Skip to Content
Applied SciencesApplied Sciences
  • Article
  • Open Access

25 November 2026

30 Pages

Impedance-Informed Battery Degradation Modeling for Sustainability Assessment: Reliability-Aware Screening Using Classical, Pseudo-FO, and Mittag–Leffler Models

,
and
1
Department of Environmental Engineering, Faculty of Engineering, Balıkesir University, Balıkesir 10145, Türkiye
2
Mechatronics Research Group, Faculty of Engineering and Physical Sciences, University of Southampton, Southampton SO17 1BJ, UK
3
Department of Electrical and Electronics Engineering, Faculty of Engineering, Balıkesir University, Balıkesir 10145, Türkiye
*
Author to whom correspondence should be addressed.

Abstract

Reliable lifetime estimates are essential when battery degradation models are used to calculate environmental indicators normalized by lifetime energy throughput. This study evaluates a cycle-only benchmark and three impedance-informed formulations (classical, pseudo-fractional-order, and Mittag–Leffler fractional-order) using causally matched discharge and EIS data from 12 NASA batteries. Under the 80/20 chronological hold-out, the best of the three impedance-informed formulations achieved lower SOH prediction RMSE than the cycle-only benchmark in 10 of 12 cells; however, this best-of-three comparison is descriptive because model ranking and evaluation used the same hold-out observations. To examine pre-EOL forecasting without future-data leakage through historical backtesting, eight pre-EOL landmark backtests were conducted across four batteries using truncated histories. The four models satisfied a 20% EOL-relative error tolerance in 2/8, 1/8, 4/8, and 5/8 cases, respectively, whereas the corresponding RUL-relative tolerance was satisfied in 0/8, 0/8, 3/8, and 3/8 cases. The five full-data Reliable Observed outcomes, therefore, represent retrospective EOL agreement rather than independently validated lifetime forecasts. The environmental findings should consequently be interpreted as screening-level, model-dependent energy-throughput scenarios rather than demonstrated emission reductions.

1. Introduction

Lithium-ion batteries (LIBs) are central to electric mobility, renewable-energy integration, portable electronics, and many other electrified systems. Their degradation affects not only operational reliability and remaining useful life (RUL), but also the useful energy delivered over the battery lifetime. When a manufacturing burden is normalized by lifetime energy throughput, uncertainty in battery lifetime propagates directly into the resulting environmental intensity [1,2,3]. A degradation model can, therefore, appear accurate over the measured region yet still bias a downstream sustainability indicator if its end-of-life (EOL) extrapolation is poor.
Battery aging is nonlinear, path-dependent, and influenced by electrochemical, thermal, and operational conditions. Empirical and polynomial models are attractive because they are computationally simple, while more flexible electrochemical and data-driven formulations can represent additional structure [1,4]. FO methods have also attracted attention because non-integer-order representations can describe distributed and non-exponential dynamic behavior [5,6,7,8,9]. However, additional flexibility does not guarantee improved future prediction. A fitted stretched/compressed exponential exponent is also not mathematically equivalent to a fractional differential equation. The present study, therefore, distinguishes an empirical pseudo-FO model from a Mittag–Leffler FO representation and avoids assigning a direct electrochemical memory interpretation to fitted order parameters.
Electrochemical impedance spectroscopy (EIS) offers complementary aging information. Parameters such as electrolyte resistance ( R e ) and charge-transfer resistance ( R c t ) have been used in battery diagnosis, state-of-health (SOH) estimation, and increasingly in real-time battery monitoring [10,11,12,13,14,15]. Because EIS measurements are not necessarily synchronized with discharge measurements and their sampling frequency varies across experimental groups, integrating impedance information into degradation modeling requires careful temporal alignment. A nearest-in-time rule may associate an earlier discharge with a later EIS measurement and thereby create look-ahead bias. A causal matching strategy is more appropriate when the objective is prediction.
Beyond causal alignment of discharge and impedance measurements, model evaluation introduces a second temporal challenge. In-sample RMSE, MAE, and R 2 describe agreement with fitted observations but do not establish prospective predictive performance. Random train–test splitting is problematic for battery-aging time series because it can mix earlier and later observations and thereby introduce temporal information leakage; time-wise validation using earlier cycles for training and later cycles for testing more closely reflects prospective deployment [16]. For impedance-informed models, future EIS must additionally be treated as unavailable during the test horizon; otherwise the validation procedure would rely on information that would not be available at the prediction time.
Recent studies have increasingly emphasized uncertainty and incomplete lifetime information rather than point prediction alone. Zou and Wen [17], for example, incorporated model and parameter uncertainty into probabilistic SOH estimation using Bayesian model averaging. In a complementary direction, Ly et al. [18] explicitly treated incomplete battery degradation trajectories as right-censored data and developed a probabilistic RUL prediction framework that retains information from such trajectories. More broadly, Liu et al. [19] identified limited data, heterogeneous operating conditions, feature acquisition, and deployment constraints as continuing challenges for data-driven battery lifetime prediction. Together, these studies advance uncertainty-aware battery prognostics and highlight the challenges associated with incomplete lifetime information, but they do not directly address whether a validation-selected degradation model can reliably support subsequent environmental interpretation.
These issues are especially important when degradation predictions are used in environmental analysis. Previous life-cycle studies have shown that battery lifetime and performance assumptions can materially affect energy-throughput-normalized environmental results [2,3]. In particular, when an upstream manufacturing burden is distributed over the energy delivered during battery life, the assumed lifetime directly affects the resulting impact intensity. Consequently, an error in predicted EOL is not merely a prognostic error; it can propagate into the environmental conclusion. A model that extrapolates to an unrealistically late EOL can generate an apparently favorable impact per kWh simply by increasing the modeled energy denominator, whereas a premature EOL can create the opposite effect. Reliability of the EOL estimate should, therefore, be evaluated separately from short-horizon SOH accuracy, while incomplete trajectories should be distinguished from experimentally observed EOL [17,18]. Experimental EOL itself also requires care because isolated low-capacity records or temporary recovery can make the first single threshold crossing unstable; trajectories that never show a persistent crossing should be treated as right-censored rather than as if the last measurement were true EOL.
Taken together, prior studies have addressed degradation prediction, lifetime uncertainty or censoring, and the environmental consequences of battery-lifetime assumptions, but less attention has been given to their interface. The present study, therefore, separates three questions: (i) whether impedance improves SOH prediction relative to a cycle-only benchmark; (ii) which impedance-informed formulation performs best under chronological validation and (iii) whether the selected model can reliably support environmental interpretation. The framework is evaluated using the heterogeneous NASA Battery Data Set [20], which provides chronologically recorded discharge and EIS measurements across heterogeneous aging conditions. This heterogeneity is used here as a demanding test of workflow robustness rather than as a set of identical experimental replicates.
The main contributions are as follows: (1) causal discharge–EIS matching and cleaning that prevent future impedance leakage; (2) chronological 80/20 hold-out validation with a cycle-only benchmark and frozen future impedance, supplemented by multi-origin temporal robustness analysis; (3) a persistent observed-EOL rule that distinguishes measured EOL from right-censored trajectories and (4) an EOL-reliability layer that classifies downstream environmental results as reliable observed comparisons, projections, unreliable extrapolations, or rejected outputs. An additional contribution is a retrospective pre-EOL landmark backtest that explicitly distinguishes full-data EOL agreement from truncated-history forecasting performance using both EOL-relative and RUL-relative errors. The central objective is, therefore, not to maximize an apparent environmental improvement, but to determine when a model-derived lifetime estimate is sufficiently credible to support sustainability interpretation.

2. Materials and Methods

2.1. NASA Battery Dataset Description

The experimental data were obtained from the NASA Prognostics Center of Excellence Battery Data Set, originally contributed by Saha and Goebel [20]. The repository contains lithium-ion cells cycled under different operating conditions using repeated charge, discharge, and EIS operations. Each MATLAB battery structure contains a chronological sequence of cycle records with operation type, ambient temperature, timestamp, and measurement data. Discharge records include terminal voltage, current, temperature, elapsed time, and measured capacity, whereas EIS records contain estimated R e and R c t values together with impedance-related quantities. EIS measurements were conducted as separate experimental operations rather than during dynamic discharge. However, the NASA documentation does not specify the resting conditions preceding each EIS measurement.
The NASA repository includes several experimental subsets rather than one homogeneous protocol applied to every cell. Temperatures, discharge thresholds, and the number and spacing of EIS observations differ among groups. This heterogeneity is useful for stress-testing a modeling workflow but means that the retained batteries should not be interpreted as homogeneous experimental replicates. The present analysis, therefore, treats each battery as an individual degradation trajectory and performs fitting, validation, EOL analysis, and energy extrapolation separately for each cell. Cross-cell comparisons are used to assess the robustness of the modeling strategy rather than to infer a single population-level degradation law.
The repository reports a nominal EOL criterion of 30% capacity fade, from 2 Ah to 1.4 Ah, for the battery-aging experiments [20]. The selected cells, however, span different experimental subsets and have substantially different first measured capacities. Accordingly, the study SOH is normalized to the first valid discharge capacity of each battery,
SOH ( k ) = Q ( k ) Q 0 ,
where Q ( k ) is measured discharge capacity at cycle k and Q 0 is the first valid measured capacity for that battery. A normalized threshold of SOH = 0.70 is then used consistently for model and experimental EOL analysis. This is a study-level normalized EOL definition and should not be interpreted as an assertion that every selected NASA test was physically terminated at exactly 1.4 Ah. Because Q 0 is the first valid measured capacity rather than a theoretical maximum capacity, the normalized SOH may temporarily exceed unity. For each battery b, a normalized SOH threshold τ corresponds to an absolute discharge-capacity threshold of Q EOL , b = τ Q 0 , b . Consequently, the common normalized threshold of 0.70 does not represent an identical absolute capacity across all cells, because the reference capacities differ among the experimental groups. Therefore, cross-battery comparisons are interpreted relative to each battery’s own initial capacity, rather than as comparisons at a common absolute capacity or identical operating conditions.

Raw Cycle Extraction and Delivered Energy

Charge, discharge, and impedance operations were extracted independently from the MATLAB structures while preserving both operation-specific indices and the original global cycle ordering. Malformed or incomplete cycle structures were logged rather than silently omitted. Here, malformed refers to cycle structures lacking the expected type or data fields, or producing an exception during extraction. Structurally unclassifiable records were not assigned a discharge index, while records removed during later cleaning leave gaps in the preserved physical discharge indices.
Delivered battery energy is not determined by nominal capacity alone and can vary with operating conditions; experimental storage-system studies have, for example, reported variations in available discharged energy with charge/discharge rate and operating configuration [21]. Therefore, the present study calculates discharge energy directly from the measured voltage and current trajectories. Instantaneous terminal power is formally given by p ( t ) = V ( t ) I ( t ) . In the discharge records analyzed here, the measured current was predominantly negative (96.3% of the samples). Because delivered discharge energy is reported as a positive throughput quantity, the magnitude of the measured current was used in the energy integration. Time vectors were sorted and duplicate timestamps were removed before numerical integration. The delivered discharge energy was then calculated as
E k = 1 3600 ∫ V ( t ) | I ( t ) | d t ,
where time is expressed in seconds and E k in Wh. As a sensitivity check, energy was also calculated using only outward power, P out ( t ) = max [ − V ( t ) I ( t ) , 0 ] . Across the 2794 extracted discharge records, this changed the total integrated discharge energy by only 0.0023%, confirming that the use of | I ( t ) | has a negligible effect on the present energy-throughput results. This measured discharge energy is later used to construct the environmental reference and to fit the battery-specific energy–SOH relation used for extrapolation beyond the observed horizon.
The variables carried forward from the three cycle types are summarized in Table 1. Although charge records were extracted for completeness and data-quality context, charging energy and charge/discharge efficiency losses were not included in the screening-level environmental indicator, which considers delivered discharge energy only. The degradation models in this study are based on discharge capacity and EIS-derived resistance variables. Using discharge capacity as the response does not imply that degradation occurs only during discharge; it reflects the accumulated operating history. Charging conditions, depth of discharge, rest periods, and temperature were not modeled as separate covariates. Representative measured SOH trajectories illustrating different degradation patterns are shown together with the fitted models in Figure 1.
Table 1. Main variables extracted from the NASA battery dataset and their role in the analysis.
Figure 1. Representative full-data descriptive fits for (a) B0006, (b) B0043, (c) B0045, and (d) B0007.

2.2. Causal Impedance Matching, Data Cleaning, and Battery Selection

2.2.1. Causal Discharge—EIS Matching

Discharge and EIS records were aligned using the causal previous rule: each discharge was matched to the latest valid EIS measurement from the same battery recorded at or before its timestamp. This follows the causal alignment principle of Meng et al. [22] and prevents look-ahead bias associated with nearest-time matching. Discharges without preceding EIS remained unmatched; future EIS was never borrowed. EIS age was defined as the discharge–EIS time difference in hours, with the battery-level mean calculated over retained modeling records. A maximum age of 24 h was applied during cleaning.
Among 2794 discharge, 1956 impedance, and 2815 charge records, 2718 discharge observations had valid causal EIS matches. EIS sampling frequency varied among experimental groups and was not one-to-one with discharge. One EIS measurement could, therefore, be matched to multiple subsequent discharges within the allowable age. Unmatched discharge records remained available for reference-energy and observed-EOL calculations, but not for impedance-informed modeling.
Only the dataset-provided scalar R e and R c t variables were modeled; comparable capacitance and diffusion/Warburg parameters were not extracted. Causal matching does not ensure equivalent SOC, temperature, or measurement conditions. Although ambient temperature was recorded for operations and cell temperature for charge/discharge, no temperature correction was applied to the impedance variables. Their association with SOH, therefore, cannot be attributed exclusively to aging.
Potential confounding was examined descriptively by comparing existing chronological hold-out RMSE values for batteries with constant versus changing recorded ambient temperature. Models were neither refitted nor reselected. Discharge temperatures were not assumed to represent EIS acquisition temperatures; thus, this comparison was not a temperature-corrected evaluation of impedance contributions.

2.2.2. Record-Level Cleaning

The impedance-modeling subset excluded records with non-finite capacity, energy, or SOH; capacity ≤ 0.3 Ah; discharge energy ≤ 0.5 Wh; SOH outside ( 0 , 1.5 ) ; missing or negative R e or R c t ; or non-finite EIS age or age exceeding 24 h. The 24-h limit is a practical recency criterion, not a guarantee of matched SOC or temperature.
EIS-age limits of 6, 12, 24, and 48 h were first compared for record retention and battery eligibility. Since only four batteries remained eligible at 6 h, complete model refitting and chronological validation were performed for 12, 24, and 48 h, retaining 24 h as the primary limit.
Local capacity increases were not removed to enforce monotonic degradation. Increases exceeding 0.5% of initial capacity were counted as descriptive diagnostics, not eligibility or model-selection criteria; possible rest, temperature, discharge-rate, and measurement effects were not separated.
Cleaning retained 1561 impedance-modeling records from 28 batteries (1233 discharge observations excluded from this subset). Each retained record corresponds to a discharge observation with a valid causal EIS match; its count need not equal the total number of discharge cycles. The full discharge reference table was kept separately for measured energy and observed-EOL calculations.

2.2.3. Battery Eligibility and Baseline-Consistency Screening

Chronological validation required at least 30 training and 8 hold-out observations, yielding a minimum of 38 retained impedance-modeling records per battery. At the primary 24-h EIS limit, no battery had exactly 38 or 39 records; thus, this criterion retained the same cohort as the previous 40-record threshold.
To assess the reliability of the first valid discharge capacity ( Q 0 ) as the SOH normalization baseline, it was compared with the maximum of the first five valid discharge capacities ( Q max , 1 : 5 ). The early-capacity-rise fraction was defined as
r early = Q max , 1 : 5 − Q 0 Q 0 ,
Batteries with r early > 0.10 were excluded because their initial capacity was considered an unsuitable normalization baseline. Thresholds of 0.10, 0.20, and 0.30 excluded the same three batteries (B0054, B0055, and B0056). Of 34 extracted trajectories, 28 remained after cleaning, 15 met the 38-record criterion, and 12 passed baseline screening. No additional top-N selection was applied (Table 2).
Table 2. Summary of data extraction, matching, cleaning, and battery eligibility.
To evaluate the effect of excluding B0054–B0056, alternative SOH normalization was performed for all 15 candidate batteries. Two reference capacities were considered: the median (Median5) and maximum (Max5) of the first five valid discharge capacities. The original Q 0 was retained unless Q max , 1 : 5 > 1.10 Q 0 , in which case it was replaced by the corresponding Median5 or Max5 value. SOH was recalculated from the original impedance-matched records before cleaning, and the same cleaning, chronological 80/20 validation, and model-fitting procedures were repeated. This sensitivity analysis assessed SOH forecasting and model ranking only; EOL and environmental indicators were not recalculated.
Figure 2 summarizes the computational workflow. The primary chronological 80/20 hold-out was used for model selection, with rolling-origin evaluations assessing temporal robustness. Selected formulations were subsequently refitted using their available full-data histories for retrospective EOL extrapolation, followed by observed-EOL assessment, environmental calculations, and reliability screening. Thus, environmental outcomes did not influence model selection.
Figure 2. Reliability-aware computational workflow.

2.3. Degradation Models

Four models were evaluated: a cycle-only benchmark and three impedance-informed formulations (classical, pseudo-FO, and Mittag–Leffler FO). Original physical discharge indices were preserved after cleaning to avoid compressing the aging history. The normalized cycle coordinate was k n = k / k max , where k max is the last physical discharge index in the relevant fitting subset. Impedance variables R e , n and R c t , n were z-score normalized using statistics from the corresponding training or full-data subset.

2.3.1. Cycle-Only Control

A quadratic cycle-only model was adopted as a low-dimensional benchmark for evaluating the contribution of impedance information [23]:
SOH ^ cycle ( k ) = β 0 + β 1 k n + β 2 k n 2 .

2.3.2. Classical Impedance-Informed Model

The classical model extends the quadratic benchmark with normalized R e and R c t , consistent with their use in battery-health diagnosis [15,24]:
SOH ^ class ( k ) = β 0 + β 1 k n + β 2 k n 2 + β 3 R e , n ( k ) + β 4 R c t , n ( k ) .
Coefficients were estimated by ordinary least squares, providing a reference for evaluating the additional flexibility of the nonlinear models.

