Influence of Post-Weld Heat Treatments on the Hydrogen Embrittlement Susceptibility of API 5L X52N Pipeline Steel Welded Joints

,
,
and
Tecnalia, Basque Research and Technology Alliance (BRTA), Mikeletegi Pasealekua 2, 20009 Donostia/San Sebastián, Gipuzkoa, Spain
*
Author to whom correspondence should be addressed.
This article belongs to the Section Metal Failure Analysis

Abstract

This work evaluates the influence of post-weld heat treatments (PWHT) on the hydrogen embrittlement (HE) susceptibility of girth-welded API 5L X52N pipeline steels. Four conditions were analyzed: as-welded, two stress-relief treatments (HT1 at 635.1 °C and HT3 at 593.5 °C), and a normalizing treatment (HT2 at 911.4 °C). Mechanical characterization was performed via Slow Strain Rate Tests (SSRT) in high-pressure hydrogen (160 bar) and air. Normalizing (HT2) homogenized the joint microstructure and increased plastic elongation in air and hydrogen; however, it produced the lowest reduction-of-area retention among the cross-weld conditions ( HEI RA = 0.57), indicating greater hydrogen sensitivity during localized final fracture, while its plastic-elongation retention remained comparable to the as-welded condition. Among stress-relief treatments, HT1 showed the most favorable ductility retention in the filler metal, although this observation rests on a single FM-fractured specimen per condition and is not statistically conclusive. Fractographic analysis revealed a transition from ductile dimples in air to mixed-mode fracture in hydrogen, characterized by transgranular quasi-cleavage. The study suggests that acicular ferrite in the filler metal offers greater resistance to hydrogen-induced crack propagation than the equiaxed polygonal-ferrite microstructure produced by normalizing.

1. Introduction

The transition toward a hydrogen-based energy system depends in part on the ability to repurpose existing natural-gas pipeline networks for hydrogen transport, making the hydrogen compatibility of pipeline steels a critical technical challenge [1,2,3]. Hydrogen embrittlement (HE) is one of the principal degradation mechanisms affecting steels exposed to hydrogen, typically manifesting as reduced ductility, increased susceptibility to premature fracture, and accelerated subcritical crack growth [3,4,5]. Its severity depends not only on steel composition but also on microstructure, service environment, stress state, and loading conditions, making reliable prediction challenging [2]. This challenge is particularly acute in welded pipeline systems, where welding introduces pronounced microstructural heterogeneity and residual stresses that can promote hydrogen-assisted damage [4,5].
Welded joints are widely recognized as the “weakest links” in hydrogen transport systems [3,5,6]. Furthermore, the process introduces welding defects (such as inclusions and porosities) and high residual tensile stresses, all of which serve as potent sites for hydrogen accumulation and subsequent crack nucleation [4,5]. Experimental evidence on carbon steels consistently indicates that while hydrogen has a limited effect on the ultimate tensile strength (UTS), it severely compromises ductility and fracture toughness, triggering a transition from ductile void coalescence to brittle cleavage or quasi-cleavage fracture modes [3,4,5,7].
The susceptibility to HE varies markedly across these weld regions [6,8]. While some literature identifies the heat affected zone (HAZ) as the most vulnerable region due to its complex microstructure and high defect density [6], other studies suggest that the filler metal may exhibit higher susceptibility depending on the grain boundary density and the distribution of dislocation networks [8]. Such discrepancies underscore that vulnerability is not intrinsic to a specific region, but is instead heavily dependent on the parent material, the specific welding procedure, and any subsequent thermal treatments. These variables collectively dictate the local microstructure, residual stress profiles, and chemical composition, rendering it difficult to designate a universally most vulnerable zone without direct experimental validation of the specific weld in question.
Thermal treatments have emerged as a critical strategy for engineering these microstructural characteristics to improve hydrogen resistance [9,10,11]. For instance, martensitic structures, characterized by high dislocation densities, often exhibit extreme susceptibility to HE, whereas ferritic or tempered structures generally demonstrate improved resilience [9]. Because hydrogen transport and trapping are strongly governed by microstructural features such as grain size, dislocation density, and precipitate distribution [12], thermal treatments can substantially alter hydrogen behavior in steels. Crucially, research suggests that the distribution and nature of the traps (reversible vs. irreversible) are more influential than the total hydrogen content [9].
In the specific case of welded pipelines, Post-Weld Heat Treatment (PWHT) is employed to modulate residual stresses, reduce dislocation density, and optimize phase distribution [10,11]. Stress-relief treatments typically lower the dislocation density, although they may not significantly enhance HE resistance if the underlying phase morphology remains unchanged [10]. More aggressive treatments, such as normalizing or quenching and tempering, can fundamentally alter the phase composition and refine the grain structure, although they may introduce new trapping sites, such as fine carbides [10,12]. The overall effect of PWHT is therefore a complex trade-off between the reduction of driving forces (residual stress) and the modification of the material’s intrinsic susceptibility (microstructure).
Adding to this complexity, several interacting factors further complicate hydrogen behavior in welded steels. Microstructural heterogeneity, inclusion chemistry, and residual stresses act synergistically to control the initiation and propagation of cracks [13,14]. Inclusions, particularly sulfides and oxide-based inclusions, are frequently identified as the dominant crack initiation sites due to their role as hydrogen traps and stress concentrators [13,14]; in certain instances, the influence of these inclusions may prevail over that of the surrounding microstructure in determining the ultimate failure behavior [14]. Zhang et al. [14] examined this interaction by applying targeted thermal treatments to specimens extracted separately from the base metal, HAZ, and weld metal of an X65 longitudinal pipeline weldment. Their results identified Ti-rich inclusions as dominant crack-initiation sites in the weld metal, while the fine interlocking acicular-ferrite microstructure was more effective in arresting propagating cracks than the polygonal-ferrite and lath-bainite microstructures produced by heat treatment. This distinction is important because a treatment may modify resistance to crack propagation without eliminating the microstructural features responsible for crack initiation. However, the treatments employed by Zhang et al. were designed to isolate selected microstructural variables in small, zone-specific specimens rather than to represent normative PWHT applied to a complete welded coupon. Furthermore, hydrogen was introduced by electrochemical precharging rather than through testing in high-pressure gaseous hydrogen.
The effect of thermal treatment on HE susceptibility has also been examined in homogeneous pipeline-steel base material. Yadav et al. [11] applied subcritical, intercritical, and intercritical-plus-tempering treatments to API 5L X70 steel and evaluated the resulting response after cathodic electrochemical hydrogen charging. The intercritical-plus-tempering condition exhibited the lowest HE index and retained a predominantly ductile fracture mode after charging. This response was associated with lower hardness, coarse cementite precipitation, recovery and recrystallization of the ferritic matrix, and a more favourable crystallographic texture. However, the study considered homogeneous base material rather than an actual welded joint and therefore did not address simultaneous deformation or competition among the base metal, HAZ, and filler metal. Moreover, hydrogen was introduced electrochemically rather than through exposure to high-pressure gaseous hydrogen.
The welding process route also plays a decisive role in defining the microstructure upon which PWHT subsequently acts [15,16]. Different welding techniques generate distinct thermal histories and consequently different grain sizes, phase distributions, local strain states, and hydrogen-transport characteristics [15]. Kim et al. [16] compared all-GTAW and combined GTAW–SMAW welds in ASTM A106 Grade B carbon-steel pipe under four thermal conditions: as-welded, 635 °C for 1 h, 650 °C for 2 h, and a sequential treatment combining 635 °C for 1 h followed by 650 °C for 2 h. Following electrochemical hydrogen precharging, the response to the two more intensive PWHT conditions differed between the welding routes. The combined GTAW–SMAW welds retained higher reduction of area than the all-GTAW welds after the 650 °C treatment and the sequential treatment, suggesting an interaction between welding route and PWHT condition. The authors associated this behavior with differences in grain size, pearlite fraction, strain distribution, and fracture morphology. Although the experimental design allowed the welding routes and PWHT conditions to be compared, the individual contributions of these concurrent microstructural changes could not be isolated. Furthermore, only subcritical stress-relief treatments were considered, and the joints were tested after electrochemical hydrogen precharging rather than under high-pressure gaseous hydrogen.
Related investigations using simulated HAZ material and actual welds under gaseous hydrogen further demonstrate the importance of specimen and environmental representativeness. Guo et al. [17] applied welding-simulated coarse-grain HAZ (CGHAZ) thermal cycles to X80 and S690QL steels, producing coarse-grained martensitic/bainitic microstructures with increased hardness. The simulated conditions exhibited severe hydrogen-induced ductility losses during SSRT with in-situ electrochemical charging, particularly in S690QL, whose simulated specimens fractured within the elastic regime. In contrast, Bortot et al. [18] evaluated partly mechanized GMAW girth welds in P690QL2 quenched-and-tempered steel using fracture-toughness testing in 200 bar gaseous hydrogen. Local CGHAZ hard spots approaching 340 HV1 were associated with tearing instabilities in HAZ specimens. Adjustment of the welding procedure and an increase in PWHT temperature and holding time substantially reduced these hard spots, after which additional HAZ specimens exhibited stable crack growth in hydrogen.
Despite the breadth of existing research, there remains a significant knowledge gap regarding the efficacy of standardized PWHT protocols on real-world girth welds under industrially relevant hydrogen pressures. Many studies rely on simplified model materials or isolate single variables, leaving a need for systematic evaluations that combine realistic welding processes, normative PWHT conditions, and high-pressure mechanical testing in hydrogen environments. Accordingly, the present study evaluates four material conditions originating from the same GMAW/MAG API 5L X52N girth weld: an as-welded reference, a stress-relief treatment near the upper limit of the ASME B31.12 temperature range, a treatment marginally below its lower temperature limit, and a full normalizing treatment. Smooth cross-weld specimens were tested by SSRT in air and in 160 bar high-purity gaseous hydrogen, while homogeneous base metal specimens were tested under identical conditions as a reference. Optical microscopy, HV10 microhardness profiling, fracture-location analysis, and scanning electron microscopy (SEM) fractography were used to relate the applied treatments to the resulting microstructure and mechanical response. The objectives were to determine how these treatments affect overall welded-joint performance, compare hydrogen-to-air retention of global plastic elongation and localized reduction of area, and establish whether the preferred failure location shifts among the base metal, HAZ, and filler metal.

