Skip to Content
MineralsMinerals
  • Article
  • Open Access

27 September 2026

20 Pages

A Cyclic Voltammetry Study on the Electrodeposition of Antimony from Oxaline (Choline Chloride–Oxalic Acid) Deep Eutectic Solvent

,
,
,
,
and
IEC Group, Institute for Industrial, Radiophysical and Environmental Safety (ISIRYM), Universitat Politècnica de València, Camí de Vera, s/n, 46022 Valencia, Spain
*
Author to whom correspondence should be addressed.
†
These authors contributed equally to this work.

Abstract

Deep eutectic solvents (DESs) have emerged as sustainable alternatives to strong acids and bases, with oxaline, a mixture of oxalic acid and choline chloride, being one of the most studied. Its high metal-dissolving capacity makes it a promising eco-friendly solvent for recovering critical raw materials. One key application is the recovery of antimony (Sb) from secondary sources, as conventional methods rely on highly acidic HCl, which is toxic and corrosive. This study systematically evaluates via cyclic voltammetry the use of oxaline as a potential solvent for the electrochemical recovery of Sb. Results show that oxaline adsorbs on the Pt electrode, an effect intensified by the presence of Sb. The Sb3+ reduction peak and the hydrogen evolution region occur at more widely separated potentials in the oxaline medium than in HCl, allowing operation over a broader potential range while minimizing potential damage to the electrodeposit caused by secondary reactions. However, the high viscosity of oxaline and the diffusion-controlled nature of the process limit the rate of Sb reduction. High operating temperatures increase the peak current density of Sb deposition but also result in thin Sb deposits. Despite these challenges, DESs represent a viable alternative to HCl if their viscosity-related limitations can be overcome.

1. Introduction

Deep Eutectic Solvents (DESs) have received increasing interest as they represent a green class of solvents with a variety of applications, e.g., in the fields of gas absorption and liquid extraction, battery technology and metallurgy [1,2]. DESs are based on binary mixtures of a hydrogen bond acceptor (HBA) and a hydrogen bond donor (HBD), which interact through hydrogen bonding to form a deep eutectic mixture. In such a mixture, the melting point at a given molar ratio is significantly lower than those of the individual compounds, which are typically solids at room temperature. One of the most common DESs is oxaline, which is formed by a 1:1 molar mixture of oxalic acid as HBD and choline chloride as HBA. Oxaline is classified as a Type III DES, as it is formed by mixing a salt halide and an organic acid [3]. Since the two compounds used to form oxaline are organic and biodegradable, and can be produced from bioresources, they arise as a greener and less hazardous alternative to inorganic acids.
One of the most promising applications of DESs is their use as electrolytes for electrochemical processes, particularly, for the electrorecovery of metals from industrial effluents, end-of-life batteries or from leachates of electronic waste [4,5,6]. In this regard, recovery of Sb from secondary sources is an increasingly relevant operation for which several alternatives are being developed [7,8]. Sb is widely used in various industrial processes, including the production of semiconductors, electrocatalysts for the CO2 reduction reaction, development of anodic materials for rechargeable batteries, such as Li/Na-ion batteries, thermoelectric materials, pharmaceuticals, chemicals, ceramics, pigments, and as an alloying element [9,10]. Despite its broad applicability, Sb production rates have declined in recent years due to stricter environmental regulations in several countries and challenges in obtaining it as a primary product from ore exploitation. Consequently, Sb has been classified as a critical raw material, and the urgent need to explore alternative Sb production methods has been emphasized [11]. One of the most important sources of antimony as a secondary material is the production of copper from sulfide minerals, where Sb is present at various stages of the process, particularly in the copper electrorefining baths [12]. Sb is usually extracted from spent baths by ion-exchange; then, it is eluted using highly concentrated (6 M) HCl [13]. Highly acidic solutions are also used to recover Sb from the processing of Sb2S3 concentrates [7]. However, the use of highly concentrated HCl poses several challenges due to its toxicity and corrosivity, the associated generation of wastewater, as well as the narrow electrochemical window of this medium in electrochemical Sb recovery [14]. In recent years, researchers have been exploring alternative and environmentally friendly solvents for Sb leaching and electrodeposition. Some authors have pointed out the suitability of some DESs for conducting the electrodeposition of Sb [14,15,16,17,18]. However, most of these studies have employed choline chloride-based DESs containing HBDs other than oxalic acid, such as ethylene glycol [14,18] and urea [15,16]. The relatively limited studies employing oxalic acid as the HBD for Sb electrodeposition have mainly focused on systems containing additional metals, such as Te and Cu [17], for applications other than the recovery of Sb itself. Consequently, there is still a lack of studies specifically addressing the electrodeposition of Sb in oxaline medium for the recovery of Sb from copper production. The application of oxaline for this purpose is not yet well established, and further research is required to elucidate both the advantages and potential challenges associated with its use as an alternative to highly concentrated inorganic acids.
In the present study, the use of oxaline as a potential medium for the electrochemical recovery of Sb is evaluated. Choline chloride was selected as the HBA because of its low cost, low toxicity, biodegradability, and ability to form stable eutectic mixtures, whereas oxalic acid was selected as the HBD owing to its chelating properties and ability to form stable complexes with metal ions [19]. In addition, compared with other commonly studied choline chloride-based deep eutectic solvents, oxaline exhibits lower viscosity and higher electrical conductivity, which are advantageous properties for electrochemical applications [20]. Sb electrodeposition has been selected as the specific case of study, because the authors have conducted previous works using highly concentrated inorganic acids in the recovery of Sb, which serve as a framework for comparison [8,21,22]. Cyclic voltammetry experiments were conducted to investigate the influence of Sb concentration, temperature and scan rate on the electrodeposition reaction. Based on the voltammetry results, electrodeposition was performed in a longer-term electrodeposition test on a Cu cathode in order to demonstrate the feasibility of the process.

2. Materials and Methods

2.1. Preparation of the Solutions

2.1.1. Preparation of Oxaline Solutions Containing Sb

The preparation of oxaline involved multiple steps. First, a small portion of approximately 15.5 g of choline chloride (99%, Merck, Darmstadt, Germany) and 10.0 g of oxalic acid (98%, Merck, Germany) were mixed in a 1:1 molar ratio, where the former acted as the HBA and the latter as the HBD. Then, the equimolar mixture was manually stirred while being heated to the temperature at which the experiments would be conducted, i.e., between 60 °C and 80 °C, until the mixture became liquid and transparent. At this point, the mixture was stirred using a magnetic stirrer while maintaining the heating. This procedure was repeated for small portions of the reagents until a total of 80 mL of the oxaline solution was obtained. Figure S1 presents images of the different stages of oxaline preparation.
Once the oxaline was prepared, Sb2O3 (99%, Sigma Aldrich, St. Louis, MO, USA) was added while keeping the solvent under stirring and heating until the complete dissolution of antimony was achieved. The concentrations of Sb in the evaluated solutions were 2.5, 5, 10, 20 and 100 mM.

2.1.2. Preparation of HCl Solution

As mentioned above, the cyclic voltammograms obtained with oxaline were compared with those obtained with HCl solutions (prepared from 37% reagent, from Panreac, Barcelona, Spain) at a concentration of 6 M, which is a reference medium commonly used in hydrometallurgical processes. Moreover, this is the most common regenerating solution used to elute Sb from ion-exchange resins used in copper electrorefining [12].

2.2. Determination of the Viscosity of the Solutions

The viscosity of the oxaline and oxaline + Sb solutions was measured using a Cannon-Fenske viscometer for transparent liquids (Figure S2 of the Supplementary Material), series 300, number 144 (Vidrafoc, Barcelona, Spain). The kinematic viscosity, ν (cSt), was calculated using Equation (1), where K ( c S t · s − 1 ) is the capillary-constant that varies as a function of the temperature and was provided by the supplier (Table S1 of the Supplementary Material) and t (s) is the time duration of the measurement. Viscosity measurements were carried out by filling ampoule A (see Figure S2) with the DES and suctioning it with a pipetting bulb until it reached point C1. From there, the liquid was released, and the time until it reached point C2 was recorded ( t of Equation (1)). The tests were performed at 60 °C, 70 °C, and 80 °C using a heated water bath to maintain the desired temperature.
ν = K · t

2.3. Cyclic Voltammetric Experiments

The cyclic voltammetry experiments were performed in an electrochemical cell, as represented in Figure 1. The working electrode consisted of a platinum disk embedded in Teflon, with an active area of 0.071 cm2; a Ag/AgCl electrode was used as the reference electrode, while the counter electrode was a platinum ring with an area of 1 cm2. The electrodes were connected to a galvanostat/potentiostat (Autolab, 302 N, Utrecht, The Netherlands), which supplied the electrical current. The electrochemical cell was equipped with a jacketed design, allowing a temperature-controlled system by circulating water, to maintain precise temperature regulation of the solution (60 °C, 70 °C and 80 °C). The cyclic voltammetric studies were performed within the potential range of −0.75 V to +1.25 V, at different scan rates, from 10 mV/s to 60 mV/s. For each experiment, the open circuit potential (OCP) was determined after allowing the electrode to stabilize for up to 60 s. To enhance reliability, up to 4 scans were performed during each cyclic voltammetry experiment. The working electrode was carefully cleaned with water, polished with emery paper (500 and 4000) and dried before each experiment to ensure consistent and accurate results.
Figure 1. Scheme of the experimental setup used for the cyclic voltammetric tests.

2.4. Linear Sweep Voltammetry and Electrodeposition Experiments

Linear sweep voltammetry (LSV) curves were constructed using a cell similar to the one described in Section 2.3. Here, the working electrode was a copper plate with an effective area of 6 cm2. The reference electrode was the same Ag/AgCl electrode mentioned in Section 2.3, and the counter electrode was a Dimensionally Stable Anode (DSA), also known as a Mixed Metal Oxide (MMO) electrode. The solution temperature was kept at 60 °C or 80 °C by circulating water through the jacketed cell. The linear sweep voltammetry studies were conducted starting at a potential equal to the OCP value of each system and reaching –1.0 V, at a scan rate of 10 mV/s.
Electrodeposition experiments were then conducted in potentiostatic mode using the same system described for the LSVs. The experiments were conducted under −0.6 V for 3 h, with samples of 1 mL being collected every 15 min during the first hour and every 30 min from the 1 h mark until the end.

2.5. Analytical Methods

Samples taken from the electrodeposition reactor (1 mL) were diluted in 50 mL of a 0.3 M HCl solution to reduce their viscosity, so that they could be analyzed using atomic absorption spectroscopy (Perkin Elmer AAnalyst 100 Spectrophotometer, Hopkinton, MA, USA). For the measurements, a hollow cathode lamp specifically designed for Sb operating at a wavelength of 217.6 nm, a spectral bandwidth of 0.2 nm, a current of 15 mA, and a fuel–comburent ratio of 2:4 ethylene to air was used. Prior to the analysis, standard solutions of known concentrations of Sb were measured to obtain a calibration curve.

3. Results and Discussion

3.1. Cyclic Voltammetric Curves

3.1.1. Voltammetric Study of Oxaline Solutions Without Sb and Comparison with HCl Solutions

The voltammetric response of oxaline without Sb is shown in Figure 2 and compared to that obtained with 6 M HCl, which, as mentioned above, has been selected as a reference solvent widely used in metallurgical applications.
Figure 2. Cyclic voltammograms of oxaline and 6 M HCl solutions without Sb. Inset: zoom of the cathodic region of the voltammogram obtained with oxaline.
The voltammogram of oxaline shows a subtle wave in the reduction region (at −0.068 V), which is marked as C0 in the inset plot. Since the oxidation scan does not exhibit any peak that could represent the reverse process occurring at C0, the wave observed at −0.068 V may be attributed to the adsorption of oxalic acid at the electrode surface, a phenomenon which is well documented for this type of systems [23,24,25]. Nevertheless, this assignment remains a hypothesis that requires further investigation for confirmation. The voltammogram obtained with HCl does not show reduction nor oxidation peaks; thus, no reduction or adsorption phenomena was observed with this solution, as expected.
Upon reaching extreme potential values, a sharp increase in current density (in absolute value) is observed in the cathodic and anodic regions for both solutions, with an increase in current much sharper for the HCl solution. This behavior can be attributed to gas evolution reactions, resulting from the reduction and oxidation of the medium. A notable difference between the electrochemical windows of oxaline and HCl can be observed. The cathodic branch starts at −0.19 V for HCl and −0.45 V for oxaline, while the anodic branch starts at +0.92 V for HCl and at +1.0 V for oxaline.
In both media, the current decrease observed in the reduction region can be attributed to the same electrochemical process: the Hydrogen Evolution Reaction (HER). The considerably less cathodic HER potential obtained with HCl could be explained by the larger mobility of H+ ions in aqueous solutions. On the contrary, the HER observed for oxaline is likely associated with the dissociation of free carboxylic acid molecules, since the oxalic acid used in the experiments was anhydrous and no additional water was introduced in the solution [26,27]. The more cathodic potential of the HER that was verified for this solvent may also be explained by the presence of choline chloride in the DES, which has been reported to decrease the intensity of hydrogen formation [28,29]. The overpotential shift observed for oxaline suggests that it may be a more suitable solvent for electrochemical applications, as it provides a broader potential window, potentially minimizing interference from side reactions in the desired process.
A similar behavior was observed in the oxidation region of the curves. Note that at a potential of approximately +0.92 V, the HCl curve exhibits a sharp increase in current density, while the oxaline curve shows a less intense increase, extending to more positive potential values. In both cases, this behavior may be attributed to the Chlorine Evolution Reaction (CER), by which Cl− ions are converted into Cl2 [30].

