Mixture-Design Optimisation of LC3-Based Self-Compacting Mortar with Partial Substitution of Calcined Clay by Fly-Ash Cenospheres and Natural Pozzolan

,
,
,
,
,
,
,
and
1
LABMAT Laboratory, Department of Civil Engineering, National Polytechnic School of Maurice Audin, Oran 31000, Algeria
2
SREML Laboratory, Faculty of Civil Engineering and Architecture, Department of Civil Engineering, Amar Telidji University, Laghouat 03000, Algeria
3
SREML Laboratory, Faculty of Civil Engineering and Architecture, Department of Architecture, Amar Telidji University, Laghouat 03000, Algeria
4
Faculty of Mechanical Engineering, Technical University of Košice, Letná 1/9, 042 00 Košice, Slovakia

Abstract

Limestone calcined clay cement (LC3) can reduce CO2 emissions by 30–40% compared with Portland cement, but requires kaolinitic clay, which is not available everywhere. This study examined whether part of the calcined clay (metakaolin, MK) of an LC3-based self-compacting mortar can be replaced by two materials that need no calcination: fly-ash cenospheres (CS), which act as a low-density filler, and a local natural pozzolan (PZ), which supplies pozzolanic reactivity. Twenty-one mixtures with a fixed SCM fraction of 30 wt.% of the binder were designed with a {3, 5} simplex lattice and modelled with Scheffé polynomials; selected blends were characterised by XRD, TGA, and SEM-EDS. The highest 28-day strength (70.1 ± 1.5 MPa, against 48.9 ± 1.0 MPa for the LC3 reference) was obtained with 60% CS, 20% MK, and 20% PZ in the SCM fraction, with better flow at 20% less superplasticiser. The CS–PZ and CS–MK interactions were positive and significant at 28 days, indicating non-additive blending benefits. TGA showed that portlandite consumption scales with the metakaolin content, so the strength gain is mainly physical (packing). Replacing 80% of the calcined clay lowers the estimated binder footprint by about 8% per tonne and 17% per cubic metre of mortar.

1. Introduction

The cement industry is responsible for approximately 5–8% of global CO2 emissions, a significant environmental burden that demands urgent mitigation [1,2]. Portland cement, the primary binding agent in concrete production, accounts for the majority of these emissions because its manufacturing involves the energy-intensive high-temperature calcination of limestone and clay. As global construction demand expands, particularly in developing economies, the urgency of developing low-carbon cementitious alternatives has intensified, driving research toward materials that reduce environmental impact while maintaining or improving mechanical performance [3,4,5].
Limestone calcined clay cement (LC3) is one of the most promising low-carbon alternatives to Portland cement (CEM I, EN 197-1 [6]), offering potential CO2 reductions of 30–40% through partial clinker substitution with calcined clay and limestone [7,8]. A typical LC3 binder contains about 50% clinker, 30% calcined clay, 15% limestone, and 5% gypsum by mass [9,10], and the synergy between the aluminate phases of the calcined clay and limestone contributes to strength development and durability [11,12]. However, LC3 performance depends strongly on the calcined kaolinite content of the clay, and good strength generally requires clays with roughly 40% kaolinite or more [13]. Such clays are unevenly distributed; high-grade kaolin is also in demand by the ceramics and paper industries; and calcination requires dedicated kilns or flash calciners and fuel [7,10,14]. Where suitable clays are scarce or costly, partial substitution of the calcined clay by materials that need no calcination is of practical interest.
Natural volcanic pozzolans are widely available and contain amorphous silica and alumina that react with portlandite, although usually more slowly than calcined kaolinite [15,16,17]. Fly-ash cenospheres are hollow aluminosilicate microspheres recovered from coal-combustion ash. They are used mainly as lightweight fillers in cement-based composites and are not a binder; the pozzolanic reaction of their aluminosilicate glass is generally reported to be limited and slow, and the glassy shell may take part in alkali–silica reaction under some conditions [18,19,20,21]. Combining a reactive calcined clay with a moderately reactive natural pozzolan and a low-density spherical filler of low reactivity may nevertheless produce non-additive effects on packing, water demand and hydration that cannot be predicted from the single materials. Mixture designs such as the simplex lattice are suited to quantifying such effects [22,23] and have been used to optimise binders containing calcined clay, slag, and limestone [24,25]. Self-compacting mortars and concretes based on LC3 have also been reported [26,27]; because of the high water demand of fine metakaolin, their rheology is sensitive to the composition of the SCM fraction [28,29,30].
Previous work has examined LC3 with alternative or low-grade calcined clays [4,14,15], LC3 in self-compacting systems [26,27], cenospheres as lightweight fillers in Portland-cement composites [18,19,20] and mixture-design optimisation of calcined-clay binders [24,25]. To the authors’ knowledge, the combined substitution of the calcined clay of LC3 by cenospheres and natural pozzolan has not been examined with a mixture design, and the interactions between these three materials within a fixed SCM fraction have not been quantified. Three constraints of the present design determine the interpretation of the results: the SCM fraction is fixed at 30 wt.% of the binder; in addition to the 15% marble powder of the binder, 5% marble powder was added as filler, giving about 19% limestone in the total powder; and the superplasticiser dosage was adjusted for each mixture to obtain a fluid mortar without visible segregation, so that it varies with composition (0.6–1.0%). The three SCMs are therefore not equivalent: metakaolin and natural pozzolan are the reactive (pozzolanic) components, whereas the cenospheres act mainly as a low-density filler that replaces part of the reactive SCM fraction.
The study addresses three questions. (i) At a fixed SCM content, can a ternary blend of cenospheres, natural pozzolan, and a reduced amount of calcined clay exceed the strength and flow of the LC3 reference and of the two binary blends from which it is composed (60% CS + 40% MK, and 80% MK + 20% PZ)? (ii) Which binary interactions between the three materials are statistically significant at 7 and 28 days? (iii) Which microstructural and thermal differences between the ternary blend, the reference, and the two binary blends accompany the strength gain, and what does each SCM contribute? The contribution of this work is the application of a {3,5} simplex-lattice design to this new ternary SCM combination, the identification of the composition range giving the highest strength, and a multi-technique characterisation of the best-performing and reference mixtures that provides mechanistic hypotheses for further testing.
Because cenospheres and natural pozzolan require no calcination, the substitution also reduces the calcination demand of the binder; this effect is assessed at screening level in Section 5.

2. Materials and Methods

2.1. Materials and Mix Design

Twenty-one self-compacting mortar mixtures were prepared. The LC3-type binder consisted of 50% clinker, 5% gypsum, 15% marble powder (as the limestone component), and an SCM fraction of 30%, by mass. In the reference mixture (Mix 6), the SCM fraction consisted entirely of metakaolin (MK); in the other 20 mixtures, it was a blend of MK, cenospheres (CS), and natural pozzolan (PZ) defined by the mixture design (Section 2.2.1) (substitution by mass). Although the cenospheres are not cementitious, they are counted in this fraction and in the binder used for W/B, so that all mixtures have the same mass proportions; the term “SCM fraction” is used in this sense. An additional 5% marble powder, by mass of binder, was added as filler, so that the total powder is 105 parts per 100 parts of binder and the total limestone content is about 19% of the powder. River sand (0–5 mm; fineness modulus 2.5; sand equivalent 82%) was used. The water-to-binder ratio (W/B) was 0.40 for all mixtures, where the binder comprises clinker, gypsum, the 15% marble powder, and the SCM fraction. A polycarboxylate-ether superplasticiser (Sika ViscoCrete 775; Sika El Djazair, Algiers, Algeria) was dosed at 0.6–1.0% by mass of powder (cement and filler) to obtain a fluid and stable mortar (Section 2.2.2). Each batch contained 1001.6 g of cement (500.8 g clinker, 50.1 g gypsum, 150.2 g marble powder, and 300.5 g SCM), 50.1 g of marble-powder filler, 1536 g of river sand and 400.7 g of water, plus the superplasticiser; the filler is not included in the binder mass used for W/B. Because the masses were kept constant and the cenospheres have a low particle density (0.80 g/cm3), the batch volume increases with the cenosphere content, from about 1.36 L (Mix 6) to 1.63 L (Mix 21); the sand content decreases from about 41% to 34% of the mortar volume, and the binder and water contents per cubic metre decrease accordingly (Table S2). The proportions per cubic metre were calculated with the measured particle densities of the raw materials (see below), a particle density of 2.78 g/cm3 for the river sand, and an assumed air content of 1.5%.
Clinker and gypsum were obtained from AMOUDA Cement (El Beidha, Laghouat, Algeria); metakaolin was produced by calcining a kaolinitic clay at 850 °C; marble powder from southern Algeria was used as the limestone component; natural pozzolan was supplied by GICA Cement (Beni Saf, Algeria); and floating fly-ash cenospheres were obtained from a coal-fired power plant located about 600 km from the laboratory. The materials were characterised by X-ray fluorescence (Table 1), laser diffraction for the particle size of the powders, the Le Chatelier flask (ASTM C188) for particle density, and nitrogen adsorption (BET method) for specific surface area (Table 2, Figure 1). Based on its Al2O3 (28.0 wt.%) and K2O (2.4 wt.%) contents, the calcined clay is of medium grade, containing an estimated 50–60% calcined kaolinite together with illite [13,31]; it is referred to as metakaolin (MK) for brevity.
Table 1. Chemical composition of raw materials determined by X-ray fluorescence (wt.%).
Table 2. Physical properties of the materials used (n.d. = not determined).
Figure 1. Particle size distribution of the materials used.
The particle size distributions of the powders were measured by laser diffraction (HORIBA LA-960, HORIBA Ltd., Kyoto, Japan) in isopropanol after ultrasonic dispersion, and D10, D50, and D90 were obtained from the volume-based cumulative curves (Table 2). Marble powder, metakaolin, and natural pozzolan are the finest powders (D50 ≈ 1.5–3.5 µm), followed by gypsum and clinker. The cenospheres are much coarser (D50 ≈ 116 µm), closer in size to fine sand than to the binder. The river sand (0–5 mm; fineness modulus 2.5, determined by sieving; sand equivalent 82%) is not listed in Table 2 because laser diffraction cannot describe its full grading: the coarse grains settle in the circulation cell and are not measured, so that no particles above 59 µm were detected and the transmission remained at 98.5%. The laser-diffraction PSD of the fine fraction (<63 µm) of the river sand is (D10 = 4.2 µm, D50 = 13.8 µm, D90 = 28.1 µm).
X-ray diffraction (XRD) was carried out on the raw materials using a PANalytical X’Pert Pro diffractometer (Malvern Panalytical, Almelo, The Netherlands), with phase identification and quantification performed using Profex 5.6.1 software. The raw materials were imaged by scanning electron microscopy (SEM) with a Thermo Scientific Quattro S (Thermo Fisher Scientific, Waltham, MA, USA; clinker, metakaolin, and marble powder) and a TESCAN VEGA 3 (TESCAN, Brno, Czech Republic; gypsum, natural pozzolan, and cenospheres). The XRD patterns and SEM images are presented in Figure 2, Figure 3, Figure 4, Figure 5 and Figure 6.
Figure 2. XRD and SEM images of clinker.
Figure 3. XRD and SEM images of marble powder.
Figure 4. XRD and SEM images of metakaolin.
Figure 5. XRD and SEM images of natural pozzolan.
Figure 6. XRD and SEM images of floating fly-ash cenospheres.

