Abstract
Basalt fiber-reinforced polymer (BFRP) offers the advantages of high strength, excellent corrosion resistance, and low weight, providing a promising material solution to the durability problems associated with conventional steel anti-floating anchors. However, a systematic understanding of the interfacial bonding behavior, load-transfer mechanisms, and long-term evolution of BFRP anti-floating anchors remains lacking. Focusing on the interfacial bonding and load-transfer mechanisms of BFRP anti-floating anchors, this review systematically summarizes their structural configurations and the dual-interface system consisting of the BFRP anchor rod-anchorage body interface and the anchorage body-rock and soil mass interface. Particular emphasis is placed on the bonding mechanisms and typical failure modes of these two interfaces. The axial-force distribution along the BFRP anchor rod, interfacial shear-stress distribution, critical anchorage length, and their major influencing factors are also analyzed. Furthermore, the load-transfer and deformation characteristics under monotonic, cyclic, and sustained loading conditions are comparatively discussed. Existing studies indicate that load transfer in BFRP anti-floating anchors is markedly nonuniform and progressive. The axial force gradually decreases from the loading end toward the deeper anchorage zone, while the interfacial shear stress is concentrated within a limited load-transfer zone. With the progressive development of local slip and interfacial damage, the peak shear stress and effective load-transfer zone gradually migrate toward greater anchorage depths. The load-bearing capacity and failure mode are jointly governed by the mechanical properties of the BFRP anchor rod, the relative stiffness and strength of the two interfaces, the properties of the anchorage body, the confinement provided by the rock and soil mass, and construction quality. Cyclic and sustained loading further induce the accumulation of residual deformation, stiffness degradation, and stress redistribution. Future research should focus on long-term constitutive models and reliability-based design methods that account for coupled damage at the dual interfaces and environmental load-coupling effects.
1. Introduction
With increasing high-density urban development and the continuous extension of building functions into underground space, the burial depths of high-rise buildings, large public buildings, urban complexes, and other engineering structures have continued to increase. Meanwhile, the construction scale of underground structures, including underground stations, underground commercial spaces, and utility tunnels, has also expanded substantially [1]. In areas with high groundwater levels, groundwater buoyancy has become an important factor governing the construction safety, serviceability, and long-term reliability of underground building structures [2,3]. When the self-weight of an underground structure and the permanent loads acting above it are insufficient to resist groundwater buoyancy, problems such as base-slab heave, overall structural uplift, cracking of structural components, and damage to waterproofing systems may occur. These problems not only impair the load-bearing performance and durability of underground structures, but may also lead to basement leakage, damage to equipment and pipelines, and restrictions on the normal use of buildings [4]. Therefore, the rational control of groundwater buoyancy and the assurance of anti-floating safety have become important considerations in the design of deeply embedded building foundations and underground structures. Existing anti-floating measures for underground structures mainly include increasing structural self-weight, installing uplift piles, using anti-floating anchors, and adopting drainage and pressure-relief systems [5]. Among these measures, anti-floating anchors are characterized by flexible arrangement, high adaptability to construction conditions, efficient material utilization, and limited impacts on the clear space and functional use of underground structures. They are particularly suitable for the anti-floating design of basement slabs, raft foundations, and other large-area underground structures and have become a commonly used anti-floating technique in building and geotechnical engineering [6].
Conventional anti-floating anchors generally use steel bars or steel strands as tensile members. However, because anchors are embedded for long periods in groundwater and rock and soil mass, steel is susceptible to corrosion under the combined effects of moisture, chlorides, sulfates, stray currents, and other aggressive factors [7]. Therefore, for anti-floating projects with long design service lives and exposure to aggressive groundwater environments, the durability of conventional steel anchors has become an issue that cannot be neglected. Fiber-reinforced polymer (FRP), characterized by low weight, high strength, and excellent corrosion resistance, provides an alternative material for overcoming the durability limitations of conventional metallic anchors [8,9]. In recent years, considerable progress has been made in the application of glass fiber-reinforced polymer (GFRP) anchors to structural anti-floating engineering, demonstrating the feasibility of FRP materials in geotechnical anchorage applications. Nevertheless, the bond strength of GFRP may deteriorate to a certain extent in alkaline environments, which limits its applicability in some special engineering conditions [10]. Several researchers have further investigated the effects of concrete strength, fiber volume fraction, anchorage length, and manufacturing processes on the bond performance between FRP bars and 3D-printed concrete [11]. Regarding durability, Zhou et al. [12] found that the tensile strength of FRP bars decreased by approximately 70% after exposure to an alkaline solution at 40 °C. The elevated temperature accelerated the aging of the bar material, thereby leading to a significant reduction in its tensile strength.
Basalt fiber-reinforced polymer (BFRP) is a composite material consisting of continuous basalt fibers embedded in a polymer resin matrix. Compared with steel, BFRP offers several advantages, including low density, high tensile strength, and resistance to electrochemical corrosion [13]. It therefore has considerable potential for application in anti-floating engineering where anchors are subjected to long-term exposure to groundwater and aggressive rock and soil environments. However, the corrosion resistance of BFRP does not imply that its mechanical and interfacial properties remain unchanged in the face of long-term environmental exposure. As a fiber-reinforced polymer composite, its long-term durability depends not only on the basalt fibers themselves, but also on the stability of the polymer resin matrix, the fiber-matrix interface, and the surface structure of the BFRP anchor rod [14,15]. Dong et al. [16] investigated the long-term bond durability between FRP bars and cementitious materials under environmental exposure conditions. Zeng et al. [17] studied the bond performance between FRP bars and seawater–sea-sand concrete and found that larger rod diameters and longer anchorage lengths could improve the bond performance. Hussain et al. [18] conducted tests in alkaline and seawater environments and reported that the bond-strength retention ratios of BFRP bars were approximately 86% and 82%, respectively. These results indicate that, although BFRP exhibits good resistance to aggressive environments, its interfacial bond performance may still undergo a certain degree of degradation after long-term exposure.
Furthermore, BFRP anti-floating anchors are subjected to sustained uplift loads induced by groundwater over their service life; therefore, environmental degradation generally does not occur independently, but interacts with sustained tensile loading. Sustained loading can induce time-dependent deformation of the BFRP anchor rod, continuous interfacial slip, and stress redistribution, while environmentally induced degradation of the material and interface may further alter the long-term load-transfer path. Therefore, the combined effects of alkaline environments, saline media, temperature, and sustained loading should be given particular consideration when evaluating the long-term service performance of BFRP anti-floating anchors.
The load-bearing performance of anti-floating anchors is a key factor governing the anti-floating safety of underground structures. Accordingly, extensive studies have been conducted worldwide on the mechanical behavior of BFRP anti-floating anchors, with particular emphasis on interfacial bonding behavior and load-transfer mechanisms. Wang et al. [19] investigated the bonding performance between BFRP bars and concrete using three different surface-treatment schemes for the BFRP bars. The effects of effective bond length and the distributions of strain and stress along the interface were analyzed, and an analytical bond stress–slip model was established through data fitting. Shen et al. [20] investigated the bonding behavior of BFRP-reinforced concrete members with different strain rates. Based on bond-performance tests conducted at various strain rates, they demonstrated that the bond strength of BFRP-reinforced concrete members increased with increasing strain rate, whereas the corresponding slip decreased, and further proposed a slip model incorporating the strain-rate effect. Yang et al. [21] employed an improved numerical model to investigate the effects of BFRP bar diameter, corrosion duration, and concrete strength on slip behavior. Their results showed that, with increasing corrosion duration and bar diameter, the maximum bond stress and the corresponding slip gradually decreased, while the frictional resistance between the BFRP bar and concrete declined sharply. Bai et al. [22] further investigated the load-bearing performance, interfacial interaction, and load-transfer process of BFRP anti-floating anchors through a combination of field tests and numerical simulations. They found that, as the applied load increased, the load was progressively transferred toward the deeper anchorage zone rather than being uniformly distributed over the entire anchorage length. These findings indicate that both the interfacial bonding behavior and the internal load-transfer path of BFRP anti-floating anchors evolve during loading and may be further influenced by time-dependent effects. The low elastic modulus and long-term interfacial performance of BFRP anchors require further investigation.
Although these studies have provided a preliminary understanding of the interfacial bonding behavior and load-transfer mechanisms of BFRP anti-floating anchors, the existing findings still require systematic synthesis and further in-depth investigation. On the one hand, a large proportion of current interface-related studies are based on BFRP bar-concrete specimens, whose dimensions, confinement conditions, and loading boundaries differ substantially from those of actual anti-floating anchors. Consequently, the corresponding conclusions and constitutive models cannot be directly applied to engineering analysis of BFRP anti-floating anchors. On the other hand, most existing studies have focused on a single BFRP anchor rod-anchorage body interface or on short-term monotonic pull-out loading, whereas the coordinated mechanical response of the BFRP anchor rod-anchorage body interface and the anchorage body-rock and soil mass interface, load redistribution following local debonding, and time-dependent degradation under cyclic and sustained loading remain insufficiently understood.
Therefore, based on existing studies concerning the interfacial bonding behavior and load-transfer mechanisms of BFRP anti-floating anchors, this review first introduces the system composition and structural configurations of BFRP anti-floating anchors, as well as their fundamental differences from GFRP and steel anchors, and defines the dual-interface system consisting of the BFRP anchor rod–anchorage body interface and the anchorage body-rock and soil mass interface. The bonding mechanisms, typical failure modes, and interfacial bond-slip models associated with the two interfaces are then comprehensively summarized. The load-transfer path, axial-force distribution along the BFRP anchor rod, and interfacial shear-stress distribution are further systematically analyzed. In addition, the load-bearing and load-transfer characteristics of BFRP anti-floating anchors under monotonic, cyclic, and sustained loading conditions are comparatively discussed. This review is intended to provide a scientific basis for the theoretical development, design optimization, and broader engineering application of BFRP anti-floating anchor systems.
2. System Composition and Interfacial Characteristics of BFRP Anti-Floating Anchors
2.1. Composition and Structural Configurations of BFRP Anti-Floating Anchors
BFRP anti-floating anchors are mainly composed of an anchor head and bearing components, a BFRP anchor rod, an anchorage body, the surrounding rock and soil mass, and necessary positioning components, as illustrated in Figure 1. The anchor head and bearing components connect the anchor to the underground structure and transfer the concentrated uplift load to the BFRP anchor rod. As the primary tensile member, the BFRP anchor rod generally adopts surface configurations such as spiral wrapping, indentations, ribs, or full-thread profiles to enhance interfacial bonding and carries the axial tensile force transmitted from the structure [23]. The anchorage body fills the borehole, encapsulates the BFRP anchor rod, and distributes the load transferred from the rod, while simultaneously providing radial confinement to the rod. The surrounding rock and soil mass provides uplift resistance through interfacial friction and cohesive resistance.
Figure 1.
Schematic Diagram of a BFRP Anti-Floatation Anchor.
According to the bonding condition between the BFRP anchor rod and the anchorage body along the longitudinal direction, BFRP anti-floating anchors can be classified into fully bonded and partially bonded types. As shown in Figure 2a, in a fully bonded anchor, the BFRP anchor rod is completely surrounded by the anchorage body along the entire borehole length, and the load carried by the BFRP anchor rod is progressively transferred to the anchorage body and the rock and soil mass along the anchorage length. This configuration is currently one of the most commonly adopted forms in field tests of BFRP anti-floating anchors. Fully bonded anchors are suitable for non-prestressed anti-floating systems or systems dominated by passive load resistance; however, their deformation and internal force distributions under service loads are closely related to the stress state of the entire bonded section. As shown in Figure 2b, the partially bonded type consists of an upper free section and a lower anchorage section. Sleeves or similar isolation devices are generally installed within the free section to prevent bonding between the BFRP anchor rod and the surrounding anchorage body, thereby allowing the BFRP anchor rod to undergo axial elongation within this section. In the anchorage section, the load carried by the BFRP anchor rod is transferred through the anchorage body to the deeper stable stratum. This structural configuration is conducive to the application of prestress, adjustment of the initial stress state of the anchor, and control of underground structural deformation, but imposes relatively high requirements on the reliability of free-section isolation, grouting in the anchorage section, and end connections. Dai et al. [24] designed four different BFRP anchorage systems and investigated the effects of different design parameters on the ultimate load-bearing capacity of the anchorage systems through tensile tests. The results showed that the anchorage efficiency coefficient of the wedge anchorage system was less than 90%; the maximum anchorage efficiency coefficient of the BFRP anti-floating anchor fixed in a steel tube reached 97.7%; after grooving the steel strands, removing rust from and drying the connectors, and extending the injection time, the anchorage system achieved the highest ultimate load-bearing capacity, with an anchorage efficiency coefficient of 98.5%.
Figure 2.
Schematic diagrams of different bonding configurations of anti-floating anchors: (a) fully bonded type; (b) partially bonded type.
2.2. Dual-Interface System of BFRP Anti-Floating Anchors
Because field-test data directly addressing the dual interfaces of BFRP anchor rods remain relatively limited, the following discussion first draws on field tests of GFRP anti-floating anchor rods to examine the dual-interface load transfer characteristics of fully bonded FRP anti-floating anchor rods. It should be noted that GFRP and BFRP differ in elastic modulus, surface configuration, and interfacial properties. Therefore, the relevant results are used primarily to identify the fundamental physical processes governing dual-interface load transfer, while the associated quantitative results are not directly extrapolated to BFRP anchor rods.
BFRP anti-floating anchors primarily involve two bonding interfaces, as shown in Figure 3. The first interface is the BFRP anchor rod-anchorage body interface, which is responsible for transferring the axial tensile force along the BFRP anchor rod to the anchorage body. The second interface is the anchorage body-rock and soil mass interface, through which the load carried by the anchorage body is further transferred to the surrounding rock and soil mass. Bai et al. [25] investigated the bonding characteristics of the BFRP anchor rod-anchorage body interface and the anchorage body-rock and soil mass interface through destructive field pull-out tests. The results showed that the axial stress at the anchorage body-rock and soil mass interface reached its maximum near the borehole opening and decreased with increasing depth, whereas the interfacial shear stress first increased and then decreased. The BFRP anchor rod-anchorage body interface and the anchorage body-rock and soil mass interface act synergistically in load transfer and therefore cannot be simplified as a single bonding interface.
Figure 3.
Schematic diagram of the dual-interface system of BFRP anti-floating anchors.
The first interface directly transfers shear forces between the BFRP anchor rod and the anchorage body, and its performance is primarily influenced by the surface configuration and diameter of the BFRP anchor rod, anchorage length, and anchorage body strength. During loading, the axial force in the BFRP anchor rod is progressively transferred to the anchorage body through interfacial adhesion, friction, and mechanical interlocking. When the local shear stress reaches the interfacial strength, surface slip, rib shearing, or local cracking of the anchorage body may occur. Field tests conducted by Sun et al. [26] showed that, with increasing load, the dominant load-transfer mechanism at the BFRP anchor rod-anchorage body interface gradually shifted from interfacial friction and chemical bonding to mechanical interlocking. Subsequently, damage occurred in the anchorage body near the loading end and progressively propagated toward greater depths until failure of the anchorage system.
The second interface governs load transfer from the anchorage body to the surrounding rock and soil mass, and its load-bearing capacity is mainly derived from cohesion, friction, mechanical interlocking induced by borehole-wall roughness, and confining pressure. The mechanical performance of this interface is significantly affected by the strength of the rock and soil mass, the diameter of the anchorage body, and construction quality. Bai et al. [27] investigated the anchorage body-rock mass interface of anti-floating anchors through field tests and found that both the axial stress and interfacial shear stress exhibited pronounced non-uniform distributions along the anchorage depth, with a limited region near the loading end serving as the principal load-transfer zone of the second interface. Grindheim et al. [28], based on full-scale pull-out tests conducted at a limestone site, reported that failure at both the BFRP anchor rod-anchorage body interface and the anchorage body-rock mass interface constituted major failure modes. The failure location may shift depending on the BFRP anchor rod configuration, anchoring material, and rock mass conditions. The bond strength of the BFRP anchor rod-anchorage body interface was approximately 20% of the uniaxial compressive strength of the anchorage body, whereas that of the anchorage body-rock and soil mass interface was approximately 5%. The relative strengths of the two interfaces determine the failure location of the anchor. When the first interface is weaker, the BFRP anchor rod may slip relative to the anchorage body. When the second interface is weaker, the BFRP anchor rod and anchorage body may be pulled out together as an integral unit relative to the surrounding rock and soil mass. When the load-bearing capacities of the two interfaces are comparable, mixed failure involving debonding at the first interface, cracking of the anchorage body, and slip at the second interface may develop simultaneously.
The two interfaces of a BFRP anchor rod are not independent of each other; instead, they form a coupled load-transfer system through the axial force transmission and deformation compatibility of the anchorage body. Let the axial forces in the bar and the anchorage body be denoted by Nb(x) and Ng(x), respectively. The shear stresses at the bar-anchorage body interface and the anchorage body-rock and soil mass interface are denoted by τ1(x) and τ2(x), respectively, while the diameters of the bar and the anchorage body are denoted by (d) and (D), respectively. For an infinitesimal segment with a length of (dx), the following relationships can be obtained from axial force equilibrium:
It can thus be seen that the first interface governs the transfer of axial force from the bar to the anchorage body, whereas the second interface controls the transfer of axial force from the anchorage body to the surrounding rock and soil mass. Therefore, the anchorage body serves as an intermediate load-transfer medium between the two interfaces. As shown in Figure 4, when the tangent stiffness of the first interface near the loaded end decreases or local debonding occurs, the interfacial shear stress in this region gradually decreases from its peak value to the softening or residual level. According to the local equilibrium relationship of the bar, a reduction in the shear stress at the first interface results in a lower rate of axial-force decay along the anchorage depth. Consequently, a greater proportion of the axial force is retained and transferred to the deeper intact bonded zone. As a direct consequence, the peak shear stress and the effective load-transfer zone of the first interface migrate toward greater depths. Meanwhile, the location at which the anchorage body receives load from the bar also shifts downward, causing the mobilized region of the second interface to extend deeper. Therefore, the interfacial coupling induced by degradation of the first interface does not simply manifest as an increase in the shallow shear stress at the second interface; rather, it is primarily characterized by a redistribution of the load-transfer path of the entire dual-interface system toward deeper anchorage regions.
Figure 4.
Schematic diagram of dual-interface load transfer in a BFRP anchor rod.
When stiffness degradation or local debonding first occurs at the second interface, the ability of the shallow anchorage body to transfer axial force to the surrounding rock and soil mass is reduced. Under this condition, the axial force in the anchorage body cannot decay rapidly within the original short transfer zone, but instead remains at a relatively high level and is transmitted over a greater depth, accompanied by increased displacement of the shallow anchorage body. Because deformation compatibility must be satisfied among the bar, anchorage body, and rock and soil mass, changes in the displacement of the anchorage body further alter the relative slip and shear-stress distribution at the first interface, leading to a readjustment of its effective load-transfer range and peak-stress position. Therefore, degradation of the second interface can likewise feed back to the first interface through the axial deformation of the anchorage body and promote further load sharing by the remaining intact anchorage length.
At present, numerous analytical models have also been applied to investigate the interfacial bonding behavior of anti-floating anchors. Wang et al. [19], considering bond failure between the anchorage body and concrete, established a three-dimensional anchorage-system model incorporating interfacial bond failure and demonstrated that the relative stiffness, peak strength, and post-peak softening characteristics of the two interfaces jointly govern the overall load-displacement response and failure evolution process. Ren et al. [29] proposed a trilinear bond-slip model that accounts for the residual bond strength at the anchor rod-anchorage body interface and investigated the mechanical behavior and debonding process of grouted anti-floating anchors under different loading conditions. The deformation process of anti-floating anchors was divided into five stages: the elastic stage, elastic-softening stage, elastic-softening-debonding stage, softening-debonding stage, and debonding stage.
It should be noted that direct evidence from full-scale tests, field monitoring, and long-term performance investigations specifically conducted on BFRP anchor rods remains relatively limited. Therefore, the evidence reviewed in this study is classified into three categories according to its relevance to BFRP anchor rods. The first category includes field tests, full-scale tests, and laboratory anchorage tests directly conducted on BFRP anchor rods, which can be regarded as direct evidence for analyzing their bearing capacity and load transfer characteristics. The second category consists of studies on the interface behavior between BFRP bars and cementitious materials, as well as BFRP geotechnical anchorage systems, which are mainly used to understand the interfacial bonding behavior, deformation characteristics, and damage mechanisms of BFRP materials. The third category includes studies on GFRP anti-floating anchor rods, conventional fully grouted rock anchors, and other FRP anchorage systems, which are only considered as analogical evidence for interpreting common load transfer mechanisms and variation trends.
Due to the differences among these systems in terms of bar material and axial stiffness, surface configuration, anchorage scale, boundary conditions, rock and soil mass confinement, and surrounding media, quantitative parameters obtained from the latter two categories, including bond strength, interfacial shear stress, critical anchorage length, and failure thresholds, are not directly extrapolated to BFRP anchor rods. In this review, qualitative comparisons are only conducted when fundamental load-transfer paths and interfacial mechanisms exhibit sufficient physical similarity, and the sources of evidence and their applicable scopes are explicitly clarified in the relevant discussions.
3. Interfacial Bonding Mechanisms and Failure Modes of BFRP Anti-Floating Anchors
BFRP anti-floating anchors transfer uplift loads sequentially through the BFRP anchor rod-anchorage body interface and the anchorage body-rock and soil mass interface. The bond strengths of these two interfaces govern the axial force distribution along the anchor, the interfacial slip, and the ultimate failure mode. Owing to the substantial differences in mechanical properties between BFRP anchors and steel anchors, the interfacial bonding mechanism of BFRP anti-floating anchors cannot be directly interpreted using conventional bond theories developed for steel anchors, but should instead be analyzed by considering the material characteristics of FRP and the geotechnical anchorage conditions.
3.1. Bonding Mechanism of the BFRP Anchor Rod-Anchorage Body Interface
The bond between the BFRP anchor rod and the anchoring cement mortar is mainly composed of three components: the chemical adhesion between the surface of the BFRP anchor rod and the cementitious matrix in the anchoring mortar, the mechanical interlocking between the surface ribs of the BFRP anchor rod and the cementitious matrix in the anchoring mortar, and the physical friction between the surface of the BFRP anchor rod and the anchoring mortar. When the BFRP anchor rod is subjected to external loading, these three mechanisms do not act independently, but interact synergistically to resist the applied load. The interfacial force-transfer mechanism is illustrated in Figure 5.
Figure 5.
Schematic diagram of force transfer at the BFRP anchor rod-anchorage body interface.
At the initial stage of loading, relatively small frictional resistance and chemical adhesion are the primary mechanisms acting between the BFRP anchor rod and the anchoring mortar. The interfacial shear stress between the BFRP anchor rod and the mortar is relatively low and remains far below the bond strength between the BFRP anchor rod and the anchoring mortar, as shown in Figure 6a. As the applied load increases, the frictional resistance and chemical adhesion between the BFRP anchor rod and the anchoring mortar reach their limiting values and gradually decrease, resulting in the initiation of relative slip at the interface. At this stage, most of the applied load is resisted by the mechanical interlocking between the surface ribs of the BFRP anchor rod and the anchoring mortar, as shown in Figure 6b. With a further increase in load, wear develops on the surface ribs of the BFRP anchor rod, reducing the mechanical interlocking in the shallow section and causing the load-transfer zone to progressively migrate toward deeper portions of the BFRP anchor rod. Meanwhile, cracks within the anchorage body gradually propagate outward from the inner region, as shown in Figure 6c. When the applied load reaches the maximum bond stress between the BFRP anchor rod and the anchoring mortar, debonding occurs at the BFRP anchor rod-anchorage body interface, accompanied by cracking or crushing of the anchorage body. This induces relative slip between the BFRP anchor rod and the anchorage body, ultimately leading to failure of the anchorage system and loss of its load-bearing capacity, as shown in Figure 6d [30,31]. The green arrows in the figure represent radial stress, the orange arrows represent shear stress, and the blue arrows represent mechanical anchoring force.
Figure 6.
Schematic diagram of the bonding evolution stages at the BFRP anchor rod-anchorage body interface. (a) Chemical adhesion stage; (b) Mechanical biting force stage; (c) The crack propagation stage of the anchorage body; (d) Interface detachment stage.
Interfacial bonding behavior is jointly influenced by the surface morphology and diameter of the BFRP anchor rod, anchorage length, and external confinement. Achillides [32] investigated various parameters affecting interfacial bond strength and its development process, including anchorage length, FRP type, and surface treatment of FRP rods. Okelo et al. [33] found through pull-out tests that, in the BFRP anchor rod rupture failure mode, the average bond strength of FRP rods was approximately 40–100% of that of steel reinforcement, and that increases in rod diameter and variations in confinement conditions could alter both the average bond strength and the interfacial stress distribution. Baena et al. [34] reported that increasing the compressive strength of concrete enhanced the interfacial bond strength to a certain extent, while also altering the failure mode and failure surface. Analyses of the effects of surface treatment on bonding performance have further demonstrated that different surface treatments result in distinct bonding mechanisms. The surface configuration of the BFRP anchor rod not only affects the peak bond stress, but also governs the slip corresponding to the peak stress and the residual load-bearing capacity.
3.2. Bonding Mechanism of the Anchorage Body-Rock and Soil Mass Interface
The resistance of the anchorage body-rock and soil mass interface mainly originates from interfacial cohesion, friction induced by borehole-wall roughness, and surface mechanical interaction. The interfacial force-transfer mechanism is shown in Figure 7. During the initial bonding stage, as illustrated in Figure 8a, the slip at the anchorage body-rock and soil mass interface is small, and no significant damage occurs, with chemical bonding playing the dominant role. As the load increases, as shown in Figure 8b, the interfacial bond stress increases, and friction and mechanical interlocking jointly contribute to load transfer, while local microcracks at the interface begin to propagate. With a further increase in load, the interfacial bond stress reaches its peak value, and friction and mechanical interlocking continue to act, accompanied by local crushing of the anchorage body and the surrounding rock and soil mass, as shown in Figure 8c. When the failure load is reached, the cracks propagate further, the anchorage body and the surrounding rock and soil mass are subjected to more severe crushing, and the interfacial bonding effect gradually degrades, as shown in Figure 8d [35].
Figure 7.
Schematic diagram of force transfer at the anchorage body-rock and soil mass interface.
Figure 8.
Schematic diagram of the bonding evolution stages at the anchorage body-rock and soil mass interface. (a) Chemical adhesion stage; (b) Mechanical biting force stage; (c) The crack propagation stage of the rock and soil mass; (d) Interface detachment stage.
The bonding performance of the anchorage body-rock and soil mass interface depends not only on interfacial cementation, friction, and mechanical interlocking, but also on the confinement provided by the surrounding rock mass and the stiffness compatibility among the BFRP anchor rod, anchorage body, and rock and soil mass. Based on tests on fully grouted anchors, Hyett et al. [36] found that radial confinement of the rock mass is a key factor governing interfacial bond strength and failure mode. Under low-confinement conditions, the anchorage body-rock mass interface is more susceptible to slip, debonding, or overall pull-out failure. As radial confinement increases, interfacial shearing is increasingly restrained, and the resulting additional normal stress enhances frictional resistance and mechanical interlocking, thereby increasing both the peak bond strength and the residual load-bearing capacity of the outer interface. In addition to strength conditions, the relative stiffness among the BFRP anchor rod, anchorage body, and rock and soil mass also governs the distribution of interfacial shear stress. Hyett et al. [37] further pointed out that, when the stiffness of the BFRP anchor rod or anchorage body is relatively high and the confinement provided by the surrounding rock mass is strong, load transfer is generally concentrated within a relatively short region near the loading end, resulting in higher peak interfacial shear stresses and more pronounced stress concentration. In contrast, in weaker strata or strata with greater deformability, larger relative displacements can develop between the anchorage body and the surrounding rock mass, thereby extending the load-transfer range and making slip and debonding at the second interface, namely the anchorage body-rock and soil mass interface, more pronounced. Therefore, in stronger rock masses, the governing failure mode may shift to failure within the anchorage body or at the first interface, namely the BFRP anchor rod-anchorage body interface, whereas in weak strata, the second interface is more likely to become the critical weak link controlling the overall load-bearing capacity.
3.3. Failure Modes of BFRP Anti-Floating Anchors
Based on existing pull-out tests of BFRP anchors and related studies on fully grouted anchorage systems, the failure of BFRP anti-floating anchors is not independently controlled by a single component or a single interface, but is jointly governed by the relative strength and stiffness of the BFRP anchor rod, anchorage body, rock and soil mass, and the two interfaces. Four typical failure modes of BFRP anti-floating anchors are illustrated in Figure 9. Rupture failure of the BFRP anchor rod may occur due to defects within the rod, such as weak fibers and microcracks. Slip at the BFRP anchor rod-anchorage body interface is generally caused by insufficient shear strength of the bonded interface between the BFRP anchor rod and the anchorage body. Slip at the anchorage body-rock and soil mass interface occurs when the bonding performance of this interface is relatively weak. Failure of the surrounding rock and soil mass is characterized by pull-out of the anchorage body together with the surrounding rock and soil mass in an inverted-cone shape and is more likely to occur in anchorage systems installed in strata with relatively poor mechanical properties [38]. The ultimate failure mode is governed by the strength of the BFRP anchor rod, the relative load-bearing capacities of the two interfaces, and the geological conditions.
Figure 9.
Schematic diagram of typical failure modes of BFRP anti-floating anchors. (a) Tensile failure of the anchor rod shaft; (b) Slip failure at the interface between the anchor rod and the anchored material; (c) Slip failure at the interface between the anchor and the rock-soil mass; (d) Failure of rock and soil masses.
Some researchers have investigated the effects of BFRP anchor rod diameter, anchorage length, cover thickness, and anchorage body material properties on interfacial bonding performance. The anchorage body itself may also become a weak link in the anchorage system. When the mechanical interlocking effect at the surface of the BFRP anchor rod is strong but the radial confinement of the anchorage body is insufficient, the local bearing stress and radial splitting action generated around the ribs of the rod may cause cracking, splitting, or local crushing of the anchorage body. Wang et al. [39] found that the failure mode was related to the cover thickness and BFRP rod diameter, while the bond strength was governed by the shear resistance of the BFRP anchor rod surface. When the cover thickness was sufficient, most specimens exhibited pull-out failure of the BFRP anchor rod without cracking of the cover, as shown in Figure 10a. When the cover thickness was relatively small, splitting failure of the anchorage body occurred due to insufficient shear resistance, as shown in Figure 10b.
Figure 10.
Failure diagram from the pull-out test on BFRP anti-floatation anchor bolts. (a) pullout; (b) pullout with matrix splitting.
When the cohesion, friction, and mechanical interlocking at the second interface between the anchorage body and the rock and soil mass are relatively weak, the BFRP anchor rod and the anchorage body may slide or be pulled out together relative to the surrounding rock and soil mass. Feng et al. [40] investigated the effects of anchor type, anchor diameter, anchorage length, and anchorage body diameter on interfacial shear stress through laboratory pull-out tests. One group of anchors exhibited slip failure at the second interface, as shown in Figure 11, which was attributed to the relatively low overburden pressure and the resulting low bond strength of the second interface. Further analysis indicated that, with increasing anchorage length and anchorage body diameter, the failure mode tended to shift from the first interface to the second interface. In another study [41], field pull-out tests were conducted on BFRP anchors with different diameters and anchorage lengths in loess strata. The results showed that failure characteristics at both the inner and outer interfaces of the anchorage body coexisted during pull-out, and the overall failure mode of the anchorage system was governed by the relative strengths of the constituent interfaces. Anchors with smaller diameters predominantly exhibited shear failure at the BFRP anchor rod-anchorage body interface, whereas anchors with larger diameters were more prone to slip failure at the anchorage body-rock and soil mass interface.
Figure 11.
Failure modes of BFRP anchorage systems.
3.4. Constitutive Model of the Interfacial Bond-Slip Relationship
The interfacial bond-slip model is used to quantitatively characterize the relationship between interfacial shear stress and the relative slip between the BFRP anchor rod and the anchorage body and provides an important basis for establishing the load-displacement response of anchors, analyzing axial force transfer, and revealing the evolution of interfacial damage. Existing studies generally idealize the interfacial loading process into several successive stages and describe the entire evolution from initial bonding and peak load resistance to debonding and slip through piecewise constitutive relationships. Ren et al. [29] employed a trilinear bond–slip relationship to describe the full-process response of the bar-anchorage body interface. This relationship can be expressed as
where (τp) is the peak bond shear stress, (τr) is the residual bond shear stress, (sp) is the interfacial slip corresponding to the peak bond strength, and (sr) is the slip at the onset of the residual friction stage. The main model parameters can be back-calculated from the characteristic points of the load-displacement curves obtained from pull-out tests and subsequently validated using the distributions of axial stress in the bar and interfacial shear stress. Ren et al. calibrated and validated the model parameters using two sets of pull-out tests. The trilinear model has the advantage that its parameters possess relatively clear physical meanings and can independently characterize the initial stiffness, peak strength, post-peak softening, and residual friction. It is therefore well suited to describing the evolution of the surface ribs or threads of BFRP bars through the stages of adhesion-mechanical interlocking-sliding-residual friction.
Ma et al. [42] further employed a continuous nonlinear relationship to describe the interfacial softening and complete debonding processes. The corresponding local bond shear stress-slip relationship can be expressed as
In the equation, Eb and db represent the elastic modulus and diameter of the bar, respectively, while a and b are empirical parameters determined from pull-out tests. The corresponding load-slip relationship at the loading end is
This model uses a continuous function to replace the piecewise linear softening relationship, enabling a smooth description of the process by which interfacial shear stress increases, reaches a peak, and then gradually decays and allowing for the representation of the interface’s eventual complete delamination. Compared to the trilinear model, this model avoids abrupt changes in the constitutive relationship between different loading stages, making it more convenient for numerical calculations and continuous damage simulation. However, its parameters a and b are highly empirical and are relatively sensitive to the interface surface topography, the properties of the anchoring material, and confining pressure conditions.
He et al. [43] established an analytical framework for fully grouted anchors. Rather than simply prescribing a local τ-s constitutive relationship, this approach directly characterizes the distribution of interfacial shear stress along the anchorage length and the propagation of the debonding zone. Before interfacial debonding occurs, the interfacial shear stress can be approximated as exhibiting an exponential decay from the loading end toward the deeper anchorage zone:
where (x) is the distance from the loading end, (τp) is the peak interfacial shear stress, (db) is the diameter of the BFRP anchor rod, and (α) is a load-transfer parameter reflecting the relative stiffness of the anchor rod, anchorage body, and surrounding rock. As the applied load increases, the model further introduces a fully debonded zone, a residual shear stress zone, a post-peak transition zone, and an intact bonded zone, while accounting for different failure modes, such as anchor rod rupture and interfacial pull-out.
In summary, existing models are mathematically capable of separately describing the pre-peak increase, post-peak softening, residual friction, and complete debonding of the interface. However, most of these models were developed based on steel rock anchors or pull-out tests involving a single anchor rod-cementitious material interface and therefore cannot be directly regarded as representative of the actual dual-interface response of BFRP anti-floating anchors. The relatively low elastic modulus, linear-elastic brittle failure characteristics, and surface rib configuration of the BFRP anchor rod can alter the initial stiffness, peak slip, and residual strength of the BFRP anchor rod-anchorage body interface. Meanwhile, the anchorage body-rock and soil mass interface is additionally governed by the confining pressure of the rock and soil mass, borehole-wall roughness, and the deformation characteristics of the ground. Therefore, for BFRP anti-floating anchors, a more appropriate modeling approach is to separately define the (τ1-s1) relationship for the BFRP anchor rod-anchorage body interface and the (τ2-s2) relationship for the anchorage body-rock and soil mass interface, and then couple the two interfaces through the axial equilibrium and deformation compatibility of the BFRP anchor rod and anchorage body.
4. Load-Transfer Behavior and Influencing Factors of BFRP Anti-Floating Anchors
4.1. Axial Force Distribution
The distribution of axial force along the anchorage length of the BFRP anchor rod directly reflects the interfacial load-transfer process. For fully bonded anchors subjected to tension, the axial force generally reaches its maximum at the loading end and gradually decreases with increasing distance from the loading end. Vlachopoulos et al. [44] employed distributed optical fiber sensing technology to continuously monitor the axial response of fully grouted anchors, thereby revealing in detail the process by which axial force is transferred from the loading end toward deeper portions of the anchorage section. The test results showed that, at low load levels, the interface remained in an elastic bonding state, and most of the applied load was carried by the interface near the loading end. Consequently, the axial force in the BFRP anchor rod decreased rapidly within this region, while the axial force and strain in deeper sections remained relatively small. As the applied load increased, the interfacial shear stress near the loading end gradually reached a higher level, and local slip developed. The original load-transfer region could no longer sustain the additional load, causing the load to be redistributed toward deeper portions of the anchorage section and indicating the progressive extension of the effective load-transfer zone into the anchorage depth. This observation is consistent with the findings of Benmokrane, Zhang, Chen, et al. [45,46,47], who monitored the internal mechanical response of anchors using sensors and reported that the stress in the anchor rod decreased with depth. At low load levels, the load was primarily concentrated near the borehole opening, whereas deeper anchorage sections gradually became mobilized only as the applied load increased.
A similar load-diffusion phenomenon has also been confirmed by tests on BFRP-cement-based material interfaces. Wang et al. [19] adopted various surface treatment methods for the BFRP anchor rod–anchorage body interface and evaluated the interfacial bonding performance based on the interfacial stress distribution. The results showed that the bond stress between the BFRP anchor rod and the anchorage body was mainly concentrated near the loading end of the anchor. As shown in Figure 12, the strain increased rapidly near the loading end, whereas the strain at the free end of the BFRP anchor rod was nearly zero. The strain near the loading end first reached its maximum, after which the peak strain progressively shifted toward the free end. Eventually, debonding occurred at the interface near the loading end, and the debonding zone gradually propagated from the loading end toward the free end. This process indicates that axial force transfer between BFRP and cement-based materials does not occur simultaneously along the entire bonded length, but instead evolves through a sequence characterized by load concentration near the loading end, local debonding, and progressive expansion of the load-transfer zone.
Figure 12.
Axial stress distribution along the BFRP anchor rod: (a) fixed with a single adhesive layer; (b) fixed with double adhesive layers [19].
The axial force distribution also changes with the development of interfacial damage. Nemcik et al. [48] incorporated a nonlinear bond-slip relationship into a numerical model and found that, before the occurrence of interfacial damage, the axial force in the BFRP anchor rod continuously decreased from the loading end toward the deeper anchorage section, with the axial force gradient primarily governed by the initial interfacial stiffness. Once debonding first occurred near the loading end, the interfacial shear stress in this region decreased from the peak value to the residual level, causing the local axial force profile to gradually change from a steep decrease to a relatively gentle decline. At this stage, the boundary between the intact and debonded regions became a new location of shear stress concentration. As the debonding zone propagated toward deeper portions of the anchorage section, the region with the maximum axial force gradient shifted accordingly, indicating that the load-transfer capacity of an anchor cannot be comprehensively evaluated solely on the basis of the axial force distribution at a single load level. Comparison between the numerical predictions and experimental results, as shown in Figure 13, demonstrated that the model could effectively predict the axial stress distribution along the anchor rod.
Figure 13.
Comparison of numerical model predictions with experimental results [42,48,49].
4.2. Interfacial Shear Stress Distribution
Interfacial shear stress directly reflects the transfer of axial force from the BFRP anchor rod to the anchorage medium, and its magnitude is governed by the rate of change in the axial force of the BFRP anchor rod along the anchorage depth. Compared with the axial force distribution, interfacial shear stress is more sensitive to local slip, material defects, and other localized effects, and therefore generally exhibits more pronounced stress concentration and non-uniformity. Ghadimi et al. [50] comprehensively considered the structural characteristics of anchors and the compatible deformation among the BFRP anchor rod, anchorage body, and surrounding rock mass under pull-out loading conditions in a numerical model. The results showed that the interfacial shear stress generally reached a relatively high value near the loading end and decreased approximately exponentially with increasing anchorage depth. This indicates that the applied load is not carried simultaneously by the entire anchorage section, but is initially concentrated within a limited region near the loading end. Only as the applied load increases and slip or damage develops at the interface near the loading end do deeper portions of the interface gradually become mobilized in load transfer. This distribution pattern corresponds to the progressive attenuation of axial force from the loading end toward deeper sections, while the magnitude and spatial extent of the shear stress peak provide a more direct indication of the location and progressive expansion of the effective load-transfer zone.
Zhang Shubo et al. [51] conducted laboratory direct shear tests to comparatively investigate the shear performance of jointed rock masses reinforced with BFRP bars and conventional steel bars. The results showed that the shear strength-displacement curve increased approximately linearly before the peak. After reaching the peak, the specimens did not immediately lose their load-bearing capacity completely, but instead exhibited a relatively gradual nonlinear decrease in shear resistance with increasing shear displacement. This behavior was attributed to the extensive stretching of the fiber material at the displaced joint surface when the specimen reached the peak load. A considerable amount of energy was absorbed during fiber shearing or tensile rupture, thereby imparting a certain degree of toughness to the system, as shown in Figure 14a. Compared with steel bars, BFRP bars have a lower elastic modulus, resulting in a relatively lower overall shear stiffness of the anchored joint system during the linear elastic stage, while the shear displacement corresponding to the peak shear stress is generally larger. In addition, the evolution of shear resistance in BFRP-reinforced specimens can be clearly divided into four stages: the linear elastic stage, pre-peak nonlinear stage, nonlinear softening stage, and residual strength stage, as shown in Figure 14b.
Figure 14.
Shear strength-displacement curves and schematic illustration of shear-displacement characteristics [50]. (a) Shear Strength–Displacement Curve; (b) Schematic diagram of the shear test strength–displacement curve.
Overall, the interfacial shear stress of BFRP anti-floating anchors exhibits pronounced concentration near the loading end and decreases with increasing depth, while its distribution continuously evolves with the development of interfacial slip and damage. Existing studies have revealed the shear stress transfer characteristics of fully grouted anchors and have also provided preliminary insights into the deformation behavior of BFRP bars under shear loading. However, direct experimental investigations of the local shear stress distribution, migration of peak shear stress, and synergistic damage evolution of the first and second interfaces in BFRP anti-floating anchors remain limited. Future studies could combine distributed optical fiber strain monitoring with dual-interface slip measurements and cross-validate the results against the locations of local interfacial damage, thereby enabling more accurate identification of the effective load-transfer length and progressive failure process of BFRP anti-floating anchors.
4.3. Critical Anchorage Length
For fully bonded BFRP anchor rods, the anchorage length directly affects the extent to which the tensile capacity of the bar can be mobilized, the distribution of interfacial shear stress, and the overall failure mode [52,53]. When discussing anchorage length, it is necessary to distinguish between the effective load-transfer length and the critical anchorage length. The effective load-transfer length refers to the portion of the anchorage zone in which the interfacial shear stress is substantially mobilized and carries the major part of the load transfer under a given load level. Its magnitude varies with increasing load, interfacial slip, and the development of local damage. In contrast, the critical anchorage length is defined as the minimum anchorage length required to fully mobilize the target load-bearing capacity of the bar while preventing overall pull-out of the anchorage system or significant slip at the free end. Therefore, the effective load-transfer length reflects the actual range mobilized during the loading process, whereas the critical anchorage length is more closely related to the design control parameter at the ultimate limit state of the anchorage system.
Under the simplest assumption of uniform bonding, if the average interfacial bond strength is () and the bar diameter is (d), the total bond force provided by the bar-anchorage body interface over an anchorage length (L) can be expressed as
Accordingly, the critical anchorage length required to resist the target tensile load (Pd) can be obtained as
Equation (3) indicates that, under the idealized condition of a constant average bond strength, increases in bar diameter and tensile strength lead to a greater critical anchorage length required to fully mobilize the tensile capacity of the bar, whereas an increase in interfacial bond strength reduces the required anchorage length. However, this approach assumes a uniform distribution of interfacial shear stress along the anchorage length and therefore cannot capture the shear-stress concentration near the loaded end, local slip, and progressive debonding observed in actual anchor rods. Consequently, it is more suitable for a first-order estimation of the critical anchorage length. Tighiouart et al. [54] conducted tests on FRP bars with different diameters and bond lengths and found that, as the bond length increased, the pull-out load gradually approached the tensile capacity of the bar, while the average bond strength was not constant. This indicates that the use of a single average bond strength to evaluate long anchorage zones may neglect the pronounced non-uniformity of the stress distribution.
Compared with the average bond-strength approach, models based on bond-slip relationships can further describe the evolution of the effective load-transfer length during loading. For the single bar-anchorage body interface, the interfacial shear stress in the elastic bonding stage can be approximately expressed as
where (k1) is the initial shear stiffness of the first interface, and (s1) is the relative slip between the bar and the anchorage body. By combining this relationship with the axial equilibrium equation of the bar:
Together with (Nb = EbAbdub/dx), it can be seen that the decay scale of the interfacial stress is jointly governed by the axial stiffness of the bar (EbAb), the interfacial stiffness (k1), and the bar perimeter. Accordingly, the characteristic load-transfer length can be expressed in a simplified form as
Therefore, the effective load-transfer length is governed not only by the peak bond strength, but also by the relative stiffness between the bar and the interface. Zou et al. [55] adopted a bond model that evolves with slip to describe the progressive development of the interface of fully grouted anchor rods from the bonded zone to the softening and debonded zones and further derived analytical relationships for the distributions of shear stress, axial force, and relative displacement along the anchorage length. Similarly, Zhang et al. [56] divided the entire pull-out process into elastic, softening, and debonding stages, and indicated that, as the local interface enters the softening or debonding state, the remaining intact anchorage zone is progressively mobilized, while the distributions of axial force and interfacial shear stress are continuously adjusted with increasing load.
The above relationships also indicate that the effect of the elastic modulus of BFRP on the effective load-transfer length and critical anchorage length is twofold. The elastic modulus of BFRP is generally lower than that of steel reinforcement, resulting in greater axial deformation of the bar under the same tensile load and consequently altering the relative slip and shear-stress distribution between the bar and the anchorage body. On the one hand, (EbAb), together with the interfacial stiffness, governs the stress-decay scale during the elastic stage. On the other hand, greater relative slip near the loaded end may cause the first interface to reach its peak bond stress earlier and subsequently enter the softening stage. Therefore, the critical anchorage length cannot be determined solely on the basis of the elastic modulus of BFRP; rather, the axial stiffness of the bar, initial interfacial stiffness, peak bond strength, peak slip, and residual bond strength should be considered jointly.
The bar diameter simultaneously affects the tensile capacity of the bar and the interfacial area per unit anchorage length. For geometrically similar circular bars, the tensile capacity of the bar increases approximately with (d2), whereas the bonding perimeter of the bar-anchorage body interface increases only with (d). Therefore, under otherwise identical conditions and when the design objective is to fully mobilize the tensile capacity of the bar, a larger bar diameter generally requires a greater critical anchorage length. In practice, however, an increase in diameter may also alter the rib geometry, radial confinement, and local splitting effects; therefore, its influence cannot be simply extrapolated linearly from Equation (3). Wang et al. [57] investigated BFRP bars with different anchorage lengths and found that, when the anchorage length increased from 5 d to 10 d, the bond strength decreased by 24.30%, 3.73%, and 6.44% at different loading rates, respectively, while the bond stiffness decreased by 53.87%, 40.12%, and 39.28%, respectively, as shown in Figure 15. These results demonstrate that the additional anchorage length cannot be utilized proportionally according to the assumption of a constant average bond strength. This is essentially because the interfacial shear stress is concentrated within a limited load-transfer zone, whereas the remote interface is only progressively mobilized after slip and damage develop near the loaded end.
Figure 15.
Effect of anchorage length on bond strength and bond stiffness [56].
Geological conditions primarily affect the effective load-transfer range through the stiffness, frictional resistance, cohesion, and radial confinement of the second interface. In intact rock masses with relatively high strength and sufficient radial confinement, the second interface generally exhibits a relatively high load-transfer capacity, and the critical weak interface of the system may shift to the first interface between the bar and the anchorage body. Under such conditions, improving the performance of the first interface becomes more critical for controlling the critical anchorage length. In contrast, under conditions of weak soil, fractured rock masses, or low confinement, slip is more likely to occur at the second interface. Its relatively low shear stiffness and strength may extend the load-transfer range toward deeper anchorage zones and may cause the second interface to become the controlling factor for the critical anchorage length. Therefore, the rational design of BFRP anchor rods should not simply pursue an increase in anchorage length. Instead, the anchorage length should be determined in accordance with the principal load-transfer range by comprehensively considering the axial stiffness and tensile capacity of the bar, the bond–slip performance of the first interface, the stiffness and strength of the grout, the shear performance of the second interface, and the confinement provided by the rock and soil mass.
The different methods for analyzing anchorage length and their applicability to BFRP anchor rods are summarized in Table 1.
Table 1.
Comparison of Different Anchorage-Length Analysis Methods and Their Applicability to BFRP Anchor Rods.
4.4. Factors Influencing Load Transfer
The load-transfer behavior of BFRP anti-floating anchors is not governed by a single material or interface, but results from the combined effects of the mechanical properties of the BFRP anchor rod, material properties of the anchorage body, conditions of the rock and soil mass, and construction quality. These factors determine not only the peak bond strength and residual shear resistance of the interfaces, but also the attenuation rate of axial force, the degree of interfacial shear stress concentration, and the effective load-transfer length [9,58]. Therefore, analyses of factors influencing load transfer should not be limited to the isolated effect of a single parameter on the ultimate pull-out capacity, but should instead consider the stiffness compatibility and strength coordination of the BFRP anchor rod-anchorage body-rock and soil mass system as a whole.
The surface configuration of the BFRP anchor rod directly governs adhesion, friction, and mechanical interlocking at the first interface. Cao et al. [59] proposed that the optimal surface configuration is not fixed, but depends on the cohesion, friction angle, and compressive strength of the anchorage body. When the anchoring material is relatively weak, excessively high or steep ribs may generate large local bearing and shear stresses in front of the ribs, causing the anchorage body to undergo crushing first. In contrast, when the anchorage body has relatively high strength and sufficient radial confinement, appropriate increases in rib height, rib spacing, or surface roughness are beneficial for enhancing mechanical interlocking and allowing the relatively high tensile capacity of the BFRP anchor rod to be more fully mobilized. Using fiber Bragg grating sensors, strain gauges, and other monitoring techniques, Zhu et al. [10] identified differences in the load-transfer mechanisms of FRP and steel anchors. Parameters such as BFRP anchor rod diameter, interfacial shear strength, and interfacial shear stress coefficient jointly affect the rate at which load spreads from the loading end toward deeper portions of the anchorage section. When the axial stiffness of the BFRP anchor rod is relatively low, the axial force attenuates more gradually along the anchorage length, allowing a greater portion of the deeper interface to participate in load transfer. However, the larger deformation of the BFRP anchor rod also increases the relative slip near the loading end, causing local interfacial damage to occur at an earlier stage.
In addition, the material properties of the anchorage body and rock and soil mass are another key factor influencing load-transfer efficiency. Higher compressive strength and elastic modulus of the anchorage body generally contribute to improved bearing resistance in front of the ribs and higher initial interfacial stiffness, while reducing local crushing deformation. However, excessively high stiffness may also intensify shear stress concentration near the loading end, making it difficult to fully mobilize the anchorage length farther from the loading end at low load levels. The conditions of the rock and soil mass influence load transfer mainly through external confinement and the shear resistance of the second interface. Intact rock masses with relatively high strength can provide strong radial confinement to the anchorage body, thereby fully mobilizing interfacial friction and mechanical interlocking, with the load generally transferred within a relatively short region near the loading end. In contrast, in weak strata with relatively high deformability, larger relative slip is more likely to develop at the anchorage body-rock and soil mass interface, resulting in an expanded load-transfer range and more pronounced progressive debonding at the second interface.
Compared with material parameters, the effects of construction defects on load transfer are generally more localized and abrupt. Inadequate cleaning of the borehole wall, incomplete grouting, local necking, and eccentricity of the BFRP anchor rod may interrupt the originally continuous load-transfer path and induce additional stress concentrations at the ends of the defects. Xu et al. [60] found that increasing the debonded length reduced the peak load and produced a relatively flat region in the axial force distribution of the BFRP anchor rod, as shown in Figure 16a. The closer the debonded region was to the loading end, the longer the nonlinear portion of the axial force distribution became, as shown in Figure 16b. For the same total debonded length, concentrated debonding was more detrimental than distributed debonding because several intact bonded regions remained between discrete defects, allowing the load to be transferred and redistributed in stages. In contrast, continuous debonding creates a relatively long interruption in the load-transfer path, resulting in more pronounced shear stress concentration at the end of the defective region and accelerating the subsequent progressive failure of the interface. Therefore, construction quality control for BFRP anti-floating anchors should focus not only on the total grouting volume and strength of the anchorage body, but also on ensuring the continuity and compactness of the anchorage body near the loading end and the proper centering of the BFRP anchor rod, while avoiding the formation of continuous debonded zones.
Figure 16.
Axial force distribution of the anchor under multiple load levels: (a) different defect lengths; (b) different defect locations.
A summary and comparison of existing research on FRP/BFRP anchoring was conducted, focusing on key factors such as material types, anchoring system configurations, geometric parameters, anchorage lengths, grouting and soil conditions, load types, interfacial bond properties, and failure modes, as shown in Table 2.
Table 2.
Summary of representative FRP/BFRP anchorage studies and their relevance to BFRP anchor rods.
5. Load-Transfer Characteristics of BFRP Anti-Floating Anchors Under Different Loading Modes
5.1. Load-Bearing Characteristics Under Monotonic Loading
Monotonic pull-out tests are a fundamental method for evaluating the short-term load-bearing capacity, interfacial bonding performance, and failure modes of BFRP anti-floating anchors. Under continuously increasing load without unloading, the anchorage system sequentially undergoes elastic elongation of the BFRP anchor rod, interfacial bonding, development of local slip, and ultimate failure [61]. The load-displacement response of BFRP anti-floating anchors under monotonic pull-out loading can generally be divided into the initial compaction and bonding stage, approximately linear growth stage, nonlinear strengthening stage, peak failure stage, and post-peak residual stage.
At the initial stage of loading, the displacement of the BFRP anchor rod is relatively small, while pores within the anchorage body, micro-gaps along the borehole wall, and local interfacial defects gradually close. Both the BFRP anchor rod-anchorage body interface and the anchorage body-rock and soil mass interface remain intact, and the applied load is mainly resisted within a relatively short region near the loading end. Because the elastic modulus of the BFRP anchor rod is lower than that of steel reinforcement, its elastic elongation is generally more pronounced under the same load level, and consequently, deformation of the BFRP anchor rod accounts for a relatively larger proportion of the total displacement at the anchor head. Serbescu et al. [62] investigated the mechanical properties of BFRP bars and showed that BFRP materials remain essentially linearly elastic until failure. Their relatively low axial stiffness and brittle fracture characteristics mean that no pronounced plastic deformation similar to post-yield behavior in steel reinforcement occurs during monotonic loading. As the load increases, the axial force in the BFRP anchor rod is progressively transferred from the loading end toward deeper portions of the anchorage section, and the interfacial shear stress near the loading end is mobilized first.
When the first interface near the loading end reaches its peak bond strength, local failure or relative slip of the BFRP anchor rod begins to occur. Pull-out tests on BFRP bar-concrete interfaces conducted by El Refai et al. [63] showed that the surface configuration of BFRP bars significantly affects both the peak bond strength and the failure path. For BFRP bars with relatively smooth surfaces, failure generally develops along the contact interface between the BFRP bar and the cement-based material. For sand-coated or strongly wrapped BFRP bars, enhanced mechanical interlocking causes the failure path to shift into the surface resin layer or the shallow concrete.
After local debonding occurs near the loading end, the interfacial shear stress in this region decreases from the peak value to the softening or residual level, and the additional load is subsequently redistributed toward deeper portions of the anchorage section. Nemcik et al. [48] incorporated a nonlinear bond-slip relationship into a numerical model and found that, during the undamaged stage, the axial force in the BFRP anchor rod continuously decreases from the loading end toward the deeper anchorage section. Once debonding occurs near the loading end, the axial force gradient within the debonded region decreases significantly, while the peak interfacial shear stress shifts to the boundary between the debonded region and the intact bonded region. As the debonding front propagates toward deeper portions of the anchorage section, the distributions of axial force and interfacial shear stress continuously evolve [64].
Existing studies have relatively clearly revealed the monotonic loading behavior of BFRP anchors, but direct experimental investigations of the cooperative load-transfer process between the two interfaces of BFRP anti-floating anchors remain limited. Future studies should integrate anchor-head load-displacement measurements, distributed strain monitoring along the BFRP anchor rod, and relative slip measurements at both interfaces to distinguish the respective contributions of elastic deformation of the BFRP anchor rod, slip at the first interface, and slip at the second interface to the total displacement and to establish monotonic load-bearing models capable of reflecting the material characteristics of BFRP and progressive damage at the two interfaces.
5.2. Interfacial Bond Degradation and Stress Transfer Under Cyclic Loading
In practical engineering, deep foundation pits of high-rise buildings in coastal cities are significantly affected by cyclic groundwater loading. Repeated unloading and reloading can induce irreversible slip, degradation of interfacial stiffness, and migration of the load-transfer zone within the anchorage system. Long-term accumulation of these effects may lead to base-slab cracking, basement leakage, and local uplift. Based on unidirectional cyclic tensile tests, Tistel et al. [65], based on conventional unidirectional cyclic tensile tests on rock anchors, proposed a model for predicting anchorage capacity by considering the cyclic load level, cyclic load ratio, and number of loading cycles and established a constitutive model for the bond-slip behavior of the anchors. Through cyclic pull-out tests, Oh et al. [66] found that both loading slip and residual slip increased with the number of cycles, while the increase in bond stress became more pronounced during repeated loading. A local bond stress-slip model for anchors under cyclic loading was subsequently established.
Cyclic loading does not simply reproduce the monotonic loading path, but instead induces cumulative interfacial slip, stiffness degradation, and migration of the load-bearing zone through repeated unloading and reloading. Based on field multi-cycle loading tests, Wu et al. [67] found that the load-displacement curves of both the BFRP anchor rod and the anchorage body exhibited pronounced hysteresis. Although the BFRP anchor rod showed a relatively high recovery rate during unloading, a certain amount of residual deformation remained after each loading cycle. The residual deformation after each load level and the BFRP anchor rod strain at the same depth accumulated with increasing number of cycles, as shown in Figure 17a. As the number of cycles increased, both the axial force level and load-transfer depth increased. The interfacial shear stress reached its peak at approximately 0.75 m below the borehole opening, while the peak value gradually decreased with increasing number of cycles, as shown in Figure 17b,c. These observations indicate that cyclic damage initially weakens the load-bearing capacity of the shallow interface, after which the load is progressively transferred toward deeper regions.
Figure 17.
Stress-strain curves and stress variation curves of BFRP anti-floating anchors under cyclic loading. (a) Load–displacement curves from multi-cycle loading tests; (b) Axial force distribution curve; (c) Shear stress distribution curve.
The effects of cyclic loading are closely related to the applied load level. Benmokrane et al. [68] conducted repeated loading tests on conventional anchors in the field and found that, when the upper limit of the cyclic load remained below the initial prestress of the prestressed anchors, repeated cyclic loading did not significantly reduce their service life. However, once the applied load exceeded the initial prestress, the residual deformation increased markedly. These findings indicate that cyclic effects cannot be evaluated solely in terms of the number of cycles; the relative relationships among the mean load, load amplitude, and initial prestress also play important roles. Wang et al. [19] compared the behavior of BFRP anchors under monotonic and cyclic loading. Figure 18 shows the interfacial slip curves under cyclic loading conditions and the evolution of slip with the number of cycles. The interfacial slip under cyclic loading was greater than that under monotonic loading. The slip curves showed a pronounced increase in slip from the first cycle to the 100,000th cycle, after which the slip increased gradually and eventually approached a stable state. During cyclic loading, the interfacial bonding capacity continuously degraded, with the most severe degradation occurring during the first few loading cycles.
Figure 18.
Load-displacement curves under cyclic loading conditions: (a) loading end; (b) free end.
Differences exist in the plastic displacement behavior of BFRP anchors and steel anchors under cyclic loading conditions. Li Guowei et al. [4] found that the measured effective anchorage depth of the steel anchors was far shorter than the distance to the anchor tip. In addition, owing to the high elastic modulus of steel and its poor deformation compatibility with the anchorage body, no relative displacement occurred at the interface between the steel anchor rod and the anchorage body. Meanwhile, the maximum stress applied in the tests was far below the yield strength of the steel anchor rod, indicating that the rod itself did not undergo plastic deformation. Therefore, the plastic displacement at the end of the steel anchor was entirely attributable to the relative displacement at the interface between the anchorage body and the surrounding rock and soil mass.
In contrast, the elastic moduli of the BFRP anchor rod and the anchorage body are relatively close. Under cyclic loading conditions, the anchorage body can provide higher interfacial shear stress to the BFRP anchor rod, thereby allowing the frictional resistance, chemical bonding, and mechanical interlocking at the interface between the BFRP anchor rod and the anchorage body to be more effectively mobilized. Consequently, the deformation compatibility between the BFRP anchor rod and the anchorage body is better than that of steel anchors.
Overall, BFRP anti-floating anchors under cyclic tensile loading exhibit the following fundamental evolution pattern: the initial loading cycles first induce interfacial slip and stiffness degradation near the loading end; subsequently, residual displacement and BFRP anchor rod strain gradually accumulate, accompanied by a reduction in the bonding capacity of the shallow interface; as cyclic damage develops, the axial force and interfacial shear stress are progressively redistributed toward deeper portions of the anchorage section.
5.3. Creep Characteristics Under Sustained Loading Conditions
Under sustained loading conditions, the long-term deformation of BFRP anti-floating anchors does not arise solely from the material behavior of the BFRP anchor rod, but results from the combined effects of viscoelastic deformation of the BFRP anchor rod, sustained slip at the BFRP anchor rod-anchorage body interface, creep and shrinkage of the anchorage body, and deformation at the anchorage body-rock and soil mass interface. Unlike the axial force transfer and interfacial debonding observed under monotonic pull-out loading, sustained loading causes continuous stress redistribution within the anchorage system over time. Even when the external load remains constant, the axial force in the BFRP anchor rod, interfacial shear stress, and local slip continue to redistribute with time. Bai et al. [69] conducted full-scale laboratory tests on GFRP anti-floating anchors under long-term sustained loading conditions. As shown in Figure 19, when the applied load increased to approximately 38–45% of the failure load, the time-dependent deformation of the anchors became more pronounced. With a further increase in load level, both the creep rate and long-term displacement increased significantly. These results indicate that the long-term deformation of anti-floating anchors exhibits a clear load-level dependence. At relatively low load levels, the anchorage system is dominated by relatively stable viscoelastic deformation, whereas, when the sustained load approaches a certain critical level, the contributions of interfacial slip and material damage gradually increase, causing the system to evolve from stable creep to accelerated creep. Furthermore, the experimental results were described using damage mechanics and the standard linear solid model, and the time-dependent damage was correlated with the long-term pull-out capacity, thereby enabling prediction of the long-term load-bearing capacity of anti-floating anchors.
Figure 19.
Anchor displacement curves: (a) displacement-time curves; (b) isochronous load-displacement curves.
The effects of sustained loading on the interfaces are manifested not only by the continuous increase in anchor-head displacement, but more importantly by the time-dependent redistribution of interfacial shear stress. Vilanova et al. [70] subjected 12 GFRP anti-floating anchors to sustained loading for 90–130 days. Based on internal strain measurements along the anchor rods, they obtained the time-dependent evolution of end slip and further analyzed the time-varying distribution of interfacial bond stress. The results showed that, under sustained loading conditions, the initially high interfacial shear stress near the loading end gradually decreased, while the interfacial stress at greater depths increased correspondingly, indicating a progressive transfer of load from the near-end region toward deeper portions of the anchorage section. Feng et al. [71] conducted sustained pull-out loading tests on BFRP anchors. Their study not only determined the short-term failure load of the anchorage system, but also identified the creep failure load under sustained loading conditions, demonstrating that time-dependent deformation and interfacial creep effects in BFRP anchorage systems cannot be neglected.
From the long-term loading behavior of anchors, the creep response of BFRP anti-floating anchors can be generally divided into three stages. The initial stage is dominated by instantaneous elastic deformation and rapid interfacial adjustment, during which displacement increases relatively rapidly shortly after loading. This is followed by a steady creep stage, in which the rates of time-dependent deformation of the BFRP anchor rod and the interfaces gradually decrease, while the axial force and interfacial shear stress undergo slow redistribution. When the sustained load is excessively high or local interfacial damage continues to accumulate, the anchorage system may enter an accelerated creep stage, characterized by a renewed increase in displacement rate, propagation of local debonding, and continuous migration of the effective load-transfer zone toward deeper portions of the anchorage section, eventually leading to interfacial pull-out failure or rupture of the BFRP anchor rod. Therefore, the sustained load level governs not only the total creep deformation, but also whether the anchor can maintain a stable long-term service state.
To improve the transparency and reproducibility of the literature review process, this study employed a combination of keyword-based searches and reference tracking for literature identification and screening. The literature was primarily retrieved from databases including the Web of Science Core Collection, Scopus, Engineering Village, and China National Knowledge Infrastructure (CNKI). The selection of databases was intended to cover both international English-language journal publications and Chinese studies related to field applications of BFRP anchor rods. According to the scope of this review on interfacial bonding and load transfer mechanisms of BFRP anchor rods, the search terms were organized into three categories: material type, anchorage system, and mechanical behavior. Material-related keywords included “BFRP”, “basalt fiber reinforced polymer”, “GFRP”, and “fiber reinforced polymer”; anchorage-system-related keywords included “anti-floating anchor”, “anchor rod”, “ground anchor”, “rock bolt”, “fully grouted anchor”, and “grouted bolt”; and mechanical-behavior-related keywords included “bond”, “bond-slip”, “interface”, “pull-out”, “load transfer”, “shear stress”, “anchorage length”, “critical anchorage length”, “cyclic loading”, “sustained loading”, “creep”, and “durability”.
Because studies directly addressing BFRP anchor rods remain relatively limited, a hierarchical evidence-retrieval strategy was adopted. The first level comprised field studies, full-scale tests, and laboratory investigations conducted specifically on BFRP anchor systems. The second level included studies on BFRP bar-cementitious material interfaces and BFRP geotechnical anchorage systems, which were mainly used to supplement the understanding of interfacial bonding and damage characteristics of BFRP materials. The third level included studies on GFRP anti-floating anchor rods, conventional fully grouted rock anchors, and other FRP anchorage systems, which were used only to analyze physically analogous load transfer mechanisms and general trends. This classification is consistent with the applicability of different levels of evidence adopted throughout the manuscript.
6. Conclusions and Prospects
6.1. Main Conclusions
- (1)
- Existing studies on BFRP anti-floating anchors and related BFRP anchorage tests indicate that the main failure modes include rupture of the BFRP anchor rod, shear-slip failure at the BFRP anchor rod–anchorage body interface, slip failure at the anchorage body-rock and soil mass interface, and failure of the surrounding rock and soil mass. The load-bearing system involves the synergistic interaction of multiple media, including the BFRP anchor rod, anchorage body, and rock and soil mass, together with the two interfaces. The stiffness, peak strength, post-peak softening behavior, and residual load-bearing capacity of the two interfaces jointly govern the overall load–displacement response and ultimate failure mode.
- (2)
- The resistance of the BFRP anchor rod-anchorage body interface mainly originates from chemical bonding, friction, and surface mechanical interlocking, with the dominant mechanism evolving during loading. In contrast, the anchorage body-rock and soil mass interface is mainly governed by cohesion, friction, borehole-wall roughness, and confining pressure provided by the surrounding rock and soil mass. After the interface reaches its peak strength, local slip and debonding do not immediately cause overall failure of the anchorage system. Instead, load transfer continues through post-peak softening, residual friction, and the remaining intact bonded regions, resulting in a progressive failure process.
- (3)
- Field tests conducted directly on BFRP anti-floating anchors have demonstrated that: Both axial force and interfacial shear stress exhibit non-uniform distributions along the anchorage length. The axial force in the BFRP anchor rod generally reaches its maximum at the loading end and gradually decreases toward deeper portions of the anchorage section, whereas the interfacial shear stress is mainly concentrated within a limited region near the loading end. As the applied load increases or interfacial slip develops, the peak shear stress and effective load-transfer zone progressively migrate toward deeper sections, thereby mobilizing deeper portions of the anchorage section to carry the load. Once the anchorage length exceeds the critical anchorage length, the additional anchorage section carries only a very limited proportion of the applied load.
- (4)
- Field cyclic loading tests on BFRP anti-floating anchors have directly demonstrated that: Different loading paths significantly alter the interfacial state and load-transfer mechanism of BFRP anti-floating anchors. Under monotonic loading conditions, the anchorage system undergoes elastic deformation, local interfacial slip, propagation of debonding, and ultimate failure. Cyclic loading further induces the accumulation of residual deformation, degradation of interfacial stiffness, and reduction in the load-bearing capacity of the shallow interface, causing the load to be progressively redistributed toward deeper portions of the anchorage section. Under sustained loading conditions, the long-term response results from the combined effects of time-dependent deformation of the BFRP anchor rod, sustained slip at the two interfaces, creep of the anchorage body, and deformation of the rock and soil mass.
6.2. Existing Limitations and Future Prospects
- (1)
- Long-term service mechanisms under coupled environmental–mechanical conditions
In actual underground engineering environments, BFRP anchor rods are subjected over long periods to the combined effects of multiple factors, including groundwater-level fluctuations, temperature variations, chemical attack, and sustained uplift loads. However, existing studies generally consider environmental actions and mechanical loads separately, making it difficult to reproduce the degradation processes occurring under actual service conditions. Therefore, future studies should establish coupled environmental–load testing systems, with particular emphasis on sustained pull-out and cyclic loading tests under groundwater cycling, wet–dry cycling, chloride attack, and sulfate attack. Research should focus not only on the strength retention of BFRP bars, but also on revealing the effects of environmental actions on the dual-interface load-transfer system, including ① the effects of environmental factors on the BFRP resin matrix, fiber–resin interface, and long-term mechanical properties of the bar; ② the degradation of bond stiffness, peak bond strength, and residual bond strength at the bar–anchorage body interface under environmental exposure; and ③ the evolution of long-term slip, crack development, and confinement capacity at the anchorage body–rock and soil mass interface.
- (2)
- Development of a full-process performance model for creep–fatigue–fracture evolution
Current studies on the long-term performance of BFRP anchor rods mainly focus on displacement development and creep deformation, while a unified description of material damage accumulation, progressive interfacial debonding, and eventual fracture under long-term loading is still lacking. Future research should therefore develop full-process analytical models incorporating time-dependent effects and integrate the following factors within a unified framework: ① viscoelastic deformation and long-term strength reduction of the BFRP bar; ② bond creep and cyclic damage at the bar–anchorage body interface; ③ time-dependent slip at the anchorage body–rock and soil mass interface; and ④ the progressive fracture process through which local damage develops into overall failure.
- (3)
- Statistical variability analysis and full-scale engineering validation
The mechanical properties of BFRP materials, surface treatment, bar manufacturing quality, grouting compactness, and ground parameters all exhibit a certain degree of variability. Therefore, results obtained from individual specimens or small-scale tests are insufficient to directly support engineering design. Future research should accordingly progress from deterministic analysis toward probabilistic analysis. Specific research directions include ① establishing statistical databases for the tensile strength, elastic modulus, interfacial bond parameters, and long-term degradation coefficients of BFRP; ② evaluating the effects of material variability, construction defects, and variations in geological parameters on pull-out capacity and failure probability; and ③ conducting full-scale field tests under different ground conditions, structural dimensions, and service environments to validate the theoretical models.
- (4)
- Reliability-based design methods and code provisions for BFRP anchor rods
At present, the design of BFRP anchor rods mainly refers to methods developed for conventional steel anchor rods or FRP reinforcement systems, while dedicated design approaches accounting for the material characteristics and long-term degradation behavior of BFRP remain insufficient. Future studies should establish a reliability-based design framework based on long-term performance databases and probabilistic models. This framework should comprehensively account for the statistical variability in BFRP strength and stiffness, performance degradation induced by environmental actions, uncertainty in the bonding performance of the dual interfaces, and the effects of grouting quality and construction defects. Appropriate safety factors or partial factors should then be determined through reliability-index analysis to establish design methods capable of satisfying target service-life requirements. Ultimately, an integrated design framework should be developed, including ① material performance evaluation methods; ② dual-interface bearing models; ③ long-term performance degradation models; and ④ reliability-based design methods.
Author Contributions
Conceptualization, F.W., X.B., Z.W. and N.Y.; methodology, F.W., X.B., Z.W. and N.Y.; validation, F.W., X.B. and Z.W.; formal analysis, F.W. and Z.W.; investigation, F.W. and Z.W.; resources, F.W., X.B. and Z.W.; data curation, F.W. and Z.W.; writing—original draft preparation, F.W.; writing—review and editing, F.W. and Z.W.; visualization, F.W., X.B. and Z.W.; supervision, N.Y. All authors have read and agreed to the published version of the manuscript.
Funding
This research was supported by the Qingdao Huanghai University scientific research project 2024KJ28.
Data Availability Statement
The raw data supporting the conclusions of this article will be made available by the authors on request.
Conflicts of Interest
The authors declare no conflicts of interest.
References
- Von der Tann, L.; Sterling, R.; Zhou, Y.; Metje, N. Systems approaches to urban underground space planning and management—A review. Undergr. Space 2020, 5, 144–166. [Google Scholar] [CrossRef] [Scilit]
- Yang, M.; Fu, X.; Liu, H.; Wang, L.; Li, Q. Influencing factors, design methods, and buoyancy reduction measures for basement anti-flotation engineering. Buildings 2024, 14, 3005. [Google Scholar] [CrossRef] [Scilit]
- Wu, Z.; Li, Z.; Fan, J.; Cao, H.; Huang, B.; Liu, H. Up-floating destruction and reinforcement measures of damaged basement based on the bending moment and deformation analysis. Buildings 2023, 13, 1918. [Google Scholar] [CrossRef] [Scilit]
- Li, G.; He, X.; Wu, J.; Chen, W.; Xiong, L.; Cao, X. Insitu test on bond fatigue characteristics of bolts for reinforcing soft shaly sandstone slopes. Chin. J. Rock Mech. Eng. 2020, 39, 1729–1738. [Google Scholar]
- Kong, D.; Guan, Y.; Yuan, H. Study on the anti-floating water level of the underground structure’s comprehensive anti-floating. Structures 2023, 56, 104921. [Google Scholar] [CrossRef] [Scilit]
- Cao, H.; Pan, H.; Luo, G.Y. A new anti-floatation method by drainage: Concept and application. Chin. J. Rock Mech. Eng. 2016, 35, 2542–2548. [Google Scholar]
- Wang, Y.; Sun, X.; Ren, A. Investigations of rock anchor corrosion and its influence factors by exhumations in four typical field sites. Eng. Fail. Anal. 2019, 101, 357–382. [Google Scholar] [CrossRef] [Scilit]
- Gao, K.; Li, Z.; Zhang, J.; Tu, J.; Li, X. Experimental Research on Bond Behavior between GFRP Bars and Stirrups-Confined Concrete. Appl. Sci. 2019, 9, 1340. [Google Scholar] [CrossRef] [Scilit]
- Benmokrane, B.; Zhang, B.; Chennouf, A. Tensile properties and pullout behaviour of AFRP and CFRP rods for grouted anchor applications. Constr. Build. Mater. 2000, 14, 157–170. [Google Scholar] [CrossRef] [Scilit]
- Zhu, H.H.; Yin, J.H.; Yeung, A.T.; Jin, W. Field pullout testing and performance evaluation of GFRP soil nails. J. Geotech. Geoenviron. Eng. 2011, 137, 633–642. [Google Scholar] [CrossRef] [Scilit]
- Zeng, J.J.; Sun, H.Q.; Deng, R.B.; Yan, Z.T.; Zhuge, Y. Bond performance between FRP bars and 3D-printed high-performance concrete. Structures 2025, 73, 108377. [Google Scholar] [CrossRef] [Scilit]
- Zhou, J.K.; Hao, Z.H.; Zeng, J.J.; Feng, S.Z.; Liang, Q.J.; Zhao, B.; Feng, R.; Zhuge, Y. Durability assessment of GFRP bars embedded in UHP-ECCs subjected to an accelerated aging environment with sustained loading. Constr. Build. Mater. 2024, 419, 135364. [Google Scholar] [CrossRef] [Scilit]
- Sim, J.; Park, C.; Moon, D.Y. Characteristics of basalt fiber as a strengthening material for concrete structures. Compos. Part B Eng. 2005, 36, 504–512. [Google Scholar] [CrossRef] [Scilit]
- Zhao, W.; Wang, H.; Chen, Y.; Hu, Y. Laboratory and field tests use of bfrp anchor bolt in supporting soil slope. J. Eng. Geol. 2021, 24, 1008–1015. [Google Scholar]
- Fiore, V.; Scalici, T.; Di Bella, G.; Valenza, A. A review on basalt fibre and its composites. Compos. Part B Eng. 2015, 74, 74–94. [Google Scholar] [CrossRef] [Scilit]
- Dong, Z.Q.; Wu, G.; Zhao, X.L.; Lian, J.L. Long-term bond durability of fiber-reinforced polymer bars embedded in seawater sea-sand concrete under ocean environments. J. Compos. Constr. 2018, 22, 04018042. [Google Scholar] [CrossRef] [Scilit]
- Zeng, J.J.; Liao, J.; Zhuge, Y.; Guo, Y.C.; Zhou, J.K.; Huang, Z.H.; Zhang, L. Bond behavior between GFRP bars and seawater sea-sand fiber-reinforced ultra-high strength concrete. Eng. Struct. 2022, 254, 113787. [Google Scholar] [CrossRef] [Scilit]
- Hussain, S.; Khan, M.Z.N.; Khan, H.A. Bond performance of basalt FRP bar against aggressive environment in high-strength concrete with varying bar diameter and bond length. Constr. Build. Mater. 2022, 349, 128779. [Google Scholar] [CrossRef] [Scilit]
- Wang, X.; Su, C.; Deng, W.; Wu, Z. Bond behavior between corrugated BFRP shell and concrete under monotonic and cyclic loads. Constr. Build. Mater. 2019, 210, 596–606. [Google Scholar] [CrossRef] [Scilit]
- Shen, D.; Li, C.; Feng, Z.; Wen, C.; Ojha, B. Influence of strain rate on bond behavior of concrete members reinforced with basalt fiber-reinforced polymer rebars. Constr. Build. Mater. 2019, 228, 116755. [Google Scholar] [CrossRef] [Scilit]
- Yang, Y.; Li, Z.; Zhang, T.; Wei, J.; Yu, Q. Bond-slip behavior of basalt fiber reinforced polymer bar in concrete subjected to simulated marine environment: Effects of BFRP bar size, corrosion age, and concrete strength. Int. J. Polym. Sci. 2017, 2017, 5156189. [Google Scholar] [CrossRef] [Scilit]
- Bai, X.; Ma, H.; Yan, N.; Wang, F.; Hou, D.; Wang, P.; Sun, G.; Xu, F. Anchorage performance of BFRP anti-floating anchors: Field investigation and numerical simulation. Case Stud. Constr. Mater. 2025, 23, e04903. [Google Scholar] [CrossRef] [Scilit]
- Elgabbas, F.; Ahmed, E.A.; Benmokrane, B. Physical and mechanical characteristics of new basalt-FRP bars for reinforcing concrete structures. Constr. Build. Mater. 2015, 95, 623–635. [Google Scholar] [CrossRef] [Scilit]
- Dai, Z.; Zhou, S.; Yin, Y.; Fu, X.; Zhang, Y.; Guo, J.; Du, Z.; Tao, Y.; Wu, X. Experimental study on the mechanical properties and failure modes of BFRP bar anchor systems under static tension loading. Front. Earth Sci. 2023, 11, 1106920. [Google Scholar] [CrossRef] [Scilit]
- Bai, X.; Jing, D.; Wang, H.; Zhang, M.; Jia, Y.; Yan, N. Field test of interface bonding performance of GFRP anti-floating anchors. Chin. J. Rock Mech. Eng. 2022, 41, 748–763. [Google Scholar]
- Sun, G.; Yan, N.; Bai, X.; Liu, J.; Hou, D.; Sang, S.; Zhang, M.; Wang, P.; Jing, D. Laboratory full-scale test on the bond property of GFRP anchor to concrete. Constr. Build. Mater. 2023, 396, 132216. [Google Scholar] [CrossRef] [Scilit]
- Bai, X.; Zhao, X.; Yan, N.; Sun, G.; Hou, D.; Liu, J. Field test of GFRP bar anti-floating anchor slurry-rock interface bonding performance. Compos. Struct. 2024, 331, 117893. [Google Scholar] [CrossRef] [Scilit]
- Grindheim, B.; Li, C.C.; Høien, A.H. Full-scale pullout tests of rock anchors in a limestone quarry focusing on bond failure at the anchor-grout and grout-rock interfaces. J. Rock Mech. Geotech. Eng. 2023, 15, 2264–2279. [Google Scholar] [CrossRef] [Scilit]
- Ren, F.F.; Yang, Z.J.; Chen, J.F.; Chen, W.W. An analytical analysis of the full-range behaviour of grouted rockbolts based on a tri-linear bond-slip model. Constr. Build. Mater. 2010, 24, 361–370. [Google Scholar] [CrossRef] [Scilit]
- Kuang, Z.; Zhang, M.; Bai, X.; Wang, Y.H.; Yan, N.; Zhu, L. Field tests on mechanics and deformation properties of GFRP anti-floating anchors in decomposed rock foundation. Chin. J. Geotech. Eng. 2019, 41, 1882–1892. [Google Scholar]
- Meng, F.; Chen, W.; Sun, H.; Wang, D.; Xie, T.; Fan, P. Bond-slip test and constitutive model between BFRP barwith anchorage and concrete. Eng. Mech. 2023, 40, 171–184. [Google Scholar]
- Achillides, Z.; Pilakoutas, K. Bond behavior of fiber reinforced polymer bars under direct pullout conditions. J. Compos. Constr. 2004, 8, 173–181. [Google Scholar] [CrossRef] [Scilit]
- Okelo, R.; Yuan, R.L. Bond strength of fiber reinforced polymer rebars in normal strength concrete. J. Compos. Constr. 2005, 9, 203–213. [Google Scholar] [CrossRef] [Scilit]
- Baena, M.; Torres, L.; Turon, A.; Barris, C. Experimental study of bond behaviour between concrete and FRP bars using a pull-out test. Compos. Part B Eng. 2009, 40, 784–797. [Google Scholar] [CrossRef] [Scilit]
- Martín, L.B.; Tijani, M.; Hadj-Hassen, F. A new analytical solution to the mechanical behaviour of fully grouted rockbolts subjected to pull-out tests. Constr. Build. Mater. 2011, 25, 749–755. [Google Scholar] [CrossRef] [Scilit]
- Hyett, A.; Bawden, W.; Reichert, R. The effect of rock mass confinement on the bond strength of fully grouted cable bolts. Int. J. Rock Mech. Min. Sci. Geomech. Abstr. 1992, 29, 503–524. [Google Scholar] [CrossRef] [Scilit]
- Hyett, A.J.; Moosavi, M.; Bawden, W.F. Load distribution along fully grouted bolts, with emphasis on cable bolt reinforcement. Int. J. Numer. Anal. Methods Geomech. 1996, 20, 517–544. [Google Scholar] [CrossRef] [Scilit]
- Dong, Z.; Wu, G.; Zhao, X.-L.; Wang, Z.-K. A refined prediction method for the long-term performance of BFRP bars serviced in field environments. Constr. Build. Mater. 2017, 155, 1072–1080. [Google Scholar] [CrossRef] [Scilit]
- Wang, H.; Sun, X.; Peng, G.; Luo, Y.; Ying, Q. Experimental study on bond behaviour between BFRP bar and engineered cementitious composite. Constr. Build. Mater. 2015, 95, 448–456. [Google Scholar] [CrossRef] [Scilit]
- Feng, J.; Lai, B.; Zhang, S.; Wang, D.; Liu, Y. Laboratory pull-out test study of basalt fiber reinforced polymer bolt for strengthening mixed soil. J. Southwest Jiaotong Univ. 2022, 57, 1193–1200. [Google Scholar]
- Feng, J.; Wang, Y.; Wu, H.; Lai, B.; Xie, D. Field pullout tests of basalt fiber-reinforced polymer ground anchor. Rock Soil Mech. 2019, 40, 2563–2573. [Google Scholar]
- Ma, S.; Nemcik, J.; Aziz, N. An analytical model of fully grouted rock bolts subjected to tensile load. Constr. Build. Mater. 2013, 49, 519–526. [Google Scholar] [CrossRef] [Scilit]
- He, L.; An, X.M.; Zhao, Z. Fully grouted rock bolts: An analytical investigation. Rock Mech. Rock Eng. 2015, 48, 1181–1196. [Google Scholar] [CrossRef] [Scilit]
- Vlachopoulos, N.; Cruz, D.; Forbes, B. Utilizing a novel fiber optic technology to capture the axial responses of fully grouted rock bolts. J. Rock Mech. Geotech. Eng. 2018, 10, 222–235. [Google Scholar] [CrossRef] [Scilit]
- Benmokrane, B.; Chekired, M.; Xu, H. Monitoring behavior of grouted anchors using vibrating-wire gauges. J. Geotech. Eng. 1995, 121, 466–475. [Google Scholar] [CrossRef] [Scilit]
- Zhang, M.-Y.; Kuang, Z.; Bai, X.-Y.; Chen, X.-Y. Pullout behavior of GFRP anti-floating anchor based on the FBG sensor technology. Math. Probl. Eng. 2018, 2018, 6424791. [Google Scholar] [CrossRef] [Scilit]
- Chen, W.; Hong, C.; Chen, X.; Luo, G.; Su, D. Comparative analysis of anchor cables in pullout tests using distributed fiber optic sensors. Can. Geotech. J. 2023, 60, 1861–1876. [Google Scholar] [CrossRef] [Scilit]
- Nemcik, J.; Ma, S.; Aziz, N.; Ren, T.; Geng, X. Numerical modelling of failure propagation in fully grouted rock bolts subjected to tensile load. Int. J. Rock Mech. Min. Sci. 2014, 71, 293–300. [Google Scholar] [CrossRef] [Scilit]
- Rong, G.; Zhu, H.; Zhou, C. Testing study on working mechanism of fully grouted bolts of thread steel and smooth steel. Chin. J. Rock Mech. Eng. 2004, 23, 469–475. [Google Scholar]
- Ghadimi, M.; Shahriar, K.; Jalalifar, H. An analytical model to predict shear stress distribution in fully grouted rock bolts. Geotech. Geol. Eng. 2015, 33, 59–68. [Google Scholar] [CrossRef] [Scilit][Green Version]
- Zhang, S.; Wang, C.; Wang, G.; Wu, X.; Zheng, X.; He, P.; Xu, F. Experimental study on the shear behaviors of bolted rock joints reinforced with BFRP bars. Chin. J. Rock Mech. Eng. 2022, 41, 712–724. [Google Scholar]
- Høien, A.H.; Li, C.C.; Zhang, N. Pull-out and critical embedment length of grouted rebar rock bolts-mechanisms when approaching and reaching the ultimate load. Rock Mech. Rock Eng. 2021, 54, 1431–1447. [Google Scholar] [CrossRef] [Scilit]
- Li, C.C.; Kristjansson, G.; Høien, A.H. Critical embedment length and bond strength of fully encapsulated rebar rockbolts. Tunn. Undergr. Space Technol. 2016, 59, 16–23. [Google Scholar] [CrossRef] [Scilit]
- Tighiouart, B.; Benmokrane, B.; Gao, D. Investigation of bond in concrete member with fibre reinforced polymer bars. Constr. Build. Mater. 1998, 12, 453–462. [Google Scholar] [CrossRef] [Scilit]
- Zou, J.; Zhang, P. Analytical model of fully grouted bolts in pull-out tests and in situ rock masses. Int. J. Rock Mech. Min. Sci. 2019, 113, 278–294. [Google Scholar] [CrossRef] [Scilit]
- Zhang, W.; Huang, L.; Juang, C.H. An analytical model for estimating the force and displacement of fully grouted rock bolts. Comput. Geotech. 2020, 117, 103222. [Google Scholar] [CrossRef] [Scilit]
- Wang, L.; Yuan, C.; Huang, D.; Deng, X.; Gu, J. Experimental Investigation of Bond Behavior between Basalt Fiber Reinforced Polymer Bars and Coral Aggregate Concrete under Different Loading Rates. J. Build. Eng. 2026, 116901. [Google Scholar] [CrossRef] [Scilit]
- Ghadimi, M.; Shahriar, K.; Jalalifar, H. Optimization of the fully grouted rock bolts for load transfer enhancement. Int. J. Min. Sci. Technol. 2015, 25, 707–712. [Google Scholar] [CrossRef] [Scilit]
- Cao, C.; Ren, T.; Cook, C.; Cao, Y. Analytical approach in optimising selection of rebar bolts in preventing rock bolting failure. Int. J. Rock Mech. Min. Sci. 2014, 72, 16–25. [Google Scholar] [CrossRef] [Scilit]
- Xu, C.; Li, Z.; Wang, S.; Wang, S.; Fu, L.; Tang, C. Pullout performances of grouted rockbolt systems with bond defects. Rock Mech. Rock Eng. 2018, 51, 861–871. [Google Scholar] [CrossRef] [Scilit]
- Chen, J.; Saydam, S.; Hagan, P.C. Numerical simulation of the pull-out behaviour of fully grouted cable bolts. Constr. Build. Mater. 2018, 191, 1148–1158. [Google Scholar] [CrossRef] [Scilit]
- Serbescu, A.; Guadagnini, M.; Pilakoutas, K. Mechanical characterization of basalt FRP rebars and long-term strength predictive model. J. Compos. Constr. 2015, 19, 04014037. [Google Scholar] [CrossRef] [Scilit]
- El Refai, A.; Ammar, M.A.; Masmoudi, R. Bond performance of basalt fiber-reinforced polymer bars to concrete. J. Compos. Constr. 2015, 19, 04014050. [Google Scholar] [CrossRef] [Scilit]
- Giot, R.; Auvray, C.; Raude, S.; Giraud, A. Experimental and numerical analysis of in situ pull-out tests on rock bolts in claystones. Eur. J. Environ. Civ. Eng. 2021, 25, 2277–2300. [Google Scholar] [CrossRef] [Scilit]
- Tistel, J.; Grimstad, G.; Eiksund, G. Testing and modeling of cyclically loaded rock anchors. J. Rock Mech. Geotech. Eng. 2017, 9, 1010–1030. [Google Scholar] [CrossRef] [Scilit]
- Oh, B.H.; Kim, S.H. Realistic models for local bond stress-slip of reinforced concrete under repeated loading. J. Struct. Eng. 2007, 133, 216–224. [Google Scholar] [CrossRef] [Scilit]
- Wu, Z.K.; Bai, X.Y.; Sun, G.; Wang, F.J.; Yan, N.; Dong, X.G. Field test of anchorage performance of BFRP anti-floating anchors under multiple cyclic loads. Chin. J. Rock Mech. Eng. 2024, 43, 2314–2328. [Google Scholar]
- Benmokrane, B.; Chekired, M.; Xu, H.; Ballivy, G. Behaviour of grouted anchors subjected to repeated loadings in field. J. Geotech. Eng. 1995, 121, 413–420. [Google Scholar] [CrossRef] [Scilit]
- Bai, X.; Zheng, C.; Zhang, M.Y.; Wang, Y.H.; Wang, H.G. Creep tests and standard linear solid model for large-diameter glass fiber-reinforced polymer anti-floating anchors. Chin. J. Geotech. Eng. 2020, 42, 1304–1311. [Google Scholar]
- Vilanova, I.; Baena, M.; Torres, L.; Barris, C. Experimental study of bond-slip of GFRP bars in concrete under sustained loads. Compos. Part B Eng. 2015, 74, 42–52. [Google Scholar] [CrossRef] [Scilit]
- Feng, J.; Wang, R.; Zhang, Y.; Tu, Z.; Yang, T. Examining the creep characteristics of basalt fiber-reinforced polymer grouted bolts in mixed soil. Int. J. Geomech. 2023, 23, 04023164. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.