Abstract
Orbital wall reconstruction with titanium meshes provides mechanical support, but the bio-inert metal surface limits osseointegration and may favor soft-tissue entrapment. This study evaluated a nanostructured hydroxyapatite–collagen (HAp-COL) hybrid derived from Rapana thomasiana (syn. Rapana venosa) shells as a 3D-printed coating for titanium orbital implants. The hybrid powder (HAp:COL mass ratio of 4:1) was obtained via high-pressure hydrothermal synthesis and spray drying and characterized using FAAS, ICP-OES, XRD, SEM–EDS, DLS, and DSC–TG. A solvent-free paste with polyvinyl alcohol and aqueous polyurethane binders was robocast at room temperature onto titanium meshes. Cytocompatibility was assessed using MTT assays on normal human osteoblasts, murine Swiss 3T3 fibroblasts, and adipose-derived mesenchymal stem cells (MSCs). Local tolerance was evaluated in a rabbit orbital bone defect model over 2 months. The powder was mainly crystalline hydroxyapatite with minor whitlockite (Ca:P = 1.68; Z-average hydrodynamic diameter: 75.81 nm). Cell viability exceeded the 70% threshold under all conditions except undiluted extracts on MSCs at 24 h (66.63%), which recovered to 75.47% at 48 h. In a single experiment, robocast HAp-COL coatings showed numerically higher osteoblast viability values (80.61–96.47%) than sprayed HAp coatings (70.62–93.63%). Descriptive histology and CD31/CD34 immunohistochemistry showed fibrovascular colonization and neovascularization without necrosis. These preliminary results indicate cytocompatibility and short-term local tissue tolerance; osteogenic activity, osseointegration, and the mechanical reliability of the coating remain to be demonstrated in controlled studies.
1. Introduction
Orbital wall fractures require precise surgical interventions to reconstruct complex bony geometries, prevent soft-tissue entrapment, and restore normal intraorbital volume [1,2,3]. While standard titanium mesh plates are widely used due to their superior mechanical load-bearing capacity, their inherent biological inertness often limits rapid, direct osseointegration with host tissues [4,5,6,7]. Consequently, modern maxillofacial and orthopedic research has shifted toward additive manufacturing (AM) and surface functionalization to develop patient-specific implants that match the defect’s precise anatomical architecture while presenting essential biochemical cues to the injury site [2,8,9,10,11,12,13].
Recent advancements have emphasized the critical importance of multifunctional surface modification strategies for implant materials [14,15,16]. In addition to facilitating bone growth, an ideal biomaterial surface must simultaneously regulate local inflammation, exhibit robust antibacterial properties, and stimulate accelerated osteogenesis to ensure long-term implant integration and reduce secondary failure rates [17,18,19,20]. To mimic the native bone extracellular matrix, hybrid composite systems integrating bioceramics and natural polymers have gained prominence [21,22]. Hydroxyapatite (HAp) provides biomimetic osteoconductivity, while collagen (COL) provides structural elasticity and cell adhesion motifs, mirroring the inorganic and organic phases of native trabecular bone, respectively [21,23,24].
Traditional manufacturing techniques for composite coatings often involve separate crystallization or separate procurement of mineral phases, which are subsequently combined using synthetic binders or high-temperature deposition methods, such as plasma spraying [25,26]. These high-velocity techniques cannot preserve fine organic components and fail to generate a homogeneous, porous structural framework [27]. Furthermore, using commercial synthetic precursors may restrict the biomimetic trace-element profile of the resulting ceramic phase [28,29,30]. The use of natural marine byproducts, such as the shells of the invasive marine invertebrate Rapana thomasiana, represents a sustainable approach to overcome these hurdles [31,32,33,34,35,36]. Extracting HAp from this natural resource yields a high-purity crystalline phase with enhanced biological affinity and minor essential trace elements [37], while simultaneously assisting regional marine ecosystems by controlling a destructive, overpopulated species [38].
Among various additive-manufacturing methods, robocasting, also known as direct ink writing (DIW), allows for the precise, layer-by-layer extrusion of highly loaded composite pastes at room temperature without the damaging thermal effects of lasers or ultraviolet light [39,40]. This technique produces highly porous, interconnected geometries that optimize nutrient exchange and cellular infiltration [41,42,43]. However, achieving a uniform mineral phase distribution and retaining geometric stability post-extrusion remain key manufacturing bottlenecks [44,45,46].
2. Materials and Methods
2.1. Extraction and High-Pressure Hydrothermal Synthesis of HAp-COL Hybrid Powder
The Ca precursor of the inorganic phase was sourced directly from the shells of the marine invertebrate Rapana thomasiana. The raw shells were thoroughly cleaned, dried, and mechanically ground using a Retsch RS 200 mill to yield a highly homogeneous precursor powder. The obtained precursor powder was dissolved in a 2:1 (vol%) mixture of HCl:HNO3 to obtain an aqueous solution of Ca, which is the Ca precursor of hydroxyapatite (HAp). Ammonium dihydrogen phosphate (NH4H2PO4), which is the P precursor of hydroxyapatite, and commercial hydrolyzed collagen were dissolved separately in distilled water, resulting in aqueous solutions with concentrations of up to 20%.
The resulting Rapana thomasiana-derived component (Ca precursor solution), P precursor solution, and hydrolyzed collagen solution were mixed under magnetic stirring in well-established proportions until homogenized to synthesize the hybrid HAp-COL matrix. Finally, the desired Ca:P molar ratio of 1.67 for the formation of stoichiometric hydroxyapatite and a mass ratio of 4:1 for the HAp:COL hybrid were obtained. The 4:1 HAp:COL mass ratio (80:20 wt%) was adopted from previous work of our group. It approximates the mineral-to-organic composition of native bone, in which carbonated apatite is the main component and type I collagen forms most of the organic matrix. The high mineral fraction also provides a sufficient solid loading of the paste for extrusion, whereas the collagen fraction contributes to granule cohesion and provides cell-adhesive sites.
The combined solution was then precipitated via the gradual, dropwise addition of 25% aqueous ammonia (NH3) until an alkaline target environment (pH = 10) was established. The resulting suspension was transferred into the Teflon vessel of a Berghof hydrothermal autoclave system (Berghof Products + Instruments GmbH, Eningen, Germany). Hydrothermal crystallization was maintained for 3 h under controlled conditions at a temperature of 80–100 °C and a high pressure of 100 atmospheres [47]. Pressure was created inside the Teflon vessel by bubbling argon—supplied from an argon cylinder equipped with a pressure gauge—over the suspension. The Berghof autoclave is equipped with a PID controller and computerized parameter recording to monitor pressure variations with temperature. Argon is bubbled over the suspension when the temperature inside the Teflon vessel reaches 80 °C and is controlled so as not to exceed 100 °C.
The nanostructured precipitate was separated from the aqueous phase via vacuum filtration and washed repeatedly with distilled water until reaching a neutral pH of 7 ± 0.5. The neutralized slurry was subsequently processed with a LabPLANT spray dryer at temperatures between 100 and 150 °C until the final residual water content was below 5%. This sequential co-precipitation and spray-drying approach yielded a nanostructured, granulated hybrid powder with a hydroxyapatite-to-collagen (HAp:COL) mass ratio of 4:1.
2.2. Physicochemical, Structural, and Morphological Characterization
The synthesized marine-derived hybrid powder was subjected to physicochemical characterization. Quantitative chemical analysis of the calcium (Ca) content was performed using flame atomic absorption spectrometry (FAAS). The total phosphorus (P) concentration was determined by inductively coupled plasma–optical emission spectrometry (ICP-OES). Metallic trace elements were quantified using the same techniques.
The crystalline phases and phase purity were evaluated via X-ray diffraction (XRD) using a Bruker-AXS D8 ADVANCE Bragg–Brentano diffractometer configured with a copper (Cu) radiation source and a SOL X detector in a vertical θ–θ geometry. Diffraction patterns were collected continuously within an angular window of 6–70° with a step size of 0.02°, processed using the DIFFRAC.EVA software (version 5.2; Bruker AXS GmbH, Karlsruhe, Germany),and indexed against the ICDD PDF-4+ database to yield qualitative raw patterns for the biogenic precursor and finalized hybrid structures.
Surface topography, particle morphology, and elemental distribution were analyzed using scanning electron microscopy (SEM) on an FEI Quanta 250 microscope (FEI Company, Eindhoven, The Netherlands) operated in high-vacuum (HV) mode with an Everhart–Thornley secondary electron detector (ETD) and an energy-dispersive X-ray spectroscopy (EDS) detector. Prior to analysis, the samples were sputter-coated with a 5 nm thick gold layer.
Hydrodynamic diameter of the filtered HAp:COL suspension was measured using dynamic light scattering (DLS) with a Zetasizer Nano ZS90 laser granulometer with a zeta potential module (Malvern Instruments, Worcestershire, UK), measurement range ≈ 0.3 nm–0.6 µm, a temperature range of 20–90 °C, a wet dispersion type, and specialized Zetasizer software 7.02 (Malvern Instruments Ltd., Malvern Panalytical Ltd., Cambridge, UK).
Thermal stability, material degradation, and mass loss profiles were recorded using differential scanning calorimetry and thermogravimetry (DSC–TG) with a Setaram Setsys Evolution instrument (Setaram Instrumentation, Caluire, France), heating up to 300 °C in alumina crucibles at a continuous rate of 10 K/min under an inert gas atmosphere.
2.3. Preparation of the Bio-Active Paste and 3D Robocasting Fabrication
For the formulation of the print-ready composite paste, 5 g of the hydrothermally synthesized HAp-COL hybrid powder (4:1 mass ratio) was mixed with a multi-component, non-toxic water-based binding system consisting of 8–10 mL of a 3% (w/v) aqueous polyvinyl alcohol (PVA) solution and 0.2–1 mL of an aqueous polyurethane dispersion [48]. The polyurethane dispersion possessed a solid content of 50–60%, a stable alkaline pH of 7–9, and a fluid viscosity of <2000 mPa·s at 23 °C.
The paste was processed using a Thinky-ARE 250 planetary centrifugal mixer to eliminate entrapped air bubbles and ensure chemical uniformity, which allowed the compounding and de-gassing sequences to occur directly inside the sterile 3D-printing syringe.
Robocasting (direct ink writing) was performed using a 3D Bio-Plotter Starter Series system (EnvisionTEC GmbH, Gladbeck, Germany). The paste was extruded layer by layer at room temperature onto medical-grade cranial osteosynthesis titanium mesh plates (dimensions: 40 × 60 mm, thickness: 0.3 mm, and configured for 1.6/2.0 mm surgical fixation screws; Table 1). The deposition of 3 successive structural layers was accomplished using a 0.4 mm nozzle diameter at an extrusion pressure of 3 bar with a strand distance of 0.8 mm. Alternative structural matrices were produced using a 0.6 mm nozzle diameter at 1.5 bar with identical spacing parameters. The layer deposition geometry followed an angled offset (0°/45°/90°) deposition pattern to construct an interconnected, porous layout with a final coating height of 0.96 mm. The configuration of the surgical fixation plates, comparing the bio-inert medical-grade titanium mesh wires with the 3D-printed HAp-COL composite layout, is macroscopically illustrated in Figure 1 (Sample 2).
Table 1.
Optimized formulation and extrusion parameters for room-temperature 3D robocasting.
Figure 1.
Evaluated substrates: sprayed HAp meshes (Sample 1); 3D-robocasted HAp-COL implants (Sample 2).
2.4. Multi-Lineage In Vitro Biological Screening
A multi-lineage biological screening matrix was structured to establish a comprehensive preclinical blueprint reflecting the unique intraorbital microenvironment encountered during orbital fracture repair. The rationale for this multi-cellular configuration stems directly from the target anatomical reconstructive site, which demands synchronized hard- and soft-tissue compatibility. Normal human osteoblasts (NHOsts) simulate the active bony boundaries of the fractured orbital walls and predict early osteoconductive anchoring. Adipose-derived mesenchymal stem cells (MSCs) mirror the regenerative and differentiation responses of native progenitor niches exposed to the dynamic signaling framework within the highly vascularized retrobulbar space. Lastly, fibroblasts were included to evaluate connective-tissue adaptations, specifically modeling the local tissue reactions required to mitigate risks of orbital tissue adherence, muscle entrapment, or chronic mucosal scarring at the posterior margins of the implant.
Three distinct cell models were employed to thoroughly map cytocompatibility and surface interactions: normal human osteoblasts (NHOsts; Lonza code CC-2538), murine Swiss 3T3 fibroblasts (ATCC CCL-92), and adipose-derived mesenchymal stem cells (MSCs; ATCC PCS-500-011).
NHOst lines were propagated in osteoblast growth medium enriched with 10% fetal bovine serum (FBS) and 50 μg/mL gentamicin. Swiss 3T3 cells were maintained in Dulbecco’s modified Eagle’s medium (DMEM) containing 10% calf serum and 50 μg/mL gentamicin. MSC populations were sustained in complete mesenchymal stem cell basal medium supplemented with an MSC growth kit.
Dose-dependent cytotoxicity screening was implemented via extract eluates prepared following ISO 10993-12 protocols [49,50]. All evaluated substrates—sprayed HAp meshes (Sample 1), 3D-robocasted HAp-COL implants (Sample 2 in Figure 1), 3D-compressed sintered tablets (Samples 6.2–6.12), and loose hybrid HAp-COL powders—were incubated in the respective cell growth media at a weight-to-volume ratio of 200 mg/mL for 24 h for loose powders and 72 h for coated meshes and sintered tablets at 37 °C under orbital agitation (450 rpm) using a Heidolph 1000 shaking incubator (Heidolph Scientific Products GmbH, Schwabach, Germany). Following extraction, the supernatants were collected and serially diluted twofold with fresh growth medium to obtain 1/2 (100 mg/mL), 1/4 (50 mg/mL), and 1/8 (25 mg/mL) test concentrations.
Cells were seeded in flat-bottom 96-well culture plates in 200 µL at the following target densities: 2.2 × 104 cells/well for NHOst (1.10 × 105 cells/mL stock), 3.34 × 104 cells/well for 3T3 (1.67 × 105 cells/mL stock), and 1.14 × 104 cells/well (5.7 × 104 cells/mL stock) for MSCs. After a 24 h attachment phase, cells were exposed to the varying extract dilutions and incubated for 24 and 48 h at 37 °C in a humidified 5% CO2 atmosphere.
Metabolic cell viability was quantified using a colorimetric MTT assay kit (Sigma-Aldrich; Roche Diagnostics GmbH, Mannheim, Germany) following the manufacturer’s instructions. After treatment, 20 μL of MTT reagent (5 mg/mL in PBS) was added to each well, and the plates were incubated for 4 h in the dark at 37 °C to allow the formation of insoluble formazan crystals. The supernatant was then carefully aspirated and replaced with 200 μL of anhydrous isopropanol containing 0.04 M HCl per well to completely solubilize the formazan crystals. Optical density (OD) was measured at 570 nm using an EnSight™ Multimode Microplate Reader (PerkinElmer, Waltham, MA, USA). Each plate included cell-free medium-plus-solvent wells as background blanks and untreated cells maintained in fresh growth medium as negative controls (set as 100% viability); a dedicated chemical positive cytotoxicity control was not included in this preliminary screening.
Cell survival percentages were determined by subtracting blank values and normalizing against untreated negative controls. Each condition was tested in four technical replicate wells within a single experiment; independent biological replicates were not performed. The viability data are therefore reported descriptively as mean values, and no statistical comparisons between samples were made.
The evaluation of potential material-related interference with the MTT assay, independent of cellular viability, was not performed in this study, as the primary objective was to assess the overall metabolic activity of cells following exposure to the tested materials. Nevertheless, potential interference arising from direct interactions between the material and the MTT reagent or formazan products cannot be entirely excluded and should be considered a limitation of the study.
2.5. In Vivo Local Tissue Response Model
An in vivo pilot biocompatibility trial was conducted using 5 adult male New Zealand White rabbits (Oryctolagus cuniculus), obtained from the animal facility of the Cantacuzino National Military Medical Institute for Research and Development, aged 6–8 months and weighing 3.2–3.8 kg [51,52]. The animals were housed in individual cages in a temperature-controlled environment (21 ± 2 °C, 55 ± 10% humidity, and a 12 h light/dark cycle) with ad libitum access to standard chow and water. As this study was designed as a descriptive pilot observation without bare titanium or unfilled defect control groups, qualitative histopathological and immunohistochemical endpoints at 2 months were analyzed descriptively. No formal sample size calculation was performed, as this was a descriptive pilot study. Because all animals received the same implant and no comparator groups were included, randomization and blinding were not applicable; histological sections were evaluated descriptively by an experienced pathologist.
A standard surgical exposure of the lower orbital region was performed under general anesthesia induced with xylazine (3 mg/kg, intramuscularly) and ketamine (5 mg/kg, intravenously). A controlled bone defect of approximately 5–10 mm was created using a surgical trephine mounted on a dental micromotor near the lacrimal gland (Figure 2).
Figure 2.
Intraoperative aspect of the bone defect created by drilling (black arrow) in the inferior border of the orbit near the lacrimal gland (yellow star).
The coated implants (approximately 5–10 mm in size) were adapted to the bony defects and stabilized using medical-grade titanium fixation screws. Postoperative monitoring was conducted over 2 months, with systemic enrofloxacin (0.5 mL/kg/day) and topical tobramycin/dexamethasone ophthalmic ointment as local therapy. Postoperative analgesia consisted of carprofen (4 mg/kg, subcutaneously, every 24 h) and buprenorphine (0.05 mg/kg, subcutaneously, every 8 h), both administered for 72 h after surgery. At the 6-week postoperative checkpoint, a computed tomography (CT) scan was recorded to verify implant positioning (Figure 3).
Figure 3.
CT scan of a rabbit performed at 6 weeks to verify the correct positioning of the titanium implant with the 3D-printed HAp-COL coating (black arrow).
At 2 months, the animals were euthanized with intravenous pentobarbital (200 mg/kg) after prior anesthesia with ketamine (5 mg/kg, intravenously). The explanted tissue blocks containing the implant cores and surrounding bony margins were fixed in 10% formalin and embedded in paraffin without decalcification to preserve structural layout interfaces. Sagittal sections (4 µm) were prepared using a rotary microtome and stained with hematoxylin–eosin (H&E) and Movat pentachrome protocols for qualitative light microscopy. Parallel 4 µm sections were deparaffinized, rehydrated, and subjected to heat-induced epitope retrieval in 10 mM sodium citrate buffer (pH 6.0) at 95 °C for 20 min, followed by blocking of non-specific binding sites. Sections were incubated overnight at 4 °C with primary monoclonal antibodies against Cluster of Differentiation 31 (CD31, clone JC/70A, Novus Biologicals, Centennial, CO, USA, 1:25) and Cluster of Differentiation 34 (CD34, clone MEC14.7, GeneTex, Irvine, CA, USA, 1:250). For chromogenic immunohistochemistry (brightfield microscopy), endogenous peroxidase activity was quenched with 3% H2O2, and immunoreactivity was detected using an HRP-conjugated anti-mouse polymer detection system with 3,3′-diaminobenzidine (DAB) as the chromogen and hematoxylin nuclear counterstaining. For laser-scanning confocal immunofluorescence (CD31), sections were incubated with Alexa Fluor 594-conjugated anti-mouse IgG and counterstained with Hoechst nuclear dye. Native host blood vessels within the surrounding peri-implant tissues served as internal positive controls, whereas sections processed with omission of the primary antibodies served as negative controls. Calibration data were embedded during image acquisition, where available; scale bars are displayed directly on the micrographs. For archived micrographs in which spatial calibration metadata were not retained at acquisition, calibrated scale bars could not be retrospectively generated, and relative magnifications (low or high magnification) are indicated in the corresponding figure legends.
All animal procedures were conducted in strict compliance with EU Directive 2010/63/EU and are reported in accordance with the ARRIVE 2.0 guidelines; they were approved by the Ethics Committee of the Cantacuzino Institute (approval no. A7440/2022).
3. Results and Discussion
3.1. Physicochemical, Structural, and Thermal Validation
Quantitative chemical analysis of the raw Rapana thomasiana ground shell precursor was performed using ICP-OES and revealed high calcium concentrations (41.2% Ca) alongside minor trace fractions of structural elements such as magnesium (0.10% Mg), strontium (0.11% Sr), sodium (0.19% Na), and iron (0.023% Fe; Table 2). Crucially, phosphorus was absent in the raw shell mass (<0.005%), confirming that the natural material consists entirely of pristine calcium carbonate phases. Phase mapping via X-ray diffraction verified that the raw shell powder was composed of highly crystalline calcite (rhombohedral CaCO3), aragonite (orthorhombic CaCO3), and trace quartz impurities (SiO2).
Table 2.
Elemental composition (wt.%) of the powder obtained by grinding Rapana thomasiana shells.
Following high-pressure hydrothermal synthesis, elemental analysis of the final HAp-COL hybrid powder confirmed a significant structural transformation, yielding a calcium content of 35.94% and a phosphorus content of 16.5%. This corresponded to an empirical Ca:P molar ratio of 1.68, in close agreement with the theoretical stoichiometric ratio of native bone hydroxyapatite (Ca:P = 1.67).
Elemental analysis of the powder obtained by grinding Rapana shells (Table 2) revealed a predominantly calcium-based mineral composition, with a calcium content of 41.2% (412,000 mg/kg). This high calcium concentration confirms the mineral-rich nature of the raw material and supports its suitability as a precursor for hydroxyapatite-based biomaterials. In addition to calcium, measurable concentrations of sodium (0.19%; 1900 mg/kg), strontium (0.11%; 1100 mg/kg), magnesium (0.10%; 1000 mg/kg), sulfur (0.058%; 580 mg/kg), aluminum (0.057%; 570 mg/kg), silicon (0.049%; 490 mg/kg), iron (0.023%; 230 mg/kg), and potassium (0.008%; 80 mg/kg) were detected.
From a toxicological perspective, particular attention should be paid to aluminum and iron, which were detected at concentrations of 570 mg/kg and 230 mg/kg, respectively. Although these elements are present at relatively low concentrations compared with calcium, their potential biological effects depend on their chemical speciation, solubility, and bioavailability. When present in bioavailable forms and at sufficiently high concentrations, aluminum may interfere with cellular metabolic processes and mineralization pathways [53]. Similarly, iron is an essential trace element involved in numerous cellular functions; however, an excess of free iron ions may promote oxidative stress through the generation of reactive oxygen species, including via Fenton-type reactions [54]. Nevertheless, the total concentrations determined in the raw powder cannot be directly interpreted as the concentrations of bioavailable Al3+ or Fe ions in the cell culture extracts.
The detected strontium concentration (1100 mg/kg) is particularly relevant to the intended bone-regenerative applications of the HAp-COL material. Strontium has been associated with bone metabolism and osteoblast activity, although its biological effects strongly depend on the concentration and chemical form in which it is released [55,56,57]. Magnesium, detected at 1000 mg/kg, is also an important constituent owing to its involvement in cellular metabolism, enzymatic activity, and bone mineralization [58]. The high calcium content (412,000 mg/kg), together with the presence of magnesium and strontium, may contribute to the mineralogical and biological characteristics of the synthesized material.
Sodium, detected at 1900 mg/kg, may also influence the biological response, as changes in the ionic composition of the surrounding medium can affect osmotic balance and cellular homeostasis. In particular, the combined release of calcium, sodium, magnesium, and other soluble ionic species from concentrated powder extracts may alter the physicochemical conditions of the culture environment. Such changes could partly explain the reduced cell viability observed at the highest extract concentration.
Regarding potentially toxic trace elements, arsenic (As), cadmium (Cd), lead (Pb), chromium (Cr), nickel (Ni), copper (Cu), and barium (Ba) were all below 0.005% (i.e., <50 mg/kg). These findings indicate a favorable chemical purity of the starting material, particularly given the recognized toxicological relevance of arsenic, cadmium, and lead. However, values below the analytical quantification limit should not be interpreted as a complete absence of these elements. Furthermore, their potential biological relevance depends on their actual release into the aqueous extraction medium and their subsequent bioavailability. Because the shells are a natural raw material, their trace-element content may vary between batches. In this study, the Ca:P ratio of the final powder was controlled through the precursor stoichiometry, but the batch-to-batch variability of the trace elements was not assessed.
Qualitative X-ray diffraction analysis of the HAp-COL hybrid powder showed a well-crystallized hydroxyapatite—(Ca5(PO4)3(OH)—as the main phase, with a hexagonal crystal structure, alongside a minor secondary phase of whitlockite—(Ca9Mg(HPO4)(PO4)6—with a rhombohedral crystal structure (Figure 4b, Table 3) [51]. This multi-phase profile is consistent with the diffraction curves in Figure 4. Figure 4a shows the crystalline phase profile of the raw Rapana thomasiana ground shell precursor, indexing its calcite (▼), aragonite (●), and trace quartz (◊) reflections. The relative amounts of hydroxyapatite and whitlockite were not quantified in this study (e.g., by Rietveld refinement). Because whitlockite is more soluble than hydroxyapatite, its content may influence ion release, biological activity, and the stability of the coating [51]. In the absence of quantitative phase analysis, the contribution of whitlockite to the dissolution of the coating and to the ion content of the cell culture extracts cannot be estimated, and the biological results reported here cannot be attributed to a defined phase composition. For the same reason, the degradation and remodeling observed in vivo cannot be related to the solubility of a specific phase, and conclusions regarding the long-term chemical stability of the coating cannot be drawn. Quantitative phase analysis by Rietveld refinement is planned for future batches.
Figure 4.
(a) XRD phase analysis of the raw Rapana thomasiana ground shell precursor, where (▼) denotes calcite, (●) denotes aragonite, and (◊) indicates trace quartz impurities; (b) XRD phase analysis of the hydrothermally processed hybrid matrix, where (▼) denotes hydroxyapatite as the major crystalline phase, and (◊) denotes whitlockite as a minor secondary phase.
Table 3.
Crystalline phases and structural orientations via XRD validation.
SEM examination in high-vacuum mode revealed a uniform, spheroidal particle morphology consisting of porous aggregates ranging in size from several hundred nanometers to a few micrometers (Figure 5a). This spheroidal particle shape is expected to favor paste flowability and a uniform viscosity during extrusion. Semi-quantitative EDS analysis of the hybrid powder identified Ca, P, O, and C, with the corresponding mass percentages shown in Figure 5b; the C signal is consistent with the presence of the collagen component. However, EDS is semi-quantitative and has limited accuracy for light elements such as carbon, and the C signal alone does not confirm the presence or structural integrity of collagen. Because collagen was not characterized using complementary methods (e.g., FTIR spectroscopy or thermogravimetric analysis extended to the decomposition range of collagen), its presence in the final powder is inferred from the synthesis route rather than demonstrated directly. Notably, the Ca:P molar ratio derived from the EDS data is consistent with the theoretical stoichiometric ratio of bone hydroxyapatite (Ca:P = 1.67), corroborating the results of the chemical analysis of the HAp-COL powder reported above.
Figure 5.
(a) SEM image of the HAp-COL hybrid powder acquired in high-vacuum mode; (b) EDS spectrum of the hybrid powder (elemental composition, wt.%: C, 2.70; O, 49.51; P, 15.14; Ca, 32.65).
The particle size distribution was measured using DLS by preparing a stable suspension based on HAp-COL powder, double-distilled water, ethanol, and the commercial dispersant Duramax D3005. The suspension was filtered through a Millipore membrane (pore size: 0.22 μm). DLS analysis of the HAp-COL suspension showed an average hydrodynamic diameter (Z-average) of 75.81 nm (Figure 6). Because the suspension was passed through a 0.22 µm membrane prior to measurement, this Z-average value represents the hydrodynamic diameter of the dispersed sub-micron fraction in liquid medium rather than the primary crystallite size or the larger spheroidal aggregates (0.77–3.58 µm) observed in the dry state using SEM.
Figure 6.
Particle size distribution of the HAp-COL sample in stable suspension after filtration through a Millipore membrane with a pore size of 0.22 µm.
The thermal behavior of the hybrid powder was examined using DSC–TG analysis (Figure 7). The sample (HAp-COL hybrid powder) was thermally stable in the studied temperature range (25–300 °C); the total mass loss was 1.97%. The DSC curve displays two endothermic peaks: a primary peak at 63.5 °C due to surface moisture evaporation, and a minor peak at 142.5 °C (ΔH ≈ 6 J/g), representing the loss of residual bound water (the final dehydration phase). The analyzed range did not include the main thermal decomposition of collagen, which occurs above 300 °C.
Figure 7.
DSC–TG curve of the hydrothermally processed hybrid matrix. The blue line represents heat flow, while the green line represents the thermogram (indicating the mass loss).
3.2. Robocasting Performance and Coating Geometry
The processing method directly governs the biological and mechanical performance of the formulated paste. Traditional scaffolds that incorporate separately crystallized raw components with volatile organic solvents often exhibit heterogeneous mineral distribution, which predisposes them to nozzle clogging [59], and carry a risk of trapped cytotoxic chemical residues [60,61].
In contrast, with the co-precipitation strategy used here, the nanostructured hydroxyapatite crystals precipitate within the collagen network, so that the mineral cores are surrounded by an organic collagen layer. Bare, medical-grade titanium meshes typically present smooth, commercially pure, bio-inert substrates that lack intrinsic cell-binding motifs, as reviewed in the recent craniofacial literature [62]; the robocast coating adds a porous, calcium phosphate-based layer to these surfaces. The printing parameters define a nominal filament diameter of 0.4 mm (nozzle diameter) and a strand distance of 0.8 mm. Measurements on optical micrographs of a standalone robocast HAp-COL structure showed filament widths of 354.1–377.7 µm, close to the nozzle diameter, and transverse gaps of 657.6–762.3 µm. The resulting 0°/45°/90° layered design yields an interconnected porous topology that is expected to allow tissue cell migration [42,43]. These values represent the range observed on a single standalone printed structure and indicate the printing fidelity of the paste; they were not measured on the coating applied to the titanium mesh. A statistical characterization of the coating geometry on the coated meshes (number of measurements, mean ± SD, and specimen-to-specimen reproducibility) was not performed; the reproducibility of the coating geometry therefore remains to be established and is listed as a limitation of this study.
During placement, the surrounding soft tissues are expected to be in contact with the collagen component of the coating rather than with exposed mineral surfaces, which may help to limit foreign-body reactions and soft-tissue adhesion in the delicate periocular region; this hypothesis requires confirmation in comparative studies. No detachment of the coating from the titanium mesh was observed during sample handling and measurements; however, this observation is not a substitute for quantitative adhesion testing. The adhesion strength of the coating to the titanium substrate was not measured, and the mechanical reliability of the coated mesh under surgical conditions (e.g., contouring of the mesh, screw fixation, and contact with the surrounding tissues) has therefore not been confirmed. Standardized adhesion testing is required before any clinical application.
3.3. Multi-Lineage Quantitative Biological Evaluation
The quantitative colorimetric MTT datasets across all three tested cellular models established a favorable cytocompatibility profile for the HAp-COL structures. All evaluated samples showed a dose-dependent response. The lowest metabolic viabilities were recorded when cells were exposed to the raw, unmodified 200 mg/mL stock eluates, with cell survival increasing progressively as extract concentrations were reduced and reaching maximum values at the 1/8 dilution (Table 4). The data are presented as mean values of four technical replicate wells from a single experiment. Because independent biological replicates were not performed, measures of between-experiment variability and statistical comparisons are not reported, and the data should be interpreted descriptively.
Table 4.
Multi-lineage cell viability (%) after exposure to hybrid HAp-COL precursor extracts. Values are means of four technical replicates from a single experiment.
The relationship between the chemical composition and the biological findings presented in Table 4 indicates a concentration-dependent cellular response to the hybrid HAp-COL precursor extracts. After 24 h of exposure to the undiluted stock extract (200 mg/mL), 3T3 fibroblasts exhibited a viability of 80.69%, whereas adipose-derived MSCs showed a lower viability of 66.63%, suggesting that susceptibility to the extract depends on the cell population investigated. The reduction in MSC viability below the 70% threshold commonly used to interpret cytotoxicity according to ISO 10993-5 [63] indicates a potential cytotoxic response under this specific experimental condition.
This initial reduction in MSC viability may be associated with the combined effects of soluble mineral constituents released from the powder, including calcium, sodium, magnesium, and potentially bioavailable aluminum and iron species. Changes in ionic balance, osmolarity, and extracellular pH may also contribute to the observed metabolic suppression. However, the individual contribution of each element cannot be established solely on the basis of the total elemental composition of the starting powder.
The concentration-dependent nature of this response is supported by the progressive increase in MSC viability upon extract dilution, which reached 77.27%, 85.04%, and 91.35% at the 1/2, 1/4, and 1/8 dilutions, respectively, after 24 h. These findings indicate improved cellular tolerance as the extract concentration decreases. After 48 h, MSC viability remained above the 70% threshold under all tested conditions, with values of 75.47%, 81.34%, 84.65%, and 87.08% for the stock, 1/2, 1/4, and 1/8 dilutions, respectively. This suggests that the initial inhibitory effect observed at the highest concentration was not sustained at the same magnitude during prolonged exposure.
The 3T3 fibroblast population showed comparatively higher tolerance, with viability values ranging from 80.69% to 89.24% after 24 h and from 79.10% to 91.79% after 48 h, indicating that the tested extracts did not induce substantial metabolic suppression in this cell line. The differences between fibroblasts and MSCs may reflect distinct metabolic characteristics and differential sensitivity to changes in the ionic and physicochemical composition of the culture environment.
According to ISO 10993-5, a reduction in cell viability of more than 30% (i.e., viability below 70%) indicates a cytotoxic effect. Therefore, the undiluted extract of the raw hybrid powder (200 mg/mL) had a cytotoxic effect on MSCs at 24 h (66.63%). This effect may be related to osmotic stress and rapid ion release from high-concentration powder eluates in static culture; extract-based tests of calcium phosphate powders are known to be sensitive to these factors [50]. Viability exceeded 70% when the extract was diluted (77.27% at 1/2 and 91.35% at 1/8) and after 48 h of exposure to the undiluted extract (75.47%).
At 48 h, the undiluted extract slightly decreased 3T3 viability (79.10%), whereas viability with the diluted extracts reached up to 91.79%.
In MSCs exposed to the undiluted extract, viability increased from 66.63% at 24 h to 75.47% at 48 h. This may reflect a partial adaptation of the cells to the extract; however, the underlying mechanism was not investigated.
The findings presented in Table 5 provide additional information on the biological compatibility of the two implant coating configurations with NHOsts. At the highest extract concentration (200 mg/mL), the sprayed HAp mesh (Sample 1) yielded a viability of 70.62% after 24 h, whereas the 3D-robocasted HAp-COL structure (Sample 2) yielded a higher viability of 80.61%. This difference of 9.99 percentage points was obtained in a single experiment and was not tested statistically; it should therefore be regarded as a preliminary observation.
Table 5.
Osteoblast viability (%) over sprayed versus 3D-robocasted implant interfaces. Values are means of four technical replicates from a single experiment.
After 48 h, osteoblast viability increased to 77.28% for the sprayed HAp mesh and to 83.35% for the 3D-robocasted HAp-COL structure, and a similar trend was observed across all dilution levels. Notably, at the 1/8 dilution, the HAp-COL structure reached the highest viability value (96.47%) after 48 h, compared with 93.63% for the sprayed HAp mesh. These findings suggest favorable osteoblast compatibility for both configurations, with numerically higher viability values for the 3D-robocasted HAp-COL structure at all dilutions; confirmation in independent experiments with statistical analysis is required.
If confirmed, the higher viability values observed with the HAp-COL configuration may be associated with differences in surface architecture, mineral distribution, and porosity, as well as with the presence of the collagen component, which may provide additional cell-interactive domains [22]. Furthermore, the calcium- and strontium-containing mineral constituents may contribute to the biological behavior of the coating through their potential involvement in bone-related cellular processes. Nevertheless, the observed differences cannot be attributed exclusively to the elemental composition, since comparative ion-release measurements for the two coating configurations were not available.
Overall, the chemical composition results demonstrate that the Rapana shell-derived powder is characterized by a high calcium content and low concentrations of the potentially toxic elements investigated. Although aluminum and iron were detected at 570 mg/kg and 230 mg/kg, respectively, their actual contribution to the reduced MSC viability observed at the highest extract concentration remains undetermined. The biological findings more plausibly reflect the combined influence of extract concentration, ionic composition, physicochemical changes in the culture medium, and cell-specific metabolic responses.
The viability observed in fibroblasts, MSCs, and osteoblasts is relevant to orbital reconstruction, in which the implant is in contact with both bone and soft tissues. These results indicate that the HAp-COL coating is cytocompatible with cell types relevant to this site; they do not demonstrate osteogenic differentiation.
Osteoblast viability remained above 70% for both implant configurations at 24 and 48 h (Table 5).
The higher viability obtained with the robocast HAp-COL coating may be related to the preservation of the collagen component and of the porous architecture during room-temperature processing, which cannot be achieved with high-temperature thermal-spraying methods; this interpretation requires confirmation.
Overall, the in vitro data indicate that the HAp-COL coating is cytocompatible, with the exception of the undiluted powder extract on MSCs at 24 h. Because the MTT assay measures metabolic activity only, these results demonstrate cytocompatibility and not osteogenic activity. Alkaline phosphatase activity, the expression of osteogenic markers (e.g., RUNX2 and osteocalcin), and matrix mineralization (e.g., Alizarin Red staining) were not assessed and are required to establish the osteogenic potential of the coating.
While this multi-lineage screening indicates cytocompatibility, static in vitro models cannot fully simulate the immune cascades, vascular remodeling dynamics, or mechanical stresses encountered in vivo. Furthermore, commercial primary cells, such as the adipose-derived MSC lines used, carry inherent risks of phenotypic drift over successive passages compared with patient-isolated primary lines. In addition, the fibroblasts used were a murine cell line (Swiss 3T3), which does not fully represent human orbital fibroblasts. Therefore, evaluating these robocast configurations within animal defect models is essential to validate degradation rates, soft-tissue attachment kinetics, and long-term osseointegration. Pairing quantitative MTT screening with tissue-level qualitative evaluations will provide direct visual tracking of cellular spreading, mature collagen matrix organization, and angiogenesis across identical extended endpoints.
3.4. Qualitative In Vivo Biocompatibility and Tissue Integration Evaluation
To expand the biocompatibility assessment beyond the static limits of quantitative in vitro metabolic screening (MTT), the dynamic biological interface between the 3D-printed hybrid matrix and host cellular environments was qualitatively characterized using an in vivo animal model.
Microphotographs obtained with conventional and special histological stains were used to evaluate the local tissue response to the HAp-COL coating. Hematoxylin–eosin (H&E)-stained sections showed cellular infiltration throughout the three-dimensional robocast macroporous architecture. Host cells were present within the interconnected pore channels of the scaffold, and no localized tissue necrosis, thick fibrous encapsulation, or acute polymorphonuclear infiltrates were observed at the implant boundaries (Figure 8). A well-preserved bundle of eosinophilic skeletal muscle fibers, with normal morphology and peripheral nuclei, ran diagonally through the section. A cluster of mature adipose tissue, composed of adipocytes within a delicate connective tissue meshwork, was adjacent to the inferior boundary of the muscle. The left part of the biopsy contained several intact lobules of a serous gland, identified as the adjacent lacrimal gland, with tightly packed basophilic acini, uniform round nuclei, and normal secretory compartments. Spindle-shaped fibrocytes and fibroblasts were present within a loose connective tissue matrix at the superior margin of the muscle, consistent with a regenerative response along the surgical tract. Overall, these descriptive findings indicate good local tolerability of the Rapana thomasiana-derived coating in the multi-tissue environment of the orbit at 2 months; in the absence of control groups, they cannot be considered evidence of bone regeneration or osseointegration.
Figure 8.
Panoramic histopathological overview of the peri-implant orbital tissue beds and the implanted biomaterial matrix 2 months post-surgery (H&E staining). (A) Adjacent normal tissues, showing a diagonal central band of striated skeletal muscle (blue arrow), an adjacent cluster of mature adipocytes (yellow arrow), and healthy basophilic acini of the neighboring serous lacrimal gland (red arrow). (B) Panoramic cross-section of the undecalcified hydroxyapatite–collagen implant filling the defect. Host cells infiltrate the open macroporous architecture, without thick fibrous encapsulation or focal necrosis.
The tissue response at the implant site was further examined with Movat pentachrome staining (Figure 9, panel A), which showed a well-preserved tissue fragment with the native periosteum (1) and adjacent skeletal muscle fibers (2) bordering a zone of granulation tissue within a fibrin matrix (3). At higher magnification (Figure 9, panels B–D), numerous newly formed vessels were visible within the yellow–red-stained fibrin network, together with erythrocytes and inflammatory cells, indicating an ongoing remodeling process. The endothelial nature of these vessels was examined using immunofluorescence and chromogenic immunohistochemistry (IHC). Confocal immunofluorescence (Figure 9, panel E) showed CD31 expression (red) along the endothelial cell membranes of the newly formed capillaries, with nuclei counterstained with Hoechst (blue). Chromogenic CD31 IHC (Figure 9, panel F) showed linear endothelial staining lining patent capillary lumina. Together, these observations indicate that the macroporous coating did not induce tissue necrosis or ischemia at 2 months and was associated with local angiogenesis and provisional matrix remodeling.
Figure 9.
Characterization of newly formed vascular structures and tissue remodeling inside the peri-implant granulation zone 2 months post-implantation in a rabbit model. (A) Low-magnification overview via Movat pentachrome staining illustrating the structural hierarchy: (1) periosteum, (2) skeletal muscle, and (3) active granulation tissue developed within a provisional fibrin matrix. (B–D) High-magnification microphotographs detailing localized microvascular beds. Blue arrows mark the proliferation of newly formed vessels, black arrows define the structural grids of the provisional fibrin matrix, and green arrows trace localized erythrocytes and infiltrating inflammatory cells. (E) Confocal immunofluorescence confirming distinct membrane expression of CD31 (red) in the newly formed capillaries, counterstained with Hoechst nuclear dye (blue). (F) Chromogenic CD31 immunohistochemistry highlighting distinct vascular endothelial profiles (red arrows) within the tissue architecture, indicating local angiogenesis.
Movat pentachrome staining (Figure 10, panel A) showed the anatomical relationships within the explanted tissue block: the fibrous periosteum (arrow 1) and multi-fascicular skeletal muscle (arrow 2) adjacent to a zone of granulation tissue within a provisional fibrin matrix (arrow 3). At higher magnification (Figure 10, panel B), capillaries were visible within the turquoise/green-stained ground substance and collagen matrix near the material border. Newly formed vessels containing erythrocytes, together with monocytes and other inflammatory cells, were present in the provisional matrix, without signs of an acute toxic reaction or tissue necrosis. Chromogenic immunohistochemistry for endothelial markers (Figure 10, panel C) showed brown staining of the continuous endothelial linings (red arrows) of capillaries extending into the pore spaces. These findings indicate vascularized tissue ingrowth into the multilayer robocast structure.
Figure 10.
Histological and immunohistochemical characterization of newly formed vascular structures and tissue remodeling inside the peri-implant granulation zone 2 months post-implantation in a rabbit model. (A) Low-magnification overview via Movat pentachrome staining mapping the structural hierarchy: (1) periosteum, (2) skeletal muscle tissue, and (3) specialized granulation tissue developed within a provisional fibrin matrix. (B) High-magnification details within the matrix meshwork. The white arrow indicates cells within the ground substance; black arrows indicate newly formed microvascular spaces containing erythrocytes and inflammatory cells. (C) Chromogenic immunohistochemistry confirming distinct endothelial lining positivity (red arrows) of newly formed capillaries, indicating local angiogenesis.
Immunohistochemistry for CD31 (PECAM-1) showed membranous staining along the endothelial borders of microvascular channels penetrating the macroporous architecture (Figure 11). Areas of osteoid-like matrix were observed at the material interface; because this finding was not confirmed by specific staining or histomorphometry, it is reported descriptively. Multinucleated giant cells were also observed adjacent to the bioceramic granules. The observed features are limited to their morphology (large cells with multiple nuclei) and their location next to the material. Their identity and function were not determined: in the absence of specific markers (e.g., TRAP and CD68), they could correspond to foreign-body giant cells or to osteoclast-like cells [20,64], and no conclusion can be drawn as to whether they participate in material degradation or remodeling. Likewise, the absence of thick fibrous encapsulation and necrosis at 2 months is compatible with a mild foreign-body reaction, but the stains used do not allow the underlying mechanism to be established, and a chronic inflammatory component cannot be excluded. The endothelial identity of the vessels was further supported by CD34 staining (Figure 12), which labeled the endothelial lining of newly formed capillaries, together with small clusters of leukocytes. This vascular network within the pores suggests that the macroporous architecture allows the supply of oxygen and nutrients to the ingrowing tissue [65,66].
Figure 11.
Brightfield immunohistochemical expression of CD31 at the tissue–implant interface after a 2-month observation period in the rabbit model. Brown chromogenic DAB staining highlights endothelial cell linings (blue arrow) of patent capillaries and cells within the fibrovascular tissue along the porous hydroxyapatite grid (yellow star).
Figure 12.
Immunohistochemical CD34 evaluation of the non-decalcified hydroxyapatite–collagen implant interface in the rabbit model 2 months post-implantation. (A) Low-magnification overview mapping the structural organization and host tissue infiltration within the robocasted macroporous framework. (B,C) High-magnification microphotographs detailing distinct, dark-brown CD34+ expression (white arrows) along the endothelial borders of newly formed capillaries and in spindle-shaped cells lining the spheroidal mineral granules (black arrowheads), consistent with local angiogenesis. (D) Isolated tissue strand demonstrating CD34+ staining in cells and microvascular channels (yellow arrows) bridging the host–implant contact points.
The material (the large, granulated pinkish-grey spherical clusters; Figure 11, yellow stars) is not a solid, dense block; it is organized into distinct clusters with wide, open channels breaking through them. This indicates that the robocast structure retained its open, interconnected macroporous architecture after implantation and that the pores were large enough to allow host tissue to grow into the implant core.
CD34 immunohistochemistry was used to further evaluate microvascular remodeling at the interface of the 3D-printed hydroxyapatite–collagen implant (Figure 12). At low magnification (Figure 12, panel A), the undecalcified sections showed preserved interconnected macroporous channels between the robocast bioceramic structures. Host cells infiltrated the pore spaces, without thick fibrous encapsulation. At higher magnification (Figure 12, panels B and C), CD34+ staining was localized in endothelial cells and spindle-shaped cells lining the spheroidal hydroxyapatite granules. Because CD34 is expressed by endothelial cells and by some progenitor and stromal cells, these findings are consistent with early angiogenesis within the printed 0°/45°/90° geometry [67], but they do not identify the cell lineages unequivocally. Panel D (Figure 12) shows CD34+ cells and vascular channels in a tissue strand bridging the host–implant margin. Overall, the CD34 staining supports the presence of vascularized fibrovascular tissue within the coating at 2 months; long-term integration and bone formation remain to be demonstrated.
4. Conclusions
In this study, a hydroxyapatite–collagen (HAp-COL) hybrid powder was synthesized from Rapana thomasiana shells using a high-pressure hydrothermal process. The powder consisted mainly of crystalline hydroxyapatite with minor whitlockite, had a Ca:P molar ratio of 1.68, close to that of stoichiometric hydroxyapatite, and was composed of particles with an average hydrodynamic diameter (Z-average) of 75.81 nm organized into spheroidal aggregates.
Using non-toxic, solvent-free polymer binders, a paste was prepared at room temperature and robocast onto medical-grade titanium meshes without nozzle clogging. In vitro, cell viability was above the 70% threshold of ISO 10993-5 for NHOst, Swiss 3T3, and MSC cells under all conditions, except for the undiluted powder extract on MSCs at 24 h (66.63%), which increased to 75.47% at 48 h. In a single experiment, osteoblast viability values were numerically higher for the robocast HAp-COL coating (80.61–96.47%) than for the sprayed HAp coating (70.62–93.63%).
In a rabbit orbital defect model, histology and CD31/CD34 immunohistochemistry at 2 months showed good local tolerability, fibrovascular tissue ingrowth into the porous coating, newly formed capillaries, and areas of osteoid-like matrix at the material interface, without necrosis or thick fibrous encapsulation. These descriptive findings do not constitute evidence of bone regeneration or osseointegration.
This study has several limitations. The in vivo experiment was a descriptive pilot study in five rabbits, with a single time point (2 months), without bare titanium or empty-defect control groups, and without histomorphometric quantification. The adhesion strength of the coating to the titanium substrate and the mechanical behavior of the coated mesh were not measured; therefore, the mechanical reliability of the coating for surgical use has not been confirmed. The phase composition was not quantified (e.g., by Rietveld refinement), the batch-to-batch variability of the natural raw material was not assessed, and the coating geometry was not characterized statistically. The cytocompatibility data were obtained in a single experiment with technical replicates only, without statistical analysis, and the fibroblast model was a murine cell line. The presence and integrity of collagen in the final material were not confirmed using complementary methods. Osteogenic differentiation markers (alkaline phosphatase activity, osteogenic gene expression, and matrix mineralization) were not evaluated in vitro, and the multinucleated giant cells were not characterized with specific markers. In addition, the HAp:COL ratio was not optimized with respect to the mechanical and degradation properties of the coating.
Therefore, the present results provide preliminary evidence of the cytocompatibility, local tolerability, and fibrovascular colonization of the robocast HAp-COL coating on titanium meshes. Its osteogenic activity, mechanical reliability, and long-term efficacy in orbital reconstruction require further validation in controlled studies.
Author Contributions
Conceptualization, O.L., R.I. and S.I.; methodology, L.-M.C. and D.M.P.; investigation, A.M.C., C.H. and V.S.; writing—original draft preparation, O.L.; writing—review and editing, A.P.-C. and E.S. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded through the project “INO-ORBITAL”; SMIS code: 108688.
Institutional Review Board Statement
The animal study protocol was approved by the Ethics Committee of the Cantacuzino National Military Medical Institute for Research and Development (approval no. A7440/2022). All animal procedures were conducted in accordance with EU Directive 2010/63/EU on the protection of animals used for scientific purposes and are reported following the ARRIVE 2.0 guidelines.
Informed Consent Statement
Not applicable.
Data Availability Statement
The data presented in this study are available on request from the corresponding authors.
Conflicts of Interest
The authors declare no conflicts of interest.
Abbreviations
The following abbreviations are used in this manuscript:
| 3T3 | A standard continuous cell line of mouse embryonic fibroblasts |
| AM | Additive manufacturing |
| ATCC | American Type Culture Collection |
| CD31 | Cluster of Differentiation 31 (PECAM-1) |
| CD34 | Cluster of Differentiation 34 |
| COL | Collagen |
| CT | Computed tomography |
| DIW | Direct ink writing (robocasting) |
| DLS | Dynamic light scattering |
| DMEM | Dulbecco’s modified Eagle’s medium |
| DMSO | Dimethyl sulfoxide |
| DSC-TG | Differential scanning calorimetry–thermogravimetry |
| EDS | Energy-dispersive X-ray spectroscopy |
| ETD | Everhart–Thornley detector (secondary electron detector) |
| FAAS | Flame atomic absorption spectrometry |
| FBS | Fetal bovine serum |
| H&E | Hematoxylin–eosin |
| HAp | Hydroxyapatite |
| HV | High vacuum |
| ICDD | International Centre for Diffraction Data |
| ICP-OES | Inductively coupled plasma–optical emission spectrometry |
| IHC | Immunohistochemistry |
| ISO | International Organization for Standardization |
| MSC | Mesenchymal stem cell |
| MTT | 3-(4,5-dimethylthiazol-2-yl)-2,5-diphenyltetrazolium bromide (colorimetric metabolic cell viability assay) |
| NHOst | Normal human osteoblast |
| Powder diffraction file | |
| PVA | Polyvinyl alcohol |
| SEM | Scanning electron microscopy |
| XRD | X-ray diffraction |
References
- Eldek, Y.; Sleem, H.; Katamesh, M.; Hasanin, F. Perspective Chapter: Orbital Reconstruction and Orbital Volume. In Dental Trauma and Adverse Oral Conditions—Practice and Management Techniques; Moolla, A., Ed.; IntechOpen: London, UK, 2023. [Google Scholar] [CrossRef] [Scilit]
- Yang, M.K.; Sa, H.-S. Patient-specific implants for orbital fracture surgery. Taiwan J. Ophthalmol. 2026, 16, 35–43. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Sivam, A.; Enninghorst, N. The Dilemma of Reconstructive Material Choice for Orbital Floor Fracture: A Narrative Review. Medicines 2022, 9, 6. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Marin, E.; Lanzutti, A. Biomedical Applications of Titanium Alloys: A Comprehensive Review. Materials 2024, 17, 114. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Feldman, A.; Assad, M.; Davies, M.B.; Mangwani, J.; Alabort, E.; Tuncer, M. Cortico-cancellous osseointegration into additively manufactured titanium implants using a load-bearing femoral ovine model. Front. Bioeng. Biotechnol. 2024, 12, 1371693. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Hou, C.; An, J.; Zhao, D.; Ma, X.; Zhang, W.; Zhao, W.; Wu, M.; Zhang, Z.; Yuan, F. Surface Modification Techniques to Produce Micro/Nano-scale Topographies on Ti-Based Implant Surfaces for Improved Osseointegration. Front. Bioeng. Biotechnol. 2022, 10, 835008. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Sheng, X.; Wang, A.; Wang, Z.; Liu, H.; Wang, J.; Li, C. Advanced Surface Modification for 3D-Printed Titanium Alloy Implant Interface Functionalization. Front. Bioeng. Biotechnol. 2022, 10, 850110. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Cui, Y.-W.; Wang, L.; Zhang, L.-C. Towards load-bearing biomedical titanium-based alloys: From essential requirements to future developments. Prog. Mater. Sci. 2024, 144, 101277. [Google Scholar] [CrossRef] [Scilit]
- Singh, A.K.; Khanal, N.; Chaulagain, R.; Sharma, N.; Thieringer, F.M. Is the Pre-Shaping of an Orbital Implant on a Patient-Specific 3D-Printed Model Advantageous Compared to Conventional Free-Hand Shaping? A Systematic Review and Meta-Analysis. J. Clin. Med. 2023, 12, 3426. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- D’Alpaos, D.; Badiali, G.; Ceccariglia, F.; Tarsitano, A. Delayed Orbital Floor Reconstruction Using Mirroring Technique and Patient-Specific Implants: Proof of Concept. J. Pers. Med. 2024, 14, 459. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Kallaverja, E.; Barca, I.; Ferragina, F.; Cristofaro, M.G. Classical Orbital Floor Post-Traumatic Reconstruction vs. Customized Reconstruction with the Support of “In-House” 3D-Printed Models: A Retrospective Study with an Analysis of Volumetric Measurement. Diagnostics 2024, 14, 1248. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Schorn, L.; Wilkat, M.; Lommen, J.; Borelli, M.; Muhammad, S.; Rana, M. Plasma Electrolytic Polished Patient-Specific Orbital Implants in Clinical Use—A Technical Note. J. Pers. Med. 2023, 13, 148. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Matheus, H.R.; Hadad, H.; Guastaldi, F.P.S. The State of 3D Printing of Bioengineered Customized Maxillofacial Bone Scaffolds: A Narrative Review. Front. Oral Maxillofac. Med. 2024, 6, 5. [Google Scholar] [CrossRef] [Scilit]
- Zhu, G.; Wang, G.; Li, J.J. Advances in implant surface modifications to improve osseointegration. Mater. Adv. 2021, 2, 6901–6927. [Google Scholar] [CrossRef] [Scilit]
- Homa, K.; Zakrzewski, W.; Dobrzyński, W.; Piszko, P.J.; Piszko, A.; Matys, J.; Wiglusz, R.J.; Dobrzyński, M. Surface Functionalization of Titanium-Based Implants with a Nanohydroxyapatite Layer and Its Impact on Osteoblasts: A Systematic Review. J. Funct. Biomater. 2024, 15, 45. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Drevet, R.; Fauré, J.; Benhayoune, H. Bioactive Calcium Phosphate Coatings for Bone Implant Applications: A Review. Coatings 2023, 13, 1091. [Google Scholar] [CrossRef] [Scilit]
- Lu, X.; Wu, Z.; Xu, K.; Wang, X.; Wang, S.; Qiu, H.; Li, X.; Chen, J. Multifunctional Coatings of Titanium Implants Toward Promoting Osseointegration and Preventing Infection: Recent Developments. Front. Bioeng. Biotechnol. 2021, 9, 783816. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Akshaya, S.; Rowlo, P.K.; Dukle, A.; Nathanael, A.J. Antibacterial Coatings for Titanium Implants: Recent Trends and Future Perspectives. Antibiotics 2022, 11, 1719. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Zhai, S.; Tian, Y.; Shi, X.; Liu, Y.; You, J.; Yang, Z.; Wu, Y.; Chu, S. Overview of Strategies to Improve the Antibacterial Property of Dental Implants. Front. Bioeng. Biotechnol. 2023, 11, 1267128. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Lv, B.; Wu, J.; Xiong, Y.; Xie, X.; Lin, Z.; Mi, B.; Liu, G. Functionalized Multidimensional Biomaterials for Bone Microenvironment Engineering Applications: Focus on Osteoimmunomodulation. Front. Bioeng. Biotechnol. 2022, 10, 1023231. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ielo, I.; Calabrese, G.; De Luca, G.; Conoci, S. Recent Advances in Hydroxyapatite-Based Biocomposites for Bone Tissue Regeneration in Orthopedics. Int. J. Mol. Sci. 2022, 23, 9721. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Veronesi, F.; Brogini, S.; De Luca, A.; Bellini, D.; Casagranda, V.; Fini, M.; Giavaresi, G. Cell Adhesion and Initial Bone Matrix Deposition on Titanium-Based Implants with Chitosan–Collagen Coatings: An In Vitro Study. Int. J. Mol. Sci. 2023, 24, 4810. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ciulla, M.G.; Massironi, A.; Sugni, M.; Ensign, M.A.; Marzorati, S.; Forouharshad, M. Recent Advances in the Development of Biomimetic Materials. Gels 2023, 9, 833. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Indurkar, A.; Choudhary, R.; Rubenis, K.; Locs, J. Role of Carboxylic Organic Molecules in Interfibrillar Collagen Mineralization. Front. Bioeng. Biotechnol. 2023, 11, 1150037. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Mehta, A.; Singh, G. Consequences of hydroxyapatite doping using plasma spray to implant biomaterials. J. Electrochem. Sci. Eng. 2023, 13, 5–23. [Google Scholar] [CrossRef] [Scilit]
- Kadyroldina, A.; Alontseva, D.; Voinarovych, S.; Łatka, L.; Kyslytsia, O.; Azamatov, B.; Khozhanov, A.; Prokhorenkova, N.; Zhilkashinova, A.; Burburska, S. Microplasma Spraying of Hydroxyapatite Coatings on Additive Manufacturing Titanium Implants with Trabecular Structures. Mater. Sci.-Pol. 2022, 40, 28–42. [Google Scholar] [CrossRef] [Scilit]
- Nayak, G.S.; Carradò, A.; Masson, P.; Pourroy, G.; Mouillard, F.; Migonney, V.; Falentin-Daudre, C.; Pereira, C.; Palkowski, H. Trends in Metal-Based Composite Biomaterials for Hard Tissue Applications. J. Miner. Met. Mater. Soc. 2022, 74, 102–125. [Google Scholar] [CrossRef] [Scilit]
- Cestari, F.; Agostinacchio, F.; Galotta, A.; Chemello, G.; Motta, A.; Sglavo, V.M. Nano-Hydroxyapatite Derived from Biogenic and Bioinspired Calcium Carbonates: Synthesis and In Vitro Bioactivity. Nanomaterials 2021, 11, 264. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Radulescu, D.-E.; Vasile, O.R.; Andronescu, E.; Ficai, A. Latest Research of Doped Hydroxyapatite for Bone Tissue Engineering. Int. J. Mol. Sci. 2023, 24, 13157. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Galli, C.; Landi, E.; Belletti, S.; Colangelo, M.T.; Guizzardi, S. New Sintered Porous Scaffolds of Mg, Sr Co-Substituted Hydroxyapatite Support Growth and Differentiation of Primary Human Osteoblasts In Vitro. Appl. Sci. 2021, 11, 9723. [Google Scholar] [CrossRef] [Scilit]
- Yoleva, A.; Mihailova, I.; Djambazov, S. Solid-state synthesis of hydroxyapatite from black sea Rapana venosa shells. J. Chem. Technol. Metall. 2023, 58, 385–393. [Google Scholar] [CrossRef] [Scilit]
- Azarian, M.H.; Sutapun, W. Biogenic Calcium Carbonate Derived from Waste Shells for Advanced Material Applications: A Review. Front. Mater. 2022, 9, 1024977. [Google Scholar] [CrossRef] [Scilit]
- Fernández-Penas, R.; Verdugo-Escamilla, C.; Triunfo, C.; Gärtner, S.; D’Urso, A.; Oltolina, F.; Follenzi, A.; Maoloni, G.; Cölfen, H.; Falini, G.; et al. A Sustainable One-Pot Method to Transform Seashell Waste Calcium Carbonate to Osteoinductive Hydroxyapatite Micro-Nanoparticles. J. Mater. Chem. B 2023, 11, 7766–7777. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Duta, L.; Dorcioman, G.; Grumezescu, V. A Review on Biphasic Calcium Phosphate Materials Derived from Fish Discards. Nanomaterials 2021, 11, 2856. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Al-Rawe, R.A.; AL-Rammahi, H.M.; Cahyanto, A.; Ma’amor, A.; Liew, Y.M.; Sukumaran, P.; Wan Hassan, W.N. Cuttlefish-Bone-Derived Biomaterials in Regenerative Medicine, Dentistry, and Tissue Engineering: A Systematic Review. J. Funct. Biomater. 2024, 15, 219. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Muntean, F.L.; Olariu, I.; Marian, D.; Olariu, T.; Petrescu, E.L.; Olariu, T.; Drăghici, G.A. Hydroxyapatite from Mollusk Shells: Characteristics, Production, and Potential Applications in Dentistry. Dent. J. 2024, 12, 409. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Cursaru, L.M.; Iota, M.; Piticescu, R.M.; Tarnita, D.; Savu, S.V.; Savu, I.D.; Dumitrescu, G.; Popescu, D.; Hertzog, R.-G.; Calin, M. Hydroxyapatite from Natural Sources for Medical Applications. Materials 2022, 15, 5091. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Dağtekin, M. The Invasive Mollusk Rapana venosa (Mollusca: Neogastropoda: Muricidae) in the Mid-Southern Black Sea: Distribution, Growth, and Stock Structure. Acta Ichthyol. Piscat. 2023, 53, 191–199. [Google Scholar] [CrossRef] [Scilit]
- Montoya, C.; Du, Y.; Gianforcaro, A.L.; Orrego, S.; Yang, M.; Lelkes, P.I. On the road to smart biomaterials for bone research: Definitions, concepts, advances, and outlook. Bone Res. 2021, 9, 12. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Yan, M.; Awad, H.A. Optimizing Rheological Properties for Printability: Low-Temperature Extrusion 3D Printing of Hydroxyapatite-Polycaprolactone Mixture Inks for Bone Tissue Engineering. Front. Mater. 2023, 10, 1239692. [Google Scholar] [CrossRef] [Scilit]
- Khalaf, A.T.; Wei, Y.; Wan, J.; Zhu, J.; Peng, Y.; Abdul Kadir, S.Y.; Zainol, J.; Oglah, Z.; Cheng, L.; Shi, Z. Bone Tissue Engineering through 3D Bioprinting of Bioceramic Scaffolds: A Review and Update. Life 2022, 12, 903. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Peng, W.; Liu, Y.; Wang, C. Definition, Measurement, and Function of Pore Structure Dimensions of Bioengineered Porous Bone Tissue Materials Based on Additive Manufacturing: A Review. Front. Bioeng. Biotechnol. 2023, 10, 1081548. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Toosi, S.; Javid-Naderi, M.J.; Tamayol, A.; Ebrahimzadeh, M.H.; Yaghoubian, S.; Mousavi Shaegh, S.A. Additively Manufactured Porous Scaffolds by Design for Treatment of Bone Defects. Front. Bioeng. Biotechnol. 2024, 11, 1252636. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Koushik, T.M.; Miller, C.M.; Antunes, E. Bone Tissue Engineering Scaffolds: Function of Multi-Material Hierarchically Structured Scaffolds. Adv. Healthc. Mater. 2023, 12, 2202766. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Belgin Paul, D.L.; Praveen, A.S.; Čepová, L.; Elangovan, M. Rheological Behavior and Printability Study of Tri-Calcium Phosphate Ceramic Inks for Direct Ink Writing Method. Polymers 2023, 15, 1433. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Zhao, X.; Li, L.; Zhang, Y.; Liu, Z.; Xing, H.; Gu, Z. 3D Printing and Property of Biomimetic Hydroxyapatite Scaffold. Biomimetics 2024, 9, 714. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Szterner, P.; Antosik, A.; Pagacz, J.; Tymowicz-Grzyb, P. Morphology Control of Hydroxyapatite as a Potential Reinforcement for Orthopedic Biomaterials: The Hydrothermal Process. Crystals 2023, 13, 793. [Google Scholar] [CrossRef] [Scilit]
- Zhang, G.; Zhen, A.; Chen, J.; Du, B.; Luo, F.; Li, J.; Tan, H. In Vitro Effects of Waterborne Polyurethane 3D Scaffolds Containing Poly(lactic-co-glycolic acid)s of Different Lactic Acid/Glycolic Acid Ratios on the Inflammatory Response. Polymers 2023, 15, 1786. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- ISO 10993-12:2021; Biological Evaluation of Medical Devices—Part 12: Sample Preparation and Reference Materials. International Organization for Standardization: Geneva, Switzerland, 2021.
- Kovrlija, I.; Menshikh, K.; Abreu, H.; Cochis, A.; Rimondini, L.; Marsan, O.; Rey, C.; Combes, C.; Locs, J.; Loca, D. Challenging Applicability of ISO 10993-5 for Calcium Phosphate Biomaterials Evaluation: Towards More Accurate In Vitro Cytotoxicity Assessment. Biomater. Adv. 2024, 160, 213866. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ku, J.-K.; Kim, I.-h.; Shim, J.H.; Kim, Y.h.; Kim, B.H.; Kim, Y.-K.; Yun, P.-Y. The Effect of Whitlockite as an Osteoconductive Synthetic Bone Substitute Material in Animal Bony Defect Model. Materials 2022, 15, 1921. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Vladova, D.; Sbirkov, Y.; Stoyanova, E.; Chaprazov, T.; Dimitrov, K.K.; Hristov, H.; Kostov, D.; Veleva, P.; Stoeva, D.; Sarafian, V. Osteogenic Potential of 3D Bioprinted Collagen Scaffolds Enriched with Bone Marrow Stromal Cells, BMP-2, and Hydroxyapatite in a Rabbit Calvarial Defect Model. J. Funct. Biomater. 2026, 17, 68. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Sharma, A.R.; Lee, Y.-H.; Gankhuyag, B.; Chakraborty, C.; Lee, S.-S. Effect of Alumina Particles on the Osteogenic Ability of Osteoblasts. J. Funct. Biomater. 2022, 13, 105. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Wang, J.; Chen, T.; Gao, F. Mechanism and Application Prospect of Ferroptosis Inhibitors in Improving Osteoporosis. Front. Endocrinol. 2024, 15, 1492610. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- You, J.; Zhang, Y.; Zhou, Y. Strontium Functionalized in Biomaterials for Bone Tissue Engineering: A Prominent Role in Osteoimmunomodulation. Front. Bioeng. Biotechnol. 2022, 10, 928799. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Tsai, S.-W.; Hsu, Y.-W.; Pan, W.-L.; Vadivelmurugan, A.; Hwang, P.-A.; Hsu, F.-Y. Influence of the Components and Orientation of Hydroxyapatite Fibrous Substrates on Osteoblast Behavior. J. Funct. Biomater. 2022, 13, 168. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Tsuchiyama, N.; Tamura, Y.; Gondo, T.; Ikeda, M.; Shimada, Y. The Effect of Ions Used in Bioactive Dental Materials on Proliferation and Differentiation of MC3T3-E1 Cells. Asian Pac. J. Dent. 2023, 23, 15–19. [Google Scholar] [CrossRef] [Scilit]
- Nie, X.; Zhang, X.; Lei, B.; Shi, Y.; Yang, J. Regulation of Magnesium Matrix Composites Materials on Bone Immune Microenvironment and Osteogenic Mechanism. Front. Bioeng. Biotechnol. 2022, 10, 842706. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Iqbal, M.Z.; Riaz, M.; Biedermann, T.; Klar, A.S. Breathing new life into tissue engineering: Exploring cutting-edge vascularization strategies for skin substitutes. Angiogenesis 2024, 27, 587–621. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Nejedlá, Z.; Poustka, D.; Herma, R.; Liegertová, M.; Štofik, M.; Smejkal, J.; Šícha, V.; Kaule, P.; Malý, J. Class II biocompatible E-Shell 300 3D printing material causes severe developmental toxicity in Danio rerio embryos and reduced cell proliferation in vitro—Implications for 3D printed microfluidics. RSC Adv. 2021, 11, 16252–16267. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Rengarajan, V.; Clyde, A.; Pontsler, J.; Valiente, J.; Peel, A.; Huang, Y. Assessing Leachable Cytotoxicity of 3D-Printed Polymers and Facile Detoxification Methods. 3D Print. Addit. Manuf. 2023, 10, 1110–1121. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Vasile, V.A.; Pirvulescu, R.A.; Iancu, R.C.; Garhöfer, G.; Schmetterer, L.; Ghita, A.M.; Ionescu, D.; Istrate, S.; Piticescu, R.M.; Cursaru, L.M.; et al. Titanium Implants Coated with Hydroxyapatite Used in Orbital Wall Reconstruction—A Literature Review. Materials 2024, 17, 1676. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- ISO 10993-5:2009; Biological Evaluation of Medical Devices—Part 5: Tests for In Vitro Cytotoxicity. International Organization for Standardization: Geneva, Switzerland, 2009.
- Brum, I.d.S.; Frigo, L.; Ribeiro da Silva, J.F.; Ciambarella, B.T.; Nascimento, A.L.R.; Pereira, M.J.d.S.; Elias, C.N.; de Carvalho, J.J. Comparison Between Nano-Hydroxyapatite/Beta-Tricalcium Phosphate Composite and Autogenous Bone Graft in Bone Regeneration Applications: Biochemical Mechanisms and Morphological Analysis. Int. J. Mol. Sci. 2025, 26, 52. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Lv, N.; Zhou, Z.; Hou, M.; Hong, L.; Li, H.; Qian, Z.; Gao, X.; Liu, M. Research Progress of Vascularization Strategies of Tissue-Engineered Bone. Front. Bioeng. Biotechnol. 2024, 11, 1291969. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Jang, H.-J.; Yoon, J.-K. The Role of Vasculature and Angiogenic Strategies in Bone Regeneration. Biomimetics 2024, 9, 75. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Steiner, D.; Reinhardt, L.; Fischer, L.; Popp, V.; Körner, C.; Geppert, C.I.; Bäuerle, T.; Horch, R.E.; Arkudas, A. Impact of Endothelial Progenitor Cells in the Vascularization of Osteogenic Scaffolds. Cells 2022, 11, 926. [Google Scholar] [CrossRef] [Scilit] [PubMed]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.