Featured Application
Screening equal-capacity trap distributions under sustained contact loading and providing conditional equilibrium hydrogen fields for transient standstill and restart analysis.
Abstract
Hydrogen absorbed during bearing operation can redistribute under contact stress retained during loaded standstill. This study examines how trap spatial distribution changes equilibrium lattice hydrogen at equal total trap capacity. Using the published 100Cr6–81104-TV configuration and a selected total inventory of 1.5 wppm, fixed profiles were compared under maintained chemical potential and retained inventory. Established equilibrium relations were used to derive capacity- and occupancy-dependent concentration bounds, including finite limits on local trap density. Under retained inventory, allocating traps to locations with a higher occupancy at a common activity increased storage and lowered lattice hydrogen. At the maintained chemical potential, the trap position changed the trapped hydrogen but left the lattice hydrogen unchanged. At 90 °C, the low-capacity benchmark gave a negligible positional effect. A theoretical capacity-matched state gave a 3.07% difference between two layers, while the density-limited mean range was 19.28%. Inventory, binding-energy, and residual-stress sensitivities identify the conditions governing these comparisons. Conditional linear relaxation bounds show that excess-capacity states can contain very slow modes. The concentration bounds screen spatial trapping effects within the prescribed equilibrium model; their application to an operating hold requires evidence of sufficient relaxation and the assumed hydrogen boundary.
1. Introduction
Rolling-bearing steels can absorb hydrogen supplied by hydrogen-containing service media, the tribo-chemical decomposition of lubricants, and electrochemical reactions involving moisture at steel surfaces [1,2]. These entry routes are relevant to bearings in hydrogen compression equipment, offshore wind turbines, and automotive transmissions, with their contribution depending on the local exposure and lubrication conditions [3]. Once absorbed, hydrogen can diffuse into steel and occupy lattice sites and microstructural traps.
Stopping rotation leaves the absorbed hydrogen in a bearing available for further diffusion. When support loads or assembly preload remain, the contact can also be maintained at approximately the same raceway position during a shutdown or operating pause. Stationary bearing loading has been reported for automotive transmission applications [4]. The retained stress contributes to the hydrogen chemical potential, so hydrogen can continue to diffuse and exchange with microstructural traps while the contact position is fixed. Consequently, the hydrogen state at restart depends on redistribution during the hold as well as uptake during previous operation. A stationary contact calculation addresses this part of the operating history when the retained load and temperature vary sufficiently slowly.
Hydrogen effects on bearing performance have been investigated using charged steel balls and bearing-steel specimens [5,6]. Experiments have also examined the hydrogen-assisted butterfly and white-etching crack formation [7], microcrack formation [8], and the development of white-etching areas under rolling contact fatigue [9]. These observations connect hydrogen exposure with damage development and motivate an examination of the causal role of microstructural alterations [10]. Connecting the total hydrogen content with local damage requires distinguishing hydrogen in lattice sites from hydrogen stored in traps.
Hydrogen damage depends on the interaction of hydrogen with the host material and its deformation processes [11,12,13]. Bearing-steel microstructures contain dislocations and phase interfaces whose populations also influence strength and fatigue resistance [14]. Some of these features provide sites at which hydrogen is energetically favored relative to ordinary lattice sites. The hydrogen stored in such traps is determined by both their number and their occupied fraction [15]. A region containing more traps can therefore have a higher total hydrogen concentration without having a higher lattice concentration. If the total hydrogen inventory is retained, a greater amount stored in traps leaves less hydrogen in the lattice. The question is whether placing a given trap population at different depths changes the lattice hydrogen under the retained contact stress, independently of changing its total number or binding energy.
The 100Cr6 steel used in 81104-TV cylindrical roller thrust bearings provides a documented configuration for examining this question. Khader et al. [16] investigated the bearing damage using experiments and a hydrogen diffusion model incorporating dislocation trapping and residual stress. Baur et al. [17] subsequently examined residual stresses, hydrogen trapping, and premature damage in the same bearing type. Related experiments link lubricant degradation to hydrogen-assisted rolling contact fatigue [18], while recent work examines conductive lubricants as a means of controlling hydrogen-related bearing damage [19]. These studies establish the relevance of the hydrogen supply and material state and provide the literature basis for the present calculation.
Continuum models describe the hydrogen redistribution through stress-assisted transport and reversible trapping [20,21]. Static and rolling-contact calculations distinguish the response to a sustained stress field from that to a moving contact [22,23]. At chemical equilibrium, we see the concentration and stress contributions to hydrogen chemical potential balance; a nonuniform concentration can therefore persist without the net transport [24]. Reversible trapping relates the occupied fractions of trap and lattice sites [25]. The hydrogen boundary determines how much hydrogen is available to fill these sites: an external reservoir can maintain the chemical potential by supplying hydrogen, whereas a retained inventory must be shared between the lattice and trap sites [26,27]. Under prescribed stress and unchanged host properties, trapping consequently has different effects under these two boundaries. Cyclic loading [27] and heterogeneous microstructures [28] introduce the further dependence on transport history and spatial variation.
A small difference between two trap-rich layers does not establish that trap depth is unimportant. The layers may sample similar occupancies, or the entire trap population may store too little hydrogen for any spatial arrangement to have an appreciable effect. An upper bound that includes both the trap count and occupancy is needed to distinguish these possibilities. This distinction determines whether a detailed depth characterization can materially change the assessment.
Applying this comparison requires material quantities that correspond to the equilibrium model. Effective diffusivity measured in hardened 100Cr6 [29] describes transport, while changes following rolling/sliding tribo-testing [30] characterize a modified trapping state. Hydrogen contents associated with surface-initiated damage [31] include the contributions sampled by the measurement. Thermal desorption further depends on diffusion, specimen dimensions, heating history, and trap saturation [32]. Together, these studies identify inventory, trap capacity, and occupancy as the quantities needed to connect measured hydrogen behavior with its local equilibrium distribution.
Trap distributions reflect both material preparation and the preceding contact history. Heat treatment changes the phases and interfaces available for trapping in bearing steel [14,15]. Surface deformation also modifies the trapping state: rolling/sliding tests on 100Cr6 produced a deformed surface layer together with altered hydrogen desorption behavior [30]. Local modification is also possible by ion implantation. Brass et al. [33] reported that nitrogen implantation changed trapping in an approximately 100–120 nm surface layer of low-carbon steel, together with hydrogen solubility and entry behavior. This example establishes that processing can modify near-surface trapping; its affected depth differs substantially from the micrometer-scale layers compared below. Comparing profiles at equal capacity and binding energy isolates the contribution of position within the combined changes produced by processing.
The present study uses established stress-assisted equilibrium and trapping relations to compare spatial trap distributions at equal total capacity. Capacity- and occupancy-dependent concentration bounds are derived, followed by tighter bounds under prescribed local density limits. Their application to a sustained Hertz contact identifies when a selected trap arrangement approaches the range permitted by the model. Geometry, primary load, and source material inputs follow the 100Cr6–81104-TV literature [16,17]. Inventory, binding energy, residual stress, load, and closed-domain size are varied to assess the physical conditions controlling the comparison. The resulting fields provide conditional equilibrium references for transient analyses of standstill and restart.
2. Theoretical Analysis and Calculation Procedure
2.1. Bearing Configuration and Material Parameters
Figure 1 relates the 81104-TV thrust bearing to the local contact model. The bearing comprises a shaft washer, a housing washer, and an axial roller and cage assembly. Its bore diameter, outside diameter, and overall height are 20, 35, and 10 mm, respectively [34]. The calculation holds the axial load, temperature, contact position, and trap profile constant. The force represents the load retained by the support or preload arrangement after rotation stops. Previous hydrogen uptake is represented by the prescribed inventory or reservoir activity, from which the equilibrium distribution under the retained load is calculated. Tangential traction is omitted. The baseline uses the normal Hertz field with zero residual stress; a prescribed residual field is added in Section 3.6. The preceding mechanical loading path is not simulated, and the trapping state is fixed during the hold.
