Abstract
Resource-efficient construction binders must increase secondary-material use without losing performance needed for building products. Copper smelting slag (CSS) replaced 0%, 20%, 40%, or 60% of a blast furnace slag (BFS)-fly ash (FA) precursor (BFS:FA = 3:2; liquid-to-solid ratio = 0.6). Paste flow, strength, phase composition, porosity, and microstructure were characterized; strength in 5 wt.% Na2SO4 and water-extractable chloride after 7% NaCl exposure were measured. Raising CSS from 0% to 60% increased paste spread from 189.30 to 198.35 mm but reduced 28-day paste and mortar compressive strengths from 60.0 to 31.4 MPa and 44.7 to 22.3 MPa, respectively. Mortar with 20% CSS reached 40.5 MPa (90.6% of the reference). Intrudable porosity increased from 5.11% to 12.17%, and mean pore-entry diameter from 14.71 to 29.76 nm. Higher CSS contents showed smaller late-age strength decreases during sulfate immersion, but the CSS-free reference retained the highest 90-day strength. CSS-containing mortars had lower water-extractable chloride. Moderate CSS replacement can increase resource use while retaining mortar strength.
1. Introduction
The construction sector consumes large quantities of mineral resources while generating demand for lower-impact cementitious products. Incorporating metallurgical residues into binder-based construction materials can reduce waste storage and conserve conventional raw materials, provided that the resulting products retain the mechanical capacity and exposure-specific performance required for their intended applications. Copper smelting slag (CSS) is generated during the pyrometallurgical production of copper and commonly contains substantial amounts of iron and silicon. On the basis of global primary copper production and a slag-to-copper mass ratio of approximately 2.2, Klaffenbach et al. estimated that more than 45 Mt of copper slag was generated worldwide in 2021 [1]. Reported construction uses include aggregate, road materials, cemented mine backfill, cement replacement, and precursors for alkali-activated binders [2,3,4,5]. These applications show the scale of the resource-utilization opportunity, but they also demonstrate that CSS performance depends strongly on its mineralogy, fineness, processing history, and role within the composite.
CSS should be distinguished from copper mine tailings. CSS is formed at high temperature during smelting, whereas copper tailings remain after ore beneficiation. The two residues can differ markedly in particle size, glass content, mineralogy, iron-bearing phases, and dissolution behavior; conclusions obtained for tailings-based binders therefore cannot be transferred directly to smelting slag. In alkali-activated BFS-FA binders, the calcium-rich and predominantly amorphous BFS can contribute to calcium aluminosilicate hydrate formation, while FA supplies aluminosilicate species and can participate in calcium-containing or low-calcium reaction products [6]. By contrast, Fe-rich CSS dominated by crystalline fayalite and magnetite is expected to react more slowly under conventional alkaline activation. It may contribute through particle packing, limited dissolution, or interaction with surrounding reaction products, but replacing BFS and FA with CSS can also dilute the reactive precursor and reduce the amount of binding phase. Recent work on copper and fayalite slags confirms that the balance between CSS content, reactive co-precursors, and activation conditions governs strength, pore development, and thermal response [4,7,8].
Recent studies have substantially broadened the construction applications of slag- and fly-ash-based binders. Off-specification fly ash has been incorporated into ultra-high-performance concrete together with mixture-design and life-cycle assessment approaches [9]. Alkali-activated FA-slag matrices have also been developed as high-strength, strain-hardening composites with high tensile ductility [10,11], while FA-GGBS-silica-fume binders have been combined with recycled aggregates to address both engineering performance and environmental impact [12,13]. Other investigations have examined fiber-reinforced FA-based geopolymer mortars at elevated temperatures [14], fly-ash-dominated engineered geopolymer composites under different alkalinity levels [15], and the thermal degradation of hybrid FA-slag geopolymers [16]. Together, these studies demonstrate that slag and fly ash can serve in concretes, mortars, high-performance composites, recycled-aggregate systems, and other construction products. They also show that performance cannot be inferred from precursor classification alone because it depends on calcium availability, activator chemistry, aggregate incorporation, curing, and the intended exposure condition.
Resistance to aggressive salts requires separate consideration. The sulfate response of alkali-activated BFS-FA cements varies with the BFS/FA ratio, Na2O concentration, silicate modulus, and sulfate type; MgSO4, for example, can cause substantially different reactions from Na2SO4 [17]. In chloride-containing systems, the BFS/FA ratio and solution chemistry affect AFm-related chemical binding and chloride retention by calcium- and sodium-aluminosilicate gels [18]. Environmental testing of Fe-rich fayalite-slag mortars further shows that performance under combined sulfate-chloride solutions, freeze–thaw exposure, and other conditions depends on the presence of reactive ladle slag or BFS co-precursors [19]. These findings indicate that strength retention during sulfate immersion, water-extractable chloride, chloride transport, and chemical binding are related but distinct indicators. A favorable result from one measurement therefore should not be treated as proof of a general improvement in durability.
Existing CSS studies have mainly addressed mechanical performance, thermal behavior, shrinkage, mine-backfill applications, or environmental assessment, while sulfate and chloride behavior has often been examined in different material systems or as a single exposure condition. Limited information is available on how progressive replacement of the same BFS-FA precursor by crystalline CSS simultaneously affects fresh behavior, load-bearing capacity, matrix continuity, sulfate-immersion strength response, and water-extractable chloride. The construction task is therefore to increase the use of a secondary metallurgical resource while retaining the strength and exposure compatibility required for binder-based products. This study compares 0%, 20%, 40%, and 60% CSS replacement in a BFS-FA binder with a fixed total liquid-to-solid ratio. Flowability, paste and mortar strengths, XRD, MIP, FTIR, TG, and SEM were used to characterize the initial materials, while sodium sulfate immersion and NaCl exposure were used to obtain exposure-specific strength and chloride-extraction indicators. The objective is to define the resulting performance trade-offs and formulation limits, rather than to assume that CSS addition necessarily improves sulfate durability or chloride transport resistance.
2. Materials and Methods
2.1. Raw Materials
Blast furnace slag (BFS), fly ash (FA), and copper smelting slag (CSS) were used as the powder constituents, while quartz sand was used as the fine aggregate for mortar preparation. The BFS was obtained from a tailings-sand plant in Henan, China, and the FA was Grade II fly ash from Henan Borun Casting Materials Co., Ltd., China (Zhengzhou, Henan, China). The CSS was obtained from Zijin Mining at Zijinshan, Fujian, China. It was received as a fine, dry powder and passed through a 200-mesh sieve before use. According to the product specification, the sodium silicate solution had a nominal modulus of 3.4 and contained 59.5 wt.% SiO2, 19.5 wt.% Na2O, and 21.0 wt.% H2O. Analytical-grade flake NaOH was purchased from Babaiwantang Daily Necessities in Bincheng, Shandong Province, China. Table 1 summarizes the oxide compositions of the powder constituents. BFS mainly consisted of SiO2 (32.54 wt.%), Al2O3 (18.83 wt.%), and CaO (33.67 wt.%), whereas FA was predominantly composed of SiO2 (45.10 wt.%) and Al2O3 (36.80 wt.%). CSS was characterized by a high iron content, expressed as 57.51 wt.% Fe2O3 equivalent, together with 27.73 wt.% SiO2.
Table 1.
Oxide compositions of BFS, FA, and CSS (wt.%).
Figure 1 presents the particle size distributions measured by laser diffraction using a Malvern Mastersizer particle size analyzer. The mean particle sizes of BFS, FA, and CSS were 13.40, 16.58, and 30.39 μm, respectively, indicating that CSS was coarser than BFS and FA. Figure 2 shows their X-ray diffraction (XRD) patterns. BFS exhibited a predominantly amorphous structure, while quartz and mullite were the main crystalline phases identified in FA. The principal crystalline phases in CSS were fayalite (Fe2SiO4) and magnetite (Fe3O4). The iron-rich crystalline mineralogy of CSS may influence the grinding requirements needed to achieve a target fineness. However, the reported bulk iron content and particle-size distribution alone do not establish greater grinding difficulty than for BFS or FA.
Figure 1.
Particle size distributions of BFS, FA, and CSS.
Figure 2.
XRD patterns of BFS, FA, and CSS.
2.2. Mixture Proportions and Specimen Preparation
Table 2 gives the formulations of the geopolymer specimens. Figure 3 summarizes the experimental program, including formulation levels, preparation conditions, specimen allocation, test schedules and measured indicators. Four mixtures, designated FS, FS-20, FS-40, and FS-60, were prepared by replacing 0%, 20%, 40%, and 60% of the combined BFS–FA precursor with CSS by mass, respectively. The BFS-to-FA mass ratio in the remaining precursor was maintained at 3:2. This ratio was selected on the basis of extensive prior laboratory screening of candidate BFS-to-FA proportions, in which 3:2 gave the best overall performance under the formulation conditions used in the present study. At this ratio, BFS remained the majority calcium-bearing precursor, while FA supplied a substantial aluminosilicate fraction. The ratio was then kept constant across the CSS replacement series so that CSS replacement remained the principal powder-composition variable. The selected ratio is specific to the present raw materials and activation and curing conditions and is not presented as a universal optimum for alkali-activated BFS-FA binders. Sodium silicate and NaOH were used as the alkaline activator, and the liquid-to-solid (L/S) ratio was fixed at 0.6 for all mixtures. Based on the stated sodium-silicate composition and the nominal NaOH addition in Table 2, the complete activator had a nominal Ms of 1.72, where Ms is the molar SiO2/Na2O ratio after NaOH addition. Its nominal total Na2O dosage was 7.16 wt.% of the total powder mass. Both values were calculated on an anhydrous NaOH basis. Both paste and mortar specimens were prepared for each formulation. The mortars additionally contained quartz sand at a sand-to-precursor mass ratio of 0.4. This relatively low ratio produced a binder-rich comparative mortar and was kept constant across the series so that the effects of CSS replacement could be compared under the same aggregate loading. The sand content was not optimized, and the ratio is not intended to represent a conventional structural-mortar proportion; the mortar results are therefore limited to this formulation.
Table 2.
Formulations of geopolymer specimens.
Figure 3.
Experimental program for CSS-containing alkali-activated BFS–FA pastes and mortars.
Deionized water was produced using a water purification unit. To prepare the alkaline activator for each batch, 240.6 g of sodium silicate solution was placed in a beaker. Subsequently, 50.4 g of flake NaOH and half of the total deionized water (214 g) were added, and the mixture was stirred until homogeneous. It was then allowed to stand for 12 h and cool naturally to room temperature. The remaining 214.5 g of deionized water was subsequently added, and the activator was stirred again until homogeneous before use. For paste preparation, BFS, FA, and CSS were first dry-mixed, followed by the addition of the prepared alkaline activator. The mixture was homogenized in a JJ-5 mortar mixer for 2 min at low speed and then 2 min at high speed. For mortar preparation, quartz sand was incorporated together with the powder constituents, and the mixture was blended with the alkaline activator using the same mixing procedure.
The fresh pastes and mortars were cast into 40 mm × 40 mm × 160 mm three-gang plastic molds and compacted on a vibrating table for 2 min to remove entrapped air. Photographs of the prepared prismatic specimens during immersion are provided in Figure 3. All specimens were covered with plastic film and maintained at room temperature for 24 h. After demolding, they were transferred to a constant-temperature and constant-humidity curing chamber maintained at 25 °C and 95% relative humidity until the designated testing ages or subsequent immersion. The test program used two flowability determinations per mixture, three prisms per mixture and test condition for strength measurements, and three mortar specimens per mixture and chloride-exposure period.
2.3. Test Methods
2.3.1. Flowability
The flowability of geopolymer pastes was determined using a truncated cone test. The apparatus consisted of a horizontal glass plate measuring 500 mm × 500 mm and a truncated cone mold with an upper inner diameter of 36 mm, a lower inner diameter of 60 mm, and a height of 60 mm. Before testing, the glass plate and cone were cleaned with a damp cloth. The freshly mixed paste was poured into the cone and leveled, after which the cone was lifted vertically. After 30 s, the spread diameters were measured along two perpendicular directions, and their mean was taken as the result of one determination. Each mixture was tested twice, and the average was reported as its flowability.
2.3.2. Mechanical Properties
The flexural and compressive strengths of geopolymer pastes and mortars were measured using a WDW-100C universal testing machine. Prismatic specimens measuring 40 mm × 40 mm × 160 mm were subjected to three-point bending at a loading rate of 0.1 kN/s. The resulting prism halves were subsequently tested in compression at a loading rate of 1 kN/s. Three prisms were tested for each mixture and condition, and the mean strengths were reported. Mechanical tests were conducted at the designated curing ages and after immersion in sodium sulfate solution or distilled water.
2.3.3. Microstructural Characterization
Thermogravimetric analysis (TG, Mettler-Toledo LF 1100, Switzerland) was performed to examine the mass-loss behavior of the geopolymer pastes after 28 days of curing. For the 28-day paste characterization, material remaining after compressive strength testing was used, with powders or fragments prepared as required by each technique. Powder samples were collected from the central regions of the specimens. For the present reanalysis, normalized mass-temperature coordinates were recovered from the vector outlines of the original TG figure using its axis ticks for calibration. The four traces were interpolated onto a common 1 °C grid over 31–895 °C. A cubic local polynomial was fitted over a 41-point moving window (a 40 °C span), equivalent to Savitzky–Golay smoothing, and its analytical temperature derivative was displayed as the positive mass-loss rate, -dM/dT, where M is normalized mass (%). Full-window DTG estimates are shown over 51–875 °C; the first and last 20 °C were excluded to avoid endpoint estimates. The reconstructed DTG curves are figure-derived estimates, and the 1 °C grid describes numerical interpolation rather than the original acquisition interval. Sensitivity to 31 -and 61-point windows was also checked. Peak positions and rates are approximate because graphical recovery and smoothing affect the derivative.
Crystalline phases were identified using an X-ray diffractometer (XRD, Bruker D8 Advance, Germany) with Cu Kα radiation. Measurements were conducted over a 2θ range of 10–80° at a scanning rate of 0.2°/s. Before analysis, the samples were ground and passed through a 200-mesh sieve.
Fourier transform infrared spectra (FTIR, Agilent Technologies, USA) were recorded over 400–4000 cm−1 using the KBr pellet method. The samples were dried, finely ground, mixed uniformly with spectroscopic-grade KBr, and pressed into pellets. The spectra were baseline-corrected and normalized before comparison.
Mercury intrusion porosimetry (MIP, AutoPore IV 9510, USA) was used to determine the intrudable porosity and pore-entry size distribution of the 28-day pastes. The instrument operated over a pressure range of 5–30,000 psi (approximately 0.03–207 MPa). Pore sizes were expressed as equivalent pore-entry diameters derived from the intrusion pressure. For descriptive classification, the IUPAC pore-width limits were applied to these equivalent entry diameters: below 2 nm, 2–50 nm and above 50 nm for the micropore, mesopore and macropore ranges, respectively [20]. The available MIP output comprised intrudable porosity, average pore-entry diameter and plotted differential intrusion distributions. A critical or threshold pore diameter and pore-class volume fractions were not calculated because an extractable and validated raw cumulative intrusion series and a predefined calculation criterion were not available for the present reanalysis.
Microstructure and elemental distributions were examined using scanning electron microscopy coupled with energy-dispersive X-ray spectroscopy (SEM-EDS, SEM5000, China). Specimens approximately 6 mm × 6 mm × 1 mm were collected from the central regions of the samples. A natural fracture surface was selected for observation, while the opposite face was ground to facilitate mounting. The specimens were vacuum-dried for 12 h before analysis. SEM images were acquired at an accelerating voltage of 7 kV and a working distance of 10.91 mm, whereas EDS analysis was conducted at 15 kV. Elemental mapping was performed on the chloride-exposed specimens. The EDS maps were used only for qualitative comparison of local elemental distributions in selected fields; no quantitative elemental concentrations or phase assignments were derived from them.
2.3.4. Sulfate Exposure
The corrosion resistance of the geopolymer specimens under sulfate exposure was evaluated by immersion testing with reference to GB/T 749–2008, with adaptations to the material system and exposure conditions. After 28 days of curing at 25 °C and 95% relative humidity, specimens from each mixture were divided into two groups (Figure 4). One group was immersed in a 5 wt.% sodium sulfate (Na2SO4) solution, while the other was immersed in distilled water as a reference. Both groups were maintained at 20 °C throughout immersion. The specimens were placed in covered plastic containers, with the liquid level maintained at least 10 mm above their upper surfaces to ensure complete immersion and minimize evaporation.
Figure 4.
Photographs of the prepared prismatic specimens during immersion in (a) distilled water and (b) sodium sulfate solution.
Both immersion media were renewed every seven days to limit changes in solution composition caused by leaching and ion accumulation. During each renewal, the specimens were carefully removed and gently rinsed with deionized water to remove loosely attached surface deposits. Excess surface water was wiped off before the specimens were returned to freshly prepared immersion media. At 7, 28, and 90 days of immersion, the specimens were removed from the media, surface water was wiped off, and flexural and compressive strengths were measured in the surface-dried condition. These durations refer to exposure times following the initial 28-day curing period.
Following the flexural-strength-based coefficient definition in GB/T 749–2008, the corrosion resistance coefficient was calculated as follows:
where (K(t)) is the dimensionless sulfate resistance coefficient at exposure time (t), and Rn and Rw are the mean flexural strengths (MPa) of specimens immersed in sodium sulfate solution and distilled water, respectively. The coefficient was reported to two decimal places. The value above unity indicates a higher flexural strength under sulfate exposure than under the corresponding water-reference condition. Compressive strength after sulfate exposure was measured and reported separately in Section 3.4.1 as a complementary mechanical indicator; it was not substituted into K because the adopted standard definition uses flexural strength. K provides an exposure-specific comparison of flexural strengths, and the strength measurements alone do not quantify sulfate penetration, expansion or the associated reaction mechanisms.
K(t) = Rn/Rw
2.3.5. Chloride Exposure
Chloride exposure testing was performed with reference to GB/T 50082–2009, with adaptations for the single-face immersion and subsequent chloride extraction procedure. Three mortar specimens were used for each mixture and chloride-exposure period. The geopolymer mortar specimens were first cured for 14 days at 25 °C and 95% relative humidity. Five faces of each specimen were then sealed with epoxy resin, leaving one face exposed. The specimens were immersed in a 7% NaCl solution for 30 and 90 days. These durations refer to immersion times following the initial 14-day curing period.
After each exposure period, powder samples were collected for water-extractable chloride measurements. For each determination, 1.0 g of powder was added to 50 mL of deionized water and magnetically stirred for 1–2 min. The suspension was sealed and allowed to stand for 24 h before the chloride concentration in the aqueous extract was measured using a chloride analyzer (SSWY-820, China). Three determinations were performed for each mixture and exposure period, and the mean value was reported.
The measured chloride originated from the external NaCl solution and represented the fraction recovered from the sampled material by water extraction. The results were used to compare water-extractable chloride accumulation among mixtures under identical exposure conditions. SEM-EDS mapping was additionally performed on the exposed specimens to examine the spatial distributions of chlorine and other constituent elements.
3. Results and Discussion
3.1. Flowability
Table 3 presents the flowability of geopolymer pastes containing different CSS contents. At a constant L/S ratio of 0.6, the mean flowability values were 189.20, 193.35, 196.20, and 198.35 mm for FS, FS-20, FS-40, and FS-60, respectively. The difference between FS and FS-60 was 9.15 mm, or approximately 4.8%. Because only two determinations were performed per mixture and no inferential significance test was conducted, this small numerical difference is reported descriptively and does not establish a statistically significant improvement in paste flowability. The mean increments also became smaller at successive replacement steps. At 60% replacement, the 4.8% difference in mean flowability accompanied a 47.7% reduction in 28-day paste compressive strength (Section 3.2).
Table 3.
Flowability of geopolymer pastes containing different CSS contents.
3.2. Mechanical Properties
Figure 5 presents the mechanical properties of geopolymer pastes and mortars at different curing ages. Increasing the CSS content reduced the compressive strengths of both specimen types. At 28 days, the paste compressive strength decreased from 60.0 MPa for FS to 31.4 MPa for FS-60, corresponding to a reduction of 47.7%. The mortar compressive strength decreased from 44.7 to 22.3 MPa, a reduction of 50.1%. Paste flexural strength also decreased from 7.1 to 3.8 MPa. These reductions are consistent with replacement of the BFS–FA fraction by predominantly crystalline CSS, although the present measurements do not independently quantify the reaction degree of each precursor. As the replacement level increased, the amount of reactive precursor available to form binding products decreased. At 28 days, FS-20, FS-40 and FS-60 retained 80.7%, 71.8% and 52.3% of the FS paste compressive strength, respectively; the corresponding mortar values were 90.6%, 75.8% and 49.9%. All formulations nevertheless gained compressive strength between 7 and 28 days. FS-60 paste increased from 20.9 to 31.4 MPa, a relative gain of 50.2%, while its mortar increased from 17.6 to 22.3 MPa, a gain of 26.7%. These changes indicate continued hardening, although the age-related gains did not compensate for the loss in absolute strength relative to FS. They also do not isolate the contribution of CSS reaction from that of the remaining BFS and FA.
Figure 5.
Mechanical properties of geopolymer specimens at different curing ages: (a) paste compressive strength, (b) paste flexural strength, (c) mortar compressive strength, and (d) mortar flexural strength.
Although mortars exhibited lower compressive strengths than the corresponding pastes, their seven-day flexural strengths were higher. The flexural strengths of FS, FS-20, FS-40, and FS-60 mortars were 10.7, 10.1, 8.5, and 5.6 MPa, respectively, compared with 3.9, 3.2, 2.9, and 1.8 MPa for the corresponding pastes. Quartz sand reduces the volume fraction of shrinkable paste and can restrain bulk deformation [21,22,23]. Where adequate aggregate–paste bonding develops, sand particles may also deflect propagating cracks and increase the crack path length, contributing to resistance under bending. Conversely, interfacial discontinuities can introduce weak regions that reduce compressive strength. The different responses under compression and bending thus reflect the competing effects of aggregate incorporation on matrix continuity, deformation, and crack propagation.
The age-dependent mortar flexural response differed from the compressive response and was not monotonic with CSS content at 28 days. FS decreased from 10.7 MPa at 7 days to 4.8 MPa at 28 days, whereas FS-20 remained at a reported mean of 10.1 MPa. FS-40 and FS-60 increased from 8.5 to 9.2 MPa and from 5.6 to 8.8 MPa, respectively. Consequently, all CSS-containing mortars had higher mean 28-day flexural strengths than FS despite their lower compressive strengths. This suggests that bending was influenced by factors beyond matrix compressive strength. Under air curing, moisture loss can induce shrinkage [24,25,26,27], while aggregate restraint can generate local interfacial tensile stresses [28,29,30]. Precursor replacement may modify these stresses [19,31,32], but shrinkage, interfacial debonding and crack evolution were not measured directly. Their individual contributions therefore remain possible explanations rather than demonstrated causes of the observed flexural response.
3.3. Microstructural Characteristics
3.3.1. Phase Assemblage
Figure 6 shows the XRD patterns of the geopolymer pastes after 28 days of curing. The FS specimen exhibited sharp reflections assigned to quartz and mullite, mainly inherited from FA, together with reflections attributed to calcite. A broad diffuse feature was also observed at approximately 20–30° 2θ, indicating the presence of disordered phases. This diffuse contribution may include overlapping signals from unreacted precursor glass and poorly ordered reaction products. Possible C-(A)-S-H-type or N-A-S-H-type contributions are literature-informed interpretations for related alkali-activated systems [4,16,33]. These candidate assignments do not establish the identity, coexistence or relative amounts of individual gels in the present mixtures.
Figure 6.
XRD patterns of geopolymer pastes containing different CSS contents after 28 days of curing.
As the CSS content increased from 20% to 60%, the reflections of fayalite and magnetite became more prominent, consistent with the increasing proportion of CSS-derived crystalline phases. In contrast, the reflections associated with quartz and mullite became relatively less prominent as the FA fraction decreased. These changes mainly reflect the altered proportions of the constituent phases following precursor replacement, rather than the formation of new crystalline reaction products.
