Effects of Local Stirrup Deficiency on Load-Bearing Performance and Crack Evolution in GFRP-Strengthened RC Beams

,
,
,
,
and
School of Civil Engineering, Chongqing Jiaotong University, Chongqing 400074, China
*
Author to whom correspondence should be addressed.

Abstract

To address the problem of local stirrup deficiency in existing reinforced concrete (RC) beams, three-point bending tests were conducted on glass fiber-reinforced polymer (GFRP)-strengthened beams. A total of 16 specimens in 8 groups were designed to comparatively investigate the bearing capacity, load–deflection curve characteristics, ductility and crack evolution of specimens with two stirrup configurations, i.e., full-length uniformly distributed stirrups and a 300 mm mid-span stirrup-deficient zone, under 0 to 3 GFRP layers. The results indicate that mid-span stirrup deficiency significantly impairs the strengthening efficiency of GFRP. Compared with stirrup-deficient beams, beams with full-length stirrups exhibit 6.1–15.1% higher ultimate bearing capacity; they better enable multi-layer GFRP to exert its strengthening efficiency, with more remarkable improvement in sectional stiffness and a gentler post-peak descending branch. The deterioration effect of stirrup absence on ductility is evident, and beams with full-length stirrups show a 6.6–18.1% higher ductility coefficient. This study reveals the synergistic mechanism between stirrups and GFRP. For beams with full-length stirrups, GFRP delivers superior crack confinement performance on major cracks and results in more uniform crack distribution, while stirrup-deficient beams exhibit larger crack widths and non-uniform crack distribution.

1. Introduction

Owing to its convenient construction, favorable corrosion resistance and excellent mechanical properties, externally bonded fiber-reinforced polymer (FRP) strengthening has emerged as a mainstream technique for enhancing the flexural performance of existing reinforced concrete (RC) structures [1,2,3]. Extensive studies have been carried out worldwide on the flexural behavior of FRP-strengthened RC beams, covering material selection, strengthening processes, mechanical mechanisms and service life assessment, forming a relatively well-established theoretical and technical framework [4,5,6,7,8]. In engineering practice, carbon fiber-reinforced polymer (CFRP) is widely utilized for strengthening critical load-bearing members due to its high strength and high elastic modulus [9,10,11,12]. By contrast, glass fiber-reinforced polymer (GFRP), with the merits of low cost, favorable ductility compatibility and outstanding fatigue resistance, has gradually demonstrated remarkable cost-effectiveness in strengthening a wide range of low-stirrup-ratio members, including municipal secondary beams, industrial workshop floor slabs and aged civil building components, with satisfactory engineering performance [13,14].
In addition to conventional externally bonded (EB) strengthening, various advanced strengthening configurations have been developed in academia, including near-surface mounted (NSM) FRP, FRP grid-reinforced composite systems, and post-tensioned FRP. Extensive studies have also been carried out on scenarios such as internal GFRP bar reinforcement, hybrid reinforcement systems, and FRP-confined compression zones, further broadening the application scope of FRP strengthening technology [15,16,17,18,19].
Meanwhile, the strengthening performance under extreme service conditions has attracted widespread research attention, covering post-high-temperature mechanical behavior, mechanical response under fire exposure, and performance under impact loads, which has refined the strengthening design theory applicable to diverse service environments [20,21,22,23,24,25]. In terms of performance evaluation and prediction, apart from traditional experimental and theoretical models, intelligent methods such as symbolic regression and machine learning have been adopted to predict the bearing capacity and crack width of FRP-strengthened beams, providing novel analytical tools for engineering design [26].
Most existing studies and engineering design practices typically assume that strengthened beams are equipped with intact transverse stirrup configurations. Nevertheless, in engineering practice, numerous early-built RC beams are subject to low initial design standards, construction quality defects and long-term corrosion and thus commonly suffer from inadequate stirrup reinforcement, excessive stirrup spacing and even local stirrup deficiency in mid-span flexure-governed zones [27,28,29]. As the mid-span region is generally governed by normal-section flexure, the confinement effect of transverse stirrups has long been underestimated. Meanwhile, owing to its lower elastic modulus compared with CFRP, the interfacial bond performance of GFRP is more sensitive to substrate crack defects. Accordingly, the influence mechanism of stirrup deficiency on the bearing performance and crack evolution of GFRP-strengthened beams cannot be directly extrapolated from established findings for CFRP-strengthened beams. The direct adoption of conventional strengthening design approaches may therefore lead to overestimation of the bearing capacity and crack control effect [30].
Extensive systematic studies have been conducted worldwide on the flexural behavior of externally bonded (EB) FRP-strengthened RC beams, forming a well-established theoretical framework centered on interfacial debonding failure mechanisms, load-bearing capacity calculation methods and crack control theories. Based on a large body of experimental data, Teng et al. developed a classical calculation model for intermediate crack-induced (IC) debonding in FRP-strengthened RC beams and clarified the distribution characteristics and governing parameters of interfacial bond stress. This model has served as a core theoretical cornerstone in this research field [31]. Previous bending tests have further demonstrated that transverse stirrups can effectively redistribute FRP-concrete interfacial shear stress by restraining crack opening displacement (COD), thereby improving the ultimate load-bearing capacity and ductility of strengthened beams [32,33,34]. With respect to the influence of stirrup configuration, the existing literature mainly focuses on two scenarios. The first is the shear and flexural performance of FRP-strengthened beams with no web reinforcement along the full span, with particular attention paid to failure mode transition and load-bearing capacity degradation under stirrup-free conditions [35]. The second investigates the effect of stirrup deficiency or corrosion in the shear span on the shear performance of strengthened beams, aiming to evaluate the risk of diagonal section failure and propose corresponding strengthening countermeasures [36,37,38]. However, for the commonly encountered engineering scenario of local stirrup deficiency in the mid-span region, most existing experiments adopt four-point bending loading to form a uniform pure bending zone. In contrast, a large number of in-service members, including simply supported secondary beams, pedestrian trestles and culvert slabs, are typically subjected to concentrated loading at the mid-span. The bending moment of such members follows a triangular distribution peaking at the mid-span, which aligns with the three-point bending loading regime. Under this loading configuration, the peak bending moment coincides exactly with the locally stirrup-deficient segment, creating an unfavorable stress state that is more conducive to elucidating the influence mechanism of stirrup deficiency on strengthening performance [39]. Accordingly, experimental results derived exclusively from four-point bending tests may not fully capture the actual mechanical behavior of such members in practical engineering. Notably, beams with full-length web reinforcement deficiency and beams with local mid-span stirrup deficiency exhibit distinctly different failure mechanisms. For the former, cracks are randomly distributed along the entire span, with pronounced combined stress characteristics in the shear-bending zone. For the latter, cracks are highly concentrated in the mid-span region with the maximum bending moment, which readily induces abrupt local interfacial stress variations. Therefore, research conclusions obtained from full-length web-reinforcement-free beams cannot be directly extrapolated to beams with local mid-span stirrup deficiency [23].
Furthermore, although stirrups in the mid-span region primarily function to confine flexural cracks and do not directly govern the diagonal section shear capacity, they can modulate sectional stress distribution through multiple mechanisms: restraining the transverse deformation of concrete, engaging a wider range of concrete matrix in tension via bond confinement, limiting crack width and promoting crack dispersion. These effects further influence the interfacial bond performance between FRP and concrete, as well as the material utilization efficiency of FRP. Ceroni and Pecce reported that appropriate reinforcement detailing can markedly optimize the distribution of crack spacing and width in FRP-strengthened beams, thus improving their serviceability-limit-state performance [40]. Yost et al. also found that stirrups can alleviate stress concentration at FRP ends through the crack redistribution effect, thereby delaying the initiation of debonding failure [41]. However, the above findings are mostly derived from four-point bending tests under uniform moment conditions. Under the concentrated moment profile of three-point bending, there remains no consensus on quantitative conclusions regarding whether local mid-span stirrup deficiency triggers rapid crack concentration, whether the dominant crack width exceeds code-specified limits, the risk of interfacial debonding rises significantly, and how these effects evolve with an increasing number of GFRP strengthening layers. Current domestic and international design codes for FRP strengthening also fail to provide explicit correction methods for load-bearing capacity and crack width targeting the scenario of local mid-span stirrup deficiency [42,43]. The scarcity of relevant experimental data has constrained the refined development of GFRP strengthening design for existing RC beams with stirrup defects [44,45,46].
To address the aforementioned research gaps, stirrup deficiency in engineering practice—commonly resulting from construction omissions, design modifications, stirrup corrosion, or updated seismic codes—is frequently encountered in the retrofitting of existing buildings. This paper presents an experimental investigation into the flexural performance of GFRP-strengthened RC beams with local mid-span stirrup deficiency under three-point bending loading. Two stirrup reinforcement configurations are designed for the specimens: full-length uniformly distributed stirrups and local stirrup deficiency in the mid-span region, combined with externally bonded GFRP strengthening schemes of 1 to 3 layers [47,48,49,50]. During the stepwise loading procedure, full-range data of load, displacement and strain are acquired, and the evolution of crack distribution, dominant crack width and secondary crack propagation is continuously monitored. Comparative analysis is performed on the load–displacement response, ultimate load-bearing capacity, ductility coefficient and crack behavior of strengthened beams with different stirrup arrangements, to elucidate the influence mechanism of mid-span stirrup deficiency on crack evolution. The results quantitatively clarify the impact of local mid-span stirrup deficiency on the flexural performance of GFRP-strengthened beams. The degradation of sectional stiffness and ductility is found to be progressively exacerbated as the number of GFRP layers increases. This study refines the understanding of the synergistic mechanism between stirrup confinement and FRP strengthening. Specifically, an intact stirrup configuration can mitigate the stress transfer effect, homogenize crack propagation across the entire section, and yield a desirable cracking pattern characterized by multiple fine cracks with uniform dispersion. The findings provide experimental evidence and theoretical reference for the GFRP strengthening design and serviceability limit state assessment of existing RC beams with stirrup defects.

2. Experimental Program

2.1. Design and Fabrication of Test Beams

To investigate the regulatory effect of mid-span stirrup configuration on the flexural performance and crack evolution of GFRP (Haining Anjie Composite Material Co., Ltd., Jiaxing, China) -strengthened RC beams, two groups of specimens were designed with stirrup configuration as the primary test variable. The two groups differ exclusively in stirrup arrangement within the mid-span region, while all other design parameters remain fully consistent.
Two stirrup configuration schemes are adopted. The full-length stirrup group (Series S) serves as the fully confined reference case, with stirrups uniformly distributed at 50 mm intervals along the entire beam length. For the local mid-span stirrup deficiency group (Series N), stirrups are omitted only in the symmetric 300 mm mid-span zone governed by the maximum bending moment, while the stirrup size and spacing in the remaining regions are identical to those of Series S.
All specimens share an identical baseline design: Grade C30 concrete is used; the tensile longitudinal reinforcement consists of two 10 mm-diameter HRB335 deformed bars, corresponding to a reinforcement ratio of 1.21% and falling within the under-reinforced beam category; both erection bars and stirrups are fabricated from 6 mm-diameter HPB300 plain round steel bars. However, due to constraints in experimental conditions and casting batches, the two groups of beams were cast in two separate pours.
Verification of diagonal section shear capacity confirms that the provided stirrups can effectively prevent shear failure in the test beams, ensuring that normal-section flexure acts as the governing failure mode for all specimens. Shear capacity checks yield 13.5 kN for the stirrup-deficient zone and 54.7 kN for the fully stirruped zone, both exceeding the maximum shear demand (≈11.7 kN) at the flexural capacity (Mu = 5.59 kN·m). This ensures that shear failure does not occur prior to flexural yielding, consistent with the “strong shear–weak bending” design principle. This provides a controlled experimental baseline for performance comparison across different GFRP strengthening schemes. The key material properties are summarized in Table 1, Table 2 and Table 3, and the detailed dimensions and reinforcement layout of the test beams are illustrated in Figure 1.
Table 1. Mechanical properties of concrete.
Table 2. Mechanical properties of steel bars.
Table 3. Tensile properties of GFRP sheets.
Figure 1. Reinforcement details of test beams. (a) Reinforcement layout and sectional dimensions of the RC beam with full-length stirrups (Series S). (b) Reinforcement layout and sectional dimensions of the RC beam with local mid-span stirrup deficiency (Series N). (c) Assembly details of the steel reinforcement cage for Series S. (d) Assembly details of the steel reinforcement cage for Series N. (All dimensions are in mm).
A total of 16 RC beams were designed for the test. The specimen designation, group assignment and structural details are summarized in Table 4, and the strengthening schemes are illustrated in Figure 2.
Table 4. Comparison of different strengthening schemes of test beams.
Figure 2. Schematic diagram of strengthening schemes for test beams (units: mm).
The casting process of the RC test beams is illustrated in Figure 3. Upon completion of concrete curing, GFRP sheets were bonded to the beam soffits. The bonding procedure was performed in accordance with the provisions of relevant technical specifications [47,50], and the bonding process is illustrated in Figure 4. The GFRP-strengthened RC beams were subsequently cured at ambient temperature for 7 days [50]. Loading tests were conducted once the bonding adhesive achieved full curing.
Figure 3. Fabrication of test beams.
Figure 4. GFRP bonding process of test beams.

2.2. Loading Scheme and Test Procedure

A three-point simply supported static bending loading scheme was adopted in the test [51]. The loading setup consists of a reaction frame, a manual hydraulic jack, a load-stabilizing spring and a load cell, with a concentrated load applied at the midpoint of the beam’s calculated span. To observe crack propagation and analyze the evolution of failure modes, a stepwise loading protocol with load holding was implemented [52]. After each load level stabilized, the load and mid-span deflection data were automatically and synchronously collected by a data acquisition system. The system continuously recorded the relevant data throughout the test at a sampling rate of 10 Hz. Crack width was measured using a handheld crack width gauge, and the crack distribution and development patterns were recorded simultaneously. The overall loading arrangement is illustrated in Figure 5 and Figure 6.
Figure 5. Schematic of three-point simply supported bending loading (units: mm).
Figure 6. Photograph of the loading test setup.
A total of 16 specimens across 8 groups were tested in accordance with the predefined loading protocol. The test results are analyzed and discussed in the following sections.

3. Test Results and Analysis

3.1. Comparison of Bearing Capacity Indices and Stiffness

Table 5 summarizes the average characteristic loads of all specimen groups. Based on the table, the effects of stirrup arrangement and GFRP ply count on the load-bearing performance of RC beams are systematically analyzed. Externally bonded GFRP effectively enhances the cracking, yield and ultimate flexural capacities of RC beams, with the enhancement ratio rising monotonically with increasing GFRP plies. The mid-span stirrup configuration exerts a pronounced governing effect on strengthening efficiency.
Table 5. Bearing capacity data of test beams with different strengthening forms.
As evident from Table 5, GFRP strengthening yields an increase in cracking load for both Series S and Series N specimens.
In terms of yield load, the unstrengthened beam in Series S attains a value 5.6% higher than its counterpart in Series N. For specimens strengthened with 1 to 3 GFRP plies, the yield load of Series S increases by 42.1%, 50.9% and 59.6% respectively relative to the corresponding unstrengthened beam, compared with increments of 37.0%, 42.6% and 53.7% for Series N. This finding suggests that full-length stirrups can disperse interfacial shear stress at crack locations, improve FRP stress transfer efficiency, and establish a well-coordinated dual confinement system with GFRP. The two components jointly suppress lateral concrete expansion, thereby retarding the progression of plastic yielding in longitudinal reinforcement. Consequently, beams with full stirrup configuration achieve a more pronounced yield flexural capacity gain at an identical GFRP ply count.
Regarding ultimate load, the unstrengthened Series S beam outperforms its Series N counterpart by 6.1%, which is attributed to the lateral confinement effect of stirrups on concrete in the compression zone. With GFRP strengthening, the ultimate flexural capacity enhancement ranges from 37.1% to 52.9% for Series S and 31.8% to 40.9% for Series N. A more significant ultimate capacity gain is observed for beams with full stirrup configuration at equivalent GFRP ply numbers; however, the marginal enhancement diminishes progressively as GFRP ply count increases. Consistent observations have been documented in four-point bending investigations [31,33].
Based on the measured GFRP strain data in Table 5, the single-ply ultimate stress and strength utilization ratio decrease progressively with increasing GFRP ply count, with values ranging only from 28% to 50%. At an identical ply count, the S series outperforms the N series in both ultimate stress and strength utilization ratio, indicating more efficient GFRP material utilization in fully stirruped beams. In particular, specimen N-RC-G-3 exhibits a strength utilization ratio of only 28.0%, suggesting that stirrup deficiency and interfacial bonding issues render mere accumulation of externally bonded plies wasteful.
It should be noted that, owing to variability in strain gauge quality, bonding process variations, and systematic loading errors, all GFRP strain gauges failed prior to the ultimate load. Accordingly, the measured strains in Table 5 are lower than the true values at the ultimate state, and with gauge failure times varying across specimens, the derived stresses, tensile forces, and strength utilization ratios are subject to certain errors. Nevertheless, these data serve as a reference for evaluating GFRP material utilization and qualitatively comparing strength utilization between fully stirruped and locally stirrup-deficient beams.
Figure 7 and Figure 8 present the load–deflection curves of all test beams. The mechanical response of each specimen exhibits three distinct behavioral stages: elastic stage, cracked stage, and post-yield failure stage. GFRP strengthening and stirrup configuration primarily govern the post-cracking stiffness degradation rate and post-yield deformation characteristics.
Figure 7. Load–deflection curves of beams with two stirrup configurations at identical GFRP ply counts: (a) unstrengthened beams, (b) beams with 1 GFRP ply, (c) beams with 2 GFRP plies, (d) beams with 3 GFRP plies.
Figure 8. Load–deflection curves of test beams grouped by stirrup configuration series: (a) Series S, (b) Series N.
In the elastic stage, all specimen groups exhibit comparable curve slopes and negligible differences in initial stiffness. Sectional stiffness is primarily governed by the concrete matrix, while the contributions of GFRP and stirrups remain insignificant.
In the cracked stage, a marked reduction in sectional stiffness occurs following concrete cracking. Higher GFRP ply counts correspond to stronger sectional stiffness retention and slower stiffness degradation. Taking the secant stiffness at a mid-span deflection of 5 mm as the quantitative index, specimens strengthened with 1, 2 and 3 GFRP plies in Series S exhibit 22%, 35% and 46% higher stiffness than the corresponding control beam S-RC, respectively, while in Series N, the stiffness of 1-, 2- and 3-ply strengthened specimens is increased by 19%, 30% and 40% respectively relative to the control beam N-RC. At an identical GFRP ply count, Series S consistently maintains higher secant stiffness than Series N, with a stable stiffness difference of 10–15%, indicating that stirrups effectively mitigate post-cracking stiffness degradation by restricting crack mouth opening displacement and preserving interfacial bond integrity.
In the post-yield stage, Series N specimens exhibit a steeper descending branch and more rapid capacity degradation in their load–deflection curves. This demonstrates that mid-span stirrup deficiency exacerbates the brittle behavior of members after yielding and substantially reduces plastic deformation capacity. Analogous results have been reported in four-point bending studies [45].
Overall, Series S beams with full stirrup configuration outperform Series N counterparts with the same GFRP ply count in load-bearing performance across nearly the entire loading process from yielding to ultimate failure. An intact stirrup configuration is a critical prerequisite for maximizing GFRP strengthening efficiency and maintaining adequate ductility reserve in structural members.

3.2. Comparison of Ductility Coefficients

The deflection ductility coefficient is a critical index for quantifying the plastic deformation capacity and failure warning capability of members. In this study, the ductility coefficient is defined as:
μΔ = Δu/Δy
where Δu is the ultimate deflection and Δy is the equivalent yield deflection. Specifically, Δy corresponds to the mid-span deflection at which the tensile longitudinal reinforcement attains its yield strength. Δu is taken as the mid-span deflection at which the applied load decays to 85% of the peak load on the descending branch. Table 6 summarizes the ductility indices of test beams with varying stirrup configurations and GFRP ply counts [29,45,53].
Table 6. Comparison of displacement ductility coefficients.
As shown in Table 6, the unstrengthened specimens have ductility coefficients of 3.56 for Series S and 3.34 for Series N, representing a 6.6% relative improvement for Series S. With increasing GFRP ply count, the ductility of both series declines consistently. However, at an identical GFRP ply count, Series S consistently outperforms Series N in ductility coefficient, and the disparity between the two series widens progressively as ply count rises. Specifically, the relative increment of Series S over Series N reaches 7.6% at 1 GFRP ply, 10.7% at 2 plies, and 18.1% at 3 plies. This demonstrates that the adverse effect of local mid-span stirrup deficiency on ductility is progressively amplified with increasing GFRP ply count.

3.3. Comparison of Crack Evolution Characteristics

3.3.1. Crack Patterns at Failure for Two Stirrup Configuration

All specimens were observed to fail with tensile steel yielding as the precursor. After steel yielding, continued loading induced GFRP strain concentration at the major flexural crack, where partial fiber bundles ruptured upon reaching their ultimate tensile strength; the rupture propagated along the sheet with longitudinal splitting until the beam lost its load-bearing capacity. A few specimens exhibited interfacial debonding initiating from flexural cracks, followed by partial GFRP rupture or longitudinal splitting. The failure process remained essentially flexure-controlled, with GFRP rupture and IC debonding representing secondary phenomena that occurred after steel yielding as the GFRP assumed a larger share of the tensile load. Accordingly, the failure mode is classified as a flexure-dominated hybrid failure mode.
As shown in Figure 9, when all test beams reach the critical failure state, the width of the major crack at the mid-span soffit decreases progressively with increasing GFRP ply count for both Series S and Series N; this is further illustrated in Section 3.3.2. As summarized in Table 7, at an identical GFRP ply count, beams in Series S develop more cracks with smaller individual widths than those in Series N (see Figure 9), indicating that the presence of full stirrups improves the overall deformation compatibility of the beam and promotes a more uniform crack distribution.
Figure 9. Crack patterns of test beams at ultimate failure. (a) S-RC; (b) N-RC; (c) S-RC-G-1; (d) N-RC-G-1; (e) S-RC-G-2; (f) N-RC-G-2; (g) S-RC-G-3; (h) N-RC-G-3.
Table 7. Summary of the number of cracks for all test beams.
Moreover, with increasing GFRP plies, the inclined cracks in the N-series (stirrup-deficient) beams became progressively more pronounced, suggesting a tendency toward diagonal tension failure; in contrast, no such trend was observed in the S-series (fully stirruped) beams, indicating that adequate stirrup configuration effectively suppresses inclined crack development and maintains a flexure-controlled failure mode. These failure mode characteristics are consistent with the ductility analysis in Section 3.2.

3.3.2. Comparison of Mid-Span Major Crack Widths for Test Beams

Figure 10a and Figure 10b present the variation in mid-span major crack width with applied load for Series S and Series N beams with varying GFRP ply counts, respectively.
Figure 10. Curves of applied load versus major crack width at the tensile longitudinal reinforcement level for test beams: (a) Series S, (b) Series N.
As shown in Figure 10a, at an identical load level, the major crack width decreases markedly with increasing GFRP ply count, corresponding to a progressively enhanced crack resistance effect. The unstrengthened beams exhibit the fastest crack propagation rate, with a maximum crack width of 1.0 mm at the peak load. Under the same load condition, the crack widths of 1-, 2- and 3-ply strengthened beams are 0.22 mm, 0.17 mm and 0.09 mm, corresponding to 78%, 83% and 91% reductions respectively relative to the unstrengthened beam. For GFRP-strengthened specimens, all curves nearly coincide at the early loading stage. As the GFRP ply count rises, divergences emerge in crack width development: a higher ply count corresponds to a smaller crack width, indicating stronger crack confinement capacity of GFRP.
Comparison with Figure 10b reveals that the two series follow generally consistent trends. The unstrengthened beam in Series N reaches a crack width of 1.3 mm at the peak load, while those of 1-, 2- and 3-ply strengthened beams are 0.24 mm, 0.18 mm and 0.1 mm under the same load condition. The presence of GFRP can effectively restrain the width development of mid-span major cracks, and the confinement effect intensifies with increasing GFRP ply count. Overall, however, the developed crack width of Series S is consistently smaller than that of Series N. This demonstrates that the presence of full-length stirrup configuration can more effectively suppress the development of crack width.

4. Conclusions

Three-point bending tests were conducted on 16 RC beams across 8 groups, with identical geometric dimensions and longitudinal reinforcement ratios, two stirrup configurations (i.e., full-length stirrup arrangement and local mid-span stirrup deficiency), and strengthening with varying GFRP ply counts. The key conclusions are summarized as follows:
(1) Externally bonded GFRP effectively improves the cracking, yield and ultimate loads of RC beams with both stirrup configurations. Beams in Series S with full-length stirrup configuration outperform those in Series N with the same GFRP ply count in load-bearing performance at all loading stages. The yield and ultimate loads of the unstrengthened beam in Series S are 5.6% and 6.1% higher than those in Series N, respectively, which is attributed to the lateral confinement effect of stirrups on concrete in the compression zone. After strengthening with 1 to 3 plies of GFRP, the yield load increments in Series S specimens range from 42.1% to 59.6%, and the ultimate load increments range from 37.1% to 52.9%, both higher than those of Series N specimens with the same ply count. This demonstrates that beams with full-length stirrups can form a well-coordinated dual confinement system with GFRP, which synergistically restrains the lateral dilation of concrete and delays the plastic development of longitudinal steel reinforcement. This verifies that the integrity of stirrup configuration is a critical prerequisite for fully mobilizing the strengthening efficiency of GFRP.
(2) Test beams with full-length stirrups are more conducive to fully mobilizing the strengthening effectiveness of multi-ply GFRP, with a more pronounced improvement in sectional stiffness and a more gradual post-peak descending branch. The sectional stiffness rises with increasing GFRP ply count. Based on the secant stiffness at a mid-span deflection of 5 mm, the 1- to 3-ply strengthened beams in Series S show stiffness enhancements of 22–46% relative to the corresponding unstrengthened beam, while those in Series N exhibit improvements of 19–40% compared with their respective control beam. The stiffness difference between the two series remains stable at 10–15%. At an identical GFRP ply count, the stiffness of Series S is consistently greater than that of Series N.
(3) At an identical GFRP ply count, the ductility of Series S is superior to that of Series N, with an enhancement range of 6.6–18.1%. The ductility disparity between the two series widens progressively with increasing ply count. This indicates that the adverse effect of local mid-span stirrup deficiency on ductility is progressively amplified as the number of GFRP plies increases.
(4) Increasing the number of GFRP plies can effectively confine the width of mid-span major cracks. GFRP delivers a better confinement effect on major cracks in test beams with full-length stirrups, accompanied by a more uniform crack pattern. By contrast, beams with local mid-span stirrup deficiency exhibit larger crack widths and non-uniform crack distribution. At the peak load, the major crack width of Series S is 5.6–10% smaller than that of Series N.
(5) Limitations and future work: This study is limited to static three-point bending and does not address seismic loading or other reversed cyclic loading conditions, which are relevant to the design of RC beams and will be investigated in future work.
In summary, full-length stirrups can form a synergistic strengthening system with GFRP, fully mobilizing the strengthening efficiency of GFRP while preserving a reasonable ductility reserve of the members. Full stirrup configuration is a critical structural prerequisite for ensuring the load-bearing capacity and deformation reserve of FRP-strengthened members. In the case of stirrup deficiency, GFRP-strengthened beams exhibit degraded load-bearing capacity, stiffness and ductility, alongside weakened crack confinement capacity. In such cases, shear-enhancement measures such as externally bonded FRP U-wraps or side strips, steel plate bonding, and section enlargement with additional stirrups should be implemented. The test findings provide direct reference for the FRP strengthening design of weak segments with stirrup deficiency in existing structures.

Author Contributions

Conceptualization, T.Z. and Z.Y.; methodology, T.Z.; validation, T.Z.; formal analysis, T.Z.; investigation, T.Z., X.Z. and Z.W.; resources, Y.M.; data curation, Z.W. and N.R.; writing—original draft, T.Z.; writing—review & editing, T.Z., X.Z. and Z.Y.; supervision, Y.M.; project administration, T.Z.; funding acquisition, Z.Y. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Data Availability Statement

The data presented in this study are available on request from the corresponding author. The data are not publicly available due to [Data unavailable due to ongoing related research].

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Jahami, A.; Issa, C.A. An updated review on the effect of CFRP on flexural performance of reinforced concrete beams. Int. J. Concr. Struct. Mater. 2024, 18, 14. [Google Scholar] [CrossRef] [Scilit]
  2. Sengun, K.; Arslan, G. Performance of RC beams strengthened in flexure and shear with CFRP and GFRP. Iran. J. Sci. Technol. Trans. Civ. Eng. 2024, 48, 117–130. [Google Scholar] [CrossRef] [Scilit]
  3. Adel, K.; Abdelazeem, M.; Sherif, A.; Saadeldin, M.; Rashed, H.; Omran, M.M.; Tawfik, N.M. Strengthening RC beams and columns with CFRP, GFRP and KFRP laminates. Sci. Rep. 2026, 16, 11004. [Google Scholar] [CrossRef] [Scilit]
  4. Syed, S.I.; Selvaraj, K. Experimental investigation on flexural strengthened RC beams using FRP bonding system-A review. In Proceedings of the 5th International Conference on Innovative Design, Analysis & Development Practices in Aerospace & Automotive Engineering: I-Dad’22; AIP Conference Proceedings (AIP): Melville, NY, USA, 2023; Volume 2766, p. 020083. [Google Scholar]
  5. Smith, S.T.; Teng, J.G. FRP-strengthened RC beams. I: Review of debonding strength models. Eng. Struct. 2002, 24, 385–395. [Google Scholar] [CrossRef] [Scilit]
  6. Yao, J.; Teng, J.G. Plate end debonding in FRP-plated RC beams—I: Experiments. Eng. Struct. 2007, 29, 2457–2471. [Google Scholar] [CrossRef] [Scilit]
  7. Ortiz, J.D.; Khedmatgozar Dolati, S.S.; Malla, P.; Nanni, A.; Mehrabi, A. FRP-Reinforced/Strengthened Concrete: State-of-the-Art Review on Durability and Mechanical Effects. Materials 2023, 16, 1990. [Google Scholar] [CrossRef] [Scilit]
  8. Askar, M.K.; Hassan, A.F.; Al-Kamaki, Y.S.S. Flexural and shear strengthening of reinforced concrete beams using FRP composites: A state of the art. Case Stud. Constr. Mater. 2022, 17, e01189. [Google Scholar] [CrossRef] [Scilit]
  9. Tran, H.; Nguyen-Thoi, T.; Dinh, H.-B. State-of-the-art review of studies on the flexural behavior and design of FRP-reinforced concrete beams. Materials 2025, 18, 3295. [Google Scholar] [CrossRef] [Scilit]
  10. Vijayan, D.S.; Sivasuriyan, A.; Devarajan, P.; Stefańska, A.; Wodzyński, Ł.; Koda, E. Carbon fibre-reinforced polymer (CFRP) composites in civil engineering application—A comprehensive review. Buildings 2023, 13, 1509. [Google Scholar] [CrossRef] [Scilit]
  11. Sengun, K.; Arslan, G. Investigation of CFRP strengthening efficiency experimentally and analytically on reinforced concrete beams. Res. Eng. Struct. Mater. 2025, 11, 2351–2379. [Google Scholar] [CrossRef] [Scilit]
  12. Jin, L.; Qin, P.; Zhang, J.; Li, D.; Jiang, X.-A.; Du, X. Size effect in shear failure of RC beams reinforced with CFRP sheets: Influences of CFRP adhesion angle and shear-span ratio. Eng. Struct. 2025, 326, 119543. [Google Scholar] [CrossRef] [Scilit]
  13. Wang, H.; Xu, J.; Jiang, X.; Han, X.; Pan, K.; Yu, R.C.; Wu, Z. Flexural behavior of GFRP-RC beams confined with CFRP in compression zone. Eng. Struct. 2024, 302, 117348. [Google Scholar] [CrossRef] [Scilit]
  14. Rodsin, K.; Ngamkam, K.; Parichatprecha, R.; Pongpeng, J.; Mehmood, T. Enhancement of flexural strength capacity of RC-beams using LC-GFRP plates with effective debonding techniques. Appl. Sci. Eng. Prog. 2026, 19, 8041. [Google Scholar] [CrossRef] [Scilit]
  15. Hassan, E.A.; Zahran, M.S.; Osman, A.; Nagy, N.M. Experimental investigation of RC beams reinforced with GFRP bars and strengthened using the NSM technique: Flexural performance. Build. Pathol. Rehabil. 2026, 11, 68. [Google Scholar] [CrossRef] [Scilit]
  16. Salah, M.; Farag, A.; Mostafa, H.; Elansary, A. Flexural behavior of bonded post-tensioned concrete beams with steel or GFRP bars. Structures 2024, 70, 107549. [Google Scholar] [CrossRef] [Scilit]
  17. Krall, M.; Polak, M.A. Concrete beams with different arrangements of GFRP flexural and shear reinforcement. Eng. Struct. 2019, 198, 109333. [Google Scholar] [CrossRef] [Scilit]
  18. Alsuhaibani, E.; Aldukail, A. Experimental study on hybrid steel-GFRP reinforced concrete beams with different stirrup types and spacings. Buildings 2025, 15, 4047. [Google Scholar] [CrossRef] [Scilit]
  19. Wu, F.; Lei, S.; Liu, Z.; Cao, J.; Liu, L. Flexural behavior of RC beams strengthened with CFRP grid-reinforced engineering cementitious composite. Structures 2024, 67, 106978. [Google Scholar] [CrossRef] [Scilit]
  20. Zhao, J.; Pan, H.; Wang, Z.; Li, G. Experimental and theoretical study on flexural behavior of GFRP- and CFRP-reinforced concrete beams after high-temperature exposure. Polymers 2022, 14, 4002. [Google Scholar] [CrossRef] [Scilit]
  21. Firmo, J.P.; Arruda, M.R.T.; Correia, J.R.; Rosa, I. Three-dimensional finite element modelling of the fire behaviour of insulated RC beams strengthened with EBR and NSM CFRP strips. Compos. Struct. 2018, 183, 124–136. [Google Scholar] [CrossRef] [Scilit]
  22. Yu, J.T.; Wang, Y.C.; Hu, K.X.; Yu, K.; Xiao, J. The performance of near-surface mounted CFRP strengthened RC beam in fire. Fire Saf. J. 2017, 90, 86–94. [Google Scholar] [CrossRef] [Scilit]
  23. Duan, L.; Zhang, Y.; Yan, L.; Bao, S.; Liu, H.; Lu, J. Investigation on the crack development behaviour of CFRP strengthened RC beams under static and impact loading. Eng. Fail. Anal. 2025, 171, 109369. [Google Scholar] [CrossRef] [Scilit]
  24. Rosa, I.C.; Firmo, J.P.; Correia, J.R.; Bisby, L.A. Fire behavior of GFRP-reinforced concrete structural members: A state-of-the-art review. J. Compos. Constr. 2023, 27, 04023058. [Google Scholar] [CrossRef] [Scilit]
  25. Huang, Z.; Chen, W.; Tran, T.T.; Pham, T.M.; Hao, H.; Chen, Z.; Elchalakani, M. Experimental and Numerical Study on Concrete Beams Reinforced with Basalt FRP Bars Under Static and Impact Loads. Compos. Struct. 2021, 263, 113648. [Google Scholar] [CrossRef] [Scilit]
  26. Megahed, K. Predicting flexural strength of hybrid FRP-steel reinforced beams using symbolic regression and ML techniques. Sci. Rep. 2025, 15, 20277. [Google Scholar] [CrossRef] [Scilit]
  27. Liu, X.; Thermou, G.E. Shear performance of RC beams strengthened with high-performance fibre-reinforced concrete (HPFRC) under static and fatigue loading. Materials 2024, 17, 5227. [Google Scholar] [CrossRef] [Scilit]
  28. Tang, Z.; He, Z.; Chen, Z.; Chen, L.; Xue, H.; Zhuge, H. Experimental and numerical study on ultimate shear load carrying capacity of corroded RC beams. Adv. Civ. Eng. 2021, 2021, 4848483. [Google Scholar] [CrossRef] [Scilit]
  29. Rodriguez, J.; Ortega, L.M.; Casal, J. Load carrying capacity of concrete structures with corroded reinforcement. Constr. Build. Mater. 1997, 11, 239–248. [Google Scholar] [CrossRef] [Scilit]
  30. Al-Saawani, M.A.; El-Sayed, A.K.; Al-Negheimish, A.I. Effect of shear-span/depth ratio on debonding failures of FRP-strengthened RC beams. J. Build. Eng. 2020, 32, 101771. [Google Scholar] [CrossRef] [Scilit]
  31. Teng, J.G.; Chen, J.F.; Smith, S.T. Debonding Failures in FRP-Strengthened RC Beams: Failure Modes, Existing Research and Future Challenges. In Composites in Construction; ASCE: Reston, VA, USA, 2001; pp. 139–148. [Google Scholar]
  32. Barros, J.A.O.; Dias, S.J.E.; Lima, J.L.T. Efficacy of CFRP-based techniques for the flexural and shear strengthening of concrete beams. Cem. Concr. Compos. 2007, 29, 203–217. [Google Scholar] [CrossRef] [Scilit]
  33. Sengun, K.; Arslan, G. Investigation of the parameters affecting the behavior of RC beams strengthened with FRP. Front. Struct. Civ. Eng. 2022, 16, 729–743. [Google Scholar] [CrossRef] [Scilit]
  34. Al-Negheimish, A.I.; El-Sayed, A.K.; Al-Saawani, M.A.; Alhozaimy, A.M. Effect of stirrups on plate end debonding in reinforced concrete beams strengthened with fiber reinforced polymers. Polymers 2021, 13, 3322. [Google Scholar] [CrossRef] [Scilit]
  35. Bousselham, A.; Chaallal, O. Shear strengthening reinforced concrete beams with fiber-reinforced polymer: Assessment of influencing parameters and required research. ACI Struct. J. 2004, 101, 219–227. [Google Scholar] [CrossRef] [Scilit]
  36. Do-Dai, T.; Chu-Van, T.; Tran-Van, P.; Nguyen-Minh, L.; Le-Nguyen, K.; Pham, T.M. Influence of stirrup corrosion on the shear strength of reinforced concrete beams strengthened with FRP U-wraps. J. Compos. Constr. 2025, 29, 04025009. [Google Scholar] [CrossRef] [Scilit]
  37. Yu, K.; Yang, J.; Li, J.; Shu, J.; Strauss, A.; Zandi, K. Shear tests of reinforced concrete beams with the influence of initial shear cracks. In Proceedings of the 13th International Workshop on Structural Health Monitoring, Stanford, CA, USA, 15–17 March 2022. [Google Scholar]
  38. Cong, L.Y.; Zhang, F.; Qian, Y.J. Investigation into the shear performance of pre-damaged RC beams reinforced with ECC and FRP grid. Structures 2026, 85, 111130. [Google Scholar] [CrossRef] [Scilit]
  39. Kadhim, S.; Özakça, M. Flexural performance of RC beams externally strengthened with a single-layer of basalt fiber reinforced polymer sheets. Compos. Adv. Mater. 2022, 31, 263498332211024. [Google Scholar] [CrossRef] [Scilit]
  40. Ceroni, F.; Pecce, M. Design provisions for crack spacing and width in RC elements externally bonded with FRP. Compos. Part B Eng. 2009, 40, 17–28. [Google Scholar] [CrossRef] [Scilit]
  41. Xie, J.H.; Huang, K.H.; Guo, Y.C. Energy release rate of interface crack in rc beams strengthened with fiber reinforced polymer under four point bending. Polym. Polym. Compos. 2014, 22, 661–668. [Google Scholar] [CrossRef] [Scilit]
  42. ACI 440.2R-17; Guide for the Design and Construction of Externally Bonded FRP Systems for Strengthening Concrete Structures. American Concrete Institute: Farmington Hills, MI, USA, 2017.
  43. Ju, M.; Park, Y.; Park, C. Cracking control comparison in the specifications of serviceability in cracking for FRP reinforced concrete beams. Compos. Struct. 2017, 182, 674–684. [Google Scholar] [CrossRef] [Scilit]
  44. Kopiika, N.; Blikharskyy, Y.; Sobko, Y.; Khmil, R.; Blikharskyy, Z. Impact of CFRP-strengthening on crack formation in RC structures. IOP Conf. Ser. Earth Environ. Sci. 2025, 1499, 012021. [Google Scholar] [CrossRef] [Scilit]
  45. Hammad, M.; Bahrami, A.; Khokhar, S.A.; Khushnood, R.A. A state-of-the-art review on structural strengthening techniques with FRPs: Effectiveness, shortcomings, and future research directions. Materials 2024, 17, 1408. [Google Scholar] [CrossRef] [Scilit]
  46. Liu, K.; Wulan, T.; Yao, Y.; Bian, M.; Bao, Y. Assessment of damage evolution of concrete beams strengthened with BFRP sheets with acoustic emission and unsupervised machine learning. Eng. Struct. 2024, 300, 117228. [Google Scholar] [CrossRef] [Scilit]
  47. Uzdil, O.; Sayın, B.; Coşgun, T. Examination of parameters impacting flexural and shear strengthening of RC beams. J. Struct. Eng. Appl. Mech. 2022, 5, 117–134. [Google Scholar] [CrossRef] [Scilit]
  48. Sümer, Y.; Zakour, M.N.; Aldhabir, W.M.H. Effect of GFRP anchor on the performance of reinforced concrete beams to mitigate the debonding failure. Türk Doğa Ve Fen Derg. 2025, 14, 109–119. [Google Scholar] [CrossRef] [Scilit]
  49. El-Emam, H.M.; Ata, B.; Ahmad, S.S.E.; Salim, H.A.; Reda, R.M. Enhancing Flexural Resistance in Pre-Damaged RC Beams with Near-Surface Mounted GFRP Bar and Bolt Anchoring System. Buildings 2024, 14, 723. [Google Scholar] [CrossRef] [Scilit]
  50. GB 50367-2013; Code for Design of Strengthening Concrete Structures. China Architecture & Building Press: Beijing, China, 2013.
  51. Elbawab, Y.; Elbawab, Y.; El Zoughby, Z.; ElKadi, O.; AbouZeid, M.; Sayed-Ahmed, E. Flexural Testing of Steel-, GFRP-, BFRP-, and Hybrid Reinforced Beams. Polymers 2025, 17, 2027. [Google Scholar] [CrossRef] [Scilit]
  52. Muflikhun, M.A.; Fiedler, B. Failure Prediction and Surface Characterization of GFRP Laminates: A Study of Stepwise Loading. Polymers 2022, 14, 4322. [Google Scholar] [CrossRef] [Scilit]
  53. GB 50011-2010; Code for Seismic Design of Buildings. China Architecture & Building Press: Beijing, China, 2010.
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.