2.2. Testing Methodology

2.2.1. Experimental Design

A {3, 5} simplex-lattice mixture design [22,23] was used to vary the proportions of CS, MK, and PZ within the fixed 30 wt% SCM fraction. The component proportions sum to unity (xCS + xMK + xPZ = 1) and take six levels (0, 0.2, 0.4, 0.6, 0.8, and 1.0), giving 21 compositions: three single-SCM mixtures, 12 binary mixtures, and 6 ternary mixtures (Table 3, Figure 7). The rest of the binder (50% clinker, 5% gypsum, and 15% marble powder) and W/B = 0.40 were kept constant. The response was modelled with the Scheffé quadratic polynomial:
Y = b 1 x 1 + b 2 x 2 + b 3 x 3 + b 12 × x 1 x 2 + b 13 × x 1 x 3 + b 23 × x 2 x 3
where Y is the compressive strength (MPa); x1, x2, and x3 are the proportions of CS, MK, and PZ in the SCM fraction; b1, b2, and b3 are the linear coefficients; and b12, b13, and b23 are the interaction coefficients of the CS–MK, CS–PZ, and MK–PZ pairs, estimated by least squares (JMP 7, SAS Institute Inc., Cary, NC, USA). The number of lattice points is:
C = q + m − 1 ! m ! q − 1 !
where q = 3 is the number of components and m = 5 is the lattice degree (six levels), giving C = 21.
Figure 7. Triangular representation of the 21 combinations studied with three components (MK, CS, and PZ).
The 21 compositions, which include the LC3 reference (Mix 6), are shown in Figure 7.
Table 3. Mixture compositions generated by the DoE.
Table 4. Composition of the mortars (g per batch): (a) constituents kept constant in all 21 mixtures; (b) variables of the mixture design, i.e., the proportions of cenospheres, metakaolin, and natural pozzolan in the 30% SCM fraction and the superplasticiser dosage.

2.2.2. Mixing, Casting, and Curing Protocol

The mortars were prepared in a 2-litre planetary mixer at a room temperature of 20 ± 2 °C. The dry constituents (cement constituents, SCMs, marble-powder filler, and sand) were first mixed for 60 s at low speed. About 70% of the mixing water was then added, and mixing continued for 60 s; the superplasticiser, dissolved in the remaining water, was added, and the mortar was mixed at high speed for 120 s. After a 60 s rest, during which the bowl was scraped, the mortar was mixed at high speed for a final 120 s. Fresh properties were measured within 10 min of mixing with a mini-slump cone and a mini V-funnel for mortar (cone: 70 mm top diameter, 100 mm base diameter, 60 mm height; V-funnel outlet 30 × 30 mm) [32,33]. The stability of each mixture was assessed visually on the mini-slump patty (homogeneity, absence of bleeding, aggregate segregation, and cenosphere flotation), and a mixture was accepted only when its patty showed none of these defects. The superplasticiser dosage of each mixture was optimised on this basis, as the dosage giving a fluid and homogeneous patty with a slump flow of at least 27 cm and without any visible segregation or bleeding. Specimens were cast in oiled steel moulds without vibration, demoulded after 24 ± 2 h and cured in saturated lime water at 20 ± 1 °C until testing at 7 and 28 days.

2.2.3. Compressive Strength

Compressive strength was determined according to EN 196-1 [34] on 40 × 40 × 160 mm prisms using a Controls universal press (Controls S.p.A., Liscate, Italy; capacity 3000 kN) at a loading rate of 2.4 kN/s. Three prisms were tested per mixture and age; each prism was broken in flexure, and both halves were tested in compression, giving six results per mixture and age. Results are reported as the mean ± standard deviation of all six values; the individual results are given in Table S1a (7 days) and Table S1b (28 days). When the ±10% criterion of EN 196-1 is applied, the 7-day sets of Mixes 6, 9 and 16 and the 28-day set of Mix 2 do not meet it, because more than one value deviates by more than 10% from the mean; these sets are marked in Table 5 and interpreted with caution. In three further sets (7 days: Mixes 8 and 13; 28 days: Mix 11), one value deviates by more than 10%; discarding it would change the mean by at most 1.5 MPa. For consistency with the statistical analysis, which uses all six values, the six-value means are reported for these sets; EN 196-1 would report the mean of the remaining five values. Differences between the four blends selected for microstructural analysis (Mixes 5, 6, 17, and 18) were assessed by one-way ANOVA followed by Tukey’s HSD test, and all mixtures were compared with the best-performing Mix 17 by Dunnett’s test (α = 0.05). Because the six specimens of a mixture come from a single batch, these tests compare batches and do not include batch-to-batch variability.
Table 5. Experimental matrix, fresh properties and compressive strength of the LC3-based self-compacting mortars (mean ± standard deviation of six half-prisms; † = set not meeting the EN 196-1 ±10% criterion; Mixes 7 and 19: see Section 3.2.1).

2.2.4. X-Ray Diffraction (XRD)

X-ray diffraction was performed on paste samples, prepared with the same binder compositions, W/B (0.40) and superplasticiser as the mortars and cured in the same way, using a PANalytical X’Pert Pro diffractometer with Cu Kα radiation (λ = 1.542 Å) at 40 kV and 45 mA, scanning 5–70° 2θ with a step of 0.02° and 1 s per step; the Rietveld refinement was performed over 7–45° 2θ. Phases were identified with the ICDD PDF-4+ database, and their relative fractions were estimated by Rietveld refinement in Profex. The structure models used for the poorly crystalline hydrates were taken from the Profex/BGMN structure library: tobermorite 11 Å for C-S-H, an Al-substituted tobermorite for C-A-S-H, and a separate Fe-bearing structure model for the Fe-bearing hydrate. No internal or external standard was used, so the X-ray amorphous content could not be determined; the phase fractions are therefore quantitative relative to the refined phases, i.e., normalised to 100% of the fitted phases, and the values obtained for the poorly crystalline hydrates, which depend on the structure models used, are interpreted with caution [35,36]. The weighted-profile R factors (Rwp) and goodness-of-fit (GOF) values are given with the phase fractions in Section 3.3.1, where the phase identification is also shown.
XRD was applied to the LC3 reference (Mix 6) and to the best-performing ternary blend (Mix 17). Two binary counterparts were characterised by TGA and SEM-EDS: Mix 18 (CS–MK binary; 60% CS, 40% MK), which retains the cenosphere fraction of Mix 17, and Mix 5 (MK–PZ binary; 80% MK, 20% PZ), which retains its natural pozzolan fraction. They were used to examine the contribution of the third component. XRD data for the binary blends are not available, which limits the phase-level comparison.

2.2.5. Thermal Analysis (TGA/DTG/DSC)

Thermogravimetric analysis was performed at 7 and 28 days on paste samples using a SETARAM Labsys Evo analyser (SETARAM Instrumentation, Caluire, France). Samples were crushed after hydration stoppage in acetone, vacuum-dried at 40 °C for 24 h, and heated from 30 to 1000 °C at 10 °C/min under nitrogen (50 mL/min) in alumina crucibles (100 µL), with α-alumina as reference. DTG and DSC signals were recorded simultaneously [37]. Bound water, portlandite, and carbonate contents are expressed per 100 g of dry binder, i.e., divided by the residual mass at 550 °C [35].
Bound water was taken as the mass loss between 105 and 400 °C. Portlandite was quantified from the dehydroxylation step between about 400 and 500 °C by the tangent method, i.e., as the vertical distance between the tangents to the TG curve before and after the step, taken at the temperature of the DTG peak [35]; this excludes the background dehydration of C-S-H and other hydrates that overlaps the portlandite step. Portlandite water was converted with M(Ca(OH)2)/M(H2O) = 74/18 = 4.11; carbonate was estimated from the mass loss between 550 and 800 °C and converted with M(CaCO3)/M(CO2) = 100/44 = 2.27 [35,38]. DTG signals were assigned approximately as follows: ettringite and C-S-H (about 50–200 °C), AFm phases such as hemi- and monocarboaluminate (about 150–200 °C), hydrotalcite (about 220–250 °C and about 400 °C), hydrogarnet (about 300–350 °C), portlandite (400–500 °C), and calcium carbonate (550–800 °C) [35,37,39].

2.2.6. Scanning Electron Microscopy (SEM-EDS)

The microstructure was examined at 28 days with a Thermo Scientific Quattro S environmental SEM equipped with an EDS detector and APEX software (EDAX, Mahwah, NJ, USA). Hydration of fragments of the hardened mortars was stopped by immersion in acetone for more than 72 h, followed by vacuum drying at 40 °C for 48 h. Freshly fractured fragments were mounted on SEM stubs and examined in low-vacuum mode (30 Pa), which does not require a conductive coating, using the low-vacuum secondary-electron detector (LVD) at 10 kV and a working distance of about 10 mm; images were recorded at magnifications of 300–10,000×. In secondary-electron images, contrast reflects mainly surface topography and not composition. EDS spectra were acquired at 10 kV and 2500× over an area of about 87 × 65 µm (one area per blend), with 128 eV energy resolution and a 100 s acquisition time, and were quantified without standards; such analyses carry large uncertainties, particularly on rough surfaces [40]. Because the analyses were made on unpolished fracture surfaces, over areas containing several phases, the EDS results are used only as area-averaged atomic ratios (Ca/Si and Al/Si, excluding C and O, which are not reliably quantified) and are treated as qualitative [41].

3. Results and Discussion

3.1. Fresh and Hardened Properties

The fresh properties (slump flow and V-funnel time) and the compressive strengths at 7 and 28 days of the 21 mortars are given in Table 5.

3.1.1. Fresh Properties

Slump-flow diameters ranged from 27.0 cm (Mix 3) to 42.0 cm (Mix 1) and V-funnel times from 1.15 s (Mix 2) to 7.20 s (Mix 6, LC3 reference) (Table 5). Measured with the mini-slump cone, these values exceed the EFNARC target for self-compacting mortar (about 24–26 cm) [32], and except for Mix 6, the V-funnel times are below the 7–11 s range recommended for mortar, which indicates highly fluid mixtures. Visual inspection of the mini-slump patties showed homogeneous mixtures without bleeding, aggregate segregation, or cenosphere flotation (Section 2.2.2). All 21 mixtures were therefore highly flowable and showed no visible segregation; they are referred to as self-compacting mortars in this sense, although their slump-flow and V-funnel values lie outside the EFNARC ranges for mortar. The stability assessment is visual, and a quantitative static segregation test would be needed to confirm it, particularly for the most fluid mixtures. The mixture with 100% natural pozzolan (Mix 1) had the largest slump flow and one of the shortest flow times, whereas the reference (Mix 6) had a relatively low slump flow (30.25 cm) and the longest flow time despite the highest superplasticiser dosage (1.0%), consistent with the high water demand of fine metakaolin, whose BET surface area (20.8 m2/g) is about five times that of the natural pozzolan (3.9 m2/g) and 10 times that of the clinker (2.0 m2/g) [28,29,42]. Cenosphere-containing mixtures generally flowed more easily than MK-rich ones, which can be attributed to the spherical shape of the cenospheres [18,19]. The best-performing mixture (Mix 17) reached 32.0 cm and 3.4 s with 0.8% superplasticiser, i.e., 20% less admixture than the reference. Because the dosage was adjusted for each mixture (Section 2.2.2), it varies with composition; its possible effect on strength (through air content or retardation) cannot be separated from that of composition and is discussed in Section 3.2.1.

3.1.2. Compressive Strength Development

The 28-day strength ranged from 33.95 ± 1.29 MPa (Mix 1, 100% PZ) to 70.10 ± 1.49 MPa (Mix 17) (Table 5; Figure S2). The coefficient of variation of the six specimens was below 6% for most sets and reached about 12% for the 28-day set of Mix 2. The LC3 reference (Mix 6) reached 48.90 ± 0.96 MPa at 28 days; its 7-day set is bimodal (three values of about 26.7 MPa and three of about 38.1 MPa) and does not meet the EN 196-1 criterion, so its 7-day mean (32.40 MPa) is uncertain. Mix 17 (60% CS, 20% MK, and 20% PZ in the SCM fraction) reached 38.47 ± 2.13 and 70.10 ± 1.49 MPa at 7 and 28 days, i.e., 43% more than the reference at 28 days, with one-fifth of its metakaolin content. It also exceeded the single-SCM cenosphere mixture (Mix 21; 58.03 ± 1.16 MPa) by 21% and the best metakaolin-free binary (Mix 7; 67.65 ± 3.14 MPa, a result that requires confirmation; Section 3.2.1) by 3.6%. Among the four blends characterised in Section 3.3, all differences at 28 days were significant (one-way ANOVA with Tukey’s test, p < 0.001), giving the ranking Mix 17 > Mix 18 (CS–MK binary, 63.40 MPa) > Mix 5 (MK–PZ binary, 53.85 MPa) > Mix 6 (reference). At 7 days, Mix 17 was significantly stronger than the reference (p = 0.034, although the 7-day set of the reference is bimodal) and the MK–PZ binary (p < 0.001) but not than the CS–MK binary (p = 0.096). Compared with Mix 17 by Dunnett’s test, only Mixes 13 and 7 were not significantly weaker at 28 days (p = 0.94 and 0.63).
The cenosphere-only mixture (Mix 21) was stronger than the metakaolin-only reference (Mix 6) at 28 days (58.03 against 48.90 MPa), although cenospheres act mainly as a filler, with little or no pozzolanic contribution at early ages [19,20]. Several factors may contribute to this inversion: (i) the calcined clay is of medium grade (Section 2.1), and LC3 strength depends strongly on the calcined kaolinite content [13]; (ii) the gypsum content (5%) was not optimised for this calcined clay, and under-sulphated LC3 binders lose strength [7,10]; (iii) the reference was the most viscous mixture (V-funnel 7.2 s), so more air may have been entrapped in the non-vibrated prisms; (iv) the spherical cenospheres reduce water and admixture demand; and (v) because W/B was fixed by mass, the cenosphere mortars contain less binder and less water per cubic metre than the reference (Mix 21: 616 kg/m3 binder and 247 L/m3 water, against 735 kg/m3 and 294 L/m3 for Mix 6; Table S2), so the mixtures differ in paste composition and not only in SCM type. Notably, Mix 17 reaches a strength 43% higher than that of the reference with about 10% less clinker per cubic metre (330 against 367 kg/m3). The reference is therefore a demanding but not necessarily optimised LC3 benchmark, and strength gains relative to it should be read with this in mind. The lowest strengths were obtained for PZ-rich mixtures without cenospheres (Mixes 1–3: 33.95–48.85 MPa). Mix 7 (20% CS, 80% PZ) reached 67.65 MPa, much more than its neighbours on the CS–PZ edge (Mix 1: 33.95 MPa; Mix 12: 54.50 MPa), whereas Mix 19 (80% CS, 20% PZ) reached only 46.40 MPa; these two mixtures are discussed in Section 3.2.1.
To describe the departure of a mixture from linear blending, a synergy index (SI) is defined as the ratio of its measured strength to the linear part of the Scheffé model (Equation (3)). It is a descriptive measure of non-additivity and is evaluated in Section 3.2.4.
SI = Factual Flinear   = Factual ( bCS · xCS + bMK · xMK + bPZ · xPZ )

3.2. Mixture Design, Statistical Modelling, and Optimisation

The {3,5} simplex-lattice design (Section 2.2.1) was used to model the compressive strength at 7 and 28 days as a function of the proportions of CS, MK and PZ in the fixed 30 wt.% SCM fraction. Each composition was prepared once and tested with six half-prisms per age, so the design contains no replicated mixtures.

3.2.1. Regression Model Development and Validation

Scheffé quadratic models (Equation (1)) were fitted to the strengths at both ages. Two mixtures with anomalous results were excluded from the fits (see below), so the models in Table 6 are based on 19 mixtures. The quadratic form was retained because the special-cubic term (b123x1x2x3) was not significant at 28 days (p = 0.081); at 7 days it was significant (b123 = 152 ± 57 MPa, p = 0.021), which is one more reason to regard the 7-day model as indicative only.
Table 6. Scheffé quadratic model coefficients (± standard error; p-value in parentheses) and fit statistics for compressive strength at 7 and 28 days (19 mixtures; Section 3.2.1).
The 28-day model is significant (F-test p < 0.001) and explains 84% of the variance (adjusted R2 = 0.78; predicted R2 = 0.68; RMSE = 3.99 MPa). The 7-day model is also significant (R2 = 0.66, p = 0.008) but has little predictive value (predicted R2 = 0.09); it is therefore regarded as indicative only, and the interpretation is based on the 28-day model.
Treatment of anomalous mixtures. Two mixtures on the CS–PZ edge, Mix 7 (20% CS, 80% PZ), and Mix 19 (80% CS, 20% PZ), gave results that depart strongly from those of their neighbours on the same edge (Table 5) and had the largest residuals in a preliminary 28-day fit to all mixtures (externally studentised residuals +3.03 and −2.77; all other mixtures within ±1.8). Their six specimen results are internally consistent (coefficients of variation at 28 days: 4.6% and 4.3%), so the anomaly arises at batch level and not from individual specimens; no batching record explains it. Both mixtures lie outside the 95% prediction interval of the model fitted to the other 19 mixtures (Mix 7: measured 67.65 MPa, predicted 49.4 MPa, interval 39.4–59.4 MPa; Mix 19: measured 46.40 MPa, predicted 63.5 MPa, interval 53.5–73.6 MPa). Because the anomaly concerns the batch, both mixtures were excluded from the regression at both ages. At 7 days, Mix 19 is not an outlier (externally studentised residual −1.42 in the fit to all 21 mixtures, against +4.41 for Mix 7); it was excluded at this age because its 28-day result indicates a batch-level anomaly. Their measured values are retained in Table 5, and the fit to all 21 mixtures is given in Table S3 for completeness. Replicated batches of these two compositions are needed to establish whether their results reflect an experimental error or a local feature of the CS–PZ edge that the quadratic model does not describe.
Because the design has no replicated mixtures, pure error between batches cannot be estimated and a meaningful lack-of-fit test is not defined. The six specimens of each mixture measure only within-batch scatter: a lack-of-fit test against this error is highly significant at both ages (p < 0.001), which indicates that batch-to-batch variation, not captured by the specimen replicates, is larger than the scatter between specimens of one batch. Model adequacy was judged from R2, adjusted and predicted R2, and residual diagnostics (Figure S1). The residuals of the 28-day model showed no trend with the fitted values and were consistent with a normal distribution (Shapiro–Wilk p = 0.21; largest absolute residual 5.76 MPa, Mix 14).
The quadratic Scheffé model assumes a smooth response surface and is sensitive to experimental noise at the pure-component vertices. The superplasticiser dosage (0.6–1.0%) was adjusted for each mixture (Section 2.2.2) and is therefore partly confounded with composition; when added as a covariate to the 28-day model, its coefficient was not significant (16.8 ± 20.0 MPa per % SP, p = 0.42), but because the dosage is partly confounded with composition, an effect of the admixture on strength cannot be excluded. The XRD, TGA, and SEM-EDS results in Section 3.3 characterise specific mixtures but do not validate the regression models.

3.2.2. Individual Component Contributions

The linear coefficients estimate the strength of a mortar whose SCM fraction consists of a single component. At 28 days, cenospheres have the highest coefficient (57.57 MPa), followed by metakaolin (45.91 MPa) and natural pozzolan (34.04 MPa), in agreement with the measured strengths of Mixes 21, 6, and 1 (58.03, 48.90, and 33.95 MPa). The same ranking is obtained at 7 days (35.14, 28.27, and 25.81 MPa). The higher strength of the cenosphere mortar does not indicate reactivity: the cenospheres act as a filler with no measurable pozzolanic contribution at the ages tested (Section 4.2), and in Mix 21 the strength is provided mainly by the clinker (with the limestone and gypsum). Given their coarse size (D50 ≈ 116 µm) and low specific surface, cenospheres are unlikely to be effective nucleation sites; their contribution is mainly physical, through improved packing, lower water and admixture demand, and the lower binder and water contents per cubic metre of the cenosphere mortars (Section 3.1.2; Table S2) [18,19].
Metakaolin has intermediate coefficients (28.27 MPa at 7 days and 45.91 MPa at 28 days). The coefficient describes the behaviour of this medium-grade calcined clay in the present design and should not be read as a general measure of metakaolin reactivity.
Natural pozzolan has the lowest coefficients (25.81 MPa at 7 days and 34.04 MPa at 28 days), consistent with the slower reaction of an untreated volcanic pozzolan compared with metakaolin [15,16,17]. It is nevertheless the reactive component of the two non-calcined materials, and it takes part in the largest interaction of the design (CS × PZ, Section 3.2.3), so its behaviour in blends cannot be inferred from its single-component coefficient.

