Featured Application
The proposed equal-curvature framework and empirical correction relationship provide practical guidance for improving the accuracy of surface strain measurements in carbon fiber reinforced polymer (CFRP) structures.
Abstract
Surface strain measurements on carbon fiber-reinforced polymer (CFRP) structures using bonded strain gauges are often systematically underestimated due to strain transfer effects associated with the surface resin-rich layer. To investigate this issue, comparative bending experiments were performed on steel and CFRP beams, where the steel beam served as a reference structure with negligible strain transfer loss under equal-curvature conditions. An equal-curvature bending framework was established to ensure identical bending curvature at the strain measurement location for both materials, thereby eliminating the influence of material stiffness on global deformation. In parallel, controlled surface polishing was employed to precisely regulate the thickness of the resin-rich layer on CFRP specimens, enabling systematic evaluation of its influence on strain transfer behavior. Experimental results under equal-curvature conditions reveal a stable strain underestimation in CFRP surface measurements, with an average strain transfer coefficient of approximately 0.968. Furthermore, reducing the resin-rich layer thickness leads to a consistent increase in measured strain. Based on these observations, a practical strain correction model was established to improve the reliability and engineering applicability of surface strain measurements in CFRP structures.
1. Introduction
Accurate strain measurement is a fundamental requirement in experimental mechanics, structural testing, and structural health monitoring of engineering components. Among various sensing technologies, surface-mounted electrical resistance strain gauges remain one of the most widely used tools due to their high sensitivity, mature instrumentation, robustness, and compatibility with both laboratory and field environments [1,2,3]. For metallic structures, which are typically homogeneous and isotropic, surface-mounted strain gauges are generally assumed to provide reliable measurements of surface strain when appropriate bonding procedures are applied [4].
With the increasing application of carbon fiber-reinforced polymer (CFRP) structures in aerospace, civil infrastructure, and mechanical engineering, surface strain measurement has become more challenging. CFRP materials exhibit strong anisotropy, laminated architectures, and pronounced microstructural heterogeneity, which fundamentally distinguish them from conventional metallic materials [5,6,7]. Consequently, apparent discrepancies between surface strain gauge readings and the actual strain state within the load-bearing fiber layers have been frequently reported in CFRP components [8,9,10]. Such discrepancies may adversely affect experimental interpretation, model validation, and engineering assessment if not properly understood.
The mismatch between measured and actual strain is commonly associated with strain transfer effects. In practical measurements, the sensing grid of a surface-mounted strain gauge does not directly experience the strain of the structural fibers. Instead, strain is transmitted through a sequence of intermediate layers, including the substrate surface layer, the adhesive layer, the gauge backing, and protective coatings. As a result, the measured strain represents an attenuated response governed by the mechanical properties, thicknesses, and interfacial conditions of these layers [2,6,7,8,9]. Accordingly, surface-mounted strain gauges on composite substrates are inherently susceptible to strain transfer losses. Extensive studies have been devoted to strain transfer mechanisms using analytical, numerical, and experimental approaches. Based on shear-lag theory, multilayer strain transfer models have been developed to quantify the influence of adhesive thickness, shear modulus, sensor geometry, and bonding length on strain transfer efficiency [11,12,13]. These models have been widely validated for metallic substrates and subsequently extended to composite materials [14,15,16,17]. Parallel developments in optical fiber sensing, particularly for fiber Bragg grating (FBG) sensors bonded to or embedded in composites, have further demonstrated the critical role of interfacial layers in governing strain transfer behavior [18,19,20,21]. Although electrical strain gauges and optical fiber sensors operate on different sensing principles, both rely on strain transfer from the host structure to the sensing element, rendering these findings conceptually relevant.
Despite the substantial progress in adhesive- and interface-focused strain transfer studies, most existing investigations implicitly assume that the composite substrate surface mechanically represents the underlying load-bearing laminate. This assumption may be reasonable for metals but becomes questionable for CFRP structures, where the surface layer is often not fiber-dominated. A characteristic feature of CFRP components manufactured by autoclave curing, resin transfer molding, or vacuum-assisted processes is the presence of a resin-rich layer [22,23,24]. This layer, formed due to resin flow, fiber distribution, and tooling effects, is dominated by polymer matrix material and typically exhibits a substantially lower elastic modulus than the underlying fiber-reinforced laminate. Previous studies have primarily examined resin-rich layer from the perspectives of damage initiation, stiffness degradation, and failure behavior [25,26,27], demonstrating that such regions can significantly alter local deformation and stress distributions. However, their influence on surface strain measurement accuracy has received comparatively limited systematic investigation.
Several experimental and numerical studies have suggested that surface resin-rich layers may contribute to additional strain attenuation before deformation reaches the bonded sensor [9,10]. These observations imply that, even when adhesive properties and sensor installation procedures are carefully controlled, the mechanical compliance of the CFRP surface layer itself may influence strain transfer efficiency. Nevertheless, quantitative experimental evidence isolating the effect of resin-rich layer thickness on strain transfer behavior in surface-mounted electrical strain gauges remains scarce.
Another important challenge in evaluating strain transfer behavior lies in the experimental comparison methodology. Conventional approaches based on equal applied load or equal nominal stress do not ensure identical deformation states when materials with significantly different elastic moduli are compared. In bending-dominated structures, such as beams, different materials subjected to identical loads generally exhibit different curvature distributions, leading to different surface strain levels and obscuring the distinction between global structural response and local strain transfer effects [28].
From a kinematic standpoint, surface strain under elastic bending is directly related to local curvature and cross-sectional geometry. For beams with identical geometry, equal curvature at a given location implies equal theoretical surface strain, independent of material stiffness. Therefore, an equal-curvature comparison provides a physically consistent basis for evaluating strain measurement discrepancies between different materials. Although non-contact techniques such as digital image correlation and thermoelastic stress analysis offer valuable alternatives for strain measurement [29], their practical limitations in field deployment mean that surface-mounted electrical strain gauges remain indispensable in many engineering applications.
Motivated by these considerations, the present study proposes an equal-curvature bending framework to investigate apparent strain underestimation in CFRP surface strain measurements. By enforcing identical curvature at the strain gauge location, the influence of material stiffness on global structural response is minimized, allowing measured strain differences to be attributed more directly to strain transfer behavior. Furthermore, the thickness of the CFRP surface resin-rich layer is systematically investigated as a key factor through controlled surface polishing and combined experimental–numerical analysis.
Accordingly, the present study is organized into two stages: an initial equal-curvature comparison between steel and CFRP beams to identify systematic strain transfer differences, followed by a second-stage investigation focusing on the influence of surface resin-rich layer thickness. The main contributions of this study are threefold. First, an equal-curvature-based experimental framework is developed to decouple global structural response from local strain transfer effects. Second, the influence of CFRP surface resin-rich layer thickness on strain transfer behavior is systematically investigated. Third, a practical strain correction strategy is proposed to improve the reliability of surface strain measurements in CFRP structures.
2. Experimental Methodology and Specimen Preparation
2.1. Equal-Curvature Bending Principle
When comparing surface strain measurements obtained from structures made of dissimilar materials, the loading strategy plays a decisive role in the physical consistency of the comparison [30]. For beam specimens with identical geometry but different elastic moduli, conventional comparison methods based on equal applied load or equal nominal stress inevitably lead to different global bending responses [31,32]. As a result, the curvature distribution and surface strain levels differ between specimens, making it difficult to distinguish the influence of global structural stiffness from local strain transfer behavior [33].
Under small-deformation linear elastic bending conditions, a deterministic geometric relationship exists between the axial surface strain and the local curvature of a beam. For specimens with identical cross-sectional geometry, the theoretical surface strain at a given location is uniquely determined by the local curvature, independent of the elastic modulus of the material [34]. Therefore, enforcing an equal-curvature condition at the strain measurement location provides a physically consistent basis for strain comparison between different materials, effectively eliminating the influence of global stiffness differences [35].
Based on this principle, an equal-curvature bending framework is adopted in the present study. During testing, the curvature at the strain gauge location is controlled indirectly by monitoring the free-end displacement of the equal-strength beam. By applying different load levels to steel and CFRP beams, identical curvature is achieved at the strain measurement location [36]. As a homogeneous and isotropic material, structural steel does not exhibit significant strain transfer attenuation between the internal material and the surface. Consequently, under equal-curvature conditions, the surface strain measured on the steel beam can be used as a practical comparative reference for evaluating the strain transfer behavior of surface-mounted strain gauges on CFRP beams [37,38]. From classical beam theory, the curvature at an arbitrary cross-section of an equal-strength beam under elastic bending can be expressed as
where denotes the bending moment at position , is the elastic modulus of the material, and is the second moment of area of the beam cross-section [39]. For beams with identical geometric dimensions and subjected to the same loading configuration, the surface strain at a given location is uniquely determined by the local curvature. Therefore, when specimens made of different materials exhibit the same curvature at the strain measurement location, their theoretical surface strains should be identical [32,33]. This physical relationship provides the theoretical foundation for comparing surface strain measurements under equal-curvature conditions. Considering a steel beam and a CFRP beam with the same geometry, the equal-curvature condition at the strain gauge location can be written as
Under identical loading configurations, the bending moments at the measurement location are given by and , where is the applied load and is the beam length. Substituting these expressions into the equal-curvature condition yields
Using the elastic modulus of structural steel () and the equivalent longitudinal elastic modulus of the CFRP beam (), the theoretical load ratio is approximately 2.9. This relationship provides the basis for load matching in both the numerical simulations and the experimental tests, thereby ensuring that the steel and CFRP beams experience the same bending curvature at the strain measurement location. A schematic illustration of the equal-curvature bending concept is provided in Figure 1.
Figure 1.
Schematic illustration of steel and CFRP beams under equal-curvature bending conditions. The principal fiber direction (0° direction) of the CFRP laminate is aligned with the beam axis, consistent with the experimental configuration and finite element model.
2.2. Specimen Preparation and Resin-Rich Layer Thickness Control
The CFRP specimens used in this study were laminate plates with a 0°/90° stacking sequence. CFRP components manufactured by autoclave curing and related composite processing techniques commonly exhibit a resin-rich layer. This layer is formed by resin flow, fiber distribution, and tooling effects during fabrication, and is dominated by polymer matrix material with an elastic modulus substantially lower than that of the underlying fiber-reinforced laminate. In surface strain measurements, deformation in the load-bearing fiber layers must be transferred sequentially through this resin-rich layer and the adhesive layer before reaching the surface-mounted strain gauge, as schematically illustrated in Figure 2a. Owing to its relatively low stiffness, the resin-rich layer is expected to play a significant role in strain attenuation along the transfer path.
Figure 2.
Schematic illustration, microstructural characterization, and thickness abstraction of the surface resin-rich layer in CFRP specimens: (a) Schematic illustration of the strain transfer path through the adhesive layer and resin-rich layer; (b) Cross-sectional micrograph showing the resin-rich layer and its interface with the fiber-reinforced laminate (scale bar: 200 μm); (c) Representative surface morphologies of CFRP specimens under different surface treatment conditions (scale bar: 1 mm); (d) Conceptual abstraction of resin-rich layer thickness corresponding to different surface treatment states.
To characterize the surface structure of the CFRP specimens and to quantify the thickness scale of the resin-rich layer, cross-sectional microscopic observations were performed on the as-received specimens. As shown in Figure 2b, a distinct resin-rich layer can be clearly identified above the fiber-reinforced laminate. Although local thickness variations are observed along the specimen surface, the average thickness of the resin-rich layer is approximately 0.25 mm. This observation provides a quantitative basis for defining the initial surface condition and for designing a controlled thickness variation strategy.
Based on the microscopic characterization, controlled surface grinding was employed to systematically adjust the thickness of the resin-rich layer. Four representative surface conditions were prepared: an as-received surface with the resin-rich layer fully retained (h ≈ 0.25 mm), a lightly polished surface (h ≈ 0.20 mm), a moderately polished surface (h ≈ 0.10 mm), and a fully polished surface in which the fiber layer is exposed (h ≈ 0). Representative surface morphologies corresponding to these conditions are presented in Figure 2c. Through this procedure, the thickness of the resin-rich layer is effectively transformed into a continuous and controllable experimental variable. In addition, the characteristic surface waviness observed in Figure 2c is much smaller than the effective gauge length of the strain gauge (2.8 mm), indicating that the measured strain represents an averaged response over local surface undulations rather than a pointwise fluctuation.
For subsequent analysis, the resin-rich layer thickness is abstracted as a single scalar parameter h, as schematically illustrated in Figure 2d. The fiber-exposed surface condition (h ≈ 0) is treated as a reference state corresponding to minimal strain transfer attenuation. It is acknowledged that a thin residual resin film or surface roughness may still exist after polishing; however, compared with the as-received condition, the contribution of the resin-rich layer is significantly reduced. Since the present study focuses on the relative variation in strain transfer efficiency with surface layer thickness, this state is used as a practical normalization baseline within the present experimental framework, rather than as an absolute theoretical strain-transfer limit.
