Skip to Content
EngEng
  • Article
  • Open Access

23 November 2026

42 Pages

Source-Dependent Processing and Printability of Recycled HDPE and PP Filaments for Fused Filament Fabrication

,
,
,
,
,
,
,
,
and
1
Research Group in Industrial Engineering (Giii), Faculty of Industrial Engineering, Universidad Tecnológica de Panamá, Panama City 0819-07289, Panama
2
Centro de Estudios Multidisciplinarios en Ciencia, Ingeniería y Tecnología (CEMCIT-AIP), Panama City 0819-07289, Panama
3
Research Group in Design, Manufacturing and Materials (DM + M), School of Mechanical Engineering, Universidad Tecnológica de Panamá, Panama City 0819-07289, Panama
4
Sistema Nacional de Investigación (SNI), Clayton, Panama City 0819-07289, Panama
Eng2026, 7(12), 665;https://doi.org/10.3390/eng7120665 
(registering DOI)

Abstract

Post-consumer high-density polyethylene (HDPE) and polypropylene (PP) are promising feedstocks for fused filament fabrication (FFF), but source-dependent variability can limit filament quality and printability. Eight source-segregated streams were evaluated, using ATR-FTIR (27 spectra) to support identification of predominant PE- and PP-based matrices and extrusion with longitudinal diameter analysis as the core assessment. Seven streams underwent extrusion, yielding 405 runs and 14,175 sequential diameter measurements relative to the 1.75 mm target. For HDPE, screw rotational speed produced the largest change in mean filament diameter, whereas increasing spooler speed consistently reduced PP filament diameter. Across all extrusion-screening runs, HDPE-White (H-W) had lower average within-run variability (SD = 0.041 mm; CV = 2.33%) than PP-Transparent (P-T; SD = 0.212 mm; CV = 14.43%). In separate printing trials, H-W yielded complete specimens without feeding assistance, whereas P-T required manual feeding. Preliminary apparent maximum tensile stress across recycled-material groups ranged from 10.90 to 15.21 MPa, and qualitative SEM documented deposited-road architecture and void-like open regions on selected fracture surfaces. Overall, polymer-family identification and mean diameter alone were insufficient for qualification; longitudinal stability, feeding continuity, adhesion, and printer configuration should be considered jointly when screening recycled polyolefin feedstocks for FFF.

1. Introduction

1.1. Post-Consumer HDPE and PP Recycling

High-density polyethylene (HDPE) in particular is one of the most commonly produced polymers in the world, accounting for approximately 12.9% of the nearly 367 million metric tons produced each year [1]. However, HDPE and polypropylene (PP), as major members of the polyolefin family, account for approximately 42% of the polymer content in plastic waste [2]. It is for this reason that their prevalence in the waste stream poses a significant environmental and economic challenge [3,4].
In this context, mechanical recycling provides a practical route to recover value from post-consumer polyolefin waste and support more sustainable material use [4,5]. For instance, the manufacture of recycled HDPE (r-HDPE) needs only 34% of the energy required for producing virgin polymer, which means there is a genuine decrease of 66% in energy use, comparing 8.7 MJ/kg with 25.9 MJ/kg for virgin polymer, and it results in a 70% reduction in carbon dioxide emissions (the emission being only 0.56 kg CO2e/kg) [3]. Nevertheless, despite these clear benefits, global recycling rates remain very low, at just 9–10% of total production [2,6].

1.2. Recycled Polyolefins as FFF Feedstock

Fused Filament Fabrication (usually referred to as FFF or FDM) is a widely used, comparatively low-cost extrusion-based additive manufacturing process that is based on extrusion [6,7]. In the past, the range of materials that could be used in FFF has been restricted to amorphous or low-crystallinity thermoplastics such as ABS and PLA [8]. Semi-crystalline polyolefins like PP and HDPE pose considerable processing difficulties in FFF since they suffer from substantial volumetric shrinkage and warpage as they cool from the molten state [9,10]. This shrinkage results from the long-range ordering of the polymer chains when they crystallize [9]. Nevertheless, there is increasing interest in overcoming these limitations and in using recycled HDPE and PP to produce sustainable filaments, thereby offering a good opportunity for upcycling to recover value from this plastic waste [7,11,12].

1.3. Importance of Feedstock Source

A major challenge in recycling polyolefins is the wide variation in raw-material properties depending on where they came from or how they were first used after being sold to consumers. PP from disposable plastic cups used at fast food chains was designed for blow molding, which means it has a high molecular weight and high melt viscosity and therefore requires very high extrusion temperatures to mold successfully [13]. For HDPE, its physical properties and the extent of thermal degradation depend strongly on whether it comes from bottle caps, milk containers, or marine components exposed to open air for a long time [4,11]. These different origins lead to variations in crystallinity and the introduction of impurities and cross-contamination (for example, the presence of low-density polyethylene, LDPE, in HDPE bottle caps), all of which directly affect the homogeneity of the final filament [14].

1.4. Research Gap

Previous studies have reported the recycling of commercial polymers for FFF [15], including the development and characterization of recycled PP- and HDPE-based composite filaments [8,9].
Karaki et al. [16] reviewed the challenges associated with material extrusion of polyethylene, particularly those related to its semicrystalline nature, shrinkage, warpage, and adhesion behavior. Strano et al. [17] investigated the printability of recycled thermoplastic feedstocks and the properties of printed components. Furthermore, Zhu et al. [13] demonstrated that differences among post-consumer PP sources can influence rheological behavior and the characteristics of FFF-printed components. These studies establish that feedstock characteristics and processing conditions influence the feasibility of recycled-polymer additive manufacturing (AM).
However, although previous research has established that post-consumer feedstock source can influence the processing and printability of recycled PP [13], further comparative experimental evidence is needed to understand how multiple source-segregated HDPE and PP streams respond to controlled filament-extrusion conditions, particularly in terms of short-window dimensional variability and subsequent qualitative FFF printability outcomes.

1.5. Contribution

This study addresses this gap through a laboratory-scale comparative evaluation of source-segregated post-consumer HDPE and PP streams from different consumer-product sources, processed into filament for FFF [4,12,13]. By preserving feedstock-source identity throughout material preparation, extrusion, dimensional characterization, and printing trials, the study examines whether streams assigned to the same nominal polymer family exhibit different processing and functional behaviors.
Furthermore, this study evaluates how extrusion conditions affect filament diameter and short-window longitudinal dimensional variability through 405 experimental extrusion runs and 14,175 sequential diameter measurements. This experimental approach enables the assessment of processing effects and the identification of source-specific conditions associated with improved filament consistency. It extends filament assessment beyond nominal or mean diameter by considering within-run variability, extrusion continuity, feeding behavior, and qualitative printability outcomes.
Accordingly, this study integrates ATR-FTIR spectral characterization, extrusion behavior, filament dimensional analysis, qualitative printability evaluation, preliminary tensile characterization, and low-magnification SEM examination of printed specimens. The combined analysis provides experimental evidence of source-dependent processing behavior within the investigated material streams and demonstrates the importance of evaluating additional processing and feeding characteristics alongside nominal filament diameter when assessing the suitability of recycled polyolefin filaments for FFF.

2. Materials and Methods

2.1. Study Design

An experimental feasibility assessment was conducted on post-consumer HDPE and PP streams to produce recycled filaments intended for FFF. Feedstocks were sourced from various post-consumer products and segregated by polymer family and source to ensure individual traceability throughout the experimental workflow.
The methodology included feedstock preparation, chemical identification using attenuated total reflectance Fourier-transform infrared spectroscopy (ATR-FTIR), filament extrusion, longitudinal dimensional characterization, printability assessment, preliminary tensile characterization, and qualitative scanning electron microscopy (SEM) examination of fracture surfaces generated during tensile testing. For each source-segregated feedstock stream, the prepared material was subdivided into three separately processed experimental batches drawn from the same recovered stream. These batches served as experimental blocks to evaluate the consistency of filament production under the specified processing conditions.
The experimental workflow was structured to determine whether post-consumer streams within the same polymer family exhibit distinct processing and functional behaviors during filament production and FFF. The investigation focused on the relationships among feedstock source, polymer family identification, extrusion conditions, filament dimensional stability, and subsequent printability. The scope of the study was limited to a laboratory-scale feasibility assessment rather than an industrial-scale validation of recycled HDPE or PP filament production.
Figure 1 summarizes the complete experimental workflow, encompassing post-consumer feedstock collection and preparation, extrusion, dimensional characterization, printability assessment, tensile testing, and SEM examination.
Figure 1. Experimental workflow for producing and characterizing source-segregated post-consumer HDPE and PP filaments, including feedstock collection and preparation, ATR-FTIR characterization, filament extrusion, longitudinal dimensional analysis, FFF printability evaluation, preliminary tensile testing, and SEM fracture-surface examination.

2.2. Feedstock Origin and Coding

Post-consumer HDPE and PP materials were collected from different discarded consumer products and maintained as source-segregated streams throughout the study. Polymer classification was initially determined using the resin identification codes molded on the original products: code 2 for HDPE and code 5 for PP. To ensure traceability during ATR-FTIR characterization, extrusion, dimensional analysis, and printability assessment, each feedstock stream received an alphanumeric identifier reflecting polymer family and visual characteristics, such as color or transparency. Table 1 summarizes the origin, source coding, and polymer classification for the eight post-consumer streams evaluated in this study.
Table 1. Origin, coding, and experimental use of the post-consumer HDPE and PP streams.
The P-R stream was retained for ATR-FTIR characterization but was excluded from extrusion and subsequent analyses because the recovered quantity was insufficient to conduct an extrusion experiment. Stream codes identified the specific recovered product-origin and color categories rather than isolated color effects or verified resin grades. Because product origin, pigmentation, formulation, and prior service history were not controlled independently, the observed differences among feedstock streams cannot be attributed uniquely to any one of these characteristics. Accordingly, these comparisons apply only to the recovered material lots evaluated in this study. The number of individual recovered products, the starting mass for each stream, and verified resin-grade specifications were not consistently retained in the source records and therefore cannot be reported.

2.3. Feedstock Preparation

The feedstock preparation procedure was applied to all post-consumer streams that progressed to the extrusion experiments. The P-R stream was excluded from this stage because the recovered quantity was insufficient for downstream processing and was retained only for ATR-FTIR characterization.
Labels, adhesives, and visible contaminants were manually removed. When necessary, materials were washed in soapy water for approximately 1 h. Subsequently, the materials were dried in a convection oven at 60 °C in 2-h cycles until no visible surface moisture remained.
Each source-segregated stream was shredded separately, without intentional mixing of materials from different product types or brands. The shredding equipment was cleaned between processing different streams. Resulting particles were sieved using a 3.5 mm mesh, and oversized fragments were returned to the shredding process.
Following shredding and sieving, each feedstock stream was divided into three experimental batches. Each batch underwent a second washing step, performed separately with approximately 2 gallons of water and 0.5 g of detergent. The material was filtered through cloth to retain small particles and rinsed until detergent residues were eliminated.
The washed batches were dried at 80 °C for approximately 5 h, with additional drying applied as needed. Each batch was stored separately in vacuum-sealed resealable plastic bags until extrusion.

2.4. ATR-FTIR Spectral Acquisition and Polymer Identification

ATR-FTIR spectroscopy was used as a complementary method to identify the predominant polymer family of the source-segregated post-consumer streams and to generate spectral data for evaluating within- and between-stream variability. Spectra were acquired using a Fourier-transform infrared spectrometer (IRXross, Shimadzu Corporation, Kyoto, Japan) equipped with an attenuated total reflectance (ATR) accessory fitted with a zinc selenide (ZnSe) crystal, allowing direct analysis of the polymer samples with minimal sample preparation.
Spectra were collected over a nominal wavenumber range of 4000–600 cm−1 at a spectral resolution of 8 cm−1, using 40 scans per spectrum. Spectral acquisition was performed using LabSolutions IR Version 2.31 software (Shimadzu Corporation, Kyoto, Japan). For each measurement, the polymer specimen was placed directly on the ZnSe ATR crystal and pressed against the crystal using the pressure-clamp mechanism integrated into the ATR accessory to maintain contact during acquisition. No additional surface preparation was applied before spectral measurement.

2.4.1. Sample Groups

ATR-FTIR spectra were available for all eight source-segregated post-consumer streams identified during the collection stage. Multiple spectra were acquired for each stream to evaluate within-stream spectral repeatability. The final dataset comprised 27 ATR-FTIR spectra: 12 from the four HDPE streams and 15 from the four PP streams. The distribution of ATR-FTIR measurements among the eight source-segregated feedstock streams is summarized in Table 2.
Table 2. ATR-FTIR spectra available for each post-consumer feedstock stream.
The P-R stream was included in the ATR-FTIR characterization despite its exclusion from the subsequent extrusion experiments because sufficient material was available for spectroscopic analysis but not for preparing an experimental extrusion batch.

2.4.2. Spectral Preprocessing

The spectral files were first inspected to determine whether the recorded intensity values were expressed as percentage transmittance (%T) or absorbance. Spectra recorded in percentage transmittance were converted to absorbance according to:
A = − log 10 % T 100
where (A) is absorbance and (%T) is percentage transmittance.
All spectra were ordered by wavenumber and interpolated onto the spectral interval common to all 27 measurements, approximately 600–3250 cm−1. The upper limit of 3250 cm−1 was defined by the exported spectral range available for the P-B measurements. It was therefore adopted to maintain a common spectral domain across the complete dataset.
Baseline correction was performed on the absorbance spectra using an asymmetric least-squares (AsLS) procedure with a smoothing parameter of λ = 10 6 an asymmetry parameter of (p = 0.01) and 15 iterations. Spectral regions from 2300–2400 cm−1 and 650–675 cm−1 were excluded from the quantitative analysis because they are susceptible to atmospheric CO2 contributions. Spectra already exported in absorbance were retained in that form. Unit-vector normalization was then applied to the retained, baseline-corrected absorbance spectra before Pearson correlation and principal component analyses.
For graphical comparison in Figure 2, a mean baseline-corrected absorbance spectrum was calculated for each feedstock stream from its replicate spectra and subsequently transformed to corrected transmittance for display. Vertical offsets were applied only to improve visual separation among the stream-averaged spectra. The spectral regions excluded from quantitative analysis (2300–2400 cm−1 and 650–675 cm−1) are indicated by shaded areas in Figure 2 to distinguish them from polymer-specific absorption features.
Figure 2. Stream-averaged baseline-corrected ATR-FTIR spectra of the source-segregated post-consumer feedstock streams: (a) HDPE streams H-R, H-W, H-B, and H-ST; and (b) PP streams P-W, P-B, P-R, and P-T. For each stream, replicate spectra were processed using a common baseline-correction procedure, averaged in absorbance space, and transformed to corrected transmittance for graphical display. Vertical offsets were applied only for visual clarity. Shaded regions indicate the spectral intervals excluded from quantitative correlation and PCA analyses because of potential atmospheric CO2 contributions.
Quantitative correlation and PCA analyses were performed using the baseline-corrected and unit-vector-normalized absorbance spectra rather than the displayed corrected-transmittance spectra.

2.4.3. Spectral Analysis

The ATR-FTIR spectra were evaluated at two complementary levels. The stream-averaged baseline-corrected spectra displayed in corrected transmittance form in Figure 2 were examined qualitatively to assess the presence of characteristic absorption bands associated with PE- and PP-based materials. Quantitative comparisons among replicate spectra and feedstock streams were performed using the baseline-corrected and unit-vector-normalized absorbance spectra described in Section 2.4.2. Section 2.12.1 describes the statistical procedures used to evaluate within-stream repeatability, between-stream spectral similarity, and exploratory multivariate grouping.

2.4.4. Polymer-Characteristic Spectral Bands

Polymer family identification was based primarily on comparison of the measured spectral profiles with characteristic absorption regions expected for polyethylene (PE)- and PP-based materials. The principal absorption bands used to support HDPE and PP identification are summarized in Table 3 and Table 4, respectively.
Table 3. Reference ATR-FTIR bands used for qualitative identification of PE-based materials assigned to the HDPE streams.
Table 4. Reference ATR-FTIR bands used for qualitative identification of PP-based materials.
Streams exhibiting the principal PE fingerprint were described as having a PE-based matrix compatible with HDPE [18], whereas spectra exhibiting the characteristic PP fingerprint were considered supportive of classification as PP-based materials, according to [19].

2.5. Extrusion Equipment and Procedure

Before extrusion, the prepared feedstocks were preconditioned at 80 °C for 1 h to reduce residual moisture before processing. HDPE was extruded using a Felfil Extruder coupled with a Felfil Spooler for filament take-up and winding. This system allowed adjustment of extrusion temperature, screw speed, and spooler speed.
PP was processed using a Wellzoom filament extruder, while the Felfil Spooler was retained for filament collection. The Wellzoom unit was used because PP was more difficult to process adequately with the Felfil Extruder. As the Wellzoom extruder did not provide a direct screw-speed reading, it was operated at its maximum setting, corresponding to an estimated speed of approximately 9 rpm.
Each feedstock stream and experimental batch were processed separately. The molten strand leaving the extrusion die was guided to the spooler and collected as filament for subsequent dimensional evaluation. The processing-factor levels evaluated for HDPE and PP are described in Section 2.6.
Both extrusion systems used their original nominal 2 mm die outlets. Following extrusion, the filament was cooled under ambient conditions, with additional airflow provided by the fans of the Felfil filament-handling system. The estimated distance between the die outlet and the spooler was approximately 0.50–0.60 m. The operator estimated the ambient temperature to be approximately 20 °C, although no continuous temperature record was retained.
Each processing-parameter combination was operated for approximately 5 min. After changing the settings, approximately 3 min and 30 s elapsed before a 60 s video recording of the spooler diameter display was initiated. The 35 sequential diameter readings retained for analysis were transcribed from the corresponding video recordings at approximately one-second intervals, as described in Section 2.7. During transitions between feedstock streams, the extruder was purged with the incoming material for approximately 30 min, and the transition filament was discarded.
The HDPE streams were processed in the sequence H-W, H-R, H-ST, and H-B, followed by the PP streams in the sequence P-W, P-B, and P-T. The exact chronological order of parameter combinations within individual batches was not preserved in the analytical dataset. The reported operating times, distances, and cooling conditions were reconstructed from the operator’s account and were not independently verified against complete contemporaneous equipment logs. The mass processed in each individual run was not recorded. No contemporaneous randomization schedule was retained, and therefore random allocation of the processing-condition order cannot be verified.

2.6. Experimental Design

The extrusion experiments were conducted using source-segregated HDPE and PP feedstocks. Within each stream, the recovered material was redistributed into three processing batches after shredding. The resulting batches were subsequently processed in separate sessions, but they did not represent independent feedstock collections or fully independent material preparations. Each unique combination of feedstock stream, processing batch, and extrusion settings was assigned a RunID and treated as one run-level observation for dimensional analysis. This operational definition does not imply an independent extruder restart between successive processing conditions. Separate experimental designs were used for HDPE and PP because different extrusion systems were required.

2.6.1. HDPE Experimental Design

Four HDPE streams were evaluated: H-R, H-W, H-B, and H-ST. For each stream, three extrusion temperatures (190, 200, and 210 °C), three screw rotational speeds (4, 6, and 8 rpm), and three spooler-speed levels (0.32, 0.34, and 0.36 m/min) were investigated.
For each HDPE stream, a full-factorial design combined the three extrusion temperatures, three screw-speed levels, and three spooler-speed levels, yielding 27 processing conditions. Each of the 27 processing conditions was evaluated in each of the three experimental batches, resulting in 81 extrusion runs per HDPE stream and 324 HDPE extrusion runs in total.
Temperature, screw speed, and spooler speed were treated as categorical factors in the statistical analysis to avoid assuming a linear relationship between factor level and dimensional response. Batch was included as a fixed blocking factor.

2.6.2. PP Experimental Design

Three PP streams progressed to the extrusion experiments: P-W, P-B, and P-T. The P-R stream was excluded because the quantity recovered during collection was insufficient for extrusion.
The Wellzoom extruder was operated at its maximum setting, corresponding to an estimated screw speed of approximately 9 rpm, which remained approximately constant throughout the PP experiments. Therefore, extrusion temperature and spooler speed were the processing factors varied experimentally.
P-W and P-B were evaluated at 180, 190, and 200 °C, whereas P-T was evaluated at 170, 180, and 190 °C. All PP streams were evaluated at spooler speeds of 0.36, 0.42, and 0.52 m/min.
For each PP stream, a full-factorial design combined three extrusion temperatures and three spooler-speed levels, yielding nine processing conditions. Each condition was evaluated in each of the three experimental batches, resulting in 27 extrusion runs per PP stream and 81 PP extrusion runs in total.
Because the absolute temperature range used for P-T differed from those used for P-W and P-B, the PP streams were analyzed separately. The extrusion factors, processing levels, number of batches, and total runs are summarized in Table 5.
Table 5. Experimental factors and levels used during filament extrusion.

2.7. Filament Diameter Measurement

Filament diameter was monitored longitudinally during each extrusion run using the diameter-measurement system integrated into the Felfil Spooler. The system operates through a roller-based mechanism consisting of a fixed reference roller and a vertically movable roller through which the filament passes. Variations in filament thickness displace the movable roller relative to the reference position, and the integrated sensor system converts this displacement into a filament diameter value displayed in millimeters on the spooler interface.
For each combination of feedstock stream, experimental batch, and extrusion condition, the diameter display was video recorded for approximately 1 min. The recording preserved only the sequence of instrument-displayed diameter values; filament diameter was not determined from image dimensions or pixel-based measurements. The recordings were subsequently reviewed at approximately 1 s intervals, and the numerical diameter value shown on the spooler display was transcribed from the corresponding frames.
A consistent extraction procedure was applied to all extrusion runs. For each run, 35 consecutive instrument-displayed diameter values were transcribed from the corresponding video recording at approximately one-second intervals and retained for analysis. These measurements were indexed sequentially using a TimeIndex from 1 to 35. The 35 observations represented longitudinal temporal subsamples from a single extrusion run and were therefore not treated as independent experimental replicates. Each extrusion run, defined by the unique combination of feedstock stream, batch, and processing condition, constituted the experimental unit. These 35 consecutive observations characterize only the sampled portion of each extrusion run and do not establish sustained dimensional stability over the full length of the produced filament. Furthermore, the video-frame sampling interval should not be interpreted as the independently verified update frequency of the diameter-measurement system.
No pixel calibration or image-based conversion was applied because the numerical diameter values were obtained directly from the spooler display. The exact hardware revision, display resolution, manufacturer-specified measurement accuracy, and calibration history of the integrated diameter-monitoring system were not available in the retained experimental records. Consequently, the recorded diameter values were treated as instrument-reported estimates and used primarily to compare target deviation and longitudinal dimensional stability across experimental runs.
The resulting dataset included the feedstock-stream identifier, batch, extrusion temperature, extrusion speed level (where applicable), spooler-speed level, RunID, TimeIndex, and displayed filament diameter. These sequential measurements were subsequently summarized at the run level using the dimensional indicators described in Section 2.8.
An independent post-experiment dimensional assessment was conducted on three retained filament segments identified in the laboratory records as H-R, transparent PP, and white HDPE. At 15 longitudinal positions spaced approximately 50 mm apart along each retained filament segment, diameter measurements were obtained in two perpendicular orientations (0° and 90°), with three repeated readings per orientation, using a Mitutoyo 293–330 digital micrometer with a stated resolution of 0.001 mm. This procedure yielded 270 individual measurements. Dimensional characterization included the mean diameter at each position, between-position variability, and the absolute difference between mean diameters measured in the two orientations. Because the retained segments could not be linked to specific historical extrusion runs or printed specimens, these measurements were analyzed separately from the original spooler-monitoring dataset. The measurement records and descriptive results are provided in Supplementary Table S11.

2.8. Run-Level Dimensional Indicators

Because the 35 sequential filament-diameter measurements obtained within each extrusion run represented temporal subsamples of the same experimental unit, dimensional performance was summarized at the run level before statistical analysis. Each RunID therefore contributed one set of run-level dimensional indicators rather than 35 independent experimental observations.
The nominal filament diameter of 1.75 mm was used as the reference target for the laboratory-scale extrusion experiments. A narrow interval of 1.73–1.77 mm (±0.02 mm around the nominal target) was predefined as a study-specific screening criterion, informed by a dimensional tolerance associated with commercially available PLA filament. This interval described dimensional deviations in the recorded filament-diameter measurements and was not intended to represent a universal FFF filament standard, a validated acceptance limit for recycled HDPE or PP, a certified filament specification, or a statement of measurement uncertainty. For each extrusion run, 35 consecutive measurements were used to characterize mean diameter, within-run variability, deviation from the nominal target, and the percentage of measurements within the predefined screening interval. The standard descriptive indicators calculated for each RunID were mean diameter, within-run standard deviation (SD), coefficient of variation (CV), minimum diameter, maximum diameter, and diameter range. Mean diameter described the average filament size during the analyzed sequence, whereas SD and CV quantified absolute and relative longitudinal variability within the run.
To quantify the deviation of the run-average diameter from the nominal filament diameter, the absolute target error ( E a b s ) was calculated as
E a b s = | D ¯ − 1.75 |
where D ¯ is the mean filament diameter calculated from the 35 sequential measurements within a given extrusion run. Smaller E a b s values indicate greater proximity of the run mean to the nominal 1.75 mm target.
The percentage of measurements falling within the predefined dimensional tolerance was calculated as:
P t o l = 100 n ∑ i = 1 n I ( 1.73 ≤ D i ≤ 1.77 )
where D i is the i -th filament-diameter measurement, n = 35 is the number of sequential measurements retained for each extrusion run, and I ⋅ is an indicator function equal to 1 when the measurement falls within the 1.73–1.77 mm tolerance interval and 0 otherwise.
The run-level indicators were interpreted jointly. A mean diameter close to 1.75 mm was not considered sufficient evidence of dimensional stability when the same run exhibited high within-run variability or a low proportion of measurements within the predefined tolerance interval. These indicators were subsequently used to evaluate processing effects and their relationship with filament printability. The run-level indicators retained for dimensional characterization are summarized in Table 6.
Table 6. Run-level indicators used to characterize filament dimensional performance.
In particular, a mean diameter close to 1.75 mm was not considered sufficient evidence of dimensional stability when the same run exhibited high within-run variability or a low percentage of measurements within the predefined tolerance interval.

2.9. Printability Evaluation

Printability trials were conducted to evaluate whether the recycled filaments could be continuously fed through an FFF system and used to complete the intended specimen geometry. Filaments selected for printing were obtained from extrusion conditions considered suitable based on their dimensional behavior and continuity.
HDPE trials were performed using an Ender 3 S1 Pro and a Bambu P1S. Nozzle temperatures of 230, 235, and 240 °C and bed temperatures of 60, 70, and 80 °C were evaluated. Specimens were printed using 15% triangular infill, and Bambu Lab solid and liquid adhesives were used to improve bed adhesion. On the Bambu P1S, different combinations of the part, chamber, and auxiliary fans were evaluated to assess the influence of cooling on printing stability. The printing parameters and conditions evaluated during the HDPE printability trials are summarized in Table 7.
Table 7. Printing parameters evaluated for recycled HDPE filaments.
The archived Bambu P1S project specifies a flat build orientation, a 0.4 mm nozzle, a nominal filament-diameter setting of 1.75 mm, a 0.20 mm layer height, two perimeter walls, five top layers, three bottom layers, and 15% triangular infill with a 45° infill-direction setting. A two-layer raft was configured on a textured PEI build plate. The filament profile assigned to the specimen in this project records a flow ratio of 0.98. These settings refer specifically to the archived Bambu P1S HDPE project and should not be generalized to all exploratory configurations or to the PP trials conducted with the Ender 3 S1 Pro.
PP printing trials were conducted primarily using the Ender 3 S1 Pro. Nozzle temperatures of 230, 235, 240, and 245 °C and bed temperatures of 60, 70, and 80 °C were evaluated. The same 15% triangular infill, build-plate strategy, and adhesion aids used for the HDPE trials were applied. Cooling conditions were adjusted during exploratory trials; the final successful P-T configuration was printed without forced part cooling, under ambient cooling conditions. The corresponding parameters evaluated for the recycled PP filaments are summarized in Table 8.
Table 8. Printing parameters evaluated for recycled PP filaments.
Printing trials were repeated during the exploratory assessment. For configurations that ultimately yielded completed specimens, at least three printing attempts were performed. However, complete records of the outcomes of individual attempts under identical final configurations were not retained. Consequently, configuration-specific success rates and printing reproducibility could not be quantitatively established.
Manual feeding assistance was not used for the evaluated HDPE streams or for P-W and P-B. P-T required manual assistance during filament feeding because of its greater filament dimensional irregularity and associated feeding instability. Accordingly, the successful P-T classification refers to successful specimen fabrication under the evaluated printing configuration with assisted filament feeding and should not be interpreted as fully autonomous filament feeding. The frequency and duration of manual feeding interventions during the P-T trials were not recorded. Therefore, assisted P-T specimen completion is not directly comparable with the unassisted P-W and P-B outcomes, and it remains unknown whether those streams would have produced complete specimens under equivalent assistance.
Printability was evaluated based on filament-feeding continuity, absence of severe nozzle obstruction, build-plate adhesion, continuity of material deposition, completion of the intended geometry, and absence of severe warping or layer separation.
Printing outcomes were classified as follows:
•
Completed without feeding assistance: The intended specimen geometry was completed without manual intervention in filament feeding, with sufficient deposition continuity and geometric integrity for subsequent handling.
•
Completed with feeding assistance: The intended specimen geometry was completed, but manual intervention was required to maintain filament feeding. This outcome demonstrates assisted specimen fabrication rather than autonomous printability.
•
Partially successful: Printing progressed and substantial portions of the intended geometry were produced, but defects or interruptions prevented consistent completion or acceptable geometric integrity.
•
Unsuccessful: Continuous printing could not be maintained, the intended specimen geometry could not be satisfactorily completed, or severe warping or dimensional distortion prevented a usable printing outcome.
For the Bambu P1S cooling-configuration trials, the available printing outcomes were summarized by feedstock stream and active-fan configuration (Supplementary Table S5). Prints interrupted during the initial layers were recorded as failed, those progressing beyond 50% of the intended geometry without completion were recorded as incomplete, and those reaching full geometric completion were recorded as completed. Because complete records of individual printing attempts were not retained, configuration-specific success rates could not be reliably calculated. These observations supported the qualitative printability assessment but did not establish printing reproducibility. Printing continuity was qualitatively categorized as good when material deposition could be maintained sufficiently to complete the intended geometry; interrupted when deposition progressed but recurrent interruptions prevented consistent completion; and deficient when continuous material deposition could not be maintained adequately during the trial.
Printability classification was based on observed deposition continuity, bed adhesion, specimen completion, and final printed-part quality under the evaluated conditions, rather than the mere production of an individual specimen. For HDPE, printing outcomes were documented across four cooling configurations on the Bambu P1S, using three, two, one, or no active fans. Prints interrupted during the initial layers were classified as failed, whereas prints interrupted after more than 50% completion were classified as incomplete. H-W produced a complete specimen without active fans, while H-R and H-B yielded incomplete prints and H-ST failed under that cooling configuration.
Consequently, mechanically testable specimens obtained during exploratory printing trials were retained for preliminary tensile characterization even when the corresponding feedstock stream did not satisfy the criteria for successful printing under the selected configuration.
HDPE and PP printing outcomes were evaluated separately because the two polymer families were processed using different printer configurations and printing conditions.

2.10. Preliminary Tensile Characterization

Preliminary tensile characterization was conducted on FFF specimens manufactured from H-R, H-W, and P-T recycled filaments. The specimen geometry was based on ASTM D638 Type IV [20], with nominal dimensions of 115 mm overall length, 19 mm maximum width, 6 mm reduced-section width, and 3.4 mm main-body thickness. The printing configurations evaluated in this study are described in Section 2.9.
The available laboratory records comprised five tensile-test groups: one for H-R and two each for H-W and P-T, with two or three specimens per group. The two H-W and P-T groups were designated Group 1 and Group 2 solely to distinguish their reported mechanical results, as their correspondence to specific printing stages, extrusion runs, or printing configurations could not be established from the retained records. Mechanically testable specimens were also obtained from H-R, although deformation and process instability prevented this stream from consistently meeting the final printability criteria. Tensile testing was performed using a Shimadzu Autograph AGS-J universal testing machine (Shimadzu Corporation, Kyoto, Japan) equipped with the manufacturer-supplied 5 kN load cell and grips. Tests were controlled using TRAPEZIUM 2 software, Version 2.22c (Shimadzu Corporation). A crosshead speed of 25 mm/min was applied, and testing continued until specimen failure. The specimen-specific reference lengths of 35 or 40 mm were used to calculate percentage elongation. The reported values were derived from crosshead displacement at maximum load rather than from extensometer measurements. Accordingly, these values represent nominal displacement-based elongation at maximum load and should not be interpreted as local material strain or elongation at fracture.
Before testing, the width and thickness of each specimen were measured individually using a Mitutoyo vernier caliper with a measurement range of 0–150 mm. The initial cross-sectional area, A 0 , used for the stress calculation, was determined individually for each specimen as the product of the measured width and thickness. The specimen-specific cross-sectional areas used in the original laboratory calculations are reported in Supplementary Table S10.
Engineering tensile stress was calculated as:
σ = F A 0
where σ is the engineering tensile stress, F is the applied tensile load, and A 0 is the individually determined initial cross-sectional area. Because the printed specimens contained 15% triangular infill, tensile stress was calculated using the measured external width and thickness rather than the effective load-bearing polymer area. Accordingly, the reported maximum tensile stress represents the apparent strength of the printed structures and should not be interpreted as the intrinsic tensile strength of the solid polymer. Complete specimen-linked force–displacement curves and verified fracture locations within the gauge section were not retained in the available records.
Crosshead-displacement-based percentage elongation was calculated as:
E l o n g a t i o n i     ( % ) = Δ L i , m a x L 0 , i × 100
where Δ L i , m a x is the crosshead displacement recorded at maximum load relative to the zeroed initial position and L 0 , i is the specimen-specific reference length used to calculate percentage elongation for specimen i, corresponding to either 35 or 40 mm, as reported by the testing laboratory. Because elongation was derived from crosshead displacement rather than from an extensometer, the reported elongation values should be interpreted as crosshead-displacement-based percentage elongation rather than as extensometer-measured strain. For each experimental group, the laboratory retained individual tensile stress and percentage elongation values, and calculated group means and standard deviations for descriptive comparison. No ANOVA, t-tests, significance groupings, or claims of statistical superiority were applied because of the limited number of specimens and incomplete specimen-level processing traceability.
As supplementary post-test characterization, the geometric apparent density of eight sections obtained from previously tensile-tested specimens (H-R, n = 3; H-W, n = 3; and P-T, n = 2) was estimated from each section’s measured mass and external geometric volume. Recovered or reassembled whole-specimen masses were documented separately and were not used in the density calculation. The section-level measurements are reported in Supplementary Table S9.

2.11. Low-Magnification SEM Examination of Tensile-Generated Fracture Surfaces

Fracture surfaces generated during tensile testing were examined by SEM to qualitatively characterize the printed mesostructure and fracture morphology of selected FFF specimens manufactured from post-consumer recycled HDPE and PP filaments. The analysis focused on preserving the tensile-generated fracture surfaces so that deposited-road architecture and fracture-related features could be examined without grinding or polishing of the region of interest.
Selected fractured specimens from the H-W, H-R, and P-T mechanically tested groups were examined using a ZEISS EVO 10 scanning electron microscope. The specimens were positioned to provide a direct view of the tensile-generated fracture region and deposited-road architecture. Where trimming was required for specimen mounting, material was removed away from the fracture surface to avoid altering the region of interest.
The retained SEM records identified the feedstock streams (H-W, H-R, and P-T), but did not provide unique specimen identifiers or a verifiable correspondence with the individual tensile-test sets. Consequently, the SEM observations were interpreted qualitatively and were not linked to individual tensile-test measurements.
Low-magnification overview images were acquired at 15–18× to document the overall FFF mesostructure and tensile-generated fracture configuration. The images retained for qualitative comparison were acquired at an accelerating voltage of 20.0 kV using the BSD1 backscattered-electron detector under variable-pressure conditions. The working distance ranged from 17.34 to 28.85 mm depending on specimen positioning. Scale bars of 500 µm or 1 mm were used according to the field of view.
The SEM assessment was qualitative and focused on specimen-scale features visible in the retained micrographs, including deposited-road arrangement, local continuity and separation between adjacent deposited roads, locally open or void-like regions, irregular deformation, filamentary or stretched material, and the apparent fracture path. Observations from H-W, H-R, and P-T fracture surfaces were considered alongside the preliminary tensile findings at the feedstock level only, because individual micrographs could not be linked to specific tensile-test specimens. No intact, untested cross-sections were available for a matched comparison.
Because the SEM analysis was intended as a qualitative examination of FFF mesostructure and tensile-generated fracture morphology, the micrographs were not used to quantify bulk porosity or interlayer bonding strength. Likewise, SEM observations were not interpreted as direct evidence of changes in molecular weight, rheological behavior, crystallinity, oxidation, or chemical degradation.

2.12. Statistical Analysis

Statistical analyses followed the hierarchical organization of the experimental data. Each extrusion run, defined by a unique combination of feedstock stream, batch, and processing condition, was considered the experimental unit. The 35 sequential diameter measurements within each RunID were treated as temporal subsamples and summarized using the run-level indicators described in Section 2.8.
Statistical inference was performed at a significance level of α = 0.05. Effect estimates were interpreted with 95% confidence intervals, emphasizing effect magnitude and uncertainty rather than p-values alone.

2.12.1. ATR-FTIR Analysis

ATR-FTIR spectra were analyzed descriptively and using exploratory multivariate methods. For each feedstock stream, replicate spectra were used to evaluate within-stream repeatability. Pairwise Pearson correlation coefficients were calculated among the preprocessed replicate spectra. Between-stream spectral similarity was assessed using Pearson correlation coefficients calculated between the stream-averaged preprocessed spectra.
Principal component analysis (PCA) was applied to the 27 preprocessed replicate spectra to explore grouping according to polymer family and feedstock stream. PCA was used as an exploratory visualization method.
Spectral grouping was interpreted only as evidence of differences in the measured spectral profiles and not as direct evidence of differences in molecular weight, viscosity, crystallinity, oxidation, degradation, or other physicochemical properties that were not independently measured.

2.12.2. HDPE Filament-Diameter Analysis

For HDPE, the primary run-level responses were mean diameter, absolute target error, within-run standard deviation, and coefficient of variation. Standard deviation and coefficient of variation were log-transformed when needed to improve model behavior.
The primary HDPE model was:
Y = S t r e a m + T + E + S + T : E + T : S + E : S + S t r e a m : T + S t r e a m : E + S t r e a m : S + B a t c h
where T is extrusion temperature, E is screw speed, S is spooler speed, and Batch represents the experimental block.
Temperature, screw speed, and spooler speed were treated as categorical factors. Two-factor interactions were included to evaluate dependencies among processing variables and source-specific responses. Batch was included as a fixed blocking factor. The primary model did not include higher-order interactions.
Because the experimental batches were prepared separately within each HDPE feedstock stream, a sensitivity analysis was conducted using an alternative model with stream-specific batch effects (Stream × Batch). Both models were fitted to the same 324 run-level observations using HC3 heteroscedasticity-consistent covariance estimates. The results of this comparison are reported in Supplementary Table S6. Additional marginal contrasts with 95% confidence intervals were calculated to quantify selected processing effects for HDPE and PP (Tables S7 and S8, respectively). Because the chronological order of the extrusion runs was not fully documented, potential serial dependence between successive runs could not be assessed directly.

2.12.3. PP Filament-Diameter Analysis

PP streams were analyzed separately because their absolute temperature ranges were not identical. For each PP stream, the primary model was:
Y = T + S + T : S + B a t c h
where T   represents extrusion temperature, S represents spooler speed, and Batch represents the experimental block. The estimated Wellzoom screw speed of approximately 9 rpm was not included as a model factor because it remained approximately constant throughout the experiments.
The same primary dimensional responses used for HDPE, mean diameter, absolute target error, within-run standard deviation, and coefficient of variation, were evaluated. Percentage within tolerance was retained as a complementary descriptive indicator of dimensional performance.

2.12.4. Robust Estimation and Type III Tests

Residual Q–Q plots and residual-versus-fitted plots were examined to assess approximate residual normality and variance behavior. Because unequal residual variance was observed across the experimental data, final inference for the run-level regression models was based on HC3 heteroscedasticity-consistent covariance estimates.
The HC3 estimator addresses heteroscedasticity in the run-level errors but does not, by itself, account for possible correlation among successive extrusion runs or runs within the same material batch.
Type III omnibus tests were calculated using sum-to-zero contrasts and HC3 heteroscedasticity-consistent covariance estimates. Four run-level responses were examined: mean filament diameter and absolute target error to assess proximity to the nominal target, and within-run SD and CV to characterize absolute and relative dimensional variability, respectively. The main processing questions concerned the associations between extrusion settings and diameter-related performance, while interactions and stream-specific effects were also examined. Tables S1–S4 report the resulting F statistics and nominal p-values. Adjusted marginal means and 95% confidence intervals are reported where available. Because multiple responses, factor effects, and interactions were evaluated without adjustment for multiple testing, the statistical findings were interpreted as exploratory. In particular, p-values close to 0.05 were not considered conclusive in isolation.

2.12.5. Printability and Mechanical Data Analysis

Printability outcomes were summarized descriptively as completed without feeding assistance, completed with feeding assistance, partially successful, or unsuccessful, and interpreted in relation to filament dimensional performance and processing conditions. Because only two or three tensile specimens were available per material group, mechanical results were treated as preliminary descriptive evidence. Individual observations, group means, and measures of dispersion were reported for maximum tensile stress and crosshead-displacement-based percentage elongation. No ANOVA, t-tests, or statistical significance groupings were applied to the tensile data.

2.13. Data Processing and Software

Experimental data were organized in structured spreadsheets according to feedstock stream, batch, extrusion conditions, and measurement sequence. Each extrusion run was assigned a unique RunID, and the 35 sequential diameter measurements within each run were indexed using a TimeIndex to preserve their longitudinal order.
Initial data organization and quality-control procedures were performed using Microsoft Excel. IBM SPSS Statistics, version 30.0.0.0, was used during initial exploratory analysis and data verification. The final run-level statistical analyses reported in the manuscript were performed using Python 3.13.5.
Ordinary least-squares models, Type III factorial tests, HC3 heteroscedasticity-consistent covariance estimates, and adjusted marginal means were calculated using Statsmodels 0.14.6, with NumPy 2.3.5, SciPy 1.17.0, and Patsy 1.0.2 supporting numerical operations and model-matrix construction.
ATR-FTIR spectral preprocessing, including transmittance-to-absorbance conversion where required, interpolation to the common spectral grid, AsLS baseline correction, exclusion of atmospheric CO2 regions, unit-vector normalization, Pearson-correlation analysis, and exploratory PCA, was performed using Python-based computational scripts. The original ATR-FTIR spectra (n = 27), spectral quality-control results (Figure S1), and the corresponding correlation and PCA results are provided as Supplementary Data. The spectral preprocessing procedure is described in Section 2.4.2.

3. Results

The experimental results are presented in the order of feedstock identification to functional filament performance. ATR-FTIR characterization first supported the identification of predominant polymer families and evaluated spectral variability among source-segregated streams. Filament extrusion was then assessed for overall diameter, run-level dimensional stability, and the effects of processing conditions. Finally, the study examined the relationship between filament quality and functional performance through printability trials and preliminary tensile characterization.

3.1. Feedstock Traceability

The experimental study included eight source-segregated post-consumer streams: four HDPE streams (H-R, H-W, H-B, and H-ST) and four PP streams (P-W, P-B, P-R, and P-T). ATR-FTIR characterized all eight streams, yielding 27 spectra. The P-R stream was retained for spectroscopic characterization but did not progress to extrusion because the recovered material was insufficient to prepare an experimental extrusion batch.
Seven streams therefore entered the extrusion stage. Each of the four HDPE streams comprised 81 extrusion runs, whereas each of the three PP streams comprised 27 runs, resulting in a total of 405 extrusion runs. In both polymer families, the evaluated processing conditions were replicated across three experimental batches. Each run contributed 35 sequential diameter measurements for subsequent run-level dimensional analysis. The resulting experimental coverage of the eight source-segregated streams across ATR-FTIR characterization, batching, and extrusion is summarized in Table 9.
Table 9. Experimental coverage of the source-segregated post-consumer streams.
This distribution preserved source identity throughout the analytical workflow and provided the basis for the subsequent comparison of chemical identity, extrusion behavior, dimensional stability, and printability.

3.2. ATR-FTIR Identification of HDPE and PP Streams

ATR-FTIR analysis supported the identification of predominant PE- and PP-based matrices in the eight source-segregated post-consumer streams. The HDPE designation was based on resin identification codes and feedstock origin; ATR-FTIR alone cannot distinguish HDPE from other polyethylene grades or exclude PE-rich mixtures. The available dataset comprised 27 spectra, including 12 HDPE spectra from H-R, H-W, H-B, and H-ST and 15 PP spectra from P-W, P-B, P-R, and P-T. The stream-averaged baseline-corrected ATR-FTIR spectra used for graphical comparison are presented in Figure 2.

3.2.1. HDPE Streams

The mean spectra of H-R, H-W, H-B, and H-ST exhibited a common PE fingerprint. The principal C–H stretching bands were consistently observed at approximately 2918 cm−1 and 2849 cm−1. In the fingerprint region, CH2 deformation features occurred within approximately 1473–1462 cm−1, while the characteristic PE rocking doublet was detected near 730 and 719–720 cm−1. These features were present in all four HDPE streams despite differences in relative band intensity among the source materials. An additional broad feature around 1100 cm−1 was observed in selected HDPE stream spectra. Because this feature was not consistently present across all HDPE streams and no complementary compositional analysis was performed, no specific chemical assignment was made.
Accordingly, the combined occurrence of these characteristic bands supported the classification of H-R, H-W, H-B, and H-ST as materials with a predominant PE-based matrix compatible with HDPE, as shown in Figure 2a.

3.2.2. PP Streams

The mean spectra of P-W, P-B, P-R, and P-T showed the characteristic PP fingerprint. C–H stretching bands were observed at approximately 2950–2953 cm−1 and 2918–2920 cm−1, together with weaker features within approximately 2866–2869 cm−1 and 2837–2840 cm−1. Additional characteristic bands were identified at approximately 1458–1459 cm−1 and 1376 cm−1, while the fingerprint region contained features near 1166–1167, 997–998, 973, and 841 cm−1.
The combined occurrence of these bands supported the classification of P-W, P-B, P-R, and P-T as materials with a predominant PP-based matrix, as shown in Figure 2b. P-R was therefore spectroscopically identified as PP even though this stream did not subsequently enter the extrusion experiments because insufficient material was available. The principal ATR-FTIR absorption regions observed for both polymer families are summarized in Table 10.
Table 10. Characteristic ATR-FTIR bands observed in the source-segregated HDPE and PP streams.

3.3. Spectral Repeatability and Exploratory Grouping

The replicate spectra showed high within-stream repeatability after consistent preprocessing. Mean pairwise Pearson correlation coefficients ranged from 0.924 to 0.998 across the eight feedstock streams, indicating that the characteristic spectral profiles were reproducible within each source-segregated stream.
Comparison of the stream-averaged preprocessed spectra showed greater similarity within each polymer family than between HDPE and PP. Pairwise correlations among the HDPE stream means ranged from 0.952 to 0.991, whereas correlations among the PP stream means ranged from 0.827 to 0.960. Correlations between HDPE and PP stream means were lower, ranging from 0.501 to 0.698. The similarity matrix therefore preserved the principal distinction between the two polymer families while also revealing measurable spectral variation among streams assigned to the same nominal polymer family.
Exploratory principal component analysis showed the same overall pattern. PC1 accounted for 71.8% of the total spectral variance and provided the principal separation between the HDPE and PP spectra, while PC2 accounted for an additional 10.7%. Together, the first two principal components explained 82.5% of the total spectral variance.
These differences were interpreted only as variation in the measured ATR-FTIR profiles. They do not independently demonstrate differences in molecular weight, melt viscosity, crystallinity, oxidation, degradation, or other physicochemical properties that were not directly measured in this study. Accordingly, the correlation and PCA results were used for comparative spectral characterization rather than for inference of unmeasured material properties.
The between-stream spectral relationships and exploratory multivariate grouping are presented in Figure 3 through the spectral-similarity matrix and PCA score plot, respectively.
Figure 3. Exploratory comparison of the preprocessed ATR-FTIR spectra: (a) Pearson correlation matrix calculated between the stream-averaged preprocessed spectra of H-R, H-W, H-B, H-ST, P-W, P-B, P-R, and P-T; and (b) PCA score plot of the 27 preprocessed replicate spectra showing their distribution according to polymer family and feedstock stream. PC1 and PC2 accounted for 71.8% and 10.7% of the total spectral variance, respectively, explaining 82.5% cumulatively.

3.4. Overall Filament Diameter

Filament diameter was evaluated from 14,175 sequential measurements, comprising 11,340 HDPE measurements and 2835 PP measurements. Each HDPE stream contributed 2835 observations, whereas each extruded PP stream contributed 945 observations. These measurements originated from the 35 sequential observations retained for each extrusion run across the three experimental batches.
At the observation level, the four HDPE streams exhibited mean diameters close to the nominal 1.75 mm target. H-W showed the closest overall mean at 1.751 mm, followed by H-B (1.770 mm), H-R (1.773 mm), and H-ST (1.793 mm). The pooled HDPE mean was 1.772 mm. In contrast, the PP streams exhibited greater departures from the nominal target. P-B presented the closest PP mean at 1.706 mm, whereas P-T and P-W averaged 1.515 mm and 1.444 mm, respectively. The pooled PP mean was 1.555 mm. These overall means are consistent with the grand-total values reported from the experimental dataset.
The dispersion of the pooled measurements also differed between the polymer families. Overall standard deviations for the HDPE streams ranged from 0.119 to 0.162 mm, compared with 0.245 to 0.308 mm for PP. P-T showed the widest observed diameter range, from 0.60 to 2.37 mm, while P-B ranged from 1.12 to 2.65 mm. Among the HDPE streams, H-W and H-B showed the lowest pooled standard deviations. The overall descriptive statistics for filament diameter across the seven extruded streams are summarized in Table 11. The corresponding filament-diameter distributions and their relationship to the nominal 1.75 mm target are shown in Figure 4.
Table 11. Overall descriptive statistics of filament diameter for the seven extruded post-consumer streams.
Figure 4. Distribution of filament diameter measurements for H-R, H-W, H-B, H-ST, P-W, P-B, and P-T. The horizontal reference line indicates the nominal filament diameter of 1.75 mm, with the 1.73– 1.77 mm tolerance interval indicated around the target. The vertical dotted line separates the HDPE streams (left) from the PP streams (right).
Importantly, the standard deviations reported in Table 11 represent the pooled variability across all processing conditions and batches within each stream. They therefore incorporate both within-run fluctuations and differences among extrusion conditions. Consequently, proximity of the overall mean to 1.75 mm should not be interpreted as evidence of stable extrusion by itself. The longitudinal behavior of individual extrusion runs is evaluated separately in Section 3.5 using the run-level dimensional indicators defined in Section 2.8.

3.5. Run-Level Dimensional Stability

Run-level analysis provided a different assessment of filament quality from the pooled descriptive statistics because each extrusion run was treated as the experimental unit and its 35 sequential measurements were summarized independently. The indicators therefore distinguished proximity to the nominal diameter from short-term dimensional stability and continuity.
Across the HDPE streams, the average within-run standard deviation ranged from 0.041 to 0.070 mm, with corresponding coefficients of variation between 2.33% and 3.99%. H-W exhibited the lowest average within-run variability, followed by H-ST and H-B, whereas H-R showed the greatest variability among the HDPE streams. The average absolute deviation of the run mean from the 1.75 mm target ranged from approximately 0.096 to 0.122 mm.
The PP streams showed substantially greater run-level instability. Average within-run standard deviations were 0.080 mm for P-W, 0.110 mm for P-B, and 0.212 mm for P-T, corresponding to coefficients of variation of 5.71%, 6.48%, and 14.43%, respectively. Although P-B had the mean diameter closest to the nominal target among the PP streams, its average absolute target error remained 0.218 mm, while P-W and P-T presented average errors of 0.329 and 0.260 mm, respectively. The run-level dimensional indicators for each extruded feedstock stream are summarized in Table 12.
Table 12. Run-level dimensional indicators summarized across all evaluated extrusion conditions and experimental batches for each extruded feedstock stream.
The percentages within the predefined dimensional screening interval reported in Table 12 summarize all evaluated extrusion conditions and experimental batches for each feedstock stream. Each HDPE stream contributed 81 extrusion runs, whereas each extruded PP stream contributed 27 runs, with 35 sequential diameter measurements per run. Across these screening conditions, H-W exhibited the highest average percentage of measurements within the interval (12.4%), whereas the PP streams ranged from 1.9% to 6.0%. These values characterize the complete extrusion-screening dataset and should not be interpreted as tolerance percentages for the selected filament-production conditions or for the filament segments subsequently used in FFF printing. Thus, the predefined interval served as a descriptive dimensional indicator rather than a standalone criterion of functional printability. A comparison of individual runs further illustrates the limitation of using mean diameter alone. One representative H-W run had a mean diameter of 1.743 mm, a within-run SD of only 0.012 mm, a CV of 0.68%, and 91.4% of its measurements within the predefined tolerance. In contrast, a representative P-T run produced a nearly nominal mean diameter of 1.758 mm but exhibited an SD of 0.176 mm, a CV of 10.01%, and only 8.6% of measurements within tolerance. In the latter case, 32 of the 35 measurements were outside the tolerance interval. Representative longitudinal diameter profiles illustrating this contrast between similar mean diameter and markedly different within-run stability are shown in Figure 5.
Figure 5. Representative sequential filament-diameter profiles from the factorial extrusion-screening experiments, illustrating differences in short-window dimensional variability between selected H-W and P-T screening runs. These profiles were chosen to illustrate contrasting diameter behavior and do not represent confirmed measurements of the specific filament segments subsequently used to manufacture the tensile specimens. The solid horizontal line indicates the nominal target of 1.75 mm, and the shaded region represents the study-specific screening interval of 1.73–1.77 mm.
The runs shown in Figure 5 were selected to illustrate contrasting short-term diameter variability at similar mean diameters rather than to represent the extrusion conditions selected for the completed printing trials. Figure 5a corresponds to H-W, Batch B, at 190 °C, 6 rpm, and 0.36 m/min, whereas Figure 5b corresponds to P-T, Batch B, at 170 °C, approximately 9 rpm, and 0.52 m/min. These examples differ from the selected extrusion conditions subsequently used for specimen fabrication.
This contrast demonstrates that a filament can present a mean diameter close to 1.75 mm while remaining highly variable longitudinally. Accordingly, mean diameter, within-run variability, absolute target error, and percentage within tolerance were considered jointly in the subsequent assessment of processing effects and printability. These run-level indicators provided a more complete assessment of dimensional performance than pooled or mean diameter values alone.
The observed dimensional differences reflect the behavior of each recovered feedstock stream under its respective extrusion system and processing conditions. Because HDPE and PP were processed using different extruders, these differences cannot be attributed solely to polymer-family characteristics.
The complementary micrometer measurements of retained filament segments revealed differences in both longitudinal diameter variation and cross-sectional dimensional asymmetry (Table S11). Mean diameters were 1.669 mm for the H-R segment, 1.380 mm for transparent PP, and 1.884 mm for white HDPE, with corresponding between-position standard deviations of 0.037, 0.130, and 0.057 mm. The mean absolute differences between perpendicular diameter measurements were 0.030, 0.063, and 0.114 mm, respectively. These results document dimensional variation and two-axis asymmetry in the preserved filament segments. However, because their correspondence to individual extrusion runs was not established, the measurements were not used to recalibrate or retrospectively validate the original spooler-based diameter dataset.

3.6. Processing Effects in HDPE

The run-level analysis showed that HDPE filament diameter was strongly associated with the extrusion conditions, with screw rotational speed producing the largest change in mean diameter. The HC3-robust Type III model identified significant effects of feedstock stream (p < 0.001), extrusion temperature (p = 0.003), and screw speed (p < 0.001) on mean filament diameter. In contrast, spooler speed had no significant overall effect (p = 0.135). The analysis used 324 HDPE extrusion runs, with temperature, screw speed, and spooler speed treated as categorical factors and batch included as a fixed blocking factor.
Tables S1 and S2 of the Supplementary Materials provide complete HC3-robust Type III model results for the prespecified HDPE responses, including the main effects, two-factor interactions, and batch blocking term.
Screw rotational speed produced the clearest overall effect. The adjusted mean filament diameter increased from 1.634 mm at 4 rpm to 1.798 mm at 6 rpm and 1.883 mm at 8 rpm. The corresponding 95% confidence intervals were 1.621–1.647 mm, 1.786–1.810 mm, and 1.869–1.898 mm, respectively. The intermediate screw speed of 6 rpm produced the lowest mean absolute target error and the highest proportion of measurements within the predefined 1.73–1.77 mm tolerance interval. The adjusted mean diameter and associated dimensional-performance indicators for the three screw-speed levels are summarized in Table 13.
Table 13. Effect of screw rotational speed on HDPE filament diameter and dimensional performance.
Screw speed had a significant overall effect on absolute target error (p < 0.001). However, significant feedstock stream × screw speed (p < 0.001) and extrusion temperature × screw speed (p = 0.004) interactions were also identified (Table S1). These interactions indicate that the absolute-error response to screw speed was not uniform across the evaluated material sources and processing temperatures. For the 6-versus-4 rpm contrast, the reduction in absolute target error was −0.102 mm for H-W (95% CI: −0.130 to −0.074 mm), compared with −0.028 mm for H-ST (95% CI: −0.056 to 0.00007 mm). At 200 °C, the corresponding contrast was −0.027 mm (95% CI: −0.052 to −0.003 mm; Table S7). Consequently, the pooled advantage observed at 6 rpm should be interpreted as an overall experimental trend rather than as a universally optimal operating condition.
Screw speed also had a significant effect on log-transformed within-run standard deviation (p = 0.001), whereas its effect on log-transformed coefficient of variation was not statistically significant (p = 0.258; Table S2). This distinction indicates that evidence of screw-speed-related differences in absolute diameter variability does not necessarily extend to relative variability, particularly because mean filament diameter also changed substantially with screw speed. Therefore, the results do not establish a consistent improvement in relative longitudinal stability at 6 rpm. Extrusion temperature had a smaller but statistically significant overall effect on mean diameter. A significant stream × temperature interaction was observed (p = 0.004), indicating that the temperature response differed among the four HDPE feedstock streams. This result supports evaluating temperature effects in relation to the specific source-segregated stream rather than defining a single temperature optimum for all recycled HDPE feedstocks.
By comparison, spooler speed produced relatively small differences in the overall adjusted mean diameter, and its main effect was not statistically significant. None of the two-factor interactions involving spooler speed showed a comparable influence on mean diameter.
Among the evaluated HDPE conditions, the combination subsequently selected for successful H-W printing (190 °C, 6 rpm, and 0.34 m/min) showed consistent behavior across the three experimental batches. The corresponding run means were 1.751, 1.759, and 1.743 mm, with within-run standard deviations of 0.040, 0.043, and 0.034 mm, respectively. This condition combined proximity to the nominal diameter with comparatively low longitudinal variability and was therefore advanced to the functional printability assessment. The principal HDPE processing effects, including the overall screw-speed response and the stream-specific temperature behavior, are illustrated in Figure 6.
Figure 6. Processing effects on HDPE filament diameter: (a) adjusted mean diameter according to screw rotational speed with 95% confidence intervals; and (b) mean diameter according to extrusion temperature for H-R, H-W, H-B, and H-ST, illustrating the significant stream × temperature interaction.
The sensitivity analysis incorporating stream-specific batch effects supported the robustness of the principal screw-speed findings (Table S6). Screw speed remained significantly associated with mean filament diameter and absolute target error (both p < 0.001), as well as log-transformed within-run SD (p < 0.001), but not log-transformed CV (p = 0.234). The stream × screw-speed and temperature × screw-speed interactions for absolute target error also remained significant.
The Stream × Batch interaction was also significant for mean diameter (p < 0.001), absolute target error (p = 0.002), log-transformed within-run SD (p = 0.001), and log-transformed within-run CV (p = 0.002) (Table S6). These findings indicate that batch-related variation differed among the HDPE feedstock streams, reinforcing the importance of accounting for stream-specific batch effects when interpreting the processing responses.
In the supplementary marginal contrasts, 6 rpm showed a lower pooled mean absolute target error than 4 rpm (difference: −0.060 mm; 95% CI: −0.074 to −0.045 mm) and 8 rpm (difference: −0.078 mm; 95% CI: −0.092 to −0.064 mm). However, stream-specific differences and the significant interactions indicate that 6 rpm should not be interpreted as a universally optimal setting. The corresponding contrasts are reported in Table S7.

3.7. Processing Effects in PP

Because the PP streams were evaluated over different absolute temperature ranges, processing effects were analyzed separately for P-W, P-B, and P-T. P-W and P-B were evaluated at 180, 190, and 200 °C, whereas P-T was evaluated at 170, 180, and 190 °C. The Wellzoom screw speed remained approximately constant at 9 rpm; therefore, extrusion temperature and spooler speed were the processing factors included in the within-stream models.
Complete HC3-robust Type III model results for the PP responses, including temperature, spooler speed, their interaction, and the Batch blocking term, are provided in Tables S3 and S4 of the Supplementary Materials.
Within-stream HC3-robust Type III analyses identified a significant spooler-speed effect on mean filament diameter for P-W (p < 0.001) and P-B (p < 0.001), with a smaller but still significant effect for P-T (p = 0.030).
The spooler-speed effect observed for P-T (nominal p = 0.030) should be interpreted cautiously because multiple stream-specific responses and model terms were examined without adjustment for multiple testing.
Increasing spooler speed consistently reduced the estimated mean filament diameter in all three PP streams. For P-W, the mean diameter decreased from 1.672 mm at 0.36 m/min to 1.435 mm at 0.42 m/min and 1.227 mm at 0.52 m/min. P-B showed a similar response, decreasing from 1.988 to 1.647 and 1.483 mm, respectively. For P-T, the corresponding estimated means were 1.664, 1.560, and 1.323 mm. The estimated mean filament diameters according to spooler speed are summarized in Table 14. HC3-robust spooler-speed contrasts with 95% confidence intervals for the individual PP streams are provided in Supplementary Table S8.
Table 14. Estimated mean filament diameter according to spooler speed for the three PP streams.
Temperature effects were less uniform among the PP streams. Because P-T was processed over a temperature range 10 °C lower than that used for P-W and P-B, absolute temperature levels were not interpreted as directly equivalent across all three streams. The results therefore did not support defining a single common extrusion temperature as optimal for all recycled PP feedstocks.
The lowest spooler speed, 0.36 m/min, generally produced mean diameters closest to the nominal 1.75 mm target. However, proximity to the target did not necessarily correspond to low longitudinal variability. This distinction was particularly evident for P-T. The condition subsequently selected for successful P-T printing (180 °C and 0.36 m/min at approximately 9 rpm) produced run means of 1.686, 1.806, and 1.575 mm across the three batches, with corresponding within-run standard deviations of 0.149, 0.197, and 0.126 mm.
The inverse relationship between spooler speed and filament diameter for the three PP streams is illustrated in Figure 7. These results indicate that spooler speed was the most consistent processing factor associated with PP filament diameter under the evaluated Wellzoom extrusion conditions.
Figure 7. Run-level mean filament diameter as a function of spooler speed for the P-W, P-B, and P-T streams. Markers represent the averages of extrusion-run mean diameters at each speed, and error bars indicate the 95% confidence intervals displayed in the plot. The dashed horizontal line denotes the nominal diameter target of 1.75 mm, whereas the dotted lines indicate the predefined 1.73–1.77 mm dimensional screening interval.

3.8. Printability Outcomes

Printability outcomes differed among the seven extruded feedstock streams. Under the selected final printing configurations, H-W produced complete specimens without manual filament-feeding assistance, whereas P-T produced complete specimens with manual feeding assistance. These outcomes were therefore distinguished as autonomous and assisted specimen fabrication, respectively, rather than treated as equivalent demonstrations of printability. H-B showed partial printability, whereas H-R, H-ST, P-W, and P-B did not consistently satisfy the final printability criteria under the evaluated conditions. Among the HDPE streams, H-W exhibited high bed adhesion and good printing continuity and was classified as successful. H-B showed medium adhesion but interrupted deposition, allowing the printing process to progress without consistently completing the specimen and was therefore classified as partially successful. H-R exhibited medium adhesion but deficient continuity, whereas H-ST showed both low adhesion and deficient continuity; both were classified as unsuccessful.
During the broader exploratory printing trials, mechanically testable specimens could nevertheless be recovered from some streams ultimately classified as unsuccessful. These specimens generally exhibited substantial deformation or other print-quality deficiencies and were therefore not considered evidence of successful or reproducible printability. The final printability classification, bed-adhesion behavior, and printing continuity of each extruded stream are summarized in Table 15.
Table 15. Printability outcomes of the recycled HDPE and PP filament streams, distinguishing autonomous and assisted specimen fabrication.
Cooling configuration influenced the observed printing outcomes of the HDPE streams on the Bambu P1S. As summarized in Supplementary Table S5, all four HDPE streams exhibited printing failure during the initial layers when three, two, or one cooling fans were active. With all cooling fans disabled, H-W completed the intended specimen geometry, whereas H-R and H-B progressed beyond 50% of the print but remained incomplete. H-ST continued to exhibit printing failure. These observations highlight the importance of cooling configuration for the investigated recycled HDPE streams. The successful H-W specimens were produced using filament extruded at 190 °C, 6 rpm, and 0.34 m/min. Printing was performed on the Bambu P1S at a nozzle temperature of 235 °C and a bed temperature of 80 °C, using a raft, 15% triangular infill, combined solid and liquid Bambu adhesives, and no active cooling fans.
For PP, P-W and P-B both exhibited low bed adhesion and deficient printing continuity and were classified as unsuccessful. In contrast, P-T achieved medium-to-high bed adhesion and produced complete specimens under the selected printing conditions; however, manual assistance during filament feeding was required. The successful P-T filament corresponded to an extrusion condition of 180 °C, approximately 9 rpm, and 0.36 m/min. Printing was performed using the Ender 3 S1 Pro at 245 °C nozzle temperature and 80 °C bed temperature, with a raft, 15% triangular infill, combined solid and liquid adhesives, and ambient cooling. Accordingly, the P-T outcome is interpreted as successful specimen fabrication under assisted filament feeding rather than fully autonomous printability.
The P-T results were particularly relevant when considered together with the dimensional analysis. Although P-T showed substantially greater run-level diameter variability than H-W, it could still be processed into complete specimens under the selected printing conditions. Conversely, several streams with overall mean diameters closer to the nominal 1.75 mm value did not print successfully. Figure 8 shows representative specimens illustrating the range of observed printability outcomes. These results indicate that mean filament diameter alone did not discriminate printable from non-printable recycled feedstocks; longitudinal stability, feeding continuity, adhesion, and the selected printer configuration also contributed to functional performance. Section 3.11 examines this relationship integratively.
Figure 8. Representative printability outcomes for the recycled filaments: (a) completed H-W specimen, classified as successful; (b) H-B specimen showing partial printability; (c) H-R specimen representative of an unsuccessful HDPE printing outcome; (d) P-B specimen representative of an unsuccessful PP printing outcome; (e) unsuccessful exploratory P-T trial; and (f) completed P-T specimen obtained under the selected printing conditions with manual filament-feeding assistance.

3.9. Preliminary Tensile Performance

Preliminary tensile characterization was performed on mechanically testable specimens manufactured from H-R, H-W, and P-T recycled filaments. Because only two or three specimens were available for each material group, the tensile results were treated as descriptive rather than inferential. Inclusion of a specimen group in the tensile analysis did not imply that the corresponding feedstock stream satisfied the final criteria for successful or reproducible printability. This distinction was particularly relevant for H-R, for which mechanically testable specimens were produced during exploratory trials despite the stream being ultimately classified as unsuccessful because of deformation and process instability.
All percentage-elongation values reported in this section were derived from crosshead displacement at maximum load using specimen-specific reference lengths of either 35 or 40 mm, as written in Section 2.10. Accordingly, these values represent nominal displacement-based elongation at maximum load rather than extensometer-measured strain or elongation at fracture.
Representative photographs of the H-R and P-T specimens before and during tensile testing are shown in Figure 9. The images document the appearance and positioning of the printed Type IV specimens during tensile loading. They provide qualitative documentation of specimen condition and testing configuration and were not used for quantitative strain measurement or fracture-morphology analysis.
Figure 9. Representative photographic documentation of recycled-polymer specimens used for preliminary tensile characterization: (a) P-T PP Type IV specimens produced from the transparent storage container feedstock before tensile testing; (b) H-R HDPE Type IV specimens produced during exploratory printing trials before tensile testing; (c) representative H-R specimen during tensile loading; and (d) representative P-T specimen during tensile loading. The photographs document specimen appearance and testing configuration and were not used to derive quantitative mechanical measurements or fracture-morphology measurements.
For H-R, three mechanically tested specimens exhibited a mean apparent maximum tensile stress of 13.19 ± 1.21 MPa and a mean crosshead-displacement-based elongation at maximum load of 10.50 ± 1.07%. Although mechanically testable specimens were obtained, H-R did not consistently meet the final printability criteria because of deformation and process instability. For H-W, Group 1 (n = 2) exhibited an apparent maximum tensile stress of 10.90 ± 0.81 MPa and elongation of 7.22 ± 0.40%, whereas Group 2 (n = 3) exhibited corresponding values of 11.27 ± 0.65 MPa and 8.38 ± 0.96%.
For P-T, Group 1 (n = 2) exhibited an apparent maximum tensile stress of 11.31 ± 1.00 MPa and elongation of 6.47 ± 0.06%, whereas Group 2 (n = 3) exhibited corresponding values of 15.21 ± 3.07 MPa and 10.64 ± 2.25%. Because the retained records did not establish the processing conditions associated with the individual tensile-test groups, differences between groups were not attributed to specific printing stages or process optimization. The descriptive tensile results for the recycled-polyolefin specimen groups are summarized in Table 16.
Table 16. Preliminary apparent maximum tensile stress, calculated from the measured external cross-sectional area, and crosshead-displacement-based percentage elongation at maximum load for FFF specimens manufactured from recycled polyolefin filaments. Values are presented as mean ± sample standard deviation. Group 1 and Group 2 are reporting labels and do not indicate printing chronology or specific processing conditions.
Across the five recycled-polyolefin specimen groups, mean apparent tensile strength ranged from 10.90 to 15.21 MPa, while mean crosshead-displacement-based elongation at maximum load ranged from 6.47% to 10.64%. Because only two or three specimens were available per group and specimen-level processing traceability was incomplete, these results provide preliminary descriptive evidence of mechanical testability under the evaluated conditions. They do not establish statistically significant differences among feedstock streams or printing configurations, nor can they be generalized to the intrinsic mechanical properties of recycled HDPE or PP.
Supplementary Table S9 additionally reports post-test section-level geometric apparent density measurements for H-R, H-W, and P-T. Because these sections could not be linked to specific tensile-test sets and were obtained after mechanical testing, the measurements were treated as complementary descriptive observations rather than as predictors of tensile performance.
The individual specimen values and corresponding group means are presented in Figure 10 to show the dispersion within each small experimental group without implying statistical significance.
Figure 10. Individual apparent maximum tensile stress and crosshead-displacement-based elongation at maximum load for H-R and the two laboratory result groups of H-W and P-T. Individual measurements are shown together with group means and standard deviations. Group labels do not imply specific printing stages or processing conditions.

3.10. SEM Fracture-Surface Morphology

SEM examination of the tensile-generated fracture surfaces revealed the deposited-road architecture of the FFF specimens and qualitative differences among the evaluated recycled polymer streams (Figure 11). The parallel arrangement of deposited roads remained clearly visible in all specimens, although the continuity of the printed structure and the morphology of the fractured regions differed among materials.
Figure 11. Representative low-magnification SEM images of tensile-generated fracture surfaces of recycled-polyolefin FFF specimens. (a) H-W showing deposited-road architecture; (b) H-W exhibiting localized separation between adjacent deposited roads; (c) H-R showing irregularly deformed material and open regions; and (d) P-T exhibiting deposited roads, localized separations, and filamentary features. Arrows indicate representative morphological features discussed in Section 3.10. Magnification and scale bars are provided in each micrograph.
The two H-W fracture surfaces [Figure 11a,b] exhibited comparatively well-defined and regularly aligned deposited roads over substantial portions of the cross-section. Localized disruption of the surrounding material and separation between adjacent deposited regions were nevertheless observed, particularly near the specimen perimeter and fracture boundaries.
The H-R specimen [Figure 11c] showed a more heterogeneous fracture morphology, with irregularly deformed material, pronounced open regions, and less uniform continuity of the deposited-road structure. The fractured cross-section showed large void-like spaces and locally distorted deposited material.
The P-T specimen [Figure 11d] also retained a clearly recognizable deposited-road architecture but exhibited localized inter-road separation, open void-like regions, and filamentary or stretched material spanning portions of the fractured surface. Irregular fracture paths were observed around the perimeter and through the deposited structure.
Overall, the SEM observations revealed the deposited-road architecture characteristic of FFF specimens and local morphological variations within the examined fracture regions. Because the specimens were manufactured with 15% triangular infill, the observed open regions cannot be attributed unambiguously to intentionally unfilled spaces, deposition-related discontinuities, or openings generated or enlarged during tensile fracture. Accordingly, the observations were interpreted qualitatively and were not used to establish specific fracture mechanisms, bulk porosity, inter-road bonding strength, or causal relationships between feedstock source and fracture morphology.

3.11. Integrated Dimensional Stability-Printability Relationship

The factorial extrusion experiments evaluated the effects of processing conditions on the dimensional performance of each source-segregated feedstock stream. Based on the experimental results, a processing-parameter combination was selected for each stream and subsequently used for filament production and FFF printability assessment. Thus, the printing trials represented a subsequent functional evaluation of filaments produced under conditions selected from the experimental design, rather than an independent set of extrusion conditions. While Table 12 summarizes dimensional indicators across the complete factorial design, the dimensional results obtained under the selected conditions provide a more appropriate basis for interpreting the subsequent printability outcomes. Under the selected H-W extrusion condition (190 °C, 6 rpm, and 0.34 m/min), the three experimental batches produced run-mean filament diameters of 1.751, 1.759, and 1.743 mm, with corresponding within-run standard deviations of 0.040, 0.043, and 0.034 mm. For the selected P-T condition (180 °C, approximately 9 rpm, and 0.36 m/min), the corresponding run means were 1.686, 1.806, and 1.575 mm, with within-run standard deviations of 0.149, 0.197, and 0.126 mm. These selected-condition results provide a more appropriate dimensional context for interpreting subsequent printing outcomes than stream-level averages across all extrusion conditions. H-W produced complete specimens without manual feeding assistance, whereas P-T required manual assistance during filament feeding. Nevertheless, the available data do not yet establish which specific experimental run or filament segment was used in each printing attempt.
Conversely, H-B presented an overall mean diameter close to the nominal target (1.770 mm) and lower within-run variability than H-R, but its printing performance remained only partially successful because deposition continuity was interrupted. H-R also exhibited a mean diameter close to the target (1.773 mm) but failed to consistently complete the intended geometry. These observations further demonstrate that a favorable mean diameter alone did not ensure functional filament performance.
Taken together, the results indicate that recycled filament qualification should not be based solely on mean diameter or compliance with a narrow dimensional tolerance. Instead, suitability should be evaluated by considering longitudinal dimensional stability, extrusion continuity, feeding behavior, adhesion performance, and printing configuration together for source-segregated post-consumer HDPE and PP for FFF.
This integrated behavior also reinforces the source-dependent nature of the experimental system. Although the ATR-FTIR spectra were consistent with the predominant PE- and PP-based matrices indicated by the resin identification codes, streams assigned to the same nominal polymer family exhibited different extrusion stability and printability outcomes. Therefore, polymer family identification alone was insufficient to predict functional processing performance. Figure 12 provides a descriptive comparison of dimensional indicators obtained across the extrusion-screening conditions and the qualitative printing outcomes observed in subsequent trials.
Figure 12. Descriptive relationship between run-level dimensional indicators obtained during extrusion screening and qualitative FFF outcomes for the seven recycled-polyolefin feedstock streams. H-W completed printing without feeding assistance, whereas P-T completed printing with manual feeding assistance. Values represent averages across all experimental screening conditions and do not correspond to direct dimensional measurements of the additional filament spools used for specimen fabrication. The comparison is exploratory and does not establish a validated predictive relationship between dimensional performance and printing success.

4. Discussion

4.1. Polymer-Family Identification and Between-Stream Spectral Variability

ATR-FTIR characterization supported the initial classification of the source-segregated feedstocks into HDPE- and PP-based materials. Characteristic PE and PP absorption regions were consistently observed across their respective streams, and exploratory PCA further distinguished the two polymer families. These results indicate that the resin identification codes used during collection broadly matched the predominant polymer matrices observed spectroscopically. For the HDPE-labeled streams, this agreement supports a predominant PE-based matrix consistent with resin identification code 2, but does not independently establish PE density or grade.
Despite this polymer-family consistency, the spectra were not identical across feedstock streams. Replicate similarity varied within both HDPE and PP, and the stream-averaged spectra retained measurable differences within each polymer family. Such variation is plausible for post-consumer materials because products carrying the same nominal resin classification may differ in formulation, pigments, fillers, additives, previous service conditions, surface contamination, and manufacturing history. Differences in ATR contact and surface condition may also contribute to variation in relative band intensity.
Accordingly, the observed spectral differences were interpreted conservatively. ATR-FTIR supported the identification of the predominant polymer family and revealed measurable spectral variation among feedstock streams, but the present analysis cannot determine whether those differences originated from changes in molecular weight, melt viscosity, crystallinity, oxidation state, or degradation. Determining those properties would require complementary characterization, such as melt flow measurements, thermal analysis, or targeted chemical degradation indices. Accordingly, the principal value of ATR-FTIR in the present workflow was polymer-family identification and comparative spectral characterization rather than direct prediction of processing behavior.

4.2. Chemical Similarity Does Not Imply Equivalent Processability

The processing results show that confirming a common polymer family does not imply equivalent extrusion behavior. Although H-R, H-W, H-B, and H-ST exhibited HDPE-compatible FTIR fingerprints, their dimensional stability and printability differed substantially. A similar pattern was observed among the PP streams. This indicates that source-specific characteristics retained after consumer use and recycling can remain relevant even when the predominant polymer chemistry is nominally the same.
From a recycling perspective, this finding suggests that resin-code segregation alone may not provide sufficiently uniform feedstock for applications that require controlled melt processing. Maintaining source identity, when operationally feasible, can provide an additional level of process control because materials derived from different products may contain different grades, additive packages, pigments, fillers, and prior thermal or environmental histories.
However, because MFI/MFR, DSC, molecular-weight distribution, and additive composition were not independently measured, the present results cannot identify which material property caused the observed source-dependent behavior. The extrusion differences therefore demonstrate that the specific source-segregated streams evaluated in this study did not exhibit equivalent processing behavior, while the underlying rheological or compositional causes remain unresolved.

4.3. Processing Control of Filament Diameter in the HDPE and PP Systems

The extrusion experiments showed that the processing variable most strongly associated with filament diameter differed between the HDPE and PP systems. For HDPE, screw rotational speed was the dominant factor, whereas for PP, spooler speed produced the clearest and most consistent diameter response.
For HDPE, screw rotational speed produced the largest overall change in mean filament diameter. The intermediate setting of 6 rpm yielded the lowest pooled mean absolute target error and the highest pooled percentage of measurements within the predefined dimensional screening interval among the evaluated screw-speed levels. Nevertheless, significant feedstock stream × screw speed and extrusion temperature × screw speed interactions for absolute target error indicate that this overall result cannot be generalized to every material source or temperature combination. Furthermore, screw speed significantly affected absolute within-run variability, expressed as SD, but its effect on relative variability, expressed as CV, was not statistically significant. These findings support evaluating screw-speed settings in relation to the specific feedstock and processing conditions rather than assuming a single optimal setting for all recycled HDPE streams. The observed dependence on processing conditions is consistent with previous studies examining extrusion rate and thermal effects on filament dimensional behavior [21].
For PP, increasing spooler speed consistently reduced filament diameter in all three streams. Mean diameter decreased from 1.672 to 1.227 mm for P-W, from 1.988 to 1.483 mm for P-B, and from 1.664 to 1.323 mm for P-T as spooler speed increased from 0.36 to 0.52 m/min. This behavior is consistent with the drawing effect imposed by the take-up system, where higher spooler speeds can stretch the molten strand and reduce its diameter [9,22].
These differences should not be interpreted solely as intrinsic HDPE–PP behavior because different extrusion systems were used. HDPE was processed with the Felfil Extruder, where screw speed was directly varied, whereas PP was processed with the Wellzoom extruder at an approximately constant maximum screw speed. Therefore, the results are better interpreted as material-, equipment-, and process-specific responses. Overall, the findings support stream-specific processing windows rather than a single extrusion condition for all recycled HDPE or PP feedstocks.

4.4. Mean Diameter Versus Longitudinal Stability

The results showed that mean filament diameter alone was insufficient to describe filament quality. Although several streams presented overall mean diameters close to the nominal 1.75 mm target, their longitudinal behavior differed substantially. This distinction is important for recycled filaments because local diameter fluctuations can affect material feeding and deposition even when the average diameter appears acceptable. Previous studies similarly identify dimensional consistency as a critical requirement for reliable FFF processing [9,22].
The comparison between H-W and P-T illustrates this limitation particularly well. A representative H-W run exhibited a mean diameter of 1.743 mm, an SD of only 0.012 mm, and 91.4% of measurements within the predefined tolerance. In contrast, a P-T run with a similarly near-target mean of 1.758 mm showed an SD of 0.176 mm, with only 8.6% of measurements within tolerance. Thus, similar average diameters could correspond to markedly different levels of longitudinal stability.
This finding supports using complementary indicators such as within-run SD, CV, absolute target error, and percentage within tolerance when evaluating recycled filament. These metrics provide information about both the magnitude of longitudinal dimensional variability and the consistency with which the filament remains near the nominal diameter, rather than relying solely on the average filament diameter.
However, dimensional stability was not the only determinant of printability. P-T ultimately produced complete specimens despite considerably greater diameter variability than H-W. Therefore, longitudinal dimensional stability should be considered an important component of filament qualification, but together with feeding continuity, adhesion behavior, and printing conditions rather than as an isolated acceptance criterion.

4.5. Printability and Observed Failure Modes

The printability trials showed that dimensional performance alone did not determine functional FFF behavior. Feeding continuity, bed adhesion, thermal management, and printer configuration interacted with filament dimensional characteristics to determine whether a specimen could be completed.
The HDPE trials also demonstrated the importance of thermal management. When active cooling was used on the Bambu P1S, the HDPE streams generally failed during the initial printing stages. Disabling the cooling fans under the Bambu P1S conditions evaluated improved printing behavior, allowing H-W to complete the intended geometry. This response is consistent with the known sensitivity of semicrystalline polyolefins to cooling-induced contraction and warping, for which bed temperature, adhesion strategy, and cooling conditions can strongly affect print stability [14,23].
The PP results further showed that greater dimensional variability did not necessarily prevent successful specimen fabrication. P-T exhibited substantially higher within-run variability than H-W but could still produce complete specimens after adjustment of the printing conditions and with manual assistance during filament feeding. This distinction matters because the P-T result shows successful assisted fabrication under the evaluated configuration rather than fully autonomous filament feeding. Conversely, other streams with mean diameters closer to the nominal target did not print successfully. These observations reinforce that functional performance depended on the combined effects of filament dimensions, feeding behavior, bed adhesion, thermal conditions, and printer settings rather than on a single dimensional criterion.
The observed failures should therefore be interpreted as different manifestations of process instability. In some cases, failure was associated primarily with inadequate bed adhesion or warping, whereas in others, interrupted filament feeding or inconsistent deposition prevented completion of the specimen. Similar failure modes have been reported for recycled HDPE and PP, where semicrystalline shrinkage, filament irregularity, and feedstock variability can compromise FFF processing [8,11,24].
However, direct comparison of H-W and P-T should be made cautiously because the successful specimens were produced using different printer platforms and different optimized printing conditions, and P-T additionally required manual assistance during filament feeding. Therefore, the results demonstrate the technical feasibility of producing specimens from selected recycled HDPE and PP streams under their respective configurations, but they do not establish equivalent autonomous printability or that one polymer family was intrinsically more printable than the other.

4.6. Preliminary Mechanical Response and Fracture-Surface Morphology

Preliminary tensile and SEM observations extend the filament-level assessment to printed-specimen performance. Mechanically testable specimens were obtained from H-R, H-W, and P-T, although these streams exhibited different printing outcomes. In particular, H-R yielded specimens suitable for tensile testing despite not consistently meeting the final printability criteria because of deformation and process instability. Given the small sample sizes (n = 2–3 per group) and incomplete specimen-level processing traceability, differences among tensile-test groups cannot be attributed to specific printing conditions or interpreted as controlled comparisons of intrinsic material properties. These results provide preliminary evidence of specimen-level mechanical performance rather than definitive material-property characterization. Low-magnification SEM examination showed that the tensile-fracture regions retained the deposited-road architecture characteristic of FFF specimens. Local variations in road arrangement, separation, and deformation were visible among the examined images. However, the observed openings could not be reliably distinguished as designed infill spaces, deposition-related discontinuities, or tensile-induced damage. Furthermore, the absence of verifiable specimen-level linkage between the SEM images and individual tensile measurements prevented direct morphological–mechanical correlations. Therefore, these observations provide qualitative context for the printed structures rather than evidence of feedstock-dependent fracture mechanisms, bulk porosity, or inter-road bonding strength.
Accordingly, the tensile and SEM results should be considered complementary specimen-level evidence rather than independent validation of material properties. The present data support the feasibility of producing mechanically testable recycled-polyolefin FFF specimens, while more extensive mechanical testing and quantitative microstructural characterization will be required to establish relationships among filament dimensional stability, printed mesostructure, and mechanical performance.

4.7. Practical Implications

The results support a multistage qualification approach for using post-consumer HDPE and PP as FFF feedstocks. Polymer identification alone was insufficient to predict extrusion stability or printability; therefore, feedstock evaluation should combine source segregation, polymer family verification, controlled extrusion, longitudinal diameter monitoring, feeding continuity, and functional printing trials.
The source-dependent behavior observed in both HDPE and PP also indicates that recycled materials within the same nominal polymer family should not automatically be processed under a single set of conditions. Instead, extrusion parameters should be adjusted to the specific waste stream and equipment configuration. For HDPE, screw speed was particularly influential, while PP diameter was strongly affected by spooler speed under the conditions evaluated.
From a distributed-recycling perspective, the experimental workflow therefore suggests a practical sequence that begins with source segregation to preserve feedstock identity, followed by polymer verification and feedstock preparation. The material then proceeds through controlled extrusion, longitudinal dimensional assessment, and feeding/continuity evaluation before undergoing printability validation. Mechanical characterization can then be performed, as needed, to further assess specimen-level performance.
This approach can help identify streams requiring further optimization before additional resources are invested in printing. It also shifts filament qualification away from reliance on a single nominal diameter value toward evaluation of the material–process–printer system as a whole.
These findings are especially relevant to laboratory-scale and distributed recycling applications, where post-consumer feedstocks are inherently variable and industrial-level material homogenization may not be available. The proposed workflow provides a practical basis for screening recycled HDPE and PP streams while preserving source traceability and identifying the processing conditions required for their potential use in FFF.

4.8. Limitations and Future Work

Several limitations should be considered when interpreting the present results. First, the study did not include direct measurements of melt-flow rate, rheological behavior, thermal transitions, molecular-weight distribution, or additive composition. Consequently, the source-dependent differences observed during extrusion and printing cannot be assigned to specific physicochemical mechanisms. Future work should incorporate techniques such as MFI/MFR testing, DSC, and complementary chemical characterization to better relate material properties to processing behavior.
Mechanical characterization was limited by the small number of specimens (n = 2–3 per group) and incomplete documentation linking individual tensile-test groups to specific extrusion and printing conditions. The results should therefore be considered preliminary and descriptive. Controlled mechanical comparisons will require larger specimen populations and complete specimen-level processing traceability. The three experimental batches were derived from the same source-segregated feedstock stream and therefore represent separately processed subsamples rather than independent collections of post-consumer material. Accordingly, source-related findings should be interpreted as differences among the specific feedstock streams evaluated rather than as population-level estimates of source effects.
Additional limitations arise from experimental equipment and feedstock selection. HDPE and PP were processed using different extrusion systems, while the successful H-W and P-T specimens were printed using different printer configurations. These differences limit direct polymer-family comparisons. In addition, the post-consumer streams were selected according to material availability and were not compared with equivalent virgin HDPE or PP controls.
Filament diameter during extrusion was monitored using the measurement system integrated into the Felfil Spooler. The retained equipment records did not establish its calibration history, manufacturer-specified measurement accuracy, or measurement uncertainty. Independent micrometer measurements were subsequently performed on three preserved filament segments, providing complementary evidence of diameter variation and two-axis dimensional asymmetry. Nevertheless, because these segments could not be linked to specific original RunIDs, the supplementary measurements do not constitute a retrospective calibration of the integrated monitoring system. Consequently, the original diameter measurements remain instrument-reported estimates, and the 1.73–1.77 mm interval should be interpreted as a descriptive screening criterion rather than a metrologically validated acceptance limit. Future studies should also evaluate material changes across the complete recycling pathway, including waste feedstock, extruded filament, and printed part, and should investigate the repeatability of optimized processing windows across larger material batches. Improved filament metrology and automated longitudinal diameter control would further strengthen dimensional assessment.
Finally, SEM characterization in this study is qualitative and should be interpreted as supporting evidence of fracture morphology rather than a quantitative measure of porosity or interlayer bonding. Future work could combine SEM with quantitative image analysis and more extensive mechanical testing to better connect filament stability, printed mesostructure, and final part performance.

5. Conclusions

This study demonstrated that source-segregated post-consumer HDPE and PP streams classified within the same nominal polymer family can exhibit substantially different extrusion behavior, dimensional stability, and FFF printability. ATR-FTIR characterization of 27 spectra supported the presence of predominant PE- and PP-based matrices consistent with the recorded resin identification codes and revealed measurable spectral variability among feedstock streams. Seven streams subsequently progressed to filament extrusion, comprising 405 extrusion runs and 14,175 sequential diameter measurements.
For the HDPE system, screw rotational speed was strongly associated with mean filament diameter. Although 6 rpm provided the lowest pooled mean absolute target error and the highest pooled percentage of measurements within the predefined dimensional screening interval, significant interactions involving feedstock stream, extrusion temperature, and screw speed indicate that this result should not be interpreted as a universal processing optimum. Screw speed was significantly associated with absolute within-run variability but not with relative variability expressed as CV. These findings support source- and condition-specific optimization of recycled HDPE extrusion. For PP, spooler speed produced the clearest and most consistent effect on filament diameter, with increasing take-up speed reducing the estimated mean diameter across P-W, P-B, and P-T. However, dimensional proximity to the nominal 1.75 mm target did not directly predict functional printing performance.
The longitudinal analysis showed that mean filament diameter alone was insufficient to characterize filament quality. H-W exhibited comparatively low within-run variability and achieved successful autonomous printing, whereas P-T retained substantially greater diameter variability but could also be fabricated into complete specimens after process optimization with manual assistance during filament feeding. Conversely, other streams with mean diameters closer to the nominal target did not consistently print successfully.
Preliminary tensile testing demonstrated that selected recycled HDPE and PP printing trials produced mechanically testable specimens, while SEM examination showed that the fracture surfaces retained the deposited-road architecture characteristic of FFF and exhibited qualitative differences in local fracture morphology among the evaluated streams. These observations were treated as supporting evidence of specimen-level functionality rather than as definitive measurements of intrinsic material properties.
Overall, the findings support evaluating source-segregated recycled feedstocks as material–equipment–process systems, considering polymer-family identification, source-specific extrusion conditions, short-window dimensional variability, feeding continuity, bed adhesion, and printer configuration. The study contributes to developing evidence-informed screening procedures tailored to recovered material streams and their processing conditions. Further dimensional metrology, documented printing repeatability, and mechanical validation are needed before reliable process qualification or broader industrial application.

Supplementary Materials

The following supporting information can be downloaded at https://www.mdpi.com/article/10.3390/eng7120665/s1. The supporting information includes an Excel workbook containing Tables S1–S11, covering HC3-robust statistical analyses, processing-factor contrasts, qualitative printability outcomes, batch sensitivity analysis, geometric apparent density, individual tensile-test results, and supplementary filament-diameter and two-axis dimensional asymmetry measurements. Additional supporting files include the complete sequential filament-diameter dataset (14,175 measurements), extrusion-run metadata, available statistical analysis scripts, and the 27 original ATR-FTIR spectra. An additional ATR-FTIR workbook provides the spectral inventory, quality-control results, correlation analyses, and PCA results, together with Figure S1 showing the spectral baseline-correction quality-control assessment.

Author Contributions

Conceptualization, J.M., C.C., M.D.L.Á.O.-D.-R.; methodology, J.M. and C.C.; validation, J.M., C.C. and M.D.L.Á.O.-D.-R.; formal analysis, J.M., C.C., B.B. and M.D.L.Á.O.-D.-R.; investigation, J.M. and C.C.; resources, J.M., C.C., M.D.L.Á.O.-D.-R. and R.C.; data curation, J.M., B.B., C.H., J.C., R.D. and M.A.M.D.; writing—original draft preparation, J.M., B.B., C.C. and M.D.L.Á.O.-D.-R.; writing—review and editing, M.D.L.Á.O.-D.-R., R.C., M.A.M.D., C.H., J.C., R.D. and M.F.; visualization, J.M., C.C. and M.D.L.Á.O.-D.-R.; supervision, C.C. and M.D.L.Á.O.-D.-R.; project administration, J.M.; funding acquisition, J.M., C.C. and M.D.L.Á.O.-D.-R. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the National Secretariat for Science, Technology, and Innovation (Secretaría Nacional de Ciencia, Tecnología, e Innovación, SENACYT) under the grant APY-NI-2024A-61.

Institutional Review Board Statement

Not applicable.

Data Availability Statement

The underlying sequential filament-diameter dataset (14,175 observations), extrusion-run metadata, supplementary analysis tables, available statistical analysis scripts, original ATR-FTIR spectra (n = 27), and supplementary micrometer measurements are provided with the Supporting Information. Additional experimental records not included in the Supplementary Files may be obtained from the corresponding authors upon reasonable request, where available.

Acknowledgments

The authors would like to thank the Research Groups in Industrial Engineering (Giii) and Design, Manufacturing, and Materials (DM + M) within the Technological University of Panama (https://utp.ac.pa/) for their collaboration. Likewise, special thanks to the Sistema Nacional de Investigación (SNI) for its support. During the preparation of this manuscript, the authors used generative AI tools to assist with language editing, structural refinement, and manuscript readability. These tools were not used to generate research data, select or fabricate references, perform evidence coding, or develop conclusions. After using these tools, the authors carefully reviewed, verified, edited, and approved all content and take full responsibility for the accuracy, integrity, and originality of the published article.

Conflicts of Interest

The authors declare no conflicts of interest. The funders had no role in the design of the study; in the collection, analyses, or interpretation of data; in the writing of the manuscript; or in the decision to publish the results.

References

  1. Angulo, C.; Shackleford, L.; Ning, H.; Pillay, S. Comparative study on the mechanical behaviors of compression molded, additively manufactured, and injection molded recycled carbon fiber reinforced rHDPE composites. Compos. Part B Eng. 2024, 275, 111323. [Google Scholar] [CrossRef] [Scilit]
  2. Zhang, Y.; Bai, H.; Mi, D.; Zhang, L.; Jiang, J.; Yang, T.; Ren, Z. Mixing screw design and high density polyethylene toughening modification for recycled polypropylene based on screw 3D printing. J. Appl. Polym. Sci. 2024, 141, e56192. [Google Scholar] [CrossRef] [Scilit]
  3. Borkar, A.; Hendlmeier, A.; Simon, Z.; Randall, J.D.; Stojcevski, F.; Henderson, L.C. A comparison of mechanical properties of recycled high-density polyethylene/waste carbon fiber via injection molding and 3D printing. Polym. Compos. 2022, 43, 2408–2418. [Google Scholar] [CrossRef] [Scilit]
  4. Daniele, R.; Armoni, D.; Dul, S.; Alessandro, P. From Nautical Waste to Additive Manufacturing: Sustainable Recycling of High-Density Polyethylene for 3D Printing Applications. J. Compos. Sci. 2023, 7, 320. [Google Scholar] [CrossRef] [Scilit]
  5. Mi, D.; Zhang, J.; Zhou, X.; Zhang, X.; Jia, S.; Bai, H. Direct 3D Printing of Recycled PET/PP Granules by Shear Screw Extrusion. Polymers 2023, 15, 4620. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  6. Suescun Gonzalez, C.; Cruz Sanchez, F.A.; Boudaoud, H.; Nouvel, C.; Pearce, J.M. Multi-material distributed recycling via material extrusion: Recycled high density polyethylene and poly (ethylene terephthalate) mixture. Polym. Eng. Sci. 2024, 64, 1555–1570. [Google Scholar] [CrossRef] [Scilit]
  7. Shiferaw, M.Z.; Gebremedhen, H.S. (Eds.) Recycled Polymer for FDM 3D Printing Filament Material: Circular Economy for Sustainability of Additive Manufacturing. In Advances of Science and Technology: Recycled Polymer for FDM 3D Printing Filament Material: Circular Economy for Sustainability of Additive Manufacturing; Springer International Publishing: Cham, Switzerland, 2022; pp. 243–261. ISBN 978-3-030-93711-9. [Google Scholar]
  8. Morales, M.A.; Atencio Martinez, C.L.; Maranon, A.; Hernandez, C.; Michaud, V.; Porras, A. Development and Characterization of Rice Husk and Recycled Polypropylene Composite Filaments for 3D Printing. Polymers 2021, 13, 1067. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  9. Atsani, S.I.; Sing, S.L. Optimization of Glass-Powder-Reinforced Recycled High-Density Polyethylene (rHDPE) Filament for Additive Manufacturing: Transforming Bottle Caps into Sound-Absorbing Material. Polymers 2024, 16, 2324. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  10. Vidakis, N.; Petousis, M.; Tzounis, L.; Maniadi, A.; Velidakis, E.; Mountakis, N.; Papageorgiou, D.; Liebscher, M.; Mechtcherine, V. Sustainable Additive Manufacturing: Mechanical Response of Polypropylene over Multiple Recycling Processes. Sustainability 2021, 13, 159. [Google Scholar] [CrossRef] [Scilit]
  11. Phillis Teng, S.P.; Hiong Tee, C.; Boon Tan, H.; Fai Leong, K. Material extrusion-based printing optimization of recycled HDPE filaments made from used milk jugs. Mater. Sci. Addit. Manuf. 2024, 3, 4084. [Google Scholar] [CrossRef] [Scilit]
  12. Arrigo, R.; Battegazzore, D.; Bernagozzi, G.; Cravero, F.; Ribero Pedraza, D.N.; Frache, A. Recycled PP for 3D Printing: Material and Processing Optimization through Design of Experiment. Appl. Sci. 2022, 12, 10840. [Google Scholar] [CrossRef] [Scilit]
  13. Zhu, Y.; Fink, W.; Yost, S.F.; Mather, P.T.; Vogt, B.D. Subtle differences in recycled polypropylene from rheology to additives impacts ease of circularity in materials extrusion additive manufacture. Addit. Manuf. 2024, 86, 104209. [Google Scholar] [CrossRef] [Scilit]
  14. Spina, R.; Gurrado, N. Green Recycling for Polypropylene Components by Material Extrusion. Polymers 2024, 16, 3502. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  15. Byard, D.J.; Woern, A.L.; Oakley, R.B.; Fiedler, M.J.; Snabes, S.L.; Pearce, J.M. Green fab lab applications of large-area waste polymer-based additive manufacturing. Addit. Manuf. 2019, 27, 515–525. [Google Scholar] [CrossRef] [Scilit]
  16. Karaki, A.; Hammoud, A.; Masad, E.; Khraisheh, M.; Abdala, A.; Ouederni, M. A review on material extrusion (MEX) of polyethylene—Challenges, opportunities, and future prospects. Polymer 2024, 307, 127333. [Google Scholar] [CrossRef] [Scilit]
  17. Strano, M.; Farioli, D.; Di Landro, L.A.; Mussi, V. Printability of recycled feedstock for extrusion additive manufacturing. Adv. Mater. Process. Technol. 2025, 11, 46–71. [Google Scholar] [CrossRef] [Scilit]
  18. Shiferaw, M.Z.; Gebremedhen, H.S.; Mengistie, A.K. Developing Filament Extruder and Characterization of Recycled High-Density Polyethylene for 3D Printing Filament Material. Heliyon 2023, 1, 5–20. [Google Scholar] [CrossRef] [Scilit]
  19. Kristiawan, R.B.; Rusdyanto, B.; Imaduddin, F.; Ariawan, D. Glass Powder Additive on Recycled Polypropylene Filaments: A Sustainable Material in 3D Printing. Polymers 2021, 14, 5. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  20. ASTM D638-22; Standard Test Method for Tensile Properties of Plastics. ASTM International: West Conshohocken, PA, USA, 2022.
  21. Arendra, A.; Akhmad, S.; Mu’alim, M.; Hidayat, K.; Prasnowo, M. Development of Low Cost Recycled HDPE Filament Extruder for 3D Printing Filament. In Proceedings of the 2nd International Conference on Advance and Scientific Innovation, ICASI 2019, Banda Aceh, Indonesia, 18 July 2019; Hidayat, R., Mesran, M., Diansyah, T., Supriyanto, S., Siregar, D., Eds.; EAI: Ghent, Belgium, 2019; ISBN 978-1-63190-208-6. [Google Scholar]
  22. Satya, S.K.; Sreekanth, P.R. An experimental study on recycled polypropylene and high-density polyethylene and evaluation of their mechanical properties. Mater. Today Proc. 2020, 27, 920–924. [Google Scholar] [CrossRef] [Scilit]
  23. Chu, J.S.; Koay, S.C.; Chan, M.Y.; Choo, H.L.; Ong, T.K. Recycled plastic filament made from post-consumer expanded polystyrene and polypropylene for fused filamant fabrication. Polym. Eng. Sci. 2022, 62, 3786–3795. [Google Scholar] [CrossRef] [Scilit]
  24. Kalinke, C.; Crapnell, R.D.; de Oliveira, P.R.; Janegitz, B.C.; Bonacin, J.A.; Banks, C.E. How to Improve Sustainability in Fused Filament Fabrication (3D Printing) Research? Glob. Chall. 2024, 8, 2300408. [Google Scholar] [CrossRef] [Scilit] [PubMed]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Article metric data becomes available approximately 24 hours after publication online.