Abstract
Thermal degradation of InGaN quantum dots (QDs) during the temperature ramp for GaN quantum-barrier growth can compromise micro-light-emitting-diode active regions. Five-period InGaN/GaN QD structures with low-temperature-grown GaN (LT-GaN) caps of 0 nm (C0), 2 nm (C2), and 4 nm (C4) were studied. The nominal total GaN quantum barrier was fixed at 10 nm by adjusting the higher-temperature-grown GaN portion to 10, 8, and 6 nm, respectively. The active regions were characterized by high-resolution X-ray diffraction, aberration-corrected transmission electron microscopy, and temperature-dependent photoluminescence; post-ramp surface-reference specimens were examined by atomic force microscopy; and 10 μm × 10 μm micro-LEDs were evaluated by electroluminescence spectroscopy and integrating-sphere external quantum efficiency measurements. Compared with C0 and C2, C4 displayed clearer satellite reflections, more laterally continuous InGaN-rich contrast, and weaker thermal photoluminescence quenching; its surface reference also showed a more continuous terrace-like morphology with fewer fine depressions. The C4 micro-LED reached a peak external quantum efficiency of 4.45% at 20 A cm−2, compared with 2.58% at 150 A cm−2 for C0 and 1.80% at 140 A cm−2 for C2. Together, these results associate more effective thermal protection with a reduced relative contribution from defect-assisted nonradiative recombination and enhanced device efficiency.
1. Introduction
III-nitride micro-light-emitting diodes (micro-LEDs) are attractive for high-resolution displays, visible-light communication, and integrated photonics because of their high brightness, fast response, and long operating life. As the lateral dimensions decrease, however, nonradiative recombination at etched sidewalls becomes increasingly important [1,2]. Longer-wavelength InGaN emitters introduce an additional materials challenge because the higher In content required in the active region makes it more difficult to maintain compositional uniformity and abrupt heterointerfaces. In conventional c-plane InGaN/GaN quantum wells, strain-induced polarization fields spatially separate electrons and holes, while carrier-induced field screening and state filling contribute to wavelength shifts under electrical injection [3,4].
Self-assembled InGaN quantum dots (QDs) provide three-dimensional carrier localization and can partially relax strain relative to planar quantum wells. Localization can restrict carrier transport toward nonradiative centers and can mitigate, although not eliminate, polarization-related effects [5,6]. Vertically stacked QD layers are commonly employed to increase the effective emitting volume of the active region. Plasma-assisted molecular-beam epitaxy (PA-MBE) enables controlled growth across the blue-to-red spectral range [7]. In the present growth sequence, the InGaN QDs and LT-GaN caps were deposited at approximately 600 °C, whereas the remaining GaN barrier portion was deposited at 700 °C; the intervening thermal cycles therefore make the heterointerfaces particularly sensitive to thermal history.
A key challenge in the growth of InGaN/GaN multiple-quantum-dot active regions arises from the different thermal conditions used for InGaN QD formation and GaN barrier growth. Before deposition of the GaN barrier portion at 700 °C, the substrate temperature must be increased from the QD-growth temperature of approximately 600 °C. Any InGaN surface that remains exposed during this step, including the upper QD surface and thin interdot wetting-layer regions, may undergo thermal decomposition accompanied by preferential In desorption. This process can modify the morphology and composition of the active region.
An LT-GaN cap deposited immediately after QD growth is intended to protect the InGaN-rich surface during the subsequent thermal treatment. However, its effectiveness depends on the lateral continuity of the cap over the three-dimensional QD/wetting-layer topography. A nominal 2 nm deposition cannot be assumed to form a continuous 2 nm film at every local position; uncovered or weakly covered regions may therefore remain susceptible to thermal degradation. Previous studies of InGaN/GaN quantum wells and QDs have likewise shown that low-temperature GaN caps can suppress In loss and interface roughening, with the resulting protection depending strongly on cap thickness and growth conditions [8,9,10,11,12,13,14].
Atomistic modeling provides an important complement to experimental optimization by relating nanoscale composition, dimensionality, and interface configuration to the stability and optoelectronic properties of III-nitride nanostructures. Pela et al. benchmarked several density-functional-theory-based approaches against GW and Bethe–Salpeter-equation descriptions for core–shell InAlN nanorods, illustrating both the utility and method-dependent accuracy of atomistic calculations for predicting electronic and optical properties [15]. Complementarily, Sfuncia et al. used metalorganic chemical vapor deposition together with conductive AFM and atomic-resolution scanning/transmission electron microscopy to resolve structurally selective ultrathin GaN formed under graphene/SiC interfacial confinement [16]. Although these material systems differ from the present InGaN/GaN MQDs, they highlight the value of combining atomistic understanding with advanced structural characterization when investigating ultrathin nitride layers and interfaces.
Here, five-period InGaN/GaN multi-quantum-dot (MQD) active regions in samples C0, C2, and C4, containing 0, 2, and 4 nm LT-GaN caps, respectively, were compared. C0 served as an uncapped reference for thermal degradation during the temperature ramp, C2 probed whether an ultrathin protective layer could stabilize the three-dimensional QD/wetting-layer topography, and C4 tested the effect of increasing the nominal protective thickness under the same thermal cycle. In each period, the nominally 10 nm total GaN quantum barrier comprised an LT-GaN cap with a thickness of 0, 2, or 4 nm and a subsequently deposited HT-GaN portion with a corresponding thickness of 10, 8, or 6 nm, respectively. This design allowed the cap-protection effect to be evaluated without changing the nominal MQD period thickness. High-resolution X-ray diffraction (HRXRD), aberration-corrected transmission electron microscopy (AC-TEM), atomic force microscopy (AFM), and temperature-dependent photoluminescence (TDPL) were combined with electroluminescence (EL) and integrating-sphere external quantum efficiency (EQE) measurements on corresponding micro-LEDs. Among the three conditions investigated, the 4 nm LT-GaN cap was the best-performing thickness, providing the clearest convergence of structural, optical, and device-level evidence for effective thermal protection and reduced nonradiative loss.
2. Materials and Methods
2.1. Epitaxial Design and Growth
Two matched epitaxial sets were grown by PA-MBE on GaN-on-c-plane-sapphire templates, with reflection high-energy electron diffraction used for in situ surface monitoring. One set contained the MQD active-region test structures used for structural and optical characterization; the other comprised complete LED structures incorporating the same active-region designs. The InGaN QDs were grown at approximately 600 °C using the calibrated PA-MBE procedure reported previously [7]. After each QD layer, no LT-GaN cap was deposited for C0, whereas nominally 2 and 4 nm LT-GaN caps were deposited at the same temperature for C2 and C4, respectively. The substrate temperature was subsequently increased to 700 °C and held for 5 min. The remaining 10, 8, and 6 nm higher-temperature-grown GaN barrier portions (HT-GaN portions) were then deposited at 700 °C for C0, C2, and C4, respectively. Thus, the nominal total GaN quantum-barrier thickness was maintained at 10 nm in all three structures. Five QD/GaN-barrier periods were used in every sample (Table 1 and Figure 1).
Table 1.
Active-region designs used for the structural samples and corresponding complete LED wafers.
Figure 1.
Schematic of the InGaN/GaN MQD active-region stack (three of five periods are shown for clarity; not to scale). The nominal total GaN quantum-barrier thickness was fixed at 10 nm in each period, with LT-GaN-cap/HT-GaN-portion thicknesses of 0/10 nm for C0, 2/8 nm for C2, and 4/6 nm for C4.
Dedicated surface-reference samples were also prepared to isolate the morphology remaining after the thermal cycle. C0 was terminated after the final InGaN QD layer, whereas C2 and C4 were terminated after deposition of the nominally 2 and 4 nm LT-GaN caps, respectively. Each specimen underwent the same ramp to 700 °C and the same 5 min hold as its corresponding complete MQD structure; however, no HT-GaN portion was deposited. The resulting post-hold surfaces therefore probe the effects of the three termination conditions on the preservation of the InGaN QD/wetting-layer region during the pre-overgrowth thermal cycle.
2.2. Complete LED Structures and Micro-LED Fabrication
The complete LED epitaxial structures comprised a 500 nm n-GaN layer, a five-period InGaN QD/GaN quantum-barrier active region, a 10 nm p-AlGaN electron-blocking layer, and a 120 nm p-GaN layer. Square mesas with lateral dimensions of 10 μm × 10 μm were fabricated from the three corresponding LED wafers using an identical micro-LED process. Photolithography and dry etching were employed to define the mesas and expose the n-type layer. Indium tin oxide (ITO) was deposited as the transparent p-side current-spreading electrode, followed by formation of the p- and n-type metal contacts using established micro-LED fabrication procedures [2,17,18]. The mesa geometry and all processing conditions were kept identical among the three device groups. Current density was calculated using the nominal mesa area of 100 μm2.
