Skip to Content
ProcessesProcesses
  • Article
  • Open Access

24 November 2026

15 Pages

Synthesis and Characterization of Cross-Linked Cardo Polymer-Based Anion Exchange Membranes via Two Different Synthetic Routes

,
,
,
,
and
1
Department of Chemistry, Hannam University, Yuseong-gu, Daejeon 34054, Republic of Korea
2
Department of Cosmetic Science, Hannam University, Daedeok-gu, Daejeon 34430, Republic of Korea
3
Center for Gas Analysis, Korea Research Institute of Standards and Science (KRISS), Daejeon 34113, Republic of Korea
*
Authors to whom correspondence should be addressed.

Abstract

Two series of cardo polymer-based anion exchange membranes (AEMs) were prepared through different functionalization and crosslinking routes and evaluated in terms of ion-exchange capacity (IEC), ionic conductivity, water uptake, and dimensional swelling. In the first route, cardo poly(arylene ether ketone sulfone) (PAEKS) was brominated, treated with N,N,N′,N″,N″-pentamethyldiethylenetriamine (PMDETA), and subsequently reacted with iodomethane. In the second route, cardo poly(arylene ether ketone) (PAEK) was brominated, functionalized with 1-vinylimidazole, and subjected to radical crosslinking. The precursor polymers were characterized by 1H NMR, while ATR-IR spectroscopy and thermogravimetric analysis were used to examine the prepared polymers and membranes. The cPAEKS-0.75 membrane exhibited an IEC of 1.51 meq g−1 and ionic conductivity of 5.64 mS cm−1, compared with 1.25 meq g−1 and 2.66 mS cm−1 for cPAEKS-0.5, despite its lower water uptake. The cPAEK(1:5) membrane exhibited an IEC of 2.25 meq g−1, ionic conductivity of 15.00 mS cm−1, water uptake of 8.74%, and swelling ratio of 3.17%. Its swelling ratio was lower than that of the non-crosslinked PAEK-Im(1:5) membrane (7.41%). These results suggest that exchangeable ionic-site concentration and hydration behavior are both relevant to the measured membrane properties. Differences in polymer structure and measurement conditions limit direct quantitative comparisons between the two synthetic routes.

1. Introduction

Fuel cells and redox flow batteries (RFBs) have been widely investigated as electrochemical energy conversion and storage systems [1,2,3,4]. A recent review has summarized advances in anion-exchange membranes for water electrolysis, fuel cells, and redox-flow batteries [5]. In these systems, ion-exchange membranes play an important role in facilitating selective ion transport while limiting the crossover of undesired species [2,6]. Accordingly, membrane properties such as ionic conductivity and dimensional stability are important factors affecting the performance of these electrochemical systems.
Anion exchange membranes (AEMs) contain fixed cationic groups that enable the transport of anionic species and have been investigated for applications in fuel cells and flow batteries [2,3]. Various polymer backbones and cationic functional groups have been introduced to improve their ion-transport properties [7,8,9,10,11]. A recent review has further examined how ether-containing and ether-free polymer backbones and different cationic groups influence AEM design and performance [12]. One common approach to increasing ionic conductivity is to increase the density of ionic groups, which generally results in a higher ion-exchange capacity (IEC). However, an increase in IEC is often accompanied by increased water uptake and membrane swelling, which can adversely affect dimensional stability [8,11]. Therefore, achieving an appropriate balance between ion transport and swelling remains an important consideration in the design of AEMs.
Crosslinking has been widely employed to suppress excessive membrane swelling while maintaining ion-conducting properties. Lai et al. reported AEMs prepared by crosslinking ion-cluster regions and demonstrated an improved balance between ionic conductivity and swelling [8]. More recently, macromolecular crosslinking of poly(arylene piperidinium)-based membranes has been reported as an approach to limiting dimensional swelling while retaining ionic conductivity [13]. Various crosslinked AEMs based on poly(arylene ether sulfone), poly(ether ether ketone), poly(phenylene oxide), and polysulfone structures have also been investigated [10,14,15,16]. Imidazole-functionalized polyethersulfone AEMs with multiquaternary side chains have also been investigated [17]. In addition, the distribution and organization of ionic groups within a polymer can influence ion transport. Membranes with defined ionic domains or ion-conducting pathways have shown improved conductivity while controlling membrane swelling [9,18]. These results indicate that both ionic-group incorporation and crosslinked polymer structure are important factors in determining AEM properties.
Cardo-containing poly(arylene ether ketone) backbones have previously been investigated for AEMs. Yun et al. developed derivatized cardo-polyetherketone AEMs for all-vanadium RFBs [7], while piperidinium-functionalized poly(ether ketone-cardo) membranes were reported more recently [19]. In parallel, crosslinking has been investigated as a strategy to suppress excessive swelling in various AEM systems [8,13,14,15,16]. However, the relationships among ionic functionalization, crosslinking chemistry, and membrane properties remain important considerations in the development of cardo polymer-based AEMs. The present study examines two distinct combinations of functionalization and crosslinking chemistry to evaluate the relationships among ion-exchange capacity, ionic conductivity, water uptake, and dimensional swelling within each polymer series. Because the two systems also differ in backbone composition and ionic functional groups, differences in their measured properties cannot be attributed solely to the crosslinking route.
In this study, two cardo polymer-based AEM series were prepared using different functionalization and crosslinking procedures. In the first route, brominated poly(arylene ether ketone sulfone) (PAEKS) was treated with N,N,N′,N″,N″-pentamethyldiethylenetriamine (PMDETA) during membrane casting, followed by iodomethane treatment to quaternize the remaining tertiary amine groups. The effects of PMDETA feed composition were examined using 0.5 and 0.75 equiv. In the second route, brominated poly(arylene ether ketone) (PAEK) was functionalized with 1-vinylimidazole and subsequently subjected to AIBN-initiated radical crosslinking during membrane formation. PAEK membranes prepared with different monomer feed ratios (1:1 and 1:5) were investigated, together with a non-crosslinked PAEK-Im(1:5) reference membrane. The polymers and membranes were characterized by 1H NMR, ATR-IR spectroscopy, and thermogravimetric analysis, while their IEC, ionic conductivity, water uptake, and linear swelling were evaluated. Within both membrane series, higher measured IEC and ionic conductivity were accompanied by lower water uptake, suggesting that total water uptake alone does not determine the measured ionic transport properties. Nevertheless, the results are interpreted within each polymer series, without assuming that differences between the two series establish a causal advantage of either synthetic route.

2. Experimental

2.1. Materials and Characterization

Phenolphthalein, potassium carbonate, 4,4′-difluorobenzophenone, toluene, sulfuric acid, and CDCl3 were purchased from Alfa Aesar (Ward Hill, MA, USA). 4,4′-Sulfonylbis(2-methylphenol), iodomethane, and 1-vinylimidazole were purchased from Sigma-Aldrich (St. Louis, MO, USA). N-bromosuccinimide (NBS), sodium chloride, hydrochloric acid, methanol, ethanol, and chlorobenzene were obtained from Samchun Pure Chemical Co., Ltd. (Pyeongtaek, Republic of Korea). Potassium nitrate was purchased from Kanto Chemical Co., Inc. (Tokyo, Japan). N,N-Dimethylacetamide (DMAc), N-methyl-2-pyrrolidone (NMP), 1,1,2,2-tetrachloroethane (TCE), N,N,N′,N″,N″-pentamethyldiethylenetriamine (PMDETA), 2,2-bis(4-hydroxy-3-methylphenyl)propane, 2,2′-azobis(2-methylpropionitrile) (AIBN), silver nitrate, potassium chloride, and potassium chromate were purchased from Sigma-Aldrich (St. Louis, MO, USA).
1H NMR spectra were recorded using an Inova 600 spectrometer (Varian, Palo Alto, CA, USA). ATR-IR spectra were obtained using a Thermo Scientific instrument (Thermo Fisher Scientific, Waltham, MA, USA). Thermogravimetric analysis was performed using a TGA N-1000 analyzer (SCINCO, Seoul, Republic of Korea), and ionic conductivity was measured using an IM6ex impedance analyzer (ZAHNER-Elektrik, Kronach, Germany).

2.2. Synthesis and Preparation of Cardo Polymer-Based Anion Exchange Membranes

2.2.1. Synthesis of PAEKS and PAEKS-Br

Cardo poly(arylene ether ketone sulfone) (PAEKS) was synthesized by nucleophilic aromatic substitution polymerization. 4,4′-Sulfonylbis(2-methylphenol) (1.1133 g, 0.004 mol), phenolphthalein (5.0933 g, 0.016 mol), 4,4′-difluorobenzophenone (4.364 g, 0.020 mol), and potassium carbonate (8.295 g, 0.060 mol) were placed in a three-neck flask equipped with a mechanical stirrer, condenser, and Dean–Stark trap. DMAc (approximately 70 mL) and toluene (approximately 25 mL) were added, and the reaction mixture was stirred at 145 °C for 4 h under a nitrogen atmosphere. After the removal of toluene, the reaction was continued at 165 °C for 20 h. The resulting polymer was precipitated in 700 mL of 1 M HCl, washed several times with methanol, and dried. The yield of PAEKS was 91.32%.
For bromination, PAEKS was dissolved in 1,1,2,2-tetrachloroethane (TCE) at a concentration of 2% (w/v). N-Bromosuccinimide (NBS, 2.5 equiv.) and 2,2′-azobis(2-methylpropionitrile) (AIBN, 0.2 equiv.) were added relative to the reactive sites of PAEKS. The reaction was carried out at 85 °C for 12–24 h. After completion of the reaction, the solution was cooled, and the product was precipitated and washed with methanol. The brominated polymer, PAEKS-Br, was dried in a vacuum oven at 80 °C. The yield of PAEKS-Br was 80.25%.

2.2.2. Preparation of Crosslinked PAEKS-Based AEMs

PAEKS-Br was dissolved in NMP at 5% (w/v), and PMDETA was added as the crosslinking agent. Two membrane compositions were prepared using 0.5 and 0.75 equiv. of PMDETA relative to the reactive sites of PAEKS-Br. Each polymer solution was cast onto a glass plate and maintained at 80 °C for approximately 24 h to form the crosslinked membranes.
The membranes were subsequently detached from the glass plate using distilled water and immersed in a 0.05 M iodomethane solution in ethanol for 24 h. This treatment was intended to quaternize the remaining tertiary amine groups via the Menshutkin reaction. The resulting membranes were designated as cPAEKS-0.5 and cPAEKS-0.75, according to the amount of PMDETA used during crosslinking. The prepared membranes were stored in 0.1 M sulfuric acid prior to characterization. The synthetic route for the preparation of cPAEKS-0.5 and cPAEKS-0.75 membranes is illustrated in Scheme 1.
Scheme 1. Synthetic route for the preparation of cPAEKS-0.5 and cPAEKS-0.75 membranes.

2.2.3. Synthesis of PAEK and PAEK-Br

Cardo poly(arylene ether ketone) (PAEK) was synthesized by nucleophilic aromatic substitution polymerization. Phenolphthalein (1.5916 g, 0.005 mol), 4,4′-difluorobenzophenone (6.5460 g, 0.030 mol), 2,2-bis(4-hydroxy-3-methylphenyl)propane (6.4085 g, 0.025 mol), and potassium carbonate (20.7307 g, 0.150 mol) were placed in a three-neck flask equipped with a mechanical stirrer, condenser, and Dean–Stark trap. DMAc (100 mL) and toluene (50 mL) were added, and the reaction mixture was stirred at 140 °C for 4 h under a nitrogen atmosphere. After removal of toluene, the polymerization was continued at 170 °C for 20 h. The resulting polymer was precipitated in 1 M HCl, washed at least three times with methanol, and dried in a vacuum oven for 24 h to obtain PAEK(1:5). In this designation, 1:5 corresponds to the molar feed ratio of phenolphthalein to 2,2-bis(4-hydroxy-3-methylphenyl)propane. PAEK(1:1) was synthesized using the same polymerization and purification procedures, with phenolphthalein (4.7748 g, 0.015 mol), 4,4′-difluorobenzophenone (6.5460 g, 0.030 mol), 2,2-bis(4-hydroxy-3-methylphenyl)propane (3.8451 g, 0.015 mol), and potassium carbonate (20.7307 g, 0.150 mol).
For bromination, PAEK was dissolved in chlorobenzene at a concentration of 5% (w/v). N-Bromosuccinimide (NBS, 2.5 equiv.) and AIBN (0.2 equiv.) were added relative to the reactive sites of the polymer. The reaction was carried out at 100 °C for 12 h under nitrogen. After completion of the reaction, the product was precipitated in methanol, washed, and dried in a vacuum oven for 24 h to obtain PAEK-Br.

2.2.4. Preparation of 1-Vinylimidazole-Functionalized and Crosslinked PAEK AEMs

PAEK-Br was dissolved in NMP at 6% (w/v), and 1-vinylimidazole was added at 1.2 equiv. relative to the reactive sites of PAEK-Br. The reaction mixture was stirred at room temperature for 48 h. After completion of the reaction, the polymer was precipitated in distilled water, washed at least three times with methanol, and dried to obtain PAEK-Im.
For membrane preparation, PAEK-Im was dissolved in NMP at 5% (w/v), followed by the addition of AIBN at 0.02 equiv. relative to the reactive sites. The mixture was stirred for 5 min at room temperature and subsequently cast onto a glass plate. Radical crosslinking was carried out at 80 °C for 5 h before complete removal of the solvent. The membrane was then dried under vacuum at 80 °C for at least 12 h. After drying, the membrane was detached from the glass plate using distilled water. The crosslinked membranes were designated as cPAEK(1:1) and cPAEK(1:5) according to the corresponding PAEK compositions. A non-crosslinked PAEK-Im(1:5) membrane was also prepared without the addition of AIBN and used as a reference sample. The preparation conditions and sample designations of the PAEKS- and PAEK-based anion exchange membranes are summarized in Table 1. The synthetic route for the preparation of cPAEK(1:1) and cPAEK(1:5) membranes is illustrated in Scheme 2.
Table 1. Preparation conditions and sample designations of the PAEKS- and PAEK-based anion exchange membranes.
Scheme 2. Synthetic route for the preparation of cPAEK(1:1) and cPAEK(1:5) membranes.

2.3. Structural and Thermal Characterization

1H NMR spectra of PAEKS, PAEKS-Br, PAEK, and PAEK-Br were recorded using an Inova 600 spectrometer (Varian, USA) with CDCl3 as the solvent to examine structural changes associated with bromination.
ATR-IR spectroscopy was used to characterize the chemical structures of the precursor polymers and the corresponding crosslinked membranes. For the PAEKS-based system, PAEKS, PAEKS-Br, PMDETA-crosslinked samples before iodomethane treatment, and the final cPAEKS-0.5 and cPAEKS-0.75 membranes were analyzed. For the PAEK-based system, PAEK-Im(1:5), cPAEK(1:1), and cPAEK(1:5) were examined to evaluate the structural changes associated with functionalization and crosslinking.
Thermogravimetric analysis (TGA) was performed using a TGA N-1000 instrument (SCINCO, Republic of Korea) from ambient temperature to 700 °C under a nitrogen atmosphere at a heating rate of 10 °C/min to evaluate the thermal degradation behavior of the PAEKS- and PAEK-based polymers and membranes.

2.4. Physicochemical and Electrochemical Characterization

2.4.1. Ion-Exchange Capacity

The ion-exchange capacity (IEC) of the membranes was determined by chloride-ion exchange followed by argentometric titration (Mohr method), which has been reported as an established method for characterizing anion exchange membranes [20,21]. For the PAEKS-based membranes, the dried membrane samples were immersed in 2 M NaCl solution for at least 24 h to exchange the membrane counterions with Cl−. The membranes were then washed thoroughly with distilled water and immersed in 2 M KNO3 solution for at least 24 h to release the exchanged Cl− ions into the solution. The resulting solution was titrated with 0.1 N AgNO3 using K2CrO4 as an indicator.
For the PAEK-based membranes, the dried membrane samples were immersed in 2 M KCl solution for at least 48 h, washed thoroughly with distilled water, and subsequently immersed in 2 M KNO3 solution for at least 48 h. The released Cl− ions were titrated with 0.1 N AgNO3 using K2CrO4 as an indicator.
The argentometric method is based on the precipitation reaction between Ag+ and Cl− to form AgCl, with K2CrO4 serving as the endpoint indicator. Unlike acid–base titration, this approach determines IEC from the amount of chloride released during counterion exchange without requiring conversion of the membranes to the hydroxide form. Acid–base titration is also an established method for determining the IEC of AEMs; however, measurements involving hydroxide-form membranes can be affected by the conversion of OH− to carbonate or bicarbonate species upon exposure to atmospheric CO2 [20,21]. Therefore, the IEC values reported in this study represent the chloride-exchangeable capacity measured under the specified experimental conditions and do not independently establish the degree of quaternization or imidazolium functionalization.
The IEC was calculated according to Equation (1):
IEC (meq g−1) = (VAgNO3 × NAgNO3)/Wdry
where VAgNO3 is the volume of AgNO3 solution used for titration (mL), NAgNO3 is its normality (eq L−1), and Wdry is the dry mass of the membrane (g).

2.4.2. Ionic Conductivity

The ionic conductivity of the membranes was determined from the electrical resistance measured by AC impedance spectroscopy using platinum electrodes [2]. For the PAEKS-based membranes, samples stored in 0.1 M sulfuric acid were cut into approximately 1 cm × 4 cm specimens, washed with distilled water, and mounted between the platinum electrodes. The measurement cell containing the membrane was immersed in water during resistance measurement.
For the PAEK-based membranes, the samples were immersed in 1 M sulfuric acid for conditioning with sulfate-containing counterions prior to conductivity measurement. The membranes were then cut into approximately 1 cm × 4 cm specimens and mounted between platinum electrodes for resistance measurement using a four-point probe AC impedance method. A similar four-point probe AC impedance method using platinum-wire electrodes and a Zahner IM6 EX analyzer has been reported previously [22].
The sulfuric acid concentrations represent the membrane-conditioning procedures rather than standardized conductivity measurement conditions. The experiments followed sulfate-based conditioning procedures instead of a NaCl-based protocol. Therefore, the reported values should not be directly compared with conductivity data obtained under chloride-form or other measurement conditions. Differences in conditioning and electrode configurations also limit direct quantitative comparisons between the two membrane series.
Ionic conductivity was calculated according to Equation (2):
σ = L/(R × A) × 103
where σ is the ionic conductivity (mS cm−1), L is the distance between the electrodes (cm), R is the measured membrane resistance (Ω), and A is the cross-sectional area of the membrane (cm2).

2.4.3. Water Uptake and Swelling Ratio

Water uptake was determined from changes in membrane mass, whereas the linear swelling ratio was calculated from changes in membrane length. The membrane samples were dried under vacuum for 24 h, and their dry mass (Wdry) and dry length (Ldry) were measured. The dried samples were subsequently immersed in distilled water for at least 24 h. The immersion was conducted at room temperature for the PAEK-based membranes. After immersion, the wet mass (Wwet) and wet length (Lwet) were measured.
Water uptake and swelling ratio were calculated according to Equations (3) and (4), respectively:
Water uptake (%) = [(Wwet − Wdry)/Wdry] × 100
Swelling ratio (%) = [(Lwet − Ldry)/Ldry] × 100
where Wwet and Wdry represent the wet and dry membrane masses, respectively, and Lwet and Ldry represent the corresponding wet and dry membrane lengths. The reported IEC, ionic conductivity, water uptake, and swelling ratio values were each obtained from a single measurement per membrane sample (n = 1). Accordingly, uncertainties based on replicate measurements are not available.

3. Results and Discussion

3.1. Synthesis and Structural Characterization

The successful bromination of the PAEKS and PAEK backbones was confirmed by 1H NMR spectroscopy. For the PAEKS system, the aromatic proton signals of PAEKS and PAEKS-Br were observed mainly in the range of 7–8 ppm. The methyl proton signal of PAEKS appeared at approximately 2.3 ppm, whereas this signal markedly decreased after bromination and a new signal corresponding to the –CH2Br group appeared at approximately 4.6 ppm. Based on the integrated peak areas, the degree of bromination was estimated to be 86.19%, indicating substantial conversion of the methyl groups to bromomethyl groups.
A similar spectral change was observed for the PAEK system, with aromatic proton signals mainly appearing in the 6–8 ppm region. After bromination, the methyl proton signal near 2.4 ppm, associated with the brominated sites, decreased, while a new signal assigned to –CH2Br appeared at approximately 4.5 ppm. The corresponding peak integration indicated a bromination degree of approximately 99%.
These spectral changes confirm the successful introduction of bromomethyl groups into both cardo polymer backbones, providing reactive sites for the subsequent functionalization and crosslinking reactions. The 1H NMR spectra of PAEKS, PAEKS-Br, PAEK, and PAEK-Br are presented in Figure 1.
Figure 1. 1H NMR spectra of (a) PAEKS, (b) PAEKS-Br, (c) PAEK, and (d) PAEK-Br in CDCl3.

3.2. ATR-IR Characterization

The precursor polymers and prepared membranes were further examined by ATR-IR spectroscopy to evaluate their characteristic absorption bands. The ATR-IR spectra of the PAEKS- and PAEK-based samples are presented in Figure 2. For the PAEKS-based system, characteristic absorption bands corresponding to the polymer backbone were observed at 1770 and 1649 cm−1 for C=O stretching, 1593 and 1498 cm−1 for aromatic C=C stretching, 1239 cm−1 for S=O stretching, and 1085 cm−1 for C–O–C stretching. The C–Br absorption band expected near 609 cm−1 could not be observed because it was outside the measured spectral range of 650–4000 cm−1.
Figure 2. ATR-IR spectra of (A) PAEKS-based samples: (a) PAEKS, (b) PAEKS-Br, (c) PMDETA-crosslinked PAEKS (0.5 equiv., before iodomethane treatment), (d) cPAEKS-0.5, (e) PMDETA-crosslinked PAEKS (0.75 equiv., before iodomethane treatment), and (f) cPAEKS-0.75; and (B) PAEK-based samples: (a) cPAEK(1:1), (b) cPAEK(1:5), and (c) PAEK-Im(1:5).
For the PAEK-based membranes, the aromatic C=C bands were observed at 1491 and 1595 cm−1, while the C–N band associated with the ion-exchange groups appeared at 1118 cm−1. In the non-crosslinked PAEK-Im(1:5) membrane, a band assigned to the vinyl C=C group of 1-vinylimidazole was observed at 1686 cm−1. This band was not observed in the cPAEK(1:1) and cPAEK(1:5) membranes, consistent with the consumption of vinyl groups during the radical reaction. However, the disappearance of this band alone does not conclusively establish the formation of a crosslinked polymer network.
Additional evidence supporting crosslinking in the PAEK-based system was obtained from the solubility and swelling behavior. In the previously conducted solubility test, the crosslinked PAEK-Im membrane remained insoluble in DMSO at 80 °C for 24 h, whereas the non-crosslinked PAEK-Im membrane dissolved under the same conditions (Figure 3). Furthermore, the linear swelling ratio decreased from 7.41% for PAEK-Im(1:5) to 3.17% for cPAEK(1:5) (Table 2), corresponding to a reduction of approximately 57.2%. These results provide complementary evidence consistent with crosslinked network formation. Nevertheless, the crosslink density and the actual degrees of quaternization and imidazolium functionalization were not quantitatively established in this study.
Figure 3. Solubility comparison of (a) crosslinked PAEK-Im and (b) non-crosslinked PAEK-Im membranes after immersion in DMSO at 80 °C for 24 h.
Table 2. Physicochemical and ionic transport properties of the prepared membranes.

3.3. Thermal Properties

The thermal degradation behavior of the PAEKS- and PAEK-based membranes was investigated by TGA, as shown in Figure 4. For the PAEKS-based system, PAEKS exhibited an initial mass loss of approximately 10% over the range of 140–340 °C. PAEKS-Br showed a slightly greater mass loss of approximately 14% between 130 and 355 °C, which may be associated with residual solvent removal and the decomposition of bromomethyl-containing groups. The cPAEKS-0.5 and cPAEKS-0.75 membranes exhibited initial mass losses of approximately 12% and 14%, respectively, over the range of 180–380 °C. These mass losses may involve the decomposition of ionic functional groups and residual bromomethyl-containing species, as well as the removal of residual NMP. The initial mass loss was slightly greater for cPAEKS-0.75 than for cPAEKS-0.5, although the individual contributions of the functional groups and residual species could not be distinguished from the TGA curves alone.
Figure 4. TGA curves of (a) PAEKS, PAEKS-Br, cPAEKS-0.5, and cPAEKS-0.75 and (b) cPAEK(1:1) and cPAEK(1:5).
For the PAEK-based membranes, a small mass loss was observed at approximately 100–200 °C and was attributed to residual moisture and/or NMP. The cPAEK(1:1) membrane exhibited an additional mass loss of approximately 13% in the 250–300 °C region, which was tentatively attributed to the decomposition of residual bromomethyl groups. At higher temperatures, both cPAEK membranes showed progressive degradation, with cPAEK(1:5) exhibiting a greater mass loss than cPAEK(1:1).

3.4. Water Uptake and Swelling Behavior

The physicochemical and ionic transport properties of the prepared membranes are summarized in Table 2.
For the PAEKS-based membranes, cPAEKS-0.5 exhibited a water uptake of 4.77% and a swelling ratio of 0.82%, whereas cPAEKS-0.75 showed lower values of 3.04% and 0.75%, respectively. The higher PMDETA feed was associated with reduced water uptake and linear swelling, suggesting greater restriction of membrane hydration and dimensional expansion. However, the actual crosslink density was not quantitatively determined.
For the PAEK-based system, cPAEK(1:1) and cPAEK(1:5) exhibited water uptake values of 13.74% and 8.74%, respectively, with corresponding swelling ratios of 2.49% and 3.17%. Although cPAEK(1:5) absorbed less water, its linear swelling ratio was slightly higher than that of cPAEK(1:1), indicating that water uptake and dimensional swelling did not follow the same trend. The non-crosslinked PAEK-Im(1:5) membrane exhibited a water uptake of 11.38% and a swelling ratio of 7.41%, compared with a swelling ratio of 3.17% for cPAEK(1:5). This difference is consistent with restricted dimensional expansion following crosslinking.
These observations suggest that membrane hydration and swelling are influenced by polymer composition, ionic functional groups, and crosslinking. Because the PAEKS and PAEK systems differ in these characteristics, their hydration behavior should be interpreted within each polymer series rather than as a direct comparison of the crosslinking methods.

3.5. Ion-Exchange Capacity and Ionic Conductivity

The ion-exchange capacity and ionic conductivity of the prepared membranes are summarized in Table 2. In the PAEKS-based system, the experimental IEC increased from 1.25 meq g−1 for cPAEKS-0.5 to 1.51 meq g−1 for cPAEKS-0.75 as the amount of PMDETA increased. The corresponding ionic conductivity also increased from 2.66 to 5.64 mS cm−1, despite the decrease in water uptake from 4.77% to 3.04%. The higher IEC indicates a greater measured concentration of exchangeable ionic sites, which may contribute to improved ionic transport even with lower overall water uptake. However, the actual degree of quaternization and the crosslink density were not independently quantified.
For the PAEK-based system, cPAEK(1:1) exhibited an IEC of 1.20 meq g−1 and an ionic conductivity of 12.07 mS cm−1, whereas cPAEK(1:5) showed higher values of 2.25 meq g−1 and 15.00 mS cm−1, respectively. The higher IEC of cPAEK(1:5) is consistent with its greater proportion of the monomer bearing the precursor sites for ionic functionalization. Although cPAEK(1:5) exhibited lower water uptake than cPAEK(1:1), its higher measured IEC may provide more exchangeable ionic sites for ion transport. Ionic conductivity depends not only on total water uptake but also on the availability of ionic sites, local hydration, and ion mobility. These factors may explain the observed conductivity differences, although the ionic-domain structure and local ion transport mechanisms were not directly investigated.
The non-crosslinked PAEK-Im(1:5) and crosslinked cPAEK(1:5) membranes exhibited IEC values of 2.17 and 2.25 meq g−1, respectively, with corresponding ionic conductivities of 13.56 and 15.00 mS cm−1. Together with the lower swelling ratio observed for cPAEK(1:5) (Section 3.4), these results indicate that the crosslinked sample exhibited reduced dimensional swelling without a decrease in measured ionic conductivity under the reported conditions.
Because the PAEKS- and PAEK-based membranes differ in backbone composition, ionic-group chemistry, crosslinking route, and membrane conditioning prior to conductivity measurements, their absolute conductivity values should not be interpreted as a direct comparison of the crosslinking methods alone. Overall, the observations suggest that the measured ionic conductivity is influenced by exchangeable ionic-site concentration and hydration behavior, rather than total water uptake alone.

3.6. Chemical Stability and Potential Applications

Chemical stability is an important consideration for the application of AEMs in electrochemical systems. Although the prepared membranes were conditioned in sulfuric acid for conductivity measurements, their long-term stability in acidic and alkaline environments was not evaluated. Quaternary ammonium and imidazolium groups may undergo degradation under alkaline conditions through mechanisms such as nucleophilic substitution, elimination, and ring-related reactions [23]. However, these degradation processes were not directly investigated in the present study.
The prepared membranes may be considered candidates for further evaluation as separators in electrochemical systems, including fuel cells and redox flow batteries. Nevertheless, their practical applicability cannot be established from the present measurements alone. Further evaluation of chemical stability, ion selectivity, and performance under relevant operating conditions is required before recommending these membranes for specific applications.

4. Conclusions

In this study, two cardo polymer-based anion exchange membrane systems were prepared through different functionalization and crosslinking routes. In the PAEKS-based system, brominated PAEKS was treated with PMDETA followed by iodomethane treatment, whereas the PAEK-based system was functionalized with 1-vinylimidazole and subsequently subjected to radical crosslinking. The structural changes associated with bromination and membrane preparation were supported by 1H NMR and ATR-IR analyses. The solubility behavior of the PAEK-based membranes provided additional qualitative evidence consistent with crosslinked network formation, although the actual crosslink density and degrees of ionic functionalization were not quantitatively established.
For the PAEKS-based membranes, increasing the PMDETA feed from 0.5 to 0.75 equiv. was accompanied by an increase in IEC from 1.25 to 1.51 meq g−1 and ionic conductivity from 2.66 to 5.64 mS cm−1, while water uptake decreased from 4.77% to 3.04% and the swelling ratio decreased from 0.82% to 0.75%. These results suggest that the concentration of exchangeable ionic groups may contribute to ionic conductivity even when the overall water uptake is reduced.
For the PAEK-based membranes, cPAEK(1:5) exhibited an IEC of 2.25 meq g−1 and an ionic conductivity of 15.00 mS cm−1, compared with 1.20 meq g−1 and 12.07 mS cm−1 for cPAEK(1:1), despite its lower water uptake. Furthermore, cPAEK(1:5) exhibited a lower swelling ratio (3.17%) than the non-crosslinked PAEK-Im(1:5) membrane (7.41%), without a decrease in measured ionic conductivity. These observations suggest that ionic-group concentration and dimensional swelling are both relevant to membrane performance.
Overall, the results demonstrate differences in measured ionic transport and swelling behavior within each cardo polymer series. However, differences in backbone composition, ionic functional groups, membrane conditioning, and measurement configurations prevent a direct quantitative comparison of the two synthetic routes. In addition, the measurements were not independently replicated, and long-term chemical stability under acidic, alkaline, or electrochemical operating conditions was not evaluated. Therefore, standardized and replicated measurements, together with chemical stability testing, are necessary before the membranes can be recommended for specific electrochemical applications.

Author Contributions

Conceptualization, S.-B.L. and S.-H.C.; methodology, J.-T.K. and S.-H.C.; formal analysis, S.-B.L., H.-Y.Y. and S.-H.O.; data curation, S.-B.L. and H.-Y.Y.; visualization, S.-B.L. and H.-Y.Y.; writing—original draft preparation, S.-B.L.; writing—review and editing, H.-Y.Y., J.-T.K., S.-H.O., J.J. and S.-H.C.; supervision, S.-H.C. All authors have read and agreed to the published version of the manuscript.

Funding

This research was supported by the ANCHOR program through the Daejeon ANCHOR Center, funded by the Ministry of Education (MOE) and the Daejeon Metropolitan City, Republic of Korea (2026-ANCHOR-06-013). This research was also supported by the Nano-Semiconductor Convergence Research Institute of Hannam University.

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Leung, P.; Li, X.; Ponce de León, C.; Berlouis, L.; Low, C.T.J.; Walsh, F.C. Progress in redox flow batteries, remaining challenges and their applications in energy storage. RSC Adv. 2012, 2, 10125–10156. [Google Scholar] [CrossRef] [Scilit]
  2. Varcoe, J.R.; Atanassov, P.; Dekel, D.R.; Herring, A.M.; Hickner, M.A.; Kohl, P.A.; Kucernak, A.R.; Mustain, W.E.; Nijmeijer, K.; Scott, K.; et al. Anion-exchange membranes in electrochemical energy systems. Energy Environ. Sci. 2014, 7, 3135–3191. [Google Scholar] [CrossRef] [Scilit]
  3. Yuan, Z.; Zhang, H.; Li, X. Ion conducting membranes for aqueous flow battery systems. Chem. Commun. 2018, 54, 7570–7588. [Google Scholar] [CrossRef] [Scilit]
  4. Zhang, H.; Shen, P.K. Advances in the high performance polymer electrolyte membranes for fuel cells. Chem. Soc. Rev. 2012, 41, 2382–2394. [Google Scholar] [CrossRef] [Scilit]
  5. Neelima, J.; Singh, R.K. Recent advances in anion-exchange membranes for electrolyzers, fuel cells and redox-flow batteries. J. Mater. Chem. A 2025, 13, 36853–36880. [Google Scholar] [CrossRef] [Scilit]
  6. Li, X.; Zhang, H.; Mai, Z.; Zhang, H.; Vankelecom, I. Ion exchange membranes for vanadium redox flow battery (VRB) applications. Energy Environ. Sci. 2011, 4, 1147–1160. [Google Scholar] [CrossRef] [Scilit]
  7. Yun, S.; Parrondo, J.; Ramani, V. Derivatized cardo-polyetherketone anion exchange membranes for all-vanadium redox flow batteries. J. Mater. Chem. A 2014, 2, 6605–6615. [Google Scholar] [CrossRef] [Scilit]
  8. Lai, A.N.; Guo, D.; Lin, C.X.; Zhang, Q.G.; Zhu, A.M.; Ye, M.L.; Liu, Q.L. Enhanced performance of anion exchange membranes via crosslinking of ion cluster regions for fuel cells. J. Power Sources 2016, 327, 56–66. [Google Scholar] [CrossRef] [Scilit]
  9. Miyanishi, S.; Fukushima, T.; Yamaguchi, T. Synthesis and property of semicrystalline anion exchange membrane with well-defined ion channel structure. Macromolecules 2015, 48, 2576–2584. [Google Scholar] [CrossRef] [Scilit]
  10. Lee, K.H.; Cho, D.H.; Kim, Y.M.; Moon, S.J.; Seong, J.G.; Shin, D.W.; Sohn, J.Y.; Kim, J.F.; Lee, Y.M. Highly conductive and durable poly(arylene ether sulfone) anion exchange membrane with end-group cross-linking. Energy Environ. Sci. 2017, 10, 275–285. [Google Scholar] [CrossRef] [Scilit]
  11. Kim, J.H.; Ryu, S.; Lee, J.Y.; Moon, S.H. Preparation of high-conductivity QPPO (quaternary-aminated poly(2,6-dimethyl-1,4-phenyleneoxide)) membranes by electrical treatment. J. Membr. Sci. 2018, 553, 82–89. [Google Scholar] [CrossRef] [Scilit]
  12. Hameed, A.S.; Munusamy, S.; Gokulapriyan, R.; Yoo, D.J. Comprehensive Review of Anion Exchange Membrane with Ether and Ether-Free Backbone. ACS Appl. Polym. Mater. 2024, 6, 12341–12361. [Google Scholar] [CrossRef] [Scilit]
  13. Wang, X.; Thomas, A.M.; Lammertink, R.G.H. Dimensionally Stable Anion Exchange Membranes Based on Macromolecular-Cross-Linked Poly(arylene piperidinium) for Water Electrolysis. ACS Appl. Mater. Interfaces 2024, 16, 2593–2605. [Google Scholar] [CrossRef] [Scilit]
  14. Xu, S.; Zhang, G.; Zhang, Y.; Zhao, C.; Zhang, L.; Li, M.; Wang, J.; Zhang, N.; Na, H. Cross-linked hydroxide conductive membranes with side chains for direct methanol fuel cell applications. J. Mater. Chem. 2012, 22, 13295–13302. [Google Scholar] [CrossRef] [Scilit]
  15. Zhu, L.; Zimudzi, T.J.; Li, N.; Pan, J.; Lin, B.; Hickner, M.A. Crosslinking of comb-shaped polymer anion exchange membranes via thiol–ene click chemistry. Polym. Chem. 2016, 7, 2464–2475, Correction in Polym. Chem. 2016, 7, 2589–2589. https://doi.org/10.1039/c6py90044e. [Google Scholar] [CrossRef] [Scilit]
  16. Cha, M.S.; Jeong, H.Y.; Shin, H.Y.; Hong, S.H.; Kim, T.H.; Oh, S.G.; Lee, J.Y.; Hong, Y.T. Crosslinked anion exchange membranes with primary diamine-based crosslinkers for vanadium redox flow battery application. J. Power Sources 2017, 363, 78–86. [Google Scholar] [CrossRef] [Scilit]
  17. Li, S.; Du, S.; Xie, N.; Zhang, T.; Xu, Y.; Ning, X.; Chen, P.; Chen, X.; An, Z. Imidazole-Functionalized Multiquaternary Side-Chain Polyethersulfone Anion-Exchange Membrane for Fuel Cell Applications. ACS Appl. Energy Mater. 2022, 5, 10023–10033. [Google Scholar] [CrossRef] [Scilit]
  18. Zhang, X.; Shi, Q.; Chen, P.; Zhou, J.; Li, S.; Xu, H.; Chen, X.; An, Z. Block poly(arylene ether sulfone) copolymers tethering aromatic side-chain quaternary ammonium as anion exchange membranes. Polym. Chem. 2018, 9, 699–711. [Google Scholar] [CrossRef] [Scilit]
  19. Zhang, Z.; Yu, N.; Sun, H.; Liu, R.; Xu, Y.; Yang, J. New anion exchange membranes based on long side-chain piperidinium cation grafted poly(ether ketone-cardo). Eur. Polym. J. 2023, 195, 112212. [Google Scholar] [CrossRef] [Scilit]
  20. Karas, F.; Hnát, J.; Paidar, M.; Schauer, J.; Bouzek, K. Determination of the ion-exchange capacity of anion-selective membranes. Int. J. Hydrog. Energy 2014, 39, 5054–5062. [Google Scholar] [CrossRef] [Scilit]
  21. Hagesteijn, K.F.L.; Jiang, S.; Ladewig, B.P. A review of the synthesis and characterization of anion exchange membranes. J. Mater. Sci. 2018, 53, 11131–11150. [Google Scholar] [CrossRef] [Scilit]
  22. Kim, Y.-S.; Choi, S.-H. Synthesis of an Anion-Exchange Membrane Based on Imidazolium-Type Ionic Liquids for a Capacitive Energy Extraction Donnan Potential Device. J. Chem. 2014, 2014, 858541. [Google Scholar] [CrossRef] [Scilit]
  23. Sun, Z.; Lin, B.; Yan, F. Anion-Exchange Membranes for Alkaline Fuel-Cell Applications: The Effects of Cations. ChemSusChem 2018, 11, 58–70. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.