Abstract
This study investigates interfacial reactions, intermetallic compound evolution, and impact-related dynamic shear reliability of Ga-incorporated Sn–Ag–Cu composite (SACG) solder joints on ENIG substrates. Interfacial reaction layers were developed by soldering reactions at 230–270 °C for 5–40 min, followed by isothermal aging at 120 °C for 200–1000 h. Microstructural characterization was performed using SEM/EDS and XRD. The initial reaction at all temperatures rapidly forms a Ga-containing diffusion layer of (Ni,Cu)2Ga3, whose growth is limited to approximately 1 µm. With longer reaction durations and higher temperatures, an upper brittle layer of (Ni,Cu)3Sn4 thickened on top of (Ni,Cu)2Ga3, giving rise to a two-layer IMC architecture. Importantly, the subsequent solid-state aging behavior strongly depended on the initial reaction condition: after a 230 °C/40 min reaction, (Ni,Cu)3Sn4 emerged during aging (≥500 h), whereas a shorter 230 °C/10 min reaction suppressed (Ni,Cu)3Sn4 formation even after 1000 h. High-speed ball shear tests performed at a shear speed of 1 m/s demonstrate a transition from ductile to brittle fracture governed by the development and continuity of the (Ni,Cu)3Sn4 layer. As the brittle fracture fraction increases, dynamic shear strength systematically decreases. Overall, the results demonstrate that tailoring the reaction time and temperature to stabilize (Ni,Cu)2Ga3 and suppress excessive growth of (Ni,Cu)3Sn4 is critical for improving the impact-related reliability of SACG/ENIG solder joints.
1. Introduction
The rapid advancement of the modern microelectronics industry and the increasing demand for high-performance, multifunctional devices have driven continuous miniaturization and higher-density integration in semiconductor packaging technologies. In advanced packaging architectures, solder joints act as critical electrical interconnects while simultaneously providing mechanical support and heat-dissipation pathways between the die and the substrate [1,2,3]. Consequently, the mechanical integrity and interfacial reliability of solder joints strongly influence overall system lifetime and structural stability under operational loading conditions.
For decades, lead-containing solders were widely used due to their excellent wettability, reliable bonding performance, and cost-effective manufacturability. However, environmental regulations, such as the Restriction of Hazardous Substances (RoHS) directive, restrict the use of lead in consumer electronics [4]. To address these requirements, extensive efforts have led to the development of lead-free solder systems. Among them, Sn–Ag–Cu (SAC) alloys—particularly SAC305 (Sn–3.0Ag–0.5Cu)—have become a mainstream choice owing to their balanced mechanical properties, relatively low melting temperature compared with alternative systems, and compatibility with existing manufacturing processes [5,6,7,8].
Despite these advantages, Sn-based lead-free solders still suffer from intrinsic reliability limitations associated with thermal aging. In particular, microstructural coarsening and excessive growth of brittle intermetallic compounds (IMCs) can degrade joint performance over time. Therefore, alloying and microstructural engineering using minor additive elements have been widely investigated to improve thermal–mechanical resilience. Gallium (Ga) has attracted significant attention as a promising dopant for Sn-based solders. Previous studies have reported that small Ga additions can suppress interfacial IMC growth kinetics, modify interfacial reaction behavior and grain morphology, and lower the melting temperature of the solder matrix [9,10,11,12,13,14,15]. For example, Zhang et al. [9] showed that trace Ga addition depresses the liquidus temperature and refines the bulk microstructure. In addition, Ga can suppress the excessive formation of interfacial Cu–Sn IMCs (e.g., Cu6Sn5 and Cu3Sn), thereby improving mechanical strength and long-term reliability. Collectively, these effects suggest that Ga is highly effective for enhancing the long-term reliability of solder joints.
However, practical implementation of Ga-containing composite solders faces a key manufacturing challenge. Unlike many conventional alloying elements or solid reinforcements (e.g., Al2O3, TiO2, or carbon-based nanomaterials), Ga is a liquid near room temperature due to its low melting point (approximately 29.8 °C). As a result, Ga is difficult to produce as stable dry powders under ambient conditions and cannot be easily incorporated through conventional powder metallurgy or direct dry blending. Although Ga-containing composite solders are often fabricated via casting, it remains difficult to precisely control the size and distribution of minor Ga constituents within the final alloy microstructure, often leading to severe macro-segregation and inconsistent mechanical or interfacial properties. To enable reproducible Ga-containing microstructures, specialized processing routes are required to convert bulk liquid Ga into stable micro- or nano-sized dispersions. Among various approaches, ultrasonic liquid dispersion (sonochemical processing) has been recognized as an effective strategy to generate metal microparticles and composite structures derived from molten Ga [16,17,18,19,20,21]. During sonication, acoustic cavitation in a suitable immiscible medium overcomes the high interfacial tension of Ga and allows liquid Ga to be dispersed into relatively uniform microparticles [19,20,21]. Leveraging this principle, our developed dispersion-assisted fabrication method offers superior microstructural homogeneity and precise compositional control compared to conventional casting routes, providing a highly practical pathway to uniformly incorporate Ga microparticles into solder matrices.
Owing to the distinct physical properties of Ga and the associated fabrication constraints, systematic studies on the high-speed dynamic mechanical behavior of Ga-reinforced composite solders remain limited. In this work, we developed a Ga-containing composite solder by incorporating Ga microparticles prepared via ultrasonic liquid dispersion into a Sn–Ag–Cu matrix. The solder was reacted on an Electroless Nickel Immersion Gold (ENIG) finish, which is widely used in high-density electronic assemblies due to its excellent surface flatness and oxidation resistance [22]. To evaluate both long-term reliability and thermal stability, the solder joints were subjected to accelerated isothermal aging. The evolution of interfacial microstructures was systematically examined by characterizing phase transformations and morphology changes at the solder/ENIG interface before and after aging.
Furthermore, conventional low-speed shear testing may not adequately represent the dynamic drop-impact reliability relevant to modern portable electronics. Accordingly, this study evaluates joint mechanical integrity using high-speed ball shear testing. The dynamic shear force and fracture modes are analyzed to clarify how ultrasonically dispersed Ga microparticles contribute to interfacial stabilization and mechanical reinforcement under high-rate loading conditions [23,24].
2. Materials and Methods
2.1. Materials
A Sn–3.0Ag–0.5Cu (SAC305) solder paste (M705-GRN360-K2-V, particle size 25–36 μm) and gallium (Ga, 99.999%, Thermo Fisher Scientific, Waltham, MA, USA) were used to fabricate the Ga-incorporated composite solder. The reaction substrates were ENIG-surface-finished substrates consisting of electroless Ni–P with a thickness of 5 μm and a Au layer with a thickness of 0.03 μm.
Gallium microparticles were synthesized via an ultrasonic liquid dispersion method. First, 1 g of Ga was placed into a 50 mL conical tube containing 20 mL of acetone. Ultrasonication was performed for 20 min using an ultrasonic processor (Branson Ultrasonic 4520AA, Branson Ultrasonics Corp., Brookfield, CT, USA) operating at a frequency of 20 kHz and a maximum power of 2800 W, with the output amplitude set to 10% (280 W). Upon completion of sonication, the suspension was left undisturbed until the dispersed Ga particles settled, after which the supernatant acetone was carefully decanted. Subsequently, the conical tube containing the sedimented Ga particles was immersed in liquid nitrogen (−196 °C) for 1 min to induce rapid cryo-solidification. Finally, the solidified Ga microparticles were collected and handled in a temperature-controlled laboratory maintained at 20 °C to prevent remelting prior to composite solder fabrication.
To verify the morphology and size distribution of the dispersed Ga particles, representative characterization results are shown in Figure 1. The average particle size was measured to be 2.03 ± 0.25 μm. The spatial distribution of Ga particles within the composite solder was examined using EDS elemental mapping after heat treatment at 210 °C for 1 min (Figure 1c). The results indicate that Ga atoms diffuse into the SAC305 matrix prior to reaching the SAC305 melting temperature (~217 °C). According to the Sn–Ga binary phase diagram [25], approximately 1.5 wt% Ga can dissolve into solid Sn, while the excess Ga exists as a liquid phase. Although the solder used in this study is SAC305 (i.e., consisting of pure Sn with small amounts of Ag and Cu), when 2 wt% Ga is added at 210 °C, it is reasonable to expect that ~1.5 wt% Ga dissolves into the solid Sn phase, whereas the remaining ~0.5 wt% Ga is likely to remain in a liquid state and segregate at local regions such as the solder surface and/or interfaces. However, Ga is expected to mix completely with the molten solder above its melting temperature.
Figure 1.
(a) Morphology and (b) size distribution of ultrasonically dispersed Ga particles. (c) EDS elemental mapping of the SACG/ENIG joint after reaction at 210 °C for 1 min.
2.2. Preparation of Composite Solders and Heat Treatment
Ga microparticles were incorporated into the SAC305 solder paste using a plane-planetary mixer (PDM-300, Daehwa Tech Co., Ltd., Yongin, Republic of Korea). Initially, SAC305 paste was mixed at a plane rotation speed of 800 rpm and a revolution speed of 500 rpm. Ga microparticles were then added to achieve a Ga content of 2 wt%. The mixture was subsequently homogenized through repeated mixing cycles at the same speed conditions for 1 min per cycle, with three additional mixing steps to ensure uniform dispersion. The resulting material is referred to as SACG composite solder.
For interfacial reaction observations, the SACG composite solders were stencil-printed onto ENIG substrates. The fabrication process is schematically illustrated in Figure 2. The substrate had a circular pad diameter of 400 μm, and the composite solder paste was printed using a stencil mask with a thickness of 200 μm, yielding a heat-treated solder bump height of approximately 200 μm. No additional flux was applied beyond that inherently contained within the commercial SAC305 solder paste. All soldering reactions were conducted in an ambient air atmosphere. Specifically, the specimens were directly inserted into a preheated furnace and isothermally reacted at 230, 250, and 270 °C for various durations of 1, 5, 10, 20, and 40 min to examine the time-dependent interfacial microstructural evolution, followed by natural air cooling to room temperature for 30 min. To assess long-term reliability, isothermal aging was further performed at 120 °C for 200 h, 500 h, and 1000 h to investigate the stability of interfacial reactions and the progression of IMC growth.
Figure 2.
Schematic illustration of Ga dispersion and the composite solder fabrication process.
2.3. Characterization
After thermal exposure and aging, specimens were cold-mounted, followed by mechanical polishing to obtain cross-sectional microstructure samples. To clearly reveal IMC formation and interfacial layers, chemical etching was performed using an etchant solution composed of ethanol (C2H6O), nitric acid (HNO3), and hydrochloric acid (HCl) in a volumetric ratio of 95:4:1.
Cross-sectional microstructures were characterized using field emission scanning electron microscopy (FE-SEM, JSM-7900F, JEOL Ltd., Akishima, Tokyo, Japan) combined with energy dispersive spectroscopy (EDS, JXA-8500F, JEOL Ltd., Akishima, Tokyo, Japan) for elemental analysis and mapping. Phase identification was carried out by X-ray diffraction (XRD, SmartLab, Rigaku Corporation, Akishima, Tokyo, Japan) to determine crystallographic phases formed at the solder/ENIG interface.
The mechanical reliability of solder joints was evaluated using high-speed ball shear tests. A Dage 4000HS system (Nordson DAGE, Aylesbury, UK) was employed. Ball shear testing was conducted at a shear speed of 1000 mm/s. The shear punch height was set to 30 μm above the substrate surface. For each experimental condition, ten independent ball shear tests were performed (n = 10) to ensure statistical reliability of the dynamic shear response.
3. Results and Discussion
3.1. Interfacial IMC Evolution During Soldering and Thermal Aging
Figure 3 illustrates the interfacial microstructures developed between the SACG composite solder and the ENIG finish after thermal reactions at 230, 250, and 270 °C for 5–40 min. During the initial stage of interfacial reaction, a Ga-containing intermetallic compound, , rapidly forms at the solder/ENIG interface for all tested temperatures. This preferential interfacial formation indicates that Ga readily participates in early-stage interdiffusion and reaction with Ni–Cu species from the ENIG finish.
Figure 3.
Cross-sectional SEM images of SACG/ENIG solder joints reacted at (a–d) 230 °C, (e–h) 250 °C, and (i–l) 270 °C for various reaction times. (Scale bar: 1 µm).
With increasing reaction time, additional interfacial products emerge. After persists and thickens slightly, a secondary phase, , nucleates and grows on top of the Ga-containing layer. As a result, the interfacial IMC structure evolves from an initial single-layer morphology to a distinct two-layer configuration. This layered evolution suggests a time-dependent change in the dominant reaction kinetics: early growth is governed by Ga-assisted compound formation, whereas later-stage growth becomes progressively dominated by Sn-driven intermetallic development.
Beneath , the Ni–P layer of ENIG undergoes progressive Ni depletion as the reaction proceeds. A thin P-rich dark layer forms at the /Ni–P interface, as indicated by the arrows in Figure 3f,j. Importantly, the thickness of remains limited throughout the entire reaction range, not exceeding approximately 1 µm even at longer reaction times. This restrained growth is consistent with the role of Ga in moderating interfacial reaction kinetics and stabilizing the IMC sequence. As develops and thickens, Ni consumption from the underlying Ni–P layer accelerates, leading to a more pronounced degradation of the Ni–P microstructure, which becomes evident in Figure 3l under long-time/high-temperature conditions. Overall, Figure 3 demonstrates a clear time- and temperature-dependent interfacial reaction mechanism: early formation of , followed by subsequent emergence of an upper layer accompanied by progressive P-rich layer formation and Ni–P degradation during extended reaction.
Meanwhile, during the interfacial reaction between Ga-free Sn-Ag-Cu solders and ENIG substrates, needle-type or polygonal (Cu,Ni)6Sn5 IMCs preferentially form at the uppermost interface when the Cu concentration in the solder exceeds approximately 0.4–0.5 wt.% (e.g., SAC305 and SAC387). However, when the Cu content is insufficient or becomes depleted in the solder matrix, a layer-type (Ni,Cu)3Sn4 phase nucleates and grows beneath the pre-existing (Cu,Ni)6Sn5 layer [26,27,28]. Furthermore, prolonged high-temperature aging (at 125–150 °C) accelerates the growth of this (Ni,Cu)3Sn4 phase, accompanied by a pronounced thickening of the underlying P-rich layer [29,30,31].
Based on these comparative findings, whereas the phase transition from (Cu,Ni)6Sn5 to (Ni,Cu)3Sn4 in Ga-free systems is governed simply by Cu consumption, the formation of (Ni,Cu)3Sn4 atop the (Ni,Cu)2Ga3 layer in the Ga-containing solder system requires a substantially prolonged incubation period. During this extended timeframe, the (Ni,Cu)2Ga3 phase effectively suppresses the nucleation and growth of (Ni,Cu)3Sn4, thereby demonstrating its remarkable capability as an interfacial diffusion barrier.
Figure 4 presents the cross-sectional microstructures of SACG joints reacted at 230 °C for 10 and 40 min, followed by isothermal aging at 120 °C for 200–1000 h. The aging behavior strongly depends on the initial interfacial condition established during the preceding soldering step. For the specimen initially reacted at 230 °C for 40 min, the interfacial IMC is dominated by up to 200 h. After longer aging (≥500 h), begins to appear and coexists with , forming a clear two-layer IMC structure. This delayed emergence indicates that Sn-driven growth requires sufficient interdiffusion, which becomes feasible only after prolonged aging partially modifies the effective interfacial barrier conditions.
Figure 4.
Cross-sectional SEM images of joints bonded at 230 °C for (a–c) 10 min and (d–f) 40 min, followed by aging at 120 °C for various durations (scale bar: 1 µm).
In contrast, the specimen reacted at 230 °C for only 10 min exhibits markedly improved stability against further IMC evolution. Even after aging up to 1000 h, only is detected, and no upper layer is observed. In addition, the growth of remains limited during aging. These findings indicate that a sufficiently established layer effectively retards the transport of Sn-containing species necessary for nucleation and growth. The comparison between the 10 min and 40 min initial reactions further highlights that both the initial formation state and the degree of interfacial conditioning critically determine long-term reliability.
Figure 5 shows the interfacial microstructures of SACG joints reacted at 270 °C for 10 and 40 min, followed by isothermal aging at 120 °C for 200–1000 h. The overall aging trend is consistent with that observed for the 230 °C soldering route, confirming the robustness of the Ga-assisted interfacial evolution mechanism. For the specimen reacted at 270 °C for 10 min, does not form even after aging up to 1000 h, again demonstrating the strong diffusion-barrier capability of the initially formed layer. However, compared with the 230 °C route, a slightly higher propensity for further development is observed over extended aging, suggesting that the higher thermal reaction temperature can promote more noticeable interfacial rearrangement during long-duration solid-state exposure.
Figure 5.
Cross-sectional SEM images of joints bonded at 270 °C for (a–c) 10 min and (d–f) 40 min, followed by aging at 120 °C for various durations. (Scale bar: 1 µm).
For the specimen reacted at 270 °C for 40 min, interfacial evolution becomes more pronounced. After 200 h of aging, is clearly formed above the Ga-containing layer, and a two-layer IMC configuration is established. As aging proceeds to longer times, the layer thickness increases substantially. Notably, after 1000 h of aging, cracking is observed along the / interface. Such interfacial cracking implies that continued aging may promote embrittlement-driven fracture along this brittle boundary under subsequent impact/shear loading, which is relevant to long-life reliability design.
Wang et al. [32] investigated solid-state interfacial reactions at 160–200 °C and reported that the Ni3Sn4 phase dominated the reaction with a 0.5 wt% Ga addition, whereas increasing the Ga content to 1 wt% resulted in only a thin Ni2Ga3 layer even after aging at 160 °C for over 1200 h. In the present study, controlled soldering conditions (10 min at 230–270 °C) enabled the formation of a stable diffusion barrier. Under these conditions, the layer remained sufficiently stable even after solid-state aging for up to 1000 h, suppressing the formation of and thereby maintaining its barrier effectiveness.
Although Ga-containing Sn-based solders reacted with Cu can produce IMCs such as or [9,11], reactions with Ni generally lead to the formation of as the dominant Ga-containing intermetallic phase [32]. However, reports on the interfacial reaction behavior between Ga-modified Sn-based solders and ENIG finishes remain limited. In this study, the interfacial IMCs formed during thermal reactions were therefore examined using EDS and XRD. Figure 6 presents representative cross-sectional SEM images and corresponding EDS line-scan results for specimens reacted at (a) 230 °C for 10 min and (b) 250 °C for 40 min. For the 230 °C/10 min specimen, the EDS-derived atomic ratio Ni:Cu:Ga is approximately 21:13:55, which falls within the expected composition range for . For the 250 °C/40 min specimen, the measured atomic ratio is approximately 30:0:42, which is consistent with a -type Ga-rich intermetallic phase. In particular, Cu is not expected to be present in the Ni–P region; therefore, the Cu-related signal within that region is likely close to the noise level. This supports the conclusion that the interfacial Ga-containing IMC is predominantly consistent with phase under the corresponding reaction conditions.
Figure 6.
Cross-sectional SEM micrographs and EDS line-scan profiles of specimens reacted at (a) 230 °C for 10 min and (b) 250 °C for 40 min.
Figure 7 presents the XRD patterns of SACG/ENIG specimens reacted at 230–270 °C for different reaction times. Before XRD measurement, the solder remaining after completion of interfacial reactions was completely etched. Therefore, the diffraction peaks mainly represent (i) interfacial IMCs formed during the reaction and (ii) IMCs originating from the solder matrix that become exposed and/or concentrated during etching and specimen preparation. Across all conditions, Ag3Sn is the dominant phase and exhibits the strongest reflections in the low-to-mid 2 range. As the reaction time increases from 20 to 40 min, the Ag3Sn peak intensity increases consistently at each temperature, and the strongest overall Ag3Sn signal is obtained for 270 °C after 40 min. This time- and temperature-dependent enhancement is attributed to the increased formation of Ag3Sn during the soldering reaction, as well as to the preferential release and accumulation of Ag3Sn particles during etching, which improves their detectability by XRD.
Figure 7.
XRD patterns of specimens reacted at 230–270 °C for various reaction times. XRD specimens were prepared by complete etching of residual solder after interfacial reactions.
In contrast, the diffraction peaks assigned to (Ni,Cu)2Ga3 are relatively weak. These reflections appear mainly around 2 ≈ 44.8°, corresponding to the expected (102) reflection [32,33]. The weak intensity is attributed to the limited thickness and overall fraction of this interfacial phase, which results in a minor contribution to the total diffraction intensity after solder etching.
The Ni3Sn4 phase is identified by its characteristic reflections, most prominently around 2 ≈ 30.7°, corresponding to the (002) and planes. The Ni3Sn4 peak intensity shows a clear dependence on both reaction temperature and time. At 230 °C, Ni3Sn4 reflections are weak at 20 min and become more evident at 40 min, indicating progressive development during prolonged heating. Although is inferred to be less pronounced at the interface at the early stage, it can be detected after etching due to the presence of Ni3Sn4-containing regions within the solder matrix and the precipitation/collection effect during specimen preparation.
The Ni peak near 2 ≈ 44.5° is assigned to Ni derived from Ni–P. Electroless Ni–P typically consists of FCC Ni with P in a supersaturated state and shows preferential orientation toward the Ni (111) plane [34].
3.2. Fracture Mode and Dynamic Shear Performance Under High-Rate Loading
Figure 8 shows plane-view SEM images of SACG/ENIG specimens after high-speed ball shear testing. The specimens were reacted at 230, 250, and 270 °C for 10 and 40 min (Figure 8a–f). The high-speed ball shear tests were performed at a shear speed of 1 m/s to evaluate the impact-related mechanical reliability under rapid loading conditions [35,36]. The fracture mode depends strongly on the reaction condition and the interfacial microstructure evolution [37].
Figure 8.
Plane-view SEM images of SACG/ENIG specimens after high-speed ball shear tests. The specimens were reacted for 10 and 40 min at (a,b) 230 °C, (c,d) 250 °C, and (e,f) 270 °C.
A ductile failure is observed when cracks preferentially propagate through the solder matrix, indicating that the interfacial reaction products do not effectively constrain plastic deformation. By contrast, brittle failure occurs when cracks initiate and propagate along interfacial IMC layers, where the crack path is mainly associated with the IMC. To clearly delineate the boundary between these two fracture regions, an orange dashed line has been added to Figure 8d,f.
As shown by the comparison with the interfacial reaction sequence in Figure 3, the fracture mechanism can be linked to the IMC layering. For low-temperature/short-time reactions, only (Ni,Cu)2Ga3 forms at the interface, and the fracture mode is dominated by ductile failure. This behavior is attributed to the thin (Ni,Cu)2Ga3 layer, which provides limited continuity for forming a stable brittle crack path. In addition, the interfacial region associated with the thin Ga-containing IMC exhibits relatively fewer defects such as voids or microcracks, making crack deflection into the solder matrix more favorable.
For higher temperatures and longer reaction times, a thicker layer forms on top of (Ni,Cu)2Ga3. Owing to its higher brittleness and larger thickness, acts as a preferential crack propagation route. As a result, cracking progresses along the continuous IMC layer with reduced resistance, leading to a transition from ductile to brittle failure. Moreover, the increased IMC thickness can enhance local stress concentration during rapid loading, further accelerating interfacial crack advancement.
Figure 9 summarizes the mechanical response and fracture-mode evolution. Figure 9a quantifies the ductile/brittle ratio of the fractured area, while Figure 9b shows the dynamic shear strength for joints reacted at 230–270 °C for 10 and 40 min. To ensure statistical reliability, ten independent tests were performed for each condition (n = 10).
Figure 9.
(a) Ductile/brittle ratio of the fractured area. (b) Dynamic shear strength of SACG/ENIG solder joints reacted for 10 min and 40 min at 230–270 °C. For each condition, ten independent tests were performed (n = 10) to ensure statistical reliability.
A strong correlation is observed between interfacial microstructure evolution and mechanical performance. As reported in Figure 3, the (Ni,Cu)3Sn4 IMC layer progressively thickens with increasing reaction temperature and time. This development is reflected in Figure 9a, where the brittle fracture region expands as the amount and thickness of (Ni,Cu)3Sn4 increase. Consequently, the dynamic shear strength decreases with the increase in brittle fracture area. For the 10 min reacted group, the specimen reacted at 270 °C exhibits the largest brittle fraction and therefore the lowest shear strength among the 10 min samples. For the 40 min reacted group, increasing reaction temperature again increases the brittle fraction and reduces shear strength in a systematic manner. Overall, these trends confirm that brittle crack propagation along the (Ni,Cu)3Sn4-dominated fracture path governs the dynamic shear reliability under high-rate loading.
Therefore, impact-related reliability is determined not only by the presence of specific IMC phases but also by their thickness and continuity. It is thus crucial to control the reaction time and temperature to regulate the formation and growth of (Ni,Cu)2Ga3 and (Ni,Cu)3Sn4. Suppressing excessive thickening of (Ni,Cu)3Sn4 is expected to promote ductile failure characteristics and improve the overall impact resistance of SACG/ENIG joints.
3.3. Morphological Characteristics of the Interfacial IMCs
Figure 10 presents plane-view SEM images of IMCs formed during reactions of SACG/ENIG. Figure 10a shows the IMCs associated with Ag3Sn and (Ni,Cu)2Ga3 after reaction at 230 °C for 40 min, while Figure 10b shows those associated with Ag3Sn and (Ni,Cu)3Sn4 after reaction at 270 °C for 40 min. Consistent with the XRD results, a large fraction of Ag3Sn is exposed on the specimen surface after solder etching. The Ag3Sn phase mainly exhibits a dendritic/leaf-like morphology, suggesting diffusion-controlled growth from nucleation sites.
Figure 10.
