Skip to Content
  • Proceeding Paper
  • Open Access

27 November 2026

8 Pages

Demonstration of Manual Refinishing Procedures in Modern Automotive Coatings †

and
Department of Innovative Vehicles and Materials, GAMF Faculty of Engineering and Computer Science, John von Neumann University, 10 Izsáki Street, H-6000 Kecskemét, Hungary
*
Author to whom correspondence should be addressed.
†
Presented at the Sustainable Mobility and Transportation Symposium 2026, Győr, Hungary, 8 October 2026.
Eng. Proc.2026, 157(1), 74;https://doi.org/10.3390/engproc2026157074 
(registering DOI)
This article belongs to the Proceedings of The Sustainable Mobility and Transportation Symposium 2026

Abstract

Automotive refinishing must restore damaged vehicle surfaces while meeting strict esthetic and protective requirements. This paper examines the visual, technical, and adhesion-related challenges of manual refinishing, with particular attention to color matching, effect pigments, viewing angle, and substrate preparation. Best-practice procedures are presented through two real vehicle repair case studies and complementary adhesion tests on polymer substrates. The results show that revealing the original paint structure, selecting the appropriate color formula instrumentally, careful cleaning, test-panels, and controlled blending into adjacent areas are essential for achieving visually invisible repairs. Multi-angle visual inspection under different light sources proved decisive for final acceptance, especially for metallic and pearlescent finishes. Adhesion tests indicated sufficient coating performance when primer was applied, despite variations in layer thickness and preparation route. This preliminary study confirms that systematic refinishing procedures can satisfy both appearance and durability expectations in modern automotive repair.

1. Introduction

To improve the automotive coatings, a wet-on-wet surface coating technology was developed in the 1970s consisting of a thin pigmented basecoat (BC) and a thicker, transparent clearcoat (CC) layer to ensure both appearance and resilience [1]. For special effects, in addition to the aluminum flakes, interference pigments also became widespread, in which case the appearance varies with the incident-detection angle, making the corrections more complicated [2,3]. Consequently, obtaining a visual match after applying touch-up painting is a real challenge; however, there is a lack of technical guidelines. In OEM (Original Equipment Manufacturer) production, controlled application processes yield consistent color and gloss, whereas in refinishing, painters must replicate these under variable workshop conditions [4].
Automotive manufacturers often specify strict tolerances (e.g., ΔE < 1 in CIEDE2000 units) for color deviations [5,6]. However, in practice, refinished panels can fall outside these tolerances due to formulation or application differences. Effect finishes (metallic and pearlescent) are especially challenging: their appearance “flops” with angle as aluminum or mica flakes reflect light directionally [7,8]. Mismatches can be minimized by careful spraying techniques and evaluation at multiple angles and light sources. Beyond color, gloss and DOI (Distinctness of Image, clarity of reflection) are key aspects of appearance [9]. Gloss is the mirror-like shininess, quantified by specular reflection (e.g., 60° gloss in gloss units, GUs) [10]. Reproducing the factory finish’s surface texture is thus integral to refinishing. In the case of even refinishing, the painting must be free of defects [11]. Variations in thickness, color and surface structure may compromise quality [12], and proper adhesion must be ensured. Polymers pose challenges because of their low surface energy, but flame, plasma or corona discharge activation, which is utilized for OEM plastic components [13,14], is rarely available for repairs; therefore, surface roughening and adhesion promoters remain the main tools for practical repair applications [15,16]. On top of this, adhesion tests are generally destructive [17,18]. The number of publications on practices in refinishing workshops is minor despite high demand and frequent challenges. Ye focused on the Chinese market in his study [19]. Bellissario et al. found that the drying method affects gloss and that roughness is determined by the type of CC. Scratch resistance can be enhanced by aging and using high-solid CC; however, oven-drying has a negative effect [20]. Ulbrich et al. revealed that, among paint removal techniques, soda blasting and abrasive blasting with plastic granulates cause less shading of the zinc coating [21]. Description and examination of the whole high-precision refinishing process in manual workshops, however, have not been investigated in scientific papers.
The present study demonstrates the principles, perspectives and barriers in refinishing through examples involving the painting of real car parts. The effect of heat treatment and complete touch-up painting processes are demonstrated.

2. Materials and Methods

2.1. Specimens

Two real vehicle repair cases were selected for color evaluation (C series). Sample C1 involved a front bumper and a fender arch area requiring localized refinishing across adjacent components. Sample C2 involved a hood, together with the front fender arches and the front bumper, requiring multi-part refinishing. Adhesion tests were performed on ABS side mirror housings and rear bumper parts made from PP/PE and TPO (A series).

2.2. Materials

For cleaning, Glasurit 541-30 cleaner and 3M 50401 tack cloth (3M, St. Paul, MN, USA) were used. As a 2K polyurethane (PU) primer, a mixture of Glasurit 285-270, Glasurit 929-58 and Glasurit 522-10 (or Glasurit 352-91 for soft parts Sample A5-8) at 4:1:1 ratio was applied, except for Sample C1, where a Glasurit 151-170 UV curable filler was used. BCs were mixed from the Glasurit 90 series at the required ratios. In the 2K PU CC, A component was a Glasurit P-C-30 high-gloss lacquer, mixed with a Glasurit P-H-430 hardener and a Glasurit P-R-120 thickener at a 2:1 + 10% ratio. All Glasurit grades were obtained from BASF Coatings GmbH, Münster, Germany.

2.3. Test Panel Preparation

First, the color of the BC was determined by a PPG X-rite KOH Rapid Match XI spectrophotometer (X-Rite Incorporated, Grand Rapids, MI, USA). After finding the closest color, a recipe with the recommended grayshade (a color ranging from white to black, with no dominant hue used for primers) was created instrumentally. Test panels (approximately 30 cm × 20 cm) were prepared to simulate common automotive refinish scenarios. Wet-to-wet technology using a mini SATAjet X 5500 HVLP (High-Volume, Low-Pressure) spraying gun (SATA GmbH & Co. KG, Kornwestheim, Germany) with an incoming pressure of 2 bar, external pressure of 0.7 bar and nozzle diameter of 1.2 mm was used for the primer and the BC, and a SATAjet X 5500 RP (Reduced Pressure) gun (SATA GmbH & Co. KG, Kornwestheim, Germany) with an external pressure of 1.2–1.3 bar for the CC. Distance from the substrate was kept at 20 ± 2 cm.

2.4. Microscopic Analysis of the Test Panels

SEM images were taken with a Zeiss Sigma 300 VP instrument (Carl Zeiss AG, Oberkochen, Germany). The accelerating voltage was set to 1 or 2 kV.

2.5. Coating of the Specimens

Surfaces were sanded with a MirlonTotal (Mirka Ltd., Leppo, Finland) P800 abrasive sponge, except for non-sanded specimens. Static charging and contaminations were eliminated using an Ionstar antistatic gun D15391823 (Herrmann Innovations GmbH, Pösung, Germany). Heat-treated specimens were conditioned in the paint booth at a substrate temperature of 60 °C for 30 min. A mini SATAjet X 5500 HVLP spraying gun with an incoming pressure of 2 bar and an external pressure of 0.7 bar with a 1.2 mm nozzle diameter was used for the primer and the BC, and a SATAjet X 5500 RP gun with an external pressure of 1.2–1.3 bar was used for the CC. Paint applications were carried out at an air temperature of 22 ± 2 °C and a substrate temperature of 30 ± 2 °C, at 50 ± 5% relative humidity. After application of the filler, a ventilation time of 25 min was applied. BC coverage was carried out with a “0.5 + 1” spreading process. The BC layer was ventilated for approximately 5 min at 30 °C. The CC was sprayed using a “1 + 0.5” technique; then the samples were tempered at an air temperature of 80 °C and a substrate temperature of 60 °C for 30 min.

2.6. Evaluation of the Visual Match

Evaluation of the appearance of the Sample C series was performed in the paint spray booth under a fluorescent lamp, in the open air and under the illumination of a SATA trueSun D65 light source (SATA GmbH & Co. KG, Kornwestheim, Germany) according to ISO 13076 [22]. Distance and the observation period were kept at 60–80 cm and 10–15 s, respectively. Experienced professionals and laypersons, after a short training period, took part in the experiment, including two male professionals with more than 5 years of experience in refinishing, and two male and two female laypersons. All participants received the same short training period prior to evaluation, using reference images and definitions of orange peel, haze, and gloss.

2.7. Layer Thickness Measurements

Layer thicknesses were determined on dry test plates that were masked intermittently and coated together with the samples, using a Byko-test 1500 NFe measuring device (BYK Instruments, Geretsried, Germany) in accordance with SSPC-PA 2 [23]. Each panel was tested at 6 different locations.

2.8. Measurement of Adhesion

Cross-cut tests were carried out according to ISO 2409:2020 using an Elcometer 107 & 121/4 6 × 3 mm cutter (Elcometer Limited, Manchester, UK), and ASTM D3359 Method A was applied in case of X-cross experiments [18,24].

3. Results and Discussion

3.1. Test Panel Evaluation

The test plate is usually covered with the BC in three very different ways, resulting in different effect pigment orientations. In our case a high proportion of horizontally oriented particles could be observed on the microscopic images at all variations (Figure 1), which is expected to result in a more uniform and consistent visual appearance, with enhanced metallic brightness and a more pronounced surface reflection.
Figure 1. SEM images of (a) sprayed metallic BC layer and (b) as-received metallic basecoat paint applied on the surface with a palette knife.

3.2. Refinishing Procedure

Blending is essential in automotive refinishing. The technique involves gradually fading the BC into adjacent areas, minimizing visible color differences and ensuring continuity of appearance. The application of CC over the blended area further protects the repair and restores a uniform finish.
Figure 2 shows the repair documentation for Sample C1. Sanding of the damaged surface (Figure 2a) was carried out to determine the undercoat color and layers, and to enhance adhesion at the intact part. After color equalization and creating the transition areas (Figure 2b), a clear coat layer was applied (Figure 2c). The paint produced a flop effect, for which uniform layers and sufficient quantities were fundamental. In our case optically satisfying results could be obtained after polishing Sample C1, as presented in Figure 2d.
Figure 2. Repair of Sample C1. (a) Preparation and coverage with UV curable filler—A: damaged area after sanding; B: area with removed CC; C: unmodified original paint. (b) Appearance after BC application, (c) appearance after CC application, (d) visual evaluation of the painted area and its surroundings.
In Figure 3 the steps of the repair painting of Sample C2 are depicted. In this case the hood and the bumper were coated together with the CC to obtain the optimal visual effect.
Figure 3. Sample C2 refinishing. (a) Parts after primer application, (b) parts after BC application, (c) parts after CC coating and (d) all the painted parts including the bumper.

3.3. Analysis of the Appearance After Refinishing

Refinishing quality can be evaluated using spectrophotometric and gloss measurements; however, in workshop practice, careful visual assessment remains the primary criterion for evaluating the quality of a repair, making instrumental color and gloss measurements less relevant to the scope of this study. Because of the complex reflectance behavior of the finishes, both visual and instrumental evaluations should be conducted from multiple angles. The present study demonstrated that, when proper refinishing procedures are followed, homogeneous coatings can be achieved without visible transitions or defects. Observer perception also plays a role: while minor metallic mismatches were nearly imperceptible at typical viewing angles, they became slightly noticeable under extreme conditions. The uncertainty of the non-experts was clear, especially regarding orange peel, haze and gloss. Color itself and flop seemed to be easier to understand. Adherence to established standards ensured consistent and repeatable evaluation. In the present study, visual assessment was performed under controlled lighting conditions according to ISO 13076, while layer thickness and adhesion were evaluated according to SSPC-PA 2, ISO 2409, and ASTM D3359. In this study, both experienced professionals and trained laypersons evaluated coatings under various lighting and viewing conditions. Although color and flop differences were identified reliably, less experienced observers showed greater uncertainty when assessing orange peel, haze, and gloss. These results indicate that visual assessment skills can be improved through structured training and correlation with instrumental measurements.

3.4. Adhesion Test Results

As is widely known, adhesion of paints on plastic parts requires advanced surface treatment technologies at OEMs; however, in the refinishing workshops such solutions are not feasible. To analyze the effect of the available pre-treatment methods, two types of plastic parts were tested, with variations in heat treatment and sanding. Layer thickness was measured on the test panels that were sprayed together with the samples, and the results are summarized in Table 1. Due to the manual operations, the results show high variability. It is worth emphasizing that the specific layer thickness requirements change from manufacturer to manufacturer, and even among colors differences can be defined. Typical layer thicknesses depend on the coating system and manufacturer specification; therefore, the measured values should primarily be evaluated in relation to the applied product data sheets.
Table 1. Mean layer thicknesses in μm.
Adhesion was tested according to the ISO 2409 cross-cut test and the ASTM D3359 Method A X-cross tests. All specimens exhibited good adhesion and could be categorized as 0 and 5B according to ISO 2409 and ASTM D3359, respectively (Figure 4) [18,24].
Figure 4. Sample A1 after coating. (a) Cross-cut test and (b) X-cross test results.
Although the adhesion tests confirmed adequate coating adhesion, they cannot fully replicate the more demanding OEM qualification procedures. Consequently, reliable adhesion in refinishing depends on strict compliance with manufacturers’ recommendations and controlled application processes. The results showed that the applied coating system provided at least the minimum adhesion on the investigated plastic substrates under all tested preparation routes. However, the simplified adhesion tests did not allow a clear ranking of the individual pretreatment methods.

4. Conclusions

The presented preliminary findings highlight that successful automotive refinishing depends not only on accurate color matching but also on process control, surface quality, and human visual perception. Blending techniques are essential for localized repairs, particularly for metallic and pearlescent finishes, as they minimize visible color and effect differences and ensure visual continuity. Surface characteristics such as gloss and distinctness of image (DOI) are equally important, since mismatches can make repairs noticeable even when color reproduction is accurate. The present study demonstrates the main principles, practical limitations, and evaluation aspects of manual automotive refinishing through real vehicle repair examples and complementary adhesion tests on plastic substrates. As automotive coatings become increasingly complex, continued advances in color measurement, formulation software, and technician training will be necessary.
Overall, the challenges of color matching, flake orientation, gloss control, metamerism, and adhesion can be effectively managed through a combination of modern technology, adherence to standards, and skilled application techniques, enabling repairs that are virtually very close to factory finishes.

Author Contributions

Conceptualization, K.K. and E.V.; methodology K.K. and E.V.; validation, K.K. and E.V.; formal analysis, K.K.; investigation, K.K. and E.V.; resources, K.K.; data curation, E.V.; writing—original draft preparation, E.V.; writing—review and editing, K.K. and E.V.; visualization, K.K. and E.V.; supervision, K.K.; project administration, E.V.; funding acquisition, K.K. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

Not applicable.

Data Availability Statement

All data are available upon request from the corresponding author.

Acknowledgments

The authors express their sincere gratitude to János Katona for his skilled execution of the refinishing procedures on the test panels.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Seubert, C.; Nietering, K.; Nichols, M.; Wykoff, R.; Bollin, S. An Overview of the Scratch Resistance of Automotive Coatings: Exterior Clearcoats and Polycarbonate Hardcoats. Coatings 2012, 2, 221–234. [Google Scholar] [CrossRef] [Scilit]
  2. Burgos-Fernández, F.J.; Pujol, J.; Perales, E.; Martínez-Verdú, F.M.; Vilaseca, M. Texture Evaluation of Automotive Coatings by Means of a Gonio-Hyperspectral Imaging System Based on Light-Emitting Diodes. Coatings 2020, 10, 320. [Google Scholar] [CrossRef] [Scilit]
  3. Maile, F.J.; Pfaff, G.; Reynders, P. Effect Pigments—Past, Present and Future. Prog. Org. Coat. 2005, 54, 150–163. [Google Scholar] [CrossRef] [Scilit]
  4. Ulbrich, D.; Kowalczyk, J.; Jósko, M.; Sawczuk, W.; Chudyk, P. Assessment of Selected Properties of Varnish Coating of Motor Vehicles. Coatings 2021, 11, 1320. [Google Scholar] [CrossRef] [Scilit]
  5. ISO 3668:2017; Paints and Varnishes—Visual Comparison of the Colour of Paints. International Organization for Standardization: Geneva, Switzerland, 2017.
  6. DIN 6175:2019; Colour Tolerances for Automotive Coatings—Solid and Effect Coatings. Deutsches Institut für Normung: Berlin, Germany, 2019.
  7. Challener, C. Automotive Coatings: Creating Excitement with Effect Pigments. CoatingsTech Mag. 2016, 13, 26–32. [Google Scholar]
  8. ASTM E2194-14; Standard Test Method for Multiangle Color Measurement of Metal Flake Pigmented Materials. ASTM International: West Conshohocken, PA, USA, 2021.
  9. ASTM D5767-18; Standard Test Methods for Instrumental Measurement of Distinctness-of-Image Gloss of Coating Surfaces. ASTM International: West Conshohocken, PA, USA, 2018.
  10. Beuckels, S.; Audenaert, J.; Hanselaer, P.; Leloup, F.B. Development of an Image-Based Measurement Instrument for Gloss Characterization. J. Coat. Technol. Res. 2022, 19, 1567–1582. [Google Scholar] [CrossRef] [Scilit]
  11. Zarin, I.; Arissi, G.; Barias, E.; Hoque, M.J.; Ma, J.; Rabbi, K.; Miljkovic, N. Characterization of Nanoscale Pinhole Defects in Hydrophobic Coatings Using Copper Electrodeposition. Appl. Phys. Lett. 2023, 123, 231602. [Google Scholar] [CrossRef] [Scilit]
  12. Tiedje, O.; Paustian, S.; Rosenkranz, S.; Hecker, M.; Tropea, C. Detection of Production Relevant Deviations in Paint Sprays. J. Coat. Technol. Res. 2025, 22, 877–884. [Google Scholar] [CrossRef] [Scilit]
  13. Primc, G.; Mozetič, M. Surface Modification of Polymers by Plasma Treatment for Appropriate Adhesion of Coatings. Materials 2024, 17, 1494. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  14. Varga, E.; Palásti, F.; Bata, A.; Kovács, P.I. Comparative Study of Plasma, Laser, and Flame Induced Activation of HDPE Liner Surfaces of Type 4 Hydrogen Vessels. J. Adhes. 2025, 101, 909–929. [Google Scholar] [CrossRef] [Scilit]
  15. Morgese, G.; Siegmann, K.; Winkler, M. Specific, Nondestructive, and Durable Adhesion Primer for Polyolefins. J. Coat. Technol. Res. 2024, 21, 1921–1930. [Google Scholar] [CrossRef] [Scilit]
  16. Peng, X.; Zhang, Z.; Zhang, R. Effects of Sanding Process on Adhesion of Waterborne Paint Film on a Polypropylene Membrane Surface. For. Prod. J. 2020, 70, 232–240. [Google Scholar] [CrossRef] [Scilit]
  17. ASTM D4541-22; Standard Test Method for Pull-Off Strength of Coatings Using Portable Adhesion Testers. ASTM International: West Conshohocken, PA, USA, 2022.
  18. ISO 2409:2020; Paints and Varnishes—Cross-Cut Test. International Organization for Standardization: Geneva, Switzerland, 2020.
  19. Ye, Q. Progress in Global Waterborne Automotive Repair Paint. Paint. Coat. Ind. 2018, 48, 83–87. [Google Scholar] [CrossRef]
  20. Bellisario, D.; Quadrini, F.; Santo, L. Study and Characterization of Automotive Coating Repairs. Int. J. Mod. Manuf. Tech. 2012, IV, 21–28. [Google Scholar]
  21. Ulbrich, D.; Kowalczyk, J.; Stachowiak, A.; Sawczuk, W.; Selech, J. The Influence of Surface Preparation of the Steel during the Renovation of the Car Body on Its Corrosion Resistance. Coatings 2021, 11, 384. [Google Scholar] [CrossRef] [Scilit]
  22. ISO 13076:2019; Paints and Varnishes—Lighting and Procedure for Visual Assessments of Coatings. International Organization for Standardization: Geneva, Switzerland, 2019.
  23. SSPC-PA 2:2022; Procedure for Determining Conformance to Dry Coating Thickness Requirements. The Society of Protective Coatings: Pittsburgh, PA, USA, 2022.
  24. ASTM D3359-23; Standard Test Methods for Rating Adhesion by Tape Test. ASTM International: West Conshohocken, PA, USA, 2023.
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations