Abstract
Framework-level comparisons of cast and selective laser-melted (SLM) cobalt–chromium (Co–Cr) fixed dental prosthesis (FDP) frameworks remain limited. This exploratory pilot study compared the monotonic load-bearing capacity of ten unveneered posterior maxillary four-unit Co–Cr frameworks (abutments 14 and 17) manufactured from one CAD design either by casting of milled wax patterns (n = 5) or by SLM (n = 5), using two alloys of practically identical composition. Frameworks were loaded monotonically (1 mm/min) to fracture or to a preset 4500 N test limit. All five cast frameworks fractured, at 938.53–1134.63 N (mean 1012.47 ± 77.40 N). None of the SLM frameworks fractured: all five reached the test limit (4498.36–4501.34 N) without macroscopic fracture (run-outs), so their fracture loads exceed the attained loads. The lowest SLM run-out load exceeded the highest cast fracture load by a factor of 3.96. Under these conditions, the SLM frameworks showed a substantially higher monotonic load-bearing capacity. These results characterize laboratory static strength only; fatigue behavior and clinical durability require cyclic testing of veneered restorations.
1. Introduction
The performance of a cobalt–chromium (Co–Cr) fixed dental prosthesis (FDP) is a structural outcome: alloy properties, connector geometry, processing history, and the supporting assembly jointly determine its response to load. Contemporary comparisons have documented manufacturing-dependent differences in hardness, strength, grain structure, and porosity among cast, milled, and additively produced dental Co–Cr alloys [1,2]. A load measured on a complete framework therefore cannot be interpreted as an intrinsic alloy strength without specifying the geometry and boundary conditions. Framework testing remains useful precisely because it interrogates the manufactured component rather than an idealized material coupon.
Selective laser melting (SLM), a laser powder bed fusion process, changes the thermal history through localized melting and rapid solidification. A controlled comparison of cast and SLM Co–Cr specimens linked differences in bend-fatigue behavior with their microstructures [3]. Residual stresses, phase constitution, strength, and ductility can subsequently respond to thermal treatment [4,5]. Such evidence establishes plausible pathways by which fabrication affects performance, but the direction and magnitude of those pathways depend on the actual alloy, processing parameters, and postprocessing sequence.
Geometry creates a second, interacting pathway. Experiments modifying the internal architecture of multiunit Co–Cr frameworks have shown that changes in mass need not map directly onto changes in measured flexural response [6]. Recent experimental and finite element work on metal–ceramic FDPs identified an association between pontic volume, connector stress, and fracture resistance [7]. These findings make connector failure a relevant outcome and show why a nominally common digital design must be distinguished from verified as-built dimensions. A study of one design can compare its recorded outcomes; it cannot identify a span–resistance relationship.
Evidence from ceramic CAD/CAM restorations also shows why geometry requires material-specific assessment. Hajaj et al. found that cervical margin design affected fracture performance in lithium disilicate crowns but not in zirconia crowns under their test conditions [8]. A posterior zirconia single-retainer case report illustrates a different approach to preparation and supplementary support [9]. These findings motivate explicit reporting of preparation and support geometry; they do not establish fracture-load thresholds for Co–Cr frameworks.
Manufacturing can affect dimensional adaptation and material response. Layer thickness and build orientation have affected the fit of laser-produced multiunit Co–Cr frameworks [10,11]. Orientation and thermal treatment can interact with fit and hardness, while manufacturing direction influences the deformation and tensile response of heat-treated specimens [12,13]. Studies of posterior and anterior FDPs report workflow-dependent adaptation [14,15], and clinical measurements show that marginal and internal fit may favor different workflows [16]. These distinctions matter mechanically because seating and support contact help define how a framework transmits the applied force.
Digital design transfer also requires a clear distinction between workflow feasibility and quantitative validation. Titihazan et al. described printed and milled preparation guides as a qualitative technical feasibility study, without a statistical comparison of dimensional accuracy [17]. For this manufacturing question, a common CAD design remains the intended geometry; equivalence between the manufactured connectors and their seating requires direct measurement.
The completed restoration introduces further processing and additional failure endpoints. Annealing and porcelain firing have altered adaptation in additive workflows [18], while firing studies of cast and milled implant-cemented frameworks document dimensional and microstructural changes [19,20]. A framework-only test therefore addresses a narrower question than veneer adhesion, fatigue durability, or clinical survival. That narrower question becomes statistically challenging when a framework remains intact at the maximum permitted test load: the terminal reading indicates a lower bound on fracture resistance rather than a measured fracture load.
The present exploratory pilot study analyzes endpoint data from ten Co–Cr FDP frameworks assigned to casting or SLM to characterize initial mechanical observations and inform independent validation. Its primary analytical objective was to compare load tolerance over a common, fully observed force range while retaining the distinction between fractures and intact specimens stopped at the test limit (run-outs). A secondary objective was to express, using only the recorded observations, how far the unobserved SLM fracture loads must exceed the measured cast fracture loads. The documented experiment used one nominal digital design. Supplementary analyses that do not contribute to the conclusions (prior sensitivity of failure probability, influence diagnostics, prospective sample-size scenarios, and an elementary beam illustration) are reported in the Supplementary Materials.
2. Materials and Methods
2.1. Pilot Study Design and Provenance of the Experimental Data
This exploratory pilot study compared ten Co–Cr FDP frameworks: five cast (MELT_1–MELT_5) and five produced by SLM (SINT_1–SINT_5). The frameworks were scanned (Medit Link 3.4.12), designed (exocad DentalCAD), and fabricated in a dental laboratory, and mechanical testing was performed at the Faculty of Mechanical Engineering, Politehnica University Timișoara, Romania. For every test, testXpert recorded the maximum attained force, the fracture status, and the crosshead displacement at maximum force. The complete load–displacement curves were retrieved for six tests (MELT_1–MELT_3 and SINT_1–SINT_3) and are provided in the Supplementary Materials (Figure S7, Table S11, raw data file). For MELT_4, MELT_5, SINT_4, and SINT_5, the original curve files were not retained, and only the endpoint values are available. Therefore, no stiffness, yield, or energy-based property is claimed for the full sample; matched-force stiffness is reported descriptively for the six recovered curves only, and the conclusions rest on the recorded fracture/run-out outcomes and endpoint loads.
This study used a posterior maxillary segment with an edentulous space bounded by two abutments—14 and 17. Both workflows used a common nominal digital framework design: one design and one span. Each framework was the unit of observation. We did not count connectors, photographs, sampled curve points, or the 25 possible cross-workflow specimen pairs as independent replicates. Specimens were not randomly allocated, testing order was not randomized, and outcome assessment was not blinded. The five SLM frameworks were built in a single job on one build plate; the wax patterns for the cast frameworks were milled from discs of the same wax lot, and the number of casting cycles was not recorded. Each workflow therefore represents a single production run, production batch is confounded with fabrication workflow, and between-batch variability within a workflow could not be estimated. Table 1 summarizes the materials, fabrication, and test conditions.
Table 1.
Materials, fabrication, and test conditions.
The pilot sample comprised all ten available force/event records, with five specimens per workflow. An a priori sample-size calculation was not documented. The pilot designation reflects the analysis’s exploratory scope and its role in identifying endpoint, measurement, and reporting requirements for independent validation. Prospective sample-size scenarios for a future confirmatory study are reported only in the Supplementary Materials (Supplementary Results S1 and Methods S4).
2.2. Fabrication Workflows and Exposure Definition
For casting, the working models were scanned and digital files were prepared in a workflow using hyperDENT. The model was scanned with a Medit scanner (Medit Link 3.4.12), the frameworks were designed in exocad DentalCAD, and the connector cross-sections were checked digitally before manufacture (Table 1). Wax patterns were milled from breCAM.wax discs (Bredent) using hyperDENT Compact V9.1. Wax patterns were milled using an imes-icore CORiTEC 250i dry unit, checked on the model, invested in refractory material, and subjected to wax elimination. The Co–Cr alloy listed in Table 1 was cast into the molds. After cooling and recovery, frameworks were finished, airborne-particle abraded, and checked for seating. Frameworks of both workflows were finished with tungsten carbide burs; airborne-particle abrasion parameters were not recorded.
The SLM workflow used the same nominal digital design and Co–Cr powder. Frameworks were produced layer by layer, removed from the build plate, finished, airborne-particle abraded, and checked for seating and interference. The frameworks were built on a SISMA MYSINT 100 system (Sisma S.p.A., Piovene Rocchette, Italy) with the powder, processing parameters, support strategy, and post-build heat treatment listed in Table 1. The equipment allows laser powers up to 200 W and layer thicknesses of 10–50 µm; the values in Table 1 are the settings actually used for these frameworks, not equipment limits or values taken from other studies. The frameworks were tested unveneered. Visual seating checks establish the intended assembly procedure but do not demonstrate equivalent connector dimensions or quantify adaptation.
The exposure therefore the recorded fabrication workflow, casting versus SLM. It was not an isolated intervention on manufacturing technology with chemically identical alloys and verified equivalent final geometry. This definition prevents an alloy-composition difference, dimensional discrepancy, or postprocessing effect from being automatically attributed to laser melting. No undocumented parameter was filled in using typical settings from another laboratory or manufacturer. The cast alloy (Wirobond SG, Bremen, Germany) and the SLM powder (Mediloy S-Co, Bremen, Germany), both from the same manufacturer, have practically identical nominal compositions (differences ≤ 0.1 wt% for every element; Table 1). A difference in chemical composition is therefore an unlikely explanation for the observed difference, which is more plausibly related to processing-dependent microstructure, porosity, and as-built geometry; batch-specific composition was not analyzed.
2.3. Mechanical Loading and Stopping Rule
Frameworks were positioned on a common experimental support to reproduce the relationship between the two abutments. The support was an SLM-printed metal master model with the two prepared abutments (Figure 1a), clamped in a machine vise on the testing machine base (Figure 1b,c); the frameworks were seated on the abutments without cement. The photographs show the seating and indenter configuration for the photographed subset (Figure 1). Load was applied perpendicular to the occlusal plane at mid-span, over the 15–16 connector region between the two pontics, with the same fixture and contact location for all ten frameworks (Figure 1b,c).
Figure 1.
Available photographic documentation: (a) laboratory model; (b) loading arrangement; (c) lateral view of indenter contact; (d) grouped frameworks after testing in the photographed six-specimen subset. Panels are reproduced from the experimental record and are not scaled. They illustrate the documented setup and specimen appearance; photographs of MELT_4, MELT_5, SINT_4, and SINT_5 were unavailable. These panels do not constitute microscopic fracture analysis. Fracture sites of all cast specimens are listed in Table 2.
Testing used a Zwick/Roell Z005 universal testing machine, a 5 kN load cell with accuracy class 0.5, and testXpert III (ZwickRoell) software under displacement control at ambient temperature. The test applied a 100 N preload at 10 mm/min, then loaded at 1 mm/min using a 10 mm hemispherical indenter. Force and crosshead displacement were recorded. Crosshead displacement was zeroed once the 100 N preload had been reached, so all reported displacements are referenced to the preloaded state. Each test ended either at macroscopic fracture or when the force reached the upper force limit of 4500 N, which was set in testXpert at 90% of the 5 kN load-cell capacity to protect the load cell. All cast frameworks fractured below this limit, whereas all SLM frameworks reached it without fracture (run-outs). The limit was an equipment-related end point, not a property of the frameworks, and it prevented observation of SLM fracture loads. The load-cell class was retained as an equipment specification and was not converted into specimen-specific uncertainty without calibration records.
2.4. Event Definition and Endpoint Extraction
The event of interest was macroscopic structural fracture. Fracture was confirmed for all five cast frameworks by the test record and visual inspection of the separated parts; the fracture site of each specimen and its source of evidence are listed in Table 2 and Supplementary Table S10. For specimen i, Ti denotes its latent load at that event, Ci the stopping load, Xi the observed endpoint, and δi the event indicator. Equation (1) expresses the observation mechanism. A run-out, i.e., a framework that reached the test limit without fracture, provides Ti > Ci; it does not provide Ti = Ci. The five SLM readings were 4500.07, 4499.41, 4499.62, 4498.36, and 4501.34 N with δi = 0. All five cast readings had δi = 1. Every available force/event record was included. In statistical terms, a run-out is a right-censored observation; the term run-out is used throughout this article.
Table 2.
Individual specimen measurements, fracture status, and fracture site.
Endpoint crosshead displacement was available for all five specimens per workflow. All ten reported values were included without imputation. Cast displacement occurred at fracture, whereas SLM displacement occurred at the stopping limit. Because displacement was referenced to the preloaded state, the force increment above the preload divided by the endpoint displacement, (F − 100 N)/d, can be calculated for each specimen. This terminal force-to-displacement ratio is a simple arithmetic ratio of two endpoint values obtained at different load levels and in different physical states (fracture for casting; continued loading without fracture, possibly with plastic deformation, for SLM). It does not represent structural stiffness or any mechanical property, it is not compared between workflows, and it is reported only as a supplementary arithmetic summary (Supplementary Table S2). Permanent set, local strain, flexural stress, yield load, and integrated energy absorption were not recoverable from endpoint records.
2.5. Statistical Analysis
2.5.1. Descriptive Summaries and the Restricted Estimand
The pilot analysis was developed after inspection of the record and was not preregistered. Individual reported values are presented with means, sample standard deviations (denominator n − 1), medians, ranges, and sample coefficients of variation where the endpoint is observed. Force, event, and displacement summaries use five specimens per workflow. No measurement was imputed and no normality screen was used to justify a large-sample test. We did not treat attained SLM loads as a fracture-strength distribution; their proximity to 4500 N reflects the stopping rule. Displacement summaries are descriptive because workflows ended at different forces and event states. Because each workflow represents a single production run, the specimen-level observations are the primary results; inferential quantities are secondary and conditional on the ten tested specimens.
We defined the common truncation load τ as the smallest attained load in the pooled set of run-outs (tests that ended without fracture): 4498.36 N. All five such tests belonged to SLM, but the selection rule used event records rather than reassigned workflow labels. Every specimen was observed through either fracture or τ, so no run-out occurred before this common limit. Capped load tolerance Yi(τ) and its group means are defined in Equation (2). The primary contrast is SLM minus cast; the capped mean ratio was also reported. This is an analysis over an empirically supported force range, not a claim that τ is a clinically validated limit.
