The Effects of Austempering Time on Wear Behavior of the Novel GCr15Si1MoNbV Bearing Steel

,
,
,
,
,
,
,
,
…
1
School of Mechanical and Automotive Engineering, Science and Technology College of Hubei University of Arts and Science, Xiangyang 441025, China
2
China Ordnance Industry Group Jiangshan Heavy Industry Research Institute Co., Ltd., Xiangyang 441005, China
3
National United Engineering Laboratory for Advanced Bearing Tribology, Henan University of Science and Technology, Luoyang 471023, China
4
Hubei Provincial Key Laboratory of Design and Testing for Power Systems of Pure Electric Vehicles, Hubei University of Arts and Science, Xiangyang 441053, China

Abstract

This paper investigates the wear resistance of Nb- and V-microalloyed bearing steel GCr15Si1Mo under different loads after isothermal treatment at 190 °C for 2 h, 10 h, and 48 h. The results show that the average friction coefficient of the 2 h isothermally treated specimen exhibits a first decreasing and then increasing trend, while that of the 10 h specimen increases slowly with increasing load, and that of the 48 h specimen displays a first increasing and then decreasing trend. For the 2 h and 10 h isothermally treated specimens, the wear weight loss does not increase linearly with time, whereas for the 48 h bainite-dominated specimen, the wear weight loss increases linearly with time. The wear mechanism of the 2 h martensitic microstructure is dominated by abrasive ploughing. The 10 h martensite–bainite–retained austenite composite microstructure possesses a certain load-bearing capacity but is also prone to adhesive tearing. For the 48 h specimen, abrasive action dominates at low loads; at intermediate loads, enhanced adhesion leads to an increase in the friction coefficient; and at high loads, a relatively continuous and dense tribolayer forms at the interface.

1. Introduction

Bearings, as one of the most fundamental and critical functional components in modern mechanical equipment, are widely used in fields such as aerospace, rail transit, wind power generation, high-end CNC machine tools, the automotive industry, and major engineering equipment [1]. At present, the most widely used bearing steel worldwide is still represented by high-carbon chromium GCr15, which is generally subjected to quenching and tempering to obtain a martensitic matrix with dispersed carbides [2]. This type of bearing steel possesses high hardness and wear resistance under conventional service conditions and has been widely and persistently applied in the industrial sector. However, as equipment develops toward high speed, heavy load, long life, and high reliability, the wear resistance of conventional martensitic bearing steel can hardly meet the demands of a new generation of high-end equipment for ultra-long-life bearing materials [3,4,5,6]. Therefore, developing novel bearing steel materials through innovations in microstructural design and heat treatment processes has become an important direction in the field of bearing steel research.
Bainitic bearing steel, as a novel microstructural system distinct from conventional martensitic structures, has attracted extensive attention from researchers both domestically and internationally in recent years [7,8,9,10]. Bainitic microstructures simultaneously possess relatively high strength and good toughness, and their formation involves a relatively low internal stress level and good microstructural stability, offering potential advantages in suppressing the initiation and propagation of fatigue cracks. In particular, lower bainite or nanobainite obtained through austempering exhibits fine ferrite laths, high dislocation density, and a reasonable distribution of retained austenite, demonstrating promising application potential under complex loading conditions [11,12,13,14,15]. Meanwhile, the service performance of bearing steel depends not only on the type of matrix microstructure but also closely on carbide morphology, retained austenite stability, and the synergistic effects among multiphase constituents [16,17,18]. Bainitic bearing steel typically exhibits a multiphase composite structure composed of bainitic ferrite, retained austenite, and carbides [19,20,21,22], and its performance is highly sensitive to microstructural details and heat treatment parameters. Under different heat treatment paths, significant differences exist in bainitic lath size, transformation amount, carbide precipitation behavior, and retained austenite content [23,24,25,26], which consequently lead to pronounced variations in the wear behavior of the material. Microalloying is an important means of enhancing the comprehensive performance of bearing steel [27,28], which can play a positive role in grain refinement, regulation of carbide precipitation, and stabilization of retained austenite by introducing microalloying elements, thereby providing a new pathway for the further optimization of the microstructure and properties of nanobainitic bearing steel [19,27,29,30].
Heat treatment significantly affects the tribological behavior and the dominant wear mechanism of bearing steel by altering its microstructure (such as bainitic lath size, retained austenite morphology and stability, and carbide size/type and distribution) as well as macroscopic mechanical indicators (hardness, toughness, and strain response capability). Differences in austempering temperature, holding time, and subsequent tempering schedule lead to systematic changes in the degree of microstructural refinement, average carbide size, and damage mode, thereby altering the wear volume and wear morphology characteristics.
Austempering temperature is a key factor controlling the microstructural scale and phase composition of bainite. Both Wang et al. [31] and Su et al. [32] pointed out that a lower isothermal temperature generally favors the formation of fine and dense bainitic lath structures and highly stable film-like retained austenite, thereby improving the hardness and resistance to plastic deformation of the material. Under sliding or rolling contact conditions, such refined microstructures can reduce surface shear deformation and suppress abrasive particle formation, exhibiting superior wear resistance [33]. Conversely, a higher isothermal temperature often leads to microstructural coarsening and reduced retained austenite stability, making the material more susceptible to localized plastic flow and surface damage. Holding time affects microstructural uniformity and stability by regulating carbon partitioning kinetics and the phase transformation process. Wei et al. [34] showed that an appropriate holding time favors sufficient microstructural transformation and the formation of a relatively stable multiphase structure; however, when the holding time is excessively long, the microstructure may undergo further recovery or coarsening, or the precipitation behavior may become more pronounced, resulting in decreased hardness or an increased amount of brittle phases and interfacial defects, leading to increased wear volume.
For bearing steel, heat treatment can substantially alter the size, type, and content of carbides, which may, on the one hand, improve resistance to micro-cutting, but, on the other hand, may also initiate microcracks at interfaces, thereby becoming a source of abrasive particles and causing a transition in the wear mechanism [35]. Qin [36] pointed out that refining cementite or completely dissolving it can significantly improve the wear resistance of nanobainitic bearing steel, with cementite refinement increasing wear resistance by approximately 23%. Li et al. [37] also reported that the hardness level and the content of spherical carbides have a significant influence on wear volume and damage morphology, indicating that achieving a match between “hardness and carbide state” through heat treatment is an important approach for controlling wear behavior.
In summary, heat treatment parameters ultimately determine the dominant wear mechanism and wear degree of bearing steel under different service conditions by (i) regulating the scale and stability of bainitic/martensitic microstructures, (ii) altering the morphology/size/distribution of retained austenite and carbides, and (iii) influencing hardness and local deformation/crack response mechanisms. Therefore, in the design of bearing steel, it is necessary to take service conditions as constraints and comprehensively optimize the isothermal temperature, holding time, and carbide characteristics in the microstructure so as to achieve synergistic enhancement of wear resistance and damage resistance.
Nevertheless, although existing studies have demonstrated that the tribological performance of nanobainitic bearing steel is sensitive to austempering temperature, carbide features and microalloying modification, key research gaps still exist. Most available works focus primarily on austempering temperature, while the coupled effect of austempering holding time on the evolution of multiphase microstructures (bainitic ferrite, retained austenite and carbides) and wear mechanism transition remains insufficiently understood, especially for Nb–V microalloyed GCr15Si1Mo nanobainitic bearing steel.
Therefore, this paper investigates the wear resistance performance under different loads of Nb-V microalloyed GCr15Si1Mo nanobainitic bearing steel with distinct microstructures induced by varied austempering holding times. The wear resistance in three typical microstructural states (martensite-dominated, martensite–bainite–retained austenite composite, and bainite-dominated) is systematically explored. This paper further analyzes how microstructural constituents, including matrix phases, retained austenite and carbides, dominate wear mechanism transitions and interprets the different load-dependent wear behavior from the competition between interfacial tribolayer compaction and shear disturbance. The correlation among austempering holding time, multiphase microstructural features and service tribological performance is established, which reveals the influence of multiphase composite microstructure on wear resistance and provides experimental support for heat treatment process optimization of this novel bearing steel.

2. Materials and Methods

This experiment employed a self-designed GCr15Si1MoNbV bearing steel, with the chemical composition by weight as follows: 1.0% carbon (C), 1.46% silicon (Si), 0.34% manganese (Mn), 1.4% chromium (Cr), 0.38% molybdenum (Mo), 0.075% niobium (Nb), and 0.065% vanadium (V), and the balance is Fe.
Prior to austempering treatment, the experimental steel was subjected to annealing in order to eliminate coarse and network carbides in the as-cast microstructure and to obtain a uniform and fine initial microstructure. By employing cyclic heating to near the critical temperature combined with slow cooling, lamellar or network cementite gradually decomposes, breaks up, and transforms into dispersed spherical carbides, thereby improving microstructural uniformity and reducing the influence of carbide segregation on subsequent phase transformation behavior. The phase transformation temperatures and bainitic transformation kinetics of the experimental steel were measured using a DIL805 dilatometer. The results showed that the Ac1, Ac3, and Ms temperatures were 792 °C, 812 °C, and 172 °C, respectively. Based on the results, the austenitization temperature was determined to be 900 °C, and the austempering temperature and time were determined to be 190 °C and 2 h, 10 h and 48 h. According to the spheroidizing annealing process route shown in Figure 1a, the experimental steel was subjected to a four-cycle cyclic spheroidizing annealing treatment. The experimental steel was first heated from room temperature to 10 °C below Ac1 within 60 min and held for 30 min, then cooled in the furnace to 80 °C below Ac1 within 25 min and held for 45 min. The above processes of holding after heating and holding after cooling constitute one spheroidizing cycle, which was repeated for a total of 4 cycles. Finally, the specimen was cooled in the furnace to room temperature, completing the spheroidizing annealing treatment. After the spheroidizing annealing treatment was completed, based on the results of bainitic transformation kinetics, the experimental steel was subjected to austempering treatment according to the process shown in Figure 1b. The specimen was heated to 900 °C in a box-type resistance furnace for austenitization for 0.75 h, and then rapidly transferred to a salt bath furnace at 190 °C for isothermal treatment for 2 h, 10 h, and 48 h, respectively. After isothermal treatment, the specimen was air-cooled to room temperature, then tempered at 200 °C for 1 h, and finally air-cooled to room temperature to complete the austempering heat treatment. The salt bath medium used was a mixed salt solution of KNO3 and NaNO2 with a mass fraction of 50% each. In this study, three heat treatment processes with different isothermal holding times were designed to systematically investigate the microstructural evolution of GCr15Si1MoNbV bearing steel under low-temperature austempering conditions and its effect on wear resistance.
Figure 1. The process of heat treatment: (a) spheroidizing annealing; (b) austempering.
End-face friction and wear tests were carried out using an MMU-5G end-face friction and wear testing machine. The wear specimens were disc-shaped specimens prepared under three heat treatment processes, with a diameter of 38 mm. The counterpart specimen was a GCr15 specimen with a hardness of 63 HRC and was machined into a tubular shape with an outer diameter of 27 mm and a wall thickness of 3 mm. The contact end faces of both the specimens and the counterpart specimens were precisely machined by a grinding machine to ensure consistent surface roughness of each friction pair, with Ra controlled at 0.2 μm. The schematic diagram of friction and wear is shown in Figure 2. To investigate the influence of different service conditions on the wear behavior of the experimental steel, three loads of 1000 N, 1300 N, and 1600 N were set, with a rotational speed of 200 r/min and a total wear test duration of 120 min. The nominal contact area was determined from the annular contact surface of the counterpart specimen, which had an outer diameter of 27 mm and an inner diameter of 21 mm, yielding a nominal contact area of approximately 226.18 mm2. Based on this area, the nominal average contact pressures under applied loads of 1000, 1300, and 1600 N were calculated to be 4.42, 5.75, and 7.07 MPa, respectively. To avoid aging-induced microstructural changes caused by temperature rise in the wear track, the test was stopped every 20 min, and the specimens were ultrasonically cleaned and then weighed for wear weight loss using an ATX224R balance with an accuracy of 0.1 mg. The morphology and surface condition of the wear track were observed and analyzed using a KC-X3000 three-in-one precision measuring microscope. The wear morphology was observed using an optical microscope (OM) and a scanning electron microscope (SEM), and the morphology and surface condition of the wear track were observed and analyzed using a KC-X3000 three-in-one precision measuring microscope to measure the wear volume and compare the wear resistance of the material under different process conditions.
Figure 2. Schematic of the end-face friction and wear configuration.

3. Results

Figure 3, Figure 4, Figure 5 and Figure 6 show the corresponding microstructures (OM, SEM, TEM and XRD) and were introduced in Reference [21]. Figure 3 shows that with the extension of the austempering holding time from 2 h to 48 h, the microstructure exhibits an obvious trend of refinement and homogenization. It can be seen from Figure 4 that the microstructure is dominated by martensite with a small amount of unevenly distributed bainite after austempering for 2 h. When the austempering holding time reaches 10 h, the fraction of bainite increases remarkably, forming a typical martensite–bainite composite microstructure. After 48 h of austempering, the microstructure evolves toward a bainite-dominated state. Figure 5a reveals that nanobainite with a lath structure partially forms after 2 h of austempering. Nevertheless, martensite remains the major constituent, and retained austenite is predominantly blocky. For the 10 h-austempered sample, the density of nanobainitic laths rises substantially. Carbon-enriched retained austenite tends to form thin interlath films with improved stability. After 48 h, bainite transformation is essentially finished, accompanied by coarsened bainitic laths and trace retained austenite. The volume fractions of each phase of the experimental steel austempered at 190 °C for different holding times are listed in Table 1. With increasing austempering holding times, the volume fraction of retained austenite does not decrease linearly; instead, it first increases and then decreases. This behavior is governed jointly by austenite stability and transformation kinetics.
Figure 3. OM microstructures of samples with different austempering times: (a) 2 h; (b)10 h; and (c) 48 h [21].
Figure 4. SEM microstructures of samples with different austempering times: (a) 2 h; (b) 10 h; and (c) 48 h [21].
Figure 5. TEM microstructures of samples with different austempering times: (a) 2 h; (b) 10 h; and (c) 48 h [21].
Figure 6. XRD patterns of samples with different austempering times: (black) 2 h; (red) 10 h; and (blue) 48 h [21].
Table 1. The volume fractions of retained austenite (Vγ), carbides (Vc), bainite (VB), and martensite (VM) at different austempering times.
Figure 7 shows the effect of load on the friction coefficient of specimens with different austempering times. The coefficient of friction (COF) was obtained from real-time friction force recorded by the tribometer. The error bars in Figure 7d represent the standard deviation (SD) from repeated parallel tests. Following the Guide to the Expression of Uncertainty in Measurement (GUM), the overall measurement uncertainty of COF was further assessed. The uncertainty sources include the repeatability of tribological tests, the calibration error of the load sensor, the speed fluctuation of the rotary stage, and the signal drift of the data acquisition module. The combined standard uncertainty uc was calculated, and the expanded uncertainty U = k × uc was reported with a coverage factor k = 2, corresponding to a confidence level of approximately 95%. The expanded uncertainty for COF in this work is U = ±0.03.
Figure 7. Effect of different loads on the friction coefficient of specimens with different austempering times: (a) 2 h; (b) 10 h; and (c) 48 h. (d) Average friction coefficient in the steady-state stage.
The friction coefficient (COF) curves of the three microstructural specimens under different loads are generally relatively stable, with the steady-state stage fluctuating slightly around the mean value and no obvious continuous drift. The steady-state average friction coefficient and the statistical bar chart in Figure 7d indicate that the average friction coefficients of the three processes are generally concentrated in the range of 0.31–0.35. This indicates that at 200 r/min, the interfacial shear process is more continuous, and the effect of transient shear concentration in elevating the friction coefficient is weakened, placing the interface in a stronger state of dynamic renewal. The participation of wear debris and the load-bearing tribolayer in the interface is enhanced, and shear tends to occur within the interfacial layer, thereby reducing the steady-state average friction coefficient and improving curve stability.
The average friction coefficient of the 2 h isothermally treated specimen exhibits a “first decreasing and then increasing” trend (0.327 → 0.319 → 0.347). In terms of curve morphology, relatively obvious transient spikes are still visible at 1000 N; at 1300 N, the curve is smoother with fewer spikes; and at 1600 N, the fluctuation increases slightly, accompanied by a rebound in the mean value. This indicates that interfacial shear is more uniform at intermediate loads, but at high loads, the friction coefficient rebounds due to enhanced local shear disturbance (more frequent local destruction and reconstruction of the load-bearing layer as well as enhanced adhesion). The average friction coefficient of the 10 h specimen increases slowly with increasing load (0.322 → 0.330 → 0.336). Figure 7 shows that the steady-state fluctuation amplitudes of the three curves are small and generally stable, and their response to load changes is relatively mild. This is usually related to the “buffering” effect of the multiphase microstructure in contact stress distribution, so that an increase in load mainly manifests as a slight elevation in the mean value without causing significant amplification of fluctuations. The average friction coefficient of the 48 h specimen exhibits a “first increasing and then decreasing” trend (0.312 → 0.332 → 0.322). As shown in Figure 7c, the fluctuation differences among different loads are not significant at the curve level, and the mean value at 1300 N is slightly higher but is not accompanied by the concentrated appearance of obvious instability spikes, indicating that for this microstructure at 200 r/min, the load variation is more reflected in the adjustment of the steady-state shear resistance level rather than a substantial change in interfacial stability.
Figure 8 shows the wear weight loss evolution of the microstructures austempered for different times under different load conditions. As shown in Figure 8a, for the 2 h martensite-dominated specimen, the wear weight loss does not increase linearly with time, and an obvious anomaly appears in the early stage of loading: within 40 min, the wear weight loss under 1600 N is instead significantly smaller than that under 1000 N. Subsequently, as time extends and the wear process proceeds, the wear increment gradually tends toward an overall trend more consistent with load enhancement. Meanwhile, the 2 h specimen also exhibits the characteristic that 1300 N is overall greater than 1600 N, i.e., wear at intermediate load is greater than that at high load. This phenomenon indicates that at a rotational speed of 200 r/min, load does not increase wear merely by raising the contact stress; rather, a higher load may promote the more rapid formation of a relatively stable load-bearing state at the interface, thereby suppressing material removal in the early stage. Under intermediate load, the interface lies in a regime of “insufficient stability coupled with enhanced shear disturbance,” causing wear to accumulate more readily, ultimately producing the non-monotonic result of 1300 N being higher than 1600 N. This is consistent with the previously observed characteristics of the friction coefficient exhibiting an inflection point and a rearrangement of the load effect at 200 r/min.
Figure 8. Wear mass loss evolution of three microstructures under different loads at 200 r/min: (a) 2 h; (b) 10 h; and (c) 48 h.
As shown in Figure 8b, the time evolution law of the 10 h martensite–bainite–retained austenite composite specimen is basically consistent with that of the 2 h specimen, likewise exhibiting nonlinear growth and an overall ranking of “1300 N > 1600 N”; its stage characteristics are also consistent with those of the 2 h specimen, i.e., the early stage does not show a wear gradation that increases monotonically with load. However, compared with the 2 h specimen, the difference between 1000 N and 1600 N for the 10 h specimen in the first few stages is smaller, indicating that the composite microstructure responds more mildly to load changes in the early stage at intermediate speed, and the difference in interfacial load-bearing state between low and high loads is not as “strongly separated” as that of the martensitic microstructure, thereby making the early wear amounts closer. Nevertheless, as time extends, the wear under 1300 N continues to accumulate and gradually becomes the highest overall, still reflecting the tendency toward sustained material removal under intermediate load.
For the 48 h bainite-dominated specimen, the wear weight loss increases linearly with time, indicating that its wear rate is relatively stable with small stage-wise fluctuations, and overall, it still reflects a trend of increasing wear with increasing load; however, in the first few time intervals, the phenomenon of 1300 N being greater than 1600 N is also observed, after which it gradually returns to a gradation law more consistent with load enhancement. This indicates that even though the steady-state wear characteristics of the bainitic microstructure are more pronounced, the early-stage establishment process of the interfacial load-bearing structure at intermediate speed is still affected by load, and the stronger compaction effect under high load may inhibit wear to a certain extent in the early stage, so that 1600 N does not immediately manifest as higher wear.
Combining the wear laws with the load dependence of the friction coefficient, it can be seen that at a rotational speed of 200 r/min, the interface is in a stronger state of dynamic renewal, and load simultaneously affects the compaction stability of the load-bearing structure and the intensity of shear disturbance, with the two exhibiting a competitive relationship. A higher load in the early stage may reduce the material removal rate through more sufficient compaction and formation of the load-bearing structure, whereas the intermediate load regime is more prone to a state of enhanced shear disturbance coupled with insufficient load-bearing stability, thereby leading to faster wear accumulation and ultimately manifesting as 1300 N being higher than 1600 N in the overall or partial stages. Thus, the stage-wise complex variations in wear weight loss at 200 r/min and the non-monotonic load effect of the friction coefficient at intermediate speed corroborate each other.
Figure 9 shows the wear morphology observation results of the 2 h martensitic specimen. As shown in Figure 9a, under 1000 N, the wear track mainly exhibits relatively regular parallel ploughing grooves with clear grooves and good overall continuity, a small spalling scale, and no large-area sheet-like delamination or lamellar tearing. As shown in Figure 9b, when the load increases to 1300 N, a more obvious dark covering band and sheet-like smearing structure appear in the center of the wear track, accompanied by numerous irregular bright spots and localized spalling. After further increasing to 1600 N, the dark region in the middle of the wear track becomes more continuous, the dense tribolayer becomes wider, and the grooves become relatively refined. Boundary extrusion is obvious, but large-scale sheet-like spalling actually decreases.
Figure 9. Wear morphology of the specimens austempered for 2 h under different load conditions at 200 r/min: (a) 1000 N; (b) 1300 N; and (c) 1600 N.
Figure 10 shows the wear morphology observation results of the 10 h martensite–bainite–retained austenite composite microstructure specimen. From the wear track morphology, under 1000 N, the wear track is dominated by relatively regular parallel ploughing grooves with good groove continuity, while adhesive smearing and dark covering zones are relatively scattered. At 1300 N, more obvious sheet-like smearing/covering bands and irregular adhesive tearing appear in the wear track, and the dark tribolayer exhibits the coexisting characteristics of “formation–shearing–localized tearing,” with localized spalling and lamellar delamination traces becoming more prominent. Under 1600 N, the dark covering zone of the wear track becomes more continuous, the tribolayer (dense compacted layer) is more readily formed and participates in load bearing, and the ploughing grooves become relatively refined, but boundary extrusion/piling-up and signs of localized damage are visible.
Figure 10. Wear morphology of the specimens austempered for 10 h under different load conditions at 200 r/min: (a) 1000 N; (b) 1300 N; and (c) 1600 N.
Figure 11 shows the wear morphology observation results of the 48 h bainitic microstructure specimen. At 1000 N, the wear track surface is dominated by relatively continuous and comparatively uniform abrasive ploughing grooves, accompanied locally by slight adhesive smearing and fine spalling pits. The overall interface is still dominated by shallow-layer shearing and micro-cutting, and a distinct compacted tribolayer has not yet formed. When the load increases to 1300 N, the interfacial contact stress is markedly enhanced, and the adhesive action is intensified. Irregular bright-spot adhesive tearing zones and localized tribolayer fracture phenomena are visible in the wear track, indicating that the interface is in a cyclic state of “formation–shearing–tearing.” When the load is further increased to 1600 N, a relatively continuous dense tribolayer (compacted layer) gradually forms in the center of the wear track, accompanied by the appearance of boundary material extrusion ridges, indicating that the surface-layer material undergoes plastic flow and compaction reconstruction under high stress.
Figure 11. Wear morphology of the specimens austempered for 48 h under different load conditions at 200 r/min: (a) 1000 N; (b) 1300 N; and (c) 1600 N.
Figure 12 shows the SEM observation results of the wear morphology of the 2 h martensitic specimen at 200 r/min. As shown in Figure 12a, under this load, the wear track surface exhibits relatively smooth characteristics, and obvious adhesives form at the edge region of the wear track. As shown in Figure 12b, under a load of 1300 N, in addition to the continued presence of adhesion phenomena, fine spalling pits begin to form in the middle of the wear track, indicating that wear becomes more severe. As shown in Figure 12c, at 1600 N, although the load further increases, excessive spalling pits are not observed compared with at 1300 N.
Figure 12. The SEM wear morphology of the specimens austempered for 2 h under different load conditions at 200 r/min: (a) 1000 N; (b) 1300 N; and (c) 1600 N.
As shown in Figure 13a, under a load of 1000 N, the wear track surface of the specimen austempered for 10 h is relatively flat, and the wear is mild. The SEM image shows that the surface mainly exhibits uniform abrasive grooves, and these grooves are relatively shallow with relatively smooth boundaries. Figure 13b shows that when the load increases to 1300 N, the wear track surface begins to exhibit stronger wear characteristics. Figure 13c indicates that under a load of 1600 N, the SEM image of the wear track of the specimen austempered for 10 h shows a relatively uniform compacted tribolayer.
Figure 13. The SEM wear morphology of the specimen austempered for 10 h under different load conditions at 200 r/min: (a) 1000 N; (b) 1300 N; and (c) 1600 N.
As shown in Figure 14, under relatively low load, the wear track of the specimen austempered for 48 h mainly exhibits a smooth compacted layer, with a small amount of adhesives appearing at the edges. Under a load of 1300 N, as the load increases, the adhesives increase significantly, and the tribolayer is distributed more uniformly on the surface. It can be seen from the image that the compacted layer is further densified, and some fine spalling pits appear. Under a load of 1600 N, the adhesives are significantly reduced, and the wear track surface appears flatter and smoother. The SEM image shows that the compacted tribolayer is more uniform and dense, and no large number of spalling pits is observed.
Figure 14. The SEM wear morphology of the specimen austempered for 48 h under different load conditions at 200 r/min: (a) 1000 N; (b) 1300 N; and (c) 1600 N.
Figure 15 shows the statistical results of wear volume of the three specimens as a function of load. The wear volume of the specimen austempered for 2 h exhibits a trend of first increasing and then decreasing with increasing load. The wear volume of the specimen austempered for 10 h exhibits a trend of first increasing and then decreasing with increasing load. The wear volume of the specimen austempered for 48 h increases continuously, and as the load increases, the wear volume increases significantly.
Figure 15. The wear volume variation of samples with different isothermal holding times under different load conditions at 200 r/min.
As shown in Figure 16, the wear track cross-sectional morphologies corresponding to the three austempering times exhibit obvious differences and are closely related to the microstructure and mechanical properties. The specimen austempered for 2 h is mainly martensitic, with the highest hardness and the poorest toughness. From the cross-sectional morphology in Figure 16, its wear track width is relatively small, and the bottom is relatively flat. The specimen austempered for 10 h has a martensite–bainite–retained austenite composite microstructure, with the second-highest hardness but the best toughness. From the wear track morphology, it can be seen that its wear track depth increases markedly, the bottom undulation is relatively obvious, and it is accompanied by a certain degree of material extrusion and plastic flow traces. The specimen austempered for 48 h has a bainitic microstructure, with the lowest hardness and toughness, second only to the specimen austempered for 10 h. Its wear track width is the largest, the edge transition is relatively gentle, and the bottom exhibits obvious plastic indentation characteristics.
Figure 16. Cross-sectional morphologies of wear tracks of specimens with different isothermal quenching times under rolling wear at a rotational speed of 200 r/min: (a) 2 h; (b) 10 h; and (c) 48 h.

4. Discussion

4.1. Wear Morphology Analysis

4.1.1. OM Morphology Analysis

Under the load of 1000 N, for the specimen with martensitic microstructure austempered for 2 h, the wear mechanism is dominated by stable abrasive ploughing; material removal is mainly “shallow-layer cutting”; and no strong adhesive tearing occurs at the interface. Although the matrix directly participates in shearing at this time, the contact stress has not yet reached the level that triggers severe adhesive damage or lamellar instability; therefore, the material removal amount is relatively low, manifesting as the smallest weight loss. Such limited interfacial disturbance is also consistent with the relatively stable characteristics of the friction coefficient. When the load increases to 1300 N, the interface enters a stage of enhanced adhesion, the third-body compaction has not yet fully stabilized, and the shear stress is sufficient to trigger localized lamellar tearing. That is, in this intermediate load range, the interface possesses relatively strong adhesion while a sufficiently stable and dense load-bearing layer has not yet formed, resulting in repeated cycles of “formation–shearing–tearing.” Material removal is no longer shallow-layer abrasive cutting but rather lamellar tearing-type spalling, and the amount of material detachment per unit time increases significantly. This leads to the maximum wear weight loss shown in Figure 8a. After further increasing to 1600 N, the third body is more fully compacted, the interfacial load-bearing capacity is enhanced, and shearing gradually transfers into the interior of the tribolayer. Consequently, despite the higher load, because the compacted layer bears part of the shear, the proportion of direct matrix spalling decreases, so the overall weight loss is lower than that at 1300 N. These mechanistic processes also account for the evolution of the friction coefficient shown in Figure 7.
Figure 10a indicates that the interface is mainly in a relatively stable state dominated by abrasive ploughing, and material removal is mainly shallow-layer cutting; therefore, the weight loss is the smallest. As the load increases, the shear action is enhanced and the frictional resistance rises. At 1300 N, the interface is in the regime where adhesion and tribolayer instability are most active, and the material is more readily removed in sheet-like form; therefore, the weight loss reaches its maximum, while the friction coefficient also continues to increase (increased adhesive contribution and more complex shear paths). Figure 10c indicates that although the overall shear resistance is still greater under high load (hence, the highest friction coefficient), the more stable compacted tribolayer can reduce the proportion of direct matrix cutting and large-scale delamination, making the material removal intensity somewhat milder than that at 1300 N; therefore, the weight loss tends to decrease.
For the specimen with bainitic microstructure austempered for 48 h, a low friction coefficient is observed under the load of 1000 N. Material removal is dominated by surface cutting, and the wear mass loss reaches the minimum value. When the load increases to 1300 N, the shear resistance rises and the friction coefficient peaks. Meanwhile, flaky spalling and local fragmentation increase the material removal rate, leading to a marked rise in wear mass loss. This stage essentially corresponds to the transition of the interfacial structure from a loose state to a compacted state, which is not yet fully stabilized. As the load further increases to 1600 N, shear deformation is transferred more into the interior of the tribolayer, and interfacial slip tends to stabilize, resulting in a drop in the friction coefficient. Nevertheless, deeper ploughing grooves and local delamination still occur under higher contact stress, and the total material removal continues to increase. Consequently, the wear mass loss keeps rising.
In summary, the 2 h martensitic microstructure is dominated by abrasive ploughing, and it is difficult for the interface to form a stable and dense tribolayer; load variation mainly changes the groove depth and shear strength. When the load increases, stage-wise adhesive disturbance readily occurs, but a sustained compacted structure is difficult to form. Therefore, its friction behavior is relatively sensitive to load; wear is dominated by groove cutting and localized spalling; and the weight loss ranking exhibits non-monotonic variation, the essence of which is instability caused by the “formation–destruction” of the interface. The 10 h martensite–bainite–retained austenite composite microstructure is in a transitional state, possessing a certain load-bearing capacity while also being prone to adhesive tearing. As the load increases, interfacial adhesion is enhanced, but full compaction and stabilization have not yet been achieved, resulting in obvious adhesive tearing and tribolayer fracture under intermediate load, and the friction coefficient continuously increases. Meanwhile, sheet-like detachment of the material occurs, causing the weight loss to reach a peak at intermediate load. Although localized compaction is enhanced under high load, the overall behavior is still dominated by adhesion and shear damage; therefore, its wear resistance stability is inferior to that of the bainitic specimen. In contrast, the microstructure of the specimen austempered for 48 h exhibits stronger structural stability and compaction capability. At low load, abrasive action dominates; at intermediate load, enhanced adhesion leads to an increase in the friction coefficient; and at high load, a relatively continuous and dense tribolayer (compacted layer) forms at the interface, with shearing occurring more extensively within the interior of the tribolayer, causing the friction coefficient to decrease. However, because the overall contact stress increases, the grooves deepen, and the material removal amount continues to increase, thus exhibiting the characteristics of the friction coefficient first increasing and then decreasing, and weight loss continuously increasing. Its advantage lies in the more stable interfacial load-bearing structure and smaller friction fluctuations under high load.

4.1.2. SEM Morphological Analysis

For the 2 h martensitic specimen, obvious adhesives form at the edge of the raceway under the load of 1000 N. These adhesives originate from iron debris generated by friction between mating materials and the compression effect. At 1300 N, the increased adhesives and formation of spalling pits indicate more severe wear at this load. Local materials undergo an “adhesion–tearing” process, which gives rise to spalling pits. This observation is consistent with the increase in wear mass loss, demonstrating aggravated friction-induced damage under this load. At the higher load of 1600 N, the frictional surface of the material tends to stabilize with good interfacial stability, and excessive spalling is not observed.
Under the load of 1000 N, the surface of the 10 h specimen is more stable with less spalling and adhesion compared with the 2 h specimen. The low friction coefficient and mild surface wear result in a small wear mass loss. This phenomenon indicates that the interface suffers limited disturbance under low load; the wear is dominated by abrasive action without obvious adhesive accumulation. When the load rises to 1300 N, the raceway surface exhibits intensified wear features, and adhesion increases evidently. Thin transfer layers form in partial regions, suggesting substantial material transfer and adhesion during friction. Nevertheless, the accumulation of adhesives is not as prominent as that of the 2 h specimen, and the surface still retains a certain degree of flatness. At 1600 N, adhesives decrease significantly, and no large-area spalling pits are observed, revealing that a stable and compacted tribolayer has formed on the surface. Compared with 1300 N, the extensive compaction at 1600 N suppresses the detachment of local materials and, thus, reduces the mass loss.
The austempered 48 h specimen undergoes more intense friction at 1300 N, accompanied by adhesion and tearing of the material, which accounts for its higher friction coefficient and maximum wear mass loss. At 1600 N, although the friction coefficient decreases, the wear mass loss rises compared with 1300 N despite reduced adhesives and improved surface stability. This reveals that a higher load can reduce the friction coefficient and stabilize the frictional interface; nevertheless, continuous material wear still occurs owing to the large shear force and compaction effect.

4.2. Three-Dimensional Morphology Quantitative Analysis

4.2.1. Wear Volume

At a load of 1000 N, the wear volume is the smallest, indicating that material loss is relatively low under lower load. As the load increases to 1300 N, the wear volume increases significantly, indicating that higher friction force leads to material detachment and wear. At a load of 1600 N, the wear volume decreases slightly; despite the relatively large load, the surface gradually tends to stabilize, and the compacted tribolayer formed at the friction interface reduces large-scale wear. At a load of 1000 N, the wear volume is relatively small; the surface remains in good condition; and no significant spalling or adhesion phenomena are observed, indicating that friction is mild and material loss is relatively low. When the load increases to 1300 N, the wear volume increases significantly and reaches its maximum value. This is closely related to the increase in friction force; under higher load, the friction force is enhanced, leading to more material detachment and wear, and producing more abrasive particles and spalling pits. However, under a load of 1600 N, although the friction force is greater, the wear volume decreases slightly. This indicates that under higher load, although the friction force increases, a denser tribolayer and sufficient mechanical phase transformation gradually form on the material surface, effectively slowing further material detachment and reducing the increment in wear volume. In particular, at 1300 N, the wear volume increases substantially, indicating that the higher friction force promotes material detachment and loss. Under a load of 1600 N, the wear volume continues to increase, but due to the stability of the surface tribolayer, the wear rate is somewhat slowed down.

4.2.2. Wear Track Profile Analysis

For the 2 h isothermally treated specimen dominated by a martensitic microstructure, moderate local fluctuations and irregular undulations can be observed under loads of 1300 N and 1600 N. As the load increases from 1300 N to 1600 N, the overall plastic indentation degree of the wear track depth is limited. This indicates that high hardness improves the resistance of the material to plastic deformation, making it less prone to obvious indentation under contact stress. However, due to insufficient toughness, microcracks are more readily formed under cyclic contact stress, and brittle spalling occurs; therefore, its wear mechanism is dominated by contact-fatigue crack initiation and propagation, manifesting as relatively steep edge morphology and localized spalling characteristics.
For the 10 h isothermally treated specimen with martensite–bainite–retained austenite composite microstructure, the raceway depth reaches its maximum value under 1300 N, which is distinctly higher than that of the 2 h specimen. Because this microstructure has a good strength–toughness match, it is not prone to brittle fracture under contact stress; instead, it releases stress concentration through plastic deformation. Therefore, under intermediate and high loads, the material undergoes repeated shear plastic deformation, forming obvious plastic flow zones and fatigue accumulation damage zones, thereby leading to deepening of the wear track. This indicates that when toughness is significantly improved, the wear mechanism gradually transitions from brittle spalling to a combined plastic deformation and fatigue mechanism, and the wear track morphology becomes rougher, more localized, and greater in depth.
The wear track depth of the austempered 48 h specimen with bainitic microstructure does not change significantly with increasing load. Under lower load, due to the relatively low hardness, the material has already undergone obvious plastic indentation, and the initial formation stage of the wear track enters a state dominated by plastic deformation. When the load continues to increase, the surface layer of the material does not simply increase the indentation depth linearly; instead, it disperses stress concentration through a larger range of plastic flow, effectively expanding the contact area and thereby reducing the actual contact stress per unit area. This stress redistribution effect causes the growth of wear track depth to moderate, while the wear track width further increases.

5. Conclusions

(1)
The average friction coefficient of the specimen austempered for 2 h exhibits a “first decreasing and then increasing” trend. The average friction coefficient of the 10 h specimen increases slowly with increasing load. The average friction coefficient of the specimen austempered for 48 h exhibits a first increasing and then decreasing trend.
(2)
For the specimens austempered for 2 h and 10 h, the wear weight loss does not increase linearly with time, and both exhibit the characteristic that 1300 N is overall greater than 1600 N, i.e., wear at intermediate load is greater than that at high load. For the 48 h bainite-dominated specimen, the wear weight loss increases linearly with time, indicating that its wear rate is relatively stable with small stage-wise fluctuations, and overall, it still reflects a trend of increasing wear with increasing load.
(3)
The specimen austempered for 2 h with a martensitic microstructure is dominated by abrasive ploughing, and the specimen austempered for 10 h with a martensite–bainite–retained austenite composite microstructure is in a transitional state, possessing a certain load-bearing capacity while also being prone to adhesive tearing. For the 48 h specimen, abrasive action dominates at low load; at intermediate load, enhanced adhesion leads to an increase in the friction coefficient; and at high load, a relatively continuous and dense tribolayer forms at the interface.
(4)
The specimen austempered for 2 h has relatively strong load-bearing capacity under high load; the specimen austempered for 10 h has relatively good friction stability under intermediate load; and the specimen austempered for 48 h has a stable friction process but no obvious wear resistance advantage.
(5)
This study provides a theoretical reference for the optimization of heat treatment processes, microstructural design, and engineering application of high-performance bearing materials, and is of important value for improving the service life and reliability of mechanical equipment.

Author Contributions

Conceptualization, J.Z., W.X.; methodology, Z.L., Y.Y. and N.H.; software, J.W., H.M. and N.H.; validation, J.Z., N.H. and G.Y. (Gang Yu); formal analysis, Y.Y. and Y.W.; investigation, N.H., H.M. and H.D.; resources, H.M. and J.Z.; data curation, Y.W., Z.L. and G.Y. (Gang Yu); writing—original draft preparation, N.H.; writing—review and editing, J.Z., W.X. and Y.W.; visualization, D.L., H.M. and N.H.; supervision, W.X. and J.W.; project administration, H.D. and G.Y. (Guolin Yu); funding acquisition, Y.W., Y.Y., D.L. and W.X. All authors have read and agreed to the published version of the manuscript.

Funding

This work was supported by the Open Fund Project of the National United Engineering Laboratory for Advanced Bearing Tribology (No. 202606), the Scientific Research Projects of Higher Education Institutions in Hebei Province (CXZX2025027), the Science and Technology Plan Project of Xingtai City (No. 2024ZZ001) and the Nature Science Foundation of Hubei Province (2024AFD031, 2025AFD032 and 2026AFC0158).

Data Availability Statement

The data presented in this study are available upon request from the corresponding author.

Conflicts of Interest

Author Hanyong Ma was employed by the company China Ordnance Industry Group Jiangshan Heavy Industry Research Institute Co., Ltd. Authors Guolin Yu and Jianxiang Wu were employed by Hubei Tri-ring Forging Co., Ltd. The remaining authors declare that this research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.

References

  1. Li, Z.; Lei, J.; Xu, H.; Yu, F.; Dong, H.; Cao, W.Q. Current status and development trends of bearing steels in China and abroad. J. Iron Steel Res. 2016, 28, 1–12. [Google Scholar]
  2. Li, Y. Research on the Control of Characteristic Microstructures and Performance Evaluation of High-Carbon Chromium Bearing Steel; University of Science and Technology of China: Hefei, China, 2024. [Google Scholar]
  3. Fukui, D.; Kawahito, Y.; Miyazawa, N.; Nakada, N. Anisotropic cleavage fracture caused by transformation-induced internal stress in an as-quenched martensite. Mater. Charact. 2022, 191, 112157. [Google Scholar] [CrossRef] [Scilit]
  4. Hutchinson, B.; Lindberg, F.; Lynch, P. Origins and resulting effects of internal stresses in martensite. ISIJ. Int. 2022, 62, 1981–1989. [Google Scholar] [CrossRef] [Scilit]
  5. Mostafa, E.; Laithy, L.; Wang, T. Mechanistic study of dark etching regions in bearing steels due to rolling contact fatigue. Acta. Mater. 2023, 246, 118698. [Google Scholar] [CrossRef] [Scilit]
  6. Davood, J.; Mohammad, A. Rail vehicle axlebox roller bearing life and failure analysis based on the Hertz contact theory, finite element modeling, and field observations. World J. Eng. 2024, 21, 1183–1192. [Google Scholar] [CrossRef] [Scilit]
  7. Zheng, S.; Qi, P.; Yi, S.; Feng, S.Y.; Zhao, J.; Mu, J.; Zhang, W.; Zhang, Y.; Yin, L.; Xu, R. Effect of bainitic transformation during bainite quenching and tempering (BQT) on the tensile properties of 51CrMnV spring steel. J. Mater. Eng. Perform. 2026, 7, 35. [Google Scholar] [CrossRef] [Scilit]
  8. Zhao, X.; Yang, Z.; Zhang, F. In situ observation of the effect of AlN particles on bainitic transformation in a carbide-free medium carbon steel. Int. J. Miner. Metall. Mater. 2020, 27, 10. [Google Scholar] [CrossRef] [Scilit]
  9. Hua, L.; Du, Y.; Qian, D.; Sun, M.; Wang, F. Influence of prior cold rolling on bainite transformation of high carbon bearing steel. Metall. Mater. Trans. A. 2025, 56, 640–654. [Google Scholar] [CrossRef] [Scilit]
  10. Tung, P.; Tsai, S.; Tsai, Y.-T.; Yang, J.-R. Effects of ausforming on the microstructure and stability of blocky austenite in nanostructured bainite. Mater. Charact. 2025, 221, 114792. [Google Scholar] [CrossRef] [Scilit]
  11. Bhadeshia, H.K.D.H. Steels for bearings. Prog. Mater. Sci. 2012, 57, 268–435. [Google Scholar] [CrossRef] [Scilit]
  12. Li, Z.; Yang, C.; Liu, P. Rolling contact fatigue behavior of bainite/martensite bearing steel with rare earth addition. Int. J. Fatigue. 2026, 206, 109434. [Google Scholar] [CrossRef] [Scilit]
  13. Morales-Rivas, L.; Kerscher, E. Advanced bainitic steels containing retained austenite: Microstructural effects across fatigue stages. Mater. Sci. Eng. A 2010, 942, 21. [Google Scholar]
  14. Gupta, S.; Manna, R.; Chattopadhyay, K. Low cycle fatigue behaviour of high carbon carbide-free nanostructured bainitic steels. Metall. Mater. Trans. A 2025, 56, 9. [Google Scholar] [CrossRef] [Scilit]
  15. Matteis, P.; Sesana, R. Bainitic transformation in 100Cr6 steel for bearing balls: Effect on fatigue endurance. Metals 2025, 15, 931. [Google Scholar] [CrossRef] [Scilit]
  16. Xia, T.; Liu, Y.; Zhu, J.; Chen, Z.; Song, T.; Cui, P. Mesoscopic modeling and simulation of microscopic residual stress for 8Cr4Mo4V steel bearing ring after heat treatment. JMEP 2025, 34, 30086–30096. [Google Scholar] [CrossRef] [Scilit]
  17. Li, H.; Yuan, J.; Wu, X.; Wu, Z.; Li, J.; Li, S.; Zhou, L.; Bu, H.; Qi, H.; Li, M. Correlation of microstructural evolution and hardness distribution of vacuum-carburized low-carbon stainless bearing steel based on thermodynamic calculation and experiments. Mater. Charact. 2025, 230, 115793. [Google Scholar] [CrossRef] [Scilit]
  18. Xu, B.; Jiang, Z.; Zheng, C.; Wang, P.; Zhang, X.; Li, D. Heterogeneous microstructure induced by multi-step phase transformation enhances the mechanical properties and wear resistance of bearing steels. Mater. Charact. 2026, 233, 116134. [Google Scholar] [CrossRef] [Scilit]
  19. Wang, H.; Liu, S.; Qiang, P.; Zhao, J.; Zhao, X.; Sun, H.; Xu, D.; Yang, Z. Effect of austempering on mechanical properties of Nb/V microalloyed bainitic bearing steel. Crystals 2022, 12, 1001. [Google Scholar] [CrossRef] [Scilit]
  20. Du, Y.; Qian, D.; Ren, H.; Wu, M.; Wang, F. Improving mechanical and wear properties of multiphase M50 steel by tailoring bainite morphology. SSRN Electron. J. 2023, 4197682. [Google Scholar] [CrossRef] [Scilit]
  21. Wang, Y.; Liu, Z.; Wang, X.; Chen, X.; Zhang, X.; Shen, W.; Yang, Q.; Zhao, L.; Yang, Z. The effects of austempering time on mechanical properties of the novel GCr15Si1MoNbV bearing steel and on its rolling contact fatigue behaviors. Int. J. Fatigue. 2026, 207, 109519. [Google Scholar] [CrossRef] [Scilit]
  22. Zhou, L.; Yang, X.; Ma, J.; Wei, Y.H.; Yu, X.F. Effect of nanostructured bainite on M/Bn composite microstructure and mechanical properties of GCr15 bearing steel. Heat Treat. Met. 2025, 50, 40–45. [Google Scholar]
  23. Jia, D.; Zhang, C.; Wang, Q.; Wang, H.; Yang, Z.; Zhang, F. Unleashing the potential of nano-bainite bearing steels: Controllable selection of microstructure evolution enables concurrent improvement of toughness and hardness by pre-cold deformation. Mater. Sci. Eng. A 2024, 906, 146715. [Google Scholar] [CrossRef] [Scilit]
  24. Li, T.; Gao, X.; Qiao, Y.; Zheng, H.; Feng, G.; Li, W.; Liu, C.; Lan, H. Study of a bainite-based quenching and partitioning process for regulating the stability of RA. Mater. Sci. Eng. A 2025, 942, 148668. [Google Scholar] [CrossRef] [Scilit]
  25. Mehrbod, M.; Roohollah, R. Enhanced mechanical properties of 100Cr6 bearing steel through formation of nanobainite structure during ausforming treatment. JALMES 2025, 11, 100206. [Google Scholar]
  26. Wei, C.; Du, S.; Fu, L. Effect of compound isothermal quenching on bainite transformation and wear properties of GCr15Si1Mo steel. Tribology 2024, 44, 1–12. [Google Scholar]
  27. Xia, L.; Li, H.; Feng, H.; Jiang, Z.; Zhu, H.; Zhang, S.; Wang, X. Enhanced strength and toughness of high nitrogen stainless bearing steel by controlling interstitial partitioning via V-microalloying. J. Mater. Sci. Technol. 2023, 151, 204–218. [Google Scholar] [CrossRef] [Scilit]
  28. Wu, Y.; Zhang, C.; Dong, S.; Wang, W.; Mao, X.; Wang, S.; Wu, G.; Gao, J.; Wu, H.; Zhao, H. The dual role of Nb microalloying on the high-cycle fatigue of 1.0%C–1.5%Cr bearing steel. Fatigue Fract. Eng. Mater. Struct. 2025, 48, 1301–1314. [Google Scholar] [CrossRef] [Scilit]
  29. An, X.; Cao, W.; Zhang, X.; Yu, J. Suppress austenite grain coarsening by Nb alloying in high–temperature–pseudo–carburized bearing steel. Materials 2024, 17, 2962. [Google Scholar] [CrossRef] [Scilit]
  30. Dong, G.; Gao, B.; Yang, Y.; Wang, Z. Enhanced rolling contact fatigue property of a rare earth addition bearing steel with a gradient nanostructured surface layer. J. Mater. Sci. Technol. 2025, 211, 267–277. [Google Scholar] [CrossRef] [Scilit]
  31. Wang, E.; He, Q.; Gu, C.; Wang, Y.; Chen, H.; Che, Y.; Misra, R.; Gong, N.; Wu, H.; Niu, G. Effect of austempering temperature on microstructure evolution, mechanical properties and wear resistance of carbon-free nano-bainite steel. J. Mater. Res. Technol. 2023, 26, 6703–6718. [Google Scholar] [CrossRef] [Scilit]
  32. Su, Y.; Yang, S.; Yu, X.; Zhou, C.; Liu, Y.; Feng, X.; Zhao, Q.; Wu, J. Effect of austempering temperature on microstructure and mechanical properties of M50 bearing steel. J. Mater. Res. Technol. 2022, 20, 4576–4584. [Google Scholar] [CrossRef] [Scilit]
  33. He, T.; Chen, W.; Liu, Z.; Gong, Z.; Du, S.; Zhang, Y. The impact of surface roughness on the friction and wear performance of GCr15 bearing steel. Lubricants 2025, 13, 187. [Google Scholar] [CrossRef] [Scilit]
  34. Wei, Z.; Hu, H.; Liu, M.; Tian, J.; Xu, G. Effect of austempering below and above Ms on the microstructure and wear performance of a low-carbon bainitic steel. Metals 2022, 12, 104. [Google Scholar] [CrossRef] [Scilit]
  35. Liu, X.; Yu, L.; Zhong, M.; Qian, J.; Dai, J.; Min, Y. Friction and wear behavior of carburized steels against ceramic balls under starved lubrication. Lubricants 2026, 14, 2075–4442. [Google Scholar] [CrossRef] [Scilit]
  36. Qin, Y. Research on the Effects of Cementite on the Microstructure and Properties of Nanobainitic Bearing Steel; Yanshan University: Qinhuangdao, China, 2022. [Google Scholar]
  37. Li, Y.; Jiang, Z.; Li, L.; Wang, P.; Li, D.; Xue, W.; Duan, D. Wear behavior and damage characterization for AISI 52100 bearing steels: Effect of hardness and spherical carbides. J. Mater. Res. Technol. 2024, 30, 8359–8370. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.