2.3.3. Pseudo Fractional-Order Model

Motivated by the stretched-exponential capacity-fade representation of Cuervo-Reyes and Flückiger [25], the pseudo-FO model combines empirical non-exponential decay with impedance covariates:
SOH ^ pFO ( k ) = a exp ( − b k n α ) + c 0 + c R e R e , n ( k ) + c R c t R c t , n ( k ) .
The parameter α is an empirical decay-shape exponent, not a fractional-derivative order. The range 0 < α ≤ 2 permits stretched-like ( α < 1 ) and compressed-like ( α > 1 ) decay. The upper bound of 2 is a pragmatic regularization choice that limits extreme shapes, not a physical or fractional-calculus constraint. Thus, α > 1 is permissible in this empirical pseudo-FO formulation.

2.3.4. Mittag–Leffler Fractional-Order Model

The Mittag–Leffler FO formulation uses a generalized non-exponential decay function that recovers the classical exponential response at unit order [26]:
SOH ^ FO ( k ) = c 0 + a E α ( − b k n α ) + c R e R e , n ( k ) + c R c t R c t , n ( k ) ,
where
E α ( z ) = ∑ m = 0 ∞ z m Γ ( α m + 1 ) , 0 < α ≤ 1 .
At α = 1 , E 1 ( z ) = exp ( z ) . The series was evaluated using up to 80 terms and a convergence tolerance of 10 − 12 . The model is a data-driven fractional-decay representation rather than a formulation derived from a cell-specific fractional differential equation. Its fitted order describes decay shape, not an independently measured electrochemical memory coefficient.

2.3.5. Parameter Identification and Monotonicity-Promoting Objective

Both nonlinear models contained six fitted coefficients and were optimized using Nelder–Mead with five deterministic initializations. Only finite solutions satisfying the positivity and α constraints were accepted.
Both nonlinear models were identified with the same objective:
J = ∑ i ( y i − y ^ i ) 2 + 20 ( y ^ 1 − y 1 ) 2 + 100 ∑ i max ( Δ y ^ i , 0 ) 2 .
The additional objective terms penalize initial-offset error and increases in predicted SOH, respectively. They promote monotonicity without imposing a hard constraint or modifying the measured capacity-recovery behavior. The primary penalty weights ( 20 , 100 ) were pragmatic rather than physically derived or optimized. Sensitivity was assessed using ( 10 , 50 ) , ( 20 , 100 ) , and ( 40 , 200 ) . Optimization stability was evaluated across the five starts; solutions satisfying J ≤ 1.01 J min were considered near-optimal, where J min is the lowest finite valid objective value for the corresponding battery and model.

2.4. Chronological Within-Cell Validation and Model Selection

We evaluated within-cell forecasting by training on earlier impedance-modeling records and testing on later records from the same battery. Records were chronologically ordered without shuffling. The primary split used the first 80% for training and approximately 20% for hold-out evaluation, requiring at least 30 training and 8 test records. The split followed retained-record order while preserving original physical discharge indices, including gaps introduced by cleaning.
Normalization was based exclusively on the training subset. The normalized cycle coordinate used the final training discharge index, while impedance variables were standardized as
R e , n = R e − μ R e , train σ R e , train ,
and
R c t , n = R c t − μ R c t , train σ R c t , train ,
Training-derived means and standard deviations were applied unchanged to hold-out predictions, preventing test-period information leakage.
Future EIS measurements were unavailable during hold-out prediction; therefore, R e and R c t were fixed at their last training values. The same persistence assumption was applied beyond the final modeling record during EOL extrapolation. This assumption does not imply physically constant resistance and may introduce prediction bias in either direction. Under frozen EIS, impedance-dependent terms remain constant during forecasting: the classical model evolves through its quadratic cycle terms, whereas the pseudo-FO and Mittag–Leffler FO models retain their nonlinear cycle-dependent degradation functions. Thus, the analysis evaluates the contribution of historical impedance to model identification and subsequent open-loop SOH forecasting, not the potential benefit of updated, time-varying EIS measurements.
Validation was performed within each battery: model parameters and normalization statistics were estimated from its training history, and later observations from the same cell formed the test set. No entire battery was withheld, and no shared degradation model was trained across cells. Therefore, the results do not demonstrate generalization to unseen batteries. Such evaluation would require a transferable model tested on entirely withheld battery trajectories without using their observations for parameter estimation or preprocessing.
An expanding-window rolling-origin analysis used training cutoffs at 60%, 70%, and 80% of each battery’s retained records. Each cutoff was followed by a test window equal in length to the primary approximately 20% hold-out; later records were excluded from that validation origin. Original physical discharge indices were preserved. At each cutoff, model parameters and normalization statistics were re-estimated using training observations only, while test-period EIS values were frozen at their last training values. The 80/20 split remained the primary model-selection configuration used for the environmental pathway; the other origins assessed temporal robustness. RMSE means and standard deviations across overlapping windows were treated as descriptive measures of split sensitivity, not confidence intervals or independent experimental replications.
Prediction performance was quantified using the root mean square error (RMSE), mean absolute error (MAE), and coefficient of determination ( R 2 ):
RMSE = 1 N ∑ i = 1 N y ^ i − y i 2 ,
MAE = 1 N ∑ i = 1 N y ^ i − y i ,
and
R 2 = 1 − ∑ i = 1 N y i − y ^ i 2 ∑ i = 1 N y i − y ¯ 2 .
Chronological hold-out RMSE was the primary model-selection metric, with MAE and R 2 as complementary diagnostics. The latter may be negative when hold-out SOH variability is small. For each battery, the best impedance-informed model minimized RMSE among the classical, pseudo-FO, and Mittag–Leffler FO formulations. The best overall model was selected separately from all four formulations, including the cycle-only benchmark. The impedance-related RMSE gain was defined as
G imp ( % ) = RMSE cycle − min RMSE class , RMSE pFO , RMSE FO RMSE cycle × 100 .
Positive G imp indicates that at least one impedance-informed model outperformed the cycle-only benchmark; negative values favor the cycle-only model. The hold-out-selected best impedance-informed formulation was used for the primary environmental analysis, with the cycle-only model retained as a predictive benchmark. When cycle-only achieved the lowest overall RMSE, its EOL and environmental results were also examined as a secondary comparison. Model selection preceded all environmental calculations.
Because the same hold-out observations were used to select and evaluate the best-of-three impedance-informed model, its reported gain is descriptive and subject to post-selection bias. Each predefined impedance-informed formulation was, therefore, also compared separately against cycle-only using Δ RMSE b , m = RMSE b , cycle − RMSE b , m . Positive differences and median paired differences were summarized across 12 batteries. No additional untouched test set was reserved after model selection.
For each predefined model, the median and interquartile range (IQR) of paired RMSE differences were calculated across 12 batteries. Exploratory uncertainty was assessed using 20,000 battery-level bootstrap resamples, each containing 12 batteries sampled with replacement. The median difference was recalculated per resample, and its 2.5th and 97.5th percentiles were reported. Overlapping rolling-origin windows were not treated as independent samples. Given the small cohort and related experimental groups, these intervals were interpreted descriptively rather than as definitive population-level uncertainty estimates.
After validation, each formulation was refitted using all cleaned impedance-modeling records of the corresponding battery, with normalization statistics recomputed from that full-data subset. These refits were used for descriptive assessment and retrospective EOL extrapolation, not independently validated pre-EOL forecasting. Measured impedance values were used within the observed modeling region; beyond it, R e and R c t were fixed at their final available values. The primary EOL search ended at cycle 300; models without a threshold crossing within this horizon had undefined EOL. Search limits of 400 and 500 cycles were additionally evaluated without changing model fits or other settings.

2.5. Rule-Based Observed EOL and Right-Censoring

Observed EOL was determined from the broader STEP 2 discharge table, independently of EIS availability, using capacity > 0.3 Ah, discharge energy > 0.5 Wh, and 0 < SOH < 1.5 . The first raw threshold crossing was recorded but not used as the EOL reference. Instead, a causal five-record moving median was applied, and persistent EOL was assigned to the first of three consecutive smoothed SOH values ≤ 0.70 . Each smoothed value uses only current and past observations, although persistence is confirmed after the subsequent two records. This deterministic reference is neither a statistical confidence bound nor proof of irreversible battery failure.
Sensitivity was assessed using a 3 × 3 grid combining causal moving-median windows of 3, 5, and 7 records with persistence requirements of 2, 3, and 4 consecutive crossings. For each rule, observed EOL or right-censored status, EOL error, reliability class, and environmental intensity change were recalculated for the previously selected model. SOH thresholds of 0.70, 0.75, and 0.80 were also evaluated. Model fitting and selection remained fixed, with the five-record median, three consecutive crossings, and 0.70 threshold defining the primary analysis.
Trajectories without a persistent crossing by the final discharge were classified as Right Censored Observed Horizon. The final observed cycle represents a lower bound on lifetime, not a measured EOL. For these trajectories, a finite model-predicted EOL beyond the observed horizon was classified as Projected, not as validated lifetime extension. No EOL prediction error was calculated without an experimental EOL reference.

2.6. Retrospective Pre-EOL Landmark Backtesting

A retrospective pre-EOL landmark backtest evaluated four predefined models: cycle-only, classical impedance-informed, pseudo-FO, and Mittag–Leffler FO. Each model was independently fitted using the first n ∈ { 30 , 50 , 75 } chronologically available cleaned, impedance-matched records. Training sizes were predefined without reference to future EOL observations or errors. Only landmarks preceding both the first raw SOH threshold crossing and persistent observed EOL were eligible.
At each landmark, model parameters and normalization statistics were estimated using the truncated training history. Future EIS was unavailable; therefore, R e and R c t were frozen at their last training values. Predicted EOL was the first subsequent physical discharge cycle with forecast SOH ≤ 0.70 , searched up to cycle 300. Otherwise, the forecast was classified as non-crossing.
Observed EOL followed the previously defined causal five-record moving median and three-consecutive-crossing criterion. Relative EOL and RUL errors were calculated as
ε EOL = 100 N pred − N obs N obs ,
ε RUL = 100 N pred − N obs N obs − N 0 ,
where N pred and N obs denote predicted and observed EOL cycles, and N 0 is the forecast-origin cycle. An absolute relative-error tolerance of 20% was applied separately to EOL and RUL. Non-crossing forecasts were counted as unsuccessful rather than excluded. All predefined models were evaluated without selecting the lowest eventual EOL error.
Landmarks from the same battery were treated as correlated evaluations. This retrospective historical backtest does not constitute prospective testing or independent cross-cell validation.

2.7. Screening-Level Energy-Normalized Environmental Assessment

The environmental assessment is a screening-level energy-normalized comparison, not a complete cradle-to-grave life-cycle assessment (LCA). It examines how model-estimated lifetime affects environmental intensity under a fixed upstream manufacturing burden. For each battery, E ref is the measured cumulative discharge energy up to persistent observed EOL (Section 2.5) or the final observed discharge for right-censored cells. E model is the cumulative discharge energy up to the EOL predicted by the validation-selected, full-data-refitted degradation model. The corresponding intensities are
I ref = B E ref , I model = B E model ,
Here, B = 100 kg CO2-eq is a fixed illustrative manufacturing-burden scenario, not a measured footprint of the NASA cells. The relative intensity change is
Δ I ( % ) = I ref − I model I ref × 100 .
The common burden B cancels from Δ I , making the relative change independent of its assumed value. Positive Δ I indicates lower model-estimated intensity per delivered kWh; negative values indicate higher intensity. These changes do not establish actual emission reductions.
Predicted EOL is always determined by the validation-selected, full-data-refitted degradation model. When it lies within the observed discharge horizon, E model uses measured per-cycle energies only. Beyond the observed horizon, unavailable future discharge energies are estimated using a battery-specific linear energy–SOH relationship:
E k = max 0 , θ 1 SOH ^ m ( k ) + θ 0 ,
Here, SOH ^ m ( k ) is predicted by the same selected full-data-refitted model used for EOL estimation. The auxiliary energy–SOH relationship was fitted using measured discharge data, with RMSE and R 2 recorded. It was used only for future-energy extrapolation, not SOH model identification. Within the observed history, SOH was calculated from measured capacity; beyond it, model-predicted SOH was used. The max ( 0 , · ) operator prevents negative energy predictions but imposes no upper bound. Before clipping, the relation is linear and monotonic with respect to SOH for fixed θ 1 , without a separate cycle-wise monotonicity constraint.
Future-energy extrapolation sensitivity was examined for the four right-censored Projected batteries. First, the auxiliary linear energy–SOH relationship was evaluated using an 80/20 chronological split of valid discharge observations. The first 80% were used for fitting, and the remaining 20% were evaluated using experimentally measured SOH values. This assesses the conditional energy–SOH mapping, not independent future SOH or EOL forecasting. As an alternative extrapolation scenario, future per-cycle energy was held constant at the median of the last five valid measured discharge energies. Selected degradation models, predicted EOL cycles, observed reference energy, and the manufacturing-burden assumption remained unchanged. Thus, differences in environmental indicators arose solely from the future-energy extrapolation method.

2.8. Reliability Classification for Environmental Interpretation

The first screening layer requires a finite model-predicted EOL within the numerical search horizon and plausible SOH and energy trajectories. The primary safeguards include a minimum lifetime-energy ratio of 0.50, a future-SOH range of [ 0 , 1.05 ] , and a maximum future-energy factor of 1.20, limiting extrapolated per-cycle energy to 120% of the largest measured value. For batteries with observed EOL, an additional directional rule requires N EOL , pred ≥ 0.80 N EOL , obs before final EOL-error classification. This is equivalent to a relative EOL error of at least − 20 % . Consequently, earlier predictions with errors below − 20 % are Rejected, whereas late predictions exceeding + 20 % may be classified as Unreliable EOL if other conditions pass. This asymmetry reflects the screening sequence, not evidence that early errors are intrinsically more severe.
These limits are pragmatic safeguards, not universal physical thresholds or optimized model-selection parameters. Sensitivity analyses varied the maximum future SOH (1.00, 1.05, 1.10), future-energy factor (1.10, 1.20, 1.30), minimum observed-EOL fraction (0.70, 0.80, 0.90), and minimum lifetime-energy ratio (0.40, 0.50, 0.60), holding degradation-model predictions and other settings fixed. The future-SOH limits of 1.00, 1.05, and 1.10 produced identical primary classifications.
For batteries with persistent observed EOL, the second layer evaluates the relative prediction error:
ε EOL ( % ) = N EOL , pred − N EOL , obs N EOL , obs × 100 .
A prediction passing the first-layer checks is classified as Reliable Observed when
| ε EOL | ≤ 20 % .
The 20% EOL-error tolerance is a pragmatic screening criterion, not a universal battery standard. Sensitivity was assessed using 10%, 20%, and 30% tolerances, without changing model predictions or persistent observed-EOL references. For observed-EOL batteries that satisfy the feasibility checks, errors within ± 20 % yield Reliable Observed; errors above + 20 % yield Unreliable EOL. Errors below − 20 % are Rejected by the preceding directional screening rule. For batteries without experimentally observed EOL, admissible extrapolations beyond the right-censored horizon are labeled Projected, since EOL accuracy cannot be verified. Outputs failing the screening safeguards are Rejected. Environmental changes associated with unreliable or rejected outcomes remain visible for transparency but are not interpreted as credible benefits.
Reliability denotes deterministic, rule-based screening rather than probabilistically calibrated confidence. In particular, Reliable Observed reflects retrospective agreement of a full-data-derived EOL estimate with the persistent experimental EOL. It does not establish independently validated pre-EOL forecasting accuracy. Likewise, Projected indicates an admissible estimate beyond a right-censored horizon, not confirmed lifetime extension. The battery-level bootstrap intervals quantify exploratory variability in paired chronological SOH prediction errors; they do not propagate parameter uncertainty into EOL estimates or provide EOL prediction intervals.
The primary computational workflow was implemented in MATLAB R2022a (MathWorks, Natick, MA, USA). To facilitate reproducibility, the analysis scripts, processed data tables, configuration settings, and instructions for reproducing the reported results are provided as Supplementary Materials.

3. Results

3.1. Selected Battery Characteristics

Cleaning retained 1561 impedance-modeling records from 28 batteries. Of the 15 batteries meeting the minimum 38-record requirement, B0054, B0055, and B0056 were excluded because of inconsistent initial-capacity baselines. The same batteries were excluded at early-capacity-rise thresholds of 10%, 20%, and 30%, leaving 12 for the modeling and environmental assessment.
Table 3 summarizes the 12 retained batteries, which differ in trajectory length, impedance-measurement density, and degradation extent. Final SOH refers to the last retained impedance-modeling record, not an eligibility threshold; records below SOH = 0.70 were retained when they passed the data-quality checks. Mean R e and R c t values were calculated across each battery’s retained modeling records, rather than within individual discharge cycles.
Table 3. Characteristics of the 12 retained batteries.
Table 4 shows that the normalized SOH = 0.70 criterion corresponds to absolute capacities ranging from 0.7484 Ah (B0053) to 1.4247 Ah (B0006). Thus, the normalized EOL threshold does not imply identical absolute EOL capacities across the cells.
Table 4. Battery-specific absolute capacity thresholds corresponding to the adopted normalized EOL criterion of SOH = 0.70.

3.2. Descriptive Full-Data Fit Performance

Table 5 presents descriptive full-data RMSE, with the lowest value in each row shown in bold. These fits describe agreement with measured trajectories, not independent forecasting performance, and were not used for validation-based model selection. The classical model achieved the lowest RMSE in nine batteries, pseudo-FO in B0005 and B0007, and Mittag–Leffler FO in B0045.
Table 5. Descriptive full-data RMSE for the four model formulations.
Full-data and chronological hold-out model rankings differed for B0005, B0006, B0007, and B0018 (4/12 batteries). Thus, favorable descriptive fit does not necessarily imply superior forecasting of later observations. Figure 1 illustrates representative full-data model fits; these should not be interpreted as independently validated predictive performance.

3.3. Chronological Hold-Out Performance

Table 6 reports the primary 80/20 chronological hold-out RMSE, with the best overall result in each row highlighted in bold. The best of three impedance-informed formulations outperformed cycle-only in 10 of 12 batteries, with positive RMSE gains ranging from 9.23% (B0018) to 85.72% (B0043). Cycle-only performed best for B0007 and B0047. However, G imp (Equation (15)) is descriptive because model selection and evaluation used the same hold-out.
Table 6. Chronological 80/20 hold-out RMSE for the four degradation-model formulations.
Table 7 compares each predefined impedance-informed formulation separately with cycle-only, avoiding best-of-three selection. The classical, pseudo-FO, and Mittag–Leffler FO models achieved lower RMSE in 7/12, 8/12, and 8/12 batteries, respectively. Their median paired RMSE improvements were 0.00303, 0.00456, and 0.00239.
Table 7. Battery-level paired RMSE comparison under the primary 80/20 chronological hold-out.
Although all three median differences were positive, their IQRs and exploratory battery-level bootstrap intervals included zero. These results indicate substantial battery-to-battery heterogeneity and do not establish a statistically robust or universally generalizable impedance-related improvement. The 10/12 best-of-three count must, therefore, be distinguished from the individual-model comparisons.
Under the primary hold-out, classical was the best impedance-informed model for nine batteries, pseudo-FO for B0006 and B0018, and Mittag–Leffler FO for B0045. Including cycle-only among the candidates, the benchmark achieved the lowest overall RMSE for B0007 and B0047. These results concern separately fitted within-cell models and do not demonstrate transferability to unseen batteries.
Figure 3 illustrates representative predictions: pseudo-FO was preferred for B0006, Mittag–Leffler FO for B0045, and classical for B0042. B0047 provides a counterexample favoring cycle-only.
Figure 3. Representative chronological 80/20 hold-out validation trajectories for (a) B0006, (b) B0045, (c) B0042, and (d) B0047.
The best-of-three impedance-informed RMSE was lower than cycle-only in 31/36 battery–origin comparisons (86.1%). Eight batteries showed an advantage at all three origins, although the preferred formulation sometimes changed (Table 8). These are descriptive post-selection results: origins within each battery are correlated and test windows overlap. Table 8 reports mean ± standard deviation of RMSE across origins. “Imp. wins” counts favorable origins, while C, P, and R denote classical, pseudo-FO, and Mittag–Leffler FO.
Table 8. Rolling-origin prediction robustness at the 60%, 70%, and 80% training origins.
EIS-age limits of 6, 12, 24, and 48 h retained 808, 1140, 1561, and 1612 modeling records, respectively. Only four batteries remained eligible at 6 h, whereas the other limits retained the same 12-battery cohort. For 12, 24, and 48 h, the best-of-three impedance formulation outperformed cycle-only in 11/12, 10/12, and 10/12 primary hold-outs, respectively, and in 33/36, 31/36, and 31/36 rolling-origin comparisons. Relative to 24 h, the selected impedance model changed for five batteries at 12 h and two at 48 h. Thus, aggregate advantages were broadly stable, although individual model selection depended on EIS recency.
Negative hold-out R 2 values occurred when test segments contained little SOH variation; RMSE was, therefore, retained as the primary selection metric. All five nonlinear-model starts yielded valid solutions, and the selected nonlinear models showed at most one-cycle variation in full-data EOL among near-optimal solutions.

3.4. Sensitivity to Baseline Normalization

Both Median5 and Max5 normalization retained all 15 candidate batteries, including B0054, B0055, and B0056. Under the conditional normalization rule, the original 12 batteries retained their reference capacities and model rankings. Table 9 compares the primary and expanded-cohort chronological hold-out results.
Table 9. Sensitivity of model-wise chronological hold-out performance to alternative SOH baseline normalization.
The best-of-three impedance-informed formulation outperformed cycle-only in 10/12 batteries under the primary normalization and 12/15 under both alternative normalizations. For Median5 and Max5, the individual classical, pseudo-FO, and Mittag–Leffler FO models achieved lower RMSE in 8/15, 10/15, and 9/15 batteries, respectively. Median paired RMSE improvements were 0.00163, 0.00337, and 0.00069 for Median5, compared with 0.00156, 0.00337, and 0.00069 for Max5. These improvements were generally smaller than those in the primary 12-battery cohort. Thus, the qualitative advantage of impedance-informed modeling persisted after reintroducing the excluded cells, although the best-of-three comparison remains descriptive and subject to post-selection bias.
Table 10 reports hold-out RMSE for the three reintroduced batteries. For B0054, cycle-only achieved the lowest RMSE under both normalizations. For B0055, pseudo-FO performed best (0.01903 for Median5 and 0.01801 for Max5), whereas Mittag–Leffler FO produced markedly higher errors (0.96410 and 0.92063, respectively). For B0056, pseudo-FO and Mittag–Leffler FO only marginally outperformed cycle-only under both scenarios. These cell-specific differences demonstrate that the effect of alternative normalization is model-dependent. The expanded-cohort results support the qualitative sensitivity finding, but do not identify a universally superior degradation model.
Table 10. Chronological hold-out RMSE for the three batteries reintroduced using alternative SOH normalization.

3.5. Sensitivity to Ambient-Temperature Regime

Table 11 stratifies existing chronological hold-out RMSE comparisons by recorded discharge ambient-temperature regime. Nine batteries had constant recorded ambient temperatures: four at 24 °C and five at 4 °C. In B0042–B0044, the first 40 retained records were associated with 22 °C and the next 24 with 4 °C; the transition, therefore, coincided with aging stage.
Table 11. Post hoc comparison of model-wise chronological hold-out performance across discharge ambient-temperature regimes.
All three impedance-informed models outperformed cycle-only for each of the three transition batteries. Among the nine constant-regime cells, classical, pseudo-FO, and Mittag–Leffler FO outperformed cycle-only in 4/9, 5/9, and 5/9, respectively; the best-of-three did so in 7/9. These are descriptive post hoc comparisons of previously evaluated models, without refitting, reselection, or temperature correction. The best-of-three result remains subject to post-selection bias. Temperature, aging stage, and protocol remain confounded; no temperature- independent or aging-specific causal impedance contribution can be inferred.

3.6. Fractional-Order Parameter Behavior

Table 12 reports the parameters estimated from full-data fits. The pseudo-FO exponent α pseudo ∈ ( 0 , 2 ] is an empirical decay-shape parameter, whereas the Mittag–Leffler order α real ∈ ( 0 , 1 ] governs its generalized decay function. Neither represents an independently measured electrochemical memory coefficient.
Table 12. Estimated pseudo-FO shape exponents and Mittag–Leffler FO orders from the full-data fits.
Five pseudo-FO fits yielded α pseudo > 1 , consistent with its empirical decay-shape definition rather than a fractional-derivative order. Seven Mittag–Leffler FO fits reached α real = 1.0000 at the reported numerical precision, corresponding to the exponential limit of the Mittag–Leffler decay component. These are full-data parameter estimates, not evidence of forecasting superiority.
Under the primary chronological hold-out, the classical impedance-informed model achieved the lowest RMSE among the three impedance-informed formulations for nine batteries, compared with two for pseudo-FO and one for Mittag–Leffler FO (B0045). Thus, the fractional-order formulations showed no systematic forecasting advantage over the classical model.

3.7. Effect of Persistent EOL Detection

Table 13 compares the first raw SOH ≤ 0.70 crossing with persistent observed EOL, defined using a causal five-record median and three consecutive smoothed crossings. Both references were calculated from valid discharge records independently of EIS matching or model predictions.
Table 13. Raw and persistent observed-EOL references for the 12 retained batteries.
Persistent EOL was observed in five batteries and occurred 2–4 discharge cycles after the first raw crossing. Seven trajectories remained right-censored. Notably, B0048 crossed the raw threshold at discharge 53 but did not satisfy the persistence criterion by its final observed discharge at cycle 72.
Sensitivity was evaluated using causal moving-median windows of 3, 5, and 7 records combined with persistence requirements of 2, 3, and 4 consecutive smoothed values ≤ 0.70 (nine combinations). Model-predicted EOL cycles remained fixed; only the experimental reference and derived EOL errors, reliability classes, and environmental indicators were recalculated (Table 14).
Table 14. Sensitivity of the observed-EOL reference to smoothing and persistence settings.
Across all nine combinations, the five observed-EOL cases remained within the ± 20 % prediction-error tolerance, and seven trajectories remained right-censored. No primary reliability classification changed. Thus, the results were insensitive to the tested smoothing and persistence settings, although sensitivity to the SOH threshold is examined separately.

3.8. EOL Extrapolation Reliability

Good chronological SOH prediction performance did not guarantee reliable long-horizon EOL extrapolation. Five batteries satisfied the predefined 20% EOL-error tolerance and were classified as Reliable Observed. B0018 and B0042–B0044 had finite predicted EOL beyond their right-censored experimental horizons and were labeled Projected. B0007, B0048, and B0053 were Rejected because no admissible finite EOL was obtained.
Thus, the primary analysis yielded five Reliable Observed, four Projected, zero Unreliable EOL, and three Rejected cases (25%). All rejections resulted from the absence of admissible finite EOL, not the future-SOH upper limit. Extending the search horizon from 300 to 400 or 500 cycles did not change these classifications. No alternative model was substituted after inspecting EOL results; the chronological model-selection ranking remained fixed.
The five Reliable Observed outcomes represent deterministic retrospective EOL agreement, not independently validated pre-EOL forecasts. No statistical prediction intervals were calculated for the EOL estimates. For the four Projected cases, EOL errors could not be assessed without experimentally observed references. Search-horizon, screening-threshold, and optimization sensitivities assess methodological stability rather than probabilistically calibrated lifetime uncertainty.
Changing nonlinear penalty weights altered the selected impedance-informed model for some batteries but not the overall reliability-class distribution. Reducing EOL-error tolerance from 20% to 10% affected only B0045; a 30% tolerance caused no changes. The tested future-SOH and future-energy safeguards also left classifications unchanged, whereas increasing the minimum observed-EOL fraction to 0.90 affected only B0045.
Unlike the preceding safeguards, changing the normalized SOH threshold from 0.70 to 0.75 or 0.80 produced earlier experimental and predicted EOL crossings and substantially changed the reliability-class distribution (Table 15). The EOL definition must, therefore, be reported explicitly. Figure 4 contrasts chronological hold-out RMSE with EOL prediction error for the five batteries with persistent observed EOL.
Table 15. Sensitivity of retrospective environmental reliability classifications to the normalized SOH threshold. Model selection and fitted parameters were kept unchanged.
Figure 4. Hold-out RMSE versus absolute EOL error for the five batteries with persistent observed EOL; the horizontal line marks the 20% reliability threshold.
At SOH = 0.75, B0007 and B0048 changed from Rejected to Reliable Observed, while B0018 changed from Projected to Reliable Observed. At SOH = 0.80, B0042–B0044 additionally became Reliable Observed, yielding 11 reliable observed cases and one rejection (Table 15). These threshold-dependent categories remain retrospective screening outcomes, not independently validated lifetime forecasts.

3.9. Retrospective Pre-EOL Forecasting Results

Eight eligible pre-EOL forecasting landmarks were obtained from four batteries: three each for B0005 and B0006, and one each for B0046 and B0047. B0045 was excluded because only 16 cleaned impedance-matched records preceded its observed EOL, below the required minimum of 30. The remaining seven batteries lacked persistent observed EOL and could not support EOL-error evaluation. Table 16 reports the physical-cycle EOL forecasts of all four predefined models.
Table 16. Pre-EOL landmark backtest results: predicted EOL in physical discharge cycles for the four predefined models. A dash indicates no EOL threshold crossing within the 300-cycle prediction horizon.
Table 17 summarizes finite EOL forecasts and the separate 20% absolute relative-error tolerances for EOL and RUL across eight landmarks. Non-crossing predictions were counted as unsuccessful and retained in the denominator. Landmarks from the same battery were not statistically independent.
Table 17. Pre-EOL forecasting performance of the four predefined model formulations across eight eligible landmark cases. Multiple landmarks from the same battery are not statistically independent.
The truncated-history forecasts differed substantially from retrospective full-data agreement. For B0005 with 50 training records, classical predicted EOL at cycle 113 and Mittag–Leffler FO at 159, compared with observed EOL at 164. For B0006, none of the models produced finite EOL using 30 training records. All four models predicted cycle 35 for B0047, versus observed EOL at 44. These examples demonstrate the limitations of early lifetime forecasting.
Across eight landmarks, the four models met the 20% EOL-error tolerance in 2/8, 1/8, 4/8, and 5/8 cases, respectively, but the corresponding RUL tolerance in only 0/8, 0/8, 3/8, and 3/8 cases. For B0046, cycle-only and classical predicted EOL at cycle 36 from origin 33, versus observed EOL at 44. This yielded an EOL-relative error of − 18.18 % but a RUL-relative error of − 72.73 % . Hence, EOL-relative accuracy alone can overstate remaining-lifetime forecasting accuracy. The four-battery sample and correlated landmarks preclude claims of universal model superiority.
The five Reliable Observed outcomes reflect retrospective full-data EOL agreement, not independently validated pre-EOL forecasts. The truncated-history backtest does not alter the original full-data fits or calculated environmental indicators. Those indicators remain descriptive, screening-level, model-dependent scenarios, not demonstrated emission reductions.

3.10. Energy–SOH Surrogate Diagnostics

The battery-specific energy–SOH surrogate was used only when the EOL predicted by the validation-selected degradation model extended beyond the measured discharge horizon. Otherwise, cumulative discharge energy was calculated exclusively from measured per-cycle values. Future-energy extrapolation was required for four of the 12 batteries: B0018 and B0042–B0044. Table 18 reports their extrapolation horizons and energy–SOH fitting diagnostics.
Table 18. Energy–SOH surrogate diagnostics for the four Projected cases requiring future-energy extrapolation.
B0018 required the longest future-energy extrapolation (22 cycles, from 132 to 154). Figure 5 illustrates its fitted linear energy–SOH relationship, which achieved R 2 = 0.9995 and RMSE = 0.0126 Wh on the measured data.
Figure 5. Energy–SOH surrogate for B0018 showing the measured discharge-energy data and fitted linear relation.
All four cases remained right-censored and were classified as Projected. The surrogate supplied estimated future discharge energy but did not validate their predicted SOH trajectories or EOL cycles. All five Reliable Observed cases used measured discharge energy exclusively, while the three Rejected cases did not contribute surrogate-based environmental estimates.

3.11. Energy Extrapolation Sensitivity

Table 19 compares the original linear energy–SOH surrogate with a constant-energy scenario based on the median of the last five valid measured discharge energies for the four Projected batteries. The table also reports the auxiliary linear model’s chronological 80/20 hold-out RMSE, evaluated using measured SOH values. Predicted EOL cycles, reference energies, and the manufacturing-burden assumption were held fixed. The chronological energy–SOH hold-out R 2 values ranged from 0.9638 to 0.9970 across the four Projected batteries.
Table 19. Chronological validation of the auxiliary energy–SOH relationship and sensitivity of projected environmental changes to an alternative future-energy extrapolation assumption.
The alternative scenario changed projected environmental intensity indicators by 0.31–0.80 percentage points relative to the linear energy–SOH approach. Because predicted EOL exceeded the observed horizon in all four cases, adding positive extrapolated discharge energy increased cumulative modeled energy and necessarily produced a positive Δ I . Thus, the positive sign under both scenarios is an arithmetic consequence of the assumed extended energy horizon, not independent evidence of environmental benefit. Chronological validation using measured SOH assessed only the conditional energy–SOH mapping. Neither extrapolation scenario validated future SOH trajectories, predicted EOL, or actual emission reductions. These results quantify sensitivity to the future-energy assumption, not comprehensive lifetime or environmental uncertainty.

3.12. Reliability-Aware Environmental Results

Table 20 presents the screening-level environmental outcomes for the chronologically selected, full-data-refitted impedance-informed models. The assessment follows the predefined model selection (Section 2.4), observed-EOL definition (Section 2.5), energy-normalized calculation (Section 2.7), and reliability screening (Section 2.8).
Table 20. Retrospective full-data-fit screening-level environmental results for the validation-selected impedance-informed models.
Five batteries were classified as Reliable Observed, four as Projected, and three as Rejected. All five observed-EOL cases yielded negative environmental changes, ranging from − 10.59 % to − 2.52 % , indicating higher model-estimated intensity relative to their references. The positive changes in the four Projected cases represent conditional scenarios, not experimentally verified benefits.
Figure 6 visualizes the reliability-aware environmental results. The sign and magnitude of each modeled change must be interpreted alongside its EOL reliability classification, rather than as standalone evidence of environmental benefit.
Figure 6. Reliability-aware environmental changes across the 12 retained batteries.
The four Projected outcomes represent conditional extrapolations beyond right-censored experimental horizons. The three Rejected cases lacked admissible finite EOL and therefore had no primary environmental-change estimate. No alternative formulation was substituted after inspecting EOL or environmental results.
As a secondary check, cycle-only was evaluated for B0007 and B0047, where it had the lowest overall hold-out RMSE. B0007 remained Rejected and B0047 remained Reliable Observed, leaving the qualitative reliability interpretation unchanged.
Overall, the results did not demonstrate a systematic decrease in energy-normalized environmental intensity from impedance-informed or fractional-order modeling. Environmental interpretation depends on the credibility of the predicted lifetime and the corresponding cumulative delivered energy.

4. Discussion

4.1. Predictive Value of Impedance and Model Complexity

Chronological within-cell validation suggested a potential contribution of historical impedance to SOH forecasting, consistent with battery-diagnostic studies [10,11,12,13,14,27,28]. Classical, pseudo-FO, and Mittag–Leffler FO individually outperformed cycle-only in 7/12, 8/12, and 8/12 batteries. The best-of-three result (10/12) and rolling-origin comparisons (31/36) remain descriptive because of post-selection bias and correlated validation windows. With future EIS frozen, historical impedance contributed to model identification, while subsequent forecasts depended on fitted cycle-dependent terms. Neither benefits from updated future EIS nor aging-specific causal effects were established.
Classical achieved the lowest hold-out RMSE among impedance-informed models for nine batteries, whereas full-data and hold-out rankings differed for four. Neither FO formulation demonstrated systematic superiority. The pseudo-FO exponent describes empirical decay shape; at α = 1 , the Mittag–Leffler decay component reaches its exponential limit. Neither parameter establishes electrochemical memory. Guerra et al. [9] also reported limited fractional-dynamics benefits, but their Caputo-based model and cross-cell evaluation differ from our within-cell approach, preventing direct quantitative comparison.
Reintroducing B0054–B0056 under alternative baseline normalization preserved the best-of-three advantage in 12/15 batteries, versus 10/12 in the primary cohort, although median paired improvements decreased. Temperature transitions coincided with aging progression, confounding temperature, aging-stage, and protocol effects. Moreover, despite positive median paired RMSE improvements, all three models’ IQRs and exploratory battery-level bootstrap intervals included zero. The small heterogeneous cohort limits population-level inference. The principal contribution is, therefore, the integrated causal-matching, chronological-validation, EOL-screening, and environmental-interpretation framework, not universal model superiority. Independent cross-cell testing and controlled measurement conditions remain necessary.