3.2.3. Binary Interaction Effects

The interaction coefficients quantify the departure of binary blends from linear mixing. At 28 days, all three interactions are positive and significant: CS × PZ (66.59 ± 13.47 MPa, p = 0.0003), MK × PZ (60.93 ± 13.95 MPa, p = 0.0008), and CS × MK (35.75 ± 13.95 MPa, p = 0.024). At 7 days, only CS × PZ is significant (25.71 MPa, p = 0.026). The standard errors of the 28-day interaction terms (13–14 MPa) show that the three interactions are not clearly different from one another, so their ranking should not be over-interpreted. For equal proportions of two components, the 28-day model predicts 62.5 MPa for CS–PZ, 60.7 MPa for CS–MK, and 55.2 MPa for MK–PZ, against linear averages of 45.8, 51.7, and 40.0 MPa.
CS × PZ interaction. This is the largest and most significant interaction at 28 days and the only one already significant at 7 days. It may reflect the complementary packing of the coarse spherical cenospheres (D50 ≈ 116 µm) and the fine, irregular pozzolan particles (D50 ≈ 3.4 µm), together with the lower water and admixture demand of cenosphere-containing mixtures [18,19]. In this combination, the natural pozzolan is the reactive SCM and the cenospheres act mainly as a filler, so a chemical contribution to the interaction, if any, is more likely to come from the pozzolan. The present data do not identify a chemical mechanism.
CS × MK interaction. The CS × MK interaction could not be distinguished from zero at 7 days (8.77 MPa, p = 0.42) and was positive and significant at 28 days. Blends of cenospheres and metakaolin are therefore stronger at 28 days than linear mixing predicts, but the data do not identify the mechanism. Because the cenospheres showed no measurable reactivity, the interaction is unlikely to be chemical; it more likely reflects packing and water demand, together with the reaction of the metakaolin in a paste with less binder per cubic metre.
MK × PZ interaction. The MK × PZ interaction was not significant at 7 days (2.80 MPa, p = 0.80) but was positive and significant at 28 days. It is, however, the interaction most sensitive to the treatment of the two anomalous mixtures (Table S3) and should be confirmed with replicated mixtures. A positive interaction between metakaolin and the reactive glassy fraction of the pozzolan is plausible [14], but a regression coefficient cannot identify a phase, and no link to a specific hydration product is made.
In summary, the 28-day model shows positive, non-additive strength effects for the three binary pairs, the CS × PZ interaction being the largest and the only one already significant at 7 days. The models describe statistical departures from linear blending and do not by themselves establish the mechanisms discussed in Section 3.3 and Section 4.

3.2.4. Optimal Formulation Identification and Synergy Quantification

The 28-day model predicts a maximum of 65.5 MPa at about xCS = 0.55, xMK = 0.18 and xPZ = 0.26 (Figure 8). The mixture with the highest measured strength, Mix 17 (0.60, 0.20 and 0.20; 70.10 MPa), lies close to the predicted maximum. Its predicted strength is 65.25 MPa (95% prediction interval 56.1–74.4 MPa), so its measured strength is within the prediction interval. Mix 17 was included in the fit, so this comparison is not an independent validation.
Figure 8. Ternary contour plot of 7 days (a) and 28 days (b) compressive strength predicted by the Scheffé quadratic model (Table 6).
The predicted surface is flat around the maximum: compositions predicted to reach at least 60 MPa cover about 56% of the design space, and those predicted to reach at least 62 MPa about 40%. This region includes compositions without metakaolin, so high 28-day strength can be reached with low or no metakaolin, and about 0.2 MK gives only a modest further increase. Given the residual standard deviation of the model (3.99 MPa), predicted differences of a few MPa between neighbouring compositions are not significant.
The mixtures closest to Mix 17 reach similar strengths: Mix 13 (40% CS, 20% MK, 40% PZ; 68.35 MPa) is 2.5% lower, whereas Mix 18 (60% CS, 40% MK; 63.40 MPa) and Mix 16 (60% CS, 0% MK, 40% PZ; 62.60 MPa) are 6.7 and 7.5 MPa lower. Mix 13 was not significantly weaker than Mix 17 at 28 days (Dunnett, p = 0.94; Section 3.1.2), whereas Mixes 18 and 16 were (p < 0.001). Mix 17 is therefore regarded as the best-performing mixture of this study, within an optimal region, and not as a proven global optimum. The synergy index of Mix 17 (Equation (3)) at 28 days is 1.39 (95% interval 1.26–1.54, considering only the uncertainty of the linear part). Computed in the same way, other mixtures have similar or higher indices (Mix 8: 1.50; Mix 13: 1.49; Mix 9: 1.46), and the metakaolin-free Mix 16 reaches 1.30, within the interval of Mix 17. The index therefore describes a positive non-additive blending effect that is not specific to the composition of Mix 17 and cannot be attributed to the presence of metakaolin; it is evaluated at a composition selected for its high strength and does not identify a chemical interaction.

3.3. Microstructural Investigation

3.3.1. Phase Evolution by XRD Analysis

XRD was performed at 7 and 28 days on the LC3 reference and the best-performing ternary blend (Figure 9 and Figure 10).
Figure 9. Rietveld refinement of the XRD patterns at 7 days: LC3 reference (a) and best-performing ternary blend (b).
Figure 10. Rietveld refinement of the XRD patterns at 28 days: LC3 reference (a) and best-performing ternary blend (b).
Table 7 gives the phase fractions obtained by Rietveld refinement. Because no internal standard was used (Section 2.2.4), they are expressed relative to the refined phases (normalised to 100%), and the amorphous content (unreacted metakaolin, pozzolan, and cenosphere glass and part of the gel) is not included. For well-crystallised phases such as calcite, quartz, portlandite, and the clinker phases, the refined fractions rest on known crystal structures. C-S-H, C-A-S-H, and the Fe-bearing hydrate have no unique crystal structure and were fitted with proxy models, so their fractions depend on the model chosen and on how much of the broad diffuse scattering it absorbs; these values are therefore less reliable than those of the crystalline phases. Mono- and hemicarboaluminate were not resolved as separate phases. XRD data for the binary blends are not available. The refinements fit well at 7 days (Rwp ≤ 5.2%, GOF ≤ 1.7) but less well at 28 days, particularly for the ternary blend (Rwp = 10.1%, GOF = 3.49). The difference curves of the 28-day refinements (Figure 10) show that part of this misfit arises from sharp reflections that are not described by the refined phases (near 18.9° and 24.1° 2θ in both blends) and from the quartz reflection at about 26.6° 2θ, in addition to the poorly crystalline hydrates, which the proxy models reproduce less accurately; the 28-day fractions of the ternary blend, including the Fe-bearing hydrate, therefore carry the largest uncertainty in Table 7.
Table 7. Relative phase fractions from Rietveld refinement (wt.%, normalised to 100% of the refined phases; amorphous content not determined).
7 days
At 7 days (Figure 9, Table 7), the LC3 reference contains C-S-H (29 wt.%), portlandite (15 wt.%), C3S (16 wt.%), calcite (15 wt.%), and quartz (7 wt.%), with no detectable C-A-S-H. The ternary blend shows a higher C-S-H fraction (32 wt.%), a markedly higher quartz fraction (22 wt.%), lower C3S (13 wt.%), and portlandite (11 wt.%) fractions, and a small C-A-S-H fraction (4 wt.%). The higher quartz content in the ternary blend reflects the contribution of the cenospheres and the natural pozzolan, both of which contain quartz.
The ternary blend has lower portlandite (11 against 15 wt.%) and C3S (13 against 16 wt.%) fractions at 7 days, which would suggest more advanced clinker hydration combined with portlandite consumption [43,44]; however, TGA gives the opposite ranking for portlandite (Section 3.3.2), so this difference is not considered conclusive. A small C-A-S-H-type contribution (4 wt.%) was fitted for the ternary blend at 7 days but not for the reference.
The calcite fraction is higher in the ternary blend at 7 days (18 against 15 wt.%), in line with its higher CaCO3 content measured by TGA (23.61 against 20.61 g/100 g binder; Table 8) [37,45]. The cenospheres and natural pozzolan contain little carbonate (LOI 1.29 and 2.52 wt.%; Table 1), and both blends contain the same limestone content, so this difference is more likely related to sampling or to carbonation during sample preparation than to the composition of the SCM fraction. Phlogopite, originating from the calcined clay, is present in both blends.
Table 8. Bound water (105–400 °C), portlandite (tangent method), and calcium carbonate (550–800 °C) of the four pastes, in g per 100 g of dry binder (residual mass at 550 °C).
28 days
At 28 days (Figure 10, Table 7), both blends show advanced hydration, with lower C3S fractions (10 wt.% in the reference and 9 wt.% in the ternary blend) [8,46]. The reference blend contains portlandite (2 wt.%), calcite (19 wt.%), quartz (25 wt.%), C-S-H (28 wt.%), C-A-S-H (8 wt.%), and residual phases (8 wt.%). The ternary blend shows portlandite (3 wt.%), calcite (17 wt.%), quartz (32 wt.%), C-S-H (16 wt.%), C-A-S-H (9 wt.%), Fe-bearing hydrate (14 wt.%), and C3S (9 wt.%).
Both blends show a strong decrease in the relative portlandite fraction between 7 and 28 days (reference 15→2 wt.%; ternary 11→3 wt.%), together with an increase in the C-A-S-H-type fraction. For the reference, this is consistent with ongoing pozzolanic reaction [43,47] and with TGA (Table 8); for the ternary blend, however, TGA shows that the absolute portlandite content increased between 7 and 28 days (6.14→7.54 g/100 g binder; Section 3.3.2), so the decrease of its XRD fraction results from the normalisation to the refined phases and does not indicate portlandite consumption. The reference shows an apparent increase in calcite (15→19 wt.%) whereas TGA indicates a decrease in CaCO3 (20.61→19.57 g/100 g binder; Table 8); this is expected for relative fractions normalised to the fitted phases, and TGA is regarded as the more reliable measure of carbonate content [37]. The quartz fraction also increases with age in both blends (7→25 and 22→32 wt.%), which cannot result from hydration. Because the samples are pastes without sand, the quartz originates from the raw materials (calcined clay, natural pozzolan, and cenospheres), and the apparent increase reflects the normalisation of the relative fractions to the fitted phases or sample heterogeneity; this confirms that the fractions in Table 7 are relative and not absolute contents.
In the ternary blend at 28 days, part of the pattern was fitted with an Fe-bearing hydrate model (14 wt.% of the relative fractions), which was not required for the reference. Because Rietveld refinement without an internal or external standard cannot reliably quantify poorly crystalline gels [35,36], and the structure model used is a proxy, this result is regarded as an indication of Fe-bearing hydration products rather than as the identification of a distinct F-C-S-H phase. Iron in hydrated cements is commonly hosted by Fe-siliceous hydrogarnet and Fe-containing AFm and AFt phases, and to a limited extent by C-S-H [39,48,49]; the present data do not distinguish between these possibilities. Moreover, the two binders contain almost the same amount of iron (about 4.2 wt.% Fe2O3 in the reference and 4.4 wt.% in the ternary blend, calculated from Table 1), with more than half of it supplied by the clinker in both cases, so a difference in iron supply cannot explain why an Fe-bearing model was needed only for the ternary blend. The fitted C-S-H fraction of the reference (28 wt.%) is also close to the sum of the C-S-H and Fe-bearing hydrate fractions of the ternary blend (16 + 14 = 30 wt.%), which suggests that the two proxy models may partly share the same diffuse scattering, including that of the cenosphere glass. The natural pozzolan contains 15.07 wt.% Fe2O3, but bulk Fe2O3 content is not a measure of reactivity: iron in crystalline minerals such as hematite is essentially inert, and only iron released from the glassy fraction can be taken up by hydrates [48]. Confirmation requires internal-standard XRD, quantitative SEM-EDS and, ideally, Mössbauer or X-ray absorption spectroscopy.
The ternary blend combines a lower fitted C-S-H fraction (16 against 28 wt.%) with a 43% higher strength. Because the C-S-H fractions depend on the proxy model and exclude the amorphous part of the gel, no conclusion on the amount of hydrates is drawn; the higher strength is more likely related to the differences in packing, water demand, and microstructural uniformity discussed in Section 3.1 and Section 3.3.3.

3.3.2. Thermal Analysis and Hydration Product Quantification

TGA/DTG/DSC was used to quantify bound water, portlandite, and calcium carbonate in pastes of the reference (Mix 6), the ternary blend (Mix 17), the CS–MK binary (Mix 18), and the MK–PZ binary (Mix 5) at 7 and 28 days (Figure 11 and Figure 12). Bound water was taken as the mass loss between 105 and 400 °C, portlandite was determined from the 400–500 °C step by the tangent method, and calcium carbonate from the 550–800 °C step; all values are expressed per 100 g of dry binder (residual mass at 550 °C; Section 2.2.5) and are given in Table 8.
Figure 11. DTG curves at 7 and 28 days of the LC3 reference, the best-performing ternary blend, the CS–MK binary, and the MK–PZ binary.
Figure 12. TGA/DSC curves at 7 and 28 days of the LC3 reference, the best-performing ternary blend, the CS–MK binary, and the MK–PZ binary.
7 days
At 7 days, bound water ranged from 3.60 g/100 g (MK–PZ binary) to 6.01 g/100 g (reference), with the ternary (5.09) and CS–MK (5.16) blends in between (Table 8). Lower bound water may indicate either a smaller amount of hydrates or hydrates with a lower water content; on its own, it does not demonstrate a different gel structure [35].
Portlandite at 7 days was slightly higher in the ternary (6.14 g/100 g) and CS–MK (6.07) blends than in the reference (5.12) and the MK–PZ binary (5.28). XRD gave the opposite ranking for the reference and ternary blends (15 against 11 wt.%); because the XRD values are relative fractions normalised to the fitted phases (Section 2.2.4), the TGA values are considered more reliable [35]. The higher portlandite content of the cenosphere-containing blends is consistent with their lower metakaolin content, i.e., with less pozzolanic consumption.
The portlandite DTG peak of the ternary blend at 7 days was narrower (FWHM ≈ 24 °C; peak at ≈ 451 °C) than that of the reference (≈ 42 °C; ≈ 443 °C). Peak width depends on crystal size and distribution but also on sample mass, packing, and heating rate, so this difference is reported without mechanistic interpretation.
Except for the reference, all blends showed a small DTG signal at 240–265 °C (ternary ≈ 264 °C; CS–MK binary ≈ 257 °C; MK–PZ binary ≈ 244 °C). This range may correspond to AFm phases or hydrotalcite [35,37,45]; a definite assignment would require XRD of these blends.
At 7 days, the CS–MK binary (Mix 18) and the ternary blend had very similar bound water and portlandite contents (5.16 and 6.07 against 5.09 and 6.14 g/100 g), consistent with their 7-day strengths, which do not differ significantly (33.46 and 38.47 MPa; Section 3.1.2).
The MK–PZ binary (Mix 5) had the lowest bound water (3.60 g/100 g) at 7 days, in line with its low 7-day strength (25.89 MPa).
28 days
Between 7 and 28 days, bound water increased in all blends, most in the reference (6.01 to 11.20 g/100 g, +86%) and least in the ternary blend (5.09 to 6.62 g/100 g, +30%). At 28 days, the ranking is reference > CS–MK (8.84) > MK–PZ (8.46) > ternary, nearly the opposite of the strength ranking (Section 3.1.2): the ternary blend, with the lowest bound water, is the strongest, and the reference, with the highest, is the weakest. The higher strength of the ternary blend is therefore not explained by a larger amount of hydrates. Part of the bound water of the reference may also come from hydrogarnet (see below). Lower bound water may also reflect hydrates with a lower water content, which would require 29Si NMR or FTIR to verify [50,51].
Portlandite evolved in opposite directions depending on the metakaolin content (Table 8). Between 7 and 28 days it decreased by about 50% in the reference (30% MK; 5.12 to 2.56 g/100 g) and by about 30% in the MK–PZ binary (24% MK; 5.28 to 3.70), remained nearly constant in the CS–MK binary (12% MK; 6.07 to 6.41) and increased by about 23% in the ternary blend (6% MK; 6.14 to 7.54). At 28 days, portlandite therefore decreases steadily as the metakaolin content increases. This indicates that, at this age, portlandite consumption by pozzolanic reaction is controlled mainly by the metakaolin and that the cenospheres and the natural pozzolan consume comparatively little portlandite. With the tangent method, the 28-day portlandite content of the reference (2.56 g/100 g) agrees with the XRD value (2 wt.%), whereas for the ternary blend, TGA (7.54) remains higher than XRD (3 wt.%), because the XRD fractions are relative to the refined phases and do not include the amorphous content (Section 3.3.1). The DTG peak of the reference at about 324 °C, which is absent or very weak in the other blends, falls in the range usually assigned to hydrogarnet (katoite-type phases), which typically form in metakaolin-rich systems and can incorporate iron [39]; it is not assigned here to a specific phase.
Calcium carbonate decreased between 7 and 28 days slightly in the reference (20.61 to 19.57 g/100 g), the ternary blend (23.61 to 23.21), and the CS–MK binary (23.06 to 22.64), consistent with the consumption of calcite by carboaluminate formation [37,45], and increased in the MK–PZ binary (19.03 to 21.51). The reference has the lowest 28-day carbonate content, consistent with the larger alumina supply from metakaolin for carboaluminate formation. Contents above the roughly 19% of calcite introduced with the marble powder (Mixes 17 and 18 at both ages, Mix 6 at 7 days and marginally at 28 days, and Mix 5 at 28 days) indicate some carbonation during sample preparation or storage, so differences of 1–2 g/100 g in carbonate content are not interpreted further.
At 28 days, the CS–MK binary had more bound water (8.84 g/100 g) and less portlandite (6.41) than the ternary blend (6.62 and 7.54), in line with its higher metakaolin content (12 against 6% of binder), but a lower strength (63.40 against 70.10 MPa). A shoulder at about 142 °C, in the range of C-S-H, C-A-S-H, and ettringite, is consistent with ongoing reaction of its metakaolin [52].
At 28 days, the MK–PZ binary had more bound water (8.46 g/100 g) and much less portlandite (3.70) than the ternary blend, again reflecting its higher metakaolin content (24% of binder) and a lower strength (53.85 MPa). Across the four blends, a higher metakaolin content therefore gives more bound water and less portlandite, but not a higher strength.

3.3.3. Microstructural Morphology and Chemical Composition by SEM-EDS

SEM-EDS was used to compare fracture surfaces of the four blends at 28 days (Figure 13, Figure 14, Figure 15 and Figure 16). Unlike XRD and TGA, which were performed on pastes, SEM-EDS was performed on mortar fragments, so the EDS areas may also include fine sand particles. The images are secondary-electron images, in which contrast reflects mainly topography, and each EDS analysis is the average of an area of about 87 × 65 µm (Section 2.2.6); the EDS results are therefore used only to compare the blends and do not give the composition of individual hydrates.
Figure 13. SEM images and EDS analysis of the LC3 reference (Mix 6) at 28 days: (a) 5000×; (b) 10,000×; (c) EDS analysis area (2500×) and spectrum.
Figure 14. SEM images and EDS analysis of the ternary blend (Mix 17: 60% CS, 20% MK, 20% PZ) at 28 days: (a) fragments with embedded cenospheres, 1200×; (b) matrix with a pore and a cenosphere, 5000×; (c) EDS analysis area (2500×) and spectrum.
Figure 15. SEM images and EDS analysis of the CS–MK binary (Mix 18: 60% CS, 40% MK) at 28 days: (a) fragment with embedded and broken cenospheres, 300×; (b) 5000×; (c) 10,000×; (d) EDS analysis area (2500×) and spectrum.
Figure 16. SEM images and EDS analysis of the MK–PZ binary (Mix 5: 80% MK, 20% PZ) at 28 days: (a) 5000×; (b) 10,000×; (c) EDS analysis area (2500×) and spectrum.
28 Days
The fracture surface of the LC3 reference (Figure 13a,b) has a granular texture: angular and platy particles of about 1–5 µm remain distinguishable and are only partly covered by a fine, foil-like gel, and interparticle voids of up to a few micrometres are visible. Stacks of thin plates (Figure 13b) may be portlandite or AFm phases, but morphology alone does not identify them. The EDS area analysis (Figure 13c) gave Ca/Si = 1.14 and Al/Si = 0.76, together with K and Mg, consistent with the high calcined-clay content of this blend [52].
At low magnification (Figure 14a), fragments of the ternary blend contain embedded cenospheres whose shells appear smooth, with only scattered surface deposits. At higher magnification (Figure 14b), the fracture surface is more continuous than that of the reference: most particles are embedded in a gel-like matrix, with bundles of thin lamellar plates (possibly AFm phases), sub-micrometre particles and isolated pores of a few micrometres containing fibrous products (Figure 14b). The cenosphere in Figure 14b is in contact with the surrounding paste, without a visible gap at this magnification.
The EDS area analysis of the ternary blend (Figure 14c) gave Ca/Si = 2.08 and Al/Si = 0.52. The software also reported Fe (1.6 at.%) and Ti (0.2 at.%), but their K lines barely exceed the background, so both are close to the detection limit. Because the analysed area includes a cenosphere and natural-pozzolan particles, both of which contain Fe and Ti (Table 1), these elements cannot be attributed to hydration products. This spectrum also has the lowest number of counts of the four analyses, so its ratios are the least precise.
The low-magnification image of the CS–MK binary (Figure 15a) shows a paste fragment with numerous embedded cenospheres of about 30–80 µm. Several are broken and filled with porous, granular material; one intact sphere has a small opening, and smooth spherical sockets mark spheres pulled out during fracture. This shows that paste or pore solution can enter cenospheres whose shells are broken or perforated; it does not show a reaction of the shell itself [19]. At higher magnification (Figure 15b,c), the matrix is granular, with rounded aggregates of 2–3 µm, platy crystals and voids of a few micrometres, and resembles the reference more than the ternary blend.
The EDS area analysis of the CS–MK binary (Figure 15d) gave Ca/Si = 2.24 and Al/Si = 0.76 and detected S (0.6 at.%), which may originate from ettringite, AFm phases, or residual gypsum. In the spectra of both binary blends (Figure 15d and Figure 16c), the software assigned a small peak near 0.68 keV to fluorine and quantified it at 11–12 at.%. Fluorine is not reported in the chemical analyses of the raw materials (Table 1), and the peak lies between the F Kα (0.677 keV) and Fe Lα (0.705 keV) lines; because the Fe K lines (6.40 and 7.06 keV) are absent from these spectra, it cannot be assigned to Fe either. Given its very low intensity, its standardless quantification is not reliable, and it was excluded from the interpretation.
The MK–PZ binary (Figure 16a,b) shows a dense, continuous fracture surface dominated by a crumpled, foil- or sheet-like morphology (Figure 16b), which may correspond to C-A-S-H gel or to relics of the platy metakaolin particles, and layered regions with fine microcracks, probably caused by drying (Figure 16a). The EDS area analysis (Figure 16c) gave Ca/Si = 1.36 and Al/Si = 0.71; no Fe K lines were detected.
The area-averaged Ca/Si ratios are higher in the two blends with the least metakaolin (CS–MK binary 2.24; ternary 2.08) than in the MK–PZ binary (1.36) and the reference (1.14), which broadly follows their 28-day portlandite contents measured by TGA (Table 8). With one area per blend on fracture surfaces that may include sand grains, this agreement is qualitative and is not used as independent evidence. Qualitatively, the fracture surfaces of the ternary and MK–PZ blends appear more continuous than those of the reference and the CS–MK binary, in which individual particles and interparticle voids are more visible. These observations were made on a few fields of unpolished fracture surfaces, with one EDS area per blend, and are not a measure of porosity or of hydrate composition; quantitative SEM-EDS (point analyses on polished sections, at least 30 points per blend) and image analysis of backscattered-electron images would be needed for that [35]. The individual EDS results are given in Table S4.

4. Discussion

This section summarises what the results show and which explanations remain hypotheses.

4.1. Interpretation of the Strength Gain

The best-performing mixture reached 43% more strength than the LC3 reference at 28 days, but only 3.6% more than the best metakaolin-free binary (Mix 7, whose result requires confirmation; Section 3.2.1) and 2.6% more than Mix 13, differences that are not statistically significant (Dunnett p = 0.63 and 0.94). The main statistical result is a set of positive binary interactions at 28 days, the largest being CS × PZ. Three hypotheses, which are not mutually exclusive, may explain these interactions; each is consistent with part of the data, but none is demonstrated.
Hypothesis 1.
Packing and water demand.
Cenospheres (D50 ≈ 116 µm) are much coarser than the binder powders and the natural pozzolan (D50 ≈ 3.4 µm), so combining them may improve packing and reduce water and admixture demand [18,19]. This is consistent with the better flow of cenosphere-containing mixtures at lower superplasticiser dosage (Section 3.1.1) and with the more continuous fracture surface of the ternary blend (Section 3.3.3). It would also explain why the CS × PZ interaction is the largest and why metakaolin-free CS–PZ mixtures reached high strengths (Table 5). It is also consistent with the TGA results, which show that the strength gain is not accompanied by more hydrates or more portlandite consumption (Section 3.3.2). Packing-density and porosity measurements (e.g., mercury intrusion porosimetry) would test this hypothesis directly.
Hypothesis 2.
Hydrate assemblage.
The ternary blend has the lowest bound water of the four characterised blends at 28 days, yet the highest strength, and its portlandite content increased between 7 and 28 days, indicating less pozzolanic consumption than in the reference. Across the four blends, more metakaolin gives more bound water and less portlandite, but not more strength (Section 3.3.2), so the strength gain of the ternary blend is unlikely to result from a larger amount of hydrates. The EDS area analyses cannot test this, because each averages several phases. A different gel structure therefore remains a hypothesis that requires 29Si NMR or FTIR [50,51].
Hypothesis 3.
Fe-bearing hydration products.
Fitting the 28-day XRD pattern of the ternary blend required an Fe-bearing hydrate model, which was not needed for the reference. EDS reported Fe, close to the detection limit, only in the ternary blend, in an analysis area that includes a cenosphere and natural-pozzolan particles, and not in the MK–PZ binary, so the EDS data neither confirm nor exclude Fe-bearing hydrates. The reference and ternary binders also contain similar amounts of iron (Section 3.3.1). If confirmed, uptake of iron released from the pozzolan glass by hydrates [39,48,49] could contribute to the late-age interactions involving PZ. The positive 28-day MK × PZ interaction is consistent with such a mechanism, but it is not significant at 7 days; it is the interaction most sensitive to the treatment of the anomalous mixtures, and a regression coefficient cannot identify a phase, so it cannot be used as supporting evidence.

4.2. Role of Cenospheres

The results are consistent with cenospheres acting as a low-density spherical filler that improves flow and reduces admixture demand [18,19,20]. They are not a binder, and no pozzolanic contribution could be detected within 28 days: portlandite increases as metakaolin is replaced by cenospheres and natural pozzolan, and it remains nearly constant between 7 and 28 days in the CS–MK binary, which contains 18% cenospheres (Section 3.3.2). The hydration products observed inside some cenospheres occur in broken or perforated shells and are attributed to paste or pore solution entering them, whereas intact shells appear smooth, with only scattered surface deposits (Section 3.3.3). Their aluminosilicate glass (amorphous hump in Figure 6) may nevertheless react slowly at later ages [19] and may take part in alkali–silica reaction [21]; a reactivity test on the cenospheres alone, with an inert filler of similar particle size as reference (e.g., the R3 test or the modified Chapelle test [53,54,55]), would quantify this.

4.3. Role of Natural Pozzolan

Of the two non-calcined materials, the natural pozzolan is the reactive one: its amorphous silica and alumina react with portlandite [15,16,17], although more slowly than metakaolin, which is consistent with its low single-component strength at 28 days. In the blends, the pozzolan therefore supplies the pozzolanic contribution that the cenospheres do not measurably provide, while the cenospheres improve packing and flow; this division of roles is consistent with CS × PZ being the largest interaction of the design. Because the ternary blend consumed little portlandite by 28 days (Section 3.3.2), the reaction of the pozzolan is expected to contribute mainly at later ages, which 56- and 90-day tests should verify. Its use without thermal treatment avoids calcination energy. Its high Fe2O3 content (15.07 wt%) is a characteristic of this local material; whether iron from its glassy fraction contributes to the hydrate assemblage remains to be established.

4.4. Limitations

The main limitations of this study are: (i) the design has no replicated mixtures, and two mixtures with anomalous results were excluded from the regression (Section 3.2.1), so the model and the optimal region must be confirmed by replicated validation mixtures; (ii) the superplasticiser dosage varied with composition, and its effect cannot be separated from that of composition; because W/B was fixed by mass, the binder and water contents per cubic metre also vary with the cenosphere content (Table S2); (iii) stability was assessed visually on the mini-slump patty, without a quantitative static segregation test; (iv) the XRD phase fractions are relative to the refined phases (no internal standard; amorphous content not determined), and the binary blends were not analysed by XRD; (v) the cenospheres were treated as a filler on the basis of the literature and the TGA results, but their reactivity was not measured directly, and the reaction of the natural pozzolan beyond 28 days was not quantified; (vi) only 7- and 28-day properties were measured, and durability (sulphate, chloride, and carbonation resistance, shrinkage and alkali–silica reaction of the cenosphere glass [21]) was not studied; (vii) the cenospheres and the natural pozzolan come from single sources, and their properties vary with coal type, combustion conditions, and geology [19]; and (viii) cenosphere supply is tied to coal combustion, which is expected to decline.

4.5. Application Prospects

In regions where good kaolinitic clays are scarce, the results suggest that part of the calcined clay of an LC3-type binder can be replaced by locally available natural pozzolan and by cenospheres without loss of 28-day strength and with improved flow. Potential applications include precast elements, repair mortars, and congested sections where self-compacting placement is required. Before such use, the following steps are needed: replicated validation of the optimal region; long-term strength and durability testing; verification of stability against segregation, in particular cenosphere flotation; quality control of the cenospheres (size, shell integrity, and composition) and of the pozzolan; and an assessment of cenosphere availability and cost, since processed cenospheres are a marketed product whose price may offset part of the savings (Section 5).

5. Screening-Level Environmental Assessment

Table 9 compares the mechanical, environmental and economic indicators of the reference and ternary blends. The goal, scope, and assumptions of this screening-level assessment are summarised in Table 10. Two functional units are used: one tonne of binder and one cubic metre of mortar; the baseline is the LC3 reference binder (Mix 6), not Portland cement. The system boundary is cradle-to-gate for the binder constituents: clinker production, calcination of the clay, grinding of the marble powder and natural pozzolan, and processing of the cenospheres and their road transport from the power plant (600 km). It is not a full LCA according to ISO 14040/14044 [56].
Reducing the calcined-clay content from 30 to 6 wt.% avoids the calcination of 240 kg of clay per tonne of binder, i.e., about 168–240 kWh of thermal energy and 42.7–63.6 kg CO2 (central estimate 49.2 kg CO2) [57]. Part of this saving is offset by the cenospheres (180 kg per tonne of binder), whose processing (5–10 kg CO2/t) and road transport over 600 km (0.06–0.10 kg CO2 per t·km [58]) amount to 41–70 kg CO2/t, i.e., 7.4–12.6 kg CO2 per tonne of binder, and by the grinding of the natural pozzolan (60 kg; about 1.2 kg CO2) [59,60]. With the clinker contribution unchanged (500 kg of clinker at about 850 kg CO2/t [61]), the binder footprint decreases from about 488 to 448–453 kg CO2 per tonne, a reduction of about 35–41 kg CO2 (7–8%); transport of the cenospheres accounts for 6.5–10.8 kg CO2 of the offset, so a closer source would increase the benefit. Per cubic metre of mortar (Table S2), the difference is larger, because the low-density cenospheres also reduce the binder content: the CO2 footprint of the binder constituents decreases from about 359 kg/m3 for the reference to 296–300 kg/m3 for Mix 17 (−17%); the avoided calcination and the 10% lower clinker content per cubic metre contribute in roughly equal parts, partly offset by the cenosphere processing and transport. Normalised by 28-day strength, the CO2 intensity falls from 7.4 to 4.2–4.3 kg CO2 m−3 MPa−1 (−42%) [62]. The cost of the SCM fraction depends strongly on the cenosphere price: at 15 USD/t (transport only) the ternary SCM fraction costs about 11 USD per tonne of binder against 36 USD for the reference; at 100 USD/t it costs about 26 USD; and at 300 USD/t (about 62 USD) it exceeds the reference.
Table 9. Comparison of mechanical, environmental, and economic indicators of the reference and ternary blends.
Table 10. Goal, scope and assumptions of the screening-level environmental and cost assessment.

