Skip to Content
HeritageHeritage
  • Article
  • Open Access

23 November 2026

20 Pages

Tape Test for Evaluating Superficial Stone Cohesion in Cultural Heritage: Toward a Standardised Protocol

,
,
,
,
,
,
,
and
1
Department of Science and High Technology, University of Insubria, Via Valleggio 9/11, 22100 Como, Italy
2
Convenor CEN TC 346–WG3, Istituto Santa Paola, Piazza dei Mille 16/d, 46100 Mantova, Italy
3
Department of Physics “Aldo Pontremoli”, Università degli Studi di Milano, Via Celoria 16, 20133 Milan, Italy
4
Institute of Heritage Science, National Research Council (CNR-ISPC), Area della Ricerca di Firenze, Via Madonna del Piano 10, 50019 Sesto Fiorentino (FI), Italy

Abstract

Consolidation treatments are widely used to restore surface cohesion in deteriorated stone heritage materials, but no shared, quantitative protocol exists to assess their effectiveness. This study evaluates the Tape Test—a peel-off method quantifying material removed from a treated surface—comparing two adhesive tapes (Nitto WS-1 and Tesa Sensitive 4333) on six heritage objects: three gypsum plaster artworks and one terracotta element from the Brera Academy of Fine Arts, Milan, and two marble elements (a relief and a small head) from the Arco della Pace, Milan. Gravimetric measurements recorded the gross mass of each strip (tape plus collected material) with a portable field balance and a precision laboratory balance; the strips had not been individually pre-weighed, so the net mass of removed particles could not be derived. Stereomicroscopic binary image analysis quantified the area of particles removed. The two balances were not interchangeable (Bland–Altman bias = +0.011 g on strips weighing 0.03–0.07 g; n = 36 paired readings), confirming that instrument resolution is critical for reliable gravimetry. Gross mass was almost constant for each tape across substrates and mainly reflected the intrinsic mass of the strips, so it did not allow tapes or substrates to be compared. Image analysis revealed substrate-specific removal patterns, with terracotta showing the highest white area (13.8–15.4% across the three pulls) and the gypsum plasters generally the lowest, with the Nitto tape, while the Tesa tape gave near-zero white area on all substrates except terracotta. Individual pre-weighing of pre-cut strips is proposed as a condition of a pre-normative protocol.

1. Introduction

Inorganic porous materials, both natural (stone) and artificial (stucco, mortars, and ceramics), constitute a fundamental component of the built and sculptural cultural heritage worldwide. They are subject to physical, chemical, and biological decay processes that progressively weaken surface cohesion and lead to material loss, making consolidation treatments one of the primary conservation interventions employed [1,2,3,4,5].
Despite the widespread use of consolidants, no shared testing protocol currently exists to assess their effectiveness in terms of the surface properties they are specifically designed to improve. This contrasts with the situation for water repellent products, for which EN 16581, the European standard defining test methods for evaluating surface protection treatments on porous inorganic materials, provides a harmonised framework [6]. Among the available diagnostic approaches, the Tape Test, a peel-off method using standardised adhesive tape, first introduced by Mora and Torraca [7], offers a contribution to fill this gap, with key advantages including simplicity, low cost, minimal invasiveness, and applicability to delicate surfaces in both laboratory and field conditions. It is particularly suited to surfaces exhibiting powdering or dusting, among the most common and significant manifestations of inadequate superficial cohesion, where quantifying the reduction in particle release before and after consolidation provides direct, measurable evidence of intervention effectiveness.
The test is simple in principle: a strip of adhesive tape is applied to the stone surface, pressed with uniform pressure, and peeled off at a controlled angle. Particles detached from the surface remain on the tape and can be weighed before and after application to quantify the removed mass. Microscopic examination of the tape provides complementary information on particle morphology and spatial distribution. Three consecutive pulls on the same area are typically performed, each with a fresh strip, to probe the cohesion profile with depth. While the Tape Test itself is an established diagnostic tool, no validated protocol currently defines how its results should be measured, analysed, and interpreted in a reliable way: this study addresses that gap by integrating precision gravimetry, image analysis, and statistical validation into a single, standardisable diagnostic procedure.
This study presents a systematic experimental assessment of the Tape Test on six heritage objects of different porous inorganic materials, integrating gravimetric, statistical, and image analysis approaches to generate pre-normative evidence for proposing a protocol development. We hypothesised that instrument precision (field vs. laboratory balance) would affect the reliability of Tape Test gravimetric results, and that tape type would affect the particle removal recorded by image analysis.

1.1. Origin and Early Applications

The use of adhesive tape to assess surface cohesion in cultural heritage materials was pioneered by Mora and Torraca in the mid-1960s [7], who applied a peel-off test, originally called the “Scotch Tape Test”, to evaluate the effectiveness of consolidants on mural paintings. Despite its early introduction, the method remained largely informal for several decades: descriptions in the literature were often qualitative and procedurally incomplete, and no standardised protocol was established to ensure reproducibility across operators, materials, or laboratories. As Drdácký et al. [8] observed, most published applications provide only a general or superficial description of the measurement procedure, lacking the methodological detail required for systematic comparison.
Notwithstanding these limitations, the peeling test gradually gained traction as a practical diagnostic tool, particularly valued for its low invasiveness, minimal cost, and suitability for use on fragile heritage surfaces where more destructive testing is not feasible. Its application progressively expanded from painted surfaces to a broader range of stone materials and historic plasters [1,2].

1.2. Applications to Stone Heritage Materials

A significant body of literature documents the use of the Tape Test on historic stone surfaces, primarily in the context of evaluating pollution-related deterioration and the effectiveness of consolidation treatments. The potential of adhesive tape as a microsampling strategy for subsequent analytical characterisation has been demonstrated on stone monument surfaces by Urzì and De Leo [9], who showed that tape-based collection enables direct microscopic examination and identification of surface materials without compromising substrate integrity, illustrating how the Tape Test can function not only as a mechanical diagnostic tool but also as a non-destructive sampling interface for further analysis.
It should be noted that adhesive tape may transfer residues of its own polymer matrix to the collected material, potentially interfering with subsequent chemical characterisation, a risk documented, for instance, in carbon tape microsampling for SEM-EDS analysis, where tape-derived carbon cannot be distinguished from the sample’s own carbon content [10]. In the present study, tape strips were used exclusively for gravimetric and image-based assessment; no chemical analysis of the collected particles was performed, and adhesive contamination therefore does not affect the results reported here.
Drdácký and Slížková [11,12] extended the application of peeling tests to carbonatic plaster and render surfaces, confirming the method’s discriminative power on historic materials while highlighting the risk of excessively invasive outcomes when applied without prior assessment of substrate fragility, a consideration of particular relevance for poorly cohesive materials such as deteriorated plasters.
The evaluation of consolidation effectiveness represents a second major strand of Tape Test applications in stone conservation. Tiano [13] applied a peeling test to Carrara marble specimens subjected to weathering and subsequently treated with bio-reinforcing agents promoting calcite precipitation; a clear reinforcement effect was detected when the removed material from treated and untreated surfaces was compared. Drdácký and Slížková [14] similarly used the method to assess surface consolidation effects on materials with initially poor cohesion, concluding that, despite the absence of a validated standard, the test can provide meaningful relative comparisons when applied under controlled and consistent conditions. Drdácký & Slížková [11] extended this work to in-situ testing on historic render and plaster surfaces, confirming that the method can be reliably applied beyond controlled laboratory conditions. The work of Becerra et al. [15] further demonstrated the Tape Test as part of an on-site testing protocol for consolidant nanoparticles on stone cultural heritage, reinforcing its role within multi-method evaluation schemes.
For surfaces characterised by high porosity or irregular texture, adhesion uniformity may be compromised. Drdácký et al. [8] noted that highly uneven surfaces with pronounced roughness can prevent conformal tape contact, leading to inconsistent results, a documented limitation that underscores the need for material-specific validation before protocol adoption.

1.3. Standardisation Efforts and Normative Context

From a normative standpoint, the Tape Test in cultural heritage currently operates at the margins of existing standards. The most directly applicable frameworks are industrial adhesion test methods developed by ASTM: D3359-23 [16] describes two peel-based procedures for coating adhesion assessment: the X-cut method, in which two incisions are made through the coating in an X pattern before tape application and removal, and the cross-cut method, in which a grid of parallel incisions is used and adhesion is rated by the proportion of squares detached, while D4214-07(2015) provides protocols for quantifying chalking in exterior paint films, including tape-based variants that have been adapted to assess surface powder removal on historic substrates [17]. ASTM D903-98(2017) [18] establishes test conditions for the peel strength of adhesive bonds more generally. Notably, none of these standards were developed specifically for application to quasi-brittle or heterogeneous historic stone materials, and their direct adoption in conservation contexts requires careful methodological adaptation.
Within the European standardisation framework, CEN/TC 346, the technical committee responsible for conservation of cultural property, has developed a suite of harmonised test methods covering surface protection (EN 16581) [6] and general conservation criteria, but no equivalent standard currently exists for the quantitative assessment of superficial cohesion following consolidation treatment. The working group CEN/TC 346/WG3, which prepares standards for evaluating the products and methods used in conservation works, has so far completed a framework dealing with cleaning and surface protection [19], while the assessment of consolidation treatments is not yet covered by a published standard; a validated Tape Test protocol could help to fill this gap.
Drdácký et al. [8] provided the most systematic attempt to date to formalise peeling test methodology for historic stone and mortar surfaces, proposing operational criteria for tape type, application pressure, strip dimensions, and the number of consecutive pulls. Their work established that test outcome is sensitive to instrument choice, operator technique, and substrate characteristics, all of which must be controlled and reported to achieve meaningful interlaboratory comparability.
A further methodological variable that has received insufficient attention is whether consecutive pulls are performed on the same area or on adjacent locations. Drdácký et al. [8] and Becerra et al. [15] explicitly apply repeated pulls to the same area, considering the progressive decrease in removed material as diagnostic information on the depth profile of surface cohesion. Giorgi et al. [2], by contrast, use adjacent areas, avoiding cumulative surface damage but introducing spatial variability as an additional source of uncertainty. Each approach carries distinct implications: same-area pulls allow reconstruction of the cohesion gradient with depth but progressively alter the surface being tested; adjacent-area pulls preserve each test location intact but conflate material variability with pull sequence effects. Neither approach has been systematically compared in the literature, and the choice is rarely justified in published protocols.
The present study builds directly on this foundation, extending the experimental evidence base to a broader range of heritage lithotypes and integrating gravimetric precision analysis with quantitative image analysis.

1.4. Methodological Challenges and Research Gaps

A comparison of published applications reveals considerable procedural variation. On tape selection, Drdácký et al. [8] tested multiple commercial tapes, including TESA bi-adhesive and 3M Scotch Cristal, without establishing criteria for choosing between them, while Becerra et al. [15] adopted Scotch Cristal (3M) following the same group’s protocol without further justification. The number of pulls ranges from two [13] to ten [15], applied either to the same area or to adjacent locations, a distinction with direct implications for how the depth profile of surface cohesion is interpreted. On balance precision, Drdácký et al. [8] report a Gibertini balance at ±0.001 g, but most published protocols do not specify instrument accuracy or address the practical constraints of field weighing; Drdácký & Slížková [11] describe strips being transported to a laboratory for post-test weighing, implicitly acknowledging the problem without discussing it. Statistical treatment is similarly underdeveloped: Becerra et al. [15] report standard deviations and a consolidation percentage derived from cumulative removal, while Drdácký et al. [8] rely on descriptive comparison alone. Statistical analysis of peel tests has been developed for other materials, such as polymer films [20], but no published study has applied inferential statistical testing to Tape Test gravimetric data on heritage materials.
Across the literature, several recurring methodological challenges emerge. First, the absence of a validated standard means that published results are difficult to compare: strip dimensions, tape type, application pressure, removal angle, and measurement instrumentation vary considerably between studies, and reporting is frequently incomplete [8,11]. Second, the sensitivity of gravimetric measurements to instrument precision has received limited attention; most published protocols do not specify balance accuracy or distinguish between field and laboratory weighing conditions. Drdácký et al. [8] report a Gibertini balance at ±0.001 g, but this remains an exception rather than the norm. Third, image-based quantification of removed material has been applied only sporadically and without standardised procedures. Drdácký & Slížková [11] recommend optical microscopy as a qualitative check on tape strip content, and Drdácký et al. [8] employ reflectance measurements to rate strip loading on a numeric scale, but neither approach yields spatial or morphological data on the detached particles. No published study has applied systematic binary image analysis to tape strips for quantitative characterisation of particle distribution and removal area.
The present study addresses these gaps through a systematic comparative assessment of two adhesive tapes: Nitto WS-1 and Tesa Sensitive 4333, selected as commercially available alternatives to the tape used by Defus et al. [21], which could not be sourced, on six heritage objects of different lithotypes, evaluating the effect of balance precision on measurement reliability and integrating stereomicroscopic binary image analysis as an integral component of the protocol. The results contribute pre-normative evidence toward a future CEN-compatible Tape Test standard for the evaluation of superficial consolidation in stone cultural heritage.

2. Materials and Methods

2.1. Study Objects

The study objects were selected to ensure representativeness across different porous inorganic materials relevant to stone heritage conservation, ranging from gypsum plaster and terracotta to natural stone. Testing was conducted on six surfaces, one on each of six heritage objects (Figure 1): three gypsum plaster artworks (Plaster 1, 2, 3) and one terracotta conserved at the Brera Academy of Fine Arts, Milan, coming from the collection of copies and replicas used in the sculpture class, most probably cast during the XIX century and conserved for decades in humid underground deposits; a relief and a small marble head—likely a decorative figure (angel or putto) detached from the monument during restoration works—sculpted in the so-called Crevola d’Ossola Marble, from the Arco della Pace, Milan (Figure 2; the relief and the small head are two separate objects), where an ongoing conservation worksite provided direct access to the marble surfaces for in-situ testing. This lithotype is quarried in Piedmont close to the village of Domodossola. It is a partly dolomitic marble, medium to fine-grained. The tests on the Arco della Pace surfaces were carried out before consolidation, and post-treatment measurements are not available. A treatment with diammonium phosphate (DAP) was planned, at 1% for 24 h followed by 5% for 24 h [21,22].
Figure 1. Study objects (left to right): Terracotta with decorative motifs; Plaster 1—pedestal of a Madonna and Child statue; Plaster 2—David and Goliath, detail of the leg; Plaster 3—lower detail of the drapery of a different Madonna and Child statue. Brera Academy of Fine Arts, Milan.
Figure 2. Arco della Pace marble relief and small head (two separate objects), Milan, tested before consolidation.

2.2. Tape Test Protocol

Two tapes were compared: Nitto WS-1 (polyimide film backing, cured silicone adhesive, thickness 0.066 mm, tensile strength 61.3 N/cm, elongation at break 70%, adhesion to steel 2.96 N/cm; [23]) and Tesa Sensitive 4333 (flat paper backing, acrylic adhesive, total thickness 80 µm, tensile strength 32 N/cm, elongation at break 5%, adhesion to steel 0.5 N/cm; typical values; [24]). The Nitto tape (Nitto Denko Corporation, Osaka, Japan) was kindly provided by Erga Tapes (Sesto San Giovanni, Italy; product code WS-1); the Tesa tape (tesa SE, Norderstedt, Germany; light pink, 25 mm wide, 50 m roll) was purchased from Amazon.it (November 2024). The manufacturers’ datasheets are provided as Supplementary Materials (Figures S1 and S2). The nominal contact area of a Tesa strip was therefore 7.5 cm2 (25 × 30 mm); the width of the Nitto tape, measured on the micrographs (scale bar 5 mm), was approximately 9–11 mm (nominal contact area of a 3 cm strip about 2.8–3.4 cm2). Surface preparation was material specific. On the gypsum plaster objects of the Brera Academy the Tape Test was carried out on cleaning test patches already present on the surfaces, made by students of the Brera Academy during conservation work, independently of this study, in areas most affected by powdering (exposed to contact or water); the patches had been cleaned using gel-based systems (agar gel or PEGGY + TAC, depending on the patch) applied to areas affected by powdering and surface deposits. The terracotta surface, whose conservation state precluded chemical intervention, was cleaned mechanically before the test, since it had no cleaning patch, using a soft brush and vacuum suction. Surface preparation for the Arco della Pace marble surfaces followed the conservation protocol already in place at the site. Tape strips of nominal length 3 cm were cut by hand in situ (length tolerance ± 0.1–0.5 cm) and were not pre-weighed. Each strip was weighed once, after application and removal, together with the collected material: first with a portable field balance directly in situ, then, after storage in closed Petri dishes, with a Sartorius precision balance (4-digit, ±0.0001 g) in the laboratory. The recorded values are therefore the gross mass of the strip (tape plus collected material), not the net mass of removed particles. A fixed strip length of 3 cm was adopted across all study objects and tape types, rather than adjusting strip dimensions to the morphology of each test area, to keep the tested surface area nominally constant and allow comparison across substrates, within the limits of the cutting tolerance. This length was selected as a compromise between obtaining a measurable mass of removed particles and preserving enough intact surface for three consecutive pulls on smaller test areas. Manual cutting in situ and the absence of a pre-test weight are the main limitations of the gravimetric data of this study: the mass variation produced by the cutting tolerance (about 1–2 mg for ±0.1 cm and up to 5–10 mg for ±0.5 cm on a 3 cm strip) is comparable with the differences observed between pulls and between substrates (Section 3.1). Application was performed using a closed-cell foam roller (Axton, a commercial roller supplied by the ISPC-CNR laboratory in Sesto Fiorentino, Italy; manufacturer details not available) (Figure 3), passed five times over the strip by the same operator, maintaining consistent contact across the tape surface. The roller load was not measured: the applied pressure was kept as constant as possible by the same operator and is therefore not quantified. The foam backing of the roller absorbed minor substrate irregularities, contributing to homogeneous tape-to-surface contact. Strips were handled throughout with tweezers to avoid contamination from finger contact. Adhesion time was 10 s; removal was performed at an angle as close to 90° as practicable, maintained consistently by the same operator. Three consecutive pulls were performed on the same area, using a fresh strip for each pull. This approach was adopted to probe the depth profile of surface cohesion: consecutive pulls act on a progressively modified surface and are therefore not independent repetitions; the progressive decrease in white pixel area across pulls (Section 3.3) is interpreted as indicative of improving cohesion with depth. The tests were carried out in December 2024 in Milan: on the terracotta and gypsum objects in the storage depots of the Brera Academy, and on the marble elements at the conservation worksite of the Arco della Pace, in uncontrolled ambient conditions. Temperature and relative humidity were not recorded during testing and weighing. The paper backing of the Tesa tape can take up moisture, which would change the gross mass of the strip independently of the collected particles; the strips were weighed with the field balance immediately after the test and then stored in closed Petri dishes until they were re-weighed in the laboratory (the interval between the test and the laboratory weighing was not recorded exactly, but was at least one day), with no controlled equilibration period, so an effect of humidity on the gross masses cannot be excluded.
Figure 3. Tape Test protocol: (a) in-situ tape application with foam roller on a Brera Academy surface; (b) tape strips after testing, organised by object (Plaster 1 = pedestal, Plaster 2 = leg, Plaster 3 = drapery, Terracotta), three pulls each (numbers 1–3 beside the strips indicate the pull; hand-written Italian labels on the dishes are sample codes: G.1–G.3 = Plaster 1–3, T.C. = Terracotta; pied. = pedestal, gamba = leg, veste = drapery); (c) precision weighing with Sartorius balance; (d) digital image pre-processing (RGB-to-grayscale conversion in Adobe Photoshop) before ImageJ binarisation, shown here on the Terracotta micrograph.

2.3. Analytical Procedures

Gravimetric analysis: each strip was weighed after testing (gross mass: tape plus collected material) using both a portable field balance (Mettler PC 4400 DeltaRange, Mettler-Toledo, Greifensee, Switzerland; fine range 5–400 g with readability 0.01 g, coarse range up to 4200 g with readability 0.1 g) and the precision balance (Sartorius AG, Göttingen, Germany; 4-digit, ±0.0001 g). All field readings were multiples of 0.02 g (0.00, 0.04, 0.06, 0.08 g) and no pre-test weights were recorded. Image analysis: tape surfaces were examined by Leitz Wild M420 stereomicroscope (Wild Heerbrugg, now Leica Microsystems, Heerbrugg, Switzerland) with a Nikon DS-5M camera (Nikon Corporation, Tokyo, Japan) at 6.3× magnification, and images were binarised in Adobe Photoshop (version 25.x, “Photoshop 2024”; Adobe Inc., San Jose, CA, USA, https://www.adobe.com/products/photoshop.html) and analysed with ImageJ (version 1.54, https://imagej.net; National Institutes of Health, Bethesda, MD, USA) to quantify white pixel area (detached particles) vs. total area. Image analysis was performed on a representative portion of the tape strip surface judged to be significant and representative of the overall particle distribution, rather than on the full strip surface. All images were acquired with the same camera and magnification (6.3×), covering the same field of view; the original images are 1280 × 960 px for the Brera strips and 640 × 480 px for the small head, i.e., half the pixel resolution. The grey-level threshold was set individually for each image, so as to render the particles as faithfully as possible to the original. One image was analysed for each strip. Setting the threshold image by image introduces a degree of subjectivity, and the lower resolution of the small head image may affect the detection of small particles; both limit the comparability of absolute white-area values between images and tapes. Statistical analysis: a paired t-test and Wilcoxon signed-rank test were applied to compare matched pairs of observations (same strip weighed on the two balances). The paired t-test assesses whether the mean difference between paired measurements is statistically different from zero and assumes approximate normality of differences; the Wilcoxon signed-rank test is a non-parametric alternative that makes no distributional assumptions and is therefore preferred for small samples. Bland–Altman analysis was used to assess agreement between the two balances: it plots the difference between paired measurements against their mean, characterising systematic bias and the spread of individual disagreements through 95% limits of agreement (mean bias ± 1.96 SD of differences). Pearson’s correlation between the mean and the signed difference in the two readings was used to check for proportional bias, and Spearman’s rank correlation for the exploratory comparison between gross mass and white pixel area. The paired readings are not independent (three strips per area, each acting on a surface modified by the previous pull), so pooled statistics are descriptive and p-values are indicative only. The pooled analysis includes all 36 paired readings and is also reported without one anomalous reading (n = 35). All statistical computations were performed in Python 3.12.3 (SciPy 1.18.1, scipy.stats module, https://scipy.org) with the assistance of Claude (Anthropic, San Francisco, CA, USA; models Claude Sonnet 4.6 and Claude Sonnet 5.5), a generative AI tool, which wrote and executed the analysis code from the authors’ raw gravimetric dataset; the authors verified all resulting values against the source data and take full responsibility for their accuracy. The dataset (Table S1) and the analysis script (Code S1) are provided as Supplementary Materials.

3. Results

3.1. Gravimetric Results—Brera Academy Objects

3.1.1. Effect of Balance Precision on Measurement Reliability—Nitto WS-1 Tape, Brera Objects

Table 1 reports the variance, standard deviation and coefficient of variation in the gross mass (strip plus collected material) over the three pulls for the Nitto tape, measured with both balances. Because each strip was weighed once after use and not before, these statistics describe the variability of gross strip mass among the three strips of an area, which combines the variability of the strips themselves (cutting tolerance of 0.1–0.5 cm, i.e., roughly 3–17% of the nominal length), the mass of the collected particles and the measurement error; they are not measures of instrumental repeatability. The precision (4-digit, ±0.0001 g) Sartorius balance returned small, non-zero dispersions for all areas (SD 0.0006–0.0016 g; CV 1.8–4.4%), whereas the portable field balance (2-digit) gave coarse values, with either zero dispersion (three identical readings) or large dispersion caused by single-step changes of 0.02 g (Table 1, Figure 4 and Figure 5).
Table 1. Variance, standard deviation, and coefficient of variation (CV) of the gross mass (strip plus collected material) over the three pulls, measured using field (2-digit) and precision (4-digit) balances—Nitto WS-1 tape, Brera Academy and Arco della Pace objects.
Figure 4. Comparison of field (2-digit) vs. precision (4-digit) balance measurements—Nitto WS-1 tape, Brera Academy objects. Values are gross masses of strip plus collected material. Note the substantially different scale between the two panels.
Figure 5. Comparison of field vs. precision balance measurements—Tesa Sensitive 4333 tape, Brera Academy objects.
For the Nitto WS-1 tape, the dispersion of the field balance readings was dominated by the instrument resolution. For terracotta, the field balance gave a variance of 5.3 × 10−4 g2 (SD = 0.0231 g; CV = 43.3%), compared to 2.4 × 10−6 g2 (SD = 0.0016 g; CV = 4.4%) with the precision balance. Similar contrasts were recorded for Plaster 1 (field variance 1.3 × 10−4 g2, SD = 0.0115 g, CV = 21.7%; precision variance 1.2 × 10−6 g2, SD = 0.0011 g, CV = 3.7%) and Plaster 3 (field variance 0, SD = 0, CV = 0%; precision variance 1.5 × 10−6 g2, SD = 0.0012 g, CV = 4.1%). The zero variance recorded for Plaster 3 and for the relief with the field balance reflects the coarse resolution: the three readings were identical (0.06 g for Plaster 3, against 0.029–0.031 g on the precision balance), so apparent precision reflects insensitivity rather than genuine uniformity. The field readings also differ from the precision balance by more than the 0.02 g step in some cases (up to 0.045 g, for terracotta pull 1: 0.08 g versus 0.0345 g), so rounding alone does not explain the deviation, which is expected because the strips (0.029–0.068 g) weigh far less than the minimum load specified for this balance (5 g). Plaster 2 showed the smallest dispersion with the precision balance (variance 3.0 × 10−7 g2, SD = 0.0006 g, CV = 1.8%); this describes three strips of similar mass and is not evidence of surface compactness, which is assessed by image analysis (Section 3.3).
Formal statistical comparison of the two balances is presented for the complete gravimetric dataset, pooling all tape types and both study sites (Brera Academy and Arco della Pace), in Section 3.2 below, using a Bland–Altman analysis together with paired t-test and Wilcoxon signed-rank tests.
The zero-variance observed for both Plaster 3 and relief with the field balance, and the artificially low SD for several gypsum materials, arise from the instrument’s coarse resolution (all field readings were multiples of 0.02 g): when the three readings fall in the same step, variance collapses to zero irrespective of the actual strip mass. SD values for the field balance are reported to four decimal places for comparability with the precision balance column; given the resolution of the field instrument, these values should be considered reliable only to the second decimal place (i.e., SD ≤ 0.02 g for the values reported here).
Figure 4 shows the gross mass of the three consecutive strips for the Nitto tape, measured with the field (2-digit) and precision (4-digit) balances, for the Brera Academy objects. With the precision balance the gross mass varies by at most 0.003 g among the three pulls of an area (Terracotta 0.0345, 0.0374, 0.0350 g; Plaster 1 0.0313, 0.0299, 0.0291 g; Plaster 2 0.0320, 0.0315, 0.0309 g; Plaster 3 0.0306, 0.0310, 0.0287 g). Changes in this size are comparable with the mass variation produced by the cutting tolerance (Section 2.2) and are therefore not interpreted as a cohesion profile. Field balance readings are generally higher than precision balance readings, and the pull-to-pull pattern of the field balance for Terracotta (0.08, 0.04, 0.04 g) and Plaster 3 (0.06, 0.06, 0.06 g) does not follow that of the precision balance: this is attributable to the field balance resolution and shows that field readings cannot be used to read trends.

3.1.2. Tesa Sensitive 4333 Tape—Brera Objects

For the Tesa Sensitive 4333 tape, field and precision balance readings appear visually closer to one another in absolute terms than for the Nitto tape (Figure 5). This is because the gross mass of Tesa strips (0.053–0.068 g on the precision balance) is about twice that of Nitto strips (0.029–0.037 g) and lies further above the 0.02 g step of the field balance, so rounding effects are proportionally smaller. This should not be read as general equivalence of the two balances: the pooled analysis in Section 3.2 shows that the field balance reads systematically higher.
The inter-pull differences in the Tesa strips on the precision balance are small (at most 0.0075 g: Terracotta 0.0605, 0.0641, 0.0680 g; Plaster 1 0.0533, 0.0565, 0.0552 g; Plaster 2 0.0552, 0.0548, 0.0543 g; Plaster 3 0.0556, 0.0533, 0.0556 g) and, as for the Nitto tape, no pull-to-pull trend in gross mass is interpreted.

3.1.3. Gross Mass of the Two Tape Types

Figure 6 shows the mean gross mass by tape type and balance for the Brera Academy materials. The field balance mean exceeded the precision balance mean in 7 of the 8 tape × material combinations (exception: Tesa on Plaster 1, 0.0533 versus 0.0550 g); the largest overestimation was for Nitto on Plaster 3 (0.0600 versus 0.0301 g, a factor of about 2) and on Plaster 1 (a factor of about 1.8), while for terracotta it was a factor of about 1.5 (0.0533 versus 0.0356 g). For Tesa the two balances agree more closely in relative terms, consistent with the larger gross mass of the Tesa strips.
Figure 6. Mean gross strip mass (g) by tape type and balance across all Brera Academy materials, with ±1 SD error bars. Note: The field balance substantially overestimates Nitto WS-1 measurements.
The gross mass differs clearly between the two tapes (precision balance: Nitto 0.0287–0.0374 g, mean 0.0326 g; Tesa 0.0533–0.0680 g, mean 0.0583 g), but this mainly reflects the intrinsic mass of the strips, which differ in backing (polyimide film versus paper) and adhesive (silicone versus acrylic) and were not pre-weighed; it cannot be interpreted as a difference in the material removed. Within each tape, gross mass varied little among substrates (coefficient of variation of 7% for Nitto and 8% for Tesa across the 18 readings of each tape), a dispersion comparable with that produced by the cutting tolerance (Section 2.2). Gravimetry as performed here therefore does not allow the tapes, or the substrates, to be ranked by the amount of material removed. Without pre-weighing, the smallest amount of collected material that can be distinguished from the strip-to-strip variability can be estimated, as an upper bound, from the dispersion of the 18 gross masses of each tape (SD = 2.4 mg for Nitto and 4.6 mg for Tesa): a difference of about three standard deviations, that is about 7 mg for Nitto and 14 mg for Tesa, would be needed. The differences among substrates (up to 5.5 mg for Nitto and 9.4 mg for Tesa) are below these limits, and the 20 mg step of the field balance is larger than both.
For the Nitto tape only, gross mass and white pixel area (Section 3.3) were positively correlated across the 18 strips (Spearman ρ = 0.70, p = 0.001); no significant correlation was found for the Tesa tape (ρ = 0.29, p = 0.25). Since the strips of one area are not independent, this is an exploratory observation. In addition, the percentage of tape area covered by particles does not necessarily scale with their mass, because particle size, thickness, density and aggregation also play a role. The total gross mass over three pulls for the six areas (Figure 7) is shown for completeness only; since the difference between tapes reflects the strip mass, no statistical test is applied to it.
Figure 7. Total gross mass (strip plus collected material) over three consecutive pulls, by tape type, across all six matched study areas (Brera Academy and Arco della Pace). Grey lines connect the two tapes tested on the same substrate/area. The difference between tapes mainly reflects the intrinsic mass of the strips.

3.2. Gravimetric Results—Arco Della Pace Marble

On the two Arco della Pace marble surfaces (small head and relief), the gross masses measured with the precision balance were within the range observed on the Brera objects (Nitto 0.033–0.036 g; Tesa 0.055–0.066 g). The pull-to-pull differences are small and, for the reasons given in Section 3.1, are not interpreted. As shown by the pooled analysis in Section 3.2, the field balance is on average not interchangeable with the precision balance, and field readings on marble should therefore be treated with caution.
Figure 8 shows the gross mass of the three strips for both tapes on the Arco della Pace surfaces, with solid lines representing field balance data and dashed lines representing precision balance data.
Figure 8. Trend of the gross mass of the strips across three pulls: Nitto WS-1 and Tesa Sensitive 4333 tapes, Arco della Pace marble surfaces, pre-consolidation. Solid lines: field balance; dashed lines: precision balance. Panels: (a) relief, Nitto; (b) relief, Tesa; (c) small head, Nitto; (d) small head, Tesa.
For the Nitto WS-1 tape, the precision balance gave gross masses of 0.0353, 0.0335 and 0.0331 g for the relief, and 0.0340, 0.0355 and 0.0330 g for the small head (an increase followed by a decrease). The field balance gave 0.04 g for all three relief strips, and 0.04, 0.04 and 0 g for the small head. A gross mass of zero is not physically possible for a strip that weighs 0.0330 g on the precision balance, and the other Nitto strips of similar mass (0.033–0.036 g) were read as 0.04 g. The reading is therefore anomalous; we attribute it to the limited sensitivity and reliability of the field balance at such low loads (the strips weigh far less than its minimum load of 5 g), although a recording error cannot be excluded. It is retained in the pooled analysis in Section 3.2, which is also reported without it.
For the Tesa Sensitive 4333 tape on the marble surfaces, the precision balance gave gross masses of 0.0660, 0.0626 and 0.0633 g for the relief (a decrease followed by a slight increase at pull 3) and 0.0568, 0.0548 and 0.0592 g for the small head (mean 0.0569 g, SD = 0.0022 g); field readings were 0.06, 0.08 and 0.08 g for the relief and 0.06 g for all three small head strips. The precision balance means were 0.0640 g (relief) and 0.0569 g (small head) for Tesa, versus 0.0340 and 0.0342 g for Nitto; as discussed in Section 3.1.3, this difference reflects the mass of the strips and not the amount of material removed.
No post-consolidation measurements are available for the Arco della Pace surfaces, so the effect of the DAP treatment on surface cohesion could not be evaluated in this study.

Overall Agreement Between Field and Precision Balances: Pooled Analysis

To complement the observations above, the overall agreement between the two balances was assessed by pooling all gross mass readings (both tape types and both sites; 36 paired readings, 24 from Brera Academy objects and 12 from Arco della Pace marble surfaces). The pairs are not independent (three strips per area), so the statistics are descriptive. The Bland–Altman analysis (Figure 9) gave a mean bias of +0.0107 g, with the field balance reading higher than the precision balance, and 95% limits of agreement from −0.0205 g to +0.0419 g (paired t-test: t = 4.02, p < 0.001; Wilcoxon signed-rank test: p < 0.001). Without the anomalous reading (Nitto, small head, pull 3: field 0 g, precision 0.0330 g; Section 3.2) the bias is +0.0119 g (limits of agreement −0.0160 to +0.0399 g; t = 4.95, p < 0.0001; Wilcoxon p < 0.0001), so the conclusion does not depend on it. Given that the gross masses of the strips ranged from 0.029 to 0.068 g, the limits of agreement are a large fraction of the quantity measured, and the two instruments cannot be treated as interchangeable. The correlation between the mean of the two readings and their signed difference is significant only because of the anomalous reading (Pearson r = 0.35, p = 0.038 with all 36 readings; r = 0.19, p = 0.28 without it), so no proportional bias is claimed. Together with the observation that all field readings were multiples of 0.02 g, these results indicate that the disagreement mainly reflects the coarse resolution (and possibly the calibration) of the field balance, and support the use of a precision balance for Tape Test gravimetry on heritage surfaces. We note that the field balance used here was designed for much larger loads (minimum load 5 g), so these results show the need for a balance with adequate range and resolution, not a general limit of portable balances.
Figure 9. Bland–Altman plot comparing field (portable, 2-digit) and precision (laboratory, 4-digit) balance readings across the complete gravimetric dataset (n = 36; see text for the analysis without one anomalous reading, n = 35), by tape type. Solid line: mean bias; dashed lines: 95% limits of agreement.

3.3. Binary Image Analysis

3.3.1. Brera Academy Objects—Nitto Tape

Binary image analysis of tape strips examined by stereomicroscopy revealed marked substrate-specific differences in surface cohesion that complement and extend the gravimetric data (Table 2, Figure 10). Image analysis was performed on a representative portion of each tape strip, selected as significant and representative of the overall particle distribution; the white pixel percentages reported below refer to this analysed area rather than to the full strip surface. For the Nitto tape on Brera objects, terracotta exhibited by far the highest white pixel area across all three pulls: 15.39%, 14.26%, and 13.80% at pulls 1, 2, and 3, respectively. The relatively small decrease between pulls (approximately 1.6 percentage points from pull 1 to pull 3) indicates persistent surface fragility: the terracotta surface continues to release particles at similar rates across all three test cycles, with no sign of the marked depletion effect observed in more cohesive materials. This behaviour is consistent with the granular, loosely bound surface structure typical of deteriorated terracotta, in which weakly cohesive zones are distributed throughout the underlying surface layer rather than concentrated at the immediate surface.
Table 2. White pixel area (%) per pull for Nitto WS-1 and Tesa Sensitive 4333 tapes across all study objects.
Figure 10. Binary images of tape strips (stereomicroscope, 6.3×): (a) Terracotta (Pull 1: 15.39%), (b) Plaster 2 (Pull 1: 1.82%), and (c) Small head: Arco della Pace (Pull 1: 6.72%), tape Nitto WS-1, before consolidation. Upper row: original stereomicroscope images, with the scale bar (5 mm); lower row: binarised images of the analysed region, not at the same scale as the originals. White: detached particles; black: background.
Among the gypsum plasters, Plaster 3 showed the highest initial removal (7.89% at pull 1) and the most pronounced depletion pattern, falling to 4.34% at pull 2 and 1.56% at pull 3—a reduction of approximately 80% from the first to the third pull. This steep decrease suggests that surface fragility is largely confined to a thin, superficially disaggregated layer, beneath which cohesion improves markedly. Plaster 1 showed a similar depletion pattern (4.61%, 1.80%, 1.90%), with a sharp drop after the first pull and near-stabilisation thereafter. Plaster 2 presented the lowest and most irregular values across pulls (1.82%, 5.00%, 0.55%), with an anomalous increase at pull 2 followed by a sharp decrease at pull 3; this non-monotonic pattern may reflect local surface heterogeneity or the transient exposure of a slightly less cohesive sub-surface zone at pull 2. Plaster 2 had the lowest mean white area (2.5%, against 2.8% for Plaster 1 and 4.6% for Plaster 3), but its irregular pattern and the small difference from Plaster 1 do not allow it to be ranked with confidence as the most compact substrate.

3.3.2. Brera Academy Objects—Tesa Tape

The Tesa tape produced systematically lower white pixel values than the Nitto tape on all gypsum substrates, often approaching zero: Plaster 1 values across three pulls were 0.24%, 0.32%, 0.02%; Plaster 2 values were 0.47%, 0.44%, 0.23%; and Plaster 3 values were 0.00%, 0.24%, 0.02%. Two explanations are possible, and the present data do not discriminate between them. The first is that the Tesa tape, with its lower adhesion to steel (0.5 N/cm against 2.96 N/cm for the Nitto tape), removes fewer particles from these surfaces. The second is methodological: the binarisation separates white particles from a dark background, which suits the amber polyimide backing of the Nitto tape but may be less effective on the pale paper backing of the Tesa tape, where the contrast between particles and background is lower, so that the white area could be underestimated. The gross masses of the Tesa strips do not help to decide, because they mainly reflect the mass of the strip (Section 3.1.3). Since the threshold was set individually for each image (Section 2.3) and the segmentation has not been checked on the Tesa images (for example with a fixed threshold or a reference), the near-zero values should not be taken as evidence that the Tesa tape cannot provide diagnostic information on these substrates.
On terracotta, however, the Tesa tape produced a different pattern: white pixel areas of 8.30%, 18.82% and 22.75% across pulls 1, 2 and 3, a progressive increase rather than the slight decrease observed with the Nitto tape (Table 2). This is an observed difference; its explanation is a hypothesis that was not tested. The higher-adhesion Nitto tape may remove a large and relatively constant fraction of loosely bound particles from the first pull, whereas the lower-adhesion Tesa tape may engage the surface more gradually and reach deeper or more sheltered zones; alternatively, the increase may reflect repeated pulls on a surface that is progressively disaggregated, or differences in image contrast between the two tapes. Testing these explanations would require independent measures, such as strips pre-weighed to obtain net mass or a larger set of terracotta surfaces. The idea that the two tapes probe different layers, and that they could be used in combination, should therefore be regarded as a working hypothesis.

3.3.3. Arco Della Pace Marble Surfaces

On the Arco della Pace marble surfaces, image analysis values for the Nitto tape were intermediate and relatively stable across pulls: relief values were 6.40%, 7.73%, 6.73%, and small head values were 6.72%, 5.16%, 5.43% (Table 2). The near-constancy of these values and the slight non-monotonic pattern in both cases may reflect the greater surface complexity of in-situ marble compared to controlled laboratory specimens: environmental contamination, pre-existing microcracking and spatial heterogeneity of deterioration could contribute to variability that is not present in the Brera objects, although this was not assessed. It should be noted that some white areas observed in the marble strip images may be attributable to surface dust or external contamination rather than exclusively to cohesion-related particle removal, introducing a degree of uncertainty in the absolute values that must be considered in their interpretation.
For the Tesa tape on Arco della Pace surfaces, white pixel values were consistently low throughout: relief pulls yielded 0.31%, 0.23% and 0.10%, and small head pulls 0.10%, 0.08% and 0.08% (Table 2). The relief values decrease across pulls, but by very small amounts. These low Tesa values are in line with those observed on gypsum substrates; as discussed in Section 3.3.2, they may reflect either a limited ability of the tape to engage compact, coherent surfaces or a lower image contrast on the paper backing, and the two explanations were not distinguished.

4. Discussion and Conclusions

The Tape Test gives two complementary kinds of information on surface cohesion: gravimetry, which tells how much material came off, and binary image analysis, which tells where and in what form. In the present study only the second was obtained quantitatively, because the strips were not weighed individually before use.
The pooled Bland–Altman analysis (n = 36 paired readings, both tape types and both sites; Section 3.2) shows that the field and precision balances are not interchangeable: mean bias +0.0107 g, 95% limits of agreement from −0.0205 to +0.0419 g, against strip gross masses of 0.03–0.07 g (paired t-test and Wilcoxon signed-rank test, p < 0.001; descriptive, as the pairs are not independent). All field readings were multiples of 0.02 g, which is too coarse for the mass increments involved in Tape Test gravimetry, where the net mass of collected particles is expected to be small compared with the mass of the strip.
The main methodological lesson of this study is that strips should be cut to a fixed, measured size, pre-weighed individually on a precision balance before use, and re-weighed after testing so that net mass and mass per unit contact area can be calculated. In this study the strips were cut by hand in situ (tolerance 0.1–0.5 cm) and weighed only after use, so only gross mass is available. The strip-to-strip variability (SD of about 2–5 mg) is comparable with the differences observed between substrates. We propose pre-weighing as a requirement of a pre-normative protocol, not as a procedure carried out here.
The gross masses of the two tapes differ (Tesa 0.0583 g and Nitto 0.0326 g on average), but this reflects the mass of the strips and not the amount of material removed, so no gravimetric ranking of the tapes is made. The two tapes did differ strongly in image analysis: with the Nitto tape the white pixel area ranged from 0.55% to 15.4%, whereas with the Tesa tape it was below 1% on gypsum plaster and marble and reached 22.8% only on terracotta. Whether the low Tesa values reflect a weak engagement of compact surfaces (lower tack or backing) or a lower optical contrast of the pale paper backing in the binarisation was not tested. The choice of tape should be guided by the diagnostic question and requires further validation.
Image analysis adds something gravimetry cannot: terracotta’s persistently high removal (>13% across all three pulls) looks very different from Plaster 2′s low values (0.55–5.00%), and that contrast is visible before any numbers are calculated. The divergent Nitto and Tesa responses on terracotta, stable vs. progressively increasing, may reflect a different engagement of the surface layers by the two tapes (a hypothesis that was not tested). Whether using both tapes together gives more information than either alone remains to be verified.
The effect of DAP consolidation could not be evaluated, because post-treatment measurements are not available. In future evaluations of consolidation treatments, Tape Test data on treated surfaces should not be read in isolation: without knowing how deep the consolidant penetrated and how it distributed within the stone matrix, a surface cohesion measurement can only tell part of the story. Drilling Resistance Measurement System (DRMS) and Ultrasonic Pulse Velocity (UPV) testing remain necessary for in-depth assessment.
The Tape Test answers a specific diagnostic question, the cohesion of the outermost layer of a surface, and should be distinguished from the mechanical and material performance assessments used in conservation engineering, which concern bulk strength, stiffness, porosity or durability (for example, the mechanical tests used to design and verify the strengthening of heritage masonry [25]). In the evaluation of a consolidation treatment, surface cohesion is one element of a wider framework that includes the characterisation of the original materials [26], the compatibility of the intervention and its long-term performance. Field studies of phosphate treatments on marble, for example, combine non-destructive and microstructural methods with the monitoring of treated specimens and of a sculpture over three years of exposure [27]; the Tape Test could complement such an approach at the surface level but not replace it.
The pre-normative criteria suggested by this study are strips cut to a fixed and measured size (3 cm length; width to be reported), pre-weighed individually and re-weighed after testing on a precision balance (4-digit, ±0.0001 g), with results expressed as net mass and as mass per unit contact area; five roller passes, 10 s adhesion, removal at 90° (as close as practicable), and three pulls per area; and binary image analysis by stereomicroscopy and ImageJ, with image acquisition and segmentation parameters kept constant and reported. The requirement for a precision balance is supported by the comparison of the two balances in Section 3.2. A recommendation on tape type is deferred: the present data do not allow the Nitto and Tesa tapes to be ranked gravimetrically, and the Tesa binarisation results require further validation.
The sample size is small; most surfaces were tested under a single condition, consecutive pulls are not independent repetitions (each act on a surface modified by the previous one), and the strips were not individually pre-weighed, so net mass is not available—the limitations are real. The procedure should be regarded as a promising pre-normative contribution requiring interlaboratory validation before its adoption as a standard. Future work should extend the evidence base to a larger number of objects and lithotypes, incorporate artificial ageing conditions, and evaluate the Tape Test alongside complementary techniques such as DRMS and UPV to address in-depth consolidation effects. Tape Test data should also be interpreted in conjunction with information on consolidant penetration depth and spatial distribution within the stone matrix, as surface cohesion measurements alone may not fully capture the effectiveness of treatments with variable penetration profiles such as DAP. These are the obvious next steps toward a CEN TC 346/WG3-compatible standard.

Supplementary Materials

The following supporting information can be downloaded at https://www.mdpi.com/article/10.3390/heritage9120499/s1: Figure S1: tesa® Professional 4333 Precision Mask® Sensitive—Product Information datasheet; Figure S2: Nitto WS-1 (1-Mil Polyimide Film)—Product Data Sheet; Table S1: Dataset and statistics (gross masses of the strips, variability, agreement between the two balances and image-analysis values); Code S1: Python script for the statistical analysis and for Figure 4, Figure 5, Figure 6, Figure 7, Figure 8 and Figure 9.

Author Contributions

Conceptualization, A.E. and A.S.; Methodology, A.E.; Formal Analysis, A.E.; Investigation, A.E.; Writing—Original Draft Preparation, A.E.; Writing—Review and Editing, L.R., S.R. and V.F. (normative context); Resources, R.M.D.F., B.S. and E.V. (laboratory support); Supervision, M.G. and A.S. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Data Availability Statement

The gravimetric dataset and the analysis script are provided as Supplementary Materials (Table S1 and Code S1). The ImageJ analysis results and the original micrographs are available from the corresponding author upon reasonable request.

Acknowledgments

The authors thank the Brera Academy of Fine Arts, Milan, for granting access to the study objects, and ISPC-CNR for laboratory support. This research was developed within the Master’s thesis of A.E. at the State University of Milan (supervisor: M. Gargano; co-supervisor: A. Sansonetti).

Use of Artificial Intelligence Tools

During the preparation of this manuscript, the authors used Claude (Anthropic, San Francisco, CA, USA; see Section 2.3) for language editing and for writing and executing the statistical analysis code (paired t-test, Wilcoxon signed-rank test, Bland–Altman analysis, Pearson correlation, Spearman correlation) in Python. The authors have reviewed and edited the output and take full responsibility for the content of this publication.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Tabasso, M.L. Il consolidamento dei materiali porosi: Sviluppo storico del concetto, prodotti usati nel passato, tendenze attuali [The consolidation of porous materials: Historical development of the concept, past products and current trends]. Rendiconti dell’Accademia Nazionale delle Scienze detta dei XL 2000, XXIV, 117–133. [Google Scholar]
  2. Giorgi, R.; Dei, L.; Baglioni, P. A new method for consolidating wall paintings based on dispersions of lime in alcohol. Stud. Conserv. 2000, 45, 154–161. [Google Scholar] [CrossRef] [Scilit]
  3. Daniele, V.; Taglieri, G. Nanolime suspensions applied on natural lithotypes: The influence of concentration and residual water content on carbonatation process and on treatment effectiveness. J. Cult. Herit. 2010, 11, 102–106. [Google Scholar] [CrossRef] [Scilit]
  4. Sasse, H.R.; Snethlage, R. Methods for the evaluation of stone conservation treatments. In Saving Our Architectural Heritage: The Conservation of Historic Stone Structures; Baer, N.S., Snethlage, R., Eds.; John Wiley & Sons: Chichester, UK, 1997; pp. 223–243. [Google Scholar]
  5. Doehne, E.; Price, C.A. Stone Conservation: An Overview of Current Research, 2nd ed.; Getty Conservation Institute: Los Angeles, CA, USA, 2010. [Google Scholar]
  6. EN 16581:2014; Conservation of Cultural Heritage: Surface Protection for Porous Inorganic Materials—Laboratory Test Methods for the Evaluation of the Performance of Water Repellent Products. CEN: Brussels, Belgium, 2014.
  7. Mora, P.; Torraca, G. Fissativi per dipinti murali. Bollettino dell’Istituto Centrale del Restauro 1965, 109–132. [Google Scholar]
  8. Drdácký, M.; Lesák, J.; Rescic, S.; Slížková, Z.; Tiano, P.; Valach, J. Standardization of peeling tests for assessing the cohesion and consolidation characteristics of historic stone surfaces. Mater. Struct. 2012, 45, 505–520. [Google Scholar] [CrossRef] [Scilit]
  9. Urzì, C.; De Leo, F. Sampling with adhesive tape strips: An easy and rapid method to monitor microbial colonization on monument surfaces. J. Microbiol. Methods 2001, 44, 1–11. [Google Scholar] [CrossRef] [Scilit]
  10. Bartůněk, V.; Varadzin, L.; Zavřel, J. Carbon tape microsampling for non-destructive analyses of artefacts. Archaeol. Anthropol. Sci. 2018, 10, 2173–2177. [Google Scholar] [CrossRef] [Scilit]
  11. Drdácký, M.; Slížková, Z. In situ peeling tests for assessing the cohesion and consolidation characteristics of historic plaster and render surfaces. Stud. Conserv. 2015, 60, 121–130. [Google Scholar] [CrossRef] [Scilit]
  12. Drdácký, M.; Lesák, J.; Niedoba, K.; Valach, J. Peeling tests for assessing the cohesion and consolidation characteristics of mortar and render surfaces. Mater. Struct. 2015, 48, 1947–1963. [Google Scholar] [CrossRef] [Scilit]
  13. Tiano, P.; Cantisani, E.; Sutherland, I.; Paget, J.M. Biomediated reinforcement of weathered calcareous stones. J. Cult. Herit. 2006, 7, 49–55. [Google Scholar] [CrossRef] [Scilit]
  14. Drdácký, M.; Slížková, Z. Enhanced affordable methods for assessing material characteristics and consolidation effects on stone and mortar. J. Geophys. Eng. 2013, 10, 064005. [Google Scholar] [CrossRef] [Scilit]
  15. Becerra, J.; Ortiz, P.; Martín, J.M.; Zaderenko, A.P. Nanolimes doped with quantum dots for stone consolidation assessment. Constr. Build. Mater. 2019, 199, 581–593. [Google Scholar] [CrossRef] [Scilit]
  16. ASTM D3359-23; Standard Test Methods for Rating Adhesion by Tape Test. ASTM International: West Conshohocken, PA, USA, 2023.
  17. ASTM D4214-07; Standard Test Methods for Evaluating the Degree of Chalking of Exterior Paint Films. ASTM International: West Conshohocken, PA, USA, 2015.
  18. ASTM D903-98; Standard Test Methods for Peel or Stripping Strength of Adhesive Bonds. ASTM International: West Conshohocken, PA, USA, 2017.
  19. Fassina, V.; Sansonetti, A. The European TC 346/WG3 standards on the evaluation of conservation works. In Proceedings of the International Symposium “Stone Consolidation in Cultural Heritage” (Consolidation 2021), Lisbon, Portugal, 23–25 March 2022; LNEC: Lisbon, Portugal, 2022. [Google Scholar]
  20. Chiche, A.; Zhang, W.; Stafford, C.M.; Karim, A. A new design for high-throughput peel tests: Statistical analysis and example. Meas. Sci. Technol. 2005, 16, 183–190. [Google Scholar] [CrossRef] [Scilit]
  21. Defus, A.; Sansonetti, A.; Possenti, E.; Tedeschi, C.; Vettori, S.; Realini, M. The effectiveness of di-ammonium hydrogen phosphate (DAP) consolidation treatment on lime-based mortars weathered by freeze-thaw cycles. J. Cult. Herit. 2021, 50, 1–12. [Google Scholar] [CrossRef] [Scilit]
  22. Murru, A.; Fort, R. Diammonium hydrogen phosphate (DAP) as a consolidant in carbonate stones: Impact of application methods on effectiveness. J. Cult. Herit. 2020, 42, 45–55. [Google Scholar] [CrossRef] [Scilit]
  23. Nitto Denko Corporation. Product Data Sheet: WS-1—1-Mil Polyimide Film Tape (Document Code: PDS-WS-1-01-20). Available online: https://www.nitto.com/eu/de/others/products/file/datasheet/PDS_NA_1Mil_Polymide_Film_WS-1_012020_EN.pdf (accessed on 5 November 2026).
  24. tesa SE. Product Information: Tesa® Professional 4333 PV1 Precision Mask® Sensitive. Available online: http://l.tesa.com/?ip=04333 (accessed on 5 November 2026).
  25. Liberotti, R.; Cluni, F.; Gusella, V.; Lourenço, P.B. The Green Tape project: “In falso” walls strengthening through natural FRCM innovative techniques. Eng. Struct. 2025, 345, 121459. [Google Scholar] [CrossRef] [Scilit]
  26. Demirel, M.; Topsakal, A.; Altun, M.G. Materials characterization of historical structures: A review. Front. Struct. Civ. Eng. 2025, 19, 1461–1477. [Google Scholar] [CrossRef] [Scilit]
  27. Sassoni, E.; Delhomme, C.; Forst, S.; Graziani, G.; Henin, J.; Masi, G.; Palazzo, A.; Rolland, O.; Verges-Belmin, V. Phosphate treatments for stone conservation: 3-year field study in the Royal Palace of Versailles (France). Mater. Struct. 2021, 54, 140. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations