Skip to Content
MaterialsMaterials
  • Article
  • Open Access

27 November 2026

25 Pages

Inverse Analysis-Based Mesoscale Modeling and Microstructural Optimization of Silica Fume-Modified Asphalt Concrete

,
,
and
1
National Science Center for Earthquake Engineering, Tianjin University, Tianjin 300350, China
2
School of Civil Engineering, Tianjin University, Tianjin 300350, China
3
Key Laboratory of Earthquake Engineering Simulation and Seismic Resilience of China Earthquake Administration, Tianjin University, Tianjin 300350, China
*
Authors to whom correspondence should be addressed.

Abstract

Silica fume modification offers a potential route to improving the crack resistance of asphalt concrete used as a flexible impermeable material in earth-rock dams. However, the mechanisms linking mesoscale structure to flexural behavior remain insufficiently quantified. This study presents an integrated experimental–numerical framework combining quasi-static three-point bending tests, computed tomography (CT)-based image analysis, inverse identification of constitutive parameters, and finite element simulations. Specimens with varying silica fume contents were tested to characterize their flexural response and identify a suitable composition for mesoscale calibration. A three-phase model representing aggregates, asphalt mortar, and the interfacial transition zone was then employed to examine the effects of aggregate size, shape, content, spatial arrangement, and interfacial thickness. The results show that silica fume modification can improve flexural performance within the investigated range and that mesoscale structural characteristics significantly affect strength and cracking behavior. The proposed framework provides a basis for microstructure-informed design of hydraulic asphalt concrete.

1. Introduction

Earth rock dams have become the predominant dam type in modern hydraulic engineering due to their strong adaptability to site conditions [1], efficient utilization of locally available materials [2], construction flexibility [3], and overall cost effectiveness [4]. With the continuous expansion of project scale and the increasing complexity of operating environments, the importance of dam safety and long term durability has become increasingly prominent [5,6,7]. Although some mitigation measures have been adopted in certain practical projects, the inherent brittleness of the material has never been fundamentally resolved.
Asphalt concrete provides a promising technical solution for flexible impermeable panels owing to its viscoelastic behavior and self healing capacity [8,9]. Successful engineering applications, including the Foz do Areia Dam [10,11,12] in Brazil and the Jilintai Reservoir Dam [13,14,15] in Xinjiang, have demonstrated the excellent adaptability of asphalt panels under conditions of thermal cycling and foundation deformation. However, conventional asphalt concrete panels still exhibit several critical limitations, including relatively low tensile strength [16], inadequate high temperature stability [17,18], increased brittleness due to ultraviolet aging [19], and an insufficient understanding of their dynamic response under seismic cyclic loading [20]. These deficiencies restrict their broader application in high intensity seismic regions and in ultra high dam projects. The addition of mineral admixtures provides an effective approach to overcoming the performance limitations of traditional asphalt concrete in hydraulic engineering applications [21,22,23]. Among them, silica fume is considered a promising modifier due to its extremely high specific surface area, nanoscale particle size, and strong physicochemical interactions with asphalt components [24,25,26]. Compared with conventional fillers such as limestone powder and fly ash, silica fume exhibits superior capability in microstructural optimization and interfacial enhancement [27]. Incorporation of ultrafine silica fume particles forms a denser internal structure, improving the integrity of the asphalt–aggregate interfacial transition zone through micro-pore filling and interface reinforcement, thereby enhancing the impermeability, durability, and mechanical strength of asphalt concrete [28].
Luo et al. [29] and Zheng and Shi [30] demonstrated that incorporating 5–15% silica fume substantially enhances the high-temperature performance, complex modulus, and performance grade of asphalt while maintaining low-temperature crack resistance. Miller et al. [31] and Liu et al. [32] reported that silica fume preferentially accumulates at the aggregate–binder interface, where its high specific surface area facilitates adsorption of polar molecules, thereby strengthening interfacial bonding. Chen et al. [33] further confirmed through simulations that the interfacial adhesion energy is significantly higher than that of conventional limestone filler. Mohammed et al. [34] observed that silica fume increases Marshall stability, indirect tensile strength, and TSR. Cheraghian et al. [35] and Mazloom et al. [36] found that silica fume enhances fracture energy, critical strain energy release rate, and fatigue performance, owing to improved binder properties and interfacial bonding. Mizan et al. [37], Song et al. [38], and Li et al. [39] reported that silica fume significantly improves TSR, surface free energy, and residual strength after freeze–thaw cycling. Bahmani et al. [40] found that silica fume mitigates aging effects by suppressing oxidation reactions and reducing stiffness growth. Finally, Cui et al. [41] and Zhang et al. [42] demonstrated that under hydrocyclic loading and hydraulic action, silica fume-modified mixtures exhibit improved impermeability and erosion resistance compared with unmodified mixtures. Recent advances in mesoscale numerical modeling have provided new insights into the relationship between the internal structure and mechanical performance of asphalt mixtures. Yang et al. [43] investigated cracking behavior and construction-related deficiencies using a three-phase micromechanical finite element model. Li et al. [44] integrated X-ray computed tomography (CT) with the discrete element method to characterize mesoscale fracture behavior under indirect tensile loading. Similarly, Liang et al. [45] examined the influence of aggregate skeleton characteristics on the mechanical response of asphalt mixtures using CT-based mesoscale modeling. These studies demonstrate the importance of microstructural heterogeneity in governing the mechanical behavior of asphalt materials. However, the relationships among silica fume modification, CT-derived mesoscale characteristics, and flexural performance in hydraulic asphalt concrete require further investigation.
To address this research gap, the present study develops an integrated experimental–numerical framework combining silica fume modification, three-point bending tests, CT-based microstructural reconstruction, and inverse finite element analysis. First, three-point bending tests were performed on asphalt concrete specimens with varying silica fume contents. Combined with crack-tracking techniques based on digital image processing, these tests accurately captured the actual failure modes and load–displacement responses. Second, by integrating microstructural reconstruction from computed tomography imaging with finite element inversion analysis, the parameters of the concrete damage plasticity model were calibrated, enabling precise characterization of the damage evolution process. Building on these results, the influence of five critical microstructural design variables—aggregate gradation, aggregate shape, aggregate volume fraction, spatial distribution, and thickness of the interface transition zone—on macroscopic mechanical properties was systematically investigated, and a quantitative predictive model linking microstructural characteristics to macroscopic performance was established. This research provides a robust theoretical foundation and practical guidance for the material design optimization and performance prediction of silica fume-modified asphalt concrete in hydraulic structures.

2. Experimental Program

As a flexible impermeable material for earth-rock dams, asphalt concrete plays an important role in seepage control and deformation compatibility. Silica fume is investigated in this study as a mineral modifier for improving the flexural performance of hydraulic asphalt concrete. However, the relationships among silica fume content, crack resistance, and mesoscale failure mechanisms remain insufficiently understood. This section introduces the constituent materials, mixture design, specimen preparation, quasi-static three-point bending protocol, and experimentally observed flexural responses of asphalt concrete mixtures with different silica fume contents.

2.1. Raw Materials

2.1.1. Asphalt

The asphalt utilised in the experimental study was designated as Karamay No. 90 asphalt. The test indicators were obtained through the execution of the test procedures on the asphalt, as illustrated in Table 1.
Table 1. Karamay No. 90 asphalt test results. Measured values are from laboratory tests.

2.1.2. Mining Materials

(1) Coarse aggregate The testing structures for each parameter are shown in Table 2.
Table 2. Coarse Aggregate Testing Structures for Each Parameter.
(2) Fine aggregate The gradation sieve analysis results for the fine aggregate, along with the results of the other tests, are presented in Table 3.
Table 3. Fine aggregate test results.
(3) Filler The filler used in the experiment (mineral powder) and its corresponding test results are shown in Table 4.
Table 4. Packing Test Results.

2.1.3. Chemical Composition of Aggregates

The chemical composition of the mineral aggregate used in this study is presented in Table 5. The aggregate exhibits a silica-rich mineral composition, with SiO2 accounting for 72.25 wt.%, followed by CaO (6.84 wt.%), Al2O3 (4.95 wt.%), Fe2O3 (3.52 wt.%), and MgO (2.29 wt.%). The loss on ignition (LOI) is 2.17 wt.%.
Table 5. Chemical composition of the mineral aggregate.

2.2. Experimental Protocol Design

2.2.1. Aggregate Gradation and Mixture Design

Aggregate gradation parameters mainly include the maximum aggregate size ( D max ), the gradation index (r) or the coarse-to-fine aggregate ratio, and the mineral filler content (F). In this study, the aggregate gradation was determined based on the maximum density gradation theory. The gradation curve was calculated using the empirical relationship recommended in the Design Specification for Asphalt Concrete Pavements and Core Walls of Earth-Rock Dams [46]:
P i = F + ( 100 − F ) d i r − d 0.075 r D max r − d 0.075 r
where P i is the cumulative passing percentage corresponding to sieve size d i ; F is the mineral filler content with a particle size smaller than 0.075 mm (%); D max is the maximum aggregate size (mm); d i is the specified sieve size (mm); d 0.075 is the filler boundary particle size (0.075 mm); and r is the gradation index.
The reference mixture proportions were established from a systematic experimental mixture-selection program for hydraulic asphalt concrete conducted for the Pazi Water Conservancy Project [47]. The experimental program investigated the effects of aggregate gradation, mineral filler content, and asphalt-to-aggregate mass ratio on mixture compactness, tensile resistance, and deformation capacity.
A total of 25 candidate mixtures were designed using a maximum aggregate size of 19 mm. The investigated gradation indices were 0.36, 0.39, and 0.42, while the mineral filler contents were 11%, 13%, and 15%. Four asphalt-to-aggregate mass ratios of 6.3%, 6.6%, 6.9%, and 7.2% were considered. The 25 mixtures comprised selected combinations of these design variables. The asphalt-to-aggregate ratio was calculated as the mass of asphalt binder relative to the total mass of mineral aggregate, including mineral filler.

2.2.2. Mixture Screening and Splitting Test Results

The preliminary mixture-screening program consisted of porosity measurements and indirect tensile (splitting) tests. The porosity was determined using standard Marshall specimens to characterize mixture compactness and impermeability-related properties. The splitting tests were performed at 7.0 °C under displacement-controlled loading at a rate of 1 mm/min. Three specimens were tested for each mixture, and the average experimental values were used for subsequent analysis.
The splitting strength was determined from the maximum applied load, whereas the splitting displacement represented the deformation capacity of the specimen during indirect tensile loading. The experimental results for all 25 candidate mixtures are summarized in Table 6.
Table 6. Mixture-design parameters and experimental screening results for 25 hydraulic asphalt concrete mixtures.
The influence of asphalt content was evaluated by comparing mixtures with a constant gradation index of 0.39 and mineral filler content of 13%. As the asphalt-to-aggregate ratio increased from 6.3% to 6.6%, the splitting strength increased from 0.789 to 0.877 MPa. A further increase to 6.9% and 7.2% resulted in splitting strengths of 0.810 and 0.771 MPa, respectively.
The corresponding splitting displacements were 4.350, 4.150, 4.200, and 4.350 mm, while the porosity decreased from 1.285% to 0.768% over the investigated asphalt-content range. These results indicate that asphalt content strongly influences the balance between mixture compactness, tensile resistance, and deformation capacity. An asphalt-to-aggregate ratio of 6.9% provided a favorable combination of these properties for the subsequent engineering performance assessment.
The influence of mineral filler content was investigated using a gradation index of 0.39 and an asphalt-to-aggregate ratio of 6.9%. For filler contents of 11%, 13%, and 15%, the measured splitting strengths were 0.874, 0.810, and 0.796 MPa, respectively.
The corresponding splitting displacements were 4.433, 4.200, and 4.650 mm, while the porosities were 1.229%, 1.240%, and 0.821%, respectively. Increasing the filler content modified both the tensile resistance and the deformation characteristics of the asphalt concrete. A filler content of 13% was selected as part of the reference mixture composition based on the overall engineering performance requirements.
The effect of aggregate gradation was analyzed at a constant filler content of 13% and an asphalt-to-aggregate ratio of 6.9%. The splitting strengths corresponding to gradation indices of 0.36, 0.39, and 0.42 were 0.731, 0.810, and 0.631 MPa, respectively.
The gradation index of 0.39 produced the highest splitting strength within this series. The corresponding splitting displacement was 4.200 mm, compared with 4.683 mm and 4.733 mm for gradation indices of 0.36 and 0.42, respectively. The results indicate that the intermediate gradation index increased tensile resistance while maintaining moderate deformation under the investigated conditions.
Based on the comprehensive evaluation of the experimental results, Mix No. 13 was identified as the preferred reference composition for hydraulic asphalt concrete. This mixture combined a maximum aggregate size of 19 mm, a gradation index of 0.39, a mineral filler content of 13%, and an asphalt-to-aggregate ratio of 6.9%.
In the preliminary splitting tests, Mix No. 13 exhibited a splitting strength of 0.810 MPa, a splitting displacement of 4.200 mm, and a porosity of 1.240%. Further mechanical tests showed a compressive strength of 4.283 MPa, a tensile strength of 1.407 MPa, and a flexural strength of 1.477 MPa.
The corresponding peak compressive strain was 6.661%, while the peak tensile strain and flexural strain reached 1.732% and 3.340%, respectively. The Marshall stability was 9.975 kN, and the Marshall porosity was 0.995%. The water stability coefficient reached 0.956, while the permeability coefficient was 3.117 × 10 − 9 cm/s.
The static triaxial tests provided a modulus number of 415.6, a modulus exponent of 0.287, an internal friction angle of 28.5°, a cohesion of 0.51 MPa, and a failure ratio of 0.695. The corresponding experimental results are summarized in Table 7.
Table 7. Comprehensive mechanical and hydraulic properties of the selected reference mixture (Mix No. 13).

2.2.3. Reference Mixture and Silica Fume Modification Program

The comprehensive experimental program established Mix No. 13 as the preferred reference composition, providing a combination of tensile and compressive resistance, deformation capacity, water stability, and low permeability suitable for hydraulic asphalt concrete. The corresponding mixture-design parameters are summarized in Table 8.
Table 8. Mixture-design parameters of the selected reference composition.
The corresponding aggregate gradation was calculated using Equation (1). The cumulative passing percentages are presented in Table 9.
Table 9. Aggregate gradation parameters of the selected reference mixture.
The present silica-fume modification study adopted the selected reference aggregate gradation and mixture proportions using Karamay No. 90 asphalt.
Five nominal silica-fume contents of 0%, 5%, 10%, 15%, and 20% were investigated. Three-point bending experiments were performed to characterize the effects of silica fume incorporation on flexural strength, deformation capacity, and fracture behavior. The experimental results were subsequently used to identify a representative composition for CT-based mesoscale reconstruction and inverse constitutive parameter calibration.

