Highlights
What are the main findings?
- Eliminating the inter-bead valley requires the overlapping-side remelting zone to reach the apex of the previous bead.
- An optimum asymmetric thermal field exists when the widened-side width equals the overlapping distance.
- A ten-layer deposit shows no lack of fusion, and the layer flatness is better than 0.18 mm.
What are the implications of the main findings?
- The inter-bead valley is a heat and mass transfer issue under volume conservation.
- The required sub-current increment follows from a fitted widened-side width relation.
- Following the overlapping criterion along with edge wire feed compensation, the intra-layer height error does not accumulate.
Abstract
Surface flatness of each layer governs process stability and the forming quality of multi-layer multi-bead additive manufacturing, yet the inter-bead valley is unavoidable with the existing overlapping models: a symmetric arc cannot simultaneously satisfy volume conservation for a flat-top and promote the molten metal to fill the valley. In the twin-electrode gas tungsten arc additive manufacturing, this issue becomes acute at high deposition currents. An overlapping optimization method based on thermal field regulation is proposed. Unequal sub-currents applied to the two electrodes deflect the coupled arc towards the electrode carrying the smaller sub-current, extending the remelting zone on the overlapping side to the apex of the previous bead. The three-phase interfacial tension acts tangentially to that apex and drives the molten metal into the valley, thereby providing the missing transport mechanisms from the flat-top overlapping model and improving the layer flatness. The relationship between the sub-current increment and the widened-side width was established through regression analysis, and a parameter-planning algorithm was developed. Two-bead overlapping experiments were conducted with deposition sub-currents of 170 A, 200 A and 230 A, respectively. The intra-layer height error of the deposits was less than 0.15 mm, confirming the predictions. A ten-layer block component was deposited following the criterion along with a wire feed compensation strategy at the edge beads. The result showed no lack of fusion, and the intra-layer height error remained less than 0.18 mm rather than accumulating, validating the effectiveness of the criterion for multi-layer multi-bead additive manufacturing.
1. Introduction
Wire arc additive manufacturing (WAAM), which employs an electric arc as the heat source to melt a feed wire and builds components layer by layer along a planned path, has become one of the most rapidly developing metal additive manufacturing technologies in recent years [1,2]. Driven by the demands of the aviation, aerospace, shipbuilding and construction industries [3], the research focus of WAAM is shifting from multi-layer single-bead structures to multi-layer multi-bead components with more complex geometries, in which the buildable width is extended by overlapping adjacent beads, laying the foundation for the fabrication of thick and large-section parts.
The heat sources commonly used in WAAM include the gas metal arc (GMA) [4], the gas tungsten arc (GTA) [5] and the plasma arc (PA) [6]. Among them, the GTA offers a stable arc and a higher forming accuracy than the GMA and has therefore been widely adopted in additive manufacturing. Previous studies on GTA-based additive manufacturing have covered the effects of the process parameters on the bead geometry, the microstructure and the properties of the deposited parts [7,8,9], as well as the online measurement of the surface height and the closed-loop control of the forming dimensions [10]. However, to prevent humping and undercut defects caused by excessive arc pressure, the deposition current is generally limited to less than 200 A, which results in a low deposition rate. Therefore, improving the deposition rate of GTA-based additive manufacturing while ensuring the forming accuracy has become an urgent problem to be solved, especially for multi-layer multi-bead components.
To improve the productivity of GTA welding, Kobayashi et al. [11] proposed a high-efficiency twin-arc TIG process in 2004 for the construction of large storage tanks, demonstrating the potential of the twin-arc for high-productivity welding. Leng et al. [12] further developed this concept into a twin-electrode GTA process, in which two mutually insulated tungsten electrodes are mounted in a single welding torch and are controlled by two independent power sources. Under the action of the Lorentz force, the arcs generated by the two electrodes couple into a larger arc. They studied this coupled arc and concluded that its arc pressure is lower than that of the conventional GTA under the same welding parameters, so that a much larger current can be adopted without incurring humping and undercut defects. Schwedersky et al. [13] investigated the arc shape of the double-electrode process at different electrode distances using high-current values and found that, at a large electrode distance, the arc exhibits greater asymmetry as the travel speed increases; compared with conventional GTAW, the twin-electrode process can greatly increase the travel speed, indicating its great potential for expanding the application of GTA welding in high-productivity manufacturing. In recent years, this process has been extended to wire arc additive manufacturing, where the geometric characteristics of the deposited bead have been investigated [14]. Owing to its low arc pressure and enlarged process window, the twin-electrode GTA provides a promising route to improving the deposition rate and process stability of GTA-based additive manufacturing.
Since the twin-electrode process relaxes the arc-pressure limit on the welding current, a much higher deposition current can be adopted, which makes the surface flatness problem during overlapping more critical. A higher current brings a higher deposition rate and hence a larger bead geometry. On the one hand, it increases the volume of molten metal that must be redistributed during overlapping. If this metal cannot be delivered in time, the valley on the surface of the layer is deepened rather than filled. On the other hand, the sidewall of the larger previous bead continuously conducts heat away, aggravating the local underheating at the overlapping interface.
The inter-bead valley is essentially a local reduction in the deposited thickness: it deteriorates the surface flatness of the layer, acts as a stress-concentration notch, and provides a potential site for inter-bead lack of fusion, which severely degrades the interlayer bonding and the load-bearing capacity of the built component. Moreover, the surface height fluctuation accumulates layer by layer during multi-layer deposition, so that the distance between the torch and the deposit surface varies from layer to layer; the resulting fluctuation of the arc length destabilizes the deposition process and readily induces defects such as pores and collapse, thus threatening the continuity of the forming process. Therefore, how to eliminate the inter-bead valley and suppress the associated lack-of-fusion risk under a high-current, high-deposition-rate condition has become a key problem to be solved for multi-layer multi-bead wire arc additive manufacturing.
In multi-layer multi-bead deposition, each layer is formed by the overlapping of adjacent beads, and the overlapping quality of adjacent beads directly determines the surface morphology and dimensional accuracy of the built component. Considerable efforts have therefore been devoted to the modeling of bead overlapping.
The flat-top overlapping model was the first to be proposed and adopted. This model is fundamentally based on the principle of volume conservation, guaranteeing that the cross-sectional areas of the overlapping and valley regions remain equivalent. Cao et al. [15] simplified the cross-section of the bead profile as a sinusoidal curve and pointed out that the flattest single-layer multi-bead surface is obtained when the center distance of adjacent beads is 63.66% of the bead width. Xiong et al. [16] employed different heat sources and deposition parameters, and their experimental results indicated that the single-bead profile is close to a parabola. The best overlapping effect was obtained when the overlapping distance was 66.67% of the bead width.
Further studies have revealed that the flat-top overlapping model, by considering only volume conservation, deviates from the actual physical processes: since arc additive manufacturing is a non-equilibrium process, the molten metal often does not have enough time to flow into the inter-bead valley during overlapping. To address this issue, Ding et al. [17] found that, regardless of the overlapping distance, the deposited metal that fills the valley between the two beads is distributed tangentially along the profile of the overlapping bead. They suggested increasing the overlapping distance so that the height of the overlapping bead matches that of the previous bead. Otherwise, the deposited layer rises progressively in the direction of overlapping. The tangent overlapping model was proposed on this basis, giving an optimal overlapping distance of 73.8% of the bead width.
Fang et al. [18] studied the CMT-based additive manufacturing of 2319 aluminum alloy. On this basis, an inclined-top overlapping model was established, in which the optimal overlapping distance is 0.715 times the single-bead width. Hu et al. [19] fitted the bead profile with a rotated parabola and established a varying-cross-section multi-bead overlapping model for GMA-based additive manufacturing, with which the overlapping distance was optimized, and the forming quality was improved.
For twin-electrode GTA-based additive manufacturing, Han et al. [20] found that the three commonly used curve models (parabola, cosine, and circular arc) cannot well predict the bead section profile of this process, resulting in poor process stability and geometric accuracy. To solve this problem, the geometric characteristics of the twin-electrode GTA-AM bead section were first investigated, and an enhanced curve-fitting model, namely the power-function-curve model, was proposed. The applicable condition of the tangent overlapping model was then extended to the proposed power-function-curve-shaped bead section profile, and the derivation of the optimal overlapping coefficient was elaborated. Verification experiments showed that both the proposed curve-fitting model and the overlapping model can accurately predict the bead overlapping behavior with a maximum error of less than 6%, which is crucial for the process planning of twin-electrode GTA-AM.
In summary, the flat-top, inclined-top, tangent and power-function overlapping models, can guide the selection of the overlapping distance and improve the overlapping accuracy to a certain extent. However, they all treat the molten metal as a passive filler and do not actively intervene in the heat and mass transfer between adjacent beads during overlapping; the inter-bead valley can therefore only be minimized from a geometric point of view but is essentially not eliminated, and problems such as uneven upper surfaces of the deposited layer, inconsistent bead heights and the associated lack-of-fusion risk still need to be further solved.
The surface flatness problem of an overlapped layer is governed by the gravity and surface tension of the molten metal, both of which are closely related to the welding temperature field. In multi-bead overlapping, the subsequent bead is deposited against the sidewall of the previous bead, so the boundary condition of the molten pool is inherently asymmetric. In conventional WAAM with a symmetric arc, the heat input is evenly distributed on both sides of the bead centerline. For the twin-electrode GTA, the currents flowing through the two tungsten electrodes can be regulated independently, which offers a unique degree of freedom: by carrying unequal sub-currents on the two electrodes, the symmetry of the arc plasma is broken and the arc thermal field can be actively redistributed to match the asymmetric boundary condition of bead overlapping.
Based on this idea, an overlapping optimization method based on thermal field regulation is proposed in this paper:
The sub-current of one electrode is increased while that of the other electrode remains unchanged, so that the heating range of the coupled arc on the overlapping side can be enlarged and the remelting zone extends towards the apex of the previous bead. Then the molten metal flows and spreads under the surface tension to fill the inter-bead valley. This concept aligns with the TOM model, with the improvement that the tangent becomes the common tangent to the apexes of the two beads. In this way, the inter-bead valley can be eliminated at its physical root, and the surface flatness of the deposited layer is improved.
To this end, the coupled arc morphology and the bead geometry under asymmetric sub-currents are first investigated. The overlapping optimization method is then developed based on the spreading and filling behavior of the molten pool. Finally, the aim is to extend the method into a quantitative model covering the entire process window, so that the overlapping parameters can be planned directly. This study is expected to provide a new route for developing GTA-based additive manufacturing towards both high deposition rate and high forming quality.
2. Experimental System and Materials
According to the forming optimization requirements of thermal field regulation, a twin-electrode GTA additive manufacturing system was independently designed and built in this work, as shown in Figure 1a. It comprises two independent GTAW power sources, a water-cooled twin-electrode torch with two mutually insulated tungsten electrodes arranged in parallel, a single wire feeder, a welding robot and the signal-transmission modules connecting them. Two YC-400TX4 GTAW power sources produced by Panasonic Welding Systems (Tangshan) Co., Ltd. in Tangshan, China were used with DCEN polarity, and the robot was a ZK1900-20 unit made by Zhenkang Welding Electromechanical Co., Ltd. in Nantong, China. Only one filler wire is used. It is fed from the front of the coupled arc along the travel direction at a 20° downward angle into the molten pool shared by the two electrodes, and this arrangement is drawn in the schematic of Figure 1b.
Figure 1.
Twin-electrode GTA additive manufacturing system.
In this work, a high-speed camera produced by Hunan Rocketech Technology Co., Ltd. in Changsha China at 1500 fps with 1280 × 860 pixels was employed to record the arc morphology and the molten pool image through an 808 nm filter. The arc was viewed horizontally from directly behind the torch, and the molten pool was viewed from behind at a downward angle of 45°. During the overlapping process, the position of the molten-pool boundary can be directly observed and serves as a key indicator for characterizing thermal field changes in response to varying overlapping parameters.
In addition, the cross-sectional profiles of the deposition beads were acquired in layers with a self-made line-structured-light active vision sensor based on laser triangulation principle with an accuracy of 0.01 mm. The profile was used to quantitatively evaluate the surface flatness of the deposited beads. A handheld infrared thermometer made by UNI-Trend Technology Co., Ltd. in Dongguan, China was employed to measure the inter-layer or inter-bead temperatures.
A Q235 steel plate conforming to GB/T 700-2006, 10 mm in thickness and 300 mm by 150 mm in size, was selected as the substrate. It was ground to remove oil and oxide film before deposition. The filler was a 1.2 mm H08Mn2Si mild-steel wire conforming to GB/T 14958-1994. Cerium–tungsten electrodes of 3.0 mm diameter were ground to eccentric tips with a 30° tip angle. The inter-electrode distance was 2.0 mm, and the arc length was 5.0 mm. The shielding gas was argon with a purity of 99.99%, supplied at the flow rate of 15–25 L/min. The inter-layer temperature and inter-bead temperature were maintained at 100 °C by a necessary interlayer pause. All depositions were conducted in the flat position, and all the above-mentioned conditions were kept constant throughout the experiments. The process parameters of interest are summarized in Table 1.
Table 1.
Process parameters of the deposition experiments.
3. Results and Discussion on Thermal Field Regulation
Three aspects of the overlap-forming process under thermal field regulation are addressed in this chapter: the deflection behavior of the coupled arc, the asymmetric change in the deposited bead geometry, and the resulting overlapping effect and surface flatness.
3.1. Effect of Thermal Field Regulation on Morphology of the Coupled Arc
The twin-electrode GTA is a coupled arc formed by the interaction of the arcs generated by two independent welding circuits and differs from the conventional single-arc heat source. Its morphology needs to be observed and analyzed first. The typical twin-electrode GTA morphology with the same sub-currents is shown in Figure 2a. The arcs generated by the two eccentric-tipped tungsten electrodes attract each other and couple into a single large arc, which is distributed symmetrically on both sides of the centerline between the two electrodes and exhibits a single peak at the midpoint. For clarity, the two electrodes are referred to as the left electrode and the right electrode according to their positions as seen by the camera viewing from the back of the bead.
Figure 2.
Coupled arc morphology under different sub-current combinations.
Since the two eccentric-tipped tungsten electrodes in the torch are insulated from each other, different sub-currents can be applied to regulate the arc thermal field. The influence of sub-currents on the coupled arc morphology was studied. Figure 2 shows the morphology of the coupled arc at different sub-current combinations: the sub-current of the left electrode was kept at 200 A, while that of the right electrode was set to 200 A, 220 A, 240 A, 260 A, 280 A and 300 A, respectively. For description, the expression of two sub-currents added together is used to represent the deposition current, e.g., 200 A + 220 A.
As can be seen from Figure 2, the coupled arc remains stable and no arc separation occurs within this deposition current range, and the asymmetric sub-currents have a considerable influence on the morphology of the coupled arc. When the sub-current of one electrode is kept at 200 A and that of the other is gradually increased, the coupled arc deflects, and the deflection angle increases with the difference between the two sub-currents, as shown in Figure 2b–f. Reversing the current combination reverses the deflection direction. It is worth noting that the coupled arc does not deflect towards the electrode carrying the larger sub-current but towards the electrode carrying the smaller one, indicating that increasing one sub-current does not simply shift the arc towards that side.
This phenomenon is attributed to the guiding effect of the eccentric-tipped tungsten electrode. When the electrode is heated for thermionic emission, the electrons emitted from the vertical side of the electrode tip have an initial velocity normal to the vertical surface, whereas those emitted from the other side are normal to the inclined surface [21]. Under the Lorentz force, the former travel a shorter distance to reach the workpiece surface, so that the current paths on the two sides are asymmetric even though the deposition current and the surrounding conditions remain unchanged. A steady arc automatically selects the cross-section that minimizes the electric field intensity. Therefore, the arc generated by an eccentric-tipped electrode deflects towards the vertical side of the electrode tip. When two such electrodes are placed tip to tip, their arcs are guided towards each other, so that the mutual attraction is strengthened and a stable coupled arc is formed. When the sub-current of one electrode increases, the arc it generates becomes stiffer and keeps its own axis, whereas the arc generated by the other electrode is deflected further towards its own electrode tip. Thus, the centroid of the coupled arc shifts towards the low-current side, which accounts for the direction of the deflection observed in Figure 2.
3.2. Effect of Thermal Field Regulation on Bead Geometry
The most important process parameter of twin-electrode GTA additive manufacturing is the deposition current, and the deposited bead geometry varies with it because the molten metal undergoes different thermal–mechanical coupling processes. In this section, unless otherwise specified, the travel speed was set to 4.0 mm/s, and the wire feed speed was set to 3.5 m/min.
In the twin-electrode GTA additive manufacturing process, the spatial distribution of the arc thermal field can in addition be adjusted by the sub-currents, so that the bead width can be regulated without changing the other parameters. Therefore, it is necessary to quantify the influence of the sub-current increment ΔI on the bead width.
Keeping the other parameters unchanged, a 50 mm long bead was first deposited on the substrate at 200 A + 200 A; when the preset point was reached, the sub-current of the right electrode was increased by ΔI, i.e., 200 A + (200 A+ΔI), and the deposition was continued over another 50 mm. The experiment was repeated with ΔI increasing in steps of 10 A, and the results are shown in Figure 3, in which the black lines represent the extension lines of the bead boundaries before the sub-current increase, highlighting the impact of the sub-current variation on the bead width. Since these beads are viewed from above with the depositing direction from left to right, the left electrode as defined in Figure 2 acts on the upper side of the beads in Figure 3.
Figure 3.
Forming appearance of beads deposited at different sub-current combinations.
As shown in Figure 3, when the deposition current is 200 A + 200 A, the deposited bead is symmetric about the torch axis, and its width is denoted as W1. When the torch reaches the preset point, the sub-current of the right electrode is increased by ΔI while that of the left electrode remains unchanged, and the bead width increases to W2. The lower boundary of each bead remains unchanged, while the upper boundary of it extends outward. This is a consequence of the centroid of the coupled arc shifting towards the low-current side.
To build the multi-bead overlapping model, the bead width is quantitatively described in terms of the two sides divided by the torch axis. The side below the right electrode, whose sub-current is increased, is defined as the unchanged side, since its width remains a constant value of 0.5W1. The other side below the left electrode, whose sub-current is kept constant, is defined as the widened side, and its width ΔW is calculated as ΔW = W2 − 0.5W1.
The bead widths under different sub-current increments were measured with the line-structured-light active vision sensor. Each specified condition was deposited three times to ensure accuracy. For each 50 mm bead section, measurements were taken at three distinct positions. The mean values derived from these measurements are presented in Table 2 for further analysis.
Table 2.
Bead width measurement results at different sub-current increments ΔI.
Since the width of the widened side equals half the initial-bead width when the two sub-currents are equal, ΔW can be expressed as ΔW = 0.5W1 + f(ΔI), where f(0) = 0. An exponential function model was selected for fitting because ΔW must satisfy the physical boundary condition ΔW(0) = 0.5W1, and its growth rate first rises and then declines as ΔI increases. The coefficients were estimated by the nonlinear least squares method, employing the Origin 2024 software developed by OriginLab in Massachusetts, USA using the data in Table 2. Figure 4 presents the fitted curve, and the fitting expression is as follows:
ΔW = 0.5W1 + 4.4[1 − exp (−(0.02ΔI)1.6)]
Figure 4.
Fitting result of the widened-side width against sub-current increment ΔI.
The fit gives an R2 of 0.996, and a root mean square error (RMSE) of 0.10 mm. The model is empirical and is not extrapolated beyond ΔI = 100 A or beyond any other deposition parameter ranges used for its calibration. The exponent of ΔI is 1.6, which means that the widened-side width increases slowly at small sub-current increment and accelerates once ΔI exceeds approximately 20 A. This behavior is consistent with the measured data: the width increases by merely 0.08 mm as ΔI rises from 0 to 10 A, but jumps by 0.92 mm as ΔI rises from 10 to 20 A. This phenomenon occurs due to the arc stiffness. When the sub-current difference is small, it lacks the necessary force to make significant alterations in the arc plasma channel. As a result, the bead width showcases minimal variations. As the sub-current difference increases, the horizontal component of the Lorentz force increases, promoting arc deflection and causing significant changes in the thermal field [22]. Meanwhile, the model predicts an asymptotic limit of 10.5 mm for ΔW, indicating that the width cannot be enlarged indefinitely simply by increasing the sub-current difference. It is because the arc deflection is accompanied by an increase in arc length. Since the arc must maintain a minimum energy state, its length cannot grow indefinitely. The deflection angle is therefore bounded, and so is the widened width on the overlapping side [23].
3.3. Overlapping Optimization Method Based on Thermal Field Regulation
The available overlapping models including the flat-top, inclined-top, tangent and power-function models, improve the prediction of the bead profile and hence the optimal overlapping distance. However, all of them treat the molten metal as a passive filler and consider only the volume conservation of the filled region, without analyzing how the molten metal is driven to fill the inter-bead valley.
The physical limitation of the flat-top overlapping model can be revealed from the force balance acting on the molten pool. The geometry of the molten-pool surface is determined by the imbalance between the surface tension, the gravity and the electromagnetic force [24], and the interfacial tension at the triple point directs the molten metal along the solid–liquid interface [25]. In a symmetric arc, the arc force and the electromagnetic pressure act symmetrically on the two sides of the bead centerline, and the triple point at the edge of the molten-pool surface does not reach the apex of the previous bead, as illustrated in Figure 5. According to the Young–Laplace equation, the molten-pool surface contracts under the surface tension, so that the deposited metal lacks the driving force to spread towards the apex of the previous bead. As shown in Figure 5, the excess metal that should have filled the valley finally solidifies above the overlapping zone, producing a deep valley and an uneven deposited layer. The root of the problem is not the geometry of the overlapping model itself but the uncontrolled heat and mass transfer during overlapping. Without an external driving force, the molten metal cannot be transported into the valley within the limited time.
Figure 5.
Schematic diagram of the deposition morphology of the flat-top overlapping model.
Therefore, it is necessary to actively regulate the arc thermal field to change the heating range of the coupled arc. Increasing the sub-current flowing through one electrode while keeping that of the other unchanged will enlarge the heating range of the coupled arc on the overlapping side, so that the remelting zone of the previous bead extends to its apex during overlapping. The triple point then moves to the apex of the previous bead, and the three-phase interfacial tension acting on the molten pool becomes tangential to the apex of the previous bead, as shown in Figure 6. According to the Young–Laplace equation, the resulting change in the curvature of the molten-pool surface generates a larger driving force, and the molten metal is thus driven to flow and spread towards the apex of the previous bead, so that the valley tends to be filled and the beads attain an equal height. The optimized overlapping model based on this principle is illustrated schematically in Figure 6. This mechanism eliminates the inter-bead valley at its physical fundamental, and the improvement of the surface flatness is achieved by regulating the thermo-mechanical state of the molten pool rather than by altering the geometrical parameters of the overlapping model.
Figure 6.
Schematic diagram of the deposition morphology optimized by thermal field regulation.
It should be emphasized that among the existing overlapping models, the flat-top model is the only one that aims at a completely flat layer, and its volume-conservation condition fixes the amount of molten metal that must be available to fill the valley. The limitation of the flat-top model stems from its neglect of heating, force balance, and molten metal flow. The proposed thermal field regulation provides precisely these missing transport mechanisms, thereby complementing the flat-top model. However, the other models (e.g., tangent, inclined-top, power-function) instead reduce the inter-bead height difference by enlarging the overlapping distance. Once the overlapping distance is enlarged, the overlapping region becomes smaller than the valley region. Consequently, the inter-bead valley is necessarily present by volume conservation. The proposed thermal field regulation cannot compensate for the lack of material, which is why the coefficient 0.667 given by the flat-top model was retained.
At a deposition current of 200 A + 200 A, the width W1 was measured as 12.2 mm. Based on the analysis above, the overlapping distance d is therefore taken as 0.667W1, i.e., 8.14 mm. To obtain a flat deposited layer, the width of the widened side must fill the whole overlapping region, which requires ΔW to be equal to d, i.e., 8.14 mm. Solving Equation (1) for this target gives ΔI =38 A, i.e., an overlapping current of 200 A + 238 A.
To verify the proposed model, a set of 100 mm long initial beads were first deposited with a deposition current of 200 A + 200 A on the substrate, and the overlapping distance between the initial bead and the overlapping bead was fixed at 0.667 times the initial-bead width, i.e., 8.14 mm. The overlapping beads were deposited from the adjacent position on the right side of the initial beads. The sub-current flowing through the electrode on the overlapping side (left electrode) was kept at 200 A, while that of the other electrode on the non-overlapping side (right electrode) was set to 200 A, 220 A, 238 A, 250 A and 270 A, respectively. Forming appearances of the overlapping beads deposited under different overlapping currents are shown in Figure 7.
Figure 7.
Forming appearances of the overlapping beads deposited with a sub-current of 200 A.
As can be seen from Figure 7, within the selected process window, both beads are well formed except at the arc-starting and arc-extinguishing ends. To further evaluate the effect of overlapping, the cross-sectional profile curves of these overlapping beads were acquired with a line-structured-light active vision sensor. The results are shown in Figure 8.
Figure 8.
Cross-sectional profile curves of the overlapping beads deposited with a sub-current of 200 A.
Figure 8a shows the cross-sectional profile curve of the layer deposited at a current of 200 A + 200 A. The overlapping bead is 0.28 mm higher than the initial bead, with a distinct valley formed between them. Under the heating of the symmetric coupled arc, the remelting zone extends only to the bottom of the valley. Constrained by the three-phase interfacial tension, the molten metal lacks sufficient time and driving force to flow into and fill the valley, so that the excess metal solidifies above the overlapping zone.
Figure 8b shows the cross-sectional profile curve of the layer deposited at a current of 200 A + 220 A. The overlapping bead is 0.11 mm higher than the initial bead, indicating that the issue of bead height difference has been improved. In addition, the lowest point of the valley also shifted 0.17 mm towards the apex of the initial bead because increasing the sub-current of the electrode on the non-overlapping side enlarges the molten pool on the opposite side. Driven by the three-phase interfacial tension, the molten metal spreads towards the initial bead, which reduces the height of the overlapping bead and diminishes the valley depth.
Figure 8c shows the cross-sectional profile curve of the layer deposited at a current of 200 A + 238 A. The height of the overlapping bead is almost identical to that of the initial bead, with a height difference in less than 0.1 mm, and nearly no valley is observed between them. At this overlapping current recommended by the overlapping model, the width of the widened side of the overlapping bead reaches the overlapping distance. The remelting zone extends, approaching the apex of the initial bead, and the three-phase interfacial tension acting on the molten pool becomes tangential to the upper surface of the initial bead. Thus, the molten metal flows and spreads towards the apex of the initial bead and finally solidifies, filling the valley between the two beads, so that the surface flatness of the deposited layer is significantly improved.
Figure 8d shows the cross-sectional profile curve of the layer deposited at a current of 200 A + 250 A. In this scenario, the remelting zone failed to extend beyond the apex of the initial bead. In this case the remelting zone did not extend beyond the apex of the initial bead, which is not in accordance with the prediction of Equation (1). The reason is that the heat dissipation conditions are slightly different between depositing on the substrate and overlapping next to the initial bead. The excessive difference in sub-currents leads to a significant increase in the horizontal component of arc force, pushing the molten metal towards the initial bead. That is precisely why the apex of the overlapping bead diverges from the torch’s axis, resulting in the overlapping bead being elevated by 0.26 mm compared to the initial bead.
Figure 8e shows the cross-sectional profile curve of the layer deposited at a current of 200 A + 270 A. The height of the overlapping bead exceeds that of the initial bead by 0.38 mm, suggesting a more severe degradation of the overlapping effect. Compared with Figure 8d, it can be observed that the height of the overlapping bead remains unchanged, whereas the height of the initial bead decreases. This occurs because the thermal field generated by the twin-electrode GTA not only encompasses the initial bead but also extends beyond its uppermost region, thereby instigating a process of remelting at its apex. Due to this process, the surface of the overlapping beads gradually becomes inclined, creating a distinct angled formation.
A comparison of Figure 8a–e reveals that the optimal overlapping current of 200 A + 238 A, obtained from the overlapping model, shows excellent agreement with the experimental results. Furthermore, the measured height difference between the two beads varies with the overlapping current, reaching a minimum at this optimal value. This model successfully reproduces the experimental trends and offers a trustworthy foundation for calculating the overlapping parameters, including overlapping distance and overlapping current. The significantly reduced difference in bead height and the nearly fully filled valley confirm that regulating the arc thermal field through asymmetric sub-currents is indeed an effective strategy for enhancing the overlapping effect.
To verify the effect of asymmetric sub-current on thermal field regulation, the molten pool image during the overlapping process was recorded from the rear of the arc at a tilt angle of 45° for the symmetric and optimal conditions, as shown in Figure 9. At the symmetric overlapping current of 200 A + 200 A, the ripple cusps of the previous bead remain intact and fully visible. Thus, the overlapping boundary stops below the apex of the previous bead, and an inter-bead valley is left. At the optimal overlapping current of 200 A + 238 A, the overlapping boundary expands 2.16 mm towards the initial bead and approaches the ripple cusps, indicating that the apex is reached and remelted. The observed overlapping boundary displacement links the asymmetric arc thermal field to the molten-pool geometry. It provides direct evidence that the asymmetric thermal field enlarges the remelting zone of the overlapping bead, and it locates the three-phase line at the previous-bead apex as assumed. It has been demonstrated that the proposed thermal field regulation method provides sufficient momentum for the molten metal to fill the inter-bead valley, thereby improving the overlapping effect.
Figure 9.
Molten pool vision of the overlapping beads with different overlapping currents.
The deposited layer, characterized by beads that overlap one another, presents a unique surface topography. The regions between the apexes of these beads, which align with the torch axes, significantly influence the overall surface flatness. To quantitatively assess the flatness of these overlapping bead structures, the intra-layer height error between the torch axes is employed as the primary evaluation criterion [26]. It is defined as the maximum height difference, denoted as Δh. Δh is the comprehensive result of the valley depth and the height difference among the apexes of the beads. The optimal surface quality is achieved when the profile between the two torch axes exhibits the greatest uniformity, thereby minimizing the value of Δh.
To assess the effect of thermal field regulation on surface formation, the intra-layer height error of the overlapping beads deposited at the five overlapping currents was analyzed. For each overlapping current, the overlapping-beads samples were deposited in triplicate. Δh of each sample was obtained from the cross-sectional profiles at three positions and the maximum of them was taken. The results are illustrated in Figure 10. Error bars denote the standard deviation of three independently deposited samples. Starting from 200 A + 200 A, Δh decreased as overlapping current increased, signifying a continual enhancement in surface flatness. This value attained a minimum of 0.11 mm at the optimal overlapping current of 200 A + 238 A, at which point the heights of the two beads are virtually identical. However, above this value the thermal field regulation becomes excessive and Δh increased again.
Figure 10.
Intra-layer height error of the overlapping beads at different overlapping currents.
4. Extension of the Overlapping Optimization Method
4.1. Effect of the Deposition Parameters on the Bead Geometry
Twin-electrode GTA additive manufacturing involves a series of process parameters that act on the deposited bead simultaneously, among which the deposition sub-current (I), the sub-current increment on one electrode (ΔI) and the travel speed (v) exert the most direct influence on the bead geometry. Because these parameters are coupled through the thermo-mechanical evolution of the molten pool, their effects on the bead geometry cannot be evaluated separately by a single-factor analysis. A quantitative relation covering the entire process window is therefore required, so that the overlapping parameters, in particular the current increment ΔI required for a given deposition current and travel speed, can be planned rather than determined by experiments.
Before investigating the influence of the deposition parameters, the relation between the wire feed speed and the deposition current was determined, since the amount of filler metal fed into the molten pool must match the melting capacity of the coupled arc [27].
At a low wire feed speed, the deposition rate falls, and a larger proportion of the arc heat is consequently consumed in heating and remelting the layer that has just been deposited rather than in depositing the bead. The heat input is thus spread over a wider area, which broadens the heat-affected zone and dilutes the deposited layer. When the wire feed speed is excessive, the wire cannot melt completely before it reaches the pool. The unmelted wire tip then comes into rigid contact with the semi-solidified pool surface, so that the solid wire is pushed into the pool instead of being melted, which not only disturbs the transfer of the filler metal but also gives rise to wire-stubbing defects. The wire feed speed matching the deposition current is therefore identified as the value at which the wire is just completely melted upon reaching the molten pool. The experiment results show the matching relationship between the wire feed speed vf (m/min) and the deposition sub-current I (A) as follows:
vf = 0.03I − 2.5
Twenty single-bead deposition experiments were orthogonally designed within the process window in Table 1 and conducted following the procedure of Section 3.2. The deposition sub-current I was varied from 150 A to 250 A, and the travel speed v from 3.0 mm/s to 5.0 mm/s, while the wire feed speed was matched with the deposition current. To mitigate the adverse effects of an excessive ΔI, the range of it was constrained to 0 A–50 A.
For each condition, the bead profile was acquired with the line-structured-light vision sensor, and W1, W2 and ΔW were measured. The repetitions and the measurement method are the same as those in Section 3.2. The results of W1 and ΔW are listed in Table 3. In the entire process window, for simplicity, a linear model was adopted to fit W1 against I and v, ignoring the cross-effects between them. The coefficients were again estimated by the nonlinear least squares method with Origin 2024 software, giving the following expression:
W1 = 4.677 + 0.063I − 1.258v
Table 3.
Measurements of bead width under different deposition parameters.
The fit gives R2 of 0.972, and the RMSE of 0.26 mm.
The width of the widened side is governed by the deflection of the coupled arc, which increases with the sub-current increment but has a limit. This fitting retains the format of Equation (1), primarily revising the parameters according to the data in Table 3 to accommodate different values of I and v.
This fitting retains the exponential saturation form of Equation (1) so that the boundary condition and the finite asymptote are preserved. For simplicity, the amplitude is expressed as a power function of I and v, and the exponent of ΔI is still 1.6. All coefficients were estimated simultaneously by nonlinear least squares from the data in Table 3, employing the Origin 2024 software. The fitting result is as follows:
ΔW = 0.5W1 + 1.6 I0.215 v−0.092[1 − exp (−(0.02ΔI)1.6)]
The required current increment can be directly determined from the target overlapping distance by solving Equation (4). Three features of the model are worth noting. First, the initial-bead width increases linearly with I but decreases with v, as expressed by Equation (3), which is consistent with the way the heat input per unit length varies with these two parameters. Second, the attainable widening ΔW increases with the sub-current increment ΔI but approaches a limit, so that the overlapping side cannot be widened without bound simply by increasing the sub-current difference. Third, the overlapping distance d and the widened-side width ΔW are fixed at d = ΔW = 0.667 W1, and W1 grows with I, so the sub-current increment ΔI required to achieve this width consequently increases with I.
Separate validation experiments were conducted at parameter combinations that were not used in the regression analysis. As shown in Figure 11, the symbols show the measured ΔW of the beads and the lines show the predictions of Equations (3) and (4) for different combinations of I and v. The predicted ΔW agrees with the measurements with an R2 of 0.952, an RMSE of 0.19 mm, and a maximum relative error of 6.14%. Extrapolation beyond the process window is not supported.
Figure 11.
Fitting curves between ΔW and ΔI at different I and v.
The parameter planning procedure based on the proposed overlapping optimization method can be stated as an algorithm:
(1) Specify the overall layer width Wlayer and the number of beads n per layer. The overlap distance is d = 0.667W1, so the required initial-bead width can be calculated as follows:
W1 = Wlayer/[1 + 0.667(n − 1)]
(2) Select the deposition sub-current I and solve Equation (3) for the travel speed v that reproduces this W1. Set the wire feed speed from Equation (2).
(3) Substitute ΔW = d into Equation (4) and solve for the sub-current increment ΔI, giving the overlap current for the overlapping beads.
The procedure is valid within the above process window, and under the process conditions described in Section 2. It does not cover changes in the material, the deposition position or the electrode geometry et al.
4.2. Verification of the Overlapping Optimization Method Within the Process Window
To further verify the applicability of the proposed overlapping optimization method within the process window, two parameter sets different from those in Section 3.2 were selected for the overlapping experiments. The measurement and statistical methods used for cross-sectional profiles and feature dimensions followed those outlined in Section 3.
The first parameter set had a lower heat input, namely a deposition current of 170 A + 170 A, and a travel speed of 5.0 mm/s. The initial-bead width W1 predicted by Equation (3) was 9.10 mm, so the overlapping distance d is 6.07 mm. Substituting d for ΔW in Equation (4) gave a ΔI of 33 A and an optimal overlapping current of 170 A + 203 A. To verify the overlapping effect, overlapping currents of 170 A + 170 A, 170 A + 203 A, and 170 A + 230 A were selected for the experiments. The forming appearance of the overlapping beads are shown in Figure 12.
Figure 12.
Forming appearance of the overlapping beads deposited with a sub-current of 170 A.
The inter-bead lack-of-fusion defect is found from the overlapping beads deposited at 170 A + 170 A through visual inspection. This condition has the lowest heat input of the investigated combinations, with a symmetric coupled arc whose thermal field cannot be deflected towards the overlapping side. Therefore, the arc heat is insufficient to melt the inter-bead region, and the overlapping molten metal cannot spread along the surface of the initial bead under the surface tension. In this case, a large valley is left between the two beads, which is the effect of the inter-bead lack of fusion on the forming quality. As shown in Figure 12b,c, as the overlapping current increased, the inter-bead lack of fusion was effectively suppressed. The forming appearance of the overlapping beads was improved.
The cross-sectional profile curves of these overlapping beads were acquired with the vision sensing system. Three typical results are shown in Figure 13. When the overlapping current was 170 A + 170 A, the measurement location was chosen to avoid the inter-bead lack-of-fusion area. The overall width of the overlapping beads is 15.23 mm, which agrees with the model prediction of 15.17 mm within an error of 0.39%. However, the top of the overlapping bead is 0.14 mm higher than the initial bead, and a wide and deep valley exists between the two beads, resulting in poor surface forming quality. As the overlapping current increases to 170 A + 203 A, the overall width is 15.32 mm with a predicted error of 0.99%. The two beads have a height difference of less than 0.1 mm and the valley between them is negligible, indicating a high surface forming quality. When the overlapping current reaches 170 A + 230 A, the apex of the overlapping bead deviates from the torch axis and the top area of the initial bead is melted and destroyed. This result is similar to the one with an overlapping current of 200 A + 270 A. Under low heat input conditions, an excessive overlapping current also produced an unsatisfactory overlapping effect and poor surface quality.
Figure 13.
Cross-sectional profile curves of the overlapping beads deposited with a sub-current of 170 A.
The second parameter set had a higher heat input, namely a deposition current of 230 A + 230 A, and a travel speed of 3.5 mm/s. The initial-bead width W1 predicted by Equation (3) is 14.76 mm, so the overlapping distance d is 9.84 mm. In this case, the corresponding current increment ΔI is 42 A, giving an optimal overlapping current of 230 A + 272 A. The overlapping currents of 230 A + 230 A, 230 A + 272 A, 230 A + 300 A were selected to verify the overlapping effect. The forming appearances of the overlapping beads with a deposition sub-current of 230A are shown in Figure 14. In Figure 14c, because of the excessively high deposition current, an arc crater was left behind during arc extinction.
Figure 14.
Forming appearance of the overlapping beads deposited with a sub-current of 230 A.
Three typical cross-sectional profile curves of these overlapping beads are shown in Figure 15. When the overlapping current was 230 A + 230 A, the average overall width of the overlapping beads was 24.99 mm, with a model prediction of 24.61 mm and an error of 1.57%. The top of the overlapping bead was 0.52 mm higher than the initial bead, and a wide and deep valley existed between the two beads. Compared with the overlapping beads deposited with the symmetric sub-currents of 170 A + 170 A and 200 A + 200 A, it could be proved that the overlapping formation problem became more severe as the deposition current increases. When the overlapping current was 230 A + 272 A, the overall width was 25.06 mm with an error of 1.84%. The two beads had a height difference of less than 0.1 mm and the valley between them was shallow, indicating that the thermal field regulation method is universally applicable to solving the overlapping problem. When the overlapping current was 230 A + 300 A, the overlapping effect deteriorated again. The top area of the initial bead was melted and destroyed, leaving a height difference of 0.35 mm between the two beads. Meanwhile, the overall width increased to 26.32 mm with an error of 6.49%, demonstrating that the right boundary of the overlapping bead expanded outward by 1.71 mm, which was 11.59% of W1. This results in inaccurate overlapping distance and leads to a complex and unpredictable overlapping process in subsequent additive manufacturing [28].
Figure 15.
Cross-sectional profile curves of the overlapping beads deposited with a sub-current of 230 A.
The intra-layer height error of the overlapping beads under different overlapping currents was measured for these two additional parameter sets, as shown in Figure 16. The same trend as in Figure 10 was obtained: Δh was large when the two sub-currents were equal, attained its minimum at the overlapping current predicted by the model, and increased again once the sub-current increment became excessive, since the molten metal then accumulated between the two bead apexes and covered the top of the initial bead. The model predictions of 170 A + 203 A and 230 A + 272 A were thus confirmed experimentally, demonstrating that the model is applicable throughout the common process window of twin-electrode GTA additive manufacturing. It is worth emphasizing that the optimal condition is determined by matching the molten-pool width on the overlapping side with the overlapping distance rather than by simply increasing the total heat input, and that an optimal asymmetric arc thermal field therefore exists for bead overlapping.
Figure 16.
Variation in the intra-layer height error with the overlapping current.
With the overlapping coefficient 0.667 given by the flat-top model, the two bead apexes reached the same height within 0.15 mm at 200 A + 238 A, 170 A + 203 A and 230 A + 272 A. Three independent parameter sets confirm that this volume-conservation coefficient remains valid once thermal field regulation supplies the transport mechanism that the flat-top model lacks.
To illustrate the applicability of the proposed overlapping optimization method to multi-layer multi-bead deposition, a 45 mm wide two-layer stepped component was deposited using twin-electrode GTA additive manufacturing techniques. Each layer consisted of five overlapping beads, 80 mm long in the first layer and 40 mm long in the second, deposited from the center outwards. Equation (5) gave an initial-bead width W1 of 12.27 mm, and an overlapping distance d of 8.18 mm. The deposition sub-current was fixed at 200 A, the wire feed speed was 3.5 m/min, and the travel speed obtained from Equation (3) was 3.98 mm/s. Substituting the required widened-side width into Equation (4) gave a sub-current increment ΔI of 37 A, corresponding to an overlapping current of 200 A + 237 A for the right-side bead and 237 A + 200 A for the left-side bead. Following this plan, the stepped component was deposited, as shown in Figure 17a. A cross section was cut from the middle of the two-layer zone and examined metallographically as shown in Figure 17b. It shows a regular bead arrangement with consistent width and no discernible defects.
Figure 17.
The deposited two-layer stepped component.
The cross-sectional profile of each layer of this stepped component was acquired with a line-structured-light active vision sensor. Data was collected at three positions on each layer, ensuring a comprehensive representation of the component’s geometry. A typical result is shown in Figure 18. The average overall width of the first layer was 45.67 mm, an error of 1.49% with respect to the designed 45 mm. The maximum Δh was 0.15 mm on the first layer and 0.19 mm on the second layer. The upper surface of the second layer remained flat without obvious inclination, and the two layers were well aligned, indicating that the inter-bead valley had been successfully mitigated through the application of the overlapping optimization method. These results are better than those obtained when two beads overlap under symmetric sub-current conditions. It indicates that the parameters planned from Equations (3) to (5) were accurately realized in the deposition process, thereby validating the effectiveness of the proposed approach.
Figure 18.
Cross-sectional profile curves of the deposited two-layer stepped component.
It is found that the deepest valley of the second layer appeared between the outermost bead and its inward neighbor. The cross-sectional profiles in Figure 18 explain this observation. The outermost bead rests on the curved edge of the previous layer rather than on a flat substrate, so the molten metal sinks to fill the space beneath it, rather than filling the inter-bead valley. The increase in Δh is a direct consequence of a local material deficit at the edge, not an error accumulation from the preceding layer. This deficit is a geometric boundary condition that recurs in each layer, and the wire feed compensation proposed in [3] addresses exactly this condition. Whether the same deficit recurs when a component is deposited layer by layer, and whether Δh accumulates with the layer number, cannot be decided from this stepped component alone.
A ten-layer block component with a length of 150 mm was therefore deposited to confirm both questions. The first two layers each contained seven beads deposited from the center outwards, with the same sub-currents, travel speed, wire feed speed and overlapping distance as the stepped component described above, so that the edge deficit could be evaluated under repeated deposition. From the third layer to the tenth, each layer consisted of only the three central beads, and the wire feed speed of the two edge beads was raised to 4.5 m/min to compensate for the material deficit. No other parameter was changed. A cross section was cut from the middle of the block and prepared for metallographic examination, and the profile of each layer was measured with the line-structured-light sensor during the inter-layer cooling time. The metallograph is presented in Figure 19 and the superimposed layer profiles in Figure 20.
Figure 19.
Metallograph of the deposited 10-layer block-component.
Figure 20.
Cross-sectional profile curves of the deposited 10-layer block component.
For the second layer, the deepest valley appeared between the outermost bead and its inward neighbor again. The edge deficit is therefore reproducible in a multi-layer block and remains a boundary condition of the outermost bead rather than a consequence of the layer number.
With that compensation applied, the block did not show any deterioration in appearance. Figure 19 shows that no internal lack-of-fusion defect is visible over the ten layers. The bead geometry stays regular to the last, with no collapse or lateral drift.
Figure 20 shows that Δh reaches its maximum of 0.18 mm on the fifth layer and then stays less than 0.16 mm up to the tenth layer, so it does not grow in proportion to the layer number. The absence of Δh accumulation follows from the geometry of remelting. The maximum Δh remains less than the minimum penetration of the layer, which was 0.41 mm for these deposition parameters, so the surface irregularity of the previous layer lies entirely within the zone remelted by the next layer. It was smoothed out instead of being reproduced to the new surface.
The thermal process of a multi-layer multi-bead deposit converges rapidly to a steady condition within a few layers. The inter-layer temperature was kept constant, so every layer starts from the same thermal state. Heat from the first layer is extracted by the substrate, whereas heat from a higher layer is extracted by the bulk of metal already deposited beneath the bead. In both cases the bead is mainly cooled by conduction into a large metallic body, so the heat dissipation condition of a higher layer is already close to that of the first. After only a few layers the two conditions become essentially identical, and further layers make no difference to the thermal condition of the new bead. This rapid convergence is consistent with the bounded Δh in Figure 20, and depositing further layers introduces no systematic change.
Therefore, the proposed overlapping optimization method developed for two overlapping beads remains applicable when deposition is extended to multi-layer multi-bead components, provided that the edge deficit is compensated and the height difference stays less than the minimum penetration of the layer.
4.3. Applicability Limits of the Overlapping Optimization Method
The present results are valid for the Q235 + H08Mn2Si mild steel system in the flat position with 3.0 mm diameter electrodes, a 30° tip angle, 2.0 mm inter-electrode distance and a 5 mm arc length. The proposed method delivers a criterion rather than a fixed set of process parameters. The overlapping-side molten-pool boundary must reach the apex of the previous bead, which is realized when the widened-side width equals the overlapping distance, written as ΔW = d = 0.667W1. Derived from force balance and volume conservation, this criterion is not specific to the material or electrode geometry. What is specific to the present test conditions is the quantitative relation between the sub-current increment ΔI and the resulting widening ΔW. The inter-electrode distance, arc length and electrode tip angle govern the stiffness of the coupled arc and hence the amplitude and asymptote of the ΔW–ΔI relation. The material, through its thermal conductivity, fusion point, surface tension and wetting behavior, along with the inter-layer temperature and inter-bead temperature, governs molten-metal spreading and the position of the three-phase line. The deposition position introduces a gravity component that is absent in the flat position. The coefficients of Equations (3) and (4), and the 0.667 coefficient itself, must be re-calibrated whenever any condition changes, whereas the criterion remains applicable. Re-calibration requires a limited number of single-bead depositions. W1 is fitted against I and v, ΔW is fitted against ΔI, and the required ΔI follows from setting ΔW equal to d, as mentioned in the parameter-planning procedure of Section 4.1. A complete sensitivity study over all combinations of electrode geometry, materials and deposition positions is neither feasible nor necessary, because every new condition is simplified to the same finite calibration step.
5. Conclusions
The overlapping behavior of adjacent beads in twin-electrode GTA additive manufacturing was investigated over a process window of 150–250 A per-electrode sub-current and 3.0–5.0 mm/s travel speed. All experiments used a Q235 substrate with H08Mn2Si filler wire in the flat position. The electrodes were 3.0 mm in diameter with a 30° tip angle, an inter-electrode distance of 2.0 mm and an arc length of 5 mm. The inter-layer and inter-bead temperature was held at 100 °C throughout deposition. Unequal sub-currents were applied to the two electrodes to regulate the thermal field of the coupled arc, and an overlapping criterion was derived and validated in both single-layer and multi-layer deposition. The conclusions are as follows:
(1) A flat layer requires the overlapping-side remelting zone to reach the apex of the previous bead, where the three-phase interfacial tension drives molten metal into the valley. The inter-bead valley is therefore governed by heat and mass transfer under a volume conservation constraint.
(2) An optimum asymmetric arc thermal field exists for bead overlapping. It is obtained by widening the overlapping side with unequal sub-currents until its width matches the overlapping distance. The required sub-current increment follows the fitted widened-side width relations.
(3) Combined with a wire feed compensation strategy at the edge beads, the criterion yields multi-layer multi-bead deposits with no lack-of-fusion defects. The surface flatness of each layer is better than 0.18 mm, and the intra-layer height error does not accumulate with the layer number.
The criterion is derived from force balance and volume conservation and is not limited to a particular material or electrode geometry. The quantitative ΔW–ΔI relation and the overlapping coefficient vary with the configuration and establishing them for new conditions is the natural extension of this work. The influence of the asymmetric thermal field on microstructures and properties also warrants further study.
Author Contributions
Conceptualization, Q.H.; methodology, Q.H.; software, P.H. and T.W.; validation, Q.H., P.H., T.W. and J.G.; formal analysis, T.W., W.G. and W.Z.; investigation, Q.H., P.H., T.W. and J.G.; resources, W.G. and W.Z.; data curation, Q.H. and T.W.; writing—original draft, P.H., T.W. and J.G.; writing—review and editing, Q.H., W.L., W.G. and W.Z.; visualization, P.H. and J.G.; supervision, Q.H., W.L., W.G. and W.Z.; project administration, Q.H. and W.L.; funding acquisition, Q.H. and W.L. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by National Natural Science Foundation of China (grant number 52305367 and 52375339), and Natural Science Foundation of Jiangsu Province General Program (grant number BK20251829).
Data Availability Statement
The original contributions presented in this study are included in the article material. Further inquiries can be directed to the corresponding author.
Conflicts of Interest
The authors declare no conflict of interest.
References
- Li, X.; Zhao, Z.; Cheng, X.; Chen, H.; Xiong, J. Residual stress and distortion in arc-directed energy deposition: Formation mechanisms, analysis techniques, and mitigation strategies. J. Manuf. Processes 2025, 141, 17–35. [Google Scholar] [CrossRef] [Scilit]
- Xiong, J.; Wen, C. Arc plasma, droplet, and forming behaviors in bypass wire arc-directed energy deposition. Addit. Manuf. 2023, 70, 103558. [Google Scholar] [CrossRef] [Scilit]
- Li, Y.; Han, Q.; Zhang, G.; Horváth, I. A layers-overlapping strategy for robotic wire and arc additive manufacturing of multi-layer multi-bead components with homogeneous layers. Int. J. Adv. Manuf. Technol. 2018, 96, 3331–3344. [Google Scholar] [CrossRef] [Scilit]
- Zhang, Y.; Yan, W.D.; Guo, X.M.; Zhang, Z.W.; Xu, R.Z. Research status and prospect of shape control and property control technology based on melting electrode arc additive manufacturing. Nonferrous Met. Eng. 2021, 11, 17–23. [Google Scholar]
- Wang, Y.; Tang, Z.; Xu, K.; Luo, J.; Zheng, X. The arc design principles and mechanism analysis of pumping gas hollow tungsten negative pressure arc welding or additive manufacturing. J. Manuf. Processes 2025, 149, 364–382. [Google Scholar] [CrossRef] [Scilit]
- Kopf, T.; Glück, T.; Gruber, D.; Staderini, V.; Eugui, P.; Fritze, G.; Mansouri, A.; Schnall, M.; Meyer-Heye, P. Process modeling and control for additive manufacturing of Ti-6Al-4V using plasma arc welding—Methodology and experimental validation. J. Manuf. Processes 2024, 126, 12–23. [Google Scholar] [CrossRef] [Scilit]
- Chen, D.; Chen, H.; Zhang, G.; Xiong, J. Towards automatic control of process stability for thick-wall parts in arc-directed energy deposition based on arc voltage sensing. J. Manuf. Processes 2025, 141, 250–262. [Google Scholar] [CrossRef] [Scilit]
- Benakis, M.; Costanzo, D.; Patran, A. Current mode effects on weld bead geometry and heat affected zone in pulsed wire arc additive manufacturing of Ti-6Al-4V and Inconel 718. J. Manuf. Processes 2020, 60, 61–74. [Google Scholar] [CrossRef] [Scilit]
- Kamal, J.; Sharma, G.; Yogesh, A.; Mulik, R.S.; Swain, A.K. Microstructure Characterization and Mechanical Behavior of 3D-Fabricated Part via Gas Tungsten Arc Welding-Based Wire Arc Additive Manufacturing Process Using AISI4340 Wire. J. Mater. Eng. Perform. 2026, 35, 11574–11584. [Google Scholar] [CrossRef] [Scilit]
- Wang, X.; Wang, A.; Li, Y. An online surface height measurement method for GTAW-based additive manufacturing. Weld. World 2020, 64, 11–20. [Google Scholar] [CrossRef] [Scilit]
- Kobayashi, K.; Nishimura, Y.; Iijima, T.; Ushio, M.; Tanaka, M.; Shimamura, J.; Ueno, Y.; Yamashita, M. Practical application of high-efficiency twin-arc TIG welding method (Sedar-TIG) for PCLNG storage tank. Weld. World 2004, 48, 35–39. [Google Scholar] [CrossRef] [Scilit]
- Leng, X.; Zhang, G.; Wu, L. Experimental study on improving welding efficiency of twin electrode TIG welding method. Sci. Technol. Weld. Join. 2006, 11, 550–554. [Google Scholar] [CrossRef] [Scilit]
- Schwedersky, M.B.; Goncalves e Silva, R.H.; Dutra, J.C.; Reisgen, U.; Willms, K. Arc characteristic evaluation of the double-electrode GTAW process using high current values. Int. J. Adv. Manuf. Technol. 2018, 98, 929–936. [Google Scholar] [CrossRef] [Scilit]
- Han, Q.; Li, D.; Sun, H.; Zhang, G. Forming characteristics of additive manufacturing process by twin electrode gas tungsten arc. Int. J. Adv. Manuf. Technol. 2019, 104, 4517–4526. [Google Scholar] [CrossRef] [Scilit]
- Cao, Y.; Zhu, S.; Liang, X.; Wang, W. Overlapping model of beads and curve fitting of bead section for rapid manufacturing by robotic MAG welding process. Robot. Comput.-Integr. Manuf. 2011, 27, 641–645. [Google Scholar] [CrossRef] [Scilit]
- Xiong, J.; Zhang, G.; Gao, H.; Wu, L. Modeling of bead section profile and overlapping beads with experimental validation for robotic GMAW-based rapid manufacturing. Robot. Comput.-Integr. Manuf. 2013, 29, 417–423. [Google Scholar] [CrossRef] [Scilit]
- Ding, D.; Pan, Z.; Cuiuri, D.; Li, H. A multi-bead overlapping model for robotic wire and arc additive manufacturing (WAAM). Robot. Comput.-Integr. Manuf. 2015, 31, 101–110. [Google Scholar] [CrossRef] [Scilit]
- Fang, X.; Bai, H.; Yao, Y.; Zhang, L.; Lu, B. Research on multi-bead overlapping process of wire and arc additive manufacturing based on cold metal transfer. J. Mech. Eng. 2020, 56, 141–147. [Google Scholar] [CrossRef] [Scilit]
- Hu, Z.; Qin, X.; Li, Y.; Yuan, J.; Wu, Q. Multi-bead overlapping model with varying cross-section profiles for robotic GMAW-based additive manufacturing. J. Intell. Manuf. 2020, 31, 1133–1147. [Google Scholar] [CrossRef] [Scilit]
- Han, Q.L.; Li, X.; Dong, M.; Zhang, G. Enhanced curve-fitting model of the bead section profile and the corresponding overlapping model for twin-electrode gas tungsten arc–based additive manufacturing. Int. J. Adv. Manuf. Technol. 2021, 116, 1151–1167. [Google Scholar] [CrossRef] [Scilit]
- Qu, S.; Qin, G.; Wang, H.; Gao, Y. Evolution rules for cathode erosion and corresponding arc behaviour in tungsten inert gas welding. Sci. Technol. Weld. Join. 2024, 29, 18–28. [Google Scholar] [CrossRef] [Scilit]
- Chen, S.; Zhang, C.; Jiang, F.; Zhang, G.; Li, W.; Xu, B. The physical mechanisms of plasma directional deflection in cross-coupled arc. Phys. Fluids 2025, 37, 015207. [Google Scholar] [CrossRef] [Scilit]
- Chen, Q.; Xie, Z.; Wang, J.; Lin, S.; Dou, Q.; Huang, T. A comparison of the swing and non-swing arc behavior in arc ultrasonic assisted narrow gap GMAW. J. Mater. Res. Technol. 2023, 2, 4698–4710. [Google Scholar] [CrossRef] [Scilit]
- Cui, S.; Dai, P.; Ma, R.; Xu, L.; Pang, S.; Tian, F.; Yu, Y. Mechanism study of flow characteristics of molten pool and keyhole dynamic behavior of K-TIG welding. Int. J. Adv. Manuf. Technol. 2024, 13, 1195–1206. [Google Scholar] [CrossRef] [Scilit]
- Zhong, M.; Jiang, L.; Bai, H.-Y.; Basu, S.; Wang, Z.-J.; Wang, C. Simulating molten pool features of shipbuilding steel subjected to submerged arc welding. J. Iron Steel Res. Int. 2023, 30, 569–579. [Google Scholar] [CrossRef] [Scilit]
- Ozaner, O.C.; Talemi, R.; Tjahjowidodo, T.; Sharma, A. The influence of the wire and arc additive manufacturing parameters on the surface irregularities. J. Micromanuf. 2025, 8, 22–31. [Google Scholar] [CrossRef] [Scilit]
- Geng, H.; Li, J.; Xiong, J.; Lin, X.; Zhang, F. Optimization of wire feed for GTAW-based additive manufacturing. J. Mater. Process. Technol. 2017, 243, 40–47. [Google Scholar] [CrossRef] [Scilit]
- Li, Y.; Sun, Y.; Han, Q.; Zhang, G.; Horváth, I. Enhanced beads overlapping model for wire and arc additive manufacturing of multi-layer multi-bead metallic parts. J. Mater. Process. Technol. 2018, 252, 838–848. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.