The persistence of fayalite and magnetite indicates that residual crystalline CSS phases remained after curing. Increasing CSS replacement also reduced the initial proportions of BFS and FA in the mixture. This change in precursor proportions is consistent with the strength reductions in Section 3.2. The qualitative patterns do not exclude partial dissolution of CSS or quantify its reacted fraction, and relative peak prominence also depends on the greater initial CSS content. The overlapping diffuse contributions do not uniquely identify individual gels or determine their amounts. The XRD evidence supports residual crystalline phases and qualitative phase-composition differences; it does not independently confirm C-(A)-S-H or N-A-S-H formation, their relative abundance, or the extent of precursor activation.
3.3.2. Pore Structure
Figure 7 presents the MIP pore-entry size distributions of the 28-day pastes. All mixtures exhibited fine-pore-entry contributions below approximately 30 nm. In addition, FS-40 and FS-60 showed broader intrusion features within approximately 100–1000 nm, which were more prominent than those of FS and FS-20. Under this classification, the features below 30 nm lie in the mesopore-size entry range, whereas the 100–1000 nm features lie in the macropore-size entry range and overlap pore sizes often described as capillary-scale in cementitious matrices. Approximate coarse modal positions read from the plotted differential distributions were about 200 nm for FS-40 and 600 nm for FS-60. These plotted modes are not independently calculated critical or threshold pore diameters; the multi-peaked and broad distributions do not support a reproducible single value from the plotted image alone. Fine-entry contributions were therefore retained while the contribution from larger accessible entries increased at higher CSS replacement. This coexistence explains why the average pore-entry diameter should not be equated with the position of the largest intrusion peak.
Figure 7.
Pore-entry size distributions of geopolymer pastes after 28 days of curing.
The quantitative parameters in Table 4 confirm this trend. The average pore-entry diameter increased from 14.71 nm for FS to 15.75, 24.01, and 29.76 nm for FS-20, FS-40, and FS-60, respectively. The corresponding intrudable porosity increased from 5.11% to 6.82%, 9.15%, and 12.17%. Although the four average entry diameters fall within the IUPAC mesopore-size range, these averages do not exclude the macropore-size access features observed for FS-40 and FS-60. Because size-class volumes were not integrated from raw cumulative intrusion data, changes in the mesopore-, macropore- or capillary-void fractions cannot be quantified from Table 4. At 60% replacement, the average diameter was approximately twice that of FS, while porosity increased by 7.06 percentage points. The change was not proportional to replacement level: the average diameter increased only from 14.71 to 15.75 nm at 20% CSS, then to 24.01 nm at 40% CSS.The FS-60 porosity was 2.38 times the FS value. An exploratory ordinary least-squares regression using the four 28-day paste mixture means gave fc,28 = 77.466 − 3.818P (R2 = 0.967; n = 4), where fc,28 is compressive strength in MPa and P is intrudable porosity expressed as a percentage. The fitted slope corresponds to a 3.818 MPa decrease in mean strength per percentage-point increase in intrudable porosity within this series. The fit quantifies a strong negative association but does not establish an independent causal effect of porosity because CSS replacement, precursor composition, and effective activation conditions changed together. The regression is restricted to 28-day pastes and is not extended to mortar strength or exposure-related behavior. Greater accessible void space and larger pore entries are consistent with a reduced effective area of load-bearing matrix and more potential locations for stress concentration. The IUPAC labels describe equivalent entry-size ranges rather than pore-body dimensions or capillary-void fractions, and MIP does not quantify closed pores or total porosity. The appearance of macropore-size features is consistent with coarser accessible paths, but MIP characterized 28-day pastes before exposure, whereas sulfate strength testing used immersed pastes and chloride testing used mortars under separate histories; the classification therefore does not establish sulfate resistance or chloride transport. This pore coarsening is consistent with dilution of the reactive precursor, in which less binding material is available to fill interparticle spaces and form a continuous matrix. The resulting increase in accessible void space provides a microstructural explanation for the reduced compressive strength.
Table 4.
Average pore-entry diameter and intrudable porosity of geopolymer pastes after 28 days of curing.
3.3.3. FTIR Spectra
Figure 8 presents the FTIR spectra of the geopolymer pastes after 28 days of curing. The broad band near 3460 cm−1 is associated with O–H stretching in water and hydroxyl-bearing species, while the band near 1650 cm−1 is assigned mainly to H–O–H bending. The absorption band near 1440 cm−1 corresponds to carbonate stretching, consistent with the identification of calcite by XRD.
Figure 8.
FTIR spectra of 28-day geopolymer pastes: (a) FS, (b) FS−20, (c) FS−40, and (d) FS−60.
The principal absorption band, attributed to asymmetric Si–O–T stretching where T represents Si or Al, shifted from 995 cm−1 for FS to 989, 985 and 981 cm−1 for FS-20, FS-40 and FS-60, respectively. The total shift of 14 cm−1 indicates a change in the local silicate or aluminosilicate bonding environment as precursor proportions changed [4,7,34]. Relative to FS, the shifts toward lower wavenumber were 6, 10 and 14 cm−1 for FS-20, FS-40 and FS-60, respectively; the successive 20 percentage-point replacement steps therefore produced shifts of 6, 4 and 4 cm−1. The largest stepwise change occurred between FS and FS-20, while smaller but continuing shifts were observed at the two higher replacement levels. The bands assigned to O–H stretching, H–O–H bending and carbonate stretching remained centered near 3460, 1650 and 1440 cm−1, respectively, without a systematic peak-position displacement at the plotting resolution. In the blended BFS–FA–CSS system, the band can include overlapping contributions from different reaction products and residual precursor. The shift is consistent with a change in the relative contributions or local bonding environments of these components. Together with XRD and MIP, these observations support changes in the composite matrix but do not distinguish C-(A)-S-H from N-A-S-H or identify a unique reaction pathway. The persistence of water- and carbonate-associated bands across the mixtures indicates that these constituent types remained detectable after replacement. Because the spectra were normalized and the principal band contains overlapping contributions, neither band height nor peak position alone was used to quantify gel content or assign a unique change in gel polymerization. The peak shift is thus interpreted alongside the pore and strength changes as evidence of a modified composite matrix.
3.3.4. Thermogravimetric Behavior
Figure 9 presents the TG curves of geopolymer pastes containing different CSS contents. All mixtures exhibited a relatively rapid mass loss below approximately 200 °C, followed by more gradual mass changes at higher temperatures. The low-temperature loss is associated with the release of evaporable water and dehydration of reaction products [8,33,35]. FS exhibited a larger loss in this region than FS-60, suggesting a greater contribution from water-bearing constituents per unit mass of composite. The figure-derived DTG curves in Figure 8b resolve a dominant low-temperature mass-loss event. With the 41-point window, its approximate maxima occurred at 65, 64, 63 and 61 °C for FS, FS-20, FS-40 and FS-60, respectively, with mass-loss rates of approximately 0.23, 0.20, 0.17 and 0.09%/°C. The corresponding maxima remained within approximately 60–65 °C when the smoothing window was changed to 31 or 61 points. These small differences in estimated peak temperature are not interpreted as a systematic shift in decomposition temperature. The decrease in peak mass-loss rate with CSS replacement is consistent with a smaller contribution from water-bearing constituents on the total-composite-mass basis. The overlapping release of evaporable or adsorbed water and dehydration of reaction products cannot be separated into individual gel phases from these DTG curves alone.
Figure 9.
Thermogravimetric behavior of geopolymer pastes containing different CSS contents: (a) normalized TG traces recovered from the original figure; (b) figure-derived DTG curves expressed as -dM/dT (%/°C, calculated using cubic local polynomial fits over 41 points. The shaded interval marks the region affected by the small FS-20 step in the source trace and is not assigned to a specific decomposition process.
