Abstract
Compressive strength evolution and promotion of ultra-early-age concrete under low temperatures are essential for cast-in-place and precast construction. Strength development within 1 d at 10 °C, effects of supplementary cementing materials, and promoting measures were investigated, and the effectiveness of promoting measures was verified via long-term strength and durability tests. Three replicates were used, and results were expressed as mean ± standard deviation. Two-stage strength growth was observed at 10 °C and 20 °C: initial slow exponential growth followed by rapid logarithmic growth, with a prolonged slow-growth phase identified at 10 °C. Within 1–3 d, faster strength gain was obtained for concrete cured at 10 °C, and its strength gap with 20 °C specimens was rapidly reduced. At 10 °C, the 12 h strength was observed to increase from 2.2 ± 0.2 MPa (control) to 2.9 ± 0.2 MPa for the 5% early-strength agent group (+32%, p = 0.008), and 20.0 ± 2.0 MPa was achieved under heat curing (p < 0.001). At 3 years, 6.9% lower strength was recorded for heat-cured concrete versus the control (p = 0.23); 10% margin non-inferiority could not be verified due to limited replicates.
1. Introduction
Concrete has been widely used around the world due to numerous advantages [1,2]. And as the most commonly used construction material globally [3,4,5], the most widely used application of concrete is as a structural material to exert mechanical effects, so strength is the most important indicator for measuring the quality of concrete [6,7]. Therefore, the strength development of concrete has consistently been a subject of widespread interest [8,9,10].
Currently, many studies have been focused on the strength development of concrete, and it is generally believed that the strength development of concrete follows the logarithmic growth law [11]. It means that the strength increases rapidly in the early age, and then the trend gradually slows down. This law has played an effective guiding role in practical engineering. With the development of society, the importance of early-age concrete strength in civil engineering has become increasingly prominent [12,13,14]. However, it is still unknown whether early-age concrete strength actually follows the logarithmic growth law.
For early-age strength development, it is generally believed that ground granulated blast furnace slag (GGBS) and fly ash (FA) have a certain reducing effect [15,16]. Because, for GGBS and FA, the occurrence of secondary hydration reaction requires a certain amount of time, it is generally believed that they mainly play a filling role in the early age. But the strength of concrete mixed with high-activity GGBS or FA can reach or even exceed that of the benchmark concrete made only with cement within 1~28 d [17]. The viewpoint on the effect of adding silica fume on the early strength of concrete is not unified. Some scholars pointed that silica fume is beneficial to the early-age strength of concrete [17,18], while others argue it provides no advantages and may exert adverse effects at early age [19].
The ambient temperature has a significant impact on the early-age strength of concrete. At 20 °C, the strength can generally reach about 50~80% of the 28 d strength in 3 d and about 70~90% of the 28 d strength in 7 d [8,17]. Strength development is even worse at lower temperatures, with the strength at 7 d being only 30% of that at 28 d at 4 °C [11]. Therefore, many studies focus on promoting the early strength of concrete. The usual methods include adding early-strength materials, adopting thermal insulation curing and thermal curing measures [20,21,22,23,24]. The composite of early-strength agent prepared with Na2SO4 and C–S–H seeds [25] can increase the strength of specimens from 4.0 MPa to approximately 15.0 MPa after 1 d at 20 °C. When calcium sulfoaluminate cement of 5% is added [26], the strength of specimens can be increased from 3.5 MPa to 14.1 MPa after 12 h at 20 °C. Additionally, nanomaterials [27,28,29], seeds [30,31,32,33], graphene oxide [34,35,36,37], etc. can also be used as early-strength functional materials to promote the early strength of concrete. The use of early-strength agents at low temperatures sometimes cannot fully meet the early-strength requirements as the rapid dissipation of heat generated by hydration at low temperatures. However, under adiabatic conditions, the temperature rise of concrete can exceed 60 °C even at a low temperature of 15 °C [38]. And so, in principle, by taking reasonable insulation measures at low temperatures and utilizing the hydration heat generated by the cement itself to increase the temperature of concrete, the goal of early-strength promotion can also be achieved [39]. Whereas when the ambient temperature is very low, it is difficult to achieve the desired early-strength effect by using early-strength agents or adopting insulation measures, thermal curing measures are required to promote early strength more effectively. Thermal curing methods include damp heat, dry heat, electric heat, the infrared-spectrum curing method, etc. Among them, steam curing is widely adopted due to its advantages of high heat content, high humidity, and low cost [40,41,42,43]. Thermal curing can rapidly promote the early strength of concrete, but it may also have adverse effects on long-term performance. Attention should be paid to avoiding significant reductions in long-term performance.
Previous studies have primarily focused on strength after 3 d, with very limited research on strength development within 3 d, especially within 1 d. However, the strength within 1 d plays a crucial role in both cast-in-place concrete and precast concrete. In cast-in-place construction projects, the strength development during this period will directly determine the turnover time of formwork and the timing to proceed to the next process, which in many cases is crucial to the overall project progress. During the production of concrete products, there is a particular desire to remove the formwork as early as possible to improve the turnover rate of molds and pedestals. These practical engineering needs are even more prominent at low temperatures. Therefore, the research on the strength development and promotion of concrete within 1 d at low temperatures is also of great significance.
This study aims to investigate the compressive strength development and promotion of concrete within 1 d under low temperature. In this work, concrete age within 1 d is termed earlier age, and the target low temperature condition selected is 10 °C. Three tiers of research objectives are defined herein: (1) as the primary objective, to explore the earlier-age strength development law of concrete under low temperature; (2) as secondary objectives, to analyze the influences of ground granulated blast furnace slag (GGBS) and fly ash (FA) on earlier-age strength, and to compare the effectiveness of multiple promotion measures including early-strength agent, three grades of thermal insulation treatments and steam curing; (3) as an engineering oriented verification, to evaluate the long term strength and durability performance induced by these promotion measures, with the maximum test age reaching 3 years. This work is expected to provide experimental references for practical scenarios requiring the understanding and promotion of earlier-age concrete strength, such as rapid formwork removal for cast-in-place and precast concrete.
2. Materials and Methods
2.1. Materials
The concrete was prepared using cement, sand, crushed rock, water, and a water-reducing agent, serving as the blank group. The cement used was P·O42.5R Ordinary Portland cement, marked as OPC. Two types of crushed rock with different particle sizes were mixed in a mass ratio of 4:6, with particle sizes of 5~10 mm and 10~20 mm, respectively. The sand used was manufactured sand with the same composition as the crushed rock, having a fineness modulus of 2.40. Additionally, a water-reducing agent, marked as PCA, was added to improve the workability of the concrete mixture.
GGBS and FA were incorporated to investigate the effect of supplementary cementing materials on strength development. The specific surface area of the GGBS is 431 m2/kg, with 7 d and 28 d strength activity indices of 86% and 103%, respectively, following the test standard GB/T 18046-2017 [44]. The 45 μm square sieve residue of the FA is 18.1%, and the 28 d strength activity index is 78%, adhering to the test standard GB/T 1596-2017 [45]. Additionally, an early-strength agent of CCP and 3 types of insulation measures were adopted to promote earlier-age strength. The primary component of the early-strength agent is C–S–H-PCE nanoparticles [46,47,48]. This liquid-form nucleating agent is added by replacing an equal mass of mixing water at a fixed dosage of 5 wt% of water, and it functions by providing abundant crystal nuclei to accelerate cement hydration. The insulation measures are ranked in order of increasing insulation effectiveness as Polyethylene File (PE) < Air Bubble File (ABF) < Expanded Polystyrene Box (EPS). The chemical compositions of cement, GGBS, and FA are shown in Table 1, and the mineral compositions are shown in Figure 1.
Table 1.
Chemical components of OPC, GGBS, and FA (wt%).
Figure 1.
XRD patterns of (a) OPC, (b) GGBS, and (c) FA.
2.2. Concrete Sample Preparation
The mixture proportions of the blank group concrete are shown in Table 2. When GGBS and FA were added to the concrete, the same mass of OPC as GGBS or FA would be replaced. And when CCP was added, the same mass of water as CCP would be replaced. During the preparation of concrete, all raw materials, molds, mixer, and other tools that contact with the mixture should be maintained at approximately the temperature specified in the experimental design as much as possible. After the concrete was mixed fully, we placed it in a plastic mold as soon as possible, then vibrated it for 30 s, and finally the concrete samples with molds were placed in a constant-temperature and -humidity chamber, with temperatures set at 10 ± 0.5 °C and 20 ± 0.5 °C, respectively. The dimensions of the concrete specimen were 100 mm × 100 mm × 100 mm. When testing the earlier-age strength, we demolded the concrete 5 min before testing. When testing the performance at a long age, the demolding time was 1 d after molding. Then, they were placed back in the constant-temperature and -humidity chamber until the corresponding age for testing. If the testing age exceeds 28 d, the specimen should be removed from the constant-temperature and -humidity chamber at 28 d and cured under standard conditions.
Table 2.
Mixture proportions of blank group concrete (kg/m3). The mix proportions were adopted from our previously published study [49].
The three different levels of insulation methods are as follows: covering the freshly molded concrete along with a layer of PE or ABF, placing the freshly molded concrete inside EPS, and finally placing them into a constant temperature and humidity chamber at the preset test temperature. The internal dimensions of the EPS box are 450 mm × 150 mm × 150 mm, with a thickness of 30 mm. Steam curing was also conducted in a constant temperature and humidity chamber, with the temperature and humidity controlled at 55 ± 0.5 °C and 90%, respectively. After steam curing, the concrete test specimens were placed again into the constant-temperature and -humidity chamber at the preset test temperature and humidity.
In general, three categories of strength promotion measures were adopted in this work: chemical admixture (5% CCP early-strength agent), thermal insulation curing (PE film, ABF film and EPS box), and active thermal steam curing. All these treatments were implemented under two target curing temperatures (10 °C and 20 °C) to evaluate their strength-promoting performance. These promotion treatments were designed to explore feasible technical approaches for promoting the earlier-age compressive strength of concrete under low temperature conditions.
2.3. Test Methods
The compressive strength tests were conducted in accordance with GB/T 50081-2019 [50], and the chloride migration coefficients followed GB/T 50082-2009 [51]. For each mixture, three replicate specimens were prepared for compressive strength and chloride migration coefficient measurements at each designed age. All specimens of the same mixture were cast from one single batch of fresh mixture to eliminate batch-to-batch variation. The microstructure morphology was characterized using an environmental scanning electron microscope (Quattro S, Thermo Fisher Scientific, Eindhoven, The Netherlands). The mineral composition of hydration products was analyzed by an X-ray diffractometer (X’Pert Powder, PANalytical, Almelo, The Netherlands).
2.4. Statistical Analysis
All compressive strength and chloride migration coefficient data were analyzed according to the following statistical procedures [52]. For experimental groups with complete individual replicate measurements, the sample standard deviation (STDEV.S, n − 1 degrees of freedom) was calculated to reflect experimental variability. For groups without archived individual replicate specimens (10%, 15%, 20% dosage groups in Figures 4 and 5, and PE, ABF, EPS insulation groups in Figure 7), standard deviation values were estimated using the coefficient of variation (CV). The CV is defined as CV = SD/, where SD denotes sample standard deviation and is the mean compressive strength. At each testing age, the CV value was taken as the average of the corresponding-age CV values obtained from two reference datasets: the plain-cement series (Figure 2) and the early-strength-agent series (Figure 6). These two reference groups were fabricated, cured and tested under nearly identical low temperature static curing conditions. The steam-curing series (Figure 8) was excluded from CV calculation because steam curing triggers drastically accelerated hydration and creates distinctly different data dispersion characteristics. For a given testing age, the same reference CV was adopted for all subgroups within Figures 4, 5 and 7. We assume that the relative experimental scatter originating from specimen preparation and loading testing remains comparable among these groups. It should be noted that these estimated SD values cannot capture potential differences in material inherent heterogeneity induced by different mineral admixture dosages or insulation treatments. These estimated SD values and corresponding approximate statistical outputs are explicitly labeled throughout tables, figures and text.
Figure 2.
Strength development of concrete within 1 d at 10 °C and 20 °C, with exponential and logarithmic fitting curves. Error bars: sample standard deviation from replicate measurements, n = 3.
The normality of residuals was assumed for all statistical comparisons. The significance level was set at α = 0.05. Statistical significance was judged by p-values, with p < 0.05 considered statistically significant. One-way analysis of variance (ANOVA) combined with Tukey’s post hoc test was adopted for multi-group comparisons. Independent two-sample t-tests were used for pairwise comparisons between two groups. Effect sizes were reported using Cohen’s d for t-tests and η2 for ANOVA. It should be noted that compressive strength testing is destructive; distinct specimens were tested at different ages, and therefore repeated-measures ANOVA was not applicable in this work.
For long-term compressive strength evaluation, a two-one-sided test (TOST) non-inferiority analysis was performed to assess whether earlier-age-strength-promoting measures would induce practically relevant long term strength deterioration. A 10% relative strength reduction margin was pre-specified as the primary non-inferiority threshold prior to any statistical computation. This margin was derived from widely accepted engineering tolerances for concrete compressive strength deviation reported in relevant standards and literature [53,54]; it does not constitute a mandatory code-enforced limit. A sensitivity analysis with a stricter 8% strength reduction margin was additionally conducted to evaluate the robustness of conclusions with respect to margin selection. Non-inferiority was concluded when the one-sided 95% lower confidence bound of the relative-strength ratio lay above the pre-specified non-inferiority margin. This bound is numerically identical to the lower limit of a two-sided 90% confidence interval. Non-inferiority testing was not applied to chloride migration coefficient data, only t-test-based group comparisons are presented for durability related results.
The 95% confidence intervals for group means were computed based on the t-distribution. We acknowledge that a sample size of n = 3 per group follows standard test specifications for cementitious materials yet provides relatively low statistical power. This limitation is further elaborated within the Discussion section. All available individual replicate measurements are provided in Supplementary File S1.
In summary, this experimental program covers three research modules: (1) characterization of earlier-age strength evolution of plain concrete at 10 °C and 20 °C; (2) evaluation of the influence of GGBS and FA on earlier-age strength; (3) performance verification of multiple strength promotion measures, including investigation of their long-term compressive strength and chloride migration coefficient durability. Compressive strength at multiple ages, chloride migration coefficient, XRD and SEM micro-characterization were carried out for corresponding groups.
3. Results and Discussion
3.1. Compressive Strength Development Within 1 d
Figure 2 shows the compressive strength development rate of concrete within 1 d at a curing temperature of about 10 °C, and it gives the corresponding value at about 20 °C as a reference [50]. Only cement was used as the cementitious material to avoid the influence of supplementary cementing materials. The mixture proportions are shown in Table 2. The interval for concrete strength testing is 1 h. Non-linear fitting was carried out on the measured strength–age data, and the fitted parameters and corresponding statistical indices are summarized in Table 3. Residual plots for model performance evaluation are given in Supplementary File S1 (Figure S1). Replicate compressive strength data are given in Supplementary File S1 (Tables S1 and S2).
Table 3.
Fitted parameters and statistical indices of strength growth model for blank group concrete.
It can be seen from Figure 2 that the compressive strength of concrete continuously increases under 10 °C, yet its overall growth rate remains relatively slow. It only reaches 12.0 MPa at 24 h, markedly lower than the value of 28.9 MPa observed at 20 °C. The degree of compressive strength growth varies across different time periods, specifically, the compressive strength has maintained a slow growth within 21 h at 10 °C, especially within 12 h, where the strength is only 2.2 MPa, and the strength growth rate has slightly increased only after 21 h, but the strength has significantly increased after 12 h at 20 °C. Compared with 20 °C, the latent stage of strength growth at 10 °C is significantly longer, which has a significant negative impact on the removal of formwork for cast-in-place concrete and concrete products.
In addition, the compressive strength growth law of concrete at 10 °C is similar to that observed at 20 °C. Fitting results demonstrate that compressive strength evolves with an initial exponential stage followed by a later logarithmic stage within 1 d, although the duration of each stage differs markedly. Specifically, for concrete cured at 20 °C, slow exponential strength growth occurs from 1 to 12 h, followed by accelerated exponential growth from 12 to 18 h; the transition point from exponential to logarithmic growth appears at 18 h. For concrete cured at 10 °C, the exponential growth phase extends to 21 h, after which the strength follows a logarithmic growth trend. These transition hours were empirically determined by comparing fitting performance across multiple candidate split points. This prolonged exponential phase accounts for the slow early strength development under low temperature conditions. Meanwhile, this finding reveals that the conventional view of purely logarithmic strength gain cannot describe the strength evolution of concrete within 1 d.
3.2. Strength Development of Concrete Within 28 d
Figure 3 shows the compressive strength development of concrete within 28 d at 10 °C and 20 °C. The mixture proportions are shown in Table 2. It can be seen from the figure that the overall growth of concrete strength after 1 d at different curing temperatures follows a logarithmic pattern. Replicate compressive strength data are given in Supplementary File S1 (Table S3).
Figure 3.
Development of concrete strength within 28 d at 10 °C and 20 °C. Error bars: sample standard deviation from replicate measurements, n = 3.
When the age increases from 1 d to 3 d, the compressive strength increases significantly at 10 °C, by 36.4 MPa, while it is 23.3 MPa at 20 °C. At low temperature, the strength increases faster during 1~3 d, rapidly narrowing the strength gap with the corresponding age group at high temperature, indicating that the degree of temperature influence gradually decreased. Although the temperature has an impact on the strength after 28 d, the degree rapidly decreases. The significant effect of curing temperature on strength development is mainly reflected within 3 d.
In summary, if the required early strength target is after 3 d, the curing temperature is hardly the most important factor affecting the strength development. If there is an obvious demand for strength development within 3 d, it is necessary to focus on the impact of curing temperature.
3.3. Effect of GGBS and FA on Earlier-Age Strength Development
Supplementary cementing materials (SCMs) are added to concrete to form a part of the cementitious materials, which are likely to have a significant impact on the strength development of concrete within 1 d. In the actual production process, the optimal amount of supplementary cementing materials will be determined according to the properties and the expected effect on concrete, but the reasonable amount may vary on different occasions. When GGBS and FA were selected in this section, the influence of different dosages on the strength development within 1 d was studied without considering the compound mixing. The dosages of GGBS and FA were 10%, 15% and 20% of the cementitious materials, respectively. The mix proportions were based on Table 2; when GGBS and FA were added to the concrete, the same mass of OPC as GGBS or FA would be replaced. The strength results are shown in Figure 4 and Figure 5. Mean strength date and calculations of estimated sample standard deviation are given in Supplementary File S1 (Tables S4–S8).
Figure 4.
Effect of GGBS on earlier-age strength development at 10 °C and 20 °C. Error bars: estimated sample standard deviation.
Figure 5.
Effect of FA on earlier-age strength development at 10 °C and 20 °C. Error bars: estimated sample standard deviation.
It can be seen from Figure 4 that the addition of GGBS reduces the compressive strength within 1 d. At an identical temperature and testing age, higher GGBS replacement dosage generally leads to a greater magnitude of strength reduction. The adverse strength reducing effect induced by GGBS varies over different hydration stages, and such stage-related characteristics are strongly temperature-dependent. Taking 20 °C as an example, in the latent stage at 12 h, the strength reduction magnitudes are 12.8% (10% GGBS), 25.5% (15% GGBS), and 29.8% (20% GGBS); after entering 14 h, the corresponding reduction magnitudes increase to 13.9%, 30.6%, and 40.3%, respectively. Within each stage, strength reduction becomes more pronounced with increasing GGBS dosage. However, such consistent stage evolution behavior cannot be observed at 10 °C.
Collectively, GGBS exerts an adverse influence on earlier-age strength development, and its magnitude is jointly affected by replacement dosage, hydration stage and curing temperature. Note that these comparisons are based on descriptive relative strength reduction percentages calculated from group averaged data; formal statistical significance cannot be evaluated for these groups owing to the unavailability of individual replicate measurements.
As for FA, although there are few research results on the influence of FA on the strength development within 1 d, it will also inevitably have adverse effects on the earlier-age strength development from the role of FA in concrete [55,56], but the degree of influence is unknown. Therefore, it is necessary to study the influence of FA on the strength development of concrete within 1 d.
It can be seen from Figure 5 that FA incorporation also imposes adverse effects on compressive strength within 1 d. Similar to GGBS, at an identical temperature and age, higher FA dosage generally leads to more pronounced strength reduction, and this stage-related adverse effect is temperature-dependent. At 20 °C, strength-reduction magnitudes are 8.5% (10% FA), 23.4% (15% FA), and 34.0% (20% FA) after 12 h, and they rise to 12.5%, 23.6%, 37.5% after 14 h. Such a consistent stage-evolution trend is not clearly observed at 10 °C. Collectively, FA exerts an adverse influence on earlier-age strength development. These percentages are descriptive values calculated from group-averaged data; formal statistical significance cannot be evaluated for these groups due to missing individual replicate measurements.
As observed in Figure 4 and Figure 5, the strength-reducing effect of GGBS and FA varies obviously under different curing temperatures and is less pronounced at 10 °C. This phenomenon stems from two co-existing factors: the inherent reaction characteristics of mineral admixtures themselves and the synergistic adverse effect of low curing temperature. The slow secondary pozzolanic reaction is an inherent property of these mineral admixtures, whereby they mainly exert physical filling effects at early age. Meanwhile, the 10 °C curing condition retards cement hydration and extends the latent stage, delaying the generation of calcium hydroxide and further postponing the secondary pozzolanic reaction beyond the 1 d test window. Low absolute strength at 10 °C also compresses strength differences induced by different admixture dosages. Note that this is a mechanistic descriptive interpretation; quantitative separation of the two factors is not feasible due to missing individual replicate data for GGBS and FA groups, as noted in Section 2.4.
3.4. Promotion of Earlier-Age Concrete Strength Within 1 d
Early-age-strength-promoting technologies mainly aim to optimize the material itself and the curing methods. The material itself mainly refers to the optimization of the composition of concrete materials, so that the hydration heat with a slow original release rate can be released as soon as possible, so as to achieve the purpose of strength promoting. Among them, adding early-strength agents is considered to effectively promote the early strength of concrete, while commonly used early-strength agents are aimed at strength promotion after 1 d. There is still a lack of research results on strength development within 1 d. Curing methods including thermal insulation or thermal curing are also often adopted to promote early-age strength [57]. There is also a relative lack of research on the effect of promoting strength within 1 d. In this section, the effect of adding an early-strength agent, thermal insulation curing and steam curing on the promotion of earlier-age strength were studied.
(1) Early-strength agent
Figure 6 shows the effect of early-strength agent CCP on strength promotion at an earlier age. The test age is 6~24 h, with an interval of 1 h. Replicate compressive strength data are given in Supplementary File S1 (Tables S9 and S10). It can be seen from Figure 6 that the effect of CCP on promoting the strength is very obvious, while the curing temperature has an obvious impact on the effect. The curing temperature mainly affects the time when CCP starts to play its role on promoting the strength, and it also affects the degree of strength promoting to a certain extent. The strength of concrete added with CCP can be increased from 6.4 MPa for the blank group to 10.8 MPa after 20 h under 10 °C; when the curing temperature rises to 20 °C, the strength can be increased from 7.2 MPa to 20.6 MPa after 14 h, that is, CCP can take effect earlier.
Figure 6.
Effect of CCP on promoting earlier-age strength at 10 °C and 20 °C. Error bars: sample standard deviation from replicate measurements, n = 3.
Statistical comparisons at representative ages (12 h and 18 h) between blank and 5% CCP groups further quantify the temperature-dependent effect. At 10 °C after 12 h, the strength increment is +31.8% (Δ = +0.7 MPa, mean strength difference; 95% CI [0.25, 1.15] MPa, 95% confidence interval, Cohen’s d = 3.50); at 10 °C after 18 h, the strength increment is +88.0% (Δ = +4.4 MPa, 95% CI [2.10, 6.70] MPa, Cohen’s d = 5.79). At 20 °C after 12 h, the strength increment reaches +208.5% (Δ = +9.8 MPa, 95%CI [5.30, 14.30] MPa, Cohen’s d = 8.31); at 20 °C after 18 h, the strength increment is +69.0% (Δ = +11.6 MPa, 95%CI [4.90, 18.30] MPa, Cohen’s d = 5.32). Note that these statistical results are based on n = 3 replicates per group, leading to relatively wide confidence intervals and limited statistical power. Larger effect sizes and higher relative strength gains confirm that the strength-promoting effect of CCP is markedly stronger at 20 °C than at 10 °C under identical ages.
In general, the early-strength agent CCP has an obvious effect on promoting the strength of earlier-age concrete, and the use of an effective early-strength agent is an effective method to promote strength at an earlier age. However, it should also be noted that when the curing temperature is relatively low, the age of the early-strength agent CCP to promote the strength will be delayed. If it is necessary to promote the strength before 12 h when the curing temperature is relatively low, other measures need to be taken.
(2) Thermal insulation
When the curing temperature is relatively low, the heat released by cementitious materials under the excitation of an early-strength agent dissipates relatively easily, so the insulation of concrete can also promote earlier-age strength to a certain extent, theoretically.
Figure 7 shows the strength comparison results under different degrees of thermal insulation measures and natural curing conditions. All error-bar values in this figure represent estimated standard deviations; formal statistical significance tests cannot be performed for these insulation groups owing to a lack of archived individual replicate data. Descriptive relative-strength percentages versus the blank control are provided below for magnitude comparison only. Mean compressive strength data and estimated sample standard deviations are given in Supplementary File S1 (Tables S11 and S12). Effect of different insulation measures on temperature of concrete are given in Supplementary File S1 (Figure S2).
Figure 7.
Effect of different insulation measures on promoting earlier-age strength at 10 °C and 20 °C. Error bars: estimated sample standard deviation.
It can be seen from Figure 7 that the strength can be promoted by taking these thermal insulation measures. Whereas the effects on promoting the strength are relatively limited when the curing temperature is 10 °C, the strength of concrete cured in an insulated box is only 10.0 MPa at 20 h (122.0% relative to the blank control). When the curing temperature rises to 20 °C, the insulation measures show a promoting effect on strength from 8 h compared to the blank group (137.5% relative to the blank control). In short, when the curing temperature is low, taking insulation measures can promote the strength of concrete, while it came into effect relatively late.
(3) Steam curing
The steam curing measure adopted is to maintain the curing temperature at 55 ± 0.5 °C for 3 h from 2 h after the concrete is casted and then put it at the set curing temperature, which is 10 °C and 20 °C, respectively.
Figure 8 shows the strength development of earlier-age concrete cured by steam curing at different curing temperatures. Replicate compressive strength data are given in Supplementary File S1 (Tables S13 and S14). Temperature changes of concrete after thermal curing are given in Supplementary File S1 (Figure S3). Statistical comparisons between blank and steam curing groups at representative ages (8 h, 12 h and 20 h) quantify the steam curing effect under each ambient-temperature condition. At 10 °C after 8 h, the strength increment is +126.3% (mean difference Δ = +5.1 MPa, 95% CI [2.51, 7.69] MPa, Cohen’s d = 5.22); 10 °C and 12 h, +112.7% (Δ = +7.0 MPa, 95%CI [3.44, 10.56] MPa, Cohen’s d = 5.01); 10 °C and 20 h, +62.1% (Δ = +6.8 MPa, 95% CI [2.83, 10.77] MPa, Cohen’s d = 4.43). At 20 °C after 8 h, the strength increment is +147.2% (mean difference Δ = +6.7 MPa, 95% CI [3.42, 9.98] MPa, Cohen’s d = 6.12); 20 °C and 12 h, +130.4% (Δ = +8.3 MPa, 95% CI [4.15, 12.45] MPa, Cohen’s d = 5.84); 20 °C and 20 h, +74.6% (Δ = +7.6 MPa, 95% CI [3.31, 11.89] MPa, Cohen’s d = 4.96). Note that these statistical results are based on n = 3 replicates per group, leading to relatively wide confidence intervals and limited statistical power. All confidence intervals exclude zero, confirming measurable strength improvement by steam curing; larger relative strength gains occur at earlier ages, and the promoting effect is stronger at 20 °C than at 10 °C under matched ages.
Figure 8.
Effect of steam curing on promoting earlier-age strength at 10 °C and 20 °C. Error bars: sample standard deviation from replicate measurements, n = 3.
It can be seen from Figure 8 that the strength development law after steam curing at different curing temperatures is obviously different. The growth rate of concrete strength after steam curing is relatively uniform at 10 °C, and it is significantly higher than that of the blank group. When the curing temperature is 20 °C, the strength increases more obviously within 4 h after the end of steam curing, and then the speed of strength increase tends to be uniform. Relatively high strength can be obtained at an earlier age by steam curing. Especially when the curing temperature is 10 °C, the earlier-age strength is increased more significantly: strength can be achieved close to 15.0 MPa at 8 h, while the strength of the blank group is less than 2.0 MPa, indicating that steam curing is still one of the effective measures if it is necessary to obtain high earlier-age strength when the curing temperature is relatively low.
3.5. Microanalysis
There have been numerous studies on the early and long-term microstructure of concrete, while research on the microstructure at an earlier age remains relatively scarce. This article focuses on the microstructure of concrete at an earlier age under various insulation measures to elucidate the impact of strength-promoting measures on the microstructure of concrete.
The microstructures of the specimens cured for 20 h were observed using SEM, and their mineral compositions were analyzed by XRD. Before microanalysis, all specimens were broken into small pieces, soaked in anhydrous ethanol for 24 h and dried to stop hydration. For SEM observation, small fragments were selected as test samples. For XRD testing, coarse aggregates were removed from the dried material; the remaining paste fraction was ground and sieved through a 250-mesh sieve for subsequent mineralogical analysis.
Figure 9 and Figure 10 show the microstructure of concrete with different thermal insulation measures by XRD and SEM. The specimen without thermal insulation measures that was hydrated for 20 h at 10 °C is marked as 10 °C-20 h-B, while the samples covered with ABF insulation film and EPS insulation box are marked as 10 °C-20 h-ABF and 10 °C-20 h-EPS, respectively.
Figure 9.
XRD patterns of hydration products in concrete by different insulation measures. Green dashed box: diffraction peak position of hydration product.
Figure 10.
Microstructures of concrete by different insulation measures: (a) 10 °C-20 h-B, (b) 10 °C-20 h-ABF, and (c) 10 °C-20 h-EPS.
(1) XRD.
It can be seen from Figure 9 that diffraction peaks corresponding to Ca(OH)2 were detected for both the ABF and EPS groups at 20 h under 10 °C. The compressive strengths reached 9.5 MPa and 10.0 MPa for the ABF and EPS groups, respectively, compared with 6.4 MPa for the blank group. It can also be seen from Figure 9 that different thermal insulation measures do not change the types of hydration products formed in concrete; no new crystalline hydration phases were identified. This mineralogical observation is qualitatively consistent with the improved compressive strength performance under insulation treatments, although quantitative assessment of hydration degree cannot be achieved from conventional XRD patterns.
(2) SEM.
It can be seen from Figure 10 that the cement particle surface of the blank group shows slight etching with sporadic hydration products after 20 h, indicating limited hydration-related morphological development. Specimens treated with ABF insulation show more visible hydration products deposited on cement particle surfaces; abundant flocculent hydration products can be observed, and short-rod-shaped AFt crystals are also present. These morphological features are qualitatively consistent with macro strength promotion after insulation curing.
3.6. Long-Term Concrete Properties
Promoting earlier-age strength of concrete should not significantly affect long-term strength development and durability. The compressive strengths and durability of concrete after 28 d, 90 d, and 3 y under various promoting measures of earlier age at 10 °C were investigated. For the concrete cured with PE film, ABF film and EPS box, the thermal insulation measures shall be removed after 24 h of molding. Each group of concrete was molded and cured at a curing temperature of 10 ± 0.5 °C for 28 d, and then it was cured to the corresponding age under standard conditions (20 ± 2 °C, relative humidity ≥ 95%), according to GB/T 50081-2019 [50].
(1) Long-term compressive strength
Figure 11 shows the strengths of concrete after 28 d, 90 d and 3 years under five conditions at 10 °C: mixture with 5% CCP, three thermal insulation schemes, and steam curing. Replicate compressive strength data are given in Supplementary File S1 (Table S15). All five promoting measures produced only small reductions in long-term strength relative to the blank group (all n = 3 replicates per group). After 3 years, the mean strength was 92.2 ± 5.8 MPa for the blank group and 85.8 ± 5.4 MPa for the steam-curing group, i.e., a ratio of 0.931 (a 6.94% reduction); Welch’s t-test gave Δ = −6.40 MPa, 95% CI [−19.08, 6.28] MPa, and p = 0.233, so no statistically significant reduction was detected. The reductions for the other measures were 1.63% (PE), 2.82% (ABF), 4.12% (EPS) and 4.66% (5% CCP). However, the 95% confidence interval of the strength ratio (0.798–1.063 for steam curing) lies well below the pre-specified 10% non-inferiority margin (0.90) and the 8% sensitivity margin (0.92); therefore, formal non-inferiority could not be confirmed at these margins with n = 3 replicates, and the small point-estimate reductions should not be interpreted as proven equivalence. Full raw replicate data for all five experimental groups can be found in Supplementary Table S15; therefore, complete t-test outputs for the other four groups are not repeated within the main text. As age increased, all concrete strengths increased substantially, and the effects of different promoting measures on long-term strength differed: short-term steam curing is the most disadvantageous among the promoting measures.
Figure 11.
Strength development with different promoting measures at 10 °C: (a) 28 d, (b) 90 d, and (c) 3 years. Error bars: sample standard deviation from replicate measurements, n = 3.
(2) Chloride migration coefficients
The chloride migration coefficient is one of the most commonly used indicators for characterizing concrete durability, which can reflect the compactness of concrete [58]. In this paper, the 28 d chloride migration coefficient was selected to reflect the durability of concrete. The selection of concrete specimens is the same as that for the long-term concrete strength test. Replicate chloride migration coefficient data are given in Supplementary File S1 (Table S16).
Mean values and sample standard deviations for each group are reported in Figure 12 (unit: 10−12 m2/s): blank group = 4.0 ± 0.1; 5% CCP = 3.9 ± 0.1; PE = 4.0 ± 0.1; ABF = 4.1 ± 0.1; EPS = 4.0 ± 0.2; steam curing = 4.4 ± 0.1. Welch’s independent-sample t-test indicates that steam curing induced a statistically-significant increase in chloride migration coefficient (Δ = +0.40 × 10−12 m2/s, 95% CI [+0.17, +0.63] × 10−12 m2/s, p = 0.008, Cohen’s d = 2.81), corresponding to a point-estimate relative increase of 10.0%.
Figure 12.
Effect of earlier-age strength promoting measures on chloride migration coefficient. Error bars: sample standard deviation from replicate measurements, n = 3.
Unlike compressive strength, for which pre-specified relative non-inferiority margins are available drawing on widely accepted engineering tolerances, standards for the chloride migration coefficient provide absolute grade-based limits rather than a universally accepted relative percentage-based allowable increase margin for comparing different concrete mixtures. Those standard absolute limits are conventionally intended for 84 d assessment and cannot be directly applied to the 28 d test age used in this work. Therefore, no pre-defined quantitative relative acceptance criterion or formal non-inferiority margin was established for this durability index. Although the absolute change magnitude is moderate, this observation provides only descriptive interpretation rather than formal pass–fail judgement. No statistically significant differences in chloride migration coefficient were detected for 5% CCP, PE, ABF and EPS groups compared with the blank reference. Raw replicate data are given in Supplementary Table S16.
4. Conclusions
This paper investigated earlier-age (within 1 d) concrete strength development under a low temperature of 10 °C, its correlation with compressive strength within 28 d, and the influences of supplementary cementing materials. Several strength-promoting approaches were evaluated, together with their long-term strength and durability impacts. The following conclusions can be drawn:
- (1)
- Ambient temperature markedly governs earlier-age strength evolution. Concrete at 10 °C exhibits a two-stage growth pattern (initially exponential, subsequently logarithmic) similar to 20 °C specimens but with an extended latent slow-growth phase. Strength rises rapidly from 1 to 3 d at 10 °C, narrowing the strength gap versus 20 °C, which further diminishes after 28 d.
- (2)
- GGBS and FA reduce earlier-age strength, especially during rapid strength-growth stages. Avoiding or lowering their dosages is recommended for high earlier-age strength requirements. This inference is based on descriptive comparisons, as raw replicate data are unavailable for formal statistics.
- (3)
- Early-strength agent and thermal insulation treatments improve earlier-age strength, with stronger effects at 20 °C. Under low ambient temperatures, steam curing is required to reach target earlier-age strength.
- (4)
- Though long-term strength losses from promoting measures are moderate in engineering practice, statistical non-inferiority cannot be validated by TOST analysis with n = 3 replicates. Steam curing leads to statistically significant moderate growth of the chloride migration coefficient, while no significant durability change occurs for other treatments.
Several study limitations should be noted. Results are valid for this concrete mixture under laboratory 10 °C/20 °C curing; extrapolation to other binder systems or field conditions needs further tests. Raw replicate data are missing for the GGBS, FA and partial-insulation groups, whose dispersion values were estimated. The limited sample size (n = 3) yields wide confidence intervals and restricts statistical power.
Supplementary Materials
The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/ma19234990/s1.
Author Contributions
Conceptualization, C.F. and L.M.; methodology, C.F. and H.S.; data curation, C.F., L.M. and H.S.; writing—original draft preparation, C.F.; writing—review and editing, C.F., L.M. and H.S.; supervision, C.F. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by the National Key R&D Program of China (No. 2017YFB0310003).
Institutional Review Board Statement
Not applicable.
Informed Consent Statement
Not applicable.
Data Availability Statement
All raw experimental data are available in Supplementary File S1. Further inquiries can be directed to the corresponding author.
Conflicts of Interest
The authors declare no conflicts of interest.
References
- Damme, H. Concrete material science: Past, present, and future innovations. Cem. Concr. Res. 2018, 112, 5–24. [Google Scholar] [CrossRef] [Scilit]
- Aitcin, P. Cements of yesterday and today concrete of tomorrow. Cem. Concr. Res. 2000, 30, 1349–1359. [Google Scholar]
- Nunez, I.; Marani, A.; Flah, M.; Nehdi, M. Estimating compressive strength of modern concrete mixtures using computational intelligence: A systematic review. Constr. Build. Mater. 2021, 310, 125279. [Google Scholar] [CrossRef] [Scilit]
- Dushimimana, A.; Niyonsenga, A.; Nzamurambaho, F. A review on strength development of high performance concrete. Constr. Build. Mater. 2021, 307, 124865. [Google Scholar] [CrossRef] [Scilit]
- Scrivener, K.; Kirkpatrick, R. Innovation in use and research on cementitious material. Cem. Concr. Res. 2008, 38, 128–136. [Google Scholar] [CrossRef] [Scilit]
- Juenger, M.; Siddique, R. Recent advances in understanding the role of supplementary cementitious materials in concrete. Cem. Concr. Res. 2015, 78, 71–80. [Google Scholar] [CrossRef] [Scilit]
- Xu, D.; Cui, Y.; Li, H.; Yang, K.; Xu, W.; Chen, Y. On the future of Chinese cement industry. Cem. Concr. Res. 2015, 78, 2–13. [Google Scholar] [CrossRef] [Scilit]
- Cheung, J.; Roberts, L.; Liu, J. Admixtures and sustainability. Cem. Concr. Res. 2018, 114, 79–89. [Google Scholar] [CrossRef] [Scilit]
- Wembe, J.; Ngueyep, L.; Moukete, E.; Eslammi, J.; Pliya, P.; Ndjaka, J.; Noumowe, A. Physical, mechanical properties and microstructure of concretes made with natural and crushed aggregates: Application in building construction. Clean. Mater. 2023, 7, 100173. [Google Scholar] [CrossRef] [Scilit]
- Liu, J.; Yu, C.; Shu, X.; Ran, Q.; Yang, Y. Recent advance of chemical admixtures in concrete. Cem. Concr. Res. 2019, 124, 105834. [Google Scholar] [CrossRef] [Scilit]
- Qian, J. Building Materials Science; Wuhan University of Technology Press: Wuhan, China, 2007. [Google Scholar]
- Sakai, E.; Miyahara, S.; Ohsawa, S.; Lee, S.; Daimon, M. Hydration of fly ash cement. Cem. Concr. Res. 2005, 35, 1135–1140. [Google Scholar] [CrossRef] [Scilit]
- Gagg, C. Cement and concrete as an engineering material: An historic appraisal and case study analysis. Eng. Fail. Anal. 2014, 40, 114–140. [Google Scholar] [CrossRef] [Scilit]
- Tang, Z.; Lim, Y.; Smith, S.; Mostafa, A.; Lam, A.; Soh, C. Monitoring the curing process of in-situ concrete with piezoelectric-based techniques—A practical application. Struct. Health Monit. 2023, 22, 518–539. [Google Scholar] [CrossRef] [Scilit]
- Escalante-Garcia, J.; Sharp, J. Effect of temperature on the hydration of the main clinker phases in portland cements: Part II, blended cements. Cem. Concr. Res. 1998, 28, 1259–1274. [Google Scholar] [CrossRef] [Scilit]
- Marcialis, A.; Massidda, L. Low temperature steam curing hydration of lime-fly ash compacts. Cem. Concr. Res. 1983, 13, 887–894. [Google Scholar] [CrossRef] [Scilit]
- Kosmatka, S.; Wilson, M. Design and Control of Concrete Mixtures; Portland Cement Association: Skokie, IL, USA, 2016. [Google Scholar]
- Yan, P.; Zhang, B. Mechanical Properties of High Strength Concrete Prepared with Different Densities of Silica Fume. J. Chin. Ceram. Soc. 2016, 44, 196–201. [Google Scholar]
- Wong, H.; Razak, H. Efficiency of calcined kaolin and silica fume as cement replacement material for strength performance Cem. Concr. Res. 2005, 35, 696–702. [Google Scholar] [CrossRef] [Scilit]
- Heikal, M. Effect of calcium formate as an accelerator on the physicochemical and mechanical properties of pozzolanic cement pastes. Cem. Concr. Res. 2004, 34, 1051–1056. [Google Scholar] [CrossRef] [Scilit]
- Felekoglu, B. A method for improving the early strength of pumice concrete blocks by using alkyl alkoxy silane (AAS). Constr. Build. Mater. 2012, 28, 305–310. [Google Scholar] [CrossRef] [Scilit]
- Sandberg, P.; Doncaster, F. On the mechanism of strength enhancement of cement paste and mortar with triisopropanolamine. Cem. Concr. Res. 2004, 34, 973–976. [Google Scholar] [CrossRef] [Scilit]
- Sun, J.; Shi, H.; Qian, B.; Xu, Z.; Li, W.; Shen, X. Effects of synthetic C-S-H/PCE nanocomposites on early cement hydration. Constr. Build. Mater. 2017, 140, 282–292. [Google Scholar] [CrossRef] [Scilit]
- Kanchanason, V.; Plank, J. Effectiveness of a calcium silicate hydrate—Polycarboxylate ether (C-S-H-PCE) nanocomposite on early strength development of fly ash cement. Constr. Build. Mater. 2018, 169, 20–27. [Google Scholar] [CrossRef] [Scilit]
- Zou, F.; Hu, C.; Wang, F.; Ruan, Y.; Hu, S. Enhancement of early-age strength of the high content fly ash blended cement paste by sodium sulfate and C-S-H seeds towards a greener binder. J. Clean. Prod. 2020, 244, 118566. [Google Scholar] [CrossRef] [Scilit]
- Zhang, J.; Ye, C.; Tan, H.; Liu, X. Potential application of Portland cement—Sulfoaluminate cement system in precast concrete cured under ambient temperature. Constr. Build. Mater. 2020, 251, 118869. [Google Scholar] [CrossRef] [Scilit]
- Abhilash, P.; Nayak, D.; Sangoju, B.; Kumar, R.; Kumar, V. Effect of nano-silica in concrete; a review. Constr. Build. Mater. 2021, 278, 122347. [Google Scholar] [CrossRef] [Scilit]
- Norhasri, M.; Hamidah, M.; Fadzil, A. Applications of using nano material in concrete: A review. Constr. Build. Mater. 2017, 133, 91–97. [Google Scholar] [CrossRef] [Scilit]
- Grrit, L.; Dietmar, S. Controlling cement hydration with nanoparticles. Cem. Concr. Compos. 2015, 57, 64–67. [Google Scholar] [CrossRef] [Scilit]
- Hubler, M.; Thomas, J.; Jennings, H. Influence of nucleation seeding on the hydration kinetics and compressive strength of alkali activated slag paste. Cem. Concr. Res. 2011, 41, 842–846. [Google Scholar] [CrossRef] [Scilit]
- Ouyang, X.; Koleva, D.; Ye, G.; Breugel, K. Insights into the mechanisms of nucleation and growth of C-S-H on fillers. Mater. Struct. 2017, 50, 213. [Google Scholar] [CrossRef] [Scilit]
- Land, G.; Stephan, D. The effect of synthesis conditions on the efficiency of C-S-H seeds to accelerate cement hydration. Cem. Concr. Compos. 2018, 87, 73–78. [Google Scholar] [CrossRef] [Scilit]
- John, E.; Matschei, T.; Stephan, D. Nucleation seeding with calcium silicate hydrate—A review. Cem. Concr. Res. 2018, 113, 74–85. [Google Scholar] [CrossRef] [Scilit]
- Kang, X.; Zhu, X.; Liu, J.; Shu, X.; Qian, J.; Huang, Y. Hydration of C3A/gypsum composites in the presence of graphene oxide. Mater. Today Commun. 2020, 23, 100889. [Google Scholar] [CrossRef] [Scilit]
- Zhu, X.; Kang, X. Effect of graphene oxide (GO) on the hydration and dissolution of alite in a synthetic cement system. J. Mater. Sci. 2019, 55, 3419–3433. [Google Scholar] [CrossRef] [Scilit]
- Chintalapudi, K.; Pannem, R. An intense review on the performance of graphene oxide and reduced graphene oxide in an admixed cement system. Constr. Build. Mater. 2020, 259, 120598. [Google Scholar] [CrossRef] [Scilit]
- Jing, G.; Wu, J.; Lei, T.; Wang, S.; Strokova, V.; Nelyubova, V.; Wang, M.; Ye, Z. From graphene oxide to reduced graphene oxide: Enhanced hydration and compressive strength of cement composites. Constr. Build. Mater. 2020, 248, 118699. [Google Scholar] [CrossRef] [Scilit]
- Yan, P.; Cui, Q. Effects of Curing Regimes on Strength Development of High-Strength Concrete. J. Chin. Ceram. Soc. 2015, 43, 133–137. [Google Scholar]
- Liu, Y.; Fu, S.; Gao, J.; Yang, Y. Prediction for temperature evolution and compressive strength of non-mass concrete with thermal insulation curing in cold weather. J. Build. Eng. 2020, 32, 101737. [Google Scholar] [CrossRef] [Scilit]
- Cassagnabère, F.; Escadeillas, G.; Mouret, M. Study of the reactivity of cement/metakaolin binders at early age for specific use in steam cured precast concrete. Constr. Build. Mater. 2009, 23, 775–784. [Google Scholar] [CrossRef] [Scilit]
- Hanif, A.; Kim, Y.; Lu, Z.; Park, C. Early-age behavior of recycled aggregate concrete under steam curing regime. J. Clean. Prod. 2017, 152, 103–114. [Google Scholar] [CrossRef] [Scilit]
- Gallucci, E.; Zhang, X.; Scrivener, K. Effect of temperature on the microstructure of calcium silicate hydrate (CSH). Cem. Concr. Res. 2013, 53, 185–195. [Google Scholar] [CrossRef] [Scilit]
- Zeyad, A.; Tayeh, B.; Adesina, A.; Azevedo, A.; Amin, M.; Hadzima-Nyarko, M.; Agwa, I. Review on effect of steam curing on behavior of concrete. Clean. Mater. 2022, 3, 100042. [Google Scholar] [CrossRef] [Scilit]
- GB/T 18046-2017; Ground Granulated Blast Furnace Slag Used for Cement, Mortar and Concrete. Standards Press of China: Beijing, China, 2017.
- GB/T 1596-2017; Fly Ash Used for Cement and Concrete. Standards Press of China: Beijing, China, 2017.
- Wang, F.; Kong, X.; Wang, D.; Wang, Q. The effects of nano-C-S-H with different polymer stabilizers on early cement hydration. J. Am. Ceram. Soc. 2019, 102, 5103–5116. [Google Scholar] [CrossRef] [Scilit]
- Lu, Z.; Kong, X.; Zhang, C.; Cai, Y. Effect of highly carboxylated colloidal polymers on cement hydration and interactions with calcium ions Cem. Concr. Res. 2018, 113, 140–153. [Google Scholar] [CrossRef] [Scilit]
- Zhang, L.; Miao, X.; Kong, X.; Zhou, S. Retardation effect of PCE superplasticizers with different architectures and their impacts on early strength of cement mortar. Cem. Concr. Comp. 2019, 104, 103369. [Google Scholar] [CrossRef] [Scilit]
- Fan, C.; Qian, J.; Sun, H.; Fan, Y. Development and Promotion of Concrete Strength at Initial 24 Hours. Materials 2023, 16, 4452. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- GB/T 50081-2019; Standard for Test Methods of Concrete Physical and Mechanical Properties. Standards Press of China: Beijing, China, 2019.
- GB/T 50082-2009; Standard for Test Method of Long-Term Performance and Durability of Ordinary Concrete. Standards Press of China: Beijing, China, 2009.
- Lakens, D.; Scheel, A.M.; Isager, P.M. Equivalence Testing for Psychological Research: A Tutorial. Adv. Methods Pract. Psychol. Sci. 2018, 1, 259–269. [Google Scholar] [CrossRef] [Scilit]
- GB/T 50152-2012; Standard for Test Method of Concrete Structures. Ministry of Housing and Urban-Rural Development of the People’s Republic of China: Beijing, China, 2012. (In Chinese)
- ACI 318-19; Building Code Requirements for Structural Concrete. American Concrete Institute: Farmington Hills, MI, USA, 2019.
- Qian, J. Fly Ash Characteristics and Fly Ash Concrete; Science Press: Beijing, China, 2002. (In Chinese) [Google Scholar]
- Sarker, P.K. (Ed.) Fly Ash: Sources, Applications and Potential Environmental Impacts; Nova Science Publishers: New York, NY, USA, 2014. [Google Scholar]
- He, J.; Ma, K.; Long, G.; Xie, Y. Mechanical Properties Evolution of Concrete in Steam-Curing Process. J. Chin. Ceram. Soc. 2018, 46, 1584–1592. (In Chinese) [Google Scholar]
- Sereewatthanawut, I.; Pansuk, W.; Pheinsusom, P.; Prasittisopin, L. Chloride-induced corrosion of a galvanized steel-embedded calcium sulfoaluminate stucco system. J. Build. Eng. 2021, 44, 103376. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.