2.3. Three-Point Bending Test

The three-point bending test was employed to evaluate the flexural behavior of asphalt concrete under controlled loading conditions. This method allows the characterization of flexural strength, deformation capacity, and cracking behavior, providing experimental evidence for the calibration and assessment of the mesoscale numerical model. As shown in Figure 1, the three-point bending test was performed using a universal testing machine (UTM) equipped with a temperature-controlled environmental chamber. The testing equipment was provided by POWERCHINA Beijing Engineering Corporation Limited (Beijing, China). Figure 2 shows a comparison of the specimen before and after the three-point bending test.
Figure 1. Experimental setup for the three-point bending test.
Figure 2. Comparison of the specimen before and after the test: (a) Specimen before the test; (b) specimen after the test.
As the primary impermeable component of an earth-rock dam, the asphalt concrete core wall is subjected to sustained hydraulic pressure and self-weight stress throughout its service life, while simultaneously experiencing seasonal temperature variations. In cold seasons, reduced temperatures markedly decrease the ductility of asphalt materials and accentuate their brittle behavior, thereby increasing susceptibility to cracking. Therefore, evaluating crack resistance under low-temperature conditions is essential for ensuring the long-term safety and durability of the dam structure.
In this study, the test temperature was set at 7.0 °C. This value was determined based on multi-year meteorological records of the project region and corresponds to the average winter temperature, thereby representing typical in-service low-temperature conditions encountered by the dam. The selection of this temperature ensures both engineering relevance and a realistic assessment of the material’s low-temperature mechanical performance. The experiments were conducted under quasi-static, displacement-controlled monotonic loading at a constant rate of 1.67 mm/min, corresponding to a nominal mid-span strain rate of 1%/min. No dynamic or cyclic loading was applied. During testing, the applied load and mid-span deflection were continuously monitored using a load cell and linear variable differential transformer (LVDT), respectively, with a data acquisition frequency of 10 Hz. This configuration ensured accurate capture of the complete load–deflection response, including the post-peak softening stage.
Flexural strength, flexural strain, and the deflection–span ratio were calculated in accordance with Equations (2)–(4):
R B = 3 P L 2 b h 2
ε = 6 h f L 2
W b = f L × 100 %
where R B denotes the flexural strength (MPa); P is the peak load (N); L represents the span length (mm); b and h are the specimen width and height (mm), respectively; ε is the maximum flexural strain; f corresponds to the mid-span deflection at peak load (mm); and W b is the deflection–span ratio (%).
Fracture energy, defined as the total energy required to create a unit crack surface area, was determined from the area under the complete load–deflection curve up to failure, as expressed in Equation (5):
G f = W f A lig
where G f is the fracture energy (N/mm or J/m2); W f denotes the fracture work obtained by numerically integrating the load–deflection curve using the trapezoidal rule (N·mm); and A lig is the ligament area (mm2), calculated as A lig = b ( h − a 0 ) , with  a 0 representing the initial notch depth (mm). For unnotched specimens, a 0 = 0 , and thus A lig = b h .

2.4. Test Results

The failure characteristics of the specimens during the flexural test are shown in Figure 2. Before loading, the specimens remained intact, whereas after the test, a visible crack developed at the mid-span section, indicating typical flexural failure behavior.
The flexural strength test results of specimens with varying silica fume contents are presented in Table 10. The detailed test results are presented in Figure 3.
Table 10. Flexural Test Results with Different Silica Fume Contents.
Figure 3. Experimental results of three-point bending tests at different silica fume contents: (a) Stress–strain curves; (b) Flexural strength.
As shown in Figure 3b, the flexural strength of asphalt concrete initially increased with silica fume content, reaching a maximum mean value of 4.010 MPa at 10%, followed by a gradual decrease at higher dosages. The 15% mixture exhibited a comparable mean flexural strength of 3.937 MPa. The corresponding statistical results, including the mean values, standard deviations, and 95% confidence intervals, are summarized in Table 11.
Table 11. Statistical analysis of flexural strength for different silica fume contents.
One-way analysis of variance (ANOVA) revealed significant differences in flexural strength among the investigated mixtures ( F 4 , 10 = 8.375 , p = 0.0031 ), while Tukey’s post-hoc test indicated no significant difference between the 10% and 15% groups ( p = 0.9895 ).
The corresponding variations in flexural strain and modulus further demonstrate the influence of silica fume incorporation on the mechanical response of asphalt concrete. Overall, the mixtures containing 10–15% silica fume exhibited favorable flexural performance under the investigated experimental conditions.

3. Numerical Modeling

3.1. Image Processing

High-resolution CT imaging was used to reconstruct the asphalt concrete microstructure. The original image (1048 × 163 pixels) was cropped to 944 × 147 pixels to remove boundary artifacts. Noise reduction and contrast enhancement were performed using median filtering, adaptive histogram equalization, and Gaussian smoothing. Phase segmentation was achieved via Otsu thresholding followed by morphological processing, resulting in the removal of small regions and refinement of phase boundaries. The final three-phase digital model shows volume fractions of 48.60% aggregate, 19.25% interface transition zone, and 32.15% mortar matrix, providing a reliable geometric basis for finite element modeling (Figure 4).
Figure 4. Image Processing Workflow from Original to Digital Model.

3.2. Finite Element Mesh Generation

The CT-derived microstructure was discretized using a two-dimensional (2D) structured finite element mesh. To maintain spatial consistency between the segmented image and the numerical model, each pixel of the cropped 944 × 147 -pixel image was mapped to a four-node quadrilateral element, resulting in a mesh comprising 138,768 elements and 139,860 nodes, as illustrated in Figure 5. The nominal in-plane element size was approximately 0.1 mm.
Figure 5. Three-phase asphalt concrete microstructure and finite element discretization: (a) Three-phase microstructure showing aggregate (light gray), ITZ (green), and mortar (dark gray); (b) Finite element mesh of the asphalt concrete sample.
The ITZ was represented by a three-pixel-wide interfacial band surrounding the segmented aggregate boundaries, with its thickness treated as a prescribed geometric parameter.
Material properties were assigned to the aggregate and asphalt mortar regions according to the segmented phase distribution, whereas the interfacial transition zone (ITZ) was represented by an idealized three-pixel-wide layer surrounding the aggregate boundaries. The structured quadrilateral discretization was adopted to preserve the correspondence between image pixels and finite element material regions, thereby avoiding additional geometric reconstruction and remeshing procedures. Although triangular elements offer greater flexibility in representing irregular geometries, the adopted pixel-based quadrilateral mesh provides a straightforward and reproducible approach for incorporating the heterogeneous microstructure into the numerical model.
The two-dimensional representation enables the analysis of in-plane material heterogeneity and localized damage under flexural loading. Nevertheless, it does not account for out-of-plane aggregate connectivity or three-dimensional crack propagation, and the predicted response of thin interfacial regions may be sensitive to the adopted mesh resolution.

3.3. Material Parameter Identification

The mechanical parameters of the three-phase model require systematic calibration to ensure predictive accuracy. The experimental dataset from Table 10 (10% silica fume specimen) served as the primary calibration target, representing the baseline composition for parametric studies. Key benchmark values include:
  • Flexural strength: σ f exp = 4.01 MPa
  • Flexural modulus: E f exp = 96.30 MPa
  • Maximum bending strain: ε max = 3.83 %
An inverse analysis procedure was employed to calibrate material parameters based on the experimental load–displacement curve. The objective function minimized the squared difference between numerical and experimental responses:
f ( p ) = ∑ i = 1 n F i exp − F i sim ( p ) 2
where p represents the parameter vector, and  F i exp and F i sim denote the experimental and simulated loads at the i-th displacement increment, respectively. The material parameters were identified by minimizing the least-squares objective function defined in Equation (6).
The calibrated material parameters are summarized in Table 12. Elastic properties, including Young’s modulus (E) and Poisson’s ratio ( ν ), were assigned for the aggregate, ITZ, and mortar phases based on literature values and microindentation tests. The aggregate phase was modeled as linearly elastic due to its significantly higher stiffness compared to the asphalt mortar. Composite-level CDP parameters, including dilation angle ( ψ ), eccentricity ( ε ), and the ratio of biaxial to uniaxial compressive strength ( f b 0 / f c 0 ), were computed using the PolarisCDP plugin to capture the nonlinear damage evolution under bending. These parameters enable accurate simulation of progressive cracking and post-peak softening behavior observed in the experiments.
Table 12. Calibrated material parameters for three-phase asphalt concrete model.
The concrete damaged plasticity (CDP) model was adopted to characterize the nonlinear deformation and progressive damage of asphalt concrete under monotonic quasi-static loading. Its damage–plasticity formulation provides a constitutive representation of irreversible deformation, stiffness degradation, and post-peak softening. Previous studies have investigated mesoscale damage mechanisms in asphalt materials [48], while Zhou et al. [49] applied the CDP formulation to analyze damage evolution in cement–asphalt mortar. Furthermore, Londono et al. [50] developed a temperature-dependent viscoelastic damage model to characterize the time-dependent mechanical behavior of asphalt concrete. Within the present experimental framework, the calibrated CDP formulation was employed to represent the flexural response and damage evolution under the prescribed loading conditions.

3.4. Model Calibration and Experimental Comparison

The three-phase mesoscale model was calibrated through inverse analysis using the experimental load–displacement response of asphalt concrete containing 10% silica fume. The calibrated model successfully reproduced the principal flexural characteristics observed in the experiments. The simulated peak load and corresponding displacement were 816.31 N and 5.87 mm, respectively, compared with the experimental values of 822.51 N and 5.91 mm. The calculated flexural strength and modulus reached 3.83 MPa and 91.30 MPa, showing close agreement with the experimental values of 4.01 MPa and 95.78 MPa. Furthermore, the simulated damage distribution and crack localization were consistent with the experimentally observed flexural failure characteristics. These results demonstrate the effectiveness of the inverse parameter identification procedure in reproducing the mechanical response and damage evolution of the investigated asphalt concrete.

3.4.1. Quantitative Assessment of Calibration Agreement

Figure 6 compares the experimental and simulated load–displacement responses of the specimen containing 10% silica fume. The numerical simulation predicts a peak load of 816.31 N at a mid-span displacement of 5.87 mm, compared with the experimental reference values of 822.51 N and 5.91 mm.
Figure 6. Comparison between Physical Experiment and Numerical Simulation.
The corresponding relative errors in peak load and peak displacement are 0.75% and 0.68%, respectively, indicating good agreement in the predicted peak response.
The simulated flexural strength is calculated as:
σ f sim = 3 P L 2 b h 2 = 3 × 816.31 × 200 2 × 40 × 40 2 = 3.83 MPa
This shows reasonable agreement with the experimental average of 4.01 MPa, yielding a relative error of 4.58%. The initial slope of the simulated curve corresponds to a flexural modulus of E f sim = 91.3 MPa, closely matching the experimental value of 95.78 MPa (error = 4.68%).
Table 13 summarizes the quantitative validation metrics:
Table 13. Quantitative validation metrics for the 10% silica fume specimen.
Overall, the numerical simulation results show good agreement with the experimental data, confirming the validity of the calibrated material parameters. The slight underestimation of peak load and stiffness can be attributed to the following factors: first, the idealized boundary conditions used in the numerical model differ from those of the actual test setup and loading conditions; second, the simulation did not account for the strain rate effect at the loading point; and third, the microstructural refinement effect caused by a 10% silica fume content is difficult to fully capture in a mesoscale model using homogenized mortar parameters.

3.4.2. Comparison of Failure Morphology

Figure 7 shows the failure modes. The numerical model successfully reproduces the experimentally observed crack propagation patterns, including aggregate debonding and matrix cracking, validating the mesoscale damage mechanisms.
Figure 7. Failure behavior of composites under three-point bending: experimental and numerical comparison (a) Experimental failure morphology; (b) Mesoscale crack evolution in numerical simulation.
Key observations include:
  • Primary crack initiation: Both experimental and numerical results show crack nucleation at the bottom surface directly beneath the loading point, where tensile stress concentration is maximum. In the simulation, damage initiates in the mortar phase at approximately 90% of peak load.
  • Crack path tortuosity: The simulated crack propagates vertically through the mortar matrix while deflecting around aggregates, consistent with physical observations. This demonstrates that the mesoscale model correctly captures stress redistribution mechanisms due to material heterogeneity.
  • ITZ debonding: Secondary cracks form along aggregate-ITZ interfaces, particularly for large aggregates near the fracture process zone. The numerical results reveal localized interfacial damage near the aggregate–mortar boundaries, indicating the influence of mesoscale heterogeneity on crack propagation and damage evolution.
  • Post-peak behavior: The experimental load–displacement curve exhibits gradual softening after peak load, indicating progressive damage accumulation. The CDP model successfully replicates this behavior through strain-softening evolution laws, avoiding the brittle snap-back instabilities often seen in elastic–brittle models.
Figure 7 presents the DAMAGET contour plot at peak load, showing that damage is primarily concentrated in a narrow band (width ≈ 2–3 mm) spanning the specimen height. This localized damage zone is consistent with the thin fracture surface observed in failed specimens.
After undergoing the two validation methods described above, it was found that the model can not only accurately predict the overall mechanical response but also reasonably characterize local damage mechanisms. The relative calibration discrepancy was 4.58%, which falls within the engineering tolerance range, indicating that the inversion calibration method possesses good robustness. The slightly higher error compared to the ideal prediction may stem from the inherent limitations of the mesoscale homogenization method: when the silica fume content reaches 10%, the mortar matrix exhibits effects such as refined pore structure at the nanoscale and enhanced bonding at the aggregate–mortar interface.

3.4.3. Comparison with Published Mesoscale Studies

Previous mesoscale investigations have highlighted the critical role of microstructural heterogeneity and aggregate–binder interactions in governing the mechanical response and damage evolution of asphalt materials. Sadd et al. [51] investigated the influence of aggregate–binder interactions on nonlinear mechanical behavior, while Dai et al. [48] demonstrated the relationship between microstructural heterogeneity and localized damage evolution using image-based finite element modeling. Similarly, Li et al. [44] examined interfacial cracking and fracture propagation through CT-based mesoscale simulations. In the present study, damage was predominantly concentrated in the tensile region beneath the loading point, with crack propagation governed by aggregate distribution and interfacial characteristics. The observed damage localization, crack deflection, and interfacial debonding are consistent with the fracture mechanisms reported in previous studies, further highlighting the influence of mesoscale heterogeneity on the flexural failure of asphalt concrete.

4. Parametric Study

A series of parametric simulations was conducted to investigate the effects of aggregate size, shape, volume fraction, spatial arrangement, and ITZ thickness on the flexural performance of asphalt concrete. Each parameter was varied independently while the remaining conditions were maintained constant. The resulting comparisons provide quantitative insights into the influence of individual mesoscale structural characteristics on flexural behavior.

4.1. Aggregate Gradation

The particle size distribution of aggregates is a key microstructural parameter that significantly affects the flexural performance of asphalt concrete. This study systematically investigates how different maximum aggregate sizes influence the mechanical behavior of the material. While maintaining a constant aggregate volume fraction of 48.6 percent and an interfacial transition zone thickness of 0.3 millimeters, microstructural models with varying maximum particle sizes were established, as summarized in Table 14.
Table 14. Mechanical Performance under Different Maximum Particle Sizes.
The corresponding load–displacement curves are illustrated in Figure 8.
Figure 8. Relationship between aggregate gradation and flexural strength.
The results indicate that aggregate size significantly influences both strength and energy dissipation through different micromechanical mechanisms. Smaller aggregates produce a more uniformly distributed stress field in the mortar matrix, causing cracks to propagate in a tortuous path as they repeatedly deflect at aggregate–mortar interfaces instead of directly penetrating the weaker ITZ. This mechanism increases fracture surface area and energy consumption during failure. The optimal performance at 9.5 mm results from an appropriate aggregate spacing that promotes crack bridging and deflection without excessively increasing the ITZ volume. In contrast, larger aggregates such as 19.2 mm generate localized stress concentrations due to stiffness mismatch with the mortar, which promotes crack initiation along weak ITZ regions. Meanwhile, excessively fine aggregates increase the total ITZ area, creating numerous potential failure planes that reduce both strength and fracture resistance.

4.2. Aggregate Shape

As a key aspect of microgeometric characteristics, aggregate shape directly governs stress transfer pathways and crack propagation patterns within materials. In this study, microstructural models representing three typical aggregate shapes, circular, elliptical and prismatic, were developed while keeping the maximum aggregate size, aggregate volume fraction and ITZ thickness constant. The mechanisms by which aggregate shape affects the mechanical response of asphalt concrete were then systematically analyzed, as documented in Table 15.
Table 15. Mechanical Properties under Different Aggregate Shapes.
Figure 9 presents the comparative mechanical response across different aggregate morphologies.
Figure 9. Relationship between different aggregate shapes and flexural strength.
The performance differences among aggregate geometries mainly arise from variations in local stress concentration and crack–particle interaction mechanisms. Circular and vertically oriented elliptical aggregates perform better because their smooth curvature allows gradual stress redistribution along the interface, reducing stress discontinuities that may cause premature ITZ debonding. When cracks encounter these rounded particles, the crack path tends to deflect around the particle boundary, lowering the stress intensity at the crack tip and requiring additional energy for further propagation, thereby improving fracture toughness. The vertical ellipse is particularly effective because its major axis aligns with the tensile stress direction, forming a longer obstacle that increases crack propagation resistance. In contrast, hexagonal aggregates generate strong stress concentrations at their sharp corners, which can exceed the tensile strength of the ITZ and promote early crack initiation and rapid failure. The horizontally oriented ellipse performs worse because its major axis perpendicular to the tensile stress forms a preferential path for crack propagation, reducing load-bearing capacity.

4.3. Aggregate Volume Fraction

The aggregate volume fraction is a key parameter controlling the macroscopic mechanical behavior of asphalt concrete, with variations directly affecting the material’s stiffness, strength, and failure mechanisms. This study systematically examined seven levels of aggregate volume fraction ranging from 30 percent to 60 percent. While keeping the aggregate particle size distribution, aggregate shape, and interfacial transition zone thickness constant, the influence of volume fraction on the flexural performance of asphalt concrete was analyzed, as presented in Table 16.
Table 16. Mechanical Properties under Different Aggregate Volume Fractions.
The mechanical response trends are depicted in Figure 10.
Figure 10. Effect of aggregate volume fraction on peak load capacity.
The non-monotonic relationship between aggregate content and mechanical performance arises from competing microstructural mechanisms at different volume fractions. At low contents, the composite remains matrix-controlled, where the mortar phase dominates deformation and failure, leading to lower stiffness and inefficient load transfer to aggregates. As the content increases to 45–50%, a connected aggregate skeleton forms, enabling effective particle-to-particle load transfer while maintaining sufficient mortar to accommodate deformation and prevent interfacial debonding. The optimal performance at 50% represents a balance between the rigid aggregate framework and the ductile mortar matrix. However, further increasing the aggregate content produces negative effects. Reduced spacing between aggregates restricts mortar deformation and induces stress concentration, while the increased ITZ area introduces more weak interfaces that promote brittle interfacial cracking. At 60%, this ITZ-dominated failure significantly reduces both strength and toughness.

4.4. Aggregate Arrangement

The spatial arrangement of aggregates, as a topological characteristic of the microstructure, plays a critical role in governing stress transfer pathways, local damage evolution, and overall mechanical behavior. In this study, four representative aggregate arrangement patterns were designed for comparative analysis: random distribution, layered arrangement, gradient distribution, and regular arrangement. The random distribution model was used as the baseline, with aggregate center coordinates generated using a Monte Carlo algorithm. The comparative performance metrics are documented in Table 17.
Table 17. Mechanical Properties under Different Aggregate Arrangement Patterns.
Figure 11 illustrates the load-displacement behavior under different spatial configurations.
Figure 11. Comparison of mechanical performance under random and uniform distributions.
The significant performance improvement achieved by the bottom-layered aggregate arrangement demonstrates that spatial heterogeneity in microstructure can be used to resist specific loading conditions. In three-point bending, tensile stress is highest at the bottom fiber and compressive stress dominates at the top, while the neutral axis experiences minimal stress. By concentrating larger and stiffer aggregates in the tensile zone, the bottom-reinforced configuration increases the local modulus where tensile stress is greatest, reducing strain and delaying crack initiation. In addition, the dense aggregate layer forces cracks to repeatedly deflect around high-modulus particles, increasing crack path length and energy dissipation. In contrast, top-reinforced arrangements provide little benefit because strengthening the compression zone does not effectively delay flexural failure. The gradient distribution offers intermediate performance by maintaining reinforcement in the tensile region while avoiding abrupt material transitions. Meanwhile, the regular hexagonal arrangement shows limited strength improvement and lower toughness because its periodic structure forms uniform crack propagation paths that reduce crack deflection.

4.5. ITZ Thickness

The interface transition zone (ITZ), as a micro-weak region connecting aggregates and asphalt mortar, exhibits both thickness and mechanical properties that critically influence crack initiation and propagation. This study systematically examined six ITZ thickness levels ranging from 0.1 millimeters to 0.6 millimeters. While maintaining a constant aggregate volume fraction of 40 percent, random aggregate distribution, and spherical aggregate shape, the effect of ITZ thickness on the flexural performance of asphalt concrete was analyzed. In addition, the coupled influence of ITZ mechanical strength parameters was investigated, as summarized in Table 18.
Table 18. Mechanical Properties under Different ITZ Thicknesses.
The relationship between ITZ thickness and mechanical response is presented in Figure 12.
Figure 12. Effect of prescribed ITZ thickness on the simulated flexural response.
ITZ thickness influences failure behavior by controlling the volume fraction and connectivity of the weakest phase in the composite. A thinner ITZ reduces the proportion of weak interfacial regions, decreasing the likelihood that cracks propagate along interfaces rather than through the stronger mortar matrix. At 0.1 mm, the ITZ volume is minimal, forcing cracks to pass mainly through mortar and resulting in higher fracture energy despite relatively brittle failure. As thickness increases to about 0.3 mm, the larger ITZ volume forms a more continuous weak network around aggregates, shifting the fracture mode from matrix-controlled cracking to interfacial debonding and reducing flexural strength. At intermediate thicknesses (0.4–0.5 mm), fracture energy slightly increases because the thicker and more compliant ITZ can undergo inelastic deformation and distributed microcracking before full separation. However, when the ITZ thickness reaches 0.6 mm, the excessive weak interfacial volume allows cracks to rapidly propagate along aggregate boundaries, leading to reductions in both strength and fracture resistance.

4.6. Potential Applications and Geotechnical Engineering

The experimental–mesoscale framework developed in this study provides a microstructure-informed approach for the optimization of asphalt concrete materials in road and geotechnical engineering. By integrating silica fume modification, three-point bending experiments, CT-based microstructural reconstruction, and inverse finite element analysis, the relationships between material composition, mesoscale heterogeneity, and flexural damage behavior can be systematically investigated.
In road engineering, the proposed framework offers potential applications in asphalt mixture design, low-temperature cracking assessment, and aggregate structure optimization. The experimental results demonstrate that silica fume incorporation influences the flexural strength and deformation capacity of asphalt concrete, with the 10% silica fume mixture exhibiting the highest average flexural strength among the investigated compositions. Furthermore, the numerical investigations reveal the effects of aggregate size, morphology, volume fraction, and spatial distribution on stress concentration, crack initiation, and fracture work. These findings provide useful guidance for optimizing aggregate skeletons and interfacial characteristics to improve the cracking resistance of asphalt pavement materials.
In geotechnical engineering, the proposed approach is particularly relevant to asphalt concrete impervious cores in earth-rock dams and other hydraulic barrier structures. The deformation compatibility, crack resistance, and structural integrity of asphalt concrete are important factors influencing the performance of flexible impervious systems. The present mesoscale analysis demonstrates that aggregate distribution and interfacial transition zone characteristics significantly influence stress redistribution and localized damage evolution. These relationships provide a material-scale basis for evaluating microstructural configurations and identifying damage-sensitive regions in asphalt concrete cores. The identified mechanical characteristics may also support constitutive parameter assessment and subsequent structural-scale analyses of asphalt concrete core rockfill dams.
Overall, the integration of mixture modification, experimental characterization, and mesoscale numerical analysis establishes a systematic connection between material composition, internal structural characteristics, and macroscopic flexural performance. This framework provides useful insights for microstructure-oriented asphalt mixture optimization and damage characterization in transportation infrastructure and hydraulic geotechnical structures.

5. Conclusions

An integrated experimental–numerical framework was developed to investigate the microstructure–property relationships and flexural damage behavior of silica fume-modified asphalt concrete for hydraulic engineering applications. Three-point bending experiments, CT-based microstructural reconstruction, inverse finite element analysis, and parametric investigations were combined to evaluate the effects of silica fume content and mesoscale structural characteristics on mechanical performance. The main conclusions are as follows:
(1) The incorporation of silica fume improved the flexural performance of asphalt concrete. Among the investigated mixtures, the optimal silica fume content was 10%, achieving an average flexural strength of 4.01 MPa, approximately 25.6% higher than that of the unmodified mixture. The maximum flexural strain increased from 3.26% to 3.83%, corresponding to an improvement of 17.5%. Further increasing the silica fume content beyond 10% resulted in a reduction in flexural strength, indicating that excessive incorporation does not necessarily provide additional mechanical benefits.
(2) The CT-based three-phase mesoscale model, comprising aggregates, asphalt mortar, and the interfacial transition zone (ITZ), was calibrated through inverse finite element analysis. The calibrated model predicted a flexural strength of 3.83 MPa, compared with the experimental average of 4.01 MPa, corresponding to a relative error of 4.58%. The simulated failure pattern also showed qualitative consistency with the experimentally observed flexural cracking. These results demonstrate the capability of the calibrated model to represent the principal flexural response of the investigated asphalt concrete.
(3) Aggregate size and volume fraction significantly influenced the simulated flexural performance. Reducing the maximum aggregate size from 16.8 mm to 9.5 mm increased the flexural strength from 3.83 MPa to 4.47 MPa, representing an improvement of 16.77%. In the aggregate volume fraction study, the highest flexural strength of 4.49 MPa was obtained at 50%, corresponding to an increase of 17.39% relative to the 40% baseline. These results indicate that appropriate aggregate size and content can improve the load-bearing capacity of the mesoscale composite.
(4) Aggregate: morphology and spatial arrangement exhibited substantial effects on flexural strength. Circular aggregates achieved a flexural strength of 4.31 MPa, approximately 31.7% higher than that of hexagonal aggregates. Among the investigated spatial configurations, the bottom-reinforced layered arrangement exhibited the highest flexural strength of 4.54 MPa, representing an improvement of 18.64% relative to the random distribution. In contrast, top-reinforced arrangements provided negligible improvement in flexural strength, highlighting the importance of aggregate placement within the tensile region under three-point bending.
(5) The prescribed ITZ thickness influenced the simulated flexural response and damage evolution. Reducing the interfacial thickness from 0.3 mm to 0.1 mm increased the predicted flexural strength from 3.83 MPa to 4.29 MPa, corresponding to an improvement of approximately 12%. The nonmonotonic relationship between ITZ thickness and flexural strength highlights the influence of interfacial geometry on stress redistribution and localized damage within the mesoscale model.
Overall, this study provides insights into the relationship between mesoscale structural characteristics and macroscopic flexural performance of silica fume-modified asphalt concrete, offering a basis for microstructural design and material optimization. Nevertheless, the present investigation is limited to quasi-static bending tests and two-dimensional mesoscale simulations, and the predictive capability of the numerical model requires further independent experimental validation. Future research will integrate CT-based microstructural characterization before and after loading with three-dimensional mesoscale modeling to investigate crack propagation and damage evolution under representative service conditions, thereby improving the reliability and engineering applicability of the proposed framework. Future investigations will further incorporate multiple stochastic microstructural realizations and global sensitivity analysis to quantify parameter interactions and improve the robustness of the numerical findings.

Author Contributions

Methodology, L.B.; software, Y.C.; investigation, L.B. and Y.C.; resources, Y.C.; writing—original draft, M.Z.A. and L.B.; writing—review and editing, M.Z.A., Y.C. and H.Y.; visualization, M.Z.A. and L.B.; supervision, H.Y.; funding acquisition, H.Y. All authors have read and agreed to the published version of the manuscript.

Funding

This work was supported by the Creative Research Groups of National Natural Science Foundation of China (No. 52421005), the National Natural Science Foundation of China (No. 62502008), and the Discretionary Fund of National Science Center for Earthquake Engineering (No. 2025ZZB4004).

Data Availability Statement

The datasets presented in this study are not publicly available because they form part of an ongoing research project. The data supporting the findings of this study are available from the corresponding authors upon reasonable request.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Bhattarai, S.; Zhou, Y.; Zhao, C.; Yadav, R. An Overview on Types, Construction Method, Failure and Key Technical Issues During Construction of High Dams. Electron. J. Geotech. Eng. 2016, 21, 10415–10432. [Google Scholar]
  2. Ma, H.; Chi, F. Major Technologies for Safe Construction of High Earth-Rockfill Dams. Engineering 2016, 2, 498–509. [Google Scholar] [CrossRef] [Scilit]
  3. Wang, Y.; Zhao, Y.; Liu, B.; Wang, N.; Li, C. Key Technologies and Future Development Trends of Intelligent Earth-Rock Dam Construction. J. Intell. Constr. 2023, 1, 1–18. [Google Scholar] [CrossRef] [Scilit]
  4. Rahman, A.M.; Mustafa, N.F. Small Dam Design and Construction for Sustainable Water Resources Management: A Comprehensive Review. UHD J. Sci. Technol. 2025, 9, 55–64. [Google Scholar] [CrossRef] [Scilit]
  5. Hartford, D.N.D.; Baecher, G.B. Risk and Uncertainty in Dam Safety; Thomas Telford: London, UK, 2004. [Google Scholar]
  6. Ho, M.; Lall, U.; Allaire, M.; Devineni, N.; Kwon, H.H.; Pal, I.; Raff, D.; Wegner, D. The future role of dams in the United States of America. Water Resour. Res. 2017, 53, 982–998. [Google Scholar] [CrossRef] [Scilit]
  7. Połomski, M.; Wiatkowski, M. Impounding Reservoirs, Benefits and Risks: A Review of Environmental and Technical Aspects of Construction and Operation. Sustainability 2023, 15, 16020. [Google Scholar] [CrossRef] [Scilit]
  8. Jwaida, Z.; Dulaimi, A.; Mydin, A.O.; Kadhim, Y.N.; Al-Busaltan, S. The self-healing performance of asphalt binder and mixtures: A state-of-the-art review. Innov. Infrastruct. Solut. 2024, 9, 1–35. [Google Scholar] [CrossRef] [Scilit]
  9. Bao, L.; He, M.; Wang, S.; Wu, X. Study on the Effect of Asphalt Static Conditions on the Tensile Properties of Acidic Aggregate Hydraulic Asphalt Concrete. Materials 2024, 17, 2627. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  10. Pinto, N.L.d.; Filho, P.L.M.; Maurer, E. Closure to “Foz DO Areia Dam—Design, Construction, and Behaviour” by Nelson L. de S. Pinto, Pedro L. Marques Filho, and Edilberto Maurer (pp. 173–191). J. Geotech. Eng. 1987, 113, 1156–1158. [Google Scholar] [CrossRef] [Scilit]
  11. Soares, M.A.; Ferreira, E.S.; Faggion, P.L.; Veiga, L.A.K.; Nadal, C.A.; De Freitas, S.R.C.; Nadal, M.A.D.; Neves, R.V.; Bosczowski, R.B. Evolution of geodesical auscultation monitoring in power plants: Foz do Areia, Segredo and Salto Caxias. Espaço Energia 2009, 11, 1–9. [Google Scholar]
  12. Schumann, W.H. Discussion of “Foz DO Areia Dam—Design, Construction, and Behaviour” by Nelson L. de S. Pinto, Pedro L. Marques Filho, and Edilberto Maurer (pp. 173–191). J. Geotech. Eng. 1987, 113, 1155–1156. [Google Scholar] [CrossRef] [Scilit]
  13. Zheng, W.X. Test on the Shape Schemes of Jilintai-I Hydropower Station Flood Discharge System. Adv. Mater. Res. 2012, 490–495, 2902–2905. [Google Scholar] [CrossRef] [Scilit]
  14. Sang, L.; Wang, J.; Sui, J.; Dziedzic, M. A new approach for dam safety assessment using the extended cloud model. Water Resour. Manag. 2022, 36, 5785–5798. [Google Scholar] [CrossRef] [Scilit]
  15. Zhang, M.; Ning, Z.; Lv, G. Safety Risk Assessment of a Hydropower Dam Based on Risk Matrix Method. In Proceedings of the Twenty-Eighth International Congress on Large Dams/Vingt-Huitième Congrès International des Grands Barrages; CRC Press: Boca Raton, FL, USA, 2025; pp. 332–358. [Google Scholar] [CrossRef] [Scilit]
  16. Zweben, C. Tensile strength of hybrid composites. J. Mater. Sci. 1977, 12, 1325–1337. [Google Scholar] [CrossRef] [Scilit]
  17. Qian, G.; Yao, D.; Gong, X.; Yu, H.; Li, N. Performance evaluation and field application of hard asphalt concrete under heavy traffic conditions. Constr. Build. Mater. 2019, 228, 116729. [Google Scholar] [CrossRef] [Scilit]
  18. Wahhab, H.A.-A.; Dalhat, M.; Habib, M. Storage stability and high-temperature performance of asphalt binder modified with recycled plastic. Road Mater. Pavement Des. 2016, 18, 1117–1134. [Google Scholar] [CrossRef] [Scilit]
  19. Zheng, Q.; He, P.; Zhang, D.; Weng, Y.; Lu, J.; Wang, T. A Holistic View of Asphalt Binder Aging under Ultraviolet Conditions: Chemical, Structural, and Rheological Characterization. Buildings 2024, 14, 3276. [Google Scholar] [CrossRef] [Scilit]
  20. Wang, Q.; Liu, Y.; Dong, J.; Ning, Z.; Meng, X.; Chen, L. Deformation behavior of hydraulic asphalt concrete under triaxial increasing-amplitude cyclic loading. Constr. Build. Mater. 2025, 487, 142125. [Google Scholar] [CrossRef] [Scilit]
  21. Farzadnia, N.; Abang Ali, A.A.; Demirboga, R. Incorporation of Mineral Admixtures in Sustainable High Performance Concrete. Int. J. Sustain. Constr. Eng. Technol. 2011, 2, 44–56. [Google Scholar]
  22. Chen, Y.; Xu, S.; Tebaldi, G.; Romeo, E. Role of mineral filler in asphalt mixture. Road Mater. Pavement Des. 2020, 23, 247–286. [Google Scholar] [CrossRef] [Scilit]
  23. Kumlai, S.; Jitsangiam, P.; Nikraz, H. Assessments of moisture damage resistance of asphalt concrete mixtures and asphalt mastic with various mineral fillers. Transp. Eng. 2022, 7, 100106. [Google Scholar] [CrossRef] [Scilit]
  24. Cheraghian, G.; Wistuba, M.P.; Kiani, S.; Barron, A.R.; Behnood, A. Rheological, physicochemical, and microstructural properties of asphalt binder modified by fumed silica nanoparticles. Sci. Rep. 2021, 11, 11455. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  25. Zhou, S.; Yan, J.; Ning, W.; Li, S.; Ai, C.; Yan, C. Performance and Mechanism of Using Low-Cost Fumed Silica Nanoparticles in Enhancing High Viscosity Modified Asphalt. Constr. Build. Mater. 2023, 409, 134090. [Google Scholar] [CrossRef] [Scilit]
  26. Zhou, S.; Shi, B.; Kong, L.; Mao, C.; Yan, C.; Ai, C. Rheological and adhesive improvements of terminal blend rubberized asphalt via fumed silica nanoparticle modification. Constr. Build. Mater. 2024, 449, 138543. [Google Scholar] [CrossRef] [Scilit]
  27. Malathy, R.; Shanmugam, R.; Chung, I.-M.; Kim, S.-H.; Prabakaran, M. Mechanical and Microstructural Properties of Composite Mortars with Lime, Silica Fume and Rice Husk Ash. Processes 2022, 10, 1424. [Google Scholar] [CrossRef] [Scilit]
  28. Khan, K.; Ahmad, W.; Amin, M.N.; Nazar, S. Nano-Silica-Modified Concrete: A Bibliographic Analysis and Comprehensive Review of Material Properties. Nanomaterials 2022, 12, 1989. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  29. Luo, H.; Leng, H.; Ding, H.; Xu, J.; Lin, H.; Ai, C.; Qiu, Y. Low-temperature cracking resistance, fatigue performance and emission reduction of a novel silica gel warm mix asphalt binder. Constr. Build. Mater. 2020, 231, 117118. [Google Scholar] [CrossRef] [Scilit]
  30. Zheng, X.; Xu, W.; Feng, H.; Cao, K. High and Low Temperature Performance and Fatigue Properties of Silica Fume/SBS Compound Modified Asphalt. Materials 2020, 13, 4446. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  31. Miller, C.; Vasconcelos, K.L.; Little, D.N.; Bhasin, A. Investigating Aspects of Aggregate Properties That Influence Asphalt Mixture Performance; Research Report DTFH61-06-C-00021; Texas A&M University: College Station, TX, USA; The University of Texas at Austin: Austin, TX, USA, 2011. [Google Scholar]
  32. Liu, C.; Mazlan, D.; Wan, X.; Lau, T.L.; Kumar, S.S.N. Multifunctional thermoelectric materials for energy-harvesting concrete: Recent advances and future prospects. J. Sustain. Cem.-Based Mater. 2025, 15, 1092–1126. [Google Scholar] [CrossRef] [Scilit]
  33. Chen, X.; Wang, B.; Tang, B.; Liang, Z.; Lu, X.; Deng, Z.; Li, B. Investigation into the Adhesion Performance of the Recycled Asphalt Mastic–Limestone Filler Interface Using the Pull-Off Test and Surface Free Energy Theory. Materials 2026, 19, 394. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  34. Mohammed, W.J.; Ismael, M.Q. The Moisture Resistance of Sustainable Asphalt Mixtures Modified with Silica Fume. J. Ecol. Eng. 2024, 25, 169–181. [Google Scholar] [CrossRef] [Scilit]
  35. Cheraghian, G.; Wistuba, M.P. Effect of Fumed Silica Nanoparticles on Ultraviolet Aging Resistance of Bitumen. Nanomaterials 2021, 11, 454. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  36. Mazloom, M.; Ramezanianpour, A.A.; Brooks, J.J. Effect of silica fume on mechanical properties of high-strength concrete. Cem. Concr. Compos. 2004, 26, 347–357. [Google Scholar] [CrossRef] [Scilit]
  37. Mizan, M.H.; Ueda, T.; Matsumoto, K. Enhancement of the concrete-PCM interfacial bonding strength using silica fume. Constr. Build. Mater. 2020, 259, 119774. [Google Scholar] [CrossRef] [Scilit]
  38. Song, L.; Liu, W.; Xin, F.; Li, Y. Study of adhesion properties and mechanism of sodium silicate binder reinforced with silicate fume. Int. J. Adhes. Adhes. 2021, 106, 102820. [Google Scholar] [CrossRef] [Scilit]
  39. Li, C.; Xiao, H.; Liu, R.; Deng, H.; Lin, B.; Zhang, C. Experimental research on bond behavior of fiber-matrix subjected to monotonic and cyclic loading. Constr. Build. Mater. 2025, 490, 142533. [Google Scholar] [CrossRef] [Scilit]
  40. Bahmani, H.; Mostafaei, H.; Mostofinejad, D. Review of Energy Dissipation Mechanisms in Concrete: Role of Advanced Materials, Mix Design, and Curing Conditions. Sustainability 2025, 17, 6723. [Google Scholar] [CrossRef] [Scilit]
  41. Cui, L.; Chen, S.; Liao, B.; Chen, D.; Lv, Z.; Zhang, S.; Guo, M.; Rong, H.; Xiang, T. Silica fume modified superhydrophobic cement-based materials with enhanced anti-corrosion property and its mechanism. Constr. Build. Mater. 2025, 489, 142405. [Google Scholar] [CrossRef] [Scilit]
  42. Zhang, B.; Tan, H.; Shen, W.; Xu, G.; Ma, B.; Ji, X. Nano-silica and silica fume modified cement mortar used as Surface Protection Material to enhance the impermeability. Cem. Concr. Compos. 2018, 92, 7–17. [Google Scholar] [CrossRef] [Scilit]
  43. Yang, L.; Hou, S.; Yu, H. Micromechanical Finite Element Model Investigation of Cracking Behavior and Construction-Related Deficiencies in Asphalt Mixtures. Materials 2025, 18, 3426. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  44. Li, Y.; Wang, Q.; Liu, B.; Tan, Y. Meso-Structural Modeling of Asphalt Mixtures Using Computed Tomography and Discrete Element Method with Indirect Tensile Testing. Materials 2025, 18, 2566. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  45. Liang, H.; Shi, L.; Wang, Y.; Li, P.; Huang, J. A Study on the Mechanical Properties of an Asphalt Mixture Skeleton Meso-Structure Based on Computed Tomography Images and the Discrete Element Method. Appl. Sci. 2025, 15, 10799. [Google Scholar] [CrossRef] [Scilit]
  46. Høeg, K.; Wang, W. Asphalt Core Embankment Dams; CRC Press: Boca Raton, FL, USA, 2025. [Google Scholar] [CrossRef] [Scilit]
  47. Bao, L.; He, M.; Wang, S.; Wu, X. Effects of Resting Conditions on Tensile Properties of Acid Aggregate Hydraulic Asphalt Concrete. Materials 2024, 17, 3556. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  48. Dai, Q.; Sadd, M.H.; Parameswaran, V.; Shukla, A. Prediction of Damage Behaviors in Asphalt Materials Using a Micromechanical Finite-Element Model and Image Analysis. J. Eng. Mech. 2005, 131, 668–677. [Google Scholar] [CrossRef] [Scilit]
  49. Zhou, M.; Zhong, S.; Liu, Y.; Liu, Z.; Yang, B.; Jiang, Z.; Zhou, L.; Tang, L. Damage Evolution and Lifetime Prediction of Cement Asphalt Mortar Under High-Speed Train Frequency and Temperature Gradient Load. Materials 2025, 18, 1011. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  50. Londono, J.G.; Shen, R.; Waisman, H. Temperature-Dependent Viscoelastic Model for Asphalt–Concrete Implemented within a Novel Nonlocal Damage Framework. J. Eng. Mech. 2020, 146, 04019119. [Google Scholar] [CrossRef] [Scilit]
  51. Sadd, M.H.; Dai, Q.; Parameswaran, V.; Shukla, A. Microstructural Simulation of Asphalt Materials: Modeling and Experimental Studies. J. Mater. Civ. Eng. 2004, 16, 107–115. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.