Skip to Content
  • Article
  • Open Access

25 November 2026

22 Pages

Mechanical Debonding Resistance of Lithium Disilicate and Lithium–Silicate-Modified Zirconia Veneers on Crenelated Tooth Preparations

,
,
,
and
1
Department of Prosthodontics, University of Medicine and Pharmacy “Victor Babes”, B-dul Revolutiei 1989, No. 9, 300580 Timisoara, Romania
2
TADERP Research Center, Department of Prosthodontics, University of Medicine and Pharmacy “Victor Babes”, B-dul Revolutiei 1989, No. 9, 300580 Timisoara, Romania
*
Authors to whom correspondence should be addressed.
J. Funct. Biomater.2026, 17(12), 604;https://doi.org/10.3390/jfb17120604 
(registering DOI)
This article belongs to the Special Issue New Materials in Prosthodontics and Implantology

Abstract

This in vitro study compared maximum peel stress (σp,max) between two ceramic veneer protocols on crenelated anterior tooth preparations and examined how contour and adhesive-layer thickness affected elastic stress transfer. Sixty veneer–tooth assemblies were tested, with five specimens per protocol in each of six anterior tooth categories. Lithium disilicate (LDS) and Biomic LiSi Connect-modified zirconia (Zr–LiSi) veneers received material-specific surface conditioning and cementation. A transverse load was applied at the palatal or lingual aspect of the incisal margin, perpendicular to the tooth’s long axis. The analysis used the calculated σp,max values available in the study dataset. The original failure loads and force-to-stress conversion could not be verified. The protocol comparison was adjusted for tooth category using ordinary least squares with HC3-robust standard errors. Beam-on-elastic-foundation simulations compared straight and single-cycle sinusoidal contours at an equal projected bonded area under a common reference load of 50 N. The mean σp,max was 19.49 ± 2.17 MPa for LDS and 18.23 ± 1.94 MPa for Zr–LiSi. The adjusted difference was 1.26 MPa (95% CI, 0.55–1.97 MPa, p = 0.00085). Two LDS failures involved dental tissue. After Zr–LiSi detachment, cement generally remained on the tooth. Simulated tensile stress peaked near the loaded end. The reference sinusoidal contour reduced category-mean peak stress by 1.36–2.20% for LDS and 1.55–2.67% for Zr–LiSi. For straight contours, increasing the adhesive-layer thickness from 0.5 to 2.0 times its baseline value reduced peak stress by 30.36–31.10%. The reported maximum peel stress values were higher for the LDS protocol under the tested conditions. The simulated contour effect was small and configuration-dependent. The clinical relevance of the difference between protocols and the effect of crenelation on experimental failure resistance remain uncertain.

1. Introduction

Adhesively bonded ceramic veneers provide a conservative approach to anterior dental rehabilitation, drawing on advances in enamel etching and porcelain conditioning [1,2,3]. Long-term clinical studies have reported favorable outcomes, although debonding and fracture remain relevant complications [4,5,6]. The mechanical response of a veneer depends on the ceramic, the amount of tooth tissue removed, and the way the restoration is bonded to the prepared substrate. Laboratory comparisons have shown that restoration thickness affects load-to-failure behavior [7]. Preparation depth can also influence adhesion and clinical outcomes by changing the extent of dentine exposure [8,9].
Lithium disilicate (LDS) combines favorable optical properties with a glass-containing microstructure. Hydrofluoric acid (HF) etching creates micromechanical retention at the ceramic surface, and subsequent salinization promotes coupling between the conditioned ceramic and the resin cement [10,11]. Zirconia offers mechanical strength and masking potential, with properties that vary according to composition and translucency. Its polycrystalline structure lacks the etchable glass phase found in LDS [12]. Surface-conditioning strategies for zirconia therefore include airborne-particle abrasion and treatments containing phosphate monomers [13,14]. In both materials, the performance of the bonded assembly also depends on the resin cement, adhesive application, and curing sequence.
Silica-based coatings offer an additional route for resin bonding to zirconia [15]. Biomic LiSi Connect forms a lithium silicate surface layer after thermal processing, allowing the coated intaglio surface to be etched and salinized [16]. The silane can couple the conditioned silica-containing surface to the resin matrix. The coating also creates a layered assembly in which adhesion may depend on the integrity of both the zirconia–coating and coating–cement interfaces. Studies of ceramic interlayers in bilayered zirconia systems provide context for the behavior of such interfaces [17]. The resin-cemented veneer configuration warrants separate assessment because the coating, luting material and tooth substrate can each influence the failure path.
A retrospective clinical comparison reported debonding among LiSi-modified zirconia restorations in a series that also included LDS restorations [18]. Differences in clinical indications and cementation procedures limited attribution of those observations to ceramic composition alone. Laboratory evidence has likewise documented cohesive cement failure in bonded restorative assemblies [19]. These observations motivated a comparison of two complete restorative protocols. In the present study, the LDS and Biomic LiSi Connect-modified zirconia (Zr–LiSi) systems differed in ceramic composition, surface conditioning, resin cement and adhesive-curing sequence. The experimental comparison therefore assessed the combined performance of those protocol components.
The crenelated preparation incorporates sinusoidal proximal margins [20]. Earlier mechanical testing compared conventional and crenelated preparations restored with LDS veneers and reported higher mean detachment forces and calculated maximum peel stresses for the crenelated design [21]. That work provided the rationale for the present study. After examining the effect of preparation geometry within one restorative system, we kept the crenelated preparation constant and compared two restorative protocols. This design addressed how the protocols performed on the same preparation. The straight contour was included as a computational comparator at equal projected bonded area, allowing the effect of the reference sinusoidal contour on simulated stress transfer to be examined under controlled conditions.
A transverse load applied at the incisal margin bends the veneer and can generate local tensile stress normal to the bonded interface. This opening component is termed peel stress. Shear stress acts tangentially along the interface. For example, a published shear bond strength test of LiSi-coated zirconia used a blade to load a resin cylinder bonded to a zirconia block [16]. That test reported a nominal stress for the specimen and loading configuration used. In a veneer–tooth assembly, the failure load in N describes the resistance of the assembled specimen in the test fixture. The calculated maximum peel stress (σp,max) in MPa addresses a complementary mechanical question by estimating the local tensile stress associated with interface opening [21]. This estimate depends on the geometry, elastic properties and force-to-stress formulation used. In the present study, the primary comparison used the specimen-level σp,max values available in the study dataset.
The primary objective was to compare the reported σp,max values for the LDS and Zr–LiSi restorative protocols on crenelated anterior tooth preparations after adjustment for tooth category. The null hypothesis (H0) was that the adjusted mean σp,max would be equal between the two protocols. The alternative hypothesis (H1) was that the adjusted means would differ. The secondary objective was to examine how contour and adhesive-layer thickness influenced elastic stress transfer under a common prescribed load. Finite-length numerical simulations and a closed-form long-strip solution were used within the same beam-on-elastic-foundation framework, with the analytical solution serving as a reference for interpreting the numerical results.

2. Materials and Methods

2.1. Study Design and Specimens

This in vitro study compared two restorative protocols on crenelated anterior tooth preparations. One protocol used lithium disilicate veneers (LDS), and the other used zirconia veneers surface-modified with Biomic LiSi Connect (Aidite, Qinhuangdao, China; Zr–LiSi). The protocols comprised the ceramic, surface conditioning, resin cement and adhesive-curing sequence. The study included 60 veneer–tooth assemblies, with 30 specimens per protocol. Each assembly constituted one experimental unit.
Each group included five maxillary central incisors, five maxillary lateral incisors, five maxillary canines, five mandibular central incisors, five mandibular lateral incisors and five mandibular canines. Specimens were allocated without randomization, with equal numbers from each tooth category in the two groups. Tooth category was included in the primary statistical analysis.
The sample size reflected the number of eligible extracted teeth available for testing. No a priori sample size or power calculation was performed. Donor identifiers were unavailable in the analysis dataset, so it was not possible to establish whether multiple specimens came from the same donor.
Extracted human teeth served as bonding substrates. Specimen selection and handling followed the approach described by Măroiu et al. [21]. Teeth extracted for periodontal reasons were eligible if they were free of caries and restorations. Calculus, plaque and residual periodontal tissue were removed, and the teeth were visually inspected for defects before inclusion.
During specimen preparation, the teeth were maintained in sterile 0.9% sodium chloride solution at 25 °C to prevent dehydration, following the storage conditions of the earlier protocol [21]. The interval from extraction to preparation could not be established from the available documentation.
The study was conducted in accordance with the Declaration of Helsinki and was approved by the Ethics Committee of the Victor Babeș University of Medicine and Pharmacy, Timișoara, Romania (approval no. 38, date 3 April 2026). Written informed consent was obtained from all patients whose extracted teeth were included in the study.
All experimental specimens received crenelated preparations. The complementary numerical analysis compared straight and reference sinusoidal contours under a common prescribed load to examine the effect of contour on elastic stress transfer.

2.2. Tooth Preparation

A single operator (A. C. Măroiu) performed all tooth preparations. Both restorative groups received the crenelated preparation described in Romanian Patent RO 131840 B1 [20], following the previously published technique [21]. The sinusoidal proximal margins were positioned facial to the interdental contact areas. The target reduction was 0.5–0.8 mm facially and 1 mm incisally.
The design incorporated two or three proximal undulations, depending on tooth morphology. The target height was 2–2.5 mm for lateral incisors and mandibular central incisors and 2.5–3 mm for maxillary central incisors and canines. The target depth decreased from 0.6–0.8 mm in the cervical third to 0.4–0.6 mm in the middle third and 0.3–0.4 mm in the incisal third. An incisal butt-joint finish line was combined with a cervical and proximal chamfer. Preparation began with incisal reduction, followed by facial reduction and proximal contouring. The surfaces were then finished and polished.
Preparations were performed under 4× magnification (Univet, Rezzato, Italy), with the aim of preserving enamel [21]. Instruments included coarse- and fine-grit cylindrical diamond burs of 0.8 and 1 mm diameter (Komet Dental, Lemgo, Germany), rounded-tip Arkansas stones and superfine polishing disks. The available documentation did not specify a formal operator calibration procedure, an independent method for verifying reduction depth on individual specimens, the irrigation protocol or whether burs were replaced during preparation.
Representative photographs of a crenelated tooth preparation and the corresponding lithium disilicate veneer are presented in Figure 1.
Figure 1. Representative stages of the crenelated veneer restoration: (a) tooth preparation showing the sinusoidal proximal contour; (b) lithium disilicate veneer before cementation; and (c) veneer cemented to the prepared tooth.

2.3. Digital Design and Veneer Fabrication

The prepared teeth were digitized using a Medit i700 intraoral scanner (Medit, Seoul, Republic of Korea). Veneers were designed in exocad 3.2 Elefsina (exocad, Darmstadt, Germany), with the restoration margins following the cervical chamfer, sinusoidal proximal contours, and incisal butt-joint of each preparation.
The specimen worksheets listed nominal CAD cement spaces of 11–20 μm for LDS and 12–20 μm for Zr–LiSi. The recorded veneer thicknesses ranged from 0.24 to 0.52 mm for LDS and from 0.25 to 0.45 mm for Zr–LiSi. The nominal CAD cement space was recorded separately from the specimen geometry and adhesive-layer thickness used in the mechanical model.
Thirty veneers were milled from IPS e.max CAD lithium disilicate blocks (Ivoclar, Schaan, Liechtenstein), and 30 were milled from zirconia supplied by Aidite (Qinhuangdao, China). The commercial designation, yttria content and translucency grade of the zirconia blocks could not be verified from the available study records.
The LDS veneers were crystallized in a Programat P3010 furnace (Ivoclar, Schaan, Liechtenstein). Dental laboratory technicians sintered the zirconia veneers in an LHT 01/17 D furnace (Nabertherm, Lilienthal, Germany). The Programat P3010 was also used to fire the Biomic LiSi Connect coating. The zirconia intaglio coating and conditioning sequence is described in Section 2.4.
The fabricated veneers were visually inspected for defects before cementation, and their marginal and internal fit was checked on the corresponding preparations. The available study records did not specify the fit-checking procedure or provide quantitative measurements of marginal or internal gaps.

2.4. Surface Treatment and Adhesive Cementation

The two restorative groups received material-specific surface conditioning and cementation according to the previously reported adhesive protocol [18]. The intaglio surfaces of the lithium disilicate (LDS) veneers were etched with 5% hydrofluoric acid (HF) for 20 s, thoroughly rinsed and ultrasonically cleaned. Monobond Plus (Ivoclar, Schaan, Liechtenstein) was then applied for 60 s [10,11,18].
Biomic LiSi Connect (Aidite, Qinhuangdao, China; Zr–LiSi) was manually applied as a thin layer to the sintered zirconia intaglio surfaces and fired in a Programat P3010 furnace (Ivoclar, Schaan, Liechtenstein). The exact firing schedule could not be verified from the available study records. Following firing, the coated surfaces were air-abraded with 50 μm aluminum oxide for approximately 1 s at a working distance of 3–5 cm. The fired, silica-containing coating was then etched with 5% HF for 20 s, rinsed, ultrasonically cleaned and treated with Monobond Plus for 60 s. The brief abrasion and HF etching steps followed the previously reported protocol for LiSi-coated zirconia [18]. HF conditioning was directed at the etchable LiSi layer [16,18]. Figure 2 illustrates the conditioning sequence. Post-etch surface topography was not examined in either group.
Figure 2. Conditioning of Biomic LiSi Connect-coated zirconia intaglio. (a) HF application to fired LiSi layer. (b) Rinsing after etching. (c) Appearance after application of Monobond Plus.
The prepared tooth surfaces were etched with 37% phosphoric acid for 20 s, rinsed and gently air-dried. Adhese Universal (Ivoclar, Schaan, Liechtenstein) was then applied. In the LDS group, the adhesive was air-thinned and left uncured before veneer placement. In the Zr–LiSi group, the adhesive was light-cured for 20 s before veneer placement.
LDS veneers were cemented with Variolink Esthetic LC (Ivoclar, Schaan, Liechtenstein), and Zr–LiSi veneers were cemented with Variolink Esthetic DC (Ivoclar, Schaan, Liechtenstein). The cement and adhesive-curing sequence were retained as components of each restorative protocol [18]. The dual-cure cement used for Zr–LiSi provided a chemical curing component where reduced light transmission through the zirconia restoration could limit light activation [18].
One operator (A. C. Măroiu) manually seated all veneers. Seating force was neither controlled with a calibrated loading device nor measured. After seating, the cement was tack-cured for approximately 2 s to facilitate excess removal. Final light curing was performed for 60 s from the facial aspect and 60 s from the palatal or lingual aspect. The curing-light model, irradiance and tip-to-surface distance could not be verified from the available records.
After cementation, the assemblies in both groups were stored in sterile 0.9% sodium chloride solution at 25 °C until mechanical testing. These conditions prevented dehydration and followed the previously reported debonding protocol [21]. Both groups followed the same post-cementation schedule. The exact interval between cementation and testing could not be verified. No thermocycling was performed.

2.5. Mechanical Testing

Mechanical testing was performed by a single operator (A. C. Măroiu) using the loading configuration previously described by Măroiu et al. [21]. Each tooth was embedded in epoxy resin in a supporting mold, and the assembly was secured in a precision vice. The load was applied centrally at the palatal or lingual aspect of the incisal margin, perpendicular to the long axis of the tooth. Figure 3 shows representative specimen mounting and loading arrangements.
Figure 3. The representative mechanical testing configuration: (a) a tooth mounted in an epoxy-resin supporting mold; and (b) a specimen positioned in the universal testing machine, with loading applied centrally at the palatal or lingual aspect of the incisal margin.
The assemblies were loaded using a Zwick/Roell Z005 universal testing machine (ZwickRoell, Ulm, Germany) at a crosshead speed of 1 mm/min and a preload of 5 N. The instrument outputs were force (N) and displacement. The protocol used complete veneer detachment as the test stopping point. Tooth or ceramic fractures were noted when documented. The original force–displacement traces were unavailable for verification. As a result, the force event used to calculate maximum peel stress could not be established, including in cases where fracture preceded complete detachment.
The primary analysis used the 60 specimen-level maximum peel stress values (σp,max, MPa) already present in the source dataset. A second series of stress values in the dataset was used in a sensitivity analysis. The original force inputs and the procedure used to calculate either stress series could not be verified against instrument records.
For the complementary mechanical analysis, model-equivalent forces were subsequently reconstructed by inverse calculation from each of the two supplied stress series. The reconstruction used the specimen geometries and assigned material properties described in Section 2.7.4. These forces were reported as model-derived estimates. The original measured failure loads were unavailable for reporting.

2.6. Statistical Analysis

The primary outcome was the specimen-level maximum peel stress (σp,max, MPa) reported in the source dataset. Descriptive statistics included the number of specimens, mean, standard deviation, median and range. Individual values were plotted by restorative protocol and tooth category to show their distributions.
The primary comparison used an ordinary least-squares linear model with restorative protocol and tooth category as categorical fixed effects. The additive model estimated a common difference between protocols across the six tooth categories, without a protocol-by-category interaction. The primary effect estimate was the adjusted mean difference (LDS minus Zr–LiSi), reported with its 95% confidence interval and two-sided p value. Inference used HC3 heteroscedasticity-robust standard errors and the t distribution with the model’s residual degrees of freedom. Category-specific means were interpreted descriptively. The significance threshold for the primary comparison was p < 0.05.
The primary analysis included all 60 veneer–tooth assemblies, including the two LDS specimens whose failures involved dental tissue. The available photographs could not be linked to the corresponding specimen IDs in the dataset. To assess sensitivity to excluding two LDS observations, the same adjusted model was refitted for each of the 435 possible pairs of LDS specimens, retaining all 30 Zr–LiSi specimens in every fit. The range of adjusted differences and confidence interval bounds was summarized across these fits. A separate sensitivity analysis refitted the model using the second stress series available in the dataset.
Statistical significance was set at p < 0.05. Statistical analyses were conducted using Python 3.14 and JASP version 0.96.0.0 (JASP Team, Amsterdam, The Netherlands).

2.7. Complementary Mechanical Modeling

A browser-based application was developed to investigate elastic stress transfer in LDS and Zr–LiSi veneer systems using the specimen-level geometric inputs in the study dataset. Six anterior tooth categories were analyzed separately, with five specimens per restorative system in each category. A straight contour and a reference sinusoidal contour were compared under identical loading conditions. All experimental preparations were crenelated. The straight contour served as a computational comparator. The interactive application is provided as Supplementary File S1.
The model used the widths and the ceramic, and adhesive-layer thicknesses listed in the specimen dataset. Common-load simulations were performed independently of the reported σp,max values. Inverse calculations of model-equivalent forces were conducted separately. The closed-form long-strip solution and the finite-element formulations were analytical and numerical treatments within the same beam-on-elastic-foundation framework.

2.7.1. Model Formulation and Reference Parameters

The veneer was represented as a beam supported by a continuous elastic foundation. Both Euler–Bernoulli and Timoshenko formulations were implemented, with the latter accounting for transverse shear deformation. The ceramic and interfacial layers were assumed to behave linearly elastically, with perfect adhesion between components. The model did not include interfacial damage, progressive debonding, ceramic fracture, or time-dependent material behavior.
The model inputs comprised veneer width, ceramic thickness, adhesive-layer thickness, and the elastic moduli of the ceramic and adhesive. Geometric inputs were obtained from the authors’ experimental dataset. For calculations using cervical and incisal dimensions, mean width and adhesive-layer thickness were obtained as the arithmetic means of the corresponding values. Material properties and reference model lengths were assigned separately from the experimental geometric inputs. Nominal CAD cement space was distinguished from adhesive-layer thickness.
The assigned elastic modulus for fully crystallized LDS was 95,000 MPa, based on the manufacturer’s technical documentation [22]. Zirconia was assigned 210,000 MPa, the post-sintering modulus reported for a historical Aidite product [23]. The exact zirconia block used in this study could not be identified, so the value was used as a modeling reference. Both restorative systems were assigned a common effective adhesive-layer modulus of 5000 MPa. This assumption represented the adhesive foundation in the model. The moduli of the individual luting cements were not measured. For the Timoshenko formulation, Poisson’s ratios of 0.23 and 0.30 were assigned to LDS and zirconia, respectively. The shear modulus was calculated as G = E/2(1 + ν), with a shear correction factor of 5/6.
The normal foundation stiffness per unit area was defined as follows:
k n = E a h a
where Ea and ha denote the adhesive elastic modulus and thickness, respectively. This expression represents an equivalent homogeneous adhesive layer.
An optional multilayer configuration represented the adhesive and LiSi coating as elastic layers acting in series:
k n = h a E a + h LiSi E LiSi − 1
where ELiSi and hLiSi denote the coating modulus and thickness. The coating contribution to ceramic bending stiffness was neglected. The single-layer and multilayer configurations were treated separately.
The baseline calculations used the single-layer formulation and a rigid substrate. In the optional coating configuration, a thickness of 0.01 mm and an elastic modulus of 100,000 MPa were assigned as modeling assumptions. The nominal thickness corresponded to the upper end of the 6–10 μm range reported by the manufacturer [24]. Coating thickness was not measured in the specimens, and the assigned coating modulus was not experimentally verified for Biomic LiSi Connect. The baseline simulations did not include the optional coating layer. Additional optional settings allowed for exploration of local substrate compliance and idealized lateral confinement of the adhesive.
Reference model lengths were 10.5, 9.0, and 10.0 mm for maxillary central incisors, lateral incisors, and canines, respectively, and 8.5, 9.0, and 10.0 mm for the corresponding mandibular categories. Published measurements of anterior crown dimensions informed the anatomical scale [25]. The assigned lengths were category-level modeling presets. Individual veneer lengths were not measured. Specimen-level stress series and geometric inputs are provided in Table S1A,B, while material inputs, analytical calculations, and numerical predictions are provided in Table S1C,D.

2.7.2. Straight and Sinusoidal Contour Comparison

For the straight configuration, beam width remained constant. The sinusoidal configuration was defined by the following:
w x = w 0 + 2 A sin 2 π x L
Here, A denotes the amplitude assigned to each lateral boundary, n the number of complete waves, and L the model length. The reference sinusoidal configuration used one complete wave, A = 0.3 mm, and phase 0°. The amplitude of the total width variation was therefore 0.6 mm.
For an integer number of complete waves, both contours had the same projected area, w0L. The sinusoidal configuration represented an idealized lateral width modulation of the beam. The model omitted the three-dimensional proximal geometry, the additional adhesive area along the proximal walls and any mechanical interdigitation.
A transverse force of 50 N was applied at (x = 0), without an applied end moment. Both ends were kinematically free, with support provided by the elastic foundation. The same applied force was maintained across restorative systems and contours. The 50 N value provided a common numerical reference for comparing intact assemblies. In the linear–elastic model, the predicted stresses scaled with the applied force, so the percentage difference between the two contours was independent of the chosen reference load. The 50 N load was not used as a clinical or experimental failure threshold.
The Timoshenko formulation used two-node elements with linear interpolation of displacement and rotation. Four-point Gaussian integration was applied to the bending and foundation terms, while one-point reduced integration was used for the shear term to limit shear locking. The Euler–Bernoulli formulation used cubic Hermite interpolation and four-point Gaussian integration. The assembled symmetric positive-definite systems were solved using banded Cholesky factorization.
Each of the 60 specimen configurations was analyzed with both contours, producing 120 solutions for each selected beam theory. Results were summarized within the 12 restorative system–tooth category combinations. Group peak stresses were calculated as the mean of the five specimen-specific maxima. Stress distribution curves represented the mean response at corresponding normalized positions, x/L. The maximum of the mean curve was distinguished from the mean of the individual maxima. Figure 4 illustrates the straight and single-cycle sinusoidal contours with equal projected bonded areas.
Figure 4. Representative straight and reference sinusoidal contours with equal projected bonded areas of 85 mm2. The numerical simulations used specimen-specific geometric inputs.

2.7.3. Sensitivity Analysis and Comparison with Experimental Values

The application provided sensitivity analyses for adhesive-layer thickness, contour phase, and the optional mechanical assumptions. Adhesive thickness was varied from 0.5 to 2 times its initial value while maintaining the applied force, ceramic geometry, and elastic properties. The application also allowed for comparison of contour phases of 0°, 90°, 180°, and 270°, enabling us to examine how the orientation of the sinusoidal contour relative to the loaded end affected the response.
Additional sensitivity analyses were performed for the 60 finite-length specimen models. Reference beam lengths were set to 80% and 120% of their baseline values, and the effective adhesive modulus was set to 50% and 200% of its baseline value. Each parameter was varied separately with the other inputs held fixed. For Zr–LiSi, the optional coating was also evaluated at thicknesses of 10 and 50 μm using the assigned coating modulus of 100,000 MPa. These scenarios assessed how the model responded to its assumed inputs.
A controlled-geometry mode was implemented to distinguish assigned material properties from geometric differences between groups. Within each tooth category, both restorative systems were assigned common values of width, adhesive-layer thickness, and ceramic thickness, calculated by averaging the corresponding inputs across all ten specimens.
The baseline discretization comprised 192 elements per beam. Numerical convergence was assessed by comparison with 384-element solutions. A 96-element discretization was also available for comparison. Implementation checks included force and moment equilibrium, algebraic residuals, linear scaling with applied force, zero-load response, equivalence of the contours at zero amplitude, symmetry upon reversal of the loaded end for a straight beam, and preservation of projected area.
The constant-width Euler–Bernoulli solution was additionally checked against the analytical long-strip formulation previously applied to ceramic veneers [21]:
β = k n w 4 E v I 1 / 4
I = w t 3 12
σ model , max = 2 β F w
where Ev denotes the ceramic elastic modulus and β is the stress transfer parameter. This analytical expression assumes a sufficiently long bonded strip loaded by an end force without an applied end moment. It served as a reference for the constant-width Euler–Bernoulli solution. The Timoshenko formulation additionally accounted for transverse shear deformation.
These checks assessed numerical implementation and solution consistency. The available measurements did not permit independent experimental validation of the predicted stress distributions or calibration of a failure criterion.

2.7.4. Inverse Calculation of Model-Equivalent Forces

Model-equivalent forces were reconstructed separately from each of the two specimen-level stress series already present in the source dataset, using the inverse analytical expression
F eq = σ p , max w 2 β .
The calculations used the geometric inputs entered for each specimen and the assigned material properties. The inverse calculation estimated the force that would produce a given input stress under the assumptions of the long-strip model. The fields reserved for machine-measured maximum force were empty for all 60 specimens in the available data.
The source σp,max series was used in the primary statistical analysis. The second stress series was retained for sensitivity analysis. The original force inputs and the calculation used to produce either stress series could not be verified. Common-load simulations did not use either stress series to calibrate the applied force or model parameters. Reapplying the forward expression to an inverse force reproduces the input stress by construction. This procedure checks algebraic consistency.

3. Results

3.1. Experimental Comparison Between Restorative Systems

All 60 observations in the final dataset were included, with 30 specimens per restorative system and 5 specimens per tooth category within each system. The mean σp,max was 19.49 ± 2.17 MPa for LDS and 18.23 ± 1.94 MPa for Zr–LiSi. The corresponding medians were 19.57 and 18.09 MPa, with ranges of 15.80–23.80 and 14.45–22.15 MPa, respectively. Individual observations and category means are shown in Figure 5.
Figure 5. Calculated maximum peel stress endpoint (MPa) from the mechanical-test dataset for six anterior tooth categories: (a) maxillary central incisor; (b) maxillary lateral incisor; (c) maxillary canine; (d) mandibular central incisor; (e) mandibular lateral incisor; and (f) mandibular canine. Circles show individual specimens (n = 5 per protocol and category). Squares and error bars show the mean and ±1 standard deviation. Horizontal offsets separate the observations visually.
The mean σp,max was higher for LDS in all six tooth categories (Table 1). Maxillary canines exhibited the highest means in both systems, whereas mandibular lateral incisors exhibited the lowest.
Table 1. Calculated maximum peel stress from the mechanical-test dataset by restorative protocol and tooth category.
The adjusted mean σp,max was 1.26 MPa higher for LDS than for Zr–LiSi (95% CI, 0.55–1.97 MPa, two-sided p = 0.00085 with HC3-robust standard errors). The primary null hypothesis of equal adjusted means was rejected. The estimate describes the difference in the reported σp,max between the two complete restorative protocols.
The available dataset contained no machine-recorded failure loads in N. Both populated force columns contained model-equivalent estimates reconstructed by inversion from the two-stress series.
The two LDS specimens with documented dental tissue involvement could not be linked to specimen IDs. In the sensitivity analysis, the adjusted model was refitted for each of the 435 possible exclusions of two LDS specimens, retaining 28 LDS and 30 Zr–LiSi specimens in each fit. The adjusted LDS minus Zr–LiSi difference ranged from 1.09 to 1.41 MPa, and all 435 individual 95% confidence intervals excluded zero. The lowest lower bound was 0.40 MPa, and the highest upper bound was 2.11 MPa. When the model was fitted to the second stress series, the adjusted difference was 1.22 MPa (95% CI, 0.50–1.95 MPa, two-sided p = 0.00128).

3.2. Numerical Stress Transfer Under Common Loading

Under an applied load of 50 N, tensile foundation stress was greatest at the loaded end and decreased rapidly with distance, followed by a smaller compressive region (Figure 6). The simulations produced distinct responses across the six tooth categories. Table 2 reports the mean of the five specimen-level peak stresses for each category and restorative system.
Figure 6. Mean foundation normal-stress profiles for straight and single-cycle sinusoidal contours under a common load of 50 N: (a) maxillary central incisor; (b) maxillary lateral incisor; (c) maxillary canine; (d) mandibular central incisor; (e) mandibular lateral incisor; and (f) mandibular canine. Each curve averages five specimen-level profiles. Positive and negative values indicate tensile and compressive foundation stresses, respectively. Distance is normalized by beam length, with x/L = 0 at the loaded end. These curves describe a loading scenario and do not represent experimental stress distributions at failure.
Table 2. Predicted peak tensile foundation stress under a common load of 50 N.
The reference sinusoidal contour reduced peak stress by 1.36–2.20% for LDS and 1.55–2.67% for Zr–LiSi relative to the corresponding straight contour (Figure 7). The ordering of the restorative systems varied by tooth category. Zr–LiSi produced higher predicted peak stresses for maxillary central incisors, whereas LDS produced higher values for canines and mandibular incisors. Predictions for maxillary lateral incisors were nearly identical in the straight configuration.
Figure 7. (a) The mean specimen-level peak tensile foundation stress for each restorative system and contour. (b) The percentage reduction associated with the reference sinusoidal contour relative to the corresponding straight contour. SCI, SLI, and SC denote maxillary central incisors, lateral incisors, and canines; ICI, ILI, and IC denote the mandibular equivalents.

3.3. Adhesive Thickness Sensitivity and Numerical Verification

In the numerical straight-contour configurations, increasing the adhesive thickness multiplier from 0.5 to 2.0 reduced category-mean peak stress by 30.36–31.10%. For the analytical constant-width, long-strip case in Equations (4)–(6), peak stress scales with the fourth root of the adhesive elastic modulus at fixed thickness, veneer properties and load. Halving or doubling that modulus therefore changes the analytical peak stress by −15.9% or +18.9%, respectively. These percentages describe the analytical reference only.
The sensitivity of predicted peak tensile foundation stress to adhesive-layer thickness is illustrated in Figure S2.
In the finite-length specimen models, varying the assigned beam length by ±20% changed peak stress by at most 0.59%. Halving the effective adhesive-layer modulus reduced peak stress by 16.4–17.3%, whereas doubling it increased peak stress by 19.9–21.5% across the straight and reference sinusoidal configurations. In the optional multilayer Zr–LiSi model, including a 10 or 50 μm coating with an assigned modulus of 100,000 MPa reduced peak stress by at most 0.03% or 0.13%, respectively, relative to the single-layer baseline.
Increasing the discretization from 192 to 384 elements changed the category-mean peak stresses for the reference sinusoidal configuration by less than 0.09%. Across the specimen-level straight and sinusoidal configurations and both beam formulations, the maximum relative change was 0.13%. The relative force-equilibrium error, normalized moment-equilibrium error, and normalized assembled-system residual were below 10−8. These checks assessed numerical consistency within the implemented model. Independent experimental validation of the predicted stress fields was outside the scope of these checks.
The secondary stress series retained in the dataset was compared descriptively with the primary source endpoint for each specimen. The mean secondary-minus-primary difference was 0.086 MPa for LDS and 0.122 MPa for Zr–LiSi. Root-mean-square differences were 0.184 and 0.204 MPa, respectively. Individual differences ranged from −0.30 to 0.65 MPa for LDS and from −0.15 to 0.81 MPa for Zr–LiSi. These differences describe agreement between the two-stress series available in the dataset. The original calculations that produced the series could not be verified. The paired comparison of the primary and secondary stress series is shown in Figure S1.

3.4. Failure Characteristics

Two LDS specimens showed dental tissue involvement. One exhibited fracture of the tooth with the veneer still bonded. The other veneer detached with a small fragment of dental tissue on its intaglio surface (Figure 8a,b).
Figure 8. Representative failure patterns: (a) tooth fracture involving the bonded LDS veneer; (b) a detached LDS veneer with an attached fragment of dental tissue; and (c) Zr–LiSi veneer detachment with residual cement predominantly retained on the tooth surface.
No tooth fractures were reported in the Zr–LiSi group. Residual cement was generally observed on the tooth surface after detachment (Figure 8c). Qualitative observations included apparent cohesive failure within the cement, failure involving dental tissue, and apparent interfacial separation. Interfacial separation was the predominant visual impression. The available photographs did not provide matched views of both opposing surfaces for every specimen. Consequently, the specific interface involved could not be identified consistently, and failure-mode frequencies could not be reported by group.

4. Discussion

The present study identified a higher mean maximum peel stress endpoint, σp,max, for LDS than for Zr–LiSi veneers bonded to crenelated anterior tooth preparations. After adjustment for tooth category, the difference was 1.26 MPa (95% CI, 0.55–1.97 MPa), equivalent to approximately 6.9% of the Zr–LiSi mean. Although LDS means were higher in all six tooth categories, individual values overlapped. The adjusted difference remained positive across all 435 analyses that excluded two LDS observations, and the comparison using the second stress series gave a similar estimate of 1.22 MPa. This consistency applies to the reported stress values. The original force records and force-to-stress conversion were unavailable for verification; therefore, the ranking of the protocols by measured failure load remains unknown.
The simulations complement the mechanical tests by locating elastic stress concentrations under a common prescribed load. This loading scenario represents the intact assembly. The numerical results describe how a given load was transferred through the bonded assembly. The reported test endpoint concerns the stress associated with failure, which also depends on the resistance of the components and the path of failure.

4.1. Crenelated Preparation Geometry

Previous experimental work reported greater mean detachment forces for crenelated than for conventional LDS veneer preparations [21]. This finding provided a rationale for selecting the crenelated design in the present investigation. Using the same preparation for both groups allowed for comparison of the two restorative protocols within a common geometry. The experimental design did not include a conventional-preparation group.
The comparison at 50 N held the projected bonded area constant. Peak tensile foundation stress was located near the loaded end and decayed with distance, transitioning to a smaller compressive region. At reference phase 0°, the sinusoidal width modulation reduced category-mean peak stress by 1.36–2.20% for LDS and 1.55–2.67% for Zr–LiSi. The reduction was greatest for mandibular central incisors in LDS (2.20%) and mandibular lateral incisors in Zr–LiSi (2.67%). Figure 6 shows that the straight- and sinusoidal-contour profiles approached zero away from the loaded end after the smaller compressive region. The effect was small and concentrated near the point of loading. Its magnitude applied to the selected phase, geometry and loading direction.
The beam model represented the proximal design through a sinusoidal width variation at equal projected area. It omitted the three-dimensional proximal geometry, additional bonded surfaces and possible mechanical engagement between the veneer and the preparation. Those differences in geometry and outcome limit comparison with the earlier detachment experiment [21].

4.2. Surface Conditioning and Restorative Protocols

The etchable glass phase in LDS and the HF-plus-silane conditioning protocol provide a plausible basis for effective bonding [10,11]. In Zr–LiSi, the fired coating provides an etchable surface [15,16] and adds interfaces at which separation may occur. The cure mode of the resin cement and the pre-curing of the tooth adhesive could also have influenced the behavior of the assembly. Previous clinical comparisons used differing conditioning and cementation procedures [18,26], which supports interpreting retention at the protocol level.
The groups differed in ceramic, surface conditioning, resin cement and adhesive-curing sequence. Those factors were varied together in this study. Their individual contributions to the observed difference remain unresolved.
Evidence from other bonded assemblies also cautions against a universal material ranking. Sagen et al. [19] reported favorable tensile bonding results for zirconia under a different cementation configuration, with frequent cohesive cement failures. Such findings emphasize that the limiting component may change with the substrate, conditioning protocol, cement and loading arrangement. The higher mean σp,max in the LDS group therefore applies to the complete protocol evaluated under the conditions of this study.

4.3. Failure Patterns and Dental Tissue Involvement

The documented failure patterns provide additional context for the experimental comparison. In two LDS specimens, failure involved dental tissue. One tooth fractured with the veneer still bonded, and another veneer detached with a small fragment of dental tissue attached. These observations show that the loading sequence could produce failure involving the substrate. The path of failure also depends on substrate integrity, preparation geometry and loading conditions. The corresponding stress values therefore describe failure of the restored assembly, with an uncertain contribution from the strength of the adhesive interface itself.
No tooth fractures were reported in the Zr–LiSi group, and cement was generally retained on the tooth surface after veneer detachment. This pattern is consistent with separation at or near the restoration side of the bonded assembly. The available photographs could not resolve whether separation occurred at the cement–coating interface, within the coating or at the coating–zirconia junction.
Systematic classification would require assessment of both opposing surfaces from each specimen. Figure 8 presents representative photographs of the observed patterns. The available photographs did not provide a complete set of matched opposing surfaces for specimen-level classification, and the distribution of adhesive, cohesive and mixed failure modes remains uncertain. The two tissue-involving cases could not be linked to individual specimen IDs. The pair exclusion analysis quantified the sensitivity of the adjusted difference to removing any two LDS observations. It could not identify the effect of excluding the two documented cases specifically.

4.4. Stress Transfer and Adhesive-Layer Compliance

Mandibular incisors generally showed the largest numerical peak stresses under 50 N. In the test dataset, mandibular lateral incisors showed the lowest mean σp,max in both protocols. These rankings address different questions. At a fixed load, a higher numerical peak indicates greater local stress concentration in an intact assembly. At failure, the reported σp,max also depends on the loading history and the failure path. A specimen that concentrates stress under a common load can still reach failure at a lower reported endpoint.
The numerical response reflected the combined effects of width, ceramic thickness, adhesive-layer thickness and assigned elastic properties. The Timoshenko formulation additionally accounted for transverse shear deformation, while the Euler–Bernoulli formulation provided a complementary analytical and computational reference.
Over the ranges examined, the model was more sensitive to changes in the adhesive layer than to changes in contour or reference beam length. Increasing the adhesive thickness multiplier from 0.5 to 2.0 reduced straight-contour peak stresses by approximately 30–31%. The reference sinusoidal contour reduced peak stress by less than 3%, and varying beam length by ±20% changed peak stress by at most 0.59%. The effective adhesive modulus also influenced peak stresses substantially.
These differences describe elastic stress redistribution under the prescribed loading conditions. Fatigue, voids and progressive interface damage were outside the scope of the model.
The baseline simulations used an equivalent homogeneous adhesive layer. In the optional multilayer simulations, adding a 10 or 50 μm coating with an assigned modulus of 100,000 MPa reduced Zr–LiSi peak stresses by at most 0.03% or 0.13%, respectively. These results quantify the effect of the coating’s assumed normal compliance within the model. They provide no estimate of the strength of the coating or its interfaces.
The comparison between the two supplied stress series assessed their agreement. The inverse calculation provided the loads that would reproduce the supplied stresses under the assumptions of the analytical model. Independent validation would require measured loads and an experimentally supported link between those loads and the estimated stress field.

4.5. Tooth Category and Clinical Interpretation

Maxillary canines exhibited the highest reported mean σp,max in both systems, whereas mandibular lateral incisors exhibited the lowest. This shared pattern suggests an association with tooth category. Restoration dimensions, substrate distribution and loading geometry may contribute simultaneously.
The bonding substrate is particularly relevant. Clinical evidence associates dentine exposure with less favorable veneer outcomes [8]. Even with a common preparation design, the amount and distribution of enamel available for bonding may vary between teeth. The present model did not resolve variations in enamel and dentine or their local contribution to failure.
Because the groups were balanced by tooth category, the adjusted and unadjusted mean differences were identical. The additive model estimated a common difference between protocols across categories. With five specimens per protocol in each category, the larger descriptive difference among maxillary central incisors should be considered exploratory.
The direction of the comparison is consistent with observations from an earlier clinical series [18], although restorative indications, protocols and exposures differed. The clinical importance of the 1.26 MPa laboratory contrast is uncertain. For context, a systematic review estimated a pooled maximum voluntary incisal bite force of 209.2 N (95% CI, 132.5–285.9 N) in healthy dentulous participants [27]. Bite force in N and local peel stress in MPa describe different mechanical quantities.
A comparison of recorded test loads with clinical bite forces would also require consideration of the loading direction, contact position and loading history. Failure consequences matter clinically. An intact detached veneer may be amenable to rebounding, whereas fracture involving dental tissue can require further treatment of the tooth.

4.6. Comparison with Existing Evidence

Verniani et al. [28] evaluated 105 milled LDS veneers over 24 months and reported favorable clinical outcomes without significant differences between digital and hybrid workflows. Their findings support the clinical feasibility of CAD/CAM lithium disilicate veneers, although the ceramic product and outcomes differed from those evaluated here.
Yousry et al. [29] reported no restoration losses over one year for zirconia veneers manufactured using conventional or speed sintering. Nguyen et al. [26] found no statistically significant differences in one-year clinical outcomes between zirconia and LDS veneers treated with their respective adhesive protocols. These studies provide clinical context for interpreting the laboratory comparison, particularly because their bonding procedures, follow-up periods and outcomes differed from those used here.
Nguyen et al. [26] documented a zirconia veneer that debonded and was successfully rebonded without fracture, while an LDS veneer fractured upon debonding. Their observation involved fracture of the restoration. In the present study, two LDS failures involved dental tissue. The two studies illustrate how the consequences of failure can vary even when both events are classified broadly as loss of retention.
Yli-Urpo et al. [30] investigated occlusal veneers with different ceramic and cement-layer thicknesses. The lowest mean fracture load occurred in the thin LDS configuration with the thicker cement layer, and dental tissue fractures were observed in other configurations. Their posterior restorations and loading conditions differed from those studied here. The findings illustrate why a reduction in simulated peak stress with increasing adhesive-layer thickness should be interpreted alongside direct evidence on fracture and failure resistance.
Reis et al. [31] found that changing between the investigated resin cements did not significantly alter the biaxial flexural strength of ultrathin LDS specimens, whereas HF conditioning improved structural reliability. That study evaluated ceramic structural performance. In the present veneer–tooth assemblies, surface conditioning, cement polymerization mode and adhesive-curing sequence differed together, meaning that their individual effects could not be quantified.
Abid and Mohammed [32] reported that preparation design and loading direction influenced stress distribution in a three-dimensional LDS veneer model. Their comparison of palatal chamfer and window preparations provides context for analyzing preparation geometry under defined loading conditions. The present equal-area comparison isolated a single sinusoidal width modulation and found a small effect on simulated peak stress.

4.7. Limitations and Further Research

The sample size was determined by specimen availability, with five specimens per protocol within each tooth category. No a priori sample size or power calculation was performed. Specimens were allocated without randomization, and donor identifiers were unavailable to assess possible clustering. The same operator seated all veneers manually, but variation in seating force could not be quantified. Testing used one loading direction at a prescribed crosshead speed, and no thermocycling was performed. The results therefore reflect the specified laboratory conditions, with long-term clinical retention and failure under repeated loading beyond the scope of the study.
The main limitation was the inability to verify the original force–displacement records and the force-to-stress calculation used to generate the primary σp,max series. If that calculation used material-specific inputs, those inputs may have influenced the estimated difference between protocols. The observed difference therefore applies to the supplied calculated endpoint. The available failure photographs also limited classification of failure modes and prevented identification of the two tissue-involving cases in the statistical dataset.
The dataset provided specimen-level geometric inputs for modeling, but reference lengths and certain material properties remained modeling parameters. Averaging cervical and incisal dimensions simplified spatial variation within each specimen. Nominal CAD cement space and adhesive-layer thickness were treated as separate inputs. The one-dimensional linear–elastic model assumed a perfectly bonded interface and simplified the geometry and compliance of the tooth and adhesive layers. It omitted progressive damage, fracture and fatigue. Mesh convergence, equilibrium and residual checks assessed numerical consistency. Experimental validation and a failure criterion would be needed to predict debonding or fracture.
Further work should combine direct failure-load records with documented specimen geometry and systematic assessment of matched opposing failure surfaces. Including conventional preparations and alternative zirconia-conditioning protocols would help separate preparation effects from those of the coating and cementation sequence. Thermocycling and repeated loading would help establish how these systems respond to aging, while a validated damage formulation would be needed to connect the predicted stress field to the onset of failure.

5. Conclusions

For veneers bonded to crenelated anterior tooth preparations, the reported maximum peel stress values were higher for the LDS protocol than for the Zr–LiSi protocol. The adjusted mean difference between the two complete restorative protocols was 1.26 MPa (95% CI, 0.55–1.97 MPa). The null hypothesis of equal mean σp,max after adjustment for tooth category was therefore rejected. The adjusted difference remained positive across all analyses that excluded two LDS specimens. The original failure loads and the calculation used to derive the stress values could not be verified.
The reference sinusoidal contour reduced simulated peak tensile foundation stress by less than 3% under common loading at equal projected bonded area. This small effect was specific to the simulated configuration.
Two LDS specimens showed dental tissue involvement during failure. This observation highlights the importance of considering the extent of tissue damage and the feasibility of repair alongside retention. The clinical relevance of the laboratory difference remains uncertain.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/jfb17120604/s1. Figure S1. Paired comparison of the primary source endpoint (sigma A, source column E) and the secondary stress series (sigma B, source column S): (a) values plotted against one another, with the identity line; (b) secondary-minus-primary difference plotted against the pair mean, with a zero-difference line. Colors identify restorative systems. Source column S is originally named “Sigma din F masurat (MPa)”; this source heading is retained in the workbook and does not establish independent force measurements; Figure S2. Sensitivity of mean specimen-level peak tensile foundation stress to adhesive thickness in the straight configuration at 50 N. A multiplier of 1 denotes each specimen’s reference adhesive thickness; the other inputs remain unchanged.; Table S1A. Experimental stress series and specimen geometry—LDS (n = 30).; Table S1B. Experimental stress series and specimen geometry—Zr–LiSi (n = 30); Table S1C. Material inputs, analytical calculations, and numerical predictions—LDS (n = 30); Table S1D. Material inputs, analytical calculations, and numerical predictions—Zr–LiSi (n = 30); Supplementary File S1. Interactive application for complementary mechanical simulations (Veneer_simulations_EN.html).

Author Contributions

Conceptualization, A.C.M., A.J., M.L., A.C.; methodology, A.C.M., A.J., M.L., A.C., A.-E.A.-L.; validation, A.C.M., A.J., M.L.; formal analysis, A.C.M., A.J.; investigation, A.C.M., A.-E.A.-L., A.C.; data curation, A.C.M., A.C., A.-E.A.-L.; writing—original draft preparation—A.C.M., A.J.; writing—review and editing—A.C.M., A.J., M.L., A.C.; visualization, A.C.M., A.J.; supervision, M.L., A.C. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

The study was conducted in accordance with the Declaration of Helsinki and was approved by the Ethical Committee of the University of Medicine and Pharmacy “Victor Babeș” of Timișoara, Romania (approval no. 38/3 April 2026).

Data Availability Statement

The compiled specimen-level dataset and numerical outputs are available from the corresponding authors upon reasonable request. The retained dataset contains supplied calculated stress values and model-equivalent forces. Original machine-recorded force–displacement traces and measured failure loads were unavailable for verification.

Acknowledgments

While preparing this manuscript, the authors engaged ChatGPT 5.6 (OpenAI; accessed in October 2026) as a resource for English language refinement and data visualization. The authors undertook a rigorous review and integration of all outputs generated by this tool, thereby ensuring that the publication’s content meets the highest scholarly standards. They retain full responsibility for the integrity and accuracy of the material presented herein. We would like to acknowledge Victor Babes University of Medicine and Pharmacy Timisoara for their support in covering the costs of publication for this research paper.

Conflicts of Interest

The authors declare no conflicts of interest.

Abbreviations

The following abbreviations are used in this manuscript:
CAD/CAMComputer-aided design/computer-aided manufacturing
CIConfidence interval
DCDual-cured
FEAFinite element analysis
HC3Heteroscedasticity-consistent covariance estimator, type 3
HFHydrofluoric acid
ICMandibular canine
ICIMandibular central incisor
ILIMandibular lateral incisor
LCLight-cured
LDSLithium disilicate
MDP10-Methacryloyloxydecyl dihydrogen phosphate
OLSOrdinary least squares
SCMaxillary canine
SCIMaxillary central incisor
SDStandard deviation
SLIMaxillary lateral incisor
Zr–LiSiZirconia surface-modified with Biomic LiSi Connect

References

  1. Buonocore, M.G. A simple method of increasing the adhesion of acrylic filling materials to enamel surfaces. J. Dent. Res. 1955, 34, 849–853. [Google Scholar] [CrossRef] [Scilit]
  2. Horn, H.R. Porcelain laminate veneers bonded to etched enamel. Dent. Clin. N. Am. 1983, 27, 671–684. [Google Scholar] [CrossRef] [Scilit]
  3. Calamia, J.R. Etched porcelain facial veneers: A new treatment modality based on scientific and clinical evidence. N. Y. J. Dent. 1983, 53, 255–259. [Google Scholar]
  4. Fradeani, M.; Redemagni, M.; Corrado, M. Porcelain laminate veneers: 6- to 12-year clinical evaluation—A retrospective study. Int. J. Periodontics Restor. Dent. 2005, 25, 9–17. [Google Scholar]
  5. Beier, U.S.; Kapferer, I.; Burtscher, D.; Dumfahrt, H. Clinical performance of porcelain laminate veneers for up to 20 years. Int. J. Prosthodont. 2012, 25, 79–85. [Google Scholar]
  6. Aslan, Y.U.; Uludamar, A.; Özkan, Y. Retrospective Analysis of Lithium Disilicate Laminate Veneers Applied by Experienced Dentists: 10-Year Results. Int. J. Prosthodont. 2019, 32, 471–474. [Google Scholar] [CrossRef] [Scilit]
  7. Yıldız, P.; Ünlü, D.G.; Aydoğdu, H.M. Evaluation of vertical marginal discrepancy and load-to-failure of monolithic zirconia and lithium disilicate laminate veneers manufactured in different thicknesses. BMC Oral Health 2024, 24, 913. [Google Scholar] [CrossRef] [Scilit]
  8. Gurel, G.; Sesma, N.; Calamita, M.A.; Coachman, C.; Morimoto, S. Influence of enamel preservation on failure rates of porcelain laminate veneers. Int. J. Periodontics Restor. Dent. 2013, 33, 31–39. [Google Scholar] [CrossRef] [Scilit]
  9. Öztürk, E.; Bolay, Ş.; Hickel, R.; Ilie, N. Shear bond strength of porcelain laminate veneers to enamel, dentine and enamel-dentine complex bonded with different adhesive luting systems. J. Dent. 2013, 41, 97–105. [Google Scholar] [CrossRef] [Scilit]
  10. Puppin-Rontani, J.; Sundfeld, D.; Costa, A.R.; Correr, A.B.; Puppin-Rontani, R.M.; Borges, G.A.; Sinhoreti, M.A.C.; Correr-Sobrinho, L. Effect of Hydrofluoric Acid Concentration and Etching Time on Bond Strength to Lithium Disilicate Glass Ceramic. Oper. Dent. 2017, 42, 606–615. [Google Scholar] [CrossRef] [Scilit]
  11. Kalavacharla, V.K.; Lawson, N.C.; Ramp, L.C.; Burgess, J.O. Influence of Etching Protocol and Silane Treatment with a Universal Adhesive on Lithium Disilicate Bond Strength. Oper. Dent. 2015, 40, 372–378. [Google Scholar] [CrossRef] [Scilit]
  12. Kern, M.; Wegner, S.M. Bonding to zirconia ceramic: Adhesion methods and their durability. Dent. Mater. 1998, 14, 64–71. [Google Scholar] [CrossRef] [Scilit]
  13. Wolfart, M.; Lehmann, F.; Wolfart, S.; Kern, M. Durability of the resin bond strength to zirconia ceramic after using different surface conditioning methods. Dent. Mater. 2007, 23, 45–50. [Google Scholar] [CrossRef] [Scilit]
  14. Nagaoka, N.; Yoshihara, K.; Feitosa, V.P.; Tamada, Y.; Irie, M.; Yoshida, Y.; Van Meerbeek, B.; Hayakawa, S. Chemical interaction mechanism of 10-MDP with zirconia. Sci. Rep. 2017, 7, 45563. [Google Scholar] [CrossRef] [Scilit]
  15. Kitayama, S.; Nikaido, T.; Ikeda, M.; Sadr, A.; Miura, H.; Tagami, J. Internal coating of zirconia restoration with silica-based ceramic improves bonding of resin cement to dental zirconia ceramic. Bio Med. Mater. Eng. 2010, 20, 77–87. [Google Scholar] [CrossRef] [Scilit]
  16. El Feghaly, A.; Nasr, E.; Lukomska-Szymanska, M.; Zmysłowska-Polakowska, E.; Najjar, G.; Harouni, R.; Bourgi, R.; Hardan, L. Effect of different surface treatments on the bond strength of zirconia to resin cement. An in vitro study. Front. Dent. Med. 2026, 7, 1778379. [Google Scholar] [CrossRef] [Scilit]
  17. Maroiu, A.C.; Luca, M.M.; Jivanescu, A. Effect of Lithium-Disilicate Liners on Bond Strength and Fracture Resistance of Bilayered Zirconia Systems: A Systematic Review of In Vitro Evidence. Dent. J. 2026, 14, 5. [Google Scholar] [CrossRef] [Scilit]
  18. Măroiu, A.C.; Faur, A.-B.; Ardelean, A.; Leretter, M.; Jivănescu, A. Three-Year Clinical Outcomes of Lithium Disilicate and Lithium-Silicate-Modified Zirconia Veneers and Partial-Coverage Restorations: A Retrospective Comparative Study. Dent. J. 2026, 14, 621. [Google Scholar] [CrossRef] [Scilit]
  19. Sagen, M.A.; Kvam, K.; Ruyter, E.I.; Rønold, H.J. Debonding mechanism of zirconia and lithium disilicate resin cemented to dentin. Acta Biomater. Odontol. Scand. 2019, 5, 22–29. [Google Scholar] [CrossRef] [Scilit]
  20. Maroiu, A.C.; Sinescu, C.; Rominu, M.; Negrutiu, M.L.; Rusu, L.C.; Levai, C.M. Crenelated Dental Facets. Romanian Patent RO 131840 B1, 30 December 2020. [Google Scholar]
  21. Măroiu, A.-C.; Jivănescu, A.; Șerban, D.-A.; Negru, R.-M.; Duma, V.-F.; Sinescu, C.; Romînu, M. The Influence of a Novel, Crenelated Design of CAD-CAM Ceramic Veneers on the Debonding Strength. Materials 2023, 16, 3694. [Google Scholar] [CrossRef] [Scilit]
  22. Ivoclar Vivadent, A.G. IPS E.max CAD Scientific Documentation; Ivoclar Vivadent AG: Schaan, Liechtenstein, 2011. Available online: https://ivodent.hu/__docs/768_865d8476b1360c8ac461ae57f9c6b3c4.pdf (accessed on 24 October 2026).
  23. Qinhuangdao Aidite High-Technical Ceramics Co. Aidite Zirconia Dental Ceramics. 510(k) Summary K111291; U.S. Food and Drug Administration: Silver Spring, MD, USA, 2011. Available online: https://www.accessdata.fda.gov/cdrh_docs/pdf11/K111291.pdf (accessed on 24 October 2026).
  24. Aidite Biomedical Co., Ltd. Biomic LiSi Connect: Zirconia Bonding Pretreatment Agent. Product Brochure. Available online: https://www.aidite.com/upload/202407/%5B161710%5DBiomic%20Lisi%20connect%20brochure.pdf (accessed on 24 October 2026).
  25. Postnikov, M.A.; Butvilovsky, A.V.; Alsharifi, A.A.M.; Madatyan, A.V.; Kopetskiy, I.S.; Eremin, D.A. Justification of use of fixed retainers based on the analysis of size of the incisor and canine crowns. Bull. Russ. State Med. Univ. 2022, 6, 92–98. [Google Scholar] [CrossRef] [Scilit]
  26. Nguyen, V.A.; Vo, T.N.N.; Tong, M.S.; Nguyen, T.N.T.; Nguyen, T.T. Clinical Performance of Zirconia Veneers Bonded with MDP-Containing Polymeric Adhesives: A One-Year Randomized Controlled Trial. Polymers 2025, 17, 1213. [Google Scholar] [CrossRef] [Scilit]
  27. Daqiq, O.; Gareb, B.; Spijkervet, F.K.L.; Wubs, F.W.; Roossien, C.C.; van Minnen, B. Finite element analysis of the human mandible: A systematic review with meta-analysis of the essential input parameters. Sci. Rep. 2025, 15, 19582. [Google Scholar] [CrossRef] [Scilit]
  28. Verniani, G.; Ferrari, M.; Manfredini, D.; Ferrari Cagidiaco, E. A Randomized Controlled Clinical Trial on Lithium Disilicate Veneers Manufactured by the CAD–CAM Method: Digital Versus Hybrid Workflow. Prosthesis 2024, 6, 329–340. [Google Scholar] [CrossRef] [Scilit]
  29. Yousry, M.; Hammad, I.; El Halawani, M.; Aboushelib, M. Randomized clinical trial of zirconia laminate veneers sintered by using conventional versus speed process: 1-year follow-up. J. Prosthet. Dent. 2025, 133, 1474.e1–1474.e9. [Google Scholar] [CrossRef] [Scilit]
  30. Yli-Urpo, T.; Lassila, L.; Närhi, T.; Vallittu, P. Cement layer thickness and load-bearing capacity of tooth restored with lithium-disilicate glass ceramic and hybrid ceramic occlusal veneers. Dent. Mater. 2025, 41, 212–219. [Google Scholar] [CrossRef] [Scilit]
  31. Reis, A.F.N.; Borges, A.L.S.; Paradella, T.C.; da Silva de Assis, R.A.S.; Valandro, L.F.; de Melo, R.M. Effect of resin cement elastic modulus on the biaxial flexural strength and structural reliability of an ultra-thin lithium disilicate glass-ceramic material. Clin. Oral Investig. 2023, 27, 787–796. [Google Scholar] [CrossRef] [Scilit]
  32. Abid, S.E.; Mohammed, K.G. The Effect of Preparation Design on Stress Distribution in Lithium Disilicate Laminate Veneer using 3D Finite Element Analysis. Open Dent. J. 2023, 17, e18742106243827. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Article metric data becomes available approximately 24 hours after publication online.