6. Conclusions

This study examined the partial substitution of the calcined-clay fraction of an LC3-based self-compacting mortar by fly-ash cenospheres and natural pozzolan, using a {3,5} simplex-lattice design and XRD, TGA/DTG/DSC, and SEM-EDS characterisation. The main conclusions are:
Strength and workability: within a fixed 30 wt.% SCM fraction, substituting 80% of the calcined clay by cenospheres and natural pozzolan (Mix 17: 60% CS, 20% MK, 20% PZ) gave the highest 28-day strength (70.1 ± 1.5 MPa), 43% above the LC3 reference and not significantly different from Mix 13 (or from Mix 7, whose result requires confirmation), with better flow at a 20% lower superplasticiser dosage.
Mixture interactions: the 28-day Scheffé model (adjusted R2 = 0.78, fitted to 19 mixtures after excluding two anomalous ones) showed positive binary interactions, the largest being CS × PZ, which was also the only interaction significant at 7 days; the 7-day model has little predictive value. The CS × PZ and CS × MK interactions remain significant when all 21 mixtures are fitted. A predicted strength of at least 60 MPa was obtained over a broad composition region that includes metakaolin-free mixtures.
Microstructure: the best-performing mixture showed a more continuous fracture surface, the lowest bound water, and the highest portlandite content of the four characterised blends; portlandite consumption at 28 days scaled with the metakaolin content, indicating that the strength gain at this age is mainly physical: the cenospheres act as a filler with no measurable pozzolanic contribution at this age, and the natural pozzolan, the reactive component of the two, reacts more slowly than metakaolin. The SEM-EDS observations are qualitative, and the XRD fractions are relative to the refined phases.
Environment and application: reducing the calcined-clay content from 30 to 6 wt.% of the binder lowers the estimated cradle-to-gate footprint by about 35–41 kg CO2 per tonne of binder (about 8%) and by about 17% per cubic metre of mortar. Replicated validation, segregation testing, and durability testing are required before practical use.
Overall, partial substitution of the calcined clay of LC3 by cenospheres and natural pozzolan is a promising low-calcination route for regions with limited kaolinitic clay, with the combination of cenospheres and natural pozzolan providing the largest strength benefit.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/ma19235057/s1, Table S1a. Individual compressive strength results at 7 days (MPa; six half-prisms per mixture, EN 196-1). Table S1b. Individual compressive strength results at 28 days (MPa; six half-prisms per mixture, EN 196-1). Table S2. Mix proportions per cubic metre of mortar (kg/m3), calculated from the batch masses of Table 4 and the particle densities of Table 2, with a particle density of 2.78 g/cm3 for the river sand, assuming 1.5% air. Table S3. Scheffé quadratic models fitted to all 21 mixtures, including the two anomalous mixtures (Mixes 7 and 19) excluded from the models of Table 6 (coefficient ± standard error, p-value in parentheses). Table S4. EDS area analyses at 28 days (one area of about 87 × 65 µm per blend, 2500×, 10 kV, standardless quantification; atomic %). C and O are not reliably quantified and are excluded from the ratios. Figure S1. Diagnostics of the 28-day Scheffé quadratic models fitted to all 21 mixtures (top) and to the 19 mixtures of Table 6, without the anomalous Mixes 7 and 19 (bottom). Figure S2. Compressive strength at 7 and 28 days (mean ± 1 SD of six half-prisms).

Author Contributions

Conceptualisation, Y.S. and A.L.; methodology, T.B. and A.P.; software, Y.S., K.T. and P.F.; validation, T.B. and A.L.; formal analysis, Y.S. and M.B.; investigation, Y.S.; resources, Y.S. and T.B.; data curation, Y.S.; writing—original draft preparation, Y.S.; writing—review and editing, T.B.; visualisation, D.B., K.T. and B.S.; supervision, A.L.; project administration, T.B.; funding acquisition, A.P. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the Scientific Grant Agency of the Ministry of Education, Research, Development, and Youth of the Slovak Republic and the Slovak Academy of Sciences (VEGA) (grant numbers VEGA 1/0359/25 and VEGA 1/0001/25) and the Slovak Research and Development Agency (grant number APVV-25-0766).

Data Availability Statement

The original contributions presented in this study are included in the article/supplementary material. Further inquiries can be directed to the corresponding authors.

Acknowledgments

The authors would like to thank the LABMAT Laboratory, Department of Civil Engineering, National Polytechnic School of Maurice Audin Oran (ENP Oran), and SREML Laboratory, Department of Civil Engineering, Amar Telidji University, and CRAPC-PTAPC Laghouat for providing technical and laboratory support. During the preparation of this manuscript, the authors used Claude (Opus 5.5; Anthropic, San Francisco, CA, USA) for language editing and for restructuring the revised text in response to the reviewers. The statistical analysis was performed by the authors in JMP 7, and the figures were prepared by the authors in OriginPro (OriginLab Corporation, Northampton, MA, USA) 2018. The authors have reviewed and edited the output and take full responsibility for the content of this publication.

Conflicts of Interest

The authors declare no conflicts of interest.

Abbreviations

The following abbreviations are used in this manuscript:
C-A-S-Hcalcium aluminosilicate hydrate
C-S-Hcalcium silicate hydrate
CKClinker
CSCenospheres
DoEdesign of experiments
DSCdifferential scanning calorimetry
DTGderivative thermogravimetry
EDSenergy-dispersive X-ray spectroscopy
FWHMfull width at half maximum
GyGypsum
LC3limestone calcined clay cement
LCAlife cycle assessment
LOIloss on ignition
MKMetakaolin
MPmarble powder
NDnot detected
PZnatural pozzolan
RSriver sand
SCMssupplementary cementitious materials
SEMscanning electron microscopy
SIsynergy index
SPSuperplasticiser
TGAthermogravimetric analysis
W/Bwater-to-binder ratio
XRDX-ray diffraction

