Abstract
Hydrogen trapping is a key mechanism to mitigate hydrogen embrittlement (HE) in pipeline steels, yet how trapping behavior evolves during plastic deformation and which microstructural features are responsible remain poorly understood. In this work, interrupted slow strain rate tensile tests were performed on pipeline girth weld metal (WM) under 6.3 MPa H2 combined with thermal desorption spectroscopy (TDS), hydrogen microprint technique (HMT), and electron backscatter diffraction (EBSD). The results reveal that hydrogen trapping is highly strain-dependent. In the undeformed stage, only weak traps (Peak A at ~250 °C) and moderate traps (Peak B at ~500 °C) are present, as identified by TDS. Upon tensile straining to 15%, a new strong trap (Peak C at ~700 °C) emerges and intensifies, which is attributed to deformation-induced defects within acicular ferrite (AF). HMT shows that hydrogen distribution becomes homogeneous inside AF grains with increasing strain, while remaining localized at grain boundaries in proeutectoid ferrite (PF). EBSD indicates that AF undergoes more uniform plastic deformation and dislocation accumulation than PF. Most importantly, the WM with a higher AF content (74.5%) exhibits a significantly lower HE index (13.4%) than the WM with a lower AF content (53.9%, HE index 23.5%), confirming the beneficial role of AF. These findings demonstrate that AF is not merely a static hydrogen trap but a dynamic source of strain-induced strong traps, which effectively immobilize hydrogen and reduce embrittlement susceptibility under service-relevant deformation.
1. Introduction
Hydrogen embrittlement (HE) poses a major challenge to the safe transportation of hydrogen through steel pipelines [1,2,3]. Girth welds are particularly vulnerable due to their heterogeneous microstructure and residual stresses [4,5]. One promising mitigation strategy is to design microstructures that contain effective hydrogen traps, thereby reducing the concentration of diffusible hydrogen that can reach crack tips [6,7].
Acicular ferrite (AF)—a fine-grained, interlocking intragranular ferrite—has long been considered an ideal microstructure for HE resistance in pipeline steels [8,9,10]. Studies have shown that AF exhibits high hydrogen trapping efficiency and high resistance to hydrogen-induced cracking [11,12]. The conventional explanation focuses on its high density of high-angle grain boundaries (HAGBs) and fine grain size, which act as static traps and impede crack propagation [13,14,15,16,17,18]. However, these studies mainly focused on the effect of AF on hydrogen diffusion and hydrogen distribution under the undeformed stage and ignored its critical role during the deformation process.
However, in service, pipelines undergo local plastic deformation due to internal pressure fluctuations, thermal gradients, and ground settlement [19,20,21,22,23,24,25]. Under such dynamic conditions, the microstructure evolves. Dislocations multiply, grain boundaries rotate, and new defects form [26,27,28,29,30]. It remains unclear how hydrogen trapping behavior changes with increasing strain, whether the traps that exist in undeformed AF remain dominant after plastic deformation, and whether AF is still beneficial under these dynamic conditions [31,32,33,34,35].
Current understanding is largely based on static or pre-deformed specimens, which do not capture the co-evolution of hydrogen distribution and microstructure during active straining [36,37,38,39,40,41]. To address this gap, interrupted slow strain rate tensile (SSRT) tests were performed on pipeline girth weld metal in high-pressure hydrogen, and hydrogen desorption, hydrogen distribution, and microstructure were characterized at multiple strain levels. The aims are: (i) to reveal the strain-dependent evolution of hydrogen traps, (ii) to identify which microstructural constituents contribute to the deformation-induced traps, and (iii) to re-evaluate the role of AF content in HE susceptibility under dynamic loading.
2. Materials and Methods
In this study, an L245 pipe with an outer diameter of 610 mm and a wall thickness of 15.9 mm was selected as the welding base metal. A U-shaped groove was machined at the pipe end. Gas metal arc welding (GMAW) was employed using a shielding gas composed of 80% Ar and 20% CO2. This type of shielding gas is beneficial for improving arc stability, reducing welding spatter, ensuring weld formation and cutting down the cost. An ER70S-G solid wire conforming to the AWS A5.18 standard [42] was used as the welding consumable, with its chemical composition presented in Table 1. The welding process consisted of 7 layers and 8 passes. The AF content in the weld metal (WM) was varied by adjusting the welding process parameters. Meanwhile, the welding process parameters can guarantee adaptability to factors such as on-site assembly quality, groove machining quality and defect control. Detailed welding process parameters are listed in Table 2.
Table 1.
Chemical composition of welding wire.
Table 2.
Welding process parameters.
Slow strain rate tensile (SSRT) tests were conducted to evaluate the HE susceptibility of two WMs with different AF contents. Tensile specimens were machined from pipeline girth welds, with their longitudinal direction aligned with the circumferential direction of the weld. The specimens were sampled near the 3 o’clock position, featuring a gauge length of 30 mm and a diameter of 6 mm, as shown in Figure 1. After machining, the specimens were meticulously ground along their axial direction using 2000# fine-grit sandpaper (SHARPNESS; HuBei Yuli Abrasive Belts Group Co.,Ltd., Tongcheng,,China). Subsequently, the specimens were cleaned in a solution mixed with acetone (analytical grades, Sinopharm Chemical Reagent Co., Ltd., ShangHai, China) and alcohol (analytical grades, Sinopharm Chemical Reagent Co., Ltd., ShangHai, China) to completely remove grease or contaminants. A slow strain rate of 1 × 10−5/s was adopted. Tensile tests were conducted under both 6.3 MPa N2 and 6.3 MPa H2 atmospheres, with a gas purity of 99.999% for both environments. The SSRT testing procedure was carried out in accordance with the ASTM G129 standard [43] practice for slow strain rate testing to evaluate the susceptibility of metallic materials to environmentally assisted cracking. For each combination of WM and testing atmosphere, three repeated SSRT tests were performed.
Figure 1.
SSRT specimens’ position in the girt weld (a) and dimension (b).
Interrupted deformation experiments were performed on girth weld specimens obtained using welding procedure parameter No. 2, as listed in Table 2. Three strain levels were selected: 0% strain (undeformed stage, prior to loading), 10% strain (pre-necking, within the uniform deformation stage), and 15% strain (post-necking, within the non-uniform deformation stage). In addition, the specimen that fractured completely during tensile testing was also characterized. Specifically, WM specimens were pre-charged with hydrogen under a 6.3 MPa hydrogen atmosphere for at least 48 h, then loaded to the target strain levels, and subsequently unloaded. Afterwards, characterization tests including electron backscatter diffraction (EBSD), hydrogen microprint technique (HMT), and thermal desorption spectroscopy (TDS) were conducted on the specimens at different strain levels.
For the HMT test, a self-prepared AgBr photosensitive emulsion was used. A uniform monolayer of the AgBr photosensitive film was applied onto the surface of the hydrogen-charged specimen using the wire-winding method. After the specimen was allowed to stand in a darkroom to enable the reaction between hydrogen and the film, the unreacted AgBr was removed with a sodium thiosulfate solution. The distribution of Ag indirectly reflects the distribution of H. Finally, the distribution of silver in the metal microstructure was observed using a JEOL JSM-7200F scanning electron microscope (SEM) (JEOL Ltd., Tokyo, Japan) equipped with an Oxford X-MAX50 energy-dispersive X-ray spectrometer (EDS) (JEOL Ltd., Tokyo, Japan).
Prior to EBSD, the specimens were electropolished in a perchloric acid alcohol solution (8 vol%) at an electrolysis voltage of 30 V for 24 s. EBSD characterization was performed using a JSM-7200F SEM equipped with an EBSD detector (Oxford Instruments, Oxford, UK), operating at 20 kV, 70° tilt, and a step size of 0.2 μm. Data analysis was carried out using Channel 5 software (Version number 5.0.9.0) to obtain band contrast (BC) maps, inverse pole figure (IPF) maps, grain boundary maps, Kernel average misorientation (KAM) maps, and geometrically necessary dislocation (GND) density calculations. A maximum misorientation angle of 5° was used for KAM analysis.
For TDS, the specimens were heated at a rate of 200 °C/h over a temperature range from 30 °C to 900 °C and held at the maximum temperature for 10 min. In addition to the interrupted deformation specimens, TDS measurements were also performed on the fractured tensile specimens of both WMs after testing to fracture at 6.3 MPa H2 under the same SSRT conditions. These specimens were used to compare the hydrogen trapping characteristics between the AF-rich and AF-poor WMs at the final stage of deformation.
3. Results
3.1. Macroscopic HE Susceptibility of WMs with Different AF Contents
By adjusting the welding process parameters, two types of weld microstructures were obtained. The representative microstructures obtained with process parameters 1 and 2 (Table 2) are shown in Figure 2a,c, respectively, both of which consist of intragranular AF (dark gray) and intergranular proeutectoid ferrite (PF, light gray). The PF regions in the images were stained yellow using the image processing software ImageJ (Version number 1.46), and their area fraction in the image was statistically calculated. The staining results are presented in Figure 2b,d. Statistical analysis of the area fraction of the stained regions was performed, which reflects the PF content in the WM, with the remaining balance considered AF. It should be noted here that a certain amount of Widmanstätten ferrite (WF) is also present in the WM. In the statistics, WF is classified into the PF range. At least 30 microstructure maps were statistically recorded for each WM. The statistical results show that the AF contents of the two different WMs are 74.50% and 53.90%, respectively.
Figure 2.
Microstructures before and after PF staining at different AF contents. (a,b) ~74.50% AF; (c,d) ~53.90% AF; (a,c) original OM (un-stained); (b,d) PF stained in yellow.
The representative stress–strain curves for different WMs in N2 and H2 atmospheres are shown in Figure 3a. For both types of WM, the yield strength and tensile strength are essentially the same in both N2 and H2 gas environments. However, hydrogen significantly reduces the total strain of the WM (reflecting the overall deformation capability), and the extent of this reduction depends on the WM type: the hydrogen-induced degradation of strain capability is markedly smaller for the WM with an AF content of ~74.50% than for that with ~53.90% AF.
Figure 3.
Representative stress–strain curves in N2 and H2 (a) and HEI (b) for WMs with varying AF contents. In (a), dashed lines mark the total strain at fracture, and leftward arrows show the H2-induced decrease in total strain.
The reduction in area reflects the plastic deformation capability of a material; a higher reduction in area (Ψ) indicates a stronger plastic deformation ability. The loss in Ψ caused by hydrogen is commonly used to quantitatively evaluate the HE susceptibility of a material:
where HEI is the HE index, and ΨN2 and ΨH2 are the reductions in areas of the same WM tested in N2 and H2, respectively. The calculated HE index for the two WMs with different AF contents tested in 6.3 MPa H2 (relative to the N2 environment) is presented in Figure 3b. Clearly, the HEI at an AF content of approximately 74.5% (13.40%) is lower than that at an AF content of approximately 53.9% (23.51%). These results indicate that a higher AF content is beneficial for reducing the HE susceptibility of the WM.
3.2. Strain-Dependent Microstructure, Hydrogen Distribution, and Trapping Behavior in the WM
3.2.1. Strain-Dependent Microstructure Evolution
Figure 4a–c show the BC maps with different deformation magnitudes. It can be observed that the grain size of PF remains relatively unchanged with increasing strain. However, the grain size of AF gradually decreased from 4.8 μm in the undeformed stage to 3.2 μm under uniform plastic deformation, and further to 2.1 μm under non-uniform plastic deformation. This indicates that increased plastic deformation led to the fragmentation of AF grains.
Figure 4.
Microstructure characterization with different deformation magnitudes. (a–c) BC maps; (d–f) IPF; (g–i) statistical frequency of local misorientation.
Figure 4d–i show the IPF maps with grain boundary angles and the statistical frequency of local misorientation at grain boundaries (GBs), respectively. The grain boundary angles are classified into low-angle grain boundaries (LAGBs, 3° ≤ LAGBs < 15°, blue lines), medium-angle grain boundaries (MAGBs, 15° ≤ MAGBs < 45°, green lines), and high-angle grain boundaries (HAGBs, 45° ≤ HAGBs, red lines). It can be observed that the GBs of PF are mainly low-angle grain boundaries, whereas those of AF predominantly consist of MAGBs and HAGBs. This indicates that AF contributes the majority of HAGBs. As the strain magnitude increases, newly formed and discontinuous LAGBs appear in local regions within both PF and AF grains, indicating significant plastic deformation in these areas. Furthermore, with increasing strain magnitude, the proportion of sub-angle grain boundaries (SAGBs< 3°) gradually rises from 45.45% to 58.61% and then to 68.74%. In contrast, the proportion of HAGBs gradually decreases from 32.14% to 23.66% and then to 15.58%. It should be noted that this does not imply a reduction in the total density of HAGBs; rather, it reflects a substantial increase in local dislocation density, leading to the formation of more SAGBs.
Figure 5 shows the distributions of KAM and GNDs at different strain magnitudes. In the undeformed stage, higher KAM values are primarily concentrated at low-angle grain boundaries (LAGBs) of PF, as indicated by white arrows. As the strain magnitude increases, KAM rises inside both PF grains (red arrows) and AF grains (yellow arrows). Moreover, the KAM distribution inside AF grains is more uniform, whereas localized KAM concentration occurs inside PF grains. In other words, strain is evenly distributed within AF grains, while local strain concentration occurs in PF grains. This could be primarily attributed to the fine and densely distributed AF grains, which preferentially facilitate coordinated plastic deformation. In contrast, coarse PF grains surrounded by AF deform with difficulty in a coordinated manner. Figure 5d–f reveal that as the deformation level increases, dislocation density gradually rises from 5.96 to 10.43 and then to 12.65 (unit: 1.0 × 1014 m−3). Meanwhile, dislocations are predominantly distributed in the AF region. In the undeformed stage, a certain degree of dislocation concentration exists at local grain boundaries, as shown by magenta arrows in Figure 5g. As the deformation extent increases, the dislocation density at the grain boundaries of PF increases slightly, as indicated by the white arrows in Figure 5h. It should be noted that the dislocation density at the boundaries and inside AF grains (including fragmented grains) increases significantly.
Figure 5.
Distributions of both KAM and GNDs with different strain magnitudes. (a–c) KAM maps; (d–i) GND maps.
3.2.2. Strain-Dependent Hydrogen Distribution (HMT)
Figure 6 shows the distribution of both the microstructure and Ag element (as a tracer for hydrogen) with different strain magnitudes. During the undeformed stage, H atoms are primarily distributed at the grain boundaries of both PF and AF, as indicated by the red and white arrows in Figure 6d, respectively. It is noteworthy that this situation is basically consistent with the strain distribution of PF and distribution of AF in HAGBs. This indicates that strain concentration locations and grain boundaries serve as the initial hydrogen trapping sites. As the deformation magnitude increases to the uniform plastic deformation stage, besides the H atom aggregation at grain boundaries, the remaining H atoms are distributed relatively evenly inside the grains of both PF and AF. This could be primarily attributed to the plastic deformation occurring inside the grains of these two microstructures, leading to an increase in lattice defects such as dislocations. In turn, more H atoms can be trapped. As the deformation magnitude increases to the non-uniform plastic deformation stage, the H atoms distribution becomes more uniform in the AF region, as shown in the white box in Figure 6f. This is mainly because AF is more prone to coordinated plastic deformation. As a result, the AF grains underwent fragmentation, leading to the formation of new and finer grains, as shown in Figure 4f and Figure 5f. In addition, for PF, the H atoms remain concentrated at the grain boundaries of PF, as indicated by the red arrows in Figure 5f, which can be ascribed to the fact that the strain of PF remains primarily distributed at grain boundaries, as indicated by the white arrows in Figure 5h,i.
Figure 6.
Distributions of both microstructure and Ag element with different strain magnitudes. (a–c) Microstructure under SEM; (d–f) Ag element distribution. In (e,f), white boxes enclose acicular ferrite (AF), and yellow boxes mark proeutectoid ferrite.
3.2.3. Strain-Dependent Hydrogen Traps (TDS)
Figure 7 shows the TDS results at the different deformation stages. Figure 7a shows hydrogen desorption at the undeformed stage. It can be observed that a hydrogen desorption peak (Peak A1) appears at approximately 250 °C, and another hydrogen desorption peak (Peak B1) emerges at around 500 °C. Peak A1 corresponds to some weak hydrogen traps, while Peak B1 is a mixture of other weak hydrogen traps (such as HAGBs) and strong hydrogen traps (such as precipitates). The HAGBs mainly originate from the AF, as shown in Figure 4d–i. And the precipitates mainly come from the heterogeneous nucleation of the AF, such as Ti(C,N) [44,45,46]. As a result, H atoms are distributed at the grain boundaries of AF and PF under the undeformed stage, as indicated by the white and red arrows in Figure 6a.
Figure 7.
TDS results for different strain magnitudes: (a) undeformation stage; (b) uniform plastic deformation stage; (c) non-uniform deformation stage; (d) complete tensile fracture.
Figure 7b shows the hydrogen desorption behavior at the stage of uniform plastic deformation. It can be observed that there are three hydrogen desorption peaks, namely, one near 250 °C (Peak A2), one near 500 °C (Peak B2), and one near 700 °C (Peak C1). Essentially, the former corresponds to Peak A1 in Figure 7a and still relates to weak hydrogen traps. The latter two peaks, namely the desorption peaks appearing at 500 °C (Peak B2) and 700 °C (Peak C1), are associated with hydrogen traps with different binding energies. However, the specific types of these hydrogen traps are difficult to determine.
Figure 7c shows the hydrogen desorption behavior during the non-uniform deformation stage. It can be observed that the relative height of the first two hydrogen desorption peaks (Peak A3 and Peak B3) decreased compared with the uniform plastic deformation stage. The height of hydrogen desorption Peak C2 at around 700 °C is still the highest. Figure 7d shows the hydrogen desorption behavior after complete tensile fracture. Notably, the hydrogen desorption Peak A4 and Peak B4 have almost vanished, while high-temperature Peak C3 remains unchanged. This indicates that Peak A and Peak B could include contributions from other weak traps, such as grain boundaries, vacancies, and other microstructures [47]. However, this study focuses on identifying the source of the strong hydrogen traps responsible for the high-temperature Peak C.
Note that Figure 7d uses a different y-axis scale from Figure 7b,c. As the tensile strain increases, the high-temperature Peak C emerges, and its associated hydrogen content progressively rises, indicating that the number of strong hydrogen traps increases with plastic deformation. Specifically, the sample at the complete tensile fracture stage exhibits a substantially higher amount of hydrogen released from Peak C3 than samples at lower strain magnitudes. Based on microstructure characterization under different deformation stages, besides the unchanged precipitates, the difference between them lies in the fact that there are more dislocation defects around the AF (as shown in Figure 5). Thus, it could be inferred that the high-temperature Peak C3 is mainly associated with high-binding-energy hydrogen traps formed by the evolution of deformation-induced defects. A large number of dislocations proliferate and form tangled dislocations inside AF during straining, which are generally regarded as strong hydrogen traps. Shang et al. [37] also verified that tangled dislocations can act as potent hydrogen traps.
3.3. Comparison of Hydrogen Desorption from Fractured Specimens of AF-Rich and AF-Poor WMs
To directly assess whether a higher AF content leads to the formation of more strain-induced strong hydrogen traps, TDS measurements were performed on the fractured tensile specimens of both WMs (AF content 74.5% and 53.9%) after testing in 6.3 MPa H2. Both specimens were deformed to complete fracture under identical conditions (strain rate 1 × 10−5/s, 6.3 MPa H2, room temperature). The TDS results are presented in Figure 8.
Figure 8.
Comparison of TDS spectra from fractured specimens of AF-rich and AF-poor WMs tested in 6.3 MPa H2.
For the AF-poor WM (53.9% AF), the TDS spectrum shows a prominent high-temperature desorption peak at approximately 700 °C (Peak C), accompanied by two weaker peaks at around 250 °C (Peak A) and 500 °C (Peak B). For the AF-rich WM (74.5% AF), the high-temperature Peak C is substantially more intense, with an integrated hydrogen content approximately 140% higher than that of the AF-poor WM (quantified by peak area integration). In contrast, the low-temperature peaks (A and B) are slightly lower in the AF-rich WM.
These results indicate that, under identical deformation and hydrogen charging conditions, the AF-rich WM traps significantly more hydrogen in strong traps (Peak C) than the AF-poor WM. Since the high-temperature peak has been associated with deformation-induced tangled dislocations within AF (Section 3.2.3), the higher intensity of Peak C in the AF-rich WM directly demonstrates that a larger volume fraction of AF generates stronger trapping sites during plastic deformation. Consequently, a greater proportion of hydrogen is immobilized in these deep traps, reducing the concentration of diffusible hydrogen that can participate in embrittlement. This provides a direct mechanistic explanation for the lower HE index of the AF-rich WM (Section 3.1).
4. Discussion
4.1. Mechanisms Underlying the Reduced HE Susceptibility in AF-Rich WM
Section 3.1 demonstrates that the WM with a higher AF content (74.5%) has a significantly lower HE index (13.4%) than the one with lower AF content (53.9%, HE index 23.5%). The detailed characterization in Section 3.2, although performed on the AF-poor WM, provides critical insights into the mechanism that can explain the beneficial role of a higher AF fraction.
In the AF-poor WM, TDS (Figure 7) revealed that plastic deformation induces a new, strong hydrogen trap (Peak C at ~700 °C), which becomes increasingly dominant with rising strain. Concurrently, EBSD (Figure 4 and Figure 5) showed that AF undergoes uniform plastic deformation, grain fragmentation, and a substantial increase in GND density, especially inside AF grains. HMT (Figure 6) demonstrated that hydrogen redistributes from grain boundaries to a more uniform distribution within AF grains as deformation proceeds. These observations lead to the following interpretation: AF is not merely a static trap provider (via HAGBs and fine grains) but dynamically generates strong traps in the form of tangled dislocations during plastic deformation.
When the AF content is higher, a larger volume fraction of the microstructure contributes to this strain-induced trapping effect. Consequently, under the same applied strain, an AF-rich WM traps more hydrogen in strong, immobile states, reducing the concentration of diffusible hydrogen that can migrate to crack tips and cause embrittlement. This explains the lower HE index despite the higher overall hydrogen uptake (as suggested by the larger Peak C area in TDS). In contrast, PF deforms heterogeneously, retains hydrogen primarily at grain boundaries, and does not develop uniformly distributed strong traps, making it less effective at immobilizing hydrogen under dynamic loading.
4.2. The Dynamic Role of AF as a Strain-Induced Hydrogen Trap
Traditional studies have emphasized the static trapping ability of AF due to its high density of HAGBs and fine grain size [13,14,15,16,17,18]. The present work extends this understanding by showing that AF exhibits excellent deformation compatibility (Figure 5) and that its trapping capacity increases with plastic strain (Figure 7). This is a critical finding for service conditions where local plastic deformation is inevitable.
The emergence of the ~700 °C desorption peak (Peak C) is particularly noteworthy. Its binding energy is higher than that of typical HAGBs or precipitates, which usually desorb at lower temperatures [48]. The fact that this peak intensifies with strain and persists after fracture, while lower-temperature peaks (A and B) diminish, indicates that the strong traps are directly linked to deformation-induced defects within AF—most plausibly, tangled dislocation networks and associated vacancies or dislocation-cell boundaries. These defects are known to act as deep hydrogen traps [37].
By contrast, PF grains, being coarser and surrounded by harder AF, experience strain localization at grain boundaries (Figure 5h,i). This leads to hydrogen remaining concentrated at PF boundaries (Figure 6f), which is a classic configuration for intergranular crack initiation. Therefore, the presence of AF not only provides strong traps but also promotes a more uniform strain distribution, avoiding detrimental local hydrogen buildup.
4.3. Implications for Hydrogen-Resistant Weld Design
From an engineering perspective, this study suggests that increasing the AF content in pipeline girth welds is a viable strategy to enhance resistance to HE under dynamic loading conditions. More broadly, microstructures that can develop uniform, high-density dislocation structures during deformation (i.e., that exhibit good “deformation compatibility”) are desirable. Such microstructures act as self-tunable hydrogen traps. They are relatively less effective in the undeformed stage but become increasingly effective as deformation proceeds—exactly when hydrogen-induced cracking is most threatening.
Future weld procedure development should aim to maximize AF formation, for example, by optimizing heat input, cooling rate, and inclusion engineering to promote intragranular nucleation of AF. It is also worth exploring whether other microconstituents (e.g., fine bainite) exhibit similar strain-induced trapping behavior.
5. Conclusions
In the present work, the dynamic evolution of microstructure and hydrogen distribution in pipeline girth welds was explored, and the HE index of WMs with different AF contents was investigated. The main findings are concluded as follows:
- (1)
- The WM with a higher AF content (74.5%) exhibits a significantly lower HE index (13.4%) than that with a lower AF content (53.9%, HE index 23.5%), confirming that a higher AF fraction reduces HE susceptibility.
- (2)
- During plastic deformation, AF undergoes uniform strain distribution, grain fragmentation, and a substantial increase in dislocation density, whereas PF deforms heterogeneously with strain localized at grain boundaries.
- (3)
- Hydrogen distribution evolves from being concentrated at grain boundaries in the undeformed stage to a more uniform distribution inside AF grains with increasing strain, consistent with the proliferation of dislocations. In PF, hydrogen remains localized at grain boundaries.
- (4)
- A new, strong hydrogen trap (desorption peak at ~700 °C, Peak C) emerges during plastic deformation and intensifies with strain. This trap is attributed to deformation-induced defects—most likely tangled dislocations—within AF. The presence of such traps immobilizes hydrogen, reduces diffusible hydrogen, and thereby lowers embrittlement susceptibility. Thus, AF acts not only as a static trap but also as a dynamic source of strain-induced strong hydrogen traps.
Author Contributions
Methodology, L.H., Y.W., J.G. and X.L.; Formal analysis, Y.W. and S.S.; Investigation, L.H., J.G. and X.L.; Data curation, L.H., J.G. and S.S.; Writing—original draft, L.H., J.G. and W.Z.; Writing—review and editing, L.H., W.Z. and X.L.; Supervision, W.Z.; Funding acquisition, W.Z. All authors have read and agreed to the published version of the manuscript.
Funding
This work was supported by the Jiangsu Frontier Technology R&D Program (No. BF2024057).
Data Availability Statement
The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.
Conflicts of Interest
Authors Laihui Han, Yingwei Wang and Jin Gao were employed by the company Sinopec Petroleum Engineering Co., Ltd. The remaining authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as potential conflicts of interest.
References
- Global Hydrogen Review 2025, Revised version. In Proceedings of the International Energy Agency, Paris, France, 29 October 2025.
- Witkowski, A.; Rusin, A.; Majkut, M.; Stolecka, K. Analysis of compression and transport of the methane/hydrogen mixture in existing natural gas pipelines. Int. J. Press. Vessel. Pip. 2018, 166, 24–34. [Google Scholar] [CrossRef] [Scilit]
- Yu, L.L.; Feng, H.; Li, S.N.; Guo, Z.C.; Chi, Q. Study on Hydrogen Embrittlement Behavior of X65 Pipeline Steel in Gaseous Hydrogen Environment. Metals 2025, 15, 596. [Google Scholar] [CrossRef] [Scilit]
- Wang, Y.; Li, S.R.; Zhang, H.L.; Zhao, Q.K.; Liu, X.F.; Zhao, D.; Cao, Y.G. Study on the hydrogen diffusion behavior in pipeline girth welds based on segmented moving double ellipsoid heat source model. Int. J. Press. Vessel. Pip. 2025, 217, 105556. [Google Scholar] [CrossRef] [Scilit]
- Wang, H.Y.; Ming, H.L.; Hou, D.C.; Wang, J.Q.; Ke, W.; Han, E.-H. Comprehensive analysis of the influence of hydrogen blending ratio on the hydrogen embrittlement behavior of X42 pipeline steel. Int. J. Press. Vessel. Pip. 2025, 216, 105524. [Google Scholar] [CrossRef] [Scilit]
- Karani, A.; Shajan, N.; Bakshi, S.D.; Karande, P.H.; Agrawal, A.; Kulkarni, A.; Ghosh, P.; Arora, K.S. Effect of weld oxides on hydrogen induced cracking of API X65 sour high frequency induction welded pipe. Int. J. Press. Vessel. Pip. 2025, 216, 105516. [Google Scholar] [CrossRef] [Scilit]
- Peng, S.Y.; Zhang, Y.-H.; Chai, C.; Pei, Y.B.; Zhou, D.W.; Tian, C. Characterization of quasi-cleavage fracture of pre-strained X80 pipeline steel subjected to SSRT tests in gas hydrogen. Int. J. Press. Vessel. Pip. 2025, 214, 105448. [Google Scholar] [CrossRef] [Scilit]
- Hou, Y.H.; Huang, Y.Y.; Li, G.Q. Mechanisms of core-shell construction, interface optimization, and energy level reconstruction for hydrogen embrittlement resistance of yttrium modified X80 pipeline steel. Int. J. Hydrog. Energy 2025, 156, 159364. [Google Scholar] [CrossRef] [Scilit]
- Komoda, R.; Yamada, K.; Kubota, M.; Ginet, P.; Barbier, F.; Furtado, J.; Prost, L. The inhibitory effect of carbon monoxide contained in hydrogen gas environment on hydrogen-accelerated fatigue crack growth and its loading frequency dependency. Int. J. Hydrog. Energy 2019, 44, 29007–29016. [Google Scholar] [CrossRef] [Scilit]
- Komoda, R.; Kubota, M.; Staykov, A.; Ginet, P.; Barbier, F.; Furtado, J.; Prost, L.; Nagao, A. Effect of gas pressure on hydrogen environment embrittlement of carbon steel A106 in carbon monoxide mixed hydrogen gas. Met. Mater. Trans. A 2022, 53, 74–85. [Google Scholar] [CrossRef] [Scilit]
- Somerday, B.P.; Sofronis, P.; Nibur, K.A.; Marchi, C.S.; Kirchheim, R. Elucidating the variables affecting accelerated fatigue crack growth of steels in hydrogen gas with low oxygen concentrations. Acta Mater. 2013, 61, 6153–6170. [Google Scholar] [CrossRef] [Scilit]
- Nan, Z.; Komoda, R.; Yamada, K.; Volkert, C.; Tian, L.; Kirchheim, R.; Sofronis, P.; Zahra, H.; Dadfarnia, M.; Kubota, M.; et al. Effect of ammonia impurity on hydrogen embrittlement of SCM440 low-alloy steel in hydrogen gas. In Proceedings of the Thirtieth International Ocean and Polar Engineering Conference, Shanghai, China, 11−16 October 2020; pp. 3030–3035. [Google Scholar]
- Fan, J.; Dong, L.; Sun, D.; Ma, C.; Zhang, Z.; Wei, B.; Wang, Q.; Liu, L. Microstructure and gaseous hydrogen embrittlement of gas metal arc welding, cold metal transfer, and flux-cored arc welding weldments of X52 steel. Corros. Sci. 2026, 258, 113442. [Google Scholar] [CrossRef] [Scilit]
- Consuegra, R.F.; Alexandrov, T.B. Evaluating hydrogen embrittlement susceptibility in pipeline steel welds. Weld. World 2026, 1–13. Available online: https://link.springer.com/article/10.1007/s40194-026-02425-y (accessed on 21 June 2026). [CrossRef] [Scilit]
- Boot, T.; Riemslag, T.; Reinton, E.; Liu, P.; Walters, C.L.; Popovich, V. Assessing the susceptibility of existing pipelines to hydrogen embrittlement. In TMS 2021 150th Annual Meeting & Exhibition Supplemental Proceedings; Springer: Berlin/Heidelberg, Germany, 2021; pp. 722–729. [Google Scholar] [CrossRef] [Scilit]
- Li, T.; Zhang, H.; Hu, W.; Li, K.; Wang, Y.; Lin, Y. Hydrogen Embrittlement Behavior and Applicability of X52 Steel in Pure Hydrogen Pipelines. Materials 2025, 18, 3417. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Xu, Y.; Huang, F.; Elsabbagh, M.A.; Hu, Q.; Song, S.; Li, L.; Zhang, H.; Peng, Z.; Zhang, S.; Liu, J.; et al. Interfacial engineering of inclusions for synergistic toughening and hydrogen embrittlement resistance in high-strength pipeline steels. npj Mater. Degrad. 2025, 9, 160. [Google Scholar] [CrossRef] [Scilit]
- Masoud, M.; Bernd, L.; Mahdieh, S.; Willidal, T.; Hojo, T.; Mori, G. Hydrogen trapping and desorption affected by ferrite grain boundary types in shielded metal and flux-cored arc weldments with Ni addition. Int. J. Hydrog. Energy 2022, 47, 20676–20683. [Google Scholar] [CrossRef] [Scilit]
- Peng, Z.; Majid, L.; Zhang, P.; Laleh, M.; Hughes, A.E.; Marceau, R.K.; Hilditch, T.; Tan, M.Y. Effect of microstructure on hydrogen embrittlement and hydrogen-induced cracking behaviour of a high-strength pipeline steel weldment. Corros. Sci. 2024, 227, 111764. [Google Scholar] [CrossRef] [Scilit]
- Nguyen, T.T.; Tak, N.; Park, J.; Nahm, S.H.; Beak, U.B. Hydrogen embrittlement susceptibility of X70 pipeline steel weld under a low partial hydrogen environment. Int. J. Hydrog. Energy 2020, 45, 23739–23753. [Google Scholar] [CrossRef] [Scilit]
- Yan, C.B.; Feng, S.Q.; Zhang, H.Y.; Chen, J.; Fu, L.-W. Cyclic pressure testing of full-scale pipes to evaluate fatigue damage to girth welds containing welding defects. Eng. Fail. Anal. 2025, 169, 109216. [Google Scholar] [CrossRef] [Scilit]
- Zhao, G.Z.; Li, J.D.; Liang, H.Y. Bending stress and deformation characteristics of gas pipelines in mountainous terrain under the influence of subsidence. Energies 2025, 18, 3323. [Google Scholar] [CrossRef] [Scilit]
- Zheng, T.; Liang, Z.; Zhang, L.; Tang, S.; Cui, Z. Safety assessment of buried natural gas pipelines with corrosion defects under the ground settlement. Eng. Fail. Anal. 2021, 129, 105663. [Google Scholar] [CrossRef] [Scilit]
- Tang, H.; Li, C.P.; Xu, M.; Lv, L.; Sun, C.; Xing, B.; Qu, S.; Hua, Z. Fatigue crack growth behavior of X80 pipeline girth welded joints in natural gas/mixed hydrogen environment: Experimental and numerical investigations. Corros. Sci. 2025, 252, 112959. [Google Scholar] [CrossRef] [Scilit]
- Yu, J.; Yan, W.; Bao, R.; Zhou, X.; Xu, M.; Liu, X.; Li, Z.; Sun, Q.; Du, Y.; Zhang, M.; et al. Mechanical response and failure analysis of X80 buried pipeline under fault action. Eng. Fail. Anal. 2026, 183, 110256. [Google Scholar] [CrossRef] [Scilit]
- Shuai, K.; Liu, H.; Li, M.; Yin, S.; Li, B.; Wang, B.; Liu, Q.; Jia, S. Hydrogen Embrittlement Sensitivity of X70 Welded Pipe Under a High-Pressure Pure Hydrogen Environment. Materials 2024, 17, 5818. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Martínez-Pañeda, E.; Harris, D.Z.; Fuentes-Alonso, S.; Scully, J.R.; Burns, J.T. On the suitability of slow strain rate tensile testing for assessing hydrogen embrittlement susceptibility. Corros. Sci. 2019, 163, 108291. [Google Scholar] [CrossRef] [Scilit]
- Moallemi, M.; Kim, J.S.; Cho, J.H.; Kim, S.H.; Javaheri, V. Design considerations for hydrogen embrittlement resistance: The influence of dislocation density and substructures on hydrogen-assisted cracking in high-Mn TWIP steel. Mater. Des. 2025, 256, 114298. [Google Scholar] [CrossRef] [Scilit]
- Depover, T.; Escobar, P.D.; Wallaert, E. Effect of hydrogen charging on the mechanical properties of advanced high strength steels. Int. J. Hydrog. Energy 2014, 39, 4647–4656. [Google Scholar] [CrossRef] [Scilit]
- Olden, V.; Alvaro, A.; Akselsen, M.O. Hydrogen diffusion and hydrogen influenced critical stress intensity in an API X70 pipeline steel welded joint—Experiments and FE simulations. Int. J. Hydrog. Energy 2012, 37, 11474–11486. [Google Scholar] [CrossRef] [Scilit]
- Takai, K.; Shoda, H.; Suzuki, H. Lattice defects dominating hydrogen-related failure of metals. Acta Mater. 2008, 56, 5158–5167. [Google Scholar] [CrossRef] [Scilit]
- Boot, T.; Kömmelt, P.; Hendrikx, A.W.R.; Böttger, A.J.; Popovich, V. Effect of plastic deformation on the hydrogen embrittlement of ferritic high strength steel. npj Mater. Degrad. 2025, 9, 39. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Islam, A.; Li, Q.; Storimans, E.; Ton, K.; Alam, T.; Farhat, Z.N. Effect of microstructure on hydrogen permeation and trapping in natural gas pipeline steels. npj Mater. Degrad. 2025, 9, 70. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Zhou, G.J.; Liu, Q.L.; Zhou, H.; Shi, L.; Wang, H.; Liu, X.; Zheng, W. Hydrogen trapping characteristics of X52 pipeline base metal and weld and their influence on the embrittlement susceptibility under different hydrogen charging conditions. J. Pipeline Sci. Eng. 2025, 5, 100387. [Google Scholar] [CrossRef] [Scilit]
- Moshtaghi, M.; Safyari, M.; Mori, G. Combined thermal desorption spectroscopy, hydrogen visualization, HRTEM and EBSD investigation of a Ni–Fe–Cr alloy: The role of hydrogen trapping behavior in hydrogen-assisted fracture. Mater. Sci. Eng. A 2022, 848, 143428. [Google Scholar] [CrossRef] [Scilit]
- Jack, A.T.; Webb, A.M.; Rahman, M.K.; Fazeli, F.; Szpunar, J. Hydrogen uptake and embrittlement behavior in pipeline steels: Insights from slow strain rate testing and synchrotron micro-CT imaging. Eng. Fail. Anal. 2025, 179, 109419. [Google Scholar] [CrossRef] [Scilit]
- Shang, J.; Guo, J.X.; Hua, Z.L.; Xing, B.; Cui, T.; Wei, H. Effects of plastic deformation on hydrogen trapping and hydrogen distribution in X80 pipeline steel. Int. J. Hydrog. Energy 2025, 136, 1306–1316. [Google Scholar] [CrossRef] [Scilit]
- Zhang, X.; Yang, Z.; Li, W. Effect of plastic deformation on hydrogen trapping behavior and hydrogen embrittlement sensitivity of 7075 aluminum alloy. Mater. Charact. 2025, 229, 115502. [Google Scholar] [CrossRef] [Scilit]
- Shikomba, N.; Boellinghaus, T.; Konert, F.; Sobol, O.; Blasón, S.; Ohijeagbon, I.O.; Krafft, E.; Staudt, T. Resistance of welded low-alloyed pressure vessel and pipeline steels in gaseous hydrogen. Weld. World 2025, 1–15. [Google Scholar] [CrossRef] [Scilit]
- Ning, Y.; Yang, P.X.; Ming, S. Investigation on Hydrogen Embrittlement Behaviour of X65 Steel Base Metal and Girth Weld Metal under In-Situ Hydrogen Environment. Metals 2026, 16, 628. [Google Scholar] [CrossRef] [Scilit]
- Entezari, E.; Velázquez, J.L.G.; Mohtadi-Bonab, M.A.; López, D.R.; Zúñiga, M.A.B.; Davani, R.K.Z.; Szpunar, J. Experimental observations of nucleation and crack growth paths of hydrogen-induced cracking in pipeline steel. Eng. Fail. Anal. 2023, 154, 107650. [Google Scholar] [CrossRef] [Scilit]
- WS A5.18/A5.18M:2025; Specification for carbon steel electrodes and rods for gas shielded arc welding. American Welding Society: Miami, FL, USA, 2025.
- ASTM G129-21; Standard practice for slow strain rate testing to evaluate the susceptibility of metallic materials to environmentally assisted cracking. ASTM International: West Conshohocken, PA, USA, 2021.
- Bai, J.; Zhang, M.; Ma, H.; Li, Z.; Mao, W.; Li, J.; Zhang, J. Investigation of hydrogen embrittlement in welded joints of the L360MH pipeline steel for hydrogen transportation. Corros. Sci. 2025, 251, 112940. [Google Scholar] [CrossRef] [Scilit]
- Babu, S.S. The mechanism of acicular ferrite in weld deposits. Curr. Opin. Solid State Mater. Sci. 2004, 8, 267–278. [Google Scholar] [CrossRef] [Scilit]
- Ricks, R.A.; Howell, P.R.; Barritte, G.S. The nature of acicular ferrite in HSLA steel weld metals. J. Mater. Sci. 1982, 17, 732–740. [Google Scholar] [CrossRef] [Scilit]
- Saito, K.; Takai, K. Hydrogen desorption behavior trapped in various microstructures of high-strength steels using thermal desorption analysis. Met. Mater. Trans. A 2021, 52, 531–543. [Google Scholar] [CrossRef] [Scilit]
- Nagumo, M.; Takai, K. The predominant role of strain-induced vacancies in hydrogen embrittlement of steels: Overview. Acta Mater. 2019, 165, 722–733. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.