Skip to Content
MetalsMetals
  • Article
  • Open Access

29 September 2026

22 Pages

Time-Dependent Thermal Recovery of Irradiation Hardening in EP-450 Steel from BN-350 Spent Fuel Assembly Wrappers During Isothermal Annealing at 470 °C

,
,
,
and
1
Institute of Atomic Energy Branch of the National Nuclear Center of the Republic of Kazakhstan, Kurchatov 180010, Kazakhstan
2
National Nuclear Center of the Republic of Kazakhstan, Kurchatov 180010, Kazakhstan
*
Author to whom correspondence should be addressed.

Abstract

Ferritic–martensitic EP-450 steel has been widely used for fast-reactor fuel assembly wrappers because of its high resistance to irradiation-induced swelling; however, its radiation-hardened state formed under low-temperature, high-dose neutron exposure may evolve during subsequent thermal exposure. This study examines the time dependence of post-irradiation thermal softening in EP-450 steel taken from two BN-350 spent fuel assembly wrappers irradiated at approximately 351 °C to 61 and 71 dpa. Samples were annealed in static argon at 470 °C for cumulative durations of 10, 30, and 100 h. Vickers hardness was measured for both wrappers, while miniature tensile tests were performed for the 71 dpa material. The initial hardness values were similar, 356 and 360 HV0.2, but the thermal response differed markedly: after 100 h, hardness decreased by 10.2% and 17.9%, respectively. For the 71 dpa material, the 0.2% proof stress decreased from 815 to 752 MPa between 10 and 100 h, while total and localized strains increased from 15.33% to 17.94% and from 8.84% to 11.45%, respectively. These results demonstrate a gradual, time-dependent reduction of irradiation hardening at 470 °C and reveal that materials with similar initial hardness can exhibit substantially different thermal stability.

1. Introduction

One of the key factors determining the service life of fast-reactor core components is the ability of structural materials to retain dimensional and mechanical stability under the accumulation of high damage doses [1,2,3]. At the early stage of fast-reactor development, austenitic stainless steels were widely used for fuel pin claddings, fuel assembly (FA) wrappers, and other core components. However, the discovery of irradiation-induced void formation and the associated swelling in the late 1960s demonstrated that, under high-dose neutron irradiation, the stability of austenitic steels could become one of the factors limiting the service life of core components [4]. In contrast to austenitic stainless steels, ferritic and ferritic–martensitic steels exhibited substantially higher resistance to irradiation-induced swelling [5,6,7,8], which largely determined the subsequent development of this class of materials for fast-reactor applications.
Since the 1970s, high-chromium ferritic–martensitic steels containing approximately 9–12 wt.% Cr have been actively considered and employed as structural materials for fast reactors [5,6]. First-generation steels introduced into practical use included, in particular, HT9, EM10/EM12, PNC-FMS, and EP-450, which were employed within national fast-reactor development programs [6]. These steels were widely used for FA wrappers, combining adequate performance in the relevant temperature range with high resistance to swelling at high damage doses [6,7,9].
Within the Soviet/Russian fast-reactor program, EP-450 became one of the principal first-generation ferritic–martensitic steels. It was used for hexagonal FA wrappers in the BN-350 and BN-600 reactors and was subsequently employed for FA wrappers in the BN-800 reactor [1,6,7,10]. BN-350 occupies a special place in the accumulated operating experience with EP-450, as it was the world’s first pilot-industrial fast reactor with a liquid-metal coolant and operated from 1973 to 1999 [2,3,11].
At the same time, high resistance to irradiation-induced swelling does not imply stability of the mechanical state of ferritic–martensitic steels under neutron irradiation. One of the principal factors limiting their properties in the low-temperature operating regime is irradiation hardening and the associated embrittlement [5,6,12]. In 9–12 wt.% Cr ferritic–martensitic steels, the increase in yield strength at relatively low irradiation temperatures is associated with the formation of stable microstructural barriers to dislocation motion, including dislocation loops and irradiation-induced nanoscale precipitates, whereas at higher temperatures the contribution of irradiation hardening decreases due to the thermally activated evolution of the defect structure [6,12].
The post-irradiation mechanical state of EP-450 steel strongly depends on the irradiation temperature and damage dose. Under irradiation in the low-temperature regime, the increase in strength characteristics increased with dose and reached a maximum at approximately 30–40 dpa, followed by a partial decrease in irradiation hardening [13]. Microstructural studies of EP-450 irradiated in the BOR-60, BN-350, and BN-600 reactors revealed the formation of dislocation loops, voids, and irradiation-induced phases over a wide temperature range [14]. In the low-temperature regime, a high density of dislocation loops and χ-precipitates is considered one of the major sources of irradiation hardening and embrittlement [13,14], whereas the steel retains its high resistance to irradiation-induced swelling at substantially higher damage doses [14,15]. High-dose irradiation of EP-450 is also accompanied by pronounced changes in its mechanical properties and microstructure [16], while comparable low-temperature irradiation hardening has been reported for other high-chromium ferritic–martensitic steels, including EUROFER97 [17,18,19].
Of particular interest to the present study are recent data on the structural instability of EP-450 under prolonged high-dose irradiation. For material from a BN-350 FA wrapper irradiated to 53 dpa at approximately 410 °C, evidence of irradiation-induced recovery and structural rearrangement was observed, accompanied by changes in the morphology of tempered martensite and in the subgrain structure [20]. These results indicate that the state of EP-450 after reactor irradiation is governed not only by the accumulation of irradiation defects, but also by competing processes of their thermally activated evolution. However, Ref. [20] characterizes the final state after reactor irradiation and does not reveal the time dependence of changes in mechanical properties during subsequent controlled thermal exposure.
The possibility of thermal recovery from irradiation hardening has also been demonstrated for other ferritic–martensitic steels. For EUROFER97 and F82H, post-irradiation annealing at 500–550 °C resulted in partial or substantial recovery of hardness and mechanical properties [17,21,22]. In particular, for EUROFER97 irradiated at 330 °C to 15 dpa, annealing at 550 °C for 3 h resulted in an almost complete recovery from low-temperature irradiation hardening; TEM analysis revealed a decrease in the density of dislocation loops and cavities, accompanied by an increase in their mean size and the development of dislocation lines and networks [22]. Thus, post-irradiation recovery of ferritic–martensitic steels is closely associated with the thermally activated rearrangement of the defect structure formed during irradiation.
Actual BN-350 spent fuel assembly (SFA) wrappers are of particular value in this respect because their condition was formed by the combined effects of industrial fabrication, initial heat treatment, and prolonged neutron irradiation. The initial condition of the investigated EP-450 fragments was previously characterized in terms of microstructure and corrosion damage after reactor operation and long-term storage in the spent fuel pool [23]. Short-term 1 h annealing of the same materials in air at 450–900 °C was subsequently investigated with emphasis on corrosion damage [24], while a later study of BN-350 wrappers, including C-1, revealed phase-selective localized corrosion with preferential dissolution of tempered martensite and interphase boundaries [25]. The observed heterogeneity of the surface condition may also serve as an indication of differences in the initial state of the investigated wrappers that could manifest as different thermal stability of the irradiation-modified state. These previous studies, however, do not describe the time evolution of mechanical properties during prolonged post-irradiation annealing.
Despite the substantial body of data on the irradiation behavior of EP-450 and the post-irradiation recovery of other ferritic–martensitic steels, the time dependence of thermal recovery from irradiation hardening in actual BN-350 SFA wrapper material irradiated at approximately 350 °C to damage doses exceeding 60 dpa remains largely unexplored. In particular, it remains unclear how hardness, strength properties, and ductility evolve during prolonged moderate post-irradiation thermal exposure and whether recovery continues to develop with increasing annealing time.
In the present study, fragments from two BN-350 SFA wrappers made of EP-450 steel and irradiated at approximately 351 °C to damage doses exceeding 60 dpa were investigated. The samples were subjected to post-irradiation isothermal annealing at 470 °C in an argon atmosphere for 10, 30, and 100 h. The selected temperature is approximately 120 °C higher than the irradiation temperature, but remains substantially below the high-temperature tempering temperatures used for EP-450; thus, the applied treatment makes it possible to assess the stability of the irradiation-hardened state under moderate, prolonged thermal exposure. Moreover, according to Ref. [13], recovery of ductility in irradiated EP-450 becomes noticeable already after a 1 h anneal at 450 °C, whereas at 550 °C it is almost restored to the level of the thermally aged condition; therefore, 470 °C lies in the lower part of the post-irradiation recovery temperature range and is suitable for examining its time evolution. Thus, the applied treatment enables the stability of the irradiation-hardened state to be assessed under moderate, prolonged thermal exposure. The aim of this study was to establish the time dependence of thermal recovery from irradiation-induced hardening in EP-450 steel from BN-350 SFA wrappers during isothermal annealing at 470 °C, to compare the evolution of hardness in materials irradiated to 61 and 71 dpa, and to determine the corresponding changes in the strength and ductility of the material subjected to the higher damage dose.

2. Materials and Methods

2.1. Materials Investigated

The materials investigated in this study were fragments of hexagonal wrappers from two BN-350 SFAs, designated in the reactor records as 71517003188 and C-1, made of ferritic–martensitic EP-450 (1Cr13Mo2NbBV) steel. The fragments were plates approximately 50 × 20 × 2 mm in size, cut from the wrapper faces at the BN-350 core midplane (0 mm relative to the core midplane), where the maximum damage doses had accumulated during reactor operation. Similar fragments from the same wrappers had previously been used to investigate their post-service structural condition and corrosion damage [23,24].
According to the reactor records, the C-1 SFA was operated in the reactor from 19 June 1985 to 26 November 1987. The 71517003188 SFA was discharged from the reactor on 12 April 1992 and was the oldest modernized-type FA stored in the spent fuel pool. These data indicate differences in the operational and post-service histories of the two investigated wrappers prior to sampling for materials characterization.
The principal irradiation parameters of the investigated wrapper fragments at the BN-350 core midplane are summarized in Table 1.
Table 1. Main irradiation parameters of the investigated BN-350 SFA wrapper fragments at the core midplane.
The outer and inner surfaces of the investigated wrapper fragments are shown in Figure 1. The surface conditions of the two wrappers differed noticeably: 71517003188 exhibited more pronounced corrosion-related changes and localized pitting damage, whereas the surface of C-1 was characterized by a denser and more uniform corrosion layer; micron-scale pits were observed on both wrapper fragments. These features were previously characterized in detail by SEM/EDS [23] and were taken into account when selecting areas for the preparation of characterization and tensile specimens.
Figure 1. Outer and inner surfaces of the investigated EP-450 ferritic–martensitic steel wrapper fragments from BN-350 spent fuel assemblies: (a) wrapper 71517003188, 61 dpa; (b) wrapper C-1, 71 dpa. The fragments were taken from the core midplane after reactor service and long-term wet storage.
Further sectioning of the investigated wrapper fragments was performed according to individual cutting layouts that accounted for the geometry of the original fragments, the specific features of wire electrical discharge machining (wire EDM), and the cutting sequence. The individual cutting layouts for the 71517003188 and C-1 wrapper fragments are shown in Figure 2. The resulting blanks were used to prepare characterization and tensile specimens for subsequent material characterization and post-irradiation annealing.
Figure 2. Individual cutting layouts for the investigated EP-450 steel wrapper fragments from BN-350 SFAs: (a) wrapper 71517003188, fragments I-1 and I-2; (b) wrapper C-1, fragment P.

2.2. Microstructural and Phase Characterization of the Initial Condition

To characterize the initial irradiated condition of EP-450 steel, metallographic specimens were prepared from longitudinal and transverse sections of the investigated material. The microstructure was revealed by chemical etching in a solution containing 100 mg CuCl2, 10 mL C2H5OH, 10 mL HCl, and 10 mL HNO3; the etching time was 60–75 s.
Metallographic examinations were performed using an ICX-41M optical microscope (SopTop, Shenzhen, China) in bright-field mode at magnifications of up to ×1000. Image analysis was carried out using Altami software, version 3.5 (Altami, Russia). Surface morphology and local elemental composition were examined using a VEGA3 scanning electron microscope (TESCAN, Brno, Czech Republic) equipped with an X-Act energy-dispersive X-ray spectrometer (X-Act, Oxford Instruments NanoAnalysis, High Wycombe, UK).
X-ray diffraction (XRD) analysis of the surface layer was performed using an Empyrean diffractometer (PANalytical Ltd., Almelo, The Netherlands) equipped with a PIXcel1D linear detector and Cu Kα radiation at an accelerating voltage of 45 kV and a current of 40 mA. A fixed divergence slit of 1° and an anti-scatter slit of 2° were used. Survey diffraction patterns were recorded over the 2θ range of 5–153° with a step size of 0.026° and an exposure time of 30.6 s. To identify weak additional reflections, selected ranges were recorded over 2θ = 10–90° using the same step size and an increased exposure time of 270 s. Crystalline phases were identified and semi-quantitatively evaluated using HighScore software, version 4.0, reference diffraction data, and reference intensity ratio (RIR) values. The RIR method was used for comparative semi-quantitative characterization of crystalline phases in the surface layer; the resulting values were not interpreted as bulk phase fractions of the material. No separate XRD measurements were performed on polished metallographic sections from which the corrosion products had been removed.
When analyzing the metallic matrix, the substantial overlap of the principal diffraction reflections from the ferritic and tempered-martensitic constituents of EP-450 steel was taken into account because of the similarity of their lattice parameters. A possible contribution from the martensitic constituent was assessed from weak additional reflections resolved from the main α-Fe peaks. Quantitative determination of the ferrite-to-tempered-martensite ratio by XRD was not performed; metallographic examination was used to assess the morphology and distribution of these microstructural constituents, whereas their volume fractions were not quantitatively determined in the present study.
The initial surface condition of the investigated wrappers was characterized previously in Ref. [23], while related short-term thermal effects on their corrosion condition were reported in Ref. [24]. These previous data were used as supplementary information when characterizing the material condition prior to the present post-irradiation annealing study.

2.3. Post-Irradiation Isothermal Annealing

Post-irradiation annealing of the specimens was performed using a custom-designed ampoule assembly installed in the heating chamber of an SNOL 8.2/1100 laboratory muffle furnace (SNOL-TERM Ltd., Tver, Russia). The working section of the ampoule consisted of a quartz tube; the specimens were placed in two ceramic boats mounted on a stainless steel holder. The assembly was connected to a vacuum system and an inert-gas supply system. Temperature was monitored using a K-type thermocouple. The furnace heating unit was modified to provide two independently controlled heating zones, each regulated by a PID controller. A general view of the experimental setup and the arrangement of the specimens within the working section of the quartz ampoule are shown in Figure 3.
Figure 3. Experimental setup for post-irradiation isothermal annealing: (a) general view of the setup with the argon supply system and SNOL 8.2/1100 laboratory furnace; (b) arrangement of the specimens in two ceramic boats within the working section of the quartz ampoule.
Before filling with argon, the working volume of the ampoule was evacuated to a residual pressure of approximately 10 Pa. The ampoule was then filled with argon, sealed, and pressurized to an overpressure of 1.5 atm. The experimental assembly was heated to (470 ± 2) °C and held at this temperature in a closed, static argon atmosphere; no gas flow was maintained during annealing. The annealing temperature of 470 °C was selected on the basis of a previously performed thermal analysis of BN-350 SFA under long-term dry-storage conditions, in which the maximum calculated temperature was approximately 472 °C [26]. In the present study, however, this condition was used as a controlled post-irradiation thermal treatment to assess the stability of the irradiation-hardened state of EP-450 rather than as a direct reproduction of actual storage conditions.
The maximum cumulative duration of post-irradiation annealing was 100 h. Three time points corresponding to cumulative isothermal holding times of 10, 30, and 100 h were selected to determine the time dependence of property changes. At each time point, heating was stopped, and the specimens were cooled together with the furnace. The ampoule was opened, and the corresponding group of specimens was removed after the temperature had decreased below 60 °C. The remaining specimens were then reloaded into the setup, and annealing was continued until the next cumulative holding time was reached. The experimental scheme and specimen designations for wrappers 71517003188 and C-1 are given in Table 2.
Table 2. Scheme of post-irradiation isothermal annealing and specimen designations for BN-350 SFA wrappers.
For wrapper 71517003188, only characterization specimens were prepared and used for HV0.2 hardness measurements before and after annealing. For wrapper C-1, both characterization specimens for HV0.2 measurements and miniature tensile specimens for uniaxial tensile testing were used.

2.4. Microhardness Measurements

The microhardness of EP-450 steel was measured using the Vickers method with an automated Qness Q10A+ hardness tester (ATM Qness GmbH, Golling an der Salzach, Austria). To characterize the initial irradiated condition, the microhardness of individual microstructural constituents was measured in longitudinal and transverse sections using a diamond indenter load of 0.1 kgf (HV0.1). Changes in hardness resulting from post-irradiation annealing were determined at a load of 0.2 kgf (HV0.2), with the overall hardness of the material measured without separately determining values for the ferritic and tempered-martensitic constituents. Before thermal exposure, the initial HV0.2 value was measured on each characterization specimen. Subsequent HV0.2 measurements were performed after cumulative isothermal annealing times of 10, 30, or 100 h at 470 °C, in accordance with the scheme given in Table 2. For each specimen/condition, three individual HV0.2 measurements were performed. The results are presented as the arithmetic mean ± standard deviation (SD), calculated from the three individual Vickers indentations.

2.5. Mechanical Testing of Miniature Specimens

The strength and ductility characteristics of EP-450 steel were determined by uniaxial tensile testing of miniature flat specimens. The use of miniature specimens was necessitated by the limited amount of highly irradiated wrapper material available and the impossibility of preparing standard-sized specimens from the investigated fragments [27]. The nominal overall specimen length was 15.0 mm, the reduced-section length was 8.0 mm, the width of the gauge section was 2.0 mm, and the width of the grip sections was 5.5 mm. The specimen geometry and the gripping arrangement used for testing are shown in Figure 4.
Figure 4. Miniature flat tensile specimen and gripping fixture used for mechanical testing of the SFA wrapper material: (a) specimen geometry and principal dimensions; (b) self-centering gripping fixture; (c) installation of the gripping fixture in the Instron 5966 testing machine.
A specially designed and patented self-centering gripping fixture [28] was used to hold the specimens and ensure axial application of the tensile load. The tests were performed using an Instron 5966 universal electromechanical testing machine (Instron, Norwood, MA, USA) at a constant crosshead speed of 2.5 mm/min. For non-contact determination of strain, reference marks were applied to the gauge section of each specimen, and strain during tensile testing was determined from changes in their relative positions. Test control and acquisition of experimental data were performed using Bluehill 3 software (Instron, USA).
The 0.2% proof stress, σ 0.2 , ultimate tensile strength, σ U T S , total strain, ε t o t , uniform plastic strain, ε u , and localized plastic strain, ε l o c , were determined from the engineering stress–strain curves.
The time dependence of the mechanical properties was determined for the C-1 wrapper material. Two specimens were tested in the initial irradiated condition, and one specimen was tested after each post-irradiation annealing treatment at 470 °C for 10, 30, and 100 h, in accordance with the scheme given in Table 2. Thus, for each post-irradiation annealing time, the mechanical properties were determined from the tensile test of a single miniature specimen.

3. Results

3.1. Initial Microstructural and Phase State of EP-450 Steel

In the initial irradiated condition, the materials from both investigated wrappers exhibited a two-constituent microstructure comprising ferritic and tempered-martensitic (hereafter TM) constituents (Figure 5). Metallographic images revealed differences in the morphology and distribution of the microstructural constituents between the two wrapper materials.
Figure 5. Initial microstructure of irradiated EP-450 steel from wrappers 71517003188 (a,c) and C-1 (b,d): general microstructural appearance at ×200 (a,b) and representative regions at ×1000 (c,d). Note: F—ferrite; TM—tempered martensite.
The ferritic regions exhibited predominantly light contrast after etching, relatively large dimensions, and well-defined boundaries. The TM constituent exhibited a finer microstructure, darker contrast, and less distinct, locally discontinuous boundaries. In wrapper 71517003188, the distribution of the microstructural constituents was locally necklace-like, with regions of TM surrounding larger ferritic regions. In the C-1 material, the morphology and distribution of the microstructural constituents differed from those observed in 71517003188, although individual ferritic regions also retained predominantly light contrast.
Comparison of the longitudinal and transverse sections revealed weak structural orientation in the 71517003188 wrapper material: some large ferritic regions were elongated predominantly parallel to the rolling direction. No pronounced structural orientation was observed in the C-1 material, although some ferritic regions were also elongated. At higher magnification, chain-like and dispersed precipitates were observed in both microstructures within the ferritic and tempered-martensitic regions and near their boundaries (Figure 5c,d). Based on their morphology, these features may be attributed to carbide-type precipitates.
X-ray diffraction analysis was used to complement the metallographic characterization and to characterize the phase composition of the surface layers of the investigated wrappers. Measurements were performed on both sides of the fragments; Figure 6 shows diffraction patterns obtained from the central and peripheral regions using an extended exposure time to reveal weak additional reflections. The resulting diffraction patterns were used to characterize the metallic matrix and to identify crystalline phases present in the surface layer.
Figure 6. XRD patterns of the surface layers of EP-450 steel fuel assembly wrappers in the initial condition: (a) 71517003188; (b) C-1. For each wrapper, diffraction patterns from the central and peripheral regions of the outer and inner surfaces are shown; the patterns were acquired using an extended exposure time.
The dominant diffraction response of both investigated materials corresponded to the BCC α-Fe matrix of EP-450 steel. ICDD card 03-065-6033 for a BCC solid solution with space group Im-3m and a lattice parameter of a ≈ 2.88 Å provided the closest match in terms of reflection positions and relative intensities.
Weak additional reflections were also detected in the diffraction patterns, with positions consistent with the ICDD 00-044-1290 reference data for martensite with a tetragonal structure (I4/mmm, a = b ≈ 2.859 Å, c ≈ 2.937 Å). However, because of the similarity of the lattice parameters and the substantial overlap of the principal reflections from the ferritic and tempered-martensitic constituents, reliable quantitative separation of these constituents by XRD is not possible. Therefore, the XRD data obtained in the present study were not used to determine the ferrite-to-tempered-martensite ratio.
In addition to the reflections from the metallic matrix, the diffraction patterns of 71517003188 contained a pronounced set of reflections from crystalline corrosion products (Figure 6a). Iron oxyhydroxide FeOOH (ICDD 01-070-0714) was identified with the highest confidence, exhibiting intense and reproducible reflections clearly separated from the principal reflections of the metallic matrix. Magnetite Fe3O4 and nonstoichiometric iron monoxide Fe1−xO with a wüstite-type structure were also identified on the surface of 71517003188. Magnetite reflections were detected predominantly on one side of the fragment, whereas Fe1−xO reflections were recorded at several investigated locations.
The additional phases detected in C-1 differed substantially from those observed in 71517003188 (Figure 6b). The extended exposure time enabled the detection of weak reflections from oxide phases that could not be identified with confidence in the survey scans. According to the local semi-quantitative RIR assessment of the surface layer, magnetite was present on both investigated sides at approximately 3%, FeOOH was detected on only one side at approximately 1%, and the contributions of the remaining identified corrosion products were below 1%. These values characterize the investigated local regions of the surface layer and should not be interpreted as bulk phase fractions of the wrapper material.
Thus, metallographic examination confirmed the presence of the characteristic ferritic–martensitic microstructure of EP-450 in both wrappers, whereas XRD primarily revealed differences in the condition of their surface layers. The 71517003188 and C-1 materials differed in the morphology and distribution of their microstructural constituents, as well as in the presence and composition of crystalline corrosion products. These features characterize the heterogeneity of the initial condition of the investigated wrappers before post-irradiation annealing.

3.2. Initial Microhardness Distribution in EP-450 Steel

Given the two-constituent (duplex) ferritic–martensitic microstructure of EP-450 steel, local microhardness was measured separately in the ferritic and TM constituents. Representative Vickers indentations obtained at a load of 0.1 kgf within the corresponding microstructural regions are shown in Figure 7.
Figure 7. Representative Vickers indentations in the microstructural constituents of irradiated EP-450 steel: (a) ferrite; (b) TM.
According to the local measurements, the microhardness of the ferritic constituent exceeded that of TM in all investigated regions of both wrappers (Table 3). For the 71517003188 material, the average values were 372 and 355 HV0.1, respectively, corresponding to a difference of approximately 4.8%. For C-1, the average microhardness values of ferrite and TM were 377 and 363 HV0.1, respectively, corresponding to a difference of 3.9%. Thus, the consistently higher microhardness of the ferritic constituent was observed on the outer and inner sides, as well as in the cross-sections of both materials, with the difference being approximately 3–6%. Although the absolute values varied depending on the investigated region, no consistent dependence on the wrapper side or section was observed.
Table 3. Microhardness of the microstructural constituents of EP-450 steel from the investigated SFA wrappers in the initial irradiated condition.
The higher HV0.1 of the ferritic constituent compared with the tempered-martensitic constituent likely reflects their different sensitivity to irradiation hardening. For EP-450, a substantial contribution to low-temperature irradiation hardening has been associated with dislocation loops and irradiation-induced nanoscale precipitates [13,14]. The more developed system of lath and subgrain boundaries in tempered martensite may provide a higher density of sinks for irradiation defects, thereby limiting their accumulation compared with ferritic regions. A similar dependence on the initial microstructure was reported for HT-9 steel: after ion irradiation, the ferritic condition exhibited more pronounced irradiation hardening than the fine-lath tempered-martensitic condition [29]. Therefore, the observed difference in HV0.1 may reflect a greater irradiation-induced contribution to hardening in the ferritic constituent.
For wrapper 71517003188, additional profiling of the ferritic constituent through the wall thickness revealed a nonuniform distribution of HV0.1 (Figure 8).
Figure 8. Microhardness distribution of the ferritic constituent (HV0.1) through the wall thickness of the 71517003188 SFA wrapper in the initial irradiated condition.
The microhardness exhibited a nearly symmetric profile, with lower values in the central part of the wall and a gradual increase toward both surfaces. Thus, in addition to the consistently higher local microhardness of the ferritic constituent compared with the TM constituent, a nonuniform through-thickness distribution of ferrite HV0.1 was identified in the 71517003188 material.

3.3. Time Dependence of Thermal Recovery from Irradiation Hardening Based on Hardness Measurements

To evaluate the time dependence of thermal recovery from irradiation hardening, HV0.2 hardness was used, measured without separately distinguishing the ferritic and TM constituents. In the initial irradiated condition, the hardness values of wrappers 71517003188 and C-1 were 356 ± 4 and 360 ± 5 HV0.2, respectively, and were essentially identical within the measurement uncertainty. The appearance of the characterization specimens in the initial condition and after annealing at 470 °C is shown in Figure 9. With increasing annealing time, the surfaces of specimens from both wrappers exhibited changes in color; however, no pronounced formation or spalling of an oxide scale was observed visually. The chemical and phase composition of the surface after annealing, as well as possible decarburization, was not specifically investigated; therefore, the surface color change was not used in interpreting the mechanism of hardness reduction.
Figure 9. Appearance of EP-450 steel characterization specimens from SFA wrappers 71517003188 and C-1 in the initial irradiated condition and after post-irradiation isothermal annealing at 470 °C for 10, 30, and 100 h. Upper row—71517003188; lower row—C-1.
Isothermal annealing at 470 °C resulted in a progressive decrease in the hardness of both investigated materials (Table 4). After 10 h, the HV0.2 hardness of wrapper 71517003188 decreased from the initial 356 ± 4 to 335.0 ± 4.4, whereas that of C-1 decreased from 360 ± 5 to 332.7 ± 2.9. Further increases in annealing time were accompanied by an additional decrease in HV0.2, although the magnitude of this decrease differed markedly between the two wrappers.
Table 4. Changes in the hardness of EP-450 steel from the investigated SFA wrappers during post-irradiation isothermal annealing at 470 °C.
For wrapper 71517003188, the most pronounced initial decrease occurred within the first 10 h, when the hardness decreased by 5.9% relative to the initial level. With increasing annealing time to 30 h, the mean value was 332.0 ± 6.2 HV0.2 and changed only slightly compared with the value after 10 h. After 100 h, the hardness decreased to 319.7 ± 4.5 HV0.2, corresponding to an overall reduction of 10.2%.
For C-1, the decrease in hardness was more pronounced and continued throughout the entire investigated time interval. The HV0.2 values were 332.7 ± 2.9 after 10 h, 318.3 ± 4.5 after 30 h, and 295.7 ± 4.9 after 100 h. Relative to the initial condition, the corresponding decreases were 7.6%, 11.6%, and 17.9%.
Thus, despite the nearly identical initial hardness levels, the HV0.2 values of the two materials remained close after the first 10 h but progressively diverged with increasing annealing time (Figure 10). The difference between the mean hardness values of 71517003188 and C-1 was approximately 2 HV0.2 units after 10 h, increased to approximately 14 HV0.2 units after 30 h, and reached 24 HV0.2 units after 100 h.
Figure 10. Change in HV0.2 hardness of EP-450 steel from SFA wrappers 71517003188 and C-1 as a function of post-irradiation isothermal annealing time at 470 °C.
Over the annealing interval of 10–100 h, the time-dependent changes in HV0.2 were empirically described by logarithmic functions. For the 71517003188 wrapper material, the following relationship was obtained:
HV0.2 = 351.97 − 6.716·ln(t),
with a coefficient of determination of R 2 = 0.906 . For the C-1 wrapper material, the corresponding relationship was
HV0.2 =3 70.92 − 16.113·ln(t),
with R 2 = 0.989 , where t is the cumulative isothermal holding time at 470 °C, in hours. These relationships characterize the experimental time interval of 10–100 h and are used here as empirical descriptions of the observed hardness evolution. The logarithmic character of the dependence reflects a gradual decrease in the rate of HV0.2 change with increasing holding time, which may be associated with a decreasing recovery rate as the more mobile part of the irradiation-induced defect structure is removed or rearranged. At the same time, the form of the empirical fit alone does not allow the recovery mechanism to be identified unambiguously or the kinetics to be classified as diffusion-controlled.
Thus, despite their close initial HV0.2 values, the two investigated wrappers exhibited different thermal stability of the irradiation-hardened state during annealing at 470 °C. The recovery was less pronounced for 71517003188, whereas C-1 exhibited a larger and continuing decrease in hardness over the investigated 10–100 h interval. The accompanying changes in strength and ductility are considered in the following section.