2.3. Structural, Optical, and Device Characterization
HRXRD ω–2θ coupled scans were collected around the symmetric GaN (0002) reflection. Cross-sectional active regions were examined by AC-TEM, and the post-ramp surface-reference samples were measured by tapping-mode AFM. TDPL spectra were recorded from 10 to 300 K. For each sample, the spectrally integrated PL intensity was normalized to its own 10 K value and plotted as a function of 1000/T (K−1). Thermal quenching was fitted with a two-channel Arrhenius expression:
where I0 is the low-temperature intensity scale, kB is the Boltzmann constant, Ea1 and Ea2 are effective activation energies, and α1 and α2 are dimensionless prefactors describing the relative weights of two thermally activated quenching pathways. These fitted quantities are not treated as direct measurements of defect density or as unique identifiers of particular microscopic defects [19,20]. Room-temperature EL peak wavelengths were extracted as a function of current density. Absolute EQE was measured using a calibrated integrating-sphere system. The photograph inset in the EQE plot shows a representative operating C4 device and is used only for qualitative illustration.
I(T) = I0/{1 + α1 exp[−Ea1/(kBT)] + α2 exp[−Ea2/(kBT)]},
3. Results and Discussion
3.1. Structural Periodicity and Heterointerface Evolution
Figure 2 shows the HRXRD ω–2θ coupled scans around the GaN (0002) reflection. The dominant peak at approximately 2θ = 34.55° originates from the GaN template, whereas the satellite peaks arise from the periodic compositional modulation of the MQD stack. Satellite peaks are resolved for both capped samples and are more numerous and clearly defined for C4 than for C2, consistent with improved vertical periodicity and reduced period-to-period variations in composition or interface position. By contrast, no well-resolved satellite peaks are detected for C0, consistent with greater active-region nonuniformity and the interrupted InGaN-rich QD/wetting-layer contrast observed by AC-TEM in Figure 3a. Because satellite visibility also depends on composition modulation and thickness fluctuations, these features are interpreted as evidence of MQD periodicity and interface regularity rather than as a direct measure of dislocation or point-defect density.
Figure 2.
HRXRD ω–2θ coupled scans around the GaN (0002) reflection for C0, C2, and C4, corresponding to LT-GaN cap thicknesses of 0, 2, and 4 nm, respectively. The labeled satellite orders highlight the progressively clearer features in the capped samples, consistent with improved MQD periodicity.
Figure 3.
Cross-sectional AC-TEM images of the MQD active regions: (a) C0 with a 0 nm LT-GaN cap and a 10 nm HT-GaN portion, (b) C2 with a 2 nm LT-GaN cap and an 8 nm HT-GaN portion, and (c) C4 with a 4 nm LT-GaN cap and a 6 nm HT-GaN portion. The nominal total GaN quantum-barrier thickness is 10 nm in every case. Scale bars: 10 nm.
Self-assembled InGaN QDs form through the Stranski–Krastanov growth mode: a thin two-dimensional InGaN wetting layer is first established, followed by three-dimensional islanding after a critical coverage is reached [7]. During the temperature increase from approximately 600 to 700 °C, exposed InGaN—particularly the ultrathin wetting-layer regions between adjacent QDs—is susceptible to thermal decomposition and preferential In desorption because of the comparatively low thermal stability of InN. Depositing an LT-GaN cap at the QD-growth temperature is therefore intended to stabilize the upper QD/wetting-layer surface before the thermal excursion. For the three-dimensional QD morphology, however, a nominally thin cap may not provide continuous coverage at every local position, making the protective effect dependent on cap thickness and growth conditions [8,9,10,11,12,13,14].
Cross-sectional AC-TEM provides complementary local evidence for this evolution, as shown in Figure 3. In C0, the InGaN-rich contrast within the nominal QD/wetting-layer planes is locally interrupted. This morphology is compatible with partial degradation of exposed InGaN during the temperature ramp, although the post-growth AC-TEM image alone cannot distinguish ramp-induced degradation from pre-existing as-grown nonuniformity. In C2, neighboring InGaN QD regions remain partly connected by wetting-layer-like contrast, although appreciable lateral nonuniformity persists. C4 exhibits the most laterally continuous and vertically regular active-region contrast, with a more extended, quantum-well-like profile than C0. This evolution is consistent with stronger preservation during heating and possible cap-induced reshaping of the QDs; quantitative dot-size statistics would nevertheless be required to establish the extent of such reshaping. The 4 nm LT-GaN cap is therefore interpreted as preserving the upper QD/wetting-layer morphology during the subsequent ramp to 700 °C; this interpretation does not imply that an interface or defect formed before cap deposition is repaired.
3.2. Post-Ramp Surface Morphology and Cap-Protection Mechanism
Figure 4 compares the AFM images of the dedicated surface-reference samples after the identical temperature ramp and holding step. The uncapped surface retains self-assembled InGaN QD-related morphology with an estimated areal density of approximately 4 × 1010 cm−2. The C2 surface contains numerous nanoscale depressions. C4 instead shows a more continuous terrace-like morphology with far fewer fine depressions in the displayed scan. Because the panels use different displayed scale bars and no statistical roughness values are available, the comparison is limited to these qualitative morphological features rather than a quantitative ranking of root-mean-square roughness.
Figure 4.
AFM images of the post-ramp surface-reference samples: (a) C0, terminated after the final InGaN QD layer; (b) C2, terminated after the 2 nm LT-GaN cap; and (c) C4, terminated after the 4 nm LT-GaN cap. All specimens underwent the same temperature ramp as the corresponding complete MQD structures and were maintained at 700 °C for 5 min, but no HT-GaN portion was deposited. The displayed scale bars are 200 nm in (a) and 1 μm in (b,c).
These companion samples more directly probe the cap-protection process because subsequent HT-GaN deposition does not obscure the morphology produced during heating. The three-dimensional QD topography makes the lateral continuity of an ultrathin cap sensitive to local growth kinetics. Consequently, a nominal 2 nm deposition need not provide continuous coverage at every position. During the subsequent ramp and holding step, any locally exposed or weakly covered InGaN may decompose and lose In, potentially leaving a heterogeneous surface with depression-like features and boundaries between more strongly and more weakly protected regions. Compared with C2, C4 displays a more continuous terrace-like morphology with fewer visible fine depressions after the same thermal sequence. This qualitative difference is consistent with more effective protection of the QD/wetting-layer surface by the 4 nm LT-GaN cap and, consequently, stronger suppression of thermal decomposition and In desorption [8,9,10,11,12,13,14]. However, the present measurements do not directly establish that the cap physically fills the initial gaps between adjacent QDs or fully coalesces before heating. AFM alone also does not establish the chemical or crystallographic origin of each depression; accordingly, these features are not assigned directly to dislocations or treated as a quantitative measure of defect density.
The nonmonotonic behavior of C2 is consistent with locally nonuniform protection and need not represent a simple intermediate state between C0 and C4. A partially continuous cap may produce regions with different thermal histories, including preserved InGaN, thermally degraded areas, and boundaries between differently protected regions. Such spatial heterogeneity could contribute to nonradiative recombination even when part of the InGaN QD layer remains intact. This interpretation is supported by the mutually consistent morphology, TDPL, and device trends, but it does not constitute a chemically resolved identification of a specific defect.
3.3. Thermal Quenching and Effective Nonradiative Pathways
To assess thermally activated nonradiative losses, TDPL measurements were performed from 10 to 300 K. Figure 5 shows the integrated PL intensity of each sample, normalized independently to its value at 10 K, as a function of 1000/T (K−1). C4 retains the largest fraction of its low-temperature luminescence on approaching 300 K, whereas C2 exhibits the strongest thermal quenching. Because each trace is normalized to its own 10 K intensity, the comparison describes thermal PL retention rather than the relative absolute PL intensities of the samples. Moreover, this normalization does not require the internal quantum efficiency at 10 K to be 100% [20].
Figure 5.