References

  1. Andrew, R.M. Global CO2 emissions from cement production. Earth Syst. Sci. Data 2018, 10, 195–217. [Google Scholar] [CrossRef] [Scilit]
  2. Scrivener, K.L.; John, V.M.; Gartner, E.M. Eco-efficient cements: Potential economically viable solutions for a low-CO2 cement-based materials industry. Cem. Concr. Res. 2018, 114, 2–26. [Google Scholar] [CrossRef] [Scilit]
  3. Huang, G.; Zhuge, Y.; Benn, B.T.; Liu, Y. Environmental Assessment of Limestone Calcined Clay Cement in Australia. IOP Conf. Ser. Mater. Sci. Eng. 2023, 1289, 012082. [Google Scholar] [CrossRef] [Scilit]
  4. Humagain, S.; Shrestha, G.; Madhavan, M.K.; Sarker, P.K. Hydration, Soundness, and Strength of Low Carbon LC3 Mortar Using Waste Brick Powder as a Source of Calcined Clay. Materials 2025, 18, 3697. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  5. Basavaraj, A.S.; Muni, H.; Dhandapani, Y.; Gettu, R.; Santhanam, M. Limestone-Calcined Clay (LC2) as a supplementary cementitious material for concrete. RILEM Tech. Lett. 2023, 8, 12–22. [Google Scholar] [CrossRef] [Scilit]
  6. EN 197-1:2011; Cement—Part 1: Composition, Specifications and Conformity Criteria for Common Cements. European Committee for Standardization: Brussels, Belgium, 2011.
  7. Scrivener, K.; Avet, F.; Maraghechi, H.; Zunino, F.; Ston, J.; Hanpongpun, W.; Favier, A. Impacting factors and properties of limestone calcined clay cements (LC3). Green Mater. 2019, 7, 3–14. [Google Scholar] [CrossRef] [Scilit]
  8. Scrivener, K.; Martirena, F.; Bishnoi, S.; Maity, S. Calcined clay limestone cements (LC3). Cem. Concr. Res. 2018, 114, 49–56. [Google Scholar] [CrossRef] [Scilit]
  9. Kafodya, I.; Basuroy, D.; Marangu, J.M.; Kululanga, G.; Maddalena, R.; Novelli, V.I. Mechanical Performance and Physico-Chemical Properties of Limestone Calcined Clay Cement (LC3) in Malawi. Buildings 2023, 13, 740. [Google Scholar] [CrossRef] [Scilit]
  10. Sharma, M.; Bishnoi, S.; Martirena, F.; Scrivener, K. Limestone calcined clay cement and concrete: A state-of-the-art review. Cem. Concr. Res. 2021, 149, 106564. [Google Scholar] [CrossRef] [Scilit]
  11. Rodrigues, A.L.M.V.; Mendes, Á.Á.F.; Gomes, V.; Battagin, A.F.; Saade, M.R.M.; Da Silva, M.G. Environmental and Mechanical Evaluation of Blended Cements With High Mineral Admixture Content. Front. Mater. 2022, 9, 880986. [Google Scholar] [CrossRef] [Scilit]
  12. Parashar, A.; Bishnoi, S. Hydration behaviour of limestone-calcined clay and limestone-slag blends in ternary cement. RILEM Tech. Lett. 2021, 6, 17–24. [Google Scholar] [CrossRef] [Scilit]
  13. Avet, F.; Scrivener, K. Investigation of the calcined kaolinite content on the hydration of Limestone Calcined Clay Cement (LC3). Cem. Concr. Res. 2018, 107, 124–135. [Google Scholar] [CrossRef] [Scilit]
  14. Vargas, P.; Borrachero, M.V.; Payá, J.; Macián, A.; Tobón, J.I.; Martirena, F.; Soriano, L. Optimisation of Using Low-Grade Kaolinitic Clays in Limestone Calcined Clay Cement Production (LC3). Materials 2025, 18, 285. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  15. Danner, T.; Norden, G.; Justnes, H. Calcareous smectite clay as a pozzolanic alternative to kaolin. Eur. J. Environ. Civ. Eng. 2021, 25, 1647–1664. [Google Scholar] [CrossRef] [Scilit]
  16. Adegbemileke, S.A.; Osuji, S.O.; Ogirigbo, O.R. Exploring the Potential of Nigerian Clay-Based Pozzolans for Enhancing Concrete Performance and Sustainability: A Study on Strength, Hydration, and Durability. J. Eng. 2024, 30, 1–20. [Google Scholar] [CrossRef] [Scilit]
  17. Yoon, J.; Jafari, K.; Tokpatayeva, R.; Peethamparan, S.; Olek, J.; Rajabipour, F. Characterization and quantification of the pozzolanic reactivity of natural and non-conventional pozzolans. Cem. Concr. Compos. 2022, 133, 104708. [Google Scholar] [CrossRef] [Scilit]
  18. Mahato, J.; Yang, J.; Lee, N.; Kang, H.; Moon, J. Incorporation of a high volume of cenosphere particles in low water-to-cement matrix for developing high strength and lightweight cementitious composites. J. Sustain. Cem.-Based Mater. 2023, 12, 580–591. [Google Scholar] [CrossRef] [Scilit]
  19. Hanif, A.; Lu, Z.; Li, Z. Utilization of fly ash cenosphere as lightweight filler in cement-based composites—A review. Constr. Build. Mater. 2017, 144, 373–384. [Google Scholar] [CrossRef] [Scilit]
  20. Blanco, F.; García, P.; Mateos, P.; Ayala, J. Characteristics and properties of lightweight concrete manufactured with cenospheres. Cem. Concr. Res. 2000, 30, 1715–1722. [Google Scholar] [CrossRef] [Scilit]
  21. Wang, J.Y.; Zhang, M.H.; Li, W.; Chia, K.S.; Liew, R.J.Y. Stability of cenospheres in lightweight cement composites in terms of alkali–silica reaction. Cem. Concr. Res. 2012, 42, 721–727. [Google Scholar] [CrossRef] [Scilit]
  22. Montgomery, D.C. Design and Analysis of Experiments, 9th ed.; John Wiley & Sons: Hoboken, NJ, USA, 2017. [Google Scholar]
  23. Cornell, J.A. Experiments with Mixtures: Designs, Models, and the Analysis of Mixture Data, 3rd ed.; John Wiley & Sons: New York, NY, USA, 2002. [Google Scholar]
  24. Huang, G.; Liu, Y.; Benn, T.; Luo, L.; Xie, T.; Zhuge, Y. A Comprehensive Framework for the Design and Optimisation of Limestone-Calcined Clay Cement: Integrating Mechanical, Environmental, and Financial Performance. J. Compos. Sci. 2024, 8, 524. [Google Scholar] [CrossRef] [Scilit]
  25. Lin, R.-S.; Liao, Y.; Han, Y.; Oh, S.; Park, K.-B.; Yang, H.-M.; Wang, X.-Y.; Yang, B.; Meng, L.-Y. Low-CO2 Optimization Design of Quaternary Binder Containing Calcined Clay, Slag, and Limestone. Materials 2023, 16, 6385. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  26. Mukherjee, S.; Kumar, R.; Behera, M.; Goyal, A.; Rahman, M.R. Rheology, mechanical properties and microstructure characterization of limestone calcined clay cement (LC3) incorporated sustainable lightweight self-compacting concrete. Dev. Built Environ. 2025, 21, 100601. [Google Scholar] [CrossRef] [Scilit]
  27. Nair, N.; Mohammed Haneefa, K.; Santhanam, M.; Gettu, R. A study on fresh properties of limestone calcined clay blended cementitious systems. Constr. Build. Mater. 2020, 254, 119326. [Google Scholar] [CrossRef] [Scilit]
  28. Chen, Y.; Zhang, Y.; He, S.; Liang, M.; Zhang, Y.; Schlangen, E.; Çopuroğlu, O. Rheology control of limestone calcined clay cement pastes by modifying the content of fine-grained metakaolin. J. Sustain. Cem.-Based Mater. 2023, 12, 1126–1140. [Google Scholar] [CrossRef] [Scilit]
  29. Muzenda, T.R.; Hou, P.; Kawashima, S.; Sui, T.; Cheng, X. The role of limestone and calcined clay on the rheological properties of LC3. Cem. Concr. Compos. 2020, 107, 103516. [Google Scholar] [CrossRef] [Scilit]
  30. Kandagaddala, R.K.; Nanthagopalan, P. Rheological Characterization of Cementitious Suspensions with Limestone Calcined Clay for Pumping Applications. J. Mater. Civ. Eng. 2022, 34, 04022158. [Google Scholar] [CrossRef] [Scilit]
  31. Fernandez, R.; Martirena, F.; Scrivener, K.L. The origin of the pozzolanic activity of calcined clay minerals: A comparison between kaolinite, illite and montmorillonite. Cem. Concr. Res. 2011, 41, 113–122. [Google Scholar] [CrossRef] [Scilit]
  32. EFNARC. Specification and Guidelines for Self-Compacting Concrete; European Federation for Specialist Construction Chemicals and Concrete Systems (EFNARC): Norfolk, UK, 2002. [Google Scholar]
  33. Okamura, H.; Ouchi, M. Self-compacting concrete. J. Adv. Concr. Technol. 2003, 1, 5–15. [Google Scholar] [CrossRef] [Scilit]
  34. EN 196-1:2016; Methods of Testing Cement—Part 1: Determination of Strength. European Committee for Standardization: Brussels, Belgium, 2016.
  35. Scrivener, K.; Snellings, R.; Lothenbach, B. (Eds.) A Practical Guide to Microstructural Analysis of Cementitious Materials; CRC Press: Boca Raton, FL, USA, 2016. [Google Scholar]
  36. Scarlett, N.V.Y.; Madsen, I.C. Quantification of phases with partial or no known crystal structures. Powder Diffr. 2006, 21, 278–284. [Google Scholar] [CrossRef] [Scilit]
  37. Lothenbach, B.; Le Saout, G.; Gallucci, E.; Scrivener, K. Influence of limestone on the hydration of Portland cements. Cem. Concr. Res. 2008, 38, 848–860. [Google Scholar] [CrossRef] [Scilit]
  38. Lothenbach, B.; Scrivener, K.; Hooton, R.D. Supplementary cementitious materials. Cem. Concr. Res. 2011, 41, 1244–1256. [Google Scholar] [CrossRef] [Scilit]
  39. Dilnesa, B.Z.; Wieland, E.; Lothenbach, B.; Dähn, R.; Scrivener, K.L. Fe-containing phases in hydrated cements. Cem. Concr. Res. 2014, 58, 45–55. [Google Scholar] [CrossRef] [Scilit]
  40. Newbury, D.E.; Ritchie, N.W.M. Is scanning electron microscopy/energy dispersive X-ray spectrometry (SEM/EDS) quantitative? Scanning 2013, 35, 141–168. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  41. Goldstein, J.I.; Newbury, D.E.; Michael, J.R.; Ritchie, N.W.M.; Scott, J.H.J.; Joy, D.C. Scanning Electron Microscopy and X-Ray Microanalysis, 4th ed.; Springer: New York, NY, USA, 2018. [Google Scholar]
  42. Sabir, B.B.; Wild, S.; Bai, J. Metakaolin and calcined clays as pozzolans for concrete: A review. Cem. Concr. Compos. 2001, 23, 441–454. [Google Scholar] [CrossRef] [Scilit]
  43. Briki, Y.; Avet, F.; Zajac, M.; Bowen, P.; Haha, M.B.; Scrivener, K. Understanding of the factors slowing down metakaolin reaction in limestone calcined clay cement (LC3) at late ages. Cem. Concr. Res. 2021, 146, 106477. [Google Scholar] [CrossRef] [Scilit]
  44. Antoni, M.; Rossen, J.; Martirena, F.; Scrivener, K. Cement Substitution by a Combination of Metakaolin and Limestone. Cem. Concr. Res. 2012, 42, 1579–1589. [Google Scholar] [CrossRef] [Scilit]
  45. Matschei, T.; Lothenbach, B.; Glasser, F.P. The role of calcium carbonate in cement hydration. Cem. Concr. Res. 2007, 37, 551–558. [Google Scholar] [CrossRef] [Scilit]
  46. Sun, J.; Zunino, F.; Scrivener, K. Hydration and phase assemblage of limestone calcined clay cements (LC3) with clinker content below 50%. Cem. Concr. Res. 2024, 177, 107417. [Google Scholar] [CrossRef] [Scilit]
  47. Dhandapani, Y.; Sakthivel, T.; Santhanam, M.; Gettu, R.; Pillai, R.G. Mechanical properties and durability performance of concretes with Limestone Calcined Clay Cement (LC3). Cem. Concr. Res. 2018, 107, 136–151. [Google Scholar] [CrossRef] [Scilit]
  48. Baral, A.; Pesce, C.; Yorkshire, A.S.; Zhakiyeva, Z.; Snellings, R.; Hanein, T.; Provis, J.L.; Peys, A. Characterisation of iron-rich cementitious materials. Cem. Concr. Res. 2024, 177, 107419. [Google Scholar] [CrossRef] [Scilit]
  49. Noguchi, N.; Siventhirarajah, K.; Chabayashi, T.; Kato, H.; Nawa, T.; Elakneswaran, Y. Hydration of ferrite-rich Portland cement: Evaluation of Fe-hydrates and Fe uptake in calcium-silicate-hydrates. Constr. Build. Mater. 2021, 288, 123142. [Google Scholar] [CrossRef] [Scilit]
  50. Andersen, M.D.; Jakobsen, H.J.; Skibsted, J. A new aluminium-hydrate species in hydrated Portland cements characterized by 27Al and 29Si MAS NMR spectroscopy. Cem. Concr. Res. 2006, 36, 3–17. [Google Scholar] [CrossRef] [Scilit]
  51. Richardson, I.G. The calcium silicate hydrates. Cem. Concr. Res. 2008, 38, 137–158. [Google Scholar] [CrossRef] [Scilit]
  52. Avet, F.; Boehm-Courjault, E.; Scrivener, K. Investigation of C-A-S-H composition, morphology and density in Limestone Calcined Clay Cement (LC3). Cem. Concr. Res. 2019, 115, 70–79. [Google Scholar] [CrossRef] [Scilit]
  53. Skibsted, J.; Snellings, R. Reactivity of supplementary cementitious materials (SCMs) in cement blends. Cem. Concr. Res. 2019, 124, 105799. [Google Scholar] [CrossRef] [Scilit]
  54. Avet, F.; Snellings, R.; Alujas Diaz, A.; Ben Haha, M.; Scrivener, K. Development of a new rapid, relevant and reliable (R3) test method to evaluate the pozzolanic reactivity of calcined kaolinitic clays. Cem. Concr. Res. 2016, 85, 1–11. [Google Scholar] [CrossRef] [Scilit]
  55. Li, X.; Snellings, R.; Antoni, M.; Alderete, N.M.; Ben Haha, M.; Bishnoi, S.; Cizer, Ö.; Cyr, M.; De Weerdt, K.; Dhandapani, Y.; et al. Reactivity tests for supplementary cementitious materials: RILEM TC 267-TRM phase 1. Mater. Struct. 2018, 51, 151. [Google Scholar] [CrossRef] [Scilit]
  56. ISO 14040:2006; Environmental Management—Life Cycle Assessment—Principles and Framework. International Organization for Standardization: Geneva, Switzerland, 2006.
  57. Tasiopoulou, T.; Katsourinis, D.; Giannopoulos, D.; Founti, M. Production-Process Simulation and Life-Cycle Assessment of Metakaolin as Supplementary Cementitious Material. Eng 2023, 4, 761–779. [Google Scholar] [CrossRef] [Scilit]
  58. Smart Freight Centre. Global Logistics Emissions Council (GLEC) Framework for Logistics Emissions Accounting and Reporting, Version 3.0; Smart Freight Centre: Amsterdam, The Netherlands, 2023. [Google Scholar]
  59. Tang, W.; Pignatta, G.; Sepasgozar, S.M.E. Life-Cycle Assessment of Fly Ash and Cenosphere-Based Geopolymer Material. Sustainability 2021, 13, 11167. [Google Scholar] [CrossRef] [Scilit]
  60. Kupwade-Patil, K.; De Wolf, C.; Chin, S.; Ochsendorf, J.; Hajiah, A.E.; Al-Mumin, A.; Büyüköztürk, O. Impact of Embodied Energy on Materials/Buildings with Partial Replacement of Ordinary Portland Cement (OPC) by Natural Pozzolanic Volcanic Ash. J. Clean. Prod. 2018, 177, 547–554. [Google Scholar] [CrossRef] [Scilit]
  61. International Energy Agency (IEA). Cement: Tracking Clean Energy Progress; IEA: Paris, France, 2022; Available online: https://www.iea.org/energy-system/industry/cement (accessed on 8 October 2026).
  62. Damineli, B.L.; Kemeid, F.M.; Aguiar, P.S.; John, V.M. Measuring the eco-efficiency of cement use. Cem. Concr. Compos. 2010, 32, 555–562. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.