Abstract
The analysis of process signals is a key method for gaining experimental insight into the underlying layer formation mechanisms in plasma electrolytic oxidation (PEO). This is made possible by the simultaneous measurement of electrical and optical process signals with high temporal resolution. However, according to the current state of the art, the interaction between these signals is primarily discussed in qualitative terms. Therefore, this article presents a robust methodology for analysing the current signal, which makes it possible to categorise the charge electro-chemical and plasma-chemical dominated subprocesses and to quantify their respective contributions. The evaluation is performed by taking additional process signals into account. The experimental setup for measuring process voltage, current, and photovoltage, as well as the measurement routine, are briefly described. This is followed by a detailed description of the numerical procedure. This includes the application of fundamental mathematical methods to the time-discrete measurement data, the automated selection of the pulse segment to be examined and the identification of discharge initiation to determine the interval boundaries of the electro- and plasma-chemically dominated pulse subsegments. The description of the routine is primarily intended for experimental scientists and is meant to provide them with a tool for extracting additional information from their process data. These can then be used to better understand electro-chemical side reactions and parasitic subprocesses in PEO.
1. Introduction
Plasma electrolytic oxidation (PEO) is an innovative method in surface engineering with a wide range of applications, e.g., in corrosion and wear protection and functional purposes [1]. During the process, the component to be treated is immersed in an aqueous, passivating electrolyte and is exposed to strong anodic polarisation. If suitable process parameters have been selected, this leads to the formation of an electrically insulating reaction layer on the substrate surface and a gaseous oxygen shell enveloping the sample geometry. Their interface to the bulk electrolyte then becomes the origin of plasma-electrolytic discharge phenomena, which, starting from the electrolyte, strike into the substrate and leave behind oxidised areas. In the further course of the process, oxidic layers are formed, whose technological properties can be varied within wide limits. In addition to the electrolytes used, the applied electrical regime is a decisive influencing factor for the coating result. In order to prevent the transition from short-lived layer-forming spark discharges to long-lived layer-destroying arc discharges, pulse or alternating electrical patterns are used. The complex substrate/electrolyte interactions change depending on whether process voltage or current is selected as the controlling variable and also interact with the device-specific rectifier control behaviour [2]. Hence, it is difficult to directly compare process data from different processes and process stages. On the other hand, the analysis of a multitude of process signals opens up an experimental approach to the subprocesses taking place during PEO and thus offers a powerful tool for researching the process.
This approach is already being used by various working groups. Examples of this can be found in the work of Arrabal, Martin, and Rogov [3,4,5]. While electrical process parameters are measured using fast oscilloscopes, discharge intensity is measured using various instruments, such as high-speed cameras, photomultipliers, and emission spectrometers. In addition to simply measuring process brightness, this allows for the collection of further valuable process information regarding discharge distribution as well as spectral data. However, precise temporal synchronization with the electrical process parameters on small time scales is difficult to achieve with these devices. High-speed cameras require additional light sources during short exposure times, which can outshine weak discharges. Emission spectrometers typically require integration times spanning several pulse periods to measure a meaningful spectrum. In general, according to the current state of the art, electrical and optical process data are primarily correlated on a qualitative basis. Therefore, in this study, the process brightness is measured using a photodiode at high temporal resolution and in synchronization with the electrical process signals. Afterwards, the present work describes a computational method based on the analysis of electrical and photoelectric process data, which is designed to separate and quantify fractions of the current, which are predominantly associated with electro-chemical (passive film formation, anodic metal dissolution, electrolysis) or plasma-chemical (spark discharge) electrode processes.
Electro-chemical subprocesses occur during the entire PEO treatment time [5,6] and therefore demand detailed research in the context of fundamental understanding and energy-efficient process design. One approach is the analysis of the electro-chemically generated electrolysis gas [7], which could be accompanied by the algorithm presented in modified form. In a previous study, the algorithm was used successfully for the identification of parasitic electro-chemical subprocesses during the PEO of magnesium [2]. The anodic side reactions of metal dissolution and electrolysis were significantly more pronounced on magnesium than in comparative experiments on aluminum under otherwise identical experimental conditions. Figure 1 shows examples of how such processes can affect the layer formation based on scanning electron microscopy (SEM) images.
Figure 1.
SEM cross-section and exemplary video images of PEO processes on the Al alloy AlMgSi1 (left), the Mg alloy AZ31 (right), and a coextruded composite made from these materials ((centre), Al outside, Mg Inside) under otherwise identical experimental conditions in accordance with the experiments that provided the data sets discussed in this paper.
Shown are scanning electron microscope cross-sectional images of PEO layers on the Al alloy AlMgSi1 (left), the Mg alloy AZ31 (right), and a coextruded composite material of these materials (centre, Al outside, Mg inside). The pulse and sample geometry as well as the electrolyte were in accordance with the experiments in [2], which also provided the data for the calculation examples discussed in this article. A dense PEO layer developed on aluminum. On magnesium, however, anodic metal dissolution during PEO led to a rough substrate/layer interface. The layer shows a larger number of cavities. Cathodically formed hydrogen can accumulate inside there. In combination with the more pronounced anodic oxygen formation, flammable oxyhydrogen mixtures can form. These are caused to explode by discharges and further damage the layer. Since the resulting exposed areas at the Mg substrate/layer interface exhibit increased activity for electro-chemical processes, the effects are self-reinforcing and have a significant influence on layer formation.
