Abstract
Copper chip/substrate interconnect is a promising replacement for conventional solder due to copper’s superior electrical, thermal, and mechanical performance. In this study, a chemically assisted method for thermomechanical sintering of copper microparticles at temperatures <200 °C is reported (i.e., low-temperature sintering). Formic acid pretreatment and the incorporation of an aromatic aldehyde, o-phthalaldehyde (oPA), provided a strong local reducing environment to fuse copper microparticles into a solid fillet in ambient air. Design-of-experiment (DOE) analysis was used to optimize the mechanical strength of the sintered part with respect to bonding time, aldehyde content, temperature, and applied pressure. Under optimized conditions (50 wt% formic acid and 10 wt% oPA), strong Cu discs were obtained in 6 min at 180 °C and 20 MPa.