in the REF-F mixture. On the other hand, the intra-directional anisotropy coefficient (Idir), which isolates intrinsic directional variability from overall printing-induced strength loss, decreased in plain mixtures with curing prolongation and dropped in the presence of microfibers across most mixtures (except P-FA40-F at 28 days), highlighting the role of microfibers in homogenizing directional mechanical performance.
  • Incorporating micro-steel fibers altered the failure behavior of developed mixtures from brittle to ductile, enhancing the toughness of both printed and mold-cast samples in all mixtures, with flexural toughness increasing by up to 17.8 (M-BFS40-F) and 19.6 (P-REF-F) fold at 28 days compared to their plain counterparts. Additionally, it led to deflection hardening in P-REF-F and P-BFS40-F. Furthermore, while micro-steel fiber addition enhanced the 28-day compressive, splitting tensile, shear, and direct tensile strengths in mold-cast samples for all mixtures, its effect on printed samples changed based on the composition of the mixture. Accordingly, while it enhanced the 28-day flexural strength by 27% (P-REF-F), 12% (P-BFS40-F), and 5% (P-FA20-F); direct tensile strength by 23% (P-REF-F), 38% (P-BFS40-F), and 146% (P-FA20-F), it caused a notable 65% reduction in shear strength for P-BFS40-F; direct tensile strength also decreased by 13% for P-FA40-F; flexural strength decreased by 24% (P-BFS20-F), as well as 13%, 11%, 12%, 12%, and 11%, for M-REF-F, M-BFS20-F, M-BFS40-F, M-FA20-F, and M-FA40-F, respectively compared to their plain counterparts at 28 days.
  • The findings of this study provide engineers and designers with practical experimental insights, demonstrating that extrusion-based 3D printing combined with fiber-reinforced mixtures incorporating BFS and FA offers a viable approach to mitigating concrete’s inherent brittleness. The incorporation of micro-steel fibers significantly enhances flexural toughness and energy absorption, providing a framework to design more ductile structural elements with superior resistance against dynamic loads. Furthermore, incorporating BFS and FA allows for a reduction in cement dosage while helping to counteract printing-induced mechanical losses, expanding the practical applications of digital fabrication in structural engineering contexts.
  • Future research should investigate and establish the exact correlations between extrusion shear stresses, pumping mechanics, and the resulting micro-fiber network orientation. Overall, evaluating the interfacial bond integrity of printed elements applied to existing substrates presents a viable path for structural retrofitting applications, whereas scaling up to full-scale components subjected to cyclic and dynamic loading remains crucial to validate their constitutive post-crack energy absorption and seismic performance.

Author Contributions

The authors confirm contribution to the paper as follows: Conceptualization, Ç.Y.; methodology, B.C., E.K. and Ç.Y.; formal analysis, Ç.Y.; investigation, E.K. and B.C.; resources, Ç.Y., B.F. and H.Y.; writing—original draft preparation, B.C., E.K. and Ç.Y.; writing—review and editing, Ç.Y., B.F., H.Y. and O.Ç.; visualization, B.C. and E.K.; supervision, O.Ç.; project administration, Ç.Y.; funding acquisition, Ç.Y. All authors have read and agreed to the published version of the manuscript.

Funding

This study was supported by the Scientific and Technological Research Council of Türkiye (TÜBİTAK, Project No: 121M284). The authors gratefully acknowledge TÜBİTAK. The second author, Ebru Kaya, acknowledges the support of the YÖK 100/2000 Ph.D. Scholarship program.

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding authors.

Acknowledgments

The authors would like to thank Limak Cement, OYAK Cement, and ODAŞ Energy companies for material support. Special thanks are extended to Ebru Sipahioğlu, Erdal Sarıtop, Oğuz Kır, Şirin Arzu Ötken, and Ahmet Avcıoğlu for their assistance in supplying materials.

Conflicts of Interest

The authors declare no conflicts of interest.

Abbreviations

The following abbreviations are used in this manuscript:
3DPC3D-printed concrete
3DPPM3D-printable plain mortars
BFSblast furnace slag
FAfly ash
HPMChydroxypropyl methylcellulose
LVDTlinear variable differential transformer
OPCordinary Portland cement
PEpolyethylene
PP polypropylene
PVApolyvinyl alcohol
SCMssupplementary cementitious materials
SPsuperplasticizer

References

  1. Rehman, A.U.; Kim, J.H. 3D Concrete Printing: A Systematic Review of Rheology, Mix Designs, Mechanical, Microstructural, and Durability Characteristics. Materials 2021, 14, 3800. [Google Scholar] [CrossRef] [Scilit]
  2. Mechtcherine, V.; Buswell, R.; Kloft, H.; Bos, F.P.; Hack, N.; Wolfs, R.; Sanjayan, J.; Nematollahi, B.; Ivaniuk, E.; Neef, T. Integrating Reinforcement in Digital Fabrication with Concrete: A Review and Classification Framework. Cem. Concr. Compos. 2021, 119, 103964. [Google Scholar] [CrossRef] [Scilit]
  3. Kaliyavaradhan, S.K.; Ambily, P.S.; Prem, P.R.; Ghodke, S.B. Test Methods for 3D Printable Concrete. Autom. Constr. 2022, 142, 104529. [Google Scholar] [CrossRef] [Scilit]
  4. Zhang, C.; Nerella, V.N.; Krishna, A.; Wang, S.; Zhang, Y.; Mechtcherine, V.; Banthia, N. Mix Design Concepts for 3D Printable Concrete: A Review. Cem. Concr. Compos. 2021, 122, 104155. [Google Scholar] [CrossRef] [Scilit]
  5. Kaya, E.; Ciza, B.; Yalçınkaya, Ç.; Felekoğlu, B.; Yazıcı, H.; Çopuroğlu, O. A Comparative Study on the Effectiveness of Fly Ash and Blast Furnace Slag as Partial Cement Substitution in 3D Printable Concrete. J. Build. Eng. 2025, 108, 112841. [Google Scholar] [CrossRef] [Scilit]
  6. Panda, B.; Tan, M.J. Rheological Behavior of High Volume Fly Ash Mixtures Containing Micro Silica for Digital Construction Application. Mater. Lett. 2019, 237, 348–351. [Google Scholar] [CrossRef] [Scilit]
  7. Muthukrishnan, S.; Kua, H.W.; Yu, L.N.; Chung, J.K.H. Fresh Properties of Cementitious Materials Containing Rice Husk Ash for Construction 3D Printing. J. Mater. Civ. Eng. 2020, 32, 04020195. [Google Scholar] [CrossRef] [Scilit]
  8. Xia, Z.; Geng, J.; Zhou, Z.; Liu, G. Comparative Analysis of Polypropylene, Basalt, and Steel Fibers in 3D Printed Concrete: Effects on Flowability, Printability, Rheology, and Mechanical Performance. Constr. Build. Mater. 2025, 465, 140098. [Google Scholar] [CrossRef] [Scilit]
  9. Alonso-Canon, S.; Blanco-Fernandez, E.; Castro-Fresno, D.; Yoris-Nobile, A.I.; Castañon-Jano, L. Reinforcements in 3D Printing Concrete Structures. Arch. Civ. Mech. Eng. 2022, 23, 25. [Google Scholar] [CrossRef] [Scilit]
  10. Zat, T.; de Freitas Daudt, N.; Boaretto, J.; Robayo-Salazar, R.; de Matos, P.R.; Rodríguez, E.D. Mechanical Behavior of 3D-Printed Concretes Reinforced with Steel and Rock Wool Microfibers. J. Build. Eng. 2026, 127, 116269. [Google Scholar] [CrossRef] [Scilit]
  11. Ramezani, A.; Modaresi, S.; Dashti, P.; GivKashi, M.R.; Moodi, F.; Ramezanianpour, A.A. Effects of Different Types of Fibers on Fresh and Hardened Properties of Cement and Geopolymer-Based 3D Printed Mixtures: A Review. Buildings 2023, 13, 945. [Google Scholar] [CrossRef] [Scilit]
  12. Dilawar Riaz, R.; Usman, M.; Ali, A.; Majid, U.; Faizan, M.; Jalil Malik, U. Inclusive Characterization of 3D Printed Concrete (3DPC) in Additive Manufacturing: A Detailed Review. Constr. Build. Mater. 2023, 394, 132229. [Google Scholar] [CrossRef] [Scilit]
  13. Jia, Z.; Zhou, M.; Chen, Y.; Wang, W.; Ma, L.; Chen, Y.; Liu, C.; Zhang, Y. Effect of Steel Fiber Shape and Content on Printability, Microstructure and Mechanical Properties of 3D Printable High Strength Cementitious Materials. Case Stud. Constr. Mater. 2024, 20, e03080. [Google Scholar] [CrossRef] [Scilit]
  14. Ma, W.; Wang, G.; Zhou, Y.; Xu, Q.; Dai, Y. Polyacrylonitrile Fiber Reinforced 3D Printed Concrete: Effects of Fiber Length and Content. J. Build. Eng. 2024, 97, 110869. [Google Scholar] [CrossRef] [Scilit]
  15. Xiao, J.; Liu, H.; Ding, T. Finite Element Analysis on the Anisotropic Behavior of 3D Printed Concrete under Compression and Flexure. Addit. Manuf. 2021, 39, 101712. [Google Scholar] [CrossRef] [Scilit]
  16. Nia, S.B.; Shafei, B. Assessment of Fiber Reinforcement and Mixture Performance Requirements for 3D-Printed Fiber-Reinforced Concrete Applications. J. Build. Eng. 2026, 129, 116722. [Google Scholar] [CrossRef] [Scilit]
  17. Kaya, E.; Ciza, B.; Yalçınkaya, Ç.; Felekoğlu, B.; Yazıcı, H.; Çopuroğlu, O. Effect of Hydroxypropyl Methylcellulose and Aggregate Volume on Fresh and Hardened Properties of 3D Printable Concrete. Constr. Build. Mater. 2024, 456, 139253. [Google Scholar] [CrossRef] [Scilit]
  18. Ferrara, L.; Cremonesi, M.; Tregger, N.; Frangi, A.; Shah, S.P. On the Identification of Rheological Properties of Cement Suspensions: Rheometry, Computational Fluid Dynamics Modeling and Field Test Measurements. Cem. Concr. Res. 2012, 42, 1134–1146. [Google Scholar] [CrossRef] [Scilit]
  19. Liu, J.; An, M.; Wang, Y.; Han, S.; Yu, Z. Research on the Relation between Slump Flow and Yield Stress of Ultra-High Performance Concrete Mixtures. Materials 2022, 15, 8104. [Google Scholar] [CrossRef] [Scilit]
  20. Ahmad, J.; Kontoleon, K.J.; Majdi, A.; Naqash, M.T.; Deifalla, A.F.; Ben Kahla, N.; Isleem, H.F.; Qaidi, S.M.A. A Comprehensive Review on the Ground Granulated Blast Furnace Slag (GGBS) in Concrete Production. Sustainability 2022, 14, 8783. [Google Scholar] [CrossRef] [Scilit]
  21. Zahedi, M.; Jafari, K.; Rajabipour, F. Properties and Durability of Concrete Containing Fluidized Bed Combustion (FBC) Fly Ash. Constr. Build. Mater. 2020, 258, 119663. [Google Scholar] [CrossRef] [Scilit]
  22. Yalçınkaya, Ç. Influence of Hydroxypropyl Methylcellulose Dosage on the Mechanical Properties of 3D Printable Mortars with and without Fiber Reinforcement. Buildings 2022, 12, 360. [Google Scholar] [CrossRef] [Scilit]
  23. Yang, L.; Sepasgozar, S.M.E.; Shirowzhan, S.; Kashani, A.; Edwards, D. Nozzle Criteria for Enhancing Extrudability, Buildability and Interlayer Bonding in 3D Printing Concrete. Autom. Constr. 2023, 146, 104671. [Google Scholar] [CrossRef] [Scilit]
  24. TS EN 196-1; Methods of Testing Cement—Part 1: Determination of Strength. Turkish Standards Institution (TSE): Ankara, Türkiye, 2016.
  25. Wang, B.; Yao, X.; Yang, M.; Zhang, R.; Huang, J.; Wang, X.; Dong, Z.; Zhao, H. Mechanical Performance of 3D Printed Concrete in Steam Curing Conditions. Materials 2022, 15, 2864. [Google Scholar] [CrossRef] [Scilit]
  26. ASTM C496/C496M-04; Standard Test Method for Splitting Tensile Strength of Cylindrical Concrete Specimens; ASTM International. West Conshohocken, PA, USA, 2004. [Google Scholar] [CrossRef] [Scilit]
  27. Joh, C.; Lee, J.; Bui, T.Q.; Park, J.; Yang, I.-H. Buildability and Mechanical Properties of 3D Printed Concrete. Materials 2020, 13, 4919. [Google Scholar] [CrossRef] [Scilit]
  28. Chen, Y.; Kuva, J.; Mohite, A.; Li, Z.; Rahier, H.; Al-Neshawy, F.; Shu, J. Investigation of the Internal Structure of Hardened 3D-Printed Concrete by X-CT Scanning and Its Influence on the Mechanical Performance. Materials 2023, 16, 2534. [Google Scholar] [CrossRef] [Scilit]
  29. Wolfs, R.J.M.; Bos, F.P.; Salet, T.A.M. Hardened Properties of 3D Printed Concrete: The Influence of Process Parameters on Interlayer Adhesion. Cem. Concr. Res. 2019, 119, 132–140. [Google Scholar] [CrossRef] [Scilit]
  30. BS EN 12390-6:2023; Testing Hardened Concrete—Part 6: Tensile Splitting Strength of Test Specimens. BSI: London, UK, 2023. [Google Scholar] [CrossRef] [Scilit]
  31. Alchaar, A.S.; Al-Tamimi, A.K. Mechanical Properties of 3D Printed Concrete in Hot Temperatures. Constr. Build. Mater. 2021, 266, 120991. [Google Scholar] [CrossRef] [Scilit]
  32. Yang, Y.; Wu, C.; Liu, Z.; Wang, H.; Ren, Q. Mechanical Anisotropy of Ultra-High Performance Fibre-Reinforced Concrete for 3D Printing. Cem. Concr. Compos. 2022, 125, 104310. [Google Scholar] [CrossRef] [Scilit]
  33. Woo, S.-J.; Yang, J.-M.; Lee, H.; Kwon, H.-K. Comparison of Properties of 3D-Printed Mortar in Air vs. Underwater. Materials 2021, 14, 5888. [Google Scholar] [CrossRef] [Scilit]
  34. Pham, L.; Lu, G.; Tran, P. Influences of Printing Pattern on Mechanical Performance of Three-Dimensional-Printed Fiber-Reinforced Concrete. 33D Print. Addit. Manuf. 2022, 9, 46–63. [Google Scholar] [CrossRef] [Scilit]
  35. Park, J.; Bui, Q.-T.; Lee, J.; Joh, C.; Yang, I.-H. Interlayer Strength of 3D-Printed Mortar Reinforced by Postinstalled Reinforcement. Materials 2021, 14, 6630. [Google Scholar] [CrossRef] [Scilit]
  36. Chougan, M.; Ghaffar, S.H.; Sikora, P.; Chung, S.-Y.; Rucinska, T.; Stephan, D.; Albar, A.; Swash, M.R. Investigation of Additive Incorporation on Rheological, Microstructural and Mechanical Properties of 3D Printable Alkali-Activated Materials. Mater. Des. 2021, 202, 109574. [Google Scholar] [CrossRef] [Scilit]
  37. Liu, H.; Laflamme, S.; Cardinali, A.; Lyu, P.; Rivero, I.V.; Doyle, S.E.; Wang, K. Enhancing 3D-Printed Cementitious Composites with Recycled Carbon Fibers from Wind Turbine Blades. Constr. Build. Mater. 2025, 472, 140650. [Google Scholar] [CrossRef] [Scilit]
  38. Proske, T.; Hainer, S.; Rezvani, M.; Graubner, C.-A. Eco-Friendly Concretes with Reduced Water and Cement Contents—Mix Design Principles and Laboratory Tests. Cem. Concr. Res. 2013, 51, 38–46. [Google Scholar] [CrossRef] [Scilit]
  39. Hatungimana, D.; Özteber, S.; Mardani, A.; El-Hassan, H. Synergistic Effect of SCMs and Fibers on the Mechanical and Durability Performance of Cementitious Mortars. Mater. Today Commun. 2026, 55, 115804. [Google Scholar] [CrossRef] [Scilit]
  40. Yang, Y.; Wu, C.; Liu, Z.; Li, J.; Yang, T.; Jiang, X. Characteristics of 3D-Printing Ultra-High Performance Fibre-Reinforced Concrete under Impact Loading. Int. J. Impact Eng. 2022, 164, 104205. [Google Scholar] [CrossRef] [Scilit]
  41. Pham, L.T.; Trinh, T.D.; Do, Q.T.; Huang, J.Y. Flexural Behavior of Printed Concrete Wide Beams with Dispersed Fibers Reinforced. Res. Eng. Struct. Mater. 2023, 9, 312–322. [Google Scholar] [CrossRef] [Scilit]
  42. Zhang, H.; Zhu, L.; Zhang, F.; Yang, M. Effect of Fiber Content and Alignment on the Mechanical Properties of 3D Printing Cementitious Composites. Materials 2021, 14, 2223. [Google Scholar] [CrossRef] [Scilit]
  43. Tarhan, Y.; Şahin, R. Fresh and Rheological Performances of Air-Entrained 3D Printable Mortars. Materials 2021, 14, 2409. [Google Scholar] [CrossRef] [Scilit]
  44. Eugenin, C.; Navarrete, I.; Brevis, W.; Lopez, M. Air Bubbles as an Admixture for Printable Concrete: A Review of the Rheological Effect of Entrained Air. 3D Print. Addit. Manuf. 2022, 9, 64–80. [Google Scholar] [CrossRef] [Scilit]
  45. Şahin, H.G.; Mardani, A.; Beytekin, H.E. Effect of Silica Fume Utilization on Structural Build-Up, Mechanical and Dimensional Stability Performance of Fiber-Reinforced 3D Printable Concrete. Polymers 2024, 16, 556. [Google Scholar] [CrossRef] [Scilit]
  46. Huang, X.; Yang, W.; Song, F.; Zou, J. Study on the Mechanical Properties of 3D Printing Concrete Layers and the Mechanism of Influence of Printing Parameters. Constr. Build. Mater. 2022, 335, 127496. [Google Scholar] [CrossRef] [Scilit]
  47. Moelich, G.M.; Kruger, J.; Combrinck, R. Modelling the Interlayer Bond Strength of 3D Printed Concrete with Surface Moisture. Cem. Concr. Res. 2021, 150, 106559. [Google Scholar] [CrossRef] [Scilit]
  48. Arunothayan, A.R.; Nematollahi, B.; Ranade, R.; Bong, S.H.; Sanjayan, J.G.; Khayat, K.H. Fiber Orientation Effects on Ultra-High Performance Concrete Formed by 3D Printing. Cem. Concr. Res. 2021, 143, 106384. [Google Scholar] [CrossRef] [Scilit]
  49. Surehali, S.; Tripathi, A.; Neithalath, N. Anisotropy in Additively Manufactured Concrete Specimens under Compressive Loading—Quantification of the Effects of Layer Height and Fiber Reinforcement. Materials 2023, 16, 5488. [Google Scholar] [CrossRef] [Scilit]
  50. Guler, S.; Akbulut, Z.F. Effect of Freeze-Thaw Cycles on Strength and Toughness Properties of New Generation 3D/4D/5D Steel Fiber-Reinforced Concrete. J. Build. Eng. 2022, 51, 104239. [Google Scholar] [CrossRef] [Scilit]
  51. Kabantsev, O. Adaptation of Concrete Model to 3D Printing Technology. Buildings 2024, 14, 3806. [Google Scholar] [CrossRef] [Scilit]
  52. Ma, G.; Li, Z.; Wang, L.; Wang, F.; Sanjayan, J. Mechanical Anisotropy of Aligned Fiber Reinforced Composite for Extrusion-Based 3D Printing. Constr. Build. Mater. 2019, 202, 770–783. [Google Scholar] [CrossRef] [Scilit]
  53. Zhao, X.; Xie, J.; Dai, Q.; Mensah, C. Performance and Carbon Reduction of Binary and Ternary Concrete Systems with Slag Cement and Fly Ash. J. Build. Eng. 2026, 130, 117087. [Google Scholar] [CrossRef] [Scilit]
  54. Ait Balla, M.; Laaguel, F.E.; El Brigui, L.; Maazouz, A.; Lamnawar, K.; Arrakhiz, F.E. Sustainable PLA/PEG Biocomposites Reinforced with Moroccan Biowastes: Comparative Analysis Between Injection Molding and 3D Printing. Sustainability 2026, 18, 5536. [Google Scholar] [CrossRef] [Scilit]
  55. Adili, E.; Kheyroddin, A. Fiber Interfacial Transition Zone Concept for Steel Fiber-Reinforced Concrete by SEM Observation. J. Appl. Res. Technol. 2021, 19, 294–307. [Google Scholar] [CrossRef] [Scilit]
  56. Glotz, T.; Petryna, Y. Experimental Characterization of Anisotropic Mechanical Behaviour and Failure Mechanisms of Hardened Printed Concrete. Materials 2024, 17, 3931. [Google Scholar] [CrossRef] [Scilit]
  57. Xiao, J.; Han, N.; Zhang, L.; Zou, S. Mechanical and Microstructural Evolution of 3D Printed Concrete with Polyethylene Fiber and Recycled Sand at Elevated Temperatures. Constr. Build. Mater. 2021, 293, 123524. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Article metric data becomes available approximately 24 hours after publication online.