The group mean capped load equals the area under the empirical fracture-free proportion curve from zero to τ, as expressed in Equation (3). This identity makes the mechanical interpretation explicit: the estimand measures load tolerance accumulated over the observed force range. Its axis is applied force in N, not follow-up time. Since there is no earlier run-out, the area can be calculated directly from the ten capped endpoints without estimating an unobserved tail. The SLM capped mean equals τ by construction; a zero sample variance of its capped values would not imply a zero variance of true fracture loads.
2.5.2. Exact Inference and Frequentist Uncertainty
The two-sided permutation calculation enumerated all 252 ways to assign ten capped endpoints to groups of five. For each allocation, the difference in group means was calculated. Equation (4) gives the fraction whose absolute contrast was at least as large as the observed value. Enumeration removes reliance on an asymptotic reference distribution, but does not remove the need for independent, exchangeable specimens under the null. In the absence of documented randomization and batch replication, this is a conditional exploratory analysis of group separation within the pilot, not a randomization-based causal estimate. Because the specimens of each workflow came from one production run, the p value describes the separation of these ten specimens and cannot be generalized to the manufacturing processes; it is reported as a secondary, descriptive measure.
Failure by τ was additionally treated as a binary outcome. Group-specific equal-tailed 95% Clopper–Pearson confidence intervals were reported, and Fisher’s exact test was used only as a consistency check on the same separation. For the failure-risk difference θCast − θSLM, a conservative interval with at least 95% joint coverage at a fixed threshold was constructed by combining two 97.5% Clopper–Pearson intervals through the Bonferroni inequality. Its limits are the cast lower limit minus the SLM upper limit and the cast upper limit minus the SLM lower limit. This construction is deliberately conservative and does not provide selection-adjusted coverage for choosing τ after examining the experiment. The failure-risk difference has the opposite orientation to the capped-load contrast because fewer fractures favor SLM.
Complete cross-group ordering and Cliff’s delta were retained as descriptive summaries. No degenerate bootstrap interval from the completely separated observations was used to suggest precision. No unrestricted SLM mean or variance, finite hazard ratio, Weibull modulus, or extrapolated failure percentile was fitted. The absence of SLM fractures supports lower bounds but leaves its distribution beyond the stopping loads unidentified. An exploratory Bayesian sensitivity analysis of failure probability is reported only in Supplementary Methods S3 (Table S6, Figure S3), following the conjugate framework described in [21]; it does not contribute to the conclusions.
2.5.3. Identification Bounds
Deterministic lower bounds were calculated by retaining Ti > Ci for each run-out. The minimum SLM attained load was compared with the largest measured cast fracture load; the true SLM sample mean and its contrast with the observed cast mean were bounded using all five individual stopping loads. These are statements about the tested specimens, not population confidence limits or clinical safety factors. Computed lower bounds involving means or ratios were rounded downward to preserve the inequalities. No finite upper bound was available. Descriptive force-range and single-specimen influence diagnostics are reported in Supplementary Methods S2 (Tables S3 and S4, Figure S5).
2.6. Computational Reproducibility
Calculations used Python 3.12.14, NumPy 2.3.5, and SciPy 1.17.0. The package provides ten force/event/displacement input records with record-level provenance, all force-to-displacement ratios, every permutation allocation, truncation and deletion diagnostics, posterior results and density coordinates, exact prospective power curves, numerical verification outputs, and figure-generation code. The 96 independent numerical checks include exact rational displacement and ratio arithmetic, sample variability, and alternative posterior integrations. The uniform-prior directional probability was checked against 923/924. Reported values retain their supplied precision; full computational precision is retained in machine-readable output, and manuscript estimates are rounded for readability.
3. Results
3.1. Recorded Specimen Outcomes
All ten pilot specimens had endpoint load, macroscopic fracture status, and terminal displacement available (Table 2). MELT_1–MELT_5 fractured at 964.26, 1134.63, 938.53, 987.46, and 1037.48 N, respectively. The mean measured fracture load was 1012.47 ± 77.40 N, median 987.46 N, range 938.53–1134.63 N, and sample coefficient of variation 7.65%. Fracture was confirmed for all five cast frameworks by the test record and by macroscopic separation of the framework. In the three photographed cast frameworks (MELT_1–MELT_3; Figure 1d), fracture occurred at connector regions and separated intact units; one framework separated at the central (15–16) connector into two two-unit segments. The fracture sites of MELT_4 and MELT_5 were not documented (Table 2). No quantitative porosity measurement, metallographic section, or microscopic fracture-origin assessment was available.
SINT_1–SINT_5 remained macroscopically intact at attained loads of 4500.07, 4499.41, 4499.62, 4498.36, and 4501.34 N, respectively. Each was a run-out and provided only a lower bound on its true fracture load. These five terminal readings describe the experiment’s stopping behavior, not the distribution of SLM fracture strength. The observations do not quantify residual deformation after unloading or exclude earlier subvisual damage. Because displacement at the test limit reached approximately 2 mm, plastic deformation of the SLM frameworks before termination cannot be excluded; the photographed SLM frameworks showed no visible permanent deformation (Figure 1d), but the permanent set was not measured.
3.2. Capped Load Tolerance and Exact Test
At the common fully observed limit τ = 4498.36 N, the cast capped mean was 1012.47 N and the SLM capped mean was 4498.36 N. The primary observed contrast was 3485.89 N and the capped mean ratio was 4.44 (Table 3). Every SLM lower bound exceeded every measured cast fracture load. All 25 dependent cross-workflow specimen comparisons favored SLM, yielding a descriptive Cliff’s delta of 1.00. These comparisons reuse the same ten frameworks.
Table 3.
Primary comparison at the common load limit.
Two of the 252 equally sized allocations were at least as extreme as the observed absolute contrast, giving p = 0.00794 for the two-sided exact permutation calculation. Fisher’s exact consistency check gave the same value. For complete separation with five specimens per workflow, 2/252 is the smallest attainable two-sided value in this balanced allocation scheme. The conditional exploratory comparison is below 0.05, but neither that threshold crossing nor complete separation establishes prospective power, a causal manufacturing effect, or a confirmatory design.
Failure by τ occurred in 5/5 cast specimens and 0/5 SLM specimens. Their group-specific exact 95% confidence intervals were 47.8–100% and 0–52.2%. The observed cast-minus-SLM failure-risk difference was 100 percentage points; its conservative simultaneous 95% interval extended from −16.7 to 100 percentage points. This conservative construction can include zero despite the exact test result because it combines two simultaneous group intervals rather than inverting that test. Figure 2 retains event and run-out status alongside the force-dependent fracture-free proportions and group-specific intervals.
Figure 2.
Load tolerance and uncertainty in the ten-specimen pilot. (a) Five cast fracture loads (crosses) and five attained SLM loads without fracture (circles; arrows indicate run-outs, whose fracture loads exceed the attained loads). The dotted line marks τ = 4498.36 N. (b) Observed fracture-free proportions across force, truncated at τ without extrapolation. (c) Failure proportions by τ with exact 95% Clopper–Pearson confidence intervals, n = 5 per workflow. No SLM fracture load is imputed.
