Skip to Content
MaterialsMaterials
  • Article
  • Open Access

27 November 2026

27 Pages

Multiscale Chemical and Microstructural Characterisation of IF-WS2 Modified Anodic Coatings: From GD-OES Profiling to Local Wear Mechanisms

,
,
,
,
and
1
Institute of Materials Engineering, University of Silesia in Katowice, ul. 75 Pułku Piechoty 1a, 41-500 Chorzow, Poland
2
Department of Materials Science, Faculty of Mechanical Engineering and Aeronautics, Rzeszow University of Technology, al. Powstancow Warszawy 12, 35-029 Rzeszow, Poland
*
Author to whom correspondence should be addressed.

Abstract

This study provides a multiscale investigation of the chemical depth architecture, micromechanical properties, and dry sliding tribological performance of nanoporous anodic Al2O3 coatings on EN AW-5251 aluminium alloy modified with inorganic fullerene-like tungsten disulphide (IF-WS2) nanoparticles. Two incorporation strategies were evaluated: an active ultrasonic-assisted method (method A) and a passive gravitational sedimentation method (method B). Point EDS analysis confirmed localized tungsten enrichment (up to 6.60 wt.%) within discrete surface agglomerates, contrasting with matrix-diluted bulk area averages. Qualitative Glow Discharge Optical Emission Spectrometry (GD-OES) depth profiling revealed an overall reduction in sulphur content across the coating volume (from ~4.0 wt.% to 1.2–1.7 wt.%), which is hypothesised to result from post-anodising sulphate leaching during suspension processing rather than altered oxide growth kinetics. ISO-compliant surface roughness evaluation (Ra, N = 342 profiles) revealed a statistically significant difference using the Kruskal–Wallis H-test (p = 0.0011), with post hoc Dunn’s testing confirming a significant roughness increase exclusively for method A. Ball-on-flat tribological tests (conducted under normal loads of 3.1–4.6 N over a sliding distance of 500 m) demonstrated a distinct load-dependent friction crossover: at 3.1 N, sliding resistance was controlled by initial surface roughness (Ra), whereas at 4.6 N, solid lubrication activation in method A reduced the median friction coefficient to µ = 0.75 (compared to 0.81 for reference Al2O3). Evaluation of Archard’s volumetric specific wear rate k (mm3/(N·m)) derived from n = 10 3D profilometric cross-sections per wear track according to ISO 20808:2016 revealed a fundamental discrepancy between friction reduction and volumetric wear resistance under high contact stress. These findings demonstrate that hydrodynamic forcing during incorporation allows tailored microstructural and tribological optimisation of self-lubricating anodic oxide composite coatings.

1. Introduction

The growing demand for energy-efficient solutions in the automotive and aerospace sectors is accelerating the development of lightweight aluminium alloys enhanced with hard, self-lubricating protective coatings. Hard anodising provides a cost-effective, wear-resistant coating for aluminium alloys, particularly effective at protecting against abrasion under low-load conditions. As a result, it is widely used for aluminium components operating under sliding contact conditions, including bearings, cylinders, valves, guide rails, and other tribological systems [1,2,3]. The coating also offers protection against fluid-assisted wear, erosion, and exposure to most chemicals [4]. Plasma electrolytic oxidation (PEO), also known as micro-arc oxidation, has also gained significant popularity as a surface treatment method for aluminium alloys [5,6,7]. Although PEO coatings typically offer higher hardness, wear resistance, and thermal stability, hard anodising remains very attractive for many industrial applications due to its lower cost, simpler processing, and broader industrial acceptance. The anodic oxide coating consists of a nanometrically dense barrier layer and a porous layer up to 100 μm thick [8]. The intrinsic porosity of anodic alumina coatings enables the incorporation of functional species into the oxide layer, thereby extending their functionality beyond conventional wear and corrosion protection. Filling the pore network with lubricating additives can improve tribological performance by lowering friction and wear [9,10,11,12]. Nevertheless, the efficient incorporation of solid lubricant particles has long been limited by the disparity between particle size and the nanometric dimensions of anodic pores [13,14,15]. Furthermore, reducing the oxide thickness to facilitate particle accommodation has been shown to compromise the coating’s mechanical robustness, thereby limiting its effectiveness in demanding applications [1]. Although the tribological properties of hard anodic coatings on aluminium, both without and with incorporated solid lubricant particles, have been described in numerous publications, the diversity of measurement methods used hinders the synthesis and comparability of available data. This creates a significant research area in the field of surface engineering [16].
The relevant properties of hard anodised layers in similar material systems are briefly summarised below.
The 5xxx aluminium series alloys are characterised by the addition of magnesium, which provides them with excellent formability, weldability, and corrosion resistance, especially in marine environments. From a surface engineering perspective, these alloys are particularly amenable to anodising due to their ease of cleaning and surface preparation [17,18,19,20].
Rodrigues et al. [21] demonstrated that coatings produced by microarc oxidation (MAO) on 5086-H111 alloy had a hardness (approx. 21–25 GPa) and a modulus of elasticity approximately three times higher than those of conventional hard anodising (HA, approx. 6 GPa). Consequently, the wear rate of the MAO coating was 22 times lower than that of HA, which was destroyed during testing, exposing the substrate. The average coefficient of friction for the ground MAO coating was approximately 0.92, demonstrating high stability after a 150 s run-in phase.
Wheeler et al. [22], in their analysis of 5052 alloy, confirmed that the hardness of PEO coatings (~12 GPa) was three times greater than that of hard anodised coatings (~4 GPa). Both coatings exhibited higher adhesion than cohesion. Micro-scratch resistance scaled directly with hardness, being 2–3 times higher for PEO than for HA.
Sun et al. [23] presented tests on alloy 5083 that MAO coatings exhibit significantly better corrosion resistance than standard anodic coatings. The anodic coating exhibited numerous cracks that probably provided a diffusion pathway for corrosive ions, whereas the MAO coating was free of such structural defects.
Abid et al. [24] showed that on alloy 5083, extending the reaction time (RT) to 90 min significantly improved the durability of the oxide coating and the coefficient of friction (μ) stability. The average coefficient of friction (μ) decreased from 0.27 (at 30 min RT) to 0.14 (at 90 min RT). It was noted that increasing the current density to 2 A/dm2 did not improve the coating durability and could even cause fluctuations in its tribological behaviour. The wear mechanism involved the formation of a third-body film of compacted wear particles.
Kwolek et al. [16,20] found that coatings on alloy 5005 have a hardness of 445 ± 36 HV (approximately 4.8 GPa). However, they exhibit higher nanoporosity than coatings on alloys from the 6xxx series, which directly translates into lower wear resistance. It has been shown that the highest coating hardness does not always guarantee the best tribological resistance; coatings with lower hardness but different pore structure may exhibit lower wear. The resistance of 5005 coatings was strongly dependent on external load. At a load of 4.9 N, the specific wear coefficient was approximately 1.70 × 10−5 mm3/(N·m), but at 9.8 N, it increased dramatically, more than doubling to 4.56 × 10−5 mm3/(N·m). The coefficient of friction (μ) of oxide coatings on 5005 alloy in contact with ceramic (Al2O3) was high, approximately 1.2. At higher loads, the soft substrate of the 5xxx series alloy undergoes plastic deformation, leading to nucleation of long, sigmoidal cracks in the coating and its premature degradation. Critical coating damage (cohesive cracking and spalling) typically occurred at a load of 15–20 N for DC hard anodising or at 34–38 N with pulsed current. Understanding the relationships in new tribological systems, while accounting for the specifics of different testers and operating conditions, is crucial for the targeted design of low-resistance, durable sliding pairs [25]. While our previous work [26] focused primarily on screening micromechanical parameters (microhardness HIT, elastic modulus EIT, indentation work components, and scratch critical loads) within a two-level factorial Design of Experiments (DoE), the novelty of the present study lies in a comprehensive, multiscale investigation of the chemical depth architecture and long-distance dry sliding tribological mechanisms. For the first time, Glow Discharge Optical Emission Spectrometry (GD-OES) is employed to trace the depth distribution of elements (W, S, Al, O) across the full coating thickness, revealing the post-anodising sulphate leaching phenomenon. Furthermore, this work moves beyond localised indentation screening to evaluate steady-state sliding friction stability, 3D profilometric wear track topography, Archard’s volumetric specific wear rate k (mm3/N⋅m), and non-parametric statistical evaluation. Crucially, this study uncovers the fundamental discrepancy between sliding friction reduction and volumetric wear resistance in IF-WS2-modified Al2O3 coatings under varying contact stress.