Plane-view SEM images and phase-related observations of IMCs formed during the reactions of SACG/ENIG: (a) Ag3Sn and (Ni,Cu)2Ga3 phases after reaction at 230 °C for 40 min; (b) Ag3Sn and (Ni,Cu)3Sn4 phases after reaction at 270 °C for 40 min.
Although Ag3Sn can also form as isolated features within the solder matrix, Figure 10b indicates that Ag3Sn frequently grows attached to the surface of (Ni,Cu)3Sn4. This morphology implies a strong interfacial interaction between the IMC phases, where the (Ni,Cu)3Sn4 layer can provide favorable nucleation sites for subsequent Ag3Sn growth, resulting in a composite-like IMC microstructure.
At 230 °C (40 min), (Ni,Cu)2Ga3 predominantly develops as faceted cubes at the reaction interface. The relatively well-defined cubic morphology indicates a more constrained interfacial growth behavior compared with the dendritic Ag3Sn phase.
At 270 °C (40 min), (Ni,Cu)3Sn4 appears as angular, block-like agglomerates. The formation of coarse and brittle (Ni,Cu)3Sn4 agglomerates agrees with the enhanced (Ni,Cu)3Sn4 presence observed by XRD at higher temperature and longer reaction time. Furthermore, the SEM observations suggest that increasing reaction temperature promotes not only (Ni,Cu)3Sn4 growth but also subsequent Ag3Sn nucleation and co-growth on its surface, leading to a less uniform and more interconnected IMC microstructure.
4. Conclusions
This study investigates interfacial reactions, IMC evolution, and impact-related dynamic shear reliability of SACG/ENIG joints. Interfacial reaction layers were developed by soldering reactions at 230–270 °C for 5–40 min, followed by isothermal aging at 120 °C up to 1000 h. Based on the interfacial microstructural analysis and high-speed ball shear results, the following conclusions can be drawn:
- During soldering reactions between SACG solder and ENIG at 230–270 °C, a Ga-containing diffusion barrier of (Ni,Cu)2Ga3 rapidly forms at the solder/ENIG interface under all tested conditions. The (Ni,Cu)2Ga3 layer remains restrained in thickness (up to approximately 1 µm), accompanied by progressive Ni depletion of the underlying Ni–P layer and the development of a P-rich layer. With prolonged reactions, a two-layer IMC architecture evolves, where the upper brittle phase (Ni,Cu)3Sn4 grows on top of (Ni,Cu)2Ga3.
- The subsequent solid-state aging behavior at 120 °C (200–1000 h) is strongly dependent on the initial interfacial condition established during soldering. After an initial reaction at 230 °C for 40 min, (Ni,Cu)3Sn4 emerges only after extended aging (≥500 h) and coexists with (Ni,Cu)2Ga3. In contrast, when the initial reaction at 230 °C is limited to 10 min, (Ni,Cu)3Sn4 formation is suppressed and only (Ni,Cu)2Ga3 is detected even after 1000 h. A similar tendency is observed for the 270 °C route: (Ni,Cu)3Sn4 does not form after a 270 °C/10 min reaction even after 1000 h, whereas after a 270 °C/40 min reaction, (Ni,Cu)3Sn4 thickens substantially and interfacial cracking along the (Ni,Cu)2Ga3/(Ni,Cu)3Sn4 boundary is observed after 1000 h.
- In high-speed ball shear testing (1 m/s), fracture behavior transitions from ductile failure (solder-matrix cracking) to brittle failure (interfacial IMC-layer cracking) as the (Ni,Cu)3Sn4 layer becomes thicker and more continuous. Dynamic shear strength decreases with the increase in brittle fracture area, confirming that the amount and continuity of (Ni,Cu)3Sn4 dominate the impact-related shear reliability.
- Optimization of soldering/reaction conditions to establish a stable (Ni,Cu)2Ga3 barrier while suppressing excessive thickening of (Ni,Cu)3Sn4 is an effective strategy to enhance the long-term dynamic mechanical performance of SACG/ENIG solder joints. Based on the present findings, heat treatment at temperatures below 270 °C for less than 10 min is recommended as an optimal process window, as it effectively prevents both the excessive growth of (Ni,Cu)3Sn4 and the degradation of the Ni–P layer, even during subsequent post-annealing.
Author Contributions
Conceptualization, Y.S.; methodology, Y.S. and J.-H.C.; software, J.-H.C.; validation, Y.S. and J.-H.C.; formal analysis, J.-H.C. and Y.S.; investigation, J.-H.C. and Y.S.; resources, Y.S.; data curation, J.-H.C. and Y.S.; writing—original draft preparation, Y.S.; writing—review and editing, J.-H.C. and Y.S.; visualization, J.-H.C.; supervision, Y.S.; project administration, Y.S.; funding acquisition, Y.S. All authors have read and agreed to the published version of the manuscript.
Funding
This study was supported by a research fund from Chosun University, 2025.
Data Availability Statement
The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.
Conflicts of Interest
The authors declare no conflicts of interest.