To ensure consistency between experimental investigations and numerical simulations, the resin-rich layer is modeled as an independent material layer with assigned elastic properties. Based on material specifications and relevant literature, the elastic modulus and Poisson’s ratio of the resin-rich layer are taken as 2.8 GPa and 0.35, respectively. The corresponding material parameters are summarized in Table 1 and are used consistently in the finite element analyses described in the following sections.
Table 1.
Material parameters of the resin-rich layer.
2.3. Finite Element Model and Verification Strategy
To verify the load-matching relationship derived from the theoretical analysis and to provide numerical support for subsequent strain comparison experiments under equal-curvature conditions, finite element models of a steel beam and a CFRP beam were established [40]. The geometric dimensions of both beams were identical to those of the experimental specimens. As shown in Figure 3a, the equal-strength beam configuration adopted in this study had a length of 340 mm, a total thickness of 3 mm (including the surface resin-rich layer), a width of 40 mm at the clamping end, and a width of 10 mm at the free end. One end of the beam was fixed, while a vertical concentrated load was applied at the free end.
Figure 3.
Experimental configuration and corresponding finite element model of the equal-strength beam used for the equal-curvature bending analysis: (a) photograph of the equal-strength beam test setup; (b) finite element model employed for equal-curvature analysis.
During the finite element modeling process, the region corresponding to the strain gauge location, as indicated in Figure 3b, was treated as the area of primary interest and locally refined to improve the accuracy of surface strain calculation [41]. The geometry of the strain gauge was modeled strictly according to the electrical resistance strain gauge used in the experiments (model BE120-3AA), with a sensitive grid size of 2.8 mm × 2.0 mm and a backing size of 6.4 mm × 3.5 mm. The remaining regions of the beam were meshed using a relatively uniform element size to balance computational accuracy and efficiency.
The material parameters adopted in the finite element models are summarized in Table 2. The steel beam was modeled as a linear elastic, isotropic material. For the CFRP beam, an equivalent longitudinal elastic modulus was used to represent its mechanical behavior in the primary load-bearing direction, with the fiber orientation aligned with the beam axis. The CFRP specimens used in this study were prepared from a 0°/90° laminate, with the principal fiber direction aligned with the beam axis. The geometric parameters listed in Table 2 were taken from the actual specimen dimensions used in the experiments. For the beam-level equal-curvature analysis and the corresponding finite element comparison, an equivalent longitudinal modulus of 72 GPa was adopted to represent the dominant bending response of the CFRP beam along the primary load-bearing direction. In addition, the basic mechanical properties of the CFRP plate were referenced from a third-party test report supplied with the material, in which tensile and flexural tests were conducted according to GB/T 1447-2005 [42] and GB/T 1449-2005 [43], respectively. In other words, the present study distinguishes between beam-level equal-curvature verification, which is governed primarily by the dominant longitudinal bending stiffness, and local strain-transfer interpretation, which is discussed in a mechanistic rather than fully constitutive orthotropic sense.
Table 2.
Geometrical and material parameters of steel and CFRP beams used in experiments and finite element models.
2.4. Experimental Setup and Instrumentation
To experimentally implement the equal-curvature bending framework, a dedicated equal-strength beam test system was established, as shown in Figure 4. The system consists of a mechanical loading device, a surface strain measurement system, and a displacement measurement unit, enabling synchronized acquisition of load, displacement, and strain data during testing.
Figure 4.
Experimental setup and key components for equal-curvature bending tests: (a) overall experimental setup and strain acquisition system; (b) laser displacement sensor; (c) equal-strength beam under equal-curvature loading condition.
As illustrated in Figure 4a, the specimen was configured as an equal-strength beam with one end rigidly fixed and the other subjected to a vertical concentrated load. Surface strain was measured using bonded electrical resistance strain gauges (model BE120-3AA—AVIC Electromechanical Measurement Instruments Co., Ltd., Hanzhong, China), which were installed at the designated measurement location on the beam surface following standard surface preparation and bonding procedures. The strain signals were recorded using a YE2539 high-speed static strain acquisition system (Jiangsu Lianneng Electronic Technology Co., Ltd., Yangzhou, China).
To monitor the global bending response and to facilitate implementation of the equal-curvature condition, a laser displacement sensor (Robert Bosch Power Tools GmbH, Leinfelden-Echterdingen, Germany) was installed at the free end of the beam, as shown in Figure 4b. The displacement measurement was conducted in real time throughout the loading process. During testing, the applied load was adjusted based on the measured free-end displacement, such that steel and CFRP beams exhibited matched displacement responses under different load levels.
By using free-end displacement as a feedback control parameter, the curvature at the strain gauge location could be indirectly regulated. Under the assumption of linear elastic bending and identical beam geometry, matching the free-end displacement provides a practical means to achieve comparable curvature at the strain measurement location for specimens made of different materials. A representative experimental configuration under equal-curvature loading is shown in Figure 4c.
The applied load was increased incrementally within the elastic range of the specimens, and the corresponding strain and displacement data were recorded simultaneously. The strain signals were acquired using a YE2539 high-speed static strain acquisition system. According to the manufacturer’s specifications, the system provides a measurement accuracy of ±0.3% FS ± 2 με and a resolution of 1 με. Prior to formal testing, zero balancing and channel calibration were performed to reduce instrumental drift and improve measurement consistency. All tests were conducted under ambient laboratory conditions.
For each loading condition, three repeated measurements were performed, and the reported results are expressed as mean ± standard deviation (SD) to characterize the repeatability and scatter of the experimental data. For each condition, , corresponding to three repeated loading tests performed on the same specimen under identical instrumentation and loading procedures.
It should be noted that the present study does not assume the absolute uncertainty of an individual strain reading to be negligible. Instead, the analysis is based on comparative measurements conducted under the same sensing chain. Since the steel and CFRP beams were tested using the same strain gauge type, bonding procedure, acquisition system, and displacement-based loading strategy, the common systematic uncertainty associated with the measurement chain was largely shared by both specimens. Therefore, the persistent difference between the steel and CFRP strain responses under equal-curvature conditions is more reasonably attributed to a material-related strain transfer effect than to random measurement fluctuations alone.
3. Results and Discussion
3.1. Verification of the Equal-Curvature Framework
The effectiveness of the proposed equal-curvature bending framework was first verified through a combined analysis of numerical simulations and experimental displacement measurements. Since curvature at the strain gauge location cannot be measured directly, the free-end displacement of the equal-strength beam was adopted as an indirect but practical indicator of global bending curvature under linear elastic conditions.
Based on the theoretical load-matching relationship, vertical concentrated loads of 5, 10, 15, and 20 N were applied to the CFRP beam. Correspondingly, loads of 15, 29, 44, and 58 N were applied to the steel beam. Finite element simulations were performed under these matched load cases, and the resulting displacement contour plots are presented in Figure 5 for the CFRP beam and Figure 6 for the steel beam. The numerical results show that, under the matched loading conditions, the overall deflection profiles of the two beams are smooth and comparable, indicating consistent bending behavior.
Figure 5.
Displacement contours of the CFRP beam under applied loads of (a) 5 N, (b) 10 N, (c) 15 N, and (d) 20 N.
Figure 6.
Displacement contours of the steel beam under applied loads of (a) 15 N, (b) 29 N, (c) 44 N, and (d) 58 N.
Experimental free-end displacement responses of the steel and CFRP beams under the matched load cases are summarized in Figure 7a. The displacement–load curves of the two beams exhibit highly consistent trends over the entire loading range, demonstrating that comparable global bending deformation was achieved despite the significant difference in elastic modulus between the two materials. To further quantify the deformation consistency, the displacement mismatch between the steel and CFRP beams was calculated and is shown in Figure 7b. The results indicate that the displacement difference remains within ±1 mm for all loading cases and does not increase systematically with load level.
Figure 7.
Verification of equal-curvature loading condition: (a) free-end displacement–load responses of the steel and CFRP beams under matched load cases; (b) displacement mismatch between the two beams.
The combined numerical and experimental displacement analyses confirm that the load-matching strategy based on the equal-curvature principle is effective in practice. Under the matched loading conditions, the steel and CFRP beams exhibit comparable bending curvature at the strain measurement location, thereby minimizing the influence of global structural stiffness differences. This verification provides a reliable foundation for subsequent comparisons of surface strain measurements and for isolation of strain transfer effects in CFRP beams under equal-curvature conditions.
3.2. Identification of Systematic Strain Transfer Differences
With the effectiveness of the equal-curvature framework verified, surface strain responses of the steel beam and the unpolished CFRP beam were compared under equal-curvature conditions. The measured strain results corresponding to different matched load cases are statistically summarized in Table 3 and illustrated in Figure 8, where each value is presented as the mean ± standard deviation (SD) obtained from three repeated measurements.
Table 3.
Statistical strain test results of steel and CFRP beams under equal-curvature conditions.
Figure 8.
Comparison of measured surface strains of steel and CFRP beams under equal-curvature conditions. Data are presented as mean ± standard deviation from three repeated measurements.
For all loading conditions considered, the surface-mounted strain gauges on the CFRP beam consistently yielded strain readings lower than those measured on the steel beam under identical curvature conditions. Specifically, the steel beam exhibited surface strains of approximately 305, 641, 897, and 1251 με at increasing displacement levels, whereas the corresponding CFRP surface strains were approximately 295, 619, 860, and 1227 με. The associated standard deviations remained relatively small compared with the difference between the two material systems, indicating good repeatability of the measurements. Since the two beams experienced comparable bending curvature at the strain measurement location and were tested using the same measurement chain, the observed strain difference cannot be attributed to differences in global structural stiffness or to random measurement scatter alone.
It should be emphasized that the present conclusion is not based on a single absolute strain reading from the CFRP specimen. Instead, it is derived from a comparative equal-curvature framework in which the steel beam serves as a reference specimen tested under the same sensing and acquisition conditions. Under this framework, the common systematic deviation of the strain gauge and acquisition system is largely suppressed in the comparison, whereas the remaining stable discrepancy reflects the difference in the strain transfer path at the CFRP surface.
Notably, the magnitude of the strain difference remains relatively stable across the investigated curvature range. Although the absolute strain level increases with load, the relative discrepancy between steel and CFRP measurements does not show a clear dependence on displacement or curvature magnitude. This behavior, together with the limited scatter observed in the repeated measurements, indicates that the strain deficit in the CFRP measurements represents a stable and systematic effect rather than random experimental scatter.
To quantitatively characterize the strain underestimation observed in the CFRP beam, a strain transfer coefficient η was calculated, defined as the ratio of the strain measured on the CFRP beam to that measured on the steel beam under equal-curvature conditions. The calculated strain transfer coefficients for the four loading cases are listed in Table 4. The values of η are 0.967, 0.966, 0.959, and 0.981, with an average value of approximately 0.968.
Table 4.
Strain transfer coefficient of CFRP beams under equal-curvature conditions.
The limited variation in η across different loading conditions indicates that the strain transfer coefficient is largely insensitive to strain amplitude within the tested range. This stability confirms that the approximately 3% strain underestimation observed on the unpolished CFRP surface is a repeatable and systematic measurement bias rather than an artifact of measurement noise, load fluctuation, or short-term environmental effects. The identification of this stable strain transfer difference provides a quantitative basis for subsequent investigation of its physical origin.
3.3. Mechanistic Influence of Resin-Rich Layer Thickness on Strain Transfer
Following the identification of systematic strain underestimation in CFRP surface measurements under equal-curvature conditions, the underlying physical mechanism is further investigated through a combined finite element and experimental analysis. Particular attention is paid to the role of the resin-rich layer, which is hypothesized to govern strain attenuation along the strain transfer path.
To provide mechanistic insight, finite element simulations were first conducted to compare the equivalent elastic strain distributions in the strain gauge region of steel and CFRP beams under equal-curvature loading conditions. Figure 9 presents the strain fields for the steel beam and the unpolished CFRP beam under matched low- and high-load cases. Although the global bending responses of the two beams are comparable, the strain distributions within the strain gauge bonding region exhibit clear differences. In the CFRP beam, the peak strain transmitted to the surface-mounted strain gauge is consistently lower than that observed in the steel beam, indicating strain attenuation prior to reaching the sensor.
Figure 9.
Comparison of equivalent elastic strain distributions in strain gauge regions of steel and CFRP beams under equal-curvature conditions: (a) Steel beam under a load of 15 N; (b) CFRP beam under a load of 5 N (equal-curvature condition); (c) Steel beam under a load of 58 N; (d) CFRP beam under a load of 20 N (equal-curvature condition).
This attenuation behavior can be attributed to the presence of the low-modulus resin-rich layer in CFRP. During bending, strain generated in the fiber-reinforced laminate must be transferred through the resin-rich layer before reaching the adhesive layer and the strain gauge. Owing to its significantly lower elastic modulus, the resin-rich layer undergoes pronounced tensile and shear deformation, thereby absorbing part of the strain and reducing the effective strain transmitted to the sensor. The finite element results in Figure 9 therefore provide numerical evidence that the surface structural characteristics of CFRP play a critical role in strain transfer behavior, even when global curvature is identical.
To further isolate and quantify the influence of resin-rich layer thickness, additional finite element models were established in which the thickness of the resin-rich layer was systematically varied while all other parameters remained unchanged. Figure 10 shows the equivalent elastic strain distributions in the strain-gauge region for representative resin-rich-layer thicknesses corresponding to the four surface conditions. For descriptive convenience, the nominal thickness levels are referred to as 0, 0.10, 0.20, and 0.25 mm, whereas the representative measured values used in the quantitative analysis are 0, 0.104, 0.212, and 0.250 mm. The simulation results reveal a clear monotonic trend: as the resin-rich layer thickness increases, the strain transmitted to the surface-mounted gauge progressively decreases. When the resin-rich layer thickness approaches zero, corresponding to direct bonding of the strain gauge to the fiber-reinforced laminate through the adhesive layer, the strain transfer efficiency is maximized and approaches that of the steel reference case. Figure 10 is intended to visualize the local strain-transfer trend in the strain-gauge region, whereas the quantitative relationship between resin-rich-layer thickness and measured strain is summarized in Table 5 and Figure 11.
Figure 10.
Finite element strain distributions in the strain-gauge region for different resin-rich-layer thicknesses: (a) h = 0.250 mm (as-received); (b) h = 0.212 mm (lightly polished); (c) h = 0.104 mm (moderately polished); (d) h ≈ 0 mm (fiber-exposed).
Table 5.
Statistical strain test results of CFRP beams with different resin-rich-layer thicknesses.
Figure 11.
Measured surface strains of CFRP beams with different resin-rich-layer thicknesses under different loads. Data are presented as mean ± standard deviation from three repeated measurements.
The numerical predictions are further corroborated by experimental measurements obtained from CFRP specimens with controlled surface treatment. Table 5 and Figure 11 summarize the statistically measured surface strain responses of CFRP beams with different resin-rich layer thicknesses under equal-curvature bending conditions. All values are reported as mean ± standard deviation (SD) based on three repeated measurements for each loading condition. For all load levels considered, specimens with thinner resin-rich layers consistently exhibit higher measured strain values. The fiber-exposed surface condition yields the highest strain response, whereas the as-received surface condition yields the lowest. The standard deviations remain relatively small compared with the differences among the four surface conditions, indicating that the observed trend is stable and repeatable. This demonstrates that the influence of resin-rich layer thickness on strain transfer behavior is systematic rather than an artifact of measurement scatter.
Taken together, the finite element simulations and experimental observations establish that the resin-rich layer acts as a compliant intermediate layer along the strain transfer path. Increasing its thickness enhances strain attenuation through additional tensile and shear deformation, whereas reducing or removing the resin-rich layer shortens the transfer path and improves strain transmission. These results demonstrate that the thickness of the resin-rich layer is the dominant factor governing strain transfer efficiency in CFRP surface strain measurements under equal-curvature conditions.
3.4. Strain Correction Model and Engineering Guidance
Based on the systematic experimental observations and the mechanistic analysis, a practical empirical strain-correction relationship is established to compensate for strain transfer attenuation induced by the resin-rich layer in CFRP structures. The relationship aims to provide an engineering-oriented correction for the present laminate system and thickness range, rather than a full constitutive description of interfacial strain transfer in orthotropic composites.
To quantify the relationship between strain transfer efficiency and resin-rich-layer thickness, the fiber-exposed surface condition (h ≈ 0) is adopted as a relative reference state corresponding to the minimum resin-rich-layer-induced attenuation within the present experimental framework. It should be noted that this state does not represent an absolute theoretical strain-transfer limit because the adhesive layer and the strain-gauge backing are still present. Instead, it serves as the most appropriate practical reference among the tested surface conditions for evaluating the relative influence of the resin-rich layer thickness. Therefore, the coefficient defined in this section should be interpreted as a comparative experimental index for normalization within the present test series, rather than as an absolute interfacial transfer coefficient.
In the present study, the equal-curvature framework provides the mechanical basis for comparing the nominal strain state among different specimens, while the fiber-exposed condition is used only as an experimental reference for relative correction within the tested surface-treatment series. The corresponding reference strain at the same load level is denoted as . The relative strain transfer coefficient for a resin-rich layer thickness under an applied load is defined as:
Here, denotes the strain measured by the surface-mounted strain gauge for the surface condition with resin-rich-layer thickness under the applied load level .
The coefficient was calculated at each load level, and the average value over the load range of 10–40 N was taken as the mean coefficient for each thickness condition. As summarized in Table 6, the mean relative strain transfer coefficient decreases monotonically with increasing resin-rich-layer thickness. For the as-received surface condition, the average coefficient is approximately 0.967, which agrees well with the first-stage steel–CFRP comparison result (approximately 0.96–0.98). This consistency further supports the interpretation that the strain underestimation observed in the first-stage experiments is primarily associated with the surface resin-rich layer.
Table 6.
Relative strain transfer coefficients normalized to the fiber-exposed condition.
Within the thickness range of 0–0.25 mm, linear regression was performed on the four data points listed in Table 6. The relationship between the mean relative strain transfer coefficient and the resin-rich-layer thickness can be expressed empirically as
The corresponding coefficient of determination is .
In engineering applications, once the thickness of the surface resin-rich layer h of a CFRP component is estimated through microscopic observation or inferred from manufacturing parameters, the strain gauge readings can be corrected using the above strain transfer coefficient. For a given load level, the corrected strain can be expressed as:
where denotes the strain corrected using the proposed empirical relationship at the applied load level , is the strain directly measured by the surface-mounted strain gauge, is the mean relative strain transfer coefficient corresponding to the resin-rich-layer thickness , and is the thickness of the surface resin-rich layer.
When m, the corresponding strain-transfer loss remains within approximately 1.5%, and the correction may be omitted depending on the required accuracy. However, when the resin-rich-layer thickness approaches 0.25 mm, the strain underestimation can exceed 3%. The proposed linear relationship should be regarded as a first-order empirical approximation that is only valid within the tested thickness range of 0–0.25 mm. Although non-linear shear-lag-type behavior may arise over a wider thickness range or in different interfacial systems, the present first-order approximation is sufficient to capture the monotonic trend observed in the current experiments within the investigated thickness interval. The relationship is not extrapolated beyond the investigated thickness interval, and its applicability should be re-evaluated when the material system, sensor type, or loading condition differs significantly from those considered here.
3.5. Comprehensive Discussion
When comparing surface strain measurements obtained from structural components made of different materials, the loading strategy plays a critical role in ensuring the reliability of the comparison. In this study, an equal-curvature loading method was adopted and rigorously validated through theoretical analysis, finite element simulations, and displacement measurements, thereby eliminating the influence of material stiffness differences on global structural response. This approach enables a physically consistent comparison of surface strain measurements between steel and CFRP beams, allowing the observed strain discrepancies to be attributed to strain transfer effects rather than to differences in overall bending behavior.
Under equal-curvature conditions, the surface-mounted strain gauges on unpolished CFRP beams consistently yielded lower strain readings than those on steel beams, with an average strain transfer coefficient of approximately 0.968. This strain underestimation remained stable across different load and curvature levels, indicating a repeatable and systematic effect rather than random measurement error. Microscopic observations and numerical analysis demonstrate that this behavior is primarily associated with the presence of a low-modulus resin-rich layer in CFRP, which participates in deformation along the strain transfer path and leads to partial strain attenuation before the strain reaches the surface-mounted gauge. Although the total beam thickness reported in this study includes the surface resin-rich layer, its influence on the overall bending stiffness is limited, whereas its influence on local surface strain transfer is much more pronounced. Because the steel and CFRP specimens were measured using the same strain gauge type, bonding method, and acquisition chain, the common uncertainty of the measurement system was largely shared in the comparison. Therefore, the persistent discrepancy observed under equal-curvature conditions is more reasonably interpreted as a material-related strain transfer effect associated with the CFRP surface structure.
By systematically controlling the thickness of the resin-rich layer through surface polishing, the present study further reveals that strain transfer efficiency increases monotonically as the resin-rich layer thickness decreases, approaching unity when the resin-rich layer is fully removed and the fiber layer is exposed. The experimentally observed trends are in good qualitative agreement with finite element predictions, even though the numerical results are not intended to provide precise quantitative fits. This consistency in trend is sufficient to support the proposed mechanistic interpretation, given the inherent complexity of CFRP surface structures and interfacial conditions.
The present analysis adopts a beam-level equivalent longitudinal modulus to describe the dominant bending response of the CFRP laminate along the primary load-bearing direction. In other words, the present study distinguishes between beam-level equal-curvature verification, which is governed primarily by the dominant longitudinal bending stiffness, and local strain-transfer interpretation, which is discussed in a mechanistic rather than fully constitutive orthotropic sense. This treatment is appropriate for the equal-curvature comparison performed in this study, because the main objective is to evaluate the macroscopic trend of surface strain transfer rather than to resolve the full orthotropic stress redistribution within the laminate. It is acknowledged that local strain transfer in CFRP may also be influenced by the orthotropic substrate behavior, Poisson coupling, and the detailed interfacial shear-lag mechanism. However, within the present experimental configuration and thickness range, these factors do not alter the observed monotonic dependence of strain transfer efficiency on the resin-rich-layer thickness.
Based on the experimental data, a first-order strain correction model linking resin-rich layer thickness to strain transfer coefficient was established, providing a practical means to compensate for systematic strain underestimation in CFRP surface strain measurements. While the proposed model is specific to the material system, sensor type, and loading conditions investigated herein, it offers a straightforward engineering approach for improving measurement accuracy when the surface resin-rich layer thickness can be reasonably estimated. Under conditions involving different interface properties, environmental effects, or complex multiaxial loading, further validation is required.
Overall, this work complements existing strain transfer studies that primarily focus on adhesive layers and bonding characteristics by highlighting the previously underexplored role of the CFRP surface resin-rich layer. The findings provide experimental insight into the origin of systematic strain measurement bias in CFRP structures and offer practical guidance for improving surface strain measurement techniques in composite engineering applications.
Several limitations should be acknowledged. The present study focuses on quasi-static bending and a specific strain-gauge configuration, and the proposed empirical correction was only derived within a limited resin-rich-layer thickness range. Further validation under cyclic or dynamic loading, and for different CFRP manufacturing routes, adhesive systems, and sensor configurations, is required before broader generalization.
Nevertheless, the equal-curvature framework proposed in this study provides a robust methodology for isolating strain transfer effects from global structural response. This approach can potentially be extended to other composite sensing configurations, including fiber optic sensors and distributed sensing systems. Therefore, the present findings not only clarify the origin of strain underestimation in CFRP surface measurements but also provide a methodological reference for improving measurement reliability in composite structures.
4. Conclusions
This study investigated the strain transfer behavior of surface-mounted strain gauges on CFRP beams under equal-curvature bending, with particular emphasis on the influence of the surface resin-rich layer. The main conclusions are as follows:
- An equal-curvature bending method was established as a physically consistent framework for strain comparison between dissimilar materials. Theoretical derivation, finite element analysis, and displacement-controlled experiments demonstrated that enforcing identical curvature at the strain gauge location effectively eliminates the influence of elastic modulus and global bending stiffness differences. Under equal-curvature conditions, any measured strain discrepancy between steel and CFRP beams can be directly attributed to differences in surface structure and strain transfer paths, rather than to global deformation inconsistency.
- Surface-mounted strain gauges on CFRP beams exhibit systematic strain underestimation under equal-curvature conditions. Experimental results showed that, compared with structural steel beams, unpolished CFRP beams consistently produced lower surface strain readings, with an average strain transfer coefficient of approximately 0.96–0.98. This strain deficit remained stable across different curvature levels, indicating that the observed discrepancy is a systematic measurement bias rather than random experimental error.
- The surface resin-rich layer was identified as the dominant factor governing strain transfer efficiency in CFRP surface measurements. Microscopic observations and finite element analyses revealed the presence of a low-modulus resin-rich layer on CFRP components. This compliant layer attenuates strain transmission from the fiber-reinforced laminate to the surface-mounted sensor. By progressively reducing the resin-rich layer thickness through controlled surface polishing, a monotonic increase in strain transfer efficiency was observed, approaching unity when the fiber layer was fully exposed.
- A first-order empirical relationship between resin-rich-layer thickness and strain transfer efficiency was established within the tested thickness range of 0–0.25 mm, providing practical guidance for correcting systematic strain underestimation in CFRP surface measurements. When the surface resin-rich-layer thickness is small (e.g., ≤0.10 mm), the strain-transfer loss remains within approximately 1–2% and may be neglected depending on accuracy requirements. For thicker resin-rich layers, where the strain underestimation exceeds 3%, either surface treatment or strain correction using the proposed relationship is recommended
Author Contributions
Conceptualization, J.X. and J.G.; methodology, J.X.; software, J.G.; validation, Y.W. and J.G.; formal analysis, J.X.; investigation, J.G.; resources, Y.W.; data curation, J.G.; writing—original draft preparation, J.X.; writing—review and editing, Y.W.; visualization, J.G.; supervision, Y.W.; project administration, J.X.; funding acquisition, Y.W. All authors have read and agreed to the published version of the manuscript.
Funding
This research received no external funding.
Institutional Review Board Statement
Not applicable.
Informed Consent Statement
Not applicable.
Data Availability Statement
This is a project collaboration with Beijing Institute of Aeronautical Materials. The data involved is confidential and has not been made public.
Acknowledgments
The first author gratefully acknowledges the guidance and support provided by Junjie Gong and Yuanyuan Wei throughout this research. The authors also appreciate the assistance from members of the laboratory at the School of Mechanical Engineering, Yangzhou University, in the experimental work. In addition, the authors thank researchers Xinwen Chen and Yaowei Tian from Beijing Institute of Aeronautical Materials for their valuable technical support and cooperation.
Conflicts of Interest
The authors declare no conflicts of interest.
Abbreviation
The following abbreviation is used in this manuscript:
| CFRP | Carbon fiber-reinforced polymer |
References
- Zhao, Y.; Liu, Y.; Li, Y.; Hao, Q. Development and application of resistance strain force sensors: A review. Sensors 2020, 20, 5826. [Google Scholar] [CrossRef] [Scilit]
- Li, Y.; Wang, Z.; Xiao, C.; Zhao, Y.; Zhu, Y.; Zhou, Z. Strain transfer characteristics of resistance strain-type transducer using elastic-mechanical shear lag theory. Sensors 2018, 18, 2420. [Google Scholar] [CrossRef] [Scilit]
- Wang, Z.; Li, H.; Zhang, L.; Xue, J. Strain transfer characteristic of a fiber Bragg grating sensor bonded to the surface of carbon fiber reinforced polymer laminates. Appl. Sci. 2018, 8, 1171. [Google Scholar] [CrossRef] [Scilit]
- Wang, H.; Dai, J.-G. Strain transfer analysis of fiber Bragg grating sensor assembled composite structures subjected to thermal loading. Compos. Part B Eng. 2019, 162, 303–313. [Google Scholar] [CrossRef] [Scilit]
- Seo, S.-Y.; Park, J.-H.; Yun, H.-D.; Kim, K.-S.; Lee, G.-C.; Hong, S. Strain transfer of fiber bragg grating sensor externally bonded to FRP strip for structural monitoring after reinforcement. Materials 2021, 14, 4382. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Liang, M.; Chen, N.; Fang, X.; Wu, G. Strain transferring mechanism analysis of the surface-bonded FBG sensor. Appl. Opt. 2018, 57, 5837–5843. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ahmadian, H.; Yang, M.; Soghrati, S. Effect of resin-rich zones on the failure response of carbon fiber reinforced polymers. Int. J. Solids Struct. 2020, 188–189, 74–87. [Google Scholar] [CrossRef] [Scilit]
- Mahmood, A.S.; Summerscales, J.; James, M.N. Resin-rich volumes (RRV) and the performance of fibre-reinforced composites: A review. J. Compos. Sci. 2022, 6, 53. [Google Scholar] [CrossRef] [Scilit]
- Jiménez-Fortunato, I.; Bull, D.J.; Thomsen, O.T.; Dulieu-Barton, J.M. On the source of the thermoelastic response from orthotropic fibre reinforced composite laminates. Compos. Part A Appl. Sci. Manuf. 2021, 149, 106515. [Google Scholar] [CrossRef] [Scilit]
- Pitarresi, G.; Found, M.S.; Patterson, E.A. An investigation of the influence of macroscopic heterogeneity on the thermoelastic response of fibre reinforced plastics. Compos. Sci. Technol. 2005, 65, 269–280. [Google Scholar] [CrossRef] [Scilit]
- Geng, X.; Jiang, M.; Gao, L.; Wang, Q.; Jia, Y.; Sui, Q.; Jia, L.; Li, D. Sensing characteristics of FBG sensor embedded in CFRP laminate. Measurement 2017, 98, 199–204. [Google Scholar] [CrossRef] [Scilit]
- Di Sante, R. Fibre optic sensors for structural health monitoring of aircraft composite structures: Recent advances and applications. Sensors 2015, 15, 18666–18713. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Luyckx, G.; Voet, E.; Lammens, N.; Degrieck, J. Strain measurements of composite laminates with embedded fibre Bragg gratings: Criticism and opportunities for research. Sensors 2011, 11, 384–408. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Valença, J.; Mukhandi, H.; Araújo, A.G.; Couceiro, M.S.; Júlio, E. Benchmarking for strain evaluation in CFRP laminates using computer vision: Machine learning versus deep learning. Materials 2022, 15, 6310. [Google Scholar] [CrossRef] [Scilit]
- Weng, S.; Zhang, J.; Yan, Z.; Gao, K.; Chen, Z.; Wu, L.Y. Improved strain transfer model for flexible sensors based on non-uniform distribution of shear stress in each layer. Measurement 2024, 227, 114288. [Google Scholar] [CrossRef] [Scilit]
- Hu, Y.; Li, Y.; Yan, D.; Jiao, Z.; Yuan, D.; Qin, C.; Li, Y. Strain transfer of fiber Bragg grating sensors in fiber-reinforced polymer composites with different fiber orientations and temperatures. Measurement 2024, 225, 114005. [Google Scholar] [CrossRef] [Scilit]