2. Materials and Methods

2.1. Sample Preparation

The base material employed in this research was the EN AW-5251 aluminium alloy. This 5xxx series alloy, primarily magnesium-based, was selected for its balanced mechanical strength and excellent corrosion resistance in marine and atmospheric environments, making it ideal for lightweight structural applications. The fabrication of the self-lubricating composite coatings was carried out in two steps. In the first phase, a nanoporous Al2O3 matrix was grown on the alloy surface via electrochemical oxidation. Before anodising, the specimens underwent a two-step chemical pre-treatment at room temperature: immersion in a 5 wt.% potassium hydroxide (KOH, Avantor Performance Materials Poland S.A., Gliwice, Poland) solution for 40 min, followed by immersion in a 10 wt.% nitric acid (HNO3, Avantor Performance Materials Poland S.A., Gliwice, Poland) for 10 min, to remove surface contaminants and prepare the surface for anodising. The electrochemical process was performed in a ternary acid electrolyte consisting of sulphuric acid (33 mL/L), oxalic acid (30 g/L), and phthalic acid (76 g/L) (acids—Avantor Performance Materials Poland S.A., Gliwice, Poland). Hard anodising was carried out at a constant temperature of 303 ± 1 K and a total charge of 180 A·min/dm2. For this study, a constant current density of 3 A/dm2 was maintained. A total of 12 samples were prepared under identical anodising conditions, comprising reference specimens as well as those modified via methods A and B (4 specimens per group).
The second phase focused on impregnating the porous structure with inorganic fullerene-like tungsten disulphide (IF-WS2 NanoMaterials, Ltd., Yavne, Israel) nanoparticles. A suspension was prepared by dispersing 15 g/L IF-WS2 in ethanol, then homogenised using a VCX ultrasonic processor (Sonics & Materials Inc., Newtown, CT, USA) by ultrasonication at 20 kHz for 5 min (delivering 10 kJ of energy). Two different incorporation strategies were compared against an unmodified Al2O3 reference:
Method A (Active Force): Following the initial dispersion, the samples were subjected to an additional 15 min treatment in an ultrasonic bath (Bandelin Sonorex, 35 kHz, 60/240 W) while still submerged in the suspension. This method relies on continuous hydrodynamic forcing and cavitation to mechanically drive the nanoparticles into the oxide pores. Method B (Passive Deposition): After the initial dispersion, the samples were left undisturbed in the suspension for 24 h. This allowed the IF-WS2 particles to settle into the porous matrix through gravitational sedimentation (free falling) without any further external mechanical forcing. Subsequently, the samples were removed from the suspension and left to dry at room temperature. It should be noted as a methodological limitation that method A (15 min of ultrasonic bath treatment) and method B (24 h of gravitational sedimentation) differ not only in hydrodynamic conditions and acoustic cavitation forcing, but also in total contact duration between the porous coating and the suspension. Consequently, observed differences in nanoparticle distribution and tribological behaviour reflect the combined influence of hydrodynamic forcing and processing time, rather than acoustic cavitation alone.

2.2. Coating Thickness Measurement

The mean coating thickness and corresponding standard deviations were calculated from 10 measurements per sample surface, performed using the eddy-current method with a Fischer Dualoscope MP40 device (Helmut Fischer GmbH + Co. KG, Sindelfingen, Germany).

2.3. Microstructural Studies

To evaluate the chemical composition of the Al2O3 nanofibers embedded with self-arranged IF-WS2 nanoparticles, a HITACHI S-4700 scanning electron microscope (Hitachi High-Tech Corp., Tokyo, Japan) was utilised, featuring a NORAN Vantage digital EDS system (NORAN Instruments, Inc., Middleton, WI, USA). The morphology of both the surface and cross-sections of the Al2O3/IF-WS2 NP coatings was captured via backscattered electron (BSE) imaging with a YAG detector (Crytur, Turnov, Czech Republic). Using a single-crystal YAG allowed for a lower electron dose during observation. Freshly fractured surfaces were prepared for the cross-sectional study. Additionally, a thin carbon coating was applied to the specimens by sputtering before microscopic examination to enhance contrast and minimise charging artefacts.

2.4. Tribological Measurement

Tribological tests were conducted in a ball-on-flat setup using a T-01 M tribometer equipped with a friction-force measuring system (Institute for Sustainable Technologies, Radom, Poland). The laboratory temperature during the tests was 24 ± 2 °C, and the relative humidity was 44 ± 3%. Anodised specimens were conditioned at these parameters for 24 h before the tribological tests. During the tests, specimens were rotated at an angular velocity of 95 rpm against an immobile alumina ball of 10 mm diameter, resulting in circular sliding paths with a diameter of 5 mm. A total sliding distance for every specimen was 500 m. The alumina ball was pressed against the specimens at loads of 3.1, 3.6 and 4.6 N. Friction force was measured during experiments, and the coefficient of friction was calculated. The amount of wear was estimated using the wear track depth because the weight losses were small, below 0.3 mg. The wear of the alumina ball was neglected because no weight losses were detected during the experiments. The tribological tests at each applied normal load (3.1 N, 3.6 N, and 4.6 N) were conducted as single exploratory runs on specimens randomly selected from each coating group.

