Skip to Content
MaterialsMaterials
  • Article
  • Open Access

21 November 2026

25 Pages

Influence of Thermal and Mechanical Post-Processing on the Cavitation Erosion Resistance of LPBF Maraging Steel MS1

,
and
1
Faculty of Mechanical Engineering, University of Belgrade, 11000 Belgrade, Serbia
2
Faculty of Technology and Metallurgy, University of Belgrade, 11000 Belgrade, Serbia
*
Author to whom correspondence should be addressed.
This article belongs to the Section Manufacturing Processes and Systems

Abstract

Components exposed to flowing liquids may suffer cavitation erosion, and additively manufactured parts are no exception. This study examines the effects of age hardening, shot peening, and their combination on the cavitation erosion resistance of LPBF-produced MS1 maraging steel. Four specimen conditions, as-built, age-hardened, shot-peened, and aged + shot-peened, were tested for 24 h using an ultrasonic vibratory apparatus in accordance with ASTM G32. Cumulative mass loss, mean depth of erosion (MDE), and erosion rate were evaluated, while surface damage was examined by scanning electron microscopy. All post-processing treatments improved erosion resistance compared with the as-built condition, which reached an MDE of slightly above 14 µm after 24 h. Age hardening reduced the MDE to approximately 3 µm, whereas both shot-peened conditions remained below 2 µm. The shot-peened and aged + shot-peened specimens exhibited comparable erosion behaviour, with no clear additional benefit from aging before peening. SEM observations revealed ring-like pit patterns on age-hardened surfaces, whereas damage on shot-peened surfaces was more irregularly distributed. The results indicate that shot peening substantially improves the cavitation erosion resistance of LPBF MS1.

1. Introduction

Additive manufacturing (AM) builds components directly from digital models by layer-by-layer addition of material, enabling complex geometries, internal features and customized designs that are difficult to achieve by conventional methods [1]. AM also reduces material consumption (up to 40% for metallic materials), shortens manufacturing times and can provide favorable mechanical properties and surface characteristics [2,3,4,5]. Metal Additive Manufacturing (MAM) has therefore become a viable route for high-performance machine elements and engineering components in demanding applications. According to ISO/ASTM 52900:2021 [6], its main process families are Powder Bed Fusion (PBF), directed energy deposition, binder jetting and material extrusion, with cold gas spray emerging as an alternative for freeform metallic parts [7]. Among them, Laser Powder Bed Fusion (LPBF), also referred to as Selective Laser Melting (SLM) or Direct Metal Laser Sintering (DMLS), is one of the most widely used for components with high dimensional accuracy and complex geometries. However, the quality of AM components remains strongly process-dependent. Porosity, lack-of-fusion regions, unmelted particles and microstructural heterogeneities may form during fabrication and reduce strength, corrosion resistance, fatigue performance and reliability [1]. Careful control of process parameters and post-processing is therefore essential, particularly for components exposed to aggressive environments or severe loading.
Cavitation is the formation and collapse of vapor- or gas-filled cavities in a liquid when the local pressure falls below the vapor pressure. The collapse generates localized pressure pulses and micro-jets that cause surface damage, material removal and progressive loss of functional performance [8]. In AM alloys, including stainless steels, aluminum, titanium and nickel-based alloys, cavitation resistance depends on the manufacturing process, microstructure and surface condition. Refined microstructures generally improve it, whereas pores and lack-of-fusion defects accelerate damage initiation and propagation, and post-processing (heat treatment, surface finishing, mechanical modification, coatings) alters erosion behavior through roughness, hardness and residual stress [8].
Recent studies on AM metals have focused on manufacturing technology, build orientation, microstructure and post-processing. For Maraging Steel MS1 (1.2709), LPBF material showed lower resistance to erosion initiation than forged material, although both reached comparable steady-state erosion rates [9]. Build orientation also influences erosion behavior, while heat treatment generally improves resistance by modifying microstructure and hardness [10]. Post-processing has proven effective in related steels: shot peening of DMLS 17-4PH increased hardness and improved long-term cavitation resistance, although the initial stages were not always favorably affected [11]. Aging of Laser-Directed Energy Deposition (L-DED) maraging steel improved resistance through precipitation strengthening and reverted austenite [12], and solution treatment followed by aging gave the lowest cumulative mass loss in LMD 17-4PH [13]. In 316L, higher hardness made the LMD material more resistant than conventionally manufactured material, while pores, microstructural heterogeneities and, in LPBF material, grain morphology and grain boundaries governed damage initiation and evolution [14,15]. Laser-deposited Hastelloy C276 coatings likewise markedly improved the resistance of martensitic stainless steel [16]. Finally, sandblasting and vibratory polishing reduced roughness, increased hardness and improved the tribological performance of LPBF maraging steels [17], which suggests that surface condition may also affect their cavitation erosion resistance.
Despite this progress, the effect of shot peening on the cavitation erosion of LPBF-produced MS1 has, to the best of our knowledge, not been investigated, and the combined effect of aging and shot peening is unclear. MS1 (1.2709) is used for tooling and high-performance mechanical parts [5], where components may be exposed to cavitation [8]. Aging provides very high strength with good toughness [5], but LPBF also leaves a characteristic cellular/columnar microstructure, build-direction anisotropy, residual stresses, porosity and surface irregularities [5], which can interact with the localized stress intensification and micro-jet impacts typical of cavitation. The two treatments act differently: aging increases bulk hardness through precipitation strengthening [12], whereas shot peening hardens the surface layer [11] and can introduce compressive residual stresses. Whether their effects add up under cavitation loading is therefore an open question, particularly since peening may not favor the initial stages of erosion [11]. Our previous study [5] addressed the as-built state. The present work extends it to age-hardened, shot-peened and aged + shot-peened conditions.
Motivated by the need to improve the performance of AM components in cavitation-prone environments, this study investigates the effects of aging, shot peening and their combination on the cavitation erosion resistance of LPBF-produced MS1. Four conditions were compared (as-built, age-hardened, shot-peened and aged + shot-peened) using ASTM G32 ultrasonic vibratory testing, with mass loss, mean depth of erosion and surface morphology as evaluation metrics.

2. Materials and Methods

2.1. Characteristics of the Investigated Maraging Steel (EOS MS1, 18Ni300)

The feedstock was EOS MS1 powder [18], a gas-atomized powder produced by EOS GmbH, Krailling, Germany [19], widely used in LPBF. Its composition corresponds to the 18Ni300 (1.2709) maraging grade, a low-carbon martensitic matrix strengthened by Ni–Co–Mo–Ti intermetallic precipitates during aging. The typical chemical composition specified by the manufacturer is given in Table 1 [18].
Table 1. Chemical composition of EOS MS1 powder according to the manufacturer [18], in %.
The powder is optimized for LPBF systems such as the EOS M290. According to the manufacturer, its particle size ranges from 15 to 65 µm, ensuring good flowability and uniform powder bed formation [18]. The particles are predominantly spherical owing to gas atomization, with a small fraction of satellites and irregular particles typical of industrial AM powders [18]. Figure 1 shows a representative Scanning Electron Microscopy (SEM) image of the powder taken from the manufacturer’s datasheet [18]. It was not obtained in this study.
Figure 1. Representative SEM image of EOS MS1 powder, reproduced from the manufacturer’s datasheet [18].
Gas-atomized MS1 particles may show internal dendritic solidification patterns and chemical microsegregation, which are typical of rapidly solidified maraging steel powders. The manufacturer also reports good apparent and tap density and sufficient flowability, which support stable powder recoating and high relative density of the built parts. These characteristics depend on particle size distribution and morphology [18]. The physical and mechanical properties of EOS MS1 given in Table 2, Table 3, Table 4 and Table 5 are typical values taken from the manufacturer’s datasheet [18].
Table 2. Typical physical properties of EOS MS1 (18Ni300) AM parts [18].
Table 3. Typical mechanical properties of EOS MS1 (18Ni300) AM parts [18].
Table 4. Typical mechanical properties of EOS MS1 in age-hardened condition (490 °C/6 h) according to [18].
Table 5. Typical anisotropic mechanical properties of EOS MS1 (18Ni300) in XY and Z build directions [18].
Although MS1 powder is stable under normal storage and processing conditions, repeated reuse in LPBF systems may gradually change the particle size distribution and increase satellite formation and oxidation, which is why powder is routinely sieved and monitored between reuse cycles [20].

2.2. AM Process (LPBF Technology), Specimen Design, Processing and Post-Processing

The test specimens were manufactured from EOS MS1 powder by laser powder bed fusion (LPBF) on an EOS M290 system (EOS GmbH, Krailling, Germany) [21], in which successive powder layers are selectively melted by a focused laser beam according to the CAD model. The processing parameters followed the manufacturer’s recommendations for MS1. The build chamber (Figure 2) consists of a central build platform, flanked by the powder dispenser platform on the left and the collector platform on the right. For each layer, the recoater spreads powder from the dispenser across the build platform towards the collector, while argon flows from the gas outlet (A) across the powder bed to the extraction nozzle (B), perpendicular to the recoating direction, removing fumes and spatter from the build area.
Figure 2. Schematic top view of the build chamber filled with argon.
Figure 3 shows a schematic side view of the process. In an argon-filled chamber, which protects the molten material from oxidation, a laser beam passes through a focusing lens and is deflected by a mirror onto the powder surface, selectively melting the powder. After each exposure, the build platform is lowered by one layer thickness, and the recoater spreads a fresh powder layer, so that the part grows in the building direction. The sequence is repeated until the part is complete.
Figure 3. Schematic side view of the laser powder bed fusion (LPBF) process.
Test samples are cylindrical buttons with dimensions of Ø10 × 5 mm (Figure 4) and were built directly on the base plate in a vertical orientation.
Figure 4. Test sample.
The specimens were built with a layer thickness of 40 μm using the predefined EOS “PERFORMANCE” parameter set (laser power, scanning speed, laser offset, layer thickness), which was kept constant throughout the build. The build platform (250 × 250 mm, maximum build height 325 mm) was preheated to 40 °C. A 200 W ytterbium fiber laser (wavelength 1064 nm, beam diameter approx. 0.203 mm) was used, with the scanning direction rotated by 67° between successive layers to reduce anisotropy and promote a uniform thermal history. After the build, an additional contour scan was applied to the external surfaces to improve dimensional accuracy and surface finish. The processing parameters were not independently adjusted in this study. Since the specimens were supplied in the as-built condition and the original machine job file was not available to the authors, the individual numerical values of the laser power, scanning speed, hatch spacing, laser offset and contour-scanning parameters could not be retrieved.
The samples intended for thermal post-processing were age-hardened in a furnace according to the manufacturer’s recommended cycle for MS1 (490 °C, 6 h, air cooling) [18], at which hardening occurs through the formation of intermetallic phases and precipitates. The temperature was raised from room temperature to 490 °C within 1 h and held for 5 h, so the total treatment time of 6 h includes the heating period. The specimens were then cooled in ambient air, as recommended [18]. Besides hardening, this treatment may also relieve tensile residual stresses induced by the additive manufacturing process, which may benefit resistance to cavitation erosion.
Shot peening was employed as a mechanical post-processing treatment to strengthen the surface layer of the specimens. The treatment was performed using stainless steel shots with a diameter of 0.4 mm and a hardness of 50 HRC. A manually operated pneumatic nozzle was moved across the specimen surface to achieve uniform coverage. The compressed air pressure was set to 5 bar, with the nozzle positioned at a distance of 100 mm from the specimen and the impact angle approximately 90°. The treatment duration was 10 min, with a nominal surface coverage of 100%, assessed by visual inspection of the entire surface of each specimen after treatment. The inspection indicated a uniform distribution of shot impact marks, with no visibly untreated areas. This assessment was qualitative and was not based on image analysis. The Almen intensity was not measured because the necessary equipment was not available. The shot flow rate and impact velocity were also not independently measured during the treatment. The treatment was intended to induce plastic deformation and introduce compressive residual stresses in the near-surface region. However, residual stresses were not measured, as the required equipment was not available in our laboratory. Therefore, their contribution to the observed changes in cavitation erosion resistance could not be directly assessed. The absence of Almen intensity, shot flow rate and impact velocity measurements limits the precise characterization and reproduction of the shot-peening process in other experimental setups.
To assess both the individual and combined effects of post-processing, cavitation tests were conducted on shot-peened specimens as well as on specimens subjected to aged + shot-peened.

2.3. Cavitation Erosion Testing

Cavitation erosion testing was performed using a Branson Ultrasonics JP40022 ultrasonic vibratory apparatus based on ASTM G32 [22]. The test method employs a commercially available ultrasonic transducer operating at a frequency of 20 ± 0.5 kHz, fitted with a properly designed horn. Axial vibrations are generated by the transducer and transmitted through the horn to the specimen immersed in the test liquid, producing cavitation at the specimen surface. The vibration frequency and amplitude must be carefully controlled and monitored throughout the test. In the present study, the displacement amplitude of the horn tip was set to 50 μm, while the gap between the specimen and the horn tip was maintained at 0.5 mm. The horn-tip diameter was 16 mm, which is larger than the specimen diameter (10 mm). This arrangement differs from the standard direct vibratory configuration specified in ASTM G32, in which the specimen and horn tip have the same diameter. Therefore, the present test setup should be regarded as a modified ASTM G32 configuration. The difference in diameters may affect the distribution of cavitation intensity, particularly near the specimen edges. However, visual inspection and microscopic examination of the eroded surfaces did not reveal any noticeably more severe damage near the specimen edges compared with the central regions. The test was conducted in distilled water maintained at a temperature of 25 ± 0.5 °C. Three specimens were tested for each material condition, and the results obtained from these specimens were used for the subsequent analysis. A schematic representation of the ultrasonic cavitation testing apparatus used in this study is presented in Figure 5.
Figure 5. Cavitation test apparatus (according to ASTM G32).
Cavitation erosion performance was determined from the mass loss of the specimens, with their mass recorded prior to testing and at selected exposure intervals. The resulting mass-loss data were plotted against the testing time to characterize the progression of cavitation erosion and to enable comparison of the erosion resistance of the investigated material conditions.
Claude (Anthropic), accessed through the free web-based service, was used to assist in generating visual elements of the graphical abstract, based on the authors’ original concept and design. The tool was used exclusively for graphical illustration and not for generating or modifying experimental data or scientific results. The final graphical abstract was reviewed and approved by the authors.

3. Results and Discussion

Visual inspection after testing showed that erosion was present over the entire exposed surface of the specimens. Figure 6 shows one of the specimens, and the same was observed on all other specimens. This is consistent with the specimen diameter being smaller than the horn tip diameter (see Section 2.3), so that the whole specimen surface was exposed to the cavitating field. In addition, SEM analysis of the specimen surfaces was performed at three time points: before the start of the measurements, after 4 h, and after 24 h. No traces of embedded shot particles were observed on the SEM images of the shot-peened surfaces. However, as no EDS analysis was performed, the presence of embedded particles cannot be completely excluded.
Figure 6. Erosion damage distribution across the specimen surface.
To compare the effects of shot peening and age hardening on surface hardness, and to evaluate the changes relative to the initial (as-built) condition, hardness measurements were performed on all four specimen conditions using a ZwickRoell hardness tester. Five measurements were taken at different locations on each specimen. The values reported in Table 6 represent the mean hardness values obtained from these measurements. The maximum deviation of individual readings from the corresponding mean value did not exceed 5%.
Table 6. Measured hardness values of MS1 specimens in different post-processing conditions.
Compared with the manufacturer’s typical hardness range, the as-built specimens exhibited considerably higher hardness. The measurements show that age hardening substantially increases hardness, with the values exceeding 50 HRC, in agreement with the manufacturer’s data. Shot peening alone did not increase hardness. The measured value was even slightly lower than that of the as-built specimens, although the difference was within the measurement uncertainty. However, shot peening of the age-hardened specimens resulted in a further increase in hardness compared with the age-hardened condition.
Before cavitation erosion testing, the surface roughness of the specimens was measured using a MarSurf SD26 instrument. Two measurements were taken on each specimen along two mutually perpendicular directions. Prior to the post-processing treatments, the specimen surfaces were polished using fine-grit sandpaper and polishing pastes to achieve an N5 surface finish. The specimens were then subjected to the respective post-processing treatments, after which their final surface roughness was measured. The instrument was equipped with a diamond-tipped stylus, which was brought into light contact with the specimen surface. The measurement parameters were set as follows: a cut-off length of 0.8 mm, a traversing length of 5.6 mm, and an evaluation length of 4 mm. The values reported in Table 7 represent the mean values of the arithmetic mean deviation of the roughness profile (Ra), calculated from the two measurements, with a measurement error below 3%.
Table 7. Surface roughness values (Ra) of MS1 specimens in different post-processing conditions.
Figure 7 shows the surfaces of the age-hardened specimens before exposure to ultrasonic cavitation. Before cavitation testing, the surface shows numerous polishing marks, identified by the letter “s”, distributed irregularly and exhibiting grooves of different dimensions. These marks resulted from specimen polishing, which was performed using the figure-eight motion technique due to the specimen dimensions. In addition to the predominant polishing marks, the image also reveals traces of contaminants, identified by the letter “c”, which are not part of the material itself but originated from the external environment and were deposited on the surface.
Figure 7. SEM micrographs of age-hardened specimen surfaces before ultrasonic cavitation testing.
The surface of the age-hardened specimens after 4 h of cavitation exposure is shown in Figure 8. The presence of isolated micropits, identified by “p”, is evident, while other micropits are arranged along a circular pattern, referred to as a ring-like pattern and identified by “r”, which is characteristic of ultrasonic cavitation [9]. The marked micropits are not the only ones present. A large number of micropits can be observed, and those indicated serve merely as examples. At a larger radius, where a micropit is marked, the gradual formation of another circular pattern of grouped damage can be observed. The area between the two circular patterns contains isolated micropits and represents a less severely damaged region of the surface. In the magnified detail, the coalescence of micropits into a larger pit, identified by “g”, can be observed. The formation of these pits may be associated with pre-existing material imperfections, such as lack-of-fusion defects or non-metallic inclusions. However, these possible origins could not be confirmed by the SEM observations alone. The lighter regions within the pits may indicate the boundaries of areas where material detachment occurs [23].
Figure 8. SEM micrographs of the age-hardened specimen surface after 4 h of ultrasonic cavitation exposure.
After 24 h of cavitation exposure, the concentric circular patterns (ring-like shapes) observed after 4 h of cavitation have developed into a wider circular band, formed by micropits between the two distinct circular patterns along the perimeter marked with “r” (Figure 9).
Figure 9. SEM micrographs of the age-hardened specimen surface after 24 h of ultrasonic cavitation exposure.
Both within and outside this band, contaminants marked with “c” can be observed, along with isolated pits, which are more widely spaced towards the centre of the specimen than those within the circular band. With increasing radius, the number of small micropits increases. These are distributed irregularly but are located closer together. In the magnified view on the right, a larger group of coalesced pits is marked with “g”. Regions with lighter-coloured edges are also present and may represent the boundaries of material detachment, marked with “b”. The letter “l” indicates a deeper, irregularly shaped damaged area that appears to extend into the underlying material layers and may represent a material defect deepened by cavitation erosion. To the left of the coalesced pits, a larger isolated pit, marked with “p”, can be observed.
The initial condition of the shot-peened specimens is shown in Figure 10. Residual stresses were not measured owing to limited experimental capabilities, and their contribution is therefore discussed on the basis of the literature. Surface marks, identified by “s”, are visible on the specimen surfaces. In the image on the right, the marks appear to be arranged in a somewhat more regular pattern, with those within one band running parallel to one another at a certain angle relative to the boundary marked with “b”. These marks are less pronounced than those observed on the age-hardened specimens. Shot peening plastically deforms and may strengthen the surface. However, it can also cause pronounced plastic deformation and deep indentations in the specimen surface layers, resulting from particle impact. These indentations are marked with “d” [24]. Such cavities can significantly affect surface roughness. The distinct line marked with “b” may correspond to a boundary associated with incomplete fusion during the LPBF process, possibly affected by plastic deformation during shot peening.
Figure 10. SEM micrographs of the shot-peened specimen surfaces before cavitation testing.
The shot-peened specimens after 4 h of cavitation exposure are shown in Figure 11. In the image on the left, the pits (“p”) are distributed irregularly, with no clustering into ring-like patterns (concentric circles), as observed in the age-hardened specimens. One possible explanation for this difference is the distinct surface morphology of the shot-peened specimens, whose surfaces are more heterogeneous than those of the untreated specimens as a result of the treatment itself [25]. In the age-hardened specimens, the pits spread and cluster into circular patterns, characteristic of ultrasonic cavitation, whereas the somewhat rougher surface of the shot-peened specimens, with its surface height variations, restricts this phenomenon. The surface irregularities are clearly visible in the image on the right, where two areas exhibiting heterogeneous morphology are highlighted and identified by the letter “h”. These are examples of such areas and do not represent all their occurrences on the surface. The image on the right also shows more pronounced traces of plastic deformation (surface-layer indentation), resulting in pits with more irregular shapes than those observed in the age-hardened specimens. The letter “b” indicates a material separation boundary, while the regions outlined and identified by the letter “m” reveal portions of material from deeper layers that are yet to detach.
Figure 11. SEM micrographs of the shot-peened specimen surface after 4 h of ultrasonic cavitation exposure.
After 24 h of cavitation exposure (Figure 12), the pits are distributed irregularly but cover a large portion of the treated surface. In the first image, despite the presence of a contaminant that casts a shadow and obscures the central part of the image (“c”), a large number of pits (“p”) of various sizes can be observed. The pits have no clearly defined boundaries and extend across the entire area shown.
Figure 12. SEM micrographs of the shot-peened specimen surface after 24 h of ultrasonic cavitation exposure.
The second image clearly reveals the heterogeneous, plastically deformed surface. Pits have formed along the perimeters of the plastically deformed regions. The third image shows a magnified view of a larger pit (“p”), with a distinct bright line along its perimeter that may indicate a material separation boundary. The pit depth varies with radial position. On the left, a plastically deformed region in the form of an irregular line (“l”) is visible. This feature may be associated with an incompletely fused region in the LPBF material, possibly affected by plastic deformation. A deeper line resembling a scratch (“s”) can also be observed to the right of the isolated pit. After 24 h, the pits are more pronounced, vary in size, and are considerably more numerous. However, no regular pattern of clustering is evident, which is attributable to the heterogeneous surface, as discussed above.
The aged + shot-peened specimens before cavitation testing are shown in Figure 13. As with the shot-peened specimens, plastic deformation is visible in certain areas of the surface. Examples of these deformations and the groups they form are identified by the letter “d”. Surface marks “s” are also visible. During shot peening, particles impact and indent the surface, forming depressions in some areas. These are also identified by “d”, as they represent plastic deformation of the surface layers. The depressions are shallower than those observed in specimens treated by shot peening alone. Due to the prior aging treatment, the hardness of the specimens increased, so shot peening did not produce deep depressions.
Figure 13. SEM micrographs of the aged + shot-peened specimen surfaces before ultrasonic cavitation testing.
In the aged + shot-peened specimens, pit clustering is similar to that observed in the age-hardened specimens, although the ring-like patterns (clustering along concentric circles) are less pronounced (Figure 14). The damage is grouped into circular bands, with faint circular patterns identified by “r”. Towards the centre of the specimen, the damage is more severe, with greater pit depths and a high concentration of pits, as indicated by “g”. Some larger pits are also present, but the surface is predominantly covered by smaller pits. In the image on the right, a larger pit “p” is shown separately, with bright features along the pit edges, possibly indicating material separation boundaries, identified by “b”. The letter “c” indicates faint cracks that resemble incipient material detachment.
Figure 14. SEM micrographs of the aged + shot-peened specimen surface after 4 h of ultrasonic cavitation exposure.
After 24 h of cavitation exposure, the pits identified by “g” form dense clusters, leaving only a very small portion of the surface undamaged (Figure 15). In the image on the right, a larger, irregularly shaped pit “p” is shown separately. It is shallower than the pits observed after 24 h in the other specimens. Traces of plastic deformation caused by shot peening, as well as indentations formed by particle impact during shot peening, are visible in the surrounding areas.
Figure 15. SEM micrographs of the aged + shot-peened specimen surface after 24 h of ultrasonic cavitation exposure.
A detailed analysis of the surface condition of the as-built specimens during the first 4 h of cavitation exposure is provided in the paper [5]. After 24 h, the specimen surfaces are shown in Figure 16. In this case, densely clustered pits (“g”) occur in certain areas, with clearly visible, lighter-coloured features that may indicate material separation boundaries. This group of specimens also exhibits bands associated with plastic deformation of the material surface, identified by “s”. These slip bands may result from the shock waves generated during bubble collapse and may indicate the onset of further cavitation erosion [23].
Figure 16. SEM micrographs of the as-built specimen surfaces after 24 h of ultrasonic cavitation exposure.
The evaluation of cavitation erosion resistance was conducted in accordance with ASTM G32, with comparative diagrams presented for four specimen conditions: as-built, age-hardened, shot-peened, and aged + shot-peened. All specimens were subjected to cavitation exposure for 24 h. In accordance with the recommendations of the standard, the specimens were periodically removed from the test setup, dried, and weighed using a METTLER TOLEDO balance with a resolution of 0.01 mg, which is finer than the accuracy of 0.1 mg required by the standard. Measurement intervals were shorter during the first 4 h of testing to enable a more detailed analysis of the initial stage of cavitation erosion. For the as-built, shot-peened, and aged + shot-peened specimens, measurements were performed at 30-min intervals during the first 4 h, followed by 1-h intervals for the remainder of the test. For the age-hardened specimens, measurements were performed at 10-min intervals during the first 4 h, followed by 1-h intervals. The denser schedule for the age-hardened specimens was adopted to follow the initial stage of erosion of this condition in more detail. The use of shorter time intervals was motivated by the manufacturer’s recommendation for using age-hardened MS1 steel components, which prompted the authors to investigate the erosion development mechanism in these specimens in greater detail. Since mass loss is a cumulative quantity, the different schedules do not affect the values at a given exposure time. They only increase the resolution of the curve in the early stage. To avoid any influence of the schedule on the comparison, the conditions are compared at their common measurement times, while the additional points of the age-hardened specimens are shown for completeness. The parameters analyzed as functions of exposure time included cumulative mass loss, mean depth of erosion, and erosion rate. The curves represent the mean values of the three specimens tested for each condition, and deviations of the individual specimen values from the corresponding mean values did not exceed 3%. Given the small number of specimens (n = 3), error bars and formal significance testing would add limited information. The comparison between conditions is therefore based on the differences in mean values, and small differences, such as those between the shot-peened and aged + shot-peened specimens, are not interpreted as conclusive.
The cumulative mass loss data obtained during the cavitation erosion tests were plotted as a function of exposure time, as shown in Figure 17.
Figure 17. Cumulative mass loss as a function of cavitation exposure time for as-built, age-hardened, shot-peened, and aged + shot-peened specimens.
The comparison of the four specimen conditions is based on the common measurement times (30 min up to 4 h, then hourly). For the purpose of comparing the overall erosion response of the four specimen conditions, the experimental data were fitted by linear regression using the least-squares method. The resulting relationships were expressed in the form m(t) = a + bt, where a represents the intercept and b the slope of the fitted line. The corresponding regression parameters and coefficients of determination are summarized in Table 8. It should be noted that this linear approximation represents the average mass-loss trend over the entire 24 h exposure period and is not intended to describe possible variations in the erosion rate during individual stages of the test.
Table 8. Linear regression parameters for cumulative mass loss versus cavitation exposure time.
The cumulative mass loss can be reasonably approximated by a straight line over the investigated exposure period, although some deviations of the experimental data from the fitted lines are observed. The as-built specimens, without any subsequent surface treatment, exhibit the highest slope, indicating the greatest average mass loss and, consequently, the lowest resistance to cavitation erosion. This result is consistent with the expected lower surface resistance of the as-built condition. The approximating line for this specimen condition intersects the y-axis in the negative region, which results from the relatively steep slope of the fitted line. The results obtained during the first 4 h for the as-built specimens were previously published in the study [5], whereas the measurements in the present study were extended to 24 h.
The remaining three specimen conditions exhibit relatively similar mass-loss values and, consequently, similar linear-fit parameters. Their slopes are considerably lower, indicating lower average mass-loss rates and, therefore, higher resistance to cavitation erosion. Among these conditions, the age-hardened specimens exhibit a slightly higher slope than the shot-peened and aged + shot-peened specimens. However, as shown in the magnified detail of Figure 17, the experimental data for these specimen conditions overlap at certain exposure intervals. It should also be noted that the measurement intervals during the first 4 h differed between the specimen conditions. Owing to the considerably shorter measurement intervals used for the age-hardened specimens, mass loss could be detected at the first weighing (after 10 min for the age-hardened specimens, compared with 30 min for the other conditions). The linear approximation is used here as a descriptive tool for comparing the overall mass-loss behaviour of the different specimen conditions over the same exposure period, and the slope b should be interpreted as an average mass-loss rate over 24 h. The two-stage behaviour observed for the shot-peened specimens, characterised by a higher initial rate followed by a lower rate (see the detail in Figure 17), is not captured by a single slope. This is also reflected in the positive intercepts and somewhat lower coefficients of determination obtained for these conditions (Table 8).
Although a piecewise linear approximation could be considered for describing the different stages of mass-loss progression, its application would require the selection of a transition time between these stages. In the present study, no distinct transition point could be unambiguously identified from the experimental data, as the change from the initially higher to the subsequently lower mass-loss rate in the shot-peened specimens appears gradual. The introduction of a transition point would therefore involve an additional assumption regarding the division of the erosion process into separate stages. For this reason, a single linear approximation was retained as a consistent basis for comparing the overall mass-loss behaviour of all four specimen conditions over the same exposure period, while the observed stage-dependent differences are discussed separately.
Based on the analyses reported in the study [9], in which as-built MS1 specimens were compared with specimens made of conventional steels, together with the interpretations provided in ASTM G32, it can be concluded that the incubation period is essentially absent under the present testing conditions. Nevertheless, the initial stage of cavitation erosion is characterized predominantly by plastic deformation of the surface, while the associated mass loss remains very small. The early detection of mass loss may be related to material imperfections inherent to additively manufactured materials, such as non-metallic inclusions or insufficiently bonded regions [5]. This effect may be further enhanced by the higher resolution of the balance used in the present study. The incubation period is defined as the stage during which plastic surface deformation occurs without measurable mass loss. In the present tests, mass loss was already detected at the first weighing for all conditions (after 10 min for the age-hardened specimens and 30 min for the others), so no incubation period could be determined experimentally. As a purely comparative indicator, we therefore also report the nominal time required for the fitted line to reach a mass loss of 0.1 mg, as specified in the standard (this threshold is ten times the resolution of the balance used, 0.01 mg). This value is calculated from the fits and must not be read as a directly measured incubation period. It depends on the fit used, and its accuracy is limited when the early mass-loss behaviour deviates from linearity. The nominal times were 0.311, 0.847, 0.525 and 1.155 h for the as-built, age-hardened, shot-peened and aged + shot-peened specimens, respectively. An apparent inconsistency can be observed: the age-hardened specimens reach the nominal 0.1 mg mass loss later than the shot-peened specimens, despite exhibiting a higher slope. This behavior is also evident in the magnified detail of Figure 17, where the shot-peened specimens show a relatively pronounced initial mass loss, followed by a reduction in the slope of the mass-loss curve. One possible explanation for this behavior is related to the surface topography. Shot peening induces plastic deformation and surface strengthening, but it can also increase surface roughness and produce more pronounced asperity peaks. These surface features may be preferentially removed during the early stage of cavitation exposure, resulting in a relatively higher initial mass loss [26,27]. The shot-peened and aged + shot-peened specimens exhibit nearly identical slopes, indicating that mechanical treatment is more effective than thermal treatment in reducing cavitation erosion. However, it should be noted that if a component operates under cavitation conditions while simultaneously being required to meet stringent surface-finish requirements, shot peening may not be the most appropriate choice because of its effect on surface topography. In such cases, thermal post-treatment alone may be sufficient to satisfy both requirements. Furthermore, during the erosion development phase, overlapping data points can be observed at certain measurement intervals for the shot-peened and aged + shot-peened specimens. At later stages, the mass-loss progression for the specimens subjected to both post-treatments exhibits a slightly lower slope.
From an engineering standpoint, one of the most relevant parameters for evaluating cavitation erosion is the Mean Depth of Erosion (MDE), as it directly reflects changes in the geometry of the component, which can significantly affect its functionality. The MDE is calculated from the mass loss divided by the product of the cavitated surface area and the material density, according to the following expression [28]:
MDE ∑ i = ∑ i = 0 n ∆ MDE i = ∑ i = 0 n 4 ∆ m i ρ π d 2 10 3 µ m
The entire exposed surface area of the specimen was considered in the MDE calculation, since erosion was observed over its whole surface (Figure 6). However, the local distribution of cavitation intensity was not experimentally determined, and possible variations in erosion intensity, particularly near the specimen edges, cannot be excluded. Therefore, the calculated MDE represents an estimated mean depth of erosion over the entire exposed specimen surface, rather than the local maximum depth. A more precise calculation would require mapping the actual cavitated region. The resulting MDE–time relationship has a similar form to that obtained for cumulative mass loss, with the difference that the coefficients a and b are divided by a constant determined by the material density and the specimen surface area. The MDE as a function of cavitation exposure time is presented in Figure 18.
Figure 18. Mean depth of erosion as a function of cavitation exposure time for the investigated specimen conditions.
The highest mean depth of erosion (MDE) was observed for the as-built specimens, reaching slightly above 14 µm, followed by the age-hardened specimens with approximately 3 µm, while the shot-peened and aged + shot-peened specimens exhibited values below 2 µm.
Another important parameter is the Mean Depth of Erosion Rate (MDER), which represents the first derivative of MDE with respect to exposure time. Due to the discrete nature of the experimental data and the measurement intervals, with no continuous function initially available to describe this dependence, the MDER was determined using the following expression [28]:
MDER i = ∆ MDE i / ∆ t i   µ m h
In the case of MDER, the previous measurement intervals have no effect, as only the instantaneous erosion rate is considered. The erosion rate values calculated using the aforementioned expression are presented in Figure 19.
Figure 19. Mean depth of erosion rate (MDER) as a function of cavitation exposure time for the investigated specimen conditions.
The diagram does not reveal a clear pattern in the variation in the erosion rate. In particular, the data points for the as-built specimens are irregularly distributed, as are those for the age-hardened specimens. In contrast, the shot-peened and aged + shot-peened specimens exhibit an approximately constant erosion rate during the later measurement intervals.
The cumulative (average) erosion rate (CER), which also accounts for the preceding measurement intervals, is presented in Figure 20. The cumulative (average) erosion rate shows a distinct increase during the first 4 h, followed by a decrease and stabilization at an approximately constant value over the remainder of the exposure period. The highest average erosion rate was observed for the as-built specimens, whereas the other specimen conditions exhibited considerably lower values. For the age-hardened specimens, the average erosion rate during the developed stage of erosion did not exceed 0.15 µm/h, whereas for the shot-peened and aged + shot-peened specimens, it remained below 0.1 µm/h.
Figure 20. Cumulative (average) erosion rate (CER) as a function of cavitation exposure time for the investigated specimen conditions.
When the obtained results are compared with the curve shapes provided in the standard (Figure 21) [8], a good qualitative agreement can be observed for the cumulative mass loss and MDE curves. However, the MDER curve does not show the same qualitative correspondence.
Figure 21. Schematic representation of the erosion rate as a function of time and the corresponding cumulative erosion curve.
In the cumulative mass loss curve provided in the standard, an exponential dependence can be observed. Moreover, a linear approximation using the least-squares method does not satisfy the boundary condition at the origin, i.e., the absence of mass loss at t = 0. Instead, the regression line intersects the y-axis either in the positive region, which is particularly pronounced for materials with low cavitation erosion resistance, or in the negative region, as observed for materials with higher cavitation erosion resistance. In study [29], an exponential function was developed to approximate the mean depth of erosion (MDE), providing a better representation of the experimental data while satisfying the boundary condition at t = 0:
MDE   ( t ) = At ( 1 − e − Bt )
The resulting MDE–exposure time relationship obtained using this approximation is presented in Figure 22. The approximation coefficients and the corresponding coefficients of determination R2 are presented in Table 9. The exponential dependence appears nearly linear over the investigated time interval due to the specific values of the coefficients A and B. The approximation errors obtained for the as-built and age-hardened specimens are identical to those obtained using the least-squares method, whereas those for the shot-peened and aged + shot-peened specimens are slightly higher. Nevertheless, the quality of the approximation remains highly satisfactory. In this case, the diagram clearly shows that all curves originate at the coordinate origin, representing a significant advantage over the linear least-squares approximation. This feature enables a more accurate representation of the initial measurement intervals.
Figure 22. Exponential approximation of the mean depth of erosion (MDE) versus cavitation exposure time for the investigated specimen conditions.
Table 9. Parameters of the exponential approximation of mean depth of erosion (MDE) versus cavitation exposure time.
The results obtained for the three specimens tested under each condition showed very small deviations, indicating good repeatability of the experiments. The linear and exponential fits were performed using the mean values of the three specimens and were intended to describe the overall trends in the experimental results. Since the differences between the shot-peened and aged + shot-peened specimens were very small compared with the measured values and specimen-to-specimen scatter, no formal statistical comparison was performed. Accordingly, these two treatments are considered to exhibit comparable cavitation erosion behaviour, and the small differences in their numerical results are not interpreted as evidence of superior performance of either treatment.
Taken together, the mass-loss and MDE results show that aging before peening gave no clear additional benefit over peening alone. Since aging adds a further heat-treatment step (6 h in a furnace followed by cooling), this suggests, as a hypothesis, that peening alone may be the more economical route. This was not verified, as the aim of this study was to assess the effect of thermal and mechanical post-processing on cavitation erosion and not to analyse process costs.

4. Conclusions

The cavitation erosion resistance of LPBF-produced MS1 maraging steel was investigated in four conditions: as-built, age-hardened, shot-peened, and aged + shot-peened. Based on the 24 h ultrasonic cavitation tests performed in accordance with ASTM G32, the following conclusions can be drawn:
  • All post-processing treatments improved cavitation erosion resistance compared with the as-built condition. After 24 h, the estimated mean depth of erosion (MDE), calculated for the full specimen area, was slightly above 14 µm for the as-built specimens, approximately 3 µm for the age-hardened specimens, and below 2 µm for both shot-peened conditions.
  • Shot-peened specimens exhibited lower MDE values than age-hardened specimens. The shot-peened and aged + shot-peened specimens exhibited comparable behaviour, and, with three specimens per condition and no formal statistical comparison, no clear additional benefit from aging before shot peening was established.
  • Mass loss was detected at the first weighing for all conditions, so no incubation period could be determined experimentally. The shot-peened specimens showed a relatively higher initial mass-loss rate followed by a lower rate, which may be related to their surface topography.
  • Age hardening increased hardness, whereas shot peening alone did not, and the shot-peened conditions were rougher than the as-built and age-hardened ones, yet showed the lowest erosion. The improved resistance of the shot-peened conditions therefore cannot be explained by the measured hardness or roughness alone and may be related to near-surface effects, such as compressive residual stresses, which were not measured.
  • The SEM observations revealed differences in the surface damage patterns. Age-hardened specimens exhibited characteristic ring-like patterns of pits, whereas the damage on shot-peened surfaces was distributed more irregularly. These differences may be associated with the distinct surface conditions resulting from the respective post-processing treatments.
  • The results suggest that shot peening alone can provide cavitation erosion resistance comparable to that of the combined treatment. However, the present study did not include an economic assessment, and the influence of the treatments on surface quality should also be considered when selecting a post-processing route. Where low surface roughness is required, age hardening alone, which did not increase Ra, may be considered.
The results are limited to vertically built specimens, a single aging regime, one shot-peening pressure (5 bar), and three specimens per condition, for which no formal statistical comparison was performed. The MDE values are estimates based on the assumption that the entire exposed specimen surface was subjected to cavitation, and they represent mean rather than local maximum depths. Residual stresses were not measured, and pit initiation at defects and inclusions was not verified by EDS, cross-sectional or profilometric analysis, so the proposed mechanisms remain hypotheses. No reference material (e.g., 316L) was included, so the results are comparative within MS1. Further research should investigate other build orientations, aging regimes and shot-peening parameters, as well as the role of residual stresses and surface condition. Longer exposure tests would also help establish whether the observed differences persist over extended periods.

Author Contributions

Conceptualization, methodology, formal analysis, investigation, resources, T.L., P.L. and M.D.; writing—original draft preparation, P.L.; writing—review and editing, T.L.; visualization, T.L. and P.L.; supervision, T.L. and M.D. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the Ministry of Science, Technological Development and Innovation of the Republic of Serbia under the Agreement on financing the scientific research work of teaching staff at accredited higher education institutions in 2026, Contract numbers 451-03-34/2026-03/200105 and 451-03-34/2026-03/200135.

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.

Acknowledgments

This work was supported by the Ministry of Science, Technological Development and Innovation of the Republic of Serbia (Contract numbers 451-03-34/2026-03/200105 and 451-03-34/2026-03/ 200135), as well as by COST Action CA23155—A pan-European network of Ocean Tribology (OTC). The authors thank 3D IMPULSE for providing the specimens used in this study. During the preparation of the graphical abstract, the authors used Claude (Anthropic) to generate visual elements based on the authors’ original concept and design. The generated output was reviewed and edited by the authors, who take full responsibility for its content and accuracy. The authors would like to thank Goran Branković (University of Belgrade, Institute for Multidisciplinary Research) for performing the SEM imaging.

Conflicts of Interest

The authors declare no conflicts of interest. The funders had no role in the design of the study; in the collection, analyses, or interpretation of data; in the writing of the manuscript; or in the decision to publish the results.

References

  1. Villabona, E.; Veiga, F.; Rivero, P.J.; Uralde, V.; Suárez, A. Corrosion Behavior of Additively Manufactured Steels: A Comprehensive Review. Steel Res. Int. 2025, 96, 51–79. [Google Scholar] [CrossRef] [Scilit]
  2. Chen, L.; He, Y.; Yang, Y.; Niu, S.; Ren, H. The Research Status and Development Trend of Additive Manufacturing Technology. Int. J. Adv. Manuf. Technol. 2017, 89, 3651–3660. [Google Scholar] [CrossRef] [Scilit]
  3. Calignano, F.; Manfredi, D.; Ambrosio, E.P.; Biamino, S.; Lombardi, M.; Atzeni, E.; Salmi, A.; Minetola, P.; Iuliano, L.; Fino, P. Overview on Additive Manufacturing Technologies. Proc. IEEE 2017, 105, 593–612. [Google Scholar] [CrossRef] [Scilit]
  4. Kogo, B.; Xu, C.; Wang, B.; Chizari, M.; Reza Kashyzadeh, K.; Ghorbani, S. An Experimental Analysis to Determine the Load-Bearing Capacity of 3D Printed Metals. Materials 2022, 15, 4333. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  5. Ljubojević, P.M.; Dojčinović, M.B.; Ćitić, A.A.; Ćirić-Kostić, S.; Bogojević, N.M.; Lazović, T.M. Cavitation Resistance of Laser-Sintered MS1 Steel. Sci. Sinter. 2025, 57, 567–577. [Google Scholar] [CrossRef] [Scilit]
  6. ISO/ASTM 52900:2021; Additive Manufacturing—General Principles—Fundamentals and Vocabulary. International Organization for Standardization/ASTM International: West Conshohocken, PA, USA, 2021.
  7. Vaz, R.F.; Silvello, A.; Albaladejo, V.; Sanchez, J.; Cano, I.G. Improving the Wear and Corrosion Resistance of Maraging Part Obtained by Cold Gas Spray Additive Manufacturing. Metals 2021, 11, 1092. [Google Scholar] [CrossRef] [Scilit]
  8. Ljubojević, P.; Lazović, T.; Dojčinović, M. Cavitation in Machine Elements: A Critical Review of Cavitation Damage, Experimental Methods, Standardization Challenges, and Applied Digital Technologies. Lubricants 2026, 14, 237. [Google Scholar] [CrossRef] [Scilit]
  9. Marchini, L.; Tonolini, P.; Montesano, L.; Tocci, M.; Pola, A.; Gelfi, M. Cavitation Erosion Resistance of 1.2709 Alloy Produced via Laser-Powder Bed Fusion. Procedia Struct. Integr. 2024, 53, 212–220. [Google Scholar] [CrossRef] [Scilit]
  10. Vishwakarma, J.; Chattopadhyay, K.; Srinivas, N.C.S. Effect of Build Orientation on Wear and Erosion Behavior of Maraging Steel Processed by Powder Bed Fusion Using Laser Beam (PBF-LB). Surf. Topogr. Metrol. Prop. 2022, 10, 045006. [Google Scholar] [CrossRef] [Scilit]
  11. Świetlicki, A.; Walczak, M.; Szala, M.; Nowak, W.J.; Chocyk, D. Effect of the Shot Peening Finishing on Cavitation Erosion and Corrosion Resistance of DMLS Manufactured 17-4PH Steel. Eng. Fail. Anal. 2025, 182, 110127. [Google Scholar] [CrossRef] [Scilit]
  12. Zhao, T.Y.; Wang, Z.Y.; Wu, H.; Xu, T.Z.; Wu, C.L.; Zhang, C.H.; Zhang, S.; Chen, H.T.; Chen, J. Effect of Aging Treatment on Cavitation Erosion Resistance and Slurry Erosion Resistance of Laser Directed Energy Deposition Martensitic Aging Steel. Mater. Today Commun. 2025, 46, 112588. [Google Scholar] [CrossRef] [Scilit]
  13. Wang, T.; Wang, Z.Y.; Wang, R.; Wang, M.S.; Wu, C.L.; Zhang, C.H.; Zhang, S.; Chen, H.T.; Chen, J. Effect of Solution Aging Treatment on Corrosion Resistance and Erosion Resistance of Laser Metal Deposition 17-4PHss. Eng. Fail. Anal. 2025, 169, 109167. [Google Scholar] [CrossRef] [Scilit]
  14. Jiang, H.; Peng, S.; Hu, Q.; Wang, G.; Chen, Q.; Li, Z.; Sun, H.; Fang, J. Corrosion and Cavitation Erosion Resistance of 316L Stainless Steels Produced by Laser Metal Deposition. Acta Met. Sin. 2023, 60, 1512–1530. [Google Scholar] [CrossRef]
  15. Ding, H.; Wang, Y.; Tang, Q.; Sun, Y.; Wu, M.; Wang, W.; Bai, J.; Xie, H.; Yang, H.; Zhang, C.; et al. Enhancing Cavitation Erosion Resistance of 316L Stainless Steel through Simultaneous Microstructure Modification during Laser Powder Bed Fusion (L-PBF). Tribol. Trans. 2025, 68, 457–470. [Google Scholar] [CrossRef] [Scilit]
  16. Zhang, Z.; Zhao, L.; Si, C.; Tian, Y.; Xu, S. Microstructure Development and Cavitation Erosion Resistance Enhancement of Additive Manufactured Hastelloy C276 Alloy Coating on Martensitic Stainless–Steel via Directed Energy Deposition. Opt. Laser Technol. 2024, 171, 110395. [Google Scholar] [CrossRef] [Scilit]
  17. Hashmi, A.W.; Sagbas, B.; Argün, E.; Tian, Y.; Sankar, M.R. Investigating the Tribological Performance of Laser Powder Bed Fusion-Manufactured Maraging Steel Through Advanced Postprocessing Techniques. J. Tribol. 2026, 148, 034201. [Google Scholar] [CrossRef] [Scilit]
  18. MDS EOS MaragingSteel MS1. Available online: https://www.eos.info/metal-solutions/metal-materials/data-sheets/mds-eos-maragingsteel-ms1 (accessed on 14 June 2026).
  19. Professional 3D Printing Solutions|EOS. Available online: https://www.eos.info/ (accessed on 14 June 2026).
  20. Opatová, K.; Zetková, I.; Kučerová, L. Relationship between the Size and Inner Structure of Particles of Virgin and Re-Used MS1 Maraging Steel Powder for Additive Manufacturing. Materials 2020, 13, 956. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  21. EOS M 290—Mid-Size 3D Printing. Available online: https://www.eos.info/metal-solutions/metal-printers/eos-m-290 (accessed on 14 June 2026).
  22. ASTM G32-16; Standard Test Method for Cavitation Erosion Using Vibratory Apparatus. ASTM International: West Conshohocken, PA, USA, 2016.
  23. Omran Osman, O.; Ahmed, S.M. Understanding Surface Morphology Changes in Stainless Steel through Stepwise Cavitation Erosion: A Comprehensive Study. Eng. Fail. Anal. 2025, 167, 109017. [Google Scholar] [CrossRef] [Scilit]
  24. Walczak, M.; Szala, M. Effect of Shot Peening on the Surface Properties, Corrosion and Wear Performance of 17-4PH Steel Produced by DMLS Additive Manufacturing. Arch. Civ. Mech. Eng. 2021, 21, 157. [Google Scholar] [CrossRef] [Scilit]
  25. Azar, V.; Hashemi, B.; Rezaee Yazdi, M. The Effect of Shot Peening on Fatigue and Corrosion Behavior of 316L Stainless Steel in Ringer’s Solution. Surf. Coat. Technol. 2010, 204, 3546–3551. [Google Scholar] [CrossRef] [Scilit]
  26. Walczak, M.; Szala, M.; Okuniewski, W. Assessment of Corrosion Resistance and Hardness of Shot Peened X5CrNi18-10 Steel. Materials 2022, 15, 9000. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  27. Pohl, M.; Stella, J. Quantitative CLSM Roughness Study on Early Cavitation-Erosion Damage. Wear 2002, 252, 501–511. [Google Scholar] [CrossRef] [Scilit]
  28. Mitelea, I.; Bordeașu, I.; Frant, F.; Uțu, I.-D.; Crăciunescu, C.M.; Ghera, C. Cavitation Erosion Characteristics of the EN AW-6082 Aluminum Alloy by TIG Surface Remelting. Materials 2023, 16, 2563. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  29. Bordeasu, I.; Popoviciu, M.O.; Salcianu, L.C.; Ghera, C.; Micu, L.M.; Badarau, R.; Iosif, A.; Pirvulescu, L.D.; Podoleanu, C.E. A New Concept for Stainless Steels Ranking upon the Resistance to Cavitation Erosion. IOP Conf. Ser. Mater. Sci. Eng. 2017, 163, 012002. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.