The purpose of this work is to deduce the algorithm used for the determination of electro and plasma-chemical charge density proportions during PEO mathematically correctly and describe it clearly. Pulse segments are designated as plasma-chemically dominated if the occurrence of discharges has been identified within them based on criteria derived from the process signals of current density and photovoltage. The outlook section discusses how the process analysis could be expanded by use of additional experimental peripheral devices. The described algorithm is based on an adapted interlocking of numerical techniques [8,9,10] as well as methods for analysis [11,12] and digital signal processing [13]. The electrical regime was chosen so that the special case of soft sparking does not occur. The plasma-chemically dominated pulse segments are not examined in depth with regard to different discharge types, as described in [14,15]. The outlook discusses how the presented algorithm could be extended using additional process data from an optical emission spectrometer (OES) with a focus on these aspects.
In Section 2, the methods used for this article are described. In Section 2.1, the experimental setup is explained. As the measured process data are noisy, a digital filter was applied, which is described in Section 2.2. The pulses to be analysed are identified within the measurement data sets using the procedure described in Section 2.3. The methodology of the identification of electro-chemically and plasma-chemically dominated pulse segments is written in Section 2.4. Section 2.5 summarises the methods used to calculate the area-related charge quantity passing through the sample surface. In Section 3, some results of the methodology are discussed. In Section 3.1, numerical validation experiments are presented. In Section 3.2, the analysis of results from experimental data is shown. In Section 4, the results are summarised and an outlook to future works is given.
2. Methods
2.1. Experimental Setup and Electrical Regime
The related PEO experiments were carried out on samples of the magnesium alloy AZ31 within an alkaline silicate electrolyte. The surface area of the sample was . The signals of the process voltage , the area-related responding current density , and the photovoltage were measured simultaneously by use of a transient recorder, DL950 (Yokogawa, Tokyo, Japan), with a sampling rate of 1 MS/s for recording durations of 500 ms. While the process voltage U is tapped directly at the electrodes, the corresponding current signal response is determined based on the voltage drop over a measurement shunt with a resistance of (Isabellenhütte, Dillenburg, Germany). The photo voltage is tapped at a BPW 21 photodiode (Osram, Munich, Germany), mounted in a BNC-to-DC adapter. This is integrated into the back wall of the basin in a stationary position. The line of sight points directly at the centre of the sample and meets it orthogonally in a distance of 15 cm. The generated photovoltage is to be understood as an integral signal of the present brightness or discharge intensity. Figure 2 shows a schematic representation (a) and detailed views (b)–(d) of the experimental setup used to acquire the data, which are further processed using the algorithm presented in this paper.
Figure 2.
Schematic representation of the experimental setup (a), top view of the treatment bath (b), image of the porthole in the front (c), indicating the position of the camera (e) and the photodiode, multisensor mount for implementing an OES system, an additional camera, and better EM shielding, as addressed in the outlook (d).
The positions of the photodiode can be seen in subfigures c and d of Figure 2. Figure 2d already shows the multisensor mount (addressed within the outlook), which was designed to additionally integrate the lens of an optical emission spectrometer into the assembly and to provide mounts for a protective net to shield against EM radiation from the PEO process. These are one source of the strong noise in the photoelectric signal (see Figure 3). Figure 2e shows the position of the camera, making it clear why the photodiode was positioned in the back wall of the basin.
Figure 3.
Example of a data set of unfiltered (left) and filtered PEO process data (right) showing the course of the process voltage in working and diagnostic pulses—blue/cyan, the current response —red, the corresponding photovoltage signal (t)—green, as well as a zoom on the current response during the diagnostic pulse and a bar graph of the determined area-related electro-chemical and plasma-chemical charge components and ; reprint of data published in [2].
The layer formation during the PEO is performed by working pulses (WPs), which are defined as current-controlled, alternating, symmetrical, rectangular-wave pulses, defined by the current densities , with = = 30 A/dm−2 at a frequency of f = 50 Hz. This results in current ratio r = |/| = 1, which does not support the occurrence of the so-called soft sparking regime [5]. The occurrence of such discharge phenomena would be accompanied by a reduced anodic process voltage, which was not observed in the underlying detailed experimental study [2]. The real current pulse geometry occurring in the process shows significant deviations from the predefined regime as a response to the complex interactions mentioned above and is the subject of the presented calculation methodology. In addition, diagnostic pulses (DPs) are coupled in at certain points during the PEO process, which are defined as a single voltage-controlled v-shaped triangular pulse with a constant descending and increasing voltage slope 60 kV/s between = 300 V, = −35 V, and back to . The voltage-pulse geometry that actually occurs in the process shows only slight deviations from the predefined regime and is the subject of the presented calculation methodology. A few of the generated data sets contained not only working pulses but also a diagnostic pulse.
2.2. Digital Filter and Numerical Handling of the Process Signals
Figure 3 shows an example of PEO process data, which are the subject of this work, before (left) and after (right) the data were preprocessed using a Hanning-windowed sinc filter with a filter kernel length of 2000 and a cut-off frequency of 15 kHz. The filter design of the applied filter is based on [13].
The origins of signal noise can be divided into the following categories:
- (N0)
- stochastic noise unrelated to the experimental circumstances;
- (N1)
- unintentional acquisition of electromagnetic signatures from the PEO process;
- (N2)
- fluctuations in brightness and current resulting from highly dynamic discharge behaviour and electrochemical gas formation during the process.
The stochastic N0 noise—such as fluctuations in the brightness of ceiling lights and background electromagnetic (EM) radiation—originates from the laboratory environment and contains no relevant information. The unintentional capture of EM signatures from the PEO process is also conceivable and likely. The plasma-electrolytic discharges act as local electrical conductors whose current flow changes rapidly and consequently must emit electromagnetic fields across a broad frequency band. Depending on how the connectors on the measuring resistor and photodiode are configured, they can act as antennas in combination with the high-impedance measurement cards of the transient recorder and capture the EM signatures (N1). Furthermore, the highly dynamic onset and decay of the discharges also lead to fluctuations in the actual measured quantities—current density and sample brightness (N2). The effects mentioned also occur in the process voltage signal; however, the signal-to-noise ratio is significantly better here due to the higher magnitude of the measured quantity. N0 noise can be counteracted by adjustments to the experimental setup (see Section 3, Outlook). Looking ahead, once the experimental optimisations are complete, the filter design could be further refined and specifically tailored to the requirements of each signal type. The objective here must be to filter out any remaining N0 and N1 noise and to avoid data loss in the N2 range.
Below, the numerical evaluation of the measurement data is described. In this article, the considerations are limited to the anodic part of the electrical regime. It is assumed that the anodic branch of the current response is either dominated by electro-chemical or plasma-chemical processes at all times. In the following, the respective portions of the current response are often referred to as electro-chemical or plasma-chemical current. The identification of the plasma-chemical current as well as the electro-chemical current requires the analysis of the photovoltage as well as the approximation of derivatives of the current response.
The used electrical regime mainly consists of current-controlled working pulses (WPs) that serve to form layers according to common PEO methodology. These are supplemented at defined process times by voltage-controlled diagnostic pulses (DPs), which allow for the investigation of (U) relationships independent of the rectifier control behaviour [2]. In order to determine the extent to which the diagnostic pulses interfere with the system under investigation, the last working pulse before and the first working pulse after a diagnostic pulse are also examined. The mathematical definition of the DP and the WP is given in the following. Since it is needed during the development of the evaluation of the WPs, the DP is given as a signal in the voltage regime and the WP is given as a double pulse in the current signal. For the definition of the DP, its duration is defined by:
for a given maximal voltage and a minimal voltage , i.e., , and given decreasing slope and increasing slope . Assuming that the DP starts at a starting point , the given triangular voltage profile is described by the function , defined by:
For a given starting point , the duration of a working pulse and for given currents and , an elementray representation of the WP is given by the function and defined via:
It has to be noted that the definitions of the pulses, the WP as a current profile, and the DP in a voltage profile were chosen for convenience, as they are investigated in Section 2.3 in the corresponding units. According to Ohm’s law, , the current density response is given through:
A photodiode is positioned near the sample during the PEO process to record a voltage corresponding to the light emission when the plasma-electrolytic discharges are ignited. The response is given through a photovoltage . During a data set recording at the times , with , the process voltage , the current-density response , and the photovoltages were measured, where is the number of measurements and T the duration of the PEO process. In the following, it is assumed that functions , exist, where is the space of continuous functions on and is the space of twice differentiable functions; for a rigorous definition of the linear spaces, see [11,12]. Subsequently, for every , the notations and will be used. Since the functions are not directly accessible, but the evaluations of and are given through experiments, at the times , suitable interpolants have to be used. In this article, interpolants in the space of constant piecewise affine functions are utilised [9,10]:
In the following, the interpolant of U is denoted by , the interpolant of is denoted by , and the interpolant is denoted by . The aim of the method is the identification of the process time, in which the plasma is ignited and the computation of the charge density given by the plasma-chemical and electro-chemical dominated portions of the current response as part of the anodic current, i.e., . Note that the related charge between the times is given by:
This directly implies that the integration limits for the plasma-chemical and the electro-chemical charge have to be identified. In this work, it is assumed that plasma-electrolytic discharges during the PEO only take place in the anodic partial period of the pulse, i.e., This was the case in [2], but it can also be different under certain process conditions [16] and would then have to be taken into account accordingly, which will not be conducted in this article. For further discussion, intervals in which a plasma-chemical reaction can be identified are denoted by , where is the current number of the interval, in which a plasma-chemical current is identified, and is the total number of intervals, in which the plasma-chemical reaction dominates. Intervals, in which only electro-chemical reactions are dominant, are given by the time intervals where the condition holds true and no plasma-chemical current can be identified. With that definition, it remains to identify the intervals and the domain in which the current response is positive. The associated methodology is described in Section 2.4. By construction, the integration limits for the plasma-chemical charge are given by the limits of . Hence, for the identification of the integration bounds for the plasma-chemical and electro-chemical current, it is sufficient to identify the bounds of the intervals .
