Skip to Content
MaterialsMaterials
  • Article
  • Open Access

20 November 2026

26 Pages

Stress-State-Dependent Ductile Fracture Modeling and Burst Pressure Prediction for Alloy 690TT Steam Generator Tubes with Axial Through-Wall Cracks

and
Sino-French Institute of Nuclear Engineering and Technology, Sun Yat-sen University, Zhuhai 519082, China
*
Author to whom correspondence should be addressed.
This article belongs to the Section Energy Materials

Highlights

  • A coupled plasticity-damage model was developed for Alloy 690TT.
  • Stress triaxiality and the Lode parameter characterize ductile fracture behavior.
  • Predicted burst pressures agree with reference data, with deviations below 2.6%.
  • The model captures progressive rupture and predicts the burst pressure of cracked steam generator tubes.
  • An allowable damage coefficient enables burst-pressure assessment before fracture initiation.

Abstract

Steam generator tubes in pressurized water reactors may develop defects during long-term service, potentially leading to rupture. This study develops a ductile-fracture-based finite element framework for predicting the burst pressure of Alloy 690TT steam generator tubes containing axial through-wall cracks. The material response is described using the Johnson–Cook plasticity model coupled with a ductile damage model that accounts for stress triaxiality and the Lode parameter. Material parameters were calibrated using tensile test data obtained under different loading conditions and stress states. As the strain-rate effect on fracture strain was limited within the investigated range, strain-rate dependence was incorporated into the plasticity model but neglected in the damage model. The calibrated model was validated against tensile test results and subsequently applied to tubes containing axial through-wall cracks of different lengths. The predicted burst pressures agreed well with fracture-mechanics-based semi-empirical predictions and published experimental data, with maximum relative deviations of 2.6% and 4.0%, respectively. The predicted burst pressure decreased with increasing crack length, consistent with the reference results. The simulations also captured the progressive rupture process, from plastic deformation and damage initiation to damage evolution and final fracture. The proposed framework provides an effective approach for predicting the burst pressure of cracked Alloy 690TT steam generator tubes and supports their structural integrity assessment.

1. Introduction

The steam generator (SG) tube bundle is an important component of the primary pressure boundary in a pressurized water reactor (PWR) and serves as a critical barrier against the release of radioactive fission products between the primary and secondary circuits. Steam generator tubes are typically manufactured from nickel-based alloys with excellent ductility and fracture resistance. Their design is based on the leak-before-break (LBB) concept, which assumes that leakage can be detected before catastrophic rupture occurs. This concept provides an opportunity to implement appropriate corrective or mitigating measures before catastrophic rupture, thereby reducing the risk of tube rupture and contributing to the safe operation of the reactor system [1]. During service, ductile fracture associated with crack propagation is an important failure mechanism in SG tubes. It is characterized by substantial plastic deformation in the vicinity of defects before and during rupture [2]. The fracture behavior of ductile metallic materials is strongly influenced by the material plastic response and stress state [3]. In particular, stress triaxiality and the Lode parameter play important roles in ductile damage initiation and fracture evolution [4]. Strain rate can significantly affect the plastic response and flow stress of a material [5], whereas its effect on fracture strain depends on the material and loading conditions. Therefore, the effects of strain rate on plastic deformation and ductile fracture behavior should be evaluated separately when developing a numerical model for SG tube rupture.
Research on SG tube rupture has primarily involved fracture mechanics-based analytical and semi-analytical models, burst tests, and finite element simulations. Using a plastic instability criterion, Zahoor [6] developed analytical models to evaluate stress intensity factors and limit loads for pipes containing cracks of various configurations. B.Cochet [7] of Framatome conducted more than 1000 burst tests on Alloy 600 and Alloy 690 SG tubes and developed a correlation for predicting burst pressure, which has been widely used to assess tubes containing various types of defects. Hui Hu et al. [8] conducted burst tests on defective and defect-free Alloy 690 tubes and combined the experimental results with finite element analyses performed using ANSYS to develop a model for predicting the burst pressure of SG tubes containing geometrically regular defects. In numerical simulations, Miyajima et al. [9] investigated fracture in SUS304 SG tubes using the Gurson–Tvergaard–Needleman (GTN) model [10]. Jeon J. Y. et al. [11] proposed a finite element approach based on the stress-modified critical strain (SMCS) model to predict the burst pressure of cracked Alloy 690TT SG tubes. Finite element-based stress analysis has also been applied to damage and fracture assessment in other metallic alloys and composite materials [12].
Fracture mechanics-based approaches commonly employ parameters and criteria such as the energy release rate, the J-integral, and fracture toughness. By accounting for tube geometry and defect characteristics, these methods can predict burst pressure under specified fracture criteria and provide useful benchmarks for developing and validating numerical models. However, such approaches are generally based on simplifying assumptions and therefore have limited capability in accurately characterizing the actual mechanical response of steam generator tubes subjected to multiaxial stress states, complex defect geometries, and non-uniform loading conditions. Burst tests provide direct experimental evidence of tube deformation and rupture. However, their high cost, experimental complexity, and limited ability to cover a wide range of defect configurations can restrict systematic investigations of rupture behavior. Finite element simulation, in contrast, provides a flexible framework for analyzing plastic deformation, damage initiation, and subsequent rupture. However, many existing numerical studies calibrate their constitutive and damage models primarily using uniaxial tensile data, which may be insufficient to characterize ductile fracture under different stress states. In particular, the combined effects of strain rate, stress triaxiality, and the Lode parameter are not consistently incorporated into existing modeling frameworks. These limitations motivate the development of a ductile fracture model that can characterize the dependence of fracture strain on stress state and evaluate its implications for predicting SG tube burst pressure.
To address these limitations, the authors previously developed a finite element framework based on ductile fracture modeling to predict the burst pressure of defective Alloy 690TT SG tubes [13]. In that study, mechanical tests were conducted to characterize the plastic deformation and fracture behavior of Alloy 690TT. The Johnson–Cook constitutive model [14] was used to describe the nonlinear plastic response under different strain-rate and temperature conditions. A ductile damage model [15] was further incorporated to characterize damage initiation and evolution as functions of stress triaxiality and the Lode parameter. Strain-rate dependence was incorporated into the Johnson–Cook plasticity model, whereas its effect on ductile damage was assessed separately using the tensile test results. The framework was validated through finite element analyses of defective SG tubes and demonstrated its ability to reproduce the progression from plastic deformation and damage initiation to final rupture.
Alloy 690TT SG tubes were selected as the material of interest. Smooth and notched tensile specimens were tested to characterize the material response under different stress states, and additional tensile tests at different strain rates were conducted to quantify the strain-rate dependence of the plastic response. The experimental data were used to calibrate the Johnson–Cook plasticity and ductile damage model parameters. The effect of strain rate on fracture strain was also evaluated and found to be limited for the tested Alloy 690TT. Accordingly, strain-rate dependence was incorporated into the plasticity model but omitted from the ductile damage model. Burst simulations were then performed for SG tubes containing axial through-wall cracks of different lengths. The predicted burst pressures were compared with analytical solutions and experimental data to assess the accuracy and applicability of the proposed model. Unlike the GTN model, which describes ductile damage evolution through void nucleation, growth, and coalescence, and the SMCS model, which defines fracture using a critical-strain criterion, the present model represents fracture strain as a continuous function of stress triaxiality and the Lode parameter. The fracture-strain surface is constructed from the multi-specimen test data using radial basis function (RBF) interpolation. Building on the authors’ previous framework, the proposed model was implemented in Abaqus/Explicit 2020 through a user-defined VUMAT to predict the burst pressure of SG tubes containing axial through-wall cracks.

2. Theoretical Model

2.1. Plastic Constitutive Model

Several constitutive models have been developed to describe the strain rate and temperature-dependent plastic response of metals and nickel-based alloys. The Johnson–Cook model is a widely used phenomenological constitutive relation. The semi-empirical Zerilli–Armstrong (ZA) model, which is based on simplified dislocation mechanics, has also been applied to describe the flow behavior of Alloy 690TT under high-strain-rate and elevated-temperature conditions [16]. In addition, Arrhenius-type constitutive relations, including strain-compensated formulations, have been used to describe flow stress as a function of deformation conditions. The Johnson–Cook model was selected for this study because it describes strain hardening, strain-rate strengthening, and thermal softening through a relatively simple analytical expression. Its parameters can be calibrated using appropriately designed mechanical tests, and the model can be readily implemented in a user-defined VUMAT in Abaqus/Explicit. These features make it suitable for the present investigation of Alloy 690TT tube rupture under varying loading rates and temperatures. Compared with the Johnson–Cook model, the Zerilli–Armstrong model employs structure-dependent formulations, while Arrhenius-type and mechanical-threshold-stress models may require additional parameters and model-specific calibration procedures. The relative suitability of these models depends on the material, experimental data, and loading conditions. Given the available experimental data and the requirements of the present numerical implementation, the Johnson–Cook model provides a practical choice for describing the plastic response of Alloy 690TT. The Johnson–Cook model is a phenomenological constitutive model that typically assumes isotropic hardening and describes strain-rate effects using an empirical relation. In the present study, it is coupled with the ductile damage model to characterize plastic deformation and subsequent fracture during monotonic loading. Accordingly, the Johnson–Cook constitutive model is expressed as follows:
σ = A + B ε p n 1 + C ln ε ˙ p ε ˙ 0 1 − T − T r T m − T r m
where σ is the equivalent flow stress; ε p is the equivalent plastic strain; ε p ˙ is the equivalent plastic strain rate; ε 0 ˙ is the reference strain rate; T is the current temperature; Tr is the reference temperature; Tm is the melting temperature; A, B, n, C, and m represent the reference yield stress, strain-hardening coefficient, strain-hardening exponent, strain-rate sensitivity coefficient, and thermal-softening exponent, respectively. The parameters A, B, and n are calibrated using quasi-static tensile data obtained at room temperature and the reference strain rate. The parameter C is determined from tests conducted at different strain rates, while m is calibrated using data obtained at different temperatures.

2.2. Ductile Fracture Model

Ductile fracture is a failure mode characterized by substantial plastic deformation. In ductile fracture processes, material failure is governed by the nucleation, growth, and coalescence of voids [17].
  • Void nucleation
In the microstructure of metallic materials, inclusions, second-phase particles, and grain boundaries serve as primary nucleation sites for voids. Void nucleation occurs primarily through particle-matrix decohesion or the fracture of inclusions and second-phase particles under plastic deformation.
  • Void growth
Under continued loading, nucleated voids grow and may become elongated, depending on the local stress state and microstructure. Void growth is strongly influenced by stress triaxiality. Higher tensile stress triaxiality generally promotes void expansion, whereas shear-dominated stress states may favor shear localization and void coalescence rather than conventional volumetric void growth. The Lode parameter also characterizes the deviatoric stress state and can influence the fracture strain and the transition between tensile- and shear-dominated fracture.
  • Void coalescence
When neighboring voids grow sufficiently close to one another, they begin to link through mechanisms such as localized plastic necking or shear localization, eventually forming a continuous macroscopic crack. Void coalescence leads to the formation of a macroscopic fracture path and ultimately results in ductile fracture.
Figure 1 illustrates the typical evolution of void growth and coalescence [18]. At relatively low void volume fractions, voids may grow with limited interaction. As deformation progresses, neighboring voids increasingly interact, promoting localized plastic deformation and eventual coalescence. Plastic strain is concentrated along a band of voids, leading to void coalescence and local instabilities. The orientation of the fracture path depends on the local stress state [19].
Figure 1. Mechanism of ductile fracture.
Johnson and Cook [14] proposed a widely used empirical ductile fracture criterion in which the equivalent plastic strain at fracture depends on stress triaxiality, strain rate, and temperature. However, the original criterion does not explicitly account for the influence of the Lode parameter on fracture strain. To improve fracture prediction under complex stress states, Bao and Wierzbicki [20,21] investigated the dependence of fracture strain on stress triaxiality, while subsequent work by Xue [22] incorporated the effects of stress state into a ductile damage formulation. These developments highlighted the importance of characterizing fracture behavior beyond stress triaxiality alone. In the adopted formulation, damage accumulation is represented by a scalar damage variable, D, which increases with the accumulation of equivalent plastic strain according to the prescribed damage evolution law. As damage accumulates, the material’s load-carrying capacity progressively decreases, leading to strain localization and eventual fracture. Fracture is assumed to occur when the damage variable reaches its critical value Dc = 1. The stress–strain curve with progressive damage degradation is shown in Figure 2.
Figure 2. Stress–strain curve with progressive damage degradation.
For isotropic damage, the stress tensor is related to the effective stress tensor through a scalar damage variable, as follows:
σ = 1 − D σ ¯
where σ is the Cauchy stress tensor and σ ¯ is the effective stress tensor.
  • Ductile damage initiation criterion
Damage initiation is governed by the equivalent plastic strain at fracture, which depends on the local stress state and loading conditions. The damage initiation criterion is expressed as follows:
w D = ∫ d ε ¯ p l ε D p l η , ξ , ε ¯ ˙ p l ≥ 1
where ωD is a state variable that increases monotonically with plastic deformation; η , ξ , ε ¯ ˙ p l and ε ¯ p l denote the stress triaxiality, Lode parameter, equivalent strain rate, and equivalent plastic strain, respectively. Damage initiates when the specified criterion is satisfied.
The stress triaxiality is defined as:
η = − σ m / σ ¯
where σm is the hydrostatic pressure defined by σ m = ( σ 11 + σ 22 + σ 33 ) / 3 , σ ¯ is the von Mises equivalent stress defined by σ ¯ = 3 J 2 , and J2 is the second invariant of the deviatoric stress tensor.
The Lode parameter is defined as:
ξ = cos 3 θ = 3 3 2 J 3 J 2 3 / 2 = 27 2 J 3 σ ¯ 3
where θ is the Lode angle within the range [0°,60°], and J3 is the third invariant of the deviatoric stress tensor.
In ductile fracture research, the material stress state plays a decisive role in void nucleation, growth, and coalescence. Stress triaxiality characterizes the hydrostatic component of the stress state relative to the von Mises equivalent stress, whereas the Lode parameter characterizes the deviatoric stress state through the third invariant of the deviatoric stress tensor. Together, these parameters provide a more comprehensive description of the stress-state dependence of ductile fracture. The corresponding values of stress triaxiality and Lode angle for common loading conditions are listed in Table 1.
Table 1. Stress triaxiality and Lode angle under common loading conditions.
Because the two parameters govern distinct physical mechanisms, their individual roles should be distinguished. Stress triaxiality, defined as the ratio of the mean stress to the von Mises equivalent stress, characterizes the relative contribution of hydrostatic stress to the local stress state. Higher tensile stress triaxiality generally promotes void growth and reduces the fracture strain of ductile metals. The Lode parameter distinguishes different deviatoric stress states and can significantly influence fracture strain, particularly under low-triaxiality conditions where shear-dominated fracture mechanisms may become important. Near a crack tip, the local stress state is strongly influenced by crack-tip constraint and loading conditions. Stress triaxiality and the Lode parameter may evolve differently during loading; therefore, accounting for both parameters can improve the characterization of ductile fracture under multiaxial stress states.
For an internally pressurized SG tube, based on the thin-walled assumption, the stresses in the three cylindrical coordinate directions are expressed as: σ r = 0 (outer surface), σ θ = p r / t , σ z = p r / 2 t . Then:
σ m = σ r + σ θ + σ z 3 = p r 2 t
σ ¯ = 1 2 σ θ − σ z 2 + σ θ 2 + σ r 2 = 3 4 p r t
The triaxiality is:
η = σ m σ ¯ ≈ 0.577
The Lode parameter is:
ξ = 2 σ z − σ θ − σ r σ θ − σ r = 2 σ z − σ θ σ θ − σ r = 0
The stress state of an internally pressurized tube on the π-plane is similar to non-equi-biaxial tension. When considering the singularity near a defect or crack, the stress state becomes even more complex. This indicates that a damage model calibrated solely from uniaxial tensile test data is insufficient for accurate tube rupture simulation.
  • Damage evolution criterion
Following damage initiation, damage evolution can be defined in terms of either the effective plastic displacement u ¯ p l or the fracture energy Gf. Both approaches incorporate the characteristic length of the element to reduce mesh dependence.
The effective plastic displacement is related to the equivalent plastic strain by:
u ¯ p l = L ⋅ ε ¯ p l
where L is the characteristic length of the element, determined from its geometry.
Three formulations are available for displacement-based damage evolution: tabular, linear, and exponential. These formulations are schematically illustrated in Figure 3. For linear evolution, the failure displacement can be determined from experimental data. Tabular evolution requires a set of damage evolution data points ( u p l i , Di), whereas exponential evolution requires calibration of the corresponding model parameters using available experimental data.
Figure 3. Different definitions of damage evolution based on plastic displacement.
For energy-based damage evolution, linear and exponential formulations are available. The linear energy-based evolution law follows the same linear degradation pattern as that illustrated in Figure 3a. The equivalent plastic displacement at failure can be calculated from the specified fracture energy Gf, as follows:
u ¯ f p l = 2 G f σ y 0
where σy0 is the yield stress at damage initiation (Figure 2).
Displacement-based and energy-based damage evolution can describe equivalent softening behavior when their parameters are consistently defined. When only the failure strain is available from material tests, linear damage evolution provides a practical approximation. When sufficient experimental data describing the post-initiation response are available, a nonlinear evolution law, such as the exponential form, can be calibrated to represent the observed degradation behavior.

2.3. Coupled Plasticity-Damage Constitutive Model

Because the built-in ductile damage formulations in Abaqus do not directly accommodate the specific Lode-parameter-dependent fracture criterion adopted in this study, a user-defined constitutive model was implemented using the VUMAT subroutine. In this study, the Johnson–Cook plasticity model was coupled with a stress-state-dependent ductile damage model to describe plastic deformation and subsequent damage evolution. The main implementation procedure of the developed VUMAT subroutine is illustrated in Figure 4.
Figure 4. Flowchart for the VUMAT implementation of coupled plasticity and ductile damage.
The VUMAT implementation consists of three main components:
(1)
Stress integration using the return-mapping algorithm.
The plastic strain increment is determined by solving the nonlinear consistency equation f = 0 using the Newton–Raphson method. The yield function is defined as follows:
f σ , ε p l , ε ˙ p l , T = σ ¯ σ − σ J C ε p l , ε ˙ p l , T
where σJC is the equivalent flow stress predicted by the Johnson–Cook model.
In practical finite element calculations, the elastic predictor and plastic corrector (return mapping) framework is typically employed.
  • Trial stress
Assuming that the entire strain increment is elastic, the trial stress is calculated as follows, and the corresponding trial yield function is evaluated:
f t r i a l = σ ¯ t r i a l σ t r i a l − σ y
σ t r i a l = σ n − 1 + D e : Δ ε n
where D e is the elastic stiffness matrix and n denotes the current time increment.
If ftrial ≤ 0, the trial stress satisfies the yield condition and is accepted as the updated stress. Otherwise, plastic correction is required, and the stress state is updated through the Newton–Raphson iteration.
  • Return mapping
The return-mapping algorithm corrects the trial stress to satisfy the yield condition. Under the assumptions of isotropic hardening and associated J2 plasticity, the plastic strain increment is aligned with the deviatoric stress tensor. The corrected stress can be expressed in terms of the scalar plastic multiplier, Δλ. Substituting the stress update into the yield function yields a nonlinear scalar equation, f(Δλ) = 0, which is solved using the Newton–Raphson method.
(2)
Fracture-strain characterization.
The fracture strain model is calibrated using experimental data obtained under different stress states. Each data point consists of the stress triaxiality, η , the Lode parameter, ξ and the corresponding fracture strain ε f . The fracture strain exhibits a nonlinear dependence on stress triaxiality and the Lode parameter, with a pronounced decrease at high stress triaxiality. Therefore, a simple linear regression model may not adequately represent the fracture locus.
In this study, a radial basis function (RBF) interpolation method with the multiquadric (MQ) basis function is employed to construct the fracture strain surface:
ϕ r = 1 + r 2
where r is the Euclidean distance between a calibration point and the evaluation point in the space spanned by stress triaxiality and the Lode parameter. The RBF interpolation function is expressed as follows:
ε f x = ∑ i = 1 N λ i ϕ || x − x i ||
The interpolation coefficients are first determined by solving the linear system constructed from the calibration data. The resulting RBF interpolant is then evaluated at a given stress state to obtain the corresponding fracture strain.
The selection of the multiquadric RBF method is motivated by two considerations. First, the fracture strain exhibits a strongly nonlinear dependence on stress triaxiality and the Lode parameter, with a pronounced decrease at high triaxiality. Given the limited number and scattered distribution of the available multiaxial calibration data, an interpolation method is adopted to represent the fracture strain surface without imposing a prescribed global functional form. The multiquadric RBF provides a smooth interpolant that provides a smooth representation of the calibration data, enabling the nonlinear dependence of fracture strain on the two stress-state parameters to be represented. Second, the resulting analytical expression can be evaluated directly at arbitrary stress states, making the method computationally convenient for integration into the VUMAT and evaluation at each material point during the explicit dynamic simulation.
(3)
Damage initiation, evolution, and stress degradation
After the stress update and plastic strain increment have been determined, the stress triaxiality and Lode parameter are evaluated from the updated stress state. These quantities are then used to evaluate the equivalent fracture strain using the RBF interpolant described in Section 2.3. The damage initiation criterion is subsequently evaluated according to Equation (3). Because experimental data describing post-initiation damage evolution are limited, a linear damage evolution law based on the effective plastic displacement is adopted. The equivalent plastic displacement at failure is calculated using Equation (10).

2.4. Burst Pressure Model

The burst pressure of a steam generator tube is commonly defined as the internal pressure at which the tube ruptures. For a tube containing a defect, the burst pressure depends on both the defect characteristics and the reference burst pressure (P0) of the defect-free tube. The reference burst pressure is primarily determined by the material flow stress and the tube diameter-to-wall-thickness ratio. Under the thin-walled tube assumption, the reference burst pressure can be estimated using Barlow’s formula [23], which is widely used in engineering applications.
P 0 = σ f t R
where σf denotes the flow stress of the tube material, as defined by the selected burst-pressure model, and R and t represent the tube radius and wall thickness, respectively.
When an axial crack is present, the cracked region can deform locally under internal pressure, resulting in bulging of the tube wall. This deformation alters the stress field near the crack tip. To account for the effect of local bulging on the stress intensity factor, Folias introduced the bulging factor M for cylindrical shells containing axial cracks [24]. The factor modifies the stress intensity factor obtained from a corresponding flat-plate solution [25]. Based on this approach, the burst pressure of a tube containing an axial crack can be estimated using the following model.
P r = σ f M ⋅ t R
For a tube containing an axial through-wall crack:
M = 1 + 1.61 λ 2
where λ is the dimensionless crack length λ = a / R t , and a denotes the half-length of the axial crack.

3. Material Parameter Calibration and Finite Element Modeling

In the application of LBB technology to steam generator SG tubes, axial through-wall cracks are of particular interest in evaluating leakage and rupture behavior. Accordingly, this study focuses on the burst behavior of SG tubes containing axial through-wall cracks. The SG tube has an outer diameter of 19.05 mm and a wall thickness of 1.09 mm. The effect of axial crack length on the burst pressure is systematically investigated. To improve computational efficiency and streamline the analysis, a Python script (Python 3.14) was developed for parametric finite element modeling and automated simulation. The simulation workflow is shown in Figure 5.
Figure 5. Simulation workflow for tube rupture with defects.

3.1. Tensile Tests of Alloy 690TT

Alloy 690TT is a nickel-based, corrosion-resistant alloy widely used in steam generator tubes in PWRs. The thermally treated condition promotes the precipitation of chromium-rich carbides along grain boundaries and helps reduce residual stresses, thereby improving the alloy’s resistance to stress corrosion cracking. The chemical composition of the as-received tube material is listed in Table 2. The measured elemental contents satisfy the specified compositional limits.
Table 2. Chemical composition of Alloy 690TT (wt.%).
The material was subjected to solution treatment at 1070 °C for 10 min, followed by water quenching, and subsequent aging at 720 °C for 10 h, followed by air cooling. To characterize the mechanical response of the material and provide experimental data for calibrating the plasticity and ductile fracture models, a total of 17 tensile tests were conducted under different loading conditions. The test matrix is summarized in Table 3.
Table 3. Tensile test matrix of Alloy 690TT.
The specimen geometries are shown in Figure 6, and photographs of selected machined specimens are provided in Figure 7. Tensile tests at low strain rates were conducted using a universal testing machine (Figure 8a). Tests at nominal strain rates of 1 s−1 and 10 s−1 were performed using a high-speed tensile testing system equipped with a video extensometer (Figure 8b). For non-contact strain measurement, a black-and-white random speckle pattern was applied to the gauge section of each specimen for digital image correlation (DIC). Images recorded during testing were processed to obtain the strain response in the gauge section.
Figure 6. Geometry of specimens.
Figure 7. Parts of test specimens.
Figure 8. Figures of testing machine.

3.2. Material Parameter Calibration

The parameters of the Johnson–Cook constitutive model (Equation (1)) were calibrated using the experimental data from round-bar tensile tests (Specimens No. 1–7). The calibration procedure is described below.
(1)
At room temperature and a strain rate of 1 × 10−4 s−1, the parameters A, B, and n were determined from the true stress-true strain curves of the round-bar specimens.
(2)
The thermal softening exponent m was determined from the true stress-plastic strain curves obtained at different temperatures and the same strain rate, as shown in Figure 9.
Figure 9. Stress–strain curves at different temperatures (strain rate: 1 × 10−4 s−1).
(3)
The strain-rate sensitivity coefficient C was determined from the true stress-plastic strain curves obtained at different strain rates and the same temperature, as shown in Figure 10.
Figure 10. Stress−plastic strain curves at different strain rates (25 °C).
The calibrated Johnson–Cook plasticity parameters are summarized in Table 4.
Table 4. Johnson–Cook plasticity model parameters.
Based on tensile test data of specimens with different geometries, the parameters of the ductile damage model were calibrated. First, finite element simulations of the quasi-static tensile tests were performed. The stress triaxiality and Lode parameter were evaluated according to Equations (4) and (5). For each specimen geometry, the stress-state parameters at the critical material point in the central region of the specimen were extracted at the onset of fracture. The corresponding fracture strain data under different stress states are summarized in Table 5.
Table 5. Ductile fracture data of 690TT under different stress states.
The fracture strain is taken as the strain corresponding to the point of maximum stress in the stress–strain curve. The failure strain was estimated from the measured cross-sectional dimensions of the fractured specimens using the following expression. For the notched round-bar specimens, the failure strain was estimated from the reduction in the minimum cross-sectional area at fracture.
ε f = 2 l n ( a 0 a f )
where a0 is the initial radius of the minimum cross-section of the notched round-bar tensile specimen, and af is the radius of the minimum cross-section at the fracture surface after tensile fracture.
For the notched flat-plate specimens, the corresponding expression was formulated using the measured width and thickness of the minimum cross-section before and after fracture.
ε f = l n ( w 0 t 0 w f t f )
where w0 and t0 are the initial width and thickness of the minimum cross-section of the notched flat-plate tensile specimen, and wf and tf are the corresponding width and thickness after fracture. The values reported in Table 5 represent the averages obtained from three replicate specimens for each test condition. Some scatter is observed in the measured fracture strains, which may be attributed to variations in specimen geometry, material heterogeneity, and experimental measurements. The available test results provide the basis for characterizing the dependence of fracture strain on stress state. However, the number of repeated tests under identical conditions is limited, and a comprehensive statistical assessment of test repeatability is therefore not available. This limitation should be considered when interpreting the calibrated fracture strain surface.
The experimental results indicate that the strain rate has a limited effect on the fracture strain of Alloy 690TT within the range of loading conditions investigated. Accordingly, strain-rate dependence is incorporated into the plasticity model but neglected in the ductile damage model.
The fracture strain surface is calibrated using eight experimental data points obtained from round-bar and flat-plate specimens, covering different stress triaxialities and Lode parameters. Two data points share the same stress-state coordinates; therefore, their fracture strains are averaged, resulting in seven unique calibration points. A multiquadric RBF with a smoothing parameter of 0.01 is employed to construct the fracture strain surface, with the shape parameter automatically determined by the interpolation routine. In addition, a non-increasing constraint is applied along the stress triaxiality direction to ensure that the predicted fracture strain does not increase with increasing stress triaxiality at a fixed Lode parameter.
The resulting fracture strain surface is shown in Figure 11. For comparison, a fracture strain relationship that depends only on stress triaxiality is also constructed using four representative calibration data pairs. Piecewise linear interpolation is applied between the data points, while linear extrapolation based on the last two data points is used beyond the highest calibration triaxiality. This relationship provides a reference for assessing the influence of the Lode parameter on the predicted fracture behavior.
Figure 11. Fracture strain surface of Alloy 690TT.
Before simulating SG tube rupture, a room-temperature tensile test of a round-bar specimen was used to validate the proposed coupled plasticity-damage model and the calibrated material parameters. A three-dimensional finite element model was employed, and the mesh configuration is shown in Figure 12.
Figure 12. Finite element mesh of the specimens and location of the central node.
The comparison between the simulation results and the experimental data is presented in Figure 13. As can be seen, the tensile response predicted by the proposed plasticity-damage coupled model agrees well with the experimental results. The axial stress contours and deformation fields in the gauge section illustrate the simulated progression from plastic deformation and necking to damage evolution and final fracture. Overall, the results demonstrate that the proposed model captures the tensile response and the principal stages of specimen failure.
Figure 13. Simulated tensile response and deformation of the round-bar specimen.
Furthermore, the fracture morphology of the failed specimens shown in Figure 14 reveals good agreement between the predicted and observed failure locations and fracture modes. The agreement in fracture location and morphology provides additional evidence of the model’s capability to reproduce the specimen’s failure behavior.
Figure 14. Stress triaxiality distribution and fracture morphology of the round-bar specimen.

3.3. Finite Element Model of SG Tube

A three-dimensional solid finite element model was developed using eight-node linear brick elements with reduced integration (C3D8R). To minimize the influence of end boundary conditions on the results, the tube length was set to ten times its outer diameter. The mesh models for both the intact tube and the tube containing an axial through-wall crack are shown in Figure 15. For tubes containing defects, axial through-wall cracks were modeled using the Seam Crack technique [26]. Local mesh refinement was applied in the vicinity of the crack tip. This approach avoids the need to prescribe an artificial crack width and facilitates the representation of the local stress field near the crack tip.
Figure 15. Meshes of the intact tube and the tube containing an axial through-wall crack.
Because SG tube rupture involves severe strain localization near the crack tip, a mesh sensitivity study was conducted before the parametric analyses. Five crack-tip element sizes Le = 0.40, 0.20, 0.12, 0.10 and 0.08 mm, were examined. The global element size was maintained at 1 mm, with four elements through the wall thickness and local refinement confined to a zone extending 2 mm around the crack tip.
Both the damage-initiation pressure Pd and the burst pressure Pb decrease monotonically with mesh refinement. For meshes with Le = 0.12 mm, the pressure difference between damage initiation and burst, ΔP = Pb−Pd, remained approximately constant at 6.5 MPa. Richardson extrapolation yielded an estimated zero-mesh-size burst pressure of approximately 14 MPa. An element size of Le = 0.1 mm was selected for the subsequent simulations. At this resolution, the predicted burst pressure differed by less than 3% from that obtained with the finest mesh, while reducing the computational cost by approximately 20%.
SG tube rupture involves severe local deformation, strain localization, and progressive material failure. Abaqus/Explicit was therefore employed to solve the highly nonlinear dynamic equilibrium equations. In Abaqus/Explicit, the equations of motion Equation (22) are integrated using the central difference method (CDM), without requiring iterative equilibrium iterations or the solution of a global stiffness matrix at each time increment. The semi-discrete equations of motion are expressed as follows:
M u ¨ = F e x t − F int
where M is the mass matrix; Fext and Fint are the external and internal forces respectively; u ¨ is the node acceleration vector.
The explicit integration scheme updates the nodal accelerations, velocities, and displacements sequentially. Its numerical stability is governed by the stable time increment, which is related to the time required for a stress wave to traverse the smallest element. For a linear elastic material, the characteristic dilatational wave speed can be expressed in terms of the material’s elastic properties and density. Abaqus automatically estimates the stable time increment, which generally decreases with decreasing element size. Consequently, the fine mesh required near the crack tip can substantially increase the computational cost. The total simulation time, mesh resolution, output frequency, and available computational resources must therefore be considered when configuring the analysis.
According to an EPRI report [27], the burst pressure of SG tubes containing axial through-wall cracks is relatively insensitive to the pressurization rate within the investigated range, up to 2000 psi/s (13.8 MPa/s). Based on this finding, a pressurization rate of 10 MPa/s was adopted, corresponding to a total loading time of 5 s for the prescribed pressure increase. In the finite element model, both ends of the tube were fully constrained, and internal pressure was uniformly applied to the inner surface of the tube.
To verify the numerical stability of the steam generator tube rupture simulation, the global energy-balance indicators during loading, namely total energy, artificial strain energy, and kinetic energy, were analyzed. The total energy balance was assessed using the total energy history. The absolute total energy value immediately before rupture was 2.22 × 10−3 J, corresponding to approximately 4.46 × 10−5% of the total external work. Immediately before rupture, the maximum ratio of artificial strain energy to internal energy was approximately 2.45%, below the commonly used 5% screening guideline. The maximum ratio of kinetic energy to internal energy was approximately 0.19% as shown in Figure 16, indicating that the global kinetic-energy contribution was small at this stage.
Figure 16. Time histories of the kinetic-energy and artificial-strain-energy ratios to total internal energy.
These energy measures indicate that artificial strain energy and global kinetic energy remain small relative to the internal energy immediately before rupture, while the total energy-balance residual is small relative to the external work.

3.4. Determination of Burst Pressure

During the tube rupture simulation, the failure process was monitored using the damage variable, D, which evolves from 0 to 1 as damage accumulates. Internal pressure was applied at a constant pressurization rate. Tube rupture was assumed to occur when the damage variable reached the critical value D = 1 in the crack-tip region and a continuous path of failed material formed across the remaining ligament. The corresponding internal pressure was defined as the burst pressure.

4. Results and Discussion

4.1. Rupture Process of SG Tubes

Taking the tube containing a 20 mm axial through-wall crack as an example, Figure 17 shows the evolution of the von Mises stress and damage variable, D at the crack-tip element.
Figure 17. Evolution of von Mises stress and damage variable at the crack-tip element.
During the initial loading stage, the von Mises stress at the crack tip increases with the applied internal pressure, while the damage variable remains zero. At t = 1.1 s, the local stress state satisfies the damage initiation criterion, marking the onset of damage evolution. The damage variable, D then begins to increase from zero, indicating the progressive accumulation of material damage.
As the internal pressure continues to increase, damage accumulates and progressively degrades the local load-bearing capacity. The resulting material degradation also affects the local stress response, as reflected by the changes in von Mises stress shown in Figure 17. At t = 1.65 s, the damage variable reaches its critical value D = 1, triggering deletion of the crack-tip element. This local failure initiates rapid crack propagation, ultimately leading to rupture of the steam generator tube.

4.2. Stress State of the SG Tubes

The evolutions of stress triaxiality and Lode angle at the crack-tip region and at a location away from the crack tip are presented in Figure 18. The two locations exhibit markedly different stress-state evolutions, highlighting the pronounced spatial localization of the stress field near the crack tip.
Figure 18. Stress triaxiality and Lode angle at the crack tip and in the far-field region.
As the internal pressure increases toward the burst condition, stress triaxiality at the crack tip increases substantially, indicating an increasing contribution of hydrostatic stress relative to the von Mises equivalent stress. This high-triaxiality stress state promotes microvoid nucleation and growth and facilitates void coalescence, thereby accelerating ductile damage accumulation. These effects contribute to the degradation of the material’s load-bearing capacity and the subsequent failure process.
Meanwhile, the Lode angle at the crack tip remains within the range of 3.3–15.5°. According to the Lode-angle convention adopted in this study, this range indicates that the local stress state remains relatively close to axisymmetric tension, without a pronounced shift toward a shear-dominated state. Nevertheless, the Lode parameter provides information on the deviatoric stress state that is not captured by stress triaxiality alone. Variations in the Lode parameter can therefore affect the fracture strain and ductile damage evolution under comparable stress triaxiality levels.
Overall, the results demonstrate that stress triaxiality and the Lode parameter provide complementary descriptions of the evolving multiaxial stress state. Considering both parameters is therefore important for characterizing the ductile fracture behavior of steam generator tubes.

4.3. Comparison of Burst Pressure

Based on the tensile test results and the procedure described in Section 2.4, the flow stress of Alloy 690TT was determined to be 573.6 MPa. The theoretical burst pressures of defect-free tubes and tubes containing axial through-wall cracks were calculated using the semi-empirical model presented in Section 2.4. In the finite element simulations, the burst pressure was determined from the internal pressure corresponding to the critical damage state D = 1, with the pressure evaluated immediately before element deletion to avoid numerical fluctuations associated with the deletion process. Table 6 summarizes the burst pressures predicted by the FEA and the semi-empirical model for different axial crack lengths. The numerical predictions were also compared with the experimental results reported by Jeon et al. [11], as shown in Figure 19.
Table 6. Comparison of predicted and reference burst pressures for SG tubes with different axial crack lengths.
Figure 19. Comparison of burst pressures for tubes with different crack lengths.
The FEA predictions agree well with both the semi-empirical predictions and the experimental results, with maximum relative deviations of 2.6% and 4.0%, respectively. Both the numerical and reference results exhibit a consistent decrease in burst pressure with increasing crack length. These comparisons demonstrate that the proposed coupled plasticity-damage model can predict the burst pressure of SG tubes containing axial through-wall cracks with good accuracy over the range of crack lengths investigated.
In addition to predicting the final burst pressure, the proposed finite element model provides information on the pressure evolution from damage initiation to final failure. As shown in Figure 20, the lower and upper boundaries of the shaded region represent the pressures at damage initiation and final tube failure, respectively. The pressure interval between these boundaries characterizes the progressive damage evolution leading to rupture. This information provides additional insight into the failure process that cannot be obtained from a burst-pressure prediction alone.
Figure 20. Damage initiation and burst pressure range of steam generator tubes.
A prescribed damage threshold may be explored as a potential indicator for evaluating the pressure interval between a specified damage state and final rupture. However, using such a threshold to determine an allowable operating pressure requires appropriate calibration and validation against experimental data, as well as consistency with applicable structural integrity criteria and safety requirements.
To further assess the influence of the Lode parameter on burst-pressure prediction, additional simulations were performed using a damage model in which the fracture strain depends only on stress triaxiality, with the Lode-parameter dependence omitted. The simulations were conducted for the same crack lengths as those considered in the original model. The predicted burst pressures without the Lode parameter were slightly higher than those obtained using the full stress-state-dependent fracture model. For the tube with a 20 mm crack, the predicted burst pressure was 16.5 MPa when the Lode parameter was considered, compared with 17.0 MPa when its effect was neglected, representing an increase of approximately 3.0%. This difference can be explained by the stress state at the crack tip, where the stress triaxiality approaches 1, and the Lode parameter falls within a region in which the fracture strain surface incorporating the Lode-parameter dependence predicts a slightly lower fracture strain than the triaxiality-only relationship (Figure 11). Consequently, damage develops at a lower accumulated plastic strain, leading to earlier local failure and a slightly lower predicted burst pressure. These results indicate that incorporating the Lode parameter can influence the predicted burst pressure, although the magnitude of its effect is relatively small for the cases investigated.

4.4. Limitations and Applicability

Despite the satisfactory agreement between the predicted and experimental burst pressures, several limitations of the proposed methodology should be noted. First, material variability was not systematically quantified, and the calibrated parameters represent the tested Alloy 690TT material. Second, although mesh sensitivity was investigated, some mesh dependence may remain due to crack-tip stress localization and damage evolution. Third, the calibrated fracture parameters are applicable primarily to the stress-state range covered by the experimental data, and their transferability to other materials or heat-treatment conditions requires further validation. Finally, the present model focuses on SG tubes with axial through-wall cracks under monotonic internal pressurization. The effects of operating temperature, residual stresses, and complex service loading histories require further investigation.

5. Conclusions

Based on the mechanical testing of Alloy 690TT and the numerical simulations of SG tube rupture, the following conclusions can be drawn:
(1)
A coupled plasticity-damage constitutive model for Alloy 690TT was developed and implemented in Abaqus/Explicit using a user-defined VUMAT subroutine. The model combines a strain-rate-sensitive Johnson–Cook plasticity formulation with a ductile damage criterion that accounts for stress triaxiality and the Lode parameter. The material parameters were calibrated using tensile test data obtained under different loading conditions and stress states.
(2)
During pressurization of SG tubes containing axial through-wall cracks, the stress state near the crack tip evolved significantly, with stress triaxiality increasing substantially while the Lode angle remained within a relatively narrow range associated with tension-dominated loading. The results demonstrate that stress triaxiality and the Lode parameter provide complementary information for characterizing the local stress state and determining the fracture strain, highlighting the importance of considering both parameters in ductile fracture modeling.
(3)
The proposed model reproduced the progressive rupture process of SG tubes containing axial through-wall cracks, from plastic deformation and damage initiation to final failure. The predicted burst pressures for different crack lengths agreed well with fracture-mechanics-based semi-empirical predictions and published experimental results, with maximum relative deviations of 2.6% and 4.0%, respectively. These results demonstrate the capability of the proposed model to predict the burst pressure of Alloy 690TT SG tubes containing axial through-wall cracks over the range of crack lengths investigated.
(4)
The proposed framework also enables the evaluation of internal pressure at a specified damage level before final rupture, providing additional information on damage progression and the pressure interval between damage initiation and final failure. This capability may support the development of damage-based criteria for assessing the structural integrity of SG tubes containing axial through-wall cracks, provided that the selected damage thresholds are appropriately calibrated and validated against experimental data and relevant structural integrity requirements.

Author Contributions

B.Z.: Conceptualization, Data curation, Investigation, Methodology, Software, Validation, Visualization, Writing—original draft. N.J.: Funding acquisition, Resources, Supervision, Writing—review and editing. All authors have read and agreed to the published version of the manuscript.

Funding

This work was supported by the General Program of the National Natural Science Foundation of China (Grant No. 12472172) and the Joint Research Program of the National Natural Science Foundation of China (Grant No. U24B2004).

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.

Conflicts of Interest

The authors declare no conflicts of interest.

Abbreviations

The following abbreviations are used in this manuscript:
DICDigital Image Correlation
GTNGurson–Tvergaard–Needleman
LBBLeak before break
MQMultiquadric
PWRPressurized water reactor
RBFRadial basis function
SMCSStress modified critical strain
SGSteam generator
TTThermally treated

References

  1. IAEA. Applicability of the Leak Before Break Concept (IAEA-TECDOC-710); International Atomic Energy Agency: Vienna, Austria, 1993. [Google Scholar]
  2. Erdogan, F. Ductile fracture theories for pressurised pipes and containers. Int. J. Press. Vessels Pip. 1976, 4, 253–283. [Google Scholar] [CrossRef] [Scilit]
  3. Mirza, M.S.; Barton, D.C.; Church, P. The effect of stress triaxiality and strain-rate on the fracture characteristics of ductile metals. J. Mater. Sci. 1996, 31, 453–461. [Google Scholar] [CrossRef] [Scilit]
  4. Bai, Y.; Wierzbicki, T. A new model of metal plasticity and fracture with pressure and Lode dependence. Int. J. Plast. 2008, 24, 1071–1096. [Google Scholar] [CrossRef] [Scilit]
  5. Yan, N.; Li, Z.; Xu, Y.; Meyers, M.A. Shear localization in metallic materials at high strain rates. Prog. Mater. Sci. 2020, 119, 100755. [Google Scholar] [CrossRef] [Scilit]
  6. Zahoor, A. Ductile Fracture Handbook; EPRI Report NP-6301-D; Electric Power Research Institute: Palo Alto, CA, USA, 1989. [Google Scholar]
  7. Cochet, B. Steam Generator Tube Integrity, Volume 1: Burst Test Results and Validation of Rupture Criteria (Framatome Data); EPRI Report NP-6865-L; Electric Power Research Institute: Palo Alto, CA, USA, 1991. [Google Scholar]
  8. Hu, H.; Li, P.-N.; Tang, Y. Study of strength and plugging criteria for Inconel 690 steam generator tubes with flaw. At. Energy Sci. Technol. 2008, 42, 634–640. [Google Scholar]
  9. Miyajima, Y.; Kikuchi, M.; Takahashi, A. Ductile fracture simulation of a pipe of steam generator in PWR. In Proceedings of the ASME 2013 Pressure Vessels and Piping Conference, Paris, France, 14–18 July 2013. PVP2013-97582. [Google Scholar]
  10. Gurson, A.L. Continuum theory of ductile rupture by void nucleation and growth: Part I—Yield criteria and flow rules for porous ductile media. J. Eng. Mater. Technol. 1977, 99, 2–15. [Google Scholar] [CrossRef] [Scilit]
  11. Jeon, J.Y.; Kim, Y.J.; Kim, J.W. Numerical prediction of maximum load-carrying capacity of cracked Alloy 690TT steam generator tubes. J. Press. Vessel Technol. 2016, 138, 041601. [Google Scholar] [CrossRef] [Scilit]
  12. Yang, J.; Heogh, W.; Ju, H.; Kang, S.; Jang, T.-S.; Jung, H.-D.; Jahazi, M.; Han, S.C.; Park, S.J.; Kim, H.S.; et al. Functionally graded structure of a nitride-strengthened Mg2Si-based hybrid composite. J. Magnes. Alloys 2024, 12, 1239–1256. [Google Scholar] [CrossRef] [Scilit]
  13. Zhang, B.; Jiang, N. Finite Element Analysis of Rupture Pressure of Alloy 690 Steam Generator Tubes with Defects. In Proceedings of the 31st International Conference on Nuclear Engineering, Prague, Czech Republic, 4–8 August 2024; Paper No. ICONE31-134269; ASME: New York, NY, USA, 2024. [Google Scholar]
  14. Johnson, G.R.; Cook, W.H. Fracture characteristics of three metals subjected to various strains, strain rates, temperatures and pressures. Eng. Fract. Mech. 1985, 21, 31–48. [Google Scholar] [CrossRef] [Scilit]
  15. Dassault Systèmes. Abaqus Documentation: Damage and Failure for Ductile Metals; Dassault Systèmes: Vélizy-Villacoublay, France, 2020. [Google Scholar]
  16. Lee, W.-S.; Sun, T.-N. Plastic flow behaviour of Inconel 690 super alloy under compressive impact loading. Mater. Trans. 2004, 45, 2339–2345. [Google Scholar] [CrossRef] [Scilit]
  17. Rice, J.R.; Tracey, D.M. On the ductile enlargement of voids in triaxial stress fields. J. Mech. Phys. Solids 1969, 17, 201–217. [Google Scholar] [CrossRef] [Scilit]
  18. Kossakowski, P.G. Influence of initial porosity on strength properties of S235JR steel at low stress triaxiality. Arch. Civ. Eng. 2012, 58, 293–308. [Google Scholar] [CrossRef] [Scilit]
  19. Anderson, T.L. Fracture Mechanics: Fundamentals and Applications, 4th ed.; CRC Press: Boca Raton, FL, USA, 2017. [Google Scholar]
  20. Bao, Y.; Wierzbicki, T. On fracture locus in the equivalent strain and stress triaxiality space. Int. J. Mech. Sci. 2004, 46, 81–98. [Google Scholar] [CrossRef] [Scilit]
  21. Wierzbicki, T.; Bao, Y.; Lee, Y.W.; Bai, Y. Calibration and evaluation of seven fracture models. Int. J. Mech. Sci. 2005, 47, 719–743. [Google Scholar] [CrossRef] [Scilit]
  22. Xue, L.; Wierzbicki, T. Ductile fracture initiation and propagation modeling using damage plasticity theory. Eng. Fract. Mech. 2008, 75, 3276–3293. [Google Scholar] [CrossRef] [Scilit]
  23. Peng, Z.; Ren, S. Influence of steam heat transfer tube damage characteristics on burst pressure. E3S Web Conf. 2021, 233, 01072. [Google Scholar] [CrossRef] [Scilit]
  24. Folias, E.C. The Stresses in a Cylindrical Shell Containing an Axial Crack; GALCIT SM 64-13; California Institute of Technology: Pasadena, CA, USA, 1964. [Google Scholar]
  25. Folias, E.S. An axial crack in a pressurized cylindrical shell. Int. J. Fract. Mech. 1965, 1, 104–113. [Google Scholar] [CrossRef] [Scilit]
  26. Zehnder, A.T. Finite Elements in Fracture Mechanics: Theory, Numerics, Applications; Springer: Berlin/Heidelberg, Germany, 2012. [Google Scholar]
  27. Merilo, M. Effect of Pressurization Rate on Degraded Steam Generator Tubing Burst Pressure; EPRI Technical Report 1001441; Electric Power Research Institute: Palo Alto, CA, USA, 2001. [Google Scholar]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.