4.2. Short-Horizon Accuracy Versus EOL Reliability

Chronological hold-out RMSE evaluates SOH prediction over a finite measured interval, not long-horizon EOL accuracy. For B0042, classical impedance-informed modeling substantially improved hold-out RMSE, yet predicted EOL beyond a right-censored experimental trajectory; B0043 and B0044 showed similar behavior. With future R e and R c t frozen at their last available values, long-horizon extrapolation increasingly depends on fitted cycle-dependent degradation functions. Short-horizon SOH prediction and EOL extrapolation, therefore, require separate reliability assessments.
The persistent-EOL rule avoids treating isolated capacity excursions as confirmed EOL. Across the tested smoothing and persistence settings, five batteries retained persistent observed EOL within the 20% retrospective error tolerance, while seven remained right-censored. For right-censored trajectories, admissible finite EOL estimates beyond the observed horizon were classified as Projected. The Rejected category indicates failure of a screening requirement, including absent admissible finite EOL, physical or energy constraints, or the directional early-EOL rule. It does not imply that a battery will never reach EOL. The distinction between Rejected and Unreliable EOL follows the decision hierarchy, not calibrated prediction uncertainty.
The five Reliable Observed outcomes were based on full-data refits, potentially including observations at or beyond experimental EOL, and, therefore, represent retrospective agreement rather than independent early-lifetime forecasts. The eight eligible pre-EOL landmarks from four batteries revealed substantial forecasting variability. For B0046, classical impedance-informed modeling yielded an EOL-relative error of − 18.18 % but a RUL-relative error of − 72.73 % . Thus, acceptable EOL-relative error does not necessarily imply acceptable remaining-lifetime accuracy. These correlated landmark results cannot establish generalizable forecasting superiority.
The battery-level bootstrap intervals describe uncertainty in paired chronological RMSE differences, not in predicted EOL. Similarly, agreement among near-optimal solutions from different initializations assesses numerical stability rather than parameter uncertainty or prediction-interval coverage. The deterministic reliability categories are, therefore, not probabilistic confidence statements. Future uncertainty analysis should propagate appropriately resampled degradation histories and fitted parameters to EOL while explicitly accounting for non-crossing predictions and right-censoring.

4.3. Environmental Interpretation

The deterministic reliability-screening framework supports retrospective full-data environmental comparisons, but provides neither calibrated uncertainty nor independently validated early-lifetime forecasts. Under the feasibility and 20% EOL-error criteria, five Reliable Observed cases yielded environmental changes from − 10.59 % to − 2.52 % . Their predicted EOL cycles preceded the persistent observed references, reducing modeled lifetime energy and increasing energy-normalized intensity. The pre-EOL landmark backtest further demonstrated that retrospective EOL agreement may not persist when models are fitted using truncated histories.
The four right-censored Projected cases yielded positive modeled changes, but lacked experimentally observed EOL; their results, therefore, remain conditional scenarios rather than validated environmental benefits. The three Rejected cases had no admissible finite predicted EOL and provided no environmental-change estimates. Future-energy extrapolation was required only for the four Projected cases, whereas all five Reliable Observed comparisons used measured discharge energy.
Chronological validation of the auxiliary energy–SOH relationship used measured SOH and assessed only the conditional energy mapping. An alternative last-five-median future-energy assumption changed the four projected environmental indicators by 0.31–0.80 percentage points. Both scenarios retained the same model-predicted EOL and, therefore, did not assess lifetime uncertainty or validate future SOH and EOL. The fixed illustrative manufacturing burden of B = 100 kg CO2-eq cancels from the relative intensity change and is not a measured footprint. Consistent with prior studies emphasizing battery-lifetime assumptions [2,3], the contribution is methodological: lifetime-extrapolation reliability must be qualified before energy-normalized environmental indicators are interpreted. Neither these scenarios nor the screening-level assessment establish actual emission reductions.

4.4. Limitations and Future Work

The study has several limitations. First, the 12 retained batteries represent heterogeneous NASA experimental groups with different operating conditions, EIS sampling densities, and degradation histories. Of the 28 batteries remaining after record-level cleaning, 13 contained fewer than the required 38 modeling records. Consequently, the results cannot be treated as homogeneous experimental replications or a population-level degradation law.
Second, discharge capacity reflects accumulated aging but does not isolate charging, rest, temperature, or depth-of-discharge effects. Local capacity recovery was retained, although its underlying mechanisms could not be identified. Likewise, causal EIS matching prevents future-information leakage but does not ensure equivalent SOC, temperature, or rest conditions. The 24-h EIS-age criterion is pragmatic, and observed impedance associations cannot be attributed exclusively to electrochemical aging. Future EIS was also held constant during prediction, limiting the interpretation of long-horizon forecasts.
Third, the validation evaluates battery-specific within-cell forecasting. No complete battery trajectory was withheld for independent cross-cell testing, and model parameters were identified separately for each cell. Therefore, performance on previously unseen batteries remains unverified. Future work should investigate pooled or hierarchical models, battery-wise hold-out validation, and joint SOH–impedance forecasting.
Fourth, several screening settings are pragmatic rather than universal physical criteria. Sensitivity analyses showed that extending the EOL search horizon from 300 to 400 or 500 cycles did not change the primary classifications, although B0045 became borderline under some stricter screening settings. The reliability categories were more sensitive to the normalized SOH threshold used to define EOL. Furthermore, deterministic reliability labels do not provide statistically calibrated EOL prediction intervals.
Finally, the environmental indicator is a screening-level, lifetime-energy-normalized comparison, not a complete life-cycle assessment. Manufacturing inventories, use-phase electricity, pack-level losses, replacement processes, recycling, and second-life allocation are not modeled. Uncertainty in projected EOL and future delivered energy is not propagated into calibrated environmental confidence intervals. Future studies should integrate probabilistic or survival-based lifetime estimation with inventory-based life-cycle assessment and uncertainty propagation.

5. Conclusions

This study addressed three research questions concerning the predictive value of historical EIS information, the relative performance of degradation models, and the credibility of model-derived lifetime estimates for sustainability interpretation. First, under the 80/20 chronological hold-out, the classical, pseudo-FO, and Mittag–Leffler FO formulations individually outperformed the cycle-only benchmark in 7/12, 8/12, and 8/12 batteries, respectively. The best-of-three result (10/12) is descriptive because model selection and evaluation used the same hold-out observations. Although the median paired RMSE improvements were positive, their interquartile ranges and exploratory battery-level bootstrap intervals included zero. Thus, a systematic impedance-related advantage was not established.
Second, the classical impedance-informed model most frequently achieved the lowest hold-out RMSE among the impedance-informed formulations (9/12 batteries), whereas neither fractional-order formulation showed systematic superiority. The pseudo-FO exponent is an empirical decay-shape parameter rather than a fractional-derivative order. The 31/36 rolling-origin best-of-three comparisons were correlated and subject to post-selection effects. Reintroducing three previously excluded batteries through alternative initial-capacity normalization preserved the qualitative findings but reduced median improvements. Under the frozen-EIS assumption, these results reflect associations involving historical impedance information, not the benefit of updated future EIS or an aging-specific causal effect. The validation was within-cell and does not demonstrate cross-cell generalization.
Third, short-horizon SOH accuracy did not ensure accurate pre-EOL lifetime forecasting. The five Reliable Observed classifications reflect deterministic, retrospective agreement after full-data refitting, not independently validated forecasts. In eight truncated-history pre-EOL backtests across four batteries, the cycle-only, classical, pseudo-FO, and Mittag–Leffler FO models met the 20% EOL-relative error tolerance in 2/8, 1/8, 4/8, and 5/8 cases, respectively. The corresponding RUL-relative tolerance was met in only 0/8, 0/8, 3/8, and 3/8 cases. These correlated backtests highlight the limitations of early lifetime forecasting, while the deterministic screening labels do not provide statistically calibrated uncertainty.
For screening-level environmental interpretation, five batteries were classified as Reliable Observed, four as Projected, and three as Rejected. The observed-EOL comparisons yielded changes of −2.52% to −10.59%, whereas positive changes for the right-censored projections (+8.02% to +14.87%) remained unverified scenarios. Alternative future-energy extrapolation changed the projected indicators by 0.31–0.80 percentage points but did not quantify EOL uncertainty. The reliability classifications also depended on the adopted SOH threshold. Because the fixed manufacturing burden cancels from the relative indicator, these results do not establish actual emission reductions or constitute a complete life-cycle assessment.
The main contribution is, therefore, a reliability-aware framework combining causal EIS alignment, chronological validation, persistent EOL detection, right-censoring, and truncated-history backtesting before lifetime-energy interpretation. Future work should address joint SOH–EIS forecasting, probabilistic EOL uncertainty, independent cross-cell validation, and inventory-based life-cycle assessment.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/app162311680/s1. File S1: Supplementary computational materials, including MATLAB source codes, processed battery datasets, model fitting and validation results, pre-EOL backtesting results, environmental assessment results, sensitivity analyses, reproduction instructions, and a file integrity manifest.

Author Contributions

Conceptualization, H.C. and E.C.; methodology, H.C., S.M.S. and E.C.; software, H.C.; validation, H.C. and S.M.S.; formal analysis, H.C. and E.C.; investigation, H.C. and E.C.; data curation, H.C.; writing—original draft preparation, H.C. and E.C.; writing—review and editing, H.C., E.C., and S.M.S.; visualization, H.C.; supervision, S.M.S. All authors have read and agreed to the published version of the manuscript.

Funding

This research made use of equipment acquired through the Scientific Research Projects Unit of Balıkesir University under Project No. BAP 2024/035 and benefited from methodological developments undertaken within that project. H.C. thanks the TUBITAK BIDEB-2219 program for a postdoctoral grant (1059B192400296).

Institutional Review Board Statement

Not applicable.

Data Availability Statement

The raw battery-aging data analyzed in this study are publicly available from the NASA Prognostics Data Repository (Battery Data Set) [20] at https://www.nasa.gov/intelligent-systems-division/discovery-and-systems-health/pcoe/pcoe-data-set-repository/ (accessed on 23 April 2026). The MATLAB analysis scripts, processed data tables, and instructions required to reproduce the reported results are provided as Supplementary Materials accompanying this article.

Acknowledgments

During the preparation of this manuscript, the authors used ChatGPT (OpenAI, GPT-5.6) and Claude (Anthropic, Claude Sonnet 5) for language refinement, manuscript organization, and consistency checking. Generative AI tools were also used to assist in reviewing computational workflows and improving the clarity of selected figures and textual descriptions. All scientific decisions, model formulations, calculations, data interpretation, and conclusions were independently verified by the authors. The authors reviewed and edited all AI-assisted outputs and take full responsibility for the content of this publication.

Conflicts of Interest

The authors declare no conflicts of interest. The funders had no role in the design of the study; in the collection, analyses, or interpretation of data; in the writing of the manuscript; or in the decision to publish the results.

References

  1. Vermeer, W.; Mouli, G.R.C.; Bauer, P. A comprehensive review on the characteristics and modeling of lithium-ion battery aging. IEEE Trans. Transp. Electrif. 2021, 8, 2205–2232. [Google Scholar] [CrossRef] [Scilit]
  2. Porzio, J.; Scown, C.D. Life-cycle assessment considerations for batteries and battery materials. Adv. Energy Mater. 2021, 11, 2100771, Correction in Adv. Energy Mater. 2022, 12, 2200477. [Google Scholar] [CrossRef] [Scilit]
  3. Ambrose, H.; Kendall, A. Effects of battery chemistry and performance on the life cycle greenhouse gas intensity of electric mobility. Transp. Res. Part D. Transp. Environ. 2016, 47, 182–194. [Google Scholar] [CrossRef] [Scilit]
  4. Xu, B.; Oudalov, A.; Ulbig, A.; Andersson, G.; Kirschen, D.S. Modeling of lithium-ion battery degradation for cell life assessment. IEEE Trans. Smart Grid 2016, 9, 1131–1140. [Google Scholar] [CrossRef] [Scilit]
  5. Tian, J.; Xiong, R.; Yu, Q. Fractional-order model-based incremental capacity analysis for degradation state recognition of lithium-ion batteries. IEEE Trans. Ind. Electron. 2018, 66, 1576–1584. [Google Scholar] [CrossRef] [Scilit]
  6. Yu, M.; Li, Y.; Podlubny, I.; Gong, F.; Sun, Y.; Zhang, Q.; Shang, Y.; Duan, B.; Zhang, C. Fractional-order modeling of lithium-ion batteries using additive noise assisted modeling and correlative information criterion. J. Adv. Res. 2020, 25, 49–56. [Google Scholar] [CrossRef] [Scilit]
  7. Borja-Jaimes, V.; Valdez-Martínez, J.S.; Beltrán-Escobar, M.; Cruz-Rojas, A.; Gil-Velasco, A.; Coronel-Escamilla, A. A review of fractional order calculus applications in electric vehicle energy storage and management systems. Mathematics 2025, 13, 2920. [Google Scholar] [CrossRef] [Scilit]
  8. Manivannan, R.; Vigneswar, N. A comprehensive review of fractional-order mathematical models for lithium-ion batteries: Historical progress, recent advancements, and future outlooks. J. Energy Storage 2025, 131, 117404. [Google Scholar] [CrossRef] [Scilit]
  9. Guerra, J.; Revelo, J.; Farinango, C.; González, L.; Collaguazo, G. Fractional-Order Degradation Modeling for Lithium-Ion Batteries with Robust Identification and Calibrated Uncertainty Under Cross-Cell Transfer. Batteries 2026, 12, 150. [Google Scholar] [CrossRef] [Scilit]
  10. Inui, Y.; Hirayama, S.; Tanaka, T. Temperature dependence of impedance spectrum of charge-transfer processes in lithium-ion batteries with nickel-manganese-cobalt cathode and graphite anode. J. Energy Storage 2021, 44, 103390. [Google Scholar] [CrossRef] [Scilit]
  11. Lourenço, J.; Rosado, L.S.; Ramos, P.M.; Janeiro, F.M. Measurement of battery aging using impedance spectroscopy with an embedded multisine coherent measurement system. Batteries 2025, 11, 227. [Google Scholar] [CrossRef] [Scilit]
  12. Qian, G.; Zheng, Y.; Li, X.; Sun, Y.; Han, X.; Ouyang, M. State of health estimation for lithium-ion batteries using impedance-based simplified timescale information. Appl. Energy 2025, 382, 125272. [Google Scholar] [CrossRef] [Scilit]
  13. Li, W.; Chen, J.; Quade, K.; Luder, D.; Gong, J.; Sauer, D.U. Battery degradation diagnosis with field data, impedance-based modeling and artificial intelligence. Energy Storage Mater. 2022, 53, 391–403. [Google Scholar] [CrossRef] [Scilit]
  14. Xiang, Y.; Chauhan, D.; Srinivasan, D. Battery State-of-Health Estimation with Embedded Impedance Spectrum Features Under Multiple Battery Chemistry and Temperature Conditions. Batteries 2026, 12, 77. [Google Scholar] [CrossRef] [Scilit]
  15. Liu, K.P.; Orfanoudakis, G.I.; Cruden, A.J.; Sharkh, S.M. In-Situ EIS for Batteries With a Three-Phase Neutral Point Clamped Converter Interface. IEEE Trans. Power Electron. 2026, 41, 20321–20333. [Google Scholar] [CrossRef] [Scilit]
  16. Zhu, R.; Shaukat, H.; Zahira, F.; Huzefa, H.M.; Bin Kaleem, M.; Li, H. State-of-Health Estimation for Li-Ion Batteries of Real-World Electric Vehicles: Progress, Challenges, and Prospects. Batteries 2026, 12, 174. [Google Scholar] [CrossRef] [Scilit]
  17. Zou, Q.; Wen, J. Battery state-of-health estimation incorporating model uncertainty based on Bayesian model averaging. Energy 2024, 308, 132884. [Google Scholar] [CrossRef] [Scilit]
  18. Ly, S.; Xie, J.; Wolter, F.E.; Nguyen, H.D.; Weng, Y. T-shape data and probabilistic remaining useful life prediction for Li-ion batteries using multiple non-crossing quantile long short-term memory. Appl. Energy 2023, 349, 121355. [Google Scholar] [CrossRef] [Scilit]
  19. Liu, Y.; Chen, S.; Li, P.; Wan, J.; Li, X. Status, challenges, and promises of data-driven battery lifetime prediction under cyber-physical system context. IET Cyber-Phys. Syst. Theory Appl. 2024, 9, 207–217. [Google Scholar] [CrossRef] [Scilit]
  20. Saha, B.; Goebel, K. Battery Data Set; NASA Prognostics Data Repository, NASA Ames Research Center: Moffett Field, CA, USA, 2007. [Google Scholar]
  21. Dascalu, A.; Cruden, A.J.; Sharkh, S.M. Experimental investigations into a hybrid energy storage system using directly connected lead-acid and Li-ion batteries. Energies 2024, 17, 4726. [Google Scholar] [CrossRef] [Scilit]
  22. Meng, Y.; Sun, Q.; Xu, J.; Bian, A.; Yang, Q.; Wang, Z.; Yang, Z.; Zhi, M. Multimodal State of Health Prediction for Lithium-Ion Batteries via Mamba-Based Fusion of Discharge Curves and Impedance Spectra. Batteries 2026, 12, 196. [Google Scholar] [CrossRef] [Scilit]
  23. Xing, Y.; Ma, E.W.; Tsui, K.L.; Pecht, M. An ensemble model for predicting the remaining useful performance of lithium-ion batteries. Microelectron. Reliab. 2013, 53, 811–820. [Google Scholar] [CrossRef] [Scilit]
  24. Mc Carthy, K.; Gullapalli, H.; Ryan, K.M.; Kennedy, T. Use of impedance spectroscopy for the estimation of Li-ion battery state of charge, state of health and internal temperature. J. Electrochem. Soc. 2021, 168, 080517. [Google Scholar] [CrossRef] [Scilit]
  25. Cuervo-Reyes, E.; Flückiger, R. One law to rule them all: Stretched exponential master curve of capacity fade for Li-ion batteries. J. Electrochem. Soc. 2019, 166, A1463–A1470. [Google Scholar] [CrossRef] [Scilit]
  26. Zhang, Q.; Li, Y.; Shang, Y.; Duan, B.; Cui, N.; Zhang, C. A fractional-Order kinetic battery model of lithium-Ion batteries considering a nonlinear capacity. Electronics 2019, 8, 394. [Google Scholar] [CrossRef] [Scilit]
  27. Tröltzsch, U.; Kanoun, O.; Tränkler, H.R. Characterizing aging effects of lithium ion batteries by impedance spectroscopy. Electrochim. Acta 2006, 51, 1664–1672. [Google Scholar] [CrossRef] [Scilit]
  28. Waag, W.; Käbitz, S.; Sauer, D.U. Experimental investigation of the lithium-ion battery impedance characteristic at various conditions and aging states and its influence on the application. Appl. Energy 2013, 102, 885–897. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.