2. Materials and Methods

2.1. Material and Welding Procedure

The material selected for this study was seamless API 5L X52N steel pipe (diameter: 600 mm, wall thickness: 25 mm) supplied by Tubos Reunidos Group (Amurrio, Spain). Girth welds were performed using the GMAW/MAG process with ER70S-6/G3Si1 filler wire and M20 shielding gas ( Ar + CO 2 ). The chemical compositions of the X52N base metal and the filler metal are summarized in Table 1. The chemical composition of the X52N base metal was provided by the manufacturer. The composition of the ER70S-6/G3Si1 filler wire was taken from the supplier’s product data sheet. To ensure metallurgical integrity, a preheating temperature of 100 °C was applied, and the interpass temperature was limited to 220 °C.
Table 1. Chemical composition of X52N base metal and ER70S-6/G3Si1 filler wire (wt.%).
A single girth weld was produced for this study. The experimental design followed a coupon-splitting strategy to ensure that all heat-treatment conditions originated from an identical as-welded state. The procedure was as follows: (i) a quarter-circumference Section (300 mm longitudinal length) was cut from the pipe; (ii) this section was split circumferentially into two halves, each prepared with a 30° bevel angle per side; (iii) the two halves were joined by GMAW/MAG welding according to the procedure described above; (iv) the resulting welded joint was sectioned into four identical coupons by longitudinal cuts; (v) each coupon was assigned to one of the four material conditions (as-welded +3 heat treatments), with the as-welded coupon left untreated; (vi) SSRT specimens were then machined from each heat-treated coupon. All specimens for a given condition therefore originate from the same weld, differing only in the thermal post-treatment applied. As a consequence, the present results reflect a single weld event and cannot be directly extrapolated to the full population of welds produced under the same procedure. The specific welding parameters are summarized in Table 2.
Table 2. Welding parameters for the GMAW/MAG girth weld.

2.2. Post-Weld Heat Treatments

To evaluate the influence of microstructural modification and residual stress reduction on HE susceptibility, four material conditions were analyzed. The as-welded (AW) state served as a reference piece without any thermal treatment. Additionally, two stress-relief treatments (HT1 and HT3) were designed according to the ASME B31.12 normative range for P-No. 1 carbon steels. For thicknesses exceeding 20 mm, the standard prescribes a holding temperature between 595 °C and 650 °C. HT1 ( 635.1 °C) was selected near the upper boundary of the prescribed range, while HT3 ( 593.5 °C) was set 1.5 °C below the 595 °C minimum specified by ASME B31.12. This deviation exceeds any applicable tolerance of the standard and is therefore not code-compliant; however, given the small magnitude of the deviation ( 1.5 °C), it is considered sufficiently representative of the lower boundary of the stress-relief window for the purposes of this study. For these treatments, a holding time of ∼85 min was applied to exceed the minimum requirement of 2.4 min/mm, while the heating rate was capped at 335 °C/h in accordance with GR-3.6.5. Finally, a normalizing treatment (HT2) was performed via full austenitization at 911.4 °C, as permitted by ASME B31.12 GR-3.7.2 as an alternative to conventional PWHT. Following the austenitization hold, the coupon was removed from the furnace and allowed to cool in still laboratory air. The cooling rate was not instrumented. Cooling in still air is a standard practice for normalizing low-carbon pipeline steels for several reasons including: (i) the cooling rate is sufficient to transform austenite to a fine ferrite–pearlite microstructure, achieving grain refinement without the excessive thermal gradients that faster quenching would introduce; (ii) for a low-carbon steel of this composition and section size, still-air cooling is expected to favour predominantly ferritic transformation products rather than the high fractions of martensite that would be associated with quenching. It is noted that HT2 is not a conventional stress-relief PWHT but represents a more aggressive microstructural reprocessing alternative explicitly permitted by the standard. The temperature–time profiles for these treatments are illustrated in Figure 1.
Figure 1. Temperature vs. time profiles for the applied heat treatments (HT1, HT2, and HT3).