3.4. Time Dependence of Strength and Ductility During Post-Irradiation Annealing

The evolution of the mechanical response of EP-450 steel during post-irradiation isothermal annealing was investigated using the C-1 wrapper material. Engineering stress–strain curves for the initial irradiated condition and after annealing at 470 °C for 10, 30, and 100 h are shown in Figure 11a. The corresponding miniature specimens after uniaxial tensile testing are shown in Figure 11b–e.
Figure 11. Evolution of the mechanical response of EP-450 steel from wrapper C-1 during post-irradiation isothermal annealing at 470 °C: (a) engineering stress–strain curves in the initial irradiated condition and after annealing for 10, 30, and 100 h; appearance of the miniature specimens after uniaxial tensile testing: (b) as-irradiated condition, P1_1.1; (c) 10 h, P1_1.2; (d) 30 h, P1_1.3; (e) 100 h, P1_1.4.
Within the annealed series, the stress–strain curves generally shifted toward lower stresses and greater strain to fracture with increasing annealing time. At the same time, localization of plastic deformation in the necking region became more pronounced, as indicated by the appearance of the fractured specimens (Figure 11b–e).
The quantitative strength and ductility characteristics are summarized in Table 5. For the two specimens in the initial irradiated condition, the σ U T S was 1008.7 and 1018.7 MPa, while σ 0.2 was 938 and 975 MPa, respectively. Despite their similar strength characteristics, the total strain values differed substantially and were 10.08% and 16.15%. Thus, the scatter in the initial condition was expressed primarily in the ductility-related characteristics, whereas the scatter in the strength characteristics was substantially smaller. This scatter may be associated with local structural heterogeneity of the highly irradiated material and the small gauge volume of the miniature specimens, making characteristics related to strain localization and fracture particularly sensitive to the local condition of the investigated region. Therefore, the results of the two initial irradiated tests are presented separately in Table 5 and were not averaged. In view of this scatter, the quantitative magnitude of ductility recovery relative to the initial irradiated condition should be interpreted with caution; emphasis is placed primarily on the direction of change in the ductility characteristics within the annealed series from 10 to 100 h.
Table 5. Strength and ductility characteristics of EP-450 steel from wrapper C-1 before and after post-irradiation isothermal annealing at 470 °C.
After 10 h of annealing at 470 °C, σ U T S was 911.0 MPa and the 0.2% proof stress, σ 0.2 , was 815 MPa. With increasing annealing time to 30 h, σ U T S decreased to 833.1 MPa, whereas σ 0.2 decreased to 789 MPa. After 100 h, σ U T S remained essentially unchanged at 834.7 MPa, while the 0.2% proof stress continued to decrease to 752 MPa.
To compare the time-dependent changes in strength and ductility, the results of the mechanical tests after post-irradiation annealing are presented in Figure 12. Figure 12a shows the ultimate tensile strength, σ U T S , and 0.2% proof stress, σ 0.2 , as functions of annealing time; Figure 12b shows the changes in total strain, ε t o t , uniform plastic strain, ε u , and localized plastic strain, ε l o c . Figure 12c compares the HV0.2 hardness and σ 0.2 values for the states after 10, 30, and 100 h of annealing.
Figure 12. Changes in the mechanical properties of EP-450 steel from wrapper C-1 during post-irradiation isothermal annealing at 470 °C: (a) ultimate tensile strength, σ U T S , and 0.2% proof stress, σ 0.2 , as functions of annealing time; (b) total strain, ε t o t , uniform plastic strain, ε u , and localized plastic strain, ε l o c ; (c) relationship between HV0.2 hardness and the 0.2% proof stress, σ 0.2 , for the states after 10, 30, and 100 h. The dashed lines in panels (a,b) represent empirical logarithmic fits to σ U T S , σ 0.2 , ε t o t , and ε l o c .
As shown in Figure 12a, the most pronounced decrease in ultimate tensile strength occurred between 10 and 30 h: σ U T S decreased from 911.0 to 833.1 MPa. With further increase in annealing time to 100 h, this characteristic remained essentially unchanged at 834.7 MPa. In contrast to σ U T S , the 0.2% proof stress, σ 0.2 , decreased continuously throughout the investigated 10–100 h interval, from 815 to 789 and 752 MPa after 10, 30, and 100 h, respectively.
Over the 10–100 h interval, the change in σ 0.2 was empirically described by the logarithmic relationship
σ 0.2 = 879.54 − 27.41 ln t ,
with R 2 = 0.995 , where t is the cumulative isothermal annealing time in hours. For the ultimate tensile strength, the corresponding relationship was
σ U T S = 971.58 − 32.58 ln t
with R 2 = 0.711 . The substantially lower R 2 value for σ U T S is associated with the nearly identical values of this characteristic after 30 and 100 h. Thus, within the investigated interval, the logarithmic function describes the time-dependent change in σ 0.2 considerably better than that in σ U T S .
The ductility characteristics exhibited different trends (Figure 12b). The total strain, ε t o t , increased from 15.33% after 10 h to 15.99% after 30 h and 17.94% after 100 h. The localized plastic strain, ε l o c , also increased progressively, from 8.84 to 9.49 and 11.45%, respectively. The uniform plastic strain, ε u , varied within a comparatively narrow range, with values of 5.09, 4.80, and 5.69% after 10, 30, and 100 h, respectively. No pronounced monotonic time dependence was observed for ε u ; therefore, no separate empirical fit was applied to this characteristic.
Because the ε t o t values after 10 and 30 h (15.33% and 15.99%) lie within the range of the two as-irradiated values (10.08–16.15%), an increase in total strain relative to the initial irradiated condition cannot be regarded as unambiguous at the early annealing stages. The trend within the annealed series is therefore interpreted descriptively, particularly because each annealed condition was represented by a single miniature tensile specimen.
For the total and localized plastic strains, the experimental data over the 10–100 h interval were adequately described by the empirical logarithmic relationships
ε t o t = 12,505 + 1139 ln t , R 2 = 0.937 ,
and
ε l o c = 6007 + 1140 ln t , R 2 = 0.936 .
The increase in ε t o t over the investigated interval was accompanied predominantly by an increase in ε l o c , whereas ε u showed no pronounced time-dependent trend.
Comparison of the mechanical properties with the hardness measurements discussed in Section 3.3 revealed a particularly close relationship between HV0.2 and the 0.2% proof stress, σ 0.2 (see Figure 12c). For the states after 10, 30, and 100 h, the corresponding pairs of values were 332.7 HV0.2 and 815 MPa, 318.3 HV0.2 and 789 MPa, and 295.7 HV0.2 and 752 MPa, respectively. Within the investigated series, these data were described by the linear relationship
H V 0.2 = 0.5878   σ 0.2 − 145,95 ,
with a coefficient of determination of R 2 = 0.9999 . Because this relationship was obtained from only three annealed states, it should be regarded as an experimental correlation within the investigated range rather than as a universal relationship between hardness and the 0.2% proof stress of EP-450 steel. Confirmation of the robustness of this correlation requires data for a larger number of annealed conditions and, more generally, for materials with different damage doses and irradiation conditions.
Overall, within the investigated annealed series, σ 0.2 showed the closest correspondence with the evolution of HV0.2, whereas σ U T S remained essentially unchanged between 30 and 100 h and ε u showed no pronounced monotonic trend.

4. Discussion

The gradual recovery from irradiation hardening observed at 470 °C is consistent with the known temperature sensitivity of irradiated EP-450 steel. According to Ref. [13], the most pronounced irradiation hardening develops at irradiation temperatures below 400 °C, whereas recovery of ductility becomes noticeable after a 1 h anneal at 450 °C and is substantially advanced at 550 °C. Thus, 470 °C lies in the lower part of the post-irradiation recovery temperature range, where thermally activated evolution of the irradiation-modified structure is already possible but proceeds comparatively slowly.
Microstructural studies of post-irradiation annealing of EUROFER97 indicate that recovery in ferritic–martensitic steels may be accompanied by a decrease in dislocation-loop density together with loop coarsening and rearrangement of the dislocation structure [22]. The evolution of dislocation loops was associated with vacancy and interstitial migration, involving competition between defect annihilation and coarsening. For EP-450 itself, structural rearrangement and indications of irradiation-induced recovery have also been observed during prolonged reactor irradiation at approximately 410 °C [20]. Accordingly, the decreases in HV0.2 and σ 0.2 observed at 470 °C may reflect a gradual reduction in the effectiveness of irradiation-induced obstacles to dislocation motion through thermally activated point-defect migration and recombination, evolution of dislocation loops, and rearrangement of the dislocation structure. In the absence of post-annealing TEM characterization, the relative contributions of individual defect populations cannot be determined.
The evolution of the mechanical properties provides additional information on the character of this recovery. The closest correspondence was observed between HV0.2 and σ 0.2 , whereas σ U T S changed much less after its initial decrease. This behavior suggests that annealing predominantly reduces the resistance to the onset of plastic flow, which is directly related to the effectiveness of obstacles to dislocation motion, while the subsequent strain-hardening response is affected to a lesser extent. Within the annealed series, ε t o t and ε l o c increased with holding time, whereas ε u showed no pronounced monotonic trend. However, because of the scatter in the ductility of the as-irradiated specimens and the use of a single tensile specimen for each annealed condition, these ductility trends should be interpreted descriptively.
Despite their similar initial integral hardness, the two wrappers exhibited clearly different thermal stability during annealing. This indicates that the initial HV0.2 value alone does not uniquely characterize the irradiation-modified state controlling subsequent recovery. Differences in the density and distribution of dislocations, lath, subgrain, and interphase boundaries may result in different sink densities for point defects and thereby affect their migration, recombination, and associated solute redistribution during annealing; such differences may also influence the stability of irradiation-induced clusters and precipitates. These possibilities remain hypotheses because the corresponding defect populations were not characterized directly after annealing.
The differences in the surface corrosion products of the two wrappers may likewise reflect the combined effects of their different operational and post-service histories and the pronounced local heterogeneity of corrosion damage developed during long-term wet storage [23,25]. The phase-selective corrosion involving preferential dissolution of tempered martensite and interphase boundaries reported for material from the same C-1 wrapper [25] provides additional evidence of the complexity and heterogeneity of its initial material condition. However, the corrosion state is considered here only as an indicator of this heterogeneity and not as an established direct cause of the more pronounced recovery of C-1, because its relationship with the bulk irradiation-defect structure was not investigated in the present study. The available data therefore do not allow the contribution of any single factor, including damage dose, to the different recovery behavior of the two wrappers to be isolated.
Overall, the results indicate that the thermal stability of highly irradiated EP-450 at 470 °C is sensitive to the initial irradiation-modified material state and cannot be characterized by the initial hardness or accumulated damage dose alone. Direct identification of the microstructural processes controlling the different recovery responses would require dedicated post-annealing characterization of the irradiation-induced defect structure.

5. Conclusions

Post-irradiation annealing at 470 °C revealed a progressive, time-dependent recovery from irradiation hardening in EP-450 steel from BN-350 SFA wrappers irradiated to 61 and 71 dpa.
Despite the similar initial hardness values of the two wrappers—356 HV0.2 for 71517003188 and 360 HV0.2 for C-1—their thermal responses differed markedly. After 100 h of annealing, the hardness of 71517003188 decreased by 10.2%, whereas that of C-1 decreased by 17.9%. Thus, a similar initial overall hardness does not necessarily imply similar subsequent thermal stability of highly irradiated EP-450 steel.
Mechanical testing of the C-1 material confirmed that the decrease in hardness was accompanied by a progressive reduction in the 0.2% proof stress, σ 0.2 , and changes in ductility. Over the 10–100 h interval, σ 0.2 decreased from 815 to 752 MPa and showed a close correlation with HV0.2. The ultimate tensile strength, σ U T S , decreased from 911.0 MPa after 10 h to 833.1 MPa after 30 h and subsequently remained essentially unchanged. At the same time, the total strain, ε t o t , increased from 15.33 to 17.94%, while the localized plastic strain, ε l o c , increased from 8.84 to 11.45%; ε u showed no pronounced monotonic trend. Thus, the recovery of deformation capacity at 470 °C was manifested predominantly during the localized plastic deformation stage and by increased ductility. Over the 10–100 h interval, σ 0.2 decreased from 815 to 752 MPa, while ε t o t and ε l o c increased from 15.33 to 17.94% and from 8.84 to 11.45%, respectively. The close correspondence between HV0.2 and σ 0.2 indicates a consistent reduction in the resistance to plastic yielding during annealing.
The principal finding is that post-irradiation recovery of highly irradiated EP-450 at the relatively low annealing temperature of 470 °C develops progressively over tens of hours and remains dependent on annealing time up to 100 h. This behavior was established directly for actual BN-350 spent fuel assembly wrapper material.

6. Patents

Invention patent “Grip for Mounting Microspecimens during Tensile Testing”, Authors: Dauletkeldiyev, A.D.; Batyrbekov, E.G.; Skakov, M.K.; Sapatayev, Y.Y.; Koyanbayev, Y.T.; Baklanov, V.V.; Kurbanbekov, Sh.R. No. 32350 dated 31/08/2017 RSE “National Institute of Intellectual Property” of the Ministry of Justice of the Republic of Kazakhstan, 2017.

Author Contributions

Conceptualization, Y.S. and Y.K.; methodology, Y.S.; software, I.K.; validation, K.S., I.K., and Y.A.; formal analysis, Y.S., K.S., and I.K.; investigation, Y.S., I.K., and Y.A.; resources, Y.S. and Y.K.; data curation, Y.A.; writing—original draft preparation, K.S.; writing—review and editing, K.S.; visualization, Y.S.; supervision, Y.K.; project administration, Y.S.; funding acquisition, Y.S. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the Committee of Science of the Ministry of Science and Higher Education of the Republic of Kazakhstan, grant number BR24993104.

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.

Acknowledgments

The authors express their gratitude to the specialists of the Institute of Atomic Energy Branch of the National Nuclear Center of the Republic of Kazakhstan for their professional assistance and advice in obtaining the results.

Conflicts of Interest

The authors declare no conflicts of interest. The funders had no role in the design of the study; in the collection, analyses, or interpretation of data; in the writing of the manuscript; or in the decision to publish the results.

Abbreviations

The following abbreviations are used in this manuscript:
FAFuel assembly
SFASpent fuel assembly
dpaDisplacements per atom
EDMElectrical discharge machining
BCCBody-centered cubic
RIRReference Intensity Ratio
TMTempered martensite

References

  1. International Atomic Energy Agency. Structural Materials for Liquid Metal Cooled Fast Reactor Fuel Assemblies—Operational Behaviour; IAEA Nuclear Energy Series No. NF-T-4.2; IAEA: Vienna, Austria, 2012. [Google Scholar]
  2. International Atomic Energy Agency. Status of Fast Reactor Research and Technology Development; IAEA-TECDOC-1691; IAEA: Vienna, Austria, 2012. [Google Scholar]
  3. International Atomic Energy Agency. Liquid Metal Cooled Reactors: Experience in Design and Operation; IAEA-TECDOC-1569; IAEA: Vienna, Austria, 2007. [Google Scholar]
  4. Cawthorne, C.; Fulton, E.J. Voids in Irradiated Stainless Steel. Nature 1967, 216, 575–576. [Google Scholar] [CrossRef] [Scilit]
  5. Little, E.A.; Stow, D.A. Void-Swelling in Irons and Ferritic Steels: II. An Experimental Survey of Materials Irradiated in a Fast Reactor. J. Nucl. Mater. 1979, 87, 25–39. [Google Scholar] [CrossRef] [Scilit]
  6. Klueh, R.L.; Nelson, A.T. Ferritic/Martensitic Steels for Next-Generation Reactors. J. Nucl. Mater. 2007, 371, 37–52. [Google Scholar] [CrossRef] [Scilit]
  7. Cabet, C.; Dalle, F.; Gaganidze, E.; Henry, J.; Tanigawa, H. Ferritic–Martensitic Steels for Fission and Fusion Applications. J. Nucl. Mater. 2019, 523, 510–537. [Google Scholar] [CrossRef] [Scilit]
  8. Prasad Reddy, G.V.; Karthik, V.; Latha, S.; Venkiteswaran, C.N.; Ramachandran, D.; Albert, S.K. Core Materials for Sodium-Cooled Fast Reactors: Past to Present and Future Prospects. Mater. Perform. Charact. 2022, 11, 2–52. [Google Scholar] [CrossRef] [Scilit]
  9. Sencer, B.H.; Kennedy, J.R.; Cole, J.I.; Maloy, S.A.; Garner, F.A. Microstructural Analysis of an HT9 Fuel Assembly Duct Irradiated in FFTF to 155 dpa at 443 °C. J. Nucl. Mater. 2009, 393, 235–241. [Google Scholar] [CrossRef] [Scilit]
  10. Nikitina, A.A.; Ageev, V.S.; Mitrofanova, N.M.; Naumenko, I.A.; Tselishchev, A.V.; Chernov, V.M. Advances in Structural Materials for Fast-Reactor Cores. At. Energy 2016, 119, 362–371. [Google Scholar] [CrossRef] [Scilit]
  11. Mukhamedov, N.; Toleubekov, K.; Vityuk, G.; Bekmuldin, M.; Dolzhikov, S. Decommissioning of the BN-350 Fast Neutron Reactor: History Review and Current Status. Energies 2025, 18, 3486. [Google Scholar] [CrossRef] [Scilit]
  12. Klueh, R.L.; Shiba, K.; Sokolov, M.A. Embrittlement of Irradiated Ferritic/Martensitic Steels in the Absence of Irradiation Hardening. J. Nucl. Mater. 2008, 377, 427–437. [Google Scholar] [CrossRef] [Scilit]
  13. Khabarov, V.S.; Dvoriashin, A.M.; Porollo, S.I. Microstructure, Irradiation Hardening and Embrittlement of 13Cr2MoNbVB Ferritic–Martensitic Steel after Neutron Irradiation at Low Temperatures. J. Nucl. Mater. 1996, 233–237, 236–239. [Google Scholar] [CrossRef] [Scilit]
  14. Dvoriashin, A.M.; Porollo, S.I.; Konobeev, Y.V.; Garner, F.A. Influence of High-Dose Neutron Irradiation on Microstructure of EP-450 Ferritic–Martensitic Steel Irradiated in Three Russian Fast Reactors. J. Nucl. Mater. 2004, 329–333, 319–323. [Google Scholar] [CrossRef] [Scilit]
  15. Porollo, S.I.; Konobeev, Y.V.; Ivanov, A.A.; Shulepin, S.V.; Leont’eva-Smirnova, M.V.; Nikolaeva, N.S. Swelling and Radiation Creep of Ferrite-Martensite Steel Irradiated in the BN-350 Reactor in a Wide Range of Temperature and Damaging Dose. At. Energy 2016, 120, 189–198. [Google Scholar] [CrossRef] [Scilit]
  16. Dvoriashin, A.M.; Porollo, S.I.; Konobeev, Y.V.; Budylkin, N.I.; Mironova, E.G.; Ioltukhovskiy, A.G.; Leontyeva-Smirnova, M.V.; Garner, F.A. Mechanical Properties and Microstructure of Three Russian Ferritic/Martensitic Steels Irradiated in BN-350 Reactor to 50 dpa at 490 °C. J. Nucl. Mater. 2007, 367–370, 92–96. [Google Scholar] [CrossRef] [Scilit]
  17. van der Schaaf, B.; Petersen, C.; De Carlan, Y.; Rensman, J.W.; Gaganidze, E.; Averty, X. High Dose, up to 80 dpa, Mechanical Properties of Eurofer 97. J. Nucl. Mater. 2009, 386–388, 236–240. [Google Scholar] [CrossRef] [Scilit]
  18. Gaganidze, E.; Petersen, C.; Materna-Morris, E.; Dethloff, C.; Weiß, O.J.; Aktaa, J.; Povstyanko, A.; Fedoseev, A.; Makarov, O.; Prokhorov, V. Mechanical Properties and TEM Examination of RAFM Steels Irradiated up to 70 dpa in BOR-60. J. Nucl. Mater. 2011, 417, 93–98. [Google Scholar] [CrossRef] [Scilit]
  19. Weiß, O.J.; Gaganidze, E.; Aktaa, J. Quantitative Characterization of Microstructural Defects in up to 32 dpa Neutron Irradiated EUROFER97. J. Nucl. Mater. 2012, 426, 52–58. [Google Scholar] [CrossRef] [Scilit]
  20. Tsay, K.V.; Merezhko, D.A.; Kim, Y.R.; Merezhko, M.S. Low-Temperature Structural Instability of 12% Cr Ferritic–Martensitic Steel Irradiated to 53 dpa in the BN-350 Fast Reactor. Materialia 2025, 40, 102393. [Google Scholar] [CrossRef] [Scilit]
  21. Sacksteder, I.; Schneider, H.-C.; Materna-Morris, E. Determining Irradiation Damage and Recovery by Instrumented Indentation in RAFM Steel. J. Nucl. Mater. 2011, 417, 127–130. [Google Scholar] [CrossRef] [Scilit]
  22. Chauhan, A.; Yuan, Q.; Dethloff, C.; Gaganidze, E.; Aktaa, J. Post-Irradiation Annealing of Neutron-Irradiated EUROFER97. J. Nucl. Mater. 2021, 548, 152863. [Google Scholar] [CrossRef] [Scilit]
  23. Kozhakhmetov, Y.A.; Koyanbaev, Y.T.; Dauletkhanov, Y.D.; Mukhamedzhanova, R.M.; Urkunbay, A.S.; Sapatayev, Y.Y. Condition of the Material of the Case of Exhaust BN-350 Reactor Fuels in Long Storage. NNC RK Bull. 2019, 4, 113–118. (In Russian) [Google Scholar] [CrossRef] [Scilit]
  24. Kozhakhmetov, E.A.; Koyanbayev, E.T.; Dauletkhanov, E.D.; Mukhamedzhanova, R.M.; Urkunbay, A.S.; Sapatayev, E.E. Evaluation of Corrosion Condition of BN-350 Reactor Spent Fuel Assembly Casing Material after Short-Term Thermal Influence. NNC RK Bull. 2020, 1, 98–103. (In Russian) [Google Scholar] [CrossRef] [Scilit]
  25. Merezhko, D.A.; Merezhko, M.S.; Short, M.P. Corrosion of EP-450 Ferritic-Martensitic Steel after Neutron Irradiation and Long-Term Storage in Spent Fuel Pool. J. Nucl. Mater. 2026, 618, 156223. [Google Scholar] [CrossRef] [Scilit]
  26. Koyanbayev, Y.T.; Skakov, M.K.; Ganovichev, D.A.; Martynenko, Y.A.; Sitnikov, A.A. Simulation of the Thermal Conditions of Cask with Fuel Assemblies of BN-350 Reactor for Dry Storage. Sci. Technol. Nucl. Install. 2019, 2019, 3045897. [Google Scholar] [CrossRef] [Scilit]
  27. Kumar, K.; Pooleery, A.; Madhusoodanan, K.; Singh, R.N.; Chakravartty, J.K.; Dutta, B.K.; Sinha, R.K. Use of Miniature Tensile Specimen for Measurement of Mechanical Properties. Procedia Eng. 2014, 86, 899–909. [Google Scholar] [CrossRef] [Scilit]
  28. Dauletkeldiyev, A.D.; Batyrbekov, E.G.; Skakov, M.K.; Sapatayev, Y.Y.; Koyanbayev, Y.T.; Baklanov, V.V.; Kurbanbekov, S.R. Grip for Mounting Microspecimens During Tensile Testing. Invention Patent No. 32350, 31 August 2017. Available online: https://gosreestr.kazpatent.kz/Invention/Details?docNumber=261685 (accessed on 20 August 2026).
  29. Hosemann, P.; Vieh, C.; Greco, R.R.; Kabra, S.; Valdez, J.A.; Cappiello, M.J.; Maloy, S.A. Nanoindentation on Ion Irradiated Steels. J. Nucl. Mater. 2009, 389, 239–247. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.