2.5. GD-OES Depth Profiling Methodology

The distribution of the analysed elements was performed using a Horiba France GD Profiler HR. All analyses were performed under identical sputtering conditions, specifically with an argon pressure of 800 Pa and a power of 30 W, utilising a copper anode with a diameter of 4 mm. For plasma generation, 6 N purity argon was used. For all element measurements, integrated detectors in the polychromator were employed. Due to the exploratory nature of the chemical depth profiling, GD-OES analysis was performed as a single measurement for each variant on specimens randomly selected from the prepared batch.

2.6. Micromechanical Properties Methodology

Scratch tests were performed using the scratch tester (CSM Instruments, Peseux, Switzerland). Testing with a Rockwell diamond indenter, the indenter load increased linearly from 1 to 40 N at a speed of 39 N/min, with a scratch length of 12 mm. The scratch tests were carried out as single exploratory runs using samples randomly selected from the modified and unmodified batches for each coating variant.

2.7. SGP Parameters

SGP measurements were performed using an Intra 3D contact profilometer (Taylor Hobson, Leicester, UK). To cover the entire friction track, a measurement field of 13 × 13 mm (X × Y) was adopted with a sampling step of 1 µm × 8 µm. Accuracy in the Z axis was below 16 nm. The height of the wear track was determined using extracted oblique profiles at 90° intervals. The Ra value was determined from profiles from the central part of the samples. In accordance with the ISO 16610-21 standard [27], profile filtering was conducted using a standard Gaussian L-filter with a cut-off wavelength of λc = 0.8 mm and an evaluation length of L = 4.0 mm (comprising five sampling lengths of 0.8 mm) to separate roughness from long-wavelength surface waviness. A total of N = 342 2D surface roughness profiles (n = 114 profiles extracted per coating variant) were evaluated to determine the statistical metrics of the Ra parameter.

2.8. Use of Generative AI Tools

Google NotebookLM (web-based platform, Google LLC, Mountain View, CA, USA, accessed in November 2026) was used to support the organisation and analysis of the literature sources, the synthesis and comparison of research findings reported in the selected publications, and the preparation of the manuscript.

3. Results and Discussion

3.1. Morphological Characterisation, Thickness, and Composition of As-Prepared Coatings

The coating thickness values of the unmodified samples alongside those modified using methods A and B are illustrated in Figure 1. The mean coating thickness was 46.58 ± 2.01 μm for the unmodified reference samples, 47.47 ± 1.18 μm for method A, and 47.23 ± 0.94 μm for method B, yielding an overall average thickness of 47.09 ± 1.48 μm across all prepared coatings.
Figure 1. Thickness of coatings.
SEM image analysis of the coating surfaces (Figure 2), combined with EDS spot analyses (Table 1 and Table 2), enables assessment of the effectiveness of incorporating IF-WS2 nanoparticles into the oxide matrix for both modification methods. SEM images at 200× and 15k× magnifications (Figure 2a–f) confirm that the nanoparticles do not form a continuous layer but rather appear as point-like, unevenly distributed clusters. Chemical composition analysis in selected microenvironments (Table 1 for Figure 2e and Table 2 for Figure 2f) revealed significantly higher tungsten concentrations, documenting the presence of modifier agglomerates. For the coating obtained by method A, the tungsten content was 5.21% by weight (Table 1), whereas for method B it was even higher at 6.60% by weight (Table 2). This is accompanied by the presence of sulphur at 2.62% and 2.34% by weight, respectively, which is crucial for the potential formation of a triboactive film. Differences in the morphology of the deposits result directly from the different physics of the impregnation processes:
Figure 2. SEM images of Al2O3 oxide coatings (a,c,e)—method A; (b,d,f) method B.
Table 1. EDS analysis of the area marked in Figure 2e for the Al2O3 coating modified by method A.
Table 2. EDS analysis of the area marked in Figure 2f for the Al2O3 coating modified by method B.
Method A (sonication + ultrasonic cleaner): In this strategy, constant hydrodynamic and cavitation forces are applied. As a consequence, some of the IF-WS2 particles do not settle stably on the surface but are instead deflected or redeposited in the suspension. This dynamic state favours repositioning, chemical reorganisation, and surface passivation processes. This process is therefore more mechanical than natural adsorption.
Method B (sonication + free fall): In this process, after initial sonication, there is no further hydrodynamic forcing, allowing for undisturbed gravitational sedimentation. This leads to the formation of characteristic “islands” with larger IF-WS2 agglomerates, as confirmed by SEM images (Figure 2b,d,f).
SEM/EDS analysis allows for the clear conclusion that IF-WS2 occurs in points and is unevenly distributed within the Al2O3 matrix. While method A promotes a more dynamic interaction with the surface, method B favours the formation of local, dense clusters of nanoparticles. Under tribological loading, these larger agglomerates may undergo localised mechanical fragmentation or shearing, affecting local adhesion and friction behaviour. These structural differences in agglomeration and local W content between methods A and B are consistent with the combined effects of hydrodynamic forcing and the significantly longer contact time (24 h vs. 15 min), as outlined in Section 2.1.
High-magnification SEM micrographs detailing the localised surface morphology of the coatings after tribological testing, accompanied by regional area-scan EDS elemental analyses, are presented in Figure 3 and Table 3, Table 4 and Table 5. For the unmodified coating (Figure 3a), EDS analysis (Table 3) revealed the presence of aluminium (~73–74 wt.%) and oxygen (~21–23 wt.%), confirming the phase composition of Al2O3. The presence of sulphur was also noted at approximately 4 wt.%, attributable to the sulphur electrolyte used in the anodising process. EDS analysis performed over a larger area yields an average chemical composition for the entire scanned volume (which consists primarily of the anodic Al2O3 matrix). Consequently, the signal contribution from the discrete tungsten-based agglomerates is heavily diluted by the signal from the surrounding oxide matrix, resulting in an average value ranging from 0.03 to 0.75 wt.%. Conversely, point EDS analyses focused directly on the identified agglomerates reveal localised tungsten concentrations reaching up to 6.60 wt.%, well above the limit of detection and measurement error of the instrument. This confirms that the low bulk values stem from spatial heterogeneity rather than the absence of the modifier.
Figure 3. SEM images of friction traces and coatings (a) without Al2O3 modification, (b) Al2O3 modified by method A, (c) Al2O3 modified by method B.
Table 3. EDS analysis of the area marked in Figure 3a for the Al2O3 unmodified coating.
Table 4. EDS analysis of the area marked in Figure 3b for the Al2O3 coating modified by Method A.
Table 5. EDS analysis of the area marked in Figure 3c for the Al2O3 coating modified by Method B.