2.3. Microstructural and Hardness Characterization

The metallurgical state of the joints was characterized through optical microscopy and microhardness mapping. Samples were sectioned, polished, and etched with nital to reveal the constituent phases of the base metal (BM), filler metal (FM) and HAZ. Vickers hardness measurements (HV10) were performed along two profiling lines (R1 and R2), located approximately 1 mm from the external and root pipe surfaces, respectively. The spatial distribution of these measurement points is shown in Figure 2a. Within the HAZ, the CGHAZ measurements were positioned approximately 150–250 μ m from the fusion line. To improve local representativeness, three measurements were obtained at each CGHAZ location through a vertical arrangement of indentations (one central indentation and two additional indentations positioned above and below it). Intermediate HAZ measurements were located approximately 300 μ m from the corresponding CGHAZ positions, while fine grain HAZ measurements were positioned a further 300 μ m from the intermediate HAZ locations. Representative optical micrographs showing HV10 indentations in the CGHAZ, intermediate HAZ and fine grain HAZ are provided in the Supplementary Material. These images demonstrate that, despite the approximately 275 μ m indentation diagonal, the indentations remain predominantly within the intended metallurgical sub-regions.
Figure 2. (a) Schematic of the HV10 microhardness profiling point locations (R1, R2) and (b) location of the SSRT gauge section (red box) relative to the weld root and the HV10 testing markings within the weld.

2.4. Slow Strain Rate Testing

Mechanical degradation in hydrogen was evaluated using SSRT. Smooth specimens were machined with a nominal diameter of 6 mm and a gauge length of 28.6 mm. The samples were extracted longitudinally to the pipe (transversal to the weld) and positioned 10 mm from the weld root to ensure that the gauge section encompassed the BM, FM and HAZ, as illustrated in Figure 2b. To provide a direct reference for the base metal, homogeneous SSRT specimens were also machined from the as-received pipe in the longitudinal direction and tested in both air and high-pressure hydrogen under identical conditions (same specimen geometry, strain rate, and environment) as the cross-weld specimens.
Prior to testing, specimens were polished longitudinally up to P2400 grit SiC paper, cleaned with acetone and ethanol, and stored in a silica gel desiccator. All tests were performed using a Cortest Constant SSR/CF machine equipped with a 2.25 L high-pressure, high-temperature (HPHT) autoclave.
The tests were conducted either in ambient air as a control or in high-purity hydrogen gas (Grade 5.6, > 99.9996 % H 2 ) at a pressure of 160 bar. Tests were performed at ambient laboratory temperature (17–23 °C). To ensure gas purity, a strict purging protocol was implemented: the autoclave was purged ten times with N 2 (10 bar), leak-tested with helium at 160 bar for one hour, and finally purged ten times with H 2 (10 bar) before final pressurization. Following pressurization, a 10-min hold was allowed to stabilize temperature and pressure before the onset of loading. During loading, a constant crosshead speed of 2.86 × 10 − 4 mm/s was maintained until fracture, corresponding to a nominal strain rate of 1.0 × 10 − 5   s − 1 . Displacement was recorded using two external linear variable differential transformers (LVDTs). Because the LVDTs capture both specimen deformation and a small contribution from the load train, total displacement was not used as an assessment parameter. Instead, the plastic elongation to failure ( ε p l ) was determined in accordance with ASTM G142, where the gradient of the initial elastic region of the load–displacement curve was used to estimate the elastic component of displacement at fracture, which was then subtracted from the total displacement. The resulting plastic displacement was divided by the nominal gauge length (28.6 mm) to obtain ε p l . Yield strength was determined as the 0.2% proof stress ( R p 0.2 ). For the cross-weld conditions (AW, HT1, HT2, HT3), one specimen was tested in air and two or three in hydrogen; for the homogeneous BM reference, one specimen was tested in air and two in hydrogen. The air values therefore serve as reference baselines rather than statistically characterized populations, and the experimental variability of the air condition cannot be estimated from the present dataset. Following the tests, fracture surfaces were analyzed using SEM to identify the dominant failure mechanisms.

3. Results

3.1. Microstructural Characterization

3.1.1. Base Metal (BM)

The microstructure of the BM for all four conditions is illustrated in Figure 3. In the AW condition, the microstructure of the BM consists predominantly of a polygonal ferrite matrix with an average grain size of approximately 10 μ m , interspersed with dark-etching constituents distributed throughout the ferritic matrix. Based on the low-carbon composition of the steel and the normalizing treatment applied during pipe manufacture, these constituents are likely dominated by pearlite and cementite-containing regions. A notable feature of this condition is the presence of segregation bands, where the dark-etching constituents align with the longitudinal direction.
Figure 3. Microstructure of the BM for the four experimental conditions. SB: segregation band.
Following the stress-relief treatments (HT1 and HT3), the general phase distribution remained unchanged, as the holding temperatures ( 593.5 °C and 635.1 °C) were below the lower critical temperature ( A 1 ). However, a reduction in the optical contrast of the dark-etching constituents and a fragmentation/thinning of the segregation bands were observed. This suggests a partial spheroidization of cementite-containing constituents. Qualitative image analysis indicated that the overall amount of dark-etching features remained broadly similar following these treatments, with the most notable change being the reduced continuity and definition of the segregation bands. In contrast, the normalizing treatment (HT2 at 911.4 °C) induced a complete phase transformation. The treatment temperature was selected to exceed the expected A 3 temperature and produce full austenitization. The resulting microstructure, shown in Figure 3c, consists of refined equiaxed ferrite containing a homogeneous distribution of fine dark-etching constituents. Notably, the segregation banding observed in the AW and stress-relief conditions was almost entirely eliminated, resulting in a chemically and structurally homogenized matrix. The dark-etching features are consistent with ferrite–pearlite transformation products formed during air cooling from the austenitic region.

3.1.2. Filler Metal (FM)

The microstructure of the FM for all four conditions is illustrated in Figure 4. The FM in the AW, HT1, and HT3 conditions exhibited a comparable morphology characterized by a network of proeutectoid ferrite delineating the prior austenite grain (PAG) boundaries (average diameter ≈ 100 μ m ), with interiors composed of acicular ferrite.
Figure 4. Microstructures of the FM for the four experimental conditions. PAG: prior austenite grain boundary; AF: acicular ferrite.
High-magnification analysis (Figure 4) reveals localized differences between the micrographs. The AW specimen showed a thick and continuous proeutectoid ferrite network, while the HT1 micrograph displays a slightly finer PAG delineation. It should be emphasized that HT1 was performed at 635.1 °C, well below the lower critical temperature ( A 1 ), and therefore no grain refinement is expected. The apparent differences in PAG size and proeutectoid ferrite morphology are attributed to the inherent microstructural heterogeneity of the multipass weld and to the specific sampling locations chosen for each micrograph, reflecting local variations in cooling rates and solidification kinetics across the weld cross-section. Similarly, the HT3 condition displayed a more heterogeneous morphology; as illustrated in Figure 4d, the left side of the micrograph is dominated almost exclusively by acicular ferrite, whereas the proeutectoid ferrite network remains prominent on the right side, consistent with the spatial variation inherent to a multi-pass GMAW deposit.
The normalizing treatment (HT2) fundamentally altered the FM microstructure. The original acicular morphology was replaced by a matrix of polygonal equiaxed ferrite with an approximate grain-size range from 5 to 60 μ m . Due to the low carbon content of the ER70S-6 wire ( 0.07 wt . % C), continuous dark constituent bands were not observed. Instead, fine dark-etching features appeared dispersed throughout the ferritic matrix. Optical microscopy alone does not permit definitive identification of all dark constituents; however, these features are consistent with ferrite–pearlite.

3.1.3. Heat-Affected Zone (HAZ)

The HAZ exhibited significant gradients depending on the local thermal peak. In the AW, HT1, and HT3 conditions, the CGHAZ was characterized by extremely large PAGs (approximately > 100 μ m ) containing aligned packets of lath ferrite or bainite. The Fine-Grained HAZ (FGHAZ) showed a more chaotic and refined morphology, consisting of a mixture of fine acicular ferrite and fine laths, as seen in Figure 5 and Figure 6.
Figure 5. Microstructures of the HAZ for the four experimental conditions. PAG: prior austenite grain boundary; AF: acicular ferrite; CGHAZ: coarse-grained HAZ; FGHAZ: fine-grained HAZ.
Figure 6. High magnification microstructures of the HAZ highlighting the CGHAZ and FGHAZ regions for the four experimental conditions.
Similar to the other regions, the HT2 treatment eliminated these heterogeneities. The resulting HAZ microstructure consisted of polygonal equiaxed ferrite containing heterogeneously distributed dark-etching constituents. The coarse lath-like microstructures characteristic of the AW condition were no longer observed following normalizing.

3.2. Hardness Analysis

Vickers microhardness profiles (HV10) were used to quantify the metallurgical state of the joints and the efficacy of the PWHT, as illustrated in Figure 7. In the BM, HT1 and HT3 resulted in a slight hardness decrease (150–160 HV10) compared to the AW state (≈160–170 HV10), consistent with dislocation recovery. HT2 showed slightly higher and more uniform values (165–180 HV10), attributed to the grain refinement achieved during normalizing.
Figure 7. Vickers microhardness profiles (HV10) for X52N steel in as-welded and after three different PWHT conditions (HT1, HT2, HT3), subdivided by metallurgical zone (BM, HAZ, and FM).
The HAZ exhibited the most significant gradients. In the AW condition, hardness values ranged between 165 and 235 HV10. In HT1 and HT3, peaks reached 240–260 HV10, with maxima approaching 290 HV10 in HT3. Because measurements were obtained from different locations in a heterogeneous multipass weld, these differences cannot be assigned unambiguously to the treatments applied. Possible contributions include local variations in the original CGHAZ microstructure and carbide redistribution during subcritical treatment. Conversely, HT2 produced the most homogeneous profile across the entire joint, with HAZ values dropping to 150–185 HV10 due to the disappearance of hardened lath phases.
In the FM, a clear decreasing trend in hardness was observed: AW > HT 3 > HT 1 > HT 2 . The difference between HT3 and HT1 is most notable at the weld root (R2). The AW FM (180–220 HV10) is reinforced by the acicular ferrite. HT1 and HT3 induced a reduction in hardness via the tempering of acicular ferrite and the reduction of dislocation density. The most drastic drop was observed in HT2 (≈135–160 HV10), where the transformation from an acicular ferrite-dominated microstructure to a more homogeneous polygonal ferritic microstructure significantly reduced the intrinsic hardness of the weld.

3.3. Effect of PWHT on HE Susceptibility

The mechanical response of the welded joints under hydrogen exposure was evaluated using SSRT, with the resulting stress-strain curves of all tested specimens, including the homogeneous BM reference, presented in Figure 8. Table 3 lists the individual results for each specimen, followed by statistical summaries: the mean ± sample standard deviation for specimens that fractured in the same metallurgical zone (e.g., both AW specimens that fractured in the BM); and the global mean ± SD across all hydrogen specimens for that condition regardless of fracture location.
Figure 8. Stress-strain curves obtained from all SSRT tests for X52N welded joints (AW, HT1, HT2, HT3) and homogeneous base metal (BM) reference specimens, tested in air (dashed lines) and high-pressure hydrogen (solid lines, 160 bar).
Table 3. Mechanical properties for each specimen and statistical summaries per PWHT condition. “Zone” indicates the metallurgical region (FM: filler metal, BM: base metal) in which the fracture surface was located on the cross-section at the moment of final failure. Individual specimens are listed first, followed by zone-specific (for specimens fracturing in the same zone, N ≥ 2) and global means ± sample standard deviation (ddof = 1). YS: yield strength; UTS: ultimate tensile strength; RA: reduction of area; ε p l : plastic elongation to failure. The HEI row reports the ratio for each parameter, defined as the global H 2 mean divided by the corresponding air value ( X ¯ H 2 / X air ).
As observed, the UTS remained nearly constant when comparing tests conducted in air and hydrogen for the AW, HT1, and HT3 conditions. However, the normalizing treatment (HT2) resulted in notably lower UTS and yield strength values compared to the other conditions, with average UTS and YS of 477.1 MPa and 301.7 MPa, respectively, versus approximately 537–553 MPa (UTS) and 404–408 MPa (YS) for the remaining conditions. The UTS values in hydrogen (477–553 MPa) are broadly comparable to those in air (470–543 MPa) for each condition, with deviations of less than 3% relative to the corresponding air values. This is consistent with HE in this steel primarily affecting the strain to failure rather than the maximum tensile strength.
It should be noted that for AW and HT1, the global mean combines specimens that fractured in both the BM and the FM, whereas for HT2 and HT3 all specimens fractured exclusively in the FM. Direct comparison of these global means therefore reflects the overall welded-joint performance rather than the response of a single metallurgical region. Moreover, the FM-fractured subgroup for AW and HT1 is represented by a single specimen per condition.
The impact on ductility, measured by the Reduction of Area (RA) and plastic elongation to failure ( ε p l ), was more pronounced. In air, RA values were consistent across all conditions, ranging between 73% and 80%, including HT2. Conversely, exposure to hydrogen caused a sharp decline in RA. The homogeneous BM reference exhibited the lowest global RA ( 38.1 ± 2.1 % ), indicating a severe loss of local ductility at fracture. Among the cross-weld conditions, AW and HT1 exhibited comparable behavior, with global means of 52.6 ± 4.7 % and 53.7 ± 3.7 % , respectively. Given the overlap of their standard deviations and the limited air replicate (N = 1 per condition), this comparison indicates comparable rather than statistically indistinguishable behavior. HT3 showed lower RA values ( 49.0 ± 3.2 % ), while the normalizing treatment (HT2) exhibited the lowest global RA among the cross-weld conditions ( 43.6 ± 7.1 % ), with the largest specimen-to-specimen variability (range: 38.5–48.6%). This suggests that while HT2 may improve air-ductility, the resulting microstructure is particularly susceptible to accelerated crack propagation under hydrogen exposure during final fracture.
Regarding plastic elongation (illustrated in both Figure 8 and Figure 9), the homogeneous BM reference presented the highest value in air ( 29.5 % ), followed by HT2 (≈26%), confirming that the cross-weld specimens are limited by the weaker FM. In hydrogen, the BM reference retained a global ε p l of 20.4 ± 0.8 % , comparable to HT2 ( 20.7 % ) and higher than the stress-relief conditions. Among the cross-weld specimens, HT1 showed better elongation in air ( 23.9 % ) compared to the AW ( 22.2 % ) and HT3 ( 21.5 % ) states. In hydrogen, the elongation followed the trend of the RA: the AW ( 17.9 ± 0.9 % ) and HT1 ( 17.3 ± 2.6 % ) conditions performed similarly, while HT3 was slightly lower ( 15.4 ± 0.2 % ).
Figure 9. Distribution of RA, UTS, and plastic elongation values broken down by testing environment and fracture location (BM vs. FM) for the different PWHT conditions.
As a normalized measure of HE susceptibility, the HE Index (HEI) was computed as the ratio of the global H 2 mean to the corresponding air value for each condition: HEI = X ¯ H 2 / X air (see Table 3).
For RA, the HEI values are: BM 0.50 , AW 0.66 , HT1 0.73 , HT2 0.57 , and HT3 0.65 . For ε p l , the HEI values are: BM 0.69 , AW 0.81 , HT1 0.72 , HT2 0.80 , and HT3 0.72 . The BM reference exhibits the lowest HEI for both metrics, suggesting that the homogeneous polygonal ferrite microstructure is intrinsically more susceptible to hydrogen-induced embrittlement than the cross-weld conditions. The two metrics yield different rankings for HT2 among the cross-weld conditions: the lowest HEI RA (0.57) but a relatively preserved HEI ε p l (0.80), comparable to the as-welded value (0.81). RA is a measure of the localized deformation at the final fracture event and is therefore sensitive to the rate of crack propagation at failure, whereas ε p l reflects the cumulative plastic strain capacity of the specimen and is penalized if hydrogen-induced microcracks reduce the effective load-bearing cross-section at an early stage of loading.
It is acknowledged that ε p l is a global measure averaged over the gauge length, which encompasses the BM, HAZ, and FM. Local strain partitioning between these regions cannot be resolved with the present displacement measurement, and the reported values do not represent the intrinsic ductility of the specific metallurgical region in which the fracture surface is located. Nevertheless, because the fracture of the weakest link governs the overall deformation capacity of the specimen, the relative comparison between BM- and FM-fractured specimens within the same condition remains a valid qualitative indicator of the preferred crack nucleation site.
Finally, the distribution of these results broken down by fracture location (BM vs. FM) in Figure 9 and Table 3 reveals a critical shift in failure behavior. In air, 100% of the samples failed in the FM regardless of the heat treatment, identifying the FM as the naturally weakest link. In hydrogen, however, a divergence occurred: all HT2 and HT3 samples continued to fail in the FM, but a significant portion of the AW and HT1 samples (2 out of 3) failed in the BM. Notably, the samples that failed in the BM exhibited lower plastic elongation than those that failed in the FM. This is interpreted as a shift of the preferred crack nucleation site toward the BM under hydrogen influence, although the nucleation site was not directly observed. The homogeneous BM reference (Table 3, ε p l = 29.5% in air, 20.4% in H 2 ) provides a direct baseline: the HEI ε p l of 0.69 for the BM confirms a severe hydrogen-induced degradation of the base metal deformation capacity, and the substantially lower ε p l of BM-fractured cross-weld specimens relative to this air value reflects the combined effect of HE and the local weakening of the BM within the heterogeneous weld.

3.4. Fracture Zone and Mechanisms

The analysis of fracture surfaces via SEM revealed a clear transition in failure mechanisms induced by hydrogen. Figure 10 presents the fracture morphology of the AW specimen tested in air. A classic ductile “cup-and-cone” fracture is observed at low magnification (Figure 10a), while the high-magnification image of the central region (Figure 10b) reveals a surface entirely covered by fine micro-void coalescence (dimples) with sizes below 10 μ m . This morphology was comparable across all four heat treatment conditions in air, confirming that without hydrogen, the material fails via extensive plastic deformation and ductile void coalescence regardless of the thermal treatment.
Figure 10. SEM fractographic analysis of the AW condition for the specimen tested in air. (a) Low magnification (×19) of AW specimen in air. (b) High magnification (×500) of central region showing dimples.
In contrast, specimens tested in hydrogen displayed mixed-mode fracture morphologies, combining ductile tearing with regions of severe embrittlement, as illustrated in Figure 11. The fracture surfaces shown in Figure 11 correspond to one representative specimen per condition, selected to illustrate the dominant fracture mode observed. The relative proportions of brittle and ductile regions are described qualitatively. The characteristics varied according to the heat treatment and the fracture zone for the specific specimens shown:
  • As-welded (FM failure): Figure 11a,e show a semi-elliptical brittle crack characterized by transgranular cleavage and small secondary cracks. The remainder of the surface maintained a ductile dimple morphology, indicating that embrittlement affected only a fraction of the cross-section before final mechanical overload.
  • HT1 (BM failure): As seen in Figure 11b,f, this condition exhibited the most prominent secondary cracks (SC), visible both on the fracture surface and the cylindrical side of the specimen. The fracture was dominated by a large brittle transgranular cleavage region covering nearly half the surface.
  • HT2 (FM failure): Figure 11c,g reveal a distinct crack growth mode characterized by a multiplicity of small cracks initiating at the circumference and subsequently coalescing. These regions exhibited a flatter quasi-cleavage morphology. Quasi-cleavage is a type of brittle fracture that occurs on planes not typically associated with cleavage, characterized by fine, river-like markings that run approximately parallel to the crack propagation direction; these markings originate within the grain and, on opposing fracture surfaces, exhibit a ridge-to-ridge matching pattern [19].
  • HT3 (FM failure): The fracture surface showed two semi-elliptical cracks of unequal size growing from opposite sides of the circumference (Figure 11d). These cracks exhibited differing brittle surfaces; the high-magnification image (Figure 11h) corresponds to the rougher region with a higher density of secondary cracks. The opposite side (not shown) exhibited a quasi-cleavage surface more similar to that observed for the HT2 condition (Figure 11g).
Regardless of the heat treatment, all hydrogen-tested specimens retained a final region of ductile dimples. This indicates that once the hydrogen-induced brittle cracks reach a critical size, the remaining ligament undergoes rapid mechanical overload, failing in a ductile manner, as there is insufficient time for further hydrogen diffusion.
Figure 11. SEM fractographic analysis of representative specimens tested in high-pressure hydrogen. Top row: low magnification (×19) overview, where yellow outlines denote the HE crack regions, and labels indicate HE (hydrogen embrittlement), DT (ductile tearing), and SC (secondary cracks). The location where each high-magnification image (bottom row) was captured is marked with a small yellow × in the top row.

4. Discussion

4.1. Preferential Fracture of the Filler Metal in Air

The SSRT results conducted in air demonstrated a consistent behavior across all experimental conditions (AW, HT1, HT2, and HT3), where all specimens fractured within the FM. This indicates that, in the absence of hydrogen, the FM is the most critical region of the welded joint, acting as the primary site for failure initiation. From a mechanical perspective, this behavior correlates with the intrinsic ductility of the different metallurgical regions. While the BM exhibits a plastic elongation of 29.5% in air (Table 3), the values obtained for the FM in the AW, HT1, and HT3 conditions ranged between 21.5% and 23.9%. This difference confirms that the FM is inherently more prone to fracture than the BM under tensile loads in air. This behavior can be explained by the characteristic microstructure of the ER70S-6 filler metal. The FM presents a morphology composed of a proeutectoid ferrite network at the PAG boundaries and an interior dominated by acicular ferrite. According to [20], the relationship between these phases is decisive for mechanical properties. While acicular ferrite generally benefits toughness due to its fine lath structure that deflects cracks, the presence of continuous proeutectoid ferrite networks at grain boundaries can create preferential paths for failure propagation and reduce overall plastic deformation capacity [20]. Similarly, ref. [21] note that an increase in proeutectoid ferrite interrupts the interconnection of acicular ferrite, favoring straighter crack paths and reducing the energy required for fracture. Therefore, the observed morphology in the FM, with a marked grain-boundary ferrite network, explains its lower relative ductility compared to the ferrite-pearlite structure of the BM.
The influence of heat treatments on the FM is clearly reflected in the hardness profiles. In the FM, hardness followed a decreasing order: AW > HT 3 > HT 1 > HT 2 . The differences between the AW state and the PWHT (HT1 and HT3) are relatively moderate and can be attributed primarily to the reduction of welding residual stresses and a slight recovery of dislocation density in the acicular ferrite. However, the normalizing treatment (HT2) caused a drastic drop in hardness, a direct consequence of the deep microstructural transformation where the acicular ferrite and proeutectoid structures were replaced by a matrix of equiaxed polygonal ferrite and fine pearlite. This homogenization effect is consistent with a previous study [22], which indicates that normalizing eliminates hardened phases and reduces dislocation density, resulting in decreased hardness and increased toughness and ductility. Indeed, in air SSRT results, HT2 exhibited the highest plastic elongation (≈26%), confirming that the transition to a more homogeneous ferritic microstructure following normalizing improves FM ductility at the expense of mechanical strength. This behavior aligns with previous findings [23,24], which indicate that normalizing homogenizes the joint microstructure, eliminating heterogeneity induced by the welding thermal cycle and providing an optimal balance between strength and ductility.

4.2. Susceptibility to Embrittlement in the Filler Metal

SSRT results reveal a contrasting phenomenon in the FM when comparing behavior in air versus hydrogen. While the normalizing treatment optimized ductility in air (26.0%), this advantage was reduced but not eliminated in hydrogen (20.7%), where HT2 still exhibited the highest ε p l among the conditions tested. In contrast, the RA was the lowest of the group ( 43.6 ± 7.1 % ).
This indicates that the homogenized ferritic microstructure produced by normalizing, although superior in air, offers no significant advantage against HE compared to the original acicular ferrite and proeutectoid structure. In fact, HT2 incurred a loss of mechanical strength (notably lower UTS) without obtaining a proportional gain in ductility under hydrogen. This finding is consistent with studies identifying acicular ferrite as one of the most resistant phases to hydrogen. Previous reports [25,26,27] indicate that the chaotic and interlaced lath morphology of acicular ferrite hinders crack propagation and is associated with greater resistance to hydrogen-induced cracking. In the present observations, the lower HEI RA of HT2 relative to the acicular-ferrite conditions (HT3, AW) is consistent with this reported behavior, although direct crack-growth rate measurements are not available to quantify the difference.
The divergence between HEI RA and HEI ε p l for HT2 (0.57 vs. 0.80) is consistent with the fractographic evidence. A plausible interpretation, although neither the onset of cracking nor the crack-growth rate was directly measured, is that the homogenized ferritic microstructure does not markedly increase the propensity for early microcrack nucleation (hence the relatively preserved HEI ε p l ), but that once cracks do initiate, as evidenced by the multiplicity of small cracks observed at the circumference, they propagate with a relatively rapid loss of local ductility at the final stage (hence the pronounced reduction in HEI RA ).

4.3. Susceptibility to Embrittlement in the Base Metal

Fracture zone analysis confirms that the BM exhibits critical susceptibility to HE under certain conditions. While air fractures occurred exclusively in the FM, a significant portion of AW and HT1 specimens fractured in the BM when exposed to hydrogen. Notably, these specimens exhibited lower plastic elongation than those failing in the FM, suggesting that the BM may be the zone most prone to crack nucleation at lower deformation levels.
As noted in the Results, the global ε p l is predominantly governed by the weakest link; the substantially lower values of BM-fractured specimens relative to the homogeneous BM baseline (29.5%, Table 3) therefore reflect a severe hydrogen-induced degradation of the BM. The direct BM reference tested in hydrogen ( HEI ε p l = 0.69, the lowest of all conditions) further quantifies the intrinsic susceptibility of the ferrite–pearlite BM microstructure, independent of the weld-related heterogeneity.
This high susceptibility is related to the nature of the ferritic microstructure and its heterogeneity. According to [28], banded ferrite-pearlite structures, where ferrite/pearlite interfaces and segregation bands act as preferential fracture sites, exhibit higher vulnerability to crack initiation and propagation than more homogeneous structures containing acicular ferrite. This is consistent with the prominent secondary cracks observed in the BM (Figure 11b), reinforcing the idea that this microstructure facilitates hydrogen accumulation and hydrogen-induced fracture.
However, comparing BM fracture conditions, HT1 specimens showed lower plastic elongation than AW specimens. This suggests that stress-relief treatments in the applied temperature range do not improve, and may even slightly degrade, BM ductility under hydrogen. This could be related to the modification of trap nature due to PWHT; the partial spheroidization of cementite-containing constituents and fragmentation of segregation bands may have modified the distribution of hydrogen traps, affecting critical accumulation at certain nucleation points.

4.4. Influence of Residual Stresses

It should be noted that residual stresses, dislocation density, and hydrogen trapping characteristics were not directly measured in the present study. The discussion below therefore presents these factors as plausible mechanisms consistent with the available literature, rather than as experimentally demonstrated effects.
Residual stresses act as a thermodynamic driver for hydrogen diffusion and as a multiplier of stress intensity at crack tips. According to [29], residual stresses generate hydrostatic stress gradients that control hydrogen distribution, inducing local enrichment in maximum stress zones, often coinciding with weld interfaces. The effectiveness of PWHT in mitigating this effect is based on temperature-induced plastic relaxation, which reduces the equivalent stress intensity factor. As demonstrated by [30], the reduction of residual stresses via PWHT prevents the system from reaching the hydrogen-induced critical toughness K I H , allowing for more stable crack propagation. In these results, HT1 showed slightly superior behavior compared to HT3 and AW in the FM, although this comparison is based on a single FM-fractured specimen for both AW and HT1; the observed trend is nonetheless consistent with, though not conclusive evidence of, a contribution from stress relief and reduced dislocation density, as proposed by [16,31].
Nonetheless, the lower ductility of HT1 compared to AW in the BM suggests that stress relaxation is not the sole governing factor. This may be because the BM is further from the tensile stress peaks of the weld, or because PWHT eliminated compressive residual stresses that otherwise act as barriers to crack propagation. Additionally, partial spheroidization of pearlite may have created more critical accumulation sites [14]. Thus, while PWHT is highly effective in the FM by reducing stress intensity, its effect on the BM is more complex. Furthermore, the possible redistribution of welding residual stresses that may have occurred during specimen machining cannot be ruled out and represents an additional source of uncertainty when attributing the observed differences to the heat treatment alone.

5. Conclusions

This study evaluated the impact of various post-weld heat treatments on the susceptibility to HE of X52N welded joints. The results show that the material response is highly dependent on the metallurgical zone and the induced microstructural transformation:
  • Critical zones: In air, the FM is the weakest zone, as all specimens fractured in the FM regardless of heat treatment. In hydrogen, the fracture location shifted from the FM to the BM for several conditions, accompanied by a reduction in global ε p l ; this is interpreted as a shift in the preferred crack nucleation site toward the BM, although the nucleation site was not directly observed.
  • Effect of normalizing: While normalizing optimizes air-ductility and homogenizes the joint, it is counterproductive in hydrogen. Based on reduction of area ( HEI RA = 0.57, the lowest among the cross-weld conditions), normalizing produces the most severe loss of local ductility at fracture. However, the global plastic-elongation retention ( HEI ε p l = 0.80) remains comparable to the as-welded condition (0.81), indicating that the homogenized microstructure is more susceptible to hydrogen at the final fracture stage than during early crack nucleation.
  • Efficacy of acicular ferrite: The observed fracture behavior and embrittlement indices are consistent with the original acicular ferrite microstructure being more resistant to the advance of brittle hydrogen-induced cracks than the ferrite structure resulting from normalizing.
  • Optimization via PWHT:The stress-relief treatment HT1 (≈635 °C) likely represents the best balance; its single FM-fractured specimen exhibits higher RA and ε p l than those of HT3, a behavior consistent with the reduction of residual stresses and dislocation density expected for this treatment.
  • Failure mechanisms: HE induces a transition toward cleavage and quasi-cleavage fracture modes, with the base metal being the most prone to secondary cracking and failure at lower deformation levels.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/met16121303/s1, Tables S1–S3: furnace temperature profiles for HT1, HT2, and HT3, respectively. Table S4: Vickers hardness (HV10) measurements along profiling lines R1 and R2 for all conditions. Table S5: raw SSRT data (force, displacement, stress, strain, time) for all specimens. Tables S6–S10: processed mechanical property results (YS, UTS, RA, ε p l , and HEI ratios) for the AW, HT1, HT2, HT3, and BM conditions, respectively. Figure S1: Optical micrographs of HV10 indentations in the CGHAZ, intermediate HAZ, and FGHAZ sub-regions (HT1 condition) demonstrating that the indentation footprint remains within a single metallurgical sub-region.

Author Contributions

Conceptualization, U.D.F.V. and N.V.M.; methodology, U.D.F.V.; validation, U.D.F.V. and N.G.G.; formal analysis, U.D.F.V. and N.G.G.; investigation, U.D.F.V.; resources, P.B.U.; data curation, U.D.F.V. and N.G.G.; writing—original draft preparation, U.D.F.V.; writing—review and editing, N.V.M. and P.B.U.; visualization, U.D.F.V.; supervision, N.V.M.; project administration, P.B.U.; funding acquisition, N.V.M. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the Basque Government through the ELKARTEK Programme under project ONTZHi II, Grant No. KK-2025/00109.

Data Availability Statement

The original contributions presented in the study are included in the article/Supplementary Materials, further inquiries can be directed to the corresponding author.

Acknowledgments

The authors would like to express their gratitude to Tubos Reunidos Group, with special thanks to Elisa Sal Broco and Jon Barco for providing the materials used in this study. We also thank Mikel Basurco and Jose Manuel Iglesias (TECNALIA) for their technical support in sample preparation and the acquisition of SEM images. Additionally, the authors acknowledge Ferrocal Steel Solutions S.L. for their contribution in performing the welding process.

Conflicts of Interest

All authors were employed by Tecnalia. The authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.

References

  1. Mielich, T.; Dobler, R.; Hollnagel, J.; Akca, O.; Müller-Kirchenbauer, J. Europe’s way from natural gas to green hydrogen: Modeling and simulation of the transforming European gas transport infrastructure. Int. J. Hydrogen Energy 2025, 135, 156–171. [Google Scholar] [CrossRef] [Scilit]
  2. Haeseldonckx, D.; D’haeseleer, W. The use of the natural-gas pipeline infrastructure for hydrogen transport in a changing market structure. Int. J. Hydrogen Energy 2007, 32, 1381–1386. [Google Scholar] [CrossRef] [Scilit]
  3. Bedő, T.; Lukács, J.; Szabó, G. The effect of hydrogen on the integrity of steel pipes used in natural gas transmission systems. IOP Conf. Ser. Mater. Sci. Eng. 2026, 1348, 012009. [Google Scholar] [CrossRef] [Scilit]
  4. Zekun, Y.; Zhanli, Y.; Hao, Y.; Yan, Z.; Kai, X. Hydrogen embrittlement in welded joints of high-strength pipeline steels: A review of mechanisms, characterization, and mitigation strategies. Int. J. Press. Vessel. Pip. 2025, 218, 105615. [Google Scholar] [CrossRef] [Scilit]
  5. Kovács, J.; Lukács, J. Systematic review of factors influencing the integrity of pipeline girth welds exposed to hydrogen. Weld. World 2026, 70, 53–74. [Google Scholar] [CrossRef] [Scilit]
  6. Yanachkov, B.; Valuiska, K.; Mourdjeva, Y.; Krastev, R.; Dyakova, V.; Simeonova, T.; Petrov, R.; Kolev, K.; Cauwels, M.; Depover, T. Investigation of Welded Joints of Pipelines from an Existing Gas Transmission Network Exposed to Hydrogen—Part I: Structure, Mechanical Properties and Susceptibility to Hydrogen Embrittlement. Metals 2026, 16, 388. [Google Scholar] [CrossRef] [Scilit]
  7. Yang, P.; Li, R.; Zhang, J.; Zhao, L.; Gong, J.; Liu, C.; Li, Y. Study on the Hydrogen Compatibility of X70 Pipeline Steel and Its Weldments. Corros. Sci. 2026, 113962. [Google Scholar] [CrossRef] [Scilit]
  8. Wang, H.; Ming, H.; Wang, J. Evaluation of hydrogen embrittlement susceptibility differences among the weld, heat-affected zone, and base metal in welded pipeline steel. J. Mater. Sci. 2026, 61, 1806–1821. [Google Scholar] [CrossRef] [Scilit]
  9. Mohtadi-Bonab, M.; Szpuna, J.A.; Collins, L.; Stankievech, R. Evaluation of hydrogen induced cracking behavior of API X70 pipeline steel at different heat treatments. Int. J. Hydrogen Energy 2014, 39, 6076–6088. [Google Scholar] [CrossRef] [Scilit]
  10. Jack, T.A.; Nnoka, M.; Zhang, J.; Szpunar, J. Investigating the hydrogen diffusion and cracking susceptibility of pipeline steels after various heat treatments. Eng. Fail. Anal. 2024, 161, 108311. [Google Scholar] [CrossRef] [Scilit]
  11. Yadav, S.; Jack, T.A.; Davani, R.K.Z.; Ohaeri, E.; Szpunar, J. Effect of post-processing heat treatment on hydrogen embrittlement susceptibility of API 5L X70 pipeline steel. Int. J. Press. Vessel. Pip. 2022, 199, 104762. [Google Scholar] [CrossRef] [Scilit]
  12. Lan, L.; Kong, X.; Hu, Z.; Qiu, C.; Zhao, D.; Du, L. Hydrogen permeation behavior in relation to microstructural evolution of low carbon bainitic steel weldments. Corros. Sci. 2016, 112, 180–193. [Google Scholar] [CrossRef] [Scilit]
  13. Tabas, A.K.; Beidokhti, B.; Kiani-Rashid, A. Comprehensive study on hydrogen induced cracking of electrical resistance welded API X52 pipeline steel. Int. J. Hydrogen Energy 2021, 46, 1012–1022. [Google Scholar] [CrossRef] [Scilit]
  14. Zhang, P.; Laleh, M.; Hughes, A.E.; Marceau, R.K.; Hilditch, T.; Tan, M.Y. A study on hydrogen embrittlement of a high-strength pipeline steel weldment after microstructure manipulation by targeted heat treatments. Int. J. Hydrogen Energy 2025, 97, 1199–1211. [Google Scholar] [CrossRef] [Scilit]
  15. Zhang, R.; Wang, C.; Zhang, T.; Zhang, H.; Liu, C.; Zhu, M.; Zhang, J.; Ning, Y.; Xia, Z.; Li, Y. Effect of welding processes on hydrogen embrittlement susceptibility of pipeline steel welded joints. Corros. Sci. 2025, 258, 113396. [Google Scholar] [CrossRef] [Scilit]
  16. Kim, Y.; Kim, J.; Kim, D.; Han, S.; Hwang, B.; Choe, B. Effect of welding process combination and PWHT conditions on hydrogen embrittlement susceptibility of carbon steel pipe welded joints. SSRN Prepr. 2026, 6777495. [Google Scholar] [CrossRef] [Scilit]
  17. Guo, X.; Li, T.; Sheng, Z.; Christ, M.; Sharma, R.; Söker, M.; Reisgen, U.; Bleck, W. Impact of welding simulated heat treatment on hydrogen embrittlement behavior of high-strength fine-grained steels. Eng. Fail. Anal. 2022, 140, 106602. [Google Scholar] [CrossRef] [Scilit]
  18. Bortot, P.; Ortolani, M.; Sileo, M.; Escorza, E.; Connolly, M.; Buck, Z.N.; Chandra, A. Investigation of the fracture resistance of high strength ferritic steel welds in gaseous hydrogen environment. Int. J. Hydrogen Energy 2025, 136, 777–788. [Google Scholar] [CrossRef] [Scilit]
  19. Martin, M.L.; Fenske, J.A.; Liu, G.S.; Sofronis, P.; Robertson, I.M. On the formation and nature of quasi-cleavage fracture surfaces in hydrogen embrittled steels. Acta Mater. 2011, 59, 1601–1606. [Google Scholar] [CrossRef] [Scilit]
  20. Edmonds, D.; Cochrane, R. Structure-property relationships in bainitic steels. Metall. Trans. A 1990, 21, 1527–1540. [Google Scholar] [CrossRef] [Scilit]
  21. Peng, L.; Hong, R.; Ma, Q.-L.; Liu, N.-S.; Yin, S.-B.; Jia, S.-J. Effect of Copper in Gas-Shielded Solid Wire on Microstructural Evolution and Cryogenic Toughness of X80 Pipeline Steel Welds. Materials 2025, 18, 3519. [Google Scholar] [CrossRef] [Scilit]
  22. Chung, P.; Ham, Y.; Kim, S.; Lim, J.; Lee, C. Effects of post-weld heat treatment cycles on microstructure and mechanical properties of electric resistance welded pipe welds. Mater. Des. 2012, 34, 685–690. [Google Scholar] [CrossRef] [Scilit]
  23. Dodo, M.; Ause, T.; Adamu, M.; Ibrahim, Y. Effect of post-weld heat treatment on the microstructure and mechanical properties of arc welded medium carbon steel. Niger. J. Technol. 2016, 35, 337–343. [Google Scholar] [CrossRef] [Scilit]
  24. Joshua, T.; Fayomi, O.; Olatuja, F.; Inegbenebor, A. Hardness and microstructural behavior of normalized Steel-Welded joint under varying temperature. Procedia Manuf. 2019, 35, 1375–1382. [Google Scholar] [CrossRef] [Scilit]
  25. Mendoza, D.C.R.; Hurtado Delgado, E.; Reyes Valdés, A. Análisis del Efecto Microestructural en el Agrietamiento por Hidrógeno en Uniones Soldadas por SAW de Acero API 5L-X70. In Foro de Ingeniería e Investigación en Materiales; Aguilar, E.A., Bedolla, E., Léon, C.A., Eds.; Instituto de Investigación en Metalurgia y Materiales, UMSNH: Morelia, Mexico, 2016; Volume 13; pp. 1–8. [Google Scholar]
  26. Beidokhti, B.; Dolati, A.; Koukabi, A. Effects of alloying elements and microstructure on the susceptibility of the welded HSLA steel to hydrogen-induced cracking and sulfide stress cracking. Mater. Sci. Eng. A 2009, 507, 167–173. [Google Scholar] [CrossRef] [Scilit]
  27. Nguyen, T.T.; Tak, N.; Park, J.; Nahm, S.H.; Beak, U.B. Hydrogen embrittlement susceptibility of X70 pipeline steel weld under a low partial hydrogen environment. Int. J. Hydrogen Energy 2020, 45, 23739–23753. [Google Scholar] [CrossRef] [Scilit]
  28. Jack, T.A. Investigation of Hydrogen Induced Cracking Susceptibility of API 5L X65 Pipeline Steels. Master’s Thesis, Department of Mechanical Engineering, University of Saskatchewan, Saskatoon, SK, Canada, 2021. [Google Scholar]
  29. Xue, J.; Cheng, A.; Bai, C.; Ji, L. Research on residual stress and hydrogen diffusion of X80 pipeline welded joint. Front. Mater. 2023, 10, 1215843. [Google Scholar] [CrossRef] [Scilit]
  30. Tang, H.; Shen, C.; Xu, M.; Zheng, W.; Sun, C.; Lv, L.; Wei, H.; Wei, L.; Hua, Z. Effect of welding residual stress on hydrogen-induced fracture and fatigue life of X80 pipeline girth welded joints. Eng. Fract. Mech. 2025, 325, 111352. [Google Scholar] [CrossRef] [Scilit]
  31. Gao, Z.; Wu, S.; Xiang, T.; Gong, B.; Deng, C. Coupling effect of post-weld heat treatment and fatigue damage on the hydrogen embrittlement of X80 steel welded joints. J. Mater. Res. Technol. 2024, 31, 2646–2657. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.