Abstract
Over the last several years, researchers have noted some drawbacks to the basic Superpave test methods for assessing modified binders. This study compared atomic force microscopy (AFM), sessile drop (SD) surface free energy calculations, and the Texas Boiling Test (TBT) for characterizing binder surfaces and binder–aggregate moisture-related properties. Eighteen asphalt binders (PG 64-22, PG 70-22, and PG 76-22 from six sources) and eight aggregates (sandstone, limestone, dolomite, and novaculite, each from two quarries) were evaluated. The apparent DMT modulus from AFM ranged from 125 MPa (S5B1) to 765 MPa (S2B3). In the TBT, the S4B3–NV2 combination had the highest visually estimated coating retention (90%). The calculated dry work of adhesion ranged from 86.5 mJ/m2 (S2B2–NV1) to 174.5 mJ/m2 (S6B3–LS2). The water-induced debonding energy ranged from 7.9 mJ/m2 (S2B2–LS2) to 55.7 mJ/m2 (S5B1–NV2), where a lower value indicates a smaller driving force for stripping. The AFM images showed differences in bee-like surface morphology among binder sources. The methods ranked the materials differently, and no single binder performed best across all endpoints. Evaluating the three methods together shows which binder properties and binder–aggregate interactions each method can and cannot capture, which supports better-informed material selection and further study of moisture damage.
1. Introduction
Moisture-induced damage is one of the main reasons for pavement failure in the United States (US). This type of damage significantly reduces service life and performance, leading to potholes, rutting, cracking, and raveling. Moisture-induced damage also has financial implications, because the premature loss of pavement integrity can require additional maintenance, rehabilitation, or replacement. For Arkansas, evaluating material compatibility before construction is therefore relevant to managing pavement maintenance expenditure. However, this study does not quantify regional repair costs or estimate the savings associated with particular material combinations. Moisture damage occurs due to the loss of adhesion between the aggregate and binder, and the loss of cohesion within the binder in the presence of water [1,2,3,4,5,6]. Numerous mechanisms explain these moisture damage phenomena, i.e., pH instability, spontaneous emulsification, and hydraulic scouring [7,8,9,10,11,12]. Several techniques [13,14] have been developed to assess moisture damage; however, early research did not consider relevant parameters like adhesion forces at the micro scale or use atomic force microscopy (AFM).
Dynamic shear rheometer (DSR) testing characterizes the bulk viscoelastic response of asphalt binders through the complex shear modulus (G*) and phase angle (δ) at specified temperatures and loading frequencies. The conventional high-temperature Superpave criterion uses G*/sin δ, and multiple stress creep recovery (MSCR) testing evaluates nonrecoverable creep compliance and recovery under repeated loading. These measurements describe binder response to shear loading. AFM provides complementary information on surface morphology and spatial variations in local mechanical response; however, its measurements are not directly interchangeable with bulk rheological parameters [15].
The AFM technique has gained prominence in pavement engineering because it can assess surface characteristics and mechanical attributes of materials at the nano scale. AFM captures intricate nanoscopic details, providing insights into surface morphology and mechanics. By processing the collected data, it becomes possible to discern the surface structure of asphalt binders and ascertain nanomechanical traits like the elastic modulus, adhesion, and dissipated energy. This technology offers a novel avenue for understanding the microscale behavior of asphalt materials. AFM identifies differences in surface topography, pull-off force, and indentation response that are averaged within bulk measurements. The Derjaguin–Muller–Toporov (DMT) model describes elastic contact while accounting for adhesive interactions. In PeakForce QNM, fitting the probe–sample force curve gives a reduced modulus, which can be converted to a sample modulus using the Poisson ratios and the probe properties. The quantitative result depends on the force calibration, tip radius, fitting procedure, and applicability of the model. For a viscoelastic material such as asphalt, temperature and loading timescale also affect the response. Several researchers have used this tool to measure surface topography [16], the structure of asphalt [17], pull-off forces [18], distinct phases of asphalt [19], material properties [20], and moisture damage [21,22]. Loeber et al. (1996) studied the AFM microstructures caused by aging and modification of asphalt binders [17]. Furthermore, he studied the application of several modes of AFM to characterize asphalt binders and explored the relationship between asphalt binders’ nano-morphology and different macro-level tests. Tarefder and Zaman [21] explored the application of AFM and nanoindentation techniques to assess the moisture damage performance of asphalt materials at the nano scale. They conducted experiments under wet and dry conditions using AFM-based adhesion values. Results indicated higher adhesion force values in wet samples than dry ones, suggesting moisture-induced damage in the asphalt film, resulting in a rougher surface. Bhasin [20] investigated the adhesion in dry and wet conditions to evaluate the moisture sensitivity of asphalt binders. This researcher employed a universal sorption device and the Wilhelmy plate technique to measure surface free energy. The surface free energy-related thermodynamic parameters were found to be useful for quantifying the debonding of asphalt binder and aggregate in the presence of moisture.
On the other hand, the Texas Boiling Test (TBT) is a fundamental method for assessing the susceptibility of asphalt mixtures to moisture-induced damage. It offers valuable insights into pavement performance and longevity. Originating from the Texas Transportation Institute (TTI), this test provides a standardized approach to evaluating moisture damage potential in asphalt materials. A comprehensive body of literature has explored the efficacy of the Texas Boiling Test in predicting moisture-induced distresses in asphalt pavements. Kim et al. (2015) conducted a seminal study [23] to investigate the correlation between TBT results and the field performance of asphalt mixtures. Their findings underscored the test’s capability to identify moisture-sensitive materials, thus informing pavement design and material selection strategies to mitigate potential damage. Moreover, researchers have endeavored to refine the testing protocols and parameters of the Texas Boiling Test to enhance its accuracy and reliability. Ahmad et al. (2018) proposed modifications [24] to the TBT procedure, including adjustment of the test temperature and duration, to better simulate the real-world moisture conditions experienced by asphalt pavements. Their contributions have advanced the understanding of moisture damage mechanisms and improved the predictive capabilities of the test. In addition, studies have explored the relationship between TBT outcomes and other key performance indicators for asphalt pavements. Chen et al. (2020) investigated the correlation between moisture susceptibility [25], as determined by the Texas Boiling Test, and rutting resistance in asphalt mixtures. Their research revealed significant associations between moisture-induced distresses and pavement rutting, highlighting the predictive value of the TBT in assessing long-term pavement performance.
The sessile drop (SD) method is widely employed for accurately measuring contact angles (CAs) between aggregate/asphalt and reference liquids. This method is known for its convenience and has been extensively used by researchers to obtain the CAs of asphalt and aggregate samples [26]. In this study, the SD technique was used to measure the CAs of virgin and modified binder samples. Additionally, it was used to build a surface free energy (SFE) database for various binder types [27]. The SD method has also been found useful for obtaining CAs of aggregate samples. However, differences in the magnitude of SFE components between the SD method and other popular methods for aggregate samples have also been noted. In the context of asphalt mixes, cohesion energy is used to assess the energy needed for microcracks to develop in a binder [28]. The work of adhesion refers to the effort required to separate two dissimilar materials (asphalt binder and aggregate) at their interface in a vacuum. The dry work of adhesion measures the bond strength between asphalt binder and aggregate under normal conditions, with no water at the interface. On the other hand, the wet work of adhesion test measures the bond strength between the binder and aggregate when water penetrates the interface, simulating moisture intrusion in the pavement. Higher dry separation work indicates greater reversible energy required to separate the interface. Water-induced debonding energy is reported here as the positive quantity −ΔGwet, where larger values indicate a stronger thermodynamic driving force for stripping. Adhesive bond energy between asphalt binder and aggregate without water is known as dry work of adhesion. A higher dry adhesion energy value indicates a more durable mixture [20]. Nonetheless, the adhesive’s energy at the aggregate–binder interface drops in wet conditions, making the stripping process thermodynamically advantageous. Therefore, a lower magnitude of the water-induced debonding energy indicates a smaller thermodynamic driving force for stripping [20].
Earlier work has connected surface energy parameters to asphalt–aggregate moisture susceptibility and looked at how specific binder–aggregate pairs perform together [29]. However, a binder’s own surface mechanics and how well it actually bonds with a particular aggregate are different. AFM pull-off force only reflects how the binder responds to a single probe, and it does not directly discuss the aggregate. Surface free energy calculations consider both materials, and the TBT captures how much coating survives boiling water exposure. Whether a binder with favorable AFM characteristics also performs well with an aggregate in interfacial energy and coating retention terms has not been explored yet. This question must be resolved before binder-only measurements can be used to guide aggregate-specific material selection.
This study answers this question by comparing AFM morphology and local mechanical response across 18 commercial binders (three PGs from six sources) against sessile drop interfacial energies and TBT coating retention with eight aggregates (four aggregate types from two quarries each). It builds on the aggregate–binder compatibility work of Oyan et al. [29]. However, rather than proposing a new test, it evaluates how well rankings from one method perform against those from another. The results show whether AFM finds any additional binder properties, i.e., binder morphology and mechanical response. AFM also shows where binder surface data alone are not enough to predict how a binder will actually behave with a given aggregate under moisture. These cross-method patterns are exploratory and not validated predictors of field performance.
2. Materials and Methods
2.1. Asphalt Binders
Table 1 provides the nomenclature for the three distinct types of PG binders approved by the Arkansas Department of Transportation (ARDOT), Little Rock, Arkansas, USA, that were tested in this study. Each type of PG binder was obtained from six different sources, resulting in a total of 18 binder samples directly from refinery facilities. According to supplier information, sources S1–S4 used Canadian crude (“sour”, containing over 0.5% sulfur) and sources S5–S6 used Arabian crude (“sweet”, containing less than 0.5% sulfur). These binders were prepared in commercial laboratories and marketed by ARDOT-approved suppliers located in Tennessee, Texas, Oklahoma, Missouri, and Louisiana all in the USA. PG 64-22 is the base binder, termed B1, and the other two polymer-modified binders are PG 70-22 and PG 76-22, termed B2 and B3.
Table 1.
Designations of asphalt binders tested in this study.
The material matrix includes three PGs from each of the six commercial sources. Source comparisons are therefore interpreted within PG where possible, and source averages pooled across grades are descriptive summaries only. Comparisons between B1 and B2 or B3 combine differences in PG and modification status. They do not isolate polymer modification as a cause.
2.2. Aggregates
Table 2 lists the nomenclature assigned to the eight distinct aggregate samples that were collected and used for testing within the scope of this investigation. The aggregates tested are of four primary types: sandstone, novaculite, limestone, and dolomite, with each type originating from two distinct sources. As a result, a total of eight aggregate samples were acquired for laboratory evaluation. All aggregate quarries are located in different parts (northeast, northwest, west, and central) of Arkansas. Specific gravity and absorption were determined according to AASHTO T 85 on three specimens per aggregate. Abrasion loss was determined according to AASHTO T 96, and pH was measured on an aggregate–water mixture. All aggregates were basic (pH > 8) and met the 40% abrasion loss limit of ARDOT. SS1 was the only aggregate with absorption above 2% (3.72%). The TBT used particles passing the 3/8 in. sieve and retained on the No. 4 sieve. Surface energy components are reported separately in Section 2.3.3. Detailed mineralogical composition was not measured and is not used to explain differences among aggregates.
Table 2.
Designations of aggregates used in this study.
2.3. Laboratory Tests
2.3.1. Atomic Force Microscopy (AFM) Test
Within the framework of this study, AFM was employed to examine both surface roughness/morphology and mechanical properties. These properties are adhesion force, deformation, dissipated energy, and the Derjaguin–Muller–Toporov (DMT) modulus. The AFM system is depicted in Figure 1.
Figure 1.
AFM system used in this study.
The PeakForce Quantitative Nanomechanical Mapping (PFQNM™) mode was selected. It can generate maps illustrating the binder’s morphology and mechanical characteristics at the micro level. Similar to tapping mode, peak force tapping provides information regarding surface roughness and the force–displacement curve of individual points within the area scanned. These data are subsequently analyzed through quantitative nanomechanical mapping to ascertain the properties of the scanned surface.
AFM measurements were performed with a Bruker Dimension Icon in PeakForce QNM mode in air, with ScanAsyst autocontrol enabled. Each field measured 10 × 10 µm2 at 512 samples/line, with a scan rate of approximately 0.5 Hz. PeakForce tapping used a frequency of 2 kHz, an amplitude of 150 nm, and a peak force setpoint of 203.4 nN. The probe had a spring constant of 40.19 N/m, a tip radius of 74.9 nm, and a half angle of 18°. Images were processed offline using NanoScope software (version 9.0).
The heat-casting method was utilized to prepare specimens for AFM testing from the selected binder samples. This heat-casting method is a protocol widely utilized in asphalt binder characterization by various researchers [2,21,29,30]. The procedural steps involved in specimen preparation for AFM testing are outlined as follows:
- The asphalt binder sample was heated in an oven at 160 °C until it was flowable enough for pouring.
- A small quantity of asphalt binder, typically two drops, was dispensed onto a thin glass plate measuring 2″ by 3″.
- Subsequently, the binder-coated glass plates were placed in the oven for approximately 15 min to achieve a consistent and smoother surface. For stiffer binders, such as the higher-grade binders, the heating duration was extended until the desired consistency was attained.
- Afterward, the specimens were cooled at room temperature for half an hour and then kept in a desiccator under humidity control for 24 h before the test. The samples were kept in a desiccator for three and seven days at room temperature.
- AFM tests were performed using the prepared asphalt binder specimens.
- The NanoScope (Version 9.0) tool was used to examine the PFQNM-scanned maps to measure asphalt binders’ nanomechanical properties and surface roughness.
The three- and seven-day periods describe post-preparation storage; they are not standardized short-term or long-term aging treatments.
2.3.2. Texas Boiling Test
The Texas Boiling Test (TBT) was conducted according to ASTM D3625 to evaluate the stripping potential of each binder–aggregate combination. Oven-dried aggregate (100 g) passing the 3/8 in. sieve and retained on the No. 4 sieve was heated at 163 °C for at least 30 min. The binder was heated to the same temperature, and 5 g of binder was poured onto the heated aggregate and mixed by hand. The coated aggregate was cooled to room temperature, and the particles were separated from one another (Figure 2a,b). Distilled water (500 mL) was brought to 100 °C in a 1000 mL beaker, and the loose mixture was added (Figure 2c). The mixture was boiled for 10 min and stirred with a glass rod three times at 3 min intervals. Stripped binder was skimmed from the water surface during boiling to prevent recoating. After boiling, the water was decanted, and the aggregate was spread on aluminum foil and allowed to dry and cool to room temperature for 30 min (Figure 2d). One loose mixture was prepared and boiled for each of the 144 binder–aggregate combinations. Three observers independently rated the dried aggregate using the rating board developed by the Texas Transportation Institute (TTI) (Figure 3) [13], and the mean of the three ratings is reported. The TBT endpoint is the visually estimated percentage of aggregate surface retaining asphalt coating; it is not a measurement of retained binder mass. Because each combination was boiled once, the three ratings capture observer variability only. They do not capture variability between independent boiling runs.
Figure 2.
Texas Boiling Test: (a) prepared asphalt mixture, (b) segregated coated aggregates, (c) boiling the sample, and (d) air-drying after boiling.
Figure 3.
TBT image rating.
2.3.3. Sessile Drop Test
Surface free energy (SFE) tests were carried out on the asphalt binders and aggregate samples following the authors’ previous work [29]. Static contact angles (θ) were measured with an optical contact angle analyzer using three reference liquids: water, ethylene glycol, and formamide. The drop volume was 3 µL for binders and 5 µL for aggregates. For each liquid, contact angles were recorded at no fewer than three locations on each sample surface, with more than 100 readings per location over 30 s, and the average of all readings represented the sample [31].
The SFE components were calculated using the Good–van Oss–Chaudhury theory and the Young–Dupré equation [29]:
where L and S denote the liquid (reference solvent) and the solid (binder or aggregate), and ΓLW, Γ+, and Γ− are the Lifshitz–van der Waals, acid, and base components. Solving Equation (1) for the three reference liquids gives the components of each binder and aggregate sample. The work of adhesion is reported as a positive value. For water displacing the binder from the aggregate surface, the free energy change is
where subscripts 1, 2, and 3 denote the binder, the aggregate, and water, respectively. Under this definition, a more negative ΔGwet indicates a stronger thermodynamic driving force for water displacement. In this paper, the water-induced debonding energy is reported as the positive value −ΔGwet, so larger values indicate a stronger driving force for stripping. These quantities are calculated thermodynamic values; they are not direct measurements of mechanical work or mixture performance.
3. Results
3.1. AFM Test Results
In the tested asphalt binder samples, three distinct phases were identified: dispersed (Catana), interstitial (Peri), and matrix (Perpetua), as illustrated in Figure 4. Bee-like structures are elongated surface features with alternating raised and depressed bands in the AFM height maps. The patterned region is termed the Catana phase, the region surrounding it is the Peri phase, and the comparatively smooth region is the Perpetua phase.
Figure 4.
Three distinct phases of asphalt binders from the AFM height sensor map.
Figure 5, Figure 6, Figure 7, Figure 8, Figure 9 and Figure 10 display the surface roughness (morphology) of B1, B2, and B3 binder samples from different sources after three and seven days of storage. The AFM images show differences in the bee-like surface morphology among binder sources. The highest counts of bee structures were observed in sources S1, S2, and S3 and the lowest for source S4. These observations characterize the surfaces produced by the preparation protocol used; they do not independently establish differences in molecular mobility or moisture resistance.
Figure 5.
Height sensor maps of B1 binders after three days: (a) S1B1, (b) S2B1, (c) S3B1, (d) S4B1, (e) S5B1, and (f) S6B1.
Figure 6.
Height sensor maps of B1 binders after seven days: (a) S1B1, (b) S2B1, (c) S3B1, (d) S4B1, (e) S5B1, and (f) S6B1.
Figure 7.
Height sensor maps of B2 binders after three days: (a) S1B2, (b) S2B2, (c) S3B2, (d) S4B2, (e) S5B2, and (f) S6B2.
Figure 8.
Height sensor maps of B2 binders after seven days: (a) S1B2, (b) S2B2, (c) S3B2, (d) S4B2, (e) S5B2, and (f) S6B2.
Figure 9.
Height sensor maps of B3 binders after three days: (a) S1B3, (b) S2B3, (c) S3B3, (d) S4B3, (e) S5B3, and (f) S6B3.
Figure 10.
Height sensor maps of B3 binders after seven days: (a) S1B3, (b) S2B3, (c) S3B3, (d) S4B3, (e) S5B3, and (f) S6B3.
Figure 5 and Figure 6 show the differences in bee structure counts between the three- and seven-day storage periods. The count decreased by 15%, 11%, 13%, 20%, and 33% for S1B1, S3B1, S4B1, S5B1, and S6B1, respectively, and increased only for S1B2. A low count of “bees” may reflect coalescence of structures rather than their disappearance. Similar patterns can be observed in Figure 7, Figure 8, Figure 9 and Figure 10 for B2 and B3. Whether these morphological changes are associated with changes in local pull-off force requires quantitative analysis; their implications for binder–aggregate moisture resistance cannot be established from morphology alone.
A comparison of the DMT modulus values of different samples is presented in Figure 11. The highest DMT modulus (765 MPa) was recorded for the S2B3 binder, while the S5B1 asphalt binder sample exhibited the smallest DMT modulus of 125 MPa. The DMT modulus values of the tested samples were smaller in the matrix or para phase in contrast to the other two phases. The DMT modulus is improved with the asphalt binder’s PG. On average, the S1-sourced binders had the highest DMT modulus (420 MPa) after three days, but after seven days, S2-sourced binders had the highest average DMT modulus (402 MPa). A higher apparent DMT modulus indicates a stiffer local response to indentation under the AFM conditions used in this study.
Figure 11.
Comparison of DMT modulus of all asphalt binders.
Figure 12 displays the adhesion values of various samples of asphalt binders. S3B1 exhibited the highest reported tip–binder pull-off force under the AFM conditions used. On the other hand, the S5B2 binder had the lowest adhesion force (139 nN). The Catana and the Peri phases exhibited higher adhesion force (ranging from 110 to 670 nN) than the Perpetua phase (ranging from 30 to 300 nN) for all the tested asphalt binder samples. The measured pull-off forces characterize the interaction between the selected AFM probe and the binder surface; they do not directly measure adhesion to the aggregates evaluated in the TBT and SFE analyses. The average adhesion values were higher in S3-sourced asphalt binders. The S3-sourced binders also had higher bee structure counts. The study did not establish bee structure abundance as the cause of the observed differences in pull-off force. AFM pull-off force is relevant to investigating moisture damage because it characterizes local adhesive interactions at the binder surface. Water-induced damage can involve disruption of adhesive interactions at the binder–aggregate interface and changes in cohesion within the binder. Consequently, AFM measurements obtained before and after controlled moisture exposure can help characterize changes in surface interaction associated with moisture conditioning. Previous research has applied wet-to-dry force comparisons using probes with specified surface chemistry to investigate these effects [22]. The apparent DMT modulus and tip–binder pull-off force do not need to produce the same material ranking because they describe different aspects of the probe–sample interaction: the apparent DMT modulus characterizes local indentation response; on the other hand, pull-off force characterizes separation from the selected probe. Neither of these parameters establishes any relation to adhesion of a particular aggregate or retention of that adhesion after moisture exposure.
Figure 12.
Comparison of the adhesion force of all asphalt binders.
The deformation values of the asphalt binder samples are illustrated in Figure 13. The S4B1 binder had the lowest deformation of 0.975 nm, while the S5B1 binder had the highest deformation of 5.15 nm. On average, binders sourced from S3 showed a lower deformation value of 2.07 nm after seven days. The lower deformation values from S3 binders suggest that the asphalt binders can withstand deformation under microscopic loads. Higher-PG binders exhibit lower deformation values due to their increased stiffness from polymer modification. However, in this study, B2 binders displayed the highest average deformation value of 3.32 nm after seven days. As expected, higher adhesion forces and lower deformation were observed for polymer-modified binders at hot temperatures, with PG 76-22 showing more stiffness than PG 64-22. However, at low or room temperatures, the stiffness of these binders may not differ as significantly, as both PGs share the same low-temperature specification.
Figure 13.
Comparison of the deformation of all asphalt binders.
Figure 14 shows the dissipation values of various binder samples. The S5B3 sample had the lowest dissipation value of 47.3 keV among all asphalt binders, while the S1B3 binder had the highest dissipation value of 438.9 keV. The dispersed and interstitial phases had dissipation values of 35.8–427.0 keV, and the matrix phase had a dissipation value of 10.8–160.9 keV. On average, the binders from the S4 source showed the highest dissipation energy values of 310.8 keV and 327.2 keV after three days and seven days, respectively. AFM energy dissipation comes from the hysteresis between the loading and unloading portions of the force–distance curve. Local viscoelastic deformation and adhesive interactions contribute to the energy loss. Dissipation energy adds a measure of local energy loss besides the AFM modulus and pull-off measurements.
Figure 14.
Comparison of the dissipation energy of all asphalt binders.
3.2. Texas Boiling Test Results
The TBT was conducted for all binder–aggregate combinations, and the visually estimated coating retention is presented in Figure 15, Figure 16 and Figure 17. Each reported value is the mean rank of three replicates. The variations in the TBT ranks among replicates are shown as error bars (one standard deviation) in Figure 15. It can be seen that the variation is not significant. Figure 15 shows satisfactory performance of SS2, LS1, DM1, and DM2, demonstrating good asphalt retention percentages. The S3B1–SS2 system exhibited the highest asphalt binder percentage (75%) retained after the boiling. Among all the B1-grade binders, the S6B1 binder showed the highest percentage retained on average (52%). On the other hand, the S1B1 binder showed the lowest average percentage retained after boiling. Figure 16 displays the percentage of asphalt retained for the B2 binders and different aggregate samples. The asphalt binder retained more than 50% after boiling for SS2, LS1, and DM1. Similar to the B1 binders, the S3B2–SS2 system showed the highest asphalt percentage (80%) retained. The S6B2 binder showed the highest average percentage (58%) retained with all the aggregates. Figure 17 reveals a similar trend for the B3 binders as was noticed in Figure 15 for the B1 binder samples. Additionally, every type of aggregate sample displayed excellent asphalt retention percentages exceeding 70% when paired with the S4B3 binder. The S4B3–NV2 system had the highest asphalt binder retention (90%) after the boiling test, representing the highest observed coating retention under the tested boiling conditions. On the other hand, the S1B1–NV2 system had the lowest asphalt binder retention. On average, LS1 aggregates retained 70% of the asphalt binder after the Texas Boiling Test, with the highest retention rate at 85% and the lowest at 50%. LS1 exhibited the highest average coating retention among the aggregates under the tested conditions.
Figure 15.
Texas Boiling Test results for B1 binders.
Figure 16.
Texas Boiling Test results for B2 binders.
Figure 17.
Texas Boiling Test results for B3 binders.
3.3. Sessile Drop Test Data
Figure 18, Figure 19 and Figure 20 show the dry work of adhesion and the water-induced debonding energy for each binder–aggregate combination. The S2B2–NV1 combination had the lowest dry work of adhesion (86.5 mJ/m2), and all binders had their lowest dry work of adhesion with NV1. The S6B3–LS2 combination had the highest (174.5 mJ/m2). The Source 1 sandstone had a higher dry work of adhesion than the Source 2 sandstone, by 8.8 mJ/m2 (7.1%) on average. A higher dry work of adhesion means that more energy is required to separate the interface in the dry state.
Figure 18.
Work of adhesion between the aggregates and B1 binder.
Figure 19.
Work of adhesion between the aggregates and PG B2 binder.
Figure 20.
Work of adhesion between the aggregates and B3 binder.
For novaculite, limestone, and dolomite, the Source 2 aggregates had a higher dry work of adhesion than the Source 1 aggregates, with average increases of 16.5 mJ/m2 (13.3%), 24.9 mJ/m2 (16.2%), and 22.4 mJ/m2 (15.1%), respectively.
Water-induced debonding energy was evaluated separately from dry separation work because the two quantities describe different interfacial processes [26]. Figure 18, Figure 19 and Figure 20 show that the water-induced debonding energy was lowest for S2B2–LS2 (7.9 mJ/m2) and highest for S5B1–NV2 (55.7 mJ/m2). Lower values indicate a weaker thermodynamic driving force for stripping, so S2B2–LS2 had the weakest driving force and S5B1–NV2 the strongest among the evaluated combinations. A stronger bond between asphalt and aggregates with high lime content in the presence of water has also been reported in the literature [30,32]. The aggregate source also affected the results: the Source 2 sandstone, novaculite, and dolomite had higher debonding energies than their Source 1 counterparts, which indicates a greater thermodynamic driving force for water displacement [30,33]. The Source 1 samples had lower water-induced debonding energies than the Source 2 samples by 3.1 mJ/m2 (7.6%) for sandstone, 4.8 mJ/m2 (9.2%) for novaculite, and 10.2 mJ/m2 (24.3%) for dolomite. The differences were small for sandstone and novaculite and larger for dolomite, indicating a weaker thermodynamic driving force for stripping for Source 1 dolomite. For limestone, the Source 2 samples had lower debonding energies than the Source 1 samples by 22.0 mJ/m2 (51.2%) on average, indicating a weaker thermodynamic driving force for stripping for Source 2 limestone.
4. Discussion
The findings of this study offer practical ways to enhance the durability of pavements, particularly in areas affected by moisture. The AFM descriptors ranked the binder sources differently. As reported in Section 3.1, the source-average apparent DMT modulus was highest for S1 after three days of storage (420 MPa) and for S2 after seven days (402 MPa). In contrast, S3 binders showed the highest tip–binder pull-off forces. Local stiffness and the adhesive response are therefore different properties, and these results do not identify a single best-performing source. In the Texas Boiling Test, coating retention was assessed separately for each binder–aggregate combination, so the TBT results are discussed per combination and not by source alone. AFM characterizes the exposed binder surface and its interaction with the selected probe. The SD measurements provide surface energy components, from which the binder–aggregate interfacial quantities are calculated. The TBT evaluates coating retention for each coated aggregate combination. An AFM value is measured on the binder alone, so it cannot identify an aggregate-specific response unless a relationship has been established independently. For this reason, the AFM source rankings are not transferred directly to rankings of binder–aggregate compatibility.
In the AFM test results, after three days of curing, the S1-sourced binders had the highest DMT modulus, indicating they were the stiffest at this point. However, by seven days, the S2-sourced binders showed greater stiffness, with their modulus surpassing that of the other binders. Even though the S2 binders had the highest stiffness after seven days, they did not have the strongest adhesive properties. Instead, the S3-sourced binders showed the highest adhesion force. The study did not establish bee structure abundance as the cause of the observed differences in pull-off force. For this reason, stiffness (as measured by the DMT modulus) and adhesion do not always go hand in hand. Both factors are important when evaluating binder performance, but they can evolve differently over time, depending on the binder’s source and composition.
Regression analyses were performed using the Minitab 21.4.3 statistical software. They were conducted among Texas Boiling Test results, work of adhesion, and AFM adhesion values at three and seven days. Across all 144 binder–aggregate combinations, approximate TBT retention (estimated from the visual rating bins) was positively correlated with the dry work of adhesion (n = 144, r = 0.32, 95% CI 0.16 to 0.46, p = 0.0001). It was negatively correlated with the water-induced debonding energy (n = 144, r = −0.19, 95% CI −0.35 to −0.03, p = 0.019). A higher debonding energy is the larger driving force for stripping, so the negative sign is the expected direction. Both correlations are weak (R2 ≈ 0.10 and 0.04), so SFE parameters explain only a small part of the variation in TBT retention. The 144 combinations comprised 18 binders paired with 8 aggregates. Those combinations sharing a binder or aggregate were not independent material replicates. The reported correlations and fitted relationships are interpreted as descriptive, exploratory associations within the tested material matrix; these correlations do not establish predictive validity. Regression analyses were also performed between percentages of asphalt retained and wet work of adhesion. For the wet case, regression values ranged between −0.01 and −0.44. The negative correlations mean that, with the increase in the percentage of asphalt binder retained, the wet work of adhesion decreases. Previous researchers observed this phenomenon [19] and stated that moisture susceptibility can be less thermodynamically possible due to lower wet work of adhesion.
Regression analyses were also performed on the work of adhesion from the sessile drop test and adhesion force from AFM tests. Regression coefficients from the analyses ranged between −0.05 and −0.17. The weak negative relation is due to the test’s contact area between these two tests. The contact area between liquid and solid is several mm2, and the contact area between the AFM tip and the asphalt binder is several nm2. The difference between the contact angles of the two tests can be a reason for the weak relationships. Previous researchers also found weak relationships between AFM adhesion force and dry and wet work of adhesion [32]. Such findings warrant additional research considering the scaling effects of test results at multiscale levels (e.g., macro, meso, micro, and nano).
From the AFM test results, S3-sourced binders had the highest, and S5-sourced binders had the lowest adhesion values. Differences among commercial sources may reflect composition, refining, blending, and modification practices. Their individual contributions were not measured. This research can be extended to observe the chemical composition of various sourced binders and their mechanical properties. Binders’ relative asphaltene content and polar functional groups can be compared. Previous researchers found that these chemical components affect mechanical properties [33,34].
5. Conclusions
The main goal of this research was to evaluate the adhesion properties of asphalt binders with aggregates by using three diverse types of tests at different scales. Three PG binders (PG 64-22, PG 70-22, and PG 76-22, each from six sources) and four types of aggregates (limestone, sandstone, dolomite, and novaculite, each from two sources) were evaluated in the laboratory. Overall, AFM was found to be a viable tool for gathering morphological and mechanistic data on asphalt binders at a micro level. The B2 and B3 binders differed from the B1 binders in pull-off force and deformation, but these comparisons combine PG and modification status. The apparent DMT modulus from AFM ranged from 125 MPa (S5B1) to 765 MPa (S2B3). The highest source-average modulus was 420 MPa for S1 after three days of storage and 402 MPa for S2 after seven days. These values describe the local indentation response. The associations between the SFE-based work of adhesion and the visually estimated TBT coating retention were generally weak. The S4B3–NV2 combination had the highest visually estimated TBT coating retention (90%). This was the highest observed retention under the tested boiling conditions; it was not established as statistically superior or as best under field conditions. The calculated dry work of adhesion ranged from 86.5 mJ/m2 (S2B2–NV1) to 174.5 mJ/m2 (S6B3–LS2), and the water-induced debonding energy ranged from 7.9 mJ/m2 (S2B2–LS2) to 55.7 mJ/m2 (S5B1–NV2). These thermodynamic quantities characterize specific binder–aggregate interfaces and are distinct from the AFM tip–binder pull-off forces. Approximate TBT retention showed only weak correlations with them (r = 0.32 for dry work of adhesion and r = −0.19 for debonding energy), and these were exploratory. AFM provided spatially resolved information on tip–binder pull-off force and apparent local indentation response. These measurements were not interpreted as direct measurements of binder–aggregate adhesion or pavement rutting resistance. Associations with SFE parameters and TBT retention were generally weak, and further validation is required before AFM descriptors can be used to predict mixture moisture performance.
Author Contributions
Design and concept: Z.H.; collection of data: Z.H., A.S.M.A., M.N.S.O., and K.S.S.; analysis, and data interpretation: Z.H., K.S.S., A.S.M.A., and M.N.S.O.; manuscript preparation and review: Z.H., K.S.S., A.S.M.A., and M.N.S.O. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by the Arkansas Department of Transportation (ARDOT), Little Rock, Arkansas, USA, under Grant No. Transportation Research Committee (TRC) 2102.
Data Availability Statement
The data presented in this study are available from the corresponding author upon reasonable request.
Acknowledgments
The authors appreciate the financial assistance provided by the Arkansas Department of Transportation (ARDOT). They also extend their gratitude to all the suppliers of aggregates and binders for their contributions to and support of this study.
Conflicts of Interest
The authors declare no conflicts of interest.
References
- Santucci, L. Minimizing Moisture Damage in Asphalt Pavements. Pavement Technol. Update 2010, 2, 1–12. [Google Scholar]
- Roy, S.; Hossain, Z. Use of Molecular-Level Dissipated Energy of Asphalt Binders to Predict Moisture Effects on Pavements. Int. J. Pavement Eng. 2011, 22, 1351–1362. [Google Scholar] [CrossRef] [Scilit]
- Little, D.N.; Jones, D.R. Chemical and Mechanical Processes of Moisture Damage in Hot-Mix Asphalt Pavements. In Moisture Sensitivity of Asphalt Pavements: A National Seminar; Transportation Research Board: Washington, DC, USA, 2003; pp. 37–70. ISBN 0-309-09450-X. [Google Scholar]
- Zollinger, C.J. Application of Surface Energy Measurements to Evaluate Moisture Susceptibility of Asphalt and Aggregates. Master’s Thesis, Texas A&M University, College Station, TX, USA, 2005. [Google Scholar]
- Hicks, R.G.; Santucci, L.; Aschenbrener, T. Introduction and Seminar Objectives. In Proceedings of the Moisture Sensitivity of Asphalt Pavements—A National Seminar, San Diego, CA, USA, 4–6 February 2003. [Google Scholar]
- Lu, Q. Investigation of Conditions for Moisture Damage in Asphalt Concrete and Appropriate Laboratory Test Methods. Ph.D. Dissertation, University of California, Berkeley, CA, USA, 2005. [Google Scholar]
- Sebaaly, P.E.; Hajj, E.Y.; Little, D.N.; Shivakolunthar, S.; Sathanathan, T.; Vasconcelos, K. Evaluating The Impact of Lime on Pavement Performance. National Lime Association. 2010. Available online: http://hdl.handle.net/11714/4915 (accessed on 7 March 2019).
- Taylor, M.A.; Khosla, N.P. Stripping of Asphalt Pavements: State-of-the-Art. Transp. Res. Rec. J. Transp. Res. Board 1983, 911, 150–158. [Google Scholar]
- Fromm, H.J. The Mechanisms of Asphalt Stripping from Aggregate Surfaces; Report RR190; Research and Development Division, Ontario Ministry of Transportation and Communication: Downsview, ON, Canada, 1974. [Google Scholar]
- Tarrer, A.R.; Wagh, V.P.; Harrigan, E.T.; Youtchef, J.S. The Effect of the Physical and Chemical Characteristics of the Aggregate on Bonding. SHRP-A/UIR-91, 507, Strategic Highway Research Program, National Research Council. 1991. Available online: https://onlinepubs.trb.org/onlinepubs/shrp/shrp-91-507.pdf (accessed on 21 September 2026).
- Scott, J. Adhesion and Disbonding Mechanisms of Asphalt Used in Highway Construction And Maintenance. In Proceedings of the Association of Asphalt Paving Technologists, Lake Buena Vista, FL, USA, 13–15 February 1978. [Google Scholar]
- Terrel, R.L.; Shute, J.W. Summary Report on Water Sensitivity. SHRP-A/IR-89-003, Strategic Highway Research Program. 1989. Available online: https://trid.trb.org/View/306353 (accessed on 21 September 2026).
- Kennedy, T.W.; Roberts, F.L.; Lee, K.W. Evaluating Moisture Susceptibility of Asphalt Mixtures Using the Texas Boiling Test. Transp. Res. Rec. J. Transp. Res. Board 1984, 968, 45–54. [Google Scholar]
- Ford, M.C., Jr.; Manke, P.G.; O’Bannon, C.E. Quantitative Evaluation of Stripping by the Surface Reaction Test. In Proceedings of the 53rd Annual Meeting of the Highway Research Board, Washington, DC, USA, 21–25 January 1974. [Google Scholar]
- Aljarrah, M.F.; Masad, E. Nanoscale Viscoelastic Characterization of Asphalt Binders Using the AFM-nDMA Test. Mater. Struct. 2020, 53, 110. [Google Scholar] [CrossRef] [Scilit]
- Binnig, G.; Quate, C.F.; Gerber, C. Atomic Force Microscope. Phys. Rev. Lett. 1986, 56, 930–933. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Loeber, L.; Sutton, O.; Morel, J.; Valleton, J.-M.; Muller, G. New Direct Observations of Asphalts and Asphalt Binders by Scanning Electron Microscopy and Atomic Force Microscopy. J. Microsc. 1996, 182, 32–39. [Google Scholar] [CrossRef] [Scilit]
- Beach, E.R.; Tormoen, G.W.; Drelich, J. Pull-off Forces Measured between Hexadecanethiol Self-Assembled Monolayers in Air Using an Atomic Force Microscope: Analysis of Surface Free Energy. J. Adhes. Sci. Technol. 2002, 16, 845–868. [Google Scholar] [CrossRef] [Scilit]
- Masson, J.-F.; Leblond, V.; Margeson, J. Bitumen Morphologies by Phase-Detection Atomic Force Microscopy. J. Microsc. 2006, 221, 17–29. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Bhasin, A. Development of Methods to Quantify Bitumen-Aggregate Adhesion and Loss of Adhesion Due to Water. Ph.D. Dissertation, Texas A&M University, College Station, TX, USA, 2007. [Google Scholar]
- Tarefder, R. A Study of Moisture Damage in Plastomeric Polymer Modified Asphalt Binder Using Functionalized AFM Tips. J. Syst. Cybern. Inform. 2011, 9, 23–24. [Google Scholar]
- Tarefder, R.A.; Zaman, A.M. Nanoscale Evaluation of Moisture Damage in Polymer Modified Asphalts. J. Mater. Civ. Eng. 2010, 22, 714–725. [Google Scholar] [CrossRef] [Scilit]
- Kim, S.; Lee, H.; Choi, H. Evaluation of Moisture Sensitivity of Asphalt Mixtures Using the Texas Boiling Test. Constr. Build. Mater. 2015, 101, 493–500. [Google Scholar]
- Ahmad, M.R.; Faisal, S.N.; Asif, M. A Review on Evaluation of Moisture Damage in Asphalt Concrete Mixtures. Int. J. Pavement Res. Technol. 2018, 11, 155–164. [Google Scholar]
- Chen, L.; Wang, D.; Zhang, Y. Investigation of Moisture Damage in Asphalt Mixtures Using the Texas Boiling Test. Road Mater. Pavement Des. 2020, 21, 931–945. [Google Scholar]
- Hefer, A.; Little, D.N.; Lytton, R. A Synthesis of Theories and Mechanisms of Bitumen-Aggregate Adhesion Including Recent Advances in Quantifying the Effects of Water. In Proceedings of the Association of Asphalt Paving Technologists, Long Beach, CA, USA, 7–9 March 2005. [Google Scholar]
- Hossain, Z.; Bairgi, B.; Belshe, M. Investigation of Moisture Damage Resistance of GTR-Modified Asphalt Binder by Static Contact Angle Measurements. Constr. Build. Mater. 2015, 95, 45–53. [Google Scholar] [CrossRef] [Scilit]
- Hossain, Z.; Roy, S.; Rashid, F. Microscopic Examination of Rejuvenated Binders with High Reclaimed Asphalts. Constr. Build. Mater. 2020, 257, 119490. [Google Scholar] [CrossRef] [Scilit]
- Oyan, M.N.S.; Hossain, Z.; Islam, M.R.; Braham, A.; Chun, S. Relative Compatibility Analysis of Aggregate-Binder Systems in Arkansas against Stripping. J. Mater. Civ. Eng. 2023, 35, 04023285. [Google Scholar] [CrossRef] [Scilit]
- Baldi Sevilla, A.; Aguiar-Moya, J.; Vargas-Nordcbeck, A.; Salazar, L.L. Effect of Aggregate–Bitumen Compatibility on Moisture Susceptibility of Asphalt Mixtures. Road Mater. Pavement Des. 2017, 18, 318–328. [Google Scholar] [CrossRef] [Scilit]
- Hossain, Z.; Rashid, F.; Mahmud, I.; Rahaman, M.Z. Morphological and Nanomechanical Characterization of Industrial and Agricultural Waste–Modified Asphalt Binders. Int. J. Geomech. 2017, 17, 04016084. [Google Scholar] [CrossRef] [Scilit]
- Gong, M.; Zhu, H.; Pauli, T.; Yang, J.; Wei, J.; Yao, Z. Evaluation of Bio-Binder Modified Asphalt’s Adhesion Behavior Using Sessile Drop Device and Atomic Force Microscopy. Constr. Build. Mater. 2017, 145, 42–51. [Google Scholar] [CrossRef] [Scilit]
- Sadat, K.S. Prediction of Moisture Resistance of Aggregate Binder System Through Physicochemical and Mechanical Assessment. Master’s Thesis, Arkansas State University, Jonesboro, AR, USA, 2024. [Google Scholar]
- Bhasin, A.; Dallas, L. Characterization of Aggregate Surface Energy Using the Universal Sorption Device. J. Mater. Civ. Eng. 2007, 19, 634–640. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.