Highlights
What are the main findings?
This review systematically analyzes composite-forming technologies for new energy-vehicle battery-pack structures from the perspective of process selection, defect control, and engineering application.
- •
- A component-oriented process-selection framework is established, linking service requirements, material systems, forming routes, typical defects, mechanical performance, applicable components, and engineering maturity.
- •
- Mainstream forming routes, including SMC, PCM/WCM, RTM/HP-RTM, VARTM, LFT-D/GMT, thermoplastic sheet forming, pultrusion, and multi-material joining, are compared in terms of process capability and battery-pack applicability.
- •
- The formation mechanisms, performance effects, and control strategies of typical defects in composite battery-pack components are summarized, including voids, dry spots/insufficient impregnation, resin/filler nonuniformity, delamination/interfacial debonding, warpage and residual stress, and fiber-orientation deviation/waviness/breakage.
What are the implications of the main findings?
- •
- The proposed framework provides guidance for rational material–process selection in upper covers, lower housings, trays, beams, side frames, protective structures, and joining/sealing regions.
- •
- The integration of process simulation, in-line monitoring, non-destructive testing, machine learning, and digital twins supports the transition from post-forming inspection to closed-loop quality control and certifiable manufacturing.
Abstract
Battery packs for new energy vehicles have evolved from simple load-bearing and protective assemblies into multifunctional safety structures integrating structural support, crash protection, thermal-runaway mitigation, flame retardancy, electrical insulation, electromagnetic interference shielding, waterproof sealing, and long-term reliability. Fiber-reinforced polymer composites are promising for upper covers, underbody shields, trays, cross beams, side frames, and local protective structures because of their low density, corrosion resistance, design flexibility, and functional-integration potential. However, composite-part performance is strongly governed by forming. Resin flow, impregnation, curing or cooling shrinkage, fiber orientation, filler dispersion, and interfacial bonding may induce voids, dry spots, resin-rich regions, delamination, warpage, and fiber waviness, thereby affecting load bearing, sealing, thermal protection, and durability. This review focuses on composite-forming technologies for new energy-vehicle battery packs. It summarizes component-level service requirements and material systems and compares representative forming routes, including sheet molding compound (SMC), prepreg compression molding/wet compression molding (PCM/WCM), resin transfer molding/high-pressure resin transfer molding (RTM/HP-RTM), vacuum-assisted resin transfer molding (VARTM), long-fiber thermoplastic direct processing (LFT-D), glass-mat thermoplastic (GMT), thermoplastic sheet forming, pultrusion, and multi-material joining. These routes are evaluated from six dimensions: material form, forming cycle, typical defects, representative mechanical performance, applicable components, and engineering maturity. The review further discusses defect mechanisms, performance effects, detection and control methods, and the roles of in-line monitoring, non-destructive testing, process simulation, machine learning, and digital twins in closed-loop quality manufacturing. Finally, engineering challenges are examined in multi-material joining, thermal-safety integration, low-carbon recycling, and standard certification. Composite-material battery-pack structures should therefore be developed as coordinated design and closed-loop manufacturing systems linking materials, processes, defects, performance, and validation.
1. Introduction
The rapid growth of new energy vehicles, particularly battery electric vehicles, has made the traction battery system a central element of vehicle design [1]. A battery pack is generally mounted under the vehicle floor and integrates cells, modules, electrical connections, a thermal-management system, a battery-management system, sealing structures, and an external enclosure. The enclosure must support cells and modules while maintaining system safety under crash [2,3,4], bottom impact [5], vibration fatigue [6], water exposure, thermal runaway [7], and external fire. Therefore, the evaluation criteria for battery-pack materials and structures cannot be restricted to mass reduction or a single mechanical-performance index. Mechanical protection, thermal safety, flame retardancy, electrical insulation, electromagnetic compatibility, sealing reliability, corrosion resistance, maintainability, and recyclability must be considered simultaneously.
From the perspective of regulations and standards, safety requirements for battery packs are becoming increasingly stringent. In China, GB 38031-2025, Safety Requirements of Power Battery for Electric Vehicles, has been issued [8]. Internationally, UN R100 Part II specifies safety requirements for rechargeable energy storage systems in road vehicles, whereas UL 2580 evaluates electric-vehicle battery packs, modules, and related energy storage components with respect to their ability to prevent hazards to people under simulated abuse conditions [9,10]. In addition, Regulation (EU) 2023/1542 entered into force on 17 August 2023, aiming to reduce the environmental impacts associated with rapidly growing battery use and to strengthen circular-economy and zero-pollution objectives [11]. These regulations indicate that the development of battery-pack materials and manufacturing technologies must address safety, performance, environmental impact, and life-cycle management together.
The use of composites in battery packs is driven by clear engineering needs. Fiber-reinforced polymer composites have low density and high specific strength and stiffness, and they can realize structural lightweighting through lay-up design, fiber-orientation control, local reinforcement, and sandwich construction [12,13]. In parallel, polymer matrices and functional fillers can provide flame retardancy [14,15], thermal insulation, thermal conduction, electrical insulation, or electromagnetic interference shielding [16,17]. Höhne et al. [18] noted that electric-vehicle battery-pack enclosures must provide not only structural protection but also electromagnetic shielding and flame-retardant safety functions. Although SMC-type composites show potential for battery-pack enclosures, conventional SMC generally requires modification of the fiber reinforcement, resin-matrix, and functional filler system to achieve electromagnetic shielding and flame retardancy at the same time. Thus, research on composite battery-pack parts has shifted from asking whether composites can replace metals to whether multifunctional safety structures can be manufactured stably, economically, and at scale.
The forming of fiber-reinforced polymer composites involves pronounced multiscale and multiphysics coupling. Because fibers, polymer matrices, interfaces, and functional fillers are heterogeneous and anisotropic, the final part performance is highly sensitive to forming parameters. Resin flow and fiber impregnation, curing reaction and chemical shrinkage, the cooling and crystallization of thermoplastic matrices, fiber-orientation evolution, filler dispersion, and mold temperature and pressure fields all affect microstructure, residual stress, porosity, and interfacial quality [19,20,21]. Process-induced voids, dry spots, delamination, debonding, resin-rich regions, fiber waviness, and warpage not only reduce strength, stiffness, interlaminar properties, and fatigue life but may also weaken sealing, insulation, thermal protection, and long-term service reliability [22,23]. Fu and Yao [24] reviewed manufacturing defects in fiber-reinforced polymer composites and emphasized that, because of the complexity of the material constituents and the physicochemical behavior during forming, defect formation mechanisms and detection methods are central to quality evaluation.
To review composite-forming technologies for electric-vehicle battery packs from an engineering viewpoint, this paper constructs a logic framework driven by component-level service requirements and manufacturability, as shown in Figure 1. The framework is organized around four linked modules: service requirements and composite-material systems, forming processes, typical defects and prevention strategies, and digital twins and digitalization challenges. It summarizes the technological logic from material selection and process realization to defect control and digital manufacturing. Following this framework, this review first discusses battery-pack application regions, service requirements, and material systems. It then compares mainstream forming routes, analyzes manufacturing defects and quality-control methods, and discusses the roles of in-line monitoring, non-destructive testing, process simulation, machine learning, and digital twins in closed-loop quality manufacturing. Finally, it identifies engineering development directions from multi-material joining, thermal safety, low-carbon recycling, and standard certification perspectives.
Figure 1.
Review framework for composite battery-pack manufacturing technologies.
The distinctive contribution of this review is therefore to integrate component-level service requirements, composite-material systems, forming-route capability, defect formation, quality control, digital manufacturing, and engineering certification into a single process-selection logic. This positioning shifts the review from a catalog of composite processes to a decision-oriented framework for composite battery-pack manufacturing.
2. Service Requirements and Material Systems of Battery-Pack Composites
2.1. Application Regions of Composite Materials in Battery Packs
As shown in Figure 2, a battery pack usually includes an upper cover, lower housing, longitudinal and transverse beams, fixing plates, connecting brackets, lifting lugs, ribs, and sealing flanges. The upper cover primarily requires sealing, flame retardancy, electrical insulation, and environmental protection. The lower housing and beam system bear module weight, road impact, vibration, and crash loads. Bottom and edge regions require resistance to stone impact, bottoming, puncture, and energy absorption. Joining and flange regions are more sensitive to dimensional accuracy, fatigue, interfacial durability, and maintainability. Because the risk levels of these regions differ, the material and process solution should not be uniform for the whole pack.
Figure 2.
Typical structural components of a new energy-vehicle traction battery-pack enclosure [2].
From the viewpoint of function and risk level, composite applications in battery packs can be divided into three categories: load-bearing components, such as lower housings, beams, side frames, and local reinforcement zones; protective and functional components, such as upper covers, underbody shields, thermal-barrier/flame-retardant layers, and insulating parts; and joining and multi-material integration regions, including inserts, lifting lugs, bonded flanges, and sealing grooves. The first two categories emphasize continuous-fiber load-bearing capacity and multifunctional integration, respectively, whereas the third category governs load transfer, assembly, and long-term sealing reliability. Evaluation should be extended stepwise from material coupons to representative subcomponents, full-size components, and pack-level systems.
2.2. Service Requirements: From Lightweighting to Multifunctional Safety
Composite materials for battery packs must first meet lightweighting targets [1,25,26,27]. The battery system accounts for a substantial proportion of the vehicle mass, and reducing the mass of the enclosure and protective structures can improve the driving range or release mass allowance for additional cells, thermal-management systems, and safety redundancy. However, battery-pack lightweighting cannot compromise safety. Because the pack is installed under the vehicle floor, it is exposed to crash, compression, bottom impact, vibration fatigue, and water ingress. Accordingly, sufficient stiffness, strength, impact toughness, and structural integrity are required [28].
Battery-pack composites must satisfy thermal-safety and flame-retardancy requirements. Lithium-ion batteries may undergo thermal runaway under mechanical, electrical, or thermal abuse [29,30], accompanied by high temperature, gas release, flames, and particle ejection. Enclosure and insulation materials must delay heat propagation, reduce flame-spread risk, and maintain structural integrity for a defined period. Because resin-matrix composites usually contain organic matrices, flame-retardant design is a core issue for battery-pack applications. Flame-retardant resins, expanded graphite, inorganic fillers, ceramic-forming systems, aerogel-based insulation composites [31], and surface fire-protection coatings are important routes for improving thermal safety.
Battery-pack materials must also meet electrical and electromagnetic-compatibility requirements. Metallic enclosures naturally provide electrical conductivity and electromagnetic shielding, whereas glass-fiber-reinforced resin composites are typically electrically insulating and have limited shielding performance. When used for battery-pack enclosures, shielding performance can be improved by carbon fibers, conductive carbon black, carbon nanotubes, graphite, or metal meshes. However, conductive fillers may influence resin rheology, impregnation, flame retardancy, mechanical performance, and cost. Electromagnetic shielding, flame retardancy, and formability are therefore strongly coupled. Liu et al. [32] proposed a hierarchical TPU/PZM@CP/CF composite, showing that carbon-fiber fabrics can build conductive pathways, while phosphorus–nitrogen flame-retardant nanofillers can improve flame retardancy, smoke suppression, and mechanical properties. This illustrates that multifunctional fillers and hierarchical structures are important for balancing electromagnetic shielding, flame retardancy, and mechanical performance, although battery-pack-level validation of large-size forming, crash protection, thermal runaway, and EMC are still required.
In addition, battery-pack enclosures require waterproof sealing, corrosion resistance, hygrothermal durability, chemical resistance, and maintainability. Composites generally provide better corrosion resistance than many metals, but moisture absorption by the resin, interfacial aging, the degradation of adhesive interfaces, and thermal-cycle-induced microcracking may still impair long-term reliability. Therefore, evaluation should move from material-level tests toward component-level, coupled-environment, and long-term service validation.
2.3. Classification of Composite-Material Systems
Composite materials for battery-pack structures are not a single material class. They are multicomponent systems composed of the polymer matrix, reinforcing fibers, functional fillers, interfaces, and functional layers. Different material systems and material forms must be matched to the service requirements and application regions of battery-pack components. Figure 3 summarizes the classification and selection logic of composite materials for battery-pack structures from four levels: material constituents, representative material systems/forms, key service requirements, and typical application regions.
Figure 3.
Composite-material systems, material forms, service requirements, and typical application regions for battery-pack structures.
Battery-pack composites can be classified by matrix type into thermoset and thermoplastic composites [33]. Thermoset composites commonly use epoxy, unsaturated polyester, vinyl ester, polyurethane, or modified resin systems. They feature low resin viscosity, good fiber impregnation, relatively high dimensional stability after curing, good heat resistance, and good bonding performance. SMC, BMC, RTM, HP-RTM, VARTM, and prepreg compression molding are mostly used for thermoset composites and are suitable for large, complex upper covers, lower housings, and reinforcement components that require stiffness, flame retardancy, and structural integrity. In recent years, SMC systems based on unsaturated-polyester/polyurethane hybrid resins have been used for electric-vehicle battery-pack enclosures, with flame-retardant and electromagnetic-shielding functions introduced using carbon fibers, expanded graphite, conductive carbon black, or carbon nanofillers. However, thermoset networks cannot be remelted and reshaped, so recycling is difficult. Moreover, resin flow, fiber orientation, void formation, curing shrinkage, and warpage during processing affect part performance and consistency.
Thermoplastic composites usually use polypropylene, polyamide, polyphenylene sulfide, polyether ether ketone, polyethylene terephthalate, or related matrices, reinforced with short fibers, long fibers, continuous-fiber-reinforced organosheets, prepreg tapes, or hybrid architectures. Compared with thermosets, thermoplastic composites generally offer shorter molding cycles, higher impact toughness, weldability [34], thermoformability, and better recyclability, which makes them attractive for high-throughput manufacturing and circular-economy requirements. For example, carbon-fiber/PET thermoplastic composites can be used for battery underbody protection, and flame-retardant glass-fiber-reinforced PP can be used in battery-pack enclosures or tray fire-protection designs [35]. However, the high melt viscosity of thermoplastics makes continuous-fiber impregnation and interlaminar bonding more difficult. Voids, crystallinity, residual stress, and dimensional stability must be controlled during processing. For battery-pack use, flame-retardant systems, interfacial bonding, thermomechanical reliability, and recycling routes after service must be further optimized [36].
Regarding reinforcement fibers, glass fibers are the most common reinforcement in battery-pack composites because of their low cost, good insulation, and stable overall performance. Carbon fibers provide higher specific strength and stiffness [37] and have potential for electrical conduction and electromagnetic shielding, but their cost is higher and their electrical-insulation design becomes more complex. Basalt, aramid, and ceramic fibers may be used where heat resistance, impact resistance, or fire insulation is needed. In practice, hybrid-fiber reinforcement and local continuous-fiber reinforcement are important strategies for improving the performance–cost balance.
Functional fillers are also essential. Flame-retardant fillers include aluminum hydroxide, magnesium hydroxide, phosphorus-based flame retardants, and expanded graphite. Thermally conductive fillers include boron nitride, alumina, and graphite. Conductive fillers include carbon black, carbon nanotubes, graphene, metal fibers, and metal meshes. Thermal-insulation fillers include aerogels, hollow glass microspheres, and ceramic fibers. Although fillers improve functionality, they often increase viscosity, reduce fiber impregnation efficiency, and may induce agglomeration, resin-rich regions, and interfacial weakening. Functional material systems must therefore be designed together with the forming process.
2.4. Material–Process-Performance Selection Principles
Material–process selection should start from component function and risk level. It should answer five questions in sequence: what loads and safety functions the component must carry; which resin, fiber, and functional layers meet those requirements; whether the target forming process can produce the component stably within the required cycle and size; whether the main defects can be monitored, detected, and assigned tolerance limits; and whether material-level results can be verified through component- and system-level testing. Based on this logic, Table 1 summarizes the functional requirements, preferred material systems, suitable forming processes, and key validation items for representative battery-pack components.
Table 1.
Selection matrix linking battery-pack regions, functions, materials, and processes.
For practical process selection, these questions can be further converted into an MCDM-oriented screening workflow rather than a final weighted decision model. Component function first defines the mandatory constraints, such as load bearing, sealing, flame retardancy, insulation, or thermal-runaway protection. Candidate material systems and forming routes are then screened according to mechanical-performance potential, cycle efficiency, cost level, defect sensitivity, recyclability, and engineering maturity. The result should be treated as an unweighted, literature-based screening outcome rather than an absolute ranking, because the preferred route changes with component size, production volume, safety level, and validation requirements.
As summarized in Table 1, there is no single optimal process for composite-material battery-pack structures. Functional components such as upper covers, protective covers, and module boxes emphasize flame retardancy, insulation, sealing, and lightweighting and can preferentially use glass-fiber SMC, LFT-D/GMT, or continuous-fiber thermoplastic sheets, with flame-retardant and shielding functions integrated by fillers or surface layers. Highly loaded regions such as lower housings, cross beams, and side frames rely more strongly on continuous-fiber systems and are better suited to PCM/WCM, RTM/HP-RTM, pultruded profiles, or metal–composite hybrid structures, with local reinforcement at mounting points, side beams, and impact-sensitive regions.
Process selection is also constrained by component size, complexity, production volume, and quality consistency. SMC and LFT-D/GMT are suitable for high-throughput parts with complex ribs. PCM/WCM and HP-RTM are suitable for high-performance continuous-fiber shells or plates. VARTM is more appropriate for large prototypes or low- to medium-volume manufacturing. Pultrusion is suitable for constant-section beams and side frames. The process is not an auxiliary step after material selection; it is a core variable that determines fiber form, defects, and final performance.
Defect sensitivity must be identified during selection. Highly filled systems are prone to poor impregnation and filler agglomeration. Continuous fibers in complex surfaces are sensitive to wrinkles and bridging. Thermoplastic systems require control over fiber length, orientation, crystallinity, and welding reliability. Critical defects should be linked to load bearing, sealing, insulation, and thermal-protection functions.
Engineering metrics should include static and fatigue performance, post-impact performance, flame retardancy and heat release, thermal insulation/conduction, EMI shielding and electrical insulation, moisture aging, sealing and joining, dimensional stability, cycle time, cost, repair, and recycling. High-risk components require hierarchical validation from material to subcomponent, to full-size component, and to battery-pack system; a single material property should not be used as a substitute for service evaluation.
In summary, material selection for composite-material battery-pack structures is a systems-engineering problem under multiple constraints. The core task is not to find a universal material that fully replaces steel or aluminum but rather to build coordinated relationships among material systems, forming processes, defect control, and performance validation according to the functional boundaries and risk levels of different components. Based on this logic, Section 3 compares the principal forming routes used for composite battery-pack manufacturing.
3. Mainstream Forming Technologies and Their Battery-Pack Applications
To avoid evaluating composite-forming routes only on the basis of a single strength, density, or cycle-time index, this review establishes a multi-level process-selection framework for electric-vehicle battery-pack components. As shown in Figure 4, the inner level evaluates forming routes from six dimensions: material form, forming cycle, main defects, representative mechanical performance, applicable components, and engineering maturity. The outer level further links these dimensions to manufacturability, production efficiency, defect risk, performance reliability, component compatibility, and industrialization level. Based on this framework, the following sections compare SMC, PCM/WCM, RTM/HP-RTM, VARTM, LFT-D/GMT, thermoplastic sheet forming, pultruded profiles, and multi-material joining.
Figure 4.
Multi-level evaluation framework for composite-forming processes used in electric-vehicle battery packs.
3.1. Sheet Molding Compound Compression Molding
In terms of material form, sheet molding compound (SMC) compression molding uses thermoset sheets reinforced mainly with 25–50 mm chopped glass fibers or carbon fibers. The fiber volume fraction may reach up to 50%, and the formulation usually contains low-shrinkage additives, fillers, flame retardants, thickeners, and functional additives [38]. During sheet preparation and maturation, the resin, fibers, and functional fillers are compounded in advance. During compression molding, charge flow fills the cavity. The SMC molding sequence is shown in Figure 5. Because chopped fibers reorient during resin flow, local mechanical properties are closely related to charge placement, flow path, molding pressure, mold temperature, and rib geometry [39].
Figure 5.
SMC compression molding process.
Regarding forming cycle, SMC is a mature, high-efficiency closed-mold route for automotive composites and is suitable for medium- to high-volume production. General technical data for automotive composite compression molding report a closed-mold cycle time of approximately 1–4 min [40]. The advantage is that filling, compaction, curing, and demolding are integrated in one press operation, with high material utilization and the ability to mold complex ribs, bosses, local thickening, and reinforcement around mounting holes. Compared with continuous-fiber liquid molding, SMC more readily meets automotive cycle-time and cost requirements. However, the actual cycle for large battery-pack covers or lower housings is still affected by charge area, thickness, filler-induced viscosity, demolding and inspection rhythm, and dimensional requirements at sealing surfaces. Therefore, 1–4 min should not be generalized to all large battery-pack parts.
The major defects of SMC include flow-induced fiber-orientation nonuniformity, local resin-rich regions, fiber-poor regions, voids, weld lines, insufficient strength at thickness transitions, and warpage. For battery-pack enclosures, thick sections, rib roots, insert regions, long flow-path ends, and large sealing edges are defect-sensitive. Highly filled flame-retardant or conductive SMC can improve thermal safety and electromagnetic shielding but may increase viscosity, causing filling difficulty, insufficient fiber impregnation, and local property scatter. Höhne et al. [18] showed that a UPPH hybrid resin system containing 50 wt.% carbon fibers and 11.5 wt.% expanded graphite achieved favorable combined electromagnetic-shielding and flame-retardant performance. This indicates that flame-retardant and shielding fillers do more than add functions; they also modify resin flow, fiber dispersion, and the molding window. SMC battery-pack applications should therefore focus on charge design, flow distance, local reinforcement, and molding-simulation verification [41,42,43].
Representative mechanical performance should be assessed with reference to the exact material formulation and sampling direction. Trauth et al. [44] studied an unfilled glass-fiber/vinyl-ester structural SMC with chopped-fiber lengths of 25.4 mm, or a 6:5 mixture of 25.4 and 50.8 mm, and a fiber volume fraction of approximately 17–31 vol.%. For the SMC containing only 25.4 mm fibers and sampled along the sheet-manufacturing direction, tensile strength increased from 64 to 150 MPa, flexural strength from 157 to 277 MPa, and Charpy impact strength from 51 to 91 kJ/m2. Their results also showed that increasing fiber volume fraction improved tensile, compressive, flexural, and impact performance. Meanwhile, conveyor-induced fiber orientation during sheet manufacture caused directional differences, whereas the mixed 25.4/50.8 mm fiber length had no significant effect on the quasi-static and dynamic properties of that material system. Thus, SMC design for battery packs should not quote a single tensile strength alone; fiber content, mold flow direction, weld-line position, and local reinforcement must be linked to the bending, impact, and fatigue performance of shell structures.
SMC is more suitable for battery-pack upper covers, protective covers, module boxes, non- or medium-load lower housings, local functional parts, and composite units in multi-material hybrid structures. For upper-cover-type parts dominated by flame retardancy, insulation, corrosion resistance, lightweighting, and structural integration, SMC is well matched. Teijin Automotive Technologies [45] reported a multi-material battery-pack enclosure composed of an integrated composite upper cover, an integrated composite tray, and aluminum/steel reinforcements. The design reduces mass by approximately 15% compared with a steel battery-pack enclosure, and the tray is molded as one piece without through-holes to reduce sealing and leakage risks. This case shows that SMC or SMC-dominated multi-material structures are better understood as “composite shells plus metal reinforcements plus optimized sealing structures”; their engineering value lies in multi-material coordination, not in simply replacing highly loaded metal tray structures. For lower housings, trays, and cross beams, conventional chopped-glass-fiber SMC usually cannot alone meet high stiffness, strength, impact, and fatigue requirements. Carbon-fiber SMC, glass/carbon hybrid SMC, local continuous-fiber reinforcement, metal inserts, or metal-frame–SMC hybrid structures are often needed.
In terms of engineering maturity, SMC has a mature application base in automotive exterior panels and functional structural parts and is among the routes closest to scaled use in composite battery-pack enclosures. A publicly reported enclosure mass reduction of about 15% [45] and functional SMC results for flame retardancy and electromagnetic shielding [18] indicate that this route has moved from material substitution toward functional integration. Its maturity in high-safety load-bearing battery structures, however, still depends on material-batch stability, fiber-orientation prediction, flame-retardant/electromagnetic-shielding synergy, joining and sealing reliability, and component-level impact/fatigue validation. Overall, SMC is best positioned as a high-throughput, function-integrated, medium-load composite route rather than a direct replacement for highly loaded metal trays.
3.2. Prepreg Compression Molding and Wet Compression Molding
Prepreg compression molding (PCM) mainly uses continuous-fiber prepregs, fast-curing prepregs, or non-crimp-fabric prepregs. Wet compression molding (WCM) usually uses dry continuous-fiber fabrics, non-crimp fabrics, or fiber preforms as reinforcements, with a metered amount of resin added in the mold to complete impregnation and curing. Both processes are characterized by continuous-fiber reinforcement, and they allow load-path matching through lay-up angle, ply thickness, local reinforcement, and sandwich design. Their material-design freedom is higher than that of chopped-fiber SMC. A typical PCM process includes prepreg lay-up, preheating, preforming, forming and curing, trimming, and demolding. Vacuum-assisted prepreg compression molding (VA-PCM) further uses a vacuum bag and negative-pressure evacuation to improve resin flow and interlaminar compaction in curved or complex regions, as shown in Figure 6.
Figure 6.
Schematic drawing of PCM and VA-PCM processes [46].
The overall cycle time of PCM/WCM is determined by prepreg cutting, lay-up, preforming and transfer, mold heating, resin curing, demolding, and in-line inspection. Resin curing time is not the only limiting factor. For example, Huntsman [47] reported that a fast-curing epoxy system can cure in about 2 min at 130 °C with a total cycle of about 2.5 min; a later system can reduce curing time to 30 s at 140 °C, with a theoretical press cycle close to 1 min. These data show that fast-curing resins can substantially shorten the in-mold curing stage. For PCM/WCM battery-pack parts, however, the actual throughput is still controlled by cutting, lay-up, preform stability, transfer, venting, in-line inspection, and component-level quality consistency. Therefore, PCM/WCM normally cannot reach the overall high throughput of SMC or LFT-D but is suitable for continuous-fiber load-bearing parts and medium-volume high-performance components.
Typical PCM defects include fiber wrinkles, bridging, sliding, local accumulation, interlaminar damage, trapped voids, curing shrinkage, residual stress, warpage, and spring-in in complex geometries [48,49]. WCM is more sensitive to resin flow and fiber-bed impregnation. Resin-metering errors, local permeability variation, insufficient compaction, and nonuniform flow can cause dry spots, voids, resin-rich regions, and nonuniform fiber volume fraction [50,51]. Therefore, preform stability, resin viscosity, gel time, in-mold pressure distribution, and venting paths must be controlled.
Continuous-fiber compression-molded parts generally exhibit high specific strength and stiffness along the principal fiber direction, whereas interlaminar properties are governed by curing degree, fiber–matrix interface, void content, and lay-up quality. For PCM, Wu et al. [52] used T700/2626 carbon-fiber/epoxy prepreg with a fiber volume fraction of 67%, a 20-ply 0° unidirectional lay-up, and a compression pressure of 0.6 MPa. Short-beam shear tests according to GB/T 30969-2014 showed interlaminar shear strengths of 62.88–90.88 MPa under different curing schedules. Holding time, curing temperature, and heating rate all affected interlaminar performance. For WCM, Sears et al. [53] statistically optimized wet compression molding parameters for carbon-fiber/epoxy composites and found that press speed, resin amount, and heating temperature jointly affected flexural strength, flexural modulus, and fracture strain. Under optimized parameters, flexural strength and modulus increased by approximately 15.5% and 10.5%, respectively. Thus, the mechanical performance of PCM/WCM parts depends not only on fiber grade, fiber content, and lay-up design but also on curing schedule, impregnation quality, porosity, and fiber–matrix interfacial bonding.
PCM/WCM is more suitable for battery-pack components with higher safety levels and continuous-fiber load-bearing requirements, such as continuous-fiber upper covers, impact-resistant underbody shields, thermal-runaway protective sandwich panels, local reinforcement plates, cross-beam connection regions, and load-bearing connectors. The advantage is the ability to place continuous fibers along the principal load direction and improve bending, impact, crushing, and vibration-fatigue performance. PCM/WCM can also be combined with foam cores, honeycomb cores, aerogel mats, mica sheets, or other thermal-insulation/flame-retardant layers to form sandwich structures with both specific stiffness and thermal-protection capacity.
In terms of engineering maturity, PCM has a strong technical basis in high-performance composite structures, but the material cost, lay-up automation, preform transfer, and stable forming of complex parts limit its economic feasibility for large-scale battery-pack use. WCM has the potential to reduce material cost and accommodate large parts, but its maturity depends more strongly on in-mold impregnation control, in-line monitoring, and defect detection. Overall, PCM/WCM should be viewed as high-performance, continuous-fiber, designable load-bearing routes for critical protective plates, local load-bearing plates, and high-safety structural components, rather than as universal low-cost enclosure processes.
3.3. Resin Transfer Molding and Its Derivative Processes
Resin transfer molding (RTM) [54], high-pressure resin transfer molding (HP-RTM) [55], and vacuum-assisted resin transfer molding (VARTM) [56] use dry continuous-fiber fabrics, non-crimp fabrics, three-dimensional fabrics, or fiber preforms as reinforcements. Their forming core is the flow, impregnation, and curing of low-viscosity resin in a fibrous porous medium. RTM/HP-RTM usually use closed molds and pressure injection. VARTM commonly uses a single rigid mold, a vacuum bag, and flow media, and resin is infused by the vacuum-pressure difference. Figure 7 and Figure 8 show schematic forming routes for HP-RTM and VARTM, respectively. Compared with chopped-fiber compression molding, these liquid molding routes better preserve fiber continuity and load-transfer paths.
Figure 7.
Schematic process of HP-RTM.
Figure 8.
Schematic process of VARTM [56].
The RTM cycle is mainly determined by preform preparation, mold closing, resin injection, impregnation, curing, and demolding. HP-RTM shortens filling and curing through high-pressure injection, fast-reacting resin, and precise mold-temperature control, which makes it closer to the automotive requirements for high throughput and batch stability. Huntsman [57] lists battery-pack enclosures as an HP-RTM application and reports low void content, high productivity, and an in-mold curing time as short as about 2 min. RTM, especially HP-RTM, is therefore suitable for continuous-fiber parts requiring high fiber volume fraction, dimensional accuracy, double-sided surface quality, and cycle-time control. VARTM has a lower equipment and mold cost and is suitable for large parts, but the infusion process depends mainly on vacuum pressure and is usually slower; thickness accuracy, porosity, and surface quality are more strongly affected by vacuum-bag compaction, flow-media design, and resin viscosity. In battery-pack applications, VARTM is better suited to prototype development, low- to medium-volume production, and the validation of large low-cost components.
The core defect risks in RTM/HP-RTM include dry spots, voids, unstable flow fronts, preform deformation, race tracking, resin-rich regions, and local impregnation deficiency. Race tracking causes resin to move rapidly along mold edges, preform gaps, or high-permeability channels, resulting in nonuniform flow fronts and dry-spot formation [58]. Hamidi et al. [59] reviewed process-induced defects in liquid composite molding (LCM) processes such as RTM and VARTM, classifying them as preform defects, flow-induced defects, and cure-induced defects. In VARTM, flow-induced defects are mainly dry spots and voids. Dry spots are associated with nonuniform flow paths, race tracking, high-permeability channels, improper convergence of multiple flow fronts, or premature gelation. Voids are affected by initial air in the resin, bubble nucleation under vacuum, resin viscosity, surface tension, and mismatches between intra-tow and inter-tow impregnation rates. Even low void contents may significantly reduce interlaminar shear, flexural, tensile, and fatigue performance.
RTM/HP-RTM and VARTM can both obtain high load-bearing capacity along the principal fiber direction through continuous fibers, but transverse, interlaminar, compressive, and impact properties are more sensitive to preform architecture, fiber volume fraction, voids, dry spots, resin-rich regions, and fiber deformation in curved regions. Holmberg and Berglund [60] studied the manufacturing quality and load-bearing behavior of RTM U-beams and showed that RTM can fabricate complex continuous-fiber sections, but preform deformation, fiber rearrangement, and local manufacturing defects in curved corners affect failure location, failure mode, and load capacity. Sun et al. [61] showed that, compared with conventional RTM, optimized compression–injection coupling in carbon-fiber/epoxy CRTM increased tensile, flexural, and interlaminar shear strengths by up to 42.9%, 41.2%, and 77.3%, respectively, while reducing porosity by 45.2%. For VARTM, Yalcinkaya et al. [62] used external pressure up to 138 kPa and resin flushing to increase the fiber volume fraction of glass-fiber/epoxy laminates from about 50% to about 62%, reduce porosity below 1%, and improve flexural performance by up to about 20%. These results show that liquid molding performance must be assessed by linking fiber architecture with impregnation quality rather than assuming that a continuous-fiber route alone guarantees high strength.
RTM/HP-RTM is suitable for high-performance upper covers, locally load-bearing lower housings, reinforcing beams, cross beams, underbody protection structures, and composite–metal hybrid load-bearing parts. It enables relatively high fiber volume fraction, good double-sided surface quality, in-mold insert integration, and integrated forming of complex structures. VARTM is more suitable for large upper covers, underbody shields, low-volume commercial-vehicle battery-pack enclosures, prototype composite packs, and sandwich protective structures. It should not be regarded as the preferred high-throughput mass-production route for passenger-vehicle battery packs.
In terms of engineering maturity, RTM/HP-RTM has a mature process base in aerospace, automotive, and other high-performance composite structures. HP-RTM, with high-pressure injection, fast-reacting resin, and precise mold-temperature control, has the potential to shorten injection and curing times and improve production efficiency. For large battery-pack upper covers, lower housings, and trays, however, several issues remain: automated preforming, fast flame-retardant resin compatibility, uniform temperature control in complex molds, in-line flow-front monitoring, and dimensional stability of large sealing flanges. Conventional RTM is more suitable for medium-throughput high-performance components, whereas HP-RTM has the potential to develop toward medium- to high-throughput automotive production. VARTM uses one-sided molds and vacuum-assisted infusion, providing low tooling cost, process flexibility, and suitability for large components but with longer infusion/curing cycles and a greater sensitivity of thickness uniformity, porosity, and surface quality to vacuum level, resin viscosity, and flow path. It is therefore more suitable for large prototypes, sandwich protective structures, and low- to medium-volume battery-pack enclosures.
3.4. Long-Fiber Thermoplastic Direct Processing, Glass-Mat-Reinforced Thermoplastics, and Thermoplastic Sheet Forming
Long-fiber thermoplastic direct processing (LFT-D) [63], glass-mat-reinforced thermoplastics (GMTs) [64], and continuous-fiber thermoplastic sheets [65] are thermoplastic composite-forming routes. In LFT-D, continuous-fiber roving or long chopped fibers are compounded in-line with thermoplastic resin, melt-impregnated, dispersed, and converted into a flowable molten charge for compression molding. GMT uses glass-mat-reinforced thermoplastic sheets that are heated and pressed. Continuous-fiber thermoplastic sheets or organosheets are based on continuous-fiber laminates and can be heated, thermoformed, over molded, and welded to integrate structural and joining functions. Figure 9 shows the compounding and compression molding route for LFT-D materials.
Figure 9.
Process scheme for compounding (left) and compression molding (right) of LFT-D materials [66].
Because thermoplastic composites do not rely on long chemical-curing times, their process mainly involves heating, plasticization, transfer, compression, cooling, and demolding, giving them high-throughput potential. LFT-D is especially suitable for in-line continuous feeding and high-cycle compression molding. Public process data report an LFT-D in-line compounding–compression molding cycle of about 30–50 s [67]. The cycles of GMT and continuous-fiber thermoplastic sheets depend on sheet-heating uniformity, forming-temperature window, cooling stabilization, over molding, and welding/assembly operations. Compared with thermoset continuous-fiber processes, thermoplastic routes have clear advantages in circular economy, welding, and rapid manufacturing but require tight temperature-field control and automated transfer to ensure consistency.
The key LFT-D defect is fiber-length loss during screw compounding, melt conveying, charge transfer, and compression flow, together with flow-induced fiber orientation that causes anisotropy and local property variation [68]. GMT and continuous-fiber thermoplastic sheets are sensitive to nonuniform sheet heating, ply deformation, wrinkles, interlaminar sliding, poor impregnation, voids, cooling shrinkage, warpage, and weakened welded interfaces [69]. When flame retardants, thermally conductive fillers, or electromagnetic-shielding fillers are added, increased melt viscosity and filler agglomeration may further reduce impregnation efficiency and interfacial quality.
Representative mechanical data for long-glass-fiber thermoplastics from public LFT-D process information include tensile strength of about 50–120 MPa, flexural strength of about 90–120 MPa, and final glass-fiber length above 20 mm [67]. These values represent only the corresponding material system and process window. Schelleis et al. [66] tested LFT-D plates based on approximately 40 wt.% glass-fiber-reinforced PC. The tensile modulus was about 10 GPa, and tensile strength exceeded 125 MPa. The flexural modulus reached about 11 GPa and flexural strength about 216 MPa. Charpy impact strength was about 43.1–45.5 kJ/m2 along the principal flow direction but decreased to about 19 kJ/m2 in the 90° direction in the flow zone. The tests followed DIN EN ISO 527-4, ISO 14125, ISO 6603-2, and ISO 179-1. These data show that glass-fiber mass fraction alone cannot represent part performance. Screw-induced fiber breakage, charge placement, flow distance, shell-core orientation structure, weld lines, and temperature/humidity state all affect tensile, flexural, and impact behavior.
LFT-D and GMT are suitable for battery-pack upper covers, module boxes, underbody shields, local reinforcements, and medium-load housing components. Continuous-fiber thermoplastic sheets are more suitable for plate and shell parts, protective plates, and local structural reinforcements that require higher load-bearing capacity and lay-up design. For thermoplastic upper covers, Trinseo [70] reported a PC-based LFT-D solution with more than 25% mass reduction compared with a steel cover and about 30% lower carbon footprint than an aluminum solution. A protective structure composed of 3 mm thick PC LFT-D and a 1 mm mica sheet met UL 2596-related thermal-runaway testing and the fire test specified in GB 38031. These mass-reduction and carbon-footprint values come from a public industrial case and depend on cover design, material consumption, and assessment boundary. The example suggests that the value of thermoplastic routes is not only recyclability but also the integration of rapid compression molding, thermal-runaway isolation, lightweighting, and assembly. Thermoplastic routes can also be combined with hot-plate welding, ultrasonic welding, vibration welding, injection over molding, mechanical riveting, adhesive bonding, and metal inserts to realize joining, sealing, protection, and local functional integration.
Thermoplastic composites have a strong engineering basis in automotive parts. LFT-D and GMT offer high-throughput potential, whereas continuous-fiber thermoplastic sheets are promising for high-performance and recyclable structures. For battery packs, their maturity still depends on flame-retardant safety, thermal and hygrothermal aging, welding and hybrid-joining reliability, retention of properties after recycling, and pack-level impact and thermal-runaway validation. Overall, this route can be considered a high-throughput, impact-resistant, weldable, and recyclable battery-pack composite solution, but recyclability alone is insufficient; structural safety, flame-retardant protection, sealing durability, and cost control must also be verified at system level.
3.5. Pultrusion and Continuous Profile Forming
Pultrusion and continuous profile forming use continuous-fiber bundles, fabrics, or mats as reinforcement. After resin impregnation, the reinforcement is pulled through a heated die for curing or cooling, producing constant-section or nearly constant-section composite profiles [71]. According to matrix type, pultruded profiles can be thermoset or thermoplastic. Thermoset systems commonly use epoxy, unsaturated polyester, vinyl ester, or polyurethane resins, whereas thermoplastic systems use polypropylene, polyamide, polyphenylene sulfide, or polyether ether ketone. Figure 10 shows an advanced industrial resin-injection pultrusion line, and Figure 11 presents the corresponding schematic.
Figure 10.
A state-of-the-art industrial resin-injection pultrusion line; material flows from left to right (courtesy of Fiberline Composites A/S) [72].
Figure 11.
Schematic of a resin-injection pultrusion line; material flows from left to right [73].
Pultrusion is a continuous manufacturing route in which material passes stably through impregnation, preforming, heating-curing or cooling-solidification zones under pulling. It provides high production efficiency, high material utilization, and good dimensional stability. Minchenkov et al. [74] reviewed thermoplastic pultrusion and noted that one advantage of pultrusion over other composite processes is a production speed of up to about 5 m/min. In GF/PP thermoplastic profile experiments, the same research team also used tape preparation speeds of 2, 5, and 8 m/min to verify the influence of speed on profile quality and mechanical performance [75]. Thus, the cycle advantage of pultrusion is primarily in long straight profiles, not complex three-dimensional shells or large variable-section structures. For side frames, cross beams, longitudinal beams, and crash beams in battery packs, pultrusion can provide continuous production and low unit-length manufacturing cost, but the above speed data cannot be extrapolated to curved trays or complex housings.
Typical defects in pultruded profiles include insufficient fiber impregnation, voids, fiber deviation, resin-rich or resin-poor regions, surface cracks, incomplete curing, residual stress, profile bending, and delamination after cutting or drilling. Because fibers are continuous along the profile length, axial strength and stiffness are high, whereas transverse, interlaminar, and joint-region properties are more sensitive. During subsequent cutting, drilling, adhesive bonding, riveting, or connection with metal nodes, hole-edge damage, interfacial debonding, and stress concentration must be controlled.
The advantage of pultruded profiles lies in axial tensile, compressive, and flexural stiffness, because continuous fibers are primarily aligned along the pulling direction. Transverse, interlaminar, hole-bearing, and joint performance are the weaker aspects. Minchenkov et al. [74] emphasized that high melt viscosity in thermoplastic pultrusion increases impregnation difficulty and that pulling speed, die temperature, fiber tension, and interfacial compatibility jointly determine voids and impregnation quality. Tipboonsri et al. [76] produced jute/glass-fiber hybrid PP by thermoplastic pultrusion and obtained a tensile modulus of 3.76 GPa, tensile strength of 118.13 MPa, flexural modulus of 5.51 GPa, and flexural strength of 69.27 MPa at 200 °C and 40 mm/min. Increasing pulling speed shortened impregnation time, increased voids and unimpregnated regions, and reduced mechanical performance. For higher-fiber-content unidirectional glass- or carbon-fiber thermoset pultruded profiles, axial strength can be much higher than that of this hybrid thermoplastic system, but transverse, interlaminar shear, and connection-region properties remain governed by resin impregnation, fiber waviness, voids, degree of cure, and drilling damage. Battery-pack beam design should therefore consider transverse compression, short-beam shear, bearing at connection holes, and post-impact residual performance, not axial tensile strength alone.
Pultruded profiles are suitable for battery-pack side frames, cross beams, longitudinal beams, crash beams, reinforcement beams, and local support structures. They are not suitable for forming a complete upper cover, tray, or complex curved shell alone. A more reasonable use is to combine pultruded profiles with SMC, RTM, thermoplastic sheets, aluminum frames, or metal joints so that beam load bearing and shell protection work together for lightweighting and crash safety.
Pultrusion is mature in construction, wind power, rail transportation, and industrial profiles, and it also has clear application potential in battery-pack beam structures. The key to industrialization is not profile manufacturing itself but rather the reliability of connections with housings, trays, sealing edges, mounting points, and metal nodes. Overall, pultrusion is a high-efficiency continuous-profile route for beam reinforcement, rather than an integrated forming route for complete battery-pack enclosures.
3.6. Multi-Material Joining, Inserts, and Sealing
Multi-material joining, inserts, and sealing are not a single composite-forming route but rather a system-integration link in composite battery-pack engineering. The objects include composite shells, metal frames, bolts, rivets, metal inserts, adhesive layers, sealants, thermal-management components, electrical connectors, and locally overmolded structures. Common methods include adhesive bonding, mechanical fastening, riveting, bolting, co-curing with metal inserts, insert embedding, thermoplastic welding, overmolding, and composite–metal hybrid structures [77,78,79].
The joining and sealing steps often determine whether composite battery-pack components can enter a stable assembly rhythm. Mechanical fastening and riveting are relatively fast single operations but may introduce drilling damage, hole-edge damage, and stress concentration. Adhesive bonding and sealing require surface treatment, adhesive-dispensing accuracy, curing-time control, and environmental control; their cycle is affected by adhesive curing and fixture holding. Rodrigues et al. [80] reviewed battery-pack manufacturing and disassembly and noted that some one-component polyurethane sealants curing by ambient moisture may require 2–30 days for full curing. By contrast, structural adhesives can form the initial load-bearing capacity needed for assembly within minutes under heat curing [81]. Therefore, the manufacturing cycle of composite battery-pack assemblies should not be evaluated only by the forming time of the main shell but should also include adhesive positioning, fixture occupation, heat curing, leak testing, and subsequent handling. Co-curing of inserts and over molding can reduce some post-assembly operations, but insert positioning accuracy, interfacial bonding quality, and thermal-expansion mismatch among materials must be controlled during the main forming stage.
Joining and sealing regions are failure-sensitive areas in composite battery-pack assemblies. Machining can cause delamination, burrs, fiber tearing, and hole-wall damage [82,83]. Stress concentration, interfacial debonding, and local cracking can occur around metal inserts because of differences in stiffness, coefficient of thermal expansion, and interfacial properties. Adhesive interfaces are affected by surface-treatment quality, adhesive-layer thickness, curing state, hygrothermal aging, and thermal cycling. Sealing grooves, flanges, and assembly surfaces are also highly sensitive to dimensional accuracy, flatness, and warpage; uneven seal compression may lead to interfacial leakage or long-term sealing failure.
The mechanical performance of joining and interface regions should be evaluated using joint-level indicators such as lap-shear strength, peel strength, mode I/II interfacial fracture toughness, bearing strength, and fatigue-retention rate, rather than the tensile strength of the composite plate alone. Rodrigues et al. [80] reported that SMP-type sealants used in battery packs have lap-shear strengths of about 1–2.5 MPa. ARALDITE 2019 A/B structural adhesive requires about 6 h at 23 °C to reach 10 MPa, whereas it takes about 10 min at 100 °C to reach the same strength level [81]. Loutas et al. [84] studied asymmetric titanium-CFRP bonded joints and showed that co-bonding, secondary bonding, composite matrix type, and manufacturing residual thermal stresses change mode I fracture toughness and failure path. Therefore, connection-region performance must be evaluated together with surface treatment, adhesive thickness, curing schedule, thermal-expansion mismatch, hygrothermal aging, and loading mode.
Multi-material joining, inserts, and sealing are involved in upper covers, lower housings, trays, side frames, cross beams, mounting brackets, lifting lugs, sealing flanges, thermal-management interfaces, and electrical-connection regions. For composite battery-pack assemblies, joining and sealing design should be brought forward to structural and forming-process design, rather than being treated as a post-forming assembly supplement. In large housings, metal-frame–composite hybrid trays, and repairable battery-pack structures, local reinforcement at joints, thickness transition, insert layout, and sealing-surface dimensional control should be designed together with the main forming process.
Adhesive bonding, mechanical fastening, metal inserts, and sealing processes are themselves mature in automotive engineering. However, once they are coupled with the large size, flame retardancy, insulation, thermal-runaway protection, and long-term durability requirements of composite battery-pack enclosures, component- and system-level validation remains necessary. This link can be regarded as a determinant of engineering-transition maturity, because it governs the reliable conversion from single-part forming to multi-material integrated manufacturing.
3.7. Multi-Route Comparison and Selection Recommendations
Based on the six dimensions discussed above, the positions of different forming routes in electric-vehicle battery packs are summarized in Table 2. From the boundary of pack-level lightweighting, public industry information indicates that a typical electric-vehicle battery pack weighs about 500 kg, of which the enclosure material accounts for about 100 kg; approximately 80% of current battery-pack enclosures use aluminum, and the remainder mainly use steel [85]. Therefore, the value of composite forming should not be vaguely described as “metal replacement” but rather should be focused on quantifiable mass reduction and functional integration in upper covers, lower housings, underbody shields, side-frame beams, local tray reinforcements, and sealing/joining regions. Overall, SMC and LFT-D/GMT emphasize high throughput and functional integration, but their performance is strongly affected by short- or long-fiber orientation. PCM/WCM and RTM/HP-RTM emphasize continuous-fiber load bearing and lay-up design but require control over interlaminar properties and voids. VARTM is suitable for large prototypes, low- to medium-volume manufacturing, and sandwich protective-structure validation. Pultruded profiles are suitable for axially loaded side frames and beams. Multi-material joining, inserts, and sealing should be evaluated primarily by joint and interface properties.
Table 2.
Six-dimensional comparison of mainstream composite-forming routes for electric-vehicle battery packs. (a) Material form, cycle, and dominant defects. (b) Mechanical-performance features, applicable components, and engineering maturity.
Zhang et al. [86] summarized battery-pack lightweighting studies and reported that an AAHP/CFRP hybrid battery-pack enclosure could achieve about 12.3% mass reduction relative to an aluminum-alloy structure; a CFRP solution could reduce mass by about 35.7% compared with an Al7075-T4 aluminum-alloy structure; and a GFRP hybrid structure could reduce mass by about 23.9% and cost by about 38.6% compared with a conventional battery-pack enclosure. These results indicate that the engineering value of composites must be evaluated together with crash/vibration response, thermal-runaway protection, sealing durability, and manufacturing cost. For upper covers and protective covers, SMC, LFT-D/GMT, or continuous-fiber thermoplastic sheets can be considered first, but mold flow orientation, impact resistance, and sealing-edge stiffness should be checked. For underbody shields and thermal-runaway isolation parts, PCM/WCM, thermoplastic sheets, or VARTM sandwich structures can be used, with emphasis on bending, low-velocity impact, interlaminar toughness, and residual load capacity after impact. For lower housings, trays, and beams, RTM/HP-RTM, continuous-fiber compression molding, pultruded profiles, or composite–metal hybrid structures are more suitable, and design should distinguish the principal load direction, transverse direction, and connection nodes. For joining, mounting, and sealing regions, lap shear, peel, bearing, interfacial fatigue, and aging retention should be treated as indicators as important as the main forming process.
Representative industrial cases also indicate that scaled application is currently most realistic in function-integrated covers, protective shells, and hybrid structures rather than in all-composite full trays. Teijin Automotive Technologies reported a multi-material composite battery-pack enclosure with integrated composite cover and tray plus aluminum/steel reinforcements [45]. Huntsman lists HP-RTM battery enclosures as a high-productivity application route [57]. Trinseo reported thermoplastic battery-enclosure concepts combining mass reduction, lower carbon footprint, and thermal-runaway testing [70]. Industrial pultrusion lines further show that continuous profiles are mature for long beams and frames, but their battery-pack value depends on integration with shells, nodes, and sealing interfaces [72]. These cases support a staged engineering pathway from low-risk protective components to semi-load-bearing and hybrid load-bearing structures.
To strengthen the cross-process comparison, the qualitative dimensions in Table 2 were further organized into a semi-quantitative MCDM-oriented screening matrix, as shown in Table 3. The scores in this matrix are unweighted, literature-based screening scores derived from the process characteristics, mechanical-performance ranges, cost information, defect tendencies, recyclability, and maturity evidence discussed in Section 3. This matrix does not provide an absolute MCDM ranking and does not replace component-level testing. Instead, it is intended to identify the dominant trade-offs among mechanical performance, cycle efficiency, cost, defect controllability, recyclability, and engineering maturity for early-stage process selection.
Table 3.
Semi-quantitative MCDM-oriented screening matrix of representative composite-forming routes for battery-pack structures.
The semi-quantitative comparison has several uncertainties. The cited data come from different fiber types, resin matrices, fiber volume fractions, specimen geometries, test standards, and process windows. Cost and cycle-time values are also sensitive to automation level, tooling amortization, part size, inspection rhythm, scrap rate, and joining/sealing operations. Therefore, Table 3 should be used as an early-stage decision tool, whereas final process selection still requires component-level trials and system-level validation.
Overall, the differences among forming routes are reflected not only in cycle time, component size, and mechanical performance but also in defect types and sensitive regions. SMC and LFT-D/GMT are more susceptible to flow-induced fiber orientation, resin-rich regions, weld lines, and fiber-length retention. PCM/WCM requires attention to ply wrinkles, bridging, voids, and interlaminar properties. RTM/HP-RTM and VARTM are mainly governed by flow-front behavior, insufficient impregnation, dry spots, and voids. Pultruded profiles require control over fiber continuity, section stability, and connection-interface reliability. Future progress will therefore depend on matching material form, forming cycle, defect control, representative mechanical behavior, component function, and engineering maturity within a closed evidence chain that includes material systems, process windows, defect detection, mechanical characterization, joining and sealing, component-level testing, and certification.
4. Typical Defects, Formation Mechanisms, and Prevention Measures
Composite battery-pack parts experience resin flow, fiber deformation, interfacial bonding, curing shrinkage, and post-forming assembly simultaneously. Defects are, therefore, not isolated phenomena caused by a single process parameter but rather the result of interactions among the material system, forming route, mold constraint, and component geometry. The process comparison above shows that different routes differ in terms of fiber volume fraction, porosity control, forming pressure, lay-up stability, and component-size adaptability. These differences are further transformed into typical defects such as voids, dry spots, resin-rich regions, delamination, warpage, and fiber waviness. For battery-pack upper covers, underbody shields, module boxes, and local reinforcements, these defects affect not only appearance but also load bearing, sealing, thermal protection, insulation, and long-term durability. This section therefore summarizes defects from the perspective of “defect type-process source-representative morphology-performance effect-detection method-control measure”.
Based on the process comparison above, the typical defects in composite battery-pack structures can be summarized according to their process origins, performance consequences, detection methods, and control priorities. Table 4 provides a consolidated defect-control map for linking defect morphology with process source and component-level risk.
Table 4.
Typical forming defects in composite battery-pack parts and their effects, detection methods, and control measures.
This mapping emphasizes that defect evaluation should not rely only on defect morphology itself but should also consider the functional region in which the defect occurs. For example, voids in beam and load-bearing regions should be assessed with interlaminar strength and fatigue criteria; dry spots in flame-retardant or insulating layers should be evaluated in terms of functional continuity; and delamination around mounting holes or sealing interfaces should be judged together with residual strength, sealing reliability, and vibration durability.
4.1. Voids
Voids are among the most common and influential internal defects in composite forming. In composite battery-pack parts, voids may appear as isolated bubbles in the matrix, inter-tow voids, intra-tow micropores, or interlaminar voids. Binetruy et al. [87] argued that voids in RTM mainly originate from two mechanisms. First, geometric nonuniformity or permeability variation in fiber bundles distorts the resin front, and local air surrounded by resin forms elongated or pocket-shaped voids. Second, when multiple microscopic impregnation fronts inside fiber bundles converge, residual air trapped between them forms bubbles. Air entrained during resin mixing, volatile or moisture release, insufficient vacuum degassing, flow-front air entrapment, gas release induced by cure exotherm, and unreasonable mold venting may further induce voids. Figure 12 shows optical micrographs of different void morphologies.
Figure 12.
Optical micrographs of different void morphologies, including (a) irregular elongated voids, (b) circular voids, and (c) larger voids [88].
The dominant factors for void formation differ among processes. In RTM/HP-RTM and VARTM, voids are commonly related to resin viscosity, injection or infusion velocity, pressure gradient, capillary impregnation, and preform permeability. When the flow front is unstable, local pressure is insufficient, or intra-tow and inter-tow impregnation rates are mismatched, inter-tow voids or intra-tow micropores are likely to form [89]. In SMC, LFT-D, and GMT compression molding, voids are more often associated with initial air in the charge, insufficient molding pressure, blocked local flow, poor venting, and filler or chopped-fiber agglomeration. These factors make it difficult for gas to escape during compaction and curing, leaving residual voids in the matrix or interface.
The effect of voids depends strongly on material system and loading direction. Protz et al. [90] showed that, for glass-fiber non-crimp-fabric/epoxy composites with void contents of 0.02–4.53%, voids had no significant effect on quasi-static tensile modulus, failure strain, or tensile strength in the fiber-dominated direction. However, stiffness reduction was more easily observed in directions where the matrix contribution was more pronounced and fiber content was lower. Increasing void content also increased the scatter in modulus, strength, failure strain, and fatigue life. Chen et al. [88] further investigated HP-RTM CFRP parts and found that most voids were smaller than 50 µm and that increasing the resin-injection flow rate markedly increased the number of voids. When the void content increased by about 0.5%, flexural strength decreased by about 8%. As shown in Figure 13, flexural strength generally decreased with increasing void content, whereas flexural modulus changed much less, which indicates that voids tend to affect strength-related indices more strongly than stiffness-related indices. Therefore, void evaluation for battery-pack parts should consider not only average porosity but also void location, size, connectivity, and local clustering.
Figure 13.
Effect of void content on flexural properties of HP-RTM-molded CFRP: (a) flexural strength; (b) flexural modulus [88].
Void control should cover material preparation, mold design, processing, and post-cure evaluation. Liquid molding should focus on resin degassing, vacuum level, injection pressure, flow path, and venting. VARTM should ensure reliable vacuum-bag sealing and match gel time with filling time. HP-RTM can use pressure sensors, in-line flow monitoring, and filling simulation to identify regions where air may become trapped. SMC and LFT-D should optimize charge placement, closing speed, compression pressure, and venting sequence. In detection, ultrasonic testing, X-ray CT, infrared thermography, and acoustic emission can identify voids at different scales. CT is suitable for three-dimensional quantitative characterization, ultrasonic testing for rapid screening, and infrared thermography and acoustic emission for thermal-response anomalies and damage evolution under loading [91].
4.2. Dry Spots, Insufficient Impregnation, and Resin/Filler Nonuniformity
Dry spots, insufficient impregnation, resin-rich/resin-poor regions, and filler nonuniformity are all material-distribution defects, but they differ in terms of formation scale and control priority. Dry spots and insufficient impregnation mainly reflect incomplete filling and wetting of fiber preforms by resin and are common in RTM/HP-RTM and VARTM. Resin-rich, resin-poor, and filler-agglomerated regions reflect local imbalance among resin, fibers, and functional fillers, and may also occur in SMC, prepreg compression molding, and filler-modified functional systems. This section therefore discusses them as two groups: flow/impregnation deficiency and constituent-distribution nonuniformity.
In liquid molding, preform-permeability variation, resin viscosity and gel time, injection pressure, gate/vent layout, and sudden changes in component geometry all alter the flow front. For battery-pack upper covers, underbody shields, and ribbed trays, ribs, sharp corners, thickness transitions, cores, and metal inserts may cause local insufficient compaction or fiber bridging. When low-flow-resistance channels form between the preform and mold edge, inserts, or reinforcement ribs, resin advances rapidly along the edge or gap. The main flow front is bypassed, split, or closed prematurely, generating a sealed, unimpregnated region, namely race-tracking-induced dry-spot risk [58,92].
Dry spots and insufficient impregnation weaken fiber–resin interfacial load transfer, causing stress concentration, matrix damage, and premature failure near the defect. Li et al. [93] used resin-missing regions in carbon-fiber/epoxy laminates as controlled representations of insufficient impregnation and resin-poor defects, preparing specimens with resin-missing defect contents of 5.3%, 8.0%, 10.7%, 13.3%, and 16.7%. The results showed that resin-missing defects changed the stress distribution and reduced tensile strength: the defect-free specimens had a tensile strength of about 1615.01 MPa, whereas defective specimens decreased to about 1570.46–1384.72 MPa, with a maximum reduction of about 14.26%. The maximum prediction error of the numerical model was 3.06%. These results indicate that defect evaluation should consider not only defect area but also defect location, morphology, and relationship to the main load path.
Resin-rich and resin-poor regions represent constituent-distribution nonuniformity. Resin-rich regions reduce local fiber volume fraction, lowering stiffness and strength and possibly inducing microcracks because of cure-shrinkage mismatch. Resin-poor regions can cause incomplete impregnation, poor interfacial bonding, and increased porosity. Pang et al. [94] simulated transverse pure shear in resin-rich regions of unidirectional CFRP and found that resin-rich regions reduced the maximum model load and accelerated failure. Figure 14 further shows typical resin-rich morphologies in carbon-fiber composites, including interlaminar, inter-tow, and stitched-fabric regions.
Figure 14.
Resin-rich defects and their distribution in different fabric structures and stitching regions: (a) local resin-rich defect morphology [95]; (b,c) resin-rich morphologies in fabric and stitching regions [96].
As illustrated in Figure 14, resin-rich regions are not caused only by excessive resin content; they are closely related to fiber-bundle arrangement, textile architecture, local compaction, and resin flow path. Stelzer et al. [97] observed process-related voids and resin-rich regions in discontinuous-carbon-fiber compression-molded composite components and showed that local material distribution and defect state affect failure mode. In flame-retardant, thermally conductive, or electromagnetic-shielding filler systems for battery packs, nonuniform filler dispersion, sedimentation, migration, or filtration may cause filler agglomeration or filler-poor regions. These regions can lead to material embrittlement, discontinuous conductive pathways, nonuniform heat conduction, fluctuations in flame retardancy, and processing difficulty.
Reducing dry-spot and insufficient-impregnation risk requires coordinated consideration of material rheology, preform structure, mold flow channels, and process monitoring. Preform design should reduce excessive local compaction, fiber bridging, and thickness jumps. Gate and vent positions should be optimized through flow simulation to avoid premature resin arrival at vents or the formation of closed unimpregnated regions. The Monte Carlo analysis of Agogué et al. [58] showed that proper vent placement helps reduce race-tracking-induced dry spots and can guide online sensor placement. Chai et al. [98] proposed an injection-configuration optimization framework for RTM, demonstrating that simulation-driven gate design can improve filling efficiency and product quality.
For systems containing functional fillers such as flame retardants, filler content, dispersion state, resin viscosity, and processability must be evaluated together. Pérez-de-Eulate et al. [99] studied glass-fiber-reinforced thermoset composites containing aluminum hydroxide flame-retardant fillers and evaluated the relationships among additive proportion, matrix-viscosity evolution, processability, and flame retardancy. Shi et al. [17] further showed that flame-retardant modification of fiber-reinforced polymer composites must be matched with flame-retardant effect, material system, and application requirements. Therefore, functional filler systems for battery packs should not be evaluated only by a single flame-retardant, thermal-conductive, or electrical-conductive index; rheology, forming window, and component-level performance validation are also necessary.
4.3. Delamination, Interfacial Debonding, and Adhesive Failure
Delamination, interfacial debonding, and adhesive failure are interface-related defects that must be controlled in composite battery-pack structures. They correspond respectively to separation between adjacent plies in a laminate, interfacial failure between composites and metal inserts or functional layers, and interfacial or cohesive failure in bonded joints. The load-bearing capacity of an adhesive joint is not governed by a single parameter but rather by joint geometry, adhesive properties, substrate characteristics, surface treatment, manufacturing process, environmental exposure, and the damage-detection method [77].
Interface defects formed during processing are commonly related to insufficient impregnation, voids, insufficient curing pressure, resin shrinkage, unsymmetric lay-up, and thermal-expansion mismatch. In multi-material battery-pack structures, composite–metal inserts, load-bearing layers-thermal-barrier layers, housing-sealant interfaces, and bonded flanges can all become failure-sensitive regions. Local thickness changes, stiffness discontinuities, and free edges amplify peel and shear stresses. During service, crash impact, road vibration, and thermal cycling may cause initial microdefects to develop into detectable delamination or debonding. Because the dominant failure mode differs among structures and material systems, battery-pack applications should identify critical interfaces through component-level testing rather than directly applying conclusions from single-material coupons.
Post-processing operations such as drilling, cutting, and trimming introduce additional interlaminar-damage risks. Xu et al. [100] reviewed CFRP drilling and identified common damage forms, including delamination, burrs, fiber tearing, surface cavities, and thermal damage. Damage formation is affected by lay-up configuration, feed rate, cutting speed, tool geometry and material, machining environment, and processing strategy. Figure 15 shows cutting morphologies formed by different drill bits in fiber composites. For battery-pack mounting holes, bolted connections, and service ports, hole-edge delamination not only reduces local load-bearing capacity but can also couple with assembly preload and vibration loads, promoting damage growth.
Figure 15.
Cutting morphologies of fiber composites produced by different drill bits [100].
Long-term reliability of bonded and sealed regions is strongly affected by temperature, humidity, loading, and salt environment. Qin et al. [101] studied the effects of temperature, humidity, load, and their combinations on aging failure of automotive CFRP/aluminum-alloy bonded joints and showed that service environment and load jointly change the aging degree of the adhesive and CFRP. Vigón et al. [102] compared the effects of hygrothermal and salt environments on mode I delamination behavior of carbon-fiber/epoxy bonded joints. Epoxy adhesive joints exhibited significant loss of delamination resistance after salt exposure, whereas acrylic adhesive joints were less affected. Vigón et al. [103] further studied mode II static and fatigue delamination after 1, 2, 4, and 12 weeks of salt exposure and found that the fracture energy corresponding to infinite fatigue life was about 20% of the static loading capacity. These results show that battery-pack bonding and sealing design cannot rely only on room-temperature static strength; residual performance under hygrothermal, salt-spray, thermal-cycling, and fatigue-coupled conditions must also be considered.
Interface-failure control requires coordinated material, structural, and process design. Before bonding, substrate cleanliness, surface morphology, and wettability should be controlled. Liu et al. [104] reviewed surface-treatment methods and showed that surface treatment can remove CFRP surface contaminants, improve adhesive spreading, and enhance bonding through mechanical interlocking, adsorption, or chemical bonding. Chen et al. [105] found that the failure strength of CFRP/aluminum-alloy single-lap joints decreased with hygrothermal aging time, while sealing treatment clearly slowed strength degradation. For safety-sensitive regions such as sealing flanges, mounting holes, and thermal-protection layers, a graded system linking interface position, potential defect, detection method, service condition, and acceptance criterion should be established.
4.4. Warpage, Deformation, and Residual Stress
Warpage, spring-in, angular deviation, and dimensional drift are common process-induced deformations in composite parts. Their direct origin is the redistribution of residual stress after demolding. In thermoset composites, curing reactions involve chemical shrinkage, modulus evolution, and thermal-expansion mismatch. Tool-part interaction, lay-up structure, temperature gradients, compaction, and demolding constraints also affect final shape. Wang et al. [106] noted that cure-induced deformation in thermoset composites has pronounced thermal-chemical-mechanical coupling, which can reduce assembly accuracy and shorten service life. Hwang [107] summarized the factors affecting plate warpage and spring-in/spring-back in angular parts, including part angle, thickness, lay-up sequence, corner radius, flange size, tool material, tool surface, and curing schedule.
For electric-vehicle battery packs, dimensional stability is not a mere appearance issue. If warpage or local deformation occurs around enclosure sealing flanges, mounting holes, module-positioning surfaces, bolted joints, or metal inserts, assembly interference, hole misalignment, uneven sealant compression, and abnormal preload distribution can result. Hwang [107] pointed out that shape deviation causes assembly mismatch, and forced assembly may further increase internal residual stress. Al-Tameemi et al. [108] investigated L-shaped composite specimens experimentally and numerically, showing that lay-up, thickness, tool material, and curing cycle all affect spring-in deformation, and accurate prediction requires consideration of tool contact boundary conditions.
Although thermoplastic composites do not undergo thermoset crosslinking, rapid heating and cooling can also introduce residual stress. Parambil et al. [109] developed and validated a residual-stress evolution model for a semicrystalline polypropylene-based single-fiber model composite under non-isothermal cooling, showing that cooling rate, crystallization-related shrinkage, and temperature-dependent matrix modulus must be included. For thermoplastic battery-pack components, rapid forming improves throughput, but through-thickness temperature gradients and cooling-rate differences may increase warpage risk and complicate assembly and joining.
Flow compression systems such as SMC and LFT-D also require attention to anisotropic shrinkage caused by fiber orientation. During mold filling, charge position, flow distance, local thickness, and rib geometry change local fiber orientation and material distribution. Because fiber orientation influences anisotropic shrinkage and local mechanical response, fiber orientation, shrinkage, and deformation should be measured jointly rather than represented only by empirical coefficients. Public component-level quantitative data for warpage in SMC/LFT-D battery-pack enclosures remain limited, making this a priority for future experimental and simulation validation.
Residual-stress and deformation control should be developed from material, structural, mold, and process levels. At the material level, curing kinetics, chemical shrinkage, viscoelasticity, coefficient of thermal expansion, and thermoplastic crystallization should be characterized. Structurally, symmetric and balanced lay-ups should be prioritized, with reduced stiffness discontinuities and unnecessary thickness jumps. At the mold level, temperature uniformity and tool-part contact/thermal-expansion mismatch should be evaluated. At the process level, heating rate, holding time, cooling curve, holding pressure, and demolding temperature should be optimized. Barcenas et al. [110] showed that cure-degree gradients generated during filling significantly affect final part shape and that thermo-viscoelastic models can more accurately predict deformation of thermoset liquid-molded parts. Cameron et al. [111] and Zhang et al. [112] further demonstrated that forming simulation can predict temperature field, degree of cure, residual stress, and deformation trends, supporting lay-up adjustment, process-window design, and tool compensation.
4.5. Fiber-Orientation Deviation, Fiber Waviness, and Fiber Breakage
Fiber-orientation deviation, fiber waviness, and fiber breakage are common reinforcement-phase defects in composite forming. They correspond to fibers deviating from the designed direction, continuous fibers or fiber bundles forming local undulations, and loss of reinforcement continuity, respectively. Fu and Yao [24] noted that fiber waviness, wrinkles, and orientation deviation affect flexural and compressive performance and that orientation deviation may significantly reduce structural modulus, strength, and stability. Maes et al. [113] further argued that composite quality evaluation should record not only whether a defect exists but also its position, size, distribution, and relationship with geometry and process parameters so that the information can support virtual validation and component certification.
Waviness in continuous-fiber composites is usually associated with lay-up, preforming, compaction, and adaptation to complex geometries. In curved surfaces, corners, thickness transitions, and deep-cavity structures, in-plane shear, interlaminar sliding, and local compression may lead to wrinkling or bridging. Shen et al. [114] proposed a surface-waviness-based method for wrinkle morphology characterization and found that surface fiber direction and through-thickness stitching changed wrinkle amplitude and curvature. In particular, a multilayer preform with +/−45 deg surface plies reduced the average wrinkle amplitude by 44% and the average wrinkle curvature by 79%. Codolini et al. [115] studied wrinkle variability in the double-diaphragm forming of non-crimp fabrics and showed that vacuum pressure, diaphragm tension, ply-tool alignment, and inter-ply friction affect forming quality. Figure 16 shows wrinkle morphologies.
Figure 16.
Wrinkle morphologies in double-diaphragm forming of non-crimp fabrics [115].
Waviness not only changes local geometry but also causes stress concentration and failure-mode transition. Chen et al. [116] performed compression, out-of-plane shear tests, and finite-element analysis on T700/7901 CFRP cross-ply laminates containing different levels of out-of-plane waviness. A hybrid “gap plus transverse strip” method was used to manufacture controllable sinusoidal waviness, and waviness angle was used to represent defect severity. The results showed that the waviness region significantly reduced compressive load-bearing capacity and intensified delamination growth during compressive failure. Under the most severe waviness condition, compressive strength decreased by up to 26.9%, whereas interlaminar shear strength decreased by up to 2.8%. The study also indicated that failure strain was more sensitive to waviness angle than compressive strength and that out-of-plane waviness had a relatively small effect on interlaminar shear strength but changed the location and severity of delamination failure. Fu and Yao [24] further summarized the fatigue-failure process of composites containing fiber waviness, showing that waviness regions often become initiation sites for crack nucleation, damage growth, and final failure, as shown in Figure 17. Therefore, in upper covers, underbody shields, and reinforcement plates, waviness risk should be evaluated preferentially in regions with large curvature variation, local thickening, flange transitions, and concentrated load transfer.
Figure 17.
Fatigue-failure process of composites with fiber-waviness defects [24].
For discontinuous-fiber materials such as SMC, BMC, GMT, and LFT-D, orientation deviation more often appears as flow-induced local anisotropy. Charge position, filling path, flow distance, cavity geometry, local thickness, and ribs jointly affect fiber-orientation distribution. Romanenko et al. [38] established a three-dimensional virtual process chain for C-SMC in automotive mass production, enabling the prediction of local fiber orientation, mechanical performance, flow front, weld lines, and warpage from flow characterization and numerical simulation. Scheuring et al. [117] used micro-CT, experiments, and homogenization modeling to verify the orientation dependence of long-fiber-reinforced thermoplastic composites produced by compression molding. These studies demonstrate that discontinuous-fiber parts cannot be evaluated using a single isotropic material parameter.
Fiber breakage mechanisms must be distinguished by forming route. In continuous-fiber preforming, sharp corners, deep cavities, and excessive stretching may damage bundle integrity. In long-fiber thermoplastic processes, compounding, conveying, and filling may cause fiber-length loss. Around battery-pack connection holes, metal inserts, and local load paths, fiber breakage or interruption of continuity can increase stress concentration. Direct quantitative evidence for battery-pack components since 2022 remains limited, so this review treats fiber breakage as a key validation risk rather than generalizing a specific strength-reduction ratio.
Controlling these defects requires integrated material design, preforming, mold design, and simulation evaluation. Continuous-fiber parts should optimize lay-up path, stacking sequence, transition radius, and local constraints to reduce bridging and waviness. Trenam et al. [118] proposed an analytical wrinkle-prediction model for double-diaphragm forming, which can rapidly evaluate formability and screen wrinkle-free solutions during design. Discontinuous-fiber compression-molded parts should optimize charge size, position, flow distance, and forming parameters and should map local orientation fields from process simulation into structural simulation. In critical regions, microscopy, micro-CT, ultrasonic testing, and surface-profile measurement can be combined to establish a closed relationship among process parameters, defect morphology, local orientation, and component performance.
In summary, defect control for composite battery-pack parts should move beyond a qualitative judgment of whether defects exist. It should specify defect type, spatial location, scale, forming route, and performance sensitivity. Voids and dry spots primarily reflect impregnation and venting quality. Delamination and adhesive failure reflect interface and post-processing reliability. Warpage and residual stress affect assembly and sealing. Fiber-orientation deviation, waviness, and breakage determine whether local load paths deviate from design. Because forming defects are process-dependent, region-sensitive, and performance-coupled, post-forming defect identification alone is insufficient. Materials input, process parameters, mold design, in-line monitoring, non-destructive testing, and defect tolerance must be connected into a whole-process quality-control system. The next section therefore discusses quality control, defect detection, and engineering evaluation methods for composite battery-pack manufacturing.
5. Manufacturing Quality Control, Defect Detection, and Process Optimization
The preceding sections summarized the formation mechanisms, performance effects, and control logic of typical defects in composite battery-pack parts. For automotive mass-production components, defect control cannot remain a single isolated process measure. It should cover material input, process parameters, mold and flow-channel design, in-line monitoring, post-forming inspection, and defect-tolerance evaluation. Only by connecting process data, defect-detection results, and component service requirements can a traceable and verifiable closed loop for manufacturing quality be established. Table 5 summarizes such a closed-loop quality-control framework.
Table 5.
Closed-loop quality-control framework for composite battery-pack manufacturing.
As summarized in Table 5, quality control for composite-material battery-pack structures is a chain process. Material input governs resin flow, fiber distribution, and functional-filler stability. Process parameters and mold flow channels directly affect filling, impregnation, curing, and residual stress. In-line monitoring identifies process anomalies during forming. Post-forming inspection confirms hidden defects such as voids, delamination, waviness, and dimensional deviation. Defect tolerance links inspection results with component-level safety requirements. Based on this logic, this section discusses material-side control, process and mold control, in-line monitoring, non-destructive testing, and defect tolerance.
5.1. Material-Side Quality Control
Defect control begins with the material side. Resin systems should have viscosity, gel time, curing exotherm, shrinkage behavior, and compatibility with flame-retardant, thermally conductive, or electromagnetic-shielding fillers appropriate for the target process. Fiber reinforcements should be controlled in areal density, moisture content, lay-up form, surface treatment, and preform stability. Intermediate materials such as SMC, BMC, LFT, and GMT should also be evaluated in terms of maturation degree, fiber-length distribution, volatile content, storage conditions, and batch consistency. Variability in material input directly changes the filling, impregnation, compaction, curing, and cooling windows. Accordingly, incoming inspection, rheological characterization, thermal analysis, dielectric curing monitoring, small-sample molding trials, and batch traceability should be established in mass production.
The goal of material-side quality control is not to maximize a single property but rather to ensure that material batches remain within the manufacturable window. Excessive resin viscosity increases the risk of insufficient impregnation and dry spots. Too short a gel time narrows the infusion window. High moisture or volatile content increases void risk. Filler agglomeration causes local embrittlement and fluctuation in flame-retardant, electromagnetic-shielding, or thermal-conductive properties. Hall et al. [119] studied the effect of through-thickness dielectric sensors on the curing monitoring of carbon-fiber/epoxy composites, showing that dielectric monitoring can track cure evolution, while sensor structure-material system interactions must also be evaluated.
5.2. Process Parameters and Mold Design
Process parameters are direct control factors for defect formation. For RTM/HP-RTM, injection pressure, resin temperature, mold temperature, vacuum level, preform compaction, and gate/vent positions should be controlled. For VARTM, flow media, vacuum-bag sealing, resin gel time, and infusion path are critical. For SMC/LFT-D, charge size, charge position, compression speed, pressure, temperature, and holding time should be controlled. For PCM/WCM, lay-up quality, heating rate, holding time, compaction state, and demolding temperature should be controlled.
Mold design is equally important for defect control. Complex ribs, thickness transitions, sharp corners, inserts, and sealing grooves are prone to dead flow zones, trapped-air zones, and stress concentrations. Agogué et al. [58] analyzed the influence of race tracking on dry-spot formation in RTM using Monte Carlo simulation, showing that the positions of vents, injection gates, and high-permeability channels significantly affect defect risk. Chai et al. [98] proposed a radial injection-configuration optimization framework for RTM, further indicating that gate layout should not rely solely on experience but should also be determined through filling simulation and optimization algorithms. Peng et al. [120] proposed ultrasonic-vibration-assisted RTM to suppress void formation in CFRP laminates, demonstrating that external-field assistance and process-window control can serve as defect-control measures, although their applicability must be evaluated with respect to component scale, resin system, and equipment complexity.
5.3. In-Line Monitoring and Digital Quality Traceability
Traditional quality control relies on post-forming inspection, but for automotive mass production, after-the-fact inspection cannot fully meet the requirements for high throughput, low scrap rate, and full-process traceability. In-line monitoring can collect temperature, pressure, resin flow-front, degree-of-cure, dielectric, acoustic, and mold-displacement data during forming to judge filling state, cure progress, and defect risk. RTM and HP-RTM can use pressure, temperature, dielectric, piezoelectric, or fiber-optic sensors to monitor resin flow and curing. SMC and LFT-D can monitor cavity pressure, mold temperature, and closing displacement. Prepreg and hot-press forming can monitor curing through temperature fields, dielectric analysis, and in-mold pressure. Yu et al. [121] constructed a piezoelectric–fiber-optic hybrid sensor network combining the area-monitoring capability of PZT sensors and point measurement of FBG optical fibers to identify the three-dimensional resin flow front in liquid composite molding, as shown in Figure 18. This work suggests that multisensor fusion can overcome the limitation of single sensors that provide only local information or cannot identify internal flow fronts, providing a reference for filling-state judgment, abnormal flow recognition, and process traceability in large battery-pack composite parts.
Figure 18.
Piezoelectric–fiber-optic hybrid sensor network for monitoring the three-dimensional resin flow front [121].
The key to in-line monitoring is not only data acquisition but also converting sensor signals into production decisions. Pressure, temperature, dielectric, acoustic, piezoelectric, and fiber-optic signals should be linked with filling and curing models to identify abnormal flow, estimate process state, and record traceable quality data. Studies combining pressure sensing with flow prediction, neural networks, or surrogate models for RTM show that sensor-model coupling can accelerate online state estimation [122,123,124]. For large composite battery-pack components, these monitoring data provide the input basis for subsequent non-destructive testing, component-level validation, and the digital-twin-based closed-loop manufacturing discussed in Section 6.
5.4. Non-Destructive Testing and Defect Evaluation
Post-forming non-destructive testing is essential for the quality assurance of composite-material battery-pack structures. Because defects such as voids, delamination, interfacial debonding, fiber waviness, and local deformation differ in terms of size, location, and accessibility, detection methods differ in terms of penetration depth, spatial resolution, inspection efficiency, and production-line adaptability. Before selecting inspection methods, non-destructive evaluation approaches should, therefore, be classified. Mortada et al. [125] categorized composite non-destructive evaluation methods into contact and non-contact types and summarized typical methods including ultrasonic testing, infrared thermography, shearography, and X-ray CT, as shown in Figure 19.
Figure 19.
Classification of contact and non-contact non-destructive testing methods for composites [125].
As summarized in Figure 19, there is no universal inspection method for all composite defects. Ultrasonic testing is suitable for detecting delamination, voids, and interfacial debonding. X-ray CT can visualize internal voids, fiber waviness, and complex three-dimensional defects, but its cost, specimen size, and inspection cycle are limited. Infrared thermography is suitable for rapid detection of near-surface defects, debonding, and heat-diffusion anomalies. Acoustic emission can monitor damage during loading. Shearography is suitable for detecting debonding and local deformation anomalies, and DIC can measure surface strain fields under load. Chen et al. [91] reviewed the applicability of multiple non-destructive methods for defect detection in fiber-reinforced polymer composites. Mortada et al. [125] further noted that non-contact ultrasonic testing can reduce the limitations imposed by couplant and contact state and may improve inspection adaptability for complex parts and automated lines.
For battery-pack composites, the relationship “defect type-detection method-performance effect-acceptance criterion” should be established instead of simply increasing the number of inspection methods. Huang et al. [126] used ultrasonic thermography to detect and quantify artificial delamination in CFRP, showing that active thermography can identify near-surface delamination and estimate defect size. Marani and Campos-Delgado [127] combined long-pulse thermography with blind linear unmixing for defect-depth classification in composites, indicating that data processing strongly influences defect-recognition capability. These studies suggest that micropores near sealing surfaces, fiber waviness in load-bearing beams, dry spots in flame-retardant layers, and debonding around inserts have different safety meanings and acceptance criteria.
5.5. Defect Tolerance and Battery-Pack Safety Performance
The final goal of defect control is battery-pack system safety, not a theoretical zero-defect condition. Because completely defect-free composite manufacturing is nearly impossible, engineering practice should focus on understanding how defects affect service performance and on establishing tolerance criteria. Voids mainly affect interlaminar properties, fatigue, and moisture absorption. Dry spots affect local strength and functional continuity. Delamination affects residual strength and structural integrity after impact. Warpage affects assembly and sealing. Fiber-orientation deviation affects stiffness, strength, and crash energy absorption. Filler agglomeration affects flame retardancy, electromagnetic shielding, and mechanical uniformity. Eliasson et al. [128,129] used probabilistic frameworks and two-scale modeling to study the effect of manufacturing defects on fatigue in cross-ply carbon-fiber laminates, indicating that defect-tolerance evaluation must consider material scatter, defect distribution, and load history rather than relying only on deterministic strength values.
Quality evaluation for composite-material battery-pack structures should therefore extend from material coupons to component and system levels. Structural parts should be evaluated for static strength, bending, impact, vibration fatigue, and performance after environmental aging. Flame-retardant and thermal-insulation parts should be evaluated with respect to fire exposure, thermal-runaway simulation, or high-temperature insulation testing. Sealing structures should undergo air-tightness, water-tightness, thermal-cycling, and vibration-coupled tests. Joining structures should be evaluated for pull-off, shear, fatigue, and corrosion-aging performance. Region-based quality control is recommended: sealing flanges, mounting holes, inserts, load-bearing beams, and thermal-runaway protection layers should have stricter sampling and tolerance requirements, whereas non-load-bearing covers and protective shields may use differentiated criteria according to functional requirements.
As battery-pack components become larger, structurally more complex, and produced at faster cycles, relying only on empirical parameter adjustment and post-forming inspection cannot ensure stable manufacturing. Quality control should be further combined with flow simulation, curing/cooling deformation prediction, fiber-orientation mapping, machine learning, and digital twins so that defect risks can be predicted in advance and process optimization can become a closed-loop process.
6. Process Simulation, Data Fusion, and Digital-Twin Manufacturing
The preceding sections show that the manufacturing quality of composite battery-pack components is not determined by a single parameter but rather by material rheology, preform permeability, mold temperature, injection/compaction pressure, curing or cooling history, fiber orientation, and subsequent assembly constraints. For safety-related components such as upper covers, underbody shields, trays, beams, and joining/sealing regions, the core value of digital manufacturing should not remain in offline simulation or three-dimensional visualization. Instead, it should support process-window definition, defect-risk prediction, component-performance mapping, in-line quality judgment, and full-process traceability. Based on this logic, this chapter integrates process simulation, in-line monitoring, machine learning, and digital twins into a closed-loop framework of “model prediction-sensor updating-quality judgment-feedback optimization”, as summarized in Table 6.
Table 6.
Digital manufacturing methods and their application value for battery packs.
As summarized in Table 6, digital methods are not independent from one another. Flow/impregnation simulation predicts dry spots, voids, and filling nonuniformity. Curing/cooling simulation evaluates residual stress, warpage, and hole-position deviation. Fiber-orientation and compaction simulation transfer local material states into structural performance evaluation. Machine learning and digital twins provide fast updating channels between mechanistic models and real-time data, enabling simulation outputs to enter trial molding optimization, mass-production monitoring, and quality traceability.
6.1. Flow and Void Prediction in Liquid Molding
Resin flow in RTM, HP-RTM, and VARTM is usually described using porous-medium flow models. Resin viscosity, preform permeability, pressure boundary conditions, mold temperature, and gel time jointly determine filling. For battery-pack enclosures with ribs, inserts, thickness variations, and sealing grooves, empirical gate and vent placement can easily create dry spots and air traps. Agogué et al. [58] used a Monte Carlo method to analyze the random influence of race tracking, showing that vent placement and edge-channel uncertainty significantly affect dry-spot risk. Chai et al. [98] proposed a radial injection-configuration optimization framework for RTM, showing that simulation-driven gate design can improve filling efficiency and product quality.
Macroscopic filling simulation also needs to extend toward two-scale inter-tow/intra-tow impregnation. Facciotto et al. [130] established a model for void formation and evolution in unsaturated two-scale preforms, showing that intra-tow capillary impregnation, inter-tow pressure flow, and boundary pressure jointly control void generation. For battery-pack composite parts, flow simulation has three engineering uses: at the design stage, it screens gate, vent, and sensor locations; during trial molding, it combines pressure, temperature, and flow-front data to invert permeability and boundary conditions; and in mass production, it converts predictions into online criteria for dry spots, air traps, and void risk.
6.2. Curing, Cooling, and Dimensional-Stability Simulation
During curing, thermoset composites undergo coupled changes in temperature field, degree of cure, chemical shrinkage, modulus evolution, tool friction, and fiber anisotropy. These factors determine residual stress, spring-in, and warpage. Wang et al. [106] highlighted the thermal-chemical-mechanical coupling of cure-induced deformation in continuous-fiber thermoset composites. Barcenas et al. [110] further showed that degree-of-cure gradients formed during filling of highly reactive liquid molding resins affect final shape. For battery-pack upper covers, trays, and side frames, simulation should prioritize sealing-flange flatness, mounting-hole position, module-locating surfaces, deformation around metal inserts, and assembly compression deviation, rather than only the overall demolded shape.
Although thermoplastic composites do not undergo crosslinking, melt cooling, crystallization, temperature-dependent modulus, and fiber-orientation freezing also generate residual stress. Parambil et al. [109] validated residual-stress evolution in semicrystalline polypropylene-based model composites under non-isothermal cooling, demonstrating that cooling rate and crystallization shrinkage cannot be ignored in dimensional-stability prediction. Therefore, curing/cooling simulation should be calibrated together with three-dimensional dimensional inspection, assembly validation, and dimensional retention after environmental cycling. For battery-pack components, the key criterion for forming accuracy is not merely whether a single part shape is acceptable but also whether flange sealing, hole matching, connection preload, and post-service dimensional stability satisfy system requirements.
6.3. Fiber-Orientation, Compaction, and Structural-Performance Mapping
Discontinuous-fiber materials such as SMC, LFT-D, and GMT undergo fiber-orientation evolution, fiber-length loss, weld-line formation, and local compaction differences during compression flow. Continuous-fiber preforms may experience shear, sliding, wrinkles, or local bridging during lay-up, transfer, mold closing, and filling. Romanenko et al. [38] constructed a virtual process chain for C-SMC parts in automotive mass production, which can predict flow fronts, local orientation, weld lines, performance, and warpage. Doppelbauer et al. [43] developed a macroscopic compaction model for C-SMC. Scheuring et al. [117] demonstrated through experiments and homogenization that long-fiber thermoplastic properties have pronounced orientation dependence.
Therefore, battery-pack part simulation should not stop at orientation contour plots. Local orientation, fiber length, voids, weld lines, and resin-rich regions should be mapped into position-dependent material parameters and then transferred to crash, fatigue, vibration, thermal-deformation, joining, and sealing analyses. Principal load paths around beams, mounting points, and lifting lugs should avoid fiber deficiency. Sealing surfaces and thin-wall regions should avoid fiber-poor regions or weld-line concentration caused by long-distance flow. Underbody shields and edge-protection regions should optimize local orientation and interlaminar structure according to impact direction. This mapping must be calibrated by local sampling, microscopic imaging, micro-CT, or mechanical testing; otherwise, it is insufficient for component-level design validation.
6.4. Machine-Learning-Assisted State Estimation and Multi-Objective Optimization
High-fidelity multiphysics simulation can reveal coupled interactions among flow, curing, heat transfer, compaction, and fiber orientation, but its modeling, computation, and trial molding costs are high. It is therefore difficult to use directly for fast decisions in automotive mass production. Machine learning can act as a surrogate model, classifier, or parameter-inversion tool for flow-front estimation, void-risk classification, cure-state prediction, and multi-objective process optimization. Zhu et al. [123] estimated RTM flow fronts using pressure sensors and neural networks. Causon et al. [124] used neural surrogate models for real-time Bayesian inversion. Wang et al. [131] systematically summarized machine learning for composite molding process modeling.
The role of machine learning in composite battery-pack manufacturing is not to replace forming mechanisms but rather to accelerate model calls, recognize abnormal patterns, and infer state variables that are difficult to measure directly. Reliable application requires at least three conditions: training data should cover material batches, component geometries, process windows, and real disturbances; model outputs should maintain physical consistency and express uncertainty; and predictions should be validated by component-level tests, non-destructive inspection, and service-relevant loads. Mendikute et al. [132] used surrogate models to link RTM voids with low-velocity impact response, showing that data-driven methods can connect manufacturing defects and service performance. For safety-critical battery-pack components, physics-constrained surrogate models, Bayesian updating, and active learning are preferable to purely black-box prediction.
6.5. Digital Twins and Closed-Loop Manufacturing Architecture
A digital twin should be understood as a dynamic closed loop among the physical production line, in-line sensing, mechanistic models, data-driven models, and the quality database, rather than a static three-dimensional display. For composite battery-pack components, the digital-twin chain begins with material-batch information, lay-up/preform state, and process parameters. During forming, temperature, pressure, dielectric response, flow-front, and mold-displacement signals update the model state in real time. The updated model predicts filling, impregnation, curing, fiber orientation, residual stress, and defect risk. If predicted values exceed preset thresholds, injection pressure, mold temperature, holding/cooling strategy, or venting path can be adjusted. After forming, non-destructive testing, dimensional measurement, and component tests are fed back to the quality database for traceability.
The effective operation of a digital twin first depends on real-time acquisition of process data. Fernández-León et al. [122] developed a transparent RTM experimental system with a size of 300 mm × 300 mm and a cavity thickness of 3 mm. Five pressure sensors were arranged at the inlet and inside the cavity to obtain pressure responses during resin flow, while visualized flow fronts were used to validate model predictions, as shown in Figure 20. This experimental system demonstrates that pressure fields, flow fronts, and cavity-state data form the basis for digital-twin models of liquid molding and provide data for identifying race tracking, local impregnation anomalies, and filling nonuniformity.
Figure 20.
RTM experimental system and pressure-sensor layout (a) overall structure of the RTM experimental system; (b) mold region and arrangement of pressure sensors [122].
On the basis of real-time sensor data, digital twins require fast models for state estimation and defect prediction. Fernández-León et al. [122] further proposed an instantiated digital-twin architecture for RTM. Pressure-sensor signals are continuously collected and fed into a disturbance-identification model to infer permeability distributions and race-tracking regions. A surrogate model then rapidly predicts flow-front evolution and pressure fields according to the permeability map, boundary conditions, and time information. The model was trained using 16,000 OpenFOAM simulations, and the computational time of a single two-dimensional flow simulation was controlled at about 38 s, providing a basis for online prediction, as shown in Figure 21. This architecture shows that a liquid molding digital twin is not a simple offline simulation but rather an online prediction system composed of sensor data, disturbance identification, surrogate modeling, and state updating.
Figure 21.
Digital-twin architecture for the RTM process [122].
For automotive mass production, implementation of digital twins remains limited by sensor durability, data standards, cross-equipment model generalization, online computing speed, and certification acceptance. Composite battery-pack digital twins should therefore not immediately pursue highly complex full-process models. A staged deployment is more appropriate: first, use digital twins for parameter-window optimization and defect-mechanism validation in trial molding; second, use them for online abnormality alarms, flow-path identification, and quality traceability in production; and finally, extend them to adaptive process-parameter control and service-performance prediction. At each stage, model versions, input data, predictions, and decision records should be retained for quality audits and product-liability traceability.
In practical battery-pack production, digital manufacturing can be deployed in three increasingly mature functions. The first is offline process-window design, where filling, curing, cooling, and orientation simulations reduce trial molding iterations. The second is in-line quality judgment, where pressure, temperature, dielectric, acoustic, and fiber-optic signals identify abnormal flow, delayed cure, or mold-displacement deviations during production. The third is traceable quality release, where NDT results, component tests, and material-batch records are connected with process data. Current barriers include sensor survivability in hot resin and high-pressure molds, data-format compatibility among equipment, model transfer between part geometries, and the lack of certification rules for digital evidence.
In summary, the digital objective of composite battery-pack manufacturing is not to replace materials knowledge and forming mechanisms with algorithms. It is to integrate mechanistic models, in-line sensing, machine learning, and inspection results into an updatable, verifiable, and traceable manufacturing system. Evaluation criteria should therefore expand from single prediction accuracy to whether the system can reduce trial molding cycles, scrap rate, and quality variation, and whether it can support safety validation and quality certification. On this basis, engineering development must further address material cost, manufacturing cycle, joining and sealing, thermal safety, recycling, and standard certification.
7. Engineering Challenges and Development Trends
The preceding sections analyzed composite-forming technologies for electric-vehicle battery packs from process capability, typical defects, quality-control, and structural integration perspectives. Overall, the engineering value of composite-material battery-pack structures should not be interpreted as single-material replacement but rather as multi-objective coordination among structural lightweighting, thermal safety, electrical insulation, sealing protection, manufacturing quality, and recyclability. Scaled application is still constrained by process cost, interfacial joining, flame-retardant insulation, process monitoring, recyclability, and standard certification. It is therefore necessary to summarize current bottlenecks, near-term research priorities, and long-term development directions from the perspective of industrial application. Table 7 presents an engineering roadmap for composite-material battery-pack structures.
Table 7.
Engineering challenges and development roadmap for composite-material battery-pack structures.
As summarized in Table 7, the focus of composite battery-pack development is shifting from material replacement to integrated “structure-function-manufacturing-validation” design. In the short term, engineering applications should first solve rapid forming, joining and sealing, flame-retardant insulation, defect detection, and component-level validation to ensure that composite components meet load-bearing, thermal-protection, and safety-protection requirements. In the medium to long term, the development of fast-curing resins, automated lay-up/compression molding, in-line monitoring, digital twins, recyclable composites, and standardized evaluation systems may allow composite-material battery-pack structures to expand from local functional parts and semi-load-bearing components toward multi-material integrated load-bearing structures.
7.1. From Material Replacement to System Value
Aluminum-alloy and steel battery packs still benefit from mature processes, stable supply chains, reliable joining technologies, and well-defined validation systems. Aluminum alloys provide good lightweighting and thermal conduction, with mature extrusion and casting technologies. Steel offers high strength, low cost, and reliable impact resistance. For composites to achieve scaled application, they must demonstrate integrated value beyond lightweighting, including functional integration, corrosion resistance, flame-retardant insulation, electromagnetic shielding, structural safety, manufacturing throughput, and life-cycle cost. Wang et al. [133] performed a multidisciplinary design optimization of an electric-vehicle battery-pack enclosure with a lattice structure, showing that enclosure design must consider structural and thermal-management objectives simultaneously rather than pursuing mass reduction alone.
The advantage of composites lies in design flexibility. Fiber lay-up, local reinforcement, and sandwich structures can optimize load paths, while functional fillers can provide flame retardancy, electromagnetic shielding, thermal insulation, and thermal conduction. Höhne et al. [18] proposed a PUR/UP-based SMC battery-pack enclosure material system and evaluated electromagnetic shielding and flame retardancy simultaneously, demonstrating that composite battery-pack enclosures require coordinated design between structure and multifunctional safety. Therefore, comparisons between composite and metallic battery packs should extend beyond density or static strength to system-level safety, assembly, repair, recycling, and certification cost.
7.2. High Throughput, Low Cost, and Multi-Process Combination
The automotive industry places stringent requirements on cycle time, cost, and consistency. SMC, LFT-D, GMT, and thermoplastic sheet forming have advantages in throughput and cost, but their load-bearing performance and defect control need further improvement. HP-RTM can provide high continuous-fiber performance and good surface quality, but the costs of preforming, injection equipment, fast-curing resin, and in-line quality control are high. PCM/WCM provides relatively good performance stability, but material and lay-up costs are high. VARTM is more suitable for low-volume, large-size, or prototype validation. Romanenko et al. [38] established a C-SMC process simulation chain for automotive series production, showing that industrial composite parts require flow, orientation, weld lines, warpage, and mechanical performance to be evaluated within the same process chain.
From an economic viewpoint, composite processes should be compared by total part cost rather than by material price alone. SMC, LFT-D/GMT, and thermoplastic sheet forming are attractive for high-volume components because short cycles can dilute tooling and press costs, but fiber-orientation scatter and post-forming inspection still influence scrap cost. HP-RTM can provide structural performance and short in-mold curing, yet it requires expensive matched tooling, automated preforming, injection equipment, and process monitoring. VARTM has a low tooling cost, but long infusion and curing times increase labor and occupancy cost. Pultrusion has favorable unit-length economics for beams after tooling investment. For battery-pack structures, the economic comparison should also include joining and sealing, because adhesive curing, fixture occupation, leakage testing, and repairability may dominate assembly time and cost [80,81,85,86].
Future mass production is more likely to adopt a multi-process combination allocated by component function, rather than one process covering the entire battery pack. Upper covers and protective covers may use SMC, LFT-D, or thermoplastic sheets. Load-bearing frames may use metal profiles, pultruded profiles, or HP-RTM composites. Underbody shields may use thermoplastic composites, sandwich panels, or composite—metal hybrid structures. Thermal-barrier and flame-retardant parts may use aerogels, ceramic-forming composites, or functional coatings. High-level research should therefore focus on multi-material and multi-process coordination rather than a single-material-replacement narrative.
7.3. Integrated Forming-Structure-Function Design
The future direction of composite-material battery-pack structures is integrated forming, structural, and functional design. Section 3 showed that different processes lead to different fiber volume fractions, orientation states, porosity levels, and component-size capabilities. Section 4 further showed that these process characteristics transform into defects and property scatter. Therefore, forming constraints should be included in structural design from the beginning. For example, gate and vent positions should not conflict with rib layout; charge flow should not weaken the main load path; flame-retardant fillers should not excessively increase resin viscosity and reduce impregnation; and sealing flanges should be designed to avoid warpage caused by residual stress.
Multifunctional integration should also avoid the simple stacking of materials. Flame retardancy, thermal insulation, thermal conduction, electromagnetic shielding, electrical insulation, and load bearing may constrain each other. Conductive fillers improve shielding but may affect insulation safety. Flame-retardant fillers may increase viscosity and impregnation difficulty. Thermal-insulation materials may reduce structural stiffness. Shi et al. [17] and Höhne et al. [18] both suggest that functional composites require balance among material formulation, forming window, mechanical properties, and safety validation. For battery packs, a rational solution is not to assign all functions to a single composite layer but rather to coordinate composite shells, metal reinforcements, insulation layers, sealants, and flame-retardant coatings at the system level.
Thermal-safety design is another typical case in which material selection, structural architecture, and functional integration cannot be separated. Recent work on prismatic lithium-ion batteries has shown that anisotropic thermal conductivity should be quantified when predicting nonuniform heat transfer inside prismatic cells to predict nonuniform heat transfer inside cells [134]. At the module level, liquid-cooling plates with nonuniform spiral-fin channels can improve heat-transfer performance and temperature uniformity [135]. Liquid-immersion experiments for large energy-stored lithium-ion battery modules further indicate that thermal-runaway management depends on heat removal, flame suppression, and the interaction between coolant and module geometry [136]. These studies suggest that composite battery-pack structures should not only resist external fire and thermal runaway but also accommodate cooling channels, thermal barriers, and heat-spreading paths without compromising sealing and mechanical integrity.
7.4. Digital Manufacturing and Intelligent Quality Control
Digital manufacturing supports the transition of composite-material battery-pack structures from small-batch prototyping to stable mass production. Resin flow, curing deformation, fiber orientation, and defect formation are strongly coupled and cannot be fully covered by empirical parameter adjustment under complex geometries and batch variation. Wang et al. [131] reviewed machine learning for composite molding process modeling and showed that machine learning can act as a fast alternative to high-fidelity simulation, provided that the training data are sufficiently representative and physically consistent. Mendikute et al. [132] used machine learning surrogate models to predict the influence of RTM voids on low-velocity impact response, illustrating that data-driven methods can connect manufacturing defects with service performance.
Representative practical studies also indicate how digital manufacturing can be implemented at the process-line level. For liquid composite molding, hybrid piezoelectric-fiber sensor networks have been used to monitor three-dimensional resin flow fronts, providing real-time information for identifying delayed filling, race tracking, and dry-spot risks [121]. Pressure-sensor-based flow-front estimation and neural or Bayesian surrogate models further show that limited in-mold sensing signals can be transformed into filling-state reconstruction, permeability updating, and process-parameter feedback during RTM processes [123,124]. For composite battery-pack components, these cases suggest that digital manufacturing should be deployed around high-risk regions such as gates, vents, ribs, sealing flanges, thick sections, and local reinforcement zones. The monitored process state can then be linked with defect prediction, non-destructive inspection, and quality-release decisions according to the functional importance and safety level of each component.
Future intelligent manufacturing should establish a closed loop of process simulation, in-line sensing, defect recognition, non-destructive testing, performance prediction, and quality release. The core of a digital twin is not three-dimensional visualization but rather the integration of the physical manufacturing process, sensor data, simulation models, and data-driven algorithms to enable real-time monitoring, prediction, and optimization. For composite battery-pack mass production, key challenges include sensor stability in high-temperature, high-pressure, and resin environments; the standardization of material-batch and process data; model generalization across parts and equipment; and the matching of online computing speed with production-line cycle time.
7.5. Recyclability and Low-Carbon Manufacturing
As battery regulations, carbon-footprint requirements, and circular-economy goals become stronger, composite-material battery-pack structures must consider recyclability and environmental impact in addition to lightweighting. Thermoset composites are difficult to recycle and are mainly treated by mechanical grinding, pyrolysis, chemical recycling, or energy recovery; cost and property retention remain concerns. Thermoplastic composites have remelting and reprocessing potential, but fiber length, interface performance, and flame-retardant-system stability after recycling require validation. Montagna et al. [36] reviewed recycling technologies for carbon-fiber-reinforced thermoplastic and thermoset composites and highlighted clear differences in recycling routes, property retention, and economics. Yuan et al. [137] further summarized advances in CFRP recycling, showing that mechanical, pyrolysis, and chemical approaches must still address fiber-property retention, resin utilization, and scale-up cost.
Future studies should establish life-cycle assessment models for composite-material battery-pack structures and compare steel, aluminum, thermoset composites, and thermoplastic composites across raw-material production, manufacturing, use, repair, recycling, and reuse stages. Large-scale application can be justified only when composites show an integrated advantage among use-phase benefits from lightweighting, manufacturing energy consumption, recycling route, and safety performance. For thermoplastic composites, recyclability should not remain a conceptual selling point; it must be verified by mechanical properties after recycling, flame retardancy, welding/joining performance, and number of recycling cycles.
More specific recycling evaluation is therefore needed for battery-pack-grade composites. Mechanical recycling is simple and scalable, but it usually shortens fibers and downgrades the recycled material to fillers or lower-performance products. Pyrolysis can recover carbon fibers from thermoset composites, but energy consumption, surface damage, and reuse of the degraded matrix remain concerns. Solvolysis and other chemical recycling routes may better preserve fiber quality and recover resin-derived chemicals, but solvent recovery, process cost, and scale-up stability must be demonstrated. For thermoplastic composites, remelting and reprocessing are promising, but viable recycling cycles should be quantified by residual strength, impact resistance, flame retardancy, welding performance, and dimensional stability after repeated processing [36,137].
7.6. Standardization, Certification, and Future Roadmap
Composites are anisotropic, defect-sensitive, and process-dependent. Material-level properties cannot directly represent large battery-pack components. Existing standards such as GB 38031, UN R100, and UL 2580 mainly address battery-system safety and cannot replace process-quality and defect-tolerance evaluation for composite components. Future work should establish a multi-level certification system covering material coupons, laminates/subcomponents, full-size components, and battery-pack systems. Pepó et al. [138] reviewed standardized battery testing and showed that unified test methods are essential for safety innovation and industrial promotion.
In the short term, composite-material battery-pack structures should focus on stabilizing processes, such as SMC, PCM, HP-RTM, and thermoplastic sheet forming, and on establishing component-level evaluation methods for flame retardancy, electromagnetic shielding, sealing, and defect detection. In the medium term, recyclable thermoplastic composites, multi-material joining, in-line monitoring, and integrated forming-structure simulation should be developed to achieve high-throughput production with a low scrap rate. In the long term, composite-material battery-pack structures are expected to move toward integrated structural-function design, digital-twin-based closed-loop manufacturing, low-carbon life-cycle design, and standardized certification systems.
Overall, industrialization should begin with low-risk and functional protective components, and then gradually expand to load-bearing structures and multi-material integrated structures. Future work should build a complete evidence chain through process simulation, in-line monitoring, non-destructive testing, component-level testing, and life-cycle assessment so that composites in battery packs can move from material substitution to verifiable, traceable, and certifiable systems engineering.
8. Conclusions and Outlook
8.1. Conclusions
This review systematically analyzed composite-forming technologies for electric-vehicle battery packs, covering component-level service requirements, material systems, mainstream forming processes, typical defects, quality-control methods, and engineering development trends. The following conclusions can be drawn.
- The design target for composite-material battery-pack structures should not be limited to lightweighting. Load bearing, crash protection, flame-retardant thermal insulation, electrical insulation, electromagnetic shielding, waterproof sealing, and long-term durability should be considered simultaneously. Because different components have different risk levels and service functions, material and process selection should start from component function rather than from a single material property.
- Different forming routes have distinct capability boundaries. SMC, LFT-D/GMT, and thermoplastic sheet forming are suitable for high-throughput, complex-ribbed, and medium-load components. PCM/WCM and RTM/HP-RTM are more appropriate for continuous-fiber-reinforced and higher-performance structural parts. VARTM is suitable for large prototypes or low- to medium-volume components. Pultruded profiles are suitable for continuous constant-section parts such as side frames, cross beams, and reinforcement beams. Process selection determines not only production cycle and component size but also fiber orientation, voids, impregnation quality, residual stress, and final performance.
- Voids, dry spots, resin-rich regions, delamination, warpage, fiber waviness, and fiber breakage are typical defects that require priority control in composite battery-pack parts. These defects are strongly process-dependent and region-sensitive, and they affect interlaminar properties, fatigue life, residual strength after impact, sealing reliability, thermal-protection capability, and dimensional stability. Defect evaluation should therefore go beyond morphology description and establish links among defect type, defect location, performance effect, and tolerance criterion.
- Manufacturing quality control for composite-material battery-pack structures should move from post-forming inspection to whole-process closed-loop control. Material input, resin viscosity, fiber volume fraction, lay-up quality, mold temperature, injection pressure, vacuum level, and curing or cooling schedules should all be included. In-line monitoring, ultrasonic testing, X-ray CT, infrared thermography, DIC, acoustic emission, and shearography can identify defects at different scales and positions, but their results must be connected with component-level mechanical, sealing, thermal-safety, and environmental-aging tests.
- Process simulation, machine learning, and digital twins provide important directions for low-defect manufacturing of composite-material battery-pack structures. Resin flow simulation, cure-deformation prediction, fiber-orientation mapping, and data-driven defect prediction can shorten trial molding cycles, optimize process windows, and improve batch consistency. The key value of future digital twins is not simple visualization but rather real-time sensing, model updating, defect prediction, parameter adjustment, and quality traceability.
8.2. Outlook
Although the reviewed studies provide useful evidence for process selection and defect control, several limitations still constrain rigorous comparison among forming routes. Many mechanical-property data are obtained from coupons and cannot be directly transferred to full-size battery-pack structures. Cost comparisons are often based on public industrial information rather than peer-reviewed cost-per-part datasets. Defect data are usually reported for isolated material systems, whereas battery-pack structures require component-region-based tolerance criteria.
- Future comparative studies should therefore move from qualitative process descriptions toward quantitative, component-oriented evaluation. The comparison framework should include normalized mechanical properties, cycle time, tooling and material costs, expected defect rate, recyclability, repairability, applicable component regions, and uncertainty sources. Weighting factors may be adjusted according to whether the target component is an upper cover, tray, beam, side frame, underbody shield, or joining/sealing region.
- A second research priority is to establish defect-tolerance criteria that connect manufacturing defects with component-level safety. Voids, dry spots, resin-rich regions, delamination, warpage, residual stress, fiber misalignment, waviness, and fiber breakage should be evaluated with respect to their location, size, morphology, and service consequence. Such criteria should be validated through mechanical testing, sealing tests, thermal-safety tests, vibration durability, environmental aging, and post-impact performance.
- A third priority is to quantify multifunctional and life-cycle performance. Thermal-management design should be considered together with recyclable composite architecture because cooling plates, immersion media, flame-retardant barriers, conductive fillers, and structural composite layers interact through heat transfer, sealing, electrical insulation, and crash protection. Accordingly, thermal conductivity, cooling-channel design, liquid-immersion safety, recyclability, and joining/sealing repairability should be evaluated as coupled design variables rather than independent topics.
- Finally, digital manufacturing should be developed as an evidence-generating system rather than only a visualization tool. Future digital twins should integrate material-batch data, process simulation, in-line sensing, non-destructive testing, defect prediction, parameter feedback, and service tracking. Their reliability will depend on standardized datasets, sensor durability, model transferability, online computing speed, and validation across material coupons, subcomponents, full-size components, and complete battery-pack systems.
Author Contributions
Conceptualization, G.L., L.Z., X.L. and Q.L. (Qingqing Lü); methodology, G.L., L.Z., X.L. and Q.L. (Qingqing Lü); validation, X.S., L.Y., Q.L. (Qun Li) and Y.M.; data curation, X.S., L.Y., Q.L. (Qun Li), Y.M. and Y.Y.; writing—original draft preparation, G.L., L.Z., X.S. and Y.Y.; writing—review and editing, G.L., L.Z. and Y.Y.; supervision, L.Y., Q.L. (Qun Li) and Y.M.; project administration, X.L. and Q.L. (Qingqing Lü); funding acquisition, X.L. and Q.L. (Qingqing Lü). All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by Henan Science and Technology R&D Program Joint Fund (grant No. 202324119, 20250104, 252103810171) and Henan Key Research and Development and Promotion Special Project (Science and Technology Tackling) (grant No. 262102231017, 262102231018, 252102241063).
Institutional Review Board Statement
Not applicable.
Informed Consent Statement
Not applicable.
Data Availability Statement
The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding authors.
Conflicts of Interest
Author Xiaolu Liao was employed by the company Nanyang Weite Explosion-Proof Motor Co., Ltd. The remaining authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.
Abbreviations
The following abbreviations are used in this manuscript:
| BMC | bulk molding compound |
| CFRP | carbon-fiber-reinforced polymer |
| CMM | coordinate measuring machine |
| C-SMC | carbon-fiber sheet molding compound |
| CRTM | compression resin transfer molding |
| CT | computed tomography |
| DIC | digital image correlation |
| DSC | differential scanning calorimetry |
| EMC | electromagnetic compatibility |
| EMI | electromagnetic interference |
| FBG | Fiber Bragg grating |
| GFRP | glass-fiber-reinforced polymer |
| GMT | glass-mat thermoplastic |
| HP-RTM | High-pressure resin transfer molding |
| LCM | liquid composite molding |
| LFT | long-fiber thermoplastic |
| LFT-D | long-fiber thermoplastic direct processing |
| ML | machine learning |
| NDT | non-destructive testing |
| PC | polycarbonate |
| PCM | prepreg compression molding |
| PET | polyethylene terephthalate |
| PP | polypropylene |
| PZT | lead zirconate titanate |
| RTM | resin transfer molding |
| SEM/EDS | scanning electron microscopy/energy-dispersive X-ray spectroscopy |
| SMC | sheet molding compound |
| SMP | silane-modified polymer |
| VA-PCM | vacuum-assisted prepreg compression molding |
| VARTM | vacuum-assisted resin transfer molding |
| WCM | wet compression molding |
| X-ray CT | X-ray computed tomography |
References
- Pan, Y.; Xiong, Y.; Wu, L.; Diao, K.; Guo, W. Lightweight Design of an Automotive Battery-Pack Enclosure via Advanced High-Strength Steels and Size Optimization. Int. J. Automot. Technol. 2021, 22, 1279–1290. [Google Scholar] [CrossRef] [Scilit]
- Xiong, Y.; Pan, Y.; Wu, L.; Liu, B. Effective weight-reduction- and crashworthiness-analysis of a vehicle’s battery-pack system via orthogonal experimental design and response surface methodology. Eng. Fail. Anal. 2021, 128, 105635. [Google Scholar] [CrossRef] [Scilit]
- Wang, H.; Wang, Z.; Fan, Y.; Gao, Q.; Wang, H. Multi-objective lightweight design of automotive battery pack box for crashworthiness. Int. J. Crashworthiness 2024, 29, 292–307. [Google Scholar] [CrossRef] [Scilit]
- Wang, S.; Guo, S.; Li, R.; Hu, Z.; Leng, Q. On crashworthiness design of hybrid metal–composite battery-pack enclosure structure. Mech. Adv. Mater. Struct. 2025, 32, 2548–2559. [Google Scholar] [CrossRef] [Scilit]
- Xu, D.; Pan, Y.; Zhang, X.; Dai, W.; Liu, B.; Shuai, Q. Data-driven modelling and evaluation of a battery-pack system’s mechanical safety against bottom cone impact. Energy 2024, 290, 130145. [Google Scholar] [CrossRef] [Scilit]
- Zhang, X.; Pan, Y.; Xiong, Y.; Zhang, Y.; Tang, M.; Dai, W.; Liu, B.; Hou, L. Deep learning-based vibration stress and fatigue-life prediction of a battery-pack system. Appl. Energy 2024, 357, 122481. [Google Scholar] [CrossRef] [Scilit]
- Kvasha, A.; Gutiérrez, C.; Osa, U.; de Meatza, I.; Blazquez, J.A.; Macicior, H.; Urdampilleta, I. A comparative study of thermal runaway of commercial lithium ion cells. Energy 2018, 159, 547–557. [Google Scholar] [CrossRef] [Scilit]
- GB 38031-2025; Electric Vehicles Traction Battery Safety Requirements. State Administration for Market Regulation. Standardization Administration of China: Beijing, China, 2025. Available online: https://openstd.samr.gov.cn/ (accessed on 31 July 2026).
- United Nations Economic Commission for Europe. UN Regulation No. 100: Uniform Provisions concerning the Approval of Vehicles with Regard to Specific Requirements for the Electric Power Train. Available online: https://unece.org/transport/vehicle-regulations-wp29/standards/addenda-1958-agreement-regulations-81-100 (accessed on 31 July 2026).
- UL Standards & Engagement. UL 2580: Batteries for Use in Electric Vehicles. Available online: https://www.shopulstandards.com/ProductDetail.aspx?productId=UL2580 (accessed on 31 July 2026).
- European Parliament; Council of the European Union. Regulation (EU) 2023/1542 of the European Parliament and of the Council of 12 July 2023 Concerning Batteries and Waste Batteries, Amending Directive 2008/98/EC and Regulation (EU) 2019/1020 and Repealing Directive 2006/66/EC. 2023. Available online: https://eur-lex.europa.eu/eli/reg/2023/1542/oj (accessed on 31 July 2026).
- Boland, C.S.; De Kleine, R.; Keoleian, G.A.; Lee, E.C.; Kim, H.C.; Wallington, T.J. Life Cycle Impacts of Natural Fiber Composites for Automotive Applications: Effects of Renewable Energy Content and Lightweighting. J. Ind. Ecol. 2016, 20, 179–189. [Google Scholar] [CrossRef] [Scilit]
- Cheng, P.; Peng, Y.; Li, S.; Rao, Y.; Le Duigou, A.; Wang, K.; Ahzi, S. 3D printed continuous fiber reinforced composite lightweight structures: A review and outlook. Compos. Part B Eng. 2023, 250, 110450. [Google Scholar] [CrossRef] [Scilit]
- Zhang, Z.; Han, F.; Li, H.; Li, T.; Yang, B.; Hu, J.; Pan, Y.-T. Flame-Retardant Fiber-Reinforced Composites: Advances and Prospects in Multi-Performance Synergy. J. Compos. Sci. 2025, 9, 703. [Google Scholar] [CrossRef] [Scilit]
- Shi, X.-H.; Li, X.-L.; Li, Y.-M.; Li, Z.; Wang, D.-Y. Flame-retardant strategy and mechanism of fiber reinforced polymeric composite: A review. Compos. Part B Eng. 2022, 233, 109663. [Google Scholar] [CrossRef] [Scilit]
- Kong, W.; Yi, S.; Sun, W.; Xu, L.; Jia, L.; Yan, D.; Li, Z. Polyaniline-decorated carbon fibers for enhanced mechanical and electromagnetic interference shielding performances of epoxy composites. Mater. Des. 2022, 217, 110658. [Google Scholar] [CrossRef] [Scilit]
- Shi, J.-F.; Kong, W.-W.; Zou, K.-K.; Li, N.; Wang, Y.-Y.; Yan, D.-X. Enhanced mechanical and electromagnetic interference shielding performance of carbon fiber/epoxy composite with intercalation of modified aramid fiber. Colloids Surf. A Physicochem. Eng. Asp. 2023, 661, 130959. [Google Scholar] [CrossRef] [Scilit]
- Höhne, C.-C.; Blaess, P.; Ilinzeer, S.; Griesbaum, P. New approach for electric vehicle composite battery housings: Electromagnetic shielding and flame retardancy of PUR/UP-based sheet moulding compound. Compos. Part A Appl. Sci. Manuf. 2023, 167, 107404. [Google Scholar] [CrossRef] [Scilit]
- Ma, X.-L.; Wen, L.-H.; Wang, S.-Y.; Xiao, J.-Y.; Li, W.-H.; Hou, X. Inherent relationship between process parameters, crystallization and mechanical properties of continuous carbon fiber reinforced PEEK composites. Def. Technol. 2023, 24, 269–284. [Google Scholar] [CrossRef] [Scilit]
- Duhovic, M.; Keilmann, A.; Schommer, D.; Redenbach, C.; Schladitz, K. Quantitative fiber orientation analysis of carbon fiber sheet molding compounds using polarization imaging and X-ray computed tomography. Compos. Part B Eng. 2025, 295, 112146. [Google Scholar] [CrossRef] [Scilit]
- Zhang, C.; Zhang, G.; Xu, J.; Shi, X.P.; Wang, X. Review of curing deformation control methods for carbon fiber reinforced resin composites. Polym. Compos. 2022, 43, 3350–3370. [Google Scholar] [CrossRef] [Scilit]
- Okolie, O.; Latto, J.; Faisal, N.; Jamieson, H.; Mukherji, A.; Njuguna, J. Manufacturing Defects in Thermoplastic Composite Pipes and Their Effect on the in-situ Performance of Thermoplastic Composite Pipes in Oil and Gas Applications. Appl. Compos. Mater. 2023, 30, 231–306. [Google Scholar] [CrossRef] [Scilit]
- Azad, M.M.; Jung, J.; Elahi, M.U.; Sohail, M.; Kumar, P.; Kim, H.S. Failure modes and non-destructive testing techniques for fiber-reinforced polymer composites. J. Mater. Res. Technol. 2024, 33, 9519–9537. [Google Scholar] [CrossRef] [Scilit]
- Fu, Y.; Yao, X. A review on manufacturing defects and their detection of fiber reinforced resin matrix composites. Compos. Part C Open Access 2022, 8, 100276. [Google Scholar] [CrossRef] [Scilit]
- Rosenthal, S.; Maaß, F.; Kamaliev, M.; Hahn, M.; Gies, S.; Tekkaya, A.E. Lightweight in Automotive Components by Forming Technology. Automot. Innov. 2020, 3, 195–209. [Google Scholar] [CrossRef] [Scilit]
- Bree, G.; Horstman, D.; Low, C.T.J. Light-weighting of battery casing for lithium-ion device energy density improvement. J. Energy Storage 2023, 68, 107852. [Google Scholar] [CrossRef] [Scilit]
- Tekkaya, A.E.; Min, J. Special Issue on Automotive Lightweight. Automot. Innov. 2020, 3, 193–194. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Cebe, E.; Kalbaran, O.; Irez, A.B. A numerical investigation of ground impact for hierarchically designed hybrid composite structures in electric vehicle battery cases. J. Power Sources 2025, 638, 236594. [Google Scholar] [CrossRef] [Scilit]
- Tran, M.-K.; Mevawalla, A.; Aziz, A.; Panchal, S.; Xie, Y.; Fowler, M. A Review of Lithium-Ion Battery Thermal Runaway Modeling and Diagnosis Approaches. Processes 2022, 10, 1192. [Google Scholar] [CrossRef] [Scilit]
- Mallick, S.; Gayen, D. Thermal behaviour and thermal runaway propagation in lithium-ion battery systems—A critical review. J. Energy Storage 2023, 62, 106894. [Google Scholar] [CrossRef] [Scilit]
- Chen, M.; Zhu, M.; Zhao, L.; Chen, Y. Study on thermal runaway propagation inhibition of battery module by flame-retardant phase change material combined with aerogel felt. Appl. Energy 2024, 367, 123394. [Google Scholar] [CrossRef] [Scilit]
- Liu, M.; Chen, K.; Shi, Y.; Wu, S.; Feng, Y.; Fu, L.; Gao, J.; Tang, L.; Yang, F. Mechanically strong hierarchical nanosystem for fire protection and electromagnetic interference shielding. Compos. Part B Eng. 2023, 261, 110795. [Google Scholar] [CrossRef] [Scilit]
- Donough, M.J.; Shafaq; St John, N.A.; Philips, A.W.; Gangadhara Prusty, B. Process modelling of In-situ consolidated thermoplastic composite by automated fibre placement—A review. Compos. Part A Appl. Sci. Manuf. 2022, 163, 107179. [Google Scholar] [CrossRef] [Scilit]
- Brito, C.; Teuwen, J.; Dransfeld, C.; Villegas, I. Ultrasonic welding of thermoplastic composites: A comparison between polyetheretherketone and low-melt polyaryletherketone as resin in the adherends and energy directors. Compos. Part B Eng. 2025, 296, 112264. [Google Scholar] [CrossRef] [Scilit]
- Farhadi, M.; Aidi, B.; Goossens, H.; Chen, L.; Chang, F.; Lattimer, B.Y.; Case, S.W. Experimental response of intumescent fiber-reinforced glass fiber filled polypropylene thermoplastic battery enclosure materials to external fire and mechanical loading. Compos. Part B Eng. 2026, 310, 113102. [Google Scholar] [CrossRef] [Scilit]
- Stieven Montagna, L.; Ferreira de Melo Morgado, G.; Lemes, A.P.; Roberto Passador, F.; Cerqueira Rezende, M. Recycling of carbon fiber-reinforced thermoplastic and thermoset composites: A review. J. Thermoplast. Compos. Mater. 2023, 36, 3455–3480. [Google Scholar] [CrossRef] [Scilit]
- Alam, P.; Mamalis, D.; Robert, C.; Floreani, C.; Ó Brádaigh, C.M. The fatigue of carbon fibre reinforced plastics—A review. Compos. Part B Eng. 2019, 166, 555–579. [Google Scholar] [CrossRef] [Scilit]
- Romanenko, V.; Duhovic, M.; Schommer, D.; Hausmann, J.; Eschl, J. Advanced process simulation of compression molded carbon fiber sheet molding compound (C-SMC) parts in automotive series applications. Compos. Part A Appl. Sci. Manuf. 2022, 157, 106924. [Google Scholar] [CrossRef] [Scilit]
- Nega, B.F.; Pierce, R.S.; Yi, X.; Liu, X. Full-field effect of flow-induced fiber orientation during compression molding of carbon fiber sheet molding compounds. Polym. Compos. 2025, 46, 2664–2678. [Google Scholar] [CrossRef] [Scilit]
- Composites Knowledge Network. Compression Moulding-A302. Available online: https://compositeskn.org/KPC/A302 (accessed on 31 July 2026).
- Alnersson, G.; Lejon, E.; Zrida, H.; Aitomäki, Y.; Ljung, A.-L.; Lundström, T.S. 3D flow and fibre orientation modelling of compression moulding of A-SMC: Simulations and experimental validation in squeeze flow. Funct. Compos. Mater. 2023, 4, 11. [Google Scholar] [CrossRef] [Scilit]
- Ferré-Sentis, D.; Dumont, P.; Orgéas, L.; Martoïa, F.; Sager, M. Rheological response of compressible SMCs under various deformation kinematics: Experimental aspects and simple modelling approach. Compos. Part A Appl. Sci. Manuf. 2022, 154, 106774. [Google Scholar] [CrossRef] [Scilit]
- Doppelbauer, L.K.; Rienesl, K.; Stelzer, P.S.; Zulueta, K.; Chang, L.-Y.; Major, Z. A macroscopic model of the compaction process during compression molding of carbon fiber sheet molding compounds. Compos. Part A Appl. Sci. Manuf. 2023, 169, 107535. [Google Scholar] [CrossRef] [Scilit]
- Trauth, A.; Pinter, P.; Weidenmann, K. Investigation of Quasi-Static and Dynamic Material Properties of a Structural Sheet Molding Compound Combined with Acoustic Emission Damage Analysis. J. Compos. Sci. 2017, 1, 18. [Google Scholar] [CrossRef] [Scilit]
- Teijin Automotive Technologies. Teijin Automotive Technologies Multi-Material Battery Enclosure Named ACCE Parts Award Winner. Available online: https://www.businesswire.com/news/home/20220912005813/en/Teijin-Automotive-Technologies-Multi-Material-Battery-Enclosure-Named-ACCE-Parts-Award-Winner (accessed on 31 July 2026).
- Lee, J.-M.; Kim, B.-M.; Ko, D.-C. Development of vacuum-assisted prepreg compression molding for production of automotive roof panels. Compos. Struct. 2019, 213, 144–152. [Google Scholar] [CrossRef] [Scilit]
- Huntsman. Huntsman Advanced Materials Develops a New Compression Molding Process. Available online: https://www.huntsman.com/about/advanced-materials/news/detail/12600/huntsman-advanced-materials-develops-a-new-compression (accessed on 31 July 2026).
- Li, Y.; Liu, K.; Chen, G.; Ge, J.; Yang, J.; Li, X.; Liu, S.; Liang, J. An embedded digital element model to simulate the wrinkle defects driven by the consolidation of composites. Compos. Sci. Technol. 2024, 246, 110389. [Google Scholar] [CrossRef] [Scilit]
- Zhi, J.; Yang, B.; Li, Y.; Tay, T.-E.; Tan, V.B.C. Multiscale thermo-mechanical analysis of cure-induced deformation in composite laminates using Direct FE2. Compos. Part A Appl. Sci. Manuf. 2023, 173, 107704. [Google Scholar] [CrossRef] [Scilit]
- Lee, J.; Duhovic, M.; Allen, T.; May, D.; Kelly, P. Computational modelling and analysis of transverse liquid composite moulding processes. Compos. Part A Appl. Sci. Manuf. 2023, 167, 107433. [Google Scholar] [CrossRef] [Scilit]
- Albrecht, F.; Poppe, C.; Tiemann, T.; Sauerwein, V.; Rosenberg, P.; Henning, F. Flow-induced fiber displacement in non-bindered UD-NCF during Wet Compression Molding—Analysis and implications for process control. Compos. Sci. Technol. 2022, 228, 109574. [Google Scholar] [CrossRef] [Scilit]
- Wu, X.; Zhang, M.; Liu, Z.; Fu, X.; Liu, H.; Zhang, Y.; Yang, X. Cure Kinetics-Driven Compression Molding of CFRP for Fast and Low-Cost Manufacturing. Polymers 2025, 17, 2154. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Sears, J.; Ayatollahi, S.; Meirson, G.; Johrendt, J.; Hrymak, A. Processing parameter optimization for Carbon Fibre-Reinforced Plastics (CFRPs) using Wet Compression Molding (WCM)—A statistical approach. Compos. Part B Eng. 2026, 316, 113418. [Google Scholar] [CrossRef] [Scilit]
- Robertson, F.C. Resin transfer moulding of aerospace resins-a review. Br. Polym. J. 1988, 20, 417–429. [Google Scholar] [CrossRef] [Scilit]
- Yoon, M.; Ahn, M. Study on molding control factors to reduce void contents in manufacturing CFRP parts by HP-RTM. Compos. Part B Eng. 2025, 296, 112231. [Google Scholar] [CrossRef] [Scilit]
- Shen, R.; Liu, T.; Liu, H.; Zou, X.; Gong, Y.; Guo, H. An Enhanced Vacuum-Assisted Resin Transfer Molding Process and Its Pressure Effect on Resin Infusion Behavior and Composite Material Performance. Polymers 2024, 16, 1386. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Huntsman Transportation. High-Pressure Resin Transfer Molding. Available online: https://www.huntsman-transportation.com/EN/processes/processes-for-composites/hp-rtm.html (accessed on 31 July 2026).
- Agogué, R.; Shakoor, M.; Beauchêne, P.; Park, C.H. Analysis and Minimization of Race Tracking in the Resin-Transfer-Molding Process by Monte Carlo Simulation. Materials 2023, 16, 4438. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Hamidi, Y.K.; Altan, M.C. Process Induced Defects in Liquid Molding Processes of Composites. Int. Polym. Process. 2017, 32, 527–544. [Google Scholar] [CrossRef] [Scilit]
- Holmberg, J.; Berglund, L. Manufacturing and performance of RTM U-beams. Compos. Part A Appl. Sci. Manuf. 1997, 28, 513–521. [Google Scholar] [CrossRef] [Scilit]
- Sun, Z.; Xiao, J.; Tao, L.; Wei, Y.; Wang, S.; Zhang, H.; Zhu, S.; Yu, M. Preparation of High-Performance Carbon Fiber-Reinforced Epoxy Composites by Compression Resin Transfer Molding. Materials 2019, 12, 13. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Yalcinkaya, M.A.; Sozer, E.M.; Altan, M.C. Effect of external pressure and resin flushing on reduction of process-induced voids and enhancement of laminate quality in heated-VARTM. Compos. Part A Appl. Sci. Manuf. 2019, 121, 353–364. [Google Scholar] [CrossRef] [Scilit]
- Schelleis, C.; Scheuring, B.M.; Schreyer, L.; Liebig, W.V.; Hrymak, A.; Kärger, L.; Weidenmann, K.A.; Henning, F. Process-induced skewness of flow fronts and fiber orientations in LFT-D compression molding considering processing, characterization, and simulation. J. Thermoplast. Compos. Mater. 2025, 38, 2922–2944. [Google Scholar] [CrossRef] [Scilit]
- Dweib, M.A.; Ó Brádaigh, C.M. Compression molding of glass reinforced thermoplastics: Modeling and experiments. Polym. Compos. 2000, 21, 832–845. [Google Scholar] [CrossRef] [Scilit]
- Bondy, M.; Pinter, P.; Altenhof, W. Experimental characterization and modelling of the elastic properties of direct compounded compression molded carbon fibre/polyamide 6 long fibre thermoplastic. Mater. Des. 2017, 122, 184–196. [Google Scholar] [CrossRef] [Scilit]
- Schelleis, C.; Scheuring, B.M.; Liebig, W.V.; Hrymak, A.N.; Henning, F. Approaching Polycarbonate as an LFT-D Material: Processing and Mechanical Properties. Polymers 2023, 15, 2041. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- MDC Mould. LFT-D. 17 August 2022. Available online: https://www.zjmdc.com/IndustryNews/LFT-D.html (accessed on 31 July 2026).
- Barocio, E.; Hicks, J.; Kim, G.; Favaloro, A.; Ghosh, G.; Goodsell, J.; Pipes, R.B. Validation of shape change predictions for stamp forming of carbon fiber thermoplastic composite laminates. Compos. Part B Eng. 2024, 275, 111325. [Google Scholar] [CrossRef] [Scilit]
- Dörr, D.; Singh-Heer, N.; Xu, C.; Chang, T.; Clement-Thorne, B.; Gergely, R.C.R.; Okonski, D.; Henning, F.; Straatman, A.G.; Hrymak, A. Experimental and predictive analysis of the molding behavior of a PA6 glass mat thermoplastic (GMT). Int. J. Adv. Manuf. Technol. 2023, 129, 1159–1173. [Google Scholar] [CrossRef] [Scilit]
- Trinseo. Thermoplastic Battery Enclosures. Available online: https://www.trinseo.com/industries/mobility/electric-vehicle-support/thermoplastic-battery-casing (accessed on 31 July 2026).
- Alsinani, N.; Laberge Lebel, L. Effect of high pulling speeds on the morphologies of pultrudates in a thermoplastic pultrusion process. J. Thermoplast. Compos. Mater. 2023, 36, 3566–3584. [Google Scholar] [CrossRef] [Scilit]
- Sandberg, M.; Yuksel, O.; Baran, I.; Hattel, J.H.; Spangenberg, J. Numerical and experimental analysis of resin-flow, heat-transfer, and cure in a resin-injection pultrusion process. Compos. Part A Appl. Sci. Manuf. 2021, 143, 106231. [Google Scholar] [CrossRef] [Scilit]
- Volk, M.; Yuksel, O.; Baran, I.; Hattel, J.H.; Spangenberg, J.; Sandberg, M. Cost-efficient, automated, and sustainable composite profile manufacture: A review of the state of the art, innovations, and future of pultrusion technologies. Compos. Part B Eng. 2022, 246, 110135. [Google Scholar] [CrossRef] [Scilit]
- Minchenkov, K.; Vedernikov, A.; Safonov, A.; Akhatov, I. Thermoplastic Pultrusion: A Review. Polymers 2021, 13, 180. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Minchenkov, K.; Gusev, S.; Rogozheva, A.; Tronin, A.; Diatlova, M.; Safonov, A. Pultrusion of thermoplastic composites with mechanical properties comparable to industrial thermoset profiles. Compos. Commun. 2023, 44, 101766. [Google Scholar] [CrossRef] [Scilit]
- Tipboonsri, P.; Pramoonmak, S.; Uawongsuwan, P.; Memon, A. Optimization of Thermoplastic Pultrusion Parameters of Jute and Glass Fiber-Reinforced Polypropylene Composite. Polymers 2024, 16, 83. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Wei, Y.; Jin, X.; Luo, Q.; Li, Q.; Sun, G. Adhesively bonded joints—A review on design, manufacturing, experiments, modeling and challenges. Compos. Part B Eng. 2024, 276, 111225. [Google Scholar] [CrossRef] [Scilit]
- Miao, T.; Wang, W.; Zhai, Z.; Ding, Y. Effect of Injection Overmolding Parameters on the Interface Bonding Strength of Hybrid Thermoset–Thermoplastic Composites. Polymers 2023, 15, 2879. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Guo, J.; Zhan, L.; Ma, B.; Zhang, D.; Fan, Y.; Yao, S.; Feng, J. A review on failure mechanism and mechanical performance improvement of FRP-metal adhesive joints under different temperature-humidity. Thin-Walled Struct. 2023, 188, 110788. [Google Scholar] [CrossRef] [Scilit]
- Rodrigues, V.C.M.B.; Kasaei, M.M.; Marques, E.A.S.; Carbas, R.J.C.; da Silva, L.F.M. Adhesive bonding in automotive battery pack manufacturing and dismantling: A review. Discov. Mech. Eng. 2025, 4, 25. [Google Scholar] [CrossRef] [Scilit]
- Huntsman. ARALDITE® 2019 A/B Technical Data Sheet. Available online: https://products.huntsman.com/documents/87762bae-6779-43cd-b0cc-cb03a185116a (accessed on 31 July 2026).
- Xu, J.; Geier, N.; Shen, J.; Krishnaraj, V.; Samsudeensadham, S. A review on CFRP drilling: Fundamental mechanisms, damage issues, and approaches toward high-quality drilling. J. Mater. Res. Technol. 2023, 24, 9677–9707. [Google Scholar] [CrossRef] [Scilit]
- Rahul, K.; Yudhanto, A.; Ravindranath, P.K.; Jack, D.A. Progressive damage modeling in open hole composite laminates with ultrasound-informed drilling-induced delamination. Compos. Part A Appl. Sci. Manuf. 2024, 184, 108262. [Google Scholar] [CrossRef] [Scilit]
- Loutas, T.; Tsokanas, P.; Kostopoulos, V.; Nijhuis, P.; van den Brink, W.M. Mode I fracture toughness of asymmetric metal-composite adhesive joints. Mater. Today Proc. 2021, 34, 250–259. [Google Scholar] [CrossRef] [Scilit]
- Flaherty, N. Lightweight EV Battery Enclosures: Aluminium, Steel, Composites. Available online: https://www.emobility-engineering.com/lightweight-ev-battery-enclosures-aluminium-steel-composites/ (accessed on 31 July 2026).
- Zhang, X.; Lin, Q.; Xiao, Y.; Jia, L.; Yang, T.; Wang, L.; Ma, Q.; Wang, B. Top-Down Design Approach of Lightweight Composite Battery Pack Enclosure for Electric Vehicles Based on Numerical Modeling and Topology Optimization. Polymers 2025, 17, 2897. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Binetruy, C.; Hilaire, B.; Pabiot, J. Tow Impregnation Model and Void Formation Mechanisms During RTM. J. Compos. Mater. 1998, 32, 223–245. [Google Scholar] [CrossRef] [Scilit]
- Chen, Z.; Peng, L.; Xiao, Z. Experimental Characterization and Numerical Simulation of Voids in CFRP Components Processed by HP-RTM. Materials 2022, 15, 5249. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Neunkirchen, S.; Blößl, Y.; Schledjewski, R. A porous capillary tube approach for textile saturation. Compos. Sci. Technol. 2022, 230, 109450. [Google Scholar] [CrossRef] [Scilit]
- Protz, R.; Kosmann, N.; Gude, M.; Hufenbach, W.; Schulte, K.; Fiedler, B. Voids and their effect on the strain rate dependent material properties and fatigue behaviour of non-crimp fabric composites materials. Compos. Part B Eng. 2015, 83, 346–351. [Google Scholar] [CrossRef] [Scilit]
- Chen, J.; Yu, Z.; Jin, H. Nondestructive testing and evaluation techniques of defects in fiber-reinforced polymer composites: A review. Front. Mater. 2022, 9, 986645. [Google Scholar] [CrossRef] [Scilit]
- Cui, X.; Yu, Y.; Liu, Q.; Liu, X.; Qing, X. Full-field monitoring of the resin flow front and dry spot with noninvasive and embedded piezoelectric sensor networks. Smart Mater. Struct. 2023, 32, 085021. [Google Scholar] [CrossRef] [Scilit]
- Li, H.; Li, F.; Zhu, L. Effect of Resin-Missing Defects on Tensile Behavior of Carbon Fiber/Epoxy Composites. Polymers 2024, 16, 348. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Pang, X.; Chen, X.; He, Y.; Zhang, S.; Wang, Y.; Fan, Z.; Li, X. Effect of resin-rich areas on failure behavior of unidirectional CFRP under transverse pure shear. Comput. Mater. Sci. 2023, 219, 112023. [Google Scholar] [CrossRef] [Scilit]
- Ge, L.; Yu, M.; Fang, L.; Liu, X.; Ren, M.; Sun, J. Tensile properties and failure mechanism of carbon fiber/epoxy composite with resin-rich defects. Acta Mater. Compos. Sin. 2022, 39, 4961–4971. (In Chinese) [Google Scholar] [CrossRef]
- Mahmood, A.S.; Summerscales, J.; James, M.N. Resin-Rich Volumes (RRV) and the Performance of Fibre-Reinforced Composites: A Review. J. Compos. Sci. 2022, 6, 53. [Google Scholar] [CrossRef] [Scilit]
- Stelzer, P.S.; Plank, B.; Maurer, J.; Tiefenthaler, M.; Major, Z. Process-induced failure mode transition of compression molded discontinuous carbon fiber composites: From coupon to component level. Compos. Part B Eng. 2022, 242, 110021. [Google Scholar] [CrossRef] [Scilit]
- Chai, B.; Eisenbart, B.; Nikzad, M.; Fox, B.; Blythe, A.; Blanchard, P.; Dahl, J. A novel heuristic optimisation framework for radial injection configuration for the resin transfer moulding process. Compos. Part A Appl. Sci. Manuf. 2023, 165, 107352. [Google Scholar] [CrossRef] [Scilit]
- Pérez-de-Eulate, N.G.; Ares Elejoste, P.; Goenaga, G.; Urrutxua, M.; Vallejo, F.J.; Ballestero, J.; Allue, A.; Gómez-Alonso, J.L. On the Influence of Flame-Retardant Additives on UV-Curable Thermosetting Glass Fiber-Reinforced Composites. Polymers 2023, 15, 240. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Xu, J.; Yin, Y.; Paulo Davim, J.; Li, L.; Ji, M.; Geier, N.; Chen, M. A critical review addressing drilling-induced damage of CFRP composites. Compos. Struct. 2022, 294, 115594. [Google Scholar] [CrossRef] [Scilit]
- Qin, G.; Zheng, L.; Mi, P.; Zhu, Y.; Li, M.; Na, J.; Wang, Y. Influence of single or multi-factor coupling of temperature, humidity and load on the aging failure of adhesively bonded CFRP/aluminum alloy composite joints for automobile applications. Int. J. Adhes. Adhes. 2023, 123, 103345. [Google Scholar] [CrossRef] [Scilit]
- Vigón, P.; Argüelles, A.; Mollón, V.; Lozano, M.; Bonhomme, J.; Viña, J. Study of the Influence of the Type of Aging on the Behavior of Delamination of Adhesive Joints in Carbon-Fiber-Reinforced Epoxy Composites. Materials 2022, 15, 3669. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Vigón, P.; Argüelles, A.; Lozano, M.; Viña, J. Mode II Delamination Under Static and Fatigue Loading of Adhesive Joints in Composite Materials Exposed to Saline Environment. Materials 2023, 16, 7606. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Liu, J.; Xue, Y.; Dong, X.; Fan, Y.; Hao, H.; Wang, X. Review of the surface treatment process for the adhesive matrix of composite materials. Int. J. Adhes. Adhes. 2023, 126, 103446. [Google Scholar] [CrossRef] [Scilit]
- Chen, H.; Wang, D.; Na, J.; Chen, X. Effect of sealing treatment on mechanical properties of CFRP-Aluminum alloy single lap joints. Int. J. Adhes. Adhes. 2022, 119, 103236. [Google Scholar] [CrossRef] [Scilit]
- Wang, B.; Fan, S.; Chen, J.; Yang, W.; Liu, W.; Li, Y. A review on prediction and control of curing process-induced deformation of continuous fiber-reinforced thermosetting composite structures. Compos. Part A Appl. Sci. Manuf. 2023, 165, 107321. [Google Scholar] [CrossRef] [Scilit]
- Hwang, S.-F. An Overview of Angle Deviations of Fiber-Reinforced Polymer Composite Angular Laminates. Materials 2023, 16, 4844. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Traiforos, N.; Matveev, M.; Chronopoulos, D.; Turner, T. Spring-in of composite L-shape specimens: An experimental and numerical investigation. Compos. Struct. 2023, 310, 116772. [Google Scholar] [CrossRef] [Scilit]
- Parambil, N.K.; Chen, B.R.; Gillespie, J.W. Process-induced residual stress in a single carbon fiber semicrystalline polypropylene thin film. Compos. Part A Appl. Sci. Manuf. 2024, 178, 107969. [Google Scholar] [CrossRef] [Scilit]
- Barcenas, L.; Khoun, L.; Hubert, P. Thermoviscoelastic modelling of highly reactive thermoset resins for liquid moulding applications. Compos. Part A Appl. Sci. Manuf. 2024, 185, 108350. [Google Scholar] [CrossRef] [Scilit]
- Cameron, C.; Hozić, D.; Stig, F.; van der Veen, S. A method for optimization against cure-induced distortion in composite parts. Struct. Multidiscip. Optim. 2023, 66, 51. [Google Scholar] [CrossRef] [Scilit]
- Zhang, Y.; An, L.; Zhao, C. Predicting Curing Distortion in Composite Manufacturing—A Fast and Cost-Efficient Numerical Simulation Method. Polymers 2024, 16, 3597. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Maes, V.K.; Potter, K.; Kratz, J. Features and defects characterisation for virtual verification and certification of composites: A review. Compos. Part B Eng. 2022, 246, 110282. [Google Scholar] [CrossRef] [Scilit]
- Shen, H.; Yao, L.; Legrand, X.; Wang, P. Characterization of wrinkle morphologies by surface waviness evaluation method during deep forming of multilayer composite preforms. Compos. Struct. 2023, 306, 116586. [Google Scholar] [CrossRef] [Scilit]
- Codolini, A.; Chen, S.; Lawrence, G.; Harper, L.; Sutcliffe, M. Characterisation of process-induced variability in wrinkle defects during double diaphragm forming of non-crimp fabric. Compos. Part B Eng. 2024, 281, 111549. [Google Scholar] [CrossRef] [Scilit]
- Chen, L.; Miao, L.; Xu, Q.; Yang, Q.; Zhu, W.; Ke, Y. Damage and failure mechanisms of CFRP due to manufacturing induced wrinkling defects. Compos. Struct. 2023, 326, 117624. [Google Scholar] [CrossRef] [Scilit]
- Scheuring, B.M.; Christ, N.; Blarr, J.; Liebig, W.V.; Hohe, J.; Montesano, J.; Weidenmann, K.A. Experimental and homogenized orientation-dependent properties of hybrid long fiber-reinforced thermoplastics. Int. J. Mech. Sci. 2024, 280, 109470. [Google Scholar] [CrossRef] [Scilit]
- Trenam, A.; Aza, C.; Jones, C.; Lawrence, G.; Harper, L.; Rhead, A.; Loukaides, E.G.; Butler, R. An analytical model for wrinkle-free forming of composite laminates. Compos. Part A Appl. Sci. Manuf. 2024, 186, 108386. [Google Scholar] [CrossRef] [Scilit]
- Hall, M.; Zeng, X.; Shelley, T.; Schubel, P. Effects of through-thickness dielectric sensor on carbon fibre epoxy cure monitoring. Compos. Part A Appl. Sci. Manuf. 2024, 182, 108168. [Google Scholar] [CrossRef] [Scilit]
- Peng, Y.; Li, M.; Yang, X. Void formation and suppression in CFRP laminate using newly designed ultrasonic vibration assisted RTM technique. Compos. Struct. 2024, 329, 117796. [Google Scholar] [CrossRef] [Scilit]
- Yu, Y.; Cui, X.; Liang, Z.; Qing, X.; Yan, W. Monitoring of three-dimensional resin flow front using hybrid piezoelectric-fiber sensor network in a liquid composite molding process. Compos. Sci. Technol. 2022, 229, 109712. [Google Scholar] [CrossRef] [Scilit]
- Fernández-León, J.; Keramati, K.; Baumela, L.; González, C. A digital twin for smart manufacturing of structural composites by liquid moulding. Int. J. Adv. Manuf. Technol. 2024, 130, 4679–4697. [Google Scholar] [CrossRef] [Scilit]
- Zhu, J.; Droste, D.; Dimassi, A.; Herrmann, A.S. A neural-network-assisted method for flow-front estimation in resin transfer molding using pressure sensors. J. Compos. Mater. 2022, 56, 2979–2993. [Google Scholar] [CrossRef] [Scilit]
- Causon, M.; Iglesias, M.; Matveev, M.; Endruweit, A.; Tretyakov, M. Real-time Bayesian inversion in resin transfer moulding using neural surrogates. Compos. Part A Appl. Sci. Manuf. 2024, 185, 108355. [Google Scholar] [CrossRef] [Scilit]
- Mortada, H.; El Mousharrafie, S.; Mahfoud, E.; Harb, M. Noncontact nondestructive ultrasonic techniques for manufacturing defects monitoring in composites: A review. Struct. Health Monit. 2024, 23, 1969–1997. [Google Scholar] [CrossRef] [Scilit]
- Huang, J.; Wei, Q.; Zhuo, L.; Zhu, J.; Li, C.; Wang, Z. Detection and quantification of artificial delaminations in CFRP composites using ultrasonic thermography. Infrared Phys. Technol. 2023, 130, 104579. [Google Scholar] [CrossRef] [Scilit]
- Marani, R.; Campos-Delgado, D.U. Depth classification of defects in composite materials by long-pulsed thermography and blind linear unmixing. Compos. Part B Eng. 2023, 248, 110359. [Google Scholar] [CrossRef] [Scilit]
- Eliasson, S.; Hultgren, G.; Wennhage, P.; Barsoum, Z. Numerical fatigue assessment of a cross-ply carbon fiber laminate using a probabilistic framework. Compos. Part B Eng. 2024, 281, 111514. [Google Scholar] [CrossRef] [Scilit]
- Eliasson, S.; Hultgren, G.; Barsoum, Z.; Wennhage, P. Probabilistic fatigue strength assessment of cross-ply laminates: Exploring effects of manufacturing defects through a two-scale modeling approach. Compos. Struct. 2024, 330, 117844. [Google Scholar] [CrossRef] [Scilit]
- Facciotto, S.; Simacek, P.; Advani, S.G.; Pickett, A.; Middendorf, P. Modeling formation and evolution of voids in unsaturated dual scale preforms in Resin Transfer Molding processes. Compos. Part A Appl. Sci. Manuf. 2023, 173, 107675. [Google Scholar] [CrossRef] [Scilit]
- Wang, Y.; Xu, S.; Bwar, K.; Eisenbart, B.; Lu, G.; Belaadi, A.; Fox, B.; Chai, B. Application of machine learning for composite moulding process modelling. Compos. Commun. 2024, 48, 101960. [Google Scholar] [CrossRef] [Scilit]
- Mendikute, J.; Baskaran, M.; Llavori, I.; Zugasti, E.; Aretxabaleta, L.; Aurrekoetxea, J. Predicting the effect of voids generated during RTM on the low-velocity impact behaviour by machine learning-based surrogate models. Compos. Part B Eng. 2023, 260, 110790. [Google Scholar] [CrossRef] [Scilit]
- Wang, J.; Schutzeichel, M.; Plaumann, B.; Kletschkowski, T.; Panesar, A. Multidisciplinary design optimisation of lattice-based battery housing for electric vehicles. Sci. Rep. 2024, 14, 12265. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Sheng, L.; Lan, H.; Tao, B.; Zhang, Z.; Wang, H. Anisotropic thermal conductivity quantification in prismatic lithium-ion batteries. J. Energy Storage 2026, 162, 122112. [Google Scholar] [CrossRef] [Scilit]
- Qi, W.; Liu, Y.; Wang, X.; Ge, S.; Yu, J.; He, Z.; Tuo, J.; Wang, H.; Zhou, S.; Jin, C.; et al. Performance enhancement of battery thermal management based on liquid cooling plate channels embedded with non-uniform spiral fin structures. Appl. Therm. Eng. 2026, 300, 131501. [Google Scholar] [CrossRef] [Scilit]
- Lei, S.; Lan, H.; Tao, B.; Zhang, C.; Zhang, X.; Wang, L. Experiments on liquid-immersed thermal runaway management for large energy-stored lithium-ion battery modules. Therm. Sci. Eng. Prog. 2025, 68, 104347. [Google Scholar] [CrossRef] [Scilit]
- Yuan, M.; Li, Z.; Teng, Z. Progress and prospects of recycling technology for carbon fiber reinforced polymer. Front. Mater. 2024, 11, 1484544. [Google Scholar] [CrossRef] [Scilit]
- Pepó, M.; Fullér, S.; Cseke, T.; Weltsch, Z. Advances in Standardised Battery Testing for Enhanced Safety and Innovation in Electric Vehicles: A Comprehensive Review. Batteries 2025, 11, 157. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.