Figure 1.
Bearing geometry and loaded-standstill idealization: (a) simplified axial section of the 81104-TV bearing, with overall dimensions from Schaeffler [34]; (1) shaft washer, (2) roller and cage assembly, and (3) housing washer; and (b) the local cylinder–raceway contact viewed normal to the roller axis, with nominal roller dimensions from [17]. The connected material volume is denoted by . The 8 kN retained load and 800 N per-roller load correspond to the reduced ten-roller configuration [16,17].
Table 1 summarizes the reference bearing configuration. Mechanical and transport inputs were taken from the model of Khader et al. [16], and nominal roller dimensions were taken from the related bearing study [17]. The ten loaded rollers correspond to the reduced experimental configuration in these studies. The local Hertz field is determined by the per-roller load and nominal roller geometry; the overall dimensions in Figure 1 identify the bearing assembly. The reference load of 8 kN and temperature of 90 °C are held constant to represent the retained-contact stage. The source rotation speed provides the operating-time reference. Table 1 and Table 2 identify the source locations of the physical inputs, and Section 2.2, Section 2.3, Section 2.4 and Section 2.5 define the calculation domain, trap profiles, and parameter ranges.
Table 1.
Common bearing inputs used from the start of the calculation.
Table 2.
Source hydrogen parameters and the effective BCC matrix convention used for site conversion.
Under equal load sharing, the axial force of 8 kN gives a load of 800 N per roller. The central contact is represented by a cylinder against a flat raceway, with a reduced radius mm and nominal contact length mm. For identical elastic materials, the reduced modulus , line load , contact half-width , and maximum contact pressure are given by [35]
Equation (1) gives , , and . The subscript ref denotes the 8 kN contact used to define all fixed physical dimensions. The calculated pressure agrees with the approximate Hertz pressure of 1.7 GPa reported in [17]. This agreement supports the reconstruction of the central contact field.
Table 2 lists the hydrogen parameters taken from the 100Cr6–81104-TV model of Khader et al. [16], together with the effective matrix convention used here. The positive binding-energy magnitude corresponds to the negative binding-energy convention in [16]. is the molar density of available lattice sites; six tetrahedral sites per solvent atom are used for the idealized BCC matrix.
The calculations use the CODATA molar gas constant, 8.31446261815324 J mol−1 K−1, and Avogadro constant, 6.02214076 × 1023 mol−1 [36]. The hydrogen molar mass is taken as 0.001008 kg mol−1 (1.008 g mol−1), consistent with the abridged standard atomic weight [37]. The reference temperature of 90 °C is 363.15 K.
Using the site definitions and dislocation law in Section 2 of [16], the conversion to molar site densities is
Here, is Avogadro’s constant, is the Burgers-vector magnitude, and denotes the equivalent plastic strain. A consistent idealized BCC matrix is adopted, with lattice parameter and . The source dislocation law supplies the initial low-capacity benchmark; it is not extrapolated to generate the independently prescribed high-capacity cases.
The crystal lattice is represented as a continuum of interstitial sites with uniform site density, and its hydrogen population follows the lattice occupancy in Equation (7). Dislocations supply the separate trap-site population through Equation (2), with affinity represented by the binding energy in Table 2. The BCC description is an effective α-Fe approximation. It does not resolve martensitic tetragonality, retained austenite, individual dislocation cores, or crystallographic orientations. Interphase boundaries are not assigned a separate site density or binding energy; additional families are discussed in Section 4.3.
With the initial dislocation density of 1010 m−2, Equation (2) gives , , and . This initial value from the source model defines a low-capacity benchmark. It is not treated as the total trap population of a hardened bearing after operation. Higher capacities are prescribed separately to examine the storage comparable with the retained inventory; their dislocation-density equivalents follow from the same BCC conversion.
Section 3.2 of Khader et al. [16] reports an initial concentration of 1.5 ppm together with 0.227 mol m−3. These values do not establish a consistent mass–ppm conversion. An inventory of 1.5 wppm is prescribed here on a mass basis as a selected input. Using the steel density in Table 2, the corresponding mean total molar concentration is
where and the steel density is 7874 kg m−3. Thus, 1.5 wppm corresponds to 11.7173 mol m−3. Hereafter, denotes this mean total molar concentration. The source-reported 0.227 mol m−3 equals 0.0291 wppm under these definitions, a factor of 51.62 below the selected inventory. Since the source convention cannot be resolved uniquely, both inventories are evaluated in Section 3.6 at fixed capacity and after capacity rematching. The initial total inventory is partitioned between lattice and trap sites. The unloaded partition is obtained from the same equilibrium and conservation relations as the loaded state.
The prescribed inventory represents hydrogen already present when the loaded hold begins; no preceding charging duration is imposed. Prior exposure is therefore represented by the retained hydrogen amount, and the calculation determines its equilibrium partition under the maintained load and temperature. The hold duration governs how closely a real contact approaches this state, as discussed in Section 2.5 and Section 4.2.
2.2. Contact Stress and Hydrogen Equilibrium
The surface coordinate is denoted by , and the depth into the half-space by . With the tensile stress taken as positive, the normal pressure is within the contact and zero outside. Defining and , the plane-strain hydrostatic stress, equal to one third of the stress trace, is
For , Equation (4) can also be written as
where the square-root branches are continuous in the upper half-plane. The limiting values are and . The nonnegative kernel in Equation (4) makes the hydrostatic stress compressive throughout the prescribed field. Figure 2 compares this stress with the von Mises stress and marks the layers defined in Section 2.4. Hydrostatic stress supplies the mechanical contribution to the chemical potential used below, whereas von Mises stress measures the deviatoric intensity relevant to the elastic yield check. Their extrema therefore need not identify the same position.
Figure 2.
Hertz contact field for the 81104-TV reference at 8 kN: (a) hydrostatic stress distribution; and (b) centerline hydrostatic and von Mises stresses. The shaded bands indicate the prescribed shallow and subsurface layers.
Let and denote the occupied fractions of lattice and trap sites, respectively. The finite-site chemical potential contains a concentration contribution and a hydrostatic-stress contribution [20,21]:
Compression raises the mechanical contribution in Equation (6) because the tensile stress is positive and . At equilibrium, this increase is balanced by a lower lattice occupancy at the same chemical potential. A spatially uniform chemical potential defines the activity , which sets the overall concentration level. With and , the lattice and single-family reversible-trap occupancies are [25]
The single trap family is assumed to remain in local thermodynamic equilibrium with lattice hydrogen. The adopted binding energy specifies the equilibrium occupancy relation; it does not establish an exchange rate. Stress-independent binding is used with equal hydrogen partial molar volumes in lattice and trap sites. The normalized total concentration and its volume mean are
where angle brackets denote a volume average over the connected material volume. The density specifies the available trap sites and remains fixed. Hydrogen redistribution changes the occupied fractions and . For an ideal reservoir that maintains activity, Equation (7) fixes the lattice concentration from the stress field alone. Additional trap storage can be supplied by the reservoir, so changing the trap profile changes trapped and total hydrogen without changing the equilibrium lattice hydrogen. The same traps can still retard hydrogen entry during a transient or affect the response to cyclic loading [27].
When the total hydrogen inventory is retained, the activity must instead satisfy conservation within the closed volume:
The positive derivative gives a unique solution for . Each comparison retains the , , , temperature, and stress field, so a difference in activity arises only from spatially different trap storage. The common unloaded state is obtained by setting in Equation (9). Figure 3 summarizes the two boundaries. In the closed case, the hydrogen amount in is conserved and the boundary-normal flux is zero.
Figure 3.
Hydrogen boundary conditions under sustained contact loading: (a) an external reservoir maintains activity and permits hydrogen exchange; and (b) a closed volume retains its total hydrogen, and activity is determined by conservation. Dots and occupied-trap symbols schematically illustrate hydrogen partitioning.
To examine the effect of trap spatial distribution, consider , where and have the same total trap count. Here, interpolates between the prescribed spatial profiles. Differentiating Equation (9) yields
The numerator of Equation (10) is the change in stored hydrogen associated with changing the profile at the current activity. If occupancy is spatially uniform, this numerator vanishes because the two profiles have equal total trap count. Conversely, a profile that stores more hydrogen at the same activity lowers the activity required by conservation. The denominator is the positive change in total storage with logarithmic activity. For two equilibrated states satisfying , the local lattice-concentration ratio obeys
The activity ratio therefore bounds the concentration change at every position. At fixed stress and host properties, changing the trap profile shifts the overall lattice concentration through one common activity. The ordering of lattice concentration with hydrostatic stress is retained, so a trap-rich layer does not independently create a lattice-concentration maximum. This separates a local increase in trapped hydrogen from a local increase in lattice hydrogen.
2.3. Bounds on the Effect of Trap Spatial Distribution
The largest possible change in stored hydrogen is limited first by the number of trap sites. Since , conservation gives the following bounds for any two equal-count distributions when :
If a relative change in mean lattice concentration is required, Equation (12) gives the necessary capacity condition,
Equation (13) excludes a specified mean-concentration change when the available trap count is too small. The remaining contribution is governed by occupancy contrast: nearly uniform or nearly saturated occupancy leaves little difference in stored hydrogen. For , the site count alone gives no positive lower bound on the lattice hydrogen. Equation (12) then supplies no finite relative bound, while the occupancy-dependent bounds below remain applicable.
The stress and occupancy effects can be included by defining . Since trap occupancy increases monotonically with , its weighted average satisfies
for every nonnegative trap distribution with mean . Two limiting activities are obtained from
The expression containing the larger trap occupancy reaches the prescribed inventory at the smaller activity. Applying Equation (14) at equilibrium consequently gives
The corresponding bounds, expressed as percentages relative to the smaller concentration, are
The pointwise bound follows from Equation (11) and also bounds the mean concentration change. For dilute lattice hydrogen, concentration is nearly proportional to activity, so the two bounds nearly coincide. Each mean range uses its own lower mean concentration as the denominator. In obtaining the unrestricted bound, traps may concentrate arbitrarily close to a stress extremum; the bound describes the range permitted by capacity and occupancy before local density or processing constraints are imposed.
For the present contact, occurs at the surface center, while occurs on the unloaded surface outside contact. At 8 kN and 90 °C, . Although the stress-free surface itself has zero volume, its value remains a valid extremum for Equation (14), approached by traps concentrated in a sufficiently thin neighboring region.
For an illustrative finite-density comparison, this study prescribes a background factor , a peak factor , and the same mean trap density. These prescribed factors are illustrative rather than measured density limits for 100Cr6. They retain a nonzero background while concentrating the remaining capacity in one-eighth of the volume, so the effect of position can be assessed at equal total capacity. The constraints are
The limiting profiles follow by comparing storage at fixed activity. Moving a small amount of capacity from a lower-occupancy location to a higher-occupancy location increases the stored hydrogen without changing the total number of traps. Repeating this comparison maximizes storage when the peak density occupies the fraction with the largest ; reversing the ordering minimizes storage. Since occupancy increases with at every activity, the limiting distributions are
where each indicated region occupies fraction of the total volume. The profile with greater storage at fixed activity reaches the conserved inventory at a lower activity. Substitution into Equation (9) therefore gives the minimum and maximum lattice concentrations under the density limits. Any further restriction, such as requiring the trap-rich region to be a horizontal layer, can only narrow this range.
2.4. Trap Distributions and Calculation Conditions
The reference volume extends over and , corresponding to a width of 544.35 µm and a depth of 272.18 µm. The illustrative profiles are selected to isolate the positional effect and are not fitted to a measured microstructure. The shallow layer occupies 0–34.02 µm, and the subsurface layer occupies 68.04–102.07 µm. The domain spans eight reference contact half-widths laterally and four in depth. The two equal-thickness bands, 0–0.5 and 1–1.5 reference half-widths, are prescribed to compare contact-adjacent and deeper traps without changing their count; their micrometer values follow from Equation (1). Alongside a uniform distribution, each layered distribution is specified by
Figure 4 compares the uniform and layered profiles using a depth strip and its corresponding trap-density curve. Each enriched layer occupies one-eighth of the compartment depth, giving the same mean trap density with the prescribed background and peak values.
Figure 4.
Alternative fixed trap profiles: (a) uniform traps (gray shading), (b) a shallow enriched layer (red shading), and (c) a subsurface enriched layer (blue shading). Each profile remains fixed during its own hydrogen-equilibrium calculation. The strip shows the depth arrangement and the adjacent curve gives the normalized trap density. All three profiles have the same depth integral and total trap count. Dashed lines mark the common mean density in the layered profiles.
Each profile is fixed throughout its hydrogen-equilibrium calculation. Redistribution refers to the exchange of hydrogen among the prescribed sites, while the sites themselves remain in place.
The physical layer depths remain fixed when the axial load is varied from 2 to 12 kN; the current contact half-width changes according to Equation (1). To compare the equilibrium in closed domains of different sizes, the half-width and depth are increased from to . The original patterned core is retained, and the added material contains uniform traps. The mean total hydrogen and mean trap density remain fixed. Equal-count comparisons therefore apply within each domain, while enlarging the domain increases both total hydrogen and total trap count. This calculation compares closed systems of different sizes; it does not simulate exchange with surrounding material at a different initial concentration.
The trap capacity and occupancy are characterized by
For and , conservation becomes
Here, compares maximum trap storage with total inventory, while sets the occupancy scale together with activity. A large alone does not establish saturation because activity also changes with capacity. The state map uses and at fixed contact, temperature, and binding energy. These axes specify and . At 90 °C and 60 kJ mol−1, the inventory range is 2.54 × 10−7–2.54 wppm, covering both inventories examined explicitly and a weak through strong occupancy response. The full rectangle corresponds to mean dislocation-density equivalents of approximately 3 × 102–3 × 1016 m−2. It is a theoretical exploration of storage regimes; literature scales contextualize selected points only. The capacity-matched comparison sets at 1.5 wppm, with a mean density equivalent of 1.75 × 1015 m−2. Its capacity is prescribed independently of the source strain law.
The signed difference between the two layers is defined by
A positive indicates a lower mean lattice concentration for the subsurface layout. The denominator is the subsurface mean, so measures a relative concentration difference between equally prepared states.
2.5. Numerical Procedure and Characteristic Times
Numerical calculations were performed using Python 3.12.14 with NumPy 2.3.5 and SciPy 1.17.0. NumPy was used for array operations and Gauss–Legendre quadrature, while SciPy was used for bracketed root finding and independent numerical integration. The equilibrium calculations depend only on the equations, physical inputs, and prescribed comparison conditions reported here; no additional project-specific measurements are required as numerical inputs.
Figure 5 summarizes the numerical implementation. Inputs were converted to SI units before calculating the Hertz field. Composite tensor-product Gauss–Legendre quadrature was applied on intervals [−4, −1], [−1, 1], and [1, 4] and intervals [0, 0.5], [0.5, 1], [1, 1.5], and [1.5, 4]. Product weights were divided by the dimensionless area 32, so their sum is unity. Enlarged domains were partitioned additionally at the fixed patterned-core boundaries and normalized by their new area. Tabulated comparisons use order 64 per subinterval; load and capacity curves use orders 32 and 24, respectively; and domain-size calculations use order 48. The state map uses 51 logarithmically spaced values and 49 values with order 10; its largest sampled value is refined at order 64.
Figure 5.
Numerical workflow for equilibrium hydrogen partitioning. Maintained chemical potential prescribes activity, whereas retained inventory requires a scalar conservation solve. Time scales and conditional relaxation bounds are evaluated separately.
For the maintained chemical potential, the unloaded activity was obtained from conservation and then held fixed while evaluating Equation (7) in the loaded field. For the retained inventory, Brent’s method solved Equation (9) on , with absolute tolerance 10−14 and relative tolerance 9 × 10−16. A logistic evaluation of the occupancies avoids overflow. The unrestricted bounds follow from Equation (15), using the analytic stress extrema. For density-limited bounds, points are ranked by stress and assigned peak density until the enriched weighted fraction reaches 1/8. If the remaining fraction is at the final point, its normalized density is ; the remaining points retain 0.2. This enforces the weighted volume fraction and total capacity.
For the smallest differences, the difference of two conservation equations is solved directly for , with absolute tolerance 10−26 and relative tolerance 9 × 10−16 on [−120, 120]. For , the occupancy increment is , using the complementary logistic function for . An equal trap count permits the zero-shift profile term to use , avoiding cancellation near saturation. Table 3 reports the BCC low-capacity convergence as well as the larger matched-capacity differences. Independent direct solves at 65-digit precision on the same order-8 quadrature, using the original conversion, agree with the stable double-precision difference to the 2.1 × 10−15 relative discrepancy.
Table 3.
Numerical verification. Extra digits demonstrate numerical convergence and do not represent material-parameter accuracy.
For the arbitrary-profile check, quadrature order 32 was used, and random coefficients were generated with NumPy’s PCG64 generator using a fixed seed of 42. In the order , sixteen 4 × 4 standard-normal coefficient arrays were drawn per capacity in row-major order. Each field is the sum of for . After subtracting the sampled maximum of , exponentiation and division by the weighted mean give a nonnegative normalized profile. All 48 activities satisfy Equation (16); the maximum capacity-normalization error is 3.4 × 10−16 after rounding upward. These profiles test the unrestricted bound and need not obey the finite density limits.
Diffusivity controls how rapidly a distribution develops, but not the equilibrium solution at a specified temperature. It is used here to compare the length and time scales relevant to the stationary assumption. The lattice-diffusion law uses the prefactor and activation energy adopted in Table 2 of [16]
For locally equilibrated traps, the derivative of normalized total concentration with respect to lattice occupancy is
The storage factor measures how much total hydrogen must be transferred to produce a given local change in lattice occupancy. Reversible traps with an appreciable occupancy response increase this requirement and can therefore retard redistribution. The characteristic lattice-diffusion time and length are compared with the shaft period through
In Equation (26), n is the source shaft speed of 700 rpm [16,17], and the factor 60 converts minutes to seconds. The shaft period provides an operating-time reference. The equilibrium solution requires no time stepping. Lattice-diffusion scales alone do not establish equilibration of trapped hydrogen; Section 4.2 derives conditional bounds on linear relaxation including trap storage. Transient formulations [38,39] are needed for a specified initial distribution, thermal history, and boundary exchange.
3. Results
3.1. Hydrogen Partitioning Under Contact Loading
Under both hydrogen boundaries, the strongest depletion of lattice hydrogen occurs at the center of the loaded surface (Figure 6). For uniform traps at 8 kN and 90 °C, the surface-center concentration is 0.3335 of its unloaded value at a maintained reservoir activity and 0.3860 when the total inventory is retained. The boundary condition changes the concentration level while preserving its spatial ordering with hydrostatic stress.
Figure 6.
Equilibrium hydrogen partitioning for uniform traps at 8 kN, 90 °C, , initial total inventory 1.5 wppm, and low capacity : (a) lattice concentration at maintained activity; (b) lattice concentration at retained inventory; and (c) trap occupancy at retained inventory. Panels (a,b) share the same unloaded lattice reference and color scale.
The concentration decrease balances the increase in chemical potential caused by compression. At maintained activity, Equation (7) gives this response directly. In the closed volume, hydrogen displaced from the strongly compressed region must remain elsewhere in the same volume. Conservation therefore raises the activity and increases lattice hydrogen in less compressed regions. This increase is insufficient to offset depletion at the surface center. Hence, the subsurface maximum of von Mises stress in Figure 2b cannot be used to locate the highest equilibrium lattice concentration. The two fields characterize different parts of the contact problem.
For the selected inventory, and . The low-capacity benchmark has and . Thus, even complete filling stores only a small fraction of the total hydrogen. Trap occupancy ranges from approximately 0.999562 to 0.999854 at the quadrature points, with a trap-weighted mean of 0.999827. Figure 6c shows that compression lowers occupancy near the surface center, although the sites remain almost completely occupied.
The trap-weighted mean occupancies for the shallow and subsurface profiles are approximately 0.999814 and 0.999825, respectively. The subsurface profile stores slightly more hydrogen at an equal trap count and leaves slightly less in the lattice. Equation (23) gives , corresponding to only 7.49 × 10−10 mol m−3, or 9.59 × 10−11 wppm. Both low capacity and nearly saturated occupancy restrict the positional response.
Table 4 compares the low-capacity benchmark with capacity matching at the same 1.5 wppm inventory, 8 kN load, 90 °C temperature, and 60 kJ mol−1 binding energy. Absolute mean concentrations and trapped fractions distinguish a percentage change in lattice hydrogen from its share of the total inventory. At low capacity, the three profile means coincide at the displayed precision.
Table 4.
Absolute partitioning and relative comparisons for the low-capacity benchmark and the theoretical capacity-matched case. Concentrations are volume means; trapped fractions are percentages of total hydrogen.
3.2. Influence of Trap Capacity
For the low-capacity benchmark, the site count alone gives a mean-concentration-change bound of 5.71 × 10−4%. Including the stress range and occupancy reduces the pointwise bound to 1.67 × 10−7%. The density limits in Equation (18) further reduce the mean bound to 3.77 × 10−8%. Figure 7a shows the selected-layer difference below both placement bounds as capacity varies at fixed inventory.
Figure 7.
Capacity dependence at fixed inventory 1.5 wppm, 8 kN, 90 °C, and : (a) selected-layer difference, density-limited mean bound, and unrestricted mean bound; and (b) trap-weighted occupancy and fraction of total hydrogen in lattice sites for uniform traps. Each percentage in (a) uses its own lower mean as denominator. The gray vertical dotted lines mark the low-capacity benchmark in (a) and capacity matching at r = 1 in (b).
Figure 7a compares the selected layers, density-limited allocations, and unrestricted placement according to their spatial freedom. Even unrestricted placement gives a negligible range at low capacity. Selecting other depths therefore cannot produce an appreciable equilibrium change while this capacity and the other model inputs are retained.
At , the selected-layer difference is 3.07%, corresponding to 0.00472 mol m−3 or 0.000604 wppm. The density-limited and unrestricted mean ranges are 19.28% and 72.39%, respectively. Table 5 identifies the different lower and upper means used in these comparisons. Figure 7b shows that increasing capacity transfers a larger share of the inventory to traps, leaving less lattice hydrogen and increasing the relative effect of an occupancy difference.
Table 5.
Distinct mean-concentration ranges at matched capacity, 1.5 wppm, 8 kN, 90 °C, and . Each range is .
Increasing capacity beyond matching does not produce a continuously increasing layer effect: falls to 2.45% at and 0.506% at . Capacity also changes the activity and the response of trap occupancy. The concentration ranges in Table 5 are calculated from separate lower states; they are not reductions from a common reference microstructure.
3.3. Combined Effects of Capacity and Occupancy
Figure 8 extends the comparison to different capacities and inventories at the same contact pressure. The largest sampled layer difference is 5.67%, near , and ; order-64 refinement gives 5.67457%. This point lies on the upper boundary. It is the largest sampled value within the prescribed scan, not a global maximum over physically realizable bearing states.
Figure 8.
Theoretical capacity–inventory map at 8 kN, 90 °C, and : (a) absolute selected-layer difference; and (b) unrestricted mean-concentration bound. Inventories and capacities follow and . The star marks the low-capacity benchmark at 1.5 wppm. Labelled contours are percentages, each with the lower mean of its own comparison as denominator. The physical ranges and their interpretation are given in Section 2.4.
Figure 8 separates the overall storage constraint from the effect of the selected layer geometry. Panel (b) gives the maximum range allowed by unrestricted trap placement. Panel (a) shows the part of that range accessed by the two layers. An appreciable bound combined with a small layer difference identifies the scope for improving the spatial profile.
For an illustrative 1% change in mean lattice concentration, Equation (13) requires even if the full trap capacity could contribute to the difference. At the selected inventory and binding energy, the unrestricted mean bound reaches 1% only at . Accounting for occupancy is therefore much more restrictive than counting sites alone. The BCC conversion gives density equivalents of 1.73 × 1013 and 1.48 × 1015 m−2, respectively. These are capacity-based screening conditions within the adopted model.
The 1% objective therefore defines two stages of screening: sufficient capacity to permit the target change, followed by a spatial arrangement that produces the required occupancy contrast under the contact field.
3.4. Influence of the Spatial Distribution
For the prescribed density limits, allocating the peak trap density to the least compressed region gives the lowest lattice hydrogen, while allocating it to the most compressed region gives the highest value (Figure 9). The background density, peak density, and total trap count are identical. The comparison therefore tests where a given population stores hydrogen most effectively within the specified contact field.
Figure 9.
Allocations giving (a) minimum and (b) maximum lattice concentration under normalized local density limits 0.2 and 6.6 at equal mean capacity. Shading denotes trap density. The geometry follows the 8 kN Hertz field and is independent of prescribed capacity for the common positive partial molar volume. The quoted concentration range uses 1.5 wppm, , 90 °C, and .
At fixed activity, Equation (7) gives a higher trap occupancy where hydrostatic compression is weaker. Assigning more sites to those locations increases the stored hydrogen, so the conservation of the retained inventory requires a lower activity and, hence, a lower lattice concentration throughout the connected volume. This explains the ordering in Figure 9.
At matched capacity, the 19.28% density-limited range and 3.07% layer difference describe different spatial freedoms and use different lower-state denominators (Table 5). The limiting allocations follow the two-dimensional stress field, whereas the selected layers assign the same density across horizontal bands. The comparison identifies the additional range permitted when this geometric restriction is removed.
3.5. Influences of Load and Closed-Domain Size
Increasing the axial load from 2 to 12 kN increases the layer difference from approximately 1.02 × 10−9% to 1.11 × 10−8% at low capacity, and from 0.516% to 5.15% at matched capacity (Figure 10). The roller geometry, physical layer depths, and inventory remain fixed. Load changes both the magnitude and spatial extent of stress sampled by the layers. This occupancy contrast has little effect at low capacity and a much larger effect when traps store a substantial share of the inventory.
Figure 10.
Load dependence at fixed 1.5 wppm, 90 °C, and : (a) low capacity ; and (b) matched capacity . Curves show the selected-layer difference and unrestricted mean bound, with separate lower-state denominators. The physical domain, layer depths, and roller dimensions remain fixed; the dotted line marks 8 kN.
The nominal maximum von Mises stress is approximately 0.927 GPa at 8 kN and 1.136 GPa at 12 kN. The latter is 95.0% of the adopted initial yield strength. Since Hertz stress scales with the square root of the per-roller load, a 10% load increase raises this ratio to approximately ; reducing the yield strength by 5% also exhausts the nominal margin. The 12 kN case is therefore an upper-end sensitivity test of the ideal elastic model. The central line-contact check does not establish elasticity near the roller ends or roughness features.
The layer effect decreases across the closed-domain size comparison in Figure 11. Increasing the half-width and depth from to reduces from 6.39 × 10−9% to 4.45 × 10−10% at low capacity and from 3.07% to 0.221% at matched capacity. Added material contains uniform traps at the same mean inventory and capacity. Consequently, both total hydrogen and total trap count increase, while the fixed patterned core supplies a smaller fraction of the total storage contrast.
Figure 11.
Equilibrium comparison of closed domains of different sizes at 1.5 wppm, 8 kN, 90 °C, and : (a) low-capacity benchmark; and (b) . Only the original core is patterned; added material contains uniform traps at the same mean capacity and inventory. Symbols denote calculated domain sizes. This is not a transient exchange calculation.
Figure 11 quantifies the dilution of the storage contrast from a fixed patterned core within progressively larger closed systems. The unrestricted bound allows profiles to differ throughout each enlarged domain and therefore addresses a broader placement freedom.
3.6. Inventory, Material-Parameter, and Residual-Stress Sensitivity
Table 6 compares the two inventory interpretations. Reducing from 11.7173 to 0.227 mol m−3 at fixed capacity changes both and ; the latter decreases from 5909.5 to 114.49. The low-capacity effect remains negligible. Keeping while reducing inventory gives ; rematching to the lower inventory instead gives 2.58%. Capacity rematching changes a second physical input and is distinguished from inventory-only sensitivity.
Table 6.
Inventory sensitivity at 8 kN, 90 °C, and .
Table 7 varies the capacity, binding energy, temperature, and hydrogen partial molar volume while holding the remaining physical inputs fixed. The density sweep maps dislocation-density equivalents to capacity through the BCC conversion. Increasing the binding energy from 20 to 60 kJ mol−1 at fixed increases from 0.00163% to 3.07%. A ±10% capacity change around produces an asymmetric response because it moves the system across capacity matching. These independently selected perturbations quantify sensitivity rather than statistical uncertainty.
Table 7.
One-at-a-time sensitivity at 1.5 wppm and 8 kN. Except for the varied input, the baseline uses , 90 °C, and . The density rows prescribe from Equation (2).
For residual-stress sensitivity, and the prescribed in-plane components are , with all other residual components being zero. The depth-integrated force and first moment vanish, and the hydrostatic contribution is . A positive denotes surface compression. This idealized, uncalibrated field is added to the Hertz field before solving conservation and recomputing the ranked allocations.
Table 8 shows that changing the residual stress can reverse the selected-layer ordering. The allocation argument remains valid because it ranks the trap occupancy at common activity, but the limiting regions and numerical bounds follow the total stress field. The prescribed amplitudes assess this mechanism; they are not measurements of residual stress in the bearing.
Table 8.
Residual-stress sensitivity at matched capacity, 1.5 wppm, 8 kN, 90 °C, and .
4. Discussion
4.1. Physical Meaning of the Effect of Trap Spatial Distribution
Under retained inventory, the trap spatial distribution affects lattice hydrogen through the amount stored in traps. At a common activity, placing equal capacity in less compressed regions gives a higher occupancy. The resulting increase in storage lowers the activity required to retain the prescribed total hydrogen, thereby lowering the equilibrium lattice concentration. Strong hydrogen retention and a large positional effect are therefore not equivalent. Strong binding favors storage, but near-complete trap filling leaves little difference between equal-count profiles. Spatial sensitivity depends on the occupancy contrast and the hydrogen remaining in the lattice, as expressed by Equation (10). A trap population can retain hydrogen effectively while showing little sensitivity to where its sites are located.
The bounds distinguish a storage constraint from a limitation of the selected profile. At low capacity, the small unrestricted bound excludes an appreciable positional effect for all equal-count profiles under the prescribed conditions. A large bound combined with a small layer difference instead identifies a geometric restriction. Table 7 further shows that the thermodynamic response depends on binding energy and capacity: strong retention alone does not establish strong spatial sensitivity.
Under retained inventory, the effect of the trap position on lattice hydrogen enters through the common activity in Equation (9), with the host properties and stress prescribed. A change in activity affects the concentration level throughout the connected volume, while its spatial ordering still follows the prescribed hydrostatic stress. Changing the trap position therefore does not independently move the maximum lattice-hydrogen to another depth. Total hydrogen includes occupied trap sites as well as lattice hydrogen. A trap-rich region can consequently give a high total signal while its lattice concentration remains low. This distinction connects the predicted partitioning with the hydrogen population involved in a particular damage mechanism.
4.2. Time Scales and Experimental Interpretation
At 90 °C, Equation (24) gives . The lattice-diffusion scales are approximately 465 s across and 7436 s across . One shaft revolution at 700 rpm takes 0.08571 s, corresponding to a diffusion length of 0.924 µm (Figure 12a). To include the storage of locally equilibrated traps, consider a small perturbation about equilibrium. With flux , the linearized storage and mobility are
Figure 12.
Characteristic times at 90 °C: (a) lattice-diffusion scale compared with the source shaft period, with the gray vertical dotted line marking the reference contact half-width, ; and (b) conditional bounds on the slowest nonconstant linear relaxation time for uniform traps at 8 kN, 1.5 wppm, and . The bars in (b) assume local trap equilibrium, fixed temperature and stress, and no-flux boundaries; they are not measured hold times.
Storage and mobility are evaluated at the equilibrium state. For the no-flux rectangle, the longest side is . The slowest nonconstant linear mode has decay time bounded by
These bounds follow from the weighted Rayleigh quotient for the first positive decay rate, with conservation . The Neumann Poincaré inequality gives . Taking the first unweighted Neumann cosine mode with its -weighted mean subtracted as a trial function gives . Inverting the two inequalities yields Equation (29). Coefficient bounds use the analytic interval and the corresponding extrema of , including 1/4 if its occupancy interval crosses 1/2. Uniform profiles use constant ; layers use .
For uniform traps, the bounds on are 0.28–2.51 h at low capacity, 0.89–7.74 h at , 71–265 days at , and 1.73–13.3 years at . For the matched shallow and subsurface profiles, they are 0.39–34.7 h and 0.40–36.6 h, respectively. These intervals bound the slowest linear mode under the stated model. If that mode is excited, its amplitude falls to 5% after ; an initial condition can suppress particular modes. The excess-capacity states therefore contain slow relaxation modes even with an instantaneous local trap equilibrium and cannot generally be treated as equilibrated during an hours-long hold.
During rolling, each material point experiences a changing stress field together with its previous history of hydrogen entry and release. The large separation between the shaft period and the diffusion time explains why hydrogen redistribution during a sustained hold deserves separate treatment. The equilibrium hold state provides a reference for subsequent transient calculations of restart and cyclic loading [27].
An experimental assessment can connect the predicted partitioning with characterized trap populations and measured initial inventories. Comparing loaded and unloaded specimens at the same temperature and hydrogen boundary over several dwell times would resolve the contribution of sustained contact stress. Whole-specimen measurements quantify inventory, while desorption analysis connects trap storage with release during heating through specimen dimensions and thermal history [32]. The precharging and surface-damage measurements of Weniger et al. [31] provide an example of controlling the hydrogen history in contact experiments.
4.3. Application and Limitations
The bounds provide a screening procedure for the equilibrium effect of the trap spatial distribution under sustained contact loading. They first assess whether position can materially change the partition of a prescribed inventory between lattice and trap sites. The resulting fields can then serve as reference states for a transient hold and restart calculation once its thermal history, trap kinetics, and hydrogen boundary have been specified.
The first step is to evaluate the concentration bound using the hydrogen inventory, trap capacity, and binding energy. A small bound identifies a storage constraint that position alone cannot overcome. An appreciable bound directs attention to feasible spatial profiles, which can be compared using Equation (9) and the relevant density limits. This sequence links material characterization to profile selection and avoids optimizing trap depth before establishing whether spatial arrangement can produce the desired concentration change.
Under the baseline Hertz field, Figure 9 favors placing capacity in less compressed regions. The residual-stress comparison in Table 8 shows that the preferred layer can change when the total hydrostatic field changes. Figure 10 gives the load sensitivity, and Figure 11 compares closed domains with different amounts of unpatterned material. Thus, the selection of a spatial profile depends on the total stress field, storage state, and hydrogen domain.
Heat treatment offers one route to preparing a candidate trapping state through changes in phases and interfaces [14,15]. Its contribution can be assessed by separating changes in the total capacity and binding energy from the additional effect of their depth distribution. Experiments on martensitic bearing steels distinguish hydrogen associated with dislocations from hydrogen immobilized by fine coherent vanadium carbides [40], demonstrating the importance of the trap character in this assessment. Surface modification can be evaluated in the same way using the trap population and affected depth it produces. The resulting profile comparison provides a hydrogen-partitioning criterion to complement hardness and other mechanical requirements.
Capacity matching corresponds to a mean dislocation-density equivalent of 1.75 × 1015 m−2. The prescribed background and peak give 3.50 × 1014 and 1.16 × 1016 m−2, respectively. Fu and Rivera-Díaz-del-Castillo [41] estimated 5.69 × 1015 m−2 from dislocation cells in ferrite bands of rolling-contact-fatigued 100Cr6. Yin et al. [42] used an initial estimate of 7.95 × 1015 m−2 based on hardness and a Taylor relation. These local microstructural and constitutive estimates provide capacity scales, not measured mean densities of reversible hydrogen traps. The low-capacity benchmark represents the initial source population rather than the whole hardened microstructure. Characterized dislocations, carbide interfaces, and other trap families can be incorporated as additive storage contributions with their own occupancies.
The contact model treats steel as a homogeneous elastic solid and uses a single effective BCC trap family. Actual processing and prior service change phases, trap populations, strength, and residual stress together [14,15,17]. The high-capacity comparisons hold these properties fixed to isolate the position and do not extrapolate the source strain law to the large strain. No preparation route has been established for the particular 34 µm enriched layers while preserving the other inputs. The ideal residual profile tests sensitivity but does not replace a measured bearing stress field. The roller crown, roughness, local plasticity, and phase-dependent solubility require a more detailed contact and material description.
The equal partial-molar-volume assumption can also be relaxed. If the lattice and trap hydrogen have partial molar volumes and , the equality of chemical potential gives
Equation (7) is recovered for . Allocation must generally rank trap occupancy at a common chemical potential. With spatially uniform trap properties and positive , this ranking still follows total hydrostatic stress. Spatial variations in binding energy or molar volume can change the ranking; a difference between and alone does not imply reversal.
The closed-volume result requires the time separation , or boundary transfer to be small relative to the initial inventory over the hold. Selecting a subvolume within continuous steel does not establish this separation. No particular bearing or specimen satisfying it is identified here. The relaxation bounds quantify the internal response only, under a fixed temperature and instantaneous local trap equilibrium. Binding energy alone supplies no capture or release rate, and a desorption activation energy cannot be substituted directly for thermodynamic binding energy without its transport interpretation [32]. No measured hold schedule or cooling history is available for a specimen-specific comparison. Cooling, evolving traps, and continued entry or loss require transient transport and surface kinetics [26,39]; lubricant and surface changes [2,19] also affect supply.
The numerical checks establish the conservation, convergence, and consistency of the idealized bounds. The independent sensitivity cases quantify the dependence on selected inputs; they are not statistically calibrated uncertainty intervals. The direct experimental validation of local partitioning remains to be performed. Agreement in Hertz pressure supports contact reconstruction, while whole-specimen hydrogen measurements constrain inventory. The source parameters have not been independently calibrated to a particular hardened 100Cr6 microstructure.