- Yang, H.; Huang, Y.; Zhou, Z.; Ou, J. Long-term performance of packaged fiber Bragg grating sensors for strain monitoring inside creep medium. Int. J. Smart Nano Mater. 2022, 13, 42–63. [Google Scholar] [CrossRef] [Scilit]
- Kabbara, M.; Chapeleau, X.; Zhang, Q.; Bourquin, F. Numerical evaluation of strain transfer model for steel-reinforced optical fiber cable embedded in a cylindrical concrete beam with two void inclusions. EPJ Web Conf. 2024, 305, 00021. [Google Scholar] [CrossRef] [Scilit]
- Ferrier, E.; Michel, L.; Thiele, M.; Mercier, J. Strain-rate effect on the bond strength of external bonded reinforced carbon fiber-reinforced polymer for concrete structure. Constr. Build. Mater. 2025, 466, 140216. [Google Scholar] [CrossRef] [Scilit]
- Kim, P.; Phillips, R.; Toll, S.; Månson, J.-A.E. The dimensional stability of composite laminates: Sensitivity to gradients in fibre content and misalignment. In International Workshop on Advanced Materials for High-precision Detectors; CERN: Geneva, Switzerland, 1994; pp. 123–131. [Google Scholar]
- Li, H.; Li, F.; Zhu, L. Effect of resin-missing defects on tensile behavior of carbon fiber/epoxy composites. Polymers 2024, 16, 348. [Google Scholar] [CrossRef] [Scilit]
- Růžek, R.; Kudrna, P.; Kadlec, M.; Karachalios, V.; Tserpes, K.I. Strain and damage monitoring in CFRP fuselage panels using fiber Bragg grating sensors. Part II: Mechanical testing and validation. Compos. Struct. 2024, 107, 737–744. [Google Scholar] [CrossRef] [Scilit]
- Du, W.; Zheng, X.; Shi, B.; Sun, M.; Wu, H.; Ni, W.; Zheng, Z.; Niu, M. Strain transfer mechanism in surface-bonded distributed fiber optic sensors under different strain fields. Sensors 2023, 23, 6863. [Google Scholar] [CrossRef] [Scilit]
- Copertaro, E. Assessment of resistive strain gauges measurement performances in experimental modal analysis and their application to the diagnostics of abrasive waterjet cutting machinery. Measurement 2022, 188, 110626. [Google Scholar] [CrossRef] [Scilit]
- Wang, Q.; Liu, R.; Yan, X. Measurement of strain distribution in CFRP cross-ply laminate material based on sampling moiré method. Chin. J. Aeronaut. 2024, 45, 430384. [Google Scholar]
- Boloux, A.; Burda, I.; Bisby, L.A.; Terrasi, G.P. Comparative study of strain measurement techniques for assessing creep in CFRP tendons. Sensors 2025, 25, 6897. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Hong, C.; Yuan, S.; Chen, W.; Chen, X.; Yu, J.; Chen, A. Fabrication and verification of vertical graphene-based strain sensor. Measurement 2023, 218, 113265. [Google Scholar] [CrossRef] [Scilit]
- Sutton, M.A.; Orteu, J.-J.; Schreier, H. Image Correlation for Shape, Motion and Deformation Measurements; Springer: Berlin/Heidelberg, Germany, 2009. [Google Scholar]
- Hu, X. Measurement errors caused by strain gauge stiffness and size effects and their correction. Mech. Eng. 2025, 47, 1187–1194. [Google Scholar]
- Pan, B.; Qian, K.; Xie, H.; Asundi, A. Two-dimensional digital image correlation for in-plane displacement and strain measurement: A review. Meas. Sci. Technol. 2009, 20, 062001. [Google Scholar] [CrossRef] [Scilit]
- Linghoff, D.; Al-Emrani, M.; Kliger, R. Performance of steel beams strengthened with CFRP laminate—Part 1: Laboratory tests. Compos. Part B Eng. 2010, 41, 509–515. [Google Scholar] [CrossRef] [Scilit]
- Teng, J.G.; Yu, T.; Fernando, D. Strengthening of steel structures with fiber-reinforced polymer composites. J. Constr. Steel Res. 2012, 78, 131–143. [Google Scholar] [CrossRef] [Scilit]
- Smith, S.T.; Teng, J.G. Interfacial stresses in plated beams. Eng. Struct. 2001, 23, 857–871. [Google Scholar] [CrossRef] [Scilit]
- Stratford, T.; Cadei, J. Elastic analysis of adhesion stresses for the design of a strengthening plate bonded to a beam. Constr. Build. Mater. 2006, 20, 34–45. [Google Scholar] [CrossRef] [Scilit]
- Deng, J.; Lee, M.M.K. Behaviour under static loading of metallic beams reinforced with a bonded CFRP plate. Compos. Struct. 2007, 78, 232–242. [Google Scholar] [CrossRef] [Scilit]
- Guo, D.; Wang, H.-P.; Liu, Y.-L.; Gao, W.-Y.; Dai, J.-G. Structural behavior of CFRP-strengthened steel beams at different service temperatures: Experimental study and FE modeling. Eng. Struct. 2023, 293, 116646. [Google Scholar] [CrossRef] [Scilit]
- Wang, H.-T.; Wu, G. Bond-slip models for CFRP plates externally bonded to steel substrates. Compos. Struct. 2018, 184, 1204–1214. [Google Scholar] [CrossRef] [Scilit]
- Teng, J.G.; Fernando, D.; Yu, T. Finite element modelling of debonding failures in steel beams flexurally strengthened with CFRP laminates. Eng. Struct. 2015, 86, 213–224. [Google Scholar] [CrossRef] [Scilit]
- Deng, J.; Lee, M.M.K.; Moy, S.S.J. Stress analysis of steel beams reinforced with a bonded CFRP plate. Compos. Struct. 2004, 65, 205–215. [Google Scholar] [CrossRef] [Scilit]
- Linghoff, D.; Haghani, R.; Al-Emrani, M. Carbon-fibre composites for strengthening steel structures. Thin-Walled Struct. 2009, 47, 1048–1058. [Google Scholar] [CrossRef] [Scilit]
- Weiland, J.; Sadeghi, M.Z.; Thomalla, J.V.; Schiebahn, A.; Schroeder, K.U.; Reisgen, U. Analysis of back-face strain measurement for adhesively bonded single lap joints using strain gauge, digital image correlation and finite element method. Int. J. Adhes. Adhes. 2020, 97, 102491. [Google Scholar] [CrossRef] [Scilit]
- GB/T 1447-2005; Fibre-Reinforced Plastic Composites—Determination of Tensile Properties. Standards Press of China: Beijing, China, 2005.
- GB/T 1449-2005; Fibre-Reinforced Plastic Composites—Determination of Flexural Properties. Standards Press of China: Beijing, China, 2005.
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.