Mass retention increased with CSS content over the temperature range examined. This trend is consistent with a lower proportion of water-bearing reaction products and a higher proportion of crystalline CSS in the composite. The more gradual mass changes at higher temperatures may involve continued dehydration, dehydroxylation, and carbonate decomposition [17,35,36]. The separation between the curves developed mainly during the initial rapid mass-loss region, with FS-60 retaining more mass than FS over the subsequent heating range. As retained mass is expressed relative to total sample mass, CSS replacement changes both the proportion of water-bearing constituents and the mass basis for comparison. Smaller composite mass loss is therefore compatible with precursor dilution, but does not independently quantify gel content or demonstrate improved thermal stability of the binding gels. Thus, the TG results are consistent with the dilution-related changes inferred from XRD, MIP, and the strength measurements. Above about 200 °C, the reconstructed derivative is much smaller and shows broad changes rather than a set of clearly separated decomposition peaks. These weak features do not permit unique assignment to particular gels, hydroxides or carbonates. The small drop-and-return step visible in the original FS-20 trace near 715–735 °C produces a local positive/negative derivative feature; the region affected by the 41-point fit is indicated in Figure 9b and is not interpreted as evidence of a specific reaction. Its coordinates were retained without replacing the feature with an assumed decomposition peak.
3.3.5. SEM Observations
Figure 10 shows the microstructures of the geopolymer pastes after 28 days of curing. FS exhibited a comparatively compact matrix, with particles embedded in a relatively continuous binding phase and few visible interfacial gaps (Figure 10a). FS-20 retained a reasonably continuous matrix, although more exposed particles and localized voids were apparent (Figure 10b). At 40% replacement, particle–matrix gaps became more pronounced and the binding phase was less uniformly distributed (Figure 10c). FS-60 exhibited the most open structure, with numerous particles separated by voids and discontinuous regions of binding material (Figure 10d).
Figure 10.
SEM images of 28-day geopolymer pastes: (a) FS, (b) FS-20, (c) FS-40, and (d) FS-60.
The progressive loss of local matrix continuity is consistent with dilution-related changes as CSS replaces BFS and FA, but does not quantify the formation of binding products. In the selected fields, wider particle–matrix gaps and discontinuous binding regions were observed at higher replacement levels; these features do not establish the identity or bulk amount of the surrounding gels. These observations agree with the increased intrudable porosity and larger pore-entry diameters measured by MIP and are consistent with the observed lower compressive strengths. Collectively, the characterization results are consistent with dilution-related changes in matrix development contributing to the mechanical response. The agreement between local SEM observations and the MIP trend supports the interpretation of reduced matrix continuity at higher replacement. However, SEM fields do not quantify the entire specimen, and particle morphology alone cannot identify all residual constituents or determine the amount of surrounding gel. Because these observations used material remaining after compressive testing, visible cracks may also include damage introduced during loading. They cannot by themselves establish the extent of cracking before testing.
3.4. Response to Sulfate Exposure
3.4.1. Strength Evolution
Figure 11 presents the mechanical properties of geopolymer pastes after immersion in sodium sulfate solution. The compressive strength of FS increased from 56.3 MPa after 7 days of exposure to 62.1 MPa after 28 days, before decreasing to 53.3 MPa after 90 days. Between 28 and 90 days, the strength decreased from 48.7 to 44.1 MPa for FS-20, from 37.6 to 36.9 MPa for FS-40, and from 36.8 to 36.5 MPa for FS-60. The corresponding reductions were approximately 14.2%, 9.4%, 1.9%, and 0.8%, respectively. Increasing CSS replacement was therefore associated with smaller strength reductions during the later exposure period, although FS retained the highest absolute compressive strength after 90 days. At 90 days, FS-60 retained approximately 68.5% of the absolute compressive strength of FS, despite its smaller reduction from the 28-day value. The high-replacement mixtures therefore combined lower absolute strength with smaller later changes in the reported means. In particular, the 0.3 MPa change for FS-60 should not be interpreted as a statistically established benefit without an appropriate analysis of variability.
Figure 11.
Mechanical properties of geopolymer pastes after different durations of sodium sulfate immersion.
Flexural strength showed a different evolution, with an early decrease followed by partial recovery in the CSS-containing mixtures. FS decreased from 3.1 MPa after 7 days to 1.2 MPa after 28 days and remained at 1.2 MPa after 90 days. Over the same intervals, FS-20 changed from 4.5 to 1.6 and 1.7 MPa, FS-40 from 3.5 to 1.2 and 1.7 MPa, and FS-60 from 3.3 to 1.6 and 2.0 MPa. Consequently, FS-60 exhibited the highest 90-day flexural strength despite its lower compressive strength. The differing compressive and flexural trends may reflect the different sensitivities of the two loading modes to local defects and cracking. Continued reaction during immersion may contribute to the partial recovery, while comparison with water-immersed specimens is needed to distinguish this contribution from the net effect of sulfate exposure. The early compressive increase followed by a later reduction is compatible with competing continued hardening and exposure-related changes. The sensitivity of flexural strength to localized defects in the tensile region provides a possible interpretation of its evolution; exposure-induced cracking was not measured. However, the strength measurements alone do not identify sulfate reaction products, expansion or a specific deterioration mechanism.
3.4.2. Corrosion Resistance Coefficient
Figure 12 presents the flexural strengths of the water-immersed geopolymer pastes, which were used to calculate the corrosion resistance coefficient, K (Figure 13). After 7 days of immersion, K increased from approximately 0.6 for FS to 1.1, 1.5, and 2.7 for FS-20, FS-40, and FS-60, respectively. At 28 days, the corresponding coefficients were approximately 0.7, 0.5, 0.8, and 1.1. By 90 days, the values had converged to approximately 1.0, 1.0, 1.1, and 1.1. Thus, CSS incorporation altered the early response relative to water immersion, but the differences among mixtures diminished with exposure time. The high early coefficient of FS-60 is strongly influenced by its water-immersed reference strength. At 7 days, its sulfate-immersed and water-immersed flexural strengths were 3.3 and 1.2 MPa, respectively, giving a ratio of approximately 2.75 from the rounded means. This explains the large coefficient without implying a comparable advantage in absolute load-bearing strength. By 90 days, the coefficients were close to unity and their plotted error ranges overlapped. K near unity means that the strengths under the two immersion conditions were similar; it does not demonstrate that the initial strength was retained. These observations indicate limited differentiation among mixtures according to this measure at 90 days.
Figure 12.
Flexural strengths of geopolymer pastes after different durations of distilled-water immersion.
Figure 13.
Corrosion resistance coefficients of geopolymer pastes after different durations of sodium sulfate immersion.
3.5. Response to Chloride Exposure
3.5.1. Water-Extractable Chloride
Figure 14 presents the mean chloride concentrations in aqueous extracts from mortars after 30 and 90 days of NaCl exposure. The smooth curves serve only as visual guides and are not fitted transport models. After 30 days, FS-20, FS-40, and FS-60 showed mean concentrations approximately 9.9%, 26.8%, and 35.55% lower than FS, respectively. After 90 days, the corresponding reductions were approximately 16.0%, 26.9%, and 30.18%. The mean extract concentrations at 90 days were higher than those at 30 days for all mixtures.
Figure 14.
Water-extractable chloride of geopolymer mortars at different CSS replacement levels after 30 and 90 days of NaCl exposure.
These results should be evaluated alongside the internal structural observations. MIP showed that intrudable porosity increased from 5.11% to 12.17% and average pore-entry diameter increased from 14.71 to 29.76 nm as CSS replacement increased from 0% to 60% (Figure 7 and Table 4). SEM also revealed more pronounced particle–matrix gaps and reduced matrix continuity at higher replacement levels (Figure 10). These observations do not support a densification-based explanation for the lower water-extractable chloride.
However, MIP and the corresponding SEM observations characterized 28-day pastes before exposure, whereas chloride extraction was performed on mortars after a separate curing and NaCl-exposure schedule. These measurements therefore do not establish a direct porosity–chloride transport relationship. The extract concentration represents chloride recovered under the adopted procedure, rather than an in situ pore-solution concentration or a direct separation of free and bound chloride. Prior ingress, solid-phase retention or release, and extraction conditions may influence the recovered fraction, but their individual contributions were not measured. The results establish a lower mean chloride-extraction response in the CSS-containing mortars; the underlying cause remains unresolved.
3.5.2. Elemental Distributions
Figure 15 presents the SEM images and elemental maps of FS and FS-40 mortars after 90 days of NaCl exposure. Within the selected fields, Fe was visually more prominent in FS-40, consistent with the incorporation of Fe-rich CSS, whereas Cl was visually more prominent in FS. The local Cl observation is qualitatively consistent with the lower water-extractable chloride measured for FS-40. However, these maps do not quantify bulk elemental concentrations.
Figure 15.
SEM-EDS of geopolymer mortars after 90 days of NaCl exposure: (a) FS and (b) FS-40.
SEM–EDS provides elemental distributions but does not identify the chemical state of chlorine or demonstrate its binding to a particular Fe-bearing phase. The fayalite and magnetite identified by XRD in the cured pastes establish the presence of residual CSS-derived crystalline phases, but do not establish their transformation during subsequent chloride exposure. Consequently, the available characterization does not confirm FeOOH formation, Fe-mediated chloride binding, or altered pore-solution chemistry. An Fe-based mechanism cannot be assigned to the lower water-extractable chloride from these observations
3.6. Discussion and Implications for Binder Design
The combined mechanical and microstructural observations are consistent with less continuous matrix development as CSS replacement increased. Strength decreased as intrudable porosity and pore-entry diameter increased, while SEM revealed more pronounced particle–matrix gaps. The combination of strength loss and pore coarsening is consistent with reduced matrix development as the BFS–FA fraction decreased. The separate contributions of precursor reaction and particle packing were not quantified in the present measurements. The proposed dilution-related explanation is an inference from formulation, strength, pore structure and local morphology; it does not establish the identities or relative amounts of the binding gels, their reaction sequence, or the contribution of CSS dissolution. Moreover, because the activator dosage was fixed relative to the total powder mass, increasing replacement raised the activator dosage relative to the remaining BFS–FA fraction. The observed response thus reflects changes in both reactive precursor availability and effective activation conditions. Xu et al. [4] reported 28-day mortar strengths approximately equivalent to their control at 30 wt.% copper slag replacing GGBS. In the present BFS-FA-CSS series, 60% CSS replacement reduced the 28-day mean mortar compressive strength from 44.7 to 22.3 MPa. The different precursor systems and replacement bases mean that the earlier dosage cannot be treated as an optimum for this formulation. You et al. [32] reported higher fluidity and delayed strength development, together with lower autogenous but higher drying shrinkage. The small descriptive change in mean flowability and the lower strength observed here are partly consistent with that response, but no independent shrinkage measurement establishes the cause of the flexural trend. Zhang et al. [33] previously studied a GGBS-FA-copper-slag ternary binder and reported enhanced early reaction and pore filling. Its reported 3-day strength increase cannot be directly ranked against the present 28-day strength decrease. These comparisons indicate formulation dependence; they do not isolate an intrinsic CSS-reactivity effect from the present measurements.
The sulfate results demonstrate the importance of considering absolute strength together with the corrosion resistance coefficient. Higher CSS contents produced smaller compressive strength reductions between 28 and 90 days of exposure, but did not recover the absolute strength of FS. The convergence of K to approximately 1.0–1.1 further indicates that the large early differences were not maintained. Mass change, expansion, other dimensional changes, sulfate penetration depth and post-exposure phase or microstructural changes were not evaluated in the present sulfate-exposure assessment. The 28-day paste characterization describes the material before sulfate immersion, and SEM-EDS of NaCl-exposed mortars does not provide post-sulfate evidence. Consequently, the smaller late-stage strength decreases at higher CSS contents describe the measured mechanical response under the tested immersion conditions; they do not demonstrate reduced sulfate ingress, suppression of expansive sulfate reactions, or mitigation of sulfate attack. Accordingly, mixture selection should account for load-bearing requirements as well as the response relative to a matched water-immersed reference. Zhang et al. [17] investigated crushed BFS-FA cement particles and reported more severe chemical attack under MgSO4 than Na2SO4, with gypsum formation under MgSO4. This contrasts with the present strength-based evaluation of intact CSS-containing pastes in Na2SO4 and matched water references. The present smaller late-stage compressive-strength change in FS-60 does not establish the sulfate reaction products or MgSO4 resistance. Adediran et al. [19] examined Fe-rich fayalite-slag mortars containing reactive co-binders under combined Na2SO4-NaCl and other environmental conditions. Those combined or cyclic exposures differ from the separate salt immersions used here; the present tests therefore do not establish performance under combined salts, freeze–thaw or wetting-drying cycles.
Considered together, the MIP and SEM results support pore coarsening and reduced matrix continuity in the 28-day pastes as CSS replacement increased. These structural changes are consistent with the decrease in paste compressive strength, but do not explain the lower water-extractable chloride measured in the exposed mortars through matrix densification. The chloride-exposure SEM–EDS maps provide a local qualitative comparison consistent with the extraction results, without identifying a binding phase or mechanism. Because the structural and chloride measurements concern different specimen types and exposure histories, and extraction does not separately quantify ingress and retention, their relationship cannot be interpreted as a direct measure of chloride transport. The present findings therefore demonstrate a formulation-dependent chloride-extraction response. Its cause requires further investigation, and lower extract concentrations should not be interpreted as established improvements in chloride transport resistance or chloride-binding capacity higher paste porosity did not correspond to higher water-extractable chloride in the mortar specimens. Since these measurements concern different material scales and processes, their relationship cannot be reduced to a simple porosity–transport correlation. Chloride ingress, solid-phase retention or release, extractability and pore-solution chemistry are alternative influences on the recovered fraction, and the present measurements do not select a mechanism among them. CSS dosage should therefore be assessed through a combination of mechanical and exposure-specific indicators. The present data identify performance trade-offs rather than a single optimum replacement level; selection for a particular application requires its strength criteria and exposure conditions to be specified. Huang et al. [18] introduced chloride through seawater mixing and investigated the effects of the BFS-FA ratio and binding-phase additions on chloride retention. Those internal-chloride binding results differ from the recovered fraction measured here after external NaCl exposure. The present lower extractable values at higher CSS replacement therefore cannot be interpreted as a measured binding capacity or diffusion coefficient. Tian et al. [37] reported FeOOH formation in metakaolin/Fe-rich-tailings binders using phase-sensitive characterization under marine exposure. The present local Fe/Cl maps do not provide equivalent phase evidence. This comparison motivates further testing of an Fe-related hypothesis while preserving the distinctions between copper smelting slag and Fe-rich tailings and between the exposure and measurement scopes; it does not establish Fe-phase chloride binding or altered pore-solution chemistry in the present mortars.
Building on previous binary [4,32] and ternary [33] copper-slag binders, the present contribution is the coordinated assessment of a defined replacement series: CSS substitutes 0–60% of the BFS-FA blend while the remaining BFS:FA ratio is maintained at 3:2. Within this series, lower compressive strength and a coarser accessible paste pore structure coexist with lower mean water-extractable chloride in the corresponding mortars. Under sulfate exposure, smaller relative decreases in mean compressive strength between 28 and 90 days at higher CSS contents also coexist with lower absolute 90-day strength. These observations provide formulation-specific evidence that the investigated strength, pore-entry and salt-exposure indicators do not support a single universal ranking of CSS dosage. Table 5 places these findings alongside earlier studies while distinguishing material scales, exposure histories and measurement conditions.
Table 5.
Comparison of precursor systems, reported findings and the contribution of the present study. Differences in formulation, specimen type and test schedule preclude direct performance ranking across studies.
For construction-material development, the results support screening candidate CSS-containing binder and mortar formulations against specified mechanical requirements and exposure conditions. The reduction in the amount of BFS and FA must be considered together with the measured compressive-strength penalty and the small descriptive change in mean paste flowability. FS-20 illustrates this balance: replacing 20% of the BFS-FA precursor blend retained approximately 90.6% of the reference mortar’s 28-day mean compressive strength, whereas FS-60 retained approximately 49.9%. The prism strengths are laboratory means and do not establish characteristic concrete strength or qualification of a structural product. Application-specific development requires verification of dimensional stability, production-scale curing and material variability, exposure-specific durability and environmental leaching [2]. Water-extractable chloride alone does not establish reinforcement-corrosion resistance. Although earlier ternary-binder work included environmental and economic assessment [33], the present tests did not quantify life-cycle emissions or production costs; these depend on the actual precursor supply, activator demand and manufacturing route.
4. Conclusions
This study evaluated 0–60% CSS replacement of a BFS-FA blend while maintaining the remaining BFS:FA ratio at 3:2. Its scientific contribution is formulation-specific evidence that compressive-strength loss and paste pore-entry coarsening can coexist with lower water-extractable chloride in the corresponding mortars. The sulfate results also show the need to consider relative compressive-strength changes alongside absolute residual strength. These observations support evaluating CSS-containing building-material binders through mechanical requirements and exposure-specific indicators together, with their material scales and measurement definitions distinguished. The following conclusions can be drawn
1. Under the investigated conditions, mean paste flowability changed from 189.20 to 198.35 mm as CSS replacement increased from 0% to 60%, a numerical difference of approximately 4.8%. With only two determinations per mixture and no inferential significance test, this small difference does not support a claim of statistically significant improvement in flowability. Over the same range, the mean 28-day paste and mortar compressive strengths decreased by 47.7% and 50.1%, respectively.
2. Intrudable porosity increased from 5.11% to 12.17%, and the average pore-entry diameter increased from 14.71 to 29.76 nm. Across the four mixture means, an exploratory linear fit between 28-day paste compressive strength and intrudable porosity gave R2 = 0.967 (n = 4); this association is limited to the tested formulations and is not interpreted as an independent causal effect of porosity. The residual CSS-derived crystalline phases and less continuous matrix observed by SEM were consistent with dilution-related changes in matrix development. The characterization results did not independently quantify the reaction degree or binding-product content. Individual gel identities and the proposed reaction pathway were not independently established.
3. Between 28 and 90 days of sulfate exposure, the mean compressive strength decreased by approximately 14.2% for FS and 0.8% for FS-60. FS retained the highest absolute 90-day compressive strength. The standard flexural-strength-based K values were approximately 1.0–1.1 at 90 days, indicating similar flexural strengths relative to the matched water-immersed references under the tested conditions. The smaller compressive-strength decrease at higher CSS contents describes only the measured mechanical response; it does not establish improved overall sulfate resistance or mitigation of sulfate attack.
4. The CSS-containing mortars showed lower mean water-extractable chloride concentrations than FS after both 30 and 90 days of NaCl exposure. These concentrations represent chloride recovered under the adopted extraction procedure. Their coexistence with pore coarsening in separately characterized pastes does not establish a direct porosity–transport relationship. The underlying cause remains unresolved, and the results do not demonstrate improved chloride transport resistance, Fe-mediated chloride binding, FeOOH formation, or altered pore-solution chemistry.
5. These results support preliminary selection of CSS-containing binder and mortar formulations against specified strength and exposure requirements. FS-20 retained approximately 90.6% of the reference mortar’s 28-day mean compressive strength, whereas FS-60 retained approximately 49.9%, illustrating the balance between precursor substitution and strength. The present evidence can inform mixture screening and the planning of laboratory trials for mortar-based products. The reported prism means require application-specific strength and durability verification before use in building components. The present results do not establish a universally optimum CSS dosage.
Further work should characterize pore structure and depth-resolved total and water-extractable chloride in mortars under matched curing and exposure conditions. Paired chloride fractions should be complemented by controlled binding and release experiments, because their difference alone does not quantify chemical binding. Measurements of pore-solution chloride, pH, and composition would help evaluate chloride partitioning. Phase-specific characterization of Fe-bearing constituents, together with suitable binder and Fe-phase controls, could be used to test any proposed Fe contribution without presupposing its role. Quantitative XRD with an internal standard could constrain crystalline and amorphous fractions, while solid-state 29Si and 27Al NMR with complementary characterization would help resolve gel structural environments and test the proposed reaction interpretation. Direct shrinkage and cracking measurements, together with variation in activator dosage relative to the remaining BFS-FA fraction, would help separate dimensional and activation effects. Further sulfate-exposure assessment should combine strength measurements with mass change, expansion and dimensional-stability measurements, sulfate penetration profiles and post-exposure phase and microstructure characterization. Longer separate-salt exposures, combined-salt conditions and application-relevant cyclic environments would also be needed for broader durability assessment. Product-scale trials should assess material variability, curing, strength and durability together with leaching, production costs and life-cycle impacts for the actual manufacturing route.
Author Contributions
Conceptualization, X.T.; methodology, Q.L.; validation, Z.T.; formal analysis, Z.T.; investigation, Q.L.; resources, Q.L.; data curation, Z.T.; writing—original draft, Q.L.; writing—review and editing, X.T.; visualization, Z.T.; supervision, X.T.; project administration, X.T. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by Open Fund of Key Laboratory of Safety Control of Bridge Engineering, Ministry of Education (Changsha University of Science & Technology) grant number 22KB03.
Data Availability Statement
The data presented in this study are available on request from the corresponding author due to participant consent restrictions that limit data sharing to the original study team.
Conflicts of Interest
The authors declare no conflict of interest.
References
- Klaffenbach, E.; Montenegro, V.; Guo, M.; Blanpain, B. Sustainable and Comprehensive Utilization of Copper Slag: A Review and Critical Analysis. J. Sustain. Metall. 2023, 9, 468–496. [Google Scholar] [CrossRef] [Scilit]
- Kurniati, E.O.; Pederson, F.; Kim, H.-J. Application of steel slags, ferronickel slags, and copper mining waste as construction materials: A review. Resour. Conserv. Recycl. 2023, 198, 107175. [Google Scholar] [CrossRef] [Scilit]
- Zhou, H.; Basarir, H.; Poulet, T.; Li, W.; Kleiv, R.A.; Karrech, A. Life cycle assessment of recycling copper slags as cement replacement material in mine backfill. Resour. Conserv. Recycl. 2024, 205, 107591. [Google Scholar] [CrossRef] [Scilit]
- Xu, R.; Wang, H.; Yang, R.; Kong, F.; Hong, T. The potential of copper slag as a precursor for partially substituting blast furnace slag to prepare alkali-activated materials. J. Clean. Prod. 2024, 434, 140283. [Google Scholar] [CrossRef] [Scilit]
- Hu, J.; Luo, Z.; He, H.; Xue, Y. Measurement of the dynamic elastic modulus of concrete pavements in situ based on impact echo measurements corrected via elastic wave theory. Transp. Saf. Environ. 2026, 8, tdag032. [Google Scholar] [CrossRef] [Scilit]
- Sun, B.; Ye, G.; de Schutter, G. A review: Reaction mechanism and strength of slag and fly ash-based alkali-activated materials. Constr. Build. Mater. 2022, 326, 126843. [Google Scholar] [CrossRef] [Scilit]
- Adediran, A.; Yliniemi, J.; Moukannaa, S.; Ramteke, D.D.; Perumal, P.; Illikainen, M. Enhancing the thermal stability of alkali-activated Fe-rich fayalite slag-based mortars by incorporating ladle and blast furnace slags: Physical, mechanical and structural changes. Cem. Concr. Res. 2023, 166, 107098. [Google Scholar] [CrossRef] [Scilit]
- Adediran, A.; Yliniemi, J.; Lemougna, P.N.; Perumal, P.; Illikainen, M. Recycling high volume Fe-rich fayalite slag in blended alkali-activated materials: Effect of ladle and blast furnace slags on the fresh and hardened state properties. J. Build. Eng. 2023, 63, 105436. [Google Scholar] [CrossRef] [Scilit]
- Du, J.; Liu, Z.; Christodoulatos, C.; Conway, M.; Bao, Y.; Meng, W. Utilization of off-specification fly ash in preparing ultra-high-performance concrete (UHPC): Mixture design, characterization, and life-cycle assessment. Resour. Conserv. Recycl. 2022, 180, 106136. [Google Scholar] [CrossRef] [Scilit]
- Lao, J.-C.; Huang, B.-T.; Fang, Y.; Xu, L.-Y.; Dai, J.-G.; Shah, S.P. Strain-hardening alkali-activated fly ash/slag composites with ultra-high compressive strength and ultra-high tensile ductility. Cem. Concr. Res. 2023, 165, 107075. [Google Scholar] [CrossRef] [Scilit]
- Zhang, Z.; Xiong, J.; Zhao, Z.; Wang, F.; Zeng, Y.; Zhao, B.; Ke, L. An approach of dynamic response analysis of nonlinear structures based on least square Volterra kernel function identification. Transp. Saf. Environ. 2023, 5, tdac046. [Google Scholar] [CrossRef] [Scilit]
- Singh, R.P.; Vanapalli, K.R.; Cheela, V.R.S.; Peddireddy, S.R.; Sharma, H.B.; Mohanty, B. Fly ash, GGBS, and silica fume based geopolymer concrete with recycled aggregates: Properties and environmental impacts. Constr. Build. Mater. 2023, 378, 131168. [Google Scholar] [CrossRef] [Scilit]
- Yang, Y.; Zou, Z.; Liu, C.; Wang, Y.; Jiang, Z.; Cui, Q. Bi-level optimization of carbon emission pricing for urban road traffic and environmental impacts. Transp. Saf. Environ. 2026, 8, tdag009. [Google Scholar] [CrossRef] [Scilit]
- Zhang, P.; Han, X.; Hu, S.; Wang, J.; Wang, T. High-temperature behavior of polyvinyl alcohol fiber-reinforced metakaolin/fly ash-based geopolymer mortar. Compos. Part B Eng. 2022, 244, 110171. [Google Scholar] [CrossRef] [Scilit]
- Lao, J.-C.; Ma, R.-Y.; Xu, L.-Y.; Li, Y.; Shen, Y.-N.; Yao, J.; Wang, Y.-S.; Xie, T.-Y.; Huang, B.-T. Fly ash-dominated High-Strength Engineered/Strain-Hardening Geopolymer Composites (HS-EGC/SHGC): Influence of alkalinity and environmental assessment. J. Clean. Prod. 2024, 447, 141182. [Google Scholar] [CrossRef] [Scilit]
- Luo, Y.; Li, S.H.; Klima, K.M.; Brouwers, H.J.H.; Yu, Q. Degradation mechanism of hybrid fly ash/slag based geopolymers exposed to elevated temperatures. Cem. Concr. Res. 2022, 151, 106649. [Google Scholar] [CrossRef] [Scilit]
- Zhang, J.; Shi, C.; Zhang, Z.; Hu, X. Reaction mechanism of sulfate attack on alkali-activated slag/fly ash cements. Constr. Build. Mater. 2022, 318, 126052. [Google Scholar] [CrossRef] [Scilit]
- Huang, Z.; Guo, M.; Zhou, Y.; Wang, T.; Fang, Y.; Sui, L.; Gong, G. Chloride binding mechanism and free chloride reduction method of alkali-activated slag/fly ash mixed with seawater. Constr. Build. Mater. 2023, 409, 134079. [Google Scholar] [CrossRef] [Scilit]
- Adediran, A.; Yliniemi, J.; Carvelli, V.; Adesanya, E.; Illikainen, M. Durability of alkali-activated Fe-rich fayalite slag-based mortars subjected to different environmental conditions. Cem. Concr. Res. 2022, 162, 106984. [Google Scholar] [CrossRef] [Scilit]
- Thommes, M.; Kaneko, K.; Neimark, A.V.; Olivier, J.P.; Rodriguez-Reinoso, F.; Rouquerol, J.; Sing, K.S.W. Physisorption of gases, with special reference to the evaluation of surface area and pore size distribution (IUPAC Technical Report). Pure Appl. Chem. 2015, 87, 1051–1069. [Google Scholar] [CrossRef] [Scilit]
- Ou, Z.; Feng, R.; Li, F.; Liu, G.; Li, N. Development of drying shrinkage model for alkali-activated slag concrete. Constr. Build. Mater. 2022, 323, 126556. [Google Scholar] [CrossRef] [Scilit]
- Kong, Y.K.; Kurumisawa, K. Prediction of the drying shrinkage of alkali-activated materials using artificial neural networks. Case Stud. Constr. Mater. 2022, 17, e01166. [Google Scholar] [CrossRef] [Scilit]
- Amran, M.; Onaizi, A.M.; Makul, N.; Abdelgader, H.S.; Tang, W.C.; Alsulami, B.T.; Alluqmani, A.E.; Gamil, Y. Shrinkage mitigation in alkali-activated composites: A comprehensive insight into the potential applications for sustainable construction. Results Eng. 2023, 20, 101452. [Google Scholar] [CrossRef] [Scilit]
- Zhang, B.; Zhu, H.; Cheng, Y.; Huseien, G.F.; Shah, K.W. Shrinkage mechanisms and shrinkage-mitigating strategies of alkali-activated slag composites: A critical review. Constr. Build. Mater. 2022, 318, 125993. [Google Scholar] [CrossRef] [Scilit]
- Xu, Y.; Li, J.; Han, Y.; Gao, P.; Liu, S.; Chu, Y.; Zhan, B.; Yu, Q. Effect of coarse aggregates’ spatial distribution on drying-induced shrinkage of concrete: A combined study of digital image correlation and lattice modelling. J. Build. Eng. 2026, 119, 115143. [Google Scholar] [CrossRef] [Scilit]
- Zhang, B.; Zhu, H.; Feng, P.; Zhang, P. A review on shrinkage-reducing methods and mechanisms of alkali-activated/geopolymer systems: Effects of chemical additives. J. Build. Eng. 2022, 49, 104056. [Google Scholar] [CrossRef] [Scilit]
- Kucharczyková, B.; Nápravník, P.; Kocáb, D.; Lisztwan, D.; Rovnaník, P.; Hajzler, J.; Bílek, V. Comprehensive study of moist curing duration and activator type on mechanical properties, shrinkage, and cracking of alkali-activated slag. Constr. Build. Mater. 2024, 416, 135199. [Google Scholar] [CrossRef] [Scilit]
- Liu, L.; Xu, Y.; Liu, H.; Xie, M.; He, Y.; Shi, C. Drying shrinkage and microstructure of alkali-activated slag with different mixing time at low temperatures (−5 to 5 °C). Constr. Build. Mater. 2022, 360, 129529. [Google Scholar] [CrossRef] [Scilit]
- Liu, B.; Lin, W.; Guo, J.; Zhang, Y.; Wang, Y.; Ming, Y. Autogenous and drying shrinkage characteristics of waste marble powder-slag based alkali-activated concrete. J. Build. Eng. 2025, 110, 112992. [Google Scholar] [CrossRef] [Scilit]
- Maruyama, I.; Sugimoto, H.; Umeki, S.; Kurihara, R. Effect of fineness of cement on drying shrinkage. Cem. Concr. Res. 2022, 161, 106961. [Google Scholar] [CrossRef] [Scilit]
- Mobili, A.; Blasi, E.; Maqbool, Q.; Tittarelli, F. Copper mine tailings and metakaolin as precursors for sustainable alkali-activated mortars. J. Build. Eng. 2025, 103, 112134. [Google Scholar] [CrossRef] [Scilit]
- You, N.; Chen, Z.; Gao, Z.; Song, X. The effect of copper slag as a precursor on the mechanical properties, shrinkage and pore structure of alkali-activated slag-copper slag mortar. J. Build. Eng. 2024, 98, 111151. [Google Scholar] [CrossRef] [Scilit]
- Zhang, T.; Xu, R.; Tu, S.; Qian, Z.; Shi, T.; Zhang, K.; Zhang, G. Recycling copper slag as precursor in alkali-activated materials: Reaction mechanisms, microstructural features, and environment impact. Constr. Build. Mater. 2025, 492, 142886. [Google Scholar] [CrossRef] [Scilit]
- Luo, Y.; Brouwers, H.J.H.; Yu, Q. Understanding the gel compatibility and thermal behavior of alkali activated Class F fly ash/ladle slag: The underlying role of Ca availability. Cem. Concr. Res. 2023, 170, 107198. [Google Scholar] [CrossRef] [Scilit]
- Tu, W.; Zhang, M. Behaviour of alkali-activated concrete at elevated temperatures: A critical review. Cem. Concr. Compos. 2023, 138, 104961. [Google Scholar] [CrossRef] [Scilit]
- Zhang, L.; Ma, Y.; Ouyang, X.; Fu, J.; Li, Z. Effect of CaO on the shrinkage and microstructure of alkali-activated slag/fly ash microsphere. Constr. Build. Mater. 2024, 421, 135672. [Google Scholar] [CrossRef] [Scilit]
- Tian, X.; Chen, Z.; Wu, J.; Lv, X.; Liu, H.; Hu, S.; Gao, C.; Jiang, T.; Wang, L. Strength enhancement and resistance to chloride ions penetration mechanisms of metakaolin/Fe-rich tailings hybrid geopolymers with equivalent flowability in accelerated marine environments. Constr. Build. Mater. 2025, 493, 143273. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.