Skip to Content
Applied SciencesApplied Sciences
  • Article
  • Open Access

22 July 2026

18 Pages

Acoustic Emission Monitoring of Push-Out Testing for Early Microcrack Detection: A Proof-of-Concept on Strut-Structured Surrogate Samples

,
,
,
,
,
,
and
1
Biomedical Engineering, Fraunhofer Institute for Toxicology and Experimental Medicine ITEM, 30625 Hannover, Germany
2
Institute for Product Development IPeG, Leibniz University Hannover, 30823 Garbsen, Germany
3
Institute of Medical Device Technology IMT, University Stuttgart, 70569 Stuttgart, Germany
*
Author to whom correspondence should be addressed.

Abstract

Conventional push-out tests detect bone–implant failure only at the point of macroscopic instability, leaving earlier damage stages unresolved. Here we present a proof-of-concept for a push-out test stand combined with acoustic emission (AE) monitoring, aimed at capturing crack initiation before the macroscopic load drop. To provide a controlled failure process, samples were fabricated from SLA resin with defined breaking points, serving as mechanical surrogates rather than biological models. Four sample types with varying strut number and thickness were tested while recording AE, and post-processing was applied to remove friction and noise signals. A four-stage fracture model—initial, pre-fracture, fracture, and post-fracture—was defined, with the pre-fracture stage showing AE activity prior to any macroscopic load response. Increasing strut thickness and contact area raised maximum load resistance and AE activity, and Principal Component Analysis confirmed a progressive, intensity-driven separation of stages. The results demonstrate that AE monitoring resolves a pre-fracture regime inaccessible to conventional load measurement, establishing a methodological basis for future application to bone–implant samples.

1. Introduction

The bone–implant interface (BII) represents the biological processes that occur at the location where an implant engages with bone, leading to the implant being enveloped by newly formed bone as part of osseointegration. Osseointegration is the process where a firm and motionless fixation has been achieved together with direct functional contact to the bone [1,2,3]. Specifically, osseointegration is influenced by the implantation process and the adequate initial fixation of the implant inside the host tissue during surgery (primary stability), as well as bone remodelling of the tissue around the implantation site (secondary stability). However, bone remodelling and biological long-term integration into the tissue are the dominant components of overall stability, therefore frequently equated with osseointegration [4,5].
Haas and Pommer (2015) showed the dependence of stability on time of healing, where secondary stability contributes strongly to overall long-term stability after initial healing and leads to adequate osseointegration [6]. Multiple complex biological processes after initial implantation trigger the process of osseointegration, with most immune-driven reactions not yet fully understood [7]. Thus, initialization of biological remodelling is a key part of the implant design and testing process. Together with biofunctionality and biocompatibility, osseointegration provides the basis for implant development and design [8]. During implant design, multiple parameters can be adapted for improved osseointegration. For example, surface properties and thus higher surface roughness promotes osseointegration success through increased surface area [6,9]. Additionally, specific implant materials like titanium or hydroxyapatite can improve the osseointegration rate by chemical reactions at the implant interface [2]. In contrast, reduced osseointegration can lead to aseptic loosening, where inadequate fixation and mechanical and biological loss of stability are the impacting factors. In that case, loosening increases over time [10,11].
Improvement in osseointegration can be achieved by the adaptation of implant properties, like material, surface, or structure [12,13]. Variation in these requires thorough testing to provide evidence of increased stability and patient safety. In terms of osseointegration, Branemark and Skalak (1998) presented a method for pull-out testing of implants, where load versus displacement can be analyzed to determine the degree of stability and thus the quality of osseointegration [14]. Barckman et al. (2013) reversed this approach by utilizing push-out tests on in vivo implants to assess osseointegration success following the healing period [15]. They dissected the distal part of dog femurs after a period of 4 weeks and performed an axial push-out of the implant with analogous measurement of load and displacement. This testing process resulted in displacement under different loading conditions, with ultimate shear strength marking the point of implant failure and complete loosening [15].
Comparison of the actual loosening of the implant within the bone structure with the simulated testing conditions by push-out testing suggests poor reproduction of loosening and lack of significance for conventional push-out testing [4]. Realistic implant loosening covers loss of stability over a prolonged timespan with continuous loading, leading to initial microscopic cracks in BII. Microcrack accumulation results in the formation of macroscopic cracks with a visible influence on stability. Yet, first microscopic cracks already influence stability and need to be evaluated to identify the influence of implant properties on loosening mechanics [16].
Adaptation of conventional push-out testing is a possibility to develop an advanced testing process for the realistic determination of implant stability, as load data alone cannot lead to a conclusion on beginning loosening. Goodwin et al. (2017) [17] have already utilized acoustic emission (AE) sensors for monitoring the failure of vertebra and long bone. In their setup, four-point loading was performed on bone samples with mounted AE sensors on top [17]. They found differences in the respective bone types, with AE evaluation opening up a novel approach to fracture analysis [17].
An approach of combining AE measurement with loading and therefore push-out testing was conducted by Holweg et al. (2004) [18]. By adding AE measurement utilities to a tensile testing machine, they proposed a combined test stand for force and AE measurement. This way, the additional AE information enabled cross-correlation with load data and, therefore, advanced implant characterization of the behavior of BII in the context of osseointegration. Conventional testing methods do not display an accurate representation of implant loosening mechanics and only detect failure at a final timepoint. Visible loosening only indicates where the last stable bonding of the bone–implant connection is destroyed, which reduces the significance of conventional push-out testing of implants for precise interface evaluation. Different studies have already displayed the advantages of AE monitoring during mechanical testing [17,19,20].
Here we investigated whether AE evaluation of a push-out testing process indicates early signs of defects, i.e., microcracks, and consequently allows for more detailed and substantial testing of materials under loading. By specifically developing an adaptive sample structure for combined testing, we aimed to deliver a proof-of-concept for the detection of macroscopic and microscopic cracks inside this surrogate model, as a methodological step toward possible future application to bone–implant models. Therefore, a system design study was performed with an adapted test stand for the proof-of-concept study.

2. System Design

The test stand is realized with adjustments to the specimen fixture of Holweg et al. (2004) (Figure 1) [18]. A tensile testing machine (Quasar 2.5, Galdabini, Cardano al Campo, Italy) is used as the basis, combined with a 1 kN load cell (TSTM 1 kN, x-sensors, Diessenhofen, Switzerland) and LabTest 4.0 Software (also Galdabini). For AE data acquisition, a wideband AE sensor (WSα, Mistras, Princeton Junction, NJ, USA) with an operating frequency of 100–1000 kHz in combination with a USB AE node (1283 AE-node, Mistras, Princeton Junction, NJ, USA) for amplification and data processing is used. For data acquisition and analysis, AEWin Software (also Mistras) is used. For the production of sample structures, SLA 3D printing is used with a Formlabs printer (Form3BL, Formlabs, Somerville, MA, USA).
Figure 1. Test stand constitution with an enlarged display of the specimen grip.
The AE sensor is mounted on a levelled surface (Rz ≤ 1.6 µm) on top of a test plunger, as suggested by Holweg et al. (2004) [18]. The test plunger is custom-manufactured for this application, with levelled surfaces at each point of AE transmission (tip and sensor surface) comprising stainless steel (1.4404). A couplant is applied between the sensor and the test plunger surface (High Vacuum Grease, DOW CORNING, Midland, MI, USA). The plunger geometry is designed with a small tip, only slightly larger than the sample diameter, to minimize its influence on AE signal transmission. A custom specimen fixture was developed to accommodate cylindrical samples in a defined push-out process. The fixture permits alignment in the x- and y-directions and is, by design, not restricted to planar slices as in Holweg et al. (2004) [18]. Therefore, a frame with eight screws is the primary fixation of samples, which can be aligned to the test plunger. Samples are inserted into the frame and fixed using the screws. A 3D-printed sample holder comprising the test sample material is used for further testing. Push-out is performed from above in the z-direction.
The fixture accommodates sample diameters of 7–70 mm and lengths of 12–42 mm. This geometric range is intended to later accommodate samples with uneven surfaces; the present study, however, is restricted to the standardized surrogate geometry described below.
The software configuration, as presented in Table 1, is kept constant throughout all test runs. Peak Definition Time (PDT), Hit Definition Time (HDT), and Hit Lockout Time (HLT) setup defines the characterization of incoming signals. Each can be described as a timer, defining the interpretation of the signal. PDT starts after a signal is detected and defines the allowable time for the detection of a peak. HDT defines the maximum time for a crossing of a threshold and restarts after each crossing. HLT defines the time after HDT has ended, where no signal can be detected and avoids detection of AE wave reflections.
Table 1. Parameters for AE data acquisition.
All parameters are used for the correct identification of a hit, which is the event leading to a signal that is then registered as a threshold crossing. A hit is defined by the AE or an AE wave crossing the defined threshold, which is then displayed as a point in the amplitude–time diagram [21]. A pencil lead break (PLB) is performed on the sample surface, according to ASTM E976-10 (HSU-Nielsen Test) [19]. Therefore, a 0.5 mm 2H pencil lead is extended by 6 mm and pressed onto the sample holder at a 45° angle on the outer ring of the samples until breakage of the lead. The PLB leads to an initial AE wave, which is used for adjustment of the settings, as performed for parameter setup.

3. Materials and Methods

Sample development focused on the magnitude of fracture and the differentiation of micro- and macrocrack occurrence. The main difference between micro- and macroscopic crack initiation is the visibility of cracks without the application of any magnification, with microcracks in bone usually being below 1 mm in length [21]. The model should therefore produce visible cracks on a reproducible scale for testing inside the presented test stand. To reduce the occurrence and accumulation of cracks before total failure of the material (meaning potential microcracks) and produce the aimed-at visible fracture, a brittle material (elongation at break 5%) with a fracture-promoting geometry was designed, as displayed in Figure 2a [22]. The sample consists of a supporting outer ring with an outer diameter of 5.5 mm and an inner diameter of 3.9 mm. The outer ring is connected to a central cylindrical core with a diameter of 2.5 mm, featuring a convex top and bottom surface to ensure ideal contact with the test plunger. The connection between the outer ring and the central core is realized by radially oriented struts, whose number and thickness are varied to investigate their influence on the mechanical response of the structure.
Figure 2. Overview of the designed strut structure (a) with FEM analysis of a simplified z-directional push-out for 10 N (b) versus 500 N. (c) Von Mises stress in MPa.
SLA 3D printing was used. Samples were printed using Formlabs ClearV4 material with identical alignment on the print bed. After printing, all samples were cleaned and UV-hardened for 30 min. Additionally, the geometry was adapted to achieve defined breaking points on each strut.
A finite element analysis was used to analyze the mechanical behavior of the structure under physiological loading conditions, as presented in Figure 2b,c. The 3D geometry of the model was based on a CAD design created in Inventor 2025 (Autodesk, San Francisco, CA, USA), which accurately represents the structural features of the experimental setup. The material properties were defined according to Formlabs ClearV4 Resin, as provided in the material data sheet and assigned within Inventor’s simulation environment. The model was meshed using tetrahedral elements with an average element size of 0.1 mm. Boundary conditions were applied to replicate experimental constraints: the supporting outer ring was fully fixed (zero displacement in all directions), while a z-directional compressive force was applied uniformly over a defined contact area from above. The simulation was performed as a static, linear-elastic analysis. The results were analyzed in terms of von Mises stress distribution and total deformation. These outputs presented the mechanical integrity and potential failure regions of the structure under simulated loading conditions.
For the identification of contact area influence, a two-factor approach was developed based on simplified DoE standards for experimental analysis (Table 2). Stability and the contact area of the struts were varied by (A) the number of struts and (B) the thickness of the struts. This led to a matrix of combinations, each being tested in a push-out process. For each parameter, maximum and minimum values were identified depending on printability. As a result, 20 samples were tested. Due to a mechanical failure during push-out testing, one sample was omitted.
Table 2. Parameter combinations for strut testing.
LabTest Software was used to implement a testing scheme for push-out. Three phases can be subdivided, with (1) being the initial contact of the test plunger and the sample surface, (2) being a stationary hold of the plunger on the sample surface, and (3) being the final push-out process. A defined abortion criterion was included (maximum load of 300 N). For initial contact, the test plunger was moved with a speed of 0.1 mm/min in the z-direction until the plunger was in contact with the sample surface and a pre-load of 0.5 N was achieved (1). After that, contact was held without an increase in load (2). At this point, a PLB was performed. Finally, the process was continued with a 5 mm/min push-out of the sample until the abortion criterion of 300 N was achieved (3).
Correlation analysis was performed using a custom evaluation script in R 4.5.2 (RStudio, Posit PBC, Boston, MA, USA). Principal Component Analysis (PCA) was carried out to determine the relevance of the AE parameters and verify staging [23]. PCA identifies the directions (principal components) in which the data show the greatest variance. These directions are orthogonal and ordered by the amount of variance they capture.
Therefore, a single hit can be displayed as a vector of variables called v (see Table 3).
v = v 1 v 2 v 3 v 4 v 5 = A m p l i t u d e C o u n t s D u r a t i o n E n e r g y R i s e t i m e
Table 3. Classification of different AE occurrences.
This five-dimensional data structure displays high complexity for data analysis. Therefore, PCA can be applied to simplify the dimension. For that, all hits are centered using min–max normalization, as the differences in the gathered AE parameters and their range of values would dominate the analysis. The centered vector v i , j ,   c e n t e r e d can be calculated by following equation:
v i , j ,   c e n t e r e d = v i , j − m i n ( v i , j ) M a x ( v i , j ) − m i n ( v i , j )
These vectors can be summarized in a matrix M c e n t r e d for each analyzed strut variation.
M c e n t e r e d = v 11 v 12 … v 1 p v 21 v 22 … v 2 p ⋮ ⋮ ⋱ ⋮ v n 1 v n 2 … v n p
By calculating the covariance matrix and carrying out an eigenvalue decomposition (EVD), eigenvalues λ and eigenvectors ξ can be identified. In contrast, a singular value decomposition (SVD) can be used to simplify the computational calculation, which has been employed in this study. The eigenvalues and eigenvectors lead to the calculation of the singular value matrix D. The right singular vectors V are obtained as the orthonormal eigenvectors of M ⊤ M , corresponding to its eigenvalues.
D = λ 1     λ 2
V j = M c e n t e r e d T M c e n t e r e d − λ j I
With this, the PC values can be calculated.
P C j = M V j
The proportion of variance explained by each principal component is given by the squared singular value divided by the sum of all squared singular values.
v a r ( P C j ) = λ j ∑ k = 1 p λ k
With these values, a biplot can be created visualizing the observations in the form of PC values. Additionally, right singular vectors V in the PCA biplot represent the original variables projected onto the first two principal components. Their direction shows how each variable contributes to the new coordinate system, and their length reflects how well the variable is represented in this 2D projection. Technically, the coordinates of each arrow correspond to the variable’s loadings, i.e., the entries of the eigenvectors associated with the PC values. The term loadings refer to the coordinates of the variable vectors (arrows) in the biplot, while scores refer to the coordinates of the observations (data points) in the principal component space.

4. Results

4.1. FEM Analysis

A linear-elastic FEM analysis was used to identify the regions of highest mechanical stress in the strut structure under z-directional push-out loading. Figure 2 shows the von Mises stress distribution for two load levels (b: 10 N; c: 500 N). As a linear-elastic model, the analysis does not simulate fracture or crack propagation. Rather, the stress concentrations localize at the struts, coinciding with the breaking points observed experimentally during push-out. The predicted location of failure initiation was consistent across both load levels and matched the intended breaking points on the struts. The analysis therefore supports the qualitative design rationale. The struts act as defined breaking points, rather than providing a quantitative prediction of failure load. A mesh-convergence study was not performed, given that the analysis is used only to localize stress concentrations qualitatively rather than to predict absolute stress magnitudes or failure loads; the results are interpreted accordingly. The reported von Mises stresses (Figure 2) should therefore be read as relative distributions rather than validated absolute values.

4.2. Post-Processing

The main part of post-processing is the identification of noise and unwanted AE sources in the resulting data set. As all AE occurrences are registered, friction from the test plunger or friction on the material surface due to small particles can potentially be identified and included in the results as well. These particles result from separating support structures from the actual sample geometry during the production of samples.
This leads to the necessity of defined criteria to eliminate non-target AE from the results and gain a clear recording from solely push-out signals and damage of material connections. To achieve this, a top–down process was utilized to generate filter criteria from a data set for the push-out of the strut structures. Overall data acquisition presents various acoustic emission hits during push-out. The noticeable increase in AE after failure of the material at load drop-off hints at the occurrence of friction-induced hits.
In a single-component specimen, acoustic activity would be expected to cease once bonding has failed at maximum load. In the present strut structures, however, failure is sequential: individual struts fracture one after another, so that the load can rise again after a local drop and intact struts may fracture for the first time even when the global load is below an earlier maximum. New AE can therefore occur after the global load maximum, and a load below the previous global maximum does not preclude further fracture signals. Fracture signals are distinguished from friction-induced emission by their characteristic signal morphology (continuous waveform, low risetime share, low energy; Section 4.2, Table 3) rather than by load history. Several characteristics were analyzed for the detection of AE activity: amplitude, risetime, duration, energy (non-dimensional), and counts. Comparison of hits before drop-off and after indicated a lower share of risetime concerning total time (duration + risetime). The acoustic signal had a low risetime and, upon visible analysis in the AEWin software, a continuous form without visible peaks. Threshold crossings were therefore also low. Energy of friction-induced hits was frequently in the range of 0–1.
Table 3 displays selected hits during push-out of the strut structure. Total failure and breakage of the final bonds resulted in a loud hit at a maximum detection level of 100 dB. However, amplitude cannot be used for unambiguous identification of noise, as differentiation of hits with lower amplitude was not possible. Duration and energy provided more distinct criteria for differentiation. This way, a clear classification for cracks and friction/noise could be defined. Classification of hits included a visual check in the AEWin software. The characteristic form of a friction- or noise-induced hit could clearly be differentiated by visual inspection. The course of the load curve is comparable to conventional push-out testing results.
Figure 3 displays push-out of structures with (a) 3 struts and (b) 11 struts. The color corresponds to strut thickness. Post-processing parameters defined from the previous analysis presented were applied, as presented in Algorithm 1 (counts > 0, amplitude > 0, energy > 1, percental share of risetime < 10% and PLB has been removed). The thresholds were derived heuristically from the characteristic morphology of friction-induced signals (continuous waveform, low transient onset, low energy); their robustness is examined in the sensitivity analysis (Table S1). Regarding the 3-strut structures, the load reached maximum values of roughly 50–75 N, with low noticeable differences of 0.4 mm to 0.8 mm strut thickness for comparison.
Algorithm 1. Friction and noise rejection per recorded hit.
Input: Hit with parameters (COUN, AMP, ENER, RISE, DURATION)
 
Compute: riseshare = 100 × RISE/(RISE + DURATION)
Retain Hit if:
                    COUN > 0
AND           AMP > 0
AND           ENER > 1
AND           riseshare < 10%
ELSE reject as friction or noise
Figure 3. Comparison of AE data for 3 struts (a) and 11 struts (b) with load data and displacement rate. PLB has been removed. Load–displacement curves (top) and filtered acoustic emission hits (bottom) for (a) 3-strut and (b) 11-strut structures, at strut thicknesses of 0.4 mm (green) and 0.8 mm (dark blue). Load is shown per measurement series; AE hits are those retained after friction/noise filtering (energy > 1, risetime share < 10%), excluding pencil-lead-break reference signals.
For 11 struts, the overall load resistance increased from 150 to 200 N for 0.4 mm struts to roughly 200 to 300 N for 0.8 mm struts. The correlation of the maximum load resistance to contact area is evident, meaning a higher contact area resulted in a higher maximum load. With regard to hit occurrence, there was no visible difference in contact area increases. Neither an increase in strut thickness nor an increase in strut number resulted in a sharp increase in overall amplitude or energy level, judging from basic-load AE plotting. More struts resulted in more AE hits, potentially resulting from higher friction after damage to the struts. For every series, a characteristic course for push-out could be observed: an increase in load until a maximum value and then a drop-off to values around zero with at least one hit at the timepoint of maximum load. For some series, accumulation of multiple hits before the point of maximum load could be observed, leading to the assumption that the material had not failed instantly but rather progressively due to potential air pockets or material inhomogeneity.
However, the overall course did display a typical push-out, with additional information on AE activity. All hits at the point of total failure were considerable during testing and could be allocated to the timepoint of maximum load. Macroscopic cracks could be visibly initialized, leading to a proof-of-concept: amplitude–load plotting does indicate the occurrence of hits at a given loading condition and even hints at failure type by the accumulation of hits and, therefore, breakage just before maximum load, leading to absolute failure. Proof-of-concept had to be further evaluated regarding the type of crack to enable the identification of microcracks and differentiation from macrocracks.

4.3. Proof-of-Concept

To gain a simplified insight into macrocrack initiation, qualitative (parameter-based) analysis was limited to energy, amplitude, counts, risetime, and duration.
Figure 4 displays an exemplified course of push-out for sample 6. The structure had three struts and a 0.4 mm strut thickness. Analysis is limited to 3-strut structures, as they displayed lower overall stability and fewer AE hits in the post-fracture stage, which simplified the evaluation of results and reduced noise elimination effort. For Formlabs ClearV4 material, an elongation at break of 6% is specified. With this, fracture stages can be defined via the course of the load curve.
Figure 4. Exemplary course for a 3-strut and 0.4 mm structure (sample no. 6) with visualized fracture stages (PLB, pencil lead break; I, initial stage; II, pre-fracture stage; III, fracture stage; IV, post-fracture stage).
∆ L = ε b r e a k · L 0
In stage I (initial, emission-free), where the initial loading regime is characterized by the absence of detectable acoustic emission, no AE hits were recorded prior to the first registered event in any specimen. This emission-free character was stable across the full range of filtering thresholds tested (Table S1). The stage is therefore defined empirically by the onset of detectable AE rather than by a fixed displacement. For orientation, the corresponding displacement is in the order of 0.024 mm for the 0.4 mm struts, consistent with an estimate from the ClearV4 resin data (post-cured: tensile modulus 2.8 GPa, ultimate strength 65 MPa, elongation at break 6%), which specifies no distinct yield point, in line with the brittle behavior of the material. The absence of detectable AE indicates the absence of macroscopically significant emission events but does not exclude sub-threshold microcracking below the sensitivity of the present setup [24].
The second stage is defined by the point of fracture, meaning the hit with maximum load before drop-off. These fractures are assumed to be of microscopic type and go on to form macroscopic fractures. During this process, AE of micro- and macrocracks are emitted. This stage can be described as the pre-fracture stage (II).
The first macroscopic crack results in loss of stability, as it is a major incident concerning material homogeneity. Therefore, the hit-at load drop-off can be defined as the starting point of macroscopic crack propagation and therefore stage (III), the fracture stage, followed by the post-fracture stage (IV), where predominantly macroscopic cracks occur. In the post-fracture stage, the number of macroscopic cracks increases until absolute failure at the end of stage (IV), where the load drops to zero. The definition of stages follows the findings of Xu et al. (2021) [25], where a differentiation between post- and pre-fracture was developed. An initial stage was added for PLB, where a manual breakage was simulated via the pencil lead.
With the AE analysis, we focused on additional information on the process of material destruction and BII evaluation. Therefore, the AE results needed to not only match the information from push-out testing and the defined stages but also to deliver additional information on the progression of defects.
A PCA analysis was performed to verify the staging derived from the load course (Figure 5). The principal component values (PC) were calculated according to the previously described procedure. The results showed a high proportion of explained variance, with PC1 accounting for 94% of the total variance and PC2 accounting for 3.8%. Together, these two components explain 97.8% of the total variance, capturing the vast majority of the information in the dataset and were therefore sufficient for further analysis. Consequently, the original five-dimensional problem could be effectively reduced to two principal components, simplifying the analysis while preserving nearly all relevant information.
Figure 5. Biplot of PC1 (94%) and PC2 (3.8%) illustrating stage clustering and variable loadings for the 3-strut structures.
Since PC1, represented on the x-axis, explains 94% of the total variance, the separation of the data occurs primarily along this component. The PLB scores cluster on the negative side of PC1 in a compact formation, indicating low variability and a distinctly different condition compared with the other stages. Stage II is located mainly on the positive side of PC1 and shows a wide dispersion along PC2. Its partial overlap with stage III suggests strong similarities and indicates a transitional phase without clear separation. Stage III is positioned between stages II and IV and overlaps substantially with stage II, supporting its interpretation as an intermediate state. In contrast, stage IV is shifted markedly toward higher positive PC1 values and extends upward along PC2, while exhibiting greater variability. This suggests that post-fracture stage IV represents the most advanced stage, clearly differentiated from the preceding stages. For the 3-strut structures analyzed here, the filtered dataset comprised 8 PLB reference hits and, across the push-out phase, 12 hits assigned to the pre-fracture stage (II), 10 to the fracture stage (III), and 11 to the post-fracture stage (IV); no hits were recorded in stage I. Pre-fracture activity (stage II) was observed in 7 of the 10 specimens. These counts indicate that the present analysis rests on a limited number of events per stage, and the PCA results should be read as an exploratory, descriptive summary rather than as a statistically powered classification.
The loading vectors indicate that duration, amplitude, and energy contribute strongly to PC1, as they point prominently in the positive PC1 direction. Thus, the transition from PLB to stage IV corresponds to increasing signal intensity and duration. The nearly parallel orientation of these vectors indicates a strong positive correlation among these parameters. Risetime contributes primarily to PC2 and shows comparatively independent behavior. However, since PC2 accounts for only 3.8% of the total variance, its overall influence is minor. The counts vector is located close to the origin, indicating a weaker contribution to the explained variance. Overall, the progression of damage appears to be mainly associated with increases in amplitude, energy, and duration, with only a minor influence of risetime. These parameters therefore provide a suitable basis for staging and for further evaluation of defect characteristics, such as fracture intensity.
The AE parameter ranges of the retained hits in the three push-out stages of the 3-strut structures are summarized in Table S2. The ranges overlap substantially across stages: median amplitude is at the system ceiling (100 dB) in all three stages, and energy, duration, and counts span comparable ranges. The stages are therefore not separable by fixed parameter thresholds, and their distinction in this study rests on the temporal position of each hit relative to the macroscopic load maximum. This is consistent with the PCA result, in which stage separation is intensity-driven, and stages II and III overlap. Consequently, we report these ranges as a descriptive, surrogate-specific characterization rather than as transferable damage-classification thresholds (Table S2).

5. Discussion

In this work, we developed and evaluated a push-out test stand with integrated acoustic emission monitoring, using a controlled surrogate to characterize the acoustic signature of progressive structural failure. The longer-term motivation is a method for bone–implant interface evaluation; establishing that link, however, is beyond the scope of the present surrogate study. To assess the capability of the test stand, we also successfully developed a sample structure designed to produce progressive structural failure with defined breaking points. Additionally, we tested all samples in the test stand and aimed at the differentiation of fracture stages in 3D-printed samples. This work highlights the advantages of acoustic emission testing in this specific use case, with a significant increase in the informative value of conventional push-out testing by the addition of acoustic emission testing.
Qualitative-parameter-based analysis informed the most relevant advantages of the combined testing of load and acoustic emissions compared with conventional load testing. The first iteration of filtering provided a refinement of the data to an analyzable version, with eliminated noise and friction signals. The correct identification of noise could be verified by visual analysis in the acoustic emission software, as all continuous signals (e.g., friction) were correctly excluded. The filtering criteria (counts > 0, amplitude > 0, energy > 1, risetime share < 10%) were derived heuristically from the present dataset by visual identification of the characteristic morphology of friction-induced signals (continuous waveform, low risetime share, low energy; Section 4.2, Table 3). We emphasize that this procedure is heuristic and dataset-derived. The thresholds were not obtained from an independent calibration set, and we cannot exclude that a small number of genuine low-energy microcrack hits were removed together with friction signals. To assess whether this dependence biases the results, we performed a sensitivity analysis in which the energy and risetime thresholds were varied over a wide range (Table S1). The qualitative stage structure and, in particular, the presence of pre-fracture (stage II) activity preceding the macroscopic load drop was preserved across all tested thresholds and occurred in the majority of 3-strut specimens (7 of 10). Removing the energy threshold entirely (energy > 0) mainly added post-fracture (stage IV) hits, consistent with the interpretation that this criterion predominantly suppresses friction-dominated signals after fracture. The central observation therefore does not depend critically on the specific threshold values. A quantitative, frequency-based classification remains necessary in future work to place noise rejection on an objective, transferable basis [26].
The test sample design proved to be appropriate for the test setup, with struts as defined breaking points. The FEM stress analysis and the experimental observations together support the sample design, with stress concentrating at the struts as intended. Consistent with this, more struts and therefore a higher contact area translate to higher load resistance with increased acoustic emission activity through a larger number of potential fracture locations. Garcia-Vilana et al. (2021) have shown that acoustic emission activity and the number of hits are proportional to defects in materials and verified their hypothesis with stress–strain evaluation in bone samples [27].
In the first analysis, we observed load resistance, meaning the maximum load before fracture, to increase with the thickness of the struts for both sample types. Furthermore, the difference in each identical structure itself (for example, 11 struts 0.4 mm vs. 0.8 mm) was more significant, meaning the leap in maximum load for 11 struts was higher than for 3 struts. This indicates that the difference in load resistance is more dominant with significantly higher contact area, also indicating that high contact-area samples can be directly differentiated from lower contact-area samples by their AE during push-out.
Whether an analogous contact-area dependence holds for osseointegrated implants cannot be inferred from the present surrogate data; for real bone, Walsh et al. (2020) report a contact-area dependence of fixation strength, which motivates, but does not validate, the surrogate analogy used here [28]. Looking at the resulting data, an increase in friction-induced hits with increasing contact area is visible, meaning that the elimination of these hits from inspected datasets through filtering needs to be carried out thoroughly, emphasizing the importance of post-processing in AE analysis.
With regards to the final optimization of this testing process and post-processing strategy, a quantitative signal-based analysis can lead to improved filtering, as already suggested by Behrens et al. (2019), where centroid frequency was introduced to identify damage stages [26]. This quantitative approach can be a subsequent step for further data evaluation and noise filtering.
For our qualitative analysis, focusing on simple 3-strut samples has proven to be beneficial for an initial evaluation, as the number of noise- and friction-induced hits can be reduced compared with the 11-strut samples. Differentiation of multiple stages in defect progression is a well-defined phenomenon in mechanical material testing. Zhao et al. (2020) have defined five stages of progressive failure in rock compression, similar to the stages presented in this work [29]. Differentiation of stages differs, however, resulting from the region of interest in acoustic emission analysis of BII, as the final point of fracture marks the end of analysis, as opposed to conventional testing, where a post-fracture stage is evaluated.
He et al. (2023) have already defined some observations of crack initiation in bone samples, where the first attempts at the classification of cracks have been done [30]. However, these prevent defined staging, as a simple bone fracture is hard to classify. The findings correlate with our study, as fracture and AE rise have also been identified in tested samples. Yet, by identifying an initial, emission-free stage, we extended the classification to a four-stage process for push-out testing.
The main aim of our setup is the detection of hits during the pre-fracture stage (II), which we hypothesize to contain early microstructural failure. Accumulation of cracks will ultimately lead to the absolute failure of the material. However, failure, being a macroscopic defect, is already detectable through the load course in conventional testing. Therefore, analysis of the fracture stage (III) is of less interest, as it is already detectable through conventional push-out testing. Our samples produced consistent AE hits during loading prior to the macroscopic load drop (pre-fracture stage II). We interpret these as candidate signatures of early microstructural failure; this interpretation remains to be confirmed by independent methods such as microscopy, micro-CT, or digital image correlation and is not established by acoustic data alone. The interpretation of stage II activity as early microstructural failure remains to be tested against independent evidence, and we did not perform imaging in this study. The pre-peak activity could, in principle, also originate from interfacial friction or fixture settling. To address this, a validation experiment is planned in which push-out loading is interrupted at defined states, and the specimen is imaged in each held state, so that newly formed damage can be correlated in space and time with the recorded AE. Establishing this spatial and temporal correspondence is the defined objective of subsequent work and is a prerequisite before microcrack interpretation can be confirmed. Importantly, such pre-drop activity is not accessible to conventional push-out or pull-out testing, which is the central methodological observation of this proof-of-concept [14,15]. Therefore, test runs present proof-of-concept for this testing process and emphasize the gain in informative value. However, attenuation and reflection of AE must be taken into consideration for further testing, as complex test plunger structures, multi-material transitions, and sample structure influence the detected signals. As Qi (1999) has shown, attenuation plays a major role in the energy and amplitude of AE, although amplitude is less influenced than energy [31]. By applying the mentioned couplant, we reduced the effect of attenuation. Yet, reflection through interface transitions and complex geometries needs to be further studied. Additionally, application of couplants on the interface of the plunger and specimen should be carried out in future testing.
Simplification of the multi-dimensional AE results was performed using PCA, reducing the original five-parameter space to two principal components while retaining 97.8% of the total variance. Although this dimensionality reduction facilitates visualization and interpretation, it should be noted that PCA is a linear transformation method and therefore captures only linear relationships between variables. Potential nonlinear interactions between AE parameters are not explicitly represented.
The results indicate that stage separation is predominantly governed by amplitude, energy, and duration, as reflected by their strong contribution to PC1. This suggests that the staging procedure is largely intensity-driven, which is consistent with progressive crack growth and increasing fracture activity. However, the dominance of PC1 (94% variance) also implies that the system’s behavior is essentially one-dimensional under the investigated conditions. Consequently, the observed stage differentiation may reflect gradual signal amplification rather than fundamentally different damage mechanisms. Furthermore, the overlap between stages II and III indicates that the transition between intermediate damage states is not sharply defined. This suggests that the current parameter set may not fully capture subtle mechanistic differences at these stages.
Overall, although PCA provides a robust and transparent framework for dimensionality reduction and staging verification, further investigations incorporating additional features, nonlinear analysis techniques, and/or independent validation methods would strengthen the interpretation of damage progression and improve stage discrimination.
Additional experiments on realistic samples are necessary to establish a solid database for acoustic emission testing in the context of bone–implant connections.
This testing process provides the opportunity to evaluate samples during loading and to identify non-visible defects before final failure. However, this benefit presupposes a thorough characterization of sample geometry and material, and the transfer of the present results to bone–implant testing is not trivial. The surrogate used here is a brittle, isotropic, homogeneous SLA resin with a well-defined fracture behavior, whereas bone is anisotropic, viscoelastic, and structurally heterogeneous, with a fracture process dominated by diffuse microcracking rather than discrete brittle failure. These differences are directly reflected in the acoustic response. For human femur tissue, Aggelis et al. (2015) reported that AE activity correlates with load and the onset of microfracture occurs at roughly one sixth of the maximum load, with waveform frequency content and risetime linked to the fracture mode [32]. Goodwin et al. (2017) further found that AE burst duration and frequency content differ significantly even between bone types, with vertebral compression fractures being prolonged and long-bone fractures abrupt [17]. Consequently, the AE parameter ranges and the stage boundaries identified here for the resin surrogate cannot be assumed to hold for bone, and the threshold values reported in this work are specific to the surrogate system. A quantitative comparison of the spectral characteristics of surrogate and bone AE, which requires the frequency–domain analysis identified above as future work, is a necessary next step before any transfer to biological samples, and dedicated comparative experiments on real bone specimens will be required to establish the corresponding parameter ranges. Especially the multi-material analysis of bone and implant is challenging due to the inhomogeneous bone structure, attenuation, and different material characteristics [19].
Future work will proceed in three steps. First, full-waveform acquisition will enable frequency–domain feature extraction (e.g., centroid and peak frequency, partial-power ratios), providing an objective basis for distinguishing fracture from friction signals independent of the present heuristic thresholds. Second, these features will be used to test the unsupervised and subsequently supervised classification of signal types on a larger specimen set, with the parameter-based stages of this study as an initial reference. Third, the resulting classification will be evaluated against independent damage evidence (microscopy or micro-CT) to establish whether pre-fracture AE activity corresponds to microstructural failure.

6. Conclusions

This study introduced and demonstrated the feasibility of an advanced push-out test stand combined with acoustic emission (AE) monitoring to characterize progressive structural failure and to resolve acoustic activity preceding macroscopic load drop in strut-structured, additive-manufactured samples. Through systematic post-processing, unwanted noise and friction signals were successfully reduced, allowing AE hits to be linked directly to distinct stages of failure. A four-stage fracture progression was defined, with particular emphasis on the pre-fracture stage, in which AE activity was observed prior to any macroscopic load response—activity we attribute, pending independent validation, to early microstructural failure. The results confirmed that increasing strut thickness and contact area enhances load resistance and AE activity, thereby correlating structural parameters with fracture behavior. The PCA results suggest that AE data analysis achieves results equivalent to conventional load analysis while offering considerable additional analytical potential that remains largely unexplored in this study. Moreover, the information obtained from AE analysis is substantially richer than that derived from simple load evaluation, as the fracture stages could be clearly identified in both testing approaches.
Although qualitative-parameter-based filtering proved effective for initial evaluation, future integration of quantitative, frequency-based signal analysis and machine-learning approaches is expected to improve reliability and enable automated classification of crack types. Overall, the presented methodology constitutes a proof-of-concept for combining load testing with AE analysis in BII research. By capturing acoustic activity that precedes catastrophic failure, this approach offers added value compared with conventional load testing and provides a methodological basis for subsequent studies on biological and bone–implant samples, which are required before any statement on clinical relevance can be made.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/app16147339/s1, Table S1: Sensitivity of stage-wise hit counts to filtering thresholds in 3-strut structures, Table S2: AE parameter ranges by push-out stage (3-strut structures).

Author Contributions

Conceptualization, methodology, investigation, writing—original draft preparation, visualization: K.P.R.; conceptualization: M.S.; supervision: F.M., P.M.-R., and R.L.; writing—review and editing, supervision: U.U., P.P.P., and U.P.F. All authors have read and agreed to the published version of the manuscript.

Funding

This research did not receive any specific grant from funding agencies in the public, commercial, or not-for-profit sectors.

Data Availability Statement

Data will be made available upon request.

Acknowledgments

Declaration of generative AI and AI-assisted technologies in the manuscript preparation progress: During the preparation of this work, the authors used an AI-based tool (FhGenie, Fraunhofer) to assist with language refinement. The AI did not generate original scientific content or conclusions. All resulting texts were carefully reviewed and revised by the authors, who take full responsibility for the content of the published article.

Conflicts of Interest

The authors declare no conflict of interest.

Abbreviations

The following abbreviations are used in this manuscript:
AEAcoustic Emission
AMPAmplitude
BIIBone–implant Interface
CADComputer-Aided Design
COUNCounts
DoEDesign of Experiments
DURDuration
ENEREnergy
EVDEigenvalue Decomposition
FEMFinite Element Method
HDTHit Definition Time
HLTHit Lockout Time
PCAPrincipal Component Analysis
PDTPeak Definition Time
PLBPencil Lead Break
RISERisetime
SLAStereolithography
SVDSingular Value Decomposition
D Singular Value Matrix
L 0 Initial Length
∆ L Elongation
M c e n t e r e d Centered Matrix of AE-Observations
P C j Principal Component Value
V j Right Singular Vector
v i Entry of AE Vector
v i , j ,   c e n t e r e d Centered Entry of AE Vector
λ 1 Eigenvalue
ξ Eigenvector
ε b r e a k Elongation at Break

References

  1. Albrektsson, T.; Johansson, C. Osteoinduction, osteoconduction and osseointegration. Eur. Spine J. 2001, 10, S96–S101. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  2. Brånemark, R.; Brånemark, P.I.; Rydevik, B.; Myers, R.R. Osseointegration in skeletal reconstruction and rehabilitation: A review. J. Rehabil. Res. Dev. 2001, 38, 175–181. [Google Scholar] [PubMed]
  3. Puleo, D.A.; Nanci, A. Understanding and controlling the bone-implant interface. Biomaterials 1999, 20, 2311–2321. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  4. Gao, X.; Fraulob, M.; Haïat, G. Biomechanical behaviours of the bone-implant interface: A review. J. R. Soc. Interface 2019, 16, 20190259. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  5. Lee, J.W.Y.; Bance, M.L. Physiology of Osseointegration. Otolaryngol. Clin. N. Am. 2019, 52, 231–242. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  6. Haas, R.; Pommer, B. Die Extraktionswunde: Anatomische und Physiologische Grundlagen der Sofortimplantation. 2015. Available online: https://www.researchgate.net/publication/294871404_Die_Extraktionswunde_Anatomische_und_physiologische_Grundlagen_der_Sofortimplantation (accessed on 25 June 2026).
  7. Córdova, L.A.; Jara-Sepúlveda, M.C.; Brañes-Aroca, M.; Marchesani-Carrasco, F.; Cartes-Velásquez, R. Osteoimmunology drives dental implant osseointegration: A new paradigm for implant dentistry. Jpn. Dent. Sci. Rev. 2021, 57, 12–19. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  8. Park, J.B.; Lakes, R.S. Introduction to Biomaterials. In Biomaterials: An Introduction; Park, J.B., Lakes, R.S., Eds.; Springer: Boston, MA, USA, 1992; pp. 1–6. [Google Scholar]
  9. Shalabi, M.M.; Gortemaker, A.; Van, M.A.; Jansen, J.A.; Creugers, N.H.J. Implant surface roughness and bone healing: A systematic review. J. Dent. Res. 2006, 85, 496–500. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  10. Anil, U.; Singh, V.; Schwarzkopf, R. Diagnosis and Detection of Subtle Aseptic Loosening in Total Hip Arthroplasty. J. Arthroplast. 2022, 37, 1494–1500. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  11. Buser, D.; Schenk, R.K.; Steinemann, S.; Fiorellini, J.P.; Fox, C.H.; Stich, H. Influence of surface characteristics on bone integration of titanium implants. A histomorphometric study in miniature pigs. J. Biomed. Mater. Res. 1991, 25, 889–902. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  12. Deng, J.; van Duyn, C.; Cohen, D.J.; Schwartz, Z.; Boyan, B.D. Strategies for Improving Impaired Osseointegration in Compromised Animal Models. J. Dent. Res. 2024, 103, 467–476. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  13. Schwarz, M.L.R.; Kowarsch, M.; Rose, S.; Becker, K.; Lenz, T.; Jani, L. Effect of surface roughness, porosity, and a resorbable calcium phosphate coating on osseointegration of titanium in a minipig model. J. Biomed. Mater. Res. Part A 2009, 89, 667–678. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  14. Brånemark, R.; Skalak, R. An in-vivo method for biomechanical characterization of bone-anchored implants. Med. Eng. Phys. 1998, 20, 216–219. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  15. Barckman, J.; Baas, J.; Sørensen, M.; Bechtold, J.E.; Soballe, K. Periosteal augmentation of allograft bone and its effect on implant fixation—An experimental study on 12 dogs. Open Orthop. J. 2013, 7, 18–24. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  16. Watanabe, Y.; Takai, S.; Arai, Y.; Yoshino, N.; Hirasawa, Y. Prediction of mechanical properties of healing fractures using acoustic emission. J. Orthop. Res. Off. Publ. Orthop. Res. Soc. 2001, 19, 548–553. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  17. Goodwin, B.D.; Pintar, F.A.; Yoganandan, N. Acoustic Emission Signatures During Failure of Vertebra and Long Bone. Ann. Biomed. Eng. 2017, 45, 1520–1533. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  18. Holweg, K.; Brandt, J.; Bierögel, C.; Grellmann, W.; Altenbach, H. Schädigungscharakterisierung der Implantat-Knochen-Grenzfläche. In Grenzflächen bei Implantaten—Mechanische und Biologisch-Chemische; DVM—Deutscher Verband für Materialforschung und-prüfung e.V.: Berlin, Germany, 2004; pp. 9–17. [Google Scholar]
  19. ASTM E976-10; Standard Guide for Determining the Reproducibility of Acoustic Emission Sensor Response. ASTM International: West Conshohocken, PA, USA, 2010.
  20. García-Vilana, S.; Sánchez-Molina, D.; Abdi, H. Acoustic Emission in Bone Biomechanics: A Comprehensive Review of Mechanical Properties and Predictive Damage Modeling. Sensors 2025, 25, 598. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  21. Unthnorsson, R. Hit Detection and Determination in AE Bursts. In Acoustic Emission: Research and Applications; Sikorski, W., Ed.; IntechOpen: London, UK, 2013. [Google Scholar]
  22. Astakhov, V.P. Mechanical Properties of Engineering Materials: Relevance in Design and Manufacturing. In Materials Forming, Machining and Tribology, Introduction to Mechanical Engineering; Davim, J.P., Ed.; Springer: Cham, Switzerland, 2018; pp. 3–41. [Google Scholar]
  23. Greenacre, M.; Groenen, P.J.F.; Hastie, T.; D’Enza, A.I.; Markos, A.; Tuzhilina, E. Principal component analysis. Nat. Rev. Methods Primers 2022, 2, 100. [Google Scholar] [CrossRef] [Scilit]
  24. Bargel, H.-J.; Schulze, G. Werkstoffkunde, 12th ed.; Springer Vieweg: Berlin/Heidelberg, Germany, 2018. [Google Scholar]
  25. Xu, J.; Ashraf, S.; Khan, S.; Chen, X.; Akbar, A.; Farooq, F. Micro-cracking pattern recognition of hybrid CNTs/GNPs cement pastes under three-point bending loading using acoustic emission technique. J. Build. Eng. 2021, 42, 102816. [Google Scholar] [CrossRef] [Scilit]
  26. Behrens, B.A.; Hübner, S.; Wölki, K. Acoustic emissions during tensile test of DC06 and HCT600X. Mater. Werkst. 2019, 50, 796–809. [Google Scholar] [CrossRef] [Scilit]
  27. García-Vilana, S.; Sánchez-Molina, D.; Llumà, J.; Fernández-Osete, I.; Veláquez-Ameijide, J.; Martínez-González, E. A predictive model for fracture in human ribs based on in vitro acoustic emission data. Med. Phys. 2021, 48, 5540–5548. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  28. Walsh, W.R.; Pelletier, M.H.; Bertollo, N.; Lovric, V.; Wang, T.; Morberg, P.; Parr, W.C.H. Bone ongrowth and mechanical fixation of implants in cortical and cancellous bone. J. Orthop. Surg. Res. 2020, 15, 177. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  29. Zhao, K.; Yang, D.; Gong, C.; Zhuo, Y.; Wang, X.; Zhong, W. Evaluation of internal microcrack evolution in red sandstone based on time–frequency domain characteristics of acoustic emission signals. Constr. Build. Mater. 2020, 260, 120435. [Google Scholar] [CrossRef] [Scilit]
  30. He, W.; Yan, D.; Liu, M.; Gao, X.; Zhang, Y.; Xu, D. Acoustic Emission Characteristics of Different Porcine Bones Under Loading. Int. J. Acoust. Vib. 2023, 28, 44–49. [Google Scholar] [CrossRef] [Scilit]
  31. Qi, G. Attenuation of acoustic emission body waves in acrylic bone cement and synthetic bone using wavelet time-scale analysis. J. Biomed. Mater. Res. 2000, 52, 148–156. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  32. Aggelis, D.G.; Strantza, M.; Louis, O.; Boulpaep, F.; Polyzos, D.; van Hemelrijck, D. Fracture of human femur tissue monitored by acoustic emission sensors. Sensors 2015, 15, 5803–5819. [Google Scholar] [CrossRef] [Scilit] [PubMed]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.