2.3. Identification of Diagnostic Pulses and Working Pulses
For the analysis of given data sets, one of the two cases has to be applied, since, due to decomposition of the data sets, as performed in [2], diagnostic pulses do not have to be contained in the given data set. If a diagnostic pulse is contained in the data set, the analysis is limited to the diagnostic pulse and the two adjacent working pulses. If no diagnostic pulse is included in the data set, two working pulses in the middle of the data set are evaluated. The aimed analysis requires an identification method for finding the respective diagnostic and working pulses. For the identification of the DP, the definition displayed in (2) is used.
The method of finding the starting point of the DP is to compare the evaluation of , defined in equation (2), for every possible starting point . For this, an active set of indices , in which the distance between measured voltage in this measuring point , is compared to an evaluation of . Then, the index with an approximated starting point of the DP is given by:
where the error functional is a least-squares functional and defined by the following evaluation:
The approximated starting point of the DP is then given by . Given the length of the WP, which is assumed to be given, the neighbouring WPs are determined directly. As it is assumed that no two DPs are contained in a given data file, no DPs are neighbouring. It has to be noted that the least-squares functional , as defined in (8), can be used as a tool to determine whether a data set contains a DP or not. A convenient criterion is the check if the minimal evaluation of does not exceed a given border . If the data set does not contain a DP, two neighbouring WPs in the middle of the data set have to be identified. With a known length of the WP , the approach is the same as before, namely adapting the prediction function and duration of pulse in the index set . Since two neighbouring WP are searched, an adaption of the WP as defined in (3) is used, which connects two WPs in a function via
As constructed before, the index set is defined and used in a similar way as for the DP. The index at which the WP starts is given by the solution of the following minimisation problem:
where the error term is a least-squares functional given by:
Then, the starting point of both WPs is given by .
2.4. Identification of the Plasma-Chemical Dominated Pulse Segments
As mentioned above, the presented investigation method aims at the anodic branches of the current response . As discussed, the limits of the intervals , in which the plasma-chemical processes are dominant, have to be identified. For the characterisation of the intervals , the following assumptions are set:
- (A0)
- The measured current response is anodic, i.e., .
- (A1)
- The measured photovoltage is bounded from below by a minimal photovoltage , indicating that the plasma is ignited.
- (A2)
- The time of ignition of the plasma coincides with a local maximum of the first derivative of the current response .
Condition A2 was added in order not to interpret the surface emission of light occurring during the PEO within the anodic partial period of the pulse below the ignition voltage in the form of electroluminescence as the occurrence of the first spark discharges. These processes occur under certain conditions as a concomitant phenomenon of passive-film growth [17] and are therefore assigned to the electro-chemical subprocesses in the classification chosen here. The transition from full-surface electroluminescence to localised spark discharge or the beginning of the superposition of spark discharge and electroluminescence through the establishment of discharge channels is characterised by an abrupt increase in current. This is identified by A2. While for the starting points all three assumptions (A0)–(A2) have to be fulfilled, for the ending point , only the conditions (A0) and (A1) are needed. If a starting point was identified, the ending point is identified as the last time since starting the interval for which (A0) or (A1) are both fulfilled without interruption. Since the implementation of the conditions (A0) and (A1) are in simple comparison to (A2), the following discussion will concentrate on the fulfillment of (A2). For the identification of a local maximum of , some theory from analysis [12] has to be recollected. First note that for all differentiable functions , where J is an open subset of , and the first derivative is defined as:
From the definition of the first derivative (12), it directly follows that a difference quotient is a sufficiently good approximation of when is sufficiently small:
By application of (13) on in with the step size , an approximated derivative of in is then given through:
A similar approach as for in (14) provides an approximation of the second derivative of in :
Classically, one defines the approximations of the derivatives through difference quotients given in (14) and (15) by fixing . Using a general but still well-chosen can, for sufficiently small step sizes , be considered as smoothening the values of the approximation.
The usually used criterion for a maximum in is given through the first- and second-order criteria, which are stating that and , see, e.g., [12]. It has to be observed that this criterion is not practical since is not given as a twice-differentiable function but as an interpolation of data points which are submitted to measuring errors. In consequence, the local minima and maxima in will occur regularly. This requires a suitable replacement of the condition (A2), reflecting the nature of the given data set as a discrete set of measurements. This can be corrected by assuming that the considered local maximum exceeds the median of by a certain degree. This can be implemented by the following condition:
- (A2’)
- has a local maximum in , with
where is a chosen weighting factor. It has to be noted that .
It has to be noted that the indicated maximum in can be determined by a change in sign of from negative to positive.
With (A0), (A1), and (A2’), three easy-to-implement conditions to identify the intervals , in which the plasma is ignited, are stated. It has to be noted that the scaling factor has to be chosen carefully, depending on the investigated data. It has to be added that the scaling factor is a phenomenological parameter, which has to be chosen within a certain range, in dependence of the intensity of the variation of the measured . With our examples, a value was a successful choice. However, a convenient choice of could be necessary for other electrolyte–substrate systems or other measuring set-ups. Nevertheless, once successfully fixed, it opens up the investigation methodology.
2.5. Computation of the Area-Related Transferred Charge
This subsection is devoted to the description of the computation of the plasma-chemical and electro-chemical area-related charge passing through the electrode surface during the working and DPs, respectively. For the following discussion of the electro-chemical charge during a pulse, the plasma-chemical charge , and the anodic charge during a pulse , the following identities hold true:
where, for the starting time and the ending time of the pulse , the interval is given through:
Since is not known exactly, the charge cannot be evaluated exactly. Hence, the interpolant is used instead of . In this context, it has to be remarked that for any given index j, the following equality holds true:
When applying this strategy to , note that it coincides with the trapezoidal rule and midpoint rule for integration, respectively [8]. Applying (18) to all subintervals on the plasma-chemical charge , one obtains the following formula:
where is the number of intervals in which the plasma-chemical discharge phenomena were dominant. For a given pulse and every t, the indicator function is given by
Additionally, the index is given such that , and the index is given such that . Note that the approximated anodic charge in a pulse is computed in the same way as the plasma-chemical charge . Hence, the electro-chemical charge can be computed via (16). The following results section is divided into two subsections. In Section 3.1, a verification of the numerical methodology based on constructed voltages will be undertaken. In Section 3.2, two experimental results—one with and one without a DP—will be discussed.
3. Results
3.1. Verification of the Methodology
This subsection is devoted to the verification of the described and implemented methodology, especially the integration of the currents, the identification of measuring and WPs, and the identification of plasma-chemical currents. The performed tests in this subsection discuss constructed examples which have a clear divide between plasma-chemical and electro-chemical currents respecting the galvanoluminescence in the photovoltage. For this verification of the data-evaluation strategy discussed in Section 2, ten data sets with one DP and ten data sets without any DPs were investigated. In both cases, each data set contains one-hundred working pulses. For the construction of the current-controlled WP, the function from (3) is used. For the current response of the voltage-controlled DP, the function from (2) and the simplification of perfect ohmic behaviour are used.
In data sets with a DP, the position of the DP within the data set is set randomly to verify that the method for the identification of DPs works properly. In both cases, with and without a DP, the ten data sets were constructed numerically for the verification of the numerical methodology in a way such that during the first and second WP, and, if present, during the DP, , , …, of the process time with anodic current was plasma-chemical currents. The regions with dominantly plasma-chemical processes are indicated by a jump of from 29 A·dm−2 to 31 A·dm−2, see Figure 4, resulting in a high increase in as well as a jump in the photovoltage to 4 V. In both cases, with and without DP, before the start of the plasma-chemical currents, the photovoltage was set to a non-zero value, below the minimal threshold = 1.2 V, to indicate galvanoluminescence effects [18]. To the WPs a random function was added to reflect the expected white noise overlaying the measured signal and reflecting measuring errors.
Figure 4.
Current-density response (red), given photovoltage for a portion of the anodic current-density response being plasma-chemically active (green), electro-chemical part (orange fill) and plasma-chemical part of the current density (red fill) of the anodic partial period of computed electrical regimes without (a) and with DP (b). The green dashed lines indicate of condition (A1), red dashed lines indicate the prodact of the scaling factor = 10, and the median of the first derivative of from condition (A2)’ with .
In Figure 4a, the two identified WPs from the middle of the data set containing no DP are shown with a plasma-chemical part of . Since the time interval corresponding to the two WPs was identified with the methodology described in Section 2.3 and the result coincides with the expectations, this indicates the validity of the methodology. The graph also shows the photovoltage, which is set for of the time of the anodic current (i.e., plasma-chemical processes take place). With the given photovoltage and the given current pattern, the methodology described in Section 2.4 is applied. Additionally, and are displayed. In the corresponding graph, for is displayed. It can be seen that the identified starting point for the plasma-chemical current is identified by (A2’) correctly. It can as well be seen that the same peak in indicating the start of the plasma-chemical current can be seen in . The results are visualised by the orange and red fills. It can be seen that a portion of the anodic current is identified correctly as being plasma-chemical and hence being electro-chemical. This is a first indicator of the validity of the identification algorithm for the intervals . For the further verification, the respective charge has to be studied. First note that the length of the anodic partial period is a WP is constructed as , and the current density is given through = 29 A·dm−2 if the electro-chemical current is active and = 31 A·dm−2 if the plasma-chemical current is active. Hence, the expected area-related charge during the anodic branch during one of the WPs is given through · · dm−2, where reflects the current percentage for the given example.
The second set of examples contains DPs. In Figure 4b, the identified DP is shown with the adjacent WPs. Since the DP was found in the data file by the algorithm, this indicates that the identification of the DP as described in Section 2.3 is applicable. Additionally, the given photovoltage for a part of the anodic current density is shown. Furthermore, and are displayed; additionally, the threshold from (A2’) for is displayed, indicating the starting point for the plasma-chemical current. Note that the same starting point can be identified when using instead of . The corresponding electro-chemical and plasma-chemical parts of the anodic sections of the given current-density response are indicated by orange and red fills. As it can be seen, the calculated division is a division between the plasma-chemical and electro-chemical in the WPs, as expected. The previous observation is possible since restricted to the anodic branch of the WPs is constant and hence there is a linear connection between current and charge. This observation is an additional indicator that the intervals , in which the plasma-chemical reaction is identified, are assigned correctly by the method discussed in Section 2.4. To fully verify the methodology, the respective charges have to be discussed in more detail.
In Table 1, the plasma-chemical , and electro-chemical , charge in the first and second analysed WP, respectively, are shown for multiple percentages of the plasma-chemical portion of the total anodic charge. As it can be seen in Table 1, the indicated percentages of the plasma-chemical and electro-chemical parts of the first WP were computed correctly, as constructed. Additionally, the same behaviour can be observed for and in the data set in Table 1. In total, this behaviour validates the described methodology when no DP is included.
Table 1.
Results of the validation experiments not including a DP.
In Table 2, the plasma-chemical , and electro-chemical , charge in the first and second analysed WP, respectively, as well as the plasma-chemical and the electro-chemical charge during the DP are shown for multiple percentages of the plasma-chemical portion of the total anodic charge.
Table 2.
Results of the validation experiments including a DP.
As in the example without DP, see Table 1, the total charge for the anodic branch of during the WP can be estimated by . Summation of the corresponding computed plasma-chemical and electro-chemical charges during the two WPs provide this value of up to a small deviation . Additionally, the set values of the portion of the plasma-chemical charge of the total anodic charge can be reproduced. Considering the charges in the DP (Table 2), the summations of the electro-chemical and the plasma-chemical charges approximate the same value, and the claimed portion of the plasma-chemical charge of the total anodic charge holds true. This is validated by summation of the corresponding electro-chemical charge. The observations for this set of experiments indicate that the discussed methodology also applies when DPs are included. In total, both sets of experiments show the applicability of the methodology in a theoretical setup.
On a last remark, different values for were investigated, and the evaluation results of are relatively stable in a range = 5–15. Below 5, the complete current was detected as plasma-chemical, and a higher value led to the identification of no current.
3.2. Results from Experiments
After the theoretical validation of the developed methodology in Section 3.1, an application of the algorithm to a real, experimentally obtained data set has to be undertaken to finish the validation of its applicability. For this, two examples based on the PEO of magnesium are investigated with experimental data from [2]. The corresponding data are summarised in Figure 5, showing electrical regimes without and with DP. One major difference from the examples in Section 3.1 is that the shape of the photovoltage signal deviates significantly from being rectangular.
Figure 5.
Current-density response (red), given photovoltage for the PEO of magnesium and the plasma-chemically active (green) part of the anodic current density, electro-chemical part (orange fill), and plasma-chemical part of the current density (red fill) of the anodic partial period of measured electrical regimes on Mg without (a) and with DP (b). The green dashed lines indicate of condition (A1). The red dashed lines indicate the prodact of the scaling factor = 10 and the median of the first derivative of from condition (A2)’.
However, in combination with the condition (A2’) and the displayed difference quotients, the boarders of the intervals can be estimated by hand. Thus, due to its correspondence with the computed boarders, the identification methodology described in Section 2.4 is applicable in the case that the real measured data set does not contain a DP.
In the data set depicted in Figure 5b, the included DP was identified correctly in the experimentally determined data set. Additionally, it can be verified by the behaviour of the photovoltage, green in Figure 5, with the displayed difference quotients and , that the time spans where the plasma-chemical currents dominate were identified correctly.
Additionally, the median of the current response during the anodic branches of the WPs can be estimated to be 30 A · dm−2 with an estimated duration of the anodic branch during the WP of 10 ms. Thus, the anodic charge amounts to about · dm−2.
In the data set without a DP, in Figure 5a, it can additionally be observed that the plasma-chemical parts of the first WP have nearly the same value as in the second pulse. When a DP is included in the data set, a different behaviour is observed. As to be seen in Figure 5b, the plasma-chemical part of the second WP dominates nearly the complete pulse. Furthermore, it can be observed that the plasma-chemical parts in the DP will be low in comparison to the electro-chemical one. The observations from these graphs indicate that the described methodologies work correctly. Nevertheless, to confirm the observations, a deeper look into the measured charges has to be undertaken.
In Table 3, the plasma- and electro-chemical charges during the first and second WP and—if present—the DP are listed. In both cases in the WPs, equals to C · dm−2 in each WP. This resembles the estimated value sufficiently well. Additionally, the observation of the dominance of the plasma-chemical charge over the electro-chemical charge in the second WP (when a DP is included) is reflected in the values presented in Table 3. Additionally, the observation that the plasma-chemical currents in the first and second WP when no DP is included, see Figure 5a, are nearly identical can be confirmed. The prediction of a low plasma-chemical portion in the DP is also reflected in the values.
Table 3.
Results of physical experiments including a DP.
The correspondence of the results in Table 3 with visual information, see Figure 5, showcases together with the discussed plausibility of the computed values that the numerical methodology is applicable to experimental data, which had to be verified after verifying the method to sand-box problems in Section 3.1.
Again, the variation of has shown relative stability within a range of 8 to 20, but the optimal fit was 10 with similar side effects as described in Section 2.5. This behaviour shows that the definition of has to be well chosen and, in dependence of the investigated system, has to be adapted.
The results in this section show the applicability of the discussed methodology to evaluate the respective charges in experimental data sets. When combining these results with the theoretical investigations of Section 3.1, it can be concluded that the applied methodology can be considered validated.
4. Summary and Outlook
In Section 2, a numerical methodology to evaluate the charges in PEO data during WPs and DPs was derived. This includes the identification of WPs and a DP from data files. For this, a method to determine relevant time intervals , in which the plasma-chemical reactions are dominant, from the current-density response and the photovoltage is described. For the identification of , three assumptions are required to be fulfilled, where the last was reformulated to reduce assumptions on differentiability. The evaluation of the charges includes the evaluation of the integral of the interpolated current response using a quadrature method, which is algebraically exact.
In Section 3, the mathematical methodology was validated using both constructed examples (with known, predefined results) and experimental data from a PEO process on Mg from [2]. The methodology was already successfully applied in the identification of parasitic electro-chemical subprocesses during PEO on Mg [2]. This article finds a numerical methodology to automatically evaluate charges, which is not only applicable to PEO but also to other processes that provide large sets of in-process data—with only minor adjustments to the methodology. Additionally, the methodology can be adjusted to include more or other shapes than triangles for the DPs to obtain a more detailed view on the process-specific interactions. Due to the possibility to combine different in-process data of one experiment, mechanisms and subprocesses can be derived to create profound understanding of the process. As a first step for future investigations, the methodology can be applied to PEO processes on other substrates than Mg to identify parasitic electro-chemical subprocesses or correlate the process data to the resulting microstructure. This also allows for an in-process control of layer properties or tailored/shorter processes, which would be more energy- and resource-efficient. In conclusion, the contribution of the algorithm to current works is given by its potential for application to a broad field of experiments.
Although this article has developed a numerical method for analysing process data, validated it using numerical examples, and demonstrated its practical applicability, further investigations will be necessary in the future. This applies in particular to a practical sensitivity analysis regarding the selection of threshold values for the photovoltage and the weighting factor from (A2’), as well as the stepping size of the difference quotients as approximation of the derivatives. In this context, the algorithm’s sensitivity to small changes in the relevant values must be tested using real-world data. Although this issue is of some importance, it has not been examined in detail in this article, as the focus was instead on the development of the numerical method and demonstrating its general applicability. A detailed sensitivity analysis would go beyond the scope of this work.
Further developments of the presented approach would also require adjustments to the experimental setup. One simple measure that has already been implemented by the authors of this study is to replace the photodiode holder from a simple BNC-to-DC adapter to a 3D-printed mount with an EM sleeve. This minimises the strong noise in the photoelectric signal (plot at bottom left in Figure 3), which is likely an electromagnetic signature of the PEO process. In order to more precisely resolve the electro-chemical processes, especially gas evolution, a high-speed camera with appropriate lighting must be added. The sample holder should be designed to expose two exposure areas for one sample: a front surface for well-lit video recordings, and a back surface for optical analysis of the discharge behaviour without external light contamination. To better understand the plasma-chemical processes, an optical emission spectrometer (OES) should be added. The gained data should be included in the algorithm in order to examine the light-emitting processes more in detail, taking into account specific discharge stages (e.g., soft sparking), different discharge types (A–D discharges) [14,15], and oxyhydrogen explosions. A detailed analysis of the transient behaviour of the process voltage and system impedance, as well as their temporal derivatives, can also usefully complement the methodology presented.
Author Contributions
Conceptualisation, S.D.S., F.S., T.M. and T.L.; methodology, S.D.S. and F.S.; software, S.D.S.; validation, F.S. and S.D.S.; formal analysis, S.D.S.; investigation, F.S. and S.D.S.; resources, F.S.; data curation, F.S.; writing—original draft preparation, S.D.S. and F.S.; writing—review and editing, T.M. and T.L.; visualisation, F.S. and S.D.S.; supervision, T.M. and T.L.; project administration, F.S. and S.D.S.; funding acquisition, T.L. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by the German Research Foundation (Deutsche Forschungsgemeinschaft DFG), Project No. LA 1274/55-1, Grant No. 421508739.
Data Availability Statement
The experimental data discussed in this work are available from the corresponding author upon request.
Conflicts of Interest
The authors declare no conflicts of interest.