3.2. GD-OES Depth Profiling Results

Figure 4 shows GD-OES depth profiles obtained on the investigated materials. The curves show the intensities of light emitted by a certain element as a function of sputtering time. Considering that the oxidation products are sputtered from the surface toward the base alloy, the sputtering time indirectly indicates the depth. Meanwhile, the intensity of emitted light is directly correlated with the concentration of certain elements at a given depth: the higher the concentration of an element at that depth, the higher the intensity of emitted light. Thus, based on the obtained curves, a qualitative discussion about enrichments and depletion zones for certain elements can be done. One of the basic observations of GD-OES depth profiles is that the anodic coating formed on the reference material (Figure 4a) is thinner than that formed on the sample modified by method B (Figure 4c) and method A (Figure 4b). This observation is supported by an increase in the sputtering time required to measure the anodic coating. Namely, the sputtering time necessary for the measurement of the reference coating is about 6000 s; for method B, it is 6300 s; and for method A, it is about 6900 s (Figure 4a–c). It should be emphasised that without converting the sputtering time into absolute depth (μm) using a calibrated reference standard, these depth profiles provide a qualitative comparison of element distribution rather than a direct measurement of oxide thickness. Given that all examined coatings consist of the same Al2O3 matrix with comparable microstructure, the sputtering rate across the variants can be assumed to be practically constant. Consequently, the variations in total sputtering time directly reflect minor local thickness variations in the individual specimens selected for GD-OES analysis, which fall well within the natural thickness dispersion observed across the coating batch (Figure 1).
Figure 4. GD-OES depth profiles showing intensity of emitted light for certain elements as a function of sputtering time obtained for: (a) reference sample, (b) modification A and (c) modification B.
Detailed analysis of Al, Si, and O distributions further confirmed this statement (Figure 5a–c). It can be observed that the Al intensities measured in the anodic coating are relatively lower than those measured in the base alloy. This is because, in the oxide scale, Al2O3 (which forms in all cases) ties up 3 moles of O per 2 moles of Al. Therefore, the increase in Al intensity indicates the boundary between the coating and the base alloy (Figure 5a). A similar observation applies to the Si profile (Figure 5b). In contrast, the opposite is true for the O profile: a drop in O intensity indicates the end of the oxide scale region measurement (Figure 5c).
Figure 5. Comparison of GD-OES depth profiles of (a) Al, (b) Si and (c) O obtained on the reference sample and modifications A and B.
GD-OES profiles obtained for C and H (Figure 6a and Figure 6b, respectively) revealed some differences in the distribution of elements over the anodic coating region (Figure 6a and Figure 6b, respectively). Depth profiles obtained for C lines on the reference and modification A follow a similar trend; the intensity of C in the reference sample is slightly higher compared with modification A. At the beginning, a similar carbon peak is observed for about 130 s of measurement across all profiles. A decrease in C intensity is observed around 300 s, followed by an increase. For the reference sample and method A, a plateau in C intensity is found over the whole zone of the formed coating. A slightly different profile is observed for method B. After the second peak, a decrease in C intensity is observed between 1500 and 4500 s during the measurement. Near the coating/base alloy interface, another enrichment of C is found. Exactly at the oxide/alloy interface, a local minimum of C intensity is present (around 6000 s) with a subsequent increase in the alloy (Figure 6a).
Figure 6. Comparison of GD-OES depth profiles of: (a) C and (b) H obtained on the reference sample and modifications A and B.
For the H profile measured in the reference sample, an enrichment is observed around 200 s of measurement, followed by a slight, continuous decrease in H intensity until the end of the anodic oxide measurement. The H signal measured for method A shows a similar trend; however, a pronounced depletion zone after the first peak is observed (Figure 6b, red curve between 800 and 2000 s). After the depletion zone is mentioned, the signal remains at a constant level till the end of the measurement. For modification B, a sharp peak followed by depletion is observed; however, the H line intensity measured within the coating zone is clearly increased.
The biggest difference is observed for the S distribution in the anodic oxide zone, particularly between the reference sample and methods A and B (Figure 7). In the reference sample, significant enrichment of S in the coating zone is observed. This is indicated by a much higher light intensity in the region of the formed anodic coating (Figure 7, blue line). Profiles for S measured by methods A and B remain at the same level within most of the anodic oxide zone (Figure 7, lines red and green, respectively). The only difference is that, at the beginning of the measurement, namely for method A, a slight enrichment of S is observed at the very outer part of the oxide scale, whereas for modification B, depletion is observed in the same region (measurement time between 0 and 800 s).
Figure 7. GD-OES depth profiles of S obtained on the reference sample and modifications A and B.
The analysis of sulphur content (S) provides a key point of integration between the SEM/EDS and GD-OES measurements. Quantitative EDS analysis reveals that the unmodified Al2O3 coating contains approximately 4 wt.% sulphur, whereas in the modified coatings (methods A and B), the overall sulphur content decreases to 1.2–1.7 wt.%. The GD-OES depth profiles corroborate this reduction on a global scale across the entire coating volume: while the unmodified Al2O3 reference exhibits strong and uniform sulphur enrichment throughout the oxide coating, both modified coatings display significantly lower, flat sulphur profiles. Since the anodic oxide matrix and its initial sulphur entrapped from the sulphuric acid bath are fully established prior to nanoparticle impregnation, this overall decline cannot be attributed to altered oxide growth kinetics or blocked sulphur incorporation during anodization. Instead, it is hypothesised that the post-anodising processing steps—specifically the prolonged immersion and ultrasonic cavitation in ethanol suspensions—facilitate the partial leaching or dissolution of weakly bound sulphate ions from the porous network. Although IF-WS2 particles introduce sulphur locally, their discrete, island-like distribution is insufficient to offset the overall depletion of matrix-bound sulphur across the bulk coating volume. The localised incorporation of IF-WS2 nanoparticles and the accompanying decrease in sulphur signal within the anodic coating shed light on the physical mechanics of post-anodising nanoporous Al2O3 modification. Unlike AC-assisted electrodeposition methods [24], which result in the complete filling of nanochannels with metal disulphides, the ethanol-suspension impregnation technique employed in this study yields discrete solid lubricant reservoirs near the surface. A similar phenomenon—whereby the packing density of nano-additives within oxide pores is limited in the absence of active electric field assistance—was reported by Hatfield et al. [15], who indicated that mechanical pore penetration is strongly dependent on the powder’s agglomeration state and local hydrodynamic forcing. These discrete solid lubricant reservoirs subsequently govern the load-dependent friction performance and wear progression under dry sliding contact, which aligns with recent findings by Krbata et al. [28] on self-lubricating composite coatings tested under varying normal loads, where compliant lubricating phases modulate interfacial shear but friction reduction does not linearly correlate with volumetric wear resistance.

3.3. Roughness and Scratch Resistance of Coatings

The surface state before tribological testing was assessed based on the roughness parameter Ra. Figure 8 presents the median and interquartile range (25–75%) of this parameter, chosen as measures of position and dispersion because some measurement distributions departed from normality (confirmed by the Shapiro–Wilk test, p < 0.05). The non-parametric Kruskal–Wallis test (N = 342, n = 114 profiles per condition) revealed a statistically significant difference in Ra roughness values among the variants (H (2) = 13.71, p = 0.0011). Post hoc Dunn’s multiple comparison test confirmed that a statistically significant difference exists exclusively between method A and the unmodified Al2O3 coating (p = 0.00065). In contrast, differences between method A and method B (p = 0.145), as well as between method B and unmodified Al2O3, were not statistically significant. The lowest median Ra values were recorded for unmodified Al2O3 coatings. At the same time, the introduction of the modifier resulted in a successive increase in roughness for method B (sedimentary) and method A (active), respectively. The highest Ra values observed for method A are likely due to the intense hydrodynamic and cavitation forcing during the process, which can lead to local chemical and mechanical reorganisation of the surface.
Figure 8. Measurement of the position of Ra parameters.
Figure 9 shows the curves of normal force, friction force, and residual depth during scratch testing of the unmodified Al2O3 coating (Figure 9a); the Al2O3 coating modified by method A (Figure 9b); and the Al2O3 coating modified by method B (Figure 9c). The normal force increased linearly from approximately 1 N to 40 N over a scratch length of 12 mm. For the unmodified Al2O3 coating, the friction force increased gradually to approximately 6 N at a scratch length of approximately 5.5 mm. Beyond this value, the oscillation amplitude increased significantly. Numerous local peaks and troughs were observed in the range from approximately 6 to 12 mm. For the Al2O3 coating modified by method A, the friction force remained low up to a scratch length of approximately 4 mm and increased gradually with increasing load. In the 4–6 mm range, a further increase in the friction force was observed, reaching approximately 6 N. Beyond 6 mm, the course exhibited significant oscillations whose amplitude increased with scratch length. For the Al2O3 coating modified by method A, the friction force increased gradually up to approximately 5 mm, reaching values of approximately 5 N. In the 5 to 7 mm range, the first more rapid increase in friction force was visible, accompanied by the appearance of distinct oscillations.
Figure 9. Results of the scratch test: (a) for unmodified Al2O3 coating; (b) for Al2O3 coating modified by method A; (c) for Al2O3 coating modified by method B.
For all coatings, the residual depth curve showed a systematic increase with increasing normal force. Up to approximately 5 mm of scratch length, the changes were relatively small and stable. Later in the test, significant fluctuations in residual depth appeared. The nominal thickness of the Al2O3 coatings was approximately 47 µm; therefore, residual depth (Rd) values reaching 80–90 µm at higher normal loads reflect progressive indenter penetration, coating breakthrough, and severe localised plastic deformation (plastic ploughing) within the underlying soft aluminium alloy substrate, rather than the thickness of the oxide layer itself.
Figure 10 illustrates representative optical micrographs of the scratch tracks, detailing the characteristic coating failure stages observed during progressive loading. The failure modes transition through three distinct critical load levels: First, cohesive cracking LC1: Initiation of fine cohesive microcracks (Hertzian cracking) within the track contact area without delamination. Forward chevron cracking (LC2): Onset of V-shaped forward tensile cracking caused by plastic deformation under increasing normal load. Adhesive failure (LC3): Gross adhesive failure marked by continuous spallation of the coating and exposure of the underlying substrate. The critical load values (LC1, LC2, LC3) recorded for the unmodified Al2O3 coating and the modified surface variants are summarised in Table 6. It should be emphasised that the quantitative scratch tests were conducted as preliminary exploratory screening evaluations on randomly selected coating specimens to observe general micromechanical failure tendencies. The resulting critical load values, summarised in Table 6, should therefore be interpreted as indicative trends rather than definitive statistical metrics. For the unmodified Al2O3 reference specimen, critical load thresholds were recorded at Lc1 = 5.4 N, Lc2 = 7.1 N, and Lc3 = 21.2 N. Modification via method A exhibited a potential upward trend in the ultimate adhesive failure load (Lc3 = 24.4 N, representing a ~15% relative increase), alongside a minor shift in the initial cohesive microcracking load (Lc1 = 5.8 N), while Lc2 =7.2 N remained virtually unchanged. Within the scope of these exploratory observations, this slight increase in Lc3 may suggest a localised enhancement in resistance to macro-spallation under progressive mechanical contact. Conversely, method B displayed a slightly different exploratory response: initial microcracking Lc1 was detected at a somewhat lower load (4.7 N), which might reflect localised stress concentrations near surface nanoparticle clusters. At the same time, method B recorded a slightly elevated threshold for forward chevron cracking Lc2 = 8.0 N, whereas its ultimate adhesive failure load (Lc3 = 21.6 N) remained essentially equivalent to the unmodified reference.
Figure 10. Scratch-track of the sample: (a) for unmodified Al2O3 coating; (b) for Al2O3 coating modified by method A; (c) for Al2O3 coating modified by method B.
Table 6. Critical load values (LC1, LC2, LC3) determined during scratch testing for unmodified and modified Al2O3 coatings.
Figure 11a presents the continuous friction force (Ft) as a function of scratch length, and Figure 11b shows the residual depth (Rd) profile for the unmodified Al2O3 coating and the coatings modified by methods A and B. During the initial test range (0–4 mm), the Ft and Rd values for all coatings were very similar. Because IF-WS2 nanopowder doping occurs in the upper part of the coating, the greatest expected effect on micromechanical parameters is expected in the initial phase of the test.
Figure 11. Superimposed plots: (a) frictional force; (b) residual depth as a function of scratch length.

3.4. Tribological Properties and Wear Mechanisms

The course of the coefficient of friction (μ) as a function of friction path (Figure 12) allows for the assessment of the stability of the tested tribological node. Figure 13 presents the coefficient of friction data for the 20 m test. Based on the visual analysis and data presented in Figure 13 and their correlation with the roughness parameters in Figure 8, certain conclusions can be drawn. The box plots are characterised by very narrow interquartile ranges and short whiskers, which visually confirm the high intra-test stability of the friction conditions across all tested variants. At the early stage of friction, for the lowest load of 3.1 N (Figure 13a), only the coating modified via method B shifts upward on the coefficient-of-friction axis (μ ≈ 0.82) compared to the unmodified Al2O3 coating (μ ≈ 0.72) and method A maintains a comparable friction level (μ ≈ 0.71). This indicates that under mild contact conditions, the IF-WS2 additive does not yet reduce frictional resistance and, depending on the deposition route, may initially increase it. At higher loads of 3.6 N (Figure 13b) and 4.6 N (Figure 13c), this trend reverses: the boxes for both methods A and B drop clearly below the reference Al2O3 coating (μ ≈ 0.75), reaching comparable median friction coefficients of approximately 0.69 at 3.6 N and 0.70 at 4.6 N. This can be attributed to the effectiveness of the solid lubricant under higher contact pressures. Comparing these results with the surface roughness data (Figure 8) reveals no straightforward linear correlation between initial Ra and friction at low load. Although the unmodified Al2O3 coating exhibits the lowest median roughness and method A the highest one, both variants yield nearly identical friction coefficients at 3.1 N up to 20 m (Figure 13a). Conversely, method B shows an intermediate Ra yet generates the highest friction at this load up to 20 m (Figure 13a). This could suggest that at 3.1 N, frictional behaviour is governed not solely by the initial roughness amplitude, but by other surface characteristics resulting from the modification process. At 3.6 N and 4.6 N, where the boxes of both modified coatings separate below the unmodified reference while overlapping with each other (Figure 13b,c), initial differences in Ra lose their significance in favour of the properties of the developing IF-WS2 tribofilm.
Figure 12. Friction coefficient vs. sliding path: (a) 3.1N, (b) 3.6N, (c) 4.6N.
Figure 13. Box-and-whisker plots of the friction coefficient (μ) up to 20 m of friction for loads: (a) 3.1N, (b) 3.6N, (c) 4.6N up to 20 m of friction, illustrating intra-test process stability during representative runs.
For a detailed analysis of the stable coefficient of friction, values recorded from the 20th meter of the friction path were used, thereby eliminating the influence of the running-in phase (Figure 14). Table 7 summarises the measures of position and dispersion of the friction coefficient, which reflect intra-test friction stability recorded during representative steady-state sliding runs. Due to the non-normality of the data distribution, the median and interquartile range (IQR) were selected as the appropriate measures of position and dispersion, as summarised in Table 7. Analysis of the data in Table 7 and the steady-state friction distributions (Figure 14) demonstrates a notable sensitivity of friction mechanics to the applied load. The proximity of the mean and median within the boxes indicates that the friction coefficient distributions are relatively symmetric, demonstrating the coatings’ predictable behaviour during the test. For a load of 3.1 N, the unmodified coating exhibits the lowest friction resistance (median μ = 0.74). The introduction of IF-WS2 nanoparticles increases friction to 0.79 for method A and 0.86 for method B. For a load of 3.6 N, the μ values converge, and the error ranges overlap significantly. The coating obtained by method B (μ = 0.78) performs best, ahead of method A (μ = 0.80) and the pure oxide (μ = 0.82). For a load of 4.6 N at the highest normal stress, the modification by method A proves most effective, reducing the median friction coefficient to 0.75, compared to 0.81 for the unmodified Al2O3. The narrow interquartile ranges and stable distribution limits confirm high intra-test stability of the friction process across all tested variants.
Figure 14. Box-and-whisker plots of the friction coefficient (μ) from the 20th meter of friction (steady-state region) for loads: (a) 3.1N, (b) 3.6N, (c) 4.6N from 20 m of friction, illustrating intra-test friction stability.
Table 7. Friction coefficient position and dispersion measures representing intra-test process stability during steady-state sliding.
Modification of oxide coatings with IF-WS2 nanoparticles differentiates friction mechanics depending on the applied load and impregnation method. At low normal loads (3.1 N), contact mechanics are controlled primarily by surface microgeometry and roughness (Ra), throughout the entire sliding distance, consequently, the smoothest, unmodified Al2O3 coatings exhibiting the lowest resistance. At an intermediate load of 3.6 N, a transition regime occurs where friction distributions converge and overlap significantly as solid lubricant activation begins to offset micro-roughness resistance. Only at higher loads (4.6 N) does the modifier’s lubricating potential become active, particularly in method A (active forcing), which most effectively reduces the friction coefficient to 0.75.
The dominant role of initial surface roughness (Ra) at low load (3.1 N) and its gradual loss of significance in favour of the properties of the forming tribofilm at 4.6 N are fully consistent with the observations of Dervishi et al. [18] and Abid et al. [24]. They indicated that, during the initial stage of friction on anodic coatings, the process is governed by the micro-geometry of asperity contact. Only at higher pressures does the crushing and smearing of particles in the contact zone occur, activating internal mass flow (third-body flow) and facilitating shearing [24]. The reduction m to a level of ~0.75 achieved with method A confirms the formation of a stable tribo-active layer; however, the absence of a superlubricity state (as seen in liquid-assisted systems, e.g., Meng et al., [29]) stems from the specific nature of the dry contact between the corundum ball and the rough ceramic matrix.
Figure 15 shows example 3D images of friction paths for a load of 4.6 N, respectively Figure 15a—unmodified Al2O3 coating; Figure 15c—Al2O3 coating modified by method A; Figure 15e—Al2O3 coating modified by method B. Figure 15b shows a fragment of the unmodified Al2O3 coating with a friction trace for a load of 3.1 N; Figure 15d shows an Al2O3 coating modified by method A for a load of 3.6 N; Figure 15f shows an Al2O3 coating modified by method B for a load of 4.6 N, most likely at the end of the test, where the accumulated wear material was collected.
Figure 15. Example 3D images of friction paths for a load of 4.6 N: (a) unmodified Al2O3 coating; (c) Al2O3 coating modified by method A; (e) Al2O3 coating modified by method B; (b) unmodified Al2O3 coating (3.1 N); (d) Al2O3 coating modified by method A (3.6 N); (f) Al2O3 coating modified by method B (4.6 N).
The specific wear rate k (mm3/(N·m)) for each coating variant was calculated according to ISO 20808:2016 standard wear assessment methodology in sliding tribological contacts [30]:
k = V F N · s = A ¯ × C F N · s
where
  • V is the total wear volume (mm3);
  • A ¯ is the mean cross-sectional area of the wear track (mm2), calculated from n = 10 independent profilometric profiles measured perpendicularly to the sliding direction along the circumference of a single specimen;
  • C is the total perimeter of the circular wear track (mm);
  • FN is the applied normal load (N);
  • s is the total sliding distance (m, where s = 500 m).
The mean cross-sectional area A ¯ was determined as:
A ¯ = 1 n ∑ i = 1 n A i
where Ai represents the individual cross-sectional area derived from the 2D profilometric trace (i = 1, 2, …, 10).
Specific wear rate values (k), calculated on the basis of cross-sectional area measurements (n = 10) of the wear tracks, are presented in Figure 16. Across all tested coating variants, a clear upward trend in the specific wear rate was observed as the normal load increased from 3.1 N to 4.6 N, which aligns with standard contact mechanics principles regarding increased mechanical stress in sliding contact. For loads of 3.1 and 3.6, the unmodified Al2O3 coating and the coating modified by method B exhibited comparable wear resistance, whereas method A showed slightly higher k values, indicating a higher susceptibility to volumetric material removal under lower normal stresses. At the highest load of 4.6 N, all variants reached their maximum wear rates (k ≈ (1.07–1.14) × 10−6 mm3/Nm, with method A displaying the highest average wear rate. The fact that the reduction in the coefficient of friction observed for method B did not translate into a proportional decrease in the specific wear rate k supports the widely accepted consensus in the literature: no direct, simple relationship exists between sliding friction behaviour and volumetric wear resistance in hard anodic coatings. A similar discrepancy between friction reduction and wear resistance was reported by Krbata et al. [28], who demonstrated that coatings providing the lowest friction coefficient due to compliant self-lubricating phases may still undergo pronounced localised plastic deformation, confirming that sliding friction behaviour and volumetric wear resistance are governed by distinct mechanical mechanisms. As demonstrated by Kwolek et al. [16,20] and further corroborated by Escherova et al. [31] in dry sliding wear studies under variable contact pressure, the plastic deformation response of the underlying softer substrate leads to localised stress concentrations within the hard protective layer, accelerating wear track degradation despite the boundary-lubricating presence of the nanoparticles. The accumulation of large IF-WS2 nanoparticle agglomerates in macro-pores (characteristic of method B) creates local structural discontinuities. Under high localised contact pressures, these discontinuities are hypothesised to undergo localised mechanical breakdown, thereby accelerating wear-track degradation despite the boundary-lubricating presence of the nanoparticles.
Figure 16. Specific wear rate (k) calculated for individual exploratory coating specimens under normal loads of 3.1 N, 3.6 N, and 4.6 N. Error bars represent the standard deviation (SD) of cross-sectional wear track areas measured across 10 independent cross-profiles along a single wear track (intra-specimen geometrical variability).

4. Conclusions

  • Incorporation efficiency and the sulphur evaluation: Ethanol-suspension impregnation methods (A and B) effectively introduce IF-WS2 nanoparticles into the Al2O3 coating structure, creating discrete solid lubricant reservoirs. However, the modified coatings exhibit an overall lower sulphur signal (from ~4 wt.% to ~1.2–1.7 wt.%). Since the anodic oxide matrix and its initial sulphur content are fully established prior to impregnation, this reduction is hypothesised to result from post-anodising leaching or dissolution of weakly bound sulphate ions during suspension immersion and ultrasonic processing.
  • Modifier distribution vs. deposition kinetics: The application of active hydrodynamic forcing and ultrasonic cavitation (method A) ensures a more uniform dispersion of IF-WS2 within the oxide matrix. Passive sedimentation (method B) promotes the formation of large, island-like agglomerates due to gravitational settling during prolonged contact duration (24 h vs. 15 min).
  • Load dependence of friction mechanics: Friction behaviour exhibits a clear load-dependent crossover governed by the interplay between initial surface topography and solid lubricant activation. At low loads (3.1 N), contact mechanics are controlled by initial surface microgeometry—the higher roughness (Ra) of modified coatings increases mechanical sliding resistance (median µ = 0.79 for method A and 0.86 for method B) compared to the smoother unmodified reference (µ = 0.74). At higher normal load (4.6 N), increased contact pressure induces localised crushing and shearing of IF-WS2 particles, consolidating a shear-facilitating triboactive layer; with method A achieving the most uniform nanoparticle dispersion, effectively reducing the median friction coefficient to μ = 0.75 (compared to µ = 0.81 for the unmodified Al2O3 reference).
  • Discrepancy between friction and volumetric wear rate (k): A reduction in the friction coefficient (μ) does not directly translate into a proportional decrease in the specific wear rate k (mm3/(N⋅m)). Across all coating variants, k exhibits a clear upward trend with increasing normal load (reaching (1.07–1.14) × 10−6 mm3/(N⋅m) at 4.6 N) due to higher mechanical stress. In method B, large IF-WS2 nanoparticle agglomerates act as local structural discontinuities; under high contact pressure, these clusters are hypothesised to undergo localised mechanical fragmentation, accelerating wear track degradation despite their boundary-lubricating presence.

Author Contributions

Conceptualization, J.K. and M.B.; methodology, J.K. P.K. W.J.N., K.K.; software, J.K., W.J.N., P.K.; formal analysis, J.K., P.K., W.J.N., M.N.; investigation, J.K., P.K., W.J.N., K.K.; writing—original draft preparation, J.K., W.J.N.; writing—review and editing, J.K., W.J.N., P.K., M.N.; visualization, J.K., W.J.N., M.N.; supervision, J.K., M.B. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.