The 1% objective is a concentration-screening target rather than a damage threshold, and the 5.67% map value is a sampled maximum within the selected range. Unrestricted placement is a mathematical limit, and the finite-density allocations still need processing and microstructural validation. The lower lattice hydrogen before a restart may be relevant to hydrogen-assisted damage, but its persistence depends on trap release, renewed uptake, and deformation. Fatigue-life improvement requires those processes to be coupled to a damage model.
Future work should prioritize experimental validation under loaded standstill. For heat-treated 100Cr6, trap populations and their spatial distributions, binding energies, and initial hydrogen inventories should first be characterized. Loaded and unloaded contact specimens should then be compared at a controlled temperature and hydrogen exposure over a series of dwell times. Combining total hydrogen measurements and thermal desorption analysis with depth-resolved hydrogen measurements would test the predicted redistribution and constrain the partitioning between lattice and trap sites. The measurement response should be interpreted through the corresponding transport and desorption models to connect the measured signals with the calculated hydrogen populations. These experiments would provide the basis for extending the model to multiple trap families, measured residual stresses, and transient boundary exchange during stopping and restart. Subsequent rolling-contact fatigue tests on specimens subjected to controlled loaded holds should examine whether changes in the hydrogen state before a restart affect crack initiation and fatigue life. This sequence would connect the trap characterization, hydrogen-distribution validation, and bearing damage assessment.
5. Conclusions
Equilibrium hydrogen partitioning during loaded standstill was investigated using the 100Cr6–81104-TV reference and fixed profiles with an equal total trap capacity. The following conclusions can be drawn:
- Under retained inventory, locating an equal trap capacity in less compressed regions increases the trap storage and lowers the equilibrium lattice hydrogen throughout the connected volume. When an external reservoir maintains the chemical potential, the trap position changes the trapped hydrogen, while the equilibrium lattice hydrogen remains unchanged for the prescribed stress field and host properties. The boundary condition therefore determines whether a change in trap storage also changes lattice hydrogen.
- At the low-capacity benchmark and 1.5 wppm, the limited capacity and nearly saturated occupancy restrict the layer difference to 6.39 × 10−9%, with an unrestricted pointwise bound of 1.67 × 10−7%. Position alone cannot overcome this storage limitation. This conclusion applies to the prescribed initial trap population, not to every hardened bearing microstructure.
- At theoretical capacity matching, the selected layers differ by 3.07%, or 0.00472 mol m−3 in mean lattice concentration. The density-limited and unrestricted mean ranges are 19.28% and 72.39%, with their own lower-state denominators. Inventory, binding energy, capacity, and domain size govern the accessible response.
- The new capacity-, occupancy-, and density-limited bounds screen the concentration changes available through equal-count trap placement. Allocation follows trap occupancy at a common chemical potential. Residual stress can change the preferred layer, so the baseline shallow/subsurface ordering is conditional on the prescribed total stress field.
- Equilibrium fields provide conditional references for standstill and restart. Including locally equilibrated trap storage gives uniform-profile slowest-mode bounds of 0.89–7.74 h at and 71–265 days at under the selected 90 °C no-flux conditions. Lattice-diffusion scales alone therefore do not establish attainment during a hold. Applying these reference states requires both sufficient internal relaxation and the assumed hydrogen boundary.
Author Contributions
Conceptualization, H.L.; methodology, H.L.; software, H.L.; validation, H.L.; formal analysis, H.L. and Z.C.; investigation, H.L. and Z.C.; resources, H.L.; data curation, H.L.; writing—original draft preparation, H.L. and Z.C.; writing—review and editing, H.L. and Z.C.; visualization, Z.C.; supervision, H.L.; project administration, H.L. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by the Technological Project of Heilongjiang Province, China (the Open Competition Mechanism to Select the Best Candidates, Grant No. 2023ZXJ04A02), the National Natural Science Foundation of China (Grant No. 52105143), and the Zhongyuan Support Program for Top Young Talents in Scientific and Technological Innovation of Henan Province, China.
Institutional Review Board Statement
Not applicable.
Informed Consent Statement
Not applicable.
Data Availability Statement
The governing equations, source physical inputs, prescribed trap profiles, solver tolerances, and profile-generation procedure needed to reproduce the essential idealized calculations are provided in Section 2.1, Section 2.2, Section 2.3, Section 2.4 and Section 2.5; the relaxation analysis is given in Section 4.2. These calculations require no additional confidential input measurements. Generated numerical datasets are not publicly available because of project confidentiality restrictions. Requests for access may be directed to the corresponding author and will be evaluated in accordance with applicable confidentiality requirements.
Conflicts of Interest
The authors declare no conflicts of interest.
References
- SKF. Hydrogen Embrittlement and Other Key Challenges. Available online: https://www.skf.com/group/industries/hydrogen/hydrogen-embrittlement-and-other-challenges (accessed on 17 September 2026).
- Stadler, K.; Han, B.; Brizmer, V.; Pasaribu, R. Benefits of using black oxidized bearings in wind applications. Evolution 2015, 2, 25–30. Available online: https://evolution.skf.com/benefits-of-using-black-oxidized-bearings-in-wind-applications/ (accessed on 17 September 2026).
- Kino, N.; Otani, K. The influence of hydrogen on rolling contact fatigue life and its improvement. JSAE Rev. 2003, 24, 289–294. [Google Scholar] [CrossRef] [Scilit]
- Tanaka, S. Pulley Support Bearings for Push-Belt CVTs. NSK Motion Control 2006, 19, 13–19. Available online: https://www.nsk.com/content/dam/nsk/common/tools-resources/rd/pdf/techJournal/etj-0019.pdf (accessed on 11 October 2026).
- Ciruna, J.A.; Szieleit, H.J. The effect of hydrogen on the rolling contact fatigue life of AISI 52100 and 440C steel balls. Wear 1973, 24, 107–118. [Google Scholar] [CrossRef] [Scilit]
- Uyama, H.; Yamada, H.; Hidaka, H.; Mitamura, N. The Effects of Hydrogen on Microstructural Change and Surface Originated Flaking in Rolling Contact Fatigue. Tribol. Online 2011, 6, 123–132. [Google Scholar] [CrossRef] [Scilit]
- Evans, M.H.; Richardson, A.D.; Wang, L.; Wood, R.J.K. Effect of hydrogen on butterfly and white etching crack (WEC) formation under rolling contact fatigue (RCF). Wear 2013, 306, 226–241. [Google Scholar] [CrossRef] [Scilit]
- Liang, X.Z.; Zhao, G.H.; Owens, J.; Gong, P.; Rainforth, W.M.; Rivera-Díaz-del-Castillo, P.E.J. Hydrogen-assisted microcrack formation in bearing steels under rolling contact fatigue. Int. J. Fatigue 2020, 134, 105485. [Google Scholar] [CrossRef] [Scilit]
- Liang, X.Z.; Rivera-Díaz-del-Castillo, P.E.J. Hydrogen-accelerated white etching area formation in bearings under rolling contact fatigue. Int. J. Fatigue 2022, 159, 106753. [Google Scholar] [CrossRef] [Scilit]
- Solano-Alvarez, W.; Bhadeshia, H.K.D.H. White-Etching Matter in Bearing Steel. Part II: Distinguishing Cause and Effect in Bearing Steel Failure. Met. Mater. Trans. A 2014, 45, 4916–4931. [Google Scholar] [CrossRef] [Scilit]
- Hirth, J.P. Effects of hydrogen on the properties of iron and steel. Met. Trans. A 1980, 11, 861–890. [Google Scholar] [CrossRef] [Scilit]
- Birnbaum, H.K.; Sofronis, P. Hydrogen-enhanced localized plasticity—A mechanism for hydrogen-related fracture. Mater. Sci. Eng. A 1994, 176, 191–202. [Google Scholar] [CrossRef] [Scilit]
- Barrera, O.; Bombac, D.; Chen, Y.; Daff, T.D.; Galindo-Nava, E.; Gong, P.; Haley, D.; Horton, R.; Katzarov, I.; Kermode, J.R.; et al. Understanding and mitigating hydrogen embrittlement of steels: A review of experimental, modelling and design progress from atomistic to continuum. J. Mater. Sci. 2018, 53, 6251–6290. [Google Scholar] [CrossRef] [Scilit]
- Bhadeshia, H.K.D.H. Steels for bearings. Prog. Mater. Sci. 2012, 57, 268–435. [Google Scholar] [CrossRef] [Scilit]
- Bhadeshia, H.K.D.H. Prevention of Hydrogen Embrittlement in Steels. ISIJ Int. 2016, 56, 24–36. [Google Scholar] [CrossRef] [Scilit]
- Khader, I.; Kürten, D.; Raga, R.; Winzer, N.; Kailer, A. Modeling hydrogen diffusion in a tribological scenario: A failure analysis of a thrust bearing. Wear 2019, 438–439, 203054. [Google Scholar] [CrossRef] [Scilit]
- Baur, M.; Khader, I.; Kürten, D.; Schieß, T.; Kailer, A.; Dienwiebel, M. Premature Damage in Bearing Steel in Relation with Residual Stresses and Hydrogen Trapping. Lubricants 2024, 12, 311. [Google Scholar] [CrossRef] [Scilit]
- Kürten, D.; Khader, I.; Raga, R.; Casajús, P.; Winzer, N.; Kailer, A.; Spallek, R.; Scherge, M. Hydrogen assisted rolling contact fatigue due to lubricant degradation and formation of white etching areas. Eng. Fail. Anal. 2019, 99, 330–342. [Google Scholar] [CrossRef] [Scilit]
- Kürten, D.; Khader, I.; Amann, T.; Gatti, F.; Baur, M.; Oberle, N.; Grundei, S.; Franke, J.; Kailer, A. Conductive lubricants to prevent hydrogen assisted rolling contact fatigue. Eng. Fail. Anal. 2025, 180, 109819. [Google Scholar] [CrossRef] [Scilit]
- Sofronis, P.; McMeeking, R.M. Numerical analysis of hydrogen transport near a blunting crack tip. J. Mech. Phys. Solids 1989, 37, 317–350. [Google Scholar] [CrossRef] [Scilit]
- Krom, A.H.M.; Koers, R.W.J.; Bakker, A. Hydrogen transport near a blunting crack tip. J. Mech. Phys. Solids 1999, 47, 971–992. [Google Scholar] [CrossRef] [Scilit]
- Kadin, Y. Modeling of hydrogen transport in rolling contact fatigue conditions. Procedia Eng. 2013, 66, 415–424. [Google Scholar] [CrossRef] [Scilit][Green Version]
- Kadin, Y. Modeling of Hydrogen Transport in Static and Rolling Contact. Tribol. Trans. 2015, 58, 260–273. [Google Scholar] [CrossRef] [Scilit]
- Varias, A.G. Chemical Equilibrium Fracture Mechanics—Hydrogen Embrittlement Application. CMD 2025, 6, 5. [Google Scholar] [CrossRef] [Scilit]
- Oriani, R.A. The diffusion and trapping of hydrogen in steel. Acta Metall. 1970, 18, 147–157. [Google Scholar] [CrossRef] [Scilit]
- Martínez-Pañeda, E.; Díaz, A.; Wright, L.; Turnbull, A. Generalised boundary conditions for hydrogen transport at crack tips. Corros. Sci. 2020, 173, 108698. [Google Scholar] [CrossRef] [Scilit]
- Fernández-Sousa, R.; Betegón, C.; Martínez-Pañeda, E. Analysis of the influence of microstructural traps on hydrogen assisted fatigue. Acta Mater. 2020, 199, 253–263. [Google Scholar] [CrossRef] [Scilit]
- Díaz, A.; Cuesta, I.I.; Rodríguez, C.; Alegre, J.M. Influence of non-homogeneous microstructure on hydrogen diffusion and trapping simulations near a crack tip in a welded joint. Theor. Appl. Fract. Mech. 2021, 112, 102879. [Google Scholar] [CrossRef] [Scilit]
- Kürten, D.; Khader, I.; Kailer, A. Determining the effective hydrogen diffusion coefficient in 100Cr6. Mater. Corros. 2020, 71, 918–923. [Google Scholar] [CrossRef] [Scilit]
- Weniger, L.-M.; Sefer, B.; Pelcastre, L.; Åkerfeldt, P.; Hardell, J. Influence of Lubricated Rolling/Sliding Tribotesting on Hydrogen Trapping in 100Cr6 Bearing Steel. Tribol. Lett. 2024, 72, 69. [Google Scholar] [CrossRef] [Scilit]
- Weniger, L.-M.; Jamil, K.; Sefer, B.; Pelcastre, L.; Åkerfeldt, P.; Olsson, C.-O.A.; Hardell, J. Quantifying Hydrogen Concentrations and their Influence on Surface-Initiated Damage in Rolling/Sliding Contacts of 100 Cr6 Bearing Steel. Tribol. Lett. 2025, 73, 73. [Google Scholar] [CrossRef] [Scilit]
- Kirchheim, R. Bulk Diffusion-Controlled Thermal Desorption Spectroscopy with Examples for Hydrogen in Iron. Met. Mater. Trans. A 2016, 47, 672–696. [Google Scholar] [CrossRef] [Scilit]
- Brass, A.M.; Chene, J.; Pivin, J.C. Influence of nitrogen ion implantation on hydrogen permeation in an extra mild steel. J. Mater. Sci. 1989, 24, 1693–1699. [Google Scholar] [CrossRef] [Scilit]
- Schaeffler. 81104-TV: Axial Cylindrical Roller Bearing; Schaeffler Medias. Available online: https://medias.schaeffler.us/en/product/rotary/rolling-and-plain-bearings/roller-bearings/axial-cylindrical-roller-bearings/81104-tv/p/395849 (accessed on 20 September 2026).
- Johnson, K.L. Contact Mechanics; Cambridge University Press: Cambridge, UK, 1985. [Google Scholar] [CrossRef] [Scilit]
- National Institute of Standards and Technology. 2022 CODATA Recommended Values of the Fundamental Physical Constants. Available online: https://physics.nist.gov/cuu/Constants/Table/allascii.txt (accessed on 20 September 2026).
- Commission on Isotopic Abundances and Atomic Weights. Abridged Standard Atomic Weights 2024. Available online: https://ciaaw.org/abridged-atomic-weights.htm (accessed on 20 September 2026).
- Díaz, A.; Alegre, J.M.; Cuesta, I.I. Coupled hydrogen diffusion simulation using a heat transfer analogy. Int. J. Mech. Sci. 2016, 115-116, 360–369. [Google Scholar] [CrossRef] [Scilit]
- Díaz, A.; Alegre, J.M.; Cuesta, I.I.; Martínez-Pañeda, E. A COMSOL framework for predicting hydrogen embrittlement, Part I: Coupled hydrogen transport. Eng. Fract. Mech. 2025, 319, 111007. [Google Scholar] [CrossRef] [Scilit]
- Szost, B.A.; Vegter, R.H.; Rivera-Díaz-del-Castillo, P.E.J. Hydrogen-Trapping Mechanisms in Nanostructured Steels. Metall. Mater. Trans. A 2013, 44, 4542–4550. [Google Scholar] [CrossRef] [Scilit]
- Fu, H.; Rivera-Díaz-del-Castillo, P.E.J. Evolution of White Etching Bands in 100Cr6 Bearing Steel under Rolling Contact-Fatigue. Metals 2019, 9, 491. [Google Scholar] [CrossRef] [Scilit]
- Yin, H.; Bai, X.; Fu, H. Prediction of Work Hardening in Bearing Steels Undergoing Rolling Contact Loading with a Dislocation-Based Model. Metals 2022, 12, 555. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.