Abstract
This study evaluated the effects of prolonged self-etching ceramic primer protocols on surface roughness (Ra), topography, shear bond strength (SBS), and failure modes of three CAD/CAM ceramics. Lithium disilicate (IPS e.max CAD), advanced lithium disilicate (CEREC Tessera), and feldspathic ceramic (VITABLOCS Mark II) specimens received hydrofluoric acid etching plus silane (HF+S) or Monobond Etch & Prime (MEP). For MEP, active application and passive reaction times were increased together using paired durations of 20/40, 40/80, or 60/120 s, respectively (n = 10 per group). Ra was measured by optical profilometry, and additional specimens underwent qualitative scanning electron microscopy. SBS was measured after 10,000 thermocycles, followed by failure-mode classification. Ra and SBS were analyzed using two-way ANOVA and Tukey’s HSD; failure modes were analyzed using the Fisher–Freeman–Halton test. Ceramic material, treatment, and their interaction significantly affected Ra and SBS (p < 0.001). For both lithium disilicate-based ceramics, SBS did not differ significantly between MEP 40/80 s and HF+S, whereas MEP 60/120 s produced significantly higher SBS than HF+S. HF+S produced the highest SBS for feldspathic ceramic. Failure-mode distributions differed across the material–treatment groups (p < 0.001). Under the tested laboratory conditions, the combined 60/120 s MEP protocol produced higher SBS after thermocycling than HF+S for the two lithium disilicate-based ceramics, whereas HF+S produced the highest SBS for the feldspathic ceramic.
1. Introduction
Computer-aided design/computer-aided manufacturing (CAD/CAM) ceramic materials are widely used for indirect restorations because of their esthetic properties, biocompatibility, and favorable clinical performance [1]. Silica-based CAD/CAM ceramic materials are available in different compositions and microstructures, including feldspathic and lithium disilicate ceramics, which may influence their mechanical properties and response to surface treatment. Recent reviews of chairside CAD/CAM materials have emphasized that material composition and microstructure are important factors in clinical material selection and surface treatment planning [2], as these differences may influence mechanical properties and response to acid etching and bonding procedures.
Feldspathic (FEL) ceramic is a silica-based ceramic with a high glassy phase content and favorable esthetic properties [3,4]. However, its relatively lower strength generally restricts its indications to low-stress restorations, predominantly in anterior regions [4]. Lithium disilicate (LD) ceramic is composed of elongated lithium disilicate crystals (approximately 70% by volume) embedded within a glassy silica matrix, which contributes to its improved mechanical behavior and excellent translucency, making it suitable for both anterior and posterior restorations [5]. More recently, Dentsply Sirona has introduced advanced lithium disilicate (ALD) ceramic, in which lithium disilicate crystals are incorporated into a glassy matrix with lithium aluminosilicate [6,7]. Compared to conventional LD, ALD exhibits superior hardness, smoother surfaces, and higher resistance to wear while maintaining similar fracture behavior and esthetic properties [7,8].
Regardless of ceramic composition, inadequate bond strength between ceramic restorations and tooth structure is a major cause of clinical failure. Debonding of ceramic restorations can occur due to insufficient resin–ceramic adhesion, leading to microleakage, secondary caries, restoration loss, and patient dissatisfaction [9]. Clinical studies have reported debonding rates of approximately 2% over 10 years for glass–ceramic restorations [10], with inadequate surface treatment identified as a significant contributing factor. Therefore, optimizing surface-treatment protocols to achieve durable resin–ceramic bonding is clinically essential for long-term restoration success and patient outcomes. Surface treatment effectiveness is typically evaluated through surface roughness and topographic analysis, which reflect micromechanical retention potential, and shear bond strength testing after thermocycling, which simulates clinical aging conditions [11,12].
Hydrofluoric acid etching followed by silane application (HF+S) is considered a conventional surface treatment for silica-based ceramics because HF selectively dissolves the glassy matrix, creating surface irregularities that improve micromechanical retention [13], while silane is a bifunctional molecule that induces a chemical interaction between the silica in the glass phase of the ceramic and the methacrylate groups of the resin monomers through siloxane bonds [14,15]. Despite its effectiveness in enhancing adhesion between resin cements and glass–ceramic substrates, HF remains a hazardous substance characterized by its toxicity and corrosive properties [16,17]. Exposure to highly concentrated HF (>50%) can result in severe morbidity or death [18], whereas even the reduced concentrations (~5%) utilized in dental practice may pose risks to practitioners and patients [19]. Moreover, studies have reported that although HF etching creates desirable surface microporosities for resin infiltration, these same irregularities can also act as stress concentration points that may induce crack formation, thereby reducing the mechanical strength of glass–ceramic restorations [20,21].
To address the limitations of conventional HF etching, a one-step self-etching ceramic primer has been developed as an alternative surface treatment approach for glass–ceramics. Monobond Etch & Prime (MEP) was introduced as a self-etching ceramic primer that combines etching and priming in one step. This simplified protocol may reduce the number of clinical steps and technique sensitivity compared with separate HF etching and silane application [22]. MEP contains an ammonium polyfluoride etchant, specifically tetrabutylammonium dihydrogen trifluoride, together with silane components in an alcohol–water formulation, enabling etching and priming within a single treatment [22,23]. Despite these advantages, previous studies have reported variable effects of MEP on surface roughness and bond strength.
Several studies have compared the bonding effectiveness of MEP versus conventional HF+S treatment on glass–ceramic materials. El-Damanhoury and Gaintantzopoulou [23] reported that HF etching provided superior etching efficacy and bonding performance compared to MEP for lithium disilicate ceramic. Similarly, Azevedo et al. found that 5% HF+S achieved higher SBS than MEP for feldspathic and lithium silicate ceramics after 16 months of water storage [24]. However, a recent systematic review and meta-analysis by Awad et al. found no statistically significant difference in bond strength between MEP and HF+S treatments when evaluated using micro-shear, tensile, or micro-tensile bond strength tests, although conventional shear bond strength testing favored HF+S [25].
Given the variable bonding performance of MEP when applied according to the manufacturer’s recommended protocol of 20 s of active application followed by 40 s of passive reaction [22] compared with HF+S, researchers have investigated whether prolonged application/reaction protocols could improve MEP etching effectiveness and bonding outcomes. Cardenas et al. found that increasing MEP application time from 20 s to 60 s while maintaining the 40 s reaction time significantly improved SBS for lithium disilicate [26]. Similarly, Alsolami and Alzahrani reported that extending MEP application time to 2 min while maintaining the 40 s reaction time resulted in more durable resin–ceramic adhesion after thermocycling compared with the manufacturer’s recommended 20/40 s protocol [27]. In contrast, Alshihri found no significant difference in SBS when MEP reaction time was extended from 40 s to 80 s or 120 s after thermocycling [28]. These inconsistent findings suggest that the effect of prolonged MEP application and reaction times may be material–dependent, warranting further investigation across different ceramic compositions.
Despite these investigations, important knowledge gaps remain. First, while the manufacturer recommends different HF etching times for different ceramic materials (20 s for LD, 30 s for ALD, 60 s for FEL), it is unclear whether MEP application and reaction times should similarly be adjusted according to ceramic type and composition. Second, most previous studies have focused on conventional lithium disilicate, with limited data on advanced lithium disilicate (ALD), a relatively new material with a modified crystalline structure. Third, no studies have directly compared the surface roughness, topography, and bond strength responses of LD, ALD, and FEL ceramics to different MEP application times under standardized conditions. Finally, the relationship between surface alterations (Ra and SEM) and bonding performance (SBS after thermocycling) across different ceramic–treatment combinations remains poorly understood. Therefore, this study evaluated the effect of prolonged MEP application and reaction protocols 20/40 s, 40/80 s, and 60/120 s compared with conventional HF+S treatment on: (1) surface roughness (Ra), (2) qualitative surface topography assessed by scanning electron microscopy (SEM), (3) shear bond strength (SBS) after thermocycling, and (4) failure-mode distribution of three silica-based CAD/CAM ceramics: conventional lithium disilicate (IPS e.max CAD), advanced lithium disilicate (CEREC Tessera), and feldspathic ceramic (VITABLOCS Mark II). The null hypotheses were that ceramic material, surface treatment protocol, and their interaction would have no significant effect on Ra or SBS and that failure-mode distribution would not differ among the material–treatment groups. SEM observations were interpreted descriptively to complement the quantitative roughness findings.
2. Materials and Methods
2.1. Sample Preparation
Rectangular slices with a thickness of 2 mm (N = 120) were sectioned under continuous water cooling using a low-speed saw (Isomet LowSpeed; Buehler, Lake Bluff, IL, USA) to obtain flat, standardized specimens, similar to previous bond-strength studies on CAD/CAM silicate ceramics [29]. The slices were cut from CAD/CAM ceramic blocks of IPS e.max CAD (C14; 12.4 × 14.5 × 18 mm), CEREC Tessera (C14; 14.5 × 14.5 × 16 mm), and VITABLOCS Mark II (I-14; 12 × 14 × 18 mm) (Table 1). IPS e.max CAD and CEREC Tessera specimens were heat-treated in a ceramic furnace (Programat P500, Ivoclar Vivadent, Schaan, Liechtenstein). IPS e.max CAD specimens were crystallized using a standby temperature of 403 °C and a closing time of 6 min, followed by heating at 90 °C/min to 820 °C with a 10 s hold, and then at 30 °C/min to 840 °C with a 7 min hold. Vacuum was applied during the 550–820 °C and 820–840 °C stages, and the long-term cooling temperature was set to 700 °C [30]. CEREC Tessera specimens underwent matrix firing using a standby temperature of 403 °C, a closing time of 6 min, a heating rate of 55 °C/min, and a final temperature of 760 °C held for 2 min, without vacuum [31]. VITABLOCS Mark II specimens did not undergo additional firing. All specimens were embedded in cylindrical molds filled with self-curing acrylic resin, leaving one flat surface exposed for subsequent surface treatment. The exposed surfaces were polished under water cooling using 800, 1000, and 1200-grit silicon carbide papers for 15 s per grit at 150 rpm (POLO 2503, Jean Wirtz, Düsseldorf, Germany) to obtain a standardized, flat surface with comparable baseline roughness before surface treatments. After polishing, all specimens were ultrasonically cleaned (Dri-Clave ultrasonic cleaner, Columbus Dental, Columbus, OH, USA) in distilled water for 10 min and then air-dried before surface treatment.
Table 1.
Materials, manufacturers and compositions.
For each ceramic material, specimens were allocated into four subgroups (n = 10) according to the surface treatment protocol. The sample size was determined a priori in R using the pwr package (version 1.3-0), with shear bond strength as the primary outcome. The effect size was set conservatively at the smallest difference in bond strength between HF+S and MEP reported by Prado et al. [32], a standardized difference of 1.10 between the two groups, which places each group 0.55 standard deviations from the overall mean (f = 0.55). For a comparison of the four surface treatments, with a significance level of 0.05 and a target power of 80%, this required 10 specimens per group, applied to each of the three ceramic materials (N = 120). In the two-way ANOVA of this design, effects of f = 0.35 or larger are detectable with at least 80% power for both main effects and their interaction. This group size is also consistent with previous in vitro studies evaluating the effects of surface-treatment protocols on the bond strength of CAD/CAM glass–ceramics and to permitted a balanced factorial design [26,28]. Group 1: HF + Silane (control), 5% hydrofluoric acid etching gel (IPS Ceramic Etching Gel, Table 1) was applied for 20 s (IPS e.max CAD), 30 s (CEREC Tessera), or 60 s (VITABLOCS Mark II), in accordance with manufacturer recommendations [30,31,33]. The etchant was rinsed thoroughly with water spray and the surface was air-dried. A silane coupling agent (Monobond N, Table 1) was applied with a micro-brush and allowed to react for 60 s; excess was dispersed with a strong stream of air. Group 2: MEP (Table 1) was applied using a microbrush and agitated on the surface with light pressure for 20 s, followed by a passive reaction time of 40 s, according to the manufacturer’s instructions [22]. Group 3: The MEP application/reaction time was extended to 40 s of active application followed by 80 s of passive reaction. Group 4: The MEP application/reaction time was extended to 60 s of active application followed by 120 s of passive reaction. For groups 2, 3, and 4, MEP was thoroughly rinsed off for 20 s with water until the green color was removed. The ceramic surface was dried with a strong stream of oil- and moisture-free air for approximately 10 s.
2.2. Surface Roughness (Ra) and Topography (SEM) Evaluations
The surface roughness (Ra) was quantified using a 3-D optical non-contact profilometer (Contour GT, Bruker, Tucson, AZ, USA). For each specimen, three randomly selected areas were scanned, and the mean of three readings was recorded as the final Ra value of that specimen. The images were acquired at 5× magnification using integrated “Vision64” software (Bruker Corporation, Billerica, MA, USA). For surface topography assessment by scanning electron microscopy (SEM), three additional specimens from each group (n = 3 per group; N = 36 total) were prepared separately from those used for Ra and SBS testing, as sputter coating renders specimens unsuitable for subsequent bond strength evaluation. Specimens were sputter-coated with a thin layer of gold using an auto fine coater (Quorum Q150R, Quorum Technologies Ltd., Laughton, UK) and examined with a scanning electron microscope (JSM-7610F; JEOL, Tokyo, Japan) operated at an accelerating voltage of 15 kV. Representative micrographs were obtained at 1000× magnification.
2.3. Shear Bond Strength (SBS)
After surface treatment, resin cement cylinders were fabricated using a silicone mold (3 mm internal diameter × 2 mm height). Dual-cure resin cement (Variolink Esthetic DC; Ivoclar Vivadent, Schaan, Liechtenstein) was injected into the mold placed on the treated ceramic surface. Excess cement was removed with a hand instrument, and the assembly was covered with a translucent polyethylene strip and a 1 mm thick glass slide. The resin cement was light-cured for 20 s using an LED curing unit (Bluephase N MC, Ivoclar Vivadent, Schaan, Liechtenstein), with a manufacturer-specified wavelength range of 430–490 nm. The unit’s output was checked using a radiometer (Bluephase Meter, Ivoclar Vivadent), which recorded approximately 1180 mW/cm2. During the initial exposure, the curing tip was maintained in contact with the upper surface of the 1 mm thick glass slide to standardize the tip-to-cement distance. After careful removal of the silicone mold, an additional 20 s of light curing was performed with the curing tip maintained in contact with the glass slide. The specimens were stored in distilled water at 37 °C for 24 h before aging. Specimens were then thermocycled for 10,000 cycles between 5 °C and 55 °C using a thermocycler (THE-1100; SD Mechatronik GmbH, Feldkirchen-Westerham, Germany), with a dwell time of 30 s and transfer time of 5 s [34].
For SBS testing, specimens were mounted in a custom metal jig and positioned in a universal testing machine (Instron Machine, model 5969; Instron Corp, Norwood, MA, USA) where the resin cement–ceramic interface is perpendicular to the horizontal plane. A chisel-shaped loading blade was aligned at the resin cement–ceramic interface, and load was applied at a crosshead speed of 0.5 mm/min until failure occurred. The maximum load at failure was recorded in newtons (N), and SBS was calculated by dividing the maximum load by the bonded area and expressed in MPa.
2.4. Failure Mode Analysis
After SBS testing, the fractured interface of each specimen was examined using a digital microscope at 50× magnification (Hirox KH-7700; Hirox Co., Tokyo, Japan). Failure mode was determined based on optical inspection and classified into four types: adhesive failure (Type 1), defined as debonding at the resin–ceramic interface; cohesive failure in the ceramic (Type 2), defined as fracture within the ceramic substrate without adhesive separation; cohesive failure in the resin cement (Type 3), defined as fracture within the resin cement buildup without adhesive failure; and mixed failure (Type 4), defined as a combination of adhesive and cohesive failures [35].
2.5. Statistical Analysis
Statistical analyses were performed using R (version 4.5.3; R Foundation for Statistical Computing, Vienna, Austria). Surface roughness (Ra) and shear bond strength (SBS) were summarized as mean ± standard deviation for a balanced 3 × 4 factorial design comprising three CAD/CAM ceramic materials and four surface treatments (n = 10 per group; N = 120 per outcome). For each outcome, a two-way ANOVA was performed to assess the effects of material, surface treatment, and their interaction as fixed factors. Residual normality was assessed using the Shapiro–Wilk test, which indicated no significant departures from normality. Homogeneity of variance was assessed using Levene’s test, which indicated no significant heterogeneity (Ra: p = 0.090; SBS: p = 0.880). Effect sizes (partial eta squared, ηp2) and 95% confidence intervals are reported in Tables S1–S3. Because the interaction was significant for both Ra and SBS (p < 0.05), simple main effects were analyzed, followed by Tukey’s HSD post hoc comparisons. Failure-mode distribution was analyzed using the Fisher–Freeman–Halton exact test. Overall differences across the 12 material × surface treatment groups were tested first, followed by within-material tests comparing the four surface treatments for each ceramic. Statistical significance was set at α = 0.05.
3. Results
3.1. Surface Roughness (Ra)
Ra values ranged from 0.22 ± 0.04 µm for IPS e.max CAD treated with 20/40 s to 1.46 ± 0.08 µm for VITABLOCS Mark II treated with HF+S (Table 2, Figure 1). Two-way ANOVA showed significant effects of material (p < 0.001, ηp2 = 0.925), surface treatment (p < 0.001, ηp2 = 0.862), and their interaction (p < 0.001, ηp2 = 0.915) on Ra. Because the interaction was significant, Tukey HSD post hoc comparisons were interpreted. Within VITABLOCS Mark II, HF+S produced significantly higher Ra than all three MEP regimens, whereas the three MEP application/reaction protocols did not differ significantly from one another. Within CEREC Tessera, MEP 20/40 s yielded significantly lower Ra than HF+S and the longer MEP durations. Within IPS e.max CAD, differences among treatments were minimal, with only MEP 60/120 s producing significantly higher Ra than the shorter MEP regimens. Under HF+S, VITABLOCS Mark II showed significantly higher Ra than both IPS e.max CAD and CEREC Tessera, whereas material differences were reduced under the MEP regimens. Detailed ANOVA and pairwise comparison results are provided in Tables S1 and S2.
Table 2.
Surface roughness (Ra) values of CAD/CAM ceramics following different surface treatments.
Figure 1.
Surface roughness for the three CAD/CAM ceramic materials following different surface treatments.
3.2. Topography (SEM) Analysis
Surface topography varied according to ceramic material and surface treatment protocol (Figure 2). In LD, HF+S produced a distinct etched surface with microporosities, grooves, and striations, consistent with pronounced dissolution of the glassy matrix. The shorter MEP protocols produced milder surface changes, with relatively smooth areas between machining grooves, whereas MEP 60/120 s resulted in more evident microporosities and surface irregularities. In ALD, HF+S produced an irregular surface with scattered deposits and signs of matrix dissolution, although the etching pattern was less pronounced than in LD. MEP 20/40 s and MEP 40/80 s produced comparatively smooth surfaces with visible machining grooves and minimal topographic alteration, while MEP 60/120 s produced slightly more pronounced grooves and surface irregularities. FEL showed the most pronounced surface alteration among the tested ceramics. HF+S produced a highly irregular and porous surface with extensive dissolution of the glassy matrix. Similarly, all MEP-treated FEL groups showed marked surface roughening, pitting, and reduced visibility of machining grooves, with no obvious topographic differences among the MEP application/reaction times.
Figure 2.
Representative SEM micrographs (×1000) of lithium disilicate (LD; IPS e.max CAD), advanced lithium disilicate (ALD; CEREC Tessera), and feldspathic ceramic (FEL; VITABLOCS Mark II) following different surface treatments. (a–d) LD; (e–h) ALD; (i–l) FEL. (a,e,i) HF+S; (b,f,j) MEP 20 + 40 s; (c,g,k) MEP 40 + 80 s; (d,h,l) MEP 60 + 120 s. LD: lithium disilicate; ALD: advanced lithium disilicate; FEL: feldspathic ceramic; HF+S: hydrofluoric acid plus silane; MEP: Monobond Etch & Prime.
3.3. Shear Bond Strength (SBS)
SBS values ranged from 9.55 ± 1.53 MPa for IPS e.max CAD treated with MEP 20/40 s to 21.49 ± 2.13 MPa for VITABLOCS Mark II treated with HF+S (Table 3, Figure 3). Two-way ANOVA showed significant effects of material (p < 0.001, ηp2 = 0.680), surface treatment (p < 0.001, ηp2 = 0.626), and their interaction (p < 0.001, ηp2 = 0.274) on SBS. Because the interaction was significant, Tukey HSD post hoc comparisons were interpreted. Within IPS e.max CAD and CEREC Tessera, MEP 20/40 s produced significantly lower SBS than HF+S, whereas MEP 60/120 s produced significantly higher SBS than HF+S. SBS did not differ significantly between MEP 40/80 s and HF+S for either IPS e.max CAD (p = 0.361) or CEREC Tessera (p = 1.000). In contrast, within VITABLOCS Mark II, all MEP regimens produced significantly lower SBS than HF+S, although increasing the MEP application/reaction time partially improved SBS. Across surface treatments, VITABLOCS Mark II generally showed significantly higher SBS than IPS e.max CAD and CEREC Tessera, whereas IPS e.max CAD and CEREC Tessera did not differ significantly from each other. Detailed ANOVA and pairwise comparison results are provided in Tables S1 and S3.
Table 3.
Shear bond strength (SBS) values of CAD/CAM ceramics following different surface treatments.
Figure 3.
Shear bond strength for the three CAD/CAM ceramic materials following different surface treatments.
3.4. Failure Mode Analysis
The Fisher–Freeman–Halton exact test indicated that failure-mode distribution differed significantly across the 12 material × surface treatment groups (p < 0.001). Within-material comparisons showed that surface treatment significantly affected failure-mode distribution in CEREC Tessera (p = 0.019) but not in IPS e.max CAD (p = 0.891) or VITABLOCS Mark II (p = 0.189) (Figure 4). For IPS e.max CAD, adhesive failure predominated across all groups, accounting for 80–100% of failures, with only limited mixed failures and no cohesive failures in either the ceramic or resin cement. In contrast, CEREC Tessera showed a greater tendency toward mixed failures, particularly after HF+S treatment, where mixed failure accounted for 80% of specimens. Among the MEP-treated CEREC Tessera groups, mixed failures accounted for 30%, 50%, and 10% of specimens after the 20/40 s, 40/80 s, and 60/120 s protocols, respectively. Adhesive failures accounted for 60%, 40%, and 40%, respectively, whereas the combined proportion of cohesive failures was highest after the 60/120 s protocol. VITABLOCS Mark II showed no adhesive failures in any group and was characterized mainly by cohesive failures within the ceramic and mixed failures. Overall, IPS e.max CAD was associated mainly with adhesive failure, whereas CEREC Tessera and VITABLOCS Mark II showed higher proportions of mixed and cohesive failure modes, indicating greater involvement of the ceramic or resin cement during debonding. Failure-mode counts and percentages are provided in Table S4.
Figure 4.
Distribution of failure modes according to ceramic material and surface treatment. Each bar represents the percentage of specimens within each material–treatment group (n = 10). HF+S = hydrofluoric acid plus silane; MEP = Monobond Etch & Prime. Adhesive (Type 1), cohesive in ceramic (Type 2), cohesive in resin (Type 3), and mixed (Type 4).
4. Discussion
The present study evaluated the effect of different MEP application/reaction protocols on the surface roughness (Ra), surface topography (SEM), shear bond strength (SBS), and failure-mode distribution of three CAD/CAM ceramic materials. Both ceramic material and surface treatment protocol significantly influenced Ra and SBS, with significant material–treatment interactions for both outcomes. Ra and SEM observations revealed material–dependent surface alterations, with VITABLOCS Mark II exhibiting the most pronounced topographic changes, particularly after HF+S treatment. In general, extending the MEP application/reaction time improved SBS for IPS e.max CAD and CEREC Tessera, whereas HF+S produced the highest SBS for VITABLOCS Mark II. Accordingly, the null hypotheses for Ra and SBS were rejected because ceramic material, surface treatment protocol, and their interaction significantly affected both outcomes. The null hypothesis concerning failure-mode distribution was also rejected because the Fisher–Freeman–Halton exact test showed that failure-mode distribution differed significantly among the material–treatment groups. SEM findings were interpreted descriptively and were not subjected to null-hypothesis testing.
SBS testing was selected for its practical advantages, including straightforward specimen preparation without additional sectioning that might introduce microcracks, lower incidence of pre-test failures, and suitability for evaluating multiple surface-treatment protocols across different ceramic materials in a standardized manner [36,37,38,39]. Non-contact optical profilometry was used for Ra measurement to avoid potential surface damage from contact-based stylus probes and ensure non-destructive, reproducible measurements [40]. Thermocycling (10,000 cycles between 5 °C and 55 °C) was applied to simulate clinical aging and challenge the durability of resin–ceramic adhesion [34].
The observed differences in Ra may reflect both ceramic microstructure and the specific surface-treatment protocols used, including the ceramic-specific HF etching durations in the HF+S groups. VITABLOCS Mark II exhibited the highest Ra values after HF+S (1.46 ± 0.08 µm), which were significantly higher than all three MEP regimens (0.47–0.52 µm). In contrast, IPS e.max CAD and CEREC Tessera generally showed lower Ra values than VITABLOCS Mark II. IPS e.max CAD showed significantly higher Ra with MEP 60/120 s than with both shorter MEP protocols, whereas CEREC Tessera showed significantly higher Ra with MEP 60/120 s than with the standard 20/40 s protocol, but not the 40/80 s protocol. The greater roughness of VITABLOCS Mark II after HF+S may be related to its feldspathic, glass-rich composition, which is more susceptible to acid-induced dissolution than lithium disilicate-based ceramics [41]. Supporting this material–dependent response, Temp et al. evaluated VITABLOCS Mark II and IPS e.max CAD using 5% HF etching followed by silane application and MEP applied for 20/40 s, reporting that surface roughness and topographic changes were dependent on ceramic type, with feldspathic ceramic showing significantly more evident surface alteration (Ra = 1.2 μm for FEL vs. 0.3 μm for LD after HF+S) than lithium disilicate ceramic [42]. Regarding the effect of MEP application/reaction time on Ra, Donmez et al. evaluated two MEP protocols (20/40 s and 40/80 s) alongside 5% and 9.5% HF etching for 60 or 120 s. They found no significant difference in Ra between the two MEP protocols within each tested material [43]. The present findings extend these observations to ALD ceramic, demonstrating that extending MEP application/reaction time to 60/120 s significantly increased Ra for CEREC Tessera compared to the standard 20/40 s protocol. For IPS e.max CAD, extending MEP to 60/120 s increased Ra compared with the shorter MEP regimens but produced roughness values similar to HF+S, whereas for CEREC Tessera, MEP 60/120 s increased Ra from below to slightly above the HF+S level, indicating a more pronounced roughening response of ALD to prolonged MEP application/reaction. This more controlled surface alteration observed for lithium disilicate-based ceramics may be related to the crystalline microstructure, in which HF etching selectively dissolves the intervening glassy phase and exposes the crystalline phase rather than producing generalized surface dissolution, resulting in a more limited overall roughness increase compared with feldspathic ceramic.
The qualitative SEM observations were generally consistent with the profilometric Ra findings and illustrated material–dependent topographic changes after the different surface treatments. These qualitative observations should be interpreted as complementary to, rather than quantitative confirmation of, the Ra measurements. For VITABLOCS Mark II, HF+S produced a highly irregular and porous surface with extensive dissolution of the glassy matrix, whereas all MEP-treated groups showed marked surface roughening and pitting, with no obvious topographic differences among the three MEP application/reaction times. This pronounced surface alteration is consistent with the glass-rich composition of feldspathic ceramic and its susceptibility to acid-induced dissolution, as discussed above [41]. For IPS e.max CAD, HF+S created distinct micro-porosities, grooves, and striations consistent with pronounced dissolution of the glassy matrix, while the standard MEP protocol (20/40 s) produced milder surface changes with relatively smooth areas between machining grooves. Extending MEP application/reaction time to 60/120 s resulted in more evident microporosities and surface irregularities. Similarly, for CEREC Tessera, HF+S produced an irregular surface with scattered deposits and signs of matrix dissolution, though less pronounced than in conventional LD. MEP 20/40 s and 40/80 s produced comparatively smooth surfaces with minimal topographic alteration, while MEP 60/120 s produced slightly more pronounced surface irregularities. These findings are consistent with Alsolami and Alzahrani who used SEM to compare 5% HF etching with MEP applied for either 20/40 s or 2 min/40 s and reported that HF+S produced more pronounced microporosities, grooves, and striations than MEP in both ceramic materials, with extended MEP application (2 min) showing increased surface dissolution compared to the standard protocol [27]. Similarly, Cardenas et al. evaluated lithium disilicate ceramic and found that 5% HF etching promoted greater glass-matrix dissolution than MEP applied for 20/40 s, although prolonging MEP application time to 60 s while maintaining 40 s reaction time increased surface dissolution and porosity, approaching the topographic features created by HF etching [26]. The present qualitative SEM observations suggest that the topographic response to prolonged MEP application/reaction times may vary according to ceramic composition. Feldspathic ceramic showed marked surface alteration with the standard 20/40 s MEP regimen, whereas lithium disilicate-based ceramics showed more evident surface irregularities after the prolonged 60/120 s regimen.
Collectively, the Ra measurements and qualitative SEM observations suggest that prolonged MEP protocols produced material–dependent surface alterations. These surface changes may have contributed to the differences in SBS observed after thermocycling; however, the present design does not establish a direct causal relationship between surface morphology or roughness and bond strength. Comparisons between HF+S and MEP should also be interpreted as comparisons of complete surface-treatment protocols rather than isolated effects of etching duration. The HF+S protocol used ceramic-specific HF etching durations followed by the same silane-containing primer, Monobond N, whereas MEP combined etching and priming within a different formulation. Consequently, differences in SBS cannot be attributed solely to treatment duration or surface roughness, because the contributions of etching and priming were not evaluated independently.
The SBS results showed a pattern that was broadly consistent with the material- and protocol-dependent Ra findings and qualitative SEM observations. The observed surface alterations may have contributed to the differences in bonding performance after thermocycling, although other factors, including ceramic chemistry, silane interaction, resin cement behavior, and the nonuniform stress distribution inherent to SBS testing, may also have influenced the results. For IPS e.max CAD and CEREC Tessera, the manufacturer-recommended MEP protocol (20/40 s) produced the lowest SBS values (9.55 ± 1.53 MPa and 10.13 ± 1.84 MPa, respectively), which were significantly lower than HF+S (13.79 ± 1.74 MPa and 14.32 ± 1.19 MPa). However, extending MEP application/reaction time to 60/120 s significantly improved bonding performance, resulting in higher SBS (16.13 ± 1.75 MPa for LD and 17.53 ± 1.75 MPa for ALD) than HF+S. In contrast, for VITABLOCS Mark II, HF+S produced the highest SBS (21.49 ± 2.13 MPa), which remained significantly higher than all MEP protocols, although using the prolonged 60/120 s MEP protocol partially improved SBS (18.89 ± 1.59 MPa) compared to the standard protocol (16.14 ± 1.23 MPa). These findings are consistent with Alsolami and Alzahrani who reported that extending MEP application time to 2 min (while maintaining 40 s reaction time) resulted in more durable resin–ceramic adhesion to IPS e.max CAD and CEREC Tessera after 10,000 thermocycles compared with the manufacturer’s recommended 20/40 s protocol and achieved comparable or superior SBS to HF+S etching [27].
Similarly, Cardenas et al. found that increasing MEP application time from 20 s to 60 s (while maintaining 40 s reaction time) significantly improved SBS for lithium disilicate ceramic compared to the standard MEP protocol, attributing this improvement to increased surface dissolution and porosity with prolonged application [26]. The present findings are consistent with a benefit of prolonged MEP protocols for the tested lithium disilicate-based materials; however, this benefit did not extend to superiority over HF+S for the tested feldspathic material. In contrast, Alshihri found no significant difference in SBS among lithium disilicate specimens when MEP reaction time alone was extended from 40 s to 80 s or 120 s (while keeping application time constant at 20 s) after 3000 thermocycles [28]. Similarly, Donmez et al. reported that MEP increased Ra and SBS compared with untreated controls, but extending the active application/passive reaction times from 20/40 s to 40/80 s did not significantly affect SBS for lithium disilicate after 5000 thermocycles [43]. Differences in aging regimens (3000–5000 versus 10,000 thermocycles), together with other methodological differences, may have contributed to these discrepancies. However, whether the relative benefit of prolonged MEP protocols varies with thermocycling duration requires direct investigation.
Failure mode analysis provided additional context for interpreting the SBS findings. IPS e.max CAD showed predominantly adhesive failures across all surface-treatment protocols (80–100%), indicating that debonding occurred mainly at the resin–ceramic interface. CEREC Tessera showed a higher proportion of mixed failures after HF+S treatment (80%). Among the MEP-treated groups, mixed failures accounted for 30%, 50%, and 10% after the 20/40 s, 40/80 s, and 60/120 s protocols, respectively, whereas adhesive failures accounted for 60%, 40%, and 40%. The lower proportion of mixed failures after the 60/120 s protocol was accompanied by a greater combined proportion of cohesive failures, rather than an increase in adhesive failures. VITABLOCS Mark II showed no adhesive failures and was characterized mainly by mixed failures after HF+S treatment (70%) and cohesive failures within the ceramic across the MEP-treated groups (40–60%). The greater proportions of mixed and cohesive failures in CEREC Tessera and VITABLOCS Mark II suggest greater involvement of the ceramic substrate or resin cement during debonding. However, failure-mode interpretation should remain cautious because fracture patterns may also be influenced by ceramic composition, substrate brittleness, resin cement properties, and stress distribution during SBS testing.
The present findings provide laboratory evidence of material-dependent differences in SBS following the tested surface-treatment protocols and 10,000 thermocycles. For IPS e.max CAD and CEREC Tessera, the MEP protocol combining 60 s of active application with 120 s of passive reaction produced higher SBS than HF+S, whereas HF+S produced the highest SBS for VITABLOCS Mark II. These results identify protocols that warrant further investigation rather than establish their clinical superiority. Long-term clinical studies are needed before recommendations regarding clinical durability or changes to manufacturer-recommended application protocols can be made.
The findings of this study should be interpreted in light of certain limitations. Although 10,000 thermocycles were used to challenge resin–ceramic adhesion under laboratory thermal-aging conditions, this protocol does not establish long-term clinical durability or fully reproduce the complex oral environment. Other aging conditions, such as long-term water storage, pH cycling, mechanical fatigue loading, exposure to biofilm, and dietary beverages, were not included. In addition, only one resin cement system was evaluated; therefore, the findings may not be directly applicable to other luting agents. Each ceramic category was also represented by a single commercial material: IPS e.max CAD, CEREC Tessera, and VITABLOCS Mark II. Consequently, the findings are specific to these products and the tested experimental conditions and should not be generalized to all materials within the corresponding ceramic categories. Differences among the tested products cannot be attributed exclusively to ceramic composition because other product-specific characteristics and processing protocols were not evaluated independently. Because active application and passive reaction times were prolonged simultaneously, their independent contributions to the observed outcomes could not be distinguished. Therefore, the findings reflect differences among the tested combinations of active application and passive reaction times and should not be attributed to either timing component alone. SEM analysis was qualitative and based on representative specimens, which limits direct quantitative comparison of surface features among groups. Furthermore, specimens were allocated without a formal randomization procedure, and failure modes were classified by a single, unblinded examiner; these factors may have introduced allocation and observer bias. Finally, although SBS testing is widely used for evaluating resin–ceramic bonding and avoids additional specimen sectioning, the stress distribution at the bonded interface may be nonuniform. Future studies should include additional commercial materials within each ceramic category, vary active application and passive reaction times independently, and evaluate the long-term durability of the tested protocols using different resin cements, mechanical fatigue loading, and clinically relevant multifactorial aging conditions.
5. Conclusions
Within the limitations of this in vitro study, the effect of prolonged MEP application and reaction protocols on resin–ceramic bonding was material dependent. After thermocycling, the MEP protocol combining 60 s of active application with 120 s of passive reaction produced higher SBS than the manufacturer-recommended 20/40 s protocol and HF+S for IPS e.max CAD and CEREC Tessera, whereas HF+S produced the highest SBS for VITABLOCS Mark II. These findings apply to the tested timing combinations and do not establish the independent effects of active application or passive reaction duration. These laboratory findings are specific to the tested materials and experimental conditions and do not establish long-term clinical performance.
Supplementary Materials
The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/bioengineering13121453/s1, Table S1: Two-way ANOVA results for the effects of ceramic material, surface treatment, and their interaction on surface roughness and shear bond strength; Table S2: Tukey-adjusted pairwise comparisons for surface roughness; Table S3: Tukey-adjusted pairwise comparisons for shear bond strength; Table S4: Failure-mode counts and percentages by ceramic material and surface-treatment protocol.
Author Contributions
Conceptualization, H.A., T.A. and A.M.; methodology, H.A., A.M.S., T.A. and A.M.; validation, A.M.S.; formal analysis, H.A., A.M.S. and T.A.; investigation, H.A.; resources, H.A. and A.M.S.; data curation, H.A.; writing—original draft preparation, H.A.; writing—review and editing, A.M.S., T.A. and A.M.; visualization, H.A.; supervision, A.M.S., T.A. and A.M.; project administration, H.A. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by the Ongoing Research Funding program, Research Chairs (ORF-RC-2026-3303), King Saud University, Riyadh, Saudi Arabia.
Institutional Review Board Statement
The study involved manufactured dental ceramic specimens and no human participants, human tissue, or animals. The project was approved and registered by the College of Dentistry Research Center, King Saud University (PR-0184).
Informed Consent Statement
Not applicable.
Data Availability Statement
Summary results and detailed statistical analyses are provided in the article and its Supplementary Materials. The underlying specimen-level data supporting the findings of this study are available from the corresponding author upon reasonable request.
Acknowledgments
The authors gratefully acknowledge the Ongoing Research Funding Program, Research Chairs, for funding this project. During the preparation of this manuscript, the authors used the generative artificial intelligence (AI) tools Perplexity (Perplexity AI, San Francisco, CA, USA; automatic model selection) and Claude Opus 5.5 (Anthropic, San Francisco, CA, USA) to assist with drafting and revising manuscript text. The authors have reviewed and edited the output and take full responsibility for the content of this publication.
Conflicts of Interest
The authors declare no conflicts of interest.
Abbreviations
The following abbreviations are used in this manuscript:
| ALD | Advanced lithium disilicate |
| LD | Lithium disilicate |
| FEL | Feldspathic |
| CAD/CAM | Computer-aided design/computer-aided manufacturing |
| HF | Hydrofluoric acid |
| HF+S | Hydrofluoric acid + Silane |
| MEP | Monobond Etch and Prime |
| Ra | Arithmetic mean surface roughness |
| SBS | Shear bond strength |
| SEM | Scanning electron microscopy |
| ANOVA | Analysis of variance |
| SD | Standard deviation |
| HSD | Honestly significant difference |
References
- Miyazaki, T.; Hotta, Y.; Kunii, J.; Kuriyama, S.; Tamaki, Y. A Review of Dental CAD/CAM: Current Status and Future Perspectives from 20 Years of Experience. Dent. Mater. J. 2009, 28, 44–56. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Marchesi, G.; Piloni, A.C.; Nicolin, V.; Turco, G.; Di Lenarda, R. Chairside CAD/CAM Materials: Current Trends of Clinical Uses. Biology 2021, 10, 1170. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Höland, W.; Schweiger, M.; Watzke, R.; Peschke, A.; Kappert, H. Ceramics as Biomaterials for Dental Restoration. Expert Rev. Med. Devices 2008, 5, 729–745. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Giordano, R. Materials for Chairside CAD/CAM-Produced Restorations. J. Am. Dent. Assoc. 2006, 137, 14S–21S. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Lien, W.; Roberts, H.W.; Platt, J.A.; Vandewalle, K.S.; Hill, T.J.; Chu, T.M.G. Microstructural Evolution and Physical Behavior of a Lithium Disilicate Glass-Ceramic. Dent. Mater. 2015, 31, 928–940. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Fasbinder, D.J. CEREC Tessera Advanced Lithium Disilicate. Available online: https://assets.dentsplysirona.com/master/regions-countries/north-america/product-procedure-brand/cad-cam/CER-EN-US-document-White-Paper-CEREC-Tessera-1.pdf (accessed on 5 October 2026).
- Rosentritt, M.; Schmid, A.; Huber, C.; Strasser, T. In Vitro Mastication Simulation and Wear Test of Virgilite and Advanced Lithium Disilicate Ceramics. Int. J. Prosthodont. 2022, 35, 770–776. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Hölken, F.; Dietrich, H. Restoring Teeth with an Advanced Lithium Disilicate Ceramic: A Case Report and 1-Year Follow-Up. Case Rep. Dent. 2022, 2022, 6872542. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Blatz, M.B.; Conejo, J.; Alammar, A.; Ayub, J. Current Protocols for Resin-Bonded Dental Ceramics. Dent. Clin. N. Am. 2022, 66, 603–625. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Aslan, Y.U.; Uludamar, A.; Özkan, Y. Clinical Performance of Pressable Glass-Ceramic Veneers after 5, 10, 15, and 20 Years: A Retrospective Case Series Study. J. Esthet. Restor. Dent. 2019, 31, 415–422. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Oh, W.S.; Shen, C. Effect of Surface Topography on the Bond Strength of a Composite to Three Different Types of Ceramic. J. Prosthet. Dent. 2003, 90, 241–246. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Mair, L.; Padipatvuthikul, P. Variables Related to Materials and Preparing for Bond Strength Testing Irrespective of the Test Protocol. Dent. Mater. 2010, 26, e20–e26. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Chen, J.H.; Matsumura, H.; Atsuta, M. Effect of Different Etching Periods on the Bond Strength of a Composite Resin to a Machinable Porcelain. J. Dent. 1998, 26, 53–58. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Naves, L.Z.; Soares, C.J.; Moraes, R.R.; Gonçalves, L.S.; Sinhoreti, M.A.C.; Correr-Sobrinho, L. Surface/Interface Morphology and Bond Strength to Glass Ceramic Etched for Different Periods. Oper. Dent. 2010, 35, 420–427. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Söderholm, K.J.M.; Shang, S.W. Molecular Orientation of Silane at the Surface of Colloidal Silica. J. Dent. Res. 1993, 72, 1050–1054. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Carpena, G.; Ballarin, A. Hydrofluoric Acid—Simple Things You May Do Not Know About Something You Are So Habituated to Use. Odovtos—Int. J. Dent. Sci. 2015, 16, 15–23. [Google Scholar] [CrossRef] [Scilit]
- Xingang, W.; Yuanhai, Z.; Liangfang, N.; Chuangang, Y.; Chunjiang, Y.; Ruiming, J.; Liping, L.; Jia, L.; Chunmao, H. A Review of Treatment Strategies for Hydrofluoric Acid Burns: Current Status and Future Prospects. Burns 2014, 40, 1447–1457. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Bartlett, D. Dermal Exposure to Hydrofluoric Acid Causing Significant Systemic Toxicity. J. Emerg. Nurs. 2004, 30, 371–373. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Dennerlein, K.; Kiesewetter, F.; Kilo, S.; Jäger, T.; Göen, T.; Korinth, G.; Drexler, H. Dermal Absorption and Skin Damage Following Hydrofluoric Acid Exposure in an Ex Vivo Human Skin Model. Toxicol. Lett. 2016, 248, 25–33. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Addison, O.; Marquis, P.M.; Fleming, G.J.P. The Impact of Hydrofluoric Acid Surface Treatments on the Performance of a Porcelain Laminate Restorative Material. Dent. Mater. 2007, 23, 461–468. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Venturini, A.B.; Prochnow, C.; May, L.G.; Bottino, M.C.; Felipe Valandro, L. Influence of Hydrofluoric Acid Concentration on the Flexural Strength of a Feldspathic Ceramic. J. Mech. Behav. Biomed. Mater. 2015, 48, 241–248. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ivoclar Vivadent AG Monobond Etch & Prime® Scientific Report. Available online: https://ivodent.hu/__docs/782_c2f358651979e78e5aa3434721af58c7.pdf (accessed on 5 October 2026).
- El-Damanhoury, H.M.; Gaintantzopoulou, M.D. Self-Etching Ceramic Primer versus Hydrofluoric Acid Etching: Etching Efficacy and Bonding Performance. J. Prosthodont. Res. 2018, 62, 75–83. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Azevedo, V.L.B.; de Castro, E.F.; Bonvent, J.J.; de Andrade, O.S.; Nascimento, F.D.; Giannini, M.; Cavalli, V. Surface Treatments on CAD/CAM Glass–Ceramics: Influence on Roughness, Topography, and Bond Strength. J. Esthet. Restor. Dent. 2021, 33, 739–749. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Awad, M.M.; Alhalabi, F.; Alotaibi, N.; Alzamil, F.; Binalrimal, S.; Alrahlah, A.; Ahmed, M.H. A Systematic Review and Meta-Analysis of Bond Strength Studies Associated with Self-Etching Primer and HF Acid Etching of Dental Glass-Ceramics. Int. J. Adhes. Adhes. 2022, 118, 103216. [Google Scholar] [CrossRef] [Scilit]
- Cardenas, A.F.M.; Quintero-Calderon, A.S.; de Siqueira, F.S.F.; Campos, V.S.; Wendlinger, M.; Pulido-Mora, C.A.; Masson-Palacios, M.J.; Sarmiento-Delgado, M.L.; Loguercio, A.D. Do Different Application Modes Improve the Bonding Performance of Self-Etching Ceramic Primer to Lithium Disilicate and Feldspathic Ceramics? J. Adhes. Dent. 2019, 21, 319–327. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Alsolami, A.; Alzahrani, K.M. Self-Etching Ceramic Primer Application Time Influences Durability of Bonding to Lithium Disilicate and Advanced Lithium Disilicate Ceramics. Coatings 2024, 14, 1461. [Google Scholar] [CrossRef] [Scilit]
- Alshihri, A. Etching Efficacy and Bonding Performance of Resin to Lithium Disilicate Ceramic Using Self-Etching Primer with Different Reaction Times. J. Adhes. Sci. Technol. 2019, 33, 1215–1225. [Google Scholar] [CrossRef] [Scilit]
- Kilinc, H.; Sanal, F.A.; Turgut, S. Shear Bond Strengths of Aged and Non-Aged CAD/CAM Materials after Different Surface Treatments. J. Adv. Prosthodont. 2020, 12, 273–282. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ivocalr Vivadent AG. IPS E.Max CAD Chairside: Instructions for Use. Available online: https://www.acdrc.com/wp-content/uploads/2015/03/IPS-e-max-CAD-Chairside.pdf (accessed on 23 November 2026).
- DeguDent GmbH CEREC TesseraTM Advanced Lithium Disilicate for CEREC® and inLab® Machines: Instructions for Use. Available online: https://bulario.dentsplysirona.com.br/C/cerectesserablocks.pdf (accessed on 5 October 2026).
- Prado, M.; Prochnow, C.; Marchionatti, A.M.E.; Baldissara, P.; Valandro, L.F.; Wandscher, V.F. Ceramic Surface Treatment with a Single-Component Primer: Resin Adhesion to Glass Ceramics. J. Adhes. Dent. 2018, 20, 99–105. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- VITA Zahnfabrik H. Rauter GmbH & Co.KG VITABLOCS®: Working Instructions—Fine-Structure Feldspar Ceramic Blocks for the Fabrication of Inlays, Onlays, Veneers and Crowns. Available online: https://cdn.vivarep.com/contrib/vivarep/media/pdf/4_4664_VITABLOCSMarkIITriLuxeTriLuxeforteReallifeWorkingInstructions_20170830213954839.pdf (accessed on 11 October 2026).
- Gale, M.S.; Darvell, B.W. Thermal Cycling Procedures for Laboratory Testing of Dental Restorations. J. Dent. 1999, 27, 89–99. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Cournault, B.; Vedrenne, L.; Prudence Felix, T.; Arnaud, E.; Grégoire, H.; Hamdi, J.; Naji, K.; Olivier, E. Optimizing Failure Mode Analysis of Dental Restorative Materials: Balancing Efficiency and Accuracy. In Proceedings of the 2024 IEEE International Symposium on Biomedical Imaging (ISBI); IEEE: Athens, Greece, 2024; pp. 1–5. [Google Scholar]
- Scherrer, S.S.; Cesar, P.F.; Swain, M.V. Direct Comparison of the Bond Strength Results of the Different Test Methods: A Critical Literature Review. Dent. Mater. 2010, 26, e78–e93. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Shimada, Y.; Kikushima, D.; Tagami, J. Micro-Shear Bond Strength of Resin-Bonding Systems to Cervical Enamel. Am. J. Dent. 2002, 15, 373–377. [Google Scholar] [PubMed]
- Ismail, A.M.; Bourauel, C.; Elbanna, A.; Eldin, T.S. Micro versus Macro Shear Bond Strength Testing of Dentin-Composite Interface Using Chisel and Wireloop Loading Techniques. Dent. J. 2021, 9, 140. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Sirisha, K.; Rambabu, T.; Ravishankar, Y.; Ravikumar, P. Validity of Bond Strength Tests: A Critical Review-Part II. J. Conserv. Dent. 2014, 17, 420–426. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Whitehead, S.A.; Shearer, A.C.; Watts, D.C.; Wilson, N.H.F. Comparison of Two Stylus Methods for Measuring Surface Texture. Dent. Mater. 1999, 15, 79–86. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Bajraktarova-Valjakova, E.; Grozdanov, A.; Guguvcevski, L.; Korunoska-Stevkovska, V.; Kapusevska, B.; Gigovski, N.; Mijoska, A.; Bajraktarova-Misevska, C. Acid Etching as Surface Treatment Method for Luting of Glass-Ceramic Restorations, Part 1: Acids, Application Protocol and Etching Effectiveness. Open Access Maced. J. Med. Sci. 2018, 6, 568–573. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Temp, R.W.; Packaeser, M.G.; Machry, R.V.; Dapieve, K.S.; Rippe, M.P.; Pereira, G.K.R.; Valandro, L.F. Characteristic Fatigue Strength and Reliability of Dental Glass-Ceramics: Effect of Distinct Surface Treatments—Hydrofluoric Acid Etching and Silane Treatment vs. One-Step Self-Etching Ceramic Primer. J. Mech. Behav. Biomed. Mater. 2024, 150, 106338. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Donmez, M.B.; Okutan, Y.; Yucel, M.T. Effect of Prolonged Application of Single-Step Self-Etching Primer and Hydrofluoric Acid on the Surface Roughness and Shear Bond Strength of CAD/CAM Materials. Eur. J. Oral Sci. 2020, 128, 542–549. [Google Scholar] [CrossRef] [Scilit] [PubMed]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.