Abstract
This study investigates the fretting fatigue behavior of a 2A70 aluminum alloy/42CrMoA steel pair at 115 °C, simulating bolted connections in steel-crown aluminum-skirt composite pistons for marine diesel engines. Single-clamp-head tests were performed at 4, 5, and 6 kN. SEM characterized contact-zone wear and fracture surfaces. The contact zone showed partial slip, with wear concentrated in the peripheral slip region. Wear involved abrasive, adhesive, and contact-fatigue mechanisms. Fracture surfaces exhibited multiple crack origins, where internal metallurgical defects and wear-debris wedging jointly accelerated crack initiation and propagation. A finite element life-prediction model coupling wear and fatigue was developed using the Chaboche nonlinear kinematic hardening constitutive model and the critical plane approach. Predicted lives fell within a factor of two of experimental values. Damage preferentially concentrated at the loading-end edge of the contact zone and propagated inward at approximately 30°. With increasing load, the failure mechanism shifted from damage-propagation-dominated to plasticity-accumulation-dominated. This work provides experimental evidence and a numerical prediction tool for anti-fatigue design of aluminum alloys under high-temperature fretting.
1. Introduction
Fretting [1,2] refers to the relative microscopic sliding between contact surfaces induced by reciprocating contact loads, with displacement amplitudes typically in the micrometer and sub-micrometer range. Currently, there is no effective means to completely prevent the material damage and failure caused by fretting [3]. The resultant material degradation is collectively referred to as fretting damage, which encompasses three forms: fretting fatigue [4,5], fretting wear, and fretting corrosion. Among these, fretting fatigue differs significantly from conventional fatigue, as the contact zone simultaneously sustains both normal and tangential loads, and the damage process is highly insidious, which can markedly reduce the service life of mechanically connected structures and even lead to severe safety accidents.
To obtain the fretting fatigue performance of structures, previous studies have developed typical experimental apparatuses such as bridge-type, single-clamp-head, clamping-type, and dovetail-type devices, and have obtained various types of fretting fatigue performance data for different materials and connection structures. For Ti-6Al-4V blade/disk contacts and dissimilar metal pairings, the results showed that contact configuration and material matching significantly affect fretting fatigue life and contact response [6,7]. For single-crystal nickel and turbine materials under high-temperature environments such as 600 °C, the studies indicated that elevated temperature aggravates fretting damage and markedly changes the fatigue life characteristics [8,9]. The tangential stress range–compressive stress range fretting fatigue design curves provide an engineering criterion for anti-fretting design [10]. For GH4169/FGH96 curved dovetail joints, the high-temperature fretting fatigue performance and life prediction results demonstrated that complex joint structures under high-temperature loading require simultaneous consideration of damage accumulation and life prediction [11]. Meanwhile, the standardization efforts by ASTM International and Neu have specified fretting fatigue specimens, fixture configurations, and testing procedures [12,13]. The above experimental techniques and data provide an important basis for engineering anti-fretting design; however, under complex high-temperature and variable-load conditions such as bolted connections between the steel crown and aluminum skirt of marine diesel engines, the prediction and prevention of fretting damage still face challenges.
In the marine industry, diesel engines serve as the core power plant, and the reliability of their key components directly affects navigation safety and operational efficiency. As the “heart” component of a diesel engine, the piston operates under harsh conditions of high temperature, heavy load, and reciprocating motion, making it one of the components most prone to failure. According to statistics from Alliansz [14], piston and connecting rod failures account for 24.1% of all internal combustion engine failures. It lists various failure characteristics such as piston scuffing, scratching, cylinder seizure, cracking, corrosion, melting, burn-through, carbon deposition, and wear. The failures are then classified by location into three major parts: piston head, piston skirt, and pin boss, with detailed descriptions of the characteristics of each failure, brief analysis processes, and very comprehensive possible causes. As diesel engine performance continues to improve, the requirements for structural strength and fatigue life are increasing.
Aluminum alloys offer a series of advantages, including high thermal conductivity, high electrical conductivity, strong corrosion resistance, low density, high specific strength, excellent formability, and low cost, and they are widely used in fields such as aviation, aerospace, shipbuilding, the nuclear industry, and the ordnance industry. As a heat-resistant aluminum alloy of the Al–Cu–Mg–Fe–Ni system, 2A70 aluminum alloy exhibits pronounced heat-treatment strengthening characteristics. It mainly enhances material performance by forming the Al2CuMg strengthening phase, which has excellent stability at high temperatures and a low tendency to agglomerate, enabling 2A70 aluminum alloy to exhibit excellent heat resistance and to serve stably over the long term in high-temperature environments of 150–250 °C [15]. In addition, it possesses excellent heat-treatment strengthening performance and hot and cold working performance, as well as relatively high specific strength and ductility, and is widely used to manufacture key components such as aircraft engine pistons, impellers, compressor blades, and disks, as well as other parts required to operate in high-temperature environments.
Steel-crown aluminum-skirt composite pistons have become the mainstream choice for medium-speed high-power diesel engines because they can fully exploit the high-temperature resistance of steel and the lightweight advantage of aluminum. However, the core connection structure—the bolted contact interface between the steel crown and aluminum skirt is subject to alternating thermal stresses, reciprocating inertial forces, and differences in material expansion coefficients during service, which easily produce small relative slips with amplitudes typically less than 300 μm, thereby causing fretting damage. Studies have shown that such fretting damage can reduce the fatigue life of the connection structure by more than 30%, and the wear debris generated can further aggravate bolt loosening or fracture, seriously threatening the operational safety of diesel engines.
Currently, for the bolted connection structure of the steel-crown–aluminum-skirt composite piston in marine diesel engines, experimental data on fretting fatigue, wear–fracture mechanisms, and life prediction models considering wear effects for the mating pair of 2A70 aluminum alloy and 42CrMoA alloy structural steel at 115 °C remain insufficient. Nevertheless, experimental data on fretting fatigue, wear–fracture mechanisms, and life prediction models considering wear effects for this mating pair at 115 °C remain insufficient. The descriptions of the coupling between wear evolution and fatigue damage accumulation, the influence of the wear debris third-body layer, and the transition of failure mechanisms under changing load levels are still inadequate.