References
- Zhong, S.J.; Zhang, L.; Li, M.L.; Long, W.M.; Wang, F.J. Development of lead-free interconnection materials in electronic industry during the past decades: Structure and properties. Mater. Des. 2022, 215, 110439. [Google Scholar] [CrossRef] [Scilit]
- Laurila, T.; Vuorinen, V.; Kivilahti, J.K. Interfacial reactions between lead-free solders and common base materials. Mater. Sci. Eng. R 2005, 49, 1–60. [Google Scholar] [CrossRef] [Scilit]
- Shiau, L.C.; Ho, C.E.; Kao, C.R. Reactions between Sn–Ag–Cu lead-free solders and the Au/Ni surface finish in advanced electronic packages. Solder. Surf. Mt. Technol. 2002, 14, 25–29. [Google Scholar] [CrossRef] [Scilit]
- European Parliament and of the Council of the European Union. Directive 2011/65/EU of 8 June 2011 on the restriction of the use of certain hazardous substances in electrical and electronic equipment. Off. J. Eur. Union 2011, L174, 88–110. [Google Scholar]
- Moon, K.W.; Boettinger, W.J.; Kattner, U.R.; Biancaniello, F.S.; Handwerker, C.A. Experimental and thermodynamic assessment of Sn-Ag-Cu solder alloys. J. Electron. Mater. 2000, 29, 1122–1136. [Google Scholar] [CrossRef] [Scilit]
- Wu, J.; Xue, S.B.; Wang, J.W.; Liu, S.; Han, Y.L.; Wang, L.J. Recent progress of Sn–Ag–Cu lead-free solders bearing alloy elements and nanoparticles in electronic packaging. J. Mater. Sci. Mater. Electron. 2016, 27, 12729–12763. [Google Scholar] [CrossRef] [Scilit]
- Zeng, G.; Xue, S.; Zhang, L.; Gao, L.; Dai, W.; Luo, J. A review on the interfacial intermetallic compounds between Sn–Ag–Cu based solders and substrates. J. Mater. Sci. Mater. Electron. 2010, 21, 421–440. [Google Scholar] [CrossRef] [Scilit]
- Ho, C.E.; Yang, S.-P.; Lee, P.-T.; Lee, C.-Y.; Chen, C.-C.; Kuo, T.-T. IMC microstructure modification and mechanical reinforcement of Sn–Ag–Cu/Cu microelectronic joints through an advanced surface finish technique. J. Mater. Res. Technol. 2021, 11, 1895–1910. [Google Scholar] [CrossRef] [Scilit]
- Zhang, Q.K.; Long, W.M.; Yu, X.Q.; Pei, Y.Y.; Qiao, P.X. Effects of Ga addition on microstructure and properties of Sn–Ag–Cu/Cu solder joints. J. Alloys Compd. 2015, 622, 973–978. [Google Scholar] [CrossRef] [Scilit]
- Chen, H.M.; Guo, C.J.; Huang, J.P.; Wang, H. Influence of gallium addition in Sn–Ag–Cu lead-free solder. J. Mater. Sci. Mater. Electron. 2015, 26, 5459–5464. [Google Scholar] [CrossRef] [Scilit]
- Černičková, I.; Ďuriška, L.; Drienovský, M.; Plevachuk, Y.; Švec, P., Sr.; Danišovičová, P.; Čička, R. Influence of gallium addition on the microstructure, thermal behavior, mechanical and electrical properties of SAC305 lead-free solder and solder joints. J. Mater. Res. Technol. 2025, 39, 528–547. [Google Scholar] [CrossRef] [Scilit]
- Luo, D.X.; Xue, S.B.; Li, Z.Q. Effects of Ga addition on microstructure and properties of Sn-0.5Ag-0.7Cu solder. J. Mater. Sci. Mater. Electron. 2014, 25, 3566–3571. [Google Scholar] [CrossRef] [Scilit]
- Sun, L.; Zhang, L. Properties and Microstructures of Sn–Ag–Cu–X Lead-Free Solder Joints in Electronic Packaging. Adv. Mater. Sci. Eng. 2015, 2015, 639028. [Google Scholar] [CrossRef] [Scilit]
- Li, F.; Xu, L.; Chen, M.; Zhang, F.; Wang, Z.; Liu, X.; He, H. Effects of Ga addition on the microstructure and mechanical performance of Sn–58Bi based alloys and the solder joints. J. Mater. Sci. Mater. Electron. 2024, 35, 2159. [Google Scholar] [CrossRef] [Scilit]
- Zhang, H.; Ma, Z.; Yang, S.; Fan, M.; Cheng, X. Microstructure and mechanical properties of Sn-xGa alloys and solder joints. J. Mater. Res. Technol. 2023, 26, 3830–3839. [Google Scholar] [CrossRef] [Scilit]
- Bang, J.H.; Suslick, K.S. Applications of ultrasound to the synthesis of nanostructured materials. Adv. Mater. 2010, 22, 1039–1059. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Friedman, H.; Porat, Z.; Halevy, I.; Reich, S. Formation of metal microspheres by ultrasonic cavitation. J. Mater. Res. 2010, 25, 633–636. [Google Scholar] [CrossRef] [Scilit]
- Friedman, H.; Reich, S.; Popovitz-Biro, R.; von Huth, P.; Halevy, I.; Koltypin, Y.; Gedanken, A.; Porat, Z. Micro- and nano-spheres of low melting point metals and alloys, formed by ultrasonic cavitation. Ultrason. Sonochem. 2013, 20, 432–444. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Kumar, V.B.; Koltypin, Y.; Gedanken, A.; Porat, Z.E. Ultrasonic cavitation of molten gallium in water: Entrapment of organic molecules in gallium microspheres. J. Mater. Chem. A 2014, 2, 1309–1317. [Google Scholar] [CrossRef] [Scilit]
- Kumar, V.B.; Gedanken, A.; Kimmel, G.; Porat, Z. Ultrasonic cavitation of molten gallium: Formation of micro- and nano-spheres. Ultrason. Sonochem. 2014, 21, 1166–1173. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Kumar, V.B.; Gedanken, A.; Porat, Z.E. Sonochemistry of molten gallium. Ultrason. Sonochem. 2023, 95, 106364. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Seo, W.; Kim, M.S.; Ko, Y.H.; Kim, Y.H.; Yoo, S. Growth of intermetallic compounds and brittle fracture behavior of Sn–Ag–Cu/ENIG joint with columnar Ni–P layer. J. Mater. Sci. Mater. Electron. 2021, 32, 1042–1051. [Google Scholar] [CrossRef] [Scilit]
- Park, J.Y.; Yoo, S. Interfacial Microstructure Evolution and High-Speed Ball Shear Fracture of SAC305/Cu-20wt% Zn Solder Joints Under Isothermal Aging. Materials 2026, 19, 3138. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Song, F.; Lee, S.R.; Newman, K.; Sykes, B.; Clark, S. High-speed solder ball shear and pull tests vs. board level mechanical drop tests: Correlation of failure mode and loading speed. In Proceedings of the 57th Electronic Components and Technology Conference; IEEE: Piscataway, NJ, USA, 2007; pp. 1504–1513. [Google Scholar]
- Anderson, T.J.; Ansara, I. The Ga–Sn (gallium-tin) system. J. Phase Equilibria 1992, 13, 181–189. [Google Scholar] [CrossRef] [Scilit]
- Ho, C.E.; Lin, Y.W.; Yang, S.C.; Kao, C.R.; Jiang, D.S. Effects of limited Cu supply on soldering reactions between SnAgCu and Ni. J. Electron. Mater. 2006, 35, 1017–1024. [Google Scholar] [CrossRef] [Scilit]
- Yoon, J.W.; Jung, S.B. Interfacial reactions between Sn–0.4 Cu solder and Cu substrate with or without ENIG plating layer during reflow reaction. J. Alloys Compd. 2005, 396, 122–127. [Google Scholar] [CrossRef] [Scilit]
- Tian, R.; Tian, Y.; Huang, Y.; Yang, D.; Chen, C.; Sun, H. Comparative study between the Sn–Ag–Cu/ENIG and Sn–Ag–Cu/ENEPIG solder joints under extreme temperature thermal shock. J. Mater. Sci. Mater. Electron. 2021, 32, 6890–6899. [Google Scholar] [CrossRef] [Scilit]
- Tu, K.N.; Lee, T.Y.; Jang, J.W.; Li, L.; Frear, D.R.; Zeng, K.; Kivilahti, J.K. Wetting reaction versus solid state aging of eutectic SnPb on Cu. J. Appl. Phys. 2001, 89, 4843–4849. [Google Scholar] [CrossRef] [Scilit]
- Islam, M.N.; Chan, Y.; Rizvi, M.J.; Jillek, W. Investigations of interfacial reactions of Sn–Zn based and Sn–Ag–Cu lead-free solder alloys as replacement for Sn–Pb solder. J. Alloys Compd. 2005, 400, 136–144. [Google Scholar] [CrossRef] [Scilit]
- Sun, P.; Andersson, C.; Wei, X.; Cheng, Z.; Shangguan, D.; Liu, J. High temperature aging study of intermetallic compound formation of Sn–3.5 Ag and Sn–4.0 Ag–0.5 Cu solders on electroless Ni (P) metallization. J. Alloys Compd. 2006, 425, 191–199. [Google Scholar] [CrossRef] [Scilit]
- Wang, C.-H.; Li, K.-T. Effects of Ga addition on interfacial reactions between Sn-based solders and Ni. J. Electron. Mater. 2016, 45, 6200–6207. [Google Scholar] [CrossRef] [Scilit]
- Villars, P. PAULING FILE in Inorganic Solid Phases; SpringerMaterials (Online Database); Springer: Heidelberg, Germany, 2021; Ni2Ga3 (Hellner, 1950, P-3m1). [Google Scholar]
- Sohn, Y.C.; Yu, J.; Kang, S.K.; Choi, W.K.; Shih, D.Y. Study of the reaction mechanism between electroless Ni–P and Sn and its effect on the crystallization of Ni–P. J. Mater. Res. 2003, 18, 4–7. [Google Scholar] [CrossRef] [Scilit]
- Chia, J.Y.H.; Cotterell, B.; Chai, T.C. The mechanics of the solder ball shear test and the effect of shear rate. Mater. Sci. Eng. A 2006, 417, 259–274. [Google Scholar] [CrossRef] [Scilit]
- Song, F.; Lee, S.R.; Newman, K.; Sykes, B.; Clark, S. Brittle failure mechanism of SnAgCu and SnPb solder balls during high speed ball shear and cold ball pull tests. In Proceedings of the 57th Electronic Components and Technology Conference; IEEE: Piscataway, NJ, USA, 2007; pp. 364–372. [Google Scholar]
- Lee, H.T.; Chen, M.H.; Jao, H.M.; Liao, T.L. Influence of interfacial intermetallic compound on fracture behavior of solder joints. Mater. Sci. Eng. A 2003, 358, 134–141. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.