Integrated TDPL intensity as a function of 1000/T (K−1) for C0, C2, and C4, corresponding to LT-GaN cap thicknesses of 0, 2, and 4 nm, respectively. Each curve is normalized to its own integrated intensity at 10 K; symbols are experimental data, and lines are fits using Equation (1). The inset shows representative temperature-dependent PL spectra of C4 from 10 to 300 K.
The fitted parameters are listed in Table 2. Both thermally activated quenching pathways have the largest fitted prefactors in C2. Relative to C2, C4 reduces α1 by approximately 75% and α2 by approximately 95%. Equation (1) yields approximate I(300 K)/I(10 K) values of 2.3%, 1.3%, and 3.3% for C0, C2, and C4, respectively. The activation energies are effective barriers associated with quenching and cannot, from their numerical values alone, be uniquely assigned to threading dislocations, interface states, exciton delocalization, or another microscopic process [19,20]. Likewise, α1 and α2 are effective quenching prefactors rather than direct measurements of defect density. Nevertheless, the smaller prefactors and weaker quenching of C4 are consistent with a reduced contribution from defect-assisted nonradiative recombination, in agreement with its more regular heterointerfaces and post-ramp morphology.
Table 2.
Two-channel Arrhenius fitting parameters for the normalized TDPL intensities.
3.4. Electroluminescence Wavelength Behavior
Figure 6 presents the EL peak wavelength as a function of current density. All three devices exhibit a rapid initial blueshift followed by a more gradual variation. From the first recorded low-current point to 400 A cm−2, the plotted wavelength changes are approximately 491.0 to 485.9 nm for C0, 493.7 to 488.2 nm for C2, and 498.0 to 493.4 nm for C4, corresponding to net blueshifts of approximately 5.1, 5.5, and 4.6 nm, respectively. The starting current densities differ slightly among the curves; these shifts should therefore be regarded as comparative estimates rather than values evaluated over strictly identical current-density intervals.
Figure 6.
EL peak wavelength as a function of current density for 10 μm × 10 μm MQD micro-LEDs incorporating C0 (0 nm LT-GaN cap; red circles), C2 (2 nm LT-GaN cap; green downward triangles), and C4 (4 nm LT-GaN cap; black squares). Lines are guides to the eye.
The persistent ordering λC4 > λC2 > λC0 is compatible with greater average preservation of In-rich material as the nominal cap thickness increases. It does not, however, imply a monotonic improvement in interface quality: C2 may retain more In on average than C0 while still exhibiting spatially heterogeneous protection and a stronger contribution from nonradiative loss. The wavelength also depends on QD dimensions, strain, carrier localization, and polarization fields; the longer-wavelength emission of C4 is therefore supporting evidence for improved In retention rather than a direct compositional measurement. The current-induced blueshift can arise from screening of the polarization field together with filling of localized states [3,4]; it should not be attributed to a single mechanism on the basis of the peak-wavelength curves alone. The somewhat smaller wavelength excursion of C4 may additionally reflect changes in strain, localization, and the internal electric field.
3.5. External Quantum Efficiency and Structure–Device Relationships
Figure 7 compares device efficiency among the three cap-layer conditions. C4 reaches a peak EQE of approximately 4.45% at a current density of 20 A cm−2. By comparison, C0 reaches approximately 2.58% near 150 A cm−2, whereas C2 exhibits the lowest peak EQE of approximately 1.80% near 140 A cm−2. The maximum EQE of C4 is therefore approximately 72% higher than that of C0 and 2.47 times that of C2. Moreover, C4 maintains the highest EQE throughout the common measurement range. The simultaneous enhancement in peak efficiency and substantial reduction in the current density at which the maximum occurs indicate a markedly different magnitude and injection dependence of the recombination balance for C4.
Figure 7.
External quantum efficiency as a function of current density for 10 μm × 10 μm MQD micro-LEDs incorporating C0 (0 nm LT-GaN cap; red circles), C2 (2 nm LT-GaN cap; green downward triangles), and C4 (4 nm LT-GaN cap; gray squares). The inset shows a representative electrically driven C4 device and is included only as a qualitative illustration.
To interpret these device trends within a recombination framework, the measured EQE can be written as the product of the injection efficiency ηinj, light-extraction efficiency ηext, and recombination-limited internal quantum efficiency:
where A, B, and C are the effective Shockley–Read–Hall (SRH), radiative, and Auger recombination coefficients, respectively, and n is the carrier density. Under the simplified assumption that B and C remain unchanged among the three active-region designs, differentiation gives
ηEQE = ηinjηext[Bn2/(An + Bn2 + Cn3)],
npeak = √(A/C)
ηIQE,peak = B/(B + 2√(AC))
According to Equations (3) and (4), a reduction in the SRH coefficient A increases the peak internal efficiency and shifts the internal-efficiency maximum toward a lower carrier density when B and C are fixed [21,22]. Relating this result to the measured current density at the EQE maximum additionally requires comparable carrier-density–current-density conversion, injection efficiency, current spreading, effective active volume, and light extraction, with ηinj and ηext varying similarly near the peak among the three device groups. Under these assumptions, the much lower peak current density of C4 is consistent with a reduced relative contribution from defect-assisted SRH recombination. Because AC-TEM reveals cap-dependent active-region morphology, however, the constancy of B, C, and the effective active volume is not experimentally established; the EQE curves therefore do not uniquely isolate a change in A. This interpretation is supported by complementary evidence from HRXRD, AC-TEM, AFM, and TDPL. Conversely, the low EQE of C2 is consistent with spatially heterogeneous protection and possible boundaries between differently protected regions, rather than with a directly identified cap-edge defect.
After reaching its early maximum, C4 exhibits a more pronounced relative efficiency decrease and retains approximately 80% of its peak EQE at 400 A cm−2. This behavior is not inconsistent with reduced SRH recombination. Once defect-mediated losses are suppressed, Auger recombination can become relatively more important at elevated carrier densities, together with other high-injection loss mechanisms such as carrier leakage. Importantly, the EQE curves alone neither demonstrate an increase in the Auger recombination coefficient C nor permit the unique extraction of any individual ABC coefficient. The measured EQE also depends on carrier injection, current spreading, light extraction, and sidewall recombination, the last of which is important for 10 μm devices [1,2,23]. Identical mesa geometry and fabrication strengthen the comparison, but quantitative determination of the ABC coefficients would require complementary carrier-density or differential-lifetime measurements. Taken together, the HRXRD, AC-TEM, AFM, TDPL, EL, and EQE results collectively support a consistent interpretation in which more effective cap-mediated thermal protection is associated with better preservation of the MQD active region and lower effective nonradiative loss.
4. Conclusions
Low-temperature GaN caps were evaluated as thermal-protection layers for five-period InGaN/GaN QD active regions while the nominal total GaN quantum-barrier thickness was maintained at 10 nm. After the prescribed growth sequence, the InGaN-rich contrast within the nominal QD/wetting-layer planes of C0 was locally interrupted, whereas C2 showed numerous nanoscale depressions on its post-ramp surface, the strongest thermal quenching, and the largest fitted quenching prefactors. By contrast, C4 exhibited the most continuous and vertically regular active-region contrast, a more continuous terrace-like post-ramp morphology with fewer fine depressions, weaker thermal PL quenching, and the longest-wavelength EL across the measured current-density range. These observations are consistent with the 4 nm LT-GaN cap providing the most effective thermal protection among the three investigated conditions, but they do not directly demonstrate physical filling of the initial interdot gaps or provide a quantitative measurement of defect density. The corresponding 10 μm × 10 μm micro-LEDs exhibited peak EQEs of approximately 2.58%, 1.80%, and 4.45% for C0, C2, and C4, respectively. Notably, the peak EQE of C4 occurred at approximately 20 A cm−2, compared with approximately 150 A cm−2 for C0 and 140 A cm−2 for C2. Within the assumptions of the ABC recombination model, the simultaneous increase in peak efficiency and shift of the efficiency maximum toward a substantially lower current density are consistent with a reduced relative contribution from defect-assisted SRH recombination. Within the investigated range, the 4 nm LT-GaN cap was the best-performing condition; the combined results associate its more effective thermal protection and better active-region preservation with enhanced micro-LED efficiency without uniquely determining any individual recombination coefficient.
Author Contributions
Conceptualization and methodology, Y.G. (Yi Gong) and S.J.; formal analysis and visualization, Y.G. (Yi Gong); investigation, Y.G. (Ying Gu); data curation, W.Y.; writing—original draft preparation, Y.G. (Ying Gu) and Y.G. (Yi Gong); resources, S.L.; writing—review and editing, G.C. and L.B.; supervision, S.L. and L.B.; project administration, S.J. and L.B.; funding acquisition, S.J. and W.Y. All authors have read and agreed to the published version of the manuscript.
Funding
This work was funded by National Key Research and Development Program of China (No. 2023YFB3609800), Natural Science Foundation of Jiangsu Province (No. BK20230235), and Suzhou Key Core Technology Project: Leading the Charge with Open Competition (No. SYG2024104).
Data Availability Statement
The data supporting the findings of this research are accessible from the corresponding author upon reasonable request.
Acknowledgments
The authors acknowledge technical support from the Platform for Characterization and Testing and the Nanofabrication Facility of the Suzhou Institute of Nano-Tech and Nano-Bionics, Chinese Academy of Sciences.
Conflicts of Interest
The authors declare no conflicts of interest.
References
- Tian, P.; McKendry, J.J.D.; Gong, Z.; Guilhabert, B.; Watson, I.M.; Gu, E.; Chen, Z.; Zhang, G.; Dawson, M.D. Size-dependent efficiency and efficiency droop of blue InGaN micro-light emitting diodes. Appl. Phys. Lett. 2012, 101, 231110. [Google Scholar] [CrossRef] [Scilit]
- Chen, P.-W.; Hsiao, P.-W.; Chen, H.-J.; Lee, B.-S.; Chang, K.-P.; Yen, C.-C.; Horng, R.-H.; Wuu, D.-S. On the mechanism of carrier recombination in downsized blue micro-LEDs. Sci. Rep. 2021, 11, 22788. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Takeuchi, T.; Sota, S.; Katsuragawa, M.; Komori, M.; Takeuchi, H.; Amano, H.; Akasaki, I. Quantum-confined Stark effect due to piezoelectric fields in GaInN strained quantum wells. Jpn. J. Appl. Phys. 1997, 36, L382–L385. [Google Scholar] [CrossRef] [Scilit]
- Peng, L.; Zhao, D.; Jiang, D.; Zhu, J.; Liu, Z.; Chen, P.; Yang, J.; Liu, W.; Liang, F.; Xing, Y.; et al. Anomalous electroluminescent blue-shift behavior induced by well widths variance and localization effect in InGaN/GaN multi-quantum wells. Opt. Express 2018, 26, 21736–21744. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Chichibu, S.F.; Uedono, A.; Onuma, T.; Haskell, B.A.; Chakraborty, A.; Koyama, T.; Fini, P.T.; Keller, S.; DenBaars, S.P.; Speck, J.S.; et al. Origin of defect-insensitive emission probability in In-containing (Al,In,Ga)N alloy semiconductors. Nat. Mater. 2006, 5, 810–816. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Liu, J.; Jia, Z.; Ma, S.; Dong, H.; Zhai, G.; Xu, B. Enhancement of carrier localization effect and internal quantum efficiency through In-rich InGaN quantum dots. Superlattices Microstruct. 2018, 113, 497–501. [Google Scholar] [CrossRef] [Scilit]
- Zhang, X.; Xing, Z.W.; Yang, W.X.; Qiu, H.B.; Gu, Y.; Suzuki, Y.; Kaneko, S.; Matsuda, Y.; Izumi, S.; Nakamura, Y.; et al. Explorations on Growth of Blue-Green-Yellow-Red InGaN Quantum Dots by Plasma-Assisted Molecular Beam Epitaxy. Nanomaterials 2022, 12, 800. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Pendlebury, S.T.; Parbrook, P.J.; Mowbray, D.J.; Wood, D.A.; Lee, K.B. InGaN/GaN quantum wells with low growth temperature GaN cap layers. J. Cryst. Growth 2007, 307, 363–366. [Google Scholar] [CrossRef] [Scilit]
- Zheng, C.; Wang, L.; Mo, C.; Fang, W.; Jiang, F. Effect of same-temperature GaN cap layer on the InGaN/GaN multiquantum well of green light-emitting diode on silicon substrate. Sci. World J. 2013, 2013, 538297. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Krause, B.; Miljevic, B.; Aschenbrenner, T.; Piskorska-Hommel, E.; Tessarek, C.; Barchuk, M.; Buth, G.; Donfeu Tchana, R.; Figge, S.; Gutowski, J.; et al. Influence of a low-temperature capping on the crystalline structure and morphology of InGaN quantum dot structures. J. Alloys Compd. 2014, 585, 572–579. [Google Scholar] [CrossRef] [Scilit]
- Zhu, Y.; Lu, T.; Zhou, X.; Zhao, G.; Dong, H.; Jia, Z.; Liu, X.; Xu, B. Advantages of InGaN/GaN multiple quantum wells with two-step grown low temperature GaN cap layers. Superlattices Microstruct. 2017, 111, 960–965. [Google Scholar] [CrossRef] [Scilit]
- Wang, X.; Liang, F.; Zhao, D.; Liu, Z.; Zhu, J.; Yang, J. Investigations on the optical properties of InGaN/GaN multiple quantum wells with varying GaN cap layer thickness. Nanoscale Res. Lett. 2020, 15, 191. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Wang, Q.; Wang, T.; Parbrook, P.J.; Bai, J.; Cullis, A.G. The influence of a capping layer on optical properties of self-assembled InGaN quantum dots. J. Appl. Phys. 2007, 101, 113520. [Google Scholar] [CrossRef] [Scilit]
- Yang, J.; Zhao, D.G.; Jiang, D.S.; Chen, P.; Zhu, J.J.; Liu, Z.S.; Le, L.C.; Li, X.J.; He, X.G.; Liu, J.P.; et al. Optical and structural characteristics of high indium content InGaN/GaN multi-quantum wells with varying GaN cap layer thickness. J. Appl. Phys. 2015, 117, 055709. [Google Scholar] [CrossRef] [Scilit]
- Pela, R.R.; Hsiao, C.-L.; Hultman, L.; Birch, J.; Gueorguiev, G.K. Electronic and optical properties of core–shell InAlN nanorods: A comparative study via LDA, LDA-1/2, mBJ, HSE06, G0W0 and BSE methods. Phys. Chem. Chem. Phys. 2024, 26, 7504–7514. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Sfuncia, G.; Nicotra, G.; Giannazzo, F.; Pécz, B.; Gueorguiev, G.K.; Kakanakova-Georgieva, A. 2D graphitic-like gallium nitride and other structural selectivity in confinement at the graphene/SiC interface. CrystEngComm 2023, 25, 5810–5817. [Google Scholar] [CrossRef] [Scilit]
- Gu, Y.; Gong, Y.; Zhang, P.; Hua, H.; Jin, S.; Yang, W.; Zhu, J.; Lu, S. Investigation on the optical properties of micro-LEDs based on InGaN quantum dots grown by molecular beam epitaxy. Nanomaterials 2023, 13, 1346. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Hsu, Y.-H.; Lin, Y.-H.; Wu, M.-H.; Kuo, H.-C.; Horng, R.-H. Current confinement effect on the performance of blue light micro-LEDs with 10 μm dimension. ACS Omega 2023, 8, 35351–35358. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Yang, J.; Zhao, D.G.; Jiang, D.S.; Chen, P.; Liu, Z.S.; Zhu, J.J.; Li, X.; Liu, W.; Liang, F.; Zhang, L.Q.; et al. Physical implications of activation energy derived from temperature dependent photoluminescence of InGaN-based materials. Chin. Phys. B 2017, 26, 077101. [Google Scholar] [CrossRef] [Scilit]
- Chiu, Y.-C.; Bayram, C. Low temperature absolute internal quantum efficiency of InGaN-based light-emitting diodes. Appl. Phys. Lett. 2023, 122, 091101. [Google Scholar] [CrossRef] [Scilit]
- Ryu, H.-Y.; Kim, H.-S.; Shim, J.-I. Rate equation analysis of efficiency droop in InGaN light-emitting diodes. Appl. Phys. Lett. 2009, 95, 081114. [Google Scholar] [CrossRef] [Scilit]
- David, A.; Grundmann, M.J. Droop in InGaN light-emitting diodes: A differential carrier lifetime analysis. Appl. Phys. Lett. 2010, 96, 103504. [Google Scholar] [CrossRef] [Scilit]
- Olivier, F.; Daami, A.; Licitra, C.; Templier, F. Shockley–Read–Hall and Auger non-radiative recombination in GaN based LEDs: A size effect study. Appl. Phys. Lett. 2017, 111, 022104. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.