Abbreviations
The following abbreviations are used in this manuscript:
| DP | Diagnostic Pulse |
| PEO | Plasma Electrolytic Oxidation |
| SEM | Scanning Electron Microscopy |
| WP | Working Pulse |
References
- Simchen, F.; Sieber, M.; Kopp, A.; Lampke, T. Introduction to plasma electrolytic oxidation-an overview of the process and applications. Coatings 2020, 10, 628. [Google Scholar] [CrossRef] [Scilit]
- Simchen, F.; Schwöbel, S.; Mehner, T.; Lampke, T. Specification of parasitic electrochemical subprocesses during plasma electrolytic oxidation of magnesium. Electrochim. Acta 2023, 464, 142858. [Google Scholar] [CrossRef] [Scilit]
- Arrabal, R.; Matykina, E.; Hashimoto, T.; Skeldon, P.; Thompson, G. Characterization of AC PEO coatings on magnesium alloys. Surf. Coat. Technol. 2009, 203, 2207–2220. [Google Scholar] [CrossRef] [Scilit]
- Martin, J.; Nominé, A.; Brochard, F.; Briançon, J.L.; Noël, C.; Belmonte, T.; Czerwiec, T.; Henrion, G. Delay in micro-discharges appearance during PEO of Al: Evidence of a mechanism of charge accumulation at the electrolyte/oxide interface. Appl. Surf. Sci. 2017, 410, 29–41. [Google Scholar] [CrossRef] [Scilit]
- Rogov, A.; Yerokhin, A.; Matthews, A. The Role of Cathodic Current in Plasma Electrolytic Oxidation of Aluminum: Phenomenological Concepts of the “Soft Sparking” Mode. Langmuir 2017, 33, 11059–11069. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Yerokhin, A.; Leyland, A.; Matthews, A. Kinetic Aspects of Aluminium Titanate Layer Formation on Titanium Alloys by Plasma Electrolytic Oxidation. Appl. Surf. Sci. 2002, 200, 172–184. [Google Scholar] [CrossRef] [Scilit]
- Rogov, A.; Shayapov, V. The role of cathodic current in PEO of aluminum: Influence of cationic electrolyte composition on the transient current-voltage curves and the discharges optical emission spectra. Appl. Surf. Sci. 2017, 394, 323–332. [Google Scholar] [CrossRef] [Scilit]
- Dahmen, W.; Reusken, A. Numeric for Engineers and Natural Scientists; Springer: Berlin/Heidelberg, Germany, 2008. (In German) [Google Scholar]
- Evans, G.A.; Blackledge, J.M.; Yardley, P.D. Finite Element Method for Ordinary Differential Equations. In Numerical Methods for Partial Differential Equations; Springer: London, UK, 2000; pp. 123–164. [Google Scholar]
- Schwoebel, S.D.; Mehner, T.; Lampke, T. On a Robust and Efficient Numerical Scheme for the Simulation of Stationary 3-Component Systems with Non-Negative Species-Concentration with an Application to the Cu Deposition from a Cu-(β-alanine)-Electrolyte. Algorithms 2021, 14, 113. [Google Scholar] [CrossRef] [Scilit]
- Alt, H.W. Linear Functional Analysis, 6th ed.; Springer: Berlin/Heidelberg, Germany, 2012. (In German) [Google Scholar]
- Tao, T. Differentiation of Functions. In Analysis I; Springer Nature: Singapore, 2022; pp. 217–229. [Google Scholar]
- Smith, S.W. Digital Signal Processing: A Practical Guide for Engineers and Scientists; Newnes: Amsterdam, The Netherlands, 2003; Chapter 16. [Google Scholar]
- Cheng, Y.L.; Xue, Z.G.; Wang, Q.; Wu, X.Q.; Matykina, E.; Skeldon, P.; Thompson, G. New findings on properties of plasma electrolytic oxidation coatings from study of an Al–Cu–Li alloy. Electrochim. Acta 2013, 107, 358–378. [Google Scholar] [CrossRef] [Scilit]
- Hussein, R.O.; Nie, X.; Northwood, D.O.; Yerokhin, A.; Matthews, A. Spectroscopic study of electrolytic plasma and discharging behaviour during the plasma electrolytic oxidation (PEO) process. J. Phys. Appl. Phys. 2010, 43, 105203. [Google Scholar] [CrossRef] [Scilit]
- Rakoch, A.; Gladkova, A.; Linn, Z.; Strekalina, D. The evidence of cathodic micro-discharges during plasma electrolytic oxidation of light metallic alloys and micro-discharge intensity depending on pH of the electrolyte. Surf. Coat. Technol. 2015, 269, 138–144. [Google Scholar] [CrossRef] [Scilit]
- Stojadinović, S.; Vasilić, R.; Petković, M.; Belča, I.; Kasalica, B.; Perić, M.; Zeković, L. Luminescence during anodization of magnesium alloy AZ31. Electrochim. Acta 2012, 59, 354–359. [Google Scholar] [CrossRef] [Scilit]
- Kasalica, B.; Belca, I.; Stojadinovic, S.; Zekovic, L.D.; Nikolic, D. Light-Emitting-Diode-Based Light Source for Calibration of an Intensified Charge-Coupled Device Detection System Intended for Galvanoluminescence Measurements. Appl. Spectrosc. 2006, 60, 1090–1094. [Google Scholar] [CrossRef] [Scilit] [PubMed]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.