Acknowledgments

During the preparation of this work, the authors used Grammarly (version 1.2.311.2002) for language editing and grammar checking, and Google NotebookLM (Google LLC, Mountain View, CA, USA; web-based AI research assistant, accessed in November 2026) for organising literature sources, synthesising comparative research data, and assisting in manuscript drafting. After using these tools, the authors reviewed, edited, and revised the content as needed and took full responsibility for the final publication.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Wernick, S.; Pinner, R.; Sheasby, P.G. The Surface Treatment and Finishing of Aluminium and Its Alloys, 5th ed.; Finishing Publications Ltd.: Stevenage, UK; ASM International: Materials Park, OH, USA, 1987. [Google Scholar]
  2. Runge, J.M. The Metallurgy of Anodizing Aluminum: Connecting Science to Practice; Springer: Cham, Switzerland, 2018. [Google Scholar]
  3. Santecchia, E.; Cabibbo, M.; Hamouda, A.M.S.; Musharavati, F.; Popelka, A.; Spigarelli, S. Dry sliding tribological properties of a hard anodized AA6082 aluminum alloy. Metals 2020, 10, 207. [Google Scholar] [CrossRef] [Scilit]
  4. Shrestha, S.; Dunn, B.D. Plasma electrolytic oxidation and anodising of aluminium alloys for spacecraft applications. In Surface Engineering of Light Alloys; Woodhead Publishing: Sawston, UK, 2010; pp. 603–641. [Google Scholar] [CrossRef] [Scilit]
  5. Barua, S.; Rahman, M.A.; Chandra Bhowmik, K.; Khan, I. Corrosion Resistance of Anodized and Composite-Coated Aluminum Alloys: A Comprehensive Review on 5xxx and 6xxx Series. Adv. Mater. Sci. Eng. 2025, 2025, 7941108. [Google Scholar] [CrossRef] [Scilit]
  6. Walsh, F.C.; Low, C.T.J.; Wood, R.J.K.; Stevens, K.T.; Archer, J.; Poeton, A.R.; Ryder, A. Plasma electrolytic oxidation (PEO) for production of anodised coatings on lightweight metal (Al, Mg, Ti) alloys. Trans. Inst. Met. Finish. 2009, 87, 122–135. [Google Scholar] [CrossRef] [Scilit]
  7. Sowa, M.; Olesiński, A.; Szumski, B.; Maciej, A.; Bik, M.; Jeleń, P.; Sitarz, M.; Simka, W. Electrochemical characterization of anti-corrosion coatings formed on 6061 aluminum alloy by plasma electrolytic oxidation in the corrosion inhibitor-enriched aqueous solutions. Electrochim. Acta 2022, 424, 140652. [Google Scholar] [CrossRef] [Scilit]
  8. Thompson, G.E. Porous anodic alumina: Fabrication, characterization and applications. Thin Solid Films 1997, 297, 192–201. [Google Scholar] [CrossRef] [Scilit]
  9. Abedini, M.; Hanke, S. Improving the wear resistance of aluminum by a nickel-filled anodized porous alumina layer. Wear 2023, 522, 204858. [Google Scholar] [CrossRef] [Scilit]
  10. Tahir, N.A.M.; Liza, S.; Fukuda, K.; Yaakob, Y.; Zulkifli, N.A.; Rawian, N.A.M.; Ghazazi, N.A.M. Influence of humidity on the tribological performance of graphite reinforced aluminium anodic oxide coating. Tribol. Int. 2024, 197, 109752. [Google Scholar] [CrossRef] [Scilit]
  11. Xiong, Z.; Zhang, W.; Wu, R.; Ma, F.; Wang, X.; Wang, G. One-step hydrothermal fabrication of Co-MOFs/LDH superhydrophobic composite coating with corrosion resistance and wear resistance on anodic aluminum oxide. Appl. Surf. Sci. 2024, 677, 161023. [Google Scholar] [CrossRef] [Scilit]
  12. Skeldon, P.; Wang, H.W.; Thompson, G.E. Formation and characterization of self-lubricating MoS2 precursor films on anodized aluminium. Wear 1997, 206, 187–196. [Google Scholar] [CrossRef] [Scilit]
  13. Maejima, M.; Saruwatari, K.; Takaya, M. Friction behaviour of anodic oxide film on aluminum impregnated with molybdenum sulfide compounds. Surf. Coat. Technol. 2000, 132, 105–110. [Google Scholar] [CrossRef] [Scilit]
  14. Takaya, M.; Hashimoto, K.; Toda, Y.; Maejima, M. Novel tribological properties of anodic oxide coating of aluminum impregnated with iodine compound. Surf. Coat. Technol. 2003, 169–170, 160–162. [Google Scholar] [CrossRef] [Scilit]
  15. Hatfield, K.O.; Brown, N.; Dervishi, E.; Carpenter, B.; Janusz, J.N.; Hooks, D.E. Correlation of Fabrication Methods and Enhanced Wear Performance in Nanoporous Anodic Aluminum Oxide with Incorporated Molybdenum Disulfide (MoS2) Nanomaterials. Nanomaterials 2024, 14, 451. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  16. Kwolek, P.; Obłój, A.; Kościelniak, B.; Buszta, R.; Tokarski, T.; Krupa, K.; Gradzik, A.; Nowak, W.J.; Wojnicki, M.; Motyka, M. Wear resistance of hard anodic coatings fabricated on 5005 and 6061 aluminum alloys. Arch. Civ. Mech. Eng. 2024, 24, 51. [Google Scholar] [CrossRef] [Scilit]
  17. Anas, N.M.; Abioye, T.E.; Anasyida, A.S.; Dhindaw, B.K.; Zuhailawati, H.; Ismail, A. Microstructure, mechanical and corrosion properties of cryorolled-AA5052 at various solution treatment temperatures. Mater. Res. Express 2019, 7, 016567. [Google Scholar] [CrossRef] [Scilit]
  18. Dervishi, E.; McBride, M.; Edwards, R.; Gutierrez, M.; Li, N.; Buntyn, R.; Hooks, D.E. Mechanical and tribological properties of anodic Al coatings as a function of anodizing conditions. Surf. Coat. Technol. 2022, 444, 128652. [Google Scholar] [CrossRef] [Scilit]
  19. Abioye, T.E.; Zuhailawati, H.; Aizad, S.; Anasyida, A.S. Geometrical, microstructural and mechanical characterization of pulse laser welded thin sheet 5052-H32 aluminium alloy for aerospace applications. Trans. Nonferrous Met. Soc. China 2019, 29, 667–679. [Google Scholar] [CrossRef] [Scilit]
  20. Kwolek, P.; Drapała, D.; Krupa, K.; Obłój, A.; Tokarski, T.; Sieniawski, J. Mechanical properties of a pulsed anodised 5005 aluminium alloy. Surf. Coat. Technol. 2020, 383, 125233. [Google Scholar] [CrossRef] [Scilit]
  21. Rodriguez, L.; Vieu, A.; Balsarin, M.; Combes, P.; Alexis, J.; Esvan, J.; Lesko, S.; Denape, J.; Paris, J.-Y.; Delbé, K. Physico-chemical characterisation and tribological behaviour of ground micro-arc oxidation coating on aluminium alloy—Comparison with hard anodised oxidation. Wear 2023, 516–517, 204591. [Google Scholar] [CrossRef] [Scilit]
  22. Wheeler, J.M.; Curran, J.A.; Shrestha, S. Microstructure and multi-scale mechanical behavior of hard anodized and plasma electrolytic oxidation (PEO) coatings on aluminum alloy 5052. Surf. Coat. Technol. 2012, 207, 480–488. [Google Scholar] [CrossRef] [Scilit]
  23. Sun, H.; Li, L.; Wang, Z.; Liu, B.; Wang, M.; Yu, Y. Corrosion Behaviors of Microarc Oxidation Coating and Anodic Oxidation on 5083 Aluminum Alloy. J. Chem. 2020, 2020, 6082812. [Google Scholar] [CrossRef] [Scilit]
  24. Abid, M.; da Cruz, J.F.; Kchaou, M.; Haboussi, M. Micro- and macro-scale characterization of the microstructure and scratch resistance of the 5083-anodic aluminum oxide film. Proc. Inst. Mech. Eng. Part L J. Mater. Des. Appl. 2023, 237, 1624–1637. [Google Scholar] [CrossRef] [Scilit]
  25. Korzekwa, J. Modification of the structure and properties of oxide layers on aluminium alloys: A review. Rev. Adv. Mater. Sci. 2023, 62, 20230108. [Google Scholar] [CrossRef] [Scilit]
  26. Korzekwa, J.; Barylski, A.; Niedźwiedź, M.; Cwynar, K.; Bara, M. The Influence of Methods for Distributing the IF-WS2 Modifier into the Structure of Al2O3 Aluminium Oxide Coatings on Their Micromechanical Properties. Materials 2026, 19, 667. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  27. ISO 16610-21:2011; Geometrical Product Specifications (GPS)—Filtration—Part 21: Linear Profile Filters: Gaussian Filters. International Organization for Standardization: Geneva, Switzerland, 2011.
  28. Krbata, M.; Kohutiar, M.; Janeková, M.; Hoferica, B.; Krizan, D.; Escherova, J.; Dubec, A.; Trembach, B.; Mikuš, P.; Breznicka, A. Effect of Different PTFE Coatings Applied to 18CrNiMo7-6 Steel on the Coefficient of Friction and Wear Under Dry Sliding Contact Using the Ball-on-Disk Method at Different Loads. Polymers 2026, 18, 1991. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  29. Meng, X.; Zhang, W.; Wei, S.; Pan, K.; Wang, X.; Jiang, T.; Wang, X.; Wang, C.; Chen, C.; Mao, F.; et al. Tribological Properties of 7A04 Aluminum Alloy Enhanced by Ceramic Coating. Lubricants 2024, 12, 384. [Google Scholar] [CrossRef] [Scilit]
  30. ISO 20808:2016; Fine Ceramics (Advanced Ceramics, Advanced Technical Ceramics)—Determination of Friction and Wear Characteristics of Monolithic Ceramics by Ball-on-Disc Method. International Organization for Standardization: Geneva, Switzerland, 2016.
  31. Escherová, J.; Krbata, M.; Kohutiar, M.; Janeková, M.; Hoferica, B.; Dubec, A. Comparison of Wear Resistance of Lean Medium Mn AHSS After Q&P Heat Treatment. Metals 2026, 16, 362. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.