To address these research gaps, this paper takes the bolted connection structure of the steel-crown–aluminum-skirt composite piston as the engineering background and conducts single-clamp-head fretting fatigue experiments on the mating pair of 2A70 aluminum alloy and 42CrMoA alloy structural steel at 115 °C under three fatigue load levels. Combined with SEM characterization of the wear morphology and fracture features in the contact region, this study reveals the partial slip characteristics, the combined mechanisms of abrasive wear, adhesive wear, and contact fatigue wear, and the behavior by which wear debris wedging promotes crack initiation and propagation. Furthermore, based on the Chaboche nonlinear kinematic hardening constitutive model, the critical plane method, and the energy wear model, a finite element life prediction model considering wear–fatigue coupling is established, its prediction accuracy is verified, and the laws are clarified that damage preferentially concentrates at the loading-end edge of the contact region, propagates inward along a direction of approximately 30°, and transitions from “damage propagation-dominated” to “plastic accumulation-dominated” with increasing load. The above work can provide experimental evidence and a numerical prediction tool for fatigue-resistant design of aluminum alloys under high-temperature fretting conditions.
2. Specimen and Experimental Methods
Specimen Preparation and Experimental Setup
The fretting fatigue specimens and fretting pads were made of 2A70 aluminum alloy and 42CrMoA alloy structural steel, respectively. The chemical composition of the aluminum alloy is detailed in Table 1. According to the temperature field data for a certain type of diesel engine steel crown aluminum skirt composite piston, under the rated steady-state operating condition, the local temperature in the bolted connection contact zone at the upper part of the aluminum skirt cavity and in the near-surface aluminum skirt substrate is approximately 115 °C, and the temperature fluctuation in this region is small during the steady-state stage. Therefore, 115 °C was adopted as the test condition. The piston model is shown in Figure 1. The microstructural and mechanical properties of the aluminum alloy at 115 °C are listed in Table 2.
Table 1.
Chemical composition.
Figure 1.
Structural diagram of a steel crown aluminum skirt composite piston.
Table 2.
Structure or mechanical property.
In this study, a single-clamp-head fretting fatigue test configuration was employed, and its schematic diagram is shown in Figure 2. The specimen was subjected to an alternating fatigue load and, simultaneously, to a normal clamping load applied by the fretting pad on the contact surface. This induced micron-scale reciprocating relative motion at the contact interface, which generated an alternating tangential load on the specimen surface. Consequently, fretting wear occurred on the contact surface, leading to a significant reduction in fatigue life.
Figure 2.
Schematic diagram of the single-clamp-head fretting fatigue test.
The fretting fatigue test method in this study was designed with reference to the ASTM E2789 standard guide [12]. Owing to the limited material volume, the fretting fatigue specimen was designed with a scaled-down geometry, while the fretting pad adopted a classical configuration in which a flat contact surface was shaped as a flattened circular profile. Figure 3 shows the geometries and dimensions of the fretting fatigue specimen and the contact pad, with all units given in mm. The total length of the specimen is 70 mm, and the width of the contact region is 5 mm. To achieve the machining precision required for the actual joint structure, the contact surface of the specimen was fabricated using slow wire electrical discharge machining (slow wire EDM) (Suzhou Sanguang Science & Technology Co., Ltd., Suzhou, China). The specimen and the fretting pad are also shown in Figure 3.
Figure 3.
Specimen and fretting pad (mm). (a) Specimen. (b) Fretting pad.
The single-clamp-head fretting fatigue tests were conducted using an LF5105 series electro-hydraulic servo dynamic and static fatigue testing machine (LISHI (Shanghai) Scientific Instrument Co., Ltd., Shanghai, China). During the tests, the specimen was directly clamped at both ends by the testing machine. To ensure proper contact between the fretting pad and the specimen surface, a fixture matching the specimen geometry was designed, as shown in Figure 4. The fixture incorporates square holes on its front and rear sides, which are dimensionally consistent with the fretting pad, serving to accommodate the fretting pad and impose displacement constraints on it.
Figure 4.
Schematic diagram of the fixture: (a) three-dimensional model, (b) physical object.
In the single-clamp-head fretting fatigue test, the axial load and the normal compressive load via the fretting pad are applied separately. During the test, the specimen is directly clamped by the fatigue testing machine; therefore, the axial fatigue load is provided directly by the machine. The fatigue load is transmitted through the upper grip of the testing machine under a stress-controlled mode, while the lower grip serves only for fixation. The normal compressive load is supplied by a stress ring and a bolt rod, the configuration of which is shown in Figure 5. Prior to the tests, the stress ring was calibrated in advance. By monitoring the strain of the stress ring using strain gauges, the relationship between the strain readings and the corresponding normal load applied to the fretting pad was established. Before each fretting fatigue test, the dynamic signal test and analysis system was used to measure the strain data, based on which the pre-tightening force of the bolt rod was adjusted to achieve the desired normal load level required for the test.
Figure 5.
Schematic diagram of the stress ring clamping setup: (a) stress ring, (b) testing machine, (c) enlarged view of the clamping area.
Fretting fatigue tests were carried out at 115 °C under three loading conditions. All tests were performed under tensile–tensile cyclic loading with a stress ratio of 0.1, a frequency of 30 Hz, and a sinusoidal waveform. The test conditions are summarized in Table 3. To ensure the reliability of the experimental data, each condition was tested three times, and the results were averaged.
Table 3.
Fretting fatigue test conditions.
It should be clarified that the normal load and the fatigue load were applied independently in the single-clamp-head configuration. A constant normal load of P = 3 kN was applied to the fretting pad through the calibrated stress ring and bolt rod in all tests, so as to reproduce the clamping/contact condition of the bolted connection between the steel crown and aluminum skirt. The axial fatigue load was supplied by the upper grip of the electro-hydraulic servo testing machine, while the lower grip served only for fixation. The fatigue loads of 4, 5, and 6 kN therefore refer to the maximum axial fatigue load. The selected loading conditions are laboratory-scale equivalent conditions rather than a direct full-scale reproduction of the bolt load in the engine. The test temperature of 115 °C was determined from the temperature-field data of the actual steel crown aluminum skirt composite piston under rated steady-state operation. The constant normal load of 3 kN was used to reproduce the clamping state of the bolted contact interface in the scaled single-clamp-head specimen. The axial fatigue loads of 4, 5, and 6 kN were selected to cover the axial load range from lower to higher load operation and to produce fretting fatigue lives in the 104–105 cycles regime.
This study uses a single-clamp-head scaled specimen and a constant normal load, rather than a standard bridge-type apparatus or a full-scale connection structure; the tangential force and local slip amplitude were not directly measured in the tests; and the normal load was applied by a calibrated stress ring and bolt rod rather than by hydraulic closed-loop control. This configuration was adopted because the engineering background of this paper is the bolted connection in a steel-crown–aluminum-skirt piston, which requires simulating the fretting damage caused by axial fatigue loading under a constant clamping state, while also being constrained by the available specimen material and equipment conditions. Therefore, the tests in this paper constitute a laboratory-scale equivalent simulation rather than a complete reproduction of the ASTM E2789 standard test.
3. Fretting Fatigue Test Results and Damage Mechanism Analysis
3.1. Fretting Fatigue Test Results
The fretting fatigue lives of the 2A70 aluminum alloy and 42CrMoA alloy structural steel pair at 115 °C are listed in Table 4.
Table 4.
Fretting fatigue test conditions and lifetime results at 115 °C.
The fatigue lives of the three specimens under each load level exhibit a certain degree of scatter, which is a typical characteristic of fretting fatigue. Specifically, for the 4 kN group, the fatigue lives range from 63,129 to 79,458 cycles, with a maximum variation of approximately 1.26 times, indicating the smallest scatter and the most concentrated data. For the 5 kN group, the lives range from 26,124 to 35,256 cycles, with a variation of about 1.35 times. For the 6 kN group, the lives range from 12,451 to 19,741 cycles, with a variation of approximately 1.59 times, representing the largest scatter. Under higher loads, the wear in the fretting zone becomes more severe, amplifying the randomness of the crack initiation period. Notably, the values of 26,124 and 63,129 cycles are apparently lower than the mean values of their respective groups, which may be attributed to surface defects at the initial stage of fretting wear or localized stress concentration in the contact zone.
3.2. Surface Wear Results
The wear morphologies of the contact zones after fretting fatigue testing are shown in Figure 6, Figure 7 and Figure 8 for the 4, 5, and 6 kN conditions, respectively. In all cases, the contact zone exhibits a partial-slip character: the worn area is concentrated at the lateral edges of the contact interface, while the central stick zone remains relatively less damaged.
Figure 6.
Wear results of Al-1. (a) Worn edge region. (b) Local enlarged view. (c) SEM morphology of the wear debris layer.
Figure 7.
Wear results of Al-2. (a) Worn edge region. (b) Local enlarged view.
Figure 8.
Wear results of Al-3. (a) Worn edge region. (b) Local enlarged view.
For the 4 kN condition (Al-1, Figure 6), the worn area is relatively narrow and localized at the contact edge (Figure 6a). In the higher-magnification image (Figure 6b), grooves approximately parallel to the fretting direction, a compacted debris layer, and loose debris particles are visible. Cracks oriented roughly perpendicular to the fretting direction can be observed near the debris-embedded region. Figure 6c shows a compacted wear-debris layer formed by repeated crushing and consolidation of debris in the contact zone.
For the 5 kN condition (Al-2, Figure 7), the worn area becomes wider than that at 4 kN, indicating expansion of the slip zone with increasing fatigue load (Figure 7a). Figure 7b shows more pronounced plowing grooves, increased debris accumulation, and crack-like features at the edge of the worn region. The debris is present both as a compacted layer and as loose particles.
For the 6 kN condition (Al-3, Figure 8), the worn area expands further and the damage is more severe (Figure 8a). Figure 8b shows a more continuous debris layer, deeper grooves, and abundant loose debris. The increased groove depth and debris accumulation indicate more severe plowing and third-body abrasion under the higher load.
Based on these observations, the wear process can be described as follows. The reciprocating relative slip causes plowing of the softer 2A70 aluminum alloy by the harder 42CrMoA counterbody and by trapped debris, leading to abrasive wear. Repeated contact pressure and sliding also cause material transfer and compaction of debris, producing adhesive-wear features and a third-body debris layer. The debris layer can temporarily separate the contacting surfaces, but once it fractures or is destabilized, the fragments act as free abrasive particles and aggravate wear. Cyclic contact stresses further promote microcrack initiation at groove bottoms and debris-embedded sites, corresponding to a contact-fatigue wear mechanism. These mechanisms act together and lead to the progressive damage observed in Figure 6, Figure 7 and Figure 8. Figure 9 presents a schematic illustration summarizing the damage evolution process of the 2A70 aluminum alloy specimen under the normal pressure applied by the 42CrMoA alloy structural steel fretting pad.
Figure 9.
Schematic diagram of fretting fatigue analysis for 2A70 aluminum alloy specimen against 42CrMoA alloy structural steel fretting pad.
During the fretting process, fine wear debris particles are continuously generated at the contact interface. Owing to the relatively enclosed nature of the contact zone and the sustained normal pressure, these debris particles cannot be readily expelled. Instead, they are repeatedly crushed, fragmented, and subjected to oxidation during the reciprocating sliding motion, eventually forming a dense “third-body” layer on the contact surface. This layer typically exhibits a higher hardness than the original aluminum alloy substrate [16], thereby altering the subsequent tribological behavior of the contact interface. Under certain conditions, the third-body layer may act as a separating medium between the two opposing surfaces, partially mitigating direct metal-to-metal contact. However, when this layer fractures due to fatigue accumulation or excessive local stress, its fragments transform into free abrasive particles, exacerbating the wear process. In addition, some finer debris particles are driven by the contact pressure into the subsurface region along surface microcracks, inducing embedded-type damage. This not only enlarges the damaged area but also promotes crack propagation in the depth direction. A substantial amount of wear debris accumulates at the edges of the contact zone, where a portion becomes compacted into a stable debris layer under repeated compression, while the remainder, in a loose state, exerts a plowing action on the substrate surface, leaving behind distinct scratch grooves.
The generation of free wear debris is inherently a consequence of fatigue damage accumulation on the aluminum surface under long-term cyclic fretting contact: under the combined action of alternating shear stresses and compressive stresses, microcracks preferentially initiate at weak regions of the surface. With increasing cycles, these cracks propagate and interconnect, eventually leading to the detachment of small flaky particles, which become new sources of debris. Owing to the relatively soft nature of the 2A70 aluminum alloy and its poor resistance to plowing, the material is highly susceptible to the formation of scratches and grooves of varying depths, whether in direct contact with the harder 42CrMoA alloy steel counterbody or in interaction with its own wear debris. Consequently, scratches and debris layers appear particularly prominent in the wear morphology. Based on the combined morphological and mechanistic evidence, it can be concluded that under the present test conditions, the primary wear mechanisms of fretting wear encompass abrasive wear (dominated by the cutting action of hard debris particles), adhesive wear (caused by material transfer), and contact fatigue wear (resulting from subsurface crack initiation and propagation induced by cyclic contact stresses). These three mechanisms are intricately intertwined, collectively driving the damage evolution and eventual failure of the contact surface of the 2A70 aluminum alloy.
3.3. Fracture Analysis
To further elucidate the fracture behavior and damage mechanisms of the 2A70 aluminum alloy under fretting fatigue, the fractured specimens were sectioned after testing and systematically examined using scanning electron microscopy (SEM) (Carl Zeiss AG, Oberkochen, Germany). The typical fretting fatigue fracture morphology of the 2A70 aluminum alloy, in contact pair with the 42CrMoA alloy structural steel counterbody at an ambient temperature of 115°C, is shown in Figure 10.
Figure 10.
Fretting fatigue fracture morphology of 2A70 aluminum alloy at 115 °C: (a) Overall morphology. (b) High-magnification SEM image of the local region.
Observations indicate that the fretting fatigue fracture surface can be clearly divided into three distinct regions along the crack propagation path: the crack initiation zone (crack source region), the stable crack propagation zone, and the final fracture zone, as labeled in Figure 10a. After initiating at regions of local stress concentration on the contact surface, the crack rapidly enters the propagation stage, during which crack growth behavior is relatively stable with a high growth rate, eventually leading to overall specimen fracture. From the overall morphology of the fracture cross-section, it is evident that failure is not dominated by a single crack; rather, multiple crack origins are present, indicating a pronounced multi-source characteristic of fretting fatigue damage under this contact pair configuration.
Higher-magnification observation, as shown in Figure 10b, reveals that the primary crack predominantly initiates at the contact surface and progressively propagates inward along the contact plane under the sustained action of alternating contact stresses. The crack initiation zone exhibits typical fatigue source characteristics, attributable to the relatively high local plastic deformation sustained in this region. As the crack advances into the stable propagation zone, distinct radial ridges or striations become visible on the fracture surface. These morphological features reflect periodic variations in the stress state at the crack front and deflection of the propagation direction.
Under high-magnification SEM examination, numerous pores or porosity defects are observed within the fracture surface. These defects originate from inherent metallurgical or processing imperfections in the 2A70 aluminum alloy during its preparation. Notably, these voids are not merely passive features on the fracture surface; rather, under cyclic loading, they act as stress concentration sites in the subsurface high-stress regions, thereby inducing the initiation of secondary cracks. Microcracks around some pores propagate in multiple directions and interconnect with the primary crack. When these secondary cracks extend to the contact surface, they form new surface crack channels, further accelerating the material failure process.
Concurrently, a substantial amount of wear debris generated at the contact edge region during fretting is driven into the material along pre-existing surface cracks under the sustained normal compressive force. After being embedded at the crack tips, these debris particles not only intensify the stress concentration effect at the crack tip but may also impede crack face closure, thereby diminishing the fatigue resistance of the material and promoting accelerated crack propagation. This cascading effect “debris wedging-stress concentration-crack acceleration” constitutes one of the critical auxiliary mechanisms governing the fracture failure of the 2A70 aluminum alloy under fretting fatigue conditions.
In summary, the fracture morphology and damage characteristics of the 2A70 aluminum alloy under fretting fatigue at 115 °C reveal that the fracture process is governed by the synergistic effects of multiple factors: surface fretting wear provides crack initiation sites, internal metallurgical defects serve as channels for secondary cracks, and debris intrusion further accelerates crack propagation. These three factors collectively determine the ultimate failure mode of the material.
4. Numerical Prediction of Fretting Fatigue Considering Wear Effects
4.1. Constitutive Model
This paper is based on the critical plane approach, which is widely used in multiaxial fatigue life prediction, combined with a damage-coupled nonlinear kinematic hardening constitutive model and an energy wear model [17,18]. The modeling strategy is consistent with the systematic review by Ghadar and Fatemi [19] on fretting fatigue crack initiation models. Shen et al. [20] further demonstrated that using only initiation-type multiaxial criteria would underestimate the total life, and that a crack propagation description must be coupled into the damage constitutive model. On this basis, the fretting fatigue life influenced by fretting wear is predicted.
The Archard [21] wear model relates the total wear amount to the product of the normal force and the sliding distance:
where V is the wear volume, K is the volumetric wear coefficient, P is the contact pressure, and S is the total sliding distance.
V = KPS
Fouvry et al. [22,23,24] linked the wear amount to the work done by friction and proposed the energy wear method, whose expression is:
where Ed is the dissipated cumulative friction work, and α is the energy wear coefficient, which can be obtained as the ratio of the volumetric wear rate to the friction coefficient:
where μ0 is the friction coefficient at steady state, and K is the volumetric wear coefficient obtained by fitting using Equation (1). Thus, the energy wear model can be expressed as:
Based on the finite element method, the simulation calculations were performed in the ABAQUS 2022 software. The energy wear method in Equation (2) can be applied to the entire contact interface by applying the local energy wear method to calculate the local wear depth at each contact point on the contact surface. The local wear model is described as follows [25]:
where ∆h(x) is the total wear depth over n time increments, q(x,i) and s(x,i) are the shear stress and slip distance, respectively, of contact surface node x at the i-th time instant, and α is the energy wear coefficient. By this method, the wear depth at each node at the current time is calculated.
One friction cycle involves reciprocating motion, which is calculated through two separate analysis steps. Discretizing Equation (5) and assuming that each analysis step contains n simulation increments, the total wear depth within one analysis step can be approximately expressed as:
where ∆h(x) is the wear depth of contact surface node x within one friction cycle, and ∆s(x,i) is the relative slip distance of contact surface node x at the i-th time instant.
To efficiently simulate the wear depth, the cycle jump technique is adopted. The wear depth is assumed to increase linearly within a certain number of cycles ∆N. The corresponding wear depth ∆h(x) at a node over ∆N cycles can be simulated in one analysis step as follows:
Then, within the adaptive meshing framework, the nodal displacement in the direction perpendicular to the contact surface is constrained, thereby changing the shape of the contact region and consequently altering the stress state on the contact surface.
The Chaboche constitutive model has been extensively used in fatigue analysis due to its favorable applicability in describing the cyclic stress–strain response of metallic materials [26,27,28,29,30,31,32]. This model consists of a yield criterion, a flow rule, and a nonlinear kinematic hardening rule. During fatigue loading, material properties gradually degrade with increasing number of cycles, and such degradation can be quantified as an irreversible damage accumulation process. Chaboche introduced a damage parameter D into the constitutive framework, defining it as a scalar quantity. In the absence of fatigue loading, D = 0; as cyclic loading proceeds, D continuously accumulates, characterizing the progressive development of irreversible damage within the material; when D reaches unity, the material is considered to have completely failed.
Within the Chaboche constitutive framework, the total strain tensor, under the assumption of small deformation, can be expressed as:
where ℇe is the elastic strain tensor and ℇp is the plastic strain tensor. Hooke’s law in the elastic stage can be expressed as:
where σ is the stress tensor and C is the elastic stiffness tensor. The von Mises yield criterion with kinematic hardening, after introducing the damage parameter D, can be expressed as:
where s is the deviatoric stress tensor, and α is the kinematic hardening variable tensor, i.e., the back stress tensor. σy0 is the initial yield stress. The flow rule for the plastic strain tensor is given by:
where ∆λ is the plastic multiplier, which is equal to the effective plastic strain increment ∆p.
ℇ = ℇe + ℇp
σ = (1 − D)C:e
In the Chaboche nonlinear kinematic hardening rule, the hardening law is defined as a function of the plastic strain increment tensor ∆ℇp and the effective plastic strain increment ∆p, expressed as:
where c and γ are material parameters, which can be obtained by fitting the stress–strain curve of the material. Typically, the back stress tensor α is composed of a linear superposition of multiple hardening components αi(i = 1, 2, 3···n). The expression for the back stress tensor is as follows:
where αi is the i-th back stress tensor, and ci and γi are the corresponding material parameters associated with αi. When isotropic hardening is not considered, the stress under uniaxial tension can be expressed as:
The fundamental form of the damage evolution equation is:
where E is the elastic modulus, and S0 and m0 are material constants, which are obtained from the uniaxial strain fatigue curve of the material. ∆p is the cyclic equivalent plastic strain increment. σmax is the maximum damage equivalent stress in one cycle. By replacing the uniaxial σmax with the SSR parameter on the critical plane, and replacing ∆p with the critical-plane equivalent strain amplitude , the multiaxial form of the damage evolution equation is obtained:
where the equivalent strain amplitude on the critical plane is defined as:
The life prediction formula is:
4.2. Finite Element Modeling of Fretting Fatigue
The mechanical property parameters of the 2A70 aluminum alloy and 42CrMoA alloy structural steel at 115 °C are listed in Table 5. The mesh generation and load settings of the finite element model are shown in Figure 11. The values of the parameters of the Chaboche damage constitutive model for 2A70 aluminum alloy are shown in Table 6 below [33].
Table 5.
Mechanical properties of materials.
Figure 11.
Finite element model of the single-clamp-head structure.
Table 6.
Nonlinear kinematic hardening material parameters of 2A70 aluminum alloy.
Figure 11 shows the half-symmetry model established to exploit the structural symmetry and improve computational efficiency. The boundary conditions are defined as follows: displacement in the X-direction is constrained on the side faces of the fretting pad; fixed constraints are applied to the left end face of the specimen; and a symmetry constraint in the Y-direction is imposed on the bottom edge of the specimen. A normal load P is applied to the top of the fretting pad, while a fatigue load F is applied to the right end of the specimen. The mesh in the vicinity of the contact interface is refined to ensure numerical accuracy, with a minimum element size of 0.02 mm × 0.02 mm. The mesh was generated using the four-node plane stress element (CPS4).
The single clamp fretting fatigue specimen in this paper is a thin-plate specimen with a contact zone width of 5 mm. Its thickness is relatively small compared with its in-plane dimensions, and the fatigue load is applied along the axial direction of the specimen, so the nominal normal stress in the thickness direction is relatively small. For such thin-plate specimens, the in-plane stress state is dominant, and adopting the plane stress assumption can reduce the computational scale while ensuring the main stress distribution characteristics.
This paper focuses on the patterns of preferential damage initiation at the contact edge, inward propagation at approximately 30°, and the transition of damage mechanisms under different loads, rather than on the three-dimensional stress details in the thickness direction of the contact region. The plane stress model can reasonably capture the in-plane stress concentration, plastic accumulation, and damage evolution trends at the contact edge, and is suitable for engineering life prediction and mechanism analysis.
However, the plane stress model has potential limitations. In actual fretting contact, pronounced three-dimensional stress concentration and a stress gradient through the thickness exist at the contact edge, and the plane stress model cannot accurately describe the stress variation in the thickness direction. The actual pad involves finite-width contact, and the contact pressure is not completely uniform along the width direction; moreover, pad edge rounding, edge contact, and debris expulsion all exhibit three-dimensional characteristics. The plane model can hardly represent these three-dimensional contact details completely. In the experiments, the accumulation and compaction of wear debris at the contact edge to form a “third-body layer,” as well as the wedging of debris along cracks, exhibit obvious three-dimensional features, and the plane model can only approximately reflect their average effects. The model in this paper is mainly intended to reveal the preferential damage locations, the propagation direction, and the laws governing the transition of failure mechanisms, and to support engineering life prediction.
The master–slave algorithm in ABAQUS was employed to describe the interaction between the contact surfaces. Meanwhile, the wear of both the specimen and the fretting pad was calculated.
When calculating the wear of the specimen, the contact surface of the fretting pad was defined as the master surface, while the contact surface of the specimen was set as the slave surface. Conversely, when calculating the wear of the fretting pad, the contact surface of the specimen was designated as the master surface, and that of the fretting pad as the slave surface. The sliding formulation was defined as finite sliding. The fatigue damage accumulation was evaluated using the fretting fatigue damage accumulation model based on the critical plane approach. For the single-clamp-head fretting fatigue specimen configuration, the specimen structure is relatively simple, and the fatigue load is applied at the specimen ends. Under the same loading condition, the applied force remains constant throughout the test; however, under fretting fatigue loading, damage gradually accumulates and propagates, leading to progressive degradation of material properties. This results in a gradual increase in displacement at the loaded end and a corresponding decrease in structural stiffness. A rapid reduction in structural stiffness can thus serve as the failure criterion for the specimen. In this study, the failure of the overall structure was defined as the reduction in structural stiffness to 90% of its initial value.
Figure 12 illustrates the loading sequence of the fatigue load F and the normal load P. In the first analysis step, a constant normal load P is applied to the fretting pad and then held constant throughout the subsequent steps. Starting from the second analysis step, a cyclic fatigue load F with a stress ratio of R = 0.1 is applied to the right end of the specimen. The cycle jump increment per finite element analysis cycle, ∆N, is set to 1000 cycles.
Figure 12.
Variation in the applied finite element load with load step.
4.3. Fretting Fatigue Life Prediction
Numerical simulations were performed on the established finite element model under the three loading conditions, and the corresponding life prediction results are listed in Table 7.
Table 7.
Fretting fatigue life prediction results.
In Figure 13, the horizontal axis represents the experimental fatigue life and the vertical axis represents the predicted fatigue life. All predicted results fall within this factor-of-two scatter band, confirming that the proposed life-prediction model has acceptable engineering accuracy.
Figure 13.
Life prediction error plot under different load amplitudes.
In this paper, the energy wear model and the cycle jump technique are used to calculate the wear depth, assuming that the wear depth accumulates linearly within ∆N = 1000 cycles. This treatment can reflect the average influence of wear on the contact geometry and contact pressure, but it does not explicitly simulate processes such as the compaction and rupture of the third-body debris layer, material transfer, and debris wedging along cracks. Experiments show that as the load increases from 4 kN to 6 kN, the debris layer becomes more continuous, the grooves become deeper, and more loose debris is present, indicating that the influence of the third-body layer on the contact state and crack initiation is enhanced. Under high load, the wear evolution is more severe, and the changes in contact geometry and pressure distribution are more significant, so the deviation caused by the model simplification is also larger.
The plane stress model neglects the stress gradient through the thickness and the non-uniform pressure along the contact width direction; the failure criterion and the element failure threshold directly affect the predicted life; and fitting errors in the critical plane parameters and the damage evolution parameters S0 and m0 are also propagated into the life prediction results. In addition, the model does not explicitly consider surface roughness, residual stress, oxidation, debris wedging, or crack closure effects. The above factors together cause some deviation in the prediction results, but overall the results still fall within the factor-of-two scatter band, indicating that the model has engineering-acceptable accuracy.
When the accumulated damage of a given element reaches the preset threshold of 0.92, the element is considered to have completely failed, and its damage value ceases to accumulate further. Physically, this indicates that a microcrack with a length on the order of a single element size has initiated at that location. According to the Chaboche damage constitutive theory, a fully damaged element has essentially lost its load-bearing capacity and can hardly transmit stress; thus, its contribution to the overall structural stiffness can be neglected. However, the overall failure of the structure is not determined by the failure of a single element, as damage in adjacent and surrounding elements continues to accumulate during subsequent cyclic loading.
With increasing number of cycles, the damaged region gradually extends from the contact surface inward into the material. When the overall stiffness of the specimen decreases to 90% of its initial value, the structure is considered to have reached the failure state, corresponding to macroscopic fracture. The damage distribution corresponding to the critical moment when the stiffness drops to 90% of its initial value during the entire simulation is shown in Figure 14.
Figure 14.
Damage distribution at failure. (a) Al−1. (b) Al−2. (c) Al−3. (d) Damaged specimen.
From the simulation results, it is clearly observed that, under all loading conditions, damage preferentially concentrates at the edge of the contact region on the right side of the specimen, the side close to the fatigue load application end. This damage location feature is in good agreement with the fracture positions observed in experiments, thereby validating the effectiveness and accuracy of the present simulation model in predicting damage localization. Further analysis of the damage propagation path reveals that, after initiating at the contact edge, damage consistently propagates and accumulates inward at an angle of approximately 30° to the contact surface, exhibiting a distinct inclined propagation trajectory, as shown in Figure 14d. This angular characteristic is closely related to the principal direction of the subsurface stress field in the contact zone, reflecting the dominant role of the maximum shear stress in determining the crack propagation path.
Similar preferred crack initiation and propagation orientations have been reported in conventional multiaxial fatigue and fracture mechanics studies of wrought magnesium alloys [34]. In that work, the crack path was governed by the competition between maximum normal stress driven transverse cracking and maximum-shear-stress-driven longitudinal/helical cracking, with the shear strain energy density controlling the dominant cracking mode. Although the present fretting fatigue loading is not a conventional bulk multiaxial loading path, the contact-induced stress field near the contact edge is inherently multiaxial and non-proportional. Therefore, the approximately 30° inward propagation direction can be rationalized as a local maximum-shear-dominated crack path, consistent with the critical-plane interpretation adopted in the present model.
A comparison of the damage distributions under different loading conditions reveals that, as the fatigue load amplitude increases, the damage penetration depth at the contact edge of the specimen tends to decrease. This phenomenon does not imply that the damage severity is alleviated under higher loads. The underlying mechanism is that, under high-load conditions, the rate of plastic accumulation within the material increases significantly, leading to rapid degradation of structural stiffness. As a result, the overall stiffness drops to the failure threshold before the damage has had sufficient time to fully develop in the depth direction, thereby causing fracture. These results indicate that, under low-load conditions, the fatigue life is primarily governed by gradual damage accumulation and propagation, characterized by a greater damage depth and a more complete propagation path. In contrast, under high-load conditions, the life-controlling mechanism shifts, with rapid plastic accumulation becoming the dominant factor; the failure mechanism transitions from being “damage-propagation-dominated’’ to “plasticity-accumulation-dominated”. This ultimately manifests as a shallower observed damage depth but a more pronounced life reduction at higher load levels.
Combining the three sets of Mises stress contours in Figure 15 with the experimental and simulation data presented in this paper, the following observations can be made. As the axial load increases from 4 kN to 6 kN, the peak stress at the loading-side edge of the contact zone rises nonlinearly from 109.8 MPa to 176.3 MPa, accompanied by a sharp reduction in average fatigue life. This directly verifies the accelerating effect of high stress amplitude on the accumulation rate of the damage parameter D as described by the Chaboche damage evolution equation. Concurrently, the volume of the high-stress region expands with increasing load: it evolves from a highly localized “point-like” hot spot at 4 kN to a “volumetric” high-stress band covering a substantial sub-surface area at 6 kN. This change aligns with the transition in failure mechanism revealed in this study. Under low load (4 kN), damage is dominated by slow crack propagation in the depth direction; under high load (6 kN), extensive plastic accumulation over a larger material volume causes the structural stiffness to degrade to the failure threshold before cracks have sufficient time to penetrate deeply. Consequently, the dominant failure mode shifts from “damage-propagation-controlled” to “plastic-accumulation-controlled,” which also explains why the observed damage penetration depth at the fracture surface is shallower under high load. Furthermore, the region of peak stress coincides exactly with the contact edge where the most severe debris accumulation and plowing scratches are observed in experiments. This broad high-stress environment provides the mechanical driving force for the “third-body debris layer,” which is harder than the substrate, to be wedged into the sub-surface along surface cracks, further amplifying the coupling effect between stress concentration and damage accumulation. In addition, the stress gradient direction forms an angle of approximately 30° with the contact surface, which from a mechanical perspective confirms the dominant role of the maximum shear stress plane in dictating the crack propagation path.
Figure 15.
Mises stress distribution under different loading conditions: (a) Al-1, (b) Al-2, (c) Al-3.
In summary, the Mises stress contours intuitively demonstrate that fretting fatigue is not governed solely by a single peak stress value, but rather by the synergistic effects of high-stress region volume, plastic accumulation rate, and debris wedging. Therefore, in engineering anti-fatigue design, when the load increases to the 6 kN level, simply improving the yield strength of the material yields limited benefit. Priority should instead be given to reducing the volume of the high-stress region through local geometric optimization (e.g., increasing the transition filet radius) or surface strengthening treatments, so as to delay overall stiffness degradation.
5. Conclusions
In this study, single-clamp-head fretting fatigue tests of a 2A70 aluminum alloy/42CrMoA steel pair were conducted at 115°C under a normal load of 3 kN and axial fatigue loads of 4, 5 and 6 kN (stress ratio R = 0.1, frequency 30 Hz). The contact-zone wear morphology, fracture characteristics, and damage evolution were investigated, and a wear fatigue coupled life-prediction model was established. The main conclusions are as follows:
- (1)
- The measured fretting fatigue lives were 63,129–79,458 cycles at 4 kN, 26,124–35,256 cycles at 5 kN, and 12,451–19,741 cycles at 6 kN, with maximum/minimum scatter ratios of approximately 1.26, 1.35, and 1.59. SEM observations showed that all contact zones exhibited partial slip characteristics, with wear concentrated in the peripheral slip zones while the central stick zone remained relatively less damaged. With increasing fatigue load, the worn area expanded and the damage became more severe: at 4 kN, the worn area was narrow and localized, with shallow grooves, a compacted debris layer, and loose debris; at 5 kN, the worn area widened and plowing grooves and debris accumulation became more pronounced; at 6 kN, a more continuous debris layer, deeper grooves, and abundant loose debris were observed. The wear mechanisms involved abrasive wear, adhesive wear, and contact-fatigue wear.
- (2)
- The fracture surfaces exhibited three distinct regions, i.e., the crack-initiation zone, stable crack-propagation zone, and final fracture zone, and showed pronounced multiple crack origins. Internal porosity/metallurgical defects in the subsurface high-stress region initiated secondary cracks, which propagated and interconnected with the primary crack. Under the sustained normal pressure, wear debris was driven into surface cracks; the embedded debris intensified crack tip stress concentration and impeded crack-face closure, thereby accelerating crack propagation. Therefore, the final failure was governed by the synergistic effects of surface fretting wear, internal metallurgical defects, and debris wedging.
- (3)
- A finite element life-prediction model considering wear effects was established by coupling the Chaboche nonlinear kinematic hardening constitutive model with a damage parameter D, the critical plane approach, and an energy wear model. The finite element model used a half-symmetry configuration, CPS4 elements, a master–slave contact algorithm with finite sliding. Element failure was defined at D = 0.92, and overall structural failure was defined as a reduction in structural stiffness to 90% of its initial value. All predicted fatigue lives fell within the factor-of-two scatter band relative to the experimental values, confirming that the proposed model has engineering-acceptable accuracy.
- (4)
- The simulations showed that damage preferentially concentrated at the loading-end edge of the contact zone and propagated inward at approximately 30° to the contact surface, consistent with the experimentally observed fracture locations. As the axial load increased from 4 kN to 6 kN, the peak Mises stress at the loading-side contact edge increased nonlinearly from 109.8 MPa to 176.3 MPa, and the high-stress region evolved from a localized “point-like” hot spot to a “volumetric” high-stress band. Accordingly, the failure mechanism shifted from damage-propagation-dominated at 4 kN to plasticity-accumulation-dominated at 6 kN. This explains why the damage penetration depth at failure tended to decrease under a higher load; the life reduction was more pronounced.
Author Contributions
Conceptualization, Y.X. and H.C.; methodology, Z.C. and H.Z.; software, S.G. and Z.C.; validation, H.C., S.G. and H.Z.; formal analysis, S.G. and H.Z.; investigation, H.C. and J.L.; resources, Y.X. and J.L.; data curation, S.G. and Z.C.; writing—original draft preparation, S.G. and Z.C.; writing—review and editing, H.Z. and Z.C.; visualization, J.L. and Y.X.; supervision, H.Z.; project administration, H.Z. and H.C. All authors have read and agreed to the published version of the manuscript.
Funding
This work was supported by National Key Laboratory of Marine Engine Science and Technology (LAB-2025-16-WD), National Natural Science Foundation of China (52575182) and the Research Fund of State Key Laboratory of Mechanics and Control for Aerospace Structures (Nanjing University of Aeronautics and Astronautics) (Grant No. MCAS-I-0325K01).
Data Availability Statement
The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.
Conflicts of Interest
The authors declare no conflict of interest.
References
- Waterhouse, R.B. Fretting fatigue. Mater. Sci. Eng. 1976, 25, 201–206. [Google Scholar] [CrossRef] [Scilit]
- Hills, D.A. Mechanics of Fretting and Fretting Fatigue; Springer: Cham, Switzerland, 2021. [Google Scholar]
- Tao, F.; Zhang, X.F.; Yin, M.D.; Ouyang, Z.X. A Review of Research on Fretting Damage. Nanjing Univ. Aeronaut. Astronaut. 1999, 31, 545–551. (In Chinese) [Google Scholar]
- Li, X. Fretting Fatigue Theory and Engineering Applications for Mechanical Joint Structures; Beijing Institute of Technology Press: Beijing, China, 2019. [Google Scholar]
- Nowell, D.; Dini, D.; Hills, D.A. Recent developments in the understanding of fretting fatigue. Eng. Fract. Mech. 2006, 73, 207–222. [Google Scholar] [CrossRef] [Scilit]
- Murthy, H.; Rajeev, P.; Farris, T.; Slavik, D. Fretting fatigue of Ti-6Al-4V subjected toblade/disk contact loading. In Proceedings of the 50th Anniversary of Japan Society of Materials Science, Developments in Fracture Mechanics for the New Century, Osaka, Japan, 21–26 May 2001; pp. 41–48. [Google Scholar]
- Hutson, A.; Lee, H.; Mall, S. Effect of dissimilar metals on fretting fatigue behavior ofTi-6A1-4V. Tribol. Int. 2006, 39, 1187–1196. [Google Scholar] [CrossRef] [Scilit]
- Murthy, H.; Gao, G.; Farris, T.N. Fretting fatigue of single crystal nickel at 600 °C. Tribol. Int. 2006, 39, 1227–1240. [Google Scholar] [CrossRef] [Scilit]
- Murthy, H.; Farris, T. Elevated temperature fretting of turbine materials subjected toenginetype-loading. In Proceedings of the 44th AIAA/ASME/ASCE/AHS/ASC Structures, Structural Dynamics, and Materials Conference, Norfolk, VA, USA, 7–10 April 2003. [Google Scholar]
- Mutoh, Y.; Jayaprakash, M. Tangential stress range-compressive stress range diagram for fretting fatigue design curve. Tribol. Int. 2011, 44, 1394–1399. [Google Scholar] [CrossRef] [Scilit]
- Zhang, X.; Wei, D.; Han, L.; Chai, T.; Liu, X.; Yang, S. Fretting fatigue performance and life prediction of GH4169/FGH96 arc dovetail joints at high temperature. Wear 2026, 589, 206524. [Google Scholar] [CrossRef] [Scilit]
- ASTM E2789; Standard Guide for Fretting Fatigue Testing. ASTM International: West Conshohocken, PA, USA, 2010.
- Neu, R. Progress in standardization of fretting fatigue terminology and testing. Tribol. Int. 2011, 44, 1371–1377. [Google Scholar] [CrossRef] [Scilit]
- Greuter, E.; Zima, S. Engine Failure Analysis: Internal Combustion Engine Failure and Their Causes; SAE International: Warrendale, PA, USA, 2012; pp. 99–177. [Google Scholar]
- Ren, X.; Peng, L.; Huang, G.; Zong, R.; Xie, H.; Li, J. Effect of Nd on microstructure and properties of 2A70 alloy. J. Alloys Compd. 2018, 731, 1014–1021. [Google Scholar] [CrossRef] [Scilit]
- Erturun, V.; Odabaş, D. Investigation of microstructure of fretting wear behavior in 6061-T6 aluminum alloy. Aircr. Eng. Aerosp. Technol. 2023, 95, 1194–1200. [Google Scholar] [CrossRef] [Scilit]
- Polák, J.; Fardoun, F.; Degallaix, S. Analysis of the hysteresis loop in stainless steels I. Austenitic Ferritic Steels. Mater. Sci. Eng. A 2001, 297, 144–153. [Google Scholar] [CrossRef] [Scilit]
- Hosseini, R.; Seifir, R. Fatigue crack growth determination based on cyclic plastic zone and cyclic J-integral in kinematic–isotropic hardening materials with considering Chaboche model. Fatigue Fract. Eng. Mater. Struct. 2020, 43, 2668–2682. [Google Scholar] [CrossRef] [Scilit]
- Ghadar, S.; Fatemi, A. Fretting fatigue: A literature review of experimental studies and an overview of modeling approaches. Int. J. Fatigue 2026, 208, 109578. [Google Scholar] [CrossRef] [Scilit]
- Shen, F.; Hu, W.; Meng, Q. A damage mechanics approach to fretting fatigue life prediction with consideration of elastic–plastic damage model and wear. Tribol. Int. 2015, 82, 176–190. [Google Scholar] [CrossRef] [Scilit]
- Archard, J.F. Contact and Rubbing of Flat Surfaces. J. Appl. Phys. 1953, 24, 981–988. [Google Scholar] [CrossRef] [Scilit]
- Fouvry, S.; Paulin, C. An effective friction energy density approach to predict solid lubricant friction endurance: Application to fretting wear. Wear 2014, 319, 211–226. [Google Scholar] [CrossRef] [Scilit]
- Fouvry, S.; Kapsa, P. An energy description of hard coating wear mechanisms. Surf. Coat. Technol. 2001, 138, 141–148. [Google Scholar] [CrossRef] [Scilit]
- Mary, C.; Fouvry, S. Numerical prediction of fretting contact durability using energy wear approach: Optimisation of finite-element model. Wear 2007, 263, 444–450. [Google Scholar] [CrossRef] [Scilit]
- Li, S.; Tan, J.; Wang, C.; Zhang, H.; Cui, H. Study on the wear performance of TiAl–P/M superalloy friction pairs: An experimental investigation and wear model. Friction 2026, 14, 9441196. [Google Scholar] [CrossRef] [Scilit]
- Sun, D.; Gao, Q.; Huo, J. Experimental study and fretting fatigue life prediction in dovetail assembly considering stress–temperature nonlinear coupling effect. Fatigue Fract. Eng. Mater. Struct. 2023, 46, 2284–2298. [Google Scholar] [CrossRef] [Scilit]
- Kasar, Ç.; Kaftancioglu, U.; Bayraktar, E.; Aslan, O. Lifetime Prediction of Single Crystal Nickel-Based Superalloys. Appl. Sci. 2024, 15, 201. [Google Scholar] [CrossRef] [Scilit]
- Sajjad, H.M.; Hanke, S.; Güler, S.; Hassan, H.U.; Fischer, A.; Hartmaier, A. Modelling Cyclic Behaviour of Martensitic Steel with J2 Plasticity and Crystal Plasticity. Materials 2019, 12, 1767. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Zhang, B.; Liu, H.; Zhu, C.; Ge, Y. Simulation of the fatigue-wear coupling mechanism of an aviation gear. Friction 2021, 9, 1616–1634. [Google Scholar] [CrossRef] [Scilit]
- Shen, F.; Voyiadjis, G.Z.; Hu, W.; Meng, Q. Analysis on the fatigue damage evolution of notched specimens with consideration of cyclic plasticity. Fatigue Fract. Eng. Mater. Struct. 2015, 38, 1194–1208. [Google Scholar] [CrossRef] [Scilit]
- Zhang, T.; Harrison, N.M.; Mcdonnell, P.F.; E McHugh, P.; Leen, S.B. Micro–macro wear–fatigue of modular hip implant taper-lock coupling. J. Strain Anal. Eng. Des. 2014, 49, 2–18. [Google Scholar] [CrossRef] [Scilit]
- Šmach, J.; Halama, R.; Marek, M.; Šofer, M.; Kovář, L.; Matušek, P. Two Contributions to Rolling Contact Fatigue Testing Considering Different Diameters of Rail and Wheel Discs. Lubricants 2023, 11, 504. [Google Scholar] [CrossRef] [Scilit]
- Guo, S.; Li, M.; Zhu, F.; Zhang, H.; Cheng, Z.; Cui, H. Effect of Grain Size on High-Temperature Fretting Wear–Fatigue Coupling Damage of 2A70 Aluminum Alloy and Its Simulation. Metals 2026, 16, 1221. [Google Scholar] [CrossRef] [Scilit]
- Gryguć, A.; Behravesh, S.B.; Jahed, H.; Wells, M.; Williams, B.; Su, X. Multiaxial Fatigue and Cracking Orientation of Forged AZ80 Magnesium Alloy. Procedia Struct. Integr. 2020, 25, 486–495. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |