Fabrication of Superhydrophobic Radiative Heat-Dissipating Conductors with Porous Structures and Its Thermal Dissipation Performance

,
,
,
,
,
,
and
1
Institute of Electric Power Science of Guizhou Power Grid Co., Ltd., Guiyang 550002, China
2
Anshun Power Supply Bureau of Guizhou Power Grid Co., Ltd., Anshun 561000, China
3
College of Materials Science and Engineering, Chongqing University, Chongqing 400030, China
*
Author to whom correspondence should be addressed.
This article belongs to the Special Issue Durability of Transmission Lines

Abstract

Enhancing the ampacity of existing overhead transmission conductors through surface heat-dissipation regulation is important for grid capacity expansion. Herein, a superhydrophobic radiative heat-dissipating conductor was fabricated by combining phosphoric acid anodization with low-surface-energy modification. Porous anodic aluminum oxide (AAO) layers were in situ constructed on ACSR conductors under different anodizing current densities and oxidation times, followed by modification with hexadecyltrimethoxysilane or 1H,1H,2H,2H-perfluorodecyltrimethoxysilane to obtain H-AAO and F-AAO conductors, respectively. The surface morphology, optical properties, wettability, electrical resistance, current-induced temperature rise, and aging stability were systematically evaluated. The porous AAO layer enhanced the broadband infrared emissivity of the conductor surface while maintaining relatively high solar-band reflectance. The F-AAO conductor exhibited a water contact angle of 164.9° and a sliding angle of 1.8°, confirming excellent super-hydrophobicity. At 450 A, the steady-state temperature of the F-AAO conductor decreased from 106.85 °C for the Bare conductor to 75.34 °C. Under a 70 °C temperature limit, the allowable current increased from 343.58 to 431.57 A, corresponding to a 25.6% enhancement. Moreover, the F-AAO conductor retained stable heat-dissipation performance after 28 days of thermal aging. These findings demonstrate that anodization-assisted surface engineering is a feasible strategy for improving radiative heat dissipation, environmental adaptability, and current-carrying performance of overhead transmission conductors.

1. Introduction

In the coming decades, the continued electrification of society is expected to further drive the growth of electricity demand, making grid upgrading and capacity expansion essential for improving power delivery capability and operational reliability [1,2,3]. During peak-load periods, insufficient transmission capacity may lead to line overloading, resulting in power curtailment, outages, and even conductor overheating and line failures, thereby posing serious risks to the safe operation of power grids [4]. Therefore, enhancing the transmission capacity of existing power lines has become a critical issue in power system upgrading. As the primary current-carrying component of overhead transmission lines, the thermal stability and ampacity of transmission conductors largely determine the power transfer capability of the line.
Aluminum conductor steel-reinforced (ACSR) conductors are currently among the most widely used overhead transmission conductors worldwide. They typically consist of a steel core that provides mechanical strength and aluminum strands that provide electrical conductivity [2,5]. However, the mechanical properties of aluminum strands deteriorate at elevated temperatures, which increases conductor sag and associated safety risks. Consequently, many countries have imposed explicit limits on the maximum allowable operating temperature of ACSR conductors. For example, in China, the maximum allowable operating temperature of ACSR conductors is specified as 70 °C, which in turn limits their ampacity. To address this issue, previous studies have mainly focused on improving the high-temperature mechanical performance of aluminum strands and employing high-strength, low-sag cores, leading to the development of high-temperature low-sag (HTLS) conductors that can operate at higher temperatures while maintaining acceptable sag levels [1,6]. Representative examples include ACCR conductors [7,8], ACCC conductors [3,9], and ACSS conductors [10]. HTLS conductors can operate at temperatures above 200 °C and have been demonstrated to substantially enhance the ampacity of transmission lines. However, compared with conventional ACSR conductors, some HTLS conductors suffer from higher material costs, more stringent requirements for fittings and installation procedures, and the need for further refinement of long-term service-life assessment systems [11,12,13]. In addition, elevated operating temperatures increase conductor resistance and line losses, thereby raising operating costs. Therefore, it is of great significance to develop low-cost and easily implementable technical approaches that can enhance conductor ampacity within existing operating-temperature limits.
According to conductor ampacity calculation standards such as IEEE Std 738 [14] and CIGRE 601 [15], conductor ampacity is jointly governed by ambient temperature, conductor temperature, solar irradiance, surface emissivity, solar absorptivity, and related factors. From the perspective of thermal equilibrium, the steady-state operating temperature of an overhead conductor is determined by the balance between heat generation and heat dissipation. Heat generation mainly originates from Joule heating induced by current flow through the conductor, whereas heat dissipation primarily includes convective cooling and thermal radiation [16,17]. Compared with external conditions such as ambient temperature, wind speed, and solar irradiance, the optical properties of the conductor surface, particularly infrared emissivity and solar reflectance, are key parameters that can be tailored through surface engineering [18]. Increasing infrared emissivity enhances radiative heat dissipation, while increasing solar reflectance helps reduce solar heat gain; together, these effects influence the thermal equilibrium temperature and allowable ampacity of the conductor. Previous studies have shown that, at a current of 400 A, an ACSR conductor (135-AL1/22-ST1A) with a surface emissivity of 0.74 exhibited an operating temperature approximately 12 °C lower than that of the same conductor with an emissivity of 0.26. At a maximum operating temperature of 80 °C, its allowable current increased from 381 to 436 A, corresponding to an improvement of 14.4% [19]. Enhancing the surface emissivity of conductors can strengthen radiative heat dissipation without additional energy input and effectively increase ampacity under a fixed operating-temperature limit. These findings indicate that improving the radiative heat-dissipation performance of aluminum stranded conductors is a highly promising strategy for increasing the ampacity of overhead transmission lines.
Over the past decades, radiative heat-dissipation surfaces have attracted considerable attention because they can enhance thermal radiation without requiring additional energy input. Various strategies, including multilayer architectures [20], porous structures [21,22], polymer coatings [23,24], and metamaterials [25,26], have been developed to tailor the spectral response of materials and thereby improve radiative heat dissipation or passive radiative cooling performance. However, these approaches generally rely on precision fabrication equipment, complex processing procedures, or externally applied functional coatings, making it difficult to simultaneously meet the requirements of overhead transmission conductors for low cost, scalable fabrication, and long-term service stability. Anodic aluminum oxide (AAO) can be formed in situ on the surface of aluminum and its alloys as a structurally tunable alumina layer. Owing to its simple processing, relatively low cost, and controllable structural parameters, AAO has been widely used to regulate the optical and thermal-radiative properties of aluminum surfaces [27,28,29]. Zhang et al. [30] increased the surface emissivity of an aluminum heat sink from 0.14 to 0.92 through anodic oxidation, with radiative heat dissipation contributing 41% of the total heat dissipation. Lee et al. [31] prepared AAO layers using oxalic acid and sulfuric acid electrolytes, obtaining aluminum surfaces with emissivity of 0.87 and 0.74, respectively, and further analyzed the influence of anodizing conditions on AAO emissivity. Yang et al. [32] achieved daytime passive radiative cooling using AAO, with an emissivity of 0.98 in the 8–13 μm atmospheric window. These studies demonstrate that AAO is an effective surface-engineering approach for improving the infrared emissivity and radiative heat-dissipation capability of aluminum-based materials. However, for outdoor overhead transmission conductor applications, radiative cooling surfaces are continuously exposed to rainwater, dust, and pollutants. Surface contamination and liquid retention may alter their spectral response, thereby weakening their photothermal regulation and radiative heat-dissipation performance [33,34,35]. Therefore, imparting anti-wetting and self-cleaning capabilities to AAO while preserving its high infrared emissivity is of great importance for improving its outdoor service stability.
In this work, we propose an anodization-assisted surface engineering strategy to fabricate superhydrophobic radiative heat-dissipating conductors. Porous AAO layers were first constructed in situ on the aluminum outer strands of conductors by phosphoric acid anodization under different current densities and oxidation times. The anodized conductors were then modified with HDTMS or FAS to reduce the surface energy, yielding H-AAO and F-AAO conductors, respectively. The untreated conductor is referred to as the blank, and the anodized conductor without low-surface-energy modification is denoted as AAO. The effects of anodization parameters and surface modification on surface morphology, optical properties, wettability, electrical resistance, current-induced temperature rise, and aging stability were systematically investigated. This study aims to clarify the relationship between porous AAO-based surface regulation and conductor heat-dissipation performance, and to provide a feasible approach for improving the current-carrying capacity and environmental adaptability of overhead transmission conductors.

2. Materials and Methods

2.1. Materials and Fabrication

Commercial ACSR conductors (JL/LB20A 120/20, Chongqing Taishan Cable Co., Ltd., Chongqing, China) were used as the substrate. Each conductor consisted of seven aluminum-clad steel core wires and 26 aluminum strands, with a total cross-sectional area of 140 mm2 and a length of 1.5 m. Prior to anodization, the conductors were immersed in a 1 mol/L NaOH solution, prepared using sodium hydroxide purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. (Shanghai, China), for 15 min to remove surface contaminants and the native oxide layer. The conductors were then ultrasonically cleaned in distilled water for 20 min.
After cleaning, both ends of the conductors were sealed with waterproof tape to prevent the electrolyte from contacting the exposed steel core at the end faces during anodization. The treated conductors were clamped with titanium fixtures and used as the anode, while a ring-shaped graphite electrode was employed as the cathode. Anodization was carried out in a 0.3 mol/L H3PO4 electrolyte prepared from phosphoric acid supplied by Shanghai Aladdin Biochemical Technology Co., Ltd. (Shanghai, China). A DC power supply was used to maintain the current density in the range of 0.1–0.2 A/cm2, and the anodization time was varied from 10 to 30 min. During anodization, the electrolyte was continuously circulated and stirred using an industrial water chiller, and the temperature was maintained at 20 ± 3 °C.
After anodization, the conductors were removed from the electrolyte and ultrasonically cleaned in distilled water for 30 min to eliminate residual electrolyte. The samples were then dried in an oven at 70 °C for 2 h to obtain AAO conductors. To reduce the surface energy, the dried AAO conductors were immersed for 4 h in either a 20 wt.% HDTMS/ethanol solution or a 20 wt.% FAS/ethanol solution, prepared using hexadecyltrimethoxysilane (HDTMS) and 1H,1H,2H,2H-perfluorodecyltrimethoxysilane (FAS) purchased from Chengdu Chuandong Chemical Co., Ltd. (Chengdu, China), respectively. In the following sections, the untreated conductor is denoted as Blank and the anodized conductor as AAO, while the HDTMS-modified and FAS-modified AAO conductors are denoted as H-AAO and F-AAO, respectively.

2.2. Characterization

Scanning electron microscopy (SEM, Thermo Fisher Apreo 2, Waltham, MA, USA) equipped with energy-dispersive X-ray spectroscopy (EDS) was used to characterize the surface microstructure and elemental composition of the samples. SEM images were analyzed using ImageJ software (1.54g, National Institutes of Health, Bethesda, MD, USA) to determine the pore diameter and porosity of the AAO layers. Fourier-transform infrared spectroscopy (FT-IR, Bruker INENIO R, Bruker Optics GmbH, Ettlingen, Germany) equipped with a gold integrating sphere accessory (Bruker A562, Ettlingen, Germany) was used to characterize the optical properties and surface functional groups of the aluminum surfaces. The solar reflectance was measured using a UV–visible–NIR spectrophotometer (Shimadzu, Solidspec 3700, Kyoto, Japan). Surface wettability was evaluated using a contact angle goniometer (CA, TrueDrop SL200KS, Gothenburg, Sweden) with 3 μL water droplets. For each sample, measurements were performed at five different positions on the surface, and the average value was reported. In addition, diatomaceous earth was used as simulated dust to evaluate the self-cleaning performance of the conductors. Specifically, 0.5 g of diatomaceous earth was sprinkled onto the conductor surface, after which 3 mL of distilled water was gradually dropped onto the surface using a pipette. The self-cleaning process was recorded with a digital camera.
A current-induced temperature-rise test platform was constructed according to Ref. [19], and its schematic configuration is shown in Figure 1. The experiments were conducted in an indoor windless environment at a temperature of 18.0 ± 0.6 °C and a relative humidity of 70%. Three samples were prepared for each set of parameters, and the average value was reported. Before testing, copper lugs were crimped onto both ends of the conductor using hydraulic crimping pliers to ensure reliable electrical contact. To monitor the surface temperature distribution, four temperature sensors were evenly attached along the conductor surface at intervals of 30 cm using copper foil tape, and the temperature data were recorded in real time using a data acquisition system. The conductor was supported by insulating posts to minimize heat loss through conduction. During the experiment, a steady current of 100–450 A was applied. When the temperature remained stable for 30 min, with fluctuations within the allowable error range, the corresponding temperature was recorded as the steady-state temperature. The current was then increased stepwise, and the same procedure was repeated.
Figure 1. Schematic illustration of the current-induced temperature-rise test setup. The red/black lines indicate electrical connections, the blue lines indicate thermocouple connections, and the colored curves represent temperature-rise profiles.
The conductor resistance was measured using the four-terminal method. Before measurement, both ends of the specimen and the contact surfaces were mechanically polished with fine sandpaper to remove the oxide layer. The specimen was securely fixed in a four-terminal fixture, with the current terminals (I+ and I−) positioned on the outer sides and the voltage terminals (V+ and V−) positioned on the inner sides of the specimen. The distance between the two voltage probes was defined as the effective measurement length, L0. A high-precision DC resistance tester was then operated with the test current density set to 0.5 A/mm2. After the readings stabilized, the measured voltage drops, U, and injected current, I, were recorded, and the DC resistance at the ambient temperature was calculated according to Ohm’s law, Rx = U/I. To improve data reliability and minimize random errors, each measurement was repeated at least three times under the same environmental conditions, and the arithmetic mean was used. Finally, the average resistance was converted to the standard resistance at 20 °C.
To evaluate the stability of overhead transmission conductors under high-temperature service conditions, the conductor samples were subjected to accelerated thermal aging in a constant-temperature drying oven at 110 °C for 28 days. The samples were removed every 7 days and naturally cooled to room temperature before characterization. The performance stability of F-AAO under long-term thermal exposure was evaluated by measuring the contact angle, sliding angle, and ampacity at 70 °C before and after aging.

3. Results and Discussion

3.1. Microstructure and Optical Properties

Figure 2 shows that the current density and anodizing time jointly determine the openness and stability of the AAO pore structure. As the current density increased from 0.10 to 0.20 A/cm2, the average pore diameter increased from approximately 140–160 nm to 175–190 nm, while the porosity increased from approximately 38–45% to 49–53%. This indicates that a higher current density accelerates field-assisted oxide growth and pore-bottom dissolution, thereby promoting pore widening and pore-wall thinning. Meanwhile, the thickness of the oxide film was primarily governed by the anodizing time. When the anodizing time was 10 min, the thickness of AAO film was 13.4 ± 1.8 μm. As the anodizing time increased to 20 and 30 min, the film thickness increased to 24.2 ± 2.1 μm and 36.5 ± 2.7 μm, respectively. This process is consistent with the classical mechanism of dynamic competition between oxide formation and electrolyte-assisted dissolution in porous anodic aluminum oxide [36].
Figure 2. Surface microstructures of AAO prepared under different current densities and anodizing times.
At 0.10 A/cm2, progressively extending the anodizing time opened the pore structure and increased the oxide film thickness. However, after 30 min, both the pore diameter and porosity decreased slightly, accompanied by blurred pore openings, suggesting that further anodization provided limited structural benefit. At 0.15 A/cm2, the samples developed a relatively uniform and continuous honeycomb-like pore network, with the pore diameter increasing from approximately 165 to 180 nm and the porosity remaining stable at approximately 46–49%, indicating good structural controllability. In contrast, although 0.20 A/cm2 enabled the rapid formation of a highly porous structure within 10–20 min, pore-wall coarsening, local agglomeration, and blurred pore features appeared after 30 min, indicating that excessively high current density combined with prolonged anodization can induce over-dissolution and local structural degradation.
For heat dissipation from aluminum conductors, the advantage of AAO does not lie simply in increasing the pore size, but rather in constructing a stable Al2O3–air porous medium. This structure can enhance infrared absorption by increasing the interfacial area, extending the infrared optical path, and regulating the effective refractive index. According to Kirchhoff’s law, this corresponds to an increase in emissivity under thermal equilibrium, thereby enhancing radiative heat dissipation as described by qrad = εσ (Ts4-−Tair4). Therefore, for ampacity-enhancing heat-dissipation applications, AAO structural optimization should prioritize a stable porous network with open pore channels, continuous pore walls, and moderate porosity, rather than pursuing the largest pore size or the highest porosity. Overall, 0.15 A/cm2 for 20–30 min represents a more suitable structural-regulation window.
Figure 3 presents the infrared emissivity spectra of AAO surfaces prepared under different anodizing current densities and durations. Compared with the blank aluminum conductor, which showed consistently low emissivity over the 3–15 μm range, all anodized samples exhibited a sharp increase in emissivity near 7.5–8.0 μm and maintained a high plateau of approximately 85–90% in the 8–15 μm region. This result indicates that anodization effectively converts the low-emissivity metallic aluminum surface into a high-emissivity Al2O3-based dielectric surface. According to Kirchhoff’s law, the enhanced infrared absorption of the anodized layer corresponds to improved thermal emission capability [37]. The high emissivity in the 8–15 μm range can be mainly attributed to the infrared-active Al–O lattice vibrations of alumina, while the nano-porous structure further increases the optical path length through multiple reflection and scattering, thereby strengthening radiative heat dissipation [32].
Figure 3. Emissivity spectra of AAO surfaces prepared under different current densities and anodizing times: (a) 0.1 A/cm2 for 10–30 min, (b) 0.15 A/cm2 for 10–30 min, and (c) 0.2 A/cm2 for 10–30 min. The untreated blank conductor is shown for comparison.
Although the emissivity in the 8–15 μm region was relatively insensitive to the anodizing parameters, obvious differences appeared in the 3–8 μm region. At 0.10 A/cm2, the samples anodized for 10 and 20 min showed limited emissivity enhancement below 7 μm, whereas the 30 min sample exhibited a pronounced increase. This trend is closely related to the increase in AAO thickness from 13.4 ± 1.8 μm to 24.2 ± 2.1 μm and 36.5 ± 2.7 μm as the anodizing time increased from 10 to 20 and 30 min. A thicker and more open porous oxide layer provides a longer infrared interaction path and stronger absorption–scattering coupling, thus improving the short- to mid-infrared emissivity [38].
A similar but more distinct enhancement was observed at 0.15 A/cm2, especially for the 30 min sample, which showed higher and more continuous emissivity in the 3–8 μm range. This suggests that a moderate increase in current density promotes pore development and pore-wall dissolution, leading to a more effective broadband infrared-emitting structure. However, when the current density increased to 0.20 A/cm2, the emissivity no longer increased monotonically with anodizing time. The 20 min sample exhibited relatively high emissivity in the 3–8 μm region, whereas the 30 min sample showed a partial decrease. Combined with the SEM observations, this reduction can be attributed to excessive field-assisted dissolution, pore-wall coarsening, and local collapse of the porous framework. Therefore, high porosity alone does not necessarily lead to higher emissivity; instead, the radiative performance of AAO surfaces is governed by the balance among oxide thickness, pore openness, and structural integrity.
Overall, these results demonstrate that AAO layers can substantially enhance the infrared emissivity of aluminum conductors, particularly in the 8–15 μm region. The emissivity in the 3–8 μm range is more sensitive to anodizing conditions and porous morphology. Therefore, moderate current density combined with sufficient anodizing duration is more favorable for constructing broadband emissive AAO surfaces for radiative heat-dissipating conductors.
Figure 4 shows the solar reflectance spectra of AAO surfaces prepared under different anodizing conditions. Compared with the infrared emissivity spectra in Figure 3, the solar reflectance in the 0.3–2.5 μm range was more sensitive to changes in pore morphology and film thickness. This indicates that the photothermal regulation of AAO is not determined by pore enlargement alone, but by the combined effects of pore size, porosity, pore-wall integrity, and oxide-layer thickness.
Figure 4. Solar reflectance spectra of AAO surfaces prepared under different current densities and anodizing times: (a) 0.1 A/cm2 for 10–30 min, (b) 0.15 A/cm2 for 10–30 min, and (c) 0.2 A/cm2 for 10–30 min. The untreated blank conductor is shown for comparison.
At 0.10 A/cm2, the samples anodized for 10 and 20 min showed lower reflectance than the blank aluminum conductor, indicating that a thin or insufficiently developed porous layer may enhance light trapping and absorption losses. When the anodizing time was extended to 30 min, the reflectance increased markedly, especially in the near-infrared region. This improvement is related to the increase in AAO thickness from 13.4 ± 1.8 μm to 36.5 ± 2.7 μm, which provides stronger multiple scattering while maintaining effective infrared absorption [39].
At 0.15 A/cm2, the reflectance increased more clearly with anodizing time. The 20- and 30-min samples exceeded the blank sample in the near-infrared region, which is consistent with the formation of more open pore channels and relatively intact pore walls observed in Figure 2. Such a structure favors solar scattering and infrared emission simultaneously, explaining the balanced spectral performance shown in Figure 3 and Figure 4.
In contrast, the samples prepared at 0.20 A/cm2 exhibited a non-monotonic trend. The 20 min sample showed relatively high solar reflectance and infrared emissivity, whereas the 30 min sample displayed reduced reflectance. This decrease can be attributed to excessive field-assisted dissolution, pore-wall coarsening, pore coalescence, and partial collapse of the porous framework. These structural defects weaken the scattering ability of the AAO layer and increase optical trapping within the roughened channels.
Overall, the AAO surface should simultaneously possess high solar reflectance and high infrared emissivity for heat-dissipating conductor applications. Among the tested conditions, the sample anodized at 0.15 A/cm2 for 30 min achieved a favorable balance between pore development and structural integrity. This structure enhances infrared emission while preserving solar reflectance, making it more suitable for reducing solar heat gain and improving radiative heat dissipation of aluminum conductors.
The FT-IR spectra further confirm the successful grafting of low-surface-energy molecules onto the AAO surface (Figure 5). The unmodified AAO mainly exhibits absorption bands associated with the Al–O framework, with a relatively simple spectral profile. For H-AAO, the appearance of –CH2/–CH3 stretching vibration bands at 2923 and 2849 cm−1, together with the Si–O–Si/Si–O–Al-related absorption around 1090 cm−1, indicates that the silane molecules were bonded to surface hydroxyl groups on AAO through hydrolysis–condensation reactions [40,41]. In contrast, F-AAO shows distinct C–F stretching vibration bands at 1194 and 1140 cm−1, as well as characteristic absorption bands of fluorinated chains at 705 and 654 cm−1, demonstrating the effective incorporation of fluorinated silane onto the AAO surface [42].
Figure 5. FT−IR spectra of AAO with different surface modifiers. The red dotted lines indicate the characteristic absorption peaks of H-AAO, while the blue dotted lines indicate the characteristic absorption peaks of F-AAO.
Figure 6 further verifies the structural preservation of the AAO surface after FAS modification and the successful introduction of fluorinated elements. The SEM image (Figure 6a) shows that F-AAO retains a continuous and open honeycomb-like porous network, with no obvious pore blockage or film coverage, indicating that the low-surface-energy modification did not disrupt the Al2O3–air porous framework formed by anodization. In the EDS elemental mapping images, the Al and O signals are uniformly distributed across the entire region, corresponding to the AAO matrix. Meanwhile, the C and F signals are continuously distributed over the porous surface. Together with the characteristic C–F and Si–O–Si/Si–O–Al absorption bands observed in the FT-IR spectra (Figure 5), these results confirm that the fluorinated silane was successfully grafted onto the AAO pore walls and surface. Quantitative elemental analysis (Figure 6f) shows that the contents of Al, O, C, F, and Si are 39.0, 37.0, 12.5, 10.5, and 1.0 wt.%, respectively. The relatively low Si content is consistent with the ultrathin nature of the silane molecular layer, while the pronounced increase in F further demonstrates the effective incorporation of fluorinated groups.
Figure 6. Elemental distribution and quantitative elemental analysis of the F-AAO surface: (a) surface morphology of F-AAO; (b–e) spatial distribution of different surface elements on F-AAO; (f) surface elemental composition.
Figure 7 compares the infrared emissivity and solar reflectance of AAO and the low-surface-energy-modified samples. The results show that the low-surface-energy modification has only a minor effect on the emissivity and solar reflectance of AAO. Specifically, the emissivity spectra of F-AAO and H-AAO almost overlap with that of AAO, indicating that the silane molecular layers, as confirmed by the FT-IR (Figure 5) and EDS results (Figure 6), are sufficiently thin and do not block the AAO nanopores or disrupt the continuous open porous framework. Notably, F-AAO exhibits a slight enhancement in the 3–7 μm region, which can be associated with the mid-infrared vibrational absorption of C–F bonds. However, this enhancement serves only as a supplementary contribution to the dominant radiative effect of the AAO framework rather than acting as the primary mechanism.
Figure 7. Optical spectra of AAO with different surface modifications: (a) emissivity; (b) solar reflectance.

3.2. Ampacity and Electrical Resistance

Figure 8a shows digital photographs of different aluminum conductors. The blank exhibited a typical silvery-gray appearance with metallic luster, whereas the AAO, H-AAO, and F-AAO surfaces appeared relatively uniform gray-white, indicating that the anodized layer continuously covered the aluminum conductor surface. After modification, no obvious cracking, peeling, or local discoloration was observed, suggesting that the low-surface-energy modification did not compromise the macroscopic integrity of the AAO layer. Figure 8b,c directly verifies the enhancement of conductor heat-dissipation and ampacity performance enabled by AAO surface-structure regulation. The temperature of the blank increased rapidly with increasing current and reached 106.85 °C at 450 A. In contrast, the temperatures of the AAO, H-AAO, and F-AAO conductors decreased to 78.48, 77.28, and 75.34 °C, respectively, corresponding to temperature reductions of 28.37–31.51 °C. Accordingly, under a temperature limit of 70 °C, the allowable current of blank was only 343.58 A, whereas those of AAO, H-AAO, and F-AAO increased to 413.01, 418.54, and 431.57 A, corresponding to improvements of approximately 20.2%, 21.8%, and 25.6%, respectively. Combined with the results of electrical resistance (Figure 8d), the resistance of the anodized conductor changed only slightly compared with that of the blank (298.2 μΩ). The small resistance variation indicates that the anodic oxide layer does not significantly hinder current transport, because the current mainly flows through the metallic aluminum core rather than through the surface Al2O3 layer. Although anodization introduces an electrically insulating Al2O3 layer and consumes a small amount of surface aluminum, the oxide thickness is very small (<50 μm) relative to the overall conductor diameter (1.5 cm). These results indicate that the AAO layer formed by anodization significantly modifies the thermal-radiative heat-dissipation characteristics of the aluminum surface, enabling the conductor to reach thermal equilibrium at a lower temperature under the same current and to carry a higher current under the same temperature limit.
Figure 8. (a) digital photographs of different conductors, (b) Current-induced temperature-rise curves of conductors with different surface treatments, where the dotted line indicates the 70 °C temperature limit; (c) allowable current at 70 °C and conductor temperature at 450 A for conductors with different surface treatments, (d) electrical resistance of different conductors.
Figure 9 illustrates the mechanism by which AAO enhances the heat-dissipation performance of aluminum surfaces. The blank exhibit extremely low infrared emissivity, and therefore natural convective cooling is the dominant heat-dissipation pathway during operation. In contrast, porous AAO enhances infrared absorption through two synergistic effects, the intrinsic mid-infrared absorption arising from Al–O lattice vibrations, and the increased absorption probability induced by multiple scattering at pore wall/air interfaces, optical path extension, and an effective refractive-index gradient [43]. As a result, a high-emissivity plateau is established in the 8–15 μm region, while the broadband thermal emission capability in the 3–8 μm range is also improved. Because the conductor operating temperature is higher than the ambient temperature, enhanced infrared emission directly increases the radiative heat-loss, thereby reducing the steady-state temperature rise. The porous AAO layer formed by anodization markedly enhances infrared thermal emission and is therefore the primary reason for the reduced current-induced temperature rise and the increased allowable current at 70 °C. HDTMS modification largely preserves the radiative heat-dissipation capability of AAO, whereas FAS modification, without disrupting the porous structure, provides a slight emissivity gain through the infrared vibrational absorption of fluorinated functional groups.
Figure 9. Schematic illustration of the mechanism by which AAO enhances heat-dissipation performance.

3.3. Wettability and Self-Cleaning Propertiy

Figure 10 shows that anodization and low-surface-energy modification markedly altered the wetting behavior of the aluminum surface. The blank exhibited a water contact angle (CA) of 62.1°, indicating weak hydrophilicity. After anodization, the CA of AAO further decreased to 37.4°, suggesting that the porous Al2O3 surface did not become hydrophobic as a result of roughening. Instead, the polar Al–OH groups on the surface and the capillary infiltration effect of the nanopores promoted water spreading, consistent with the Wenzel model, in which surface roughness amplifies the intrinsic wettability of hydrophilic surfaces [44].
Figure 10. CA and SA of different surfaces: (a) water contact angle; (b) contact-angle images; (c) sliding angle.
After modification with HDTMS and FAS, the surface wettability changed fundamentally. The CAs of H-AAO and F-AAO increased to 157.1° and 164.9°, respectively. Meanwhile, the sliding angle (SA) decreased from >90° for the blank and AAO to 3.4° and 1.8°, respectively, indicating a substantial reduction in droplet adhesion and the formation of a stable superhydrophobic state. This transition originates from the chemical modification of the AAO pore walls and surface by low-surface-energy silane molecules. HDTMS introduces long alkyl chains that lower the surface energy, whereas FAS introduces fluorinated chains with even lower surface energy, enabling F-AAO to achieve the highest CA and the lowest SA.
Figure 11 further verifies the self-cleaning capability of the F-AAO surface. For the Blank conductor, obvious pollutant residues remained after rinsing with 3 mL water droplets, indicating that its hydrophilic surface and relatively strong adhesion limited the ability of flowing water to remove particulate contaminants, resulting in poor self-cleaning performance. In contrast, contaminants on the F-AAO surface were rapidly removed as water droplets rolled off, and the conductor surface was almost restored to a clean state after rinsing with 3 mL water droplets. This process demonstrates the typical superhydrophobic self-cleaning behavior of F-AAO. The underlying mechanism lies in the combined effect of the low-surface-energy fluorosilane layer and the porous AAO micro/nanostructure, which reduces the contact area between water droplets and the solid surface. As a result, rolling droplets can capture and carry away contaminant particles rather than spreading over the surface to form a water film.
Figure 11. Schematic illustration of the self-cleaning process of different conductors. The red dotted circles and box highlight the positions of water droplets, removed contaminants, and stain residues during the cleaning process.
Overall, for practical applications in overhead transmission conductors, AAO provides the basis for enhanced heat-dissipation performance but also renders the surface hydrophilic. Fluorosilane modification further converts the AAO surface into a superhydrophobic, low-adhesion interface. Therefore, F-AAO combines the heat-dissipation capability provided by the porous alumina layer with the self-cleaning ability enabled by fluorosilane modification, reducing the retention of water and contaminants on the conductor surface and thereby helping maintain stable radiative heat-dissipation performance during long-term service.

3.4. Durability

Figure 12 shows the performance evolution of F-AAO during accelerated thermal aging at 110 °C. As shown in Figure 12a, after 28 days of thermal aging, the CA of F-AAO changed only slightly from 164.9° to 164.8°, while the SA increased from 1.8° to 2.2°. Meanwhile, the allowable ampacity at the thermal equilibrium temperature of 70 °C remained approximately 430 A, with only minor fluctuations before and after aging. This result indicates that thermal aging did not significantly degrade the superhydrophobic state of the F-AAO surface or compromise its heat-dissipation and ampacity-enhancement capability. No significant deterioration in wettability was observed, demonstrating the excellent thermal-aging resistance of the F-AAO conductor. The excellent thermal stability of F-AAO can be mainly attributed to three factors. First, the fluor silane molecules form relatively stable chemical bonds with the AAO surface through Si–O–Al or Si–O–Si linkages. Second, the fluorinated chains possess low surface energy and high thermal stability, making them resistant to degradation at 110 °C. Third, the porous AAO framework remains structurally intact at this temperature, continuously supporting the Cassie–Baxter low-adhesion wetting state.
Figure 12. Evolution of F-AAO performance with thermal aging time: (a) water contact angle and sliding angle; (b) allowable current at 70 °C.

4. Conclusions

This study constructed an AAO functional layer with both high infrared emissivity and super-hydrophobicity on aluminum conductors through anodization combined with low-surface-energy modification. The results show that moderately increasing the current density and anodizing time promotes the formation of a continuous and open porous AAO structure, thereby enhancing infrared absorption and thermal emission. However, excessive anodization induces pore-wall dissolution, pore coalescence, and structural instability, which are unfavorable for optimizing photothermal performance. Therefore, the radiative heat-dissipation performance of AAO is governed by the pore structures.
Porous AAO substantially improves the radiative heat-dissipation capability of the aluminum surface, forming a high-emissivity plateau in the 8–15 μm region while increasing the emissivity in the 3–8 μm range. This enhancement is mainly attributed to the intrinsic infrared absorption of Al2O3, together with multiple scattering and optical path extension induced by the porous architecture. After HDTMS and FAS modification, the emissivity and solar reflectance of AAO were largely maintained, while the surface wettability changed from hydrophilic to superhydrophobic. In particular, F-AAO exhibited a water CA of 164.9° and a SA of 1.8°, indicating the lowest droplet adhesion.
Current-induced temperature-rise tests further confirm the effectiveness of this surface-engineering strategy. At 450 A, the temperature of the F-AAO conductor was 31.51 °C lower than that of the blank. Under an operating temperature limit of 70 °C, the allowable current increased from 343.58 to 431.57 A, corresponding to a 25.6% enhancement. In addition, F-AAO exhibited excellent super-hydrophobicity and self-cleaning performance, with no obvious performance degradation after 28 days of thermal aging. Therefore, the superhydrophobic AAO radiative heat-dissipation surface can significantly improve conductor ampacity without increasing the maximum operating temperature, providing a feasible strategy for capacity uprating of overhead transmission lines.

Author Contributions

Conceptualization, B.L. and Y.Y.; Methodology, Y.Y. and X.H.; validation, Z.G., Y.Y. and J.H.; formal analysis, B.L., J.B., Z.G.; investigation, L.Y., J.H. and T.Z.; resources, B.L. and Y.Y.; data curation, B.L.; writing—original draft preparation, B.L. and J.B.; writing—review and editing, B.L. and Y.Y.; supervision, Y.Y.; project administration, Y.Y. and X.H.; funding acquisition, B.L. and Y.Y. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the Electric Power Research Institute of Guizhou Power Grid Co., Ltd., China. Contract number 0666002024030103HX00003.

Institutional Review Board Statement

Not applicable.

Data Availability Statement

The raw/processed data required to reproduce these findings cannot be shared at this time due to legal or ethical reasons.

Acknowledgments

The author would like to thank the Key Laboratory of Ice Prevention & Disaster Reducing of China Southern Power Grid Co., Ltd. (Meihuashan Base) for its help in the current-induced temperature-rise test of aluminum conductors. Additionally, the authors would like to thank Jiaqi Jia from the Electron Microscope Center of Chongqing University for her help in taking micrographs of samples.

Conflicts of Interest

Authors Bo Li, Jie Bai, Zhengwei Guo, and Liuqing Yang are employed by the Institute of Electric Power Science of Guizhou Power Grid Co., Ltd. Author Jin Hu is employed by Anshun Power Supply Bureau of Guizhou Power Grid Co., Ltd. The remaining authors declare no conflict of interest. The authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.

Abbreviations

The following abbreviations are used in this manuscript:
HTLSHigh-temperature low-sag
ACCRAluminum conductor composite reinforced
ACCCAluminum conductor composite core
ACSSAluminum conductor steel supported
ACSRAluminum conductor steel-reinforced
AAOAnodic aluminum oxide

References

  1. Sergio, M.-S.; Andrea, M. Assessment of the influence of climate change on power grid transmission capacity. Sustain. Energy Grids Netw. 2025, 42, 101695. [Google Scholar] [CrossRef] [Scilit]
  2. Parvizi, P.; Mohammadi Amidi, A.; Jalilian, M.; Zangeneh, M.R.; Parvizi, H. High Temperature Low Sag Conductors: A Brief Review on Strategies Used To Prevent Destruction, and Maintenance Considerations. Trans. Indian Natl. Acad. Eng. 2025, 10, 271–292. [Google Scholar] [CrossRef] [Scilit]
  3. Parvizi, P.; Jalilian, M.; Dearn, K.D. Evaluating the mechanical and thermal performance of high-temperature low sag (HTLS) conductors: A comparative study of ACCC, ACSS, and ACSR conductors. Results Eng. 2025, 26, 104735. [Google Scholar] [CrossRef] [Scilit]
  4. Rashmi; Shivashankar, G.S.; Poornima. Overview of different overhead transmission line conductors. Mater. Today Proc. 2017, 4, 11318–11324. [Google Scholar] [CrossRef] [Scilit]
  5. Kopsidas, K.; Aqil, M.A.A.; Haldar, A.; Kavanagh, T. Evaluating Aeolian Vibration Performance of High-Temperature Low-Sag OHL Conductors. IEEE Trans. Power Deliv. 2022, 37, 1775–1784. [Google Scholar]
  6. Parvizi, P.; Jalilian, M.; Dearn, K.D. Beyond traditional conductors: Aluminum conductor composite core’s role in next-generation high temperature-low sag technologies—A review. Electr. Power Syst. Res. 2025, 239, 111251. [Google Scholar]
  7. Phillips, J.; Ryan, M.; Glass, D. Thinking outside the Box: Tennessee Valley Authority Uses the ACCR Conductor on a 500-kV Transmission Line. In Electrical Transmission and Substation Structures 2015; ASCE: Reston, VA, USA, 2015; pp. 227–236. [Google Scholar]
  8. Hu, X.; Wang, C.; Ma, G.; He, K. Effect of Er on Microstructure, Electrical Conductivity, Mechanical Properties, and Corrosion Resistance of an Al-Zr Alloy. J. Mater. Eng. Perform. 2025, 34, 6026–6034. [Google Scholar]
  9. Zhou, L.; Li, Z.; Ma, J.; Chen, R.; Wang, Q.; Pei, K.; Zhang, X.; Zhang, Y. Technical and Economic Analysis of ACCC Applied in UHV-DC Power Transmission Lines. In Proceedings of the 2019 4th International Conference on Intelligent Green Building and Smart Grid (IGBSG), Yichang, China, 6–9 September 2019; pp. 169–172. [Google Scholar]
  10. Thrash, F. ACSS/TW—An improved high temperature conductor for upgrading existing lines or new construction. In Proceedings of the 2001 Power Engineering Society Summer Meeting, Vancouver, BC, Canada, 15–19 July 2001; Conference Proceedings (Cat. No. 01CH37262); IEEE: Piscataway, NJ, USA, 2001; Volume 1, pp. 182–185. [Google Scholar]
  11. Parvizi, P.; Jalilian, M.; Mirazizi, P.S.; Zangeneh, M.R.; Amidi, A.M. Mechanical and physical properties of aluminum and its alloys for electrical conductors: A review. Next Mater. 2025, 9, 101090. [Google Scholar] [CrossRef] [Scilit]
  12. Li, B.; Hu, Q.; Guo, R.; Hu, J.; Fen, Z.; Hua, X.; Zhu, T.; Yuan, Y. A Review of the Developments in Capacity-Uprating Conductors for Overhead Transmission Lines. Coatings 2025, 15, 1203. [Google Scholar] [CrossRef] [Scilit]
  13. Sharma, A.; Gumaste, A.; Agrawal, P.; Thapliyal, S.; Gupta, S.; Haridas, R.S.; McWilliams, B.A.; Cho, K.C.; Mishra, R.S. Strength-conductivity synergy via lean alloy design: A study on novel solid stir extrusion of an Al-2Cu-0.1 Nb-0.15Zr (∼wt.%) alloy. J. Alloys Compd. 2024, 976, 173082. [Google Scholar]
  14. IEEE Std 738-2023 (Revision of IEEE Std 738-2012); IEEE Standard for Calculating the Current-Temperature Relationship of Bare Overhead Conductors. IEEE: Piscataway, NJ, USA, 2023.
  15. CIGRE Working Group B2. 12. Guide for Selection of Weather Parameters for Bare Overhead Conductor Ratings; Cigré: Paris, France, 2006. [Google Scholar]
  16. Li, J.; Lin, J.; Han, Y.; Zhu, L.; Chang, D.; Shao, C. Overload Risk Assessment of Transmission Lines Considering Dynamic Line Rating. Energies 2025, 18, 1822. [Google Scholar] [CrossRef] [Scilit]
  17. Wang, S.; Hu, H.; Li, L.; Wang, Y.; Ning, H. Dynamic Capacity Increasing Method For Transmission Lines. In Proceedings of the 2023 IEEE World Conference on Applied Intelligence and Computing (AIC), Varanasi, India, 29–30 July 2023; pp. 550–555. [Google Scholar]
  18. Xie, A.-Q.; Qiu, H.; Jiang, W.; Wang, Y.; Niu, S.; Zhang, K.-Q.; Ho, G.W.; Wang, X.-Q. Recent Advances in Spectrally Selective Daytime Radiative Cooling Materials. Nano-Micro Lett. 2025, 17, 264. [Google Scholar] [CrossRef] [Scilit]
  19. Riba, J.-R.; Liu, Y.; Moreno-Eguilaz, M. Analyzing the role of emissivity in stranded conductors for overhead power lines. Int. J. Electr. Power Energy Syst. 2024, 159, 110027. [Google Scholar] [CrossRef] [Scilit]
  20. Raman, A.P.; Anoma, M.A.; Zhu, L.; Rephaeli, E.; Fan, S. Passive radiative cooling below ambient air temperature under direct sunlight. Nature 2014, 515, 540–544. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  21. Wang, Y.; Chen, X.; Zhang, X.; Zang, J.; Lu, L.; Yuan, W. Biomimetic, Hierarchical-Porous Composite Aerogel Fiber with Spectral Selectivity and Water Microchannels for Synergistic Radiative-Evaporative Passive Cooling Textile. Small 2026, 22, e14581. [Google Scholar] [PubMed]
  22. Ding, D.; He, X.; Liang, S.; Wei, W.; Ding, S. Porous nanostructured composite film for visible-to-infrared camouflage with thermal management. ACS Appl. Mater. Interfaces 2022, 14, 24690–24696. [Google Scholar] [PubMed]
  23. Tang, C.; He, H.; Wu, E.; Li, H.; Hu, Y.; Liu, C.; Wang, X.; Zhuang, X. Radiative cooling PVDF aerogels with hierarchical porous structure for building energy savings. Colloids Surf. A Physicochem. Eng. Asp. 2025, 723, 137402. [Google Scholar] [CrossRef] [Scilit]
  24. Zhao, B.; Xuan, Q.; Xu, C.; Hu, M.; Dabwan, Y.N.; Pei, G. Considerations of passive radiative cooling. Renew. Energy 2023, 219, 119486. [Google Scholar] [CrossRef] [Scilit]
  25. Zhang, K.; Wu, B. Microscopic mechanism and applications of radiative cooling materials: A comprehensive review. Mater. Today Phys. 2025, 51, 101643. [Google Scholar]
  26. Bijarniya, J.P.; Sarkar, J.; Maiti, P. Review on passive daytime radiative cooling: Fundamentals, recent researches, challenges and opportunities. Renew. Sustain. Energy Rev. 2020, 133, 110263. [Google Scholar] [CrossRef] [Scilit]
  27. Yamanashi, M. Stable fabrication methods for thick porous anodic aluminum oxide films. J. Solid State Electrochem. 2026, 30, 1321–1331. [Google Scholar]
  28. Huang, C.H.; Sun, X.H.; Sun, Y.H. Effect of characteristic size on the effective thermal conductivity of anodic aluminum oxide (AAO) porous thin films. Adv. Mater. Res. 2012, 399, 641–645. [Google Scholar]
  29. Díaz-Lobo, A.; Martin-Gonzalez, M.; Song, Q.; Morales-Sabio, Á.; Retsch, M.; Manzano, C.V. Metallic coatings boost the cooling power of nanoporous alumina. ACS Appl. Eng. Mater. 2024, 2, 2069–2079. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  30. Zhang, Z.; Collins, M.; Lau, E.; Botting, C.; Bahrami, M. The Role of Anodization in Naturally Cooled Heat Sinks for Power Electronic Devices. J. Heat Transf. 2020, 142, 052901. [Google Scholar] [CrossRef] [Scilit]
  31. Lee, J.; Kim, D.; Choi, C.-H.; Chung, W. Nanoporous anodic alumina oxide layer and its sealing for the enhancement of radiative heat dissipation of aluminum alloy. Nano Energy 2017, 31, 504–513. [Google Scholar] [CrossRef] [Scilit]
  32. Fu, Y.; Yang, J.; Su, Y.; Du, W.; Ma, Y. Daytime passive radiative cooler using porous alumina. Sol. Energy Mater. Sol. Cells 2019, 191, 50–54. [Google Scholar] [CrossRef] [Scilit]
  33. Yang, Z.; Yang, Z.; Zhang, Z.; Wang, X.; Chen, Z.; Li, Y.; Cai, Y.; Zhang, H.; Liu, L.; Zhang, W.; et al. Daytime radiative cooling coating for cooling energy efficiency of conventional air conditioners. Appl. Therm. Eng. 2025, 261, 125060. [Google Scholar]
  34. Jalilian, M.; Riba, J.-R.; Parvizi, P. Aluminum conductor steel-supported conductors for the sustainable growth of power line capacity: A review and discussion. Materials 2024, 17, 4536. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  35. Chen, J.; Lu, L. Development of radiative cooling and its integration with buildings: A comprehensive review. Sol. Energy 2020, 212, 125–151. [Google Scholar] [CrossRef] [Scilit]
  36. Eessaa, A.K.; El-Shamy, A.M. Review on fabrication, characterization, and applications of porous anodic aluminum oxide films with tunable pore sizes for emerging technologies. Microelectron. Eng. 2023, 279, 112061. [Google Scholar] [CrossRef] [Scilit]
  37. He, X.; Li, Y.; Wang, L.; Sun, Y.; Zhang, S. High emissivity coatings for high temperature application: Progress and prospect. Thin Solid Films 2009, 517, 5120–5129. [Google Scholar] [CrossRef] [Scilit]
  38. Manzano, C.; Best, J.; Schwiedrzik, J.; Cantarero, A.; Michler, J.; Philippe, L. The influence of thickness, interpore distance and compositional structure on the optical properties of self-ordered anodic aluminum oxide films. J. Mater. Chem. C 2016, 4, 7658–7666. [Google Scholar] [CrossRef] [Scilit]
  39. Seman, M.H.A.; Gati, N.I.; Mahmud, A.H.; Jamil, Z.; Osman, N.; Low, K.-F.; Tseng, C.-J.; Jani, A.M.M. Nanopore architectures in anodic aluminum oxide: Effects of anodization voltage and time on planar and non-planar aluminum substrates. J. Porous Mater. 2026, 33, 907–924. [Google Scholar] [CrossRef] [Scilit]
  40. Ludwig, B. Infrared spectroscopy studies of aluminum oxide and metallic aluminum powders, part II: Adsorption reactions of organofunctional silanes. Powders 2022, 1, 75–87. [Google Scholar] [CrossRef] [Scilit]
  41. Celik, N.; Sezen, B.; Sahin, F.; Ceylan, A.; Ruzi, M.; Onses, M.S. Mechanochemical coupling of alkylsilanes to nanoparticles for solvent-free and rapid fabrication of superhydrophobic materials. ACS Appl. Nano Mater. 2023, 6, 14921–14930. [Google Scholar] [CrossRef] [Scilit]
  42. Meng, J.; Dong, X.; Zhou, H.; Liu, W.; Yin, Z. Investigation of Adhesive Resistance of Aluminum Alloy by Sandblasting and Electrochemical Machining. Micromachines 2017, 8, 91. [Google Scholar] [CrossRef] [Scilit]
  43. Abad, B.; Maiz, J.; Martin-Gonzalez, M. Rules to determine thermal conductivity and density of anodic aluminum oxide (AAO) membranes. J. Phys. Chem. C 2016, 120, 5361–5370. [Google Scholar] [CrossRef] [Scilit]
  44. Li, B.; Xiang, H.; Dai, X.; Zhu, T.; Hua, X.; Yuan, Y. A superhydrophobic anti-icing surface with a honeycomb nanopore structure. Coatings 2023, 13, 1971. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.