Abstract
Retaining serviceable timber supports longer structural service life and circular use of wood. Quantitative interpretation of drilling resistance requires calibration accuracy and sensitivity to measurement conditions to be considered together. This study combined these aspects for Scots pine, Norway spruce and silver fir. Linear calibrations linked mean drilling resistance (RM) to density and mechanical properties determined for 144 beams. Prediction errors were assessed by leave-one-out cross-validation, and density calibrations were tested for transfer between species. Separate experiments examined drilling orientation and temperature, supplemented by reanalysis of published moisture measurements. RM improved density prediction for all three species relative to a mean-based benchmark, with normalised root mean square errors of 7.4–12.9%. Mechanical prediction accuracy depended on species and the property assessed. Cross-species prediction revealed systematic bias, while differences between measurement conditions corresponded to shifts in estimated density comparable to calibration prediction errors. The combined evaluation of calibration performance and measurement sensitivity provides a practical basis for interpreting drilling resistance in timber assessment. Used alongside visual inspection and structural verification, the results can inform assessment decisions concerning the continued use, repair or further investigation of timber members.
1. Introduction
The continued use of timber that remains fit for service is an important aspect of sustainable construction. Decisions on continued use, local repair or replacement require an assessment of both material properties and the condition of individual members. In existing and historic buildings, this is particularly important: unnecessary replacement consumes new material and may lead to the loss of building fabric of architectural value. Non-destructive testing (NDT) and semi-destructive testing (SDT) complement visual inspection by providing information with limited intervention in the structure [1,2,3,4]. When interpreted in relation to the structural system and loading conditions, their results can support decisions on the retention and repair of timber members [5,6,7].
Among SDT techniques for timber assessment, drilling resistance measurement (DRM) is widely used. During drilling, the instrument records the resistance encountered by a thin drill bit, producing a profile that reflects local variations in wood structure [8,9]. The mean drilling resistance index (RM) can be related to density and, through empirical calibration, to selected mechanical properties. These measurements can be performed using Resistograph and IML-Resi instruments [10,11]. Quantitative assessment requires calibration relationships appropriate to the wood species, instrument and measurement conditions.
Previous studies have demonstrated relationships between drilling resistance and wood properties in both standing trees and structural timber [12,13]. A recent study on spruce reported strong relationships with density under controlled moisture conditions [14]. Wood anatomy also affects drilling resistance. Arnič et al. [15] identified relationships with latewood width and tracheid dimensions in spruce, whereas the associations between drilling resistance and anatomical features differed in beech. Temperature, moisture content and drilling parameters introduce additional variability [11,16,17]. The influence of drilling orientation depends on the anatomical directions being compared and the type of drill bit [18]. For practical use, calibration curves should be accompanied by estimates of prediction error and an assessment of sensitivity to measurement conditions.
Quantitative assessment of the softwood species commonly found in existing structures requires calibration performance and sensitivity to measurement conditions to be considered together. Correlation coefficients alone provide an incomplete basis for comparisons across different materials and test configurations. The importance of accounting for species has also been demonstrated for density estimation from the mass of drilling chips, where including species in calibration models improved their fit [19]. A common experimental procedure allows these comparisons across species and predicted properties. Expressing changes in RM as shifts in estimated density also helps clarify the practical significance of measurement conditions.
The present study examines drilling resistance measurements for pine, spruce and fir obtained within an experimental programme on the assessment of timber properties [20]. Species-specific calibration is combined with cross-validated estimates of prediction error and an assessment of changes in estimated density associated with measurement conditions. The analysis considers species differences and the effects of annual-ring orientation and temperature. Density serves as the main reference property. Bending strength, stiffness and the properties of small clear specimens are used to assess the potential of drilling resistance for mechanical characterization. The calibration series shares its density and mechanical reference measurements with the sclerometric study [21], while the moisture analysis is based on measurements reported separately [22]. The present analysis combines species-specific drilling-resistance calibrations with cross-validated assessment of prediction error, quantification of prediction uncertainty and evaluation of transfer between species.
The intended application is the assessment of timber for continued use or repair. Establishing the mechanical properties of reclaimed timber has also been identified as a challenge for circular wood construction [23]. Recent work on reclaimed Spruce illustrates how complementary diagnostic measurements can support the assessment of members intended for reuse [24]. By clarifying the information provided by drilling resistance measurements and the conditions affecting their interpretation, the present study contributes to assessment procedures aimed at extending service life and preserving timber as a structural resource.
2. Materials and Methods
2.1. Experimental Programme and Materials
The experimental programme comprised two parts, each involving three softwood species widely used in Central European construction: Scots pine (Pinus sylvestris L.), Norway spruce (Picea abies (L.) H. Karst.) and silver fir (Abies alba Mill.). These species are hereafter referred to as Pine, Spruce and Fir, respectively. Figure 1 outlines the experimental procedure.
Figure 1.
Schematic overview of the experimental programme. The moisture series reanalyses measurements reported in [22].
The calibration series comprised 144 beams (40 Pine, 59 Spruce and 45 Fir) obtained from Polish sawmills and originating from different forest sites to cover a broad range of densities. Their nominal dimensions were 50 × 50 × 1000 mm. Before testing, the beams were conditioned for at least three months at approximately 21 °C and 50–60% relative humidity. Moisture content at testing ranged from 11.1% to 11.7%. All beams were visually inspected before SDT.
The second part comprised separate series examining drilling direction relative to annual rings, temperature and moisture content. The directional series included 24 beams of the same nominal dimensions as the calibration specimens, with eight beams per species. Separate temperature and moisture series each comprised 18 specimens, six per species. The specimens used in the temperature tests measured 175 × 175 × 300 mm. The present paper reports the directional and temperature results, while the moisture results, published separately [22], provide context for interpreting the effects of measurement conditions.
2.2. Drilling Resistance Measurements
Drilling resistance was measured using a Resistograph 4453-S (RinnTech, Heidelberg, Germany), equipped with a drill bit with shaft and cutting head diameters of 1.5 and 3.0 mm, respectively. The feed rate was 40 cm/min, with a spatial sampling interval of 0.01 mm. The instrument was positioned horizontally and secured with clamps. In the calibration series, two measurements were taken per beam, one near each end, at least 50 mm from the end faces and perpendicular to the grain, avoiding visible knots. Drill bits were replaced after 50 measurements in air-dry wood; for wood with a high moisture content, the procedure specified replacement after 30 measurements. Testing followed specimen availability after conditioning and selection, with batches of the same species interspersed with batches of other species. No formal randomisation schedule was used. Battery voltage was maintained at a minimum of 25.0 V. Figure 2 shows the experimental setup.
Figure 2.
Experimental setup for drilling resistance measurements. Own source.
Profiles were exported using DECOM software. The analysis interval was initially identified between the first and last resistance values exceeding 85 a.u., and its boundaries were subsequently refined based on consecutive resistance values. Internal decreases in resistance were retained. The mean drilling resistance index (RM) was calculated by numerically integrating the retained profile and dividing the resulting area by the corresponding drilling length within the wood:
where R(z) is the recorded resistance signal at distance z from the entry point into the wood, and L is the drilling length within the wood. RM was expressed in instrument-specific arbitrary units. For calibration, RM values from the two profiles recorded for each beam were averaged to obtain one predictor per beam. The corresponding density reference was measured on a full-cross-section slice near the bending failure zone (Section 2.3). Thus, the calibration relates an average of two local drilling measurements to a separately sampled density reference. No correction for drill-shaft friction was applied.
Within-beam variability between the two end-region RM measurements was evaluated separately for Pine, Spruce and Fir. For each beam, the signed difference was calculated as di = RMi,2 − RMi,1. The mean and standard deviation of these differences and the mean absolute difference were calculated separately for each species. Absolute relative differences were calculated as 100|di|/mi, where mi is the arithmetic mean of the two measurements. A within-beam coefficient of variation was calculated as CVi = 100 si/mi, where si is the sample standard deviation. Relative differences and within-beam CVs were then averaged separately for each species.
2.3. Destructive Testing
Destructive tests were performed after the semi-destructive measurements. Figure A1 (Appendix A) outlines the procedure. Beam bending strength (fm) and the global modulus of elasticity in bending (E) were determined by four-point bending tests using a Walter + Bai (Löhningen, Switzerland) universal testing machine, in accordance with PN-EN 408:2004 [25]. The support span was 18 h, where h is the specimen depth (nominally 900 mm for h = 50 mm), with the loading points positioned at one-third and two-thirds of the span. The modulus was calculated from the load–deflection relationship between 10% and 40% of the maximum load. Mid-span deflection was measured with a resolution of 0.01 mm.
After beam failure, small clear specimens were prepared from the undamaged portions. Bending strength (f′m) was determined using specimens measuring approximately 20 × 20 × 300 mm in three-point bending tests with a span of 240 mm in accordance with PN-D-04103:1977 [26], while compressive strength parallel to the grain (fc,0) was measured on specimens of approximately 20 × 20 × 30 mm in accordance with PN-D-04102:1979 (Figure 3) [27]. At least two compression specimens were tested per beam, and their mean strength was used as the beam-level reference value. Sampling locations were selected according to the distribution of knots and other visible defects. Density (ρ) was calculated from the mass and volume of a knot-free slice encompassing the full cross-section, taken near the failure zone. Density and mechanical property values were adjusted to a reference moisture content of 12% using the corrections specified in the standards [28].
Figure 3.
Schematic locations of drilling resistance measurements and specimen extraction for density determination, bending tests and compression tests.
2.4. Effects of Environmental and Test Conditions
2.4.1. Drilling Direction Relative to Annual Rings
For each species, four beams were used to compare approximately radial (90°) and tangential (0°) drilling directions relative to the annual rings; the other four were used to compare angles of approximately 30° and 60°. All drilling was performed perpendicular to the grain. Six defect-free measurement areas were marked on each beam, three on each of two perpendicular faces. Two drilling paths, approximately 15 mm apart, were located within each area. Within each species, beams with similar densities and annual-ring widths were selected from a single forest stand. Mean density was approximately 600 kg/m3 for Pine and 450 kg/m3 for Spruce and Fir. Figure A2 (Appendix A) shows the specimen arrangement and drilling paths.
The results for each angle were analysed descriptively, taking into account the separate groups of four beams and repeated measurements within each beam. Drilled holes in selected Pine specimens were also examined qualitatively using computed tomography (Appendix C).
2.4.2. Temperature
The temperature series was designed to examine drilling resistance under heating and cooling conditions relevant to the inspection of timber in buildings, including, e.g., roof structures exposed to seasonal and daily temperature variations.
Three specimens per species were assigned to cooling and three to heating. Following reference measurements at approximately 20 °C, the initially air-dry specimens were wrapped in polyethylene film to limit moisture exchange. The cooling sequence consisted of 72 h at 0 °C followed by 72 h at −20 °C. Specimens in the heating series were exposed to 50 °C for 8 h, including approximately 3 h for warming. Tests were performed after the film was removed, taking care to minimise changes in specimen temperature. The measurement layout for the temperature sequence comprised two areas per specimen and three adjacent drilling cross-sections spaced approximately 15 mm apart (Figure A3a). Wood temperature was measured at the specimen surface immediately before drilling. The drilling paths were positioned off-centre, near the end faces and lateral surfaces.
The results were analysed descriptively using the mean and standard deviation of RM for each condition. For each species, the means from the separate cooling and heating series were compared with a common reference mean at 20 °C. Percentage differences were expressed relative to this reference value. The reported temperatures refer to the exposure conditions.
2.4.3. Moisture
Moisture-related differences in RM were examined by reanalysing measurements reported in [22]. The calibration equations presented here relate RM measured in air-dry timber to density and mechanical properties adjusted to a reference moisture content (MC) of 12%.
Measurements were grouped into MC intervals of 0–8%, >8–15% and >15–35%. Repeated observations within each specimen and interval were first averaged; interval means and standard deviations were then calculated across specimens. At MC above 35%, each value represented the mean of two drilling measurements from an individual specimen. Percentage differences in RM were calculated relative to the reference values at 12% MC reported in [22]: 110.18 for Pine, 111.45 for Spruce and 121.18 for Fir. The corresponding shifts in estimated density were calculated using Equation (5) as an illustrative sensitivity analysis. In particular, the calculations at approximately 85–100% MC represent a hypothetical application of the air-dry calibration outside its moisture conditions, rather than validated estimates of density at 12% MC.
2.5. Statistical Analysis
2.5.1. Calibration and Prediction Error
Pearson’s correlation coefficients r, two-sided p-values and 95% confidence intervals for r based on Fisher’s z-transformation were calculated for the 15 species-specific relationships between RM and the reference properties. Nominal significance was assessed at α = 0.05. Holm’s correction was applied across all 15 tests as a sensitivity analysis. Linear models with an intercept were fitted separately for each species and property using ordinary least squares: ŷ = aRM + b. Calibration and validation included all 144 beams. The same correlation analysis and linear calibrations were also applied to the pooled dataset. The five pooled correlations were evaluated separately and were not included in the Holm adjustment of the 15 species-specific tests.
Model fit and prediction error were evaluated separately. For residuals ei = yi − ŷi, the training root mean square error (RMSE) and residual standard deviation s were defined as follows:
The residual standard deviation in Equation (2) was calculated using (n − 2) degrees of freedom, corresponding to a model with one predictor and an intercept.
Prediction error was assessed using leave-one-out cross-validation (LOOCV), with the beam as the validation unit [29], providing a common basis for comparing model performance within the investigated dataset. Predictions for the omitted beams were used to calculate RMSE, mean absolute error (MAE) and mean prediction bias, defined as the mean of predicted minus observed values. The normalised RMSE was expressed as a percentage: 100 × RMSE/mean(y). A predictor based on the training set mean, recalculated at each validation step, served as the benchmark.
Quadratic models containing an additional RM2 term were fitted by ordinary least squares for all five reference properties, separately for each species and for the pooled dataset. Their prediction errors were compared with those of the corresponding linear models using RMSE from the same beam-level LOOCV procedure. RMSE reduction was expressed as the percentage decrease from the linear to the quadratic model, using the linear-model RMSE as the denominator.
To describe prediction uncertainty for an individual observation, a pointwise one-sided 95% lower prediction bound was calculated:
where x denotes RM, is its mean in the calibration dataset, and Sxx is the sum of squared deviations of RM from this mean. Here, n denotes the number of beams used to fit the model, and t0.95, n−2 is the 95th percentile of Student’s t-distribution with n − 2 degrees of freedom. Calculation of the bound assumes independent, approximately normally distributed errors with constant variance. The lower bound describes prediction uncertainty for an individual response at a specified RM value. It does not estimate a characteristic material strength and should not be used directly as a structural design value.
