10 September 2026

21 Pages

Effects of Protective Covering Configurations on the Fire Behavior and Charring Characteristics of Korean Larch Cross-Laminated Timber Walls

,
and
Construction Test & Assessment Center, Korea Institute of Civil Engineering and Building Technology, Ilsanseo-gu, Goyang-si 10223, Gyeonggi-Do, Republic of Korea
*
Author to whom correspondence should be addressed.

Abstract

Protective coverings are an effective means of preventing direct fire exposure and delaying the charring of cross-laminated timber (CLT). This study evaluated the effects of practical covering configurations on the fire behavior and charring characteristics of four Korean larch CLT wall assemblies through 120-min fire resistance tests. The specimens varied in fire-resistant gypsum board thickness, joint arrangement, fastening details, and insulation conditions. Fire-induced damage, internal temperatures, and post-fire charring characteristics were evaluated. Specimens with non-staggered gypsum board joints exhibited cracking and detachment of the protective covering, resulting in localized flame penetration, with a maximum measured localized charring depth of 80 mm in CW-WS-G-1 and a measured localized charring depth of 73 mm in CW-WS-G-2. In contrast, specimens with staggered joints and improved fastening details largely maintained covering integrity. Only minor surface charring was observed in CW-WS-G-3, while no distinct charring occurred in CW-WS-W-1. The highest temperature recorded by the installed thermocouples was 225.2 °C in CW-WS-G-1, whereas the highest recorded temperatures in all other specimens remained below 100 °C. Nevertheless, localized charring occurred in CW-WS-G-2 despite its low internal temperature, indicating that temperature measurements alone may not adequately capture localized fire damage. These results indicate that, within the tested configurations, covering integrity associated with the combined joint arrangement and fastening details played an important role in limiting localized flame penetration and charring.

1. Introduction

As climate change and global warming continue to intensify worldwide, achieving carbon neutrality has emerged as a major policy priority for the international community and national governments. The construction industry, in particular, consumes substantial amounts of energy and generates considerable greenhouse gas emissions throughout the entire life cycle of buildings, including material production, construction, operation, and demolition. Accordingly, continued technological and policy efforts are required to decarbonize the building sector. In response, there has been growing interest in reducing the use of conventional construction materials with high carbon emissions, such as steel and cement, and replacing them with low-carbon alternatives such as wood. Wood is a renewable construction material that absorbs atmospheric carbon dioxide during tree growth and stores the sequestered carbon within the material. Therefore, partially replacing reinforced concrete and steel structures with timber-based systems can reduce the embodied carbon of buildings while providing long-term carbon storage [1,2,3]. Owing to these environmental benefits, the construction of mid- and high-rise timber buildings using engineered wood products, including glued laminated timber and cross-laminated timber, has expanded, particularly in Europe and North America. Among these engineered wood products, cross-laminated timber (CLT) has attracted considerable attention as a low-carbon construction material because of its dimensional stability, structural performance, and construction efficiency. In Korea, research on CLT has also been actively conducted to promote the high-value utilization of domestic timber resources and expand the application of timber construction. Figure 1 illustrates the conceptual framework linking climate change mitigation and carbon-neutral policies to the decarbonization of the building sector and the expanded use of CLT.
Figure 1. Conceptual framework linking carbon neutrality policies to the adoption of cross-laminated timber (CLT) in the building sector.
Among engineered wood products, cross-laminated timber (CLT) has attracted considerable attention as a sustainable structural material owing to its excellent structural performance, dimensional stability, and carbon storage capacity. CLT is a large-scale, panelized structural wood product manufactured by stacking layers of lumber in orthogonal directions and bonding them with structural adhesives. It generally consists of three or more layers arranged in an odd number, with the grain direction of adjacent layers oriented perpendicular to each other. This crosswise configuration provides enhanced stiffness and dimensional stability in both in-plane and out-of-plane directions [4,5]. CLT is widely used for major structural components of buildings, including walls, floors, and roofs, and has become a key structural material for mid- and high-rise timber buildings because of its consistent quality through factory prefabrication, reduced on-site construction time, and excellent thermal insulation performance. In Korea, studies on the manufacturing technology and structural performance of CLT produced from domestic softwood species, including Korean larch, have been continuously conducted, thereby expanding the potential for the structural utilization of domestic timber resources.
However, because wood is a combustible material, adequate fire resistance must be ensured when it is used as a primary structural component in buildings. When wood is exposed to elevated temperatures, moisture initially evaporates, followed by the pyrolysis of cellulose, hemicellulose, and lignin. During this process, combustible gases such as CO, CH4, and H2 and non-combustible gases such as CO2 and H2O are released, while a char layer forms on the wood surface. Owing to its low thermal conductivity, the char layer acts as a thermal barrier that reduces heat transfer to the underlying wood and slows the rate of pyrolysis [6,7]. Consequently, even when the surface of a large-section timber member is exposed to fire, the uncharred residual cross-section can retain sufficient load-bearing capacity for a certain period. Based on this behavior, charring depth and charring rate are commonly used as key parameters in the fire-resistant design of timber structures [7,8]. Therefore, accurate evaluation of the charring characteristics of CLT is essential for the fire-resistant design and fire safety assessment of timber buildings.
To quantitatively evaluate the charring characteristics of CLT, an understanding of the charring depth and charring rate of wood is essential. Charring depth is generally determined based on the relationship between fire exposure time and charring rate. Eurocode 5 specifies the one-dimensional charring rate, notional charring rate, and reduced cross-section method for evaluating the residual cross-section of timber structural members under fire exposure [8]. In addition, wood species, density, moisture content, cross-sectional geometry, fire exposure conditions, and the performance of adhesive bond lines are known to be major factors affecting the charring rate and charring behavior of timber [7,9].
Unlike solid timber members, CLT consists of multiple lumber layers and adhesive bond lines, and its charring behavior under fire exposure can therefore vary depending on the layer configuration and adhesive performance. When a stable char layer remains on the fire-exposed surface of CLT, it reduces heat transfer to the underlying wood, allowing charring to progress at a relatively constant rate. However, insufficient thermal resistance of the adhesive bond lines or delamination between adjacent layers may result in char fall-off, exposing a new wood surface directly to fire. This renewed exposure can accelerate pyrolysis and combustion, leading to an increased charring rate and a more rapid reduction in the residual cross-section than expected [10,11,12]. Therefore, the fire behavior of CLT should be evaluated by considering not only the average charring depth but also localized charring characteristics, including char fall-off and non-uniformity of the char front. For these reasons, considerable research has focused on the application of protective coverings to improve the fire performance of CLT.
Frangi et al. [10] investigated the effects of lamella fall-off and adhesive bond performance on the charring behavior of CLT panels through fire resistance tests. They reported that when a stable char layer cannot be maintained, the exposure of fresh wood surfaces to fire can accelerate charring. Hadden et al. [11] investigated the influence of exposed CLT on the development and duration of compartment fires and demonstrated that sustained combustion of exposed timber surfaces and lamella fall-off can significantly alter fire behavior. Furthermore, Bartlett et al. [12] examined the conditions required for the self-extinction of engineered timber and reported that combustion may cease when the char layer sufficiently reduces the heat flux transferred to the underlying wood. However, damage to the char layer or lamella fall-off can expose fresh wood surfaces, thereby increasing the potential for re-ignition.
The application of protective board systems, such as gypsum boards, to timber surfaces is widely used to improve the fire resistance of CLT members. These protective coverings have been reported to delay the direct exposure of timber surfaces to flames and elevated temperatures, thereby postponing the onset of charring and subsequent cross-sectional reduction [5,13,14,15]. The fire-protective performance of such coverings may depend not only on the type and thickness of the boards but also on fastening methods and the location and arrangement of board joints. In particular, the joint arrangement of multi-layer gypsum board systems can influence heat transfer paths through the protective layers, potentially affecting the temperature rise at the CLT surface and the development of localized charring.
Kolaitis et al. [14] demonstrated through large-scale compartment fire tests that gypsum board protection can delay the fire exposure of timber members and reduce the progression of charring. Similarly, Hoehler et al. [15] conducted large-scale compartment fire tests on CLT and reported that gypsum board protection delayed fire exposure of the CLT and reduced the temperature rise within the timber. However, previous studies have primarily focused on the presence or absence of protective coverings or on the performance of adhesive bond lines. Systematic investigations into the effects of joint arrangement and fastening details of multi-layer fire-resistant gypsum board systems, as used in practical building applications, on the fire behavior and localized charring characteristics of full-scale Korean larch CLT walls remain limited. Therefore, to evaluate the fire protection performance of Korean larch CLT walls, it is necessary to comprehensively investigate how protective covering configurations, including the thickness, joint arrangement, and fastening details of fire-resistant gypsum boards, affect their fire behavior and charring characteristics.
Accordingly, in this study, non-load-bearing fire resistance tests were conducted on CLT wall assemblies manufactured from Korean larch to investigate their fire behavior and charring characteristics under different practical protective-covering configurations. The specimens incorporated different combinations of fire-resistant gypsum-board thickness, joint arrangement, fastening details, and insulation conditions. The fire performance of each wall assembly was evaluated by comparing the internal temperature development, post-fire charring depth and patterns, and observed damage to the protective covering. The objective of this study was to compare the fire behavior and charring characteristics of full-scale Korean larch CLT wall assemblies incorporating practical protective-covering configurations and to provide experimental data for the fire-resistant design of protected CLT walls. Because multiple detailing parameters varied simultaneously among some specimens, the experimental program was intended to evaluate the performance of the complete protective-covering configurations rather than to isolate the independent effect of each individual parameter. This system-level comparison enabled the experimental identification of differences in localized flame penetration, protective-covering damage, and CLT charring among the tested wall assemblies.

2. Materials and Methods

2.1. Materials

Cross-laminated timber (CLT) manufactured from Korean larch (Larix kaempferi) was used as the structural component of the wall specimens. CLT is an engineered wood product manufactured by orthogonally laminating structural lumber layers and bonding them with structural adhesives, providing high structural performance and dimensional stability for use as a primary structural material in mid- and high-rise timber buildings. All wall specimens consisted of Korean larch CLT panels with dimensions of 3000 mm in width, 3000 mm in height, and 90 mm in thickness. Detailed manufacturing records for the CLT panels were not available in the retained test documentation. Therefore, additional manufacturing and material parameters, including the number and thickness of lamellae, lay-up configuration, lumber density, initial moisture content, strength grade, adhesive type and spread rate, pressing conditions, and applicable manufacturing standard, could not be retrospectively verified. This lack of detailed manufacturing information should be considered a limitation when interpreting the thermal response and charring characteristics observed in this study.
The protective covering system was constructed on the fire-exposed side of the CLT panels. Timber studs and runners commonly used in light-frame wood construction were installed, and the cavities between them were filled with either glass-wool insulation (24 kg/m3) or wood-fiber insulation, depending on the specimen configuration. Depending on the specimen configuration, two layers of fire-resistant gypsum board, with a thickness of either 15 or 19 mm, were installed on the exterior side as the base and finish layers. The protective covering system was designed to represent a dry fire-protection system commonly used in light-frame timber wall construction in Korea. Detailed product information and thermal/fire properties of the insulation materials, including the manufacturer, product type, thermal conductivity, and reaction-to-fire classification, were not available in the retained test records and could therefore not be retrospectively verified. For the wood-fiber insulation, density information was also unavailable. These limitations should be considered when interpreting differences in the thermal responses associated with the insulation conditions and restrict the generalizability of quantitative comparisons related to insulation performance.

2.2. Specimen Configuration

A total of four wall specimens were fabricated to evaluate the charring characteristics of Korean larch CLT walls under different protective covering conditions. All specimens consisted of Korean larch cross-laminated timber (CLT) panels measuring 3000 mm in width, 3000 mm in height, and 90 mm in thickness. The specimen configurations differed in fire-resistant gypsum-board thickness, joint arrangement, fastening details, and insulation conditions. The protective covering systems were constructed using a dry fire-protection method commonly employed at construction sites in Korea, with timber studs and runners selected to reflect typical timber construction practices. The protective coverings were installed only on the fire-exposed side of the specimens. The joint configurations were classified as non-staggered and staggered arrangements. For CW-WS-G-1 and CW-WS-G-2, the joints of the base and finish gypsum-board layers were not intentionally offset and were therefore classified as non-staggered. For CW-WS-G-3 and CW-WS-W-1, the joints of the two layers were intentionally offset and were classified as staggered. Detailed quantitative offsets between individual board joints were not available in the retained construction records; therefore, the joint geometries are presented schematically in Figure 2. One full-scale specimen was tested for each protective-covering configuration; therefore, the experimental results represent the observed behavior of individual specimens rather than statistically replicated performance for each configuration.
Figure 2. Layout of fire-resistant gypsum board joints in CLT wall specimens. (a) Gypsum board joint layout of the CW-WS-G-1 and CW-WS-G-2 specimens (non-staggered joints). (b) Gypsum board joint layout of the CW-WS-G-3 and CW-WS-W-1 specimens (staggered joints).
The four specimens incorporated different combinations of fire-resistant gypsum-board thickness, joint arrangement, fastening details, and insulation conditions. CW-WS-G-1 was designed as the reference specimen, with 19-mm-thick fire-resistant gypsum boards used for both the base and finish layers and with a non-staggered joint configuration. CW-WS-G-2 was configured as a comparative specimen with 19-mm-thick and 15-mm-thick fire-resistant gypsum boards for the base and finish layers, respectively. CW-WS-G-3 was designed with staggered joints between the base and finish layers and modified fastening details. CW-WS-W-1 had the same joint arrangement and fastening details as CW-WS-G-3 but incorporated 30-mm wood-fiber insulation instead of 50-mm glass-wool insulation, providing a limited comparison of different insulation conditions.
All specimens were subjected to 120-min non-load-bearing fire resistance tests under identical conditions in accordance with the standard fire exposure specified in KS F 2257. The detailed configurations and test conditions of the specimens are summarized in Table 1, while the cross-sectional details and joint arrangements of the protective covering systems are presented in Figure 2. The specimens were designed to represent protective covering systems commonly used in Korean construction practice. Accordingly, this study focused on comparing the fire behavior and charring characteristics associated with practically applicable protective covering configurations.
Table 1. Configuration and test conditions of CLT wall specimens.
Timber studs with a cross-section of 50 × 40 mm were used for all specimens, and the fire-resistant gypsum boards were fastened with gypsum board screws at 150-mm intervals. For CW-WS-G-1 and CW-WS-G-2, 32-mm-long screws were used for the base layer and 50-mm-long screws for the finish layer. In contrast, CW-WS-G-3 and CW-WS-W-1 incorporated staggered joints and modified fastening details, with 50-mm-long and 65-mm-long screws used for the base and finish layers, respectively. The screw spacing was maintained at 150 mm for all specimens. The fastening details adopted for CW-WS-G-3 and CW-WS-W-1 were selected to represent construction practices commonly used for timber wall systems in Korea.

2.3. Fire Resistance Test

To evaluate the fire behavior of Korean larch CLT walls under different protective covering conditions, non-load-bearing fire resistance tests were conducted. The tests were performed in accordance with KS F 2257-1, Methods of Fire Resistance Test for Elements of Building Construction—General Requirements [16], and KS F 2257-8, Method of Fire Resistance Test for Elements of Building Construction—Specific Requirements for Non-loadbearing Vertical Separating Elements [17]. The specimens were exposed to the standard time–temperature curve specified in KS F 2257-1 [16] and ISO 834-1 [18], and the mean furnace temperature was controlled to follow the prescribed curve throughout the test. The standard time–temperature relationship is expressed by Equation (1).
T = 345 l o g 10 8 t + 1 + 20
where T is the mean furnace temperature (°C), and t is the fire exposure time (min). The standard time–temperature curve specified in KS F 2257 and adopted in this study is shown in Figure 3.
Figure 3. Standard time–temperature curve specified in KS F 2257-1 and ISO 834-1 [16,18].
Although the non-load-bearing fire resistance test method specified in KS F 2257 was adopted in this study, the evaluation objective differed from that of a conventional non-load-bearing fire resistance test. Conventional tests primarily assess insulation performance by limiting the temperature rise on the unexposed surface and thereby restricting the transmission of heat and flames during fire exposure. In contrast, this study focused on evaluating the thermal damage behavior within the CLT rather than on insulation performance itself. When wood is exposed to fire, pyrolysis progresses and a char layer forms on the surface. For the purpose of comparing the thermal responses of the specimens, approximately 200 °C was adopted in this study as a reference temperature associated with thermal degradation of wood [6,7]. This value was used only as a comparative reference and should not be interpreted as a universal temperature for the onset of char formation. Accordingly, the conventional integrity and insulation acceptance criteria specified for formal fire-resistance classification were not used as the primary evaluation criteria in this study, and the results should not be interpreted as formal fire-resistance ratings of the complete wall assemblies.
All specimens were installed vertically at the opening of a vertical furnace so that only the fire-exposed surface was subjected to heating. Gaps between the specimens and the furnace were sealed with rock wool. The specimen installation and the post-fire damage condition are shown in Figure 4a and Figure 4b, respectively. During the tests, the measured mean furnace temperature showed a trend similar to the standard time–temperature curve specified in KS F 2257-1 throughout the 120-min fire exposure. All specimens were subjected to one-sided fire exposure using the same test procedure.
Figure 4. Fire resistance test of CLT wall specimens.
To measure the temperature development within the specimens, mineral-insulated metal-sheathed thermocouples (MI thermocouples) with a diameter of 1.6 mm were used. Manufacturer-specified numerical accuracy or measurement uncertainty for the thermocouples was not available in the retained test records; therefore, no numerical uncertainty value was assigned to the measured temperatures. For CW-WS-G-1 and CW-WS-G-2, temperatures were measured at three locations along the vertical centerline of each specimen: the upper, middle, and lower regions. At each location, six thermocouples were installed at 5-mm intervals from the fire-exposed surface to a depth of 30 mm, resulting in a total of 18 measurement points per specimen. For CW-WS-G-3 and CW-WS-W-1, temperatures were measured at nine locations distributed across the specimen surface. At each location, thermocouples were installed at depths of 5 and 10 mm from the fire-exposed surface, resulting in a total of 18 measurement points per specimen. The thermocouple locations across the specimen surface and the measurement depths for each specimen are shown in Figure 5. Given the point-based nature of the temperature measurements, the measured temperatures were interpreted in conjunction with the observed protective-covering damage and post-fire charring conditions, rather than being used alone to determine the occurrence or severity of localized thermal damage.
Figure 5. Thermocouple locations for CLT wall specimens. (a) CW-WS-G-1, CW-WS-G-2 specimens: front-view thermocouple locations. (b) CW-WS-G-3, CW-WS-W-1 specimens: front-view thermocouple locations. (c) CW-WS-G-1, CW-WS-G-2 specimens: depth-wise thermocouple locations. (d) CW-WS-G-3, CW-WS-W-1 specimens: depth-wise thermocouple locations.
During the tests, the furnace temperature and internal temperatures of the specimens were continuously recorded using a data logger. Cracking and detachment of the fire-resistant gypsum boards, progression of surface charring, and other fire-induced behaviors were also continuously monitored throughout the fire exposure. However, the exact occurrence times of gypsum-board cracking, joint opening, flame penetration, and board detachment were not systematically recorded in the retained test records. Therefore, the effective duration of direct flame exposure to the CLT could not be quantitatively determined. All specimens were subjected to identical fire exposure conditions for 120 min in accordance with the standard fire curve specified in KS F 2257. After completion of the tests, the specimens were allowed to cool naturally to ambient temperature, after which the post-fire damage and charring patterns were examined. Cylindrical cores were then extracted from the unexposed side toward the fire-exposed side, perpendicular to the wall section, at locations where charring was visually observed. The charred–uncharred boundary was identified visually based on the distinct transition between the blackened charred region and the underlying uncharred wood. The remaining uncharred thickness of each core was measured using a ruler graduated in 1-mm increments, and the charring depth was calculated as the difference between the initial CLT thickness of 90 mm and the measured uncharred thickness. The 1-mm graduation represents the measurement resolution of the ruler; however, additional uncertainty may arise from the visual identification of the charred–uncharred boundary. For CW-WS-G-1, measurements were conducted at two locations corresponding to the observed flame-spread regions, whereas for CW-WS-G-2, the measurement was conducted at the localized flame-damaged region. The measured charring depths were 79 and 80 mm for CW-WS-G-1 and 73 mm for CW-WS-G-2. For CW-WS-G-1, the larger of the two measured values (80 mm) was reported as the maximum measured localized charring depth. For CW-WS-G-2, only one measurement was obtained from the localized flame-damaged region; therefore, the measured depth of 73 mm should be interpreted as a measured localized charring depth rather than as a spatially representative maximum value for the entire specimen. For CW-WS-G-3, only superficial surface charring was observed without measurable penetration into the CLT, while no distinct charring was observed for CW-WS-W-1. Accordingly, the reported charring depths represent localized measurements at damaged regions rather than spatially averaged values over the entire CLT wall surface. Quantitative measurements of the total charred width or area were not systematically recorded; therefore, the spatial extent of charring was evaluated qualitatively from post-fire observations. Based on the internal temperatures recorded during the tests and the charring depths measured after fire exposure, heat penetration characteristics and thermal damage to the CLT were evaluated for each protective covering configuration. The effects of the protective covering configuration on the fire behavior of the CLT walls were comprehensively assessed by comparing the internal temperature development, charring characteristics, and observed fire-induced behavior among the specimens.

3. Fire Behavior and Charring Characteristics

3.1. Overall Fire Behavior and Damage Observations

Figure 6 shows the fire-induced damage observed on the fire-exposed side of each specimen after the 120-min fire resistance test. Cracking and partial detachment of the fire-resistant gypsum boards were observed in some specimens, and distinct differences in the extent of damage and CLT exposure were identified depending on the protective covering configuration. Distinct differences in protective-covering damage and flame-spread patterns were observed among the tested configurations incorporating different joint arrangements and fastening details. Consequently, differences were also observed in the combustion of the timber studs and the extent of charring on the CLT surface.
Figure 6. Fire-exposed surfaces of the CLT wall specimens at the end of the 120-min fire exposure.
For CW-WS-G-1 and CW-WS-G-2, cracking and detachment of the fire-resistant gypsum boards occurred primarily around the board joints, where ignition and flame spread were observed. At locations where the protective covering detached, the underlying timber studs and CLT surface were directly exposed to flames. After the tests, combustion of the timber studs and charring of the CLT surface were observed. In CW-WS-G-1, detachment of the protective covering and flame spread occurred at two major locations corresponding to the gypsum board joints. Flames penetrating the protective covering system through these joints propagated along the timber studs, resulting in relatively deep charring of the fire-exposed CLT surface. CW-WS-G-2 exhibited similar detachment and flame spread around the gypsum board joints. Post-fire observations revealed localized charring of the CLT surface near the joints, accompanied by combustion of the timber studs.
In contrast, no distinct ignition or flame penetration through the board joints was observed in CW-WS-G-3 or CW-WS-W-1, which incorporated staggered joints together with modified fastening details. CW-WS-G-3 exhibited some surface burning and limited evidence of charring; however, the damage was confined to localized areas of the fire-exposed surface without substantial charring into the CLT. In CW-WS-W-1, no distinct char layer was observed on the fire-exposed CLT surface after the test, indicating that the protective function of the covering system was maintained more effectively than in the other specimens.
Overall, protective-covering damage and flame penetration were concentrated around the joint regions in CW-WS-G-1 and CW-WS-G-2, whereas CW-WS-G-3 and CW-WS-W-1 maintained the integrity of the protective covering more effectively. Because the joint arrangement and fastening details were modified simultaneously among the tested configurations, the individual contribution of each factor cannot be isolated. The possible progression of protective-covering damage and its relationship with CLT charring are discussed further in Section 3.3. The principal fire-induced damage observed for each specimen is summarized in Table 2.
Table 2. Summary of fire damage observed after the fire tests.

3.2. Internal Temperature Response of CLT Walls

Figure 7 shows the internal temperature development of the CLT specimens during the 120-min fire resistance tests. The channel numbers indicated in Figure 7 correspond to the thermocouple locations shown in Figure 5. For CW-WS-G-1 and CW-WS-G-2, CH1–CH6 correspond to the upper region at depths of 5, 10, 15, 20, 25, and 30 mm from the fire-exposed surface, respectively; CH7–CH12 correspond to the middle region at the same respective depths; and CH13–CH18 correspond to the lower region at the same respective depths. For CW-WS-G-3 and CW-WS-W-1, the channel pairs CH1–CH2, CH3–CH4, CH5–CH6, CH7–CH8, CH9–CH10, CH11–CH12, CH13–CH14, CH15–CH16, and CH17–CH18 correspond to positions P1–P9 shown in Figure 5, respectively, with the odd-numbered and even-numbered channels representing depths of 5 and 10 mm from the fire-exposed surface, respectively.
Figure 7. Internal temperature–time curves of the CLT wall specimens during the 120-min fire tests, with the reference temperature for thermal degradation (~200 °C).
The mean and maximum temperatures measured for each specimen are summarized in Table 3. At the end of the test, CW-WS-G-1 exhibited a mean measured temperature of 96.0 °C and a maximum measured temperature of 225.2 °C, making it the only specimen in which the temperature recorded at the installed thermocouple locations exceeded the reference temperature for thermal degradation (~200 °C). In contrast, the mean and maximum temperatures were 88.3 and 99.8 °C for CW-WS-G-2, 50.4 and 97.3 °C for CW-WS-G-3, and 55.5 and 85.9 °C for CW-WS-W-1, respectively. Thus, the temperatures recorded at the installed thermocouple locations in these three specimens remained below the reference temperature for thermal degradation (~200 °C) throughout the test.
Table 3. Summary of internal temperatures and post-fire charring observations.
In CW-WS-G-1, the internal CLT temperatures increased gradually during the initial stage of fire exposure but rose sharply at several measurement points during the later stage of the test. In particular, a substantial temperature increase was observed at locations close to the fire-exposed surface, with a maximum temperature of 225.2 °C. This increase was likely caused by damage and detachment of the fire-resistant gypsum boards at the joints, which allowed flames and hot gases to penetrate the protective covering system and locally expose the CLT surface to elevated temperatures. The post-fire observation of both timber stud combustion and CLT charring in these regions further indicates that the rapid increase in internal temperature was closely associated with localized damage to the protective covering system.
For CW-WS-G-2, the maximum temperature was 99.8 °C, and all measurement points remained below the reference temperature for thermal degradation (~200 °C) throughout the test. Nevertheless, post-fire observations revealed detachment of the protective covering, combustion of the timber studs, and charring of the CLT near the gypsum board joints. This discrepancy was likely attributable to localized charring occurring at some distance from the thermocouple locations, such that the associated temperature increase was not adequately captured by the measurements. Therefore, the absence of high temperatures at the installed thermocouple locations should not be interpreted as evidence that severe localized thermal damage did not occur elsewhere in the wall. Point-based temperature measurements alone may not adequately represent localized fire-induced damage in protected CLT walls. The temperature measurements should therefore be evaluated in conjunction with observations of protective covering detachment and post-fire charring.
For CW-WS-G-3 and CW-WS-W-1, which incorporated improved protective covering details, temperatures at all measurement points remained below 100 °C. The maximum temperature of CW-WS-G-3 was 97.3 °C. Although limited surface damage was observed on the CLT after the test, no distinct charring extending into the CLT was identified. The maximum measured temperature in CW-WS-W-1 was 85.9 °C, and no distinct charring was observed on the CLT surface after the test. These observations are consistent with improved protective-covering integrity and reduced heat transfer in the tested configurations incorporating staggered joints together with modified fastening details.
In CW-WS-W-1, a temporary reduction in the rate of temperature increase was observed during the later stage of the test. This behavior may be associated with moisture evaporation from the wood-fiber insulation, during which a portion of the thermal energy may have been consumed as latent heat, thereby delaying the temperature rise toward the CLT. However, this explanation should be regarded only as a hypothesis because neither the moisture content nor the associated heat-transfer process was directly measured. CW-WS-G-3 and CW-WS-W-1 also differed not only in insulation type but also in insulation thickness, which was 50 mm and 30 mm, respectively. Furthermore, only one specimen was tested for each condition. Therefore, the relative fire performance of the insulation materials cannot be generalized based solely on these results. The results of these two specimens should instead be interpreted as a limited comparison indicating potential differences in thermal behavior associated with the insulation conditions. Further controlled experiments are required to verify the proposed moisture-related mechanism.
The thermocouple configurations also differed between CW-WS-G-1 and CW-WS-G-2 and between CW-WS-G-3 and CW-WS-W-1. For CW-WS-G-1 and CW-WS-G-2, temperatures were measured at three locations in the upper, middle, and lower regions of the specimens at depths ranging from 5 to 30 mm from the fire-exposed surface. In contrast, for CW-WS-G-3 and CW-WS-W-1, temperatures were measured at nine locations distributed across the specimen surface at depths of 5 and 10 mm. Accordingly, the mean temperatures are presented only as indicators of the overall thermal response of each specimen and should not be interpreted as directly equivalent statistical quantities among all four configurations. Because the measurement locations and depth ranges were not identical, direct quantitative ranking of specimen performance based solely on the mean temperatures is not appropriate. The maximum measured temperatures should likewise be interpreted as the highest values captured by the installed thermocouples rather than as the absolute maximum temperatures experienced anywhere within each specimen. Therefore, the temperature results were interpreted together with the temperature histories, maximum measured temperatures, protective-covering damage, and post-fire charring observations.
Overall, localized damage to the protective covering, as observed in CW-WS-G-1, resulted in a rapid increase in the internal CLT temperature, with temperatures exceeding the reference temperature for thermal degradation (~200 °C). In contrast, CW-WS-G-3 and CW-WS-W-1, which incorporated modified protective covering details, maintained relatively low internal temperatures throughout the test. However, as demonstrated by CW-WS-G-2, localized charring may occur outside the thermocouple measurement locations even when the measured internal temperatures remain relatively low. Therefore, the fire performance of protected CLT walls should not be assessed solely on the basis of internal temperature measurements but rather through an integrated evaluation of temperature histories, damage to the protective covering, and post-fire charring conditions.

3.3. Effect of Protective-Covering Configuration on Fire Performance

Figure 8 schematically illustrates the proposed progression of fire-induced damage in the CLT walls under different protective-covering configurations, from the initial condition to the post-fire condition after the 120-min fire resistance test. The schematic represents an interpretation based on the experimental and post-fire observations and does not imply that the timing of each intermediate failure event was directly measured. It depicts the potential flame penetration paths through the fire-resistant gypsum-board joints and the associated damage progression within the protective covering system. The schematic was developed to compare the observed flame penetration and CLT damage patterns among the tested configurations incorporating different joint arrangements and fastening details. Despite the use of identical CLT wall panels, distinct differences in flame penetration and the extent of CLT damage were observed among the tested protective-covering configurations.
Figure 8. Schematic illustration of fire damage progression according to protective-covering configuration.
For CW-WS-G-1 and CW-WS-G-2, the joints of the base and finish layers were aligned or located in close proximity, with the joint regions acting as primary pathways for heat and flame penetration. As heating progressed, cracks developed in the fire-resistant gypsum boards near the joints, allowing high-temperature flames and combustion gases to penetrate the protective covering system. Flame spread along the timber studs was also observed. The resulting loss of the stud cross-section may have reduced the anchorage capacity of the screws, progressively increasing the extent of covering detachment. This process may have promoted direct flame exposure of the CLT, resulting in localized charring. This damage mechanism was further supported by the post-fire observations, in which the locations of gypsum board detachment generally corresponded to the charred regions of the CLT. This sequence should be interpreted as a proposed damage mechanism consistent with the experimental observations rather than as a directly measured chronological sequence of failure events.
In contrast, CW-WS-G-3 and CW-WS-W-1 incorporated staggered joints between the base and finish layers together with modified fastening details to improve the integrity of the protective covering system. Consequently, direct flame penetration through the joints was effectively limited, and most of the fire-resistant gypsum boards remained in place until the end of the test, substantially reducing direct flame exposure of the CLT. Only limited surface charring was observed in CW-WS-G-3, whereas no distinct charring was identified in CW-WS-W-1. These observations are consistent with previous studies demonstrating the general fire-protective effect of gypsum-board coverings on timber members [14,15]. More specifically, Yasir et al. [19] reported that the location of joints in protective covering was an important factor affecting protective covering fall-off in fire-tested CLT wall panels and that protective covering delayed the onset of CLT charring. Ramzi and Hajiloo [20], based on a synthesis of full-scale fire tests, showed that gypsum-board fall-off is sensitive to attachment conditions, including screw spacing and the remaining embedment of fasteners in uncharred wood. Sultan [21] similarly reported from full-scale wall fire tests that reduced screw spacing can help maintain gypsum-board attachment for longer periods and improve fire resistance. These findings provide relevant context for the present observations, in which localized damage near board joints and subsequent loss of protective-covering integrity were associated with increased flame penetration and localized CLT charring. However, because the joint arrangement and fastening details were modified simultaneously in the present specimens, the individual contribution of each factor cannot be isolated.
Overall, substantial differences in fire behavior were observed among the tested protective-covering configurations incorporating different joint arrangements and fastening details. CW-WS-G-1 incorporated two 19-mm-thick gypsum boards, resulting in a total covering thickness of 38 mm, whereas CW-WS-G-2 incorporated 19- and 15-mm-thick boards, resulting in a total thickness of 34 mm. Despite this difference, both specimens exhibited substantial localized damage, including flame penetration and covering detachment around the joint regions. Because only one specimen was tested for each configuration and the observed damage was highly localized, the difference in maximum charring depth between these specimens should not be interpreted quantitatively as an independent effect of gypsum-board thickness. Rather, within the tested configurations, the observations indicate that the overall integrity of the protective-covering system was closely associated with the development of localized flame penetration and charring.
In non-staggered configurations, where the joints of successive gypsum-board layers are aligned or located in close proximity, discontinuities in the protective layers may occur along similar paths, potentially creating concentrated thermal and mechanical vulnerabilities. During fire exposure, these regions may therefore be more susceptible to cracking and subsequent detachment of the protective covering, while simultaneously providing preferential pathways for flames and hot gases to penetrate the system. In the configurations incorporating staggered joints together with modified fastening details, the continuity of potential penetration paths through the successive gypsum-board layers was interrupted, while the modified fastening details may also have contributed to maintaining the integrity of the protective covering system. Because these parameters were modified simultaneously, their individual contributions cannot be distinguished from the present experiments.
In addition, although the maximum internal temperature measured in CW-WS-G-2 remained below 100 °C, post-fire examination confirmed localized deep charring of the CLT. This discrepancy indicates that relatively low temperatures recorded at discrete thermocouple locations do not necessarily demonstrate the absence of severe localized thermal damage elsewhere in the wall. Localized flame penetration through damaged joint regions may produce highly concentrated thermal exposure that is not captured by point-based temperature measurements. Therefore, the behavior of CW-WS-G-2 highlights the importance of interpreting internal temperature measurements together with protective-covering damage and post-fire charring observations when evaluating the fire performance of protected CLT walls.
Overall, within the tested configurations, the assemblies incorporating staggered joints together with modified fastening details maintained the integrity of the protective covering more effectively than the non-staggered joint configurations. However, because multiple parameters, including gypsum-board thickness, joint arrangement, fastening details, and insulation conditions, varied simultaneously in some specimens, the independent contribution of each parameter cannot be determined from the present experiments. The results should therefore be interpreted as a system-level comparison of practical protective-covering configurations rather than as an independent quantitative assessment of individual parameters. Further studies incorporating replicated specimens and systematically controlled variables are required to quantify the individual effects of these parameters and their experimental variability. Nevertheless, the present observations indicate that maintaining the integrity of the protective-covering system is an important consideration for limiting localized flame penetration and charring in protected Korean larch CLT walls.

3.4. Charring Characteristics of CLT Walls

Figure 9 shows the charred cross-sections and measured localized charring depths of CW-WS-G-1 and CW-WS-G-2, in which measurable charring was observed after the fire resistance tests.
Figure 9. Charred cross-sections and measured localized charring depths of CW-WS-G-1 and CW-WS-G-2.
CW-WS-G-1 exhibited the most severe charring because detachment of the fire-resistant gypsum boards resulted in direct flame exposure of the CLT. Charring was concentrated around the joint regions, and the maximum charring depth was measured as 80 mm. The charred area extended over a relatively wide portion of the specimen width, with deep charring observed in regions corresponding closely to the locations of timber stud combustion. CW-WS-G-2 also exhibited localized charring around the joint regions, with a measured localized charring depth of 73 mm at the investigated flame-damaged region. The charring was concentrated in regions where thermocouples were not installed.
In contrast, only limited surface charring was observed in CW-WS-G-3, and no measurable charring depth was identified. In CW-WS-W-1, no distinct char layer was observed after the test, and most of the CLT surface remained visually intact.
The measured localized charring depths were 79 and 80 mm for CW-WS-G-1 and 73 mm for CW-WS-G-2, whereas CW-WS-G-3 exhibited only superficial charring and CW-WS-W-1 showed no observable charring. Because only two measurements were available for CW-WS-G-1 and one measurement for CW-WS-G-2, these values should be interpreted as localized measurements of severe damage rather than as spatially representative statistics for the entire wall specimens. These results indicate that the tested configurations incorporating staggered joints together with modified fastening details were associated with substantially reduced direct flame exposure and charring of the CLT.
It should be noted that the charring depths measured in this study resulted from localized flame exposure occurring only after the protective covering had provided fire protection for a certain period. Therefore, direct comparison of the observed charring behavior with the nominal charring rate of unprotected CLT is not appropriate. For protected CLT, the onset of charring is governed by the protective effect of the gypsum boards, the timing of joint damage, and the time at which the covering detaches. Accordingly, comparing charring rates solely on the basis of the total fire exposure duration may lead to an underestimation or overestimation of the actual fire behavior. The fire performance of protected CLT should therefore be interpreted by considering the integrity of the protective covering system and the characteristics of localized flame exposure, rather than relying solely on a nominal charring rate.

4. Conclusions

This study comparatively investigated the fire behavior and charring characteristics of Korean larch CLT walls under different protective-covering configurations. Particular emphasis was placed on differences in thermal response and charring behavior among protective-covering configurations incorporating different gypsum-board joint arrangements and fastening details. The following conclusions were drawn:
  • In CW-WS-G-1 and CW-WS-G-2, localized flame penetration and protective-covering damage were concentrated around the gypsum-board joint regions. At these locations, cracking and detachment of the covering were accompanied by combustion of the underlying timber studs and localized charring of the CLT. These observations indicate that, within the tested non-staggered joint configurations, damage around the board joints was closely associated with localized flame penetration and subsequent CLT charring.
  • In the specimens incorporating staggered joints together with modified screw lengths and fastening details, the integrity of the protective-covering system was largely maintained throughout the test, effectively limiting direct flame penetration. In contrast, specimens with non-staggered joint configurations and conventional fastening details exhibited concentrated damage around the joint regions, allowing flames to penetrate toward the CLT. Consequently, the specimens with staggered joints and modified fastening details exhibited limited internal temperature increases and substantially reduced CLT charring.
  • Internal temperature measurements characterized the overall thermal response but did not fully capture localized fire damage occurring outside the thermocouple locations. Therefore, evaluation of protected CLT walls should integrate temperature measurements with observations of protective-covering damage and post-fire charring.
  • A maximum measured localized charring depth of 80 mm was recorded in CW-WS-G-1, while a measured localized charring depth of 73 mm was recorded at the investigated flame-damaged region of CW-WS-G-2. These values represent localized damage measurements in individual specimens and should not be interpreted as a quantitative effect of gypsum-board thickness. In contrast, CW-WS-G-3 exhibited only superficial surface charring without a measurable charring depth, while no distinct charring was observed in CW-WS-W-1.
  • This study provides full-scale experimental data on the fire behavior and charring characteristics of Korean larch CLT walls incorporating protective covering systems representative of practical construction applications. The reported results characterize the thermal response and charring behavior of the tested assemblies and should not be interpreted as formal fire-resistance ratings under KS F 2257. The findings can provide a basis for the future development of fire-resistant design and performance assessment methods for protected CLT walls. However, only one specimen was tested for each configuration, and multiple parameters, including joint arrangement, fastening details, and insulation conditions, varied simultaneously in some specimens. In addition, the thermocouple configurations differed between specimen groups. These limitations restrict the extent to which the independent effects of individual parameters can be generalized. In addition, detailed manufacturing and material characterization data for the CLT panels and the thermal/fire properties of the insulation materials were not available in the retained test records. These limitations further restrict the quantitative interpretation and generalizability of the observed differences in fire behavior among the tested configurations. Further studies using replicated specimens and systematically controlled variables are therefore required to assess experimental variability and quantitatively determine the individual effects of covering material, joint configuration, fastening details, and insulation conditions.

Author Contributions

Conceptualization, Y.C. and J.A.; methodology, J.A. and Y.C.; validation, H.A., J.A. and Y.C.; formal analysis, H.A.; investigation, J.A.; resources, J.A. and Y.C.; data curation, H.A.; writing—original draft preparation, H.A.; writing—review and editing, J.A. and Y.C.; visualization, H.A.; supervision, Y.C.; project administration, Y.C.; funding acquisition, J.A. and Y.C. All authors have read and agreed to the published version of the manuscript.

Funding

This research was supported by the Ministry of Land, Infrastructure and Transport (MOLIT) of the Republic of Korea through the project “Development of an Integrated Management Platform for Building Materials (5th Year)” (Project No. 20260470-001).

Data Availability Statement

The data presented in this study are available from the corresponding author upon reasonable request.

Acknowledgments

The authors gratefully acknowledge the support of the Korea Institute of Civil Engineering and Building Technology (KICT) in conducting this research.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Ramage, M.H.; Burridge, H.; Busse-Wicher, M.; Fereday, G.; Reynolds, T.; Shah, D.U.; Wu, G.; Yu, L.; Fleming, P.; Densley-Tingley, D.; et al. The wood from the trees: The use of timber in construction. Renew. Sustain. Energy Rev. 2017, 68, 333–359. [Google Scholar] [CrossRef] [Scilit]
  2. D’Amico, B.; Pomponi, F.; Hart, J. Global potential for material substitution in building construction: The case of cross laminated timber. J. Clean. Prod. 2021, 279, 123487. [Google Scholar] [CrossRef] [Scilit]
  3. Buchanan, A.H.; Levine, S.B. Wood-based building materials and atmospheric carbon emissions. Environ. Sci. Policy 1999, 2, 427–437. [Google Scholar] [CrossRef] [Scilit]
  4. Brandner, R.; Flatscher, G.; Ringhofer, A.; Schickhofer, G.; Thiel, A. Cross laminated timber (CLT): Overview and development. Eur. J. Wood Wood Prod. 2016, 74, 331–351. [Google Scholar] [CrossRef] [Scilit]
  5. Karacabeyli, E.; Douglas, B. (Eds.) CLT Handbook: Cross-Laminated Timber, U.S. Edition; FPInnovations and Binational Softwood Lumber Council: Pointe-Claire, QC, Canada, 2013. [Google Scholar]
  6. White, R.H.; Dietenberger, M.A. Fire safety of wood construction. In Wood Handbook: Wood as an Engineering Material; General Technical Report FPL-GTR-282; Forest Products Laboratory, U.S. Department of Agriculture: Madison, WI, USA, 2021. [Google Scholar]
  7. Buchanan, A.H.; Abu, A.K. Structural Design for Fire Safety, 2nd ed.; John Wiley & Sons: Chichester, UK, 2017. [Google Scholar]
  8. European Committee for Standardization. EN 1995-1-2: Eurocode 5—Design of Timber Structures—Part 1-2: General—Structural Fire Design; CEN: Brussels, Belgium, 2004. [Google Scholar]
  9. Friquin, K.L. Material properties and external factors influencing the charring rate of solid wood and glue-laminated timber. Fire Mater. 2011, 35, 303–327. [Google Scholar] [CrossRef] [Scilit]
  10. Frangi, A.; Fontana, M.; Hugi, E.; Jübstl, R. Experimental analysis of cross-laminated timber panels in fire. Fire Saf. J. 2009, 44, 1078–1087. [Google Scholar] [CrossRef] [Scilit]
  11. Hadden, R.M.; Bartlett, A.I.; Hidalgo, J.P.; Santamaria, S.; Wiesner, F.; Bisby, L.A.; Deeny, S.; Lane, B. Effects of exposed cross laminated timber on compartment fire dynamics. Fire Saf. J. 2017, 91, 480–489. [Google Scholar] [CrossRef] [Scilit]
  12. Bartlett, A.I.; Hadden, R.M.; Hidalgo, J.P.; Santamaria, S.; Wiesner, F.; Bisby, L.A.; Deeny, S.; Lane, B. Auto-extinction of engineered timber: Application to compartment fires with exposed timber surfaces. Fire Saf. J. 2017, 91, 407–413. [Google Scholar] [CrossRef] [Scilit]
  13. König, J.; Walleij, L. One-Dimensional Charring of Timber Exposed to Standard and Parametric Fires in Initially Unprotected and Post-Protection Situations; Report I 9908029; Swedish Institute for Wood Technology Research: Stockholm, Sweden, 1999. [Google Scholar]
  14. Kolaitis, D.I.; Asimakopoulou, E.; Founti, M.A. Fire protection of light and massive timber elements using gypsum plasterboards and wood based panels: A large-scale compartment fire test. Constr. Build. Mater. 2014, 73, 163–170. [Google Scholar] [CrossRef] [Scilit]
  15. Hoehler, M.S.; Su, J.; Lafrance, P.-S.; Bundy, M.F.; Kimball, A.; Brandon, D.; Östman, B. Fire safety challenges of tall wood buildings: Large-scale cross laminated timber compartment fire tests. In Proceedings of the 10th International Conference on Structures in Fire (SiF’18), Belfast, UK, 6–8 June 2018; pp. 513–520. [Google Scholar]
  16. KS F 2257-1; Methods of Fire Resistance Test for Elements of Building Construction—General Requirements. Korean Standards Association: Seoul, Republic of Korea, 2019.
  17. KS F 2257-8; Method of Fire Resistance Test for Elements of Building Construction—Specific Requirements for Non-Loadbearing Vertical Separating Elements. Korean Standards Association: Seoul, Republic of Korea, 2019.
  18. ISO 834-1:1999; Fire-Resistance Tests—Elements of Building Construction—Part 1: General Requirements. ISO: Geneva, Switzerland, 1999.
  19. Yasir, M.; Macilwraith, A.; O’Ceallaigh, C.; Ruane, K. Effect of protective cladding on the fire performance of vertically loaded cross-laminated timber (CLT) wall panels. J. Struct. Integr. Maint. 2023, 8, 199–208. [Google Scholar] [CrossRef] [Scilit]
  20. Ramzi, S.; Hajiloo, H. Evaluation of the fall-off of gypsum board in lightweight and mass timber constructions and implications in fire resistance. Fire Saf. J. 2025, 156, 104455. [Google Scholar] [CrossRef] [Scilit]
  21. Sultan, M.A. Review of the NRC Canada Studies on Fire Resistance of Walls: Results, Research Gaps and Design Guidelines. Fire Technol. 2022, 58, 3405–3437. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.