3.3. Lower Bounds on the Unobserved Fracture Loads
The weakest attained SLM lower bound exceeded the greatest measured cast fracture load by 3363.73 N. Their attained-load ratio was approximately 3.9646; every tested SLM fracture load was more than 3.9646 times the greatest cast fracture load observed in this set. This is a conservative ordering statement about these ten specimens; it is not a population strength ratio or an allowable clinical load.
Using all five run-out loads, the true mean SLM fracture load for these specimens was strictly greater than 4499.76 N. Its true sample mean contrast with the cast group was therefore greater than 3487.28 N, and its true sample mean ratio greater than 4.4443. There was no identifiable upper bound. The capped analysis uses one common limit, whereas these deterministic bounds retain each specimen’s own attained load. Neither calculation supplies an unrestricted population mean or its confidence interval.
3.4. Endpoint Displacement
Across all five cast specimens, mean displacement at fracture was 1.459 ± 0.357 mm, median 1.547 mm, range 0.871–1.804 mm, and sample coefficient of variation 24.46%. Across all five SLM specimens, mean displacement at the test limit was 42.078 ± 0.111 mm, median 2.053 mm, range 1.942–2.225 mm, and sample coefficient of variation 5.32%. All ten displacement values are crosshead displacements at maximum force from the testXpert endpoint record; for the six recovered curves, they coincide with the curve values (Supplementary Table S11). The larger terminal SLM displacement occurred at a substantially higher force and in a different event state. It does not establish a matched-force difference in elastic deflection or clinical deformability.
Terminal force-to-displacement ratios, (F − 100 N)/d, are listed in Supplementary Table S2 as arithmetic summaries only; they are not stiffness values and are not compared between workflows. In the six recovered load–displacement curves (Supplementary Figure S7, Table S11), loading was continuous up to maximum force; the largest force drop before maximum force was 33 N and occurred below 230 N, during initial seating, and no drop larger than 7.5 N occurred above 300 N, indicating no specimen slippage or fixture backlash during the load-bearing phase. Over the common 200–800 N interval, apparent system stiffness was 1170–1384 N/mm for SINT_1–3 and 436–1401 N/mm for MELT_1–3; MELT_1 behaved like the SLM frameworks until fracture, whereas MELT_2 and MELT_3 were more compliant. With three curves per workflow, these values are descriptive.
4. Discussion
4.1. Interpretation of the Pilot Mechanical Findings
The principal pilot observation is a separation in recorded failure behavior: all five cast frameworks fractured near 1 kN, while all five SLM frameworks remained macroscopically intact at attained loads near 4.5 kN. Fracture was confirmed in all five cast frameworks, at the sites listed in Table 2. Preserving run-out status distinguishes observed fractures from the five intact stopping records. The restricted contrast quantifies the demonstrated force-range difference, and the specimen-level lower bounds show how far the true sample fracture contrast must extend. The SLM tail remains unobserved, and the availability of continuous traces for only six of the ten tests limits verification of experimental comparability. Because no SLM framework fractured, the experiment establishes only that the SLM fracture loads exceeded approximately 4.5 kN in this configuration; the true size of the difference cannot be estimated, and a test range allowing fracture in both groups is required for that purpose.
The direction is compatible with published differences in mechanical properties and microstructure among dental Co–Cr workflows [1,2] and with improved fatigue behavior in a controlled cast-versus-SLM coupon comparison [3]. Those studies provide plausible mechanisms, not measurements of the present frameworks. The present record cannot establish whether connector failure initiated at a casting pore, an inclusion, a locally thin section, a finishing defect, or a stress concentration altered by seating. A finer laser-produced microstructure is also a hypothesis until these specimens independently demonstrate it. Conversely, laser-melted Co–Cr may contain residual porosity or lack-of-fusion defects whose effect is limited under a single monotonic load but may become critical under cyclic loading, because the fatigue behavior of SLM Co–Cr depends on its defect population and microstructure [3]. The present static test cannot detect this vulnerability.
A mechanism-focused follow-up should connect the structural event with measurements at the fracture origin. Microcomputed tomography could identify internal discontinuities before testing; dimensional scans could quantify the finished connector sections; metallography and phase-sensitive characterization could document the substrate; and scanning electron microscopy with compositional analysis could examine fracture surfaces. These measurements would distinguish a geometry-related reduction in section modulus from a defect-associated reduction in local resistance. Their proposed use should not be confused with analyses already performed in this pilot.
4.2. Connector Geometry and the Meaning of Apparent Stiffness
Nominal section area alone is insufficient for describing bending. Two sections with the same area can have different second moments if material is redistributed away from the neutral axis. Connector curvature can also create a local stress field absent from a simple rectangular beam. The nominally common digital file therefore constrains design intent, while the final metrology is required to establish a comparable section modulus, contour, and seating. In a future geometry study, force values in N should be accompanied by measured dimensions and a defensible stress model if comparisons in MPa are intended. In the present study, connector dimensions were controlled at the CAD stage (Table 1) but were not verified on the finished frameworks; nevertheless, small differences in as-built connector depth would have a disproportionate effect on bending resistance (Supplementary Methods S5) and must be considered when interpreting the difference between workflows. All three CAD connectors had cross-sectional areas of approximately 12 mm2 (11.94–12.30 mm2; Table 1). The central 15–16 connector lies directly beneath the loading point, where a centrally loaded span carries the greatest bending moment, which is consistent with the separation of one cast framework at this connector (Section 3.1).
Crosshead stiffness presents an additional identifiability problem. In a locally linear series system, machine, fixture, seating, and framework compliances are added. The reciprocal total compliance is an apparent system stiffness, which cannot be assigned to the framework alone without separate displacement or compliance measurements. Local framework displacement measured optically or by an appropriately positioned sensor would reduce this ambiguity. Repeated loading within a defined elastic interval and an unloading segment would help distinguish reversible displacement from the permanent set. These procedures were not part of the present protocol. The six recovered curves show only small seating adjustments below 230 N and no slippage or backlash during the load-bearing phase (Section 3.4); for MELT_4, MELT_5, SINT_4, and SINT_5, such artifacts cannot be excluded from the displacement values. Displacement is therefore reported descriptively, and stiffness is reported only as an apparent system value for the recovered curves. The force endpoints are less affected by such artifacts, because the fracture or run-out force is recorded directly by the load cell.
4.3. From the Framework to the Finished Restoration
The loads reached by the SLM frameworks (above 4.5 kN) far exceed physiological masticatory forces, and all loads were applied once, monotonically, to unveneered frameworks. Clinically, metal–ceramic FDPs fail predominantly through fatigue under repeated masticatory loading, chipping or delamination of the veneering ceramic, or loss of retention, rather than through static fracture of the bare metal framework. The present results therefore characterize the laboratory monotonic strength of the frameworks and must not be read as evidence of greater clinical reliability or durability of SLM restorations.
A high framework load tolerance does not resolve the failure pathways introduced by veneering. Recent interfacial studies document alloy- and workflow-dependent ceramic bonding [22,23]. Annealing temperature can affect metal–ceramic bond characteristics [24], and surface treatments may act differently across Co–Cr substrates [25]. The SLM hatch distance and laser power have altered properties relevant to porcelain bonding [26,27], while comparisons of laser texturing and conventional conditioning show that the chosen surface process matters [28]. The metal substrate, oxide formation, firing sequence, and interface therefore constitute an additional system requiring its own validation.
A recent pilot comparison reported higher flexural interface performance for the tested cast Co–Cr ceramic system than for the printed system [29]. That finding need not conflict with the present framework outcome: the events, assemblies, and loading definitions are different. Studies of screw-retained metal–ceramic restorations and aged tooth-to-implant FDPs have likewise identified veneer or connection damage that a framework-only monotonic test does not measure [30,31]. Work varying cantilever length and material combinations further demonstrates the importance of assembly and geometry [32]. Manufacturing decisions should therefore be evaluated against the intended restoration endpoint rather than a single large terminal force.
Failure detection also defines the measured tolerance. An acoustic-emission pilot on implant-supported hybrid bars detected microdamage before a conspicuous terminal event [33]. The present event was limited to source-reported macroscopic fracture, so we cannot exclude earlier microdamage. Standardized bending studies of titanium and Co–Cr [34] address a material question under controlled dimensions, whereas the present experiment measures the force tolerance of the supported framework. Coupon strength in MPa, framework force in N, and survival under fatigue are distinct outcomes and require separate translation models.
Studies of other restorative materials likewise evaluate fracture resistance and optical durability as separate endpoints [35,36]; their nonmetallic materials do not supply failure-load estimates for the present Co–Cr frameworks.
4.4. Processing Quality and Biological Performance
SLM is a process family rather than one reproducible set of material properties. Evidence that fit depends on layer thickness, orientation, thermal treatment, and firing [10,11,12,18] supports recording the entire fabrication sequence. Clinical adaptation can also differ by the measured region [16]. Adjacent removable-prosthesis evidence is useful for illustrating this dependence: a randomized crossover trial found the overall adaptation of direct digital SLM manufacture consistent with conventional manufacture, while clasp experiments linked retentive response with deformation and processing [37,38]. Optimized powder-bed-fused clasps and studies of presintered Co–Cr discs further show that the relevant performance criterion is component-specific [39,40]. These findings inform process control but do not provide survival estimates for the present FDPs.
Powder history is part of that process definition. Reuse studies have reported preserved metal–ceramic bonding while also documenting changes in powder morphology, framework microstructure, or ion release [41,42,43]. Reuse, stress relief, surface finishing, and ceramic firing can therefore produce different outcomes even when a single monotonic test suffices. Because only one powder condition and one thermal protocol were tested, the observed SLM tolerance should be attributed to the recorded workflow, not generalized to every powder reuse or thermal protocol.
Biological performance (corrosion behavior, ion release, and cytocompatibility) depends on alloy composition, manufacturing route, build orientation, and the chemical environment [44,45,46,47,48,49]; it was not assessed here and cannot be inferred from load tolerance.
Finishing and polishing affect the roughness, corrosion-related behavior, and dimensions of laser-produced frameworks [50,51]; finishing parameters should therefore be documented alongside fabrication in future studies.
4.5. Statistical Interpretation
With no fractures in the SLM group, no statistical procedure can characterize the SLM fracture-load distribution or compensate for this design limitation; the inferential results are therefore secondary to the specimen-level observations. With five specimens per workflow, the balanced permutation reference contains 252 allocations; complete ordering gives the observed two-sided p = 0.00794. This conditional exploratory evidence of separation does not establish prospective power or resolve the undocumented sampling and batch structure. The separate exact 95% intervals still permit SLM failure probabilities up to 52.2%. The conservative simultaneous risk-difference interval spans zero because it combines two group intervals rather than inverting the permutation or Fisher test. It therefore addresses uncertainty differently from the reported hypothesis test.
The restricted mean and the deterministic lower bounds solve different problems. The former is fully observed within τ and can be compared conditionally without assigning unobserved failures; the latter proves an ordering for these particular intact specimens. Neither identifies the SLM population tail. Raising τ while no SLM fracture is observed necessarily increases the capped contrast once all cast specimens have failed. That dependence is an intrinsic feature of the estimand and should be reported, as it is here, rather than hidden behind one headline ratio.
Each workflow was represented by a single production run (Section 2.1). The fabrication method and production batch therefore cannot be separated, and the exact test, which assumes independent and exchangeable specimens, describes the separation of these ten specimens rather than a property of casting or SLM in general. Replication across independently produced batches is required before the difference can be attributed to the manufacturing route. All ten terminal displacements are reported, and six of them could be verified against the recovered curves; for the remaining four, displacement origin and protocol implementation cannot be verified independently. Future inference should specify whether its target is a laboratory workflow, an independently produced batch, or a broader manufacturing process.
4.6. Implications of the Pilot for Independent Validation
The next study should retain the complete load–displacement curves and calibration records and measure the as-built connector dimensions of every specimen. A common digital file should include as-built metrology. Manufacturing should span independently replicated batches, with specimens randomized across batch positions and testing order where feasible. Specify event classification before testing, ideally separating first detectable damage, permanent set, connector fracture, and veneer damage when those outcomes are relevant. These reporting and bias-control priorities are consistent with the domains addressed by the QUIN tool for dental studies [52]; a formal QUIN score was not retrospectively assigned. A previous comparison of cast, milled, and SLM three-unit Co–Cr frameworks reported stiffer and harder SLM frameworks, consistent with the higher apparent stiffness of most SLM curves in the present study, but also found that the fabrication route altered the as-built framework design [53]; identical, metrologically verified designs are therefore essential for future strength comparisons.
For monotonic testing, a force range that produces observable failures in both workflows would improve estimation of the full fracture distribution, provided fixture and load-cell capacity remain appropriate. Retesting the present SLM frameworks to fracture was not possible: they are no longer available to the authors, and frameworks already loaded to 4.5 kN, with possible plastic deformation, would not provide valid first-loading fracture loads. A new series tested with a higher-capacity load cell (for example, 10 kN or more) is therefore required to determine SLM fracture loads. When run-outs are expected, the primary range and stopping rule should be set in advance and run-outs retained in the analysis. Local displacement measurement, machine and fixture compliance checks, and common loading intervals would support a defensible stiffness endpoint. An independent cyclic experiment with defined aging, loading, and run-out criteria is needed for fatigue resistance; monotonic force tolerance does not supply that endpoint.
A span-related question requires a factorial design with both workflows represented at multiple prespecified spans and with connector geometry documented at each span. The workflow-by-span interaction should be an explicit target rather than inferred from separate significance tests at different geometries. The batch should enter the sampling and analysis structure. Once sufficient failures are observed, a fracture-load or censoring-aware model could evaluate this interaction while accounting for measured geometry. Its sample size and assumptions must match that multivariable endpoint rather than the present ten-record pilot.
Five intact SLM specimens yield an upper limit of 52.2%, so the pilot does not establish a low population failure probability despite the high attained forces. Prospective sample-size scenarios for a confirmatory study are given in Supplementary Results S1 and Supplementary Methods S4.
4.7. Limitations
This study has several limitations. First, it exclusively characterizes the monotonic (single, quasi-static) load-bearing capacity of unveneered frameworks under laboratory conditions. It does not reflect clinical durability, which depends on fatigue under cyclic masticatory loading, the veneering ceramic, cementation, and the oral environment, and which requires cyclic (fatigue) testing of finished, veneered restorations. Second, SLM Co–Cr may contain residual porosity and lack-of-fusion defects that are largely tolerated under a single static load but can act as crack-initiation sites under cyclic loading; porosity was not assessed, so the static advantage of the SLM frameworks cannot be extrapolated to fatigue resistance. In a recent comparison of cast and SLM Co–Cr specimens, the cast specimens withstood more loading cycles than the SLM specimens at the same load, and fatigue cracks initiated at near-surface pores [54]. Third, no SLM framework fractured before the test limit, so the SLM fracture loads, and hence the true magnitude of the difference, remain unknown; the frameworks were not available for retesting. Fourth, each workflow was represented by five specimens from a single production run, one framework design, and one alloy product, so the effects of the manufacturing route and production batch cannot be separated, although the two alloys have practically identical nominal compositions. Fifth, continuous load–displacement curves were retained for only six of the ten tests, so stiffness is reported descriptively for three specimens per workflow, and testing artifacts cannot be excluded for the remaining four displacement values. The SLM processing parameters and post-build heat treatment, the casting parameters, and the as-built connector dimensions could not be retrieved. Finally, specimens were not randomized, and outcome assessment was not blinded.
5. Conclusions
Under identical monotonic loading of one four-unit posterior design, all five cast Co–Cr frameworks fractured at 938.53–1134.63 N, whereas none of the five SLM frameworks fractured up to the test limit of approximately 4500 N. Fracture was confirmed in every cast framework, at the sites listed in Table 2. The SLM frameworks therefore withstood at least about four times the load that fractured the cast frameworks, which indicates a substantially higher static load-bearing capacity of the SLM frameworks under the tested conditions. Because the SLM fracture loads were not reached, the true magnitude of the difference remains unknown. Because the cast and SLM alloys had practically identical nominal compositions, the difference is attributable to the fabrication workflow rather than to alloy chemistry; with one production run per workflow, however, it cannot yet be generalized beyond these batches. These findings exclusively describe the laboratory monotonic strength of unveneered frameworks; they do not demonstrate clinical superiority or greater durability of SLM restorations. In particular, possible internal porosity of SLM frameworks may become critical under cyclic loading, which a static test cannot reveal. Fatigue testing of veneered restorations from independently produced batches, with a load range that allows fracture in both groups, is required before clinical recommendations can be made.
Supplementary Materials
The following supporting information can be downloaded at https://www.mdpi.com/article/10.3390/jfb17120622/s1, Supplementary Results S1 (pilot sample and prospective power assessment); Supplementary Methods S1–S6 (data provenance and terminal force-to-displacement arithmetic; run-out definitions and exact comparisons; Bayesian failure-probability sensitivity; prospective planning and numerical verification; elementary beam illustration; recovered load–displacement curves); Tables S1–S11; Figures S1–S7; Supplementary Data S1 (Excel workbook: a Summary sheet with the Fmax, displacement at Fmax, event, data source, apparent stiffness, and R2 for all ten specimens, and six testXpert load–displacement sheets, Melt1–Melt3 and Sint1–Sint3); executable Python analysis and verification code.
Author Contributions
Conceptualization, F.T., T.H., C.S. and M.R.; methodology, F.T., T.H., M.-L.N. and I.-A.T.; software, I.-A.T.; validation, C.S., M.-L.N., I.V. and M.R.; formal analysis, I.-A.T.; investigation, F.T., T.H., I.V., C.M. and D.S.; resources, C.S., M.-L.N., D.S. and M.R.; data curation, F.T., I.V., I.-A.T., C.M. and D.S.; writing—original draft preparation, F.T., T.H. and I.-A.T.; writing—review and editing, F.T., T.H., C.S., M.-L.N., I.V., I.-A.T., C.M., D.S. and M.R.; visualization, F.T., I.-A.T. and C.M.; supervision, C.S., M.-L.N. and M.R.; project administration, F.T., T.H. and C.S. All authors have read and agreed to the published version of the manuscript.
Funding
The Victor Babes University of Medicine and Pharmacy, Timisoara, supported publication costs. The findings, interpretations, and conclusions drawn in this study remain entirely independent of the financial support provided.
Institutional Review Board Statement
Not applicable.
Informed Consent Statement
Not applicable.
Data Availability Statement
The specimen-level endpoint data (force, fracture status, fracture site, and displacement for all ten frameworks), the six recovered load–displacement curves (MELT_1–MELT_3, SINT_1–SINT_3) as a raw data file, and the complete analysis and figure-generation code are included in the Supplementary Materials. The original testXpert curve files for MELT_4, MELT_5, SINT_4, and SINT_5 were not retained; their endpoint values are reported as recorded. The CAD design files are available from the corresponding author upon reasonable request.
Acknowledgments
ChatGPT (OpenAI, GPT-6) assisted with minor typographical corrections and formatting adjustments to the manuscript. All authors reviewed and approved the final version and take full responsibility for its content.
Conflicts of Interest
The authors declare no conflicts of interest.
Abbreviations
| CAD/CAM | Computer-aided design and computer-aided manufacturing |
| Co–Cr | Cobalt–chromium |
| FDP | Fixed dental prosthesis |
| SLM | Selective laser melting |
| CI | Confidence interval |
| CrI | Credible interval |
| QUIN | Quality Assessment Tool for Studies |
References
- Kassapidou, M.; Stenport, V.F.; Johansson, C.B.; Syverud, M.; Hammarström Johansson, P.; Börjesson, J.; Hjalmarsson, L. Cobalt chromium alloys in fixed prosthodontics: Investigations of mechanical properties and microstructure. J. Prosthet. Dent. 2023, 130, 255.e1–255.e10. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Schettini, A.; Pesun, I.J.; França, R. Assessment of mechanical properties and microstructure of Co-Cr dental alloys manufactured by casting, milling, and 3D printing. J. Prosthet. Dent. 2025, 133, 906.e1–906.e7. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Wu, M.; Dong, X.; Qu, Y.; Yan, J.; Li, N. Analysis of microstructure and fatigue of cast versus selective laser-melted dental Co-Cr alloy. J. Prosthet. Dent. 2022, 128, 218.e1–218.e7. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ko, K.H.; Kang, H.G.; Huh, Y.H.; Park, C.J.; Cho, L.R. Effects of heat treatment on the microstructure, residual stress, and mechanical properties of Co-Cr alloy fabricated by selective laser melting. J. Mech. Behav. Biomed. Mater. 2022, 126, 105051. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Konieczny, B.; Szczesio-Wlodarczyk, A.; Andrearczyk, A.; Januszewicz, B.; Lipa, S.; Zieliński, R.; Sokolowski, J. Enhancing the Mechanical Properties of Co-Cr Dental Alloys Fabricated by Laser Powder Bed Fusion: Evaluation of Quenching and Annealing as Heat Treatment Methods. Materials 2024, 17, 5313. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Kocak, E.F.; Ekren, O.; Ucar, Y. Effect of Internal Design Modification on the Mechanical Properties of Laser Sintered Cobalt-Chromium Multi-Unit Metal-Ceramic Frameworks. J. Prosthodont. 2022, 31, 766–770. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Cebi Gul, B.; Bahce, E.; Atmaca, A.; Kuzudisli, F.; Demirci, F. Effect of pontic volume on fracture resistance of three-unit metal-ceramic fixed dental prostheses: An in vitro and finite element analysis study. BMC Oral Health 2026, 26, 1933. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Hajaj, T.; Marian, D.; Zaharia, C.; Niculescu, S.T.; Negru, R.M.; Titihazan, F.; Rominu, M.; Sinescu, C.; Novac, A.C.; Dobrota, G.; et al. Fracture Resistance of CAD/CAM-Fabricated Zirconia and Lithium Disilicate Crowns with Different Margin Designs: Implications for Digital Dentistry. J. Funct. Biomater. 2025, 16, 205. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Andrei, A.D.; Constantin, C.A.; Tabitha, A.L.; Anca, J. Zirconia single retainer fixed dental prostheses for the posterior region—A novel preparation technique and literature review. Clin. Case Rep. 2024, 12, e9460. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Daou, E.E. Effect of lamination layer thickness and abutment preparation on the fit of Co-Cr multi-unit prostheses fabricated by additive manufacturing: An in vitro study. J. Prosthet. Dent. 2024, 131, 652–657. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Daou, E.E. Does the Build Orientation Parameter Affect the Fit of Fixed Partial Dentures Fabricated by Additive Manufacturing? Int. J. Prosthodont. 2024, 37, S41–S47. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Htat, H.L.; Limpuangthip, N.; Lee, J.H.; Lee, S.J. Printing orientation and heat treatment effects on fit and hardness of selective laser melting-manufactured cobalt-chromium crowns. J. Dent. 2025, 160, 105856. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Zhou, Y.; Liu, Z.; Du, H.; Jiang, J.; Li, J.; Ma, X.; Yi, Y. Effects of rapid infrared radiation heating on the warping deformation and mechanical properties of selective laser melted Co-Cr dental alloy. J. Prosthet. Dent. 2025, 133, 907.e1–907.e9. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Pekkan, G.; Degirmenci, K.; Tuna, S.H.; Hekimoğlu, C.; Saridag, S. Comparison of the overall fit of three-unit posterior fixed dental prostheses fabricated with laser sintering and conventional casting methods. Clin. Oral Investig. 2025, 29, 153. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Pekkan, G.; Gülgezen Aydın, H.; Tuna, S.H.; Hekimoğlu, C. Fit of three-unit anterior fixed dental prosthesis frameworks fabricated by different manufacturing techniques. BMC Oral Health 2026, 26, 1466. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Bani-Younes, S.A.; Al Fodeh, R.S.; Khasawneh, L.; Tabnjh, A. Clinical internal and marginal fit of metal-ceramic fixed dental prostheses fabricated with selective laser melting and 3D-printed pattern casting using cobalt-chromium metal alloy. J. Prosthodont. 2024, 33, 861–868. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Titihazan, F.; Hajaj, T.; Novac, A.C.; Pop, D.M.; Sinescu, C.; Negruțiu, M.L.; Romînu, M.; Zaharia, C. Dental Preparation Guides—From CAD to PRINT and CAM. Oral 2026, 6, 12. [Google Scholar] [CrossRef] [Scilit]
- Daou, E.E.; Baba, N.Z. The Effect of Firing Cycles on the Fit of Cobalt-Chromium Multiunit Prostheses Fabricated by Additive Manufacturing. J. Prosthodont. 2023, 32, 71–76. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Nikolopoulos, M.; Dimitriadis, K.; Yannikakis, S.; Galiatsatos, A.; Tsolka, P. Influence of repeated porcelain firing cycles on the microstructure, marginal and internal fit of implant-cemented Co-Cr frameworks. Eur. J. Oral Sci. 2025, 133, e70009. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Nikolopoulos, M.; Dimitriadis, K.; Yannikakis, S.; Sfikas, A.K.; Galiatsatos, A.; Tsolka, P. Implant-cemented Co-Cr frameworks produced by hard and soft milling: The impact of porcelain firing cycles on microstructure and fit accuracy. Eur. J. Oral Sci. 2025, 133, e70031. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Lee, S.Y. Using Bayesian statistics in confirmatory clinical trials in the regulatory setting: A tutorial review. BMC Med. Res. Methodol. 2024, 24, 110. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Al Jabbari, Y.S.; Dimitriadis, K.; Sufyan, A.; Zinelis, S. Bond strength and interfacial analysis of six CoCr alloys made by conventional casting and selective laser melting. J. Prosthodont. 2026, 35, 936–944. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Daou, E.E.; Özcan, M. Evaluation of ceramic adherence to cobalt-chromium alloys fabricated by different manufacturing techniques. J. Prosthet. Dent. 2022, 128, 1364.e1–1364.e8. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Zhou, Y.; Dong, X.; Li, N.; Yan, J. Effects of post-treatment on metal-ceramic bond properties of selective laser melted Co-Cr dental alloy. Part 1: Annealing temperature. J. Prosthet. Dent. 2023, 129, 657.e1–657.e9. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- AboElhassan, R.G.; Morsy, N. Effect of laser etching on surface characteristics and porcelain bond to soft milled and direct metal laser sintered cobalt chromium alloys. J. Prosthet. Dent. 2024, 132, 269.e1–269.e6. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Sezer, T.; Albayrak, H.; Ayata, M.; Yavuz, H.İ.; Yamanoğlu, R. Effect of hatch distance on porcelain bond strength of metal frameworks produced by selective laser melting. J. Prosthet. Dent. 2025, 134, 469.e1–469.e8. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Karahasan, B.; Dogan, D.O.; Babacan, N. Investigation of Metal-Ceramic Bond Strength in Co-Cr Alloys Produced by Selective Laser Melting at Different Laser Powers. Int. J. Prosthodont. 2026, 39, 509–515. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ayata, M.; Albayrak, H.; Sezer, T. Effect of femtosecond and nanosecond laser and tribochemical silica coating on metal-ceramic bond strength: An in vitro study. J. Prosthet. Dent. 2026, 135, e166–e175. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Biculescu, A.E.; Popescu, A.I.; Ionescu, T.P.; Ciorniciuc, I.A.M.; Referendaru, D.A.; Coman, C.; Constantinovici, A.; Chirsanov-Capanu, S.E.; Stoian-Albulescu, M.; Comaneanu, R.M. Evaluation of Flexural Resistance in Co-Cr Ceramic Systems: Conventional Casting Versus 3D Printing-A Pilot Study. Dent. J. 2025, 13, 583. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Mohebbi, H.; Habibzadeh, S.; Alikhasi, M.; Mosaddad, S.A.; Ghodsi, S. The effect of fabrication procedures and thermomechanical loading on the structural properties of screw-retained metal-ceramic implant restorations: An in vitro study. J. Prosthodont. 2024. Advance online publication. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Waldecker, M.; Custodio, L.J.; Ohlmann, B.; Rammelsberg, P.; Rues, S. Influence of artificial aging on the in vitro fracture load of tooth-to-implant-supported fixed partial dentures with different retainer designs. J. Prosthet. Dent. 2025, 134, 435.e1–435.e8. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Rubiños, N.M.; Mosaddad, S.A.; Díaz, P.; Revilla-León, M.; Gómez-Polo, M. Mechanical behavior of complete arch implant-supported prostheses with distal cantilevers fabricated from different digital material combinations. J. Prosthet. Dent. 2026, 136, 239–249. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Arteaga-Losada, L.; Laura-Fernadez, H.; Puerta-Dominguez, M.A.; Ascaso-Terren, C.; Vives, E.; Escuin-Henar, T.; Torné-Durán, S. In-vitro mechanical performance of three CAD-CAM bar designs for implant-supported metal-resin hybrid prostheses: A preliminary pilot study. J. Oral Biol. Craniofac. Res. 2026, 16, 101407. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Audi, L.; Almustafa, A. Bending strength and hardness comparison of titanium and cobalt-chromium alloys for dentures made by selective laser melting. Sci. Rep. 2025, 15, 36463. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Titihazan, F.; Veja, I.; Zaharia, C.; Hajaj, T.; Sinescu, C.; Constantin, G.D.; Rominu, M. Comparative Evaluation of Color Stability and Fracture Resistance of CAD/CAM and Chairside Provisional Restorations: An In Vitro Study. J. Funct. Biomater. 2025, 16, 426. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Rotar, R.; Cândea, A.; Măroiu, A.; Faur, A.B.; Cuzic, C.; Rotar, R.E.; Jivănescu, A. Impact of Various Mouthwashes on the Color Stability of Hybrid Ceramic and Reinforced Composite CAD/CAM Restorative Materials: An In Vitro Study. Materials 2026, 19, 758. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Gan, N.; Yao, M.; Ruan, Y.; Wang, C.; Xiong, Y.; Jiao, T. Adaptation of maxillary removable partial denture frameworks fabricated with a direct digital workflow: A randomized crossover clinical trial. J. Dent. 2025, 154, 105588. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Husseiny, E.; Youssef, R.A.F.; Eltamaly, N.; Rokaya, D.; Mohamed, S.Z. Comparison of retentive force and deformation of selective laser melting and conventional cobalt-chromium clasps of removable partial denture. BMC Oral Health 2025, 26, 361. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ma, K.; Chen, H.; Shen, Y.; Guo, Y.; Li, W.; Wang, Y.; Zhang, Y.; Sun, Y. Feasibility study and material selection for powder-bed fusion process in printing of denture clasps. Comput. Biol. Med. 2023, 157, 106772. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Kato, Y.; Tasaka, A.; Okano, H.; Uzawa, S.; Yamashita, S. Accuracy and mechanical properties of denture clasps fabricated utilizing pre-sintered Co-Cr alloy discs. J. Prosthodont. Res. 2025, 69, 578–587. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Albayrak, H.; Ayata, M.; Demirel, B. Recycling selective laser melting alloy powder on cobalt chromium-to-ceramic bond strength. J. Prosthet. Dent. 2023, 130, 786.e1–786.e7. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Guluzade, I.; Albayrak, H.; Yamanoğlu, R.; İsmail Yavuz, H.; Ayata, M. Effect of Recycling Cobalt-Chromium Alloy Powder on Metal-Ceramic Bond Strength and Microstructure. Int. J. Prosthodont. 2026, 39, 251–259. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Berk, T.Y.; Çelik Öge, S.; Uçar, Y.; Ekren, O. Effect of reusing cobalt-chromium alloy powders in direct metal laser sintering on powder characteristics and metal-ceramic bond strength. J. Mech. Behav. Biomed. Mater. 2026, 182, 107559. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Xing, X.; Hu, Q.; Liu, Y.; Wang, Y.; Cheng, H. Comparative analysis of the surface properties and corrosion resistance of Co-Cr dental alloys fabricated by different methods. J. Prosthet. Dent. 2022, 127, 497.e1–497.e11. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Al Jabbari, Y.S.; Karavoltsos, S.; Kokkinos, C.; Polychronis, G.; Economou, A.; Zinelis, S. Electrochemical characterization of three types of Co-Cr based alloys manufactured by casting and selective laser melting according to ISO 10271. Dent. Mater. 2022, 38, 1162–1172. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Şahin, M.; Ünalan, F.; Mutlu, İ. Corrosion, ion release, and surface hardness of Ti-6Al-4V and cobalt-chromium alloys produced by CAD-CAM milling and laser sintering. J. Prosthet. Dent. 2022, 128, 529.e1–529.e10. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Sakurai, N.; Sawada, T.; Kuwajima, Y.; Yamanaka, K.; Nomura, N.; Kasahara, M.; Chiba, A.; Satoh, K.; Takemoto, S. Metallic Ion Release Behaviors from Cobalt-Chromium Alloys Fabricated by Additive Manufacturing with Mechanical Grinding in an Acidic Saline Solution. Materials 2025, 18, 432. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Atapour, M.; Standish, T.E.; Henderson, J.D.; Wei, Z.; Dehnavi, V.; Hedberg, Y.S. Influence of Proteins and Building Direction on the Corrosion and Tribocorrosion of CoCrMo Fabricated by Laser Powder Bed Fusion. ACS Biomater. Sci. Eng. 2024, 10, 2880–2893. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Reclaru, L.; Buciu, G.; Petrescu, S.M.; Gheorghe, R.I.; Grecu, D.F.; Grecu, A.F. Corrosion Behavior and Ion Release of Co-Cr Dental Alloys Fabricated by Casting, CAD/CAM, SLM and DMLS: Influence of Manufacturing Route and Microstructure. Bioengineering 2026, 13, 406. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Gan, J.; Zhang, H.; Sun, J.; Zhu, C.; Jiao, T. Effects of various polishing processes on surface morphology, corrosion resistance, and RPD framework adaptation of SLM-printed dental Co-Cr alloys. J. Prosthodont. 2026, 35, 1358–1368. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Li, X.; Wang, Q.; Guan, Y. Laser polishing for integrated enhancement of thin-walled LPBFed dental Co-Cr-Mo alloy frameworks. J. Mech. Behav. Biomed. Mater. 2026, 180, 107463. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Sheth, V.H.; Shah, N.P.; Jain, R.; Bhanushali, N.; Bhatnagar, V. Development and validation of a risk-of-bias tool for assessing in vitro studies conducted in dentistry: The QUIN. J. Prosthet. Dent. 2024, 131, 1038–1042. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Øilo, M.; Nesse, H.; Lundberg, O.J.; Gjerdet, N.R. Mechanical properties of cobalt-chromium 3-unit fixed dental prostheses fabricated by casting, milling, and additive manufacturing. J. Prosthet. Dent. 2018, 120, 156.e1–156.e7. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Klimek, L.; Bułhak, B.; Śmielak, B. A Comparison of the Structure and Selected Mechanical Properties of Cr/Co Alloys Obtained by Casting and Selective Laser Melting. J. Funct. Biomater. 2024, 15, 61. [Google Scholar] [CrossRef] [Scilit] [PubMed]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.