3.1.2. Voltammetric Study of Oxaline Solutions with Dissolved Sb and Comparison with HCl Solutions

First, the stability of the oxaline + Sb system was evaluated by recording multiple cyclic voltammetric scans, which are shown in Figure 3. A stable response was observed after the third scan. Thus, to ensure that stabilization of all electrode/solvent systems evaluated under different operating conditions is reached, the curves presented in the following sections correspond to the fourth scan. As compared with the voltammograms obtained for solutions of oxaline (Figure 2), additional reduction and oxidation peaks were detected for oxaline with dissolved Sb (e.g., at −0.14 V and + 0.94 V), which indicates the participation of Sb in electrochemical reactions.
Figure 3. Cyclic voltammograms obtained with 5 mM Sb in oxaline medium obtained at 60 °C and at a scan rate of 10 mV·s−1.
Figure 4 shows a comparison between the voltammetric curves obtained for the oxaline + Sb and HCl + Sb solutions. While the oxaline + Sb curve exhibits a flattened shape with small reduction and oxidation peaks related to Sb, the HCl curve displays much more intense and defined peaks, and well-defined HER and CER regions at less extreme potentials (when compared to the oxaline curve).
Figure 4. (a) Full cyclic voltammograms and (b) zoom of the cathodic region obtained with 10 mM Sb in oxaline and 6 M HCl medium. Both voltammograms were registered using a scan rate of 10 mV·s−1 and at 60 °C.
The oxaline + Sb curve exhibits two peaks in the reduction region (Figure 4b), one of them being likely associated with the adsorption of oxalic acid (C0) and the other with the electrochemical reduction of Sb. As discussed in Section 3.1.1, the peak related to the adsorption of oxalic acid was previously observed at a potential of −0.068 V in the oxaline solution without Sb. However, as shown in Figure 4, the addition of Sb shifts this peak to a positive potential of +0.069 V, while the other peak that corresponds to the electrochemical reduction of Sb3+ to metallic Sb appears at a potential of −0.121 V. The shift in the oxalic acid adsorption peak in the presence of Sb may indicate that Sb species influence the interfacial processes associated with oxalic acid adsorption and may also involve the adsorption of Sb–oxaline species. Further investigations are required to determine whether the formation and adsorption of Sb–oxaline species contribute to the observed potential shift. In contrast, the HCl + Sb curve displays only one peak in the cathodic region at −0.275 V, which is associated with the reduction of Sb3+ to Sb [31]. The reduction peak of Sb3+ to metallic Sb in the HCl + Sb solution is significantly more pronounced than in the oxaline + Sb solution, as in the latter case, a peak with the presence of a plateau can be observed. This indicates greater diffusional control over Sb reduction in the oxaline compared to hydrochloric acid [32]. This is consistent with a study on the electrodeposition of Sb in HCl medium, where the authors observed that the diffusion of Sb ions does not limit their electrodeposition [22]. The distinct electrochemical behavior observed in the two media may also be related to differences in Sb speciation. In 6 M HCl medium, Sb3+ is expected to be predominantly associated with chloride complexes, with (SbCl6)3− being reported as the main Sb-containing species [22]. In oxaline, the presence of oxalate may promote the formation of Sb–oxalate complexes, as reported in previous studies investigating the interaction of Sb with oxalate-containing systems [33,34]. Such complexation may result in a different chemical environment for Sb. Therefore, differences in Sb speciation between the two electrolytes may influence the reduction behavior of Sb and, consequently, contribute to the differences observed in their voltammetric responses.
Upon reversing the scan direction toward more positive potentials, a sharp oxidation peak appears in the curve obtained for HCl + Sb (at −0.122 V), which is associated with the oxidation and redissolution of metallic Sb to Sb3+. It is worth noting that a similar oxidation peak is not clearly observed in the oxaline + Sb system, which will be investigated in more detail in the following sections. Overall, the most remarkable difference between both systems is that, as shown in Figure 4b, the Sb reduction peak in the HCl solution is very close to the HER region, which can compromise Sb deposit adhesion and reduce current efficiency, thereby increasing the energy consumption of a potential Sb recovery process by electrodeposition [22].

3.1.3. Evaluation of Sb Concentration and Scan Rate in Oxaline Medium

To confirm whether the peaks shown in Figure 4 correspond to Sb, cyclic voltammetry experiments were conducted at varying Sb concentrations (Figure 5). Starting the analysis of the curves from the OCP value (+0.367 V, see inset of Figure 5a) towards more cathodic potentials, the figure clearly shows that at lower Sb concentrations, a single peak appears at the reduction region due to the adsorption of oxalic acid (see the curves of 0 mM Sb and 2.5 mM Sb). As the Sb concentration increases, this peak shifts towards more positive potentials, suggesting that the presence of Sb species affects the interfacial processes associated with the adsorption of oxalic acid and/or the Sb–oxaline species. Further studies are needed to clarify the origin of this potential shift. Moreover, at concentrations above 5 mM Sb, a second reduction peak corresponding to Sb deposition becomes also visible (peak C1). This supports the discussion presented in Section 3.1.2 on the diffusional control over Sb reduction which is consistent with an enhanced deposition of Sb in oxaline medium at increasing concentrations. The limitation in Sb deposition could be attributed to the high viscosity of the solvent, which impairs the transport of Sb species from the bulk solution towards the electrode surface at lower concentrations, thereby hindering their electrodeposition. Furthermore, at potential values more negative than −0.203 V, HER takes place [35]. As verified in Figure 5a, the presence of Sb in oxaline medium acts as a catalyst and shifts the onset of H+ reduction, which takes place at less cathodic potentials in the presence of Sb.
Figure 5. Cyclic voltammograms of oxaline solutions with various Sb concentrations (a) (2.5–10 mM) with a zoom of the curve obtained for 10 mM Sb in the inset, and (b) (20–100 mM) at a scan rate of 10 mV·s−1.
Once the cathodic limit potential is reached and the scan direction is reversed, two different oxidation peaks appear in the voltammograms. Peak A1 is less noticeable at low Sb concentrations (see inset of Figure 5a) and appears as a broad peak spanning a wide potential range. However, this peak grows notably for the highest concentration, with the peak current taking place at +0.247 V in the case of 100 mM Sb (Figure 5b). Since this peak is the first one registered after the cathodic scan, it can be attributed to the redissolution of metallic Sb that was previously deposited. When the potential is further increased and reaches a value close to +0.50 V, a second anodic peak begins to appear (peak A2). The area of this peak also increases gradually with an increase in the concentration of dissolved Sb, and therefore, can be associated with further oxidation of Sb3+ to Sb5+. Moreover, this peak splits into two different shoulders (at +0.86 V and +1.03 V for 100 mM Sb). At potentials beyond peak A2, the rapid increase in current density is attributed to the oxidation of chloride ions from choline chloride into Cl2 [30].
When reversing again the scan direction toward more cathodic potentials, two additional reduction peaks were observed: C2 (+0.907 V for 100 mM Sb) and C3 (+0.501 V for 100 mM Sb). Peak C2 may be related to the reduction of chlorine generated during the registration of the anodic branch of the curves. This peak is not directly associated with Sb, since it was also visible in the voltammograms obtained for oxaline without Sb (see Figure 2). On the contrary, peak C3 may be associated with a reduction reaction involving Sb, possibly corresponding to the reduction of Sb5+ to Sb3+ because it appeared only in the curves of solutions containing Sb.
Figure 6a shows the evaluation of the scan rate in the cyclic voltammograms obtained with the 10 mM Sb solution, while Figure 6b presents the variation in the current density of peak C1 as a function of the square root of the scan rate.
Figure 6. (a) Cyclic voltammograms obtained for 10 mM Sb at various scan rates (10–60 mV·s−1) and (b) variation in peak C1 current density as a function of the square root of the scan rate.
According to Figure 6a, increasing the scan rate significantly altered the voltammetric curves, particularly when comparing the curve obtained at 10 mV·s−1 with those obtained at higher scan rates (20, 40, and 60 mV·s−1). The curve recorded at 10 mV·s−1 exhibits a well-defined reduction peak for Sb (C1 of Figure 6a), as the slower change in applied potential allows sufficient time for Sb to be depleted near the electrode surface. In contrast, the curves obtained at higher scan rates display a plateau instead of a peak. This behavior supports the previous discussions on the diffusional control of the Sb deposition in oxaline medium, unlike what was observed for Sb deposition in HCl medium. To strengthen this discussion, the current density of the cathodic peaks ( i C 1 ) versus the square root of the scan rate ( v 0.5) was plotted based on the Randles - Sevcik equation (Equation (2)). In Equation (2), n represents the number of electrons involved in the reduction step, D 0 ( c m 2 s ) is the diffusion coefficient, C 0 ( m o l / L ) is the bulk concentration of the analyte, F denotes the Faraday constant, T ( K ) is the temperature, and R is the universal gas constant [36,37]. As shown in Figure 6b, the curve exhibits a linear behavior (R2 = 0.9995) beyond 20 mV/s (value in the x-axis corresponding to 0.14 (V/s)0.5). Therefore, the data corresponding to scan rates between 20 and 60 mV/s were used to calculate the diffusion coefficient of Sb in oxaline, and the obtained value was 8.6 × 10−12 cm2/s. This value of diffusion coefficient is significantly lower than that of Sb in HCl medium (5.29 × 10−6 cm2/s [31]), which confirms that the transfer of Sb ions in oxaline is strongly limited by diffusion, which can be explained by the solution viscosity.
i c = 0.446 n F C 0 ( n F v D 0 R T ) 1 / 2
Lastly, the increase in scan rate shifts the reduction plateaus to more negative current densities due to the decrease in the diffusion boundary layer thickness [37].

3.1.4. Evaluation of Temperature in Oxaline Medium

The results shown in the previous sections evidence that oxaline is a suitable solvent for conducting electrochemical processes, and specifically, those involving the electrodeposition of metals such as Sb. The potential window in oxaline is wider than in HCl, which may imply a decreased interference of HER on the electrodeposition of metals. However, the low diffusion coefficient of dissolved Sb in this medium and the low current densities registered for the deposition of Sb entail an important limitation for the application of this DES. Since diffusional control of the process might be influenced by the high viscosity of oxaline, the use of this solvent at higher temperatures has been further investigated, in line with previous studies dealing with metal electrodeposition in different DES systems [35,38]. The viscosity of oxaline and oxaline with 100 mM Sb at temperatures of 60, 70, and 80 °C was measured, and the results are presented in Figure 7. A sharp decrease in viscosity was observed as the temperature increased, particularly between 60 °C and 70 °C. As the temperature increased from 70 to 80 °C, the viscosity decreased further, although the reduction was less pronounced. A similar trend was reported by Mjalli et al. [39] for other DESs. Zhang et al. [20] also evaluated the effect of temperature on the viscosity of oxaline and several other DESs, and reported a nearly linear relationship over the range of 20–80 °C. To the best of our knowledge, no data on the effect of temperature on the viscosity of oxaline + Sb solutions have been reported in the literature. Finally, the dissolution of Sb in the eutectic resulted in a decrease in viscosity, which may facilitate the application of this DES in metallurgical processes.
Figure 7. Viscosity of oxaline solutions without Sb and with 100 mM Sb measured at 60 °C, 70 °C, and 80 °C.
Figure 8 shows the effect of temperature (60–80 °C) on the voltammetric curves obtained for the systems of oxaline + Sb at different Sb concentrations (10 mM and 100 mM) and for the reference system of 6 M HCl + Sb.
Figure 8. Effect of temperature on the voltammetric response of (a) oxaline solution with 10 mM Sb, (b) oxaline solution with 100 mM Sb (inset: effect of temperature on the current density of the Sb reduction peak and the kinematic viscosity), (c) 6 M HCl solution with 10 mM Sb.
The increase in temperature shifts the cathodic region of the oxaline curve with Sb to more positive potential values and intensifies the plateau C0, which is likely related to the reduction in the viscosity of oxaline and the consequent enhancement of the adsorption of oxalic acid on the electrode surface [23,24,25]. It is noted that this effect is more pronounced between 60 °C and 70 °C than between 70 °C and 80 °C, which is consistent with the viscosity reduction profile of the oxaline solution shown in Figure 7 and the work of Mjalli et al. [39]. A similar effect of temperature can be observed on peak C1, thus confirming that increasing the temperature, with the concomitant reduction in solvent viscosity, improves the deposition of Sb3+ in the form of metallic Sb. This phenomenon is also evident for higher Sb concentrations (see Figure 8b), where in general, the current density increases with temperature in all reduction and oxidation peaks. Specifically, the effect of temperature on the solution viscosity and the current density of peak C1 (electrodeposition of Sb) is shown in the inset of Figure 8b, where both present clearly opposite trends with increasing temperature. These results confirm that the reduced viscosity of the solution at higher temperatures enhances ion diffusion and allows Sb ions to reach the electrode surface more efficiently. It should be noted that the viscosity measurements were performed at the maximum Sb concentration evaluated in this study (100 mM). Therefore, further studies are required to assess the effect of Sb concentration on the viscosity of the oxaline-based solution.
Figure 8c shows that the effect of temperature on the HCl + Sb solution differs significantly from that of the oxaline solution. In the case of HCl, increasing the temperature led to a horizontal shift in the reduction peak toward less negative potentials, while the current density showed a slight decrease from 60 to 70 °C and remained almost unchanged between 70 and 80 °C. The unaltered current density despite the reduction in solution viscosity and consequent increase in Sb ion mobility at higher temperatures indicates that Sb diffusion does not limit its electrodeposition in HCl medium, as also reported in [22].
Based on the current density data of the reduction peaks related to Sb reduction in oxaline (Figure 8b) and HCl (Figure 8c) medium, a ln ( I ) vs. 1/T plot was constructed based on the Arrhenius equation (Equation (3)), and the activation energy for Sb reduction was then calculated. In Equation (3), I represents the peak reduction current (A), B is a constant, E A denotes the apparent activation energy (kJ/mol), R is the universal gas constant (kJ/mol·K), and T is the temperature (K).
ln ( I ) = B − E A R T
As shown in Figure 9a, the curve for the oxaline + Sb system exhibited a relatively linear behavior (R2 = 0.94), and the E A obtained considering the temperature range from 60 to 80 °C was 62.23 kJ/mol. On the contrary, the HCl + Sb system did not generate a straight line (R2 = 0.34) due to the nearly constant current density of the reduction peak with increasing temperature beyond 70 °C. In this case, it was not possible to calculate E A . These results show that E A for Sb in oxaline medium is significantly high, which means that the minimum energy required to initiate the electrochemical reduction of Sb ions into their metallic form is high in oxaline, making the process considerably slow. It is worth mentioning that a nearly linear behavior for the Arrhenius plot was obtained for several choline chloride-based DESs using other compounds as HBDs, such as ethylene glycol [40], malonic acid [41], and urea [42], in electrodeposition studies of various metals. However, to the best of our knowledge, no published studies have reported an Arrhenius plot for Sb electrodeposition in oxaline medium. It is also worth mentioning that the non-linear behavior observed for the HCl + Sb solution was also reported in [22], a study that evaluated in detail, by cyclic voltammetry, the electrodeposition of Sb in the same 6 M HCl medium assessed here.
Figure 9. Arrhenius plot for the solution of 10 mM Sb + (a) oxaline and (b) HCl.

3.2. Linear Sweep Voltammetry of Sb in Oxaline Medium for Electrodeposition Tests

After conducting the cyclic voltammetric study with the oxaline + Sb system using a Pt electrode, it was confirmed that this DES is a suitable medium for electrochemical applications, and more specifically for the electrodeposition of metals. Further investigation of this solvent involves demonstrating the electrodeposition of Sb on larger-area electrodes, and for this purpose, copper is a conventional substrate material. LSV was performed with this material in order to select the most appropriate conditions for the electrodeposition experiments. Figure 10 shows the cathodic scan of voltammograms obtained for the oxaline + Sb solution using copper electrode, which is frequently used in Sb deposition processes [31,43]. The curves obtained with the Pt electrode are also shown in Figure 10, as it is the electrode used in the previous sections and is frequently employed in voltammetry, mainly due to its stability in various media. The figure shows curves obtained at 60 °C and 80 °C to evaluate the effect of viscosity on the electrochemical response of both electrodes.
Figure 10. Comparison of the cathodic scan conducted at 10 mV·s−1 obtained for oxaline solutions with 10 mM Sb at 60 °C and 80 °C with the Cu and the Pt electrode.
The curves obtained with the Cu electrode show only one reduction peak at both 60 °C and 80 °C, indicating that the electrodeposition of Sb occurs at this electrode in a single step (Sb3+ to metallic Sb), with no other peaks related to the reduction or adsorption of any other species. On the contrary, as seen in previous sections, the curves obtained with the Pt electrode show two peaks in the cathodic region, one corresponding to the adsorption of oxalic acid (C0) and the other to the reduction of Sb3+ to metallic Sb (C1). This indicates that oxalic acid adsorption strongly depends on the electrode material. It is worth mentioning that oxalic acid adsorption has been widely studied in the literature, but these works are typically performed either with Pt [23,24] or with different Pt-based electrodes [25]. Therefore, there is a scarcity of studies dedicated to investigating other electrodes besides Pt in order to shed light on the relationship between the electrode material and oxalic acid adsorption.
Figure 10 shows that the peak current densities related to the reduction of Sb3+ to metallic Sb at each temperature were very similar for the electrodes (−0.265 and −0.212 mA·cm−2 at 60 °C for Cu and Pt, respectively, and −0.621 and −0.648 mA·cm−2 at 80 °C for Cu and Pt, respectively), indicating that the electrode material does not affect the current density of Sb electrodeposition. However, the increase in temperature significantly impacts the adsorption of oxalic acid on the Pt electrode due to the reduction in viscosity. Although the current density of Sb reduction remains almost unaltered when changing the electrode material, the figure shows a noticeable shift in the potential towards more cathodic values when copper was used, which was also observed in a study conducted with HCl + Sb solutions and different electrode materials [31]. Lastly, it was verified that HER occurs at less cathodic potentials on both electrodes when the temperature is increased. Additional studies should be conducted to evaluate the effect of electrode material on Sb electrodeposition in oxaline medium, using, for example, stainless steel [44] and titanium [45], which have been assessed in studies of Sb electrodeposition in HCl medium.

3.3. Electrodeposition

Based on the LSV curve shown in Figure 10, a potentiostatic electrodeposition of Sb in oxaline medium was performed on a Cu electrode, which is the most recommended material electrode for this process [43]. The applied potential was −0.6 V based on the Sb reduction peak shown for the Cu electrode, while the temperature was set at 80 °C due to the lower viscosity of the solution. Figure 11 presents images of the electrodes before and after the process, while Figure S3 of the Supplementary Material shows the evolution of the Sb concentration in the solution and the measured current density. From Figure 11, it can be observed that the electrode exhibited a dark and homogeneous aspect after electrodeposition, indicating the successful deposition of Sb. However, the concentration of Sb in the solution shown in Figure S3a changed very slowly throughout the experiment, achieving the deposition of a 22.5% of the Sb initially present in the solution towards the end of the experiment. Current density increases over time until stabilizing around a value of 0.53 mA·cm−2 (see Figure S3b), a value which approaches the peak current density of 0.621 mA·cm−2 observed for peak C1 with the Cu electrode at 80 °C in Figure 10. The small change in the bulk concentration of Sb can be explained by the electrodeposition of a thin Sb layer due to the high viscosity of the solution. However, the thickness and morphology of the deposited layer were not quantitatively characterized in the present study, and therefore this interpretation is inferred from the slight decrease in the bulk Sb concentration. Further studies involving the systematic variation in the applied potential and temperature, together with appropriate characterization of the deposited layer, should be conducted to elucidate their effects on deposition efficiency and deposit morphology. Thus, although the deposition of Sb dissolved in oxaline has been proven feasible in larger surfaces, further studies are needed to improve the process, e.g., by replacing the solvent with a DES of lower viscosity or by exploring the addition of water to the DES to finely tune the properties of the resulting mixture [46,47]. Nonetheless, besides the challenges identified for the recovery of critical materials by means of electrodeposition, it must be emphasized that the slow deposition process in oxaline medium may find potential applications in other fields, such as the deposition of thin functional coatings on metallic substrates.
Figure 11. Copper cathode (a) before and (b) after the potentiostatic electrodeposition of Sb conducted at −0.6 V.

3.4. Novelty, Limitations, and Future Perspectives

DESs have been increasingly investigated for metal recovery, but their application to Sb electrodeposition remains relatively limited. Table 1 summarizes previous studies using different DESs for Sb recovery. Most of these studies employed choline chloride + ethylene glycol, which is one of the most investigated DESs for Sb electrodeposition. High viscosity and the resulting diffusion-controlled behavior are among the main limitations reported in this literature. To the best of our knowledge, Sb electrodeposition from oxaline had not been systematically investigated before this study. Therefore, the results obtained herein provide valuable information about the electrochemical behavior of Sb in this medium and allowed direct comparison with other DESs and with concentrated HCl, a conventional medium for Sb electrodeposition. In particular, the potential range between Sb3+/Sb0 reduction and hydrogen evolution was wider in oxaline than in HCl. This wider electrochemical window may facilitate the control of Sb electrodeposition and reduce the interference of hydrogen evolution. However, the high viscosity of oxaline limits mass transfer and, consequently, the deposition rate. The deposit obtained at 80 °C on the copper electrode was very thin. Such thin Sb coatings may still be useful for applications requiring thin layers, such as electronic devices and sensors, but a higher deposition rate would be needed for large-scale Sb recovery from secondary sources.
Table 1. Comparison of reported Sb electrodeposition studies using deep eutectic solvents.
While the present study involves important findings regarding the electrochemical behavior of oxaline as a solvent for metal electrodeposition, it also has some limitations which should be addressed before developing a process for the recovery of metals from waste streams. The relatively limited Sb recovery obtained under the conditions evaluated, the lack of systematic optimization using a design of experiments (DOE) approach, and the absence of morphological and structural characterization restrict the assessment of the deposition performance and the quality and potential applications of the deposited Sb. In addition, although oxalic acid adsorption affected the voltammetric response and Sb electrodeposition on Pt, its role was not investigated in detail herein.
Further studies should evaluate these approaches to increase the Sb deposition rate. More detailed morphological and structural characterization of the deposits and systematic investigation of oxalic acid adsorption would also be useful to better understand and overcome the limitations already identified in the present study.

4. Conclusions

The suitability of oxaline as a DES medium for electrochemical processes involving metals was evaluated through cyclic voltammetry and electrodeposition tests. Solutions of Sb dissolved in oxaline were investigated, and their electrochemical response was compared with that obtained in highly concentrated HCl, a typical medium used for the recovery of Sb by electrodeposition. A peak in the reduction region of the cyclic voltammetry curves obtained with oxaline and a Pt electrode was detected at all conditions evaluated. This peak was absent in the curves obtained with HCl and occurred likely due to oxalic acid adsorption. The Sb3+ reduction peak was identified at potential values around −0.15 V, while the same process occurs at more cathodic potentials in the case of HCl solutions. On the contrary, the HER potential is less cathodic for HCl solutions. This broader potential window favors the use of oxaline in the potential recovery of metals by electrodeposition, preventing HER from degrading the consistency of the metallic deposits and decreasing energy consumption. However, Sb reduction in oxaline is diffusion-limited due to high viscosity, which has been identified as the main limitation for the process. Higher temperatures decrease oxaline viscosity, thus enhancing Sb reduction. The high activation energy calculated (62.23 kJ/mol) confirms an intensified deposition of Sb at increasing temperatures, although the process is slow even at 80 °C. The successful deposition of Sb over larger electrodes was proven using a copper electrode by means of potentiostatic operation for three hours; nonetheless, a very thin Sb layer was formed due to strong diffusion limitations. These results reveal important advantages of the use of oxaline as a greener alternative to highly concentrated acids or alkali in applications related to the recovery of critical materials. Possible solutions to the challenge related to the high viscosity include exploring the effects of dilution with water or using other additives as well as operating at higher temperatures.

Supplementary Materials

The following supporting information can be downloaded at https://www.mdpi.com/article/10.3390/min16100992/s1. Figure S1: Pictures of the preparation of oxaline solutions; Figure S2: Cannon-Fenske viscometer; Figure S3: Evolution of the (a) relative concentration of Sb and (b) measured current density during the potentiostatic electrodeposition conducted at −0.6 V; Table S1: K constants of the Cannon-Fenske viscometer corresponding to different temperatures.

Author Contributions

Conceptualization, M.C.M.-C., V.P.-H. and M.T.M.-S.; methodology, M.C.M.-C., V.P.-H. and K.S.-B.; validation, M.C.M.-C. and L.H.-P.; formal analysis, M.C.M.-C., L.H.-P. and K.S.-B.; investigation, L.H.-P. and A.M.-P.; resources, M.C.M.-C. and V.P.-H.; data curation, L.H.-P., M.C.M.-C. and K.S.-B.; writing—original draft preparation, K.S.-B. and M.C.M.-C.; writing—review and editing, K.S.-B. and M.C.M.-C.; visualization, K.S.-B. and M.C.M.-C.; supervision, M.C.M.-C., V.P.-H. and M.T.M.-S.; project administration, M.C.M.-C. and V.P.-H.; funding acquisition, M.C.M.-C. and V.P.-H. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by Agencia Estatal de Investigación (grant AEI/10.13039/501100011033) (Spain) under the project PCI2019-103535 and by FEDER A way of making Europe.

Data Availability Statement

The raw data supporting the conclusions of this article will be made available by the authors on request.

Acknowledgments

The authors thank the financial support from the Agencia Estatal de Investigación (AEI/10.13039/501100011033) (Spain) under the project PCI2019-103535 and by FEDER A way of making Europe. Universitat Politècnica de València and Ministerio de Universidades de España (Plan de Recuperación, Transformación y Resiliencia—financed by European Union—Next GenerationEU) are also acknowledged.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Hansen, B.B.; Spittle, S.; Chen, B.; Poe, D.; Zhang, Y.; Klein, J.M.; Horton, A.; Adhikari, L.; Zelovich, T.; Doherty, B.W.; et al. Deep Eutectic Solvents: A Review of Fundamentals and Applications. Chem. Rev. 2021, 121, 1232–1285. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  2. Abbott, A.P.; Boothby, D.; Capper, G.; Davies, D.L.; Rasheed, R.K. Deep Eutectic Solvents Formed Between Choline Chloride and Carboxylic Acids: Versatile Alternatives to Ionic Liquids. J. Am. Chem. Soc. 2004, 126, 9142–9147. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  3. Abbott, A.P. Deep Eutectic Solvents and Their Application in Electrochemistry. Curr. Opin. Green Sustain. Chem. 2022, 36, 100649. [Google Scholar] [CrossRef] [Scilit]
  4. Padwal, C.; Pham, H.D.; Jadhav, S.; Do, T.T.; Nerkar, J.; Hoang, L.T.M.; Kumar Nanjundan, A.; Mundree, S.G.; Dubal, D.P. Deep Eutectic Solvents: Green Approach for Cathode Recycling of Li-Ion Batteries. Adv. Energy Sustain. Res. 2022, 3, 2100133. [Google Scholar] [CrossRef] [Scilit]
  5. Guo, M.; Deng, R.; Gao, M.; Xu, C.; Zhang, Q. Sustainable Recovery of Metals from E-Waste Using Deep Eutectic Solvents: Advances, Challenges, and Perspectives. Curr. Opin. Green Sustain. Chem. 2024, 47, 100913. [Google Scholar] [CrossRef] [Scilit]
  6. Yuan, Z.; Liu, H.; Yong, W.F.; She, Q.; Esteban, J. Status and Advances of Deep Eutectic Solvents for Metal Separation and Recovery. Green Chem. 2022, 24, 1895–1929. [Google Scholar] [CrossRef] [Scilit]
  7. Tian, Q.; Huang, Z.; Xu, Z.; Guo, X.; Lu, D. An Efficient and Green Method for Extracting Antimony from Antimony Sulfide Concentrates by Cyclone Slurry Electrolysis. Sep. Purif. Technol. 2025, 363, 132061. [Google Scholar] [CrossRef] [Scilit]
  8. Hernández-Pérez, L.; Muñoz-Pérez, A.; Ortega, E.M.; Pérez-Herranz, V.; Montañés, M.T.; Martí-Calatayud, M.C. Increasing the Sustainability of Copper Electrorefining: Selective Electrodeposition of Antimony in the Presence of Bismuth from Highly Concentrated Hydrochloric Acid Effluents. J. Environ. Chem. Eng. 2024, 12, 112005. [Google Scholar] [CrossRef] [Scilit]
  9. Thanu, V.R.C.; Jayakumar, M. Electrochemical Recovery of Antimony and Bismuth from Spent Electrolytes. Sep. Purif. Technol. 2020, 235, 116169. [Google Scholar] [CrossRef] [Scilit]
  10. Nieto, K.; Windsor, D.S.; Kale, A.R.; Gallawa, J.R.; Medina, D.A.; Prieto, A.L. Structural Control of Electrodeposited Sb Anodes through Solution Additives and Their Influence on Electrochemical Performance in Na-Ion Batteries. J. Phys. Chem. C 2023, 127, 12415–12427. [Google Scholar] [CrossRef] [Scilit]
  11. Anderson, C.G. The Metallurgy of Antimony. Geochemistry 2012, 72, 3–8. [Google Scholar] [CrossRef] [Scilit]
  12. Barros, K.S.; Vielmo, V.S.; Moreno, B.G.; Riveros, G.; Cifuentes, G.; Bernardes, A.M. Chemical Composition Data of the Main Stages of Copper Production from Sulfide Minerals in Chile: A Review to Assist Circular Economy Studies. Minerals 2022, 12, 250. [Google Scholar] [CrossRef] [Scilit]
  13. Arroyo-Torralvo, F.; Rodríguez-Almansa, A.; Ruiz, I.; González, I.; Ríos, G.; Fernández-Pereira, C.; Vilches-Arenas, L.F. Optimizing Operating Conditions in an Ion-Exchange Column Treatment Applied to the Removal of Sb and Bi Impurities from an Electrolyte of a Copper Electro-Refining Plant. Hydrometallurgy 2017, 171, 285–297. [Google Scholar] [CrossRef] [Scilit]
  14. Bu, J.; Ru, J.; Hua, Y.; Wang, Z.; Zhang, Y.; Geng, X.; Zhang, W. Electrochemical Behavior of Sb(III)/Sb During the Preparation of Sb Particles in Deep Eutectic Solvent. Ionics 2021, 27, 3119–3127. [Google Scholar] [CrossRef] [Scilit]
  15. Mares, M.L.; Golgovici, F.; Visan, T. RDE Voltammetry and Impedance Spectroscopy Studies of Sb, Te and SbTe Electrodeposition from Choline Chloride—Urea Ionic Liquids. Chalcogenide Lett. 2013, 10, 259–272. [Google Scholar]
  16. Rastogi, A.C.; Janardhana, N.R. Properties of CuSbS2 Thin Films Electrodeposited from Ionic Liquids as P-Type Absorber for Photovoltaic Solar Cells. Thin Solid Film. 2014, 565, 285–292. [Google Scholar] [CrossRef] [Scilit]
  17. Catrangiu, A.S.; Sin, I.; Prioteasa, P.; Cotarta, A.; Cojocaru, A.; Anicai, L.; Visan, T. Studies of Antimony Telluride and Copper Telluride Films Electrodeposition from Choline Chloride Containing Ionic Liquids. Thin Solid Film. 2016, 611, 88–100. [Google Scholar] [CrossRef] [Scilit]
  18. Alcanfor, A.A.C.; da Silva, L.P.; de Oliveira, R.C.; Paulo, G.A.; Sousa, C.P.; Campos, O.S.; Dias, D.F.; Feitosa, F.X.; de Sant’Ana, H.B.; Monteiro, N.K.V.; et al. On the Role of Water in Antimony Electrodeposition from Choline Chloride/Ethylene Glycol/Water Mixture. J. Mol. Liq. 2024, 399, 124416. [Google Scholar] [CrossRef] [Scilit]
  19. Oke, E.A.; Fedai, Y.; Potgieter, J.H. Hydrometallurgical Leaching of Copper and Cobalt from a Copper–Cobalt Ore by Aqueous Choline Chloride-Based Deep Eutectic Solvent Solutions. Minerals 2025, 15, 815. [Google Scholar] [CrossRef] [Scilit]
  20. Zhang, H.; Lang, J.; Lan, P.; Yang, H.; Lu, J.; Wang, Z. Study on the Dissolution Mechanism of Cellulose by ChCl-Based Deep Eutectic Solvents. Materials 2020, 13, 278. [Google Scholar] [CrossRef] [Scilit]
  21. Hernández-Pérez, L.; Carrillo-Abad, J.; Pérez-Herranz, V.; Montañés, M.T.; Martí-Calatayud, M.C. Effluents from the Copper Electrorefining as a Secondary Source of Antimony: Role of Mass Transfer on the Recovery by Electrodeposition. Desalination 2023, 549, 116322. [Google Scholar] [CrossRef] [Scilit]
  22. Barros, K.S.; Machado, A.L.V.; Vielmo, V.S.; Velizarov, S.; Ferreira, J.Z.; Pérez–Herranz, V.; Bernardes, A.M. Membrane Electrolysis for Recovering Sb and Bi from Elution Solutions of Ion-Exchange Resins Used in Copper Electrorefining: A Cyclic Voltammetric Study. J. Electroanal. Chem. 2022, 924, 116867. [Google Scholar] [CrossRef] [Scilit]
  23. Berná, A.; Rodes, A.; Feliu, J.M. Oxalic Acid Adsorption and Oxidation at Platinum Single Crystal Electrodes. J. Electroanal. Chem. 2004, 563, 49–62. [Google Scholar] [CrossRef] [Scilit]
  24. Berná, A.; Rodes, A.; Feliu, J.M. An In Situ Infrared and Electrochemical Study of Oxalic Acid Adsorption at Stepped Platinum Single Crystal Electrodes in the [0 1 - 1] Zone. Electrochim. Acta 2004, 49, 1257–1269. [Google Scholar] [CrossRef] [Scilit]
  25. Martínez-Huitle, C.A.; Ferro, S.; De Battisti, A. Electrochemical Incineration of Oxalic Acid: Role of Electrode Material. Electrochim. Acta 2004, 49, 4027–4034. [Google Scholar]
  26. Cojocaru, A.; Mares, M.L.; Prioteasa, P.; Anicai, L.; Visan, T. Study of Electrode Processes and Deposition of Cobalt Thin Films from Ionic Liquid Analogues Based on Choline Chloride. J. Solid State Electrochem. 2015, 19, 1001–1014. [Google Scholar] [CrossRef] [Scilit]
  27. Cojocaru, A.; Sin, I.; Agapescu, C.; Cotarta, A.; Visan, T. Electrode Processes and SEM/EDX Analysis of Selenium Films Electrodeposited from Ionic Liquids Based on Choline Chloride. Chalcogenide Lett. 2016, 13, 127. [Google Scholar]
  28. Zhu, W.; Rosen, B.A.; Salehi-Khojin, A.; Masel, R.I. Monolayers of Choline Chloride Can Enhance Desired Electrochemical Reactions and Inhibit Undesirable Ones. Electrochim. Acta 2013, 96, 18–22. [Google Scholar] [CrossRef] [Scilit]
  29. Agapescu, C.; Cojocaru, A.; Golgovici, F.; Manea, A.C.; Cotarta, A. Electrochemical Studies of BiTeSe Films Deposition from Ionic Liquids Based on Choline Chloride with Ethylene Glycol, Malonic Acid or Oxalic Acid. Rev. Chim. 2012, 63, 911. [Google Scholar]
  30. Agapescu, C.; Cojocaru, A.; Cotarta, A.; Visan, T. Electrodeposition of Bismuth, Tellurium, and Bismuth Telluride Thin Films from Choline Chloride-Oxalic Acid Ionic Liquid. J. Appl. Electrochem. 2013, 43, 309–321. [Google Scholar] [CrossRef] [Scilit]
  31. Hernández-Pérez, L.; Carrillo-Abad, J.; Ortega, E.M.; Pérez-Herranz, V.; Montañés, M.T.; Martí-Calatayud, M.C. Voltammetric and Electrodeposition Study for the Recovery of Antimony from Effluents Generated in the Copper Electrorefining Process. J. Environ. Chem. Eng. 2023, 11, 109139. [Google Scholar] [CrossRef] [Scilit]
  32. De Oliveira, G.M.; Barbosa, L.L.; Broggi, R.L.; Carlos, I.A. Voltammetric Study of the Influence of EDTA on the Silver Electrodeposition and Morphological and Structural Characterization of Silver Films. J. Electroanal. Chem. 2005, 578, 151–158. [Google Scholar] [CrossRef] [Scilit]
  33. Pla-Vilanova, P.; Galceran, J.; Puy, J.; Companys, E.; Filella, M. Antimony Speciation in Aqueous Solution Followed with AGNES. J. Electroanal. Chem. 2019, 849, 113334. [Google Scholar] [CrossRef] [Scilit]
  34. Tella, M.; Pokrovski, G.S. Antimony(III) Complexing with O-Bearing Organic Ligands in Aqueous Solution: An X-Ray Absorption Fine Structure Spectroscopy and Solubility Study. Geochim. Cosmochim. Acta 2009, 73, 268–290. [Google Scholar] [CrossRef] [Scilit]
  35. Doneux, T.; Sorgho, A.; Soma, F.; Rayée, Q.; Bougouma, M. Electrodeposition in Deep Eutectic Solvents: The “Obvious”, the “Unexpected” and the “Wonders”. Molecules 2024, 29, 3439. [Google Scholar] [CrossRef] [Scilit]
  36. Elgrishi, N.; Rountree, K.J.; McCarthy, B.D.; Rountree, E.S.; Eisenhart, T.T.; Dempsey, J.L. A Practical Beginner’s Guide to Cyclic Voltammetry. J. Chem. Educ. 2018, 95, 197–206. [Google Scholar] [CrossRef] [Scilit]
  37. Bard, A.J.; Faulkner, L.R. Electrochemical Methods: Fundamentals and Applications, 2nd ed.; John Wiley & Sons, Inc.: Hoboken, NJ, USA, 2001. [Google Scholar]
  38. Fu, X.; Zhan, C.; Zhang, R.; Wang, B.; Sun, H.; Sun, J. Effect of Temperature on Mechanism and Kinetics of Electrochemical Nucleation of Copper in ChCl-Based Deep Eutectic Solvents. J. Solid State Electrochem. 2022, 26, 2713–2722. [Google Scholar] [CrossRef] [Scilit]
  39. Mjalli, F.S.; Naser, J. Viscosity Model for Choline Chloride-Based Deep Eutectic Solvents. Asia-Pac. J. Chem. Eng. 2015, 10, 273–281. [Google Scholar] [CrossRef] [Scilit]
  40. Bernasconi, R.; Panzeri, G.; Firtin, G.; Kahyaoglu, B.; Nobili, L.; Magagnin, L. Electrodeposition of ZnNi Alloys from Choline Chloride/Ethylene Glycol Deep Eutectic Solvent and Pure Ethylene Glycol for Corrosion Protection. J. Phys. Chem. B 2020, 124, 10739–10751. [Google Scholar] [CrossRef] [Scilit]
  41. Cao, X.; Wang, H.; Liu, T.; Shi, Y.; Xue, X. Electrodeposition of Bi from Choline Chloride-Malonic Acid Deep Eutectic Solvent. Materials 2023, 16, 415. [Google Scholar] [CrossRef] [Scilit]
  42. Zhang, Q.B.; Hua, Y.X. Electrochemical Synthesis of Copper Nanoparticles Using Cuprous Oxide as a Precursor in Choline Chloride-Urea Deep Eutectic Solvent: Nucleation and Growth Mechanism. Phys. Chem. Chem. Phys. 2014, 16, 27088–27095. [Google Scholar] [CrossRef] [Scilit]
  43. Bergmann, M.E.H.; Koparal, A.S. Electrochemical Antimony Removal from Accumulator Acid: Results from Removal Trials in Laboratory Cells. J. Hazard. Mater. 2011, 196, 59–65. [Google Scholar] [CrossRef] [Scilit]
  44. Garrido, B.; Lara, J.; Moreno, J.; Giacobbo, A.; Pino, E.; Cifuentes, G.; Bernardes, A.M. Antimony Recovery from Copper Refining Electrolyte by Membrane Electrolysis. REM—Int. Eng. J. 2025, 78, e240031. [Google Scholar] [CrossRef] [Scilit]
  45. Vielmo, V.S.; Welter, J.B.; Rotta, E.H.; Bernardes, A.M.; Meneguzzi, A. Enhancing Antimony Electrowinning from Copper Electrolyte Waste by Coupling Ion-Exchange Membrane and Mechanical Stirring. JOM 2025, 77, 2189–2196. [Google Scholar] [CrossRef] [Scilit]
  46. El Achkar, T.; Greige-Gerges, H.; Fourmentin, S. Basics and Properties of Deep Eutectic Solvents: A Review. Environ. Chem. Lett. 2021, 19, 3397–3408. [Google Scholar] [CrossRef] [Scilit]
  47. Meng, X.; Ballerat-Busserolles, K.; Husson, P.; Andanson, J.M. Impact of Water on the Melting Temperature of Urea + Choline Chloride Deep Eutectic Solvent. New J. Chem. 2016, 40, 4492–4499. [Google Scholar] [CrossRef] [Scilit]
  48. Zhao, Y.; Li, M.; Yu, J.; Jiang, Q.; Li, Y. Electrodeposition of Sb Powder in Choline Chloride-Ethylene Glycol Deep Eutectic Solvent as Anodes for Sodium-Ion Batteries. Mater. Lett. 2026, 411, 140321. [Google Scholar] [CrossRef] [Scilit]
  49. Bu, J.; Ru, J.; Wang, Z.; Hua, Y.; Xu, C.; Zhang, Y.; Wang, Y. Controllable Preparation of Antimony Powders by Electrodeposition in Choline Chloride-Ethylene Glycol. Adv. Powder Technol. 2019, 30, 2859–2867. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.