Empirical coverage was assessed by comparing the observed value for each omitted beam with the lower bound calculated from the remaining beams. The Shapiro–Wilk test was used to assess residual normality, and the Koenker–Breusch–Pagan test was used to assess constancy of variance. To assess the sensitivity of the fitted relationships to individual observations, leverage and Cook’s distance were calculated. For Pine, additional sensitivity analyses were performed by separately omitting the beam with the highest bending strength and the beam with the highest modulus of elasticity, then refitting the regressions and recalculating Pearson correlations. All observations were retained in the primary calibration analyses.
The choice of density reference was examined in a supplementary analysis comparing whole-beam density, calculated from beam mass and volume, with the corresponding full-cross-section slice density. Within each species, Pearson correlations between RM and each density measure were calculated for the same set of beams (Table A9).
2.5.2. Species Effects and Sensitivity to Measurement Conditions
Three nested models were compared for density: a common regression line for all species, a model with species-specific intercepts and a common slope, and a model with species-specific intercepts and slopes. The contribution of additional terms was assessed using F-tests for nested models. Wald tests with an HC3 heteroscedasticity-robust covariance estimator provided a robustness check. LOOCV errors were compared for the combined dataset and for each species.
Transferability of the RM–density relationship was assessed by fitting a model to two species and predicting density for the third, with each species omitted in turn [29]. RM was the sole predictor in these models. Predictions involving RM values outside the training range were identified.
The comparisons in Part 2 are exploratory. For the directional and temperature series, repeated RM measurements were first averaged within each specimen and condition. Group means and SDs were then calculated across specimen means. These SDs describe variation among specimens and do not represent confidence intervals for the percentage differences between group means. Directional percentage differences were calculated from the reported means within each angle-pair group: 0° relative to 90°, and 30° relative to 60°. These descriptive comparisons are not specimen-level paired effect estimates. For the temperature series, percentage differences in mean RM, Δ, and normalisation factors, k, were calculated separately for each species:
where the overbar denotes a group mean, the subscripts c and ref indicate the test and reference conditions, respectively, and Δ is expressed as a percentage. The reference condition was 20 °C for the temperature series. The factors reported in Table A5 describe normalisation at the group-mean level.
To assess the sensitivity of density estimates to measurement conditions, differences in mean RM were multiplied by the slope of the corresponding species-specific density calibration:
where aρ is the slope of the density calibration for the species considered. This calculation combines the calibration slopes with mean RM values from the separate temperature and moisture series. The resulting represents the corresponding shift in estimated density. Cases involving RM values outside the species-specific calibration range were marked as extrapolations.
3. Results
3.1. Characteristics of the Tested Timber
Table 1 summarises the calibration dataset. Density and mechanical properties are reported at a reference moisture content of 12%. Full descriptive statistics, including the ranges of individual variables, are provided in Table A1 (Appendix B).
Table 1.
Sample sizes and characteristics of the calibration dataset.
Pine and Fir had almost identical mean RM values, although mean density was approximately 7% higher in Pine. Spruce showed the lowest mean values for both variables. Relative variation in RM was also lowest in Spruce and highest in Fir. These descriptive differences suggest that species may influence the relationship between drilling resistance and density; species effects are examined further in Section 3.4.
The mean absolute differences between the two end-region RM measurements were 4.76, 3.82 and 3.83 arbitrary units for Pine, Spruce and Fir, respectively. The corresponding mean absolute relative differences were 4.06%, 3.41% and 3.15%, and the mean within-beam CVs were 2.87%, 2.41% and 2.23%. Mean signed differences (RM2 − RM1) were −1.85, −1.75 and −0.75 arbitrary units, with standard deviations of 5.64, 4.91 and 5.64 arbitrary units, respectively.
3.2. Relationships Between Drilling Resistance and Timber Properties
For the pooled dataset of 144 beams, the correlation between RM and density was r = 0.697. Species-specific correlation coefficients, their 95% confidence intervals and p-values are reported in Table A2. Among the three species, the RM–density correlation was strongest for Fir (r = 0.771), with similar coefficients for Pine and Spruce (r = 0.586 and 0.575, respectively). The RM–E relationship for Pine was not statistically significant (r = 0.215, p = 0.184). The remaining 14 species-specific correlations remained significant after Holm adjustment across the 15 tests.
Table 2 presents the corresponding regression equations and residual standard deviations, together with the RM range used to fit each model. The density calibrations are illustrated in Figure 4. Application of the equations outside the reported RM ranges would involve extrapolation. Prediction errors are discussed in Section 3.3.
Table 2.
Species-specific and pooled calibration equations for the mean response ŷ = aRM + b.
Figure 4.
Relationship between mean drilling resistance (RM) and density adjusted to a reference moisture content of 12%: (a) Pine; (b) Spruce; (c) Fir; (d) all species pooled.
Quadratic models reduced LOOCV RMSE in four of the 15 species-specific calibrations, with improvements ranging from 0.4% to 3.3%. For density, the only improvement occurred for Fir, where RMSE decreased from 57.08 to 55.19 kg/m3; errors increased for Pine and Spruce. In the pooled dataset, changes in RMSE were below 1% for all five properties. These limited and inconsistent gains supported retaining linear equations for the main calibration and sensitivity analyses. Full comparisons are provided in Table A7.
3.3. Prediction Error
Figure 5 compares correlation strength with cross-validated prediction error. Full error metrics for model fitting and cross-validation are provided in Table A3. Density RMSE in LOOCV was 62.46, 31.08 and 57.08 kg/m3 for Pine, Spruce and Fir, respectively, corresponding to nRMSE values of 12.9%, 7.4% and 12.6%. Compared with the training-mean predictor, RM reduced density RMSE by 16.9% for Pine, 16.6% for Spruce and 34.4% for Fir. Relative errors were higher for beam bending strength, with nRMSE ranging from 20.4% to 39.3%. For the modulus of elasticity of Pine, the RM model did not improve predictive accuracy: its LOOCV RMSE was 3.885 GPa, compared with 3.844 GPa for the training-mean predictor.
Figure 5.
Correlation strength and prediction error for species-specific RM models: (a) Pearson’s correlation coefficients with 95% confidence intervals; (b) normalised root mean square error (nRMSE, %) from leave-one-out cross-validation at the beam level. Results are shown for Pine, Spruce and Fir and the five reference properties.
Cross-validated coverage of the one-sided 95% lower prediction bounds ranged from 88.9% to 100% across the 15 RM models. For density, the observed value was at or above the bound for 39 of 40 Pine beams, 56 of 59 Spruce beams and 44 of 45 Fir beams.
These bounds provide an approximate measure of prediction uncertainty for individual observations. Departures from residual normality or constant variance in some models may cause actual coverage to differ from the nominal 95% level. The reported cross-validated coverage describes performance within the investigated dataset and does not guarantee equivalent coverage for other timber populations. Detailed diagnostic results are provided in Table A7.
The Pine models were additionally examined for sensitivity to individual observations. Leverage ranged from 0.025 to 0.177. The beam with fm = 148.24 MPa had Cook’s distance of 0.291 for bending strength. Omitting this beam reduced the corresponding RM correlations from 0.495 to 0.469. The separate beam with E = 20.2 GPa had a Cook’s distance of 0.069 in the stiffness model; its omission changed the RM–E correlation from 0.215 to 0.226. Thus, the positive RM–bending-strength association persisted after omission of the highest-strength beam, although its magnitude decreased. The RM–E association remained weak in both sensitivity analyses.
3.4. Species Effects and Cross-Species Prediction
The pooled density calibration was ρ = 4.339RM−48.578, with r = 0.697. Allowing both intercepts and slopes to vary by species reduced the overall LOOCV RMSE from 51.85 to 49.98 kg/m3, a reduction of 3.6% (Table 3). The species-by-RM interaction was statistically significant (F(2,138) = 3.341, p = 0.0383), with a similar result from the HC3-robust Wald test (p = 0.0408). Allowing species-specific intercepts while retaining a common slope significantly improved model fit relative to the common regression line (F(2,140) = 6.806, p = 0.0015; HC3-robust Wald test: p = 0.0069).
Table 3.
Comparison of pooled and species-specific density calibrations based on RM.
Predicting a species omitted from calibration increased RMSE for Pine and Spruce relative to species-specific LOOCV (Table 4). For Fir, RMSE was virtually unchanged: 56.98 kg/m3 compared with 57.08 kg/m3. Pine density was underestimated on average, whereas Spruce and Fir densities were overestimated. The mean shifts for Pine and Spruce occurred despite all their RM values falling within the training range. Four Fir observations lay outside that range.
Table 4.
Density prediction for each species using a model fitted to the other two species with RM as the sole predictor.
3.5. Effect of Annual Ring Orientation
Figure 6 presents mean RM and standard deviations for the two angle-pair groups. Within the 0°/90° group, mean RM at 0° differed from that at 90° by −2.7% for Pine, +2.0% for Spruce and −1.2% for Fir. Within the 30°/60° group, mean RM at approximately 30° was higher than at approximately 60° by 2.6%, 2.2% and 2.2%, respectively. These percentages describe differences between group means within each angle pair. The two angle pairs were tested on separate groups of beams and are therefore presented as separate descriptive comparisons. Full mean RM values and standard deviations are provided in Table A4.
Figure 6.
Mean drilling resistance (RM) for Pine, Spruce and Fir. Circles and squares represent the 0°/90° and 30°/60° angle-pair groups, respectively. Each pair was tested on a separate group of four beams per species. Points show means and error bars indicate standard deviations. Percentage labels show differences between group means at 0° relative to 90° and at 30° relative to 60°.
3.6. Effect of Temperature and Sensitivity of Density Estimates
Mean RM was lowest under the 20 °C reference condition (Figure 7; Table A5). Compared with the common reference mean for each species, values at −20 °C were 31.4%, 34.6% and 20.8% higher for Pine, Spruce and Fir, respectively. At 50 °C, the corresponding differences were 9.3%, 11.8% and 3.3%.
Figure 7.
Mean drilling resistance (RM) under four temperature conditions, with a common mean RM at 20 °C used as the reference for each species. Error bars indicate standard deviations. The cooling and heating series comprised separate groups of three specimens per species.
Applying the species-specific RM–density calibration slopes to the differences between mean RM at 0 °C and the common 20 °C reference caused upward shifts in the estimated density of 41.5, 19.6 and 64.0 kg/m3 for Pine, Spruce and Fir, respectively. The corresponding shifts at 50 °C were 35.7, 33.3 and 20.8 kg/m3. These values quantify the sensitivity of density estimates to the observed differences in RM between test conditions. The −20 °C scenarios for Spruce and Fir exceeded the RM ranges used for calibration and are identified as extrapolations in Table A5.
3.7. Effect of Moisture and Sensitivity of Density Estimates
Grouping the moisture measurements reported in [22] showed relatively small differences in mean RM across the three moisture content (MC) intervals up to 35% for Pine and Spruce. Fir showed a clearer increase (Figure 8). Relative to the species-specific reference RM values at 12% MC, the group means in the >15–35% interval differed by +3.5%, −1.7% and +5.7% for Pine, Spruce and Fir, respectively. The individual specimen means at the highest recorded MC were 16.4%, 13.7% and 13.6% above the respective reference values.
Figure 8.
Mean drilling resistance (RM) at different moisture contents for Pine, Spruce and Fir, based on measurements reported in [22]. Squares show means ± SD across specimens within the MC intervals 0–8%, >8–15%, and >15–35%. Circles represent individual specimen means, each based on two drilling measurements.
Using the species-specific density calibration slopes, the differences for the >15–35% MC interval corresponded to shifts in estimated density of +13.9, −5.2 and +35.2 kg/m3 for Pine, Spruce and Fir, respectively. At the highest recorded moisture contents, approximately 85%, 95% and 100% for the respective species, the corresponding shifts were +65.3, +41.2 and +83.6 kg/m3. For Spruce at approximately 95% MC, this calculation involved extrapolation beyond the RM range used for calibration. Full moisture results and normalisation factors are provided in Table A6.
4. Discussion
4.1. Drilling Resistance Calibration
The positive RM–density relationships confirm that drilling resistance provides information on wood density in the three coniferous species studied, consistent with previous research [1,8,9,10]. The strength of these relationships varies with the material and test arrangement. Brunetti et al. [30], for example, reported higher coefficients of determination for density using reference specimens taken at the drilling locations. The calibration was intended to assess the usefulness of local drilling measurements for characterising timber beams. Mean RM from two end-region profiles was related to bending properties measured on the beam and to density and mechanical properties determined on specimens extracted from the same beam. This arrangement incorporates within-beam spatial variation into the evaluated sampling procedure. The reported cross-validated errors therefore quantify predictive performance for this sampling arrangement, encompassing the combined effects of spatial variation, measurement variability and model approximation. For density, the reference value was obtained from a full-cross-section slice near the failure zone. The calibration measurements were taken perpendicular to the grain without a fixed angle relative to the annual rings. Variation in annual-ring orientation may therefore have contributed to the scatter in the calibration relationships.
The mean within-beam CVs of 2.23–2.87% indicate relatively limited average variation between the two end-region measurements in the analysed set. For context, the CVs calculated from the beam-averaged RM values in the full calibration dataset ranged from 7.19% to 11.12% across species (Table 1). This descriptive comparison does not constitute a formal partition of variance. The end-region differences include both local wood heterogeneity and measurement variability, and agreement between two locations does not establish representativeness of the entire beam volume. The mean absolute relative differences of 3.15–4.06% also warrant caution when interpreting condition-related changes of only a few percent. These statistics provide context rather than a universal detection threshold for the separate directional and temperature experiments.
Whole-beam and slice densities were strongly correlated within each species (r = 0.871–0.938; Table A9). For all three species, RM was positively correlated with both density measures, with consistently higher correlations for slice density than for whole-beam density.
Prediction errors provide a more direct measure of accuracy relevant to timber assessment than correlation alone. Spruce showed a lower absolute prediction error for density than Fir despite its weaker correlation, partly reflecting its narrower density range. RM-based models reduced density prediction error for all three species compared with predictions based on the training-set mean density. The equations can thus support material characterisation, with the reported errors indicating the level of accuracy to consider when comparing individual members.
For mechanical properties, the interpretation of RM relationships additionally requires consideration of the volume of wood represented by the reference test. Density prediction yielded nRMSE values of 7.4–12.9%, compared with 20.4–39.3% for beam bending strength. A drilling path samples a narrow, localised zone, whereas the mechanical response of a structural member also depends on knots, grain deviations and their positions relative to the applied stresses. Relationships obtained for small clear specimens therefore cannot, by themselves, establish predictive accuracy for structural members containing defects. Arnič et al. [15] also showed that relationships between drilling resistance and anatomical features vary between species. In the present study, RM provided information on E for Spruce and Fir; for Pine, a complementary measurement sensitive to stiffness would be appropriate. The reported calibration equations cannot independently establish characteristic strength values or replace structural grading and verification.
In addition to material characteristics and the sampling arrangement, instrument settings and measurement procedures need to be considered when applying calibration equations. Sharapov et al. [13] examined the effects of moisture content and feed rate, while Gendvilas et al. [11,31] investigated operating parameters and differences between instruments and operators. In a subsequent study, the latter authors found that the effect of drill bit wear depended on the wood material and drilling parameters [32]. Gendvilas et al. [33] further demonstrated the importance of drill shaft friction and the profile correction method for density estimation. These findings indicate that drilling path length and signal processing should be considered when comparing calibrations. Together, they support the need to record operating parameters and maintain a consistent measurement procedure when using RM quantitatively.
4.2. Species Effects and Calibration Transferability
Differences in regression slopes and the interaction test result indicate that species affects the RM–density relationship. Although the correlation for the pooled dataset was 0.697, the pooled model underestimated Pine density by an average of 24.23 kg/m3 and overestimated density for Spruce and Fir by 9.89 and 8.34 kg/m3, respectively (Table A8). Examining errors within each species is therefore useful even when the overall correlation appears satisfactory.
Allowing both intercepts and slopes to vary by species reduced the overall LOOCV RMSE by 3.6%, from 51.85 to 49.98 kg/m3. For Fir, the pooled and species-specific models yielded nearly identical errors: 56.79 and 57.08 kg/m3, respectively. In this dataset, the main practical benefit of accounting for species was the reduction in species-specific prediction bias. For Pine, the mean LOOCV bias was close to zero (+0.17 kg/m3) with the species-specific model (Table A8). Calibration selection should therefore consider systematic errors within individual species alongside overall prediction accuracy. Cross-species prediction provided a further assessment of calibration transferability. When Pine was excluded from model fitting, its density was underestimated by an average of 33.30 kg/m3, although all RM values fell within the training range. Remaining within that range was therefore insufficient to avoid species-related prediction bias.
Morales-Conde et al. [34] addressed the need for calibration representative of the assessed timber by using density measurements from cores taken close to the drilling paths. Their approach provides local reference values against which drilling resistance can be calibrated. Todoroki et al. [35] also demonstrated a difference between calibration performance and prediction on independent material: the RMSE of their best-fitting model increased from 25.0 kg/m3 in the calibration dataset to 59.5 kg/m3 in an external dataset. The latter study concerned external validation in standing Douglas-fir, whereas the present analysis examined transfer between species under a common measurement procedure. Although these represent different aspects of transferability, both highlight the need to assess prediction performance beyond the calibration dataset.
Reliable species identification is therefore important for calibration selection. Applying an equation for an incorrectly identified species may introduce systematic error into the density estimate. When species identification is uncertain, the selected calibration should be verified against representative reference measurements before quantitative application.
4.3. Measurement Conditions and Normalisation
The relatively small differences between radial and tangential drilling agree with Sharapov et al. [18], who reported more pronounced differences between longitudinal and transverse drilling. All four angles tested here retained drilling perpendicular to the grain. Variation in the earlywood and latewood sampled along each path may contribute to the observed scatter. The 0°/90° and 30°/60° comparisons involved separate beam groups. Selecting beams with similar densities and annual-ring widths does not demonstrate equivalence between these groups. The highest mean RM at approximately 30° is therefore a descriptive observation for the tested material and does not establish a general maximum attributable to drilling orientation. The CT sections in Figure A4 illustrate how the drilled path intersects the annual-ring structure and show local irregularities along the hole margins, providing qualitative context for these orientation-dependent measurements.
In the tested series, temperature-related differences in RM were larger than directional differences, especially at −20 °C. Song et al. [16] also reported increased drilling resistance at low temperatures in standing poplar. Sharapov et al. [36] found particularly large increases in water-saturated Pine at −10 °C, indicating the importance of moisture state. The initially air-dry condition of the specimens tested here means that freezing of free water cannot be assumed to explain their response. The higher mean RM at 50 °C was obtained in a separate heating group. Comparisons with the shared 20 °C reference therefore describe differences between the tested conditioning variants rather than establish a continuous temperature response. The temperature series provides evidence of RM variation under conditioning protocols relevant to timber inspection. Polyethylene wrapping was used to limit moisture exchange, while drill-bit replacement and battery-voltage control followed Section 2.2. However, the separate contributions of internal temperature gradients, surface drying or condensation, measurement order and drill-bit wear, and instrument/battery temperature were not quantified. The higher mean RM after heating should therefore be interpreted as a finding specific to the applied protocol.
The grouped moisture results show relatively little variation for Pine and Spruce at lower MC, with a more evident increase for Fir. This agrees with the weak relationships reported for Pine and Spruce below the fibre saturation point in [22]. It also helps reconcile the present results with those of Heřmánková et al. [14], who found little moisture dependence for Spruce over an MC range of 0–53%. The Spruce observation near 95% MC lies outside that range. CT images of water-saturated Pine (Figure 17 in [22]) show cuttings accumulated at the borehole walls. Such accumulation may increase friction, potentially offsetting the reduction in cutting resistance associated with moisture-induced softening. Higher RM in wet wood need not therefore indicate improved mechanical properties. Sharapov et al. [17] further showed that the direction of the moisture effect could reverse with changes in feed per cutting edge. The extreme moisture contents were obtained by oven-drying or prolonged water immersion (12 months). Conditioning-related changes in the wood may also have influenced RM, so these observations should be interpreted in the context of the conditioning history.
Interpretation of the condition-related RM differences also requires consideration of drilling geometry and friction. The 3.0 mm cutting head and 1.5 mm shaft follow the needle geometry described by Rinn et al. [8]. The friction correction investigated in [33] was developed using a different instrument and wood species, and its quantitative applicability to the present configuration has not been established. Within each temperature and moisture series, the nominal drilling length remained approximately 175 mm across conditioning variants, supporting comparisons under consistent measurement geometry.
The normalisation factors for temperature and moisture content express the reported mean RM values relative to the selected reference conditions. The density shifts were calculated using the slopes of density calibrations developed with approximately 50 mm drilling paths. These shifts express the observed RM differences on the calibration model’s density scale and illustrate their potential practical importance, with possible conditioning-related friction effects considered alongside changes in cutting resistance. For Spruce, the difference between the 50 °C mean and the shared 20 °C reference corresponded to an upward shift of 33.3 kg/m3, comparable to the LOOCV RMSE of 31.1 kg/m3. The calculated density shift is a signed change in model output associated with a difference in RM; it is not a measured change in reference density. LOOCV RMSE summarises the overall magnitude of prediction errors across omitted beams and can reflect both dispersion and systematic bias. Comparing these quantities illustrates their relative scale but does not equate them or provide an estimate of their combined effect.
In existing timber structures, temperature and moisture content may vary simultaneously, and their effects on RM may interact. The separate experimental series considered here do not quantify this interaction or establish whether the effects are additive. Consequently, the normalisation factors derived separately for temperature and moisture content should not be combined into a general correction without validation under controlled combinations of these conditions.
4.4. Implications for Service Life Extension and Circular Use
Drilling resistance measurements can support the assessment of timber in service by providing local information with limited intervention. Measurement locations should account for the stress distribution within the member; the findings of Sharapov et al. [37] support locating drilling holes outside areas of maximum tensile stress. Calibration equations convert mean resistance into property estimates, while prediction errors indicate their accuracy. In practice, these estimates should be considered alongside visual grading and the resistance profile. Member geometry and connections must also be addressed within the structural assessment described in the relevant guidance [3,4]. Monitoring and internal inspection can provide additional information where deterioration or changes in condition are suspected [38,39].
To illustrate a potential application, consider a hypothetical Pine roof member assessed using the two-profile averaging procedure and measurement conditions of the calibration. For a mean RM of 120 a.u., which lies within the calibrated range, the equation in Table 2 gives an estimated reference density of approximately 494 kg/m3 at 12% moisture content. The corresponding one-sided 95% lower prediction bound, calculated using Equation (3) and the parameters in Appendix B, is approximately 390 kg/m3. These values illustrate how the density estimate can be considered together with prediction uncertainty under the model assumptions.
In this illustrative assessment, the density estimate and its prediction uncertainty would be considered alongside visual grading, moisture measurements and examination of the drilling profiles. Retention would be supported where structural verification, accounting for defects, the remaining cross-section, loads and connections, confirms adequate performance. Localised damage could justify evaluating repair or reinforcement options, while replacement may be necessary where adequate performance cannot be achieved through feasible interventions. If uncertainty in the material properties could change the assessment outcome, targeted reference measurements or complementary tests would be required before selecting an intervention. The practical contribution of RM calibration is therefore to support material characterisation and identify where further investigation is warranted, helping preserve existing timber where continued use is structurally justified. Huber et al. [24] illustrated the role of complementary measurements by comparing visual, dynamic and CT-derived indicators for reclaimed Spruce intended for reuse as glulam lamellas. Their study and reliability-based assessment approaches [5,6] place material testing within a broader decision-making process.
For reclaimed or biologically degraded timber, reference measurements should represent the condition being assessed. Kahl et al. [40] showed that the relationship between drilling resistance and density in decaying Spruce deadwood depended on its decay state. Mirra et al. [41] related micro-drilling profiles to density, stiffness and strength distributions across historic foundation piles, using mechanical tests, CT and microscopy to characterise bacterial decay. Their results distinguished degraded outer zones from sound wood within the same cross-sections. Such spatially resolved assessment helps relate local drilling resistance to the remaining material properties after prolonged service.
The sustainability relevance of the present study lies in supporting informed decisions on timber retention, repair and reuse. When combined with structural assessment, species-specific calibrations and their prediction uncertainties can help identify members suitable for continued use and guide interventions proportionate to the identified damage. This provides a practical link between material characterisation, service life extension and circular use of timber. Quantifying the resulting environmental benefits would require a separate assessment of actual intervention scenarios.
4.5. Application and Further Research
The equations provide a basis for the quantitative interpretation of RM for Pine, Spruce and Fir under the material and measurement conditions investigated. Their applicability to timber affected by fungal decay, insect damage or other deterioration requires separate verification of the RM–property relationship for the relevant material condition. For timber from other sources or with different service histories, estimates should likewise be checked against representative reference measurements. Recording temperature, moisture content and drilling direction alongside RM would help assess whether field measurement conditions are consistent with those used for calibration.
Further research should examine how the number and distribution of drilling resistance measurements affect the accuracy of property estimates for whole members. This would help adapt the measurement programme to variability within the beam and the property being assessed. Normalisation factors should also be evaluated using paired measurements on the same members under test and reference conditions, with controlled combinations of temperature, moisture content and drilling direction. Comparing prediction errors before and after normalisation would show whether accounting for measurement conditions improves assessment accuracy.
5. Conclusions
- Drilling resistance provided quantitative information on the wood density of all three softwood species. The RM–density correlation coefficients were 0.586 for Pine, 0.575 for Spruce and 0.771 for Fir. Species-specific equations reduced density RMSE in LOOCV by 16.6–34.4% compared with the training-mean predictor, demonstrating the contribution of RM to density estimation under the measurement procedure used.
- Prediction accuracy depended on both species and the property considered. Density nRMSE ranged from 7.4% to 12.9%, compared with 20.4–39.3% for beam bending strength. For Pine, RM alone did not improve prediction of the modulus of elasticity over the training-mean predictor. These results support using RM as complementary diagnostic information, with stronger predictive performance for density than for beam bending strength. The calibrations are specific to the investigated species, instrument configuration, measurement procedure and material ranges, and do not independently establish the structural capacity of a timber member.
- Species affected both calibration slopes and prediction bias. Allowing species-specific intercepts and slopes reduced the overall density RMSE in LOOCV by 3.6% relative to the pooled model. Cross-species prediction revealed systematic biases even for RM values within the training range. Calibration selection should thus account for species and the extent to which the reference material represents the timber being assessed.
- In the directional series, mean RM differences within the 0°/90° groups ranged from −2.7% to +2.0%, while mean RM at 30° exceeded that at 60° by 2.2–2.6% within the separate 30°/60° groups. These descriptive comparisons do not establish a general ranking of drilling orientations. At −20 °C, mean RM values were 20.8–34.6% higher than the common 20 °C reference mean for each species. Reanalysis of published moisture data indicated smaller changes in mean RM at lower moisture contents for Pine and Spruce than for Fir. The normalisation factors for temperature and moisture content express the reported mean RM values relative to the selected reference conditions.
- Expressing differences in RM as shifts in estimated density showed that measurement conditions can affect estimates by amounts comparable to the prediction error. For Spruce, the difference between the 50 °C mean and the common 20 °C reference corresponded to a density shift of 33.3 kg/m3, compared with a LOOCV RMSE of 31.1 kg/m3. The combined assessment of calibration performance and measurement sensitivity provides a practical basis for interpreting drilling resistance results. Combined with visual inspection and structural verification, the findings can inform decisions on timber retention and repair, supporting the assessment of options for continued use.
Author Contributions
Conceptualization, J.J.-L. and D.W.; methodology, J.J.-L. and D.W.; software, J.J.-L.; validation, J.J.-L.; formal analysis, J.J.-L.; investigation, J.J.-L. and D.W.; resources, J.J.-L.; data curation, J.J.-L. and D.W.; writing—original draft preparation, J.J.-L.; writing—review and editing, J.J.-L. and D.W.; visualization, J.J.-L. and D.W.; supervision, D.W.; project administration, J.J.-L. All authors have read and agreed to the published version of the manuscript.
Funding
This research was partially funded by the program “Excellence initiative-research university” for the AGH University of Krakow.
Institutional Review Board Statement
Not applicable.
Informed Consent Statement
Not applicable.
Data Availability Statement
The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.
Conflicts of Interest
The authors declare no conflicts of interest.
Abbreviations
The following abbreviations are used in this manuscript:
| a.u. | Arbitrary units |
| CI | Confidence interval |
| CT | Computed tomography |
| CV | Coefficient of variation |
| DRM | Drilling resistance measurement |
| HC3 | Heteroscedasticity-consistent covariance estimator, type 3 |
| LOOCV | Leave-one-out cross-validation |
| MAE | Mean absolute error |
| MC | Moisture content |
| NDT | Non-destructive testing |
| nRMSE | Normalised root mean square error |
| RH | Relative humidity |
| RM | Mean drilling resistance index |
| RMSE | Root mean square error |
| SD | Standard deviation |
| SDT | Semi-destructive testing |
Appendix A
Figure A1.
Experimental sequence for drilling resistance measurements and determination of reference timber properties.
Figure A2.
Measurement layout for assessing the effect of drilling direction relative to annual rings: (a) measurement areas and drilling paths; (b) annual-ring arrangements for the 0°/90° and 30°/60° comparisons. Red arrows and lines indicate drilling directions and paths; dashed rectangles delimit measurement areas.
Figure A3.
Specimen geometry, drilling layout and conditioning procedures for assessing the effects of (a) temperature and (b) moisture content on drilling resistance. Red arrows and lines indicate drilling directions and paths; dashed rectangles delimit measurement areas.
Appendix B
Property symbols and units follow Table 1. Density and mechanical properties refer to 12% MC. Prediction errors have the units of the corresponding property, except nRMSE (%); bias is the mean predicted minus observed value. In Table A5 and Table A6, Δ denotes the percentage difference in RM from the species-specific reference, and k is the ratio of reference RM to the reported mean RM. The corresponding shift in estimated density, Δ, expresses calibration sensitivity to these differences (Equation (5)). An asterisk marks extrapolation beyond the species-specific RM calibration range.
For Equation (3), the pairs (mean RM, (Sxx)) are (117.63, 5667.93) for Pine, (109.88, 3620.73) for Spruce, (117.52, 7513.99) for Fir and (114.42, 18,866.81) for the pooled dataset. The corresponding sample sizes are 40, 59, 45 and 144.
Table A1.
Descriptive statistics for the species-specific and pooled calibration datasets.
Table A2.
Pearson correlations between RM and reference properties, 95% confidence intervals, coefficients of determination and p-values.
Table A3.
Training and cross-validated errors of the linear RM calibration models.
Table A4.
Mean drilling resistance for the two annual-ring angle-pair groups.
Table A5.
Mean drilling resistance and normalisation factors at different conditioning temperatures.
Table A6.
Mean drilling resistance and normalisation factors at different moisture contents.
Table A7.
Cross-validated comparison of linear and quadratic models, residual diagnostics and prediction-bound coverage.
Table A8.
Density prediction errors and bias for pooled and species-adjusted models in leave-one-out cross-validation.
Table A9.
Supplementary comparison of whole-beam density, slice density and mean drilling resistance.
Appendix C
Selected Pine specimens were examined by X-ray computed tomography to visualise the drilled hole relative to the annual-ring structure. Specimens measuring approximately 15 × 15 × 40 mm were scanned using a GE Phoenix v|tome|x m system, and the reconstructed volumes were examined in VGStudio MAX. Scan settings within this imaging series ranged from 40 to 50 kV and from 90 to 110 µA, with voxel sizes of 10–20 µm [20].
Figure A4 presents sections along the drilled holes viewed in the transverse plane of the wood. The images show the hole crossing successive growth-ring bands at approximately 90°, following the ring orientation at approximately 0°, and intersecting the bands obliquely at approximately 60°. Local irregularities in the hole margins and retained drill cuttings provide qualitative context for the directional measurements. The quantitative comparison of drilling resistance is based on the RM results in Section 3.5.
Figure A4.
CT sections along drilled holes in Pine, viewed in the transverse plane of the wood, at drilling angles of approximately (a) 90°, (b) 0° and (c) 60° relative to the annual rings. The images illustrate the relationship between the drilling path and ring structure. Scale bars: 1 mm. Adapted from [20]. Blue and green lines mark auxiliary CT sections. L denotes the displayed section along the borehole; R/R1/R2 and T denote sections showing tangential and radial wood surfaces, respectively; RT/TR denote oblique sections.
References
- Nowak, T.P.; Jasieńko, J.; Hamrol-Bielecka, K. In situ assessment of structural timber using the resistance drilling method—Evaluation of usefulness. Constr. Build. Mater. 2016, 102, 403–415. [Google Scholar] [CrossRef] [Scilit]
- Piazza, M.; Riggio, M. Visual strength-grading and NDT of timber in traditional structures. J. Build. Apprais. 2008, 3, 267–296. [Google Scholar] [CrossRef] [Scilit]
- Riggio, M.; Anthony, R.W.; Augelli, F.; Kasal, B.; Lechner, T.; Muller, W.; Tannert, T. In situ assessment of structural timber using non-destructive techniques. Mater. Struct. 2014, 47, 749–766. [Google Scholar] [CrossRef] [Scilit]
- Tannert, T.; Anthony, R.W.; Kasal, B.; Kloiber, M.; Piazza, M.; Riggio, M.; Rinn, F.; Widmann, R.; Yamaguchi, N. In situ assessment of structural timber using semi-destructive techniques. Mater. Struct. 2014, 47, 767–785. [Google Scholar] [CrossRef] [Scilit]
- Sousa, H.S.; Sørensen, J.D.; Kirkegaard, P.H.; Branco, J.M.; Lourenço, P.B. On the use of NDT data for reliability-based assessment of existing timber structures. Eng. Struct. 2013, 56, 298–311. [Google Scholar] [CrossRef] [Scilit]
- Sousa, H.S.; Branco, J.M.; Lourenço, P.B. A Holistic Methodology for Probabilistic Safety Assessment of Timber Elements Combining Onsite and Laboratory Data. Int. J. Archit. Herit. 2016, 10, 526–538. [Google Scholar] [CrossRef] [Scilit]
- Santini, S.; Borghese, V.; Baggio, C. HBIM-Based Decision-Making Approach for Sustainable Diagnosis and Conservation of Historical Timber Structures. Sustainability 2023, 15, 3003. [Google Scholar] [CrossRef] [Scilit]
- Rinn, F.; Schweingruber, F.-H.; Schär, E. RESISTOGRAPH and X-Ray Density Charts of Wood. Comparative Evaluation of Drill Resistance Profiles and X-ray Density Charts of Different Wood Species. Holzforschung 1996, 50, 303–311. [Google Scholar] [CrossRef] [Scilit]
- Gao, S.; Wang, X.; Wiemann, M.C.; Brashaw, B.K.; Ross, R.J.; Wang, L. A critical analysis of methods for rapid and nondestructive determination of wood density in standing trees. Ann. For. Sci. 2017, 74, 27. [Google Scholar] [CrossRef] [Scilit]
- Joseph, J.; Maripa, R.D.; Phua, M.H. Envisaging the Potential Use of Resistance Micro Drilling on Wood Density Assessment: A Review. In Green Infrastructure: Materials and Sustainable Management; Hashim, U.R., Arshad, A.K., Abdul Hamid, N.H., Hassan, R., Shaffie, E., Alisibramulisi, A., Mohamad Bhkari, N., Muhd Sidek, M.N., Eds.; Springer: Singapore, 2023; pp. 351–366. [Google Scholar] [CrossRef] [Scilit]
- Gendvilas, V.; Downes, G.M.; Lausberg, M.; Harrington, J.J.; Lee, D.J. Predicting Wood Density Using Resistance Drilling: The Effect of Varying Feed Speed and RPM. Forests 2024, 15, 579. [Google Scholar] [CrossRef] [Scilit]
- Barría, C.; Sandoval, S.; Rojas, G. Uso del método de resistografía para la predicción de la densidad básica de la madera en árboles en pie de Pinus radiata. Maderas Cienc. Tecnol. 2017, 19, 349–362. [Google Scholar] [CrossRef] [Scilit]
- Sharapov, E.; Brischke, C.; Militz, H.; Smirnova, E. Prediction of modulus of elasticity in static bending and density of wood at different moisture contents and feed rates by drilling resistance measurements. Eur. J. Wood Wood Prod. 2019, 77, 833–842. [Google Scholar] [CrossRef] [Scilit]
- Heřmánková, V.; Anton, O.; Hrabová, K.; Cikrle, P.; Kocáb, D. Experimental Determination of the Relationship Between the Resistance Micro-Drilling Characteristic and the Density of Spruce Wood at Different Moisture Contents. Materials 2026, 19, 3140. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Arnič, D.; Krajnc, L.; Gričar, J.; Prislan, P. Relationships Between Wood-Anatomical Features and Resistance Drilling Density in Norway Spruce and European Beech. Front. Plant Sci. 2022, 13, 872950. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Song, X.; Gao, T.; Ai, M.; Gao, S. The effect of seasonal temperature difference on estimated wood density in Populus ussuriensis Kom. trees by the resistance drilling method. Wood Mater. Sci. Eng. 2026, 21, 253–264. [Google Scholar] [CrossRef] [Scilit]
- Sharapov, E.; Brischke, C.; Militz, H.; Smirnova, E. Combined effect of wood moisture content, drill bit rotational speed and feed rate on drilling resistance measurements in Norway spruce (Picea abies (L.) Karst.). Wood Mater. Sci. Eng. 2020, 15, 198–204. [Google Scholar] [CrossRef] [Scilit]
- Sharapov, E.; Brischke, C.; Militz, H. Effect of Grain Direction on Drilling Resistance Measurements in Wood. Int. J. Archit. Herit. 2021, 15, 250–258. [Google Scholar] [CrossRef] [Scilit]
- Bobadilla Maldonado, I.; Martínez, R.D.; Taboada de la Fuente, C.; Llana, D.F. In Situ Density Estimation of Structural Timber Using Drilling Chips Extraction (Woodex+): Validation and Sustainability Contribution. Sustainability 2026, 18, 1683. [Google Scholar] [CrossRef] [Scilit]
- Jaskowska-Lemańska, J. Metodyka Określania Właściwości Fizyko-Mechanicznych Drewna w Istniejących Konstrukcjach na Podstawie Badań Semi-Nieniszczących. Doctoral Dissertation, AGH University of Science and Technology, Kraków, Poland, 2022. [Google Scholar]
- Jaskowska-Lemańska, J.; Wałach, D. Assessment of the Technical Condition of Timber Structural Elements Using Sclerometric Tests. Materials 2023, 16, 6152. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Jaskowska-Lemańska, J.; Przesmycka, E. Semi-Destructive and Non-Destructive Tests of Timber Structure of Various Moisture Contents. Materials 2021, 14, 96. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Starzyk, A.; Marchwiński, J.; Milošević, V. Circular Wood Construction in a Sustainable Built Environment: A Thematic Review of Gaps and Emerging Topics. Sustainability 2025, 17, 7333. [Google Scholar] [CrossRef] [Scilit]
- Huber, J.A.J.; Svilans, T.; Kauniste, M.; Vonk, N.H.; Broman, O.; Tuhkanen, E.; Wuyts, W.; Just, A.; Tamke, M.; Thomsen, M.R. Comparative evaluation of non-destructive and CT-derived indicators for stiffness assessment of reclaimed Norway spruce timber. Eur. J. Wood Wood Prod. 2026, 84, 81. [Google Scholar] [CrossRef] [Scilit]
- EN 408:2004; Timber Structures—Structural Timber and Glued Laminated Timber—Determination of Some Physical and Mechanical Properties. CEN: Brussels, Belgium, 2004.
- PN-D-04103:1977; Wood—Determination of Static Bending Strength. Polish Committee for Standardization: Warsaw, Poland, 1977.
- PN-D-04102:1979; Wood—Determination of Compressive Strength Parallel to the Grain. Polish Committee for Standardization: Warsaw, Poland, 1979.
- EN 384:2004; Structural Timber—Determination of Characteristic Values of Mechanical Properties and Density. CEN: Brussels, Belgium, 2004.
- Roberts, D.R.; Bahn, V.; Ciuti, S.; Boyce, M.S.; Elith, J.; Guillera-Arroita, G.; Hauenstein, S.; Lahoz-Monfort, J.J.; Schröder, B.; Thuiller, W.; et al. Cross-validation strategies for data with temporal, spatial, hierarchical, or phylogenetic structure. Ecography 2017, 40, 913–929. [Google Scholar] [CrossRef] [Scilit]
- Brunetti, M.; Aminti, G.; Vicario, M.; Nocetti, M. Density Estimation by Drilling Resistance Technique to Determine the Dynamic Modulus of Elasticity of Wooden Members in Historic Structures. Forests 2023, 14, 1107. [Google Scholar] [CrossRef] [Scilit]
- Gendvilas, V.; Lee, D.J.; Kain, D.P.; Kumar, C.; Downes, G.M.; Lausberg, M.; Harrington, J.J. Predicting Wood Density Using Resistance Drilling: The Effect of Instrument and Operator. Forests 2024, 15, 157. [Google Scholar] [CrossRef] [Scilit]
- Gendvilas, V.; Lee, D.J.; Downes, G.M.; Lausberg, M.; Harrington, J.J. Resistance drilling: The effect of needle wear. Eur. J. Wood Wood Prod. 2025, 83, 181. [Google Scholar] [CrossRef] [Scilit]
- Gendvilas, V.; Downes, G.M.; Neyland, M.; Hunt, M.; Jacobs, A.; O’Reilly-Wapstra, J. Friction correction when predicting wood basic density using drilling resistance. Holzforschung 2021, 75, 508–516. [Google Scholar] [CrossRef] [Scilit]
- Morales-Conde, M.J.; Rodríguez-Liñán, C.; Saporiti-Machado, J. Predicting the density of structural timber members in service. The combine use of wood cores and drill resistance data. Mater. Constr. 2014, 64, e029. [Google Scholar] [CrossRef] [Scilit]
- Todoroki, C.L.; Lowell, E.C.; Filipescu, C.N. Wood density estimates of standing trees by micro-drilling and other non-destructive measures. N. Z. J. For. Sci. 2021, 51, 6. [Google Scholar] [CrossRef] [Scilit]
- Sharapov, E.; Korolev, A.; Demakov, Y. The effect of temperature and moisture content on drilling resistance measurements in wood (Pinus sylvestris L.). Wood Mater. Sci. Eng. 2025, 20, 564–570. [Google Scholar] [CrossRef] [Scilit]
- Sharapov, E.; Korolev, A.; Shlychkov, S.; Mascia, N.T. Effect of drilling resistance measurement on residual load capacity of Scots pine (Pinus sylvestris L.). Eur. J. Wood Wood Prod. 2024, 82, 473–481. [Google Scholar] [CrossRef] [Scilit]
- Vössing, K.J.; Niederleithinger, E. Nondestructive assessment and imaging methods for internal inspection of timber. A review. Holzforschung 2018, 72, 467–476. [Google Scholar] [CrossRef] [Scilit]
- Kurz, J.H.; Boller, C. Some background of monitoring and NDT also useful for timber structures. J. Civ. Struct. Health Monit. 2015, 5, 99–106. [Google Scholar] [CrossRef] [Scilit]
- Kahl, T.; Wirth, C.; Mund, M.; Böhnisch, G.; Schulze, E.-D. Using drill resistance to quantify the density in coarse woody debris of Norway spruce. Eur. J. For. Res. 2009, 128, 467–473. [Google Scholar] [CrossRef] [Scilit]
- Mirra, M.; Pagella, G.; Lee, M.; Gard, W.; Ravenshorst, G.; van de Kuilen, J.-W. Characterisation of bacterial decay effects on wooden foundation piles across various historical periods. Constr. Build. Mater. 2024, 421, 135670. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |