Skip to Content
  • Editor’s Choice
  • Article
  • Open Access

9 April 2026

28 Pages

Defect Monitoring of Complex Geometries Through Machine Learning in LPBF Metal Additive Manufacturing

,
and
Department of Mechanical Engineering, McMaster University, Hamilton, ON L8S 4L7, Canada
*
Author to whom correspondence should be addressed.

Abstract

Laser powder bed fusion (LPBF) can fabricate intricate metal components but is prone to defects, such as porosity and cracks, that degrade performance. We present an in situ monitoring framework that fuses structure-borne acoustic emission (AE) and coaxial two-color pyrometry acquired synchronously at 1 MHz. Modality-specific encoders are pretrained separately, their latent representations are exported, and a lightweight feature-level fusion classifier with two binary heads predicts crack-like and porosity-like indications. Evaluation uses a held-out grouped experiment/build-machine-part split with independent Archimedes density and micro-CT ground truth. On the held-out test set, the fused model achieved F1 = 0.974 for crack-like detection and F1 = 0.987 for porosity-like detection, with AUROC = 0.998 and 0.993, respectively. Recall was 1.00 for both heads, corresponding to false-positive rates of 11.18% for crack-like and 0.945% for porosity-like indications. These results support synchronized AE-pyrometry fusion as a promising high-sensitivity in situ screening approach for LPBF. A later matched within-framework ablation campaign was also performed under stricter checkpoint-screening rules to compare AE + PY + Aux, AE + PY, AE-only, and PY-only variants under a common grouped-split protocol. Together, these results support multimodal monitoring while highlighting the need for explicit coupon/geometry-stratified reporting and for separately architecture-optimized unimodal baselines.

1. Introduction

Laser powder bed fusion (LPBF) enables the manufacture of complex metal components, yet process non-idealities produce defects such as porosity and cracks, which degrade mechanical performance and fatigue life [1,2]. Reliable in situ monitoring is, therefore, essential [3]. Structure-borne acoustic emission (AE) is sensitive to transient elastic events associated with cracking and unstable consolidation [4], whereas coaxial two-color pyrometry provides a high-rate thermal proxy of melt-pool behavior with reduced sensitivity to emissivity variation [5]. Because these modalities observe complementary elastic and thermal phenomena, they are natural candidates for feature-level fusion [6].
Prior AE-based evaluations of practical geometries suggest that performance can degrade when geometry changes sensing conditions, particularly in overhang regions and other boundary-sensitive features. Geometry modifies AE propagation and coupling and also changes local thermal conditions that influence pyrometer signatures [4,7]. These observations motivate the introduction of complementary sensing and a geometry-aware experimental design.
The present study focuses on defect detection using fused sensing. We integrate structure-borne AE with coaxial two-color pyrometry on a production LPBF platform and acquire synchronized 1 MHz data with independent Archimedes density and micro-CT ground truth. The current manuscript reports aggregate held-out crack-like and porosity-like detection on a geometry-diverse coupon set spanning overhangs, wall-thickness variation, horizontal channels, and support conditions.
This work advances in situ defect detection for LPBF through a reproducible acquisition and data-engineering pipeline, a geometry-diverse experimental design, and a downstream feature-level fusion classifier operating on pretrained modality-specific latent representations. The study is deliberately structured so that matched unimodal baselines and later geometry-stratified evaluation can be reported under the same grouped split protocol.

2. Background and State of the Art

2.1. Defect Formation Mechanisms in LPBF

2.1.1. Porosity Formation

The porosity formation mechanism and its undesirable effects have been investigated frequently in the literature [8]. The presence of porosity can affect the mechanical integrity and, thereby, the fatigue life of LPBF parts [9]. Figure 1 illustrates how process-parameter choice influences the type of porosity formed in an aluminum alloy manufactured by LPBF [10]. Generally, porosity has multiple classifications and can quickly be classified according to its geometry, both spherical and non-spherical.
Figure 1. Typical types of porosity formed under different process parameters [10].
Gas entrapped in powder particles during the gas atomization process contributes to gas-induced pores [11], which are spherical in nature. These spherical porosities can also be attributed to the vaporization of low-melting-point elements during the LPBF process [12]. Process-induced porosity formation mechanisms are mainly attributed to a lack of fusion and keyholing [13] and are non-spherical in nature. The lack of fusion mechanism affecting porosity is related to the insufficient overlap of successive melt pools [14]. Therefore, powder remains unmelted, causing a reduction in the overall density of the part. In contrast, the keyholing mechanism is caused by the significantly higher laser beam power that causes the metal evaporation and leads to the formation of plasma [2]. This causes the laser beam to penetrate the melted part deeply and forms a vapor cavity within the part [15].

2.1.2. Crack Propagation

The LPBF process is governed by extremely fast cooling rates (around 105°Ks−1), resulting in a large temperature gradient around the melt-pool [16]. This leads to residual stresses, which affect both micro- and macrocrack formation, as illustrated in Figure 2. The nature and degree of crack formation are dependent on both the LPBF process parameters and the material being used. DebRoy et al. [1] identified three types of cracks that can be observed in metal AM parts: solidification cracking, liquation cracking, and delamination.
Solidification cracking can be observed along the grain boundaries and is usually attributed to shrinkage and thermal contraction. Liquation cracking is related to the presence of liquid films [17] and is more common in alloys exhibiting high-temperature differences between the liquids and solidus, a large melt-pool size, or large thermal contractions. Delamination occurs when the residual stresses at the layer interface exceed the yield strength of the alloy [18]. It may occur between the part and the build plate or between two successive layers.
While pre-heating the build plate is a common mitigation strategy that might reduce the probability of crack and delamination formation, it is limited in its ability to do so. Therefore, acoustic emission sensors can be beneficial in the online detection of crack formation during the LPBF of metals [19].
Figure 2. Optical micrographs showing crack formations in a B4C/Ti64 composite processed by ev of: (d) 33, and (e) 297 J/mm3 [20].

2.2. In Situ Monitoring for Defect Detection

In situ monitoring for LPBF employs multiple sensing families to observe defect-relevant phenomena during exposure [3]. Visual sensing captures melt-pool size, spatter, and surface anomalies. Thermal sensing includes pyrometers and infrared imaging. Spectral sensing uses photodiodes or spectrometers to measure broadband optical emission, while acoustic sensing uses acoustic emission (AE) transducers to record elastic waves produced by rapid stress changes [4]. Together, these modalities cover complementary aspects of melt-pool behavior, powder dynamics, and part consolidation. Data volumes and rates preclude manual analysis, which motivates the use of machine learning to extract regularities from multi-sensor streams and to map signatures to defect indicators [3].
Within this landscape, AE and two-color pyrometry are particularly aligned with the defects of interest in this work. AE is sensitive to transient events linked to lack of fusion and crack initiation, and structure-borne installation on or within the build plate enables broadband capture with practical integration [4]. Two-color pyrometry mitigates emissivity variation and yields a fast scalar thermal proxy of the melt pool [5], which correlates with regimes that drive porosity and melt-pool instability [21]. Focusing on AE and pyrometry, therefore, targets complementary physical mechanisms underlying porosity and cracks while remaining compatible with high-rate acquisition and learning-based detection [6]. This is summarized in Table 1.
Table 1. In situ sensors for defect detection in L-PBF.

2.3. Acoustic Emission Techniques

Acoustic emission (AE) monitoring records transient elastic waves generated by rapid stress changes in the workpiece [4]. In LPBF, relevant sources include plastic deformation, microcrack initiation and growth, lack-of-fusion events, and keyhole dynamics [2,4]. AE is typically acquired as a structure-borne signal using piezoceramic transducers mounted on or within the build plate, which provides a broad usable bandwidth and practical integration in the build environment [4].
Effective pipelines begin with denoising and band-limiting, followed by segmentation into windows aligned to exposure events or fixed durations [19]. Representations commonly include time-domain waveforms for low-latency decisions, frequency-domain features computed via the fast Fourier transform (FFT) or discrete cosine transform (DCT), and time–frequency maps such as short-time Fourier transform (STFT) or wavelet spectrograms [29]. These representations serve as inputs to learning models and support normalization across builds and locations [19].
Reported approaches range from classical multilayer perceptrons (MLPs) and support vector machines (SVMs) to deep belief networks (DBNs) and convolutional neural networks (CNNs) trained on FFT, STFT, or wavelet features [29,30]. Across datasets and geometries, studies typically report accuracies in the ~70–90 percent range for defect or regime discrimination, with degraded performance observed for complex geometries or altered boundary conditions; encoder-based dimensionality reduction and feature learning have been used to improve robustness [4,19].
Given AE’s sensitivity to microcracking and lack-of-fusion phenomena and the demonstrated effectiveness of spectral and time–frequency representations with learned encoders, AE is a strong complementary modality to pyrometry for detecting porosity- and crack-related indications within the fused-sensor framework adopted in this work [4,6].
Representative AE-based LPBF defect-detection studies, including their target defect classes, signal-processing pipelines, machine-learning approaches, and reported findings, are summarized in Table 2.
Table 2. Acoustic emission (AE)-based defect detection studies.

2.4. Pyrometry Techniques

Pyrometry provides a fast, non-contact proxy of melt-pool temperature by measuring thermal radiation from the processing zone [16]. In LPBF, sensors may be deployed coaxially to the laser path, enabling tracking at any build location, or off-axis at a viewport to observe a fixed field of regard [5]. Two-color (ratio) pyrometers are frequently preferred because the ratioing of two spectral bands reduces sensitivity to unknown or changing emissivity, plume, and view-factor effects that complicate single-band measurements [5,16].
Practical acquisition typically yields a single high-rate scalar time series per channel [5]. Common preprocessing steps include removal of spurious spikes, baseline detrending, normalization across layers or scan vectors, and segmentation by exposure event or layer to align samples with process actions [21,33]. Feature construction then proceeds from windowed statistics and simple dynamics, for example, means, variances, ranges, slopes, and dwell-time surrogates that capture the thermal consistency of the melt track or layer [21,33]. These representations are lightweight, compatible with high data rates, and provide well-behaved inputs to standard classifiers; studies report effective use of both engineered features and compact 1D CNNs for classification of pyrometer streams [3,33].
Reported machine-learning approaches span linear and kernel methods through shallow neural networks and compact CNNs. Representative results include density prediction and pore or cavity detection using SVM, MLP, K-NN, logistic regression, and 1D CNNs with accuracies in the 80 to mid-90 percent range, depending on sensor placement, sampling, and labeling strategy [21,33]. Layer-scale thermal imaging can achieve similar accuracies for certain defect types, though at lower temporal resolution [33]; photodiodes remain a lower-cost alternative for temperature-related signals but sacrifice spatial context [34]. These comparisons position two-color pyrometers as a strong choice when a scalar, high-rate thermal proxy is needed to complement other sensors [5,21].
Limitations of pyrometry arise from its point-like nature and dependence on optical access. Single-wavelength devices are further affected by emissivity variation, whereas two-color instruments mitigate this through ratioing and are, therefore, preferred for robust monitoring of production machines [5,16]. When paired with independent ground truth and synchronized with other modalities, pyrometers have been shown to support the reliable classification of build quality and anomaly detection in LPBF [6,21].
In our setting, pyrometry is treated as a complementary channel to AE: it captures thermal regimes associated with lack of fusion and instability while remaining compatible with high-rate acquisition and feature-level fusion for defect classification [6,34]. This role leverages the strengths of two-color sensing and aligns with the literature, which reports gains from simple, robust features and supervised classifiers on pyrometer data [21].
Representative pyrometry-based LPBF defect-detection studies, including sensor configuration, target defect type, learning approach, and reported performance, are summarized in Table 3.
Table 3. Pyrometry-based defect detection studies.

2.5. Limitations of Single-Sensor Approaches

Single-sensor monitoring provides valuable but incomplete views of the LPBF process. Each modality observes a restricted set of phenomena and is subject to mode-specific sensitivities that limit standalone defect-detection performance, particularly under changing geometries and process conditions [3].
AE measures elastic waves generated by rapid stress changes, which makes it responsive to microcracking and lack-of-fusion events [4]. However, structure-borne signals depend on the coupling path from the source to the transducer and on the mechanical boundary conditions of the build plate and part; attenuation and dispersion in the substrate filter higher frequencies and distort waveforms, while reflections from fixtures and walls complicate source interpretation [4]. Overlapping sources during rastering can produce mixed signatures that are difficult to separate with time-domain features alone; segmentation and spectral representations are typically required [19]. Air-borne microphones avoid plate coupling but suffer greater damping and ambient noise [30]. In practice, AE is sensitive to geometry through changes in propagation, damping, and mode conversion, which can reduce the generalization of models trained on simple test artifacts [4,7].
Two-color instruments mitigate emissivity variation, yet pyrometry remains a point measurement with limited spatial context. The signal is line of sight and can be affected by plume, spatter, and window contamination, which introduce transient losses or bias; optical alignment and spot size influence the degree to which the melt pool rather than the surrounding halo is measured [5,16]. Variations in alloy surface conditions and oxidation can influence apparent radiance even for ratio methods [16]. As a scalar channel, pyrometry captures thermal trends but cannot alone disambiguate the mechanical events associated with crack formation [5].
Vision and infrared imaging provide spatial context but often at lower temporal resolution and substantial data volume and are sensitive to illumination, focus, and soot accumulation [33]. Spectral or photodiode channels capture broadband emissions related to process stability but are indirect with respect to specific defect mechanisms and can be confounded by plume dynamics [34].
These limitations are complementary rather than redundant. AE is most sensitive to elastic events associated with cracks and lack of fusion, while pyrometry captures thermal regimes associated with porosity-prone processing and melt-pool instability. Neither modality alone robustly separates all relevant defect states across geometries and operating conditions. This motivates approaches that combine modalities at the feature level so that weaknesses in one channel are offset by strengths in the other [6,34].

2.6. Sensor Fusion in the Literature

Published LPBF monitoring studies have combined complementary modalities to improve defect observability. Representative configurations include thermal–acoustic pairings (coaxial pyrometry with AE), thermal imaging, and broader heterogeneous sensing frameworks [34]. In defect-detection settings, fusion is typically implemented at the feature level or decision level or through hybrid architectures [34,38]. Representative machine learning studies include localized keyhole pore identification from pyrometry and acoustics [6], heterogeneous multiscale flaw detection [38], feature-level multi-sensor fusion [39], and deep learning-based data fusion for porosity detection [40].
In defect-detection contexts, fusion is typically implemented at three levels: (i) feature-level (early) fusion, in which per-sensor features or learned encodings are concatenated and passed to a common classifier; (ii) decision-level (late) fusion, which aggregates per-sensor predictions through voting or weighting; and (iii) hybrid or latent fusion, which learns shared representations while retaining sensor-specific branches [34,38,39]. In this work, we adopt feature-level fusion: AE and pyrometer streams are processed by modality-appropriate encoders, and the resulting latent features are concatenated for classification, balancing model capacity, data efficiency, and interpretability [34,38,39].
Related work has shown that in-process signals can encode geometry or source-position context even when direct defect detection is not the target. In EDM, geometry-mediated process signatures have been classified directly from in-process monitoring data [41]. In LPBF, AE frequency features have been used to identify source-motion and positioning effects associated with laser movement patterns, baseplate thickness, and printing position [42]. The present study differs in objective and validation: rather than classifying geometry or contextual factors themselves, it uses a geometry-diverse coupon set and grouped experiment/build/machine/part splits to evaluate whether synchronized AE and coaxial two-color pyrometry can support defect screening against independent Archimedes density and micro-CT ground truth. The contribution is, therefore, not simply to show that geometry affects process signals but to incorporate geometry variation into a multimodal defect-detection workflow with independent defect labels and leak-resistant evaluation.

2.7. Impact of Complex Geometries on Defect Detection

Complex geometries alter the observability of defect signatures and the distribution of sensor features used for classification [7,33]. In a prior evaluation of a practical wishbone, the AE-based model sustained high success rates in solid regions and in a band with induced porosity, but accuracy decreased in layers corresponding to a 45-degree overhang, indicating a geometry-specific shift in the recorded signatures and a gap in the training distribution. Similar behavior appears in published studies that report lower AE classification accuracy for complicated shapes relative to simple coupons [4,30]. Together, these results show that geometry can change both propagation and coupling for elastic signals and can influence thermal conditions that correlate with porosity and cracking, which in turn affects learned decision boundaries [2,4,33].
These observations motivate geometry-aware datasets and evaluation protocols in which each coupon isolates a specific feature condition, and grouped results can later be interpreted at the coupon or geometry level. In the present study, the DOE covers overhangs, wall-thickness variation, horizontal channels, and support conditions, paired with independent ground truth. This structure is intended to expose geometry sensitivity, support later stratified analysis under a common grouped-split protocol and provide a basis for assessing whether fused sensing remains more stable than single-modality models when sensing conditions change with part geometry.

3. Experimental Setup

3.1. Platform and Materials

Experiments were conducted on a production laser powder bed fusion (LPBF) system manufactured by Omnitek in São Paulo, Brazil and later configured for multi-sensor acquisition. The study employs coupons in Inconel 625 designed to elicit porosity- and crack-related behavior under varied geometry. Build files were prepared to produce both nominally sound and intentionally degraded material conditions, with geometry features selected to probe observability in regions known to be challenging for single-sensor detection. Section 5 details coupon families and ground-truth procedures.
Environmental and machine practices were held constant across builds to reduce run-to-run variability. Powder handling and recoating procedures followed routine production practices, chamber pressure and gas flow were verified prior to exposure, and build-plate preparation and alignment were repeated according to a fixed checklist. These controls supported consistent sensing conditions for the comparative analyses that follow.

3.2. AE Sensing

Acoustic emission (AE) monitors elastic waves generated by rapid stress changes and is aligned with events associated with lack of fusion and crack initiation.
A structure-borne piezoceramic transducer, was mounted within the build plate to maximize coupling and usable bandwidth while limiting variability in the acoustic path. Contact surfaces were cleaned and re-wetted prior to installation to maintain coupling. Cable runs were strain-relieved and routed away from moving assemblies and power electronics to reduce mechanically induced and electromagnetic noise.
AE was sampled continuously at 1 MHz to preserve transient content without trigger bias. Continuous acquisition avoided loss of short-duration events and simplified alignment with other channels. Channel integrity and synchronization were verified prior to data collection. Periodic health checks (baseline noise floors, clipping detection, and channel-to-channel phase agreement on test impulses) were performed at the start of each build.
Nonparticipating hardware was mechanically isolated where practical, and fixtures were inspected between builds. These measures reduced confounding signatures and improved comparability across datasets.
The acoustic-emission measurements were acquired using a Physical Acoustics WSα wideband AE sensor (100–1000 kHz), sourced from Physical Acoustics/MISTRAS, Princeton Junction, NJ, USA.

3.3. Coaxial Two-Color Pyrometry

Two-color pyrometry provides a non-contact proxy of melt-pool temperature and reduces sensitivity to emissivity variation through ratio measurements.
The pyrometer was integrated coaxially to follow the scan path and maintain a stable view factor across the field. Optical alignment and spot size were selected to favor melt-pool sensitivity while avoiding saturation from the process plume. Optical cleanliness was checked before each build, and window condition was monitored to minimize attenuation changes over time.
The pyrometer output was sampled at 1 MHz and recorded synchronously with AE. Prior to production runs, analogue output stability, alignment, and timing were verified. Short calibration sequences were used to confirm repeatable signal levels under fixed exposure patterns.
Routine checks confirmed stable analogue output after warm-up. Any observed drift or spiking led to a repeat of alignment and cleaning procedures before proceeding.
The coaxial thermal measurements were acquired using a Sensortherm METIS H322 high-speed two-color pyrometer, sourced from Sensortherm GmbH, Steinbach, Germany.

3.4. Hardware Modifications

Coaxial integration of the pyrometer required IR-compatible scan optics that provide adequate transmission in the pyrometer detection band while preserving laser performance at the processing wavelength. The original galvo mirrors and F-Theta lens attenuated the target wavelength band, preventing reliable temperature measurement. The system was upgraded with components providing adequate transmission in the pyrometer band while preserving laser efficiency at the processing wavelength. After mechanical and optical integration, alignment and calibration confirmed stable, high-rate temperature acquisition suitable for analysis.

3.5. DAQ Hardware

A dedicated multi-sensor data acquisition system provided synchronized capture from acoustic emissions and two-color pyrometer channels at 1 MHz per sensor. The DAQ accepted a digital exposure signal from the machine controller, which was recorded alongside the sensor streams as a reliable time reference for alignment. Channel synchrony and sustained 1 MHz operation were verified prior to data collection using short test exposures and loopback checks. The system stored raw, time-stamped waveforms with build identifiers and coupon metadata to support subsequent segmentation, labeling, and analysis.
The dedicated multi-sensor data-acquisition platform used in this study, including the custom acquisition hardware and supporting software, was developed by Pegmatis Inc. from Burlington, ON, Canada.

4. Data Acquisition and Synchronization

This section details the procedures used to align, segment, label, and persist synchronized AE and pyrometer signals for defect-detection analysis.

4.1. Signal Alignment and Timestamping

All analogue channels were sampled at 1 MHz per sensor from a common DAQ time base. The digital exposure line from the machine controller was recorded as a discrete channel and used as the primary reference to align sensor data with commanded laser activity.
Each sample carried a DAQ-domain timestamp. Exposure rising and falling edges were detected during ingestion and indexed. These indices provided deterministic boundaries for later segmentation at the vector, hatch, or layer level.
A short pre-build test sequence established any fixed offset between AE and pyrometer channels. The measured offset was removed so that both streams shared a consistent time origin. Phase agreement was confirmed by cross-checking the response to repeated known exposure patterns.
Clock drift was monitored over each build by comparing exposure-edge intervals in the sensor streams with the controller’s nominal timing. No material drift was observed over the acquisition intervals used; if detected, a linear correction would be applied to the timestamps before segmentation.
A run manifest recorded channel mapping, sampling settings, exposure polarity, build identifiers, and coupon metadata. This manifest accompanied every data file and served as the source of truth for downstream labeling.

4.2. Segmentation and Labeling

Two complementary schemes were used:
  • Exposure-aligned segments. Windows bounded by exposure edges, suitable for vector- or hatch-level analysis and for pairing with build-log events.
  • Fixed-duration segments. Constant-length windows for background estimation or models that expect uniform tensor sizes.
Unless otherwise stated, exposure-aligned windows were padded symmetrically by a short context on either side to capture transient onset and decay. Fixed-duration windows were advanced with controlled overlap to balance sample count and independence.
Each segment inherited labels from the run manifest and exposure index: build ID, coupon ID, geometry feature (for example, overhang, wall thickness, channel, and supports), layer number, segment type, and sensor modality. Ground-truth outcomes from Archimedes density and micro-CT were associated at the coupon or region level and propagated to the relevant segments.
To reduce run-to-run variability, channel amplitudes were normalized prior to feature construction. AE used a robust scaling based on per-build median and interquartile range. Pyrometer signals used baseline subtraction with per-build scaling so that models consumed relative thermal trends rather than absolute values. Normalization parameters were stored with the dataset for exact reproducibility.

4.3. Pipelines and Throughput

High-rate streams were buffered in memory and written to disk in contiguous chunks, while the exposure channel was processed in parallel to emit an event index for all later stages. This design sustained continuous capture without gaps and kept latency low for integrity checks.
A lightweight index recorded exposure-edge positions and timestamps, enabling random access to specific vectors or layers without rescanning the full stream.
Sustained rates and storage planning. At 1 MHz with 16-bit samples, a single channel produces 1,000,000 samples/s × 2 bytes/sample = 2,000,000 bytes/s ≈ 2 MB/s.
Over one hour: 2 MB/s × 3600 s = 7.2 GB/hour per channel.
Two channels with the same settings yield 14.4 GB/hour; four channels yield 28.8 GB/hour. With 32-bit samples, these figures double. Chunking and manifest-based indexing kept large datasets tractable without sacrificing fidelity.

4.4. Data Quality Checks

The system monitored ADC saturation, missing or malformed exposure edges, dropouts, and buffer overruns. Any alert triggered an immediate stop and repeat after remediation.
Automated checks verified: (i) equal channel lengths within tolerance; (ii) exposure-edge counts consistent with build logs; (iii) alignment of segment boundaries across modalities; (iv) absence of NaNs or clipped regions; and (v) integrity hashes for all chunks.
For each build, a small number of segments were visualized from both modalities with exposure overlays to confirm alignment and expected dynamics. Discrepancies prompted re-ingestion or re-segmentation before inclusion in analysis datasets.

5. Designed Experiments (DOE)

This section describes the coupon families, defect classes, and geometric features used to generate a geometry-aware dataset for in situ defect detection. Ground-truth procedures and the approach to evaluating signature consistency across replicates are also defined.

5.1. Coupon Designs

Coupons were printed to span both material quality and geometric complexity. The DOE includes (i) density-controlled Inconel 625 cubes for defect class separation, and (ii) feature-specific artifacts that isolate overhangs, wall-thickness variation, horizontal channels, and support strategies.

5.1.1. Defect Classes

Baseline cubes were manufactured at three target densities, ≈89.9%, ≈97.5%, and ≈99.9%, by adjusting process parameters following a process–structure–properties mapping reported previously. The DOE also includes coupons intentionally biased toward crack-dominant, porosity-dominant, and mixed outcomes to supply class diversity for detection tasks

5.1.2. Overhangs

To probe geometry effects on sensing and classification, solids with symmetric overhangs were printed at 15°, 30°, and 45°. Parts began from 10 mm square bases, increasing in planform with an angle to a nominal 10 mm height. These artifacts introduce reduced local support and altered thermal pathways that are known to modulate AE propagation and melt-pool behavior.

5.1.3. Wall Thickness

Wall-fin coupons were produced with nominal wall thicknesses of 0.5 mm, 1.0 mm, and 2.0 mm, attached to a 20 mm × 10 mm × 3 mm base. Walls were 7 mm tall and spaced at 2.5 mm intervals. This design varies the conduction area and stiffness, enabling analysis of the sensitivity of thermal and elastic signatures to thin-feature fabrication.

5.1.4. Horizontal Channels

Coupons incorporating circular horizontal channels at 6 mm, 8 mm, and 10 mm inner diameter were printed as both solid and density-controlled variants. A minimum 3 mm wall thickness to the channel exterior was enforced, with part lengths of 15–20 mm. These artifacts emulate enclosed features where both thermal view factors and elastic paths are altered.

5.1.5. Supports

Support-sensitive coupons consisted of 10 mm cubes printed with multiple support types and densities. Supports were at least 1 mm tall and arranged to represent common strategies beneath bulk sections and local features. These builds provide cases where acoustic transmission and thermal boundary conditions differ from free-standing solids.

5.2. Ground-Truth Acquisition

Independent ground truth was established using Archimedes density measurements and micro-computed tomography. Density classes for baseline cubes were confirmed by Archimedes, while micro-CT supplied volumetric evidence of pore structures and crack indications where applicable. These methods were applied across DOE factors to provide consistent labels for training and evaluation.
The X-ray computed tomography was performed using a Nikon M2 system available at McMaster University.

5.3. Signature Consistency

To assess repeatability and to separate geometry effects from random variation, the DOE includes replicated builds at each density level and across representative geometry features. Signature consistency is evaluated by:
–
Run-to-run comparison of AE and pyrometer representations using exposure-aligned windows, with per-segment statistics and correlation against matched vector or layer indices.
–
Within-part stability of descriptors across layers for nominally identical regions, tracked via coefficient of variation and distributional tests.
–
Between-geometry contrasts that hold process parameters fixed while varying a single feature (for example, overhang angle), enabling attribution of observed shifts to geometry.
These procedures are supported by synchronized acquisition and standardized segmentation policies defined in Section 4, and they ensure that detection results reflect genuine class and geometry differences rather than artefacts of acquisition or labeling.

6. Monitoring and Fusion Methods

This section describes the pretrained modality-specific encoders used to generate AE and pyrometry latent representations, the downstream feature-level fusion classifier, the grouped training procedure, and the role of auxiliary process features.
In the present manuscript, the AE and pyrometry encoders should be understood as the upstream latent-generation stage. The defect-classification results reported later in Section 7 are produced by a downstream monitoring classifier operating on exported AE and PY latent representations, rather than by retraining the full raw-signal encoder stack during each monitoring experiment. The clarifications below are added to distinguish the encoder design rationale from the downstream grouped-split monitoring study reported in the Results Section.

6.1. AE Encoder

Input and preprocessing. AE is ingested as synchronized 1 MHz waveforms segmented according to Section 4. For each segment, two parallel branches are formed:
–
Time branch. The raw waveform (after per-build robust scaling) is provided directly to a learnable feature extractor.
–
Frequency branch. The segment is transformed using FFT or DCT to produce a compact spectrum suitable for learning. Frequency-domain representations are widely reported to improve defect classification relative to raw time signals in AE for LPBF.
Each branch uses a lightweight Conv1D → pooling → recurrent stack to capture local motifs and temporal context, followed by a projection to a latent vector. Convolutions summarize short-range structure, pooling provides down-sampling, and an LSTM layer captures sequential dependencies. The two latent vectors are concatenated and projected to the final AE latent used by the fusion stage. The choice of time-plus-frequency branches reflects published evidence that frequency transforms (FFT/DCT) and learned encoders (including VAEs) increase separability for defect detection.
The purpose of this stage was to compress high-rate acoustic windows into latent vectors that preserve defect-relevant information while reducing the dimensionality presented to the monitoring head. In the present study, the reported defect-classification results are produced by the downstream classifier operating on exported AE latents rather than by end-to-end training on raw waveforms. Accordingly, detailed encoder architecture and any encoder-stage augmentation are not central to the downstream fusion analysis reported in Section 7.

6.2. Pyrometer Encoder

The coaxial two-color pyrometer stream is segmented as in Section 4 and baseline-normalized so that the model consumes relative thermal trends. The prior literature shows that engineered features or filtered bands can improve classification from thermal sensors relative to raw signals.
A filter bank is applied to each segment to form a small set of band-limited channels. Bands are identified from exploratory variance/PCA analysis of training data or from prior feature screens, yielding a compact representation with reduced noise sensitivity. The filtered multichannel sequence is processed by a Conv1D → pooling → LSTM stack and then projected to the PY latent for fusion.
As with AE, these latents summarize relative thermal behavior associated with the local melt-pool regime while avoiding direct end-to-end training on the full raw scalar sequence at the fusion stage. The results reported in Section 7 are generated by the downstream classifier consuming exported pyrometry latents rather than by retraining the full raw-signal encoder during each monitoring experiment.

6.3. Feature-Level Fusion

AE and PY latent vectors are concatenated to form the sensor feature representation used by the downstream monitoring classifier. When enabled, auxiliary process-parameter features are passed through a small embedding network before fusion with the sensor latents. The fusion head is a compact multilayer perceptron with dense layers, batch normalization, and dropout. The downstream classifier uses two binary output heads: one for crack-like indication and one for porosity-like indication. Segments with neither indication are treated as nominal/good quality.
The same downstream head can be evaluated with AE-only or PY-only inputs by disabling the unused modality pathway. These AE-only and PY-only variants are, therefore, reported as within-framework ablations rather than as separately architecture-optimized unimodal baselines.

6.4. Training and Augmentation

Splits are performed on grouped manufacturing instances rather than on individual segments so that data from the same experiment/build-machine-part unit do not appear across training, validation, and testing. The downstream classifier is trained with Adam and a weighted binary cross-entropy objective summed across the two output heads. Grouped stratification is used during split construction to improve the consistency of crack-like and porosity-like prevalence across training, validation, and testing.
AE latents, PY latents, and auxiliary process-parameter features are standardized using statistics fit on the training split only and then applied unchanged to validation and test data. Model selection uses early stopping, learning-rate reduction on plateau, and auditable checkpointing. A suspect-checkpoint guardrail is retained during checkpoint auditing: suspiciously optimistic validation checkpoints are logged but excluded from final model selection unless separately justified. Decision thresholds are calibrated on the validation set after training and then fixed for held-out test evaluation. Threshold selection can prioritize high recall, F1, or recall subject to a minimum precision floor, depending on the monitoring objective for each head. In the present monitoring study, thresholds were selected to favor high recall because, in safety-critical and tightly regulated manufacturing settings, false positives are operationally preferable to false negatives: an unnecessarily flagged region can be subjected to additional inspection or adjudication, whereas an unflagged true defect may pass forward unnoticed. The revised training pipeline writes the split groups, preprocessing statistics, threshold values, checkpoint audit, and per-segment prediction files needed to reproduce the final tables directly from saved artifacts.

6.5. Auxiliary Process Features

Auxiliary process features provide coarse process context alongside the sensor latents. These features are restricted to variables available before or during the build, such as commanded process settings and derived energy-density terms. Auxiliary variables are embedded through a small dense network and down-weighted before fusion so that process context does not dominate the sensor-derived latent features. Their influence is quantified through matched ablation studies using the same grouped split and threshold-calibration protocol.
In interpreting these results, auxiliary variables should be regarded as contextual covariates rather than direct substitutes for sensor evidence. Strong performance gains from the auxiliary pathway indicate that process context materially influences separability under the present framework.

7. Results

This section reports detection results from synchronized acoustic emission (AE) and two-color pyrometry acquired at 1 MHz. We first define the dataset and evaluation protocol, then summarize modality validation and fused defect-classification results. Models are trained on training splits, tuned on validation splits, and evaluated on held-out grouped splits with part/build/machine separation to prevent leakage. Performance is reported separately for crack-like and porosity-like detection using accuracy, precision, recall, false-positive rate, F1, AUROC, and the corresponding confusion matrices. Inputs, segmentation, and labeling follow Section 4; encoder and fusion settings follow Section 6.

7.1. Dataset and Evaluation Protocol

This subsection defines the datasets, labels, splits, and metric conventions used in this study. All signals are synchronized AE and two-color pyrometry sampled at 1 MHz and segmented as discussed in Section 4.
All segments inherit grouped identifiers from the run manifest. In the revised training pipeline, splits are performed on grouped experiment/build-machine-part instances, ensuring that no grouped manufacturing unit appears across train, validation, and test.
Each segment carries a two-element binary defect label: crack-like indication and porosity-like indication. Segments with neither indication are treated as nominal/good quality. Geometry metadata identify the relevant coupon family and feature level.
Coupon-level and region-level labels originate from Archimedes density and micro-CT (Section 5). Because direct pointwise toolpath registration was not available, segment labels inherit the finest available coupon- or region-level ground truth through the exposure index and run manifest.
Segments intersecting saturated intervals, dropouts, or malformed exposure edges are excluded prior to splitting. QC-filtered counts and split composition are recorded automatically by the revised training pipeline.
Grouped stratification is used during splitting to improve consistency of crack-like and porosity-like prevalence across train, validation, and test while preserving part/build/machine isolation.
For each output head, we report accuracy, precision, recall, false-positive rate, F1, AUROC, and the corresponding confusion matrix. The same evaluation pipeline also supports matched unimodal-ablation reporting under identical grouped-split conditions.
The primary fused-model result reported below and the later ablation campaign should be interpreted separately. The primary fused result corresponds to the original grouped split realization used for the main study and was retained under the original non-suspect checkpoint-selection rule. The later AE-only, PY-only, AE + PY, and AE + PY + Aux reruns were conducted as a matched within-framework sensitivity study under stricter checkpoint-screening criteria and should therefore not be interpreted as a direct reproduction test of the primary fused-model result.
The process-parameter combinations used to define the nominal, porosity-dominant, and crack-dominant material conditions are listed in Table 4. The coupon families, nominal dimensions, and feature levels used to implement the geometry-aware DOE are summarized in Table 5.
Table 4. Process parameters by defect class.
Table 5. Coupon geometry and feature levels.

7.2. AE Validation

AE was recorded at 1 MHz and reviewed as co-registered waveforms and spectra over multiple layers and scan lines. Signal magnitude varied systematically with applied power, and track length effects were evident in the temporal envelopes. Within a given part, layer-to-layer patterns remained consistent, and salient AE transients occurred at the same instants as features visible in the pyrometer stream. Across the DOE settings, AE signatures differed by environment yet remained stable between repeated runs.

7.3. Pyrometer Validation

Time series inspection and frequency-domain views of the coaxial two-color pyrometer show repeatable, quasi-periodic behavior across layers and scan lines. The amplitude envelope follows the scan-path length, and salient pyrometer transients occur at the same instants as events visible in the AE record. Within a given part, layer-to-layer patterns remain consistent; in regions where AE coupling diminishes with height, the pyrometer continues to report stable thermal trends and resolves single-line exposures such as support tracings. These observations are consistent with prior validation that emphasized on-axis integration readiness and cross-sensor event concurrence, and they motivate the quantitative analyses reported below.
The following subsections summarize the influence of process parameters and material on the pyrometer spectrum observed through previous experiments: power primarily scales spectral magnitude, scan speed shifts the first harmonic approximately proportionally, stripe width inversely scales the fundamental, and alloy choice produces material-dependent shifts.

7.3.1. Influence of Process Parameters and Material Properties

Initial tests to confirm the operation and accuracy of the pyrometer in the new coaxial mounting revealed interesting behavior in the recorded temperature. Where a stable temperature reading was expected, a cyclical pattern presents itself, where the recorded temperature varies significantly, as shown in the time series graph in Figure 3 below. This pattern is seen as a series of harmonic frequency peaks in the corresponding FFT. In the data from a Ti64 sample exposed to a laser power of 250 W, a scan speed of 900 mm/s, a hatch spacing of 0.08 mm, and a layer thickness of 0.04 mm, the first harmonic occurs at approximately 80 Hz. To understand the data, a DOE was developed with three levels of laser power (250, 300, and 350 W) and three levels of scan speed (900, 1000, and 1100 mm/s) and repeated for Ti64 and H13 powder. The following sections will discuss the data collected and the potential influence of the laser power, scan speed, and material on the frequency response.
Figure 3. Time series and FFT graphs of temperature data recorded during the production of a Ti64 part. (a) Time series—Ti64-250 W @ 900 mm/s; (b) FFT—Ti64-250 W @ 900 mm/s.

7.3.2. Influence of Laser Power on the Frequency Response of Temperature Data

The graphs below in Figure 4 include the FFTs for parts produced from Ti64 at varying laser power and constant scan speeds. While the amplitude of the frequency peaks increases with the increase in laser power, their relative position does not appear to change, consistently appearing at approximately 80 Hz, 160 Hz, 240 Hz, and 300 Hz.
Figure 4. FFT graphs of temperature data recorded during the production of Ti64 parts at varying power and constant scan speed: (a) 250 W @ 900 mm/s; (b) 300 W @ 900 mm/s; (c) 350 W @ 900 mm/s.

7.3.3. Influence of Scanning Speed on the Frequency Response of Temperature Data

In contrast to laser power, varying the scan speed appears to have a proportional influence on the position of the first harmonic. Figure 5 below shows the FFTs for a Ti64 part exposed to 250 W of laser power at 900, 1000, and 1100 mm/s scan speeds. It can clearly be seen that as the scan speed increases, the position of the first harmonic increases as well. At 900 mm/s, the first harmonic occurs at approximately 80 Hz; at 1000 mm/s, it occurs at approximately 87 Hz; and at 1100 mm/s, it occurs at approximately 95 Hz. This relationship is further evident when comparing the FFT of a part exposed at 1000 mm/s and one exposed at 2000 mm/s, as shown in Figure 6. While the amplitude of the peaks varies, the first harmonic in the sample exposed at 2000 mm/s occurs at approximately 180 Hz, approximately twice that of the first harmonic in the sample exposed at 1000 mm/s.
Figure 5. FFT graphs of temperature data recorded during the production of Ti64 parts at varying scan speed and constant laser power: (a) 250 W @ 900 mm/s; (b) 250 W @ 1000 mm/s; (c) 250 W @ 1100 mm/s.
Figure 6. FFT graphs of temperature data recorded during the production of Ti64 parts at 1000 and 2000 mm/s scan speeds: (a) 250 W @ 1000 mm/s; (b) 200 W @ 2000 mm/s.

7.3.4. Influence of Material Properties on the Frequency Response of Temperature Data

To identify the influence of material properties on the frequency response of temperature data, the same DOE was repeated on Ti64 and H13 powder. All parameters related to laser power, scan speed, and scan path were kept constant; therefore, any differences in the FFT would be a result of a difference in material properties.
Figure 7 below shows the FFT responses of Ti64 and H13 exposed at a laser power of 250 W, scan speed of 900 mm/s, hatch spacing of 0.08 mm, and layer thickness of 0.04 mm. While the amplitude of the frequency peaks varies, the key difference between them is in the position of the first harmonic. Despite identical process parameters, the FFT of H13 shows a first harmonic at approximately 60 Hz compared to that of 80 Hz in Ti64.
Figure 7. FFT graphs of temperature data recorded during the production of Ti64 and H13 parts at a fixed laser power and scan speed. (a) Ti64; (b) H13.

7.3.5. Influence of Scan Path on the Frequency Response of Temperature Data

An additional experiment was conducted to explore any potential influence that the scan path (scan strategy) may have on the frequency response. A DOE was developed with two levels of stripe width (visualized in Figure 8) and two different orientations, relative to the flow of the inert shield gas. All parts were exposed with the same laser power (250 W), scan speed (900 mm/s), hatch spacing (0.08 mm), and layer thickness (0.04 mm).
Figure 8. Schematic representation of scan paths and stripe widths [43].
The resulting FFTs shown below in Figure 9 present no change in the position of the first harmonic when changing the orientation of the scan path relative to the inert shield gas flow. However, a significant change is observed when the stripe width is increased from 5 to 10 mm. In these instances, the first harmonic is halved, changing from 80 Hz at 5 mm to 40 Hz at 10 mm.
Figure 9. FFT graphs of temperature data recorded during the production of Ti64 parts at constant laser power and scan speed but varying scan path: (a) 5 mm stripe width, parallel to shield gas flow; (b) 10 mm stripe width, parallel to shield gas flow; (c) 10 mm stripe width, perpendicular to shield gas flow; (d) 5 mm stripe width, perpendicular to shield gas flow.

7.4. Fused-Sensor Defect Classification

The objective of this study was defect classification using the feature-level fusion of AE and two-color pyrometry latents (Section 6). Inputs, segmentation, and labeling follow Section 4. Models are trained on a training split, tuned on a validation split, and evaluated on a held-out test set with parts and builds held out to prevent leakage. The reported metrics are accuracy, precision, recall, FPR, F1, and AUROC.

7.4.1. Overall Performance

The held-out test split with by-part/build/machine separation, summarized in Table 6, reports that the fused AE + pyrometer model achieved F1 = 0.974 for crack-like and F1 = 0.987 for porosity-like, with recall = 1.00 for both heads. AUROC values were 0.9975 and 0.9925. These values compare favorably with reported AE-based monitoring studies; within this manuscript, however, the direct internal comparison should be taken from the matched within-framework ablation reported in Section 7.5, rather than inferred from the external literature.
Table 6. Test-set performance.

7.4.2. Confusion Matrix

Table 7 and Table 8 report the fused-model confusion matrices for crack-like and porosity-like detection, respectively. The crack-like operating point is intentionally recall-oriented and, therefore, carries a larger false-positive burden than the porosity-like operating point. Specifically, the crack-like confusion matrix contains 21,074 false positives and zero false negatives, whereas the porosity-like confusion matrix contains 4055 false positives and zero false negatives. This trade-off was deliberate: for defect screening in safety-critical and regulated manufacturing environments, a false positive is operationally safer than a false negative because it triggers additional inspection, adjudication, or post-build review rather than allowing a potentially defective region to pass unflagged. Some apparent false positives are also expected near coupon- or region-level label boundaries because the model predicts at segment resolution while the available ground truth is coarser. The crack-like detector should, therefore, be interpreted as a conservative screening model whose nuisance-alarm burden must be managed through aggregation and contextualization before operator-facing deployment.
Table 7. Fused-model confusion matrix for crack detection.
Table 8. Fused-model confusion matrix for porosity detection.

7.5. Matched Within-Framework Ablation Study

Matched ablations were performed on the downstream classifier using the same grouped-split concept, the same threshold-calibration procedure, and the same suspect-checkpoint guardrail. These runs should be interpreted as component-removal studies within the shared latent-fusion framework, not as separately architecture-optimized unimodal baselines.
The ablation campaign also functioned as a sensitivity audit under a stricter checkpoint-screening policy than the original primary fused-model run. Accordingly, the values reported here reflect both modality removal and seed/checkpoint sensitivity within the shared framework. They are informative about relative dependence on AE, pyrometry, and auxiliary process context, but they are not a direct replacement for the primary fused-model result in Table 6.
AE-only and PY-only rows are modality-removal ablations within the shared latent-fusion classifier and do not represent architecture-optimized unimodal baselines separately; more broadly, Table 9 should be read as a within-framework sensitivity audit rather than as a direct replacement for Table 6.
Table 9. Matched within-framework ablation results across three seeds (held-out test set, mean ± SD).

8. Discussion

This section interprets the results in the context of in situ defect detection for LPBF using fused acoustic emission and two-color pyrometry at 1 MHz. The geometry-aware DOE and synchronized acquisition produced datasets that isolate overhangs, thin walls, horizontal channels, and supports, allowing us to examine how geometry is expected to influence sensing and classification. AE validation showed repeatable layer-to-layer patterns with events that coincide with pyrometer transients. Pyrometer characterization indicated that spectral magnitude scales with power, the first harmonic increases with scan speed, stripe width sets a geometric fundamental, and material choice shifts the spectrum. The fused model provided strong aggregate performance on the held-out test set; geometry-specific performance should be interpreted only where explicit stratified analyses are reported.
The remainder of the section addresses three questions. Section 8.1 explains why complex geometry must be present in coupon design if a monitoring system is intended for real parts. Section 8.2 summarizes the practical limits of AE plus pyrometry fusion, including coupling, view-factor, labeling, and transferability issues. Section 8.3 discusses what these findings imply for real-time monitoring, with attention to latency budgeting, synchronization, channel-health checks, and data stewardship in production settings.

8.1. Justification for Incorporating Complex Geometry in Coupon Design

Complex features change both what the sensors observe and how signals propagate [7,33]. Overhangs reduce local heat-sinking and alter stress release, which shifts AE amplitude and spectral content while modifying the pyrometer’s thermal trajectory through view-factor changes [44]. Thin walls and enclosed channels change stiffness and conduction area, affecting elastic-wave coupling and melt-pool stability [45]. Supports introduce local single-line exposures that can be thermally faint yet mechanically informative [46]. A dataset that omits these conditions risks optimistic performance estimates and poor generalization to real parts [3]. By designing coupons that isolate overhang angles, wall thickness, channel diameter, and support strategy, this study makes geometry sensitivity explicit rather than incidental. This design provides an evidence base for selecting training distributions and for setting realistic deployment expectations, even before fine-grained spatial aggregation is introduced. In short, geometry-aware coupon design turns a common failure mode of single-sensor monitoring into a measurable factor during model development and later validation.

8.2. Limitations of AE + Pyrometry Fusion

Fusion improves coverage but does not eliminate blind spots [6,39].
AE remains sensitive to how the transducer couples into the plate and to propagation paths that change with part height and feature layout; mode conversion, fixture variability, and local damping can shift amplitude independent of defect state and confound naïve thresholds [4,30]. Careful mounting and per-build normalization reduce but do not remove these effects.
Two-color pyrometry mitigates emissivity variation, yet the signal remains line of sight and can be biased by plume, spatter, window contamination, or partial occlusion; as a scalar channel, it captures thermal regimes but cannot alone disambiguate mechanical crack events [5,21].
Ground truth is often available at the coupon or region scale (Archimedes or micro-CT), whereas inference is done at the segment or vector scale; transitional zones and mixed defects, therefore, introduce label noise that can cap apparent performance even when the model is behaving sensibly [33,47].
Models trained on one machine, alloy, or gas-flow configuration may not transfer without adaptation; geometry distributions also matter [3,38].
At 1 MHz per modality, window length trades latency against context; longer windows stabilize features but delay decisions and raise memory demands [3]. Feature-level fusion retains interpretability of modality-specific latents, yet failures can be ambiguous when modalities disagree, or one channel degrades [38,39].
These limits motivate pragmatic safeguards: rigorous synchronization (including recording the exposure signal), geometry-balanced training sets, per-build normalization, channel-health checks, calibrated confidence thresholds, and periodic re-validation when optics, alloys, or flow conditions change [3].

8.3. Implications for Real-Time Monitoring in LPBF

The findings indicate that fused acoustic emission and two-color pyrometry can support near-real-time monitoring, provided several implementation constraints are addressed [6].
With exposure-aligned segmentation and lightweight Conv–LSTM encoders, low-latency inference is plausible. The end-to-end decision time will depend on window length, stride, preprocessing, and inference cost, and should be measured on the target hardware [3]. Sliding windows with a short look-ahead can balance responsiveness with sufficient context for transient events.
Reliable decisions require recording the exposure signal, estimating any fixed inter-channel offset at the start of each build, and checking for drift during the job. If alignment cannot be verified, the system should flag reduced confidence or defer decisions. Channel-health monitoring (for example, noise floor, clipping, and dropout rate) should be active at runtime, with a defined behavior when one modality degrades, such as temporary fallback to single-sensor operation with explicit operator notification [3].
Rather than streaming continuous scores, it is preferable to produce per-vector or per-layer defect likelihoods and aggregate these to layer-wise quality maps. Such summaries should be stable from layer to layer to minimize alarm fatigue and to support traceable review [33].
When storage is constrained, persistence should prioritize compact artefacts that preserve auditability: the exposure-event index, per-build normalization parameters, and fused embeddings. Short raw snippets centered on high-confidence events can be retained to support later adjudication without archiving full streams [3].
Performance should be re-checked whenever process windows, optics, alloys, gas-flow conditions, or build layouts change materially. Periodic calibration builds that reprise the geometry panel from the DOE provide a low-cost means to track drift and to confirm that monitoring remains valid for the geometries encountered in production [3].
Taken together, these considerations suggest that AE plus two-color pyrometry, fused at the feature level, can underpin a practical monitoring workflow for porosity- and crack-related indications, contingent on strong synchronization practices; continuous channel-health checks; disciplined segmentation and reporting policies; and periodic, geometry-aware re-validation [3,6].

9. Future Work

This section outlines directions that follow from the study’s findings and limitations. The emphasis is on improving spatial interpretability, extending sensing coverage, assessing generalization beyond the present platform and alloys, and preparing the monitoring front end for eventual linkage to supervisory control.

9.1. STL-Aware Mapping and Localization

Future work should map segment-level predictions to the build coordinate frame to produce STL-aware defect-likelihood fields. This requires registering exposure indices to machine coordinates through controller logs and then mapping those coordinates to the STL mesh or a voxelized part representation. Segment scores can then be spatially aggregated over voxels or toolpath neighborhoods, while uncertainty is propagated through repeated predictions. Such fields would support geometry-specific thresholds, targeted inspection, and direct comparison with post-build micro-CT on a common spatial basis.

9.2. Integration of Additional Sensors

Evaluate complementary sensors that observe phenomena not fully captured by AE and two-color pyrometry and quantify their incremental value in fusion. Candidates include on-axis or off-axis high-speed imaging for plume and spatter dynamics, photodiodes or compact spectrometers for broadband emission, and structured layer imaging for surface anomalies. Priorities are synchronization feasibility, bandwidth and storage cost, and demonstrable gains beyond the current coupon/part-level geometry-aware reporting. Fusion strategies to compare include feature-level concatenation, decision-level aggregation of modality-specific heads, and shared-latent approaches with auxiliary reconstruction losses.

9.3. Multi-Material and Cross-Machine Validation

Test generalization across alloys and platforms using leave-one-domain-out evaluation. Examples include training on IN625 and Ti-6Al-4V and testing on H13 or training on one machine and testing on another. Report absolute performance and the minimum adaptation needed to recover target metrics (for example, per-build normalization only, encoder fine-tuning, or limited labeled data). The protocol should reuse the geometry panel from the DOE so that observed changes can be attributed to material or machine rather than shifts in geometry distribution. Particular attention is required for pyrometer band calibration and AE coupling paths, which may change with optics, gas flow, or fixturing.

9.4. Integration with Process Control Frameworks

We can position the fused detector as a monitoring front end that may inform supervisory control once reliability is established. Future work should define interfaces and decision policies rather than specific controllers: latency budgets aligned to the chosen window policy and compute resources; rules for when to suppress, flag, or act on a detection; and safeguards when synchronization or channel health is out of tolerance. A staged deployment is recommended, beginning with advisory mode and progressing to limited closed-loop interventions after re-qualification on the geometry panel. Any integration should document failure modes and expose operator-visible confidence and provenance, while maintaining an audit trail through retained event indices and embeddings.

10. Conclusions

We demonstrated that feature-level fusion of structure-borne acoustic emission and coaxial two-color pyrometry (both 1 MHz) can support high-sensitivity in situ defect detection in LPBF. Using a geometry-diverse dataset with independent Archimedes and micro-CT ground truth and grouped experiment/build-machine-part splits, the primary fused model achieved strong aggregate held-out performance for both crack-like and porosity-like detection. In the primary fused-model run, F1 reached 0.974 for crack-like and 0.987 for porosity-like detection, with a recall of 1.00 for both heads and AUROC values of approximately 0.998 and 0.993, respectively. Together with the sensor-characterization results, these findings support fused AE-pyrometry monitoring as a practical basis for near-real-time defect screening.
A later matched within-framework ablation campaign further clarified modality contribution under stricter checkpoint-screening rules. These results support the value of process context and multimodal fusion within the present downstream framework, while also showing that the ablation study should be interpreted as a sensitivity audit rather than as a direct reproduction of the primary fused-model result or as a comparison against separately optimized unimodal baselines. Priority next steps are explicit coupon- or geometry-stratified reporting, false-positive aggregation analysis by part, build, and layer, calibration analysis, architecture-optimized AE-only and PY-only baselines, and STL-aware aggregation of segment-level predictions as a bridge toward eventual supervisory control.

Author Contributions

Conceptualization; methodology, software, validation, formal analysis, investigation, data curation, writing—original draft preparation, M.M.; writing—review and editing, J.B.; supervision, M.E. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Data Availability Statement

None of the data discussed will be made available for download, as the data discussed is part of additional future work requirements.

Conflicts of Interest

The authors declare no conflicts of interest.

Abbreviations

The following abbreviations are used in this manuscript:
AEAcoustic Emission
AMAdditive Manufacturing
DBNDeep Belief Network
DCNNDeep Convolutional Neural Network
DEDDirect Energy Deposition
DNNDeep Neural Network
DOEDesign of Experiments
kNNK-Nearest Neighbors
LMDLaser Metal Deposition
LPBFLaser Powder Bed Fusion
LSTMLong Short-Term Memory
MIMOMulti-In–Multi-Out
MLMachine Learning
NNNeural Network
ONNXOpen Neural Network Exchange
PBFPowder Bed Fusion
PBF-EBPowder Bed Fusion–Energy Beam
PCAPrincipal Component Analysis
PSPProcess Structure Property
PYPyrometer
SLMSelective Laser Melting
SVMSupport Vector Machine
VAEVariational Auto Encoder

References

  1. DebRoy, T.; Wei, H.L.; Zuback, J.S.; Mukherjee, T.; Elmer, J.W.; Milewski, J.O.; Beese, A.M.; Wilson-Heid, A.; De, A.; Zhang, W. Additive manufacturing of metallic components—Process, structure and properties. Prog. Mater. Sci. 2018, 92, 112–224. [Google Scholar] [CrossRef] [Scilit]
  2. King, W.E.; Barth, H.D.; Castillo, V.M.; Gallegos, G.F.; Gibbs, J.W.; Hahn, D.E.; Kamath, C.; Rubenchik, A.M. Observation of keyhole-mode laser melting in laser powder-bed fusion additive manufacturing. J. Mater. Process Technol. 2014, 214, 2915–2925. [Google Scholar] [CrossRef] [Scilit]
  3. McCann, R.; Obeidi, M.A.; Hughes, C.; McCarthy, É.; Egan, D.S.; Vijayaraghavan, R.K.; Joshi, A.M.; Garzon, V.A.; Dowling, D.P.; McNally, P.J.; et al. In-situ sensing, process monitoring and machine control in Laser Powder Bed Fusion: A review. Addit. Manuf. 2021, 45, 102058. [Google Scholar] [CrossRef] [Scilit]
  4. Kouprianoff, D.; Yadroitsava, I.; Plessis, A.D.; Luwes, N.; Yadroitsev, I. Monitoring of Laser Powder Bed Fusion by Acoustic Emission: Investigation of Single Tracks and Layers. Front. Mech. Eng. 2021, 7, 678076. [Google Scholar] [CrossRef] [Scilit]
  5. Gutknecht, K.; Cloots, M.; Sommerhuber, R.; Wegener, K. Mutual comparison of acoustic, pyrometric and thermographic laser powder bed fusion monitoring. Mater. Des. 2021, 210, 110036. [Google Scholar] [CrossRef] [Scilit]
  6. Tempelman, J.R.; Wachtor, A.J.; Flynn, E.B.; Depond, P.J.; Forien, J.-B.; Guss, G.M.; Calta, N.P.; Matthews, M.J. Sensor fusion of pyrometry and acoustic measurements for localized keyhole pore identification in laser powder bed fusion. J. Mater. Process Technol. 2022, 308, 117656. [Google Scholar] [CrossRef] [Scilit]
  7. Montazeri, M.; Rao, P. Sensor-Based Build Condition Monitoring in Laser Powder Bed Fusion Additive Manufacturing Process Using a Spectral Graph Theoretic Approach. J. Manuf. Sci. Eng. 2018, 140, 091002. [Google Scholar] [CrossRef] [Scilit]
  8. Gordon, J.V.; Narra, S.P.; Cunningham, R.W.; Liu, H.; Chen, H.; Suter, R.M.; Beuth, J.L.; Rollett, A.D. Defect structure process maps for laser powder bed fusion additive manufacturing. Addit. Manuf. 2020, 36, 101552. [Google Scholar] [CrossRef] [Scilit]
  9. Tang, M.; Pistorius, P.C. Oxides, porosity and fatigue performance of AlSi10Mg parts produced by selective laser melting. Int. J. Fatigue 2017, 94, 192–201. [Google Scholar] [CrossRef] [Scilit]
  10. Bayoumy, D.; Schliephake, D.; Dietrich, S.; Wu, X.H.; Zhu, Y.M.; Huang, A.J. Intensive processing optimization for achieving strong and ductile Al-Mn-Mg-Sc-Zr alloy produced by selective laser melting. Mater. Des. 2021, 198, 109317. [Google Scholar] [CrossRef] [Scilit]
  11. Ng, G.K.L.; Jarfors, A.E.W.; Bi, G.; Zheng, H.Y. Porosity formation and gas bubble retention in laser metal deposition. Appl. Phys. A 2009, 97, 641–649. [Google Scholar] [CrossRef] [Scilit]
  12. Gong, H.; Rafi, K.; Gu, H.; Starr, T.; Stucker, B. Analysis of defect generation in Ti–6Al–4V parts made using powder bed fusion additive manufacturing processes. Addit. Manuf. 2014, 1–4, 87–98. [Google Scholar] [CrossRef] [Scilit]
  13. Zhang, B.; Li, Y.; Bai, Q. Defect Formation Mechanisms in Selective Laser Melting: A Review. Chin. J. Mech. Eng. (Engl. Ed.) 2017, 30, 515–527. [Google Scholar] [CrossRef] [Scilit]
  14. Tang, M.; Pistorius, P.C.; Beuth, J.L. Prediction of lack-of-fusion porosity for powder bed fusion. Addit. Manuf. 2017, 14, 39–48. [Google Scholar] [CrossRef] [Scilit]
  15. Paulson, N.H.; Gould, B.; Wolff, S.J.; Stan, M.; Greco, A.C. Correlations between thermal history and keyhole porosity in laser powder bed fusion. Addit. Manuf. 2020, 34, 101213. [Google Scholar] [CrossRef] [Scilit]
  16. Hooper, P.A. Melt pool temperature and cooling rates in laser powder bed fusion. Addit. Manuf. 2018, 22, 548–559. [Google Scholar] [CrossRef] [Scilit]
  17. Sabzi, H.E.; Maeng, S.; Liang, X.; Simonelli, M.; Aboulkhair, N.T.; Rivera-Díaz-del-Castillo, P.E.J. Controlling crack formation and porosity in laser powder bed fusion: Alloy design and process optimization. Addit. Manuf. 2020, 34, 101360. [Google Scholar] [CrossRef] [Scilit]
  18. Mercelis, P.; Kruth, J.P. Residual stresses in selective laser sintering and selective laser melting. Rapid Prototyp. J. 2006, 12, 254–265. [Google Scholar] [CrossRef] [Scilit]
  19. Pandiyan, V.; Wróbel, R.; Leinenbach, C.; Shevchik, S. Optimizing in-situ monitoring for laser powder bed fusion process: Deciphering acoustic emission and sensor sensitivity with explainable machine learning. J. Mater. Process. Technol. 2023, 321, 118144. [Google Scholar] [CrossRef] [Scilit]
  20. Fereiduni, E. Laser Powder Bed Fusion of Titanium Matrix Composites. Ph.D. Thesis, Department of Mechanical Engineering, McMaster University, Hamilton, ON, Canada, 2021. [Google Scholar]
  21. Mitchell, J.A.; Ivanoff, T.A.; Dagel, D.; Madison, J.D.; Jared, B. Linking pyrometry to porosity in additively manufactured metals. Addit. Manuf. 2020, 31, 100946. [Google Scholar] [CrossRef] [Scilit]
  22. Eschner, N.; Weiser, L.; Häfner, B.; Lanza, G. Development of an Acoustic Process Monitoring System for the Selective Laser Melting (SLM). In Solid Freeform Fabrication 2018: Proceedings of the 29th Annual International; University of Texas at Austin: Austin, TX, USA, 2018. [Google Scholar]
  23. Wasmer, K.; Le-Quang, T.; Meylan, B.; Shevchik, S.A. In Situ Quality Monitoring in AM Using Acoustic Emission: A Reinforcement Learning Approach. J. Mater. Eng. Perform. 2019, 28, 666–672. [Google Scholar] [CrossRef] [Scilit]
  24. Mahmoudi, M.; Ezzat, A.A.; Elwany, A. Layerwise Anomaly Detection in Laser Powder-Bed Fusion Metal Additive Manufacturing. J. Manuf. Sci. Eng. Trans. 2019, 141, 031002. [Google Scholar] [CrossRef] [Scilit]
  25. Baumgartl, H.; Tomas, J.; Buettner, R.; Merkel, M. A deep learning-based model for defect detection in laser-powder bed fusion using in-situ thermographic monitoring. Prog. Addit. Manuf. 2020, 5, 277–285. [Google Scholar] [CrossRef] [Scilit]
  26. Elwarfalli, H.; Papazoglou, D.; Erdahl, D.; Doll, A.; Speltz, J. In Situ Process Monitoring for Laser-Powder Bed Fusion using Convolutional Neural Networks and Infrared Tomography. In Proceedings of the IEEE National Aerospace Electronics Conference, NAECON; IEEE: New York, NY, USA, 2019; Volume 2019, pp. 323–327. [Google Scholar] [CrossRef] [Scilit]
  27. Scime, L.; Beuth, J. Anomaly detection and classification in a laser powder bed additive manufacturing process using a trained computer vision algorithm. Addit. Manuf. 2018, 19, 114–126. [Google Scholar] [CrossRef] [Scilit]
  28. Gobert, C.; Reutzel, E.W.; Petrich, J.; Nassar, A.R.; Phoha, S. Application of supervised machine learning for defect detection during metallic powder bed fusion additive manufacturing using high resolution imaging. Addit. Manuf. 2018, 21, 517–528. [Google Scholar] [CrossRef] [Scilit]
  29. Ye, D.; Hong, G.S.; Zhang, Y.; Zhu, K.; Fuh, J.Y.H. Defect detection in selective laser melting technology by acoustic signals with deep belief networks. Int. J. Adv. Manuf. Technol. 2018, 96, 2791–2801. [Google Scholar] [CrossRef] [Scilit]
  30. Drissi-Daoudi, R.; Pandiyan, V.; Logé, R.; Shevchik, S.; Masinelli, G.; Ghasemi-Tabasi, H.; Parrilli, A.; Wasmer, K. Differentiation of materials and laser powder bed fusion processing regimes from airborne acoustic emission combined with machine learning. Virtual Phys. Prototyp. 2022, 17, 181–204. [Google Scholar] [CrossRef] [Scilit]
  31. Pandiyan, V.; Drissi-Daoudi, R.; Shevchik, S.; Masinelli, G.; Logé, R.; Wasmer, K. Analysis of time, frequency and time-frequency domain features from acoustic emissions during Laser Powder-Bed fusion process. Procedia CIRP 2020, 94, 392–397. [Google Scholar] [CrossRef] [Scilit]
  32. Mohammadi, M.G.; Mahmoud, D.; Elbestawi, M. On the application of machine learning for defect detection in L-PBF additive manufacturing. Opt. Laser Technol. 2021, 143, 107338. [Google Scholar] [CrossRef] [Scilit]
  33. Lough, C.S.; Liu, T.; Wang, X.; Brown, B.; Landers, R.G.; Bristow, D.A.; Drallmeier, J.A.; Kinzel, E.C. Local Prediction of Laser Powder Bed Fusion Porosity by Short-Wave Infrared Imaging Thermal Feature Porosity Probability Maps. J. Mater. Process. Technol. 2022, 302, 117473. [Google Scholar] [CrossRef] [Scilit]
  34. Gaikwad, A.; Giera, B.; Guss, G.M.; Forien, J.B.; Matthews, M.J.; Rao, P. Heterogeneous sensing and scientific machine learning for quality assurance in laser powder bed fusion—A single-track study. Addit. Manuf. 2020, 36, 101659. [Google Scholar] [CrossRef] [Scilit]
  35. Jayasinghe, S.; Paoletti, P.; Sutcliffe, C.; Dardis, J.; Jones, N.; Green, P.L. Automatic quality assessments of laser powder bed fusion builds from photodiode sensor measurements. Prog. Addit. Manuf. 2021, 7, 143–160. [Google Scholar] [CrossRef] [Scilit]
  36. Zouhri, W.; Dantan, J.Y.; Häfner, B.; Eschner, N.; Homri, L.; Lanza, G.; Theile, O.; Schäfer, M. Optical process monitoring for Laser-Powder Bed Fusion (L-PBF). CIRP J. Manuf. Sci. Technol. 2020, 31, 607–617. [Google Scholar] [CrossRef] [Scilit]
  37. Mahato, V.; Obeidi, M.A.; Brabazon, D.; Cunningham, P. Detecting voids in 3D printing using melt pool time series data. J. Intell. Manuf. 2020, 33, 845–852. [Google Scholar] [CrossRef] [Scilit]
  38. Bevans, B.; Barrett, C.; Spears, T.; Gaikwad, A.; Riensche, A.; Smoqi, Z.; Halliday, H.; Rao, P. Heterogeneous sensor data fusion for multiscale, shape agnostic flaw detection in laser powder bed fusion additive manufacturing. Virtual Phys. Prototyp. 2023, 18, e2196266. [Google Scholar] [CrossRef] [Scilit]
  39. Li, J.; Zhang, X.; Zhou, Q.; Chan, F.T.S.; Hu, Z. A feature-level multi-sensor fusion approach for in-situ quality monitoring of selective laser melting. J. Manuf. Process 2022, 84, 913–926. [Google Scholar] [CrossRef] [Scilit]
  40. Tian, Q.; Guo, S.; Melder, E.; Bian, L.; Guo, W. Deep Learning-Based Data Fusion Method for In Situ Porosity Detection in Laser-Based Additive Manufacturing. J. Manuf. Sci. Eng. 2021, 143, 041011. [Google Scholar] [CrossRef] [Scilit]
  41. Wu, M.; Yao, Z.; Ye, L.; Verbeke, M.; Karsmakers, P.; Reynaerts, D. Geometrical Feature Classification in Electrical Discharge Machining Using In-Process Monitoring and Machine Learning. Procedia CIRP 2025, 137, 462–467. [Google Scholar] [CrossRef] [Scilit]
  42. Wu, M.; Shukla, S.; Vrancken, B.; Verbeke, M.; Karsmakers, P. Data-Driven Approach to Identify Acoustic Emission Source Motion and Positioning Effects in Laser Powder Bed Fusion with Frequency Analysis. Procedia CIRP 2025, 133, 531–536. [Google Scholar] [CrossRef] [Scilit]
  43. Kuznetsov, P.; Mozhayko, A.; Shakirov, I.; Bobyr, V.; Staritsyn, M.; Zhukov, A. Modeling of LPBF Scanning Strategy and its Correlation with the Metallic 316 L, 321, and Alnico Magnets Samples Structure. In Advanced Additive Manufacturing; IntechOpen: London, UK, 2022. [Google Scholar] [CrossRef] [Scilit]
  44. Ashby, A.; Guss, G.; Ganeriwala, R.K.; Martin, A.A.; DePond, P.J.; Deane, D.J.; Matthews, M.J.; Druzgalski, C.L. Thermal history and high-speed optical imaging of overhang structures during laser powder bed fusion: A computational and experimental analysis. Addit. Manuf. 2022, 53, 102669. [Google Scholar] [CrossRef] [Scilit]
  45. Wu, Z.; Narra, S.P.; Rollett, A. Exploring the fabrication limits of thin-wall structures in a laser powder bed fusion process. Int. J. Adv. Manuf. Technol. 2020, 110, 191–207. [Google Scholar] [CrossRef] [Scilit]
  46. Molnar, B.; Heigel, J.C.; Whitenton, E. In Situ Thermography During Laser Powder Bed Fusion of a Nickel Superalloy 625 Artifact with Various Overhangs and Supports. J. Res. Natl. Inst. Stand. Technol. 2021, 126, 126005. [Google Scholar] [CrossRef] [Scilit]
  47. Snow, Z.; Reutzel, E.W.; Petrich, J. Correlating in-situ sensor data to defect locations and part quality for additively manufactured parts using machine learning. J. Mater